Rubber foam, laminate, and method for producing rubber foam

A rubber foam composition with EPDM and EVA, along with specific flame retardants, addresses contamination and adhesion issues, ensuring low sulfur content and high flame retardancy for electronic substrates.

JP7577601B2Active Publication Date: 2024-11-05INOAC CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2021075594
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-04-28
Publication Date
2024-11-05
Estimated Expiration
2041-04-28

AI Technical Summary

Technical Problem

The use of EPDM foam in electronic substrates can lead to contamination due to sulfur, risking contact failure, and existing laminates lack sufficient adhesion and flame retardancy.

Method used

A rubber foam composition containing EPDM, EVA, crosslinking agents, and nitrogen-based or phosphorus-based flame retardants, with a specific blend ratio and additives to minimize contamination and enhance adhesion and flame retardancy.

Benefits of technology

The rubber foam achieves low contamination, high adhesion to electronic boards, and meets stringent flame retardancy standards, including a 50-second combustion time in the UL94 vertical combustion test.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577601000005
    Figure 0007577601000005
  • Figure 0007577601000001
    Figure 0007577601000001
  • Figure 0007577601000002
    Figure 0007577601000002
Patent Text Reader

Abstract

To provide a rubber foam having reduced tendency to contaminate electronic boards and the like.SOLUTION: A rubber foam 1 is a foamed composition containing EPDM, EVA of the following blend ratio, a crosslinker, a crosslinking aid having a plurality of double bonds, a foamer, and a foaming aid. The blend ratio (EPDM / EVA): 95 / 5-55 / 45 (mass ratio).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a rubber foam, a laminate, and a method for producing a rubber foam. [Background technology]

[0002] Patent Document 1 discloses a method for producing a flame-retardant EPDM foam. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2007-211119 A Summary of the Invention [Problem to be solved by the invention]

[0004] When the EPDM foam described in this document is used in the production of electronic substrates, etc., contamination due to sulfur may occur. In other words, there is a risk of contact failure of the electronic substrates, etc. The present disclosure has been made in view of the above circumstances, and has an object to provide a rubber foam that causes little contamination of electronic boards, etc. Another object of the present disclosure is to provide a laminate that causes little contamination of electronic boards, etc., and has high adhesion to adherends. The present disclosure can be realized in the following forms. [Means for solving the problem]

[0005] [1] A rubber foam, which is a foam of a composition containing EPDM, EVA in the blend ratio described below, a crosslinking agent, a crosslinking aid having a plurality of double bonds, a foaming agent, and a foaming aid. Blend ratio (EPDM / EVA): 95 / 5~55 / 45 (mass ratio) Effect of the Invention

[0006] The rubber foam of the present disclosure causes less contamination of electronic boards and the like. [Brief description of the drawings]

[0007] [Figure 1] FIG. 2 is a cross-sectional view showing a rubber foam and a laminate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Here, a preferred example of the present disclosure is given. [2] Contains at least a nitrogen-based flame retardant, The rubber foam according to [1], wherein the amount of the nitrogen-based flame retardant is 50 parts by mass or more and 150 parts by mass or less, relative to 100 parts by mass of the total amount of the EPDM and the EVA.

[0009] [3] Contains at least a phosphorus-based flame retardant, The rubber foam according to [1] or [2], wherein the amount of the phosphorus-based flame retardant is 1 part by mass or more and 20 parts by mass or less, relative to 100 parts by mass of the total amount of the EPDM and the EVA.

[0010] [4] The rubber foam according to any one of [1] to [3], having a sulfur content of 1,000 ppm or less.

[0011] [5] A laminate comprising the rubber foam according to any one of [1] to [4] and a pressure-sensitive adhesive layer laminated thereon.

[0012] [6] The laminate according to [5], wherein the pressure-sensitive adhesive layer contains an acrylic polymer.

[0013] [7] The laminate according to [5] or [6], having a peel strength to an adherend of 5 N / 25 mm width or more.

[0014] [8] A method for producing a rubber foam, comprising foaming and crosslinking a composition containing EPDM, EVA in the blend ratio described below, a crosslinking agent, a crosslinking aid having a plurality of double bonds, a foaming agent, and a foaming aid. Blend ratio (EPDM / EVA): 95 / 5~55 / 45 (mass ratio)

[0015] The present disclosure will be described in detail below. In this specification, a description using "~" for a numerical range includes the lower limit and the upper limit unless otherwise specified. For example, the description "10 to 20" includes both the lower limit "10" and the upper limit "20". In other words, "10 to 20" has the same meaning as "10 or more and 20 or less".

[0016] 1. Rubber foam 1 Rubber foam 1 is a foam of a composition containing EPDM, EVA in the blend ratio described below, a crosslinking agent, a crosslinking aid having a plurality of double bonds, a foaming agent, and a foaming aid. Blend ratio (EPDM / EVA): 95 / 5~55 / 45 (mass ratio)

[0017] (1) Composition The composition contains EPDM (ethylene-propylene-diene rubber), EVA (ethylene-vinyl acetate copolymer) in the following blend ratio, a crosslinking agent, a crosslinking aid having multiple double bonds, a foaming agent, and a foaming aid. The composition may contain at least one selected from fatty acid esters, metal hydroxides, and flame retardants as an optional component. Each component of the composition will be described.

[0018] (1.1) EPDM EPDM is a rubber obtained by copolymerization of ethylene, propylene, and dienes. EPDM is made possible to vulcanize with a vulcanizing agent by further copolymerizing dienes with an ethylene-propylene copolymer to introduce unsaturated bonds. The dienes are not particularly limited, but non-conjugated dienes are preferred, and examples of the dienes that can be used include 5-ethylidene-2-norbornene, 1,4-hexadiene, and dicyclopentadiene. From the viewpoint of obtaining the characteristics of the rubber foam 1 of the present disclosure, 5-ethylidene-2-norbornene is preferred as the diene. The content of dienes in EPDM (diene content) is not particularly limited. From the viewpoint of the crosslinking (vulcanization) reaction and the influence of mechanical properties, the content of dienes is preferably 4% by mass or more and 17% by mass or less, more preferably 7% by mass or more and 15% by mass or less. The ethylene content in EPDM is not particularly limited, but from the viewpoints of heat resistance and permanent deformation resistance, the ethylene content is preferably from 40% by mass to 80% by mass, and more preferably from 45% by mass to 60% by mass. The EPDM may be used alone or in combination of two or more kinds.

[0019] (1.2) EVA EVA is flexible and has excellent elongation, and by including EVA in the rubber foam 1, defects such as warping, cracking, and pinholes are suppressed. The melting point of EVA (DSC method) is not particularly limited. The melting point of EVA is preferably 80° C. or more and 90° C. or less from the viewpoint of improving warpage of the rubber foam 1 after molding. The melting point of EVA is measured by the DSC method according to JIS K 7121. The content of vinyl acetate in EVA is not particularly limited. From the viewpoint of appropriately softening the rubber foam 1 and suppressing defects such as warping, cracking, and pinholes, the content of vinyl acetate is preferably 1% by mass or more, and more preferably 5% by mass or more, when the mass of EVA is taken as 100% by mass. On the other hand, from the viewpoint of suppressing variations in foaming caused by excessive softening, the content of vinyl acetate is preferably 30% by mass or less, and more preferably 20% by mass or less. From these viewpoints, the content of vinyl acetate is preferably 1% by mass or more and 30% by mass or less, and more preferably 5% by mass or more and 20% by mass or less. The content of vinyl acetate is based on JIS K 6924-2. The blend ratio of EPDM to EVA (EPDM / EVA) is 95 / 5 to 60 / 40 by mass, preferably 90 / 10 to 70 / 30, and more preferably 85 / 5 to 75 / 25. When the blend ratio is within this range, warping of the rubber foam 1 after molding is suppressed, the rubber foam 1 has a good appearance, and defects such as pinholes are suppressed.

[0020] (1.3) Fatty acid esters (optional) Fatty acid esters (RCOOR', where R and R' may be the same or different) are both hydrophilic and hydrophobic. It is presumed that the fatty acid ester acts as a surfactant, reducing the aggregation of metal hydroxide and EVA, and acts as a dispersant in the rubber (rubber foam 1). Examples of fatty acid esters include glycerin fatty acid esters, higher alcohol fatty acid esters, sorbitan fatty acid esters, propylene fatty acid esters, and n-butyl stearate. The fatty acid esters may be used alone or in combination of two or more. The fatty acid ester has a melting point of 50° C. or more and 80° C. or less, and is preferably at least one selected from the group consisting of glycerin fatty acid esters and higher alcohol fatty acid esters, from the viewpoint of ease of dispersion during kneading. Examples of glycerin fatty acid esters include glycerin monostearate, glycerin monobehenate, glycerin monooleate, glycerin monolaurate, stearin distearate, glycerin dibehenate, and glycerin dioleate. Examples of higher alcohol fatty acid esters include stearyl stearate, lauryl stearate, lauryl laurate, and stearyl behenate. The amount of the fatty acid ester is not particularly limited. When the total amount of EPDM and EVA is 100 parts by mass, the fatty acid ester is preferably 1 part by mass or more, more preferably 3.0 parts by mass or more, and even more preferably 5.0 parts by mass or more, from the viewpoint of uniformly dispersing the metal hydroxide and EVA without aggregation and ensuring uniform adhesion of the rubber foam 1 to the pressure-sensitive adhesive layer 3. On the other hand, the fatty acid ester is preferably 10.0 parts by mass or less, more preferably 8.0 parts by mass or less, and even more preferably 7.0 parts by mass or less, from the viewpoint of suppressing adhesion inhibition due to oil bleeding and ensuring adhesion of the rubber foam 1 to the pressure-sensitive adhesive layer 3. From these viewpoints, the amount of the fatty acid ester is preferably 1.0 parts by mass or more and 10.0 parts by mass or less, more preferably 3.0 parts by mass or more and 8.0 parts by mass or less, and even more preferably 5.0 parts by mass or more and 7.0 parts by mass or less.

[0021] (1.4) Crosslinking agent The crosslinking agent is not particularly limited, but an organic peroxide-based crosslinking agent can be suitably used as the crosslinking agent. It is preferable not to use a sulfur crosslinking agent containing sulfur as the crosslinking agent from the viewpoint of suppressing contamination of electronic substrates, etc. Here, examples of the sulfur crosslinking agent include sulfur and sulfur compounds. The crosslinking agent may be used alone or in combination of two or more. Examples of the crosslinking agent include 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 1,1-di(t-butylperoxy)cyclohexane, dicumyl peroxide, di-t-butylperoxide, di-t-butylperoxy-3,3,5-trimethylcyclohexane, t-butylhydroperoxide, t-butylcumyl peroxide, benzoyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxine)hexyne-3, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, 2,5-dimethyl-2,5-mono(t-butylperoxy)-hexane, and α,α'-bis(t-butylperoxy-m-isopropyl)benzene. As the crosslinking agent, particularly preferred are diacyl peroxides such as 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, peroxyketals such as 1,1-di(t-butylperoxy)cyclohexane, dicumylperoxide, di-t-butylperoxide, and di-t-butylperoxy-3,3,5-trimethylcyclohexane. The amount of the crosslinking agent is not particularly limited. When the total amount of EPDM and EVA is 100 parts by mass, the amount of the crosslinking agent is preferably 0.05 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1.0 parts by mass or more, from the viewpoint of improving the crosslinking density in the rubber foam 1. On the other hand, the amount of the crosslinking agent is preferably 10.0 parts by mass or less, more preferably 4.0 parts by mass or less, and even more preferably 2.0 parts by mass or less, from the viewpoint of suppressing deterioration of the physical properties of the rubber foam 1 caused by scission of the main chain of the rubber. From these viewpoints, the amount of the crosslinking agent is preferably 0.05 parts by mass or more and 10.0 parts by mass or less, more preferably 0.5 parts by mass or more and 4.0 parts by mass or less, and even more preferably 1.0 parts by mass or more and 2.0 parts by mass or less. In addition, commercially available products are often diluted with silica, clay, calcium carbonate, etc. and sold in powder form to improve dispersibility in the compound. Furthermore, when two or more crosslinking agents are used, the amount of the crosslinking agent mentioned above means the total amount.

[0022] (1.5) Crosslinking aid (co-crosslinking agent) The cross-linking auxiliary has a plurality of double bonds. The cross-linking auxiliary preferably has a plurality of carbon-carbon double bonds. The cross-linking auxiliary preferably has a conjugated double bond. Specific examples of the crosslinking aid include quinone dioxime compounds such as p-quinone dioxime, methacrylate compounds such as ethylene glycol dimethacrylate and polyethylene glycol dimethacrylate, allyl compounds such as diallyl phthalate and triallyl cyanurate, maleimide compounds, and divinylbenzene. In particular, allyl compounds having a plurality of carbon-carbon double bonds, such as diallyl isocyanurate and triallyl isocyanurate, and methacrylate compounds having a plurality of carbon-carbon double bonds, such as ethylene glycol dimethacrylate and polyethylene glycol dimethacrylate, are preferably used. The amount of the crosslinking aid is not particularly limited. When the total amount of EPDM and EVA is 100 parts by mass, the amount of the crosslinking aid is preferably 0.5 parts by mass or more, and more preferably 1.0 parts by mass or more, from the viewpoint of improving the crosslink density in the rubber foam 1. On the other hand, the amount of the crosslinking aid is preferably 10.0 parts by mass or less, and more preferably 5.0 parts by mass or less, from the viewpoint of suppressing deterioration of the physical properties of the rubber foam 1. From these viewpoints, the amount of the crosslinking agent is preferably 0.5 parts by mass or more and 10.0 parts by mass or less, and more preferably 1.0 parts by mass or more and 5.0 parts by mass or less.

[0023] (1.6) Metal hydroxide (optional component) As the metal hydroxide, a known metal hydroxide can be used. The metal hydroxide improves the flame retardancy of the rubber foam 1. As the metal hydroxide, one or more types selected from the group consisting of aluminum hydroxide, magnesium hydroxide, and calcium aluminate can be used. The amount of the metal hydroxide is not particularly limited. When the total amount of EPDM and EVA is 100 parts by mass, the amount of the metal hydroxide is preferably 20 parts by mass or more, more preferably 30 parts by mass or more, and even more preferably 50 parts by mass or more, from the viewpoint of ensuring the adhesion of the rubber foam 1 to the pressure-sensitive adhesive layer 3. On the other hand, the amount of the metal hydroxide is preferably 100 parts by mass or less, more preferably 90 parts by mass or less, and even more preferably 80 parts by mass or less, from the viewpoint of increasing the dispersibility of the filler. From these viewpoints, the amount of the metal hydroxide is preferably 20 parts by mass or more and 100 parts by mass or less, more preferably 30 parts by mass or more and 90 parts by mass or less, and even more preferably 50 parts by mass or more and 80 parts by mass or less.

[0024] (1.7) Flame retardants (optional) The flame retardant is not particularly limited. The flame retardant may be used alone or in combination of two or more kinds. The flame retardant provides the rubber foam 1 with good flame retardancy. The flame retardant is preferably a non-halogen flame retardant. The composition preferably does not contain a halogen flame retardant. The non-halogen flame retardant is not particularly limited. Examples of the non-halogen flame retardant include nitrogen-based flame retardants and phosphorus-based flame retardants.

[0025] (1.7.1) Nitrogen-based flame retardants The nitrogen-based flame retardant is not particularly limited. Examples of the nitrogen-based flame retardant include melamine-based flame retardants, triazine compounds, and guanidine compounds. Examples of the melamine-based flame retardant include melamine, melamine melam melem, melamine cyanurate, melamine phosphate, melamine pyrophosphate, melamine polyphosphate, melamine melam melem polyphosphate, and melamine sulfate. As the nitrogen-based flame retardant, melamine cyanurate is preferred. Melamine compounds are particularly representative, and their flame retardant mechanism is believed to be due to the endothermic effect of the heat of sublimation and decomposition heat, which sublimates at 200°C or higher and dilutes the oxygen on the surface of combustible materials. Melamine cyanurate is an organic salt of melamine and cyanuric acid, and has a structure in which melamine and cyanuric acid are hydrogen-bonded. It is preferably used because it has a mica-like structure and a high nitrogen content. Melamine cyanurate also has the property of not impairing the processability of rubber compounds even when highly filled. The nitrogen-based flame retardants may be used alone or in combination of two or more kinds. The amount of the nitrogen-based flame retardant is not particularly limited. When the total of EPDM and EVA is 100 parts by mass, the nitrogen-based flame retardant is preferably 50 parts by mass or more, more preferably 60 parts by mass or more, and even more preferably 65 parts by mass or more from the viewpoint of ensuring high flame retardancy. On the other hand, the nitrogen-based flame retardant is preferably 150 parts by mass or less, more preferably 110 parts by mass or less, and even more preferably 90 parts by mass or less from the viewpoint of kneading processability and molding processability. In detail, since the nitrogen-based flame retardant does not have reinforcing properties for rubber like carbon black, adding a large amount of it reduces durability and strength, so 150 parts by mass or less is preferable. In addition, if the viscosity of the composition increases, the foaming property is controlled and low density cannot be ensured, so 150 parts by mass or less is preferable. From these viewpoints, the amount of the nitrogen-based flame retardant is preferably 50 parts by mass or more and 150 parts by mass or less, more preferably 60 parts by mass or more and 110 parts by mass or less, and even more preferably 65 parts by mass or more and 90 parts by mass or less.

[0026] (1.7.2) Phosphorus-based flame retardants The phosphorus-based flame retardant is not particularly limited. The phosphorus-based flame retardant is not particularly limited as long as it contains a phosphorus atom in the molecule. Examples of the phosphorus-based flame retardant include red phosphorus-based flame retardants (flame retardants containing red phosphorus) and organic phosphorus compounds. Known red phosphorus-based flame retardants can be used. Red phosphorus has attracted attention in recent years due to its flame retardancy, low smoke generation, and low toxic gas properties. Red phosphorus generally promotes carbonization of the matrix and forms a surface carbonized layer, thereby blocking oxygen and providing flame retardancy. Furthermore, a mechanism has been proposed in which phosphorus becomes polyphosphoric acid via methanoic acid, and in this process a protective coating is formed, blocking oxygen and providing flame retardancy. It is believed that the flame retardant effect of red phosphorus is expressed by the combination of carbonization promotion and coating effect. As red phosphorus, for example, Hishiguard CP (manufactured by Nippon Kagaku Co., Ltd.), which is surface-treated with aluminum hydroxide or the like to have an average particle size of about 15 μm, and 1140T (manufactured by Rinkagaku Kogyo Co., Ltd.) can be used. Taking into consideration the dispersibility in rubber, a master batch type (EVA, etc.) of red phosphorus can also be suitably used. Examples of the organic phosphorus compound include melamine polyphosphate, ammonium polyphosphate, phosphazene compounds, melamine pyrophosphate, phosphoric acid, melamine orthophosphate, melamine phosphate, piperazine orthophosphate, piperazine pyrophosphate, and piperazine polyphosphate. The phosphazene compound is preferably a cyclic phenoxyphosphazene represented by the following general formula. Examples of the organic phosphorus compound that can be used include ADK STAB EP-2500 and BUDIT667 (Budenheim), and the phosphazene that can be used is Rabitle FP-100 (Fushimi Pharmaceutical).

[0027] [ka] (wherein n represents an integer of 3 to 25.)

[0028] The amount of the phosphorus-based flame retardant is not particularly limited. When the total of EPDM and EVA is 100 parts by mass, the phosphorus-based flame retardant is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, from the viewpoint of ensuring higher flame retardancy in a vertical combustion test. On the other hand, the phosphorus-based flame retardant is preferably 20 parts by mass or less, more preferably 18 parts by mass or less, and even more preferably 17 parts by mass or less, from the viewpoint of suppressing an increase in the viscosity of the compound (kneaded product) and controlling the foaming property to obtain a low-density rubber foam 1. From these viewpoints, the amount of the phosphorus-based flame retardant is preferably 1 part by mass or more and 20 parts by mass or less, more preferably 3 parts by mass or more and 18 parts by mass or less, and even more preferably 5 parts by mass or more and 17 parts by mass or less. In addition, non-halogen flame retardants such as nitrogen-based flame retardants and phosphorus-based flame retardants have a high flame retardant effect, but they do not provide as high an effect as halogen-based flame retardants, so it is preferable to use a combination of multiple types.

[0029] The total amount of the metal hydroxide and the flame retardant is not particularly limited. When the total amount of the EPDM and the EVA is 100 parts by mass, the total amount of the metal hydroxide and the flame retardant is preferably 50 parts by mass or more and 180 parts by mass or less, more preferably 60 parts by mass or more and 100 parts by mass or less, and even more preferably 70 parts by mass or more and 90 parts by mass or less, from the viewpoint of ensuring higher flame retardancy in a vertical combustion test.

[0030] (1.8) Foaming agents The foaming agent is not particularly limited. Known foaming agents such as organic foaming agents and inorganic foaming agents can be used as the foaming agent. The foaming agent may be used alone or in combination of two or more kinds. As the foaming agent, for example, at least one of dinitropentadienetetramine (DPT), azodicarbonamide (ADCA), 4,4'-oxybisbenzenesulfonylhydrazide (OBSH), and sodium hydrogen carbonate can be used. The amount of the foaming agent is not particularly limited. When the total amount of EPDM and EVA is 100 parts by mass, the amount of the foaming agent is preferably 5 parts by mass or more, more preferably 8 parts by mass or more, and even more preferably 9 parts by mass or more, from the viewpoint of adjusting the amount of foaming gas to obtain a low-density rubber foam 1. On the other hand, the amount of the foaming agent is preferably 35 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 25 parts by mass or less, from the viewpoint of ensuring appearance (defects such as cracks and pinholes). From these viewpoints, the amount of the foaming agent is preferably 5 parts by mass or more and 35 parts by mass or less, more preferably 8 parts by mass or more and 30 parts by mass or less, and even more preferably 9 parts by mass or more and 25 parts by mass or less.

[0031] (1.9) Foaming assistant The foaming assistant is not particularly limited. As the foaming assistant, a urea-based foaming assistant is preferably used. The urea-based foaming assistant is a foaming assistant mainly composed of urea, and examples thereof include Cellpaste K-5 and Cellpaste 101 manufactured by Eiwa Kasei Kogyo Co., Ltd. The main component refers to a substance whose content (mass%) is 90 mass% or more (100 mass% or less). The mixing ratio of the urea-based foaming aid is preferably 1.0 parts by mass or more and 9.0 parts by mass or less, and more preferably 2.0 parts by mass or more and 8.0 parts by mass or less, per 100 parts by mass of the total of EPDM and EVA, from the viewpoint of adjusting the decomposition initiation temperature of the foaming agent during foam molding.

[0032] (1.10) Paraffinic processing oil The composition may contain a paraffinic processing oil. The paraffin-based process oil may be a commercially available product, such as Diana Process Oil "PS-430", "PS-32", "PS-90", "PW-32", "PW-90", "PW-150", or "PW-380" manufactured by Idemitsu Kosan Co., Ltd. The amount of the paraffin-based process oil is not particularly limited. The paraffin-based process oil can ensure the cohesiveness of the compound during kneading and can increase the dispersibility of the filler in the clayey compound. From the viewpoint of the kneading processability, the amount of the paraffin-based process oil is preferably 0 parts by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, when the total of EPDM and EVA is 100 parts by mass. On the other hand, from the viewpoint of suppressing adhesion inhibition due to oil bleeding and ensuring adhesion of the rubber foam 1 to the pressure-sensitive adhesive layer 3, the amount of the paraffin-based process oil is preferably 80 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 10 parts by mass or less. From these viewpoints, the amount of the paraffin-based process oil is preferably 0 parts by mass or more and 80 parts by mass or less, more preferably 3 parts by mass or more and 30 parts by mass or less, and even more preferably 5 parts by mass or more and 10 parts by mass or less. Since the rubber foam 1 containing paraffin-based process oil has poor flammability, the amount of paraffin-based process oil is preferably small.

[0033] (1.11) Other ingredients The composition may contain additives such as crosslinking accelerators (vulcanization accelerators), fillers, softeners, flame retardants, glass fibers, wood flour, fibers, dehydrating agents, antioxidants, antioxidants, various micro- and nano-capsules, pigments, colorants, anti-mold agents, reinforcing materials (various carbon blacks), and expandable graphite, in addition to the above-mentioned EPDM, EVA, fatty acid esters, crosslinking agents, crosslinking assistants, metal hydroxides, flame retardants, foaming agents, and foaming assistants. The additives may be used alone or in combination of two or more.

[0034] (1.11.1) Fillers The filler is not particularly limited, but examples thereof include inorganic fillers such as calcium carbonate (heavy calcium carbonate, etc.), magnesium carbonate, silicic acid and its salts, clay, talc, mica powder, bentonite, silica, alumina, aluminum silicate, acetylene black, furnace black, and aluminum powder, organic fillers such as cork, and other known fillers. These fillers may be used alone or in combination of two or more. Calcium carbonate, clay, and silica are preferably used. The blending ratio of the filler is not particularly limited, but is preferably 30 parts by mass or more and 200 parts by mass or less, and more preferably 50 parts by mass or more and 900 parts by mass or less, per 100 parts by mass of the total of EPDM and EVA.

[0035] (1.11.2) Softeners The softener is not particularly limited. In the present disclosure, for example, known softeners such as plasticizers, liquid paraffin, rosin, chroman resin, polybutene, asphalt, etc. can be used. These softeners may be used alone or in combination of two or more. Preferably, petroleum oils and asphalts are used. From the standpoint of ensuring flexibility, kneading processability, and adhesion of the pressure-sensitive adhesive, the blending ratio of the softener is, for example, preferably 0 parts by mass or more and 100 parts by mass or less, and more preferably 5 parts by mass or more and 30 parts by mass or less, per 100 parts by mass of the total of EPDM and EVA.

[0036] (2) Apparent density of rubber foam 1 The apparent density of the rubber foam 1 is set to 0.05 g / cm from the viewpoint of obtaining flexibility for ensuring airtightness, etc. 3 More than 0.3g / cm 3 Less than 0.06 g / cm is preferred. 3 More than 0.2g / cm 3 Less than 0.07 g / cm is more preferable. 3 More than 0.09g / cm 3 The following is even more preferred: The apparent density of the rubber foam 1 is measured by a measurement method in accordance with JIS K6767.

[0037] (3) Sulfur content of rubber foam 1 There are no particular limitations on the sulfur content of the rubber foam 1. From the viewpoint of suppressing contamination of electronic boards and the like, the sulfur content is preferably 1000 ppm or less, more preferably 500 ppm or less, and even more preferably 100 ppm or less. The sulfur content is measured according to JIS-6233. The test piece is placed in a flask filled with hydrogen peroxide and burned. Organic matter is oxidized and sulfur is converted to sulfuric acid. The solution is quantified by ion chromatography.

[0038] (4) Method for producing rubber foam 1 The method for producing the rubber foam 1 is not particularly limited. The rubber foam 1 is produced, for example, by the following production method. The rubber foam 1 can be produced by foaming and crosslinking a composition containing EPDM, EVA in the blend ratio described below, a crosslinking agent, a crosslinking aid having multiple double bonds, a foaming agent, and a foaming aid. The order in which the raw materials (EPDM, EVA, crosslinking agent, crosslinking aid, foaming agent, and foaming aid) are blended and the order in which they are kneaded are not particularly limited. A portion of each raw material may be kneaded in advance. Blend ratio (EPDM / EVA): 95 / 5~55 / 45 (mass ratio)

[0039] (5) Effects of the rubber foam 1 according to the present embodiment The rubber foam 1 of the present embodiment causes little contamination of electronic boards and the like. When the rubber foam 1 of this embodiment contains a specified flame retardant, even if it does not contain a halogen-based flame retardant, it can achieve V0 pass based on the V0 standard with a burning time of 50 seconds or less in a test conforming to the vertical flame test based on the UL94 standard. The rubber foam 1 of the present embodiment has a low density (0.05 g / cm 3 More than 0.3g / cm 3 It has closed cells and exhibits high adhesion to acrylic adhesives.

[0040] In addition to these effects, the rubber foam 1 of the present embodiment has an effect of having a good appearance on the surface. This effect will be described in detail. In the rubber foam 1 using EPDM and EVA, if an organic peroxide-based crosslinking agent is used instead of a sulfur crosslinking agent, the following problem occurs. That is, air is trapped near the surface of the rubber foam 1 immediately after molding. This causes a dome-shaped bulge (air bulge, for example, a circular dome of 5 mm to 20 mm) to occur on the surface of the rubber foam 1, which may cause the surface to look bad and reduce the commercial value. The inventors have studied the cause of this and speculated it as follows. The temperature of the rubber foam 1 immediately after molding is about 160°C, and it is gradually cooled naturally to room temperature level. It is considered that the rubber foam 1 is soft because of its high temperature immediately after molding, and the foaming gas is uniformly dispersed throughout the rubber foam 1. As the cooling progresses, the surface cools, so the inside is difficult to cool. The melting point of EVA is lower than that of EPDM. Therefore, even when the rubber foam 1 is cooled and the EPDM portion starts to solidify, there is a period in which the EVA portion remains soft. At this time, it is presumed that the foaming gas is forced into the soft EVA portion and gathers therein. Then, when the rubber foam 1 is cooled to room temperature, it is presumed that the entire rubber foam 1 is cooled and solidified, and a dome-shaped bulge remains on the surface of the rubber foam 1. In the rubber foam 1 of this embodiment, it is presumed that the crosslinking aid is dispersed in both the EPDM and the EVA, and the EPDM and the EVA are crosslinked with each other by the crosslinking agent. With this crosslinking, the EPDM portion and the EVA portion are solidified integrally at approximately the same time, and the foaming gas is prevented from being forced into the soft portion and gathering therein, and the dome-shaped bulge on the surface is suppressed. Therefore, the rubber foam 1 of this embodiment has a good surface appearance.

[0041] Here, a presumed mechanism by which the rubber foam 1 exhibits flame retardancy conforming to the 94V-0 standard defined in UL-94 when a metal hydroxide is blended therein will be described. In this case, EVA and a metal hydroxide are blended into the rubber foam 1. The metal hydroxide exhibits self-extinguishing properties due to a dehydrating action, and exhibits high flame retardancy. Furthermore, since EVA has a relatively high oxidation index among olefin resins, EVA also contributes to flame retardancy. Therefore, it is presumed that when EVA and a metal hydroxide are blended, the interaction between EVA and the metal hydroxide results in excellent flame retardancy. In addition, when a metal hydroxide and a fatty acid ester are blended into the rubber foam 1, the fatty acid ester acts to disperse the EVA and metal hydroxide well, thereby increasing the adhesion between the rubber foam 1 and the adhesive layer 3, and it is presumed that the EVA and metal hydroxide effectively contribute to flame retardancy. Furthermore, when a flame retardant is blended into the rubber foam 1, high flame retardancy is ensured even when the foam is highly foamed (reduced in density).

[0042] 2.Laminate 5 (1) Configuration of Laminate 5 The laminate 5 is formed by laminating a pressure-sensitive adhesive layer 3 onto a rubber foam 1 (see FIG. 1). There is no particular limitation on the configuration of the pressure-sensitive adhesive layer 3. The pressure-sensitive adhesive layer 3 preferably contains an acrylic polymer. An acrylic polymer is a polymer obtained by polymerizing (for example, solution polymerization, emulsion polymerization, or UV polymerization) an alkyl (meth)acrylate monomer using a polymerization initiator. In other words, an acrylic polymer is a compound (resin) having a structural unit derived from an alkyl (meth)acrylate. Here, "(meth)acrylic" means acrylic or methacrylic. The acrylic polymer may contain a monomer other than the (meth)acrylic acid alkyl ester. The acrylic polymer may have a crosslinked structure formed by a crosslinking agent.

[0043] The number of carbon atoms in the alkyl group in the (meth)acrylic acid alkyl ester is not particularly limited. The number of carbon atoms in the alkyl group is preferably an integer from 1 to 20. The alkyl group may be either linear or branched. Examples of (meth)acrylic acid alkyl esters include methyl (meth)acrylate, ethyl (meth)acrylate, normal butyl (meth)acrylate, isopropyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, normal octyl (meth)acrylate, isononyl (meth)acrylate, and lauryl (meth)acrylate, etc. The (meth)acrylic acid alkyl esters may be used alone or in combination of two or more.

[0044] In 100% by mass of the acrylic polymer, the constituent units derived from a (meth)acrylic acid alkyl ester having an alkyl group with 1 to 20 carbon atoms are preferably 50% by mass or more, and more preferably 70% by mass or more. The constituent units derived from a (meth)acrylic acid alkyl ester having an alkyl group with 1 to 20 carbon atoms may be 100% by mass.

[0045] The acrylic polymer may also contain structural units derived from other monomers than the (meth)acrylic acid alkyl ester. The other monomers are not limited. Known monomers may be used.

[0046] In the polymerization of the (meth)acrylic acid alkyl ester, an acrylic polymer can be easily formed by utilizing a polymerization reaction caused by heat or ultraviolet light using a polymerization initiator such as a thermal polymerization initiator or a photopolymerization initiator. The polymerization initiator can be used alone or in combination of two or more kinds. Examples of the thermal polymerization initiator include an azo-based polymerization initiator, a peroxide-based polymerization initiator, and a redox-based polymerization initiator. The amount of the polymerization initiator used is not particularly limited. The amount of the polymerization initiator used is appropriately adjusted, for example, as follows. That is, when the adhesive layer 3 is formed by applying the adhesive with a roll coater or the like, the amount used is adjusted before application so as not to cause polymerization.

[0047] The pressure-sensitive adhesive layer 3 can contain various known compounding agents (additives) such as compounds for improving adhesion to the rubber foam 1. Examples of compounding agents that can be used include metal particles, metal oxides, carbide particles, ceramic particles, calcium carbide, aluminum hydroxide, glass, silica, various resin beads, nylon resins, organic hollow bodies, inorganic hollow bodies, hollow glass balloons, etc. Examples of metal particles include particles of copper, nickel, aluminum, chromium, iron, stainless steel, and the like. Examples of the carbide particles include silicon carbide and nitrogen carbide. Ceramic particles include particles of nitrides, glasses, alumina, zirconium, etc., oxides, etc. The compounding agents may be contained alone or in combination of two or more.

[0048] The thickness of the rubber foam 1 in the laminate 5 is not particularly limited and can be changed appropriately depending on the application. The thickness of the rubber foam 1 is, for example, 0.1 mm or more and 2.0 mm or less. The thickness of the pressure-sensitive adhesive layer 3 is not particularly limited and can be appropriately changed depending on the application. The thickness of the pressure-sensitive adhesive layer 3 is preferably 0.2 mm or more and 1.0 mm or less, and more preferably 0.3 mm or more and 0.8 mm or less.

[0049] The peel strength of the laminate 5 to the adherend (SUS plate) is preferably 5 N / 25 mm width or more. The upper limit of the peel strength is not particularly limited, but is usually 50 N / 25 mm width or less. The peel strength is measured in accordance with the 90 degree peel strength test of the general test items of the Chubu Adhesive Processing Industry Association, as described later.

[0050] (2) Adhesion mechanism between rubber foam 1 containing fatty acid ester and metal oxide and adhesive layer 3 The adhesion mechanism between rubber foam 1 and pressure-sensitive adhesive layer 3 is not clear, but is presumed to be as follows: However, the present disclosure should not be construed as being limited in any way by this presumed mechanism. First, a case where the rubber foam 1 does not contain fatty acid ester (RCOOR') will be described. In this case, since EVA is prone to self-aggregation in the rubber foam 1, it is considered that the metal hydroxide is present so as to surround the EVA. Then, it is presumed that, among the metal hydroxides in a state where they are aggregated in the EVA, only the hydroxyl group of the metal hydroxide facing the pressure-sensitive adhesive layer 3 side forms a hydrogen bond with a polar group such as a carboxyl group of the resin contained in the pressure-sensitive adhesive layer 3, thereby adhering the rubber foam 1 and the pressure-sensitive adhesive layer 3. In this embodiment, only a small part of the metal hydroxide in the aggregated state is involved in adhesion. Also, in this embodiment, since the EVA is surrounded by the metal hydroxide, it is hardly involved in adhesion. Therefore, it is presumed that, when the rubber foam 1 does not contain fatty acid ester, the adhesion between the rubber foam 1 and the pressure-sensitive adhesive layer 3 is low, and the adhesive force is weak. Next, a case where the rubber foam 1 contains a fatty acid ester (RCOOR') will be described. In this case, the hydrophilic site (C=O) of the fatty acid ester forms a hydrogen bond with the hydroxyl group (-OH) of the metal hydroxide. On the other hand, the hydrophobic site (-R, -OR') of the fatty acid ester has a high affinity with the hydrophobic segment of EVA. Such a fatty acid ester having a hydrophilic site and a hydrophobic site is considered to act as a dispersant for the metal hydroxide. It is presumed that this action keeps the EVA in a dispersed state without self-aggregation. It is presumed that the metal hydroxide does not aggregate around the EVA in the rubber foam 1. In this way, since the metal hydroxide does not aggregate, it is presumed that more metal hydroxide molecules are involved in the adhesion between the rubber foam 1 and the pressure-sensitive adhesive layer 3 than in the case of aggregation. Also, in this embodiment, since the EVA is not surrounded by the metal hydroxide, the EVA itself also participates in the adhesion. Therefore, when the rubber foam 1 contains a fatty acid ester, it is presumed that the adhesion between the rubber foam 1 and the pressure-sensitive adhesive layer 3 is high and the adhesive force is strong. When the adhesive layer 3 is formed by pressure laminating an adhesive to the rubber foam 1 with a roll, the EVA itself is thought to contribute to adhesion as follows: Due to the action of the fatty acid ester, the EVA is dispersed almost uniformly in the rubber foam 1. An adhesive (such as an acrylic adhesive containing an acrylic polymer) is pressure-welded to this rubber foam 1 while applying heat (e.g., 70°C to 80°C) with a roll. Then, the EVA near the surface of the rubber foam 1 is thermally melted, and it is presumed that this EVA itself contributes to pressure adhesion.

[0051] (3) Method for manufacturing laminate 5 The method for producing the laminate 5 is not particularly limited. The laminate 5 is produced, for example, as follows. For example, an acrylic adhesive mixture (containing a thermal polymerization initiator and a filler) is coated on a release paper using a roll coater or the like, and then thermally cured in a hot air tank to form an adhesive layer 3. Thereafter, a rubber foam 1 is pressure-bonded onto the adhesive layer 3 using a roll, and the resulting mixture is allowed to cool, thereby producing a laminate 5. For coating, in addition to a roll coater, a coating roll such as a comma coater, a slot die, etc. can also be suitably used. In particular, when the pressure-sensitive adhesive layer 3 is formed on both sides (the front and back sides) of the rubber foam 1, or when the pressure-sensitive adhesive layer 3 has a multi-layer structure, the multi-layer slot die is suitably used. In addition, a release liner may be attached to the adhesive surface of the adhesive layer 3 as a liner. EXAMPLES

[0052] The present invention will be described more specifically below with reference to examples.

[0053] 1. Preparation of Rubber Foam Various rubber foams were produced according to the compounding ratios shown in Table 1-2. Details of the main raw materials in Table 1-2 are shown below. EPDM: Mitsui EPT4021 manufactured by Mitsui Chemicals, Inc. was used. EVA: Novatec LV440 (ethylene / ethyl acetate = 85 wt% (mass%) / 15 wt% (mass%), melting point 89°C) manufactured by Japan Polyethylene Co., Ltd. was used. Fatty acid esters: As the fatty acid ester, Rikemal SL-800 (stearyl stearate) manufactured by Riken Vitamin Co., Ltd. was used. Paraffin-based process oil (abbreviated as "paraffin-based oil" in the table): Diana Process PS-430 manufactured by Idemitsu Kosan Co., Ltd. was used. Crosslinking agent (1): Mitsubishi Chemical Corporation's Taik (triallyl isocyanurate (co-crosslinking sites: 3 places)) Crosslinking agent (2): Seiko Chemical Co., Ltd. Hi-Cross ED-P (ethylene glycol dimethacrylate (co-crosslinking sites: 2 locations)) Crosslinking agent: In Examples 1-10 and Comparative Examples 1, 2, and 4, a mixture of 1.5 parts by mass of Perhexa 25B-40 (2,5-dimethyl-2,5-di(tert-butylperoxy)hexane) and 2.5 parts by mass of Perhexa C-40MB (1,1-di(t-butylperoxy)cyclohexane), both manufactured by NOF Corp., was used. In Tables 1 and 2, the total amount of the crosslinking agent is shown. Foaming assistant: A urea-based foaming assistant (Cell Paste K-5, manufactured by Eiwa Chemical Industry Co., Ltd., 5 parts by mass) was used. Foaming agent: Azodicarbonamide (Vinifoll AC#3W, manufactured by Eiwa Chemical Industry Co., Ltd., 9 parts by mass) was used. ·Metal hydroxide: The aluminum hydroxide used was C-301N (manufactured by Sumika Alchem ​​Co., Ltd.). The magnesium hydroxide used was Kisuma 5A (Kyowa Chemical Industry Co., Ltd.). Carbon black: Although carbon black is not listed in Tables 1 and 2, Asahi Carbon #50G (20 parts by mass) manufactured by Asahi Carbon Co., Ltd. was used in all of Examples 1-10 and Comparative Examples 1-6. Nitrogen-based flame retardants: As the nitrogen-based flame retardant, melamine cyanurate MC-4500 (manufactured by Nissan Chemical Industries, Ltd.) was used. Phosphorus-based flame retardants: As the phosphorus-based flame retardant (1), a red phosphorus-based flame retardant (special surface treatment coated red phosphorus 1140T, manufactured by Rin Chemical Industry Co., Ltd.) was used. As the phosphorus-based flame retardant (2), Adeka STAB FP-2500 (melamine polyphosphate, manufactured by Adeka Corporation) was used.

[0054] Specifically, each rubber foam was produced as follows. <Example 1-10> EPDM, EVA, carbon black, paraffin-based process oil, flame retardant (nitrogen-based flame retardant, phosphorus-based flame retardant (1), or phosphorus-based flame retardant (2) as listed in Table 1), fatty acid ester, crosslinking aid, and metal hydroxide were all charged into a Banbury mixer at once, and the compound was discharged when the temperature reached 130°C. Next, a crosslinking agent, foaming aid, and foaming agent were added to the compound, which was then kneaded with a mixing roll and extruded into a sheet. The sheet was set in a mold at 130° C. and subjected to primary press molding for 15 minutes, and then secondary press molding was performed at 160° C. for 15 minutes to crosslink and foam the sheet, thereby obtaining a rubber foam.

[0055] <Comparative Example 1> A rubber foam was produced in the same manner as in Example 1-10, except that EVA was not used. <Comparative Example 2> Rubber foams were produced in the same manner as in Examples 1 to 10. In Comparative Example 2, the blend ratio of EPDM and EVA (EPDM / EVA) was 50 / 50, which is outside the range of rubber foams of the present disclosure. <Comparative Example 3> A rubber foam was produced in the same manner as in Examples 1 to 10, except that no crosslinking agent or crosslinking aid was used. In Comparative Example 3, crosslinking was performed with sulfur. <Comparative Example 4> A rubber foam was produced in the same manner as in Example 1-10, except that no crosslinking aid was used.

[0056] Each of the rubber foams of Examples 1-10 is considered to have a closed cell structure because the water absorption rate is low at 1 to 3%. Generally, rubber foams with a closed cell structure have high water stop performance but poor adhesion (adhesiveness) to a pressure-sensitive adhesive layer. On the other hand, rubber foams with an open cell structure (water absorption rate of 100 to 300%) generally have low water stop performance but high adhesion (adhesiveness) to a pressure-sensitive adhesive layer.

[0057] 2. Preparation of Laminates (Examples 1-10, Comparative Examples 1-3) The acrylic copolymer used was SK Dyne 1717DT, an ethyl acetate-containing adhesive manufactured by Soken Chemical Industries, Ltd. The crosslinking agent used was E-AX (manufactured by Soken Chemical Industries, Ltd.) The raw material composition for the adhesive layer was prepared by blending 0.05 parts by mass of a crosslinking agent with 100 parts by mass of this polymer, adding 10 parts by mass of an acrylic monomer (4-hydroxybutyrate; manufactured by Osaka Organic Chemical Industry Co., Ltd.: 4HBA) and 0.02 parts by mass of t-butylperoxy-2-ethylhexarate (manufactured by NOF Corp., Perbutyl O) as a thermal polymerization initiator. The raw material composition was coated on a release paper using a roll coater, and then heat cured in a hot air tank (90°C, 10 minutes) to form an adhesive layer. Then, a rubber foam was pressed onto the adhesive layer using a roll, and the adhesive layer was cooled to produce a laminate. The adhesive layer in the laminate had a thickness of 0.3 mm. In Comparative Example 4, the rubber foam could not be molded, and therefore a laminate could not be produced.

[0058] 3. Evaluation method (1) Apparent density The apparent density was measured in accordance with JIS-K 6767.

[0059] (2) 50% compression load The compression load of the rubber foam was measured in accordance with JIS-K 6767. The skin layer of the rubber foam was removed to prepare a test piece with a thickness of 10 mm. Then, using a compression tester, the test piece was compressed by 50% at a compression speed of 10 mm / min, and the compression load after 10 seconds was measured.

[0060] (3) Measurement of water absorption rate The water absorption rate of the rubber foam was measured in accordance with ASTM D 1056. The skin layer of the rubber foam was removed to prepare a test piece having a thickness of 12.5 mm and a size of 50 mm×50 mm. After measuring the weight of the test piece, the test piece was immersed 50 mm below the water surface, placed under a reduced pressure of 17 kPa for 3 minutes, and then immersed at atmospheric pressure for 3 minutes. After immersion, the water droplets on the surface were wiped off, the weight of the test piece after immersion was measured, and the water absorption rate was calculated using the following formula.

[0061]

number

[0062] (4) 90 degree peel strength test The 90-degree peel strength test was conducted in accordance with the 90-degree peel strength test, a general test item of the Chubu Adhesive Processing Industry Association. A test piece measuring 25 mm x 250 mm was cut from the rubber foam laminated with the adhesive, and a 25 mm x 125 mm portion of the adhesive surface was pressed onto a stainless steel plate. Then, using a tensile tester (Tensilon tensile tester), the test piece was peeled off from the stainless steel plate in a 90 degree direction at a peeling speed of 300 mm / min to measure the 90 degree peel strength. Measurements were taken with n=3, and the average value was read off the graph excluding abnormal values.

[0063] (5) UL94 vertical flame test Rubber foams of each thickness were tested according to the vertical burning test based on the UL94 standard. Burning times of 50 seconds or less were rated as V0 pass based on the V0 standard. Burning times of 250 seconds or less were rated as V1 pass based on the V1 standard.

[0064] (6) Sulfur content measurement test (total sulfur) The test was conducted in accordance with JIS-K6233:2016. The test piece was placed in a flask filled with hydrogen peroxide and burned. The organic matter was oxidized and sulfur was converted to sulfuric acid. The solution was quantified using ion chromatography.

[0065] [Table 1]

[0066] [Table 2]

[0067] 4.Results The results are shown in Table 1-2. In Table 1-2, the columns for the condition of the rubber foam (molded product) are A, B, C, and D as follows: <Condition of rubber foam (condition of molded body)> A: No air swelling in the rubber foam. No warping, pinholes or cracks in the rubber foam. Good. B: No air swelling in the rubber foam. Some warping and cracking in the rubber foam. No pinholes. C: The rubber foam is swollen due to air. The rubber foam has a fair amount of warping, cracks, and pinholes. D: Numerous air bubbles in the rubber foam. Many warps, cracks, and pinholes in the rubber foam. Many air bubbles.

[0068] In Table 1-2, the A, B, C, and D in the overall judgment column have the following meanings: A: The adhesive layer has good adhesion, and the rubber foam is in good condition. B: The adhesive layer has good adhesion, but the rubber foam has some warping and cracking. C: The adhesive layer has slightly poor adhesion, and the rubber foam has some warping and cracking. D: The adhesive layer has poor adhesion. The rubber foam has many warps, cracks, and pinholes.

[0069] (1) Fulfillment of each requirement in Examples 1-10 The compositions constituting the rubber foams of Examples 1 to 10 satisfy all of the following requirements (a) to (j). · Requirement (a): Contains EPDM. · Requirement (b): Contains EVA. Requirement (c): Contains a crosslinking agent. · Requirement (d): Contains a cross-linking aid having multiple double bonds. · Requirement (e): Contains a foaming agent. · Requirement (f): Contains a foaming assistant. Requirement (g): The blend ratio (EPDM / EVA) is 95 / 5 to 55 / 45 (mass ratio).

[0070] (2) Fulfillment of each requirement in Comparative Examples 1-4 In contrast, the rubber foam of Comparative Example 1-4 does not satisfy the following requirements. Comparative Example 1 does not satisfy the requirement (b). Comparative Example 2 does not satisfy the requirement (g). Comparative Example 3 does not satisfy the requirements (c) and (d). Comparative Example 4 does not satisfy the requirement (d).

[0071] (3) Results and Discussion The rubber foams of Examples 1 to 10 had short burning times and high flame retardancy in the vertical burning test based on the UL94 standard. It was confirmed that the rubber foams of Examples 1 to 10 had a low sulfur content and caused little contamination of electronic boards and the like. The rubber foams of Examples 1 to 10 were in good condition and were also evaluated as good overall. It was confirmed that the rubber foams of Examples 1-10 had good moldability and high adhesion. The rubber foams of Examples 1 to 10 have a low apparent density (0.05 g / cm 3 ~0.30g / cm 3 ) and has a closed cell structure (water absorption rate of 3% or less), which provides good water-stopping properties. Furthermore, the laminates produced from the rubber foams of Examples 1-10 had sufficient adhesion between the rubber foam and the pressure-sensitive adhesive layer, and were therefore suitable for practical use. In contrast, Comparative Example 1, which did not contain EVA, was inferior to the Examples in the state of the rubber foam, the 90-degree peel strength, and the results of the vertical flame test, and was also inferior to the Examples in the overall evaluation. In Comparative Example 2, in which the blend ratio of EPDM and EVA (EPDM / EVA) was 50 / 50 and which was outside the range of the rubber foam of the present disclosure, the state of the rubber foam and the results of the vertical combustion test were inferior to those of the Examples, and the overall evaluation was also inferior to that of the Examples. Comparative Example 3, which was crosslinked with sulfur, received an inferior overall rating to Examples. Also, it was confirmed that Comparative Example 3 had a high sulfur content and was highly likely to contaminate electronic boards and the like. Comparative Example 4, which did not contain a crosslinking aid having a plurality of double bonds, was unable to be molded and was also evaluated as poor in overall evaluation.

[0072] 5. Effects of the embodiment According to the above examples, it is possible to provide a rubber foam having high flame retardancy and causing little contamination of electronic boards, etc. Furthermore, according to the examples, it is possible to provide a rubber foam having little swelling due to air. Furthermore, according to the examples, it is possible to provide a laminate having high flame retardancy, low density, and high adhesion to an adherend.

[0073] The present disclosure is not limited to the above-described embodiments, and various modifications and variations are possible. [Explanation of symbols]

[0074] 1...Rubber foam 3...Adhesive layer 5...Laminate

Claims

1. A foamed product of a composition containing EPDM, EVA in the following blend ratio, a crosslinking agent, a crosslinking aid having a plurality of double bonds, a foaming agent, and a foaming aid, A rubber foam having a sulfur content of 1000 ppm or less. Blend ratio (EPDM / EVA): 95 / 5 to 55 / 45 (mass ratio)

2. At least a nitrogen-based flame retardant is included, The rubber foam according to claim 1 , wherein an amount of the nitrogen-based flame retardant is 50 parts by mass or more and 150 parts by mass or less, relative to 100 parts by mass of the total amount of the EPDM and the EVA.

3. Contains at least a phosphorus-based flame retardant, 3. The rubber foam according to claim 1, wherein an amount of the phosphorus-based flame retardant is 1 part by mass or more and 20 parts by mass or less, relative to 100 parts by mass of a total amount of the EPDM and the EVA.

4. A rubber foam described in any one of claims 1 to 3, which contains at least a fatty acid ester.

5. A laminate comprising the rubber foam according to claim 1 and a pressure-sensitive adhesive layer laminated thereon.

6. The laminate according to claim 5 , wherein the pressure-sensitive adhesive layer contains an acrylic polymer.

7. The laminate according to claim 5 or 6, which has a peel strength to an adherend of 5 N / 25 mm width or more.

8. A method for producing a rubber foam having a sulfur content of 1,000 ppm or less, comprising foaming and crosslinking a composition containing EPDM, EVA in the following blend ratio, a crosslinking agent, a crosslinking aid having a plurality of double bonds, a foaming agent, and a foaming aid. Blend ratio (EPDM / EVA): 95 / 5 to 55 / 45 (mass ratio)

Citation Information

Patent Citations

  • EVA microporous shoe sole plastic

    CN103483674A

  • Elastomer foam and production thereof

    JP1991074439A

  • foam

    JP1991095238A

  • Flame-retardant epdm foam

    JP2002293976A

  • Thermosensitive blowing material, method for producing the same and soundproof sheet for automobile

    JP2004143262A