Copper alloy and its manufacturing method

A copper alloy with a specific composition and manufacturing process, including Ni-based intermetallic compounds, addresses the need for enhanced wear resistance in sliding parts by improving friction and durability.

JP7577083B2Active Publication Date: 2024-11-01NGK CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2022003397
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-31
Filing Date
2022-01-12
Publication Date
2024-11-01
Estimated Expiration
2042-01-12

AI Technical Summary

Technical Problem

Existing wear-resistant copper alloys, such as Cu-Ni-Sn alloys, require further improvements in wear resistance for applications in sliding parts like bearings and metal bushes.

Method used

A copper alloy composition with 5-25% Ni, 5-10% Sn, and specific amounts of elements like Zr, Ti, Fe, and Si, along with Mn, Zn, Mg, Ca, Al, and P, forming Ni-based intermetallic compound particles, is produced through melting, casting, hot/cold working, and heat treatment to enhance wear resistance.

Benefits of technology

The alloy exhibits improved wear resistance with a friction coefficient of 0.4 or less, enhanced ductility, and improved bendability, making it suitable for sliding parts requiring high wear resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577083000001
    Figure 0007577083000001
  • Figure 0007577083000002
    Figure 0007577083000002
  • Figure 0007577083000003
    Figure 0007577083000003
Patent Text Reader

Abstract

To provide a manufacturing method of a copper alloy excellent in abrasion resistance.SOLUTION: A copper alloy comprises: Ni: 5 to 25 wt.%, Sn: 5 to 10 wt.%, at least one element M selected from the group consisting of Zr, T, Fe and Si: 0.01 to 0.30 wt.% in total, at least one element A selected from the group consisting o Mn, Zn, Mg, Ca, Al and P: 0.01 to 1.00 wt.% in total, and the balance being Cu and unavoidable impurities, in the copper alloy, Ni-based intermetallic compound particles containing a Ni-M intermetallic compound are generated, and the number of Ni-based intermetallic compound particles present per unit area of 1 mm2 of the copper alloy is 1.0x103 to 1.0×106.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a copper alloy and a method for producing the same. [Background technology]

[0002] Conventionally, wear-resistant materials have been used in various fields such as automobiles, construction machinery, agricultural machinery, ships, etc. Such wear-resistant materials are often used as sliding parts (slide bearings) such as bearings, piston bushes, metal bushes, etc. Known examples of such materials include those made of Cu-Ni-Sn alloy, high-strength brass, and Kelmet.

[0003] As the wear-resistant material, the above-mentioned various alloys are selected according to the conditions of the place of use, such as the load and the rotation speed. For example, Patent Document 1 (JP Patent Publication 8-283889) discloses a high-strength and high-hardness copper alloy composed of, by weight, 5-20% Ni, 3-15% Sn, 0.5-5% Mn, and the balance Cu and unavoidable impurities, as a Cu-Ni-Sn alloy material. It is described that hard intermetallic compounds are crystallized in the matrix of this copper alloy, which contributes to improving wear resistance and seizure resistance. In addition, Patent Document 2 (JP Patent Publication No. 2019-524984) discloses a high-strength Cu-Ni-Sn alloy consisting of (by weight) 2.0 to 10.0% Ni, 2.0 to 10.0% Sn, 0.01 to 1.5% Si, 0.002 to 0.45% B, 0.001 to 0.09% P, specified metal elements as optional components, and the remainder being Cu and unavoidable impurities. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 8-283889 [Patent Document 2] Special Publication No. 2019-524984 Summary of the Invention

[0005] Although wear-resistant materials made of Cu-Ni-Sn alloys have been researched as described above, further improvement in wear resistance is required.

[0006] The present inventors have now discovered that a copper alloy having a specified composition in which Ni-based intermetallic compound particles are produced has excellent wear resistance.

[0007] Therefore, an object of the present invention is to produce or provide a copper alloy having excellent wear resistance.

[0008] According to one aspect of the present invention, Ni: 5~25% by weight, Sn: 5~10% by weight, at least one element M selected from the group consisting of Zr, Ti, Fe, and Si: 0.01 to 0.30% by weight in total; At least one element A selected from the group consisting of Mn, Zn, Mg, Ca, Al, and P: 0.01 to 1.00% by weight in total, and The balance is Cu and unavoidable impurities A copper alloy comprising: Ni-based intermetallic compound particles including Ni-M intermetallic compounds formed in the copper alloy; and a copper alloy having a unit area of ​​1 mm 2 The number of the Ni-based intermetallic compound particles present per unit area is 1.0 × 10 3 ~1.0×10 6 A copper alloy is provided.

[0009] According to another aspect of the present invention, there is provided a method for producing the copper alloy, comprising the steps of: Ni: 5~25% by weight, Sn: 5~10% by weight, at least one element M selected from the group consisting of Zr, Ti, Fe, and Si: 0.01 to 0.30% by weight in total; At least one element A selected from the group consisting of Mn, Zn, Mg, Ca, Al, and P: 0.01 to 1.00% by weight in total, and The balance is Cu and unavoidable impurities A step of melting and casting the raw alloy into an ingot, comprising: hot or cold working the ingot to obtain an intermediate product; a step of subjecting the intermediate product to a thermo-mechanical treatment by subjecting the intermediate product to i) a heat treatment, ii) hot working or cold working, and iii) a solution treatment in this order; A step of aging the intermediate product after the thermomechanical treatment to obtain the copper alloy; A method for producing a copper alloy is provided, comprising: [Brief description of the drawings]

[0010] [Figure 1] 1 is an electron microscope image of a cross section of the copper alloy obtained in Example 1. [Figure 2A] FIG. 2 is a schematic plan view showing a ring-shaped counterpart material used in a friction and wear test of a copper alloy. [Figure 2B] FIG. 2 is a schematic front view showing a ring-shaped counterpart material used in a friction and wear test of a copper alloy. [Diagram 3] FIG. 1 is a conceptual diagram for explaining a ring-on-disk test, which is a friction and wear test method for copper alloys. [Figure 4] 1 is an electron microscope image of a cross section of the copper alloy obtained in Example 2. [Diagram 5] 1 is an electron microscope image of a cross section of the copper alloy obtained in Example 6. [Figure 6] 1 is an electron microscope image of a cross section of the copper alloy obtained in Example 7. [Figure 7] 1 is an electron microscope image of a cross section of the copper alloy obtained in Example 8. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Copper alloy The copper alloy according to the present invention is composed of 5-25% by weight of Ni, 5-10% by weight of Sn, 0.01-0.30% by weight in total of at least one element M selected from the group consisting of Zr, Ti, Fe and Si, 0.01-1.00% by weight in total of at least one element A selected from the group consisting of Mn, Zn, Mg, Ca, Al and P, and the balance being Cu and unavoidable impurities. In addition, Ni-based intermetallic compound particles including Ni-M intermetallic compounds are generated in this copper alloy. Furthermore, in the copper alloy, the Ni-based intermetallic compound particles including Ni-M intermetallic compounds are generated in the copper alloy. 2 The number of Ni-based intermetallic compound particles per unit area is 1.0×10 3 ~1.0×10 6 Such copper alloys have excellent wear resistance. As described above, wear-resistant materials made of Cu-Ni-Sn alloys have been studied, but further improvement in wear resistance is required. In response to this, the present invention can provide a copper alloy with excellent wear resistance.

[0012] The copper alloy of the present invention preferably has a friction coefficient of 0.4 or less, more preferably 0.35 or less, and further preferably 0.3 or less. Such a copper alloy having excellent wear resistance is used for sliding parts such as plain bearings, but is not particularly limited as long as it requires wear resistance.

[0013] The copper alloy of the present invention is composed of 5 to 25 weight % Ni, 5 to 10 weight % Sn, a total of 0.01 to 0.30 weight % of at least one element M selected from the group consisting of Zr, Ti, Fe, and Si, a total of 0.01 to 1.00 weight % of at least one element A selected from the group consisting of Mn, Zn, Mg, Ca, Al, and P, and the balance being Cu and unavoidable impurities. This copper alloy is preferably composed of 8.5 to 9.5 weight percent Ni, 5.5 to 6.5 weight percent Sn, 0.0 to 0.2 weight percent Zr, 0.0 to 0.2 weight percent Ti, 0.0 to 0.2 weight percent Fe, 0.0 to 0.2 weight percent Si, 0.2 to 0.9 weight percent Mn, 0.0 to 0.2 weight percent Zn, and the balance being Cu and unavoidable impurities (with the proviso that at least one of Zr, Ti, Fe, and Si is contained within a range of 0.01 to 0.30 weight percent in total). or composed of 20.0 to 22.0 weight% Ni, 4.5 to 5.7 weight% Sn, 0.0 to 0.2 weight% Zr, 0.0 to 0.2 weight% Ti, 0.0 to 0.2 weight% Fe, 0.0 to 0.2 weight% Si, 0.2 to 0.9 weight% Mn, 0.0 to 0.2 weight% Zn, and the balance being Cu and unavoidable impurities (with the proviso that at least one of Zr, Ti, Fe, and Si is included within a range of 0.01 to 0.30 weight% in total).

[0014] The crystal grain size of the copper alloy of the present invention is preferably 1.0 to 100 μm, and more preferably 1.0 to 20 μm, which can improve the ductility of the copper alloy, ensure elongation, and improve bendability.

[0015] The element M is at least one element selected from Zr, Ti, Fe, and Si. The element M forms an Ni-M intermetallic compound together with Ni, and contributes to the generation of Ni-based intermetallic compound particles containing the Ni-M intermetallic compound. The Ni-based intermetallic compound particles are generated in the copper alloy and function as if they were rollers of a bearing, and as a result, it is considered that they contribute to improving the wear resistance of the copper alloy. Examples of the Ni-M intermetallic compound are Ni-Zr intermetallic compound, Ni-Ti intermetallic compound, Ni-Fe intermetallic compound, and Ni-Si intermetallic compound. The element M preferably contains at least Zr, and more preferably is Zr. Therefore, the Ni-M intermetallic compound is preferably a Ni-Zr intermetallic compound. Zr generates a Ni-based intermetallic compound having optimal hardness between the copper alloy and the mating material (for example, carbon steel such as JIS G 4805: SUJ2 (high carbon chromium bearing steel material)) that comes into contact with the copper alloy, and is therefore expected to have a greater effect on improving wear resistance. As described above, in addition to Zr, Ti, Fe and Si also form Ni-M intermetallic compounds, but it is preferable to include Zr in the copper alloy rather than Ti, Fe and Si from the viewpoint of rollability during production of the copper alloy. That is, by using Zr as the element M, both wear resistance and rollability can be effectively realized.

[0016] Since the copper alloy of the present invention contains Sn in addition to the element M, Ni-based intermetallic compound particles may also generate Ni-Sn intermetallic compounds (e.g., Ni2Sn3 and Ni3Sn) in addition to Ni-M intermetallic compounds. Therefore, the Ni-based intermetallic compound particles preferably contain Ni-M intermetallic compounds and Ni-Sn intermetallic compounds, and more preferably are composed of Ni-M intermetallic compounds and Ni-Sn intermetallic compounds. Technically, the proportion of Ni-Sn intermetallic compound particles generated in the copper alloy may be greater than that of Ni-M intermetallic compound particles, but the effect of wear resistance is not sufficient just by increasing the number of Ni-Sn intermetallic compound particles. On the other hand, although the number of Ni-M intermetallic compound particles tends to be smaller than that of Ni-Sn intermetallic compound particles, further improvement of wear resistance can be expected by generating Ni-M intermetallic compounds in the copper alloy. Since Ni-Sn intermetallic compounds can also contribute to improving wear resistance to some extent (although not as much as Ni-M intermetallic compounds), it is possible to produce a large amount of Ni-Sn intermetallic compounds, for example, by adjusting the heat treatment conditions in the copper alloy manufacturing process. For these reasons, the copper alloy of the present invention is characterized in that more Ni-based intermetallic compound particles are produced than in conventional copper alloys, and that the Ni-based intermetallic compound particles contain Ni-M intermetallic compounds.

[0017] The ratio of the number of Ni-M intermetallic compound particles having a particle size of 0.1 μm or more to the total number of Ni-based intermetallic compound particles having a particle size of 0.1 μm or more generated in the copper alloy is preferably 1.0 to 30%, more preferably 1.0 to 15%, from the viewpoint of improving wear resistance and rollability. The measurement method for determining the number ratio of Ni-M intermetallic compound particles is not particularly limited, but for example, a method using composition analysis by SEM-EDX (energy dispersive X-ray spectroscopy) is preferable. In this case, the number ratio of Ni-M intermetallic compound particles can be determined by the following procedure. First, the cross section of the copper alloy is polished and then etched to reveal the cross-sectional structure. Five arbitrarily selected points on the cross section are photographed and elementally analyzed by SEM-EDX (energy dispersive X-ray spectroscopy) at a magnification of 1000 times. The diameter of each of the photographs and the element mapping image is 60 mm (area 2826 mm).2 ) region, the number of Ni-based intermetallic compound particles (including Ni-M intermetallic compound particles) scattered at the grain boundaries and within the grains and the number of Ni-M intermetallic compound particles are measured. At this time, only particles having a particle size of 0.1 μm or more are counted as Ni-based intermetallic compound particles (including Ni-M intermetallic compound particles). The number of Ni-M intermetallic compound particles is divided by the number of Ni-based intermetallic compound particles, and the result is multiplied by 100 to calculate the ratio (%) of the number of Ni-M intermetallic compound particles to the number of Ni-based intermetallic compound particles. It is desirable to adopt the average value obtained from the photographs and element mapping images at the five locations as the representative value for the copper alloy.

[0018] The total content of element M is 0.01 to 0.30% by weight. This content is preferably 0.01 to 0.20% by weight. By making this content 0.30% by weight or less, it is possible to suppress the coarsening of Ni-based intermetallic compound particles and make them fine, thereby improving castability and rollability. By making this content 0.01% by weight or more, it is possible to control the particle size and number of Ni-based intermetallic compound particles and improve wear resistance and hot rolling properties.

[0019] The Ni-based intermetallic compound particles formed in the copper alloy of the present invention preferably have a particle size of 0.1 to 100 μm, more preferably 1.0 to 20 μm, and further preferably 1.0 to 10 μm. 2 The number of Ni-based intermetallic compound particles per unit area is 1.0×10 3 ~1.0×10 6 pcs, preferably 1.0×10 3 ~1.0×10 5 pcs, more preferably 1.0×10 4 ~1.0×10 5 Although there are no particular limitations on the method of measuring and calculating the particle size and number of Ni-based intermetallic compound particles, it is preferable to count particles having a particle size of 0.1 μm or more as Ni-based intermetallic compound particles.

[0020] The element A is at least one element selected from the group consisting of Mn, Zn, Mg, Ca, Al, and P. The element A in the copper alloy of the present invention is expected to have the effect of deoxidizing the molten metal by dissolving in the raw alloy during the production of the copper alloy, and to prevent the crystal grains of the parent phase from becoming coarse during the solution heat treatment. The element A preferably contains at least Mn, and more preferably is Mn.

[0021] The total content of element A is 0.01 to 1.00% by weight. This content is preferably 0.10 to 0.40% by weight, more preferably 0.15 to 0.30% by weight. When this content is 0.01% by weight or more, the above-mentioned effect due to the copper alloy containing element A can be expected to be more. When this content is 1.00% by weight or less, the above-mentioned effect due to the copper alloy containing element A can be expected to be more, but it is considered that no further effect can be expected even if element A is added in an amount exceeding this. In addition, when Mn is contained as element A in the copper alloy, the content of Mn is preferably 0.10 to 0.40% by weight. This can suppress the crystal grains from becoming coarse, and improve bending workability.

[0022] The copper alloy of the present invention contains unavoidable impurities, and an example of the unavoidable impurity is B. Typically, the content of B in the copper alloy is 0 wt % or very close to it.

[0023] Manufacturing method of copper alloy The method for producing the copper alloy according to the present invention preferably includes the steps of: (a) melting and casting a raw alloy consisting of 5-25% by weight of Ni, 5-10% by weight of Sn, 0.01-0.30% by weight in total of at least one element M selected from the group consisting of Zr, Ti, Fe and Si, 0.01-1.00% by weight in total of at least one element A selected from the group consisting of Mn, Zn, Mg, Ca, Al and P, and the balance Cu and inevitable impurities, to obtain an ingot; (b) hot working or cold working the ingot to obtain an intermediate product; (c) subjecting the intermediate product to a thermo-mechanical treatment by subjecting it to i) a heat treatment, ii) hot working or cold working, and iii) solution treatment in this order; and (d) aging the intermediate product after the thermo-mechanical treatment to obtain a copper alloy. This allows the production of a copper alloy having excellent wear resistance as described above. The preferred embodiment of the copper alloy is as described above, and therefore will not be described here.

[0024] (a) Melting and casting of raw alloys First, a raw alloy is prepared. The raw alloy is preferably composed of 5 to 25 weight % Ni, 5 to 10 weight % Sn, a total of 0.01 to 0.30 weight % of at least one element M selected from the group consisting of Zr, Ti, Fe, and Si, a total of 0.01 to 1.00 weight % of at least one element A selected from the group consisting of Mn, Zn, Mg, Ca, Al, and P, and the balance being Cu and unavoidable impurities. More preferably, this raw material alloy is composed of 8.5 to 9.5 weight percent Ni, 5.5 to 6.5 weight percent Sn, 0.0 to 0.2 weight percent Zr, 0.0 to 0.2 weight percent Ti, 0.0 to 0.2 weight percent Fe, 0.0 to 0.2 weight percent Si, 0.2 to 0.9 weight percent Mn, 0.0 to 0.2 weight percent Zn, and the balance being Cu and unavoidable impurities (with the proviso that at least one of Zr, Ti, Fe, and Si is contained within a range of 0.01 to 0.30 weight percent in total). or Ni: 20.0-22.0 wt%, Sn: 4.5-5.7 wt%, Zr: 0.0-0.2 wt%, Ti: 0.0-0.2 wt%, Fe: 0.0-0.2 wt%, Si: 0.0-0.2 wt%, Mn: 0.2-0.9 wt%, Zn: 0.0-0.2 wt%, and the balance Cu and inevitable impurities (including at least one of Zr, Ti, Fe, and Si within a range of 0.01-0.30 wt% in total). The element M preferably contains at least Zr, and more preferably Zr. The element A preferably contains at least Mn, and more preferably Mn. The preferred contents of the elements M and A are the same as those described for the copper alloy above.

[0025] In this step, the prepared raw alloy is melted and cast into an ingot. The raw alloy is preferably melted in, for example, a high-frequency melting furnace. The casting method is not particularly limited, but may be a full continuous casting method, a semi-continuous casting method, a batch casting method, or the like. In addition, a horizontal casting method, a vertical casting method, or the like may be used. The shape of the obtained ingot may be, for example, a slab, a billet, a bloom, a plate, a rod, a tube, a block, or the like, but is not particularly limited and may be other shapes.

[0026] (b) Hot or cold working of the ingot The obtained ingot is hot-worked or cold-worked to obtain an intermediate product. Examples of the processing method include forging, rolling, extrusion, drawing, etc. In this step, the ingot is preferably roughly rolled by hot-working or cold-working to obtain a rolled material (intermediate product).

[0027] (c) Thermomechanical processing The intermediate product thus obtained is subjected to a thermo-mechanical treatment by carrying out i) a heat treatment, ii) hot working or cold working, and iii) solution treatment in this order.

[0028] In the step of carrying out the thermomechanical treatment, first, the intermediate product is subjected to a heat treatment. This heat treatment is preferably performed by holding the intermediate product at 500 to 950°C for 2 to 24 hours. The heat treatment temperature is more preferably 600 to 800°C, and even more preferably 650 to 750°C. The holding time at the above temperature is more preferably 2 to 12 hours, and even more preferably 5 to 10 hours. In this way, the target Ni-based intermetallic compound particles can be dispersed in the copper alloy as a fine product, and the particle size of the Ni-based intermetallic compound particles and the surface area of ​​the copper alloy per mm2 can be improved. 2 The number of Ni-based intermetallic compound particles present per unit area can be controlled as described above.

[0029] After the intermediate product is heat-treated, it is subjected to hot working or cold working. The working method may be the same as the method in (b) above. For example, when the intermediate product is rolled to form a plate, it is preferable to roll it so that the working rate defined by the following formula: P=100×(Tt) / T (wherein P is the working rate (%), T is the thickness (mm) of the intermediate product before rolling, and t is the thickness (mm) of the intermediate product after rolling) is 0 to 95%.

[0030] The intermediate product after hot working or cold working is subjected to solution treatment. This treatment is preferably held at 700 to 1000°C for 5 seconds to 24 hours. The temperature of the solution treatment is more preferably 750 to 950°C, and even more preferably 800 to 900°C. The holding time at the above temperature is more preferably 1 minute to 5 hours, and even more preferably 1 to 5 hours. After the solution treatment, the intermediate product is preferably quenched. The cooling method is not particularly limited, but examples include water cooling, oil cooling, and air cooling. The temperature drop rate during this cooling is preferably 20°C / s or more, and more preferably 50°C / s or more. In the case of using a copper alloy containing about 9.0% by weight of Ni and about 6.0% by weight of Sn, with the balance being Cu and unavoidable impurities, or a copper alloy having a similar composition (for example, further containing Zr and Mn) containing about 21.0% by weight of Ni and about 5.0% by weight of Sn, with the balance being Cu and unavoidable impurities, or a copper alloy having a similar composition (for example, further containing Zr and Mn) as a raw material alloy, the intermediate product is preferably held at 750 to 850°C for 5 to 500 seconds, more preferably at 750 to 850°C for 30 to 240 seconds. In addition, it is preferable to immediately water-cool such intermediate products after the solution treatment.

[0031] (d) Aging treatment of intermediate products The intermediate product after the thermomechanical treatment is subjected to aging treatment to obtain a copper alloy. The strength of the obtained copper alloy can be increased by the aging treatment. The temperature of the aging treatment is preferably 300 to 500°C, more preferably 350 to 450°C. The holding time at the above temperature is preferably 1 to 24 hours, more preferably 2 to 12 hours.

[0032] By carrying out the above steps (a) to (d), a copper alloy having excellent wear resistance can be preferably produced.

[0033] In addition, the intermediate product may be finish hot worked or finish cold worked after the above-mentioned (c) heat treatment and before the above-mentioned (d) aging treatment. That is, it is preferable to further include a step of finish hot working or finish cold working the intermediate product after the heat treatment and before the aging treatment. For example, the intermediate product can be finish rolled by finish cold working after the heat treatment and before the aging treatment to have a target plate thickness. EXAMPLES

[0034] The present invention will now be further illustrated by the following examples.

[0035] Example 1 Copper alloys were prepared and evaluated according to the following procedure.

[0036] (1) Melting and casting of raw alloys A raw alloy (Ni: 8.5-9.5 wt%, Sn: 5.5-6.5 wt%, Zr: 0.14 wt%, Mn: 0.35 wt%, the balance being Cu and unavoidable impurities) was prepared. This raw alloy was melted in a high-frequency melting furnace and cast by a vertical casting method to obtain a round ingot with a diameter of 320 mm.

[0037] (2) Hot or cold working of ingots The obtained ingot was subjected to a soaking treatment, and then to hot working and cold working to obtain an intermediate product.

[0038] (3) Thermomechanical treatment The intermediate product was subjected to heat treatment. Specifically, the intermediate product was held at 730°C for 6 hours to generate Ni-based intermetallic compound particles in the intermediate product. Next, the intermediate product was rolled by cold working so that the processing rate was 50%, and the intermediate product was formed into a plate shape. Furthermore, the intermediate product was heated at 820°C for 60 seconds to be solutionized, and immediately thereafter, it was quenched by water cooling at a temperature drop rate of 20°C / s. In this manner, the intermediate product was subjected to thermomechanical processing.

[0039] (4) Finish hot processing or finish cold processing of intermediate products The thermo-mechanically treated intermediate product was cold-rolled (finish rolling) to reduce the thickness of the intermediate product to 1.5 mm.

[0040] (5) Aging treatment of intermediate products The finish-rolled intermediate product was kept at 375°C for 2 hours to age the intermediate product, thereby obtaining a copper alloy.

[0041] (6) Evaluation The obtained copper alloys were subjected to the following evaluations.

[0042] <Cross-section observation> The cross section of the copper alloy obtained in (5) above was polished and then etched, and the cross section was observed under an electron microscope at a magnification of 1000 times. The results are shown in Figure 1. In Figure 1, the black dots represent Ni-based intermetallic compound particles, and it was found that many Ni-based intermetallic compound particles were generated in a dispersed state.

[0043] In addition, the particle size of the Ni-based intermetallic compound particles formed in this copper alloy and the area per unit area of ​​the copper alloy of 1 mm 2 The number of Ni-based intermetallic compound particles present per unit area was measured. Specifically, the measurement was performed by the following method. The cross section of the copper alloy was polished and then etched to reveal the cross-sectional structure. Ten randomly selected points on the cross section were photographed at 1000x magnification using an electron microscope. Each photograph was taken within an area of ​​82 mm length and 118 mm width (area 9676 mm2). 2 ) the size and number of Ni-based intermetallic compound particles scattered at the grain boundaries and within the grains were measured. Only particles with a grain size of 0.1 μm or more were counted as Ni-based intermetallic compound particles. In each photograph, the number of Ni-based intermetallic compound particles was calculated per unit area of ​​1 mm2. 2 The number of particles per unit area of ​​1 mm2 was calculated based on the number of particles per unit area of ​​these 10 locations. 2 The number of Ni-based intermetallic compound particles per unit area of ​​1 mm2 of copper alloy was calculated by arithmetic average. 2 The number of Ni-based intermetallic compound particles per unit area of ​​1 mm2 of the copper alloy was calculated. 2The number of Ni-based intermetallic compound particles per unit area is 2.0×10 4 The number of particles was 10. The vertical and horizontal dimensions of the Ni-based intermetallic compound particles seen in each photograph were also measured, and the sum of the vertical dimensions and the sum of the horizontal dimensions of the Ni-based intermetallic compound particles seen in all 10 photographs were calculated. The sum of the vertical dimensions and the sum of the horizontal dimensions were divided by the total number of Ni-based intermetallic compound particles seen in all 10 photographs, respectively, to calculate the average values ​​of the vertical and horizontal dimensions of the Ni-based intermetallic compound particles. Finally, the average values ​​of the vertical and horizontal dimensions calculated were added together and divided by 2 to obtain the particle size of the Ni-based intermetallic compound particles. As a result, the particle size of the Ni-based intermetallic compound particles was 1.5 μm.

[0044] Furthermore, the ratio of the number of Ni-M intermetallic compound particles to the total number of Ni-based intermetallic compound particles formed in this copper alloy was determined by the following procedure. First, the cross section of the copper alloy was polished and then etched to reveal the cross-sectional structure. Five randomly selected points on the cross section were photographed at 1000x magnification using SEM-EDX (energy dispersive X-ray spectroscopy) and subjected to elemental analysis. Each of the photographs and elemental mapping images thus obtained was analyzed using a 60 mm diameter (area 2826 mm 2 ) region, the number of Ni-based intermetallic compound particles (including Ni-M intermetallic compound particles) scattered within the grain boundaries and grains and the number of Ni-M intermetallic compound particles were measured. At this time, only particles having a particle size of 0.1 μm or more were counted as Ni-based intermetallic compound particles (including Ni-M intermetallic compound particles). The ratio (%) of the number of Ni-M intermetallic compound particles to the number of Ni-based intermetallic compound particles was calculated by dividing the number of Ni-M intermetallic compound particles by the number of Ni-based intermetallic compound particles and multiplying the result by 100. The ratios of the number of Ni-M intermetallic compound particles to the number of Ni-based intermetallic compound particles in the photographs and element mapping images of the five locations were 7.5%, 4.6%, 6.4%, 5.8%, and 13.6%, respectively, and the average value of these was 7.58%.

[0045] <Friction and wear test> The copper alloy obtained in (5) above was tested as follows to evaluate the wear resistance of the copper alloy. The copper alloy was machined into a test piece (square plate) with a side length of 30 mm and a thickness of 1.0 to 5.0 mm. A steel material (ring) with a shape as shown in Figures 2A and 2B was used as a mating material for the copper alloy (the unit of the numerical values ​​in Figure 2B is mm). As shown in Figure 3, a ring-on-disk test was performed at room temperature (25°C) using the test piece and the mating material with a friction and wear tester EFM-3-H (manufactured by A&D Co., Ltd.). The wear resistance was evaluated from the wear amount and friction coefficient of the test piece obtained by this test. The details of the test conditions and test method at this time are shown below.

[0046] (Test conditions) - Load: 40N - Sliding speed: 3m / s - Test piece size: 30mm x 30mm - Surface roughness of test piece and mating material: Ra0.4μm or less - Mating material: Bearing steel (JIS G 4805: SUJ2), HRC60 or higher

[0047] (Test Method) As shown in Figure 3, with the test piece and the mating material in contact with each other at their sliding surfaces, a load of 40N was applied to the fixed mating material and the test piece was rotated for 30 minutes. The test piece was rotated and slid at a set load and sliding speed, the shear force was detected as a friction force, and the friction coefficient was calculated. In addition, the mass of the test piece was measured before and after the test, and the amount of wear (mg) was calculated. It can be said that the smaller the friction coefficient and the smaller the amount of wear, the better the wear resistance.

[0048] As a result of the test, the amount of wear of the test piece was 3.6 mg, and the friction coefficient was 0.30. When the test piece surface was observed after the test, the arithmetic mean roughness Ra measured in accordance with JIS B0601-2001 was 1.32 μm, and the ten-point mean roughness Rzjis measured in accordance with JIS B0601-2001 was 8.21 μm. The particle size of the wear powder from the test piece was 200 μm.

[0049] Example 2 The copper alloy was produced and evaluated in the same manner as in Example 1, except that in the step (3) of performing the thermo-mechanical treatment, the intermediate product was held at 565°C for 6 hours by heat treatment to generate Ni-based intermetallic compound particles in the intermediate product.

[0050] As a result of cross-sectional observation, it was found that Ni-based intermetallic compound particles were formed, as shown in Figure 4. The grain size of the Ni-based intermetallic compound particles was 1.0 μm, and the grain size of the particles was 1.0 μm per unit area of ​​the copper alloy. 2 The number of Ni-based intermetallic compound particles per unit area is 1.0×10 4 The number of Ni-M intermetallic compound particles was 17.9%, 19.3%, 14.5%, 11.5% and 13.4%, respectively, in the photographs and element mapping images of the five locations obtained by SEM-EDX, and the average value of these was 15.32%. As a result of the friction and wear test, the wear amount of the test piece was 6.8 mg, and the friction coefficient was 0.32. When the test piece surface was observed after the test, the arithmetic mean roughness Ra measured in accordance with JIS B0601-2001 was 1.47 μm, and the ten-point mean roughness Rzjis measured in accordance with JIS B0601-2001 was 9.84 μm. The particle size of the wear powder derived from the test piece was 450 μm.

[0051] Example 3 A copper alloy was prepared and evaluated in the same manner as in Example 1, except that the raw alloy (1) above was composed of 10.6 wt % Ni, 5.5 wt % Sn, 0.45 wt % Si, 0.37 wt % Mn, and the balance being Cu and unavoidable impurities (i.e., only Si was added as the element M).

[0052] Cross-sectional observation revealed that Ni-based intermetallic compound particles were formed. The particle size of the Ni-based intermetallic compound particles was 10 μm, and the diameter of the particles was 1 mm2 of the copper alloy. 2 The number of Ni-based intermetallic compound particles per unit area is 1.0×10 4The number of Ni-M intermetallic compound particles was 5.2%, 10.2%, 6.6%, 3.8% and 3.7% in the photographs and element mapping images of the five locations obtained by SEM-EDX, respectively, and the average value of these was 5.90%. As a result of the friction and wear test, the wear amount of the test piece was 0.7 mg, and the friction coefficient was 0.32. When the test piece surface was observed after the test, the arithmetic mean roughness Ra measured in accordance with JIS B0601-2001 was 0.92 μm, and the ten-point mean roughness Rzjis measured in accordance with JIS B0601-2001 was 5.49 μm. The particle size of the wear powder derived from the test piece was 300 μm.

[0053] Example 4 A copper alloy was prepared and evaluated in the same manner as in Example 1, except that the raw alloy (1) used was one having a composition of 10.5 wt% Ni, 5.4 wt% Sn, 1.38 wt% Fe, 0.02 wt% Si, 0.18 wt% Mn, and the balance being Cu and unavoidable impurities (i.e., Fe and Si were added as the element M).

[0054] Cross-sectional observation revealed that Ni-based intermetallic compound particles were formed. The particle size of the Ni-based intermetallic compound particles was 1.0 μm, and the diameter of the particles was 1 mm2. 2 The number of Ni-based intermetallic compound particles per unit area is 2.0×10 3 The results of the friction and wear test showed that the wear amount of the test piece was 3.9 mg and the friction coefficient was 0.38. When the test piece surface was observed after the test, the arithmetic mean roughness Ra measured in accordance with JIS B0601-2001 was 1.47 μm, and the ten-point mean roughness Rzjis measured in accordance with JIS B0601-2001 was 8.71 μm. The particle size of the wear powder from the test piece was 400 μm.

[0055] Example 5 A copper alloy was prepared and evaluated in the same manner as in Example 1, except that the raw alloy (1) used was one having a composition of 10.6 wt.% Ni, 5.4 wt.% Sn, 0.75 wt.% Ti, 0.07 wt.% Si, 0.41 wt.% Mn, and the balance being Cu and unavoidable impurities (i.e., Ti and Si were added as the element M).

[0056] Cross-sectional observation revealed that Ni-based intermetallic compound particles were formed. The particle size of the Ni-based intermetallic compound particles was 25 μm, and the diameter of the particles was 1 mm2 of the copper alloy. 2 The number of Ni-based intermetallic compound particles per unit area is 2.0×10 3 The results of the friction and wear test showed that the wear amount of the test piece was 5.0 mg and the friction coefficient was 0.40. When the test piece surface was observed after the test, the arithmetic mean roughness Ra measured in accordance with JIS B0601-2001 was 1.41 μm, and the ten-point mean roughness Rzjis measured in accordance with JIS B0601-2001 was 6.94 μm. The particle size of the wear powder from the test piece was 200 μm.

[0057] Example 6 A copper alloy was produced and evaluated in the same manner as in Example 1, except that the raw alloy (1) above had a composition of 20.0 to 22.0 wt % Ni, 4.5 to 5.7 wt % Sn, 0.21 wt % Zr, 0.34 wt % Mn, the balance being Cu and unavoidable impurities.

[0058] As a result of cross-sectional observation, it was found that Ni-based intermetallic compound particles were formed, as shown in FIG. 5. The grain size of the Ni-based intermetallic compound particles was 3.0 μm, and the grain size was 1 mm2 of the copper alloy. 2 The number of Ni-based intermetallic compound particles per unit area is 5.0×10 3The number of Ni-M intermetallic compound particles was 6.9%, 14.1%, 5.7%, 4.3% and 15.8%, respectively, in the photographs and element mapping images of the five locations obtained by SEM-EDX, and the average value of these was 9.36%. As a result of the friction and wear test, the wear amount of the test piece was 6.8 mg, and the friction coefficient was 0.33. When the test piece surface was observed after the test, the arithmetic mean roughness Ra measured in accordance with JIS B0601-2001 was 0.53 μm, and the ten-point mean roughness Rzjis measured in accordance with JIS B0601-2001 was 5.24 μm. The particle size of the wear powder derived from the test piece was 100 μm.

[0059] Example 7 (comparison) A copper alloy was prepared and evaluated in the same manner as in Example 1, except that the raw alloy (1) had a composition of Ni: 9.14 wt %, Sn: 6.18 wt %, Zr: 0.10 wt %, Mn: 0.33 wt %, with the balance being Cu and unavoidable impurities, and that the solution treatment and aging treatment were carried out as follows without carrying out the above steps (2) to (5).

[0060] (Solution treatment and aging treatment) The ingot obtained in (1) above was subjected to solution heat treatment (holding at 800-900°C for 2-8 hours, followed by water cooling) and aging heat treatment (holding at 300-400°C for 0.5-4 hours). time That is, the step of hot working or cold working the ingot to obtain an intermediate product in the above (2), the steps other than the solution treatment in the above (3), and the step of finish rolling in the above (4) were not performed.

[0061] As a result of cross-sectional observation, it was found that Ni-based intermetallic compound particles were formed, as shown in Figure 6. The grain size of the Ni-based intermetallic compound particles was 2.0 μm, and the grain size was 1 mm2 of the copper alloy. 2 The number of Ni-based intermetallic compound particles per unit area is 8.0×10 2The results of the friction and wear test showed that the wear amount of the test piece was 6.8 mg and the friction coefficient was 0.53. When the test piece surface was observed after the test, the arithmetic mean roughness Ra measured in accordance with JIS B0601-2001 was 4.04 μm, and the ten-point mean roughness Rzjis measured in accordance with JIS B0601-2001 was 18.2 μm. The particle size of the wear powder from the test piece was 500 μm.

[0062] Example 8 (comparison) The copper alloy was prepared and evaluated in the same manner as in Example 1, except that the raw alloy (1) had a composition of 8.5 to 9.5 wt % Ni, 5.5 to 6.5 wt % Sn, 0.35 wt % Mn, and the balance Cu and unavoidable impurities (i.e., no element M was added) and that the thermomechanical treatment (3) was not performed.

[0063] As a result of cross-sectional observation, it was found that no Ni-based intermetallic compound particles were generated, as shown in Figure 7. As a result of the friction and wear test, the wear amount of the test piece was 6.8 mg, and the friction coefficient was 0.46. When the test piece surface was observed after the test, the arithmetic mean roughness Ra measured in accordance with JIS B0601-2001 was 2.86 μm, and the ten-point mean roughness Rzjis measured in accordance with JIS B0601-2001 was 16.22 μm. The particle size of the wear powder derived from the test piece was 500 μm.

[0064] Example 9 A copper alloy was produced and evaluated in the same manner as in Example 1, except that the raw alloy (1) had a composition of 20.0 to 22.0 wt % Ni, 4.5 to 5.5 wt % Sn, 0.16 wt % Zr, 0.35 wt % Mn, and the balance being Cu and unavoidable impurities.

[0065] Cross-sectional observation revealed that Ni-based intermetallic compound particles were formed. The particle size of the Ni-based intermetallic compound particles was 4.8 μm, and the diameter of the particles was 1 mm2 of the copper alloy. 2 The number of Ni-based intermetallic compound particles per unit area is 1.66 × 10 3The number of Ni-M intermetallic compound particles was 4.3%, 7.1%, 7.4%, 7.8% and 8.1% in the photographs and element mapping images of the five locations obtained by SEM-EDX, respectively, and the average value of these was 6.94%. As a result of the friction and wear test, the wear amount of the test piece was 3.3 mg, and the friction coefficient was 0.25. When the test piece surface was observed after the test, the arithmetic mean roughness Ra measured in accordance with JIS B0601-2001 was 1.21 μm, and the ten-point mean roughness Rzjis measured in accordance with JIS B0601-2001 was 7.54 μm. The particle size of the wear powder derived from the test piece was 37 μm.

Claims

1. Ni: 5 to 25% by weight, Sn: 5 to 10% by weight, At least one element M selected from the group consisting of Zr, Ti, Fe, and Si: 0.01 to 0.30% by weight in total; At least one element A selected from the group consisting of Mn, Zn, Mg, Ca, Al, and P: 0.01 to 1.00% by weight in total; and The balance is Cu and inevitable impurities. A copper alloy comprising: Ni-based intermetallic compound particles including Ni-M intermetallic compounds formed in the copper alloy; and a unit area of ​​the copper alloy of 1 mm 2 The number of the Ni-based intermetallic compound particles having a particle size of 0.1 μm or more per unit area is 1.0 × 10 3 ~1.0 x 10 6 wherein the copper alloy has a coefficient of friction of 0.4 or less.

2. 10. The copper alloy of claim 1, wherein the copper alloy has a coefficient of friction of 0.35 or less.

3. 3. The copper alloy according to claim 1 or 2, wherein said element M is Zr.

4. The copper alloy according to any one of claims 1 to 3, wherein the element A is Mn.

5. The copper alloy according to any one of claims 1 to 4, wherein the total content of element A is 0.10 to 0.40 wt%.

6. The copper alloy according to any one of claims 1 to 5, wherein the Ni-based intermetallic compound particles have a particle size of 0.1 to 100 µm.

7. The copper alloy according to any one of claims 1 to 6, wherein the ratio of the number of the Ni-M intermetallic compound particles having a particle size of 0.1 μm or more to the total number of the Ni-based intermetallic compound particles having a particle size of 0.1 μm or more is 1.0 to 30%.

8. A method for producing the copper alloy according to any one of claims 1 to 7, Ni: 5 to 25% by weight, Sn: 5 to 10% by weight, At least one element M selected from the group consisting of Zr, Ti, Fe, and Si: 0.01 to 0.30% by weight in total; At least one element A selected from the group consisting of Mn, Zn, Mg, Ca, Al, and P: 0.01 to 1.00% by weight in total; and The balance is Cu and inevitable impurities. A step of melting and casting the raw alloy into an ingot, comprising: hot or cold working the ingot to obtain an intermediate product; a step of subjecting the intermediate product to a heat treatment in the order of i) a heat treatment at 500 to 750°C, ii) hot working or cold working, and iii) solution treatment; A step of aging the intermediate product after the thermomechanical treatment to obtain the copper alloy; A method for producing a copper alloy, comprising:

9. The method for producing a copper alloy according to claim 8, wherein the heat treatment is carried out by holding the intermediate product at 500 to 750°C for 2 to 24 hours.

10. The method for producing a copper alloy according to claim 8 or 9, wherein the solution treatment is carried out by holding the intermediate product at 700 to 1000° C. for 5 seconds to 24 hours.

11. The method for producing a copper alloy according to any one of claims 8 to 10, further comprising the step of finish hot working or finish cold working the intermediate product after the thermomechanical treatment and before the aging treatment.

Citation Information

Patent Citations

  • Wear-resistant high-elasticity copper alloy inserting sleeving material and preparation method thereof

    CN111394611A

  • High strength and high hardness copper alloy

    JP1996283889A

  • Multicomponent copper alloy and its use

    JP2007297707A

  • Copper based sintered contact material and double-layered sintered contact member

    JP2008255490A

  • Copper alloy sheet material and manufacturing method of copper alloy sheet material

    JP2017179538A