Olefin-based polymer, film produced therefrom, and method for producing same
The olefin polymer, produced with a hybrid catalyst and specific transition metal compounds, addresses poor processability and heat-sealing issues, achieving improved mechanical strength and drop impact strength in films.
Patent Information
- Application Number
- JP2023530855
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-23
- Filing Date
- 2021-11-12
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-11-12
AI Technical Summary
Existing olefin polymers produced using metallocene catalysts have poor processability and films made from them exhibit poor heat-sealing properties due to narrow molecular weight distribution, limiting their application in films requiring high mechanical strength, particularly drop impact strength.
An olefin polymer with a density of 0.915-0.935 g/cm³, melting index of 0.3-3.0 g/10 min, melt flow ratio of 20-50, and comonomer distribution slope of 3 or more, produced using a hybrid catalyst containing specific transition metal compounds, results in a film with improved mechanical strength and drop impact strength.
The olefin polymer achieves excellent processability and mechanical strength, particularly in films with enhanced drop impact strength, suitable for applications such as stretch films and overwrap films.
Smart Images

Figure 0007577211000020 
Figure 0007577211000021 
Figure 0007577211000022
Abstract
Description
[Technical field]
[0001] The present invention relates to an olefin-based polymer, a film produced therefrom, and a method for producing the same, and more particularly to an olefin-based polymer film produced therefrom and having excellent mechanical strength, in particular drop impact strength, and a method for producing the same. [Background technology]
[0002] Metallocene catalysts, which are one of the catalysts used to polymerize olefins, are compounds in which ligands such as cyclopentadienyl, indenyl, or cycloheptadienyl are coordinated to a transition metal or a transition metal halide, and have a sandwich structure as their basic structure.
[0003] Ziegler-Natta catalysts, another catalyst used to polymerize olefins, have metal components that act as active sites dispersed on an inert solid surface, and the properties of the active sites are not uniform. On the other hand, metallocene catalysts are a single compound with a fixed structure, and are known as single-site catalysts, in which all active sites have the same polymerization properties. Polymers polymerized with such metallocene catalysts have narrow molecular weight distributions, uniform comonomer distributions, and higher copolymerization activity than Ziegler-Natta catalysts.
[0004] Meanwhile, linear low-density polyethylene (LLDPE) is produced by copolymerizing ethylene and α-olefins at low pressure using a polymerization catalyst, and has a narrow molecular weight distribution, short chain branches (SCB) of a certain length, and generally no long chain branches (LCB). Films produced from linear low-density polyethylene have high breaking strength and elongation, excellent tear strength, impact strength, etc. in addition to the general properties of polyethylene, so they are widely used in stretch films and overlap films where it is difficult to use conventional low-density polyethylene or high-density polyethylene.
[0005] However, linear low density polyethylene produced by metallocene catalysts has poor processability due to its narrow molecular weight distribution, and films produced therefrom tend to have poor heat sealing properties.
[0006] Therefore, there is a demand for an olefin polymer which can be used to produce a film having excellent processability and mechanical strength, particularly excellent drop impact strength. Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide an olefin polymer from which an olefin polymer film having excellent processability and mechanical strength, particularly excellent drop impact strength, can be produced.
[0008] Another object of the present invention is to provide an olefin polymer film which is produced from the above olefin polymer and which has excellent mechanical strength, particularly excellent drop impact strength. It is still another object of the present invention to provide a method for producing the olefin polymer and the olefin polymer film. [Means for solving the problem]
[0009] According to one embodiment of the present invention, (1) the density is 0.915 to 0.935 g / cm 3 , preferably 0.915 to 0.930 g / cm 3 (2) Melt index (I 2.16 (3) a melt index (I) measured at 190° C. under a load of 21.6 kg; 21.6 ) and the melt index (I 2.16 The present invention provides an olefin-based polymer having (i) a melt flow ratio (MFR) of 20 to 50, preferably 20 to 45, and (ii) a comonomer distribution slope (CDS) defined by the following mathematical formula 1 of 3 or more, preferably 3 to 15, wherein a film produced from the olefin-based polymer has a drop impact strength of 1,200 to 1,550 g based on a thickness of 50 μm:
[0010]
number
[0011] In the above formula 1, C 20 and C 80 are the comonomer contents at the cumulative weight fractions of 20% and 80% in the comonomer distribution, respectively, and M 20 and M. 80 are the molecular weights at the cumulative weight fractions of 20% and 80%, respectively, in the comonomer distribution.
[0012] In a specific example of the present invention, the olefin polymer may be prepared by polymerizing an olefin monomer in the presence of a hybrid catalyst including at least one first transition metal compound represented by the following chemical formula 1 and at least one second transition metal compound selected from the group consisting of a compound represented by the following chemical formula 2 and a compound represented by the following chemical formula 3:
[0013] [ka] In the above Chemical Formulas 1 to 3, M 1 and M. 2 are different from each other and are each independently titanium (Ti), zirconium (Zr), or hafnium (Hf); X is independently halogen, C 1-20 Alkyl, C 2-20 Alkenyl, C 2-20 Alkynyl, C 6-20 Aryl, C 1-20 Alkyl C 6-20 Aryl, C 6-20 Aryl C 1-20 Alkyl, C 1-20 Alkylamide, or C 6-20 is an aryl amide, R 1 ~R 10 each independently represents hydrogen, a substituted or unsubstituted C 1-20 Alkyl, substituted or unsubstituted C 2-20 Alkenyl, substituted or unsubstituted C 6-20 Aryl, substituted or unsubstituted C 1-20 Alkyl C 6-20 Aryl, substituted or unsubstituted C 6-20 Aryl C 1-20 Alkyl, substituted or unsubstituted C 1-20 Heteroalkyl, substituted or unsubstituted C 3-20 Heteroaryl, substituted or unsubstituted C 1-20 Alkylamide, substituted or unsubstituted C 6-20 Arylamide, substituted or unsubstituted C 1-20 Alkylidene, or substituted or unsubstituted C 1-20Cyril, R 1 ~R 10 each independently represents a substituted or unsubstituted, saturated or unsaturated C 4-20 A ring may be formed.
[0014] In an embodiment of the present invention, M 1 and M. 2 are different from each other and are zirconium or hafnium, and X is a halogen or C 1-20 is alkyl, R 1 ~R 10 are hydrogen, substituted or unsubstituted C 1-20 Alkyl, substituted or unsubstituted C 1-20 Alkenyl, or substituted or unsubstituted C 6-20 It may be aryl. In a preferred embodiment of the present invention, M 1 is hafnium, M 2 may be zirconium and X may be chlorine or methyl.
[0015] In a preferred embodiment of the present invention, the first transition metal compound may be at least one of the transition metal compounds represented by the following chemical formulas 1-1 and 1-2, and the second transition metal compound may be at least one of the transition metal compounds represented by the following chemical formulas 2-1, 2-2, and 3-1.
[0016] [ka] In the above formula, Me is a methyl group.
[0017] In an embodiment of the present invention, the molar ratio of the secondary transition metal compound to the first transition metal compound ranges from 100:1 to 1:100.
[0018] In a specific example of the present invention, the catalyst may include at least one promoter selected from the group consisting of a compound represented by the following formula 4, a compound represented by the following formula 5, and a compound represented by the following formula 6:
[0019] [ka] [Chemical formula 6] [LH] + [Z(A) 4 ] - or [L] + [Z(A) 4 ] -
[0020] In the above Chemical Formula 4, n is an integer of 2 or more, and R a is a halogen atom, C 1-20 Hydrocarbon or halogen-substituted C 1-20 is a hydrocarbon group, In the above formula 5, D is aluminum (Al) or boron (B), and R b , R c , and R d are each independently a halogen atom, C 1-20 Hydrocarbon radicals, halogen-substituted C 1-20 Hydrocarbon group, or C 1-20 is an alkoxy group, In the above formula 6, L is a neutral or cationic Lewis base, [LH] + and [L] + is a Bronsted acid, Z is a Group 13 element, and each A is independently a substituted or unsubstituted C 6-20 an aryl group or a substituted or unsubstituted C 1-20 It is an alkyl group.
[0021] In an embodiment of the present invention, the catalyst may further comprise a support supporting the transition metal compound, the cocatalyst compound, or both. In a preferred embodiment of the present invention, the support may comprise at least one selected from the group consisting of silica, alumina, and magnesia.
[0022] Here, the total amount of the hybrid transition metal compounds supported on the support is 0.001 to 1 mmole based on 1 g of the support, and the total amount of the promoter compounds supported on the support is 2 to 15 mmole based on 1 g of the support.
[0023] In a specific example of the present invention, the olefin polymer is a copolymer of an olefin monomer and an olefin comonomer. Specifically, the olefin monomer may be ethylene, and the olefin comonomer may be at least one selected from the group consisting of propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-undecene, 1-dodecene, 1-tetradecene, and 1-hexadecene. Preferably, the olefin polymer is a linear low-density polyethylene in which the olefin monomer is ethylene and the olefin comonomer is 1-hexene.
[0024] According to one embodiment of the present invention, the present invention includes a step of polymerizing an olefin-based monomer in the presence of a hybrid catalyst containing at least one first transition metal compound represented by the above formula 1 and at least one second transition metal compound selected from the group consisting of the compound represented by the above formula 2 and the compound represented by the above formula 3 to obtain an olefin-based polymer, and the olefin-based polymer (1) has a density of 0.915 to 0.935 g / cm 3 , preferably 0.915 to 0.930 g / cm 3 (2) Melt index (I 2.16 (3) a melt index (I) measured at 190° C. under a load of 21.6 kg; 21.6 ) and the melt index (I 2.16(3) the melt flow ratio (MFR) of the copolymer is 20 to 50, preferably 20 to 45, and (4) the comonomer distribution slope (CDS) defined by the above mathematical formula 1 is 3 or more, preferably 3 to 15, and the film produced thereby has a drop impact strength of 1,200 to 1,550 g based on a thickness of 50 μm.
[0025] In an embodiment of the present invention, the polymerization of the olefinic monomer may be carried out by gas phase polymerization, specifically, the polymerization of the olefinic monomer may be carried out in a gas phase fluidized bed reactor. Effect of the Invention
[0026] The olefin polymer according to the embodiment of the present invention has excellent processability, and a film produced therefrom, in particular a linear low-density polyethylene film, has excellent mechanical strength, in particular drop impact strength. [Brief description of the drawings]
[0027] [Figure 1] 1 is a GPC-FTIR graph for explaining a method for measuring CDS defined by Equation 1. [Diagram 2] 1 is a GPC-FTIR graph for measuring CDS of the olefin polymer of Example 1. [Diagram 3] 1 is a GPC-FTIR graph for measuring CDS of the olefin polymer of Example 2. [Figure 4] 1 is a GPC-FTIR graph for measuring CDS of the olefin polymer of Example 3. [Diagram 5] 1 is a GPC-FTIR graph for measuring CDS of the olefin polymer of Example 4. [Figure 6] 1 is a GPC-FTIR graph for measuring CDS of the olefin polymer of Example 5. [Figure 7] 1 is a GPC-FTIR graph for measuring CDS of the olefin polymer of Comparative Example 1. [Figure 8] 1 is a GPC-FTIR graph for measuring CDS of the olefin polymer of Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] The present invention will now be described in more detail. Olefin Polymers According to one embodiment of the present invention, (1) the density is 0.915 to 0.935 g / cm 3 (2) Melt index (I 2.16 (3) the melt index (I 21.6 ) and the melt index (I 2.16 and (4) an olefin-based polymer having a comonomer distribution slope (CDS) defined by the following mathematical formula 1 of 3 or more, wherein a film produced from the olefin-based polymer has a drop impact strength of 1,200 to 1,550 g based on a thickness of 50 μm.
[0029] In a specific example of the present invention, the olefin polymer has a density of 0.915 to 0.935 g / cm 3 Preferably, the density of the olefin polymer is 0.915 to 0.930 g / cm 3 may be also.
[0030] In an embodiment of the present invention, the olefin polymer has a melt index (I 2.16 The melt index of the olefin polymer measured at 190° C. under a load of 2.16 kg is preferably 0.5 to 2.0 g / 10 min.
[0031] In an embodiment of the present invention, the olefin polymer has a melt index (I 21.6 ) and the melt index (I 2.16 ) is 20 to 50. The MFR of the olefin polymer may preferably be 20 to 45.
[0032] In a specific example of the present invention, the olefin-based polymer has a comonomer distribution slope (CDS) defined by the following mathematical formula 1 of 3 or more. Preferably, the CDS of the olefin-based polymer may be 3-15.
[0033]
number
[0034] In the above formula 1, C 20 and C 80 are the comonomer contents at the cumulative weight fractions of 20% and 80% in the comonomer distribution, respectively, and M 20 and M. 80 are the molecular weights at the cumulative weight fractions of 20% and 80%, respectively, in the comonomer distribution.
[0035] The CDS of an olefin polymer indicates the gradient of the comonomer content versus molecular weight at the cumulative weight fraction points of 20% and 80% in a comonomer distribution graph. The higher the CDS of an olefin polymer, the more the copolymer is concentrated in the polymer chain with a high molecular weight, and the better the mechanical strength and heat sealing properties can be. Here, the comonomer distribution of the olefin polymer can be continuously measured together with the molecular weight and molecular weight distribution of the polymer using a GPC-FTIR device.
[0036] In a specific example of the present invention, a film made from an olefin polymer has a drop impact strength of 1,200 to 1,550 g based on a thickness of 50 μm. Preferably, a film made from an olefin polymer may have a drop impact strength of 1,250 to 1,550 g based on a thickness of 50 μm.
[0037] The olefin polymer according to the embodiment of the present invention has a relatively broad molecular weight distribution and a relatively large amount of short chain branches in the high molecular weight component, and therefore, it is understood that the olefin polymer film produced therefrom has excellent mechanical strength, particularly drop impact strength.
[0038] In embodiments of the present invention, the olefin polymer films may be effectively used as stretch films, overwrap films, ramie, silage wrap, agricultural films, and the like.
[0039] In the specific example of the present invention, the method for forming a film from the olefin-based polymer according to the embodiment of the present invention is not particularly limited, and a forming method known in the technical field to which the present invention belongs may be used. For example, the above-mentioned olefin-based polymer may be processed by a conventional method such as inflation film forming, extrusion molding, casting molding, etc., to produce an olefin-based polymer film. Among them, inflation film forming is the most preferable.
[0040] In a specific example of the present invention, the olefin polymer may be produced by polymerizing an olefin monomer in the presence of a hybrid catalyst containing at least one first transition metal compound represented by the following chemical formula 1 and at least one second transition metal compound selected from the group consisting of a compound represented by the following chemical formula 2 and a compound represented by the following chemical formula 3:
[0041] [ka] In the above Chemical Formulas 1 to 3, M 1 and M. 2are different from each other and are each independently titanium (Ti), zirconium (Zr), or hafnium (Hf). 1 and M. 2 are different from each other and may be zirconium or hafnium. 1 is hafnium, M 2 may be zirconium.
[0042] X is independently halogen, C 1-20 Alkyl, C 2-20 Alkenyl, C 2-20 Alkynyl, C 6-20 Aryl, C 1-20 Alkyl C 6-20 Aryl, C 6-20 Aryl C 1-20 Alkyl, C 1-20 Alkylamide, or C 6-20 Specifically, X is a halogen or C 1-20 It may be alkyl. Preferably, X is chlorine or methyl.
[0043] R 1 ~R 10 each independently represents hydrogen, a substituted or unsubstituted C 1-20 Alkyl, substituted or unsubstituted C 2-20 Alkenyl, substituted or unsubstituted C 6-20 Aryl, substituted or unsubstituted C 1-20 Alkyl C 6-20 Aryl, substituted or unsubstituted C 6-20 Aryl C 1-20 Alkyl, substituted or unsubstituted C 1-20 Heteroalkyl, substituted or unsubstituted C 3-20 Heteroaryl, substituted or unsubstituted C 1-20 Alkylamide, substituted or unsubstituted C 6-20 Arylamide, substituted or unsubstituted C 1-20 Alkylidene, or substituted or unsubstituted C 1-20 Cyril, where R 1 ~R 10each independently represents a substituted or unsubstituted, saturated or unsaturated C 4-20 A ring may be formed. Specifically, R 1 ~R 10 are hydrogen, substituted or unsubstituted C 1-20 Alkyl, substituted or unsubstituted C 1-20 Alkenyl, or substituted or unsubstituted C 6-20 It may be aryl.
[0044] In an embodiment of the present invention, M 1 and M. 2 are different from each other and are zirconium or hafnium, and X is a halogen or C 1-20 is alkyl, R 1 ~R 10 are hydrogen, substituted or unsubstituted C 1-20 Alkyl, substituted or unsubstituted C 1-20 Alkenyl, or substituted or unsubstituted C 6-20 It may be aryl. In a preferred embodiment of the present invention, M 1 is hafnium, M 2 may be zirconium and X may be chlorine or methyl.
[0045] In a preferred embodiment of the present invention, the first transition metal compound may be at least one of the transition metal compounds represented by the following chemical formulas 1-1 and 1-2, and the second transition metal compound may be at least one of the transition metal compounds represented by the following chemical formulas 2-1, 2-2, and 3-1.
[0046] [ka] In the above formula, Me is a methyl group.
[0047] In a specific example of the present invention, the molar ratio of the second transition metal compound to the first transition metal compound is in the range of 100:1 to 1:100. Preferably, the molar ratio of the second transition metal compound to the first transition metal compound is in the range of 50:1 to 1:50. Preferably, the molar ratio of the second transition metal compound to the first transition metal compound is in the range of 10:1 to 1:10.
[0048] In a specific example of the present invention, the catalyst may include at least one promoter compound selected from the group consisting of a compound represented by the following formula 4, a compound represented by the following formula 5, and a compound represented by the following formula 6:
[0049] [ka]
[0050] In the above Chemical Formula 4, n is an integer of 2 or more, and R a is a halogen atom, C 1-20 Hydrocarbon or halogen-substituted C 1-20 Specifically, R a may be methyl, ethyl, n-butyl, or isobutyl.
[0051] [ka]
[0052] In the above formula 5, D is aluminum (Al) or boron (B), and R b , R c , and R d are each independently a halogen atom, C 1-20 Hydrocarbon radicals, halogen-substituted C 1-20 Hydrocarbon group, or C 1-20 Specifically, when D is aluminum (Al), R b , R c , and R d may each independently be methyl or isobutyl, and when D is boron (B), Rb , R c , and R d may each be pentafluorophenyl.
[0053] [Chemical formula 6] [LH] + [Z(A) 4 ] - or [L] + [Z(A) 4 ] -
[0054] In the above formula 6, L is a neutral or cationic Lewis base, [LH] + and [L] + is a Bronsted acid, Z is a Group 13 element, and each A is independently a substituted or unsubstituted C 6-20 an aryl group or a substituted or unsubstituted C 1-20 It is an alkyl group. Specifically, [LH] + may be a dimethylanilinium cation, [Z(A) 4 ] - is [B(C 6 F 5 ) 4 ] - [L] + is [(C 6 H 5 ) 3 C] + may be also.
[0055] Specifically, examples of the compound represented by Chemical Formula 4 include methylaluminoxane, ethylaluminoxane, isobutylaluminoxane, butylaluminoxane, etc., and methylaluminoxane is preferred, but is not limited thereto.
[0056] Examples of the compound represented by Chemical Formula 5 include trimethylaluminum, triethylaluminum, triisobutylaluminum, tripropylaluminum, tributylaluminum, dimethylchloroaluminum, triisopropylaluminum, tri-s-butylaluminum, tricyclopentylaluminum, tripentylaluminum, triisopentylaluminum, trihexylaluminum, trioctylaluminum, ethyldimethylaluminum, methyldiethylaluminum, triphenylaluminum, tri-p-tolylaluminum, dimethylaluminum methoxide, dimethylaluminum ethoxide, trimethylboron, triethylboron, triisobutylboron, tripropylboron, and tributylboron, among which trimethylaluminum, triethylaluminum, and triisobutylaluminum are preferred, but are not limited thereto.
[0057] Examples of the compound represented by Chemical Formula 6 include triethylammonium tetraphenylboron, tributylammonium tetraphenylboron, trimethylammonium tetraphenylboron, tripropylammonium tetraphenylboron, trimethylammonium tetra(p-tolyl)boron, trimethylammonium tetra(o,p-dimethylphenyl)boron, tributylammonium tetra(p-trifluoromethylphenyl)boron, trimethylammonium tetra(p-trifluoromethylphenyl)boron, tributylammonium tetrapentafluorophenylboron, N,N-diethylanilinium tetraphenylboron, N,N-diethylanilinium tetrapentafluorophenylboron, diethylammonium tetrapentafluorophenylboron, triphenylphosphonium tetraphenylboron, trimethylphosphonium tetraphenylboron, triethylammonium tetraphenylaluminum, and tributylammonium tetraphenylaluminum. ammonium, trimethylammonium tetraphenylaluminum, tripropylammonium tetraphenylaluminum, trimethylammonium tetra(p-tolyl)aluminum, tripropylammonium tetra(p-tolyl)aluminum, triethylammonium tetra(o,p-dimethylphenyl)aluminum, tributylammonium tetra(p-trifluoromethylphenyl)aluminum, trimethylammonium tetra(p-trifluoromethylphenyl)aluminum, tributylammonium tetrapentafluorophenylaluminum, N,N-diethylanilinium tetraphenylaluminum, N,N-diethylanilinium tetrapentafluorophenylaluminum, diethylammonium tetrapentatetraphenylaluminum, triphenylphosphonium tetraphenylaluminum, trimethylphosphonium tetraphenylaluminum, tripropylammonium tetra(p-tolyl)boron, triethylammonium tetra(o,p-dimethylphenyl)boron, tributylammonium tetra(p-trifluoromethylphenyl)boron, triphenylcarbonium tetra(p-trifluoromethylphenyl)boron, triphenylcarbonium tetrapentafluorophenylboron, etc.
[0058] In an embodiment of the present invention, the catalyst may further comprise a support supporting the transition metal compound, the cocatalyst compound, or both. Specifically, the support may support both the transition metal compound and the cocatalyst compound.
[0059] In this case, the carrier may include a substance containing a hydroxyl group on the surface, and preferably a substance having a highly reactive hydroxyl group and a siloxane group, which has been dried to remove moisture from the surface, may be used. For example, the carrier may include at least one selected from the group consisting of silica, alumina, and magnesia. Specifically, silica, silica-alumina, and silica-magnesia, etc., which have been dried at high temperatures, may be used as the carrier, and these usually contain Na 2 OK 2 CO 3 , BaSO 4 , and Mg(NO 3 ) 2 The catalyst may contain oxides, carbonates, sulfates, and nitrates such as those mentioned above. These may also contain carbon, zeolite, magnesium chloride, etc. However, the carrier is not limited to these, and is not particularly limited as long as it can support the transition metal compound and the promoter compound.
[0060] The carrier may have an average particle size of 10 to 250 μm, preferably an average particle size of 10 to 150 μm, and more preferably an average particle size of 20 to 100 μm.
[0061] The volume of the micropores in the support may be 0.1 to 10 cc / g, preferably 0.5 to 5 cc / g, and more preferably 1.0 to 3.0 cc / g.
[0062] The specific surface area of the support is 1 to 1,000 m2 / g, preferably 100 to 800m 2 / g, more preferably 200 to 600m 2 / g.
[0063] In a preferred embodiment of the present invention, the support may be silica. In this case, the drying temperature of the silica may be 200 to 900° C. The drying temperature may be preferably 300 to 800° C., more preferably 400 to 700° C. If the drying temperature is less than 200° C., the moisture content is too high, and the moisture on the surface reacts with the promoter compound, and if the drying temperature exceeds 900° C., the structure of the support may collapse.
[0064] The concentration of hydroxyl groups in the dried silica may be 0.1 to 5 mmole / g, preferably 0.7 to 4 mmole / g, and more preferably 1.0 to 2 mmole / g. If the concentration of hydroxyl groups is less than 0.1 mmole / g, the amount of the promoter compound supported will be low, and if it exceeds 5 mmole / g, a problem of inactivation of the catalyst component may occur.
[0065] The total amount of the transition metal compound supported on the carrier may be 0.001 to 1 mmole based on 1 g of the carrier. When the ratio of the transition metal compound to the carrier satisfies the above range, appropriate supported catalytic activity is exhibited, which is advantageous in terms of maintaining the activity of the catalyst and in terms of economic efficiency.
[0066] The total amount of the promoter compounds supported on the carrier may be 2 to 15 mmole per gram of carrier. If the ratio of the promoter compounds to the carrier satisfies the above range, it is advantageous in terms of maintaining the activity of the catalyst and economic efficiency.
[0067] One or more types of carriers may be used. For example, both the transition metal compound and the co-catalyst compound may be supported on one carrier, or the transition metal compound and the co-catalyst compound may be supported on two or more carriers. In addition, only one of the transition metal compound and the co-catalyst compound may be supported on the carrier.
[0068] As a method for supporting a transition metal compound and / or a cocatalyst compound that can be used in an olefin polymerization catalyst, a physical adsorption method or a chemical adsorption method may be used.
[0069] For example, the physical adsorption method may be a method in which a solution in which a transition metal compound is dissolved is brought into contact with a support and then dried; a method in which a solution in which a transition metal compound and a promoter compound are dissolved is brought into contact with a support and then dried; or a method in which a solution in which a transition metal compound is dissolved is brought into contact with a support and then dried to produce a support on which a transition metal compound is supported, and separately, a solution in which a promoter compound is dissolved is brought into contact with a support and then dried to produce a support on which a promoter compound is supported, and then these are mixed.
[0070] The chemical adsorption method may be a method in which a promoter compound is first supported on the surface of a carrier, and then a transition metal compound is supported on the promoter compound, or a method in which a catalyst compound is covalently bonded to a functional group on the carrier surface (for example, in the case of silica, a hydroxy group (-OH) on the silica surface).
[0071] In an embodiment of the present invention, the olefin-based polymer may be a homopolymer of an olefin-based monomer or a copolymer of an olefin-based monomer and a comonomer. Preferably, the olefin-based polymer is a copolymer of an olefin-based monomer and an olefin-based comonomer.
[0072] Here, the olefin monomer is C 2-20 α-olefin, C 1-20 Diolefin, C 3-20 Cycloolefin, and C 3-20 At least one selected from the group consisting of cyclodiolefins.
[0073] For example, the olefin monomer may be ethylene, propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-undecene, 1-dodecene, 1-tetradecene, or 1-hexadecene, and the olefin polymer may be a homopolymer containing only one of the olefin monomers exemplified above, or a copolymer containing two or more of them.
[0074] In an exemplary embodiment, the olefin polymer comprises ethylene and C 3-20 The olefin-based polymer may be a copolymer in which an α-olefin is copolymerized. Preferably, the olefin-based polymer may be a linear low-density polyethylene in which the olefin-based monomer is ethylene and the olefin-based comonomer is 1-hexene.
[0075] In this case, the ethylene content is preferably 55 to 99.9% by weight, more preferably 90 to 99.9% by weight, and the α-olefin comonomer content is preferably 0.1 to 45% by weight, more preferably 0.1 to 10% by weight.
[0076] Method for producing olefin polymer According to one embodiment of the present invention, there is provided a method for producing an olefin polymer, comprising the step of polymerizing an olefin monomer in the presence of a hybrid catalyst comprising at least one first transition metal compound represented by the following chemical formula 1 and at least one second transition metal compound selected from a compound represented by the following chemical formula 2 and a compound represented by the following chemical formula 3, to obtain an olefin polymer:
[0077] [ka] In the above chemical formula, M 1 , M 2 , X, and R 1 ~R 10 is the same as that explained in the section on olefin-based polymers.
[0078] As described above, the olefin polymer produced by the production method according to one embodiment of the present invention has the following characteristics: (1) density of 0.915 to 0.935 g / cm 3 , preferably 0.915 to 0.930 g / cm 3 (2) Melt index (I 2.16 (3) a melt index (I) measured at 190° C. under a load of 21.6 kg; 21.6 ) and the melt index (I 2.16 (4) the comonomer distribution slope (CDS) defined by the following mathematical formula 1 is 3 or more, preferably 3 to 15, and the film produced thereby has a drop impact strength of 1,200 to 1,550 g based on a thickness of 50 μm.
[0079]
number
[0080] C in the above formula 1 20 , C 80 , M 20 , and M. 80 is the same as that explained in the section on olefin-based polymers.
[0081] In embodiments of the present invention, the olefin-based polymer may be polymerized by polymerization reactions such as, but not limited to, free radical, cationic, coordination, condensation, and addition.
[0082] As an embodiment of the present invention, the olefin polymer may be produced by a gas phase polymerization method, a solution polymerization method, a slurry polymerization method, etc. Preferably, the polymerization of the olefin monomer may be carried out by gas phase polymerization, specifically, the polymerization of the olefin monomer may be carried out in a gas phase fluidized bed reactor.
[0083] When olefin polymers are produced by solution polymerization or slurry polymerization, examples of solvents that can be used include C tetrahydrofurans such as pentane, hexane, heptane, nonane, decane, and their isomers. 5-12 Examples of the solvent include, but are not limited to, aliphatic hydrocarbon solvents; aromatic hydrocarbon solvents such as toluene and benzene; chlorine-substituted hydrocarbon solvents such as dichloromethane and chlorobenzene; and mixtures thereof.
[0084] Working Example The present invention will be described in more detail below with reference to examples. However, the following examples are merely for the purpose of illustrating the present invention, and the scope of the present invention is not limited thereto.
[0085] Manufacturing Example The transition metal compound of formula 1-1 (bis(n-propylcyclopentadienyl)hafnium dichloride) and the transition metal compound of formula 2-1 (bis(n-butylcyclopentadienyl)zirconium dichloride) were purchased from TCI, and the transition metal compound of formula 1-2 (dimethylbis(n-propylcyclopentadienyl)hafnium dichloride), the transition metal compound of formula 2-2 (bis(i-butylcyclopentadienyl)zirconium dichloride), and the transition metal compound of formula 3-1 ((pentamethylcyclopentadienyl)(n-propylcyclopentadienyl)zirconium dichloride) were purchased from MCN and used without further purification.
[0086] Manufacturing Example 1 4.47g of the transition metal compound of formula 1-1 and 1.67g of the transition metal compound of formula 2-1 were added to 892g of a 10% methylaluminoxane toluene solution and stirred at room temperature for 1 hour. After the reaction, the solution was added to 200g of silica (XPO-2402), and 1.5 liters of toluene were added and stirred at 70°C for 2 hours. The catalyst after the support was washed with 500ml of toluene and dried overnight in a vacuum at 60°C to obtain 280g of a powdered supported catalyst.
[0087] Manufacturing Example 2 278 g of a supported catalyst was obtained in the same manner as in Preparation Example 1, except that 4.47 g of the transition metal compound of formula 1-1 and 1.67 g of the transition metal compound of formula 2-2 were used.
[0088] Production Example 3 280 g of a supported catalyst was obtained in the same manner as in Preparation Example 1, except that 4.47 g of the transition metal compound of formula 1-1 and 1.68 g of the transition metal compound of formula 3-1 were used.
[0089] Production Example 4 275 g of a supported catalyst was obtained in the same manner as in Preparation Example 1, except that 4.07 g of the transition metal compound of formula 1-2 and 1.67 g of the transition metal compound of formula 2-2 were used.
[0090] Production Example 5 278 g of a supported catalyst was obtained in the same manner as in Preparation Example 1, except that 4.07 g of the transition metal compound of formula 1-2 and 1.68 g of the transition metal compound of formula 3-1 were used.
[0091] Examples 1 to 5 Using a gas-phase fluidized bed reactor, ethylene / 1-hexene copolymers were produced in the presence of the supported catalysts obtained in Production Examples 1 to 5. The ethylene partial pressure in the reactor was about 15 kg / cm. 2 The polymerization temperature was maintained at 80 to 90°C. The polymerization conditions for the above examples are shown in Table 1 below.
[0092] [Table 1]
[0093] Comparative Examples 1-2 For comparison, Hanwha Solutions' linear low-density polyethylene M1810HN (density 0.9180 g / cm 3 , melt index 1.0 g / 10 min; Comparative Example 1) and M2010EN (density 0.9200 g / cm 3 , melt index 1.0 g / 10 min; Comparative Example 2) was used.
[0094] Test Example The physical properties of the olefin polymers of the above examples were measured according to the following methods and standards, and the results are shown in Table 2 below.
[0095] (1) Density Measured according to ASTM D1505.
[0096] (2) Melt index and melt flow ratio (MFR) According to ASTM D1238, the melt index was measured at 190°C under a load of 21.6 kg and 2.16 kg, and the ratio (MI 21.6 / MI 2.16 ) was sought.
[0097] (3) Comonomer Distribution Gradient (CDS) The measurements were performed at 170°C using gel permeation chromatography-FTIR (GPC-FTIR).
[0098] [Table 2]
[0099] Each of the resins in Examples 1 to 5 and Comparative Examples 1 and 2 was processed into a 50 μm thick film through a 40 mm blown film extruder (40 mm Φ screw, 75 mm Φ die, 2 mm die gap). The extrusion conditions were fixed as follows: C1 / C2 / C3 / A / D1 / D2=160 / 165 / 170 / 175 / 180 / 180°C, screw speed 60 rpm, blow-up ratio (BUR) 2. The physical properties of the olefin polymer films of the above examples and comparative examples were measured according to the following methods and standards, and the results are shown in Table 3 below.
[0100] (4) Drop impact strength The drop impact strength was measured according to the ASTM D1709(A) method in which a 50 μm thick film was fixed and then a weight with a diameter of 38.10±0.13 mm was dropped from a height of 0.66±0.01 m.
[0101] (5) Haze A film having a standard thickness of 50 μm was formed and measured in accordance with ASTM D1003. Each test piece was measured five times and the average value was calculated.
[0102] [Table 3] [Industrial Applicability]
[0103] The olefin polymer according to the embodiment of the present invention has excellent processability, and the olefin polymer film produced therefrom, specifically, a linear low density polyethylene film, has excellent mechanical strength, particularly drop impact strength.
Claims
1. (1) Density is 0.915 to 0.935 g / cm 3 (2) the melt index (I 2.16 (3) a melt index (I) measured at 190° C. under a load of 21.6 kg; 21.6 ) and the melt index (I 2.16 (4) a comonomer distribution slope (CDS) defined by the following Equation 1 is 3 or more, and a film produced therefrom has a drop impact strength of 1,200 to 1,550 g based on a thickness of 50 μm: The present invention is produced by polymerizing an olefin monomer in the presence of a hybrid catalyst comprising at least one first transition metal compound represented by the following chemical formulas 1-1 and 1-2, and at least one second transition metal compound represented by the following chemical formulas 2-1, 2-2, and 3-1: The olefin polymer is a copolymer of an olefin monomer and an olefin comonomer, The olefin-based polymer, wherein the olefin-based monomer is ethylene and the olefin-based comonomer is 1-hexene. 【number】 In the above formula, Me is a methyl group. [0010] Here, C 20 and C 80 are the comonomer contents at the cumulative weight fraction points of 20% and 80% in the comonomer distribution, respectively, and M 20 and M. 80 are the molecular weights at the cumulative weight fractions of 20% and 80%, respectively, in the comonomer distribution.
2. (1) The density of the olefin polymer is 0.915 to 0.930 g / cm 3 (2) a melt index measured at 190° C. under a load of 2.16 kg is 0.5 to 2.0 g / 10 min; (3) an MFR is 20 to 45; and (4) a CDS is 3 to 15.
3. 2. The olefin polymer according to claim 1, wherein the molar ratio of the second transition metal compound to the first transition metal compound is in the range of 100:1 to 1:
100.
4. The olefin polymer according to claim 1, wherein the catalyst comprises at least one promoter compound selected from the group consisting of compounds represented by the following chemical formula 4, compounds represented by the following chemical formula 5, and compounds represented by the following chemical formula 6: 【Chemistry 2】 [Chemical formula 6] [L-H] + [Z(A) 4 ] - Or [L] + [Z(A) 4 ] - In the above formula 4, n is an integer of 2 or more, R a is a halogen atom, C 1-20 Hydrocarbon group or halogen-substituted C 1-20 is a hydrocarbon group, In the above formula 5, D is aluminum (Al) or boron (B), R b , R c , and R d are each independently a halogen atom, C 1-20 Hydrocarbon groups, halogen-substituted C 1-20 Hydrocarbon group, or C 1-20 is an alkoxy group, In the above formula 6, L is a neutral or cationic Lewis base, [L-H] + and [L] + is a Bronsted acid, Z is a Group 13 element, and each A is independently a substituted or unsubstituted C 6-20 an aryl group or a substituted or unsubstituted C 1-20 It is an alkyl group.
5. The olefin-based polymer according to claim 4 , wherein the catalyst further comprises a support supporting the transition metal compound, the cocatalyst compound, or both.
6. The olefin-based polymer according to claim 5 , wherein the support comprises at least one selected from the group consisting of silica, alumina, and magnesia.
7. The total amount of the hybrid transition metal compounds supported on the support is 0.001 to 1 mmole based on 1 g of the support, and the total amount of the co-catalyst compounds supported on the support is 2 to 15 mmole based on 1 g of the support. The olefin polymer according to claim 5.
8. The olefin-based polymer according to claim 1 , wherein the olefin-based polymer is a linear low-density polyethylene.
9. The present invention relates to a method for producing an olefin polymer by polymerizing an olefin monomer in the presence of a hybrid catalyst, the hybrid catalyst comprising at least one first transition metal compound represented by the following chemical formulas 1-1 and 1-2, and the hybrid catalyst comprising at least one second transition metal compound represented by the following chemical formulas 2-1, 2-2, and 3-1, the hybrid catalyst comprising at least one first transition metal compound represented by the following chemical formulas 2-1, 2-2, and 3-1, the hybrid catalyst comprising at least one second ... 3 (2) the melt index (I 2.16 (3) a melt index (I) measured at 190° C. under a load of 21.6 kg; 21.6 ) and the melt index (I 2.16 (4) a comonomer distribution slope (CDS) defined by the following Equation 1 is 3 or more, and the film produced thereby has a drop impact strength of 1,200 to 1,550 g based on a thickness of 50 μm, The olefin polymer is a copolymer of an olefin monomer and an olefin comonomer, The method for producing an olefin polymer, wherein the olefin monomer is ethylene and the olefin comonomer is 1-hexene. 【number】 In the above formula, Me is a methyl group. [0025] C in the above formula 1 20 , C 80 , M. 20 , and M 80 is as defined in claim 1.
10. The method for producing an olefin polymer according to claim 9, wherein the polymerization of the olefin monomer is carried out by gas phase polymerization.
Citation Information
Patent Citations
Addition polymerization catalyst component, production method for addition polymerization catalyst and addition polymer, and use of metallocene transition metal compound
JP2003096125A
Ethylene polymer excellent in processability
JP2004149760A
Dual Metallocene Catalysts for Making Film Resins with Excellent Machine Direction (md) Elmendorf Tear Strength
JP2007518871A
Mixed composition of hafnium compound and zirconium compound and method for producing the same
JP2015113282A
Ethylene copolymer compositions, films and polymerization processes
JP2016504442A