Fiber-reinforced resin substrate, integrally molded product, and method for producing fiber-reinforced resin substrate
The fiber-reinforced resin base material addresses integration challenges by using resins with different properties and an anchoring structure, achieving strong bonding and improved design freedom in complex shapes.
Patent Information
- Application Number
- JP2020089419
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-05-23
- Filing Date
- 2020-05-22
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2040-05-22
AI Technical Summary
Existing fiber-reinforced composite materials using thermoplastic resins face challenges in integrating complex shapes and components due to limited design freedom, poor bonding strength, and thermal decomposition issues, particularly when combining resins with low compatibility.
A fiber-reinforced resin base material is developed with a configuration where thermoplastic resins having different properties are combined by ensuring a specific distance in Hansen solubility parameters and an anchoring structure provided by reinforcing fibers, allowing for strong integration and bonding across resin regions.
This approach enables the production of a composite material with strong bonding strength and improved design freedom, even with resins that are difficult to combine conventionally, reducing waste and manufacturing time.
Smart Images

Figure 0007577931000004 
Figure 0007577931000005 
Figure 0007577931000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a fiber-reinforced resin substrate in which reinforcing fibers are impregnated with at least two types of thermoplastic resins, an integrally molded product, and a method for producing a fiber-reinforced resin substrate. [Background technology]
[0002] Fiber-reinforced composite materials, which are combined with reinforcing fibers such as carbon fiber and glass fiber, are lightweight yet have excellent mechanical properties such as strength and rigidity, and are therefore applied to many fields such as aerospace, automobiles, railway vehicles, ships, civil engineering and construction, and sporting goods. In particular, the development of fiber-reinforced composite materials using thermoplastic resins as matrix resins is accelerating in terms of recyclability, moldability, impact resistance, and other factors. However, these fiber-reinforced composite materials are not suitable for manufacturing parts or structures with complex shapes in a single molding process, and in such applications, a process is required to prepare a member made of the fiber-reinforced composite material and then integrate it with another member. At this time, resins with different properties may be combined as necessary. As a method for integrating a fiber-reinforced composite material with another member, a joining method using mechanical joining such as bolts, rivets, and screws, and a joining method using adhesives are used. In the mechanical joining method, a process of pre-processing the joint parts, such as drilling holes, is required, which leads to a long manufacturing process and an increase in manufacturing costs, and there is also a problem that the strength of the material decreases due to the drilling of holes. In the bonding method using adhesives, the adhesive process, which includes preparing the adhesive and applying it, and the curing process are required, which leads to a long manufacturing process, and there are problems with the reliability of the adhesive strength, which is not satisfactory. Also, there are methods for obtaining molded products from different types of thermoplastic resins, such as two-color molding, but when combining resins with low compatibility, integration is mainly achieved by shape design such as fitting, which also limits the degree of design freedom.
[0003] Here, Patent Document 1 shows a prepreg sheet material in which a plurality of resin regions made of different thermoplastic resins are formed on a reinforcing fiber sheet layer aligned in a predetermined direction. Patent Document 2 shows a fiber-reinforced resin sheet in which a nonwoven fabric made of reinforcing fibers is impregnated with a plurality of different thermoplastic resins. Patent Document 3 shows a thermoplastic resin prepreg made of a thermoplastic resin having a melting point different from that of the material making up the reinforcing fibers.
[0004] Fiber-reinforced composite materials using thermoplastic resin as a matrix can be used to join components by welding, which may reduce the time required to join components. On the other hand, in recent years, the shapes required for products have become more complex, and it has become necessary to integrate various components according to the required characteristics. In the manufacture of such molded products, there is a demand for technologies to improve productivity and product yield, i.e., reduce waste rates.
[0005] Fiber-reinforced composite materials using thermoplastic resin as a matrix can be used to join components by welding, which may reduce the time required to join components. On the other hand, in recent years, the shapes required for products have become more complex, and it has become necessary to integrate various components according to the required characteristics. In the manufacture of such molded products, there is a demand for technologies to improve productivity and product yield, i.e., reduce waste rates. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2012-246442 A [Patent Document 2] International Publication No. 2014 / 103658 Brochure [Patent Document 3] International Publication No. 2013 / 8720 Brochure Summary of the Invention [Problem to be solved by the invention]
[0007] However, in the prepreg sheet material shown in Patent Document 1, the boundary between the resin regions is in a state where it penetrates into the reinforcing fiber sheet layer, but this state is not mentioned, and the bonding state of the different resins is not sufficient. In the fiber-reinforced resin sheet shown in Patent Document 2, the uneven shape of the interface layer formed by two types of thermoplastic resin is specified, and it is highly likely that the bonding strength is sufficient, but since a nonwoven fabric made of reinforcing fibers is used, the stability of the bonding strength (small variation) is not sufficient. The thermoplastic resin prepreg shown in Patent Document 3 is essentially a combination of thermoplastic resins of the same type (same type except for the molecular structure), and the purpose of obtaining a composite material made of a combination of resins with different required characteristics cannot be satisfied.
[0008] Furthermore, the composite material techniques described in these documents involve simultaneously melting different resins at a specific temperature and impregnating them into reinforcing fibers, which limits the combinations of resins that can be used, and in some cases, one of the resins may deteriorate due to thermal decomposition or the like, making it difficult to obtain a fiber-reinforced composite material in a healthy state.
[0009] Therefore, an object of the present invention is to provide a fiber-reinforced resin substrate in which a plurality of resins having different properties are firmly combined. [Means for solving the problem]
[0010] In order to solve such problems, the fiber-reinforced resin substrate of the present invention has the following configuration. That is, A fiber-reinforced resin substrate comprising the following components [A], [B] and [C]: [A] Reinforcement fiber; [B] Thermoplastic resin (b); [C] Thermoplastic resin (c); The components [A] are arranged in one direction. In the fiber-reinforced resin substrate, there are a resin region containing the component [B] and a resin region containing the component [C], A resin region containing the component [B] is present on one surface of the fiber-reinforced resin substrate, The distance Ra between the Hansen solubility parameters of component [B] and component [C] (bc) satisfies equation (1), Ra (bc) = {4(δDB-δDC) 2 +(δPB-δPC) 2 +(δHB-δHC) 2} 1 / 2 ≧8 Formula (1) Ra (bc) : The distance between the Hansen solubility parameters of component [B] and component [C]; δDB: Energy due to dispersion forces between molecules of component [B]; δDC: Energy due to dispersion forces between the molecules of the component [C]; δPB: Energy due to dipole-dipole interactions between molecules of component [B]; δPC: Energy due to dipole interactions between molecules of the component [C]; δHB: Energy due to hydrogen bonds between molecules of component [B]; δHC: Energy due to hydrogen bonds between molecules of the building blocks [C]; A fiber-reinforced resin substrate in which a component [A] contained in both resin regions is present across an interface between a resin region containing a component [B] and a resin region containing a component [C].
[0011] The present invention also includes an integrated molded product obtained by joining another member to the above-mentioned fiber-reinforced resin substrate.
[0012] Furthermore, the method for producing a fiber-reinforced resin substrate of the present invention has the following configuration. That is, A method for producing a fiber-reinforced resin substrate comprising the following components [A], [B] and [C]: [A] Reinforcement fiber; [B] Thermoplastic resin (b); [C] Thermoplastic resin (c); At least the following drawing step, first impregnation step, and second impregnation step are carried out continuously in this order while the component [A] is traveling, <Extraction step> A step of drawing the continuous constituent elements [A] together to obtain a continuous reinforcing fiber sheet in which the constituent elements [A] are arranged in one direction, and then supplying the obtained continuous reinforcing fiber sheet containing the constituent elements [A] in the fiber direction toward a subsequent step; <First impregnation step> a step of impregnating one surface of the continuous reinforcing fiber sheet with the component [B] to obtain a fiber reinforced resin intermediate having the component [B] present on the first surface of the continuous reinforcing fiber sheet; <Second impregnation step> a step of impregnating a second surface opposite to the first surface with the component [C] to obtain a fiber-reinforced resin substrate; The distance Ra between the Hansen solubility parameters of component [B] and component [C] (bc) A method for producing a fiber-reinforced resin substrate, wherein the formula (3) is satisfied: Ra (bc) = {4(δDB-δDC) 2 +(δPB-δPC) 2 +(δHB-δHC) 2} 1 / 2 ≧8 Formula (3) Ra (bc) : Distance between Hansen solubility parameters of component [B] and component [C] δDB: Energy due to dispersion forces between molecules of component [B]; δDC: Energy due to dispersion forces between the molecules of the component [C]; δPB: Energy due to dipole-dipole interactions between molecules of component [B]; δPC: Energy due to dipole interactions between molecules of the component [C]; δHB: Energy due to hydrogen bonds between molecules of component [B]; δHC: Energy due to hydrogen bonds between molecules of component [C]. Effect of the Invention
[0013] Since the fiber-reinforced resin substrate of the present invention is a composite of resins having different combinations of properties, particularly a plurality of thermoplastic resins having low compatibility with each other, it is possible to obtain a substrate having a combination of different properties that was difficult to obtain with the conventional technology. In addition, by using the fiber-reinforced resin substrate of the present invention, it is possible to provide an integrated molded product in which a plurality of members are firmly integrated, which was difficult to obtain with the conventional technology. Furthermore, by using the manufacturing method of the fiber-reinforced resin substrate of the present invention, it is possible to manufacture a fiber-reinforced resin substrate by compounding even a combination of resins that was difficult to compound with the conventional technology without causing deterioration such as thermal decomposition. [Brief description of the drawings]
[0014] [Figure 1] 1 is a schematic diagram of a fiber-reinforced resin substrate according to the present invention. [Diagram 2] FIG. 2 is a schematic diagram of an observed cross section of a fiber-reinforced resin substrate according to the present invention. [Diagram 3] FIG. 1 is a schematic diagram of a method for producing a fiber-reinforced resin substrate according to the present invention. [Figure 4] FIG. 2 is a schematic diagram of a continuous fiber-reinforced sheet in the production method of the present invention. [Diagram 5] FIG. 2 is a schematic diagram of a fiber-reinforced resin intermediate in the production method of the present invention. [Figure 6] 1 is a schematic diagram of a fiber-reinforced resin substrate according to the present invention. [Figure 7] FIG. 2 is a schematic diagram showing a method for producing a bonding strength test piece of a fiber-reinforced resin substrate according to the present invention. [Figure 8] 1 is a schematic diagram of an integrated molded product in which members made of different resins are joined together according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, the fiber reinforced resin substrate of the present invention will be described.
[0016] The fiber-reinforced resin substrate of the present invention contains at least the following components [A], [B] and [C].
[0017] (Component [A]) The reinforcing fibers of the component [A] used in the present invention include glass fibers, carbon fibers, metal fibers, aromatic polyamide fibers, polyaramid fibers, alumina fibers, silicon carbide fibers, boron fibers, and basalt fibers. These may be used alone or in combination of two or more. These reinforcing fibers may be surface-treated. Examples of surface treatments include metal deposition treatment, treatment with a coupling agent, treatment with a sizing agent, and deposition of additives. These reinforcing fibers also include conductive reinforcing fibers.
[0018] As the reinforcing fiber, carbon fiber having a low specific gravity, high strength, and high elastic modulus is preferably used. Commercially available carbon fiber products include "TORAYCA (registered trademark)" T800G-24K, "TORAYCA (registered trademark)" T800S-24K, "TORAYCA (registered trademark)" T700G-24K, "TORAYCA (registered trademark)" T700S-24K, "TORAYCA (registered trademark)" T300-3K, and "TORAYCA (registered trademark)" T1100G-24K (all manufactured by Toray Industries, Inc.).
[0019] In the component [A], the reinforcing fibers are arranged in one direction. The component [A] may be a laminate in which multiple layers of reinforcing fibers arranged in one direction are laminated. In this case, the reinforcing fibers in each layer may be arranged in one direction, and the reinforcing fibers in different layers may face in different directions. By using reinforcing fibers arranged in one direction, a molded product that is lightweight, highly durable, and has little deformation during the welding process can be obtained, which is preferable.
[0020] By forming the component [A] in such a form or arrangement, the cross-sectional curve formed by the boundary surface between the resin region containing the component [B] and the resin region containing the component [C] can be easily formed to satisfy the preferable structural requirements described later, and can be formed uniformly. This allows the reinforcing fibers to be present across the boundary surface between the resin region containing the component [B] and the resin region containing the component [C]. In addition, when the fiber-reinforced resin substrate is integrated with another member, it is also possible to reduce the variation in the bonding strength.
[0021] These forms can be obtained by arranging a plurality of reinforcing fiber bundles made of reinforcing fibers in one direction as described later. The reinforcing fiber bundle may be made of a plurality of fibers of the same form, or may be made of a plurality of fibers of different forms. The number of reinforcing fibers constituting one reinforcing fiber bundle is usually 300 to 60,000, but in consideration of the production of the base material, it is preferably 300 to 48,000, and more preferably 1,000 to 24,000. It may be a range that is a combination of any of the above upper limits and any of the above lower limits.
[0022] Regarding the reinforcing fiber of the component [A], it is preferable that the strand tensile strength measured in accordance with the resin-impregnated strand test method of JIS-R7608 (2004) is 5.5 GPa or more, since a fiber-reinforced resin substrate having excellent bonding strength in addition to tensile strength can be obtained.
[0023] The content of the component [A] in the fiber reinforced resin substrate of the present invention is preferably 30 to 90% by mass, more preferably 35 to 85% by mass, and further preferably 40 to 80% by mass. It may be a range that is a combination of any of the above upper limits and any of the above lower limits. When the mass content of the component [A] is 30% by mass or more, the reinforcing fiber of the component [A] exists in the form of a structure (anchoring structure) that exists across the boundary surface between the resin region containing the component [B] and the resin region containing the component [C], and it is possible to make the resin region containing the component [B] and the resin region containing the component [C] in a strong bonded state. In addition, when the content of the component [A] is 90% by mass or less, impregnation failure of the thermoplastic resin is unlikely to occur, and the voids in the obtained fiber reinforced resin substrate tend to be reduced.
[0024] [Impregnation rate] The impregnation rate of the fiber reinforced resin substrate of the present invention is preferably 80% or more. The impregnation rate is more preferably 85% or more, and even more preferably 90% or more. Here, the impregnation rate is the ratio of the resin selected from the components [B] and [C] impregnated into the component [A]. The higher the impregnation rate, the fewer the voids contained in the fiber reinforced resin substrate, and the fiber reinforced resin substrate with good appearance and high mechanical properties can be obtained. The impregnation rate can be measured not by the ratio of the resin impregnated into the fiber reinforced resin substrate, but by measuring and determining the ratio of the portion (called void portion) not impregnated with the resin. In observing a cross section perpendicular to the longitudinal direction of the obtained fiber reinforced resin substrate, the impregnation rate can be calculated by the following formula (4) when the total cross-sectional area of the fiber reinforced resin substrate is A0 and the cross-sectional area of the void portion in the fiber reinforced resin substrate is A1. Impregnation rate = (A0-A1) / A0 (4).
[0025] In the fiber-reinforced resin substrate of the present invention, the mass of the component [A] per unit area is 30 to 2,000 g / m 2 It is preferable that the mass of the component [A] per unit area is 30 g / m 2When the mass of the component [A] per unit area is 2,000 g / m or more, the number of laminated sheets required to obtain a predetermined thickness during molding of the fiber-reinforced resin laminate can be reduced, and the work is likely to be simplified. 2 When the mass of the component [A] per unit area is less than or equal to 300 g / m, the drapeability of the fiber-reinforced resin substrate is easily improved. 2 By setting the content within this range, the component [B] in the first impregnation step and the component [C] in the second impregnation step described below can be easily impregnated, and the production speed can be increased.
[0026] (Component [B], component [C]) The thermoplastic resin (b) constituting the component [B] and the thermoplastic resin (c) constituting the component [C] are those having a distance Ra of the Hansen solubility parameters described later. (bc)There are no particular limitations as long as the combination satisfies the relationship. Examples of the thermoplastic resin (b) and the thermoplastic resin (c) include polyester-based resins such as polyethylene terephthalate, polybutylene terephthalate, polytrimethylene terephthalate, polyethylene naphthalate, and liquid crystal polyester, polyolefins such as polyethylene, polypropylene, and polybutylene, styrene-based resins, and urethane resins, as well as polyamide-based resins such as polyoxymethylene, aliphatic polyamides such as polyamide 6 and polyamide 66, semi-aromatic polyamides, and alicyclic polyamides, polycarbonates, polymethyl methacrylates, polyvinyl chlorides, polyarylene sulfides such as polyphenylene sulfide, polyphenylene ethers, modified polyphenylene ethers, polyimides, polyamideimides, polyetherimides, polysulfones, modified polysulfones, polyethersulfones, polyarylene ether ketones such as polyketones, polyether ketones, polyether ether ketones, and polyether ketone ketones, polyarylates, polyether nitriles, phenolic resins, and phenoxy resins. These thermoplastic resins may be copolymers or modified products of the above-mentioned resins, and / or resins in which two or more types are blended, etc. From the viewpoints of good heat resistance and resistance to thermal deformation, crystalline thermoplastic resins having a glass transition temperature of 80° C. or higher and amorphous thermoplastic resins having a glass transition temperature of 160° C. or higher are preferred.
[0027] Among these, the thermoplastic resin (b) and the thermoplastic resin (c) are preferably at least one thermoplastic resin selected from the group consisting of polyolefins, polycarbonates, polyesters, polyarylene sulfides, polyamides, polyoxymethylene, polyetherimides, polyethersulfones, and polyarylene ether ketones, in terms of the balance between moldability, heat resistance, and mechanical properties.
[0028] Furthermore, the thermoplastic resin (b) and the thermoplastic resin (c) may contain other fillers and additives as appropriate depending on the application, etc., within the scope of not impairing the object of the present invention. Examples thereof include inorganic fillers, flame retardants, conductivity imparting agents, crystal nucleating agents, ultraviolet absorbers, antioxidants, vibration dampers, antibacterial agents, insect repellents, deodorants, coloring inhibitors, heat stabilizers, release agents, antistatic agents, plasticizers, lubricants, colorants, pigments, dyes, foaming agents, foam control agents, coupling agents, etc.
[0029] In the fiber reinforced resin substrate of the present invention, the weight per unit area of the component [B] and the component [C] is 10 g / m 2 It is preferable that the weight per unit area is 10 g / m or more. 2 If the thickness is more than this, a sufficiently thick welded joint area can be obtained in the weld-joining with another member described below, and excellent joint strength can be achieved. More preferably, the thickness is 20 g / m 2 That's all. Here, the basis weight is the weight of the fiber-reinforced resin substrate per 1 m 2 This refers to the mass (g) of component [B] or component [C] contained per unit.
[0030] The content of each of the components [B] and [C] in the fiber-reinforced resin substrate of the present invention is preferably 10 to 50% by mass, more preferably 20 to 40% by mass. The range may be a combination of any of the upper and lower limits. When the content of the components [B] and [C] is 10% by mass or more, impregnation of the components [B] and [C] is unlikely to occur insufficiently, and the voids in the obtained fiber-reinforced substrate tend to be small. In addition, the components [B] and [C] can be firmly compounded. In addition, when the content of the components [B] and [C] is 50% by mass or less, the component [A] is likely to form an anchoring structure in the thermoplastic resin of the components [B] and [C], and therefore it is possible to strongly compound the components.
[0031] Furthermore, in the fiber-reinforced resin substrate of the present invention, it is preferable that the relationship between the thermoplastic resin (b) and the thermoplastic resin (c) satisfies the following formula (2). 50≦ΔT≦200 ··· Formula (2) ΔT: Absolute value of the difference between Tb and Tc Tb: If the thermoplastic resin (b) is a crystalline resin, it is its melting point. If it is an amorphous resin, it is its glass transition temperature [℃]. Tc: If the thermoplastic resin (c) is a crystalline resin, it is its melting point; if it is an amorphous resin, it is its glass transition temperature [℃].
[0032] In this specification, the above Tb and Tc are collectively referred to as the melting temperature. When the fiber reinforced resin substrate of the present invention is joined to another member made of a thermoplastic resin, it is preferable to perform the joining by welding because the thermoplastic resins are mixed in a molten state, thereby improving the joining strength with the other member. In the fiber reinforced resin substrate of the present invention, when the thermoplastic resin (b) and the thermoplastic resin (c) are each welded to another member, it is preferable to increase the difference between the processing temperature (hereinafter abbreviated as "welding temperature") in the step of welding another member to the thermoplastic resin (b) and the welding temperature of the thermoplastic resin (c) because this improves the design freedom in the welding step. Here, as the welding temperature, if the thermoplastic resin is a crystalline resin, its melting point or higher is preferably used, and if the thermoplastic resin is an amorphous resin, its glass transition temperature or higher is preferably used. Therefore, if the difference ΔT between Tb and Tc is 50 ° C. or more, it is possible to sufficiently increase the difference in welding temperature on both sides, which is preferable. In addition, when the difference ΔT between Tb and Tc is 200 ° C or less, it is possible to suppress the thermal decomposition of one surface at the welding temperature of the other surface when welding each of the two surfaces, which is preferable. When welding both surfaces at a certain welding temperature, the difference ΔT between Tb and Tc is preferably 50 ° C or more and 150 ° C or less from the viewpoint of being able to apply a sufficient temperature for welding to the joint while suppressing the thermal decomposition of both surfaces. From the viewpoint of increasing the design freedom, the difference ΔT between Tb and Tc is preferably 100 ° C or more. According to the manufacturing method of the present invention described later, it is possible to obtain a fiber reinforced resin substrate having a strong bonded state even in the case of a combination of resins with such a large welding temperature difference.
[0033] The melting point and / or glass transition temperature here can be determined using a differential scanning calorimeter (DSC). 1 to 5 mg of a sample is placed in a 50 μl sealed sample container, and the temperature is increased at a rate of 10° C. / min. The step on the DSC curve detected in the range of 30 to 400° C. is taken as an index of the glass transition point, and the exothermic peak is taken as an index of the melting point. The respective temperatures are taken as the glass transition temperature and the melting point.
[0034] At least one of the melting temperature Tb of the component [B] and the melting temperature Tc of the component [C] is preferably 250° C. or lower. In the step of impregnating the reinforcing fiber with a thermoplastic resin or in the step of integrating it with another member, from the viewpoint of facilitating integration by thermal welding, it is more preferably 230° C. or lower, and even more preferably 210° C. or lower. The lower limit of the melting temperature is not particularly limited, but from the viewpoint of the heat resistance of the obtained fiber-reinforced resin substrate, it is preferably 100° C. or higher, and more preferably 130° C. or higher.
[0035] (Hansen solubility parameter) In the fiber-reinforced resin substrate of the present invention, in the relationship between the thermoplastic resin (b) constituting the component [B] and the thermoplastic resin (c) constituting the component [C], the distance Ra between the Hansen solubility parameters of the respective thermoplastic resins is (bc) It is essential that equation (1) is satisfied. Ra (bc) = {4(δDB-δDC) 2 +(δPB-δPC) 2 +(δHB-δHC) 2} 1 / 2 ≧8 ··· Formula (1) Ra (bc) : Distance between Hansen solubility parameters of component [B] and component [C] δDB: Energy due to dispersion forces between molecules of component [B] δDC: Energy due to dispersion forces between the molecules of the component [C] δPB: Energy due to dipole interactions between the molecules of the component [B] δPC: Energy due to dipole interactions between the molecules of the component [C] δHB: Energy due to hydrogen bonds between molecules of component [B] δHC: Energy due to hydrogen bonds between molecules of component [C].
[0036] Hansen solubility parameter distance Ra (bc) The values of each term that constitutes the formula can be calculated using Hansen Solubility Parameter in Practice (HSPiP) ver.5.0.06, but here, the solubility of the sample is calculated using various solvents with different solubilities, and the solubility information is analyzed by HSPiP to calculate the Hansen solubility parameter. In the formula, δD, δP, and δH represent the dispersion term, polarity term, and hydrogen bond term in the Hansen solubility parameter, respectively. Examples of the various solvents having different solubilities include n-hexane, cyclohexane, methyl isobutyl ketone, n-butyl acetate, toluene, tetrahydrofuran, methyl ethyl ketone, chloroform, methyl acetate, acetone, 1,4-dioxane, pyridine, N-methylpyrrolidone, hexafluoroisopropanol, 1-butanol, acetonitrile, diethylene glycol, N,N-dimethylformamide, γ-butyrolactone, ethanol, dimethyl sulfoxide, methanol, 2-aminoethanol, cyclohexanone, and 1,1,2,2-tetrabromoethane, and can be selected from these.
[0037] The distance Ra of the Hansen solubility parameters (bc) A value of 8 or more indicates that the affinity between component [B] and component [C] is very low. Therefore, in the conventional technology, it was not possible to obtain a strong bond between component [B] and component [C]. In the present invention, component [A] has the above-mentioned anchoring structure, which makes it possible to obtain combinations of thermoplastic resins that were previously impossible, in particular, combinations of thermoplastic resins that are different in the Hansen solubility parameters Ra of each thermoplastic resin. (bc) Even in the case of a combination in which the distance Ra is large, it is possible to easily obtain a strong bond at the interface between the components [B] and [C].(bc) From the viewpoint of increasing the degree of freedom in designing the combination of resins, the distance Ra is preferably 10 or more. (bc) There is no particular upper limit to the value, but as long as it is 30 or less, a high degree of freedom in designing the resin combination can be satisfied.
[0038] In the present invention, the resin region containing the thermoplastic resin (b) which is the component [B] is present on one surface of the fiber-reinforced resin substrate. The thermoplastic resin (b) may be present on a surface other than the surface. On the other hand, the resin region containing the thermoplastic resin (c) which is the component [C] is preferably present on the surface opposite to the surface on which the resin region containing the thermoplastic resin (b) is present.
[0039] The resin region containing the component [B] or the resin region containing the component [C] may be present over the entire surface of one surface of the reinforcing fiber resin substrate, or may be present over a portion of the surface.
[0040] It is also preferred that the resin region containing the component [B] and the resin region containing the component [C] are adjacent to each other in a layered form to form an interface, which is preferred because it increases the bonding strength between the resin region containing the component [B] and the resin region containing the component [C] and also increases the homogeneity of the fiber-reinforced resin substrate.
[0041] In the reinforced fiber resin substrate of the present invention, from the viewpoint of enhancing adhesion to the reinforcing fibers constituting the component [A], particularly to the carbon fibers, it is preferable that δHB of the component [B] and δHC of the component [C] are both 1.0 or more. It is more preferable that δHB and δHC are 2.0 or more.
[0042] In the reinforced fiber resin substrate of the present invention, the distance Ra between the Hansen solubility parameters of the component [A] and the component [B] (ab) , the distance Ra between the Hansen solubility parameters of component [A] and component [C] (ac)It is preferable that either or both of the above is less than 8. By making the above relationship, the component [B] and the component [C] have a Hansen solubility parameter distance Ra (bc) Even if the combination has a large value of Ra, it is possible to obtain a fiber-reinforced resin substrate having a strong bond via the component [A]. (ab) and Ra (ac) It is more preferable that either or both of these is less than 7, and even more preferable that either or both of these is less than 6.
[0043] (Fiber reinforced resin substrate) The thickness of the fiber reinforced resin substrate of the present invention is not particularly limited, but is preferably 0.1 mm or more, more preferably 0.3 mm or more, and even more preferably 0.5 m or more, from the viewpoint of ease of handling and lightness. By making the thickness 0.1 mm or more, when used as a joining medium for integrating with another member, the design freedom is high and it can also contribute to weight reduction. On the other hand, when the fiber reinforced resin substrate itself is used as a member, the thickness is preferably 1 mm or more, more preferably 3 mm or more, and even more preferably 5 mm or more. There is no particular limit to the upper limit of the thickness, but if the thickness is 50 mm or less, it can be fully utilized as both a joining medium and a member.
[0044] In addition, when the resin region containing the component [B] and the resin region containing the component [C] are adjacent to each other in a layered form, the thickness ratio of the resin region containing the component [B] to the resin region containing the component [C] is not particularly limited, but is preferably 1:9 to 9:1, more preferably 2:8 to 8:2, and even more preferably 3:7 to 7:3, from the viewpoint of mass productivity and flatness of the fiber reinforced resin substrate. The thickness ratio can also be adjusted so that the obtained fiber reinforced resin substrate is flat, depending on the linear expansion coefficient of the resin used and the volume content of the reinforcing fiber.
[0045] [Roughness average length, roughness average height] In the fiber-reinforced resin substrate of the present invention, the reinforcing fibers of the component [A] contained in both resin regions are present across the boundary between the resin region containing the component [B] and the resin region containing the component [C]. In addition, when the fiber-reinforced resin substrate is viewed in plan as shown in FIG. 1, in a direction of 45 degrees, regardless of whether it is clockwise or counterclockwise, with respect to the fiber direction of the component [A], a cross section perpendicular to the fiber-reinforced resin substrate, that is, a cross section obtained by cutting perpendicularly to the plane formed by the fiber-reinforced resin substrate, is observed. It is preferable that the roughness average length RSm defined by JIS B0601 (2001) of the cross-sectional curve formed by the boundary between the resin region containing the component [B] and the resin region containing the component [C] is 100 μm or less and the roughness average height Rc is 3.5 μm or more. It is preferable that the roughness average height Rc is 10 μm or more from the viewpoint of developing a stronger adhesive strength of the boundary surface.
[0046] As shown in FIG. 2, the reinforcing fibers of the component [A] contained in both resin regions straddling the boundary surface between the resin region containing the component [B] and the resin region containing the component [C] improve the strength of the resin region containing the component [C], thereby improving the bonding strength.
[0047] The presence of [A] across the boundary between the two resin regions can be confirmed by observing a cross section obtained by cutting perpendicularly to the plane direction. An example is shown in Figure 2. In the observed cross section 8 in Figure 2, the resin region 6 containing the component [B] of the fiber-reinforced resin substrate is in close contact with the resin region 7 containing the component [C], and the surface where the resin region 6 containing the component [B] and the resin region 7 containing the component [C] are in close contact is illustrated as the boundary 9. In addition, multiple components [A] 2 exist on the boundary 9. The component [A] 2 on the boundary 9 is in contact with both the resin region 6 containing the component [B] and the resin region 7 containing the component [C]. In this way, the state in which the components [B] and [C] are in contact with the periphery of the reinforcing fiber can be said to be a state in which the reinforcing fiber is "included in both resin regions across the boundary."
[0048] The component [A] present on the interface is chemically and / or physically bonded to the components [B] and [C], thereby improving the adhesion between the resin region containing the component [B] and the resin region containing the component [C]. The number of components [A] present on the interface may be one or more. The upper limit of the number is not particularly limited, but it is preferably 200 or less in a 500 μm square area in an image observed by the method described below.
[0049] The boundary surface between the resin region containing the component [B] and the resin region containing the component [C] is observed in a cross section perpendicular to the fiber reinforced resin substrate in a 45 degree direction, regardless of whether it is clockwise or counterclockwise, with respect to the fiber direction of the component [A] in a plan view of the fiber reinforced resin substrate. In this case, it is preferable to observe the part of the cross section where all of the components [A], [B], and [C] are present. By observing the state of the resin region at the boundary surface in such a cross section, the adhesion strength in the fiber direction and in a direction perpendicular thereto can be evaluated simultaneously.
[0050] In such cross-sectional observation, if the roughness average length RSm defined by JIS B0601 (2001) of the cross-sectional curve formed by the boundary surface is 100 μm or less, the component [A] is likely to be present across the boundary surface between the resin region containing the component [B] and the resin region containing the component [C], and the above-mentioned adhesion improvement effect is likely to be obtained. In addition to chemical and / or physical bonding forces, a mechanical bonding force of entanglement between the resin region containing the component [B] and the resin region containing the component [C] at the boundary surface is also added, making it difficult for the resin region containing the component [B] to peel off from the resin region containing the component [C]. The lower limit of the roughness average length RSm is not particularly limited, but is preferably 15 μm or more from the viewpoint of avoiding a decrease in mechanical bonding force due to stress concentration. In addition, by having the average roughness height Rc of the cross-sectional curve be 3.5 μm or more, the mechanical bonding strength due to intertwining is increased, and the component [A] is likely to be present across the boundary surface between the resin region containing the component [B] and the resin region containing the component [C], and the adhesive strength between the resin region containing the component [B] and the resin region containing the component [C] is improved, which is preferable. The average roughness height Rc of the cross-sectional curve is more preferably 10 μm or more, and particularly preferably 20 μm, because the component [A] is likely to be included in both resin regions and the adhesive strength is further improved. The upper limit is not particularly limited, but is preferably 100 μm or less from the viewpoint of avoiding a decrease in mechanical bonding strength due to stress concentration.
[0051] Here, the method for measuring the roughness average height Rc and the roughness average length RSm of the cross-sectional curve can be a known method. For example, a method for measuring from a cross-sectional image acquired using an X-ray CT, a method for measuring from an elemental analysis mapping image by an energy dispersive X-ray spectrometer (EDS), or a method for measuring from a cross-sectional observation image by an optical microscope, a scanning electron microscope (SEM), or a transmission electron microscope (TEM) can be mentioned. In the observation, the component [B] and / or the component [C] may be dyed to adjust the contrast. In the image obtained by any of the above methods, the roughness average height Rc and the roughness average length RSm of the cross-sectional curve are measured in a range of 500 μm square.
[0052] An example of a method for measuring the roughness average height Rc and roughness average length RSm of a cross-sectional curve is shown in Fig. 2. In the observed image 8 shown in Fig. 2, the resin region 6 containing the component [B] is in close contact with the resin region 7 containing the component [C], and in the observed image 8, the boundary surface between the resin region containing the component [B] and the resin region containing the component [C] is shown as boundary surface 9. In addition, a plurality of components [A] 2 are present on boundary surface 9.
[0053] An example of a method for measuring the roughness average height Rc and roughness average length RSm of a cross-sectional curve (cross-sectional curve element measurement method 1) is shown. Using an end 10 on the resin region side including the component [C] of a rectangular observation image 8 as a reference line, vertical base lines 11 are drawn at 5 μm intervals from the resin region 7 including the component [C] toward the resin region 6 including the component [B]. The point where the vertical base line drawn from the reference line first intersects with the component [B] is plotted, and the line connecting the plotted points is taken as the cross-sectional curve 12. The obtained cross-sectional curve 12 is subjected to a filtering process based on JIS B0601 (2001), and the roughness average height Rc and roughness average length RSm of the cross-sectional curve 12 are calculated.
[0054] (Integrated molded product) The fiber-reinforced resin substrate of the present invention can be formed into an integrated molded article by bonding to another member via the component [B] and / or the component [C].
[0055] Here, the other member may be, for example, a metal material such as aluminum, iron, magnesium, titanium, or an alloy thereof, or the fiber-reinforced resin substrate may be the same as the fiber-reinforced resin substrate, or may be a thermoplastic resin composition. When a thermoplastic resin composition reinforced with reinforcing fibers is used as the other member, it is preferable because it can provide a light weight that cannot be achieved when a metal material is used.
[0056] Here, the other member preferably contains a thermoplastic resin from the viewpoint of weldability with the constituent element [B] and / or the constituent element [C]. The thermoplastic resin contained in the other member and the thermoplastic resin contained in the part of the fiber reinforced resin substrate that is bonded (contacted) with the other member are preferably the same type of resin. Furthermore, the other member may contain other fillers and additives as appropriate depending on the application, etc., within a range that does not impair the object of the present invention. For example, inorganic fillers, flame retardants, conductive agents, crystal nucleating agents, ultraviolet absorbers, antioxidants, vibration dampers, antibacterial agents, insect repellents, deodorizers, coloring inhibitors, heat stabilizers, release agents, antistatic agents, plasticizers, lubricants, colorants, pigments, dyes, foaming agents, foam control agents, coupling agents, etc. may be mentioned.
[0057] Examples of the form of the other member include a rib, a boss, a standing wall, etc., and in particular, it is preferable to join a rib structure to the fiber-reinforced resin substrate from the viewpoint of achieving both light weight and mechanical properties of the molded product. Examples of such a rib structure include an example in which the rib structure is arranged linearly on the fiber-reinforced resin substrate, and an example in which the rib structure is arranged as a cross rib.
[0058] The method for joining another member to the fiber-reinforced resin substrate of the present invention is not particularly limited, and examples thereof include heat welding, vibration welding, ultrasonic welding, resistance welding, induction welding, laser welding, insert injection molding, outsert injection molding, etc. In particular, it is preferable to use injection molding such as insert injection molding and outsert injection molding because it is high-speed and has excellent productivity.
[0059] The strength of the joint of the integrally molded product of the present invention is preferably 10 MPa or more, more preferably 15 MPa or more, in terms of tensile bond strength measured based on the bond strength between a fiber-reinforced resin substrate and another member described later, when the test environment temperature is 23° C. In applications requiring mechanical properties at high temperatures, it is preferable that the joint exhibits high bond strength even when the test environment temperature is, for example, 80° C.
[0060] (Method of manufacturing fiber reinforced resin substrate) In the method for producing a fiber-reinforced resin substrate according to the present invention, a drawing step, a first impregnation step, and a second impregnation step, which will be described later, are carried out continuously in this order while the constituent element [A] is traveling.
[0061] Here, "continuously carried out while the component [A] is traveling" means that the component [A] is continuously subjected to each process without stopping using a roll or a belt as shown in Figure 3. By carrying out each process continuously and in order, the manufacturing cost of the substrate can be reduced.
[0062] <Drawing process> The drawing process according to the present invention is a process of aligning continuous constituent elements [A] to obtain a continuous reinforcing fiber sheet in which reinforcing fibers are arranged in one direction, and then supplying the obtained continuous reinforcing fiber sheet including the constituent elements [A] in the fiber direction toward a subsequent process. For example, it is a process of unwinding and aligning yarns from bobbins of the constituent elements [A] arranged on a creel or the like to obtain a sheet-like continuous reinforcing fiber sheet and leading it to the next process. A fiber-spreading process may be included before or / and after aligning the constituent elements [A]. In addition, after aligning, a woven fabric may be woven using auxiliary fiber yarns as weft yarns through a loom and led as a continuous reinforcing fiber sheet. The auxiliary fibers at this time may be the same fiber as the constituent elements [A] or different fibers. By directly obtaining a continuous reinforcing fiber sheet from the yarns, the manufacturing cost can be reduced compared to the case of going through warping or partial warping (beaming), which is preferable. By aligning the constituent elements [A] included in the continuous reinforcing fiber sheet in one direction, a low-cost fiber-reinforced resin substrate having excellent specific strength in the fiber direction can be obtained.
[0063] The continuous reinforcing fiber sheet obtained in the drawing step of the present invention will be described with reference to Fig. 4. The continuous fiber reinforced sheet 13 shown in Fig. 4 includes a component [A] 2, and its cross section is shown in cross section A. The continuous fiber reinforced sheet has two opposing surfaces, a first surface 19 and a second surface 20, and in the first impregnation step and the second impregnation step described below, the components [B] and [C] are impregnated from these surfaces, respectively. However, the scope of the present invention is not limited to the steps exemplified in Fig. 4.
[0064] The yarn of the component [A] may be composed of a plurality of fibers of the same form, or may be composed of a plurality of fibers of different forms. The number of reinforcing fibers constituting one yarn of the component [A] is usually 300 to 60,000, but in consideration of the production of the base material, it is preferably 300 to 48,000, and more preferably 1,000 to 24,000. It may be within a range that is a combination of any of the above upper limits and any of the above lower limits.
[0065] <First impregnation step> The manufacturing method according to the present invention includes, after the drawing step, a step of impregnating one surface of the continuous reinforcing fiber sheet with the component [B] to obtain a fiber-reinforced resin intermediate having the component [B] on the first surface. The fiber-reinforced resin intermediate obtained in the first impregnation step will be described with reference to Figs. 4 and 5. The component [B] 6 is impregnated into the continuous reinforcing fiber sheet 13 from the first surface 19 in cross section A in Fig. 4, and a fiber-reinforced resin intermediate 14 having a cross section as shown in cross section B in Fig. 5 is obtained. Here, the first surface 19 of the fiber-reinforced resin intermediate 14 is covered with the component [B] 6. However, the scope of the present invention is not limited to the steps exemplified in Figs. 4 and 5.
[0066] In the first impregnation step, the state in which the component [B] is present on the first surface is not particularly limited, but it is preferable that the component [B] is disposed on the first surface. Here, the component [B] is disposed means that 80% or more of the first surface is covered. By covering 80% or more of the surface with the component [B], it is possible to impart bonding properties to the obtained fiber reinforced resin substrate. Furthermore, a step of obtaining a fiber reinforced resin intermediate whose first surface is completely covered with the component [B] is more preferable. By adopting such a step, it is possible to prevent the component [C] from being exposed to and / or wrapping around the first surface when the component [C] is impregnated in the second impregnation step described later, which is preferable.
[0067] <Impregnation> There is no particular limitation on the method of impregnating one side of the continuous reinforcing fiber sheet with the component [B] to obtain a fiber-reinforced resin intermediate. Examples of the method include a method of laminating the component [B] in a sheet form such as a film or nonwoven fabric on the first surface of the continuous fiber-reinforced sheet, heating the component [B] to a molten state, impregnating the continuous fiber-reinforced sheet, and cooling to obtain a fiber-reinforced resin intermediate, and a method of attaching the component [B] in a molten state to the first surface of the continuous fiber-reinforced sheet, impregnating the continuous fiber-reinforced sheet, and cooling to obtain a fiber-reinforced resin intermediate. The method of laminating the component [B] in a sheet form is preferable because the basis weight of the component [B] can be stabilized. The method of applying the component [B] in a molten state to the continuous fiber-reinforced sheet is preferable in terms of production costs.
[0068] As a method for heating the sheet-shaped component [B] after laminating it on the first surface, a known method can be used. For example, a non-contact heating method using a far-infrared heater, a high-temperature oven, or induction heating, or a method for heating by contacting with a heated roll or belt can be mentioned. Among them, a method of heating through a far-infrared heater or a high-temperature oven is preferable from the viewpoint of temperature control.
[0069] There is no particular limitation on the method for attaching the molten component [B] to the first surface, and any known method can be used. Among these, dipping or coating is preferable.
[0070] Here, the dipping refers to a method of, for example, supplying the component [B] to a molten bath using a pump and passing the continuous fiber reinforced sheet through the molten bath. By immersing the continuous fiber reinforced sheet in the molten bath, the component [B] can be reliably attached to the continuous fiber reinforced sheet.
[0071] Moreover, coating refers to a method of applying the component [B] to a continuous fiber reinforced sheet using a coating means such as a reverse roll, a forward rotating roll, a kiss roll, an applicator, a spray, or a curtain. Here, the reverse roll, the forward rotating roll, and the kiss roll refer to a method of supplying the molten component [B] to a roll by a pump and applying the molten component [B] to the continuous fiber reinforced sheet. The reverse roll is a method in which two rolls rotate in opposite directions to each other and apply the molten component [B] onto the roll, and the forward rotating roll is a method in which two rolls rotate in the same direction and apply the molten component [B] onto the roll. Usually, in the reverse roll and the forward rotating roll, a method is used in which the continuous fiber reinforced sheet is sandwiched between two rolls to transfer the component [B] onto the continuous fiber reinforced sheet, and then sandwiched with another roll to ensure that the component [B] is attached. On the other hand, the kiss roll is a method in which the component [B] is attached by only contacting the continuous fiber reinforced sheet with one roll. Therefore, the kiss roll is preferably used when the viscosity of the resin is relatively low. Whichever roll method is used, a predetermined amount of the component [B] that has been heated and melted is applied, and the continuous fiber reinforced sheet is run while being adhered to the component [B], so that a predetermined amount of the component [B] can be attached per unit length of the continuous fiber reinforced sheet. The spray method utilizes the principle of a sprayer, and is a method of spraying the molten component [B] in a mist form onto the continuous fiber reinforced sheet. The curtain method is a method of allowing the molten component [B] to fall naturally from a small hole and apply it to the continuous fiber reinforced sheet, or a method of allowing it to overflow from a melting tank and apply it to the continuous fiber reinforced sheet. Since the amount required for application is easy to adjust, the loss of the component [B] can be reduced. The applicator method is a method of ejecting the molten component [B] from a small hole and running the continuous fiber reinforced sheet while being in contact with the component [B], so that a predetermined amount of the component [B] can be attached per unit length of the continuous fiber reinforced sheet. The applicator is preferably used from the viewpoint of being less susceptible to the effect of the viscosity of the component [B] and being able to increase the production speed.
[0072] Pressurization may be applied when the molten component [B] is impregnated into the continuous fiber-reinforced sheet. There is no particular limitation on the pressurization method, but when the component [B] is heated by a reverse roll, a forward rotating roll, a kiss roll, an applicator, or a belt, a method of applying pressure simultaneously with heating can be mentioned. Alternatively, a method of providing a pressurizing section consisting of a roll or a belt after the component [B] is attached and melted to the continuous fiber-reinforced sheet can be mentioned. Note that when the viscosity of the molten component [B] is low, pressurization is not necessarily required.
[0073] The fiber-reinforced resin intermediate obtained by impregnating the continuous fiber-reinforced sheet with the component [B] is preferably cooled. There is no particular limitation on the cooling method, and a known method can be used. For example, non-contact cooling using a temperature-controlled tank or a blower, or contact cooling by contacting with a temperature-controlled roll or belt can be used. Among them, the method of contacting with a temperature-controlled roll or belt is preferable from the viewpoint of temperature control, and is also preferable because it can serve as a pressurizing step after melting the component [B].
[0074] <Temperature of fiber-reinforced resin intermediate> The temperature of the fiber-reinforced resin intermediate after the first impregnation step and before the second impregnation step is preferably 70 to 180°C. By setting the temperature in this range, the component [C] is unlikely to undergo thermal decomposition or runaway reaction due to the heat of the fiber-reinforced resin intermediate in the second impregnation step described below, and the component [C] is moderately heated, improving the impregnation property of the fiber-reinforced resin intermediate. From the viewpoint of reliably preventing thermal decomposition or runaway reaction, the temperature of the fiber-reinforced resin intermediate is more preferably 150°C or less. Moreover, from the viewpoint of improving the impregnation property, the lower limit is more preferably 90°C or more.
[0075] <Second impregnation step> The manufacturing method according to the present invention includes a step of impregnating the second surface opposite to the first surface with the component [C] after starting the first impregnation step to obtain a fiber-reinforced resin substrate (second impregnation step). The fiber-reinforced resin substrate obtained in the second impregnation step will be described with reference to Figs. 5 and 6. The component [C] 7 is impregnated into the continuous reinforcing fiber sheet 13 from the second surface 20 in the cross section B of Fig. 5, and a fiber-reinforced resin substrate 1 having a cross section like the cross section C of Fig. 6 is obtained. Here, the first surface 19 of the fiber-reinforced resin substrate 1 is covered with the component [B] 6, and the second surface 20 is covered with the component [C]. However, the scope of the present invention is not limited to the steps exemplified in Figs. 5 and 6. The second impregnation step may be started before the completion of the first impregnation step.
[0076] [Impregnation] The method of impregnating the component [C] from the second surface opposite to the first surface of the fiber-reinforced resin intermediate is not particularly limited, but examples thereof include a method of laminating the component [C] in a sheet shape on the second surface of the fiber-reinforced resin intermediate, then heating it to a molten state, and then cooling it to obtain a fiber-reinforced resin intermediate, and a method of applying the component [C] in a molten state to the second surface of the fiber-reinforced resin intermediate, then cooling it to obtain the fiber-reinforced resin intermediate. The method of laminating the component [C] in a sheet shape of a film or nonwoven fabric is preferred because the basis weight of the component [C] can be stabilized. The method of applying the component [C] in a molten state to the fiber-reinforced resin intermediate is preferred in terms of production costs.
[0077] <Pick-up process> After the second impregnation step, a step of taking up the fiber-reinforced resin substrate may be included. In the taking up step, the fiber-reinforced substrate may be taken up on a take-up section, or may be introduced into an apparatus such as an ATP apparatus, an AFP apparatus, a slitting apparatus, or a cutting apparatus without being taken up, and continuously provided to another process. When taking up, a release paper or a protective film may be supplied to the second surface of the fiber-reinforced resin substrate. By supplying a release paper or a protective film, it is possible to prevent the second surface of the fiber-reinforced resin substrate from adhering or sticking to the first surface of the fiber-reinforced resin substrate in the inner layer during taking up, which is preferable.
[0078] The speed of the fiber reinforced resin substrate during withdrawal is preferably 0.1 m / min or more. By setting it in this range, a fiber reinforced resin substrate can be obtained continuously. From the viewpoint of productivity, it is more preferably 1 m / min or more, and from the viewpoint of process requirements of structural members, it is more preferably 5 m / min or more.
[0079] In the manufacturing method of the fiber-reinforced resin substrate of the present invention, it is possible to separately impregnate the component [A] with the component [B] and the component [A] with the component [C]. When different types of thermoplastic resins are impregnated into the reinforcing fibers, a method is exemplified in which a temperature at which both different resins can be molded is selected and the different types of resins are simultaneously impregnated at that molding temperature (Patent Documents 1 and 2). When simultaneously impregnating, since the molding pressure cannot be adjusted according to the resin, it is very difficult to control the boundary position of both resins, and the combination of resins is limited, which is not preferable. The manufacturing method of the present invention is preferable in that the resin viscosity and molding pressure can be arbitrarily set by changing the molding temperature in the first impregnation step and the second impregnation step, there is a large degree of freedom in designing the manufacturing conditions, and the boundary position between the component [B] and the component [C] can be easily adjusted. (Application) The fiber-reinforced resin substrate and integrally molded product of the present invention are preferably used for aircraft structural members, wind turbine blades, automobile exterior panels, computer applications such as IC trays and notebook computer housings, and sports applications such as golf shafts and tennis rackets. EXAMPLES
[0080] The present invention will be described in detail below with reference to examples. However, the scope of the present invention is not limited to these examples. The unit "parts" in the composition ratio means parts by mass unless otherwise noted. Furthermore, the measurements of various properties were performed under an environment of a temperature of 23°C and a relative humidity of 50% unless otherwise noted.
[0081] (1) Productivity The quantity that can be produced per unit time was judged comprehensively based on factors such as the take-up speed during manufacturing, the number of breaks of component [A], and the number of processes, and a relative evaluation was made on a four-level scale: A (particularly good), B (good), C (average), and D (poor).
[0082] (2) Roughness mean length RSm and roughness mean height Rc Measurement was performed using the fiber reinforced resin substrate prepared above. The fiber reinforced resin substrate was cut perpendicular to the planar direction at an angle of 45 degrees in the plan view of the fiber reinforced resin substrate with respect to the fiber direction of any reinforcing fiber selected from the constituent element [A] contained in the fiber reinforced resin substrate to obtain a cross section. An image of the cross section was taken at a magnification of 1000 times using an optical microscope. In an arbitrary observation range of 500 μm square in the obtained image, the roughness average length RSm and roughness average height Rc of the cross section curve element obtained by the measurement method 2 of the cross section curve element, as defined in JIS B0601 (2001), were measured.
[0083] (3) Bonding strength of fiber-reinforced resin substrate (bonding strength between component [B] and component [C]) As shown in FIG. 7, metal members were attached to both surfaces of the fiber-reinforced resin substrate using an adhesive to prepare a superimposed test piece (Type B) as described in ISO19095. The resulting test piece was evaluated for its bonding strength in accordance with the ISO19095 (2015) standard using an "Instron" (registered trademark) 5565 universal material testing machine (manufactured by Instron Japan Co., Ltd.) and a test piece holder. The bonding strength was evaluated as follows. 15MPa or more:A 10MPa or more and less than 15MPa: B 5MPa or more but less than 10MPa: C Less than 5MPa:D.
[0084] (4) Impregnation rate In the fiber-reinforced resin substrate, a cross-sectional image perpendicular to the fiber direction of the component [A] was taken at 500 times magnification using an optical microscope, and the impregnation rate was measured based on the above formula (4).
[0085] (5) Appearance The fiber-reinforced resin substrate was visually inspected for any irregularities in the reinforcing fibers, and was rated on a three-point scale: A (good) if the reinforcing fibers were almost parallel to the flow direction from the drawing process to the take-up process, B (small fiber irregularities) if the fibers were slightly irregular, such as curved, and C (large fiber irregularities) if the fibers were significantly irregular, such as wavy and meandering.
[0086] (6) Materials and equipment used [Carbon fiber (1)] A copolymer mainly composed of polyacrylonitrile was spun, baked, and surface-oxidized to obtain continuous carbon fibers with a total of 12,000 single fibers. The properties of this continuous carbon fiber are as follows: Single fiber diameter: 7μm Density: 1.8g / cm 3 Tensile strength: 4600MPa Tensile modulus: 220GPa.
[0087] [Glass fiber (1)] The continuous E-glass fiber used had a total of 1,600 continuous single fibers that had been subjected to bundling treatment. The properties of this continuous E-glass fiber were as follows: Single fiber diameter: 13μm Tensile strength: 3400MPa Tensile modulus: 72GPa Tensile elongation: 3% Density: 2.6g / cm 3 .
[0088] [Reinforced fiber mat (1)] Carbon fiber (1) was cut to 5 mm with a cartridge cutter to obtain chopped carbon fiber. A dispersion liquid with a concentration of 0.1% by mass consisting of water and a surfactant (Polyoxyethylene lauryl ether (trade name) manufactured by Nacalai Tesques Co., Ltd.) was prepared, and a reinforced fiber mat (1) was manufactured from this dispersion liquid and chopped carbon fiber using a manufacturing device for a reinforced fiber mat. The manufacturing device is equipped with a cylindrical container with a diameter of 1000 mm having an opening cock at the bottom of the container as a dispersion tank, and a linear transport part (inclined angle 30 °) connecting the dispersion tank and the papermaking tank. A stirrer is attached to the opening on the top surface of the dispersion tank, and chopped carbon fiber and dispersion liquid (dispersion medium) can be put in from the opening. The papermaking tank is a tank equipped with a mesh conveyor having a papermaking surface with a width of 500 mm at the bottom, and a conveyor capable of transporting a carbon fiber substrate (papermaking substrate) is connected to the mesh conveyor. Papermaking was performed with a carbon fiber concentration in the dispersion liquid of 0.05% by mass. The carbon fiber substrate was dried in a drying oven at 200°C for 30 minutes to obtain a reinforcing fiber mat (1). The weight of the obtained mat was 100 g / m 2 It was.
[0089] [PA6 resin, PA6 resin film] As the PA6 resin, "Amilan (registered trademark)" CM1001 (manufactured by Toray Industries, Inc.) was used. In addition, using PA6 resin, 2 A film (melting point 225°C) was prepared.
[0090] [PP resin, PP resin film] A resin consisting of 80% by mass of unmodified polypropylene resin (Prime Polypro (registered trademark) J105G manufactured by Prime Polymer Co., Ltd.) and 20% by mass of acid-modified polypropylene resin (Admer QB510 manufactured by Mitsui Chemicals, Inc.) was used. In addition, a PP resin was used to form a sheet having a basis weight of 100 g / m. 2 A film (melting point 165°C) was prepared.
[0091] [PPS resin, PPS resin film] The PPS resin used was a crystalline polyarylene sulfide with a melting point of 280°C. The PPS resin was used to make a sheet with a basis weight of 100g / m 2A film (melting point 280°C) was prepared.
[0092] [PEKK resin, PEKK resin film] The PEKK resin used was a polyetherketoneketone resin with a melting point of 300°C. The PEKK resin was used to fabricate a sheet with a basis weight of 100g / m 2 A film was prepared.
[0093] [PEEK resin, PEEK resin film] The PEEK resin used was polyether ether ketone resin with a melting point of 343°C. The PEEK resin was used to fabricate a 100g / m 2 A film was prepared.
[0094] [PA6 injection resin] As the PA6 injection resin, "Amilan (registered trademark)" CM1011G-45 (manufactured by Toray Industries, Inc.) was used.
[0095] [PP injection resin] The carbon fiber (1) and the above-mentioned PP resin were compounded using a twin-screw extruder (TEX-30α, manufactured by The Japan Steel Works, Ltd.) to produce pellets for injection molding with a fiber content of 30% by mass.
[0096] (7) Manufacturing process [Drawing process-1] The carbon fiber (1) or the glass fiber (1) is pulled out from a bobbin and the fiber mass per unit area is 100 g / m 2 The fiber was continuously drawn out as a continuous reinforcing fiber sheet aligned in one direction in a sheet shape having a width of 20 mm.
[0097] [Drawing process-2] The conveyor running direction during the production of the reinforcing fiber mat (1) is set as the 0° direction, and the fiber mass per unit area is 100 g / m 2 The reinforcing fiber mat (1) trimmed into a sheet shape with a width of 20 mm was continuously drawn out.
[0098] [First impregnation process-1] A resin film as shown in Table 1 or 2 was placed on one surface of the continuous reinforcing fiber sheet continuously drawn out in the drawing step, and the component [B] was melted by heating with an IR heater and adhered to the entire surface of one side of the continuous reinforcing fiber sheet. This was pressed with a nip roll set at a surface temperature of (melting point of component [B] - 100°C) to impregnate the continuous reinforcing fiber sheet with the component [B], and cooled to obtain a fiber-reinforced resin intermediate.
[0099] [First impregnation process-2] In the drawing step, a resin film as shown in Table 1 was placed on the first surface of the continuous reinforcing fiber sheet continuously drawn out, and a resin film as shown in Table 1 was placed on the second surface of the continuous reinforcing fiber sheet, so that the continuous reinforcing fiber sheet was sandwiched between the two resin films. These were heated with an IR heater to melt or soften the components [B] and [C] while running the continuous reinforcing fiber sheet, and the components [B] and [C] were attached to the continuous reinforcing fiber sheet, and the continuous reinforcing fiber sheet was impregnated with the components [B] and [C] by pressing with a nip roll set to a surface temperature 100° C. lower than the temperature indicating the lower value of the melting point or glass transition temperature of the component [B] or the component [C], and the continuous reinforcing fiber sheet was cooled to obtain a fiber-reinforced resin substrate.
[0100] [Second impregnation process-1] A resin film described in Table 1 or 2 was laminated as the component [C] on the second surface of the fiber-reinforced resin intermediate in which the component [B] was impregnated on the first surface of the continuous reinforcing fiber sheet obtained by the first impregnation step-1. These were heated with an IR heater to melt or soften the component [C], and the component [C] was attached to the second surface of the traveling continuous reinforcing fiber sheet. The component [C] was impregnated into the continuous reinforcing fiber sheet by pressing with a nip roll set at a surface temperature 100°C lower than the temperature indicating the lower value of the melting point or glass transition temperature of the component [C], and the fiber-reinforced resin substrate was obtained by cooling.
[0101] [Pickup process-1] The fiber-reinforced resin substrate obtained by the above steps was wound up on a drum winder.
[0102] [Pick-up process-2] The fiber-reinforced resin substrate obtained by the above process was cut into pieces each having a length of 1 m.
[0103] In the configuration of the fiber-reinforced resin substrate in the table, for example, [B] / [A] / [C] indicates that the constituent element [B], the constituent element [A], and the constituent element [C] are laminated in this order, and the constituent element [B] is present on one surface of the fiber-reinforced resin substrate, and the constituent element [C] is present on the other surface. In the configuration of the fiber-reinforced resin substrate obtained in each example, the resin region containing the constituent element [B] and the resin region containing the constituent element [C] were adjacent to each other in layers to form an interface.
[0104] Example 1 A fiber-reinforced resin substrate was manufactured at a speed of 5.0 m / min by a roll-to-roll continuous manufacturing device using the components [A], [B], and [C] listed in Table 1 as materials and the manufacturing process listed in Table 1. The properties of the obtained fiber-reinforced resin substrate are shown in Table 1.
[0105] Example 2 A fiber-reinforced resin substrate was produced in the same manner as in Example 1, except that PPS resin was used as component [B], PA6 resin was used as component [C], and various molding temperatures were changed according to the Tb and Tc values shown in Table 1 depending on the resin used. The properties of the obtained fiber-reinforced resin substrate are shown in Table 1.
[0106] Example 3 A fiber-reinforced resin substrate was produced in the same manner as in Example 1, except that PEKK resin was used as component [B], PA6 resin was used as component [C], and various molding temperatures were changed according to the Tb and Tc values shown in Table 1 depending on the resin used. The properties of the obtained fiber-reinforced resin substrate are shown in Table 1.
[0107] Example 4 A fiber-reinforced resin substrate was produced in the same manner as in Example 1, except that a PPS resin was used as the component [B] and that the molding temperatures were changed according to the Tb and Tc values shown in Table 1 depending on the resin used. The properties of the obtained fiber-reinforced resin substrate are shown in Table 1.
[0108] Example 5 A fiber-reinforced resin substrate was produced in the same manner as in Example 1, except that PEEK resin was used as component [B], PA6 resin was used as component [C], and various molding temperatures were changed according to the Tb and Tc values shown in Table 1 depending on the resin used. The properties of the obtained fiber-reinforced resin substrate are shown in Table 1.
[0109] Example 6 A fiber-reinforced resin substrate was produced in the same manner as in Example 1, except that PEEK resin was used as the component [B] and various molding temperatures were changed according to the Tb and Tc values shown in Table 1 depending on the resin used. The properties of the obtained fiber-reinforced resin substrate are shown in Table 2.
[0110] Example 7 A fiber-reinforced resin substrate was produced in the same manner as in Example 1, except that a fiber-reinforced resin substrate was obtained only by the first impregnation step-2 in which the constituent element [B] and the constituent element [C] were simultaneously impregnated. The properties of the obtained fiber-reinforced resin substrate are shown in Table 2.
[0111] Example 8 A fiber reinforced resin substrate was produced in the same manner as in Example 1, except that three layers of the component [A] were used and the structure of the fiber reinforced resin substrate was [B] / [A] / [B] / [A] / [C] / [A] / [C]. The properties of the obtained fiber reinforced resin substrate are shown in Table 2.
[0112] Example 9 Except for using glass fiber as the component [A], a fiber-reinforced resin substrate was produced in the same manner as in Example 1. The properties of the obtained fiber-reinforced resin substrate are shown in Table 2.
[0113] (Reference example 1) The fiber-reinforced resin substrate obtained in Example 1 was cut out and placed between injection molds. The mold was closed, and two-color molding was performed using two types of injection materials, such that PA6 injection resin was on the component [B] side and PP injection resin was on the component [C] side. As a result, an integrated molded product was obtained in which another member made of PA6 was joined via the component [B] and another member made of PP was joined via the component [C].
[0114] Comparative Example 1 An unreinforced resin substrate was produced in the same manner as in Example 7, except that component [A] was not used. The properties of the obtained unreinforced resin substrate are shown in Table 3.
[0115] Comparative Example 2 A fiber-reinforced resin substrate was produced in the same manner as in Example 1, except that a reinforcing fiber mat (carbon fiber having a random shape) was used as the component [A]. The properties of the obtained fiber-reinforced resin substrate are shown in Table 3.
[0116] Comparative Example 3 A material similar to that of Example 1 was prepared. A fiber-reinforced resin (I) consisting of the components [A] and [B] was obtained in the same manner as in Example 1, except that the component [B] was arranged on the second surface in the first impregnation step-2 (both surfaces of the continuous reinforcing fiber sheet became the component [B]). Separately, a fiber-reinforced resin (II) consisting of the components [A] and [C] was obtained in the same manner as in Example 1, except that the component [C] was arranged on the first surface in the first impregnation step-1 (both surfaces of the continuous reinforcing fiber sheet became the component [C]). The obtained fiber-reinforced resin (I) and the fiber-reinforced resin layer (II) were laminated and heated to a temperature at which only the component [C] melts with an IR heater and run, while being pressed and fused with a nip roll set to a surface temperature 100° C. lower than the melting point of the component [C], to obtain a fiber-reinforced resin substrate.
[0117] (Reference example 2) A fiber-reinforced resin substrate was produced in the same manner as in Example 7, except that PP resin was used for both the component [B] and the component [C]. The properties of the obtained fiber-reinforced resin are shown in Table 3. The obtained fiber-reinforced resin substrate was cut out and placed between the injection molding dies in the same manner as in Reference Example 1. The die was closed, and two-color molding was performed using two types of injection materials so that the PA6 injection resin was on one surface side and the PP injection resin was on the other surface side. At this time, the PA6 injection resin could not be welded to the fiber-reinforced resin and peeled off.
[0118] [Table 1]
[0119] [Table 2]
[0120] [Table 3]
[0121] <Consideration> Comparison of Examples 1 to 9 with Comparative Examples 1 to 3 shows that the fiber-reinforced resin substrate obtained by the present invention can composite resin combinations that are generally very poorly compatible and difficult to composite. In particular, in Examples 1 and 4 to 6, even in combinations of resins with a difference in melting point or glass transition temperature of 100°C or more, where one resin decomposes, in an impregnation method in which multiple resins are melted simultaneously (for example, as described in Patent Document 2), composites can be made without decomposing or deteriorating the resins. In addition, in Example 8, it was shown that a thick fiber-reinforced resin substrate can be obtained by increasing the amount of reinforcing fibers used. On the other hand, in Comparative Example 1, since the reinforcing fibers, which are the component [A], were missing, these resins were easily peeled off and could not be composited. Furthermore, in Comparative Example 2, even though the combination of resins was capable of being continuously wound in the Examples, the reinforcing fibers were torn off, resulting in intermittent production. In addition, when the obtained fiber-reinforced resin substrate was observed, it was shown that there was a large variation in the anchoring depth (such as the above-mentioned average roughness height Rc). In Comparative Example 3, even though the material composition was the same as in Example 1, the reinforcing fibers did not span the boundary surface between the fiber-reinforced thermoplastic resin (I) and the fiber-reinforced thermoplastic resin (II), so that each layer easily peeled off, and the desired substrate could not be obtained.
[0122] In Reference Example 1, the fiber-reinforced resin substrate obtained in Example 1 was used as a medium to obtain an integrated molded product in which members made of two different types of resins were bonded as shown in FIG. 8(c). As shown in Comparative Example 1, this combination of resins is a combination that is easily peeled off in the conventional technology, and it was found that by using the fiber-reinforced resin substrate of the present invention, a firmly integrated integrated molded product can be obtained. In the conventional technology, in order to ensure the bonding strength in such a combination of resins, it was necessary to form a fit as shown in FIG. 8(a) or (b), but by using the fiber-reinforced resin substrate of the present invention, this is not necessary, and it is possible to increase the design freedom of the shape, etc. Also, when the same type of resin was used on both sides of the fiber-reinforced resin substrate as in Reference Example 2, it was not possible to bond members made of different resins as in Reference Example 1. [Industrial Applicability]
[0123] The fiber-reinforced resin substrate of the present invention is a composite of resins having a combination of different properties, particularly a plurality of thermoplastic resins having low compatibility, and therefore it is possible to obtain a substrate having a combination of different properties that was difficult to obtain with conventional techniques. In addition, the fiber-reinforced resin substrate and integrally molded product of the present invention can be applied to aircraft structural members, wind turbine blades, automobile structural members, and computer applications such as IC trays and notebook computer housings, and can exhibit excellent performance as a structure and can significantly reduce the molding time and molding costs of products related to the above applications. [Explanation of symbols]
[0124] A: Section A B: Cross section B C: Cross section C 1: Fiber-reinforced resin substrate 2: Component [A] (reinforced fiber) 3: Component [B] (thermoplastic resin (b)) and component [C] (thermoplastic resin (c)) 4: Fiber direction (reference axis) 5: Observation cross section (cross section obtained by cutting perpendicular to the plane of the fiber-reinforced resin substrate) 6: Component [B] 7: Component [C] 8: Observation cross section 9: Boundary 10: End of component [C] (reference line) 11: Orthobase line 12: Cross section curve 13: Continuous fiber reinforced sheet 14: Fiber-reinforced resin intermediate 15: Pulling out process 16: First impregnation step 17: Second impregnation step 18: Pick-up process 19: First surface 20: Second Surface 21: Metal parts 22: Test piece holder 23:PA injection material 24:PP injection material
Claims
1. A fiber-reinforced resin substrate comprising the following components [A], [B] and [C]: [A] reinforcing fiber; [B] Thermoplastic resin (b); [C] Thermoplastic resin (c); The components [A] are arranged in one direction, In the fiber-reinforced resin substrate, a resin region containing the component [B] and a resin region containing the component [C] are present, A resin region containing the component [B] is present on one surface of the fiber-reinforced resin substrate, Distance Ra of Hansen solubility parameters of component [B] and component [C] (bc) satisfies formula (1), Ra (bc) = {4(δDB - δDC) 2 + (δPB - δPC) 2 + (δHB - δHC) 2} 1/2 ≥ 8 Equation (1) Ra (bc) : The distance between the Hansen solubility parameters of the component [B] and the component [C]; δDB: Energy due to dispersion forces between molecules of the component [B]; δ DC : Energy due to dispersion forces between molecules of the component [C]; δPB: Energy due to dipole interactions between molecules of component [B]; δPC: Energy due to dipole interactions between molecules of component [C]; δH: Energy due to hydrogen bonds between molecules of component [B]; δHC: Energy due to hydrogen bonds between molecules of component [C]; a resin region containing the component [B] and a resin region containing the component [C], the component [A] being present across an interface between the two resin regions; In a plan view of the fiber reinforced resin substrate, when a cross section perpendicular to the fiber reinforced resin substrate is obtained in a direction at an angle of 45 degrees to the fiber direction of the component [A], In the cross section, the roughness average length RSm of a cross-sectional curve formed by the boundary surface of both resin regions is 100 μm or less and the roughness average height Rc is 3.5 μm or more, as defined in JIS B0601 (2001); A fiber-reinforced resin substrate, in which a resin region containing the component [B] and a resin region containing the component [C] are adjacent to each other in a layered form to form the boundary surface.
2. The fiber reinforced resin substrate according to claim 1, having an impregnation rate of 80% or more.
3. The fiber reinforced resin substrate according to claim 1 or 2, which satisfies formula (2): 50≦ΔT≦200... Formula (2) ΔT: absolute value of the difference between Tb and Tc; Tb: melting point of the thermoplastic resin (b) when it is a crystalline resin, or glass transition temperature of the thermoplastic resin (b) when it is an amorphous resin [° C.]; Tc: When the thermoplastic resin (c) is a crystalline resin, it is its melting point; when it is an amorphous resin, it is its glass transition temperature [° C.].
4. The fiber reinforced resin substrate according to claim 3, wherein at least one of Tb and Tc is 250° C. or less.
5. An integrated molded product obtained by joining another member to the fiber reinforced resin substrate according to any one of claims 1 to 4.
6. The integrally molded product according to claim 5, wherein another member is joined to the fiber reinforced resin substrate via the component [B] and / or the component [C].
7. A method for producing a fiber-reinforced resin substrate comprising the following components [A], [B] and [C]: [A] reinforcing fiber; [B] Thermoplastic resin (b); [C] Thermoplastic resin (c); At least the following drawing step, first impregnation step, and second impregnation step are carried out continuously in this order while the component [A] is traveling, <Extraction step> A step of drawing continuous constituent elements [A] to obtain a continuous reinforcing fiber sheet in which the constituent elements [A] are aligned in one direction, and then supplying the obtained continuous reinforcing fiber sheet containing the constituent elements [A] in the fiber direction toward a subsequent step; <First impregnation step> A step of impregnating one surface of the continuous reinforcing fiber sheet with the component [B] to obtain a fiber-reinforced resin intermediate having the component [B] present on the first surface of the continuous reinforcing fiber sheet; <Second impregnation step> A step of impregnating the component [C] from a second surface opposite to the first surface to obtain a fiber-reinforced resin substrate; Distance Ra of Hansen solubility parameters of component [B] and component [C] (bc) A method for producing a fiber reinforced resin substrate satisfying formula (3): Ra (bc) = {4(δDB - δDC) 2 + (δPB - δPC) 2 + (δHB - δHC) 2} 1/2 ≥ 8 Equation (3) Ra (bc) : Distance between Hansen solubility parameters of component [B] and component [C] δDB: Energy due to dispersion forces between molecules of the component [B]; δ DC : Energy due to dispersion forces between molecules of the component [C]; δPB: Energy due to dipole interactions between molecules of component [B]; δPC: Energy due to dipole interactions between molecules of component [C]; δH: Energy due to hydrogen bonds between molecules of component [B]; δHC: Energy due to hydrogen bonds between molecules of component [C].
8. In the obtained fiber reinforced resin substrate, There are resin regions containing component [B] and resin regions containing component [C], a resin region containing the component [B] and a resin region containing the component [C], the component [A] being present across an interface between the two resin regions; In a plan view of the fiber reinforced resin substrate, when a cross section perpendicular to the fiber reinforced resin substrate is obtained in a direction at an angle of 45 degrees to the fiber direction of the component [A], 8. The method for producing a fiber-reinforced resin substrate according to claim 7, wherein the cross-sectional curve formed by the boundary surface of both resin regions has a roughness average length RSm defined in JIS B0601 (2001) of 100 μm or less and a roughness average height Rc of 3.5 μm or more.
9. The method for producing a fiber-reinforced resin substrate according to claim 8, wherein the resin region containing the component [B] and the resin region containing the component [C] are adjacent to each other in a layer shape to form the boundary surface.
Citation Information
Patent Citations
Carbon fiber reinforced resin molded product and its manufacture
JP1998138354A
Fiber reinforced resin board material
JP2002316376A
Prepreg sheet material and method for producing the same
JP2012246442A
Prepreg and prepreg manufacturing method
JP2013209626A
Molding and method for producing the same
JP2016196142A