Urethane resin composition
The urethane resin composition with hexamethylene diisocyanate, crude diphenylmethane diisocyanate, and an amine compound addresses bonding challenges by enhancing adhesive strength and elongation, suitable for diverse structures including vehicles.
Patent Information
- Application Number
- JP2021013483
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-29
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-01-29
AI Technical Summary
Existing adhesive technologies face challenges in bonding dissimilar materials together, particularly in structures like vehicles, requiring high adhesive strength, maximum stress, and elongation to withstand vibrations, and existing urethane resin compositions lack sufficient performance for these applications.
A urethane resin composition comprising hexamethylene diisocyanate, crude diphenylmethane diisocyanate, and an amine compound with a specific molecular weight range, along with optional additives like antioxidants and silane coupling agents, to enhance adhesive strength, maximum stress, and elongation.
The composition achieves high adhesive strength, maximum stress, and elongation, effectively bonding various structures including vehicles, demonstrating improved durability and resistance to vibrations.
Smart Images

Figure 0007576989000001 
Figure 0007576989000002 
Figure 0007576989000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a urethane resin composition that adheres civil engineering and architectural structures, such as roads, buildings, dams and embankments, which are composed of a plurality of materials and members, and mechanical structures, such as automobiles, motorcycles, trains, diesel railcars, ships and airplanes. [Background technology]
[0002] As mentioned above, various structures are made up of multiple materials and parts, and when using adhesive techniques, bonding dissimilar materials can be very difficult. Bonding structures requires high bonding reliability, whether the materials are dissimilar or homogeneous. In particular, in the case of vehicles such as automobiles, the adhesive must have high adhesive strength, and the physical properties of a hardened adhesive must be such that it does not easily break when subjected to vibrations and the like, as well as a high maximum stress and high elongation.
[0003] Patent Document 1 is a publication relating to a urethane resin composition for golf balls, but it was difficult to apply it to structural adhesion. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2003-102871 [Patent Document 2] Patent Publication 2004-204139 [Patent Document 3] Patent Publication 2009-091414 [Patent Document 4] Patent Publication No. 2015-113369
[0005] Patent Document 2 is a publication about a sealant. Although it has the performance as a sealant, it is difficult to apply it to adhesion of structures.
[0006] Patent Document 3 is a publication on a urea resin composition that can be hand-applied, has good water resistance, and is suitable for use as a peeling-prevention coating material. However, there is room for improvement in adhesive strength for use in bonding structures.
[0007] Patent Document 4 is a publication on a two-component room temperature curing urethane coating waterproofing composition. It contains a solvent, which raises concerns about its adverse effects on the environment, and there is room for improvement in adhesive strength for use in bonding structures. Summary of the Invention [Problem to be solved by the invention]
[0008] The object is to obtain a urethane resin composition which exhibits high adhesive strength when used to bond structures, and which has film properties of high maximum stress and high elongation in the cured product itself. [Means for solving the problem]
[0009] The object of the present invention is to obtain a composition comprising hexamethylene diisocyanate (A), crude diphenylmethane diisocyanate (B), and an amine compound (C) represented by formula (1) and having a number average molecular weight of 500 to 1200. Effect of the Invention
[0010] Since the urethane resin composition exhibits high adhesive strength in bonding structures, and the cured product itself has film properties that exhibit high maximum stress and high elongation, it can be used to bond a variety of structures. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] When an isocyanate compound reacts with an amine compound, a urea bond is produced, which is referred to as urethane in this application for convenience. The hexamethylene diisocyanate (HDI) of the present invention can be a commercially available product. HDI is sold by Asahi Kasei Corporation, Tosoh Corporation, Mitsui Chemicals, Inc., Wanka Chemical Co., Ltd., etc., and any of them can be used.
[0012] The crude MDI (cMDI) of the present application can be a commercially available product. cMDI is sold under the trade names Luplanate M20S, Luplanate M11S, and Luplanate M5S by BASF INOAC Polyurethanes, Millionate MR-100 by Tosoh Corporation, Millionate MR-200 by Tosoh Corporation, Millionate MR-400 by Tosoh Corporation, 44V20L by Sumika Covestro Urethanes, and SUPRASEC5005 by Huntsman. 44V20L is a more suitable material.
[0013] The amine compound (C) which is a curing agent and has a number average molecular weight of 500 to 1200 and is represented by formula (1) may be a commercially available product. A specific product name is Elasmer 650P manufactured by Kumiai Chemical Industry Co., Ltd. The number average molecular weight of Elasmer 650P is 888.
[0014] The molar ratio of the total isocyanate groups of hexamethylene diisocyanate (A) and crude diphenylmethane diisocyanate (B) to the number of moles of active hydrogen groups of an amine compound (C) having a number average molecular weight of 500 to 1200, represented by formula (1), is (number of moles of isocyanate groups) / (number of moles of active hydrogen groups)=0.7 to 1.5, more preferably (number of moles of isocyanate groups) / (number of moles of active hydrogen groups)=0.8 to 1.3.
[0015] The mass ratio of hexamethylene diisocyanate (A) to crude diphenylmethane diisocyanate (B) is crude diphenylmethane diisocyanate (B) / hexamethylene diisocyanate (A)=2-6 / 4-8, and more preferably crude diphenylmethane diisocyanate (B) / hexamethylene diisocyanate (A)=3-5 / 5-7.
[0016] In addition to hexamethylene diisocyanate (A), crude diphenylmethane diisocyanate (B), and the amine compound (C) represented by formula (1) and having a number average molecular weight of 500 to 1200, the urethane resin composition of the present application can also contain glycol-based compounds such as polyethylene glycol, polypropylene glycol, and polytetramethylene glycol, polyester polyol-based compounds, castor oil-based compounds, and alcohols such as alcohol-containing rubber, within the range that does not impair the adhesive strength and the maximum stress and elongation properties of the coating.
[0017] In addition to hexamethylene diisocyanate (A), crude diphenylmethane diisocyanate (B), and amine compound (C) represented by formula (1) and having a number average molecular weight of 500 to 1200, an antioxidant can be added to the urethane resin composition of the present application to ensure long-term adhesion within a range that does not impair the adhesive strength, maximum stress of the film properties, and elongation. Examples of the antioxidant include phosphorus-based, hydroquinone-based, bis-tris-polyphenol-based, thiobisphenol-based, and hindered phenol-based antioxidants. In addition, a silane coupling agent can be added to improve glass adhesion, as long as it does not impair the adhesive strength, the maximum stress of the film properties, and the elongation rate. Examples of the silane coupling agent include epoxy silanes such as 3-glycidoxypropylmethyldimethoxysilane and 3-glycidoxypropyltrimethoxysilane, vinyl silanes such as vinyltriethoxysilane and vinyltrimethoxysilane, methacryl silanes and acrylic silanes such as 3-methacryloxypropylmethyldimethoxysilane and 3-acryloxypropyltrimethoxysilane, mercapto silanes such as 3-mercaptopropylmethyldimethoxysilane and 3-mercaptopropyltrimethoxysilane, and amino silanes such as N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane and N-2-(aminoethyl)-3-aminopropyltrimethoxysilane.
[0018] In addition to hexamethylene diisocyanate (A), crude diphenylmethane diisocyanate (B), and the amine compound (C) represented by formula (1) and having a number average molecular weight of 500 to 1200, inorganic fillers such as calcium carbonate, talc, silica, kaolin, calcined kaolin, clay, calcium silicate, calcium sulfate, aluminum oxide (alumina), aluminum hydroxide, aluminum silicate, titanium oxide, zinc oxide, magnesium carbonate, magnesium silicate, zeolite, glass beads, and shirasu balloons can be added to the urethane resin composition of the present application, provided that the adhesive strength and the maximum stress and elongation properties of the coating are not impaired. In addition, organic fillers such as polyethylene, polypropylene, polymethyl methacrylate, ethylene-(meth)acrylic acid copolymer, ethylene-(meth)acrylic acid ester copolymer, ethylene-vinyl acetate copolymer, nylon, polyethylene terephthalate, polybutylene terephthalate, polystyrene, ABS resin, acrylonitrile-styrene copolymer, and polycarbonate can also be added.
[0019] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. Note that all parts are by weight. EXAMPLES
[0020] How to calculate the isocyanate groups (mol) of an isocyanate compound The number of moles of isocyanate groups in an isocyanate compound can be calculated by the following formula. Isocyanate group (mol) = amount added (g) x (NCO (%) / 100) x 1 / 42
[0021] How to calculate the active hydrogen group (mol) of a hardener The number of moles of active hydrogen groups in the curing agent can be calculated using the following formula. Active hydrogen group (mol) = amount added (g) x hydroxyl value (mgKOH / g) x 1 / 56110
[0022] Preparation of the composition liquid of the isocyanate compound of Example 1 In a 23°C environment, 16.8 g of hexamethylene diisocyanate (HDI, NCO [%] is 50 [%]) and 7.2 g of crude MDI (cMDI) 44V20L (NCO [%] is 31 [%]) were weighed out and stirred with a clean spatula while being careful not to introduce bubbles, to obtain a composition liquid of the isocyanate compound of Example 1.
[0023] Preparation of isocyanate compound composition liquids of Examples 2 to 5 and Comparative Examples 1 to 8 The compositions of isocyanate compounds of Examples 2 to 5 and Comparative Examples 1 to 8 were obtained in the same manner as the composition of isocyanate compounds of Example 1, with the ratios shown in Tables 1 and 2. Millionate MT (NCO [%] is 33.6 [%]) is a monomeric MDI manufactured by Tosoh Corporation. The prepolymer was obtained by weighing out 19.1 g of polypropylene glycol (product name: PP-2000) manufactured by Sanyo Chemical Industries Co., Ltd. into the kettle of a planetary mixer (product name: PLM-2) manufactured by Inoue Seisakusho Co., Ltd., dehydrating at 100°C and 6.7 kPa, confirming that the moisture content was 500 ppm or less, adding 37.2 g of Millionate MR-200, a polymeric MDI manufactured by Tosoh Corporation, replacing the system with a nitrogen atmosphere, and then reacting at 80°C for 2 hours to obtain a prepolymer (NCO [%] is 18.9 [%]).
[0024] Curing agents of Examples 1 to 5 and Comparative Examples 1 to 8 As shown in Tables 1 and 2, 100 g of Elasmer 650P (hydroxyl value: 130.4 mgKOH / g) was used as the curing agent in Examples 1 to 5, Comparative Example 1, Comparative Example 4, Comparative Example 5, and Comparative Example 8. 100 g of Elasmer 1000P (hydroxyl value: 254.0 mgKOH / g) was used as the curing agent in Comparative Examples 2 and 3, and 100 g of Elasmer 250P (hydroxyl value: 96.4 mgKOH / g) was used as the curing agent in Comparative Examples 6 and 7, and 100 g of Elasmer 250P (hydroxyl value: 96.4 mgKOH / g) was used as the curing agent, in which the number average molecular weight of Elasmer 650P is 488. In Tables 1 and 2, the isocyanate compounds are shown in parentheses as NCO (%), and the curing agents are shown in parentheses as hydroxyl values (mgKOH / g).
[0025] Preparation of compositions of Examples 1 to 5 and Comparative Examples 1 to 8 The isocyanate compound and the curing agent were weighed out in the ratios shown in Tables 1 and 2, and stirred with a clean spatula while taking care not to introduce bubbles, to prepare compositions of Examples 1 to 5 and Comparative Examples 1 to 8. Note that (moles of isocyanate groups) / (moles of active hydrogen groups) is shown on the first line, the crude MDI (:cMDI) / hexamethylene diisocyanate (:HDI) mass ratio is shown on the second line, and the curing agent / isocyanate mass ratio is shown on the third line. Note that in Comparative Examples 5 and 6, marked with (*) on the second line, monomeric MDI was used instead of crude MDI (:cMDI), so the mass ratio is (monomeric MDI / hexamethylene diisocyanate). In Comparative Examples 6 and 7, Elastomer 250P was a solid and a uniform composition could not be obtained, so that the film properties and adhesive strength were not measured.
[0026] Film property measurement The liquids of Examples 1 to 5, Comparative Examples 1 to 5, and Comparative Example 8 obtained in the previous section were each applied to silicone release paper to an area of approximately 150 mm × 150 mm × 1 mm thick, and incubated in a 23°C / 50% RH environment for one day and at 40°C for two days to obtain a cured film. Test pieces were prepared by punching out using a JIS K6251 No. 3 dumbbell. The physical properties of the film were measured using a uniaxial testing machine manufactured by INSTRON, product name: 5967. The tensile speed was 100 mm / min, the measurement environment was 23±2°C, and n=5 average. The evaluation criteria were as follows: for maximum stress, a maximum stress of 30 MPa or more was passed, and a maximum stress of less than 30 MPa was failed. For elongation, a maximum elongation of 300% or more was passed, and a maximum elongation of less than 300% was failed. The results are shown in Tables 4 and 5.
[0027] Check adhesive strength between SUS430 Two SUS430 plates, which are stainless steel plates measuring 25 mm x 100 mm x 1.5 mm thick, were prepared. The liquids of Examples 1 to 5 and Comparative Examples 2 to 4 were applied to the end of one plate at a position 12.5 mm away from the end of the other plate so that the amount was 200 g / m2. The end of the other SUS430 plate was then overlapped and fastened with two clips, and the plate was incubated in a 23°C / 50% RH environment for one day and at 40°C for two days to obtain an adhesive strength test piece. The shear adhesive strength was measured at a tensile speed of 3 mm / min using a uniaxial tester manufactured by INSTRON, product name: 5967. The measurement environment was 23±2°C, and n=5 average. The evaluation criteria were 5 MPa or more as pass, and less than 5 MPa as fail. The results are shown in Tables 4 and 5. The adhesive strength between SUS430 plates was not confirmed for Comparative Examples 1 to 5 and 8, which failed the film properties, and Comparative Examples 6 and 7, which did not obtain a uniform composition.
[0028] A1100P, SPCC-SD adhesive strength confirmation Similar to the adhesive strength check for SUS304, adhesive strength check was performed using A1100P, an aluminum alloy plate measuring 25 mm x 100 mm x 1.6 mm thick, and SPCC-SD, a cold-rolled steel plate with a dull finish measuring 25 mm x 100 mm x 1.6 mm thick. The measurement conditions and judgment criteria were the same as for SUS403. Note that for Comparative Examples 1 to 5 and 8, which were unsuccessful in terms of film properties, and Comparative Examples 6 and 7, which were unable to obtain a uniform composition, adhesive strength checks for A1100P and SPCC-SD were not performed.
[0029] Examples 1 to 5, which are compositions consisting of hexamethylene diisocyanate (A), crude diphenylmethane diisocyanate (B), and an amine compound (C) represented by formula (1) and having a number average molecular weight of 500 to 1200, passed all of the film property measurements, including maximum stress, elongation, and adhesive strength measurements using various adherends.
[0030] Example 1, which did not use hexamethylene diisocyanate (HDI) as the isocyanate compound, failed both the maximum stress and elongation percentage of the film properties.
[0031] Comparative Examples 2 and 3, which used Elasmer 1000P having a number average molecular weight outside the range of amine compound (C) having a number average molecular weight of 500 to 1200 represented by formula (1), had unacceptable film properties. Comparative Examples 6 and 7, which used Elasmer 250P having a number average molecular weight outside the range, did not provide a uniform composition.
[0032] In Comparative Examples 4 and 5, in which monomeric MDI was used instead of crude MDI (cMDI), the film elongation rate passed the test, but the maximum stress failed the test.
[0033] Comparative Example 8, in which a prepolymer was used as the isocyanate compound, failed both the maximum stress and elongation percentage in the film property measurements.
[0034] [Table 1]
[0035] [Table 2]
[0036] [Table 3]
[0037] [Table 4]
Claims
1. A composition comprising hexamethylene diisocyanate (A), crude diphenylmethane diisocyanate (B), and an amine compound (C) represented by formula (1) and having a number average molecular weight of 500 to 1,200. (1) In the above formula, m=1-2, n=2-3, and R is a polyether.
2. The composition according to claim 1, wherein the total number of moles of isocyanate groups in the hexamethylene diisocyanate (A) and the crude diphenylmethane diisocyanate (B) and the number of moles of active hydrogen groups in the amine compound (C) represented by formula (1) and having a number average molecular weight of 500 to 1,200 satisfies (molar number of isocyanate groups) / (molar number of active hydrogen groups)=0.7 to 1.
5.
3. The composition according to claim 1 or 2, wherein the mass ratio of the hexamethylene diisocyanate (A) to the crude diphenylmethane diisocyanate (B) is crude diphenylmethane diisocyanate (B) / hexamethylene diisocyanate (A)=2-6 / 4-8.
Citation Information
Patent Citations
Controller for movement of frame in box making machine
JP1985032641A
Polyurethane urea composition
JP1994128345A
Polyurethaneurea elastomer for kinetic application
JP2000248040A
Solid golf ball
JP2003102871A
Two-pack type polyurethane sealing material composition and sealing material
JP2004204139A