Blow Molding
A foam blow-molded article using a mixed resin of polyolefin and olefin thermoplastic elastomer with a specific ratio and phase formation addresses cold impact resistance and surface smoothness issues, achieving lightweight articles with enhanced mechanical properties.
Patent Information
- Application Number
- JP2021012132
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-28
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-01-28
AI Technical Summary
Conventional foam blow-molded articles made from polyolefin resins with added elastomers suffer from issues with cold impact resistance and surface smoothness, particularly when aiming for low apparent density and high expansion ratios.
A foam blow-molded article composed of a mixed resin of polyolefin resin and olefin thermoplastic elastomer, with a specific weight ratio and melting point difference, forming a continuous phase with a closed cell ratio of 70% or more, and optionally containing carbon black, to enhance cold impact resistance and surface smoothness.
The solution results in a foam blow-molded article with excellent lightness, cold impact resistance, and surface smoothness, maintaining mechanical strength and heat resistance.
Smart Images

Figure 0007576987000008 
Figure 0007576987000009 
Figure 0007576987000010
Abstract
Description
[Technical field]
[0001] The present invention relates to a foamed blow-molded article, and more particularly to a foamed blow-molded article excellent in light weight, cold impact resistance and surface smoothness. [Background technology]
[0002] A foamed blow-molded article produced by a method combining blow molding and foaming techniques has been known. The foamed blow-molded article is obtained by a foam blow molding method in which a base resin and a foaming agent are melt-kneaded using an extruder, the resulting foamable resin melt is extruded from a die as a foamed parison, the foamed parison is sandwiched between split dies, and pressurized gas is blown into the sealed parison to press the foamed parison against the inner surface of the die to give it a shape.
[0003] The foamed blow molded articles thus obtained are lightweight, have excellent heat insulating properties, and can be formed into various shapes, and are therefore used as air conditioning ducts for vehicles such as automobiles, etc. In this case, polyolefin resins, particularly polypropylene resins, are used as the base resin for the foamed blow molded articles because of their high heat resistance and excellent mechanical strength.
[0004] For example, when the foam blow molded article is used as an air conditioning duct for a vehicle, impact resistance may be required. In the conventional foam blow molding method, attempts have been made to add an elastomer to the polyolefin resin such as the polypropylene resin as a means for improving the impact resistance (Patent Document 1, Patent Document 2). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2014-37149 A [Patent Document 2] JP 2014-240743 A Summary of the Invention [Problem to be solved by the invention]
[0006] As disclosed in Patent Documents 1 and 2, it was possible to improve impact resistance by adding an elastomer to a polyolefin resin. However, the methods described in Patent Documents 1 and 2 sometimes left problems in cold impact resistance of the obtained foamed blow molded article, and sometimes the surface smoothness of the foamed blow molded article was reduced. This phenomenon was particularly noticeable when attempting to obtain a foamed blow molded article with a low apparent density and a high expansion ratio.
[0007] An object of the present invention is to obtain a blow-molded foam having excellent light weight, cold impact resistance and surface smoothness. [Means for solving the problem]
[0008] According to the present invention, there is provided the following foamed blow molded article. [1] A foamed blow molded article made of a mixed resin consisting of a polyolefin resin (A) and an olefin thermoplastic elastomer (B), The olefin-based thermoplastic elastomer (B) is an olefin block copolymer, the weight ratio (A:B) of the polyolefin resin (A) to the olefin thermoplastic elastomer (B) is 80:20 to 40:60; the olefin-based thermoplastic elastomer (B) forms a continuous phase in the mixed resin constituting the foamed blow molded article, The apparent density of the foamed blow molded body is 100 kg / m 3 More than 450kg / m 3 is as follows: The foamed blow molded article has a closed cell rate of 70% or more. [2] The foamed blow molded article according to item 1, wherein the polyolefin resin (A) has a melting point (Ta) of 110°C or more and 170°C or less, the olefin thermoplastic elastomer (B) has a melting point (Tb) of 50°C or more and 130°C or less, and the melting point difference (Ta-Tb) between the melting point (Ta) and the melting point (Tb) is 0°C or more and 80°C or less. [3] The foamed blow molded article according to 1 or 2 above, wherein the mixed resin contains carbon black, and the content of the carbon black is 0.1 to 2 parts by weight per 100 parts by weight of the total of the polyolefin resin (A) and the olefin thermoplastic elastomer (B). Effect of the Invention
[0009] According to the present invention, the foamed blow-molded product is composed of a mixed resin consisting of a polyolefin resin (A) and an olefin block copolymer (olefin thermoplastic elastomer (B)), the weight ratio of the two components forming the mixed resin is within a specific range, the olefin block copolymer forms a continuous phase in the mixed resin forming the foamed blow-molded product, and the foamed blow-molded product has an apparent density and a closed cell ratio within specific ranges, thereby making it possible to obtain a foamed blow-molded product that is lightweight, has excellent cold impact resistance, and has excellent surface smoothness. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a photograph of a cross section of a bubble film of the foamed blow molded article obtained in Example 1. [Diagram 2] FIG. 2 is a photograph of a cross section of the bubble film of the foamed blow molded article obtained in Example 5. [Diagram 3] FIG. 3 is a photograph of a cross section of a bubble film of the foamed blow molded article obtained in Comparative Example 4. [Figure 4] FIG. 4 is an explanatory diagram showing an example of an apparatus used in the production method of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The foamed blow molded article of the present invention will be described in detail below. The foamed blow molded article (hereinafter also referred to as molded article) of the present invention is composed of a mixed resin consisting of a polyolefin resin (A) and an olefin thermoplastic elastomer (B).
[0012] The polyolefin resin (A) is one in which the olefin component structural unit is present in the resin in a molar ratio of 50 mol % or more, preferably 60 mol % or more, and more preferably 80 to 100 mol %. Specific examples of polyolefin-based resins include homopolymers of olefins, copolymers of olefins, copolymers of an olefin component and another polymerizable monomer component copolymerizable with an olefin, in which the proportion (mol %) of the olefin component structural unit present satisfies the above-mentioned range, and mixtures of olefin polymers and other polymers, in which the proportion (mol %) of the olefin component structural unit present satisfies the above-mentioned range. More specific examples of polyolefin resins include polyethylene resins such as high-density polyethylene, low-density polyethylene, linear low-density polyethylene, etc., and polypropylene resins such as propylene homopolymers (homopolypropylene), propylene-ethylene copolymers, etc. Among these, polypropylene resins are more preferred from the viewpoint of obtaining molded articles having excellent mechanical strength.
[0013] The flexural modulus of the polyolefin resin (A) is preferably 100 MPa or more, more preferably 300 MPa or more, and even more preferably 500 MPa or more. The upper limit is preferably 2500 MPa, more preferably 2100 MPa. When the flexural modulus of the polyolefin resin is within the above range, the foamed blow molded article has better rigidity. The flexural modulus can be measured based on JIS K7171:2016.
[0014] The olefin-based thermoplastic elastomer (B) used in the present invention is an olefin block copolymer. By using the olefin block copolymer, it is possible to improve the impact resistance of the foamed blow molded article as well as the cold impact resistance while maintaining the foamability. Therefore, the foamed blow molded article has excellent lightness and surface smoothness. In the present invention, the block copolymer refers to a copolymer in which a plurality of polymer chains are bonded as blocks, and examples of the block copolymer include a block copolymer consisting of a hard segment and a soft segment.
[0015] Preferred examples of the olefin block copolymer include ethylene-based elastomers and propylene-based elastomers, and the olefin block copolymer preferably contains 50 mol % or more of an olefin component unit. Examples of the ethylene-based elastomer include block copolymers having high-density ethylene as a hard segment and ethylene-octene random copolymer as a soft segment. A specific example is the product name "INFUSE (registered trademark)" (manufactured by The Dow Chemical Company).
[0016] Examples of the propylene-based elastomer include block copolymers having a microcrystalline region made of isotactic propylene as a hard segment and an amorphous region of a copolymer of propylene and ethylene as a soft segment, etc. A specific example is the product name "Vistamax" (manufactured by ExxonMobil Corporation).
[0017] The flexural modulus of the olefin-based thermoplastic elastomer (B) is preferably 5 MPa or more and less than 100 MPa, more preferably 7 MPa or more and 80 MPa or less, and even more preferably 10 MPa or more and 50 MPa or less, from the viewpoint of excellent impact resistance and further excellent cold impact resistance. The flexural modulus can be measured in accordance with JIS K7171:2016.
[0018] In addition to the polyolefin resin (A) and the olefin thermoplastic elastomer (B), the mixed resin constituting the foamed blow molded article of the present invention may contain thermoplastic resins such as polystyrene resins and other thermoplastic elastomers (TPEs) other than olefin block copolymers within a range that does not impair the intended effects of the present invention. However, the amount of other components is preferably 30 parts by weight or less, more preferably 20 parts by weight or less, even more preferably 10 parts by weight or less, and particularly preferably 5 parts by weight or less, based on 100 parts by weight of the total of the polyolefin resin (A) and the olefin thermoplastic elastomer (B).
[0019] The mixed resin constituting the foamed blow molded article may be appropriately blended with additives such as flame retardants, flow regulators, ultraviolet absorbers, conductivity imparting agents, antistatic agents, colorants, heat stabilizers, antioxidants, inorganic fillers, etc., as desired, provided that the blending amount of these additives is preferably 20 parts by weight or less, more preferably 10 parts by weight or less, and even more preferably 5 parts by weight or less, per 100 parts by weight of the total of the polyolefin resin (A) and the olefin thermoplastic elastomer (B).
[0020] In the mixed resin, the weight ratio (A:B) of the polyolefin resin (A) to the olefin thermoplastic elastomer (B) is 80:20 to 40:60. If the weight ratio of the olefin-based thermoplastic elastomer (B) is less than 20% by weight, the cold impact resistance of the resulting foamed blow-molded article may be reduced, and the desired cold impact resistance may not be achieved.If the weight ratio of the olefin-based thermoplastic elastomer (B) is more than 60% by weight, the foamability of the mixed resin may be reduced, making it difficult to obtain a foamed blow-molded article with a low apparent density, and the surface smoothness of the resulting foamed blow-molded article may be reduced. For these reasons, the weight ratio (A:B) is preferably 75:25 to 45:55, and more preferably 70:30 to 50:50. The total of the polyolefin resin (A) and the olefin thermoplastic elastomer (B) is 100.
[0021] In the production of the foamed blow molded article of the present invention, defective molded products with burrs, dimensional deviations, etc. are generated, and these burrs and defective molded products may be used as recycled raw materials. As the recycled raw materials, those containing the polyolefin resin (A) and the olefin thermoplastic elastomer (B) are preferably used. When a recycled raw material containing the polyolefin resin (A) and the olefin thermoplastic elastomer (B) is used as part of the raw material, the blending amounts of the polyolefin resin (A) and the olefin thermoplastic elastomer (B) in the mixed resin constituting the foamed blow molded product are values including the polyolefin resin (A) and the olefin thermoplastic elastomer (B) in the recycled raw material.
[0022] The melting point (Ta) of the polyolefin resin (A) is preferably from 110 to 170° C., more preferably from 130 to 168° C., and even more preferably from 140 to 165° C. If the melting point (Ta) is within this range, a foamed blow molded article having excellent heat resistance can be obtained.
[0023] The melting point (Tb) of the olefin-based thermoplastic elastomer (B) is preferably 50°C or higher and 130°C or lower, more preferably 80°C or higher and 125°C or lower, and even more preferably 90°C or higher and 120°C or lower.
[0024] The melting point difference (Ta-Tb) between the melting point (Ta) and the melting point (Tb) is preferably 0 to 80° C., more preferably 10 to 70° C., even more preferably 20 to 60° C., and most preferably 25 to 50° C. If the melting point difference (Ta-Tb) is within this range, it is believed that better foam moldability is exhibited and a foam blow molded article with better surface smoothness can be obtained, particularly due to the small difference in the melting point between the olefin elastomer (B) and the polyolefin resin (A) during cooling in the foam blow molding.
[0025] The melting point of the polyolefin resin (A) or the olefin thermoplastic elastomer (B) refers to the melting peak temperature measured based on heat flux differential scanning calorimetry as described in JIS K7121:2012. The test piece is conditioned as described in "(2) Measurement of melting temperature after a certain heat treatment", and the heating rate and cooling rate are both 10°C / min. When multiple melting peaks appear on the DSC curve, the apex temperature of the melting peak with the largest area is taken as the melting point.
[0026] The polyolefin resin (A) used in the present invention preferably has a melt viscosity (ηa) of 1000 to 1800 Pa·s at a temperature of 170° C. and a shear rate of 100 / sec. If the melt viscosity is within this range, by forming a foamed parison at an appropriate foaming temperature, excessive drawdown of the foamed parison is prevented, while excessive shear heat generation in the die is prevented, and the foamed parison is prevented from becoming open cells, which leads to a decrease in the closed cell ratio of the foamed blow-molded article. From this viewpoint, the melt viscosity (ηa) of the polyolefin resin (A) at a temperature of 170°C and a shear rate of 100 / sec is preferably 1100 to 1600 Pa s, more preferably 1200 to 1500 Pa s.
[0027] The olefin-based thermoplastic elastomer (B) used in the present invention preferably has a melt viscosity (ηb) of 400 Pa·s to 2000 Pa·s at a temperature of 170° C. and a shear rate of 100 / sec. If the melt viscosity is within this range, it becomes easier to form a morphology in which a continuous phase of the olefin-based thermoplastic elastomer (B) is formed in a mixed resin consisting of the polyolefin-based resin (A) and the olefin-based thermoplastic elastomer (B) in the foamed blow molded article. From this viewpoint, the melt viscosity (ηb) of the olefin-based thermoplastic elastomer (B) at a temperature of 170° C. and a shear rate of 100 / sec is preferably 500 to 1800 Pa·s, more preferably 600 to 1700 Pa·s.
[0028] The ratio (ηb / ηa) of the melt viscosity of the olefin thermoplastic elastomer (B) at a temperature of 170°C and a shear rate of 100 / sec to the melt viscosity of the polyolefin resin (A) at a temperature of 170°C and a shear rate of 100 / sec is preferably 0.4 to 1.5, and more preferably 0.5 to 1.3. When the ratio (ηb / ηa) is within the above range, the kneadability of the polyolefin resin (A) and the olefin thermoplastic elastomer (B) is improved, and it becomes easier to form a continuous phase of the olefin thermoplastic elastomer (B) when a foamed blow-molded product is formed.
[0029] The melt viscosity of the polyolefin resin (A) and the olefin thermoplastic elastomer (B) is measured under the conditions of an orifice diameter of 1 mm, an orifice length of 10 mm, a temperature of 170° C., and a shear rate of 100 / sec. For example, a Capillograph 1D manufactured by Toyo Seiki Seisakusho Co., Ltd. can be used as the measuring device.
[0030] When the foamed blow molded article of the present invention is used as an automobile component such as a duct, it is preferable that the mixed resin contains a black pigment and the foamed blow molded article is black. In this case, the black pigment is preferably carbon black for coloring, since a deep color tone can be obtained with a small amount. Examples of the carbon black include gas furnace black, oil furnace black, acetylene black, channel black, roller black, thermal black, and ketjen black.
[0031] The carbon black content in the mixed resin is preferably 0.1 to 2 parts by weight, more preferably 0.3 to 1 part by weight, per 100 parts by weight of the polyolefin resin (A) and the olefin thermoplastic elastomer (B) combined. When a recycled raw material containing carbon black is used as part of the raw material in producing a foamed blow molded article, the total carbon black content of the mixed resin includes the carbon black in the recycled raw material.
[0032] In the present invention, the olefin-based thermoplastic elastomer (B) must form a continuous phase in the mixed resin constituting the foamed blow molded article. The olefin-based thermoplastic elastomer (B) forms a continuous phase, which results in a foamed blow molded article having excellent cold impact resistance and surface smoothness. Here, the olefin-based thermoplastic elastomer (B) forms a continuous phase in the resin constituting the foamed blow molded product means that the olefin-based thermoplastic elastomer (B) forms a phase that exists in a line or band shape along the longitudinal direction of the bubbles (direction perpendicular to the thickness direction of the bubbles) on the cross-sectional photograph of the bubble film of the foamed blow molded product. The formation of such a continuous phase improves the resistance of the bubble film to cold shocks and improves the surface smoothness of the foamed blow molded product. The cross-sectional photograph of the bubble film of the foamed blow molded product is a photograph of the part where the longitudinal bubble film constituting the bubbles and the thickness bubble film intersect.
[0033] The length of the continuous phase is preferably about 5 μm or more. Furthermore, in the continuous phase, the ratio (L / D) of the length in the bubble film direction (longitudinal length) L to the length in the bubble film thickness direction (transverse length) D is preferably about 10 or more, and the proportion of the phase is preferably 50% or more.
[0034] In addition, it is preferable that the polyolefin resin (A) and the olefin thermoplastic elastomer (B) are incompatible. The polyolefin resin (A) may be a continuous phase or a dispersed phase, but in order to improve the foam moldability, it is preferable that the polyolefin resin (A) also forms a continuous phase on the cross-sectional photograph.
[0035] The reason why the cold impact resistance is improved when the olefin-based thermoplastic elastomer (B) forms a continuous phase in the mixed resin is that the continuous phase formed continuously in the longitudinal direction of the bubble film absorbs impact, and the continuous phase is formed in layers within the bubble film, preventing the expansion of cracks caused by impact.
[0036] The apparent density of the foamed blow molded body is 100 to 450 kg / m 3 If the apparent density is too small, the foamed blow molded article will have excellent light weight, but the mechanical strength will decrease and the foamed blow molded article will be easily broken by impact, and as a result, the impact resistance and cold impact resistance of the foamed blow molded article may decrease. If the apparent density is too large, the foamed blow molded article may lose its light weight. For these reasons, the apparent density is set to 120 kg / m 3 More than 400kg / m 3 is preferable, and more preferably 130 kg / m 3 More than 350kg / m 3 More preferably, 150 kg / m 3 More than 250kg / m 3 The following is the result.
[0037] In the present invention, the apparent density (D) of the foamed blow molded article [g / cm 3 ] can be calculated as follows: For a total of three vertical cross sections in the longitudinal direction of the foamed blow molded body, near the longitudinal center and both ends, select four equally spaced locations on the circumferential flat portion of each vertical cross section, and measure the area of the area in plan view to approximately 10 cm. 2 Then, for each test piece, its weight Wi [g] is calculated by dividing the volume Vi [cm 3 The apparent density (D) of each test piece is calculated by dividing the obtained value by the mass ratio (Wi / Vi) and converting the unit. The arithmetic average of these values is the apparent density (D). The volume of each test piece, Vi [cm 3 ] can also be determined by measuring the external dimensions of the test specimen or by submerging the test specimen in water.
[0038] The average thickness of the foamed blow molded article of the present invention varies depending on the shape of the foamed blow molded article to be desired, but is usually preferably 1 mm to 5 mm, more preferably 1.2 mm to 4 mm, even more preferably 1.4 mm to 3 mm, and particularly preferably 1.5 mm to 2.5 mm. If the average thickness is within this range, the foamed blow molded article will have an excellent balance between light weight and impact resistance.
[0039] The apparent density (kg / m 3 ) and the average thickness (mm) is 350 to 700 kg mm / m 3 When the product is within the above range, the foamed blow molded article has an excellent balance between the resin amount per unit area and impact resistance, and impact resistance is effectively exhibited even in a lightweight foamed blow molded article. From this viewpoint, the apparent density (kg / m 3 The upper limit of the product of the compressive strength (MPa) and the average thickness (mm) of the foamed blow molded article is more preferably 600 kg mm / m 3 and more preferably 500 kg mm / m 3 On the other hand, the lower limit is preferably 400 kg mm / m 3 It is.
[0040] The foamed blow molded article must have a closed cell rate of 70% or more. If the closed cell ratio is less than 70%, the surface smoothness of the foamed blow molded article may decrease, and for this reason, the closed cell ratio is preferably 80% or more, and more preferably 85% or more.
[0041] In this specification, the closed cell ratio is measured as follows. Test pieces are cut out from the resulting foamed blow molded article, and Vx is measured according to (Procedure C) of ASTM D2856-70 (recertified in 1976), and calculated according to the following formula. Note that any parts with crushed cells are excluded from the measurement. Closed cell ratio (%)=(Vx-W / ρ)×100 / (Va-W / ρ) Vx: True volume of the test piece (the sum of the volume of the closed cell portion and the volume of the resin composition) (cm 3 ) Va: Apparent volume of the test piece calculated from the outer dimensions of the test piece (the sum of the volume of the closed cell part, the volume of the open cell part, and the volume of the resin composition) (cm 3 ) W: weight of test piece (g) ρ: density of the resin composition constituting the test piece (g / cm 3 ) The resin composition can be obtained by removing air bubbles from a test piece by, for example, heat pressing. As a measuring device, for example, an air comparison type specific gravity meter (Model: 930) manufactured by Toshiba Beckman Co., Ltd. can be used.
[0042] The samples used for the measurement of the closed cell ratio are preferably collected by the same method as that used for measuring the apparent density of the foamed blow-molded article described above. The samples are used to measure the closed cell ratio according to the above-mentioned measurement method, and the arithmetic average value thereof is regarded as the closed cell ratio of the foamed blow-molded article.
[0043] The foamed blow molded article of the present invention has excellent cold impact resistance. Specifically, the average Charpy impact strength at -10°C is 1.0 kJ / m 2 It is preferable that the concentration is 1.5 kJ / m or more. 2 More preferably, it is equal to or higher than 2.0 kJ / m 2 The upper limit is preferably the measured value when the measurement sample is in a non-destructive state after the measurement, and is approximately 10 kJ / m 2 It is.
[0044] The Charpy impact strength at -20℃ is 0.5kJ / m 2 For this reason, it is preferable that the electric field strength is 1.0 kJ / m or more. 2 More preferably, it is equal to or greater than 1.5 kJ / m 2 The upper limit is preferably about 9 kJ / m when the foamed blow molded article is in a non-destructive state after the measurement. 2 It is.
[0045] In this specification, the Charpy impact value is measured based on JIS K7111-1:2012.
[0046] Next, an example of the manufacturing method of the foamed blow molded article of the present invention will be described with reference to the drawings. First, as shown in FIG. 4, in an extruder (not shown), a foamable molten resin obtained by kneading a mixed resin consisting of a polyolefin resin (A) and an olefin thermoplastic elastomer (B), a black pigment, and a physical foaming agent is extruded from a die 2 between split molds 3, 3 of a desired shape located immediately below the die to form a foamed parison 1 (extrusion foaming process). Next, the lower part of the foamed parison 1 in a softened state is closed by a pinch (not shown), and gas is blown into the foamed parison to increase the internal pressure and expand the foamed parison (pre-blowing process). After the pre-blowing process or while the pre-blowing process is being performed, the molds 3, 3 are closed to sandwich the foamed parison 1 between the molds (mold clamping process). Gas is blown into the hollow part of the foamed parison 1 sandwiched between the molds 3, and the outer surface of the foamed parison 1 is pressed against the inner surface of the mold to form a hollow shape (blow molding process). After cooling, the foamed blow molded article with burrs is taken out of the mold and the burrs are removed to obtain a hollow foamed blow molded article. Note that waste materials such as burrs and defective foamed blow molded articles are collected (raw material recovery process) and reused as recovered raw materials. Although a cylindrical foam parison is illustrated in FIG. 4, a sheet-shaped foam parison may also be used. In the method for producing a foamed blow-molded article according to the present invention, it is preferable to place an accumulator between the extruder and the die 3 or within the die.
[0047] Examples of the foaming agent include aliphatic hydrocarbons such as propane, normal butane, isobutane, normal pentane, isopentane, normal hexane, isohexane, and cyclohexane, chlorinated hydrocarbons such as methyl chloride and ethyl chloride, fluorohydrocarbons such as 1,1,1,2-tetrafluoroethane and 1,1-difluoroethane, aliphatic ethers such as dimethyl ether, diethyl ether, and methyl ethyl ether, aliphatic alcohols such as methyl alcohol and ethyl alcohol, organic physical foaming agents such as dialkyl carbonates such as dimethyl carbonate and diethyl carbonate, inorganic physical foaming agents such as carbon dioxide, nitrogen, air, and water, and chemical foaming agents such as sodium hydrogen carbonate, sodium citrate, and azodicarbonamide. These foaming agents can be used alone or in combination.
[0048] When the foamed parison 1 is formed using the inorganic physical foaming agent, the foaming is completed early and the foaming agent is hardly or completely left in the resin, so that the resin is not plasticized and drawdown is prevented. As a result, a foamed parison having excellent blow moldability is obtained compared to that obtained using an organic physical foaming agent. From this viewpoint, among the above-mentioned foaming agents, it is preferable to use an inorganic physical foaming agent, it is more preferable to use an inorganic physical foaming agent containing carbon dioxide, and it is even more preferable to use a physical foaming agent consisting only of carbon dioxide.
[0049] In the present invention, when a blowing agent containing carbon dioxide is used as a physical blowing agent, the carbon dioxide is preferably blended in an amount of 20 to 100 mol %, more preferably 50 to 100 mol %, and even more preferably 70 to 100 mol %, based on 100 mol % of the physical blowing agent. When the carbon dioxide content is within the above range, a foamed blow molded article having a small bubble diameter and a high closed cell ratio can be easily obtained.
[0050] The amount of the physical foaming agent added is preferably 0.05 to 0.8 mol, and more preferably 0.1 to 0.5 mol, per 1 kg of the mixed resin. EXAMPLES
[0051] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples. The resins, elastomers, black pigments and talc used in the production of foamed blow molded articles in the examples and comparative examples are shown below.
[0052] Polyolefin resin (A) (1) Abbreviation "WB140": "Branched homopolypropylene 'Daploy WB140HMS'" manufactured by Borealis The physical properties of each polyolefin resin (A) are shown in Table 1.
[0053] Olefin-based thermoplastic elastomer (B) (1) Abbreviation "V6202": ExxonMobil Chemical Corporation: Olefin-based thermoplastic elastomer "Vistamax 6202" (2) Abbreviation "V6102": ExxonMobil Chemical Corporation: Olefin-based thermoplastic elastomer "Vistamax 6102" (3) Abbreviation "IN9530": "Infuse 9530" manufactured by Dow Chemical Japan Co., Ltd. (4) Abbreviation "IN9507": "Infuse 9507" manufactured by Dow Chemical Japan Co., Ltd. (5) "TDF8200": "Tafmer DF8200" manufactured by Mitsui Chemicals, Inc. (6) "TDF640": "Tafmer DF640" manufactured by Mitsui Chemicals, Inc. (7) "TDF605": "Tafmer DF605" manufactured by Mitsui Chemicals, Inc. (9) "CQ100F": "Catalloy Q100F" manufactured by Basell Ltd. Various physical properties of each olefin-based thermoplastic elastomer (B) are shown in Table 1.
[0054] [Table 1]
[0055] Styrenic thermoplastic elastomer (1) Abbreviation "H1062": "Hydrogenated styrene-based thermoplastic elastomer (SEBS)" manufactured by Asahi Kasei Corporation, product name "Tuftec H1062" (density 890 kg / m 3 , Melt viscosity (170℃, 100sec -1 :3240Pa·s)
[0056] Carbon Black (CB) Masterbatch Abbreviation "MB1": Carbon black-containing master batch: Product name "PP Black Master Batch, BT920F-JSJ" (manufactured by B&Tech Corporation, CB concentration 45% by weight)
[0057] Air bubble regulator Talc masterbatch: Product name "Hifiller #12" (manufactured by Matsumura Sangyo, talc concentration 20% by weight, median diameter 7.5 μm)
[0058] Examples 1 to 8, Comparative Examples 1 to 10 The polyolefin resin (A), olefin thermoplastic elastomer (B), carbon black masterbatch and talc masterbatch shown in Tables 2 and 3 in their respective amounts were fed to an extruder with a 65 mm aperture, melted and kneaded in the extruder to form a molten resin, and carbon dioxide (CO 2) was pressed into the mold so that the amount (mol / kg) per 1 kg of the mixed resin of the polyolefin resin (A) and the olefin thermoplastic elastomer (B) was shown in Tables 2 and 3, and further kneaded to obtain a foamable molten resin. The foamable molten resin was filled into an accumulator connected to an extruder. At a foaming temperature of 170°C, the foamable molten resin was extruded into a normal pressure range from an annular die arranged at the end of the accumulator, and foamed to form a cylindrical foamed parison. The foamed parison was placed between two-part molds arranged directly under the die, and the opening of the foamed parison was pinched, and then the two-part molds were closed while blowing pre-blow air into the foamed parison, and the foamed parison was sandwiched between the molds. The outer surface of the foamed parison was pressed against the inner surface of the mold by blowing air into the sandwiched foamed parison from a blow pin and sucking air from a hole provided in the mold to reduce the pressure in the space between the outer surface of the foamed parison and the inner surface of the mold, and the foamed parison was shaped to have the shape of the inner surface of the mold. After cooling, the mold was opened, the molded body was taken out, and flash and pockets were removed to obtain a duct-shaped hollow foamed blow molded body with a maximum length of 650 mm and a maximum width of 180 mm. The physical properties and evaluations of the foamed blow molded bodies obtained in the examples and comparative examples are shown in Tables 4 and 5.
[0059] [Table 2]
[0060] [Table 3]
[0061] [Table 4]
[0062] [Table 5]
[0063] Examples 9 and 10 Using the foamed blow molded articles obtained in Examples 3 and 5, recycled materials 1 and 2 were produced.
[0064] Recycled Materials (1) Recycled materials 1 The foamed blow molded article obtained in Example 3 was pulverized, and the pulverized material obtained was kneaded in an extruder set at 230° C. to form a molten resin. The molten resin was extruded and pelletized to obtain a recovered raw material 1. (2) Recycled materials 2 The foamed blow molded article obtained in Example 5 was pulverized, and the pulverized material obtained was kneaded in an extruder set at 230° C. to form a molten resin. The molten resin was extruded and pelletized to obtain a recovered raw material 2. The resin component compositions of Recycled Raw Material 1 and Recycled Raw Material 2 are shown in Table 6.
[0065] [Table 6]
[0066] Example 9 80% by weight of the recycled raw materials and 20% by weight of the new raw materials (weight ratio A:B=50:50 of polyolefin resin (A) and olefin thermoplastic elastomer (B) in the mixed resin) of the types and blending amounts shown in Table 6 were fed to an extruder with a caliber of 65 mm. The new raw materials were blended with polyolefin resin (A), olefin thermoplastic elastomer (B), carbon black master batch, and cell regulator to obtain the same blending ratio as in Example 3. Therefore, the weight ratio of polyolefin resin (A) and olefin thermoplastic elastomer (B) in the mixed resin constituting the foamed blow molded product was 50:50. Next, the mixture was melt-kneaded in the extruder, and carbon dioxide (CO 2 ) was injected so that the amount was 0.21 mol per 1 kg of the mixed resin constituting the foamed blow molded article, and further kneaded to obtain a foamable molten resin. The foamable molten resin was filled into an accumulator connected to an extruder. Next, a foamed blow molded article was obtained in the same manner as in Example 1. The physical properties and evaluation of the obtained foamed blow molded article are shown in Table 7.
[0067] Example 10 80% by weight of the recovered raw materials and 20% by weight of the new raw materials (weight ratio of polyolefin resin (A) to olefin thermoplastic elastomer (B) A:B = 70:30 parts by weight) of the types and blending amounts shown in Table 6 were fed to an extruder with a caliber of 65 mm. The new raw materials were blended with the polyolefin resin (A), olefin thermoplastic elastomer (B), carbon black master batch, and cell regulator to achieve the same blending ratio as in Example 5. Therefore, the weight ratio of polyolefin resin (A) to olefin thermoplastic elastomer (B) in the mixed resin constituting the foamed blow molded product was 70:30. Next, the mixture was melt-kneaded in the extruder, and carbon dioxide (CO 2 ) was injected so that the amount was 0.20 mol per 1 kg of the mixed resin constituting the foamed blow molded article, and further kneaded to obtain a foamable molten resin. Except for this, a foamed blow molded article was produced in the same manner as in Example 9. The physical properties and evaluation of the obtained foamed blow molded article are shown in Table 7.
[0068] [Table 7]
[0069] A cross-sectional photograph (magnification: 10,000 times) of the bubble membrane of the foamed blow molded article obtained in Example 1 is shown in Fig. 1. It can be seen that a black continuous phase originating from the olefin-based thermoplastic elastomer (B) has been formed. A cross-sectional photograph (magnification: 10,000 times) of the bubble membrane of the foamed blow molded article obtained in Example 5 is shown in Fig. 2. It can be seen that a black continuous phase originating from the olefin-based thermoplastic elastomer (B) has been formed. A cross-sectional photograph (magnification: 10,000 times) of the bubble membrane of the foamed blow molded product obtained in Comparative Example 4 is shown in Fig. 3. It can be seen that black particulate parts derived from the olefin-based thermoplastic elastomer (B) are dispersed.
[0070] Comparative Example 1 is an example in which the olefin-based thermoplastic elastomer (B) was not blended in. The obtained foamed blow molded article was poor in cold impact resistance. Comparative Example 2 is an example in which the blending amount of the polyolefin resin (A) was reduced compared to Example 3. The obtained foamed blow molded article was excellent in cold impact resistance but was poor in surface smoothness. Comparative Example 3 is an example in which the amount of polyolefin resin (A) was further reduced compared to Example 6. The obtained foamed blow molded article was excellent in cold impact resistance but inferior in surface smoothness. Comparative Examples 4 and 5 are examples in which a reactor-type olefin-based thermoplastic elastomer in which a rubber component is finely dispersed in a PP shell was used instead of the olefin block copolymer in Example 1. The obtained foamed blow molded article did not form a continuous phase derived from the olefin-based thermoplastic elastomer (B), and the component derived from the olefin-based thermoplastic elastomer (B) formed a dispersed phase, and the closed cell ratio was low and the surface smoothness was poor. Comparative Examples 6, 7, and 8 are examples in which different kinds of olefin random copolymers were used instead of the olefin block copolymer in Example 1. The obtained foamed blow molded articles had a low closed cell ratio and poor surface smoothness. Comparative Example 9 is an example in which the same olefin random copolymer as in Comparative Example 8 was used instead of the olefin block copolymer in Example 3. Although the olefin random copolymer formed a continuous phase in the obtained foamed blow molded article, the closed cell ratio was low and the surface smoothness was poor. Comparative Example 10 is an example in which a hydrogenated styrene-based thermoplastic elastomer was used instead of the olefin block copolymer in Example 2. The obtained foamed blow molded article had a low closed cell ratio and poor surface smoothness because no olefin-based thermoplastic elastomer was blended.
[0071] The physical properties in the table were measured as follows. (Apparent density, thickness) The apparent density was measured by the following method. For a total of three vertical cross sections in the longitudinal direction of the foamed blow molded body, near the longitudinal center and both ends, select four equally spaced locations on the circumferential flat portion of each vertical cross section, and measure the area of the area in plan view to approximately 10 cm. 2 Then, for each test piece, its weight Wi [g] is calculated by dividing the volume Vi [cm 3 The apparent density (Wi / Vi) of each test piece was calculated by dividing the obtained value by the unit conversion, and the arithmetic average of these values was regarded as the apparent density (D). The thickness was calculated as the arithmetic mean value of the measured values obtained by measuring the thickness of each sample using the samples whose apparent density was measured as described above. The apparent density and thickness were measured 12 times, and the arithmetic mean values of the measured values at 10 points excluding the maximum and minimum values were used as the apparent density and thickness of the foamed blow molded article.
[0072] (Closed bubble rate) The closed cell ratio was measured by the method described above.
[0073] (Cold impact resistance (-10℃ Charpy impact strength)) Ten test pieces measuring 80 mm in length, 10 mm in width, and 10 mm in thickness (thickness of the foamed blow molded body) were cut out from ten flat surfaces of the cylindrical duct-shaped foamed blow molded body. The test pieces were conditioned by placing them in an atmosphere of -10°C for 24 hours. The conditioned test pieces (with notches) were used to measure the Charpy impact strength of the test pieces in an atmosphere of -10°C based on JIS K7111-1:2012 by edgewise impact so that the side surface of the sample was the striking surface, and the arithmetic mean value of the measured values was taken as the Charpy impact strength. Individual measurements of Charpy impact strength include complete break, partial break, and non-break.
[0074] (Cold impact resistance (-20℃ Charpy impact strength)) The test piece was placed in an atmosphere of -20°C for 24 hours to condition the test piece, but the test piece was measured in the same manner as in the "-10°C Charpy impact strength".
[0075] In the table, the symbols C, H, P, and N are used with the following meanings. C: Complete break: The test specimen breaks into two or more pieces (including hinge breaks). P: Partial break: An incomplete break that does not meet the definition of a hinge break. N: Non-break The test piece simply bends on the test piece support table but does not break.
[0076] In the table, each measurement result is described as follows: The most frequently occurring failure type (C, P, N) is selected in the table, and the average impact strength for that failure type is shown in the upper column as the average impact value, and the failure type (C, P, N) is shown in the lower column. For example, in the table, the entry for -10°C in Example 1 indicates that complete failure C occurred in 10 samples (the most frequent type of failure was 10), and the average impact value was 1.4 kJ / m 2 The description in Example 2 shows that complete failure C occurred in 6 samples (the most frequent failure type was 6), and the average impact value was 2.2 kJ / m 2 This means that In addition, when the frequency of the second most frequent fracture mode is greater than 1 / 3 (3.3 / 10), the most frequent fracture mode is recorded, and the second most frequent fracture mode is added in parentheses. Specifically, in the measurement of the Charpy impact value at -10°C in Example 2, the frequency of the second most frequent fracture mode was 4 / 10, which is greater than 3.3 / 10, so C was recorded as the most frequent fracture mode, and the second most frequent fracture mode was recorded as (P).
[0077] (-10℃ drop ball test (1.5m, 1kg)) The duct-shaped foamed blow molded article was conditioned by placing it in an atmosphere of -10°C for 24 hours. The conditioned foamed blow molded article was placed on a test bench with the flat part facing up, and a 1 kg iron ball was dropped onto the flat part from 1.5 m above, and damage to the foamed blow molded article was observed. If the flat part that was hit by the falling ball bent and force was applied to parts other than the flat part, causing damage to the foamed blow molded article, the ball drop test was performed again. For each ball drop test, the cold impact resistance was evaluated according to the following criteria. ◎: Not breakable 〇: It breaks but the pieces do not fly off ×: It breaks and pieces fly off
[0078] (-10℃ drop ball test (1.5m, 0.5kg)) The ball drop test was conducted in the same manner as the "-10°C ball drop test (1.5m, 1kg)" except that a 0.5kg iron ball was used, and evaluation was performed using the same criteria.
[0079] Dispersion state in the cross section of the cell wall of the olefin-based elastomer (B) (Taking a cross-sectional photograph of the bubble film) Figures 1 to 3 are cross-sectional photographs of bubble films taken along the longitudinal direction of a cylindrical blow-molded body (the extrusion direction indicated by the arrow in Figure 4) using the following method, and are photographs of the area where the longitudinal bubble films that make up the bubbles intersect with the thickness-wise bubble films. The thickness direction of the bubbles coincides with the thickness direction of the foamed blow molded article, and the longitudinal direction of the bubbles coincides with the direction in which the foamed blow molded article is extruded.
[0080] Specifically, the measurement of the cross-sectional photograph of the bubble film was carried out as follows. A part of the obtained foamed blow molded article was cut out, and the cut sample was embedded in epoxy resin. After embedding, a surface perpendicular to the thickness direction was cut out with a glass knife, and an ultra-thin piece of the foam with a thickness of about 0.1 μm was cut out from the cross section with a diamond knife. The cut sample was placed on a Cu mesh and then cooled to 20°C. 4 Place the mixture in a petri dish with several milliliters of the aqueous solution and seal at room temperature. 4Exposure to steam and dyeing were carried out for 30 minutes. The sample was then mixed with a few ml of NaClO solution and a small spatula of RuCl 3 The crystals were placed in a petri dish together with the liquid mixed just before use and sealed at room temperature. 4 The foam plate was exposed to steam for 30 minutes for staining. Ultra-thin sections of the stained foam plate were photographed using a transmission electron microscope (JEM-1010, manufactured by JEOL Ltd.) at an acceleration voltage of 100 kV and a magnification of 10,000 times. The above photograph is a cross-section of the foamed blow molded body cut perpendicular to the circumferential direction, with the top and bottom directions of the photograph being the thickness direction of the foamed blow molded body and the direction from left to right of the photograph being the extrusion direction. The top of the photograph is the outer surface side of the foamed blow molded body, and the bottom of the photograph is the inner surface side of the foamed blow molded body.
[0081] (Inner surface smoothness) A flat portion of the duct-shaped foamed blow-molded article was cut out, and the surface smoothness of the inner surface of the flat portion of the foamed blow-molded article was visually observed and evaluated according to the following criteria. ○: The height (or depth) of adjacent peaks and valleys is 1 mm or more within 100 cm 2 There is one or less per ×: The height (or depth) of adjacent peaks and valleys of the unevenness is 1 mm or more within 100 cm 2 There are two or more per [Explanation of symbols]
[0082] 1 Foam parison 2 Die 3-piece mold
Claims
1. A foamed blow molded article made of a mixed resin of a polyolefin resin (A) and an olefin thermoplastic elastomer (B), The olefin-based thermoplastic elastomer (B) is an olefin block copolymer, the weight ratio (A:B) of the polyolefin resin (A) to the olefin thermoplastic elastomer (B) is 80:20 to 40:60; the polyolefin resin (A) has a melting point (Ta) of 110°C or more and 170°C or less, the olefin thermoplastic elastomer (B) has a melting point (Tb) of 50°C or more and 130°C or less, and the melting point difference (Ta-Tb) between the melting point (Ta) and the melting point (Tb) is 0°C or more and 80°C or less, the olefin-based thermoplastic elastomer (B) forms a continuous phase in the mixed resin constituting the foamed blow molded article, The apparent density of the foamed blow molded body is 100 kg / m 3 More than 450kg / m 3 is as follows: The foamed blow molded article has a closed cell rate of 70% or more.
2. The foamed blow molded article according to claim 1, wherein the mixed resin contains carbon black, and the content of the carbon black is 0.1 to 2 parts by weight per 100 parts by weight of the total of the polyolefin-based resin (A) and the olefin-based thermoplastic elastomer (B).
Citation Information
Patent Citations
High-flexibility super non-slip wear-resistant foam material and preparation method thereof
CN111662500A
Multilayered polypropylene resin foamed molded object, production thereof and container
JP2001047537A
Manufacturing method of polyolefin resin foamed body and polyolefin resin foamed body
JP2005194433A
Foamed blow molding and method of manufacturing the same
JP2010240892A
Method for manufacturing foamed molding, and foamed molding
JP2012030498A