Glass composition and sealing material

A glass composition with specific oxide ratios allows for improved airtight reliability and heat resistance in coaxial connectors by maintaining fluidity at lower temperatures, addressing the low fluidity issue of conventional sealing materials.

JP7577959B2Active Publication Date: 2024-11-06NIPPON ELECTRIC GLASS CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020166642
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-01
Publication Date
2024-11-06
Estimated Expiration
2040-10-01

AI Technical Summary

Technical Problem

Conventional sealing materials exhibit low fluidity at temperatures below 900°C, making it difficult to ensure airtight reliability when high-springiness metals like phosphor bronze, brass, or beryllium copper are used for metal pins in coaxial connectors, which are necessary for improved signal transmission efficiency.

Method used

A glass composition containing TeO2 40~85%, MoO3 0~20%, Li2O+Na2O+K2O 1~20%, MgO+CaO+SrO+BaO 1~20%, and MnO+Cr2O3+Fe2O3+Co3O4 0.1~8% is used, allowing the working point to be lowered to 900°C or lower, ensuring good flow and adhesion with high-springiness metal pins.

Benefits of technology

The new glass composition ensures airtight reliability and heat resistance by maintaining fluidity at lower temperatures, enhancing the sealing performance of coaxial connector terminals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577959000003
    Figure 0007577959000003
  • Figure 0007577959000001
    Figure 0007577959000001
  • Figure 0007577959000002
    Figure 0007577959000002
Patent Text Reader

Abstract

To provide a glass composition and a sealing material capable of satisfactorily flowing at a temperature of 900°C or lower, thereby improving the reliability of airtightness of coaxial connector terminals for communication and the like.SOLUTION: The inventive glass composition contains, in mol% in terms of oxides, TeO2 40-85%, MoO3 0-20%, Li2O+Na2O+K2O 1-20%, MgO+CaO+SrO+BaO 1-20%, and MnO+Cr2O3+Fe2O3+Co3O4 0.1-8%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a glass composition and a sealing material, and more particularly to a glass composition and a sealing material suitable for sealing coaxial connector terminals used for communication applications and the like. [Background technology]

[0002] Coaxial connector terminals for communication applications are manufactured by sealing a metal shell and a metal pin with an insulator such as resin or glass to maintain the insulation between the outer shell and the central conductor. In particular, for products that require high reliability and heat resistance, sealing materials containing glass powder as an insulator are used.

[0003] The sealing material is produced and used as follows. First, glass raw material is melted and molded, and the molded glass is pulverized in a ball mill and passed through a specified sieve to form fine glass powder. Ceramic powder is added to the obtained glass powder as necessary and mixed to form a powder material (sealing material). Next, this powder material is mixed with a binder and granulated to produce granules. After that, the granules are tableted to produce a green compact having a through hole, which is heated from room temperature to decompose and remove the binder and sinter to form a sintered body. Next, a metal pin is inserted into the through hole of the obtained sintered body, and the sintered body is placed in a ring-shaped metal shell, and then placed in an electric furnace, where it is fixed at a temperature higher than the working point in an inert atmosphere, and then cooled to room temperature.

[0004] When the glass powder is heated to above its working point, it has sufficient fluidity. This allows the metal member and the sealing material to be tightly attached without creating an excessive gap between them, improving the airtight reliability of the coaxial connector terminal. Since the working point of the glass powder is generally 900°C or higher, the firing temperature during sealing is generally 900°C or higher. The melting points of the metal shell and the metal pin are generally 1400°C or higher.

[0005] Fig. 1(a) is a conceptual diagram showing a coaxial connector terminal 1, which has a metal shell 11, a metal pin 12, and a sealing material 13. Fig. 1(b) is a conceptual diagram showing the state of the metal shell 11, the metal pin 12, and the sealing material 13 before firing for the main part of the coaxial connector terminal 1 in Fig. 1(a), and Fig. 1(c) is a conceptual diagram showing the state of the metal stem 11, the metal pin 12, and the sealing material 13 after firing for the main part of the coaxial connector terminal 1 in Fig. 1(a). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2014-175069 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]

[0007] In recent years, in coaxial connectors for communication, metal pins are required to have high spring properties in order to improve the degree of adhesion when mated and increase the efficiency of signal transmission. In this case, phosphor bronze, brass, beryllium copper, etc. are generally used for the metal pins. The melting points of these metals are usually 900°C or less, and the thermal expansion coefficient is 160 to 190 x 10 -7 / ℃.

[0008] However, conventional sealing materials have low fluidity at temperatures below 900°C, and it is not possible to ensure airtight reliability when using these metals in metal pins. This means that resin must be used as an insulator, making it difficult to ensure heat resistance and airtight reliability.

[0009] The present invention has been made in consideration of the above circumstances, and its technical object is to provide a glass composition and a sealing material that can flow well at a temperature of 900° C. or less, thereby improving the airtight reliability of communication coaxial connector terminals and the like. [Means for solving the problem]

[0010] The inventors have found that the above technical problems can be solved by using a glass mainly composed of TeO2 after repeated experiments, and propose it as the present invention. The glass composition of the present invention is characterized by containing, as a glass composition, 40-85% TeO2, 0-20% MoO3, 1-20% Li2O+Na2O+K2O, 1-20% MgO+CaO+SrO+BaO, and 0.1-8% MnO+Cr2O3+Fe2O3+Co3O4, in mole percent based on the following oxides. In this way, the working point can be lowered to 900°C or less, particularly 850°C or less. As a result, the glass composition can be suitably used as a sealing material for metal members having high spring properties. Here, "based on the following oxides" refers to the expression in terms of the oxides shown, regardless of the valence of the components, in the case of polyvalent oxides. For example, iron oxide includes FeO and Fe2O3, but in the present invention, it is expressed in terms of "Fe2O3" regardless of the valence of Fe. "Li2O+Na2O+K2O" refers to the combined amount of Li2O, Na2O, and K2O. "MgO+CaO+SrO+BaO" refers to the combined amount of MgO, CaO, SrO, and BaO. "MnO+Cr2O3+Fe2O3+Co3O4" refers to the combined amount of MnO, Cr2O3, Fe2O3, and Co3O4.

[0011] The sealing material of the present invention is a sealing material containing glass powder made of the above-mentioned glass composition and ceramic powder, and is characterized in that the glass powder content is 60 to 100 mass % and the ceramic powder content is 0 to 40 mass %.

[0012] In addition, the sealing material of the present invention preferably does not substantially contain ceramic powder. Here, "substantially does not contain ceramic powder" means that the content of ceramic powder in the sealing material is less than 0.1 mass%.

[0013] Moreover, the sealing material of the present invention is preferably in a granular shape.

[0014] The sealing material of the present invention is preferably a sintered body. [Brief description of the drawings]

[0015] [Figure 1] 1A is a conceptual diagram showing a coaxial connector terminal, FIG. 1B is a conceptual diagram showing the state of a metal shell, a metal pin, and a sealing material before firing, and FIG. 1C is a conceptual diagram showing the state of the metal shell, the metal pin, and the sealing material after firing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The glass composition of the present invention contains, as a glass composition, in mole percent based on the following oxides, TeO2 40-85%, MoO3 0-20%, Li2O+Na2O+K2O 1-20%, MgO+CaO+SrO+BaO 1-20%, and MnO+Cr2O3+Fe2O3+Co3O4 0.1-8%. The reasons for limiting the content of each component as described above are explained below. In the description of the content of each component, the % indication refers to mol%.

[0017] TeO2 is a main component for forming a glass skeleton, and its content is 40 to 85%, preferably 55 to 80%, and more preferably 60 to 75%. If the content of TeO2 is small, the working point may become too high. On the other hand, if the content of TeO2 is large, it becomes difficult to maintain the stability of the glass.

[0018] MoO3 is a component that stabilizes glass, and its content is 0 to 20%, preferably 6 to 15%, and more preferably 8 to 12%. If the MoO3 content is too high, vitrification becomes difficult during melting.

[0019] Alkali metal oxides (Li2O, Na2O, K2O) are components that increase melting property and decrease the bonding temperature. The content of Li2O+Na2O+K2O is 1-20%, preferably 2-17%, more preferably 3-13%. The content of Li2O is preferably 0-10%, more preferably 0.1-8%, and even more preferably 1-5%. The content of Na2O is preferably 0-10%, more preferably 0.1-8%, and even more preferably 1-5%. The content of K2O is preferably 0-10%, more preferably 0.1-8%, and even more preferably 1-5%. When the content of alkali metal oxides is decreased, melting property decreases, and the bonding temperature increases, and stress tends to remain between the metal member and the material during sealing. On the other hand, when the content of alkali metal oxides is increased, water resistance tends to decrease.

[0020] Alkaline earth metal oxides (MgO, CaO, SrO, BaO) are components that stabilize glass, and the total content thereof is 1 to 20%, preferably 3 to 15%, and particularly preferably 5 to 12%. The content of MgO is preferably 0 to 10%, more preferably 0 to 5%, and even more preferably 0 to 2%. The content of CaO is preferably 0 to 12%, more preferably 1 to 9%, and even more preferably 3 to 7%. The content of SrO is preferably 0 to 10%, more preferably 0 to 5%, and even more preferably 0 to 2%. The content of BaO is preferably 0 to 12%, more preferably 0.1 to 7%, and even more preferably 1 to 5%. When the content of alkaline earth metal oxides is low, the glass structure becomes unstable and it becomes difficult to melt the glass. On the other hand, when the content of alkaline earth metal oxides is high, it becomes difficult to vitrify during melting.

[0021] MnO, Cr2O3, Fe2O3 and Co2O3 are components that enhance the adhesion between glass and metal members. The content of MnO+Cr2O3+Fe2O3+Co3O4 is 0.1-8%, preferably 0.3-7%, more preferably 0.5-6%, and even more preferably 1.5-5%. The content of MnO is preferably 0-7%, more preferably 0-5%, and even more preferably 0.1-3%. The content of Cr2O3 is preferably 0-7%, more preferably 0-5%, and even more preferably 0.1-3%. The content of Fe2O3 is preferably 0-7%, more preferably 0-5%, and even more preferably 0.1-3%. The content of Co3O4 is preferably 0-7%, more preferably 0-5%, and even more preferably 0.1-3%. If the content of these components is low, the adhesion between glass and metal members is insufficient, and the airtight reliability of coaxial connector terminals and the like is easily reduced. On the other hand, if the content of these components is too high, there is a risk of devitrification particles occurring in the glass.

[0022] The sealing material of the present invention is a sealing material containing glass powder made of the above glass composition and ceramic powder, and the content of the glass powder is preferably 60 to 100 mass%, and the content of the ceramic powder is preferably 0 to 40 mass%, more preferably 80 to 100 mass%, and the content of the ceramic powder is more preferably 0 to 20 mass%, and even more preferably 95 to 100 mass%, and the content of the ceramic powder is still more preferably 0 to 5 mass%, and it is particularly preferable that the content of the glass powder is more than 99.9 to 100 mass%, and the content of the ceramic powder is 0 to less than 0.1 mass%, that is, the sealing material is substantially free of ceramic powder. If the amount of glass powder is small, the sealing material becomes difficult to flow during firing.

[0023] As the ceramic powder, various materials can be used, but from the viewpoint of increasing the expansion of the sealing material, any of cordierite, cristobalite, tridymite, and calcium fluoride is preferable.

[0024] In the sealing material of the present invention, the thermal expansion coefficient in the temperature range of 30° C. to 380° C. is preferably 150×10 -7 ~200×10-7 / °C, more preferably 160×10 -7 ~190×10 -7 / °C, and more preferably 165×10 -7 ~185×10 -7 / °C. If the thermal expansion coefficient is too high, the sealing material will not be sufficiently compressed by the metal shell after the coaxial connector terminal is fabricated, making it difficult to maintain the sealing strength. On the other hand, if the thermal expansion coefficient is too low, the sealing material will be excessively pulled by the metal pin after the coaxial connector terminal is fabricated, making it easy for cracks to occur in the sealing material at the interface with the metal pin. The "thermal expansion coefficient" refers to the average linear thermal expansion coefficient measured using a push rod type thermal expansion coefficient measuring device (TMA).

[0025] In the sealing material of the present invention, the working temperature is preferably 900° C. or less, more preferably 850° C. or less, even more preferably 820° C. or less, and particularly preferably 800° C. or less. If the working temperature is too high, the fluidity cannot be ensured unless sealing is performed at a temperature above the melting point of the metal member having high spring properties, and the airtight reliability of the coaxial connector terminal is likely to decrease. Note that the "working temperature" is defined as the temperature at which the high-temperature viscosity is 1×10 7.6 This refers to the temperature at which the temperature becomes poise.

[0026] The sealing material of the present invention is preferably in the form of granules, which makes it possible to easily produce a powder compact of a predetermined shape, particularly a powder compact having a through hole for passing a metal pin, by tableting.

[0027] The sealing material of the present invention is preferably a sintered body, which can prevent chipping of the sealing material when the metal pin is inserted and then housed in the metal shell.

[0028] The sintered density of the sintered body is preferably 82% or more, 85% or more, 88% or more, 92% or more, particularly 95 to 99%. The sealing density of the sintered body reflects the proportion of bubbles in the sintered body. The smaller the sintered density, the greater the proportion of bubbles in the sintered body, and the more likely sealing defects are to occur. Here, the "sintered density" refers to a value calculated by the formula {(density of the sintered body) / (density of glass bulk without bubbles)}×100. EXAMPLES

[0029] The present invention will be described below based on examples. Note that the following examples are merely illustrative and the present invention is not limited to the following examples.

[0030] Table 1 shows examples of the present invention (samples Nos. 1 to 3) and comparative examples (samples Nos. 4 and 5).

[0031] [Table 1]

[0032] First, a glass batch prepared by mixing glass raw materials to obtain the glass composition shown in the table was placed in a platinum crucible and melted at 900°C for 2 hours. When melting the glass batch, a platinum stirrer was used to stir and homogenize the mixture. The molten glass was then poured onto a carbon plate and formed into a film or plate. The plate samples were gradually cooled from a temperature about 20°C higher than the annealing point to room temperature at a rate of 3°C / min.

[0033] The thermal expansion coefficient is an average linear thermal expansion coefficient measured in a temperature range of 30 to 380° C. using a push rod type thermal expansion coefficient measuring apparatus (TMA).

[0034] The working temperature was calculated from the glass viscosity measured by the platinum ball pulling method using a plate-shaped sample. 7.6 This is the temperature at which the temperature becomes poise.

[0035] Next, the film-like glass sample was divided into 10 pieces of glass having an average particle size D 50The glass powder was obtained by crushing and classifying the glass into particles of 20 to 30 μm. If necessary, ceramic powder (cordierite was used in sample No. 3) was added in the proportions shown in the table to obtain a composite powder.

[0036] The adhesion was evaluated by molding the obtained powder sample into a pressed powder into a button shape, placing it on a brass plate and sintering it at the working temperature for 15 minutes, and then cooling it to room temperature. If the obtained sintered body could not be peeled off with the force of fingers, it was marked as "O" and if it could be peeled off, it was marked as "X".

[0037] As is clear from Table 1, for samples Nos. 1 to 3, the working temperature was 819°C or less, and the adhesion was also evaluated as good. Therefore, it is considered that samples Nos. 1 to 3 can provide good airtight reliability when used to seal coaxial connector terminals. On the other hand, the working temperature for sample No. 4 was 868°C. For sample No. 5, devitrification was observed in the sintered body during the adhesion evaluation. Therefore, it is considered that samples Nos. 4 and 5 cannot provide good airtight reliability when used to seal coaxial connector terminals. EXAMPLES

[0038] Ceramic powder (cordierite used) was added to the glass powder of sample No. 1 in the ratio shown in the table to obtain composite powder of sample No. 6. The thermal expansion coefficient, working temperature, and adhesion of sample No. 6 were evaluated as described above. The results are shown in Table 2.

[0039] [Table 2]

[0040] As is clear from Table 2, Sample No. 1 was evaluated as having good adhesion. On the other hand, the sintered body of Sample No. 6 did not flow in the adhesion evaluation. Therefore, it is considered that Sample No. 6 does not provide good airtight reliability when used for sealing coaxial connector terminals. [Explanation of symbols]

[0041] 1 Coaxial connector terminal 11 Metal stem 12 Metal Pins 13 Sealing material

Claims

1. The glass composition is, in mole percent based on the following oxides, TeO 2 40-85%, MoO 3 0-20%, Li 2 O+Na 2 O+K 2 O 1-20%, MgO+CaO+SrO+BaO 1-20%, MnO+Cr 2 O 3 +Fe 2 O 3 +Co 3 O 4 A sealing material containing a glass powder made of a glass composition containing 0.1 to 8% of a ceramic powder, The content of the glass powder is 60 to 100% by mass, and the content of the ceramic powder is 0 to 40% by mass, A sealing material characterized by being used for sealing coaxial connector terminals for communication.

2. The sealing material according to claim 1 , which is substantially free of ceramic powder.

3. 3. The sealing material according to claim 1, which is in a granular form.

4. 3. The sealing material according to claim 1, which is a sintered body.

Citation Information

Patent Citations

  • Airtight terminal

    JP2014175069A

  • Lead-free glass composition for sealing stainless steel-made vacuum double container

    JP2019001692A

  • Sealing material

    JP2019031403A

  • Joint material

    JP2019123637A

  • Non-lead glass composition and glass composite material, glass paste and sealed structure each including the non-lead glass composition

    JP2019206458A