Thermoplastic resin composition, its method of manufacture, and molded article
A thermoplastic resin composition with polyethylene, polyamide, and a compatibilizer addresses the challenge of achieving high impact resistance and fluidity using plant-derived materials, resulting in environmentally friendly molded articles with enhanced mechanical properties.
Patent Information
- Application Number
- JP2020123260
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-17
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2040-07-17
AI Technical Summary
Existing thermoplastic resin compositions using plant-derived materials face challenges in achieving high impact resistance and fluidity while reducing environmental impact, as there are limited grades suitable for various applications compared to fossil-derived resins.
A thermoplastic resin composition comprising polyethylene, polyamide, and a compatibilizer with a reactive group, where all components have a biobased carbon content of 80% or more, and specific MFR and density ranges are used, along with a melt-kneading process to enhance compatibility and properties.
The composition achieves both high impact resistance and fluidity, enabling the production of molded articles with reduced environmental impact, while maintaining excellent mechanical properties.
Smart Images

Figure 0007577943000002 
Figure 0007577943000003 
Figure 0007577943000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermoplastic resin composition, a method for producing the same, and a molded article thereof. More specifically, the present invention relates to a thermoplastic resin composition containing polyethylene, polyamide, and a compatibilizer, a method for producing the same, and a molded article thereof. [Background technology]
[0002] The following Patent Documents 1 and 2 disclose techniques for obtaining a thermoplastic resin composition having excellent impact resistance by using three components: a polyolefin, a polyamide, and a compatibilizer. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2013-094763 Brochure [Patent Document 2] International Publication No. 2013-094764 Brochure Summary of the Invention [Problem to be solved by the invention]
[0004] The above Patent Documents 1 and 2 disclose the use of a modified elastomer having a reactive group with polyamide as a compatibilizer, the use of a molten mixture of a compatibilizer and polyamide that has been melt-kneaded separately from a polyolefin, the melt-kneaded mixture obtained and a polyolefin to obtain the target thermoplastic resin composition, and the use of plant-derived polyamide 11 as the polyamide.
[0005] In recent years, the construction of a sustainable society and the associated reduction of environmental load have been highlighted, and there is an increasing demand for responses in the field of materials technology. Specifically, from the viewpoint of reducing CO2 emissions, technology that uses plant-derived raw materials instead of fossil-derived raw materials such as petroleum has attracted attention, and plant-derived products have been launched not only for polyamides but also for polyolefins as general-purpose resins. However, compared to the fossil-derived resins that have been used for a long time, there are only a few grades of each, and adjustments to suit various applications have not progressed. For this reason, it is not possible to directly replace the fossil-derived resins that have been used conventionally with plant-derived resins, and there are various problems in increasing the proportion of plant-derived resins.
[0006] The present invention has been made in view of the above circumstances, and has an object to provide a thermoplastic resin composition that can achieve both high impact resistance and high fluidity by using three components, i.e., a polyolefin, a polyamide, and a compatibilizer, while reducing the environmental impact, a method for producing the same, and a molded article using the thermoplastic resin composition. [Means for solving the problem]
[0007] That is, the present invention is as follows. [1] The thermoplastic resin composition of the present invention is a thermoplastic resin composition comprising a polyethylene, a polyamide, and a compatibilizer, the compatibilizer is a modified elastomer having a group reactive with the polyamide, The polyethylene and polyamide have a bio-based carbon content of 80% or more according to ISO 16620-2. [2] In the thermoplastic resin composition of the present invention, the MFR (230° C. / 2.16 kg) of the polyethylene can be set to 20 g / 10 min or less. [3] In the thermoplastic resin composition of the present invention, the MFR (230° C. / 2.16 kg) can be made to be 3 g / 10 min or more. [4] In the thermoplastic resin composition of the present invention, the compatibilizer may have a copolymer chain derived from ethylene and other α-olefins as its main skeleton, and the reactive group may be an acid-modified group. [5] In the thermoplastic resin composition of the present invention, the compatibilizer is present in an amount of 1 to 30 mass% when the total amount of the polyethylene, the polyamide, and the compatibilizer is 100 mass%, The mass ratio of the polyethylene when the total of the polyethylene, the polyamide, and the compatibilizer is 100 mass %, is R PE mass%, the mass ratio of the polyamide is R PA When expressed as mass%, R PE / R PA can be set to 0.3 to 3.5. [6] The molded article of the present invention is characterized in that it is made of the thermoplastic resin composition of the present invention. [7] A method for producing a thermoplastic resin composition of the present invention is summarized as comprising a melt-kneading step of melt-kneading a melt-kneaded mixture of the polyamide and the compatibilizer, and the polyethylene. Effect of the Invention
[0008] According to the thermoplastic resin composition and the method for producing the same of the present invention, it is possible to achieve both high impact resistance and high fluidity by using three components, i.e., polyolefin, polyamide, and compatibilizer, while reducing the environmental load. According to the molded article of the present invention, it is possible to achieve a molded article having high impact resistance by using three components, i.e., polyolefin, polyamide, and compatibilizer, while reducing the environmental load. [Brief description of the drawings]
[0009] [Figure 1] Phase structure obtained by magnifying the surface of the test piece in Experimental Example 6 by 5000 times [Diagram 2] Phase structure obtained by magnifying the surface of the test piece in Experimental Example 6 by 10,000 times [Diagram 3] Phase structure obtained by magnifying the surface of the test piece in Experimental Example 6 by 20,000 times [Figure 4] Phase structure obtained by magnifying the surface of the test piece in Experimental Example 8 by 5000 times [Diagram 5] Phase structure obtained by magnifying the surface of the test piece of Experimental Example 8 by 10,000 times [Figure 6] Phase structure obtained by magnifying the surface of the test piece of Experimental Example 8 by 20,000 times DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The matters shown herein are illustrative and are intended to exemplify the embodiments of the present invention, and are described for the purpose of providing what is believed to be the most effective and easily understandable explanation of the principles and conceptual features of the present invention. In this respect, it is not intended to show structural details of the present invention beyond the extent necessary for a fundamental understanding of the present invention, and the description in conjunction with the drawings will make it clear to those skilled in the art how some forms of the present invention can be actually embodied. In this specification, the expression "XX to YY" means "XX or more and YY or less."
[0011] [1] Thermoplastic resin composition The thermoplastic resin composition of the present invention is a thermoplastic resin composition comprising polyethylene, polyamide, and a compatibilizer. The compatibilizer is a modified elastomer having a reactive group with respect to polyamide. Furthermore, the polyethylene and polyamide have a bio-based carbon content of 80% or more according to ISO16620-2.
[0012] <1> Polyethylene (plant-derived PE) The polyethylene has a bio-based carbon content of 80% or more as measured in accordance with the ISO16620-2 standard (in this specification, the polyethylene is also referred to simply as "plant-derived PE"). This bio-based carbon content is the percentage of the total carbon that constitutes the polyethylene. 14 This is the plant-derived carbon content (bio-based carbon content) calculated based on the proportion of C. The plant-derived PE used in the present invention may have a bio-based carbon content of 80% or more (or 100%), and may further be plant-derived PE with a bio-based carbon content of 85% or more, or even 90% or more. In addition to ISO 16620-2, values measured according to ASTM D6866 can also be used for the bio-based carbon content. Usually, the values according to these standards are essentially the same.
[0013] Plant-derived PE is a polymer whose main skeleton is a structure (methylene chain) in which methylene groups (-CH2-) are linked. The methylene chain is a structural unit derived from ethylene in particular. Thus, plant-derived PE includes ethylene homopolymers and copolymers of ethylene and other olefins. In the case of copolymers, usually, 50% or more of the total number of structural units are ethylene-derived units. Other olefins include olefins with 3 carbon atoms (propylene), olefins with 4 carbon atoms (1-butene, etc.), olefins with 5 carbon atoms (3-methyl-1-butene, 1-pentene, etc.), olefins with 6 carbon atoms (3-methyl-1-pentene, 4-methyl-1-pentene, 1-hexene, etc.), and olefins with 8 carbon atoms (1-octene, etc.). These may be used alone or in combination of two or more. That is, examples of plant-derived PE that is a copolymer include, for example, ethylene-1-butene copolymer, ethylene-1-hexene copolymer, ethylene-1-octene copolymer, ethylene-4-methyl-1-pentene copolymer, etc. These may be used alone or in combination of two or more. Furthermore, when two or more types are used, this includes both pellets made of mixed resins and pellet mixtures.
[0014] Furthermore, regardless of whether the plant-derived PE is a homopolymer of ethylene or a copolymer of ethylene and another olefin, it becomes a plant-derived PE when the monomers that form these polymers are derived from plant raw materials. The monomers may be entirely plant-derived monomers, or only a portion of them may be plant-derived monomers (i.e., the other portion may contain fossil-derived monomers). In other words, plant-derived PE will be sufficient if it has a bio-based carbon content of 80% or more.
[0015] The properties of plant-derived PE are not limited, but the density is 0.942 g / cm 3 It is preferable that the plant-derived PE is a high-density polyolefin having a MFR (230°C / 2.16 kg) of 35 g / 10 min or less. By making the plant-derived PE have a MFR of 35 g / 10 min or less (usually 1 g / 10 min or more), the resulting thermoplastic resin composition can have excellent impact resistance and high fluidity. The MFR is more preferably 20 g / 10 min or less, more preferably 15 g / 10 min or less. The lower limit is not limited, but from the viewpoint of ease of melt kneading, it is preferably 2 g / 10 min or more, more preferably 3 g / 10 min or more. In the present invention, the MFR (230° C. / 2.16 kg) of the plant-derived PE is a value measured in accordance with the standard ISO 1133 or ASTM D 1238. The values according to these standards are usually substantially the same value.
[0016] As mentioned above, the density of plant-derived PE is 0.942 g / cm 3 More preferably, the density is 0.950 g / cm or more. 3 The upper limit of the density is not limited, but is preferably 0.954 g / cm 3 It is preferable that: The compatibility of the above-mentioned MFR and density can be adjusted by the linearity, amount of branching, molecular weight, etc. of the plant-derived PE. In the present invention, the density of the plant-derived PE is a value measured in accordance with the standard ISO 1183 or ASTM D 792. The values according to these standards are usually substantially the same value.
[0017] Furthermore, the MFR (230°C / 2.16kg) of the plant-derived PE is preferably small. Specifically, it is preferable that the MFR is closer to the MFR (230°C / 2.16kg) of the melt-kneaded product obtained from the plant-derived PA and the compatibilizer described below. That is, the kneading of the plant-derived PA and the compatibilizer is considered to be promoted by the reaction between the two, and the kneading of the two is less affected by the MFR difference. In contrast, the kneading of the plant-derived PE and the melt-kneaded product (melt-kneaded product of the plant-derived PA and the compatibilizer) is considered to be easily affected by the MFR difference between the two, since the two do not react. Therefore, it is considered that the kneadability is improved by bringing the MFR of the plant-derived PE closer to the MFR of the melt-kneaded product, and the impact resistance is improved accordingly.
[0018] Specifically, the MFR of plant-derived PE (230℃ / 2.16kg) is PE (g / 10 min), and the MFR (230°C / 2.16 kg) of the melt-kneaded mixture of plant-derived PA and compatibilizer is M PX (g / 10 min), the ratio M PE / PX (=M PE / M PX ) is 0.5≦M PE / PX ≦20, and 1≦M PE / PX ≦17 is more preferable, and 2≦M PE / PX It is more preferable that M PE / PX It is particularly preferred that it is ≦10. Furthermore, M PX The range of is not limited, but for example, 0.1≦M PX (g / 10 min)≦10, and further, 0.5≦M PX (g / 10 min)≦5, and further, 1≦M PX (g / 10 min)≦3.
[0019] <2> Polyamide (Plant-derived PA) The polyamide has a bio-based carbon content of 80% or more as measured in accordance with the ISO16620-2 standard (in this specification, the polyamide is also referred to simply as "plant-derived PA"). This bio-based carbon content is the percentage of the total carbon composition. 14 This is the plant-derived carbon content (bio-based carbon content) calculated based on the proportion of C. The plant-derived PA used in the present invention may have a bio-based carbon content of 80% or more (or 100%), and may further be a plant-derived PA with a bio-based carbon content of 90% or more, or may further be a plant-derived PA with a bio-based carbon content of 95% or more. In addition to ISO 16620-2, values measured according to ASTM D6866 can also be used for the bio-based carbon content. Usually, the values according to these standards are essentially the same.
[0020] Plant-derived PA is a polymer whose main skeleton is a structure in which hydrocarbon groups (especially methylene chains) are linked via amide bonds (-NH-CO-). Examples of monomers constituting plant-derived PA include amino acids such as 6-aminocaproic acid, 11-aminoundecanoic acid, 12-aminododecanoic acid, and para-aminomethylbenzoic acid, and lactams such as ε-caprolactam, undecanelactam, and ω-lauryllactam. These may be used alone or in combination of two or more. Among these, from the viewpoint of a high bio-based carbon content, it is preferable that the plant-derived 11-aminoundecanoic acid is contained in large amounts.
[0021] Furthermore, plant-derived PA can also be obtained by copolymerization of diamine and dicarboxylic acid. In this case, examples of diamine as a monomer include ethylenediamine, 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, 1,7-diaminoheptane, 1,8-diaminooctane, 1,9-diaminononane, 1,10-diaminodecane, 1,11-diaminoundecane, 1,12-diaminododecane, 1,13-diaminotridecane, 1,14-diaminotetradecane, 1,15-diaminopentadecane, 1,16-diaminodiamine, 1,17-diaminodiamine, 1,18-diaminodiamine, 1,19-diaminodiamine, 1,20-diaminodiamine, 1,21-diaminodiamine, 1,22-diaminodiamine, 1,23-diaminodiamine, 1,24-diaminodiamine, 1,25-diaminodiamine, 1,26-diaminodiamine, 1,27-diaminodiamine, 1,28-diaminodiamine, 1,29-diaminodiamine, 1,30-diaminodiamine, 1,31-diaminodiamine, 1,32-diaminodiamine, 1,33-diaminodiamine, 1,34-diaminodiamine, 1,35-diaminodiamine, 1,36-diaminodiamine, 1,37-diaminodiamine, 1,38-diaminodiamine, 1,39-diaminodiamine, 1,40-diaminodiamine, 1,41-diaminodiamine, 1,42-diaminodiamine, 1,43-diaminodiamine, 1,44-diaminodiamine, 1,45-diaminodiamine, Examples of the diamines include aliphatic diamines such as 2-methyl-1,5-diaminopentane, 2-methyl-1,8-diaminooctane, cyclohexanediamine, bis-(4-aminocyclohexyl)methane, and aromatic diamines such as xylylenediamine (p-phenylenediamine, m-phenylenediamine, etc.). These may be used alone or in combination of two or more. Among these, from the viewpoint of a high bio-based carbon content, it is preferable that the diamines contain a large amount of plant-derived 1,10-diaminodecane and / or 1,5-diaminopentane.
[0022] Further, examples of dicarboxylic acids as monomers include aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecane diacid, dodecane diacid, brassic acid, tetradecane diacid, pentadecanedioic acid, and octadecanedioic acid, alicyclic dicarboxylic acids such as cyclohexane dicarboxylic acid, aromatic dicarboxylic acids such as phthalic acid, terephthalic acid, isophthalic acid, and naphthalenedicarboxylic acid, and further furandicarboxylic acid. These may be used alone or in combination of two or more. Among these, from the viewpoint of a high biobased carbon content, it is preferable that plant-derived sebacic acid, furandicarboxylic acid, and / or glutaric acid are contained in large amounts.
[0023] That is, examples of plant-derived PA include polyamide 11 (PA11), polyamide 1010 (PA1010), polyamide 1012 (PA1012), polyamide 610 (PA610), polyamide 510 (PA510), polyamide (PA410), polyamide (PA10T), polyamide 11T (PA11T), polyamide MXD10 (MXD10), etc. These polyamides may be used alone or in combination of two or more. Furthermore, when two or more types are used, it includes both pellets made of mixed resins and pellet mixtures.
[0024] Furthermore, regardless of whether the plant-derived PA is a homopolymer of an amino acid or lactam, or a copolymer of a diamine and a dicarboxylic acid, the plant-derived PA is one in which the monomers forming these polymers are derived from plant materials. The monomers may be entirely plant-derived monomers, or only a portion of them may be plant-derived monomers (i.e., the other portion may contain fossil-derived monomers). In other words, the plant-derived PA may have a bio-based carbon content of 80% or more.
[0025] Although the properties of plant-derived PA are not limited, the density is 1.15 g / cm 3 The polyamide is preferably one of the above polyamides and has an MFR (230°C / 2.16 kg) of 50 g / 10 min or less. By having the MFR of the plant-derived PA be 50 g / 10 min or less (usually 1 g / 10 min or more), the resulting thermoplastic resin composition can have excellent impact resistance and high fluidity. The MFR is more preferably 40 g / 10 min or less, more preferably 35 g / 10 min or less. The lower limit is not limited, but from the viewpoint of ease of melt kneading, it is preferably 3 g / 10 min or more, more preferably 5 g / 10 min or more. In the present invention, the MFR (230° C. / 2.16 kg) of the plant-derived PA is a value measured in accordance with the standard of ISO 1133 or ASTM D 1238. The values according to these standards are usually substantially the same value.
[0026] As mentioned above, the density of plant-derived PA is 1.15 g / cm 3The density is preferably 1.08 g / cm or less. 3 The lower limit of the density is not limited, but is preferably 0.98 g / cm. 3 More preferably, it is equal to or greater than this. The compatibility of MFR and density can be adjusted by the linearity, branching amount, molecular weight, etc. of the plant-derived PA. In the present invention, the density of the plant-derived PA is a value measured in accordance with the standard of ISO 1183 or ASTM D792. The values according to these standards are usually substantially the same value.
[0027] <3> Compatibilizer The compatibilizer is a modified elastomer having a reactive group with respect to plant-derived PA. Furthermore, the compatibilizer is preferably a component having affinity for plant-derived PE. In this case, the compatibilizer is a component having a compatibilizing effect on plant-derived PE and plant-derived PA. In other words, the compatibilizer is preferably a compatibilizer for plant-derived PE and plant-derived PA. In addition, the compatibilizer may be reacted entirely with the plant-derived PA in the present thermoplastic resin composition, or only a portion of it may be reacted.
[0028] The reactive group of the modified elastomer may be any group that is reactive with plant-derived PA, and examples of such groups include acid anhydride groups (-CO-O-OC-), carboxyl groups (-COOH), epoxy groups {-CO (three-membered ring structure consisting of two carbon atoms and one oxygen atom)}, oxazoline groups (-C3H4NO), and isocyanate groups (-NCO), etc. These groups may be used alone or in combination of two or more. The amount of modification of the modified elastomer by the reactive groups is not limited, and it is sufficient that the modified elastomer has one or more reactive groups in one molecule. Furthermore, it is preferable that the modified elastomer has 1 to 50 reactive groups, more preferably 3 to 30 reactive groups, and particularly preferably 5 to 20 reactive groups.
[0029] Examples of modified elastomers include polymers using various monomers capable of introducing reactive groups (modified elastomers obtained by polymerization using monomers capable of introducing reactive groups), oxidative decomposition products of various polymers (modified elastomers in which reactive groups are formed by oxidative decomposition), and graft polymers of organic acids onto various polymers (modified elastomers in which reactive groups are introduced by graft polymerization of organic acids). These may be used alone or in combination of two or more. These may be used alone or in combination of two or more.
[0030] Examples of the monomer into which a reactive group can be introduced include a monomer having a polymerizable unsaturated bond and an acid anhydride group, a monomer having a polymerizable unsaturated bond and a carboxyl group, and a monomer having a polymerizable unsaturated bond and an epoxy group. Specifically, acid anhydrides such as maleic anhydride, itaconic anhydride, succinic anhydride, glutaric anhydride, adipic anhydride, citraconic anhydride, tetrahydrophthalic anhydride, butenyl succinic anhydride, and carboxylic acids such as maleic acid, itaconic acid, fumaric acid, acrylic acid, and methacrylic acid can be mentioned. These may be used alone or in combination of two or more. Among these compounds, acid anhydrides are preferred, maleic anhydride and itaconic anhydride are more preferred, and maleic anhydride is particularly preferred.
[0031] Furthermore, the type of resin constituting the skeleton of the modified elastomer (hereinafter referred to as "skeleton resin") is not particularly limited, and various thermoplastic resins can be used. As the skeleton resin, an olefin-based elastomer (olefin-based thermoplastic elastomer) and / or a styrene-based elastomer (styrene-based thermoplastic elastomer) can be used.
[0032] Among these, the olefin-based elastomers include those obtained by copolymerizing two or more kinds of olefins. Examples of the olefin include ethylene, propylene, and α-olefins having 4 to 8 carbon atoms. Among these, examples of the α-olefins having 4 to 8 carbon atoms include 1-butene, 3-methyl-1-butene, 1-pentene, 3-methyl-1-pentene, 4-methyl-1-pentene, 1-hexene, and 1-octene.
[0033] Among these, the olefin-based elastomer is preferably a copolymer of ethylene and other α-olefins. That is, the compatibilizer is preferably a modified elastomer having a copolymer chain derived from ethylene and other α-olefins as the main skeleton and a reactive group with respect to plant-derived PA. When such an olefin-based elastomer is used, a thermoplastic resin composition that gives a molded article having particularly excellent impact resistance properties can be obtained. And, as the α-olefin other than ethylene, an α-olefin having 3 to 8 carbon atoms is preferable, and an α-olefin having 4 to 8 carbon atoms is more preferable.
[0034] Among the above, examples of copolymers of ethylene and α-olefins having 3 to 8 carbon atoms include ethylene-propylene copolymers (EPR), ethylene-1-butene copolymers (EBR), ethylene-1-pentene copolymers, and ethylene-1-octene copolymers (EOR). Examples of copolymers of propylene and α-olefins having 4 to 8 carbon atoms include propylene-1-butene copolymers (PBR), propylene-1-pentene copolymers, and propylene-1-octene copolymers (POR). These may be used alone or in combination of two or more. Furthermore, when two or more types are used, both pellets made of mixed resins and pellet mixtures are included.
[0035] On the other hand, a styrene-based thermoplastic elastomer is a styrene-based thermoplastic elastomer having a styrene skeleton. When this styrene-based thermoplastic elastomer is used, a molded article having particularly excellent impact resistance properties can be produced. More specific examples of the styrene-based thermoplastic elastomer include block copolymers of styrene-based compounds and conjugated diene compounds, and hydrogenated products thereof. Among these, examples of the styrene-based compound include styrene, alkylstyrenes such as α-methylstyrene, p-methylstyrene, and pt-butylstyrene, p-methoxystyrene, vinylnaphthalene, etc. These may be used alone or in combination of two or more. On the other hand, examples of the conjugated diene compound include butadiene, isoprene, piperylene, methylpentadiene, phenylbutadiene, 3,4-dimethyl-1,3-hexadiene, 4,5-diethyl-1,3-octadiene, etc. These may be used alone or in combination of two or more.
[0036] That is, examples of styrene-based thermoplastic elastomers include styrene-butadiene-styrene copolymer (SBS), styrene-isoprene-styrene copolymer (SIS), styrene-ethylene / butylene-styrene copolymer (SEBS), styrene-ethylene / propylene-styrene copolymer (SEPS), etc. These may be used alone or in combination of two or more. Furthermore, when two or more types are used, this includes both pellets made of mixed resins and pellet mixtures. Among these, SEBS is preferred.
[0037] The properties of the compatibilizer are not limited, but the density is 0.90 g / cm 3 The modified elastomer is preferably one of the following modified elastomers and has an MFR (230°C / 2.16 kg) of 10 g / 10 min or less. By making the MFR of the compatibilizer 10 g / 10 min or less (usually 0.5 g / 10 min or more), the resulting thermoplastic resin composition can have excellent impact resistance and high fluidity. The MFR is more preferably 7 g / 10 min or less, more preferably 5 g / 10 min or less. There is no upper limit, but from the viewpoint of ease of melt kneading, it is preferably 0.5 g / 10 min or more, more preferably 1.0 g / 10 min or more. In the present invention, the MFR (230° C. / 2.16 kg) of the compatibilizer is a value measured in accordance with the standard of ISO 1133 or ASTM D 1238. The values according to these standards are usually substantially the same value.
[0038] The density of the compatibilizer is 0.90 g / cm as described above. 3 Preferably, the density is 0.89 g / cm or less. 3 The lower limit of the density is not limited, but is preferably 0.85 g / cm. 3 More preferably, it is equal to or greater than this. The compatibility of MFR and density can be adjusted by the linearity, branching amount, molecular weight, modification amount, etc. of the compatibilizer. In the present invention, the density of the compatibilizer is a value measured in accordance with the standard of ISO 1183 or ASTM D792. The values according to these standards are usually substantially the same value.
[0039] The molecular weight of the modified elastomer is not particularly limited, but the weight average molecular weight is preferably from 10,000 to 500,000, more preferably from 35,000 to 500,000, and particularly preferably from 35,000 to 300,000. The weight average molecular weight is measured by the GPC method (standard polystyrene conversion).
[0040] <4> Combination of ingredients The mass ratio of plant-derived PE (hereinafter, this mass ratio is referred to as "R PE ") is preferably 10 to 90 mass%, more preferably 13 to 85 mass%, more preferably 17 to 80 mass%, more preferably 20 to 75 mass%, more preferably 23 to 70 mass%, and more preferably 25 to 65 mass%. That is, when the total of the plant-derived PE, the plant-derived PA, and the compatibilizer is taken as 100% by mass, the total ratio of the plant-derived PA and the compatibilizer (hereinafter, this mass ratio is referred to as "R PA+CB ") is preferably 10 to 90 mass %, more preferably 15 to 87 mass %, more preferably 20 to 83 mass %, more preferably 25 to 80 mass %, more preferably 30 to 77 mass %, and more preferably 35 to 75 mass %.
[0041] The mass ratio of plant-derived PA (hereinafter, this mass ratio is referred to as "R PA ") is preferably 1 to 80 mass %, more preferably 3 to 75 mass %, more preferably 5 to 70 mass %, more preferably 10 to 75 mass %, more preferably 15 to 70 mass %, more preferably 20 to 65 mass %.
[0042] The mass ratio of the compatibilizer (hereinafter, this mass ratio is referred to as "R CB ") is preferably 1 to 70 mass %, more preferably 2 to 60 mass %, more preferably 2 to 50 mass %, more preferably 3 to 40 mass %, more preferably 3 to 35 mass %, and more preferably 4 to 30 mass %.
[0043] When the total of the plant-derived PA and the compatibilizer is 100% by mass, the mass proportion of the compatibilizer is preferably 3 to 70% by mass, more preferably 4 to 65% by mass, more preferably 5 to 60% by mass, more preferably 6 to 55% by mass, more preferably 7 to 45% by mass, and more preferably 8 to 40% by mass.
[0044] Furthermore, when the total of the plant-derived PE, the plant-derived PA, and the compatibilizer is taken as 100 mass%, the mass ratio R CB is 1 to 30 mass%, the mass ratio R of plant-derived PE PE and the mass ratio of plant-derived PA R PA Ratio to PE / R PA ) is preferably 0.3 to 3.5. PE / R PA ) is more preferably from 0.4 to 2.0, more preferably from 0.35 to 2.00, further preferably from 0.40 to 1.50, and particularly preferably from 0.45 to 1.20. In the above range, the Charpy impact strength is 70 to 95 kJ / m 2 (Furthermore, 73~90kJ / m 2 , especially 75~87kJ / m 2), and a thermoplastic resin composition having an MFR (230° C. / 2.16 kg) of 12 to 28 g / 10 min (further, 16 to 27 g / 10 min, particularly 17 to 26 g / 10 min) can be obtained.
[0045] In particular, the mass ratio R of plant-derived PA PA is the mass ratio R of plant-derived PE. PE The greater the range (i.e., R PA >R PE ) in order to obtain a thermoplastic resin composition having high impact resistance and high fluidity, PE :R PA :R CB is preferably 20-45 mass%:50-80 mass%:1-25 mass%, more preferably 24-40 mass%:52-70 mass%:3-18 mass%, and particularly preferably 27-35 mass%:55-65 mass%:6-14 mass%. In the above range, the Charpy impact strength is 70 to 95 kJ / m 2 (Furthermore, 73~90kJ / m 2 , especially 75~87kJ / m 2 ), and a thermoplastic resin composition having an MFR (230° C. / 2.16 kg) of 12 to 28 g / 10 min (further, 16 to 27 g / 10 min, particularly 17 to 26 g / 10 min) can be obtained. Furthermore, even within the above range, when the total of the plant-derived PA and the compatibilizer is 100% by mass, the mass proportion of the compatibilizer is preferably 4 to 24% by mass, more preferably 7 to 20% by mass, and even more preferably 11 to 17% by mass.
[0046] Furthermore, the mass ratio R of plant-derived PA PA is the mass ratio R of plant-derived PE. PE The range where it is smaller (i.e., R PA <R PE ) in order to obtain a thermoplastic resin composition having high impact resistance and high fluidity, PE :R PA :R CBis preferably 35-65 mass%:30-60 mass%:1-20 mass%, more preferably 40-60 mass%:36-55 mass%:2-13 mass%, and particularly preferably 47-55 mass%:42-48 mass%:3-8 mass%. In the above range, the Charpy impact strength is 10 to 50 kJ / m 2 (Furthermore, 15~40kJ / m 2 , especially 17-30kJ / m 2 ), and a thermoplastic resin composition having an MFR (230° C. / 2.16 kg) of 10 to 28 g / 10 min (further, 12 to 25 g / 10 min, particularly 14 to 20 g / 10 min) can be obtained. Furthermore, even within the above range, when the total of the plant-derived PA and the compatibilizer is 100% by mass, the mass proportion of the compatibilizer is preferably 5 to 24% by mass, more preferably 6 to 18% by mass, and even more preferably 7 to 13% by mass.
[0047] The flowability of the thermoplastic resin composition of the present invention is not limited, but the density is preferably 0.93 to 1.00 g / cm. 3 At the same time, the MFR (230°C / 2.16 kg) can be 3 g / 10 min or more (usually 30 g / 10 min or less). This MFR can be further increased to 6 g / 10 min or more, further increased to 12 g / 10 min or more, and further increased to 17 g / 10 min or more. There is no upper limit, but it can be 27 g / 10 min or less. In the present invention, the MFR (230° C. / 2.16 kg) of the compatibilizer is a value measured in accordance with the standard of ISO 1133 or ASTM D 1238. The values according to these standards are usually substantially the same value.
[0048] The thermoplastic resin composition of the present invention (a molded article formed using the thermoplastic resin composition of the present invention) can have specific phase structures (1) to (3). Specifically, (1) it can have a phase structure in which the plant-derived PA is the continuous phase (A) and the plant-derived PE is the dispersed phase (B) (see Figs. 1 to 3). Furthermore, the dispersed phase (B) can have a continuous phase (B1) containing the plant-derived PE (i.e., continuous phase B1 within the dispersed phase) and a finely dispersed phase (B2) dispersed in the continuous phase B1 within the dispersed phase (i.e., dispersed phase B2 within the dispersed phase) (see Fig. 3).
[0049] Also, (2) it can have a phase structure in which plant-derived PE is the continuous phase (A) and plant-derived PA is the dispersed phase (B) (see Figs. 4 to 6). Furthermore, the dispersed phase (B) can have a continuous phase (B1) containing plant-derived PA (i.e., continuous phase B1 in the dispersed phase) and a finely dispersed phase (B2) dispersed in the continuous phase B1 in the dispersed phase (i.e., dispersed phase B2 in the dispersed phase) (see Fig. 6). In particular, the phase structure having the finely dispersed phase (B2) can provide excellent impact resistance properties.
[0050] Furthermore, the phase structure (3) can exhibit a bicontinuous structure in which the phase structures (1) and (2) are mixed. In particular, when the above phase structures (1) and (2) are present, excellent impact resistance can be obtained due to the phase structure having the finely dispersed phase (B2).Similarly, when the above bicontinuous structure (3) is present, excellent impact resistance can also be obtained.
[0051] In the case of the above-mentioned phase structure, the size of the dispersed phase contained in the continuous phase is not limited, but the average diameter (average particle diameter) is preferably 10000 nm or less, more preferably 50 to 8000 nm, and even more preferably 100 to 4000 nm. The average diameter of the dispersed phase is the average value (nm) of the maximum lengths of 50 dispersed phase particles randomly selected in an image obtained using an electron microscope.
[0052] In the case where the dispersed phase is dispersed within the dispersed phase, the size of the finely dispersed phase contained in the dispersed phase is not limited, but the average diameter (average particle diameter) is preferably 5 to 1000 nm, more preferably 5 to 600 nm, further preferably 10 to 400 nm, and particularly preferably 15 to 350 nm. The average diameter of the finely dispersed phase is the average value (nm) of the maximum length of 100 finely dispersed phase particles randomly selected in an image obtained using an electron microscope.
[0053] <5> Other ingredients The thermoplastic resin composition of the present invention may contain other components in addition to the above-mentioned plant-derived PE, plant-derived PA and compatibilizer. When the other components are thermoplastic polymers that can behave similarly to the plant-derived PE, plant-derived PA, and compatibilizer (excluding components that function as packing materials, fillers, etc.), the other components, that is, the thermoplastic polymers, are preferably 20 parts by mass or less when the total of the plant-derived PE, plant-derived PA, and compatibilizer is 100 parts by mass. When other components are included, the lower limit is not limited, but can be, for example, 1 part by mass.
[0054] Other components that are thermoplastic polymers include fossil-based polyolefins (polyolefins not included in the above-mentioned plant-based PE) that have a bio-based carbon content of less than 80% according to ISO 16620-2. Fossil-based polyolefins include olefin homopolymers and / or olefin copolymers. The olefin constituting the fossil-derived polyolefin is not limited, and examples thereof include ethylene, propylene, 1-butene, 3-methyl-1-butene, 1-pentene, 3-methyl-1-pentene, 4-methyl-1-pentene, 1-hexene, 1-octene, etc. These may be used alone or in combination of two or more. That is, examples of fossil-derived polyolefins include polyethylene, polypropylene, poly-1-butene, poly-1-hexene, poly-4-methyl-1-pentene, etc. These polymers may be used alone or in combination of two or more. Furthermore, when two or more types are used, the term includes both pellets made of mixed resins and pellet mixtures.
[0055] The polyethylene may be an ethylene homopolymer or a copolymer of ethylene and another olefin. The latter may be an ethylene-1-butene copolymer, an ethylene-1-hexene copolymer, an ethylene-1-octene copolymer, an ethylene-4-methyl-1-pentene copolymer, etc. In the copolymer of ethylene and another olefin, 50% or more of the total number of constituent units are derived from ethylene.
[0056] Polypropylene includes propylene homopolymers and copolymers of propylene with other olefins, such as propylene-ethylene copolymers, propylene-1-butene copolymers, propylene-1-hexene copolymers, propylene-1-octene copolymers, and propylene-4-methyl-1-pentene copolymers. Moreover, the copolymer of propylene and another olefin may be a random copolymer or a block copolymer. Among these, a block copolymer can be used from the viewpoint of excellent impact resistance. In particular, a propylene-ethylene block copolymer in which the other olefin is ethylene can be used. A propylene-ethylene block copolymer is a block copolymer polypropylene having an ethylene block as a dispersed phase. That is, it is a polypropylene resin in which a homopolypropylene is a continuous phase and a dispersed phase containing polyethylene exists within this continuous phase. Such a block copolymer polypropylene having an ethylene block as a dispersed phase is also called, for example, an impact copolymer, a polypropylene impact copolymer, a heterophasic polypropylene, a heterophasic block polypropylene, etc. This block copolymer polypropylene is preferable from the viewpoint of excellent impact resistance. In the copolymer of propylene and another olefin, 50% or more of the total number of constituent units are units derived from propylene.
[0057] Other components that are thermoplastic polymers include fossil-derived polyamides (polyamides not included in the above-mentioned plant-derived PA) whose bio-based carbon content according to ISO16620-2 is less than 80%. Examples of fossil-derived polyamides include polyamide 6, polyamide 66, polyamide 11, polyamide 610, polyamide 612, polyamide 614, polyamide 12, polyamide 6T, polyamide 6I, polyamide 9T, polyamide M5T, polyamide 1010, polyamide 1012, polyamide 10T, polyamide MXD6, polyamide 6T / 66, polyamide 6T / 6I, polyamide 6T / 6I / 66, polyamide 6T / 2M-5T, polyamide 9T / 2M-8T, etc. These polyamides may be used alone or in combination of two or more. Furthermore, when two or more types are used, it includes both pellets made of mixed resins and pellet mixtures.
[0058] When the other components do not behave in the same manner as the plant-derived PE, plant-derived PA, and compatibilizer, the other components are preferably 500 parts by mass or less when the total of the plant-derived PE, plant-derived PA, and compatibilizer is 100 parts by mass. The lower limit when other components are included is not limited, but can be, for example, 1 part by mass. Examples of such other components include various additives such as flame retardants, flame retardant auxiliaries, fillers, colorants, antibacterial agents, and antistatic agents. These may be used alone or in combination of two or more types.
[0059] [2] Method for producing thermoplastic resin composition The method for producing a thermoplastic resin composition of the present invention is characterized by comprising a melt-kneading step of melt-kneading a melt-kneaded mixture of a plant-derived PA and a compatibilizer, and a plant-derived PE. The properties and blending ratios of the plant-derived PE, plant-derived PA, and compatibilizer are as described above.
[0060] The melt-kneading step is a step in which a melt-kneaded mixture of the plant-derived PA and the compatibilizer is melt-kneaded with the plant-derived PE. The melt-kneaded product used in this case may be a molten composition or a softened composition, or may be solidified by pelletizing or the like. In this melt-kneading step, any melt-kneading device may be used. For example, an extruder (such as a single-screw extruder or a twin-screw kneading extruder), a kneader, or a mixer (such as a high-speed flow mixer, a paddle mixer, or a ribbon mixer) may be used. These devices may be used alone or in combination of two or more types. When two or more types are used, they may be operated continuously or in batches (batch type). Furthermore, the raw materials may be mixed all at once or may be added and mixed in multiple batches (multi-stage blending). The kneading temperature in the melt-kneading step is not particularly limited, but is preferably 190 to 350°C, more preferably 200 to 300°C, and further preferably 205 to 260°C.
[0061] In this method, by using a melt-kneaded product (a melt-kneaded product of plant-derived PA and a compatibilizer) that has been melt-kneaded in advance, kneading is performed when the plant-derived PA and the compatibilizer react with each other. Therefore, it is considered that a reactive group is added to the surface of the plant-derived PA due to the compatibilizer having a reactive group, and a plant-derived PA with the compatibilizer bonded to the surface is formed. Then, by further kneading, the plant-derived PA bonded to the surface is sheared, and the surface of the unreacted plant-derived PA appears. Then, it is considered that the unreacted compatibilizer further reacts with this unreacted surface. In this way, the plant-derived PA bonded to the compatibilizer is sheared, the surface of the unreacted plant-derived PA appears, and the unreacted compatibilizer reacts with this unreacted surface. By repeating this process, it is considered that a smaller reaction product between the plant-derived PA and the compatibilizer can be stably formed without relying on high shear. Furthermore, if the amount of compatibilizer that can be supplied during the above-mentioned process is small, the plant-derived PA to which the compatibilizer is bonded will not easily become small, whereas if the amount of compatibilizer that can be supplied is sufficiently large, the plant-derived PA to which the compatibilizer is bonded will easily become small.
[0062] [3] Molded body The molded article of the present invention is characterized by being made of the above-mentioned thermoplastic resin composition of the present invention. When molding the thermoplastic resin composition, any known molding method can be used. Specific examples include injection molding, extrusion molding (sheet extrusion, profile extrusion), T-die molding, blow molding, injection blow molding, inflation molding, hollow molding, vacuum molding, foam molding, compression molding, press molding, stamping mold molding, transfer molding, insert molding, etc. These may be used alone or in combination of two or more.
[0063] The shape, size, thickness, etc. of the molded body are not particularly limited, and the use thereof is also not particularly limited. For example, the molded body may be a pellet. When the molded body is a pellet, it may be used as a modifier for modifying other resins (for example, improving impact resistance, improving fluidity, etc.). The object to be modified is not limited, but may be, for example, a polyolefin. As the polyolefin, plant-derived PE may be used. In addition, plant-derived polypropylene (plant-derived PP) similar to plant-derived PE may be used. Furthermore, the above-mentioned fossil-derived polyolefin may be used as another component.
[0064] In this modification, the present molded body can be used to utilize dry blending. That is, the present molded body is mixed with pellets of the resin or the like to be modified by dry blending, and then the mixed pellets are molded to obtain a modified molded body (a shaped body other than a simple pellet shape, etc.). In general, in modification, the two are melt-kneaded to obtain a molten kneaded product, which is then pelletized, and the modified pellets obtained are molded to obtain a modified molded body (a shaped body other than a simple pellet shape, etc.). However, when the present molded body (modifier) is used, the above melt-kneading is not required, and modification is possible by dry blending.
[0065] Furthermore, the molded articles are used as various items for vehicles such as automobiles, railroad cars (vehicles in general), aircraft bodies (aircraft bodies in general), ships and hulls (hulls in general), and bicycles (car bodies in general). Among these, automotive products include exterior parts, interior parts, engine parts, electrical parts, etc. Specifically, automotive exterior parts include roof rails, fenders, fender liners, garnishes, bumpers, door panels, roof panels, hood panels, trunk lids, fuel lids, door mirror stays, spoilers, hood louvers, wheel covers, wheel caps, grill apron cover frames, lamp bezels, door handles (pull handles), door moldings, rear finishers, wipers, engine undercovers, floor undercovers, rocker moldings, cowl louvers, cowls (motorcycles), etc.
[0066] Automotive interior parts include trim parts such as door trim base materials (FR, RR, BACK), pockets, armrests, switch bases, decorative panels, ornament panels, EA materials, speaker grilles, and quarter trim base materials; pillar garnishes; cowl side garnishes (cowl side trim); seat parts such as shields, back boards, dynamic dampers, and side airbag peripheral parts; instrument panel parts such as center clusters, registers, center boxes (doors), glove doors, cup holders, and airbag peripheral parts; center consoles; overhead consoles; sun visors; deck boards (luggage boards), undertrays; package trays; high mount stop lamp covers; CRS covers; seat side garnishes; scuff plates; room lamps; assist grips; safety belt parts; register blades; washer levers; window regulator handles; window regulator handle knobs; passing light levers, etc.
[0067] Automobile engine parts include alternator terminals, alternator connectors, IC regulators, potentiometer bases for light dimmers, exhaust gas valves, fuel pipes, cooling pipes, brake pipes, wiper pipes, exhaust pipes, intake pipes, hoses, tubes, air intake nozzle snorkels, intake manifolds, fuel pumps, engine coolant joints, carburetor main bodies, carburetor spacers, exhaust gas sensors, coolant sensors, oil temperature sensors, brake pad wear sensors, throttle position sensors, crankshaft position sensors, air flow meters, brake pad wear sensors, brake pistons, solenoid bobbins, engine oil filters, ignition device cases, and torque control levers.
[0068] Examples of electrical parts for automobiles include battery peripheral parts, thermostats for air conditioners, heating hot air flow control valves, brush holders for radiator motors, water pump impellers, turbine vanes, wiper motor related parts, distributors, starter switches, starter relays, transmission wire harnesses, windshield washer nozzles, air conditioner panel switch boards, coils for fuel-related electromagnetic valves, wire harness connectors, SMJ connectors, PCB connectors, door grommet connectors, various connectors such as fuse connectors, horn terminals, electrical part insulating plates, step motor rotors, lamp sockets, lamp reflectors, lamp housings, cleaner cases, filter cases, power trains, etc.
[0069] Furthermore, the molded article is also used as various products in non-vehicle applications other than the above-mentioned vehicles, such as industrial and industrial materials such as ropes, spunbonds, abrasive brushes, industrial brushes, filters, transport containers, trays, transport dollies, and other general materials; Connectors, coils, sensors, LED lamps, sockets, resistors, relay cases, small switches, coil bobbins, capacitors, variable capacitor cases, optical pickups, oscillators, various terminal boards, transformers, plugs, printed circuit boards, tuners, speakers, microphones, headphones, small motors, small speed change gears, magnetic head bases, power modules, semiconductors, liquid crystal, FDD carriages, FDD chassis, motor brush holders, parabolic antennas, computer-related parts, and other electronic components; Electrical equipment such as generators, motors, transformers, current transformers, voltage regulators, rectifiers, inverters, relays, power contacts, switches, circuit breakers, knife switches, multi-pole rods, electrical component cabinets;
[0070] Housings for industrial robots, housings for nursing care robots, housings for drones (flying objects that fly by remote control, flying objects that fly autonomously), VTR parts, TV parts, irons, hair dryers, rice cooker parts, microwave oven parts, audio parts, audio / LD parts, CD / DVD parts, lighting parts, refrigerator parts, washing machine parts, air conditioner parts, typewriter / word processor parts, office computer parts, PCs, game consoles, tablet devices, mobile phones, smartphones, telephones and related parts, facsimile parts, copier parts, cleaning / washing equipment, motor parts and other home appliances and office products; Optical and precision instruments such as cameras, watches, microscopes, binoculars, telescopes, spectacles, etc.; Food trays, storage boxes, storage trays, attache cases, suitcases, helmets, water bottles, storage cases for bottles, etc., toiletries, writing implements, stationery, book stands, skin care implements, tools, tableware, laundry implements, cleaning implements, clothes hangers, food containers, opening and closing lids (for glass bottles, etc.), and other daily necessities and household items;
[0071] Toys and other entertainment items; Lawnmower housings, covers, power tool housings, covers, various clips, and other general machinery and parts; Tennis racket strings, skis and boards, protectors (baseball, soccer, motor sports), shoes, shoe soles (shoe soles, soles for sports shoes), outdoor and mountain climbing equipment, and other sporting goods; Furniture related items such as wardrobe cases, tables, chairs, shoe boxes, kitchen utensils, toilet utensils, bath utensils, etc.; Interior and exterior walls and roofs, insulation materials, doors and door-related parts, window material-related parts, flooring material-related parts, seismic isolation and vibration control parts, rain shutters, rain gutters, water supply and sewage related parts (lifeline related), parking garages, gas and electricity related parts (lifeline related), civil engineering parts, traffic signals, road signs, pylons, center poles, guardrails (guard wires), construction equipment, and other housing and civil engineering related products; Medical supplies such as mouthpieces, medical devices, and medicine containers; Shoes and other clothing related items, Examples include agricultural, forestry, and fisheries related products such as farm machinery, farming tools, flower pots, fishing gear, aquaculture equipment, and forestry tools. EXAMPLES
[0072] The present invention will now be described in detail with reference to examples. [1]Each raw material component (1) Plant-derived PE The following two types of plant-derived polyethylene were prepared. PE1: HDPE (manufactured by Braskem, product name "SHA7260"), density 0.955g / cm 3 , MFR (230℃ / 2.16kg) 32g / 10min, bio-based carbon content 94% or more PE2: HDPE (manufactured by Braskem, product name "SHC7260"), density 0.953g / cm 3 , MFR (230℃ / 2.16kg) 12g / 10min, bio-based carbon content 94% or more
[0073] (2) Plant-derived PA The following polyamides were prepared as plant-derived PAs. PA: PA11 (Arkema, product name "Rilsan BMN O"), density 1.03g / cm3 , MFR (230℃ / 2.16kg) 32g / 10min, bio-based carbon content 99% or more
[0074] (3) Compatibilizer The following ethylene-1-butene copolymer was prepared as a compatibilizer. Compatibilizer: Maleic anhydride modified EBR (manufactured by Mitsui Chemicals, product name "Tafmer MH7020"), density 0.866g / cm 3 , MFR(230℃ / 2.16kg)1.5g / 10min
[0075] [2] Preparation of molten mixture The plant-derived PA and the compatibilizer were dry-blended, then fed into a twin-screw melt-kneading extruder (Plastic Engineering Research Institute, screw diameter 30 mm, L / D=42), and melt-kneaded at a kneading temperature of 210°C, an extrusion rate of 3.0 kg / hour, and a screw rotation speed of 200 rpm, and pelletized with a pelletizer to obtain pellets of the melt-kneaded product. The MFR (230°C / 2.16 kg) of the resulting melt-kneaded product was 1.5 g / 10 min.
[0076] [3] Preparation of thermoplastic resin composition The molten mixture obtained in [2] above was dry-blended with plant-derived PE, and then fed into a twin-screw melt kneading extruder (Plastic Engineering Research Institute Co., Ltd., screw diameter 30 mm, L / D=42) and mixed under conditions of a kneading temperature of 210°C, an extrusion speed of 3.0 kg / hour, and a screw rotation speed of 200 rpm. The mixture was then passed through a pelletizer to obtain pellets of Experimental Examples 1 to 8.
[0077] [4] Preparation of molded bodies for evaluation (1) Evaluation Molded Articles for Experimental Examples 1 to 8 The thermoplastic resin compositions of Experimental Examples 1 to 8 obtained in [3] above were charged into the hopper of an injection molding machine (100-ton injection molding machine), and molded bodies for physical property measurement were injection molded under injection conditions of a set temperature of 210°C and a mold temperature of 60°C.
[0078] [Table 1]
[0079] [5] Evaluation of evaluation molded bodies (1) Density measurement The density of the thermoplastic resin compositions and each raw material component of Experimental Examples 1 to 8 obtained in [4] above was measured in accordance with ISO 1183. The results are shown in Table 1 and [1]. Test temperature: 23℃ Drying conditions: Vacuum drying at 80℃ for 8 hours or more
[0080] (2) Measurement of MFR The MFR (230°C / 2.16 kg) of the thermoplastic resin compositions of Experimental Examples 1 to 8 obtained in [4] above and each of the raw material components was measured in accordance with ISO 1133. The results are shown in Table 1 and [1]. Test equipment: Melt indexer (Toyo Seiki Seisakusho Co., Ltd., model "F-F01") Test temperature: 230℃ Test load: 2.16kgf Drying conditions: Vacuum drying at 80℃ for 8 hours or more
[0081] (3) Charpy impact strength measurement Using each of the evaluation molded articles of Experimental Examples 1 to 8 obtained in [4] above, Charpy impact strength (test temperature 23° C.) was measured in accordance with ISO 179. The results are shown in Table 1. In the measurement of the Charpy impact strength, a test piece having a notch (type A) was used, and impact was measured at a temperature of 23°C by the edgewise test method.
[0082] (4) Tensile test Tensile tests were carried out in accordance with ISO 527-1 using each of the evaluation molded articles of Experimental Examples 1 to 8 obtained in [4] above. The resulting yield stress, breaking elongation, and elastic modulus are shown in Table 1. Test equipment: Autograph 50kN (manufactured by Shimadzu Corporation, model "AGS-X") Test temperature: 23℃ Specimen shape: ISO multipurpose specimen Tensile speed (elastic modulus measurement): 1 mm / min Tensile speed (strength and elongation measurement): 50 mm / min Drying conditions: Vacuum drying at 23℃ for 24 hours or more
[0083] [6] Morphology The phase structure of each thermoplastic resin composition was observed using each test piece of Experimental Example 6 (see Figs. 1 to 3) and Experimental Example 8 (see Figs. 4 to 6). This phase structure was obtained by observing the treated surface, which was subjected to oxygen plasma etching treatment (oxygen plasma etching treatment at 100 W for 1 minute) and then osmium coating treatment, with a field emission scanning electron microscope (FE-SEM).
[0084] Of the obtained SEM images, an image of the surface of Experimental Example 6 enlarged 5000 times is shown in Figure 1, an image of the surface of Experimental Example 6 enlarged 10000 times is shown in Figure 2, and an image of the surface of Experimental Example 6 enlarged 20000 times is shown in Figure 3. Furthermore, an image of the surface of Experimental Example 8 enlarged 5000 times is shown in Figure 4, an image of the surface of Experimental Example 8 enlarged 10000 times is shown in Figure 5, and an image of the surface of Experimental Example 8 enlarged 20000 times is shown in Figure 6.
[0085] [7] Effects of the embodiment From the results in Table 1, according to Examples 1 to 8, polyethylene and polyamide having a bio-based carbon content of 80% or more are used in an amount of 75% by mass or more relative to 100% by mass of the entire thermoplastic resin composition, and the density is 1.00 g / cm 3 Charpy impact strength is kept to 20~84kJ / m 2 It is possible to obtain a thermoplastic resin composition having such excellent impact resistance. Furthermore, the MFR of this thermoplastic resin composition can be controlled in a wide range of 1.86 to 22.83 g / 10 min, and it is possible to obtain a thermoplastic resin composition having particularly high fluidity of 10 g / 10 min or more. That is, it is possible to obtain a thermoplastic resin composition and a method for producing the same that can achieve both high impact resistance and high fluidity using three components, polyolefin, polyamide, and a compatibilizer, while reducing the environmental load, and also to obtain a molded article using the thermoplastic resin composition.
[0086] 1 to 3, in Experimental Example 6, a phase structure can be obtained in which the plant-derived PA is the continuous phase A, the plant-derived PE is the dispersed phase B, and further, a phase structure having a continuous phase B1 within the dispersed phase and a finely dispersed phase B2 within the dispersed phase B. Furthermore, in Experimental Example 8, a phase structure can be obtained in which the plant-derived PE is the continuous phase A, the plant-derived PA is the dispersed phase B, and further, a phase structure having a continuous phase B1 within the dispersed phase and a finely dispersed phase B2 within the dispersed phase B.
[0087] Incidentally, the present invention is not limited to the above-mentioned specific embodiments, and various modifications can be made within the scope of the present invention according to the purpose and application.
[0088] The above examples are merely illustrative and are not to be construed as limiting the present invention. Although the present invention has been described with reference to exemplary embodiments, it is understood that the words used in describing and illustrating the present invention are descriptive and exemplary, rather than limiting. As detailed herein, changes may be made within the scope of the appended claims without departing from the scope or spirit of the present invention in its form. Although the present invention has been described herein with reference to specific structures, materials and examples, it is not intended that the present invention be limited to the disclosures set forth herein, but rather that the present invention extends to all functionally equivalent structures, methods and uses within the scope of the appended claims. [Explanation of symbols]
[0089] A: continuous phase; B; dispersed phase, B1; continuous phase (continuous phase within dispersed phase B), B2; finely dispersed phase (dispersed phase within dispersed phase B);
Claims
1. A molded article made of a thermoplastic resin composition containing polyethylene, polyamide, and a compatibilizer, the compatibilizer is a modified elastomer having a group reactive with the polyamide, The polyethylene and the polyamide have a bio-based carbon content according to ISO 16620-2 of 80% or more; the polyamide (excluding a melt-kneaded product of 30 to 70 mass % of polyamide (X) containing diamine units containing 70 mol % or more of metaxylylenediamine units and dicarboxylic acid units containing α,ω-linear aliphatic dicarboxylic acid units and 30 to 70 mass % of aliphatic polyamide (Y) (the total of polyamide (X) and polyamide (Y) is 100 mass %), and a polyamide resin constituted by a monomer containing 1,5-diaminopentane and a dicarboxylic acid having 6 to 12 carbon atoms as main components) is one or more of PA11, PA1010, PA1012, PA10T and PA11T, The polyethylene has an MFR (230° C. / 2.16 kg) of 20 g / 10 min or less, the mass ratio of the compatibilizer is 1 to 15 mass% when the total of the polyethylene, the polyamide, and the compatibilizer is 100 mass%, A molded article having a phase structure represented by the following (1), (2) or (3): (1) The polyamide is a continuous phase (A), the polyethylene is a granular dispersed phase (B), and the dispersed phase (B) is a continuous phase (B) containing the polyethylene. 1 ) and the continuous phase in the dispersed phase (B 1 ) dispersed in the dispersed phase (B 2 ) and a phase structure having (2) The polyethylene is a continuous phase (A), and the polyamide is a particulate dispersed phase (B), and the dispersed phase (B) is a continuous phase (B) containing the polyamide. 1 ) and the continuous phase in the dispersed phase (B 1 ) dispersed in the dispersed phase (B 2 ) and a phase structure having (3) A bicontinuous structure in which the phase structures of (1) and (2) are mixed.
2. The molded article according to claim 1, wherein, when the mass percentage of the polyethylene is RPE mass% and the mass percentage of the polyamide is RPA mass%, RPA>RPE and RPE is 24 to 45 mass%.
3. The molded article according to claim 1, wherein, when the mass percentage of the polyethylene is RPE mass% and the mass percentage of the polyamide is RPA mass%, RPA < RPE, and RPE is 47 to 65 mass%.
4. A molded body described in any one of claims 1 to 3, wherein the MFR (230°C / 2.16 kg) of the thermoplastic resin composition is 3 g / 10 min or more.
5. 5. The molded article according to claim 1, wherein the compatibilizer has a main skeleton of a copolymer chain derived from ethylene and an α-olefin other than ethylene, and the reactive group is an acid-modified group.
6. A method for producing the molded body according to any one of claims 1 to 4, comprising the steps of: A method for producing a molded article, comprising: a melt-kneading step of melt-kneading a melt-kneaded mixture of the polyamide and the compatibilizer, and the polyethylene.
Citation Information
Patent Citations
Polyamide resin composition and molded product made therefrom
JP2010070701A
Fuel tank
JP2011132336A
Modifier and method for using the same, method for producing modifier, and carrier for additive
JP2018154843A
Insulated wire and cable
JP2019160811A
Gas barrier laminate, packaging material laminate and packaging material
JP2020040258A