Towpreg and fiber reinforced composites

The tow preg with controlled epoxy resin composition and interlaminar friction coefficient addresses slippage and tight winding issues, ensuring stable unwinding and reduced gaps for improved filament wound product quality.

JP7577965B2Active Publication Date: 2024-11-06TORAY INDUSTRIES INC
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020173752
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-15
Publication Date
2024-11-06
Estimated Expiration
2040-10-15

AI Technical Summary

Technical Problem

Existing tow preg manufacturing methods face issues with bobbin slippage, tight winding during unwinding, and poor shape stability, leading to gaps and voids in filament wound products, complicating the process and reducing product quality.

Method used

A tow preg impregnated with an epoxy resin composition having specific viscosity and resin content, with a controlled interlaminar friction coefficient, ensuring stable unwinding and expandability to minimize gaps and improve handling.

Benefits of technology

The solution provides stable unwinding, reduces gaps, and enhances the quality of filament wound products by preventing slippage and tight winding, resulting in high-quality molded products with fewer voids.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577965000008
    Figure 0007577965000008
  • Figure 0007577965000009
    Figure 0007577965000009
  • Figure 0007577965000010
    Figure 0007577965000010
Patent Text Reader

Abstract

To provide a tow preg which simultaneously satisfies prevention of slip-down from a paper tube when a bobbin is held, less winding tightness in unwinding and good shape stability of the bobbin, good widening property of a tow in filament winding molding, and prevention of formation of a gap.SOLUTION: A tow preg is obtained by impregnating a carbon fiber bundle having fineness of 30-4,000 g / 1,000 m with an epoxy resin composition having viscosity at 25°C of 5-150 Pa s, in which a resin percentage content (Rc) of the tow preg is 20-40 mass%, when the surface of the tow preg is observed at the magnification of 200 times using an optical microscope, a ratio (coverage) of an area in a part coated with a solid component that is not dissolved in an epoxy resin to a visual field area is 0% or more and less than 2.5%, and an interlayer friction coefficient measured when the tow preg is formed by laminating three layers in the same direction and the central tow preg is pulled out and measured under conditions of a temperature of 25°C, 50% RH humidity, speed of 1 mm / min and a vertical load of 20.6 N is 0.04 or more and less than 0.10.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a towpreg that is particularly suitable for use in manufacturing hollow containers and cylinders made of fiber-reinforced composite materials, and more particularly to a towpreg that is easy to handle and capable of producing high-quality molded products with few voids. [Background technology]

[0002] Fiber-reinforced composite materials using reinforcing fibers such as carbon fiber and glass fiber are used in many fields such as aerospace, automobiles, railway vehicles, ships, civil engineering and construction, and sporting goods because of their excellent light weight. In particular, fiber-reinforced composite materials using continuous reinforcing fibers are used in applications that require high performance, and carbon fiber, which has excellent specific strength and specific elastic modulus, is often used as the reinforcing fiber, and epoxy resin, which has excellent adhesion to carbon fiber, is often used as the thermosetting resin.

[0003] In response to the recent expansion of applications of carbon fiber, molding methods are also expanding. Among these, filament winding is a method that is preferably used for manufacturing hollow containers and cylinders such as pressure vessels. Instead of the conventional wet method in which a reinforced fiber bundle unwound from a bobbin is immersed in a liquid thermosetting resin and then wound up on a mold, a method in which a narrow belt-shaped intermediate base material called a tow prepreg, yarn prepreg, or strand prepreg (hereinafter referred to as a tow prepreg) in which a reinforced fiber bundle is pre-impregnated with a thermosetting resin is supplied and wound up on a mold has been attracting attention from the viewpoints of productivity and quality.

[0004] Towpregs are usually supplied in the form of bobbins, with hundreds to thousands of meters wound around a paper tube, and are unwound at high speed during the molding process of fiber-reinforced composite materials. In this case, it is required that the bobbin does not easily slip off the paper tube when it is erected, that there is little tightening during unwinding, and that the shape stability of the bobbin is good. In addition, it is also required that the tow has good width expansion during filament winding molding and that there is little gap formation. In order to provide towpregs with stable quality, it is also required that the epoxy resin does not deteriorate much when stored for a long period of time before being impregnated into the tow.

[0005] Furthermore, in pressure vessel applications for which towpregs are suitable, they are required to have sufficient heat resistance against the temperature rise that occurs when high-pressure gas is rapidly filled, and to have little performance degradation due to repeated use over a long period of time, etc. In order to satisfy these performance requirements, it is useful to improve the toughness and heat resistance (glass transition temperature) of the matrix resin.

[0006] Patent Document 1 discloses a method for manufacturing a composite container in which the towpreg is heated before being wound around a liner to reduce the viscosity of the matrix resin and suppress void formation, and then cooled after the winding to increase the viscosity of the matrix resin and suppress tow slippage. However, this method is not economically satisfactory because it requires the installation of a heating and cooling mechanism in the manufacturing equipment for winding.

[0007] Patent Document 2 discloses a technology for strengthening tack and preventing slippage of the tow during filament winding molding by applying a high-viscosity, hardener-free second resin to the surface layer of a towpreg impregnated with a low-viscosity first resin that contains a hardener. However, since the resin must be impregnated in two separate steps, this complicates the towpreg manufacturing process and is not economically satisfactory. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2010-234658 A [Patent Document 2] JP 2015-98556 A Summary of the Invention [Problem to be solved by the invention]

[0009] In view of the above background, an object of the present invention is to provide a towpreg that simultaneously satisfies the following requirements: the bobbin is less likely to slip off the paper tube when it is stood upright, there is less tightening of the winding when unwinding, resulting in good shape stability of the bobbin, and the tow has good width expandability during filament winding molding, making it less likely to produce gaps. [Means for solving the problem]

[0010] The present invention employs the following means to solve the above problems. That is, the towpreg of the present invention is a towpreg obtained by impregnating a carbon fiber bundle having a fineness of 30 to 4000 g / 1000 m with an epoxy resin composition having a viscosity of 5 to 150 Pa s at 25°C, the resin content of the towpreg is 20 to 40 mass%, and when the surface of the towpreg is observed with an optical microscope at a magnification of 200 times, the ratio of the area of ​​the part covered by solid components not dissolved in the epoxy resin to the field of view area (coverage rate) is 0% or more and less than 2.5%, and further, the towpreg is laminated in three layers in the same direction, and the interlaminar friction coefficient measured by pulling out the central towpreg under conditions of a temperature of 25°C, a humidity of 50% RH, a speed of 1 mm / min, and a normal load of 20.6 N is 0.04 or more and less than 0.10. Effect of the Invention

[0011] The towpreg of the present invention satisfies the following requirements at once: the bobbin is less likely to slip off the paper tube when it is stood up; there is less tightening during unwinding, resulting in good shape stability of the bobbin; and the tow has good width expandability during filament winding molding, resulting in less gaps. Therefore, it has excellent handleability when producing hollow containers such as pressure vessels and cylinders using the filament winding method, and it is possible to obtain high-quality molded products with few voids. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1A is a cross-sectional view showing the method for measuring the interlayer friction coefficient of the present invention, and FIG. 1B is a plan view showing the method for measuring the interlayer friction coefficient of the present invention. [Diagram 2] FIG. 1 is a schematic diagram illustrating a phenomenon in which a towpreg bobbin slips off a paper tube. [Diagram 3] FIG. 1 is a schematic diagram illustrating a phenomenon of tightening of a winding when a towpreg bobbin is unwound. [Figure 4] 1 is an example of an image of the surface of a towpreg taken with an optical microscope at 200x magnification. [Diagram 5] FIG. 2 is a front view showing a method for measuring the tightening speed of the present invention. [Figure 6] FIG. 1A is a front view showing the method for measuring the width expansion ratio of the present invention, and FIG. 1B is a side view showing the method for measuring the width expansion ratio of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention has the following configuration: That is, the towpreg of the present invention is a towpreg obtained by impregnating a carbon fiber bundle having a fineness of 30 to 4000 g / 1000 m with an epoxy resin composition having a viscosity of 5 to 150 Pa s at 25°C, the towpreg has a resin content (Rc) of 20 to 40 mass%, and when the surface of the towpreg is observed with an optical microscope at a magnification of 200 times, the ratio of the area of ​​the part covered by solid components not dissolved in the epoxy resin to the area of ​​the field of view (coverage rate) is 0% or more and less than 2.5%, and further, the towpreg is laminated in three layers in the same direction, and the interlaminar friction coefficient measured by pulling out the central towpreg under conditions of a temperature of 25°C, a humidity of 50% RH, a speed of 1 mm / min, and a normal load of 20.6 N is 0.04 or more and less than 0.10.

[0014] The interlayer friction coefficient in the present invention refers to the static friction coefficient in the friction phenomenon that occurs between layers of towpregs in a towpreg laminate in which towpregs are stacked. Here, the interlayer refers to the boundary region where the surfaces of the towpregs are in contact with each other, and in the present invention, the term interlayer is used even when it is not clearly observed with a microscope or the like.

[0015] In the present invention, the interlaminar friction coefficient is measured by the following method. First, as shown in FIG. 1, one towpreg 3 is sandwiched between two towpregs 4 with the same fiber direction, and a load of 20.6 N is applied vertically to the stacked towpregs using a pressure plate 1 (hereinafter referred to as vertical load). Next, the maximum load obtained when the sandwiched towpreg 3 is pulled out at a temperature of 25° C., a humidity of 50% RH, and a speed of 1 mm / min is read. The static friction coefficient obtained by dividing the read maximum load by twice the vertical load applied to the contact portion between the towpreg 3 and the towpreg 4 is defined as the interlaminar friction coefficient in the present invention. The reason for using a value twice the vertical load is that there are two surfaces of the towpreg that receive frictional resistance. More detailed test methods will be described in the examples below.

[0016] The interlaminar friction coefficient of the towpreg of the present invention measured by this method is 0.04 or more and less than 0.10. By satisfying this range, it is possible to obtain a towpreg that simultaneously satisfies the following: when the bobbin is erected, it is difficult for the bobbin to slip off the paper tube, there is little tightening during unwinding, the shape stability of the bobbin is good, and the tow has good width expansion during filament winding molding, and gaps are unlikely to occur. In this way, by using a towpreg in which the occurrence of defects is suppressed, it is possible to improve the yield and the quality of the molded product.

[0017] Here, slipping off the paper tube when the bobbin is set up refers to the phenomenon in which the towpreg slips off and the bobbin shape collapses when the towpreg, which is a bobbin-shaped towpreg wound around a paper tube of several hundred to several thousand meters, is placed and left to rest with the longitudinal direction of the paper tube perpendicular to the surface of the workbench. A schematic diagram showing the slipping off phenomenon is shown in Figure 2. Once the slipping off phenomenon occurs, the yarn comes off at the end of the bobbin where the shape has collapsed, causing the tow to become unwindable.

[0018] Tightening during unwinding is a phenomenon in which when a bobbin-shaped towpreg, which is made by winding hundreds to thousands of meters of towpreg around a paper tube, is attached to the creel of a filament winding machine and tension is applied to form the towpreg, the bobbin is squeezed and deformed by the applied tension, resulting in unevenness on the bobbin surface and bulging of the bobbin end. A schematic diagram showing the tight winding phenomenon is shown in Figure 3. When the tight winding phenomenon occurs, the yarn comes off at the bulging bobbin end, causing the towpreg to become unwindable.

[0019] In addition, the tow widening during filament winding is a phenomenon in which the width of the towpreg widens due to the pressure when it is wound around the liner of a pressure vessel or a mandrel used to form a cylinder. If the towpreg does not have sufficient widening properties, voids will occur in the molded product, especially near the mouthpiece when manufacturing a pressure vessel, which will reduce the burst strength.

[0020] The interlayer friction coefficient of the towpreg of the present invention can be adjusted to an appropriate range by the viscosity of the epoxy resin composition described below, the resin content (Rc) of the towpreg, the proportion of the area covered by solid components that are not dissolved in the epoxy resin (coverage rate), and the like.

[0021] The viscosity of the epoxy resin composition used in the towpreg of the present invention at 25°C must be 5 to 150 Pa·s, preferably 5 to 100 Pa·s, and more preferably 5 to 50 Pa·s. By setting the viscosity of the epoxy resin composition in this range, the interlaminar friction coefficient can be adjusted to an appropriate range. In the present invention, the lower the viscosity of the epoxy resin composition, the lower the resin content (Rc) of the towpreg can be and the higher the carbon fiber content, which can contribute to weight reduction of the fiber reinforced composite material. In addition, the lower the viscosity of the epoxy resin composition, the simpler the mechanism for adjusting the viscosity by heating and controlling the temperature of the epoxy resin composition in the towpreg manufacturing process can be, which is preferable from the viewpoint of suppressing equipment costs and energy consumption.

[0022] The epoxy resin composition used in the towpreg of the present invention has a complex shear viscosity (η 0.1 The complex shear viscosity (η 10 ) to the ratio (η 0.1 / η 10 ) is preferably 1.5 or more, and more preferably 3.0 or more. 0.1 / η 10 By satisfying this range, it is possible to suppress the bobbin from slipping off the paper tube when it is erected, and therefore it is possible to achieve a good balance between the effect of suppressing winding tightness during unwinding and the spreadability of the tow during filament winding formation. 0.1 / η 10 There is no particular upper limit to η, but it is usually 300 or less. 0.1 / η 10 Means for controlling the viscosity within this range include the addition of a viscosity modifier such as a thermoplastic resin or a thixotropic agent.

[0023] Specific examples of carbon fiber bundles used in the towpreg of the present invention include acrylic, pitch and rayon carbon fiber bundles, and acrylic carbon fiber bundles having particularly high tensile strength are preferably used.

[0024] The carbon fiber bundles used in the towpreg of the present invention must have a fineness of 30 to 4000 g / 1000 m, and typically have 1,000 to 70,000 filaments each having a diameter of 3 to 100 μm. By setting the fineness of the carbon fiber bundles within this range, it is possible to obtain a towpreg that is easy to handle as a belt-shaped intermediate substrate and is uniformly impregnated with the epoxy resin composition all the way to the inside.

[0025] In addition, the carbon fiber bundle used in the towpreg of the present invention preferably has an arithmetic mean roughness (Ra) of the single fiber surface of the carbon fiber of 1 to 20 nm. By setting the arithmetic mean roughness (Ra) of the single fiber surface of the carbon fiber in this range, it becomes easy to adjust the interlaminar friction coefficient to an appropriate range. Here, the arithmetic mean roughness (Ra) of the single fiber surface is an index of the unevenness of the carbon fiber surface, and is the arithmetic mean roughness (Ra) calculated from an image of a three-dimensional surface shape of 600 nm x 600 nm measured by an atomic force microscope (AFM), with the roundness of the fiber approximated by a three-dimensional curved surface as the average line.

[0026] The resin content (Rc) of the towpreg of the present invention must be 20-40% by mass, preferably 20-36% by mass, and more preferably 20-30% by mass. Here, the resin content (Rc) of the towpreg is the mass ratio of the epoxy resin composition to the mass of the towpreg. By setting Rc in this range, the interlaminar friction coefficient can be adjusted to an appropriate range. In addition, when Rc is 20% by mass or more, it is possible to suppress the occurrence of defects such as unimpregnated parts and voids inside the obtained fiber reinforced composite material, and when it is 40% by mass or less, it is possible to suppress the exudation of the resin composition from the bobbin of the towpreg and the scattering of the resin composition in the filament winding molding process. The smaller Rc is, the higher the carbon fiber content can be, which contributes to weight reduction of the fiber reinforced composite material, and is therefore preferable. Rc can be changed by controlling the mass of the epoxy resin composition impregnated into the carbon fiber bundle.

[0027] When the surface of the towpreg of the present invention is observed using an optical microscope at a magnification of 200 times, the ratio of the area of ​​the portion covered by solid components that are not dissolved in the epoxy resin to the area of ​​the field of view (coverage rate) must be equal to or greater than 0% and less than 2.5%.

[0028] In the present invention, the coverage is measured by the following method. First, the surface of the towpreg is imaged with an optical microscope at a magnification of 200 times while irradiating it with a ring light, and a digital image as exemplified in FIG. 4 is obtained. By irradiating it with a ring light, the reflection of light by the epoxy resin is canceled, and an image in which the solid components not dissolved in the epoxy resin are emphasized can be obtained. Next, the obtained digital image is binarized using image analysis software, and the part covered by the solid components not dissolved in the epoxy resin is recognized and its area is calculated. The area of ​​the part covered by the solid components not dissolved in the epoxy resin obtained by the above method is divided by the area actually imaged, and the value expressed as a percentage is taken as the coverage. With this measurement method, it is possible to distinguish a covered part having a size of about 1 μm at the smallest.

[0029] When the coverage of the towpreg of the present invention measured by this method satisfies this range, the interlaminar friction coefficient can be adjusted to an appropriate range.

[0030] The materials constituting the towpreg of the present invention are described below.

[0031] (About epoxy resin) The epoxy resin in the present invention can be used without any particular limitation, and examples thereof include bisphenol type epoxy resins such as bisphenol A type, bisphenol F type, and bisphenol S type, glycidyl amine type epoxy resins such as glycidyl aniline type, diaminodiphenylmethane type, diaminodiphenyl sulfone type, aminophenol type, metaxylenediamine type, and 1,3-bisaminomethylcyclohexane type, aliphatic epoxy resins such as polyethylene glycol type, polypropylene glycol type, butanediol type, neopentyl glycol type, hexanediol type, and cyclohexanedimethanol type, isocyanurate type, hydantoin type, phenol novolac type, orthocresol novolac type, dicyclopentadiene novolac type, biphenyl type, trishydroxyphenylmethane type, and tetraphenylolethane type epoxy resins. These epoxy resins may be used alone or in appropriate mixture.

[0032] Among these epoxy resins, it is preferable to include a glycidylamine type epoxy resin, since it has the effect of imparting stability to the epoxy resin composition and preventing thickening of the epoxy resin composition during the preparation process of the epoxy resin composition, the production process of the towpreg, and the storage period of the towpreg. By preventing thickening of the epoxy resin composition during such processes and periods, the impregnation state of the epoxy resin composition in the towpreg can be improved, and good releasability during molding can be maintained. Examples of glycidylamine type epoxy resins include glycidylaniline type, diaminodiphenylmethane type, diaminodiphenylsulfone type, aminophenol type, metaxylenediamine type, and 1,3-bisaminomethylcyclohexane type. Commercially available examples of such glycidylamine type epoxy resins include GAN (N,N-diglycidylaniline, manufactured by Nippon Kayaku Co., Ltd.), GOT (N,N-diglycidyl-o-toluidine, manufactured by Nippon Kayaku Co., Ltd.), "Sumiepoxy (registered trademark)" ELM-434 (tetraglycidyldiaminodiphenylmethane, manufactured by Sumitomo Chemical Co., Ltd.), "Araldite (registered trademark)" MY721 (tetraglycidyldiaminodiphenylmethane, manufactured by Huntsman Japan Co., Ltd.), and "ARALDITE (registered trademark)" MY0510 (tetraglycidyl-p-aminophenol, manufactured by Huntsman Japan Co., Ltd.).

[0033] Among such glycidylamine type epoxy resins, it is preferable to use tetraglycidyldiaminodiphenylmethane because it has an excellent balance between heat resistance and mechanical properties.

[0034] Furthermore, among tetraglycidyldiaminodiphenylmethanes, it is more preferable to use one having a viscosity of 10 Pa s or less at 50°C, more preferably one having a viscosity of 9.0 Pa s or less, and most preferably one having a viscosity of 6.0 Pa s or less, because this has an excellent effect of improving the pot life of the epoxy resin composition. Commercially available products of such tetraglycidyldiaminodiphenylmethane include "Sumiepoxy (registered trademark)" ELM-434L (viscosity at 50°C: 8.2 Pa·s, manufactured by Sumitomo Chemical Co., Ltd.), "Sumiepoxy (registered trademark)" ELM-434VL (viscosity at 50°C: 5.0 Pa·s, manufactured by Sumitomo Chemical Co., Ltd.), "Araldite (registered trademark)" MY721 (viscosity at 50°C: 3.6 to 5.0 Pa·s, manufactured by Huntsman Japan Co., Ltd.), "jER (registered trademark)" 604 (viscosity at 50°C: 5.0 to 10 Pa·s, manufactured by Mitsubishi Chemical Corporation), and YH-404 (viscosity at 50°C: 3.6 to 5.2 Pa·s, manufactured by Nippon Steel Chemical & Material Co., Ltd.).

[0035] The content of the glycidylamine type epoxy resin is preferably 10 parts by mass or more, more preferably 10 to 80 parts by mass, and even more preferably 20 to 60 parts by mass, in 100 parts by mass of the epoxy resin. By making the content of the glycidylamine type epoxy resin 10 parts by mass or more in 100 parts by mass of the epoxy resin, an effect of preventing thickening of the epoxy resin composition can be obtained. In addition, by making the content of the glycidylamine type epoxy resin 80 parts by mass or less in 100 parts by mass of the epoxy resin, an epoxy resin composition for towpreg that gives a fiber reinforced composite material having an excellent balance between heat resistance and toughness can be obtained.

[0036] (About the hardener) The curing agent in the present invention can be used without any particular limitation, and examples thereof include aromatic amines such as diethyltoluenediamine, diaminodiphenylmethane, 3,3'-diethyl-4,4'-diaminodiphenylmethane, and diaminodiphenylsulfone, as well as dicyandiamide and cyanamide, carboxylic anhydrides such as methyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, and methylnadic anhydride, Lewis acids such as boron trifluoride amine complexes and boron trichloride amine complexes, and imidazoles such as 2-ethyl-4-methylimidazole, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, and 2-phenyl-4-methyl-5-hydroxymethylimidazole. These curing agents may be used alone or in appropriate mixtures.

[0037] Commercially available dicyandiamide products include "jER Cure (registered trademark)" DICY7 and "jER Cure (registered trademark)" DICY15 (both manufactured by Mitsubishi Chemical Corporation).

[0038] Commercially available cyanamide products include "DYHARD (registered trademark)" Fluid 111 (manufactured by AlzChem).

[0039] Commercially available aromatic amines include "jER Cure (registered trademark)" WA (diethyltoluenediamine, manufactured by Mitsubishi Chemical Corporation), "KAYAHARD (registered trademark)" AA (3,3'-diethyl-4,4'-diaminodiphenylmethane, manufactured by Nippon Kayaku Co., Ltd.), and "SEIKACURE (registered trademark)" S (epoxy resin hardener, 4,4'-diaminodiphenyl sulfone, manufactured by Seika Corporation).

[0040] Commercially available carboxylic acid anhydrides include HN-2200 (methyltetrahydrophthalic anhydride, manufactured by Hitachi Chemical Co., Ltd.), "RIKACID (registered trademark)" HH (hexahydrophthalic anhydride, manufactured by New Japan Chemical Co., Ltd.), and "KAYAHARD (registered trademark)" MCD (methylnadic anhydride, manufactured by Nippon Kayaku Co., Ltd.).

[0041] Commercially available boron halide amine complexes include Accelerator DY 9577 (boron trichloride amine complex, manufactured by Huntsman Japan Co., Ltd.) and LEECURE B-550 (boron trifluoride amine complex, manufactured by Leepoxy Plastics).

[0042] Commercially available imidazole products include "Curezol (registered trademark)" 2E4MZ, "Curezol (registered trademark)" 2MZA-PW, "Curezol (registered trademark)" 2MAOK-PW, and "Curezol (registered trademark)" 2P4MHZ-PW (all manufactured by Shikoku Chemical Industry Co., Ltd.).

[0043] Among these curing agents, it is preferable to use a curing agent that is compatible with the epoxy resin at 25°C, from the viewpoint of easily controlling the coverage rate to be small and adjusting the interlaminar friction coefficient to the appropriate range of the present invention. Here, being compatible with the epoxy resin means that the epoxy resin composition to be impregnated into the towpreg does not substantially contain a solid curing agent, and compatibility can be confirmed if no particle components derived from the raw material curing agent are detected by methods such as visual observation or optical microscope observation, and particle size distribution measurement by light scattering method. For this reason, the curing agent is preferably a solid curing agent that can be dissolved in the epoxy resin in a temperature range where a rapid reaction with the epoxy resin does not start and can maintain a compatible state at 25°C, or a liquid curing agent that can maintain a compatible state at 25°C, and more preferably a liquid curing agent.

[0044] Among these curing agents, aromatic amines are particularly preferred because they can provide an epoxy resin composition for towpregs that provides fiber-reinforced composite materials with excellent balance of mechanical properties. Here, aromatic amine is a general term for compounds having an amino group directly bonded to an aromatic ring. Examples of such aromatic amines include compounds having one aromatic ring, such as aminobenzylamine and diethyltoluenediamine, and compounds having two aromatic rings, such as 3,3'-diethyl-4,4'-diaminodiphenylmethane.

[0045] Among these aromatic amines, from the viewpoint of easily controlling the coverage rate to be small and adjusting the interlayer friction coefficient to be within the appropriate range of the present invention, liquid aromatic amines that are liquid at 25° C. are more preferred.

[0046] Moreover, among such liquid aromatic amines that are liquid at 25° C., it is more preferable to contain a compound represented by the following chemical formula (1) since this provides excellent storage stability and heat resistance.

[0047] [ka]

[0048] In the formula, R 1 , R 2 , R 3 is any one of hydrogen, an alkyl group having 1 to 4 carbon atoms, an alkoxy group, and an alkylthio group, and R 1 , R 2 , R 3 may be the same or different.

[0049] Commercially available liquid aromatic amines that are liquid at 25°C and are represented by chemical formula (1) include "jER Cure (registered trademark)" WA (diethyltoluenediamine, manufactured by Mitsubishi Chemical Corporation) and "LONZACURE (registered trademark)" DETDA80 (diethyltoluenediamine, manufactured by Lonza Japan Ltd.).

[0050] The content of such aromatic amine is preferably an amount in which the active hydrogen is 0.7 to 2.0 equivalents relative to the epoxy group of the epoxy resin, and more preferably an amount in the range of 0.7 to 1.8 equivalents. By setting the content of aromatic amine within this range, it is possible to obtain an epoxy resin composition for towpreg that provides a fiber-reinforced composite material with an excellent balance of mechanical properties.

[0051] (Additives) In the present invention, in order to adjust the interlayer friction coefficient and improve the performance such as the mechanical properties of the resin cured product, various additives such as viscosity modifiers such as thermoplastic resins and thixotropic agents, toughening agents such as rubber components, and other additives such as defoamers, stabilizers, flame retardants, and pigments can be contained. The thermoplastic resin is preferably a thermoplastic resin that is soluble in epoxy resin. Examples of the thermoplastic resin that is soluble in epoxy resin include polyvinyl acetal resins such as polyvinyl formal and polyvinyl butyral, polyvinyl alcohol, phenoxy resin, polyamide, polyimide, polyvinyl pyrrolidone, and polysulfone. Examples of the thixotropic agent include organic ones such as amide wax and hydrogenated castor oil, and inorganic ones such as silica, alumina, mixed oxides of aluminum and silicon, titanium oxide, light calcium carbonate, smectite clay minerals (montmorillonite, beidellite, bentonite, hectorite, saponite, etc.), sepiolite, and carbon black. The defoaming agent includes non-silicon polymer-based defoaming agents, silicone-based defoaming agents, and the like.

[0052] The epoxy resin composition used in the towpreg of the present invention contains a toughening agent that is compatible with epoxy resins at 25°C and / or a toughening agent having a particle size of 50 nm to 1 μm, and the toughness value K of the cured product obtained by curing the epoxy resin composition at 150°C for 4 hours is Ic 1.0~3.0MPa m 0.5 By satisfying these conditions, it is possible to increase the toughness of the cured resin without excessively increasing the interlaminar friction coefficient, and to obtain a fiber-reinforced composite material that exhibits little deterioration in performance due to repeated use.

[0053] Here, being compatible with the epoxy resin at 25°C means that the epoxy resin composition to be impregnated into the towpreg does not substantially contain a solid toughening agent component and does not cause coarse liquid-liquid phase separation. Compatibility can be confirmed by mixing the epoxy resin and the toughening agent and visually observing the mixture.

[0054] In the present invention, the particle size of the toughening agent refers to the volume average particle size, and can be measured by a method such as a laser diffraction / scattering method or a dynamic light scattering method.

[0055] Examples of toughening agents compatible with epoxy resins at 25°C include liquid rubbers such as liquid butadiene nitrile rubber, CTBN (carboxyl-terminated butadiene nitrile rubber), ATBN (amino-terminated butadiene nitrile rubber), and butadiene nitrile rubber modified with a carboxyl group in the main chain. These may be used alone or in appropriate mixtures. Commercially available liquid rubbers include "Hypro (registered trademark)" 1300X31, "Hypro (registered trademark)" 1300X13, "Hypro (registered trademark)" 1300X13NA, and "Hypro (registered trademark)" 1300X8 (all manufactured by CVC Thermoset Specialties).

[0056] Examples of toughening agents having a particle size of 50 nm to 1 μm include rubber particles such as acrylic rubber particles, butadiene rubber particles, butadiene-styrene rubber particles, and silicone rubber particles, as well as core-shell rubber particles having a core-shell structure in which rubber particles are coated with a different polymer, etc. These may be used alone or in appropriate mixture.

[0057] Commercially available examples of such core-shell rubber microparticles include "Kane Ace (registered trademark)" MX-125, "Kane Ace (registered trademark)" MX-150, "Kane Ace (registered trademark)" MX-154, "Kane Ace (registered trademark)" MX-257, "Kane Ace (registered trademark)" MX-267, "Kane Ace (registered trademark)" MX-416, "Kane Ace (registered trademark)" MX-451, and "Kane Ace (registered trademark)" MX-EXP (HM5) (all manufactured by Kaneka Corporation).

[0058] The content of the toughening agent is preferably 5 parts by mass or more, and more preferably 5 to 30 parts by mass, per 100 parts by mass of the epoxy resin. By setting the content of the toughening agent within this range, it is possible to increase the toughness of the cured resin without excessively increasing the interlaminar friction coefficient, and to obtain a fiber-reinforced composite material that exhibits little deterioration in performance due to repeated use.

[0059] In the present invention, the glass transition temperature of the cured product obtained by curing the epoxy resin composition at 150° C. for 4 hours is preferably 120 to 160° C., and more preferably 120 to 150° C. By controlling the glass transition temperature of the cured resin product to fall within this range, it is possible to achieve a good balance between the heat resistance and toughness of the cured resin product.

[0060] In the towpreg of the present invention, it is preferable to contain 3 to 5 parts by mass of fumed silica having a primary particle diameter of 5 to 50 nm per 100 parts by mass of epoxy resin. By satisfying this condition, a better balance can be achieved between the effect of suppressing tight winding during unwinding and the spreadability of the tow during filament winding molding. Here, fumed silica is fine particle silica having a primary particle diameter of several nanometers to several tens of nanometers, and is obtained by a combustion pyrolysis method or the like. The primary particle diameter of fumed silica refers to the average diameter of the primary particles, and can be measured by analysis of an image observed by a transmission electron microscope or the like.

[0061] Among such fumed silica, the η 0.1 / η 10Hydrophobic fumed silica that has been subjected to hydrophobic surface treatment is more preferred because it is easy to adjust the surface area of ​​the silica to the preferred range of the present invention. Here, the hydrophobic surface treatment is a treatment in which a hydrophobic substituent such as an alkylsilyl group such as a dimethylsilyl group or a trimethylsilyl group, or dimethylpolysiloxane is bonded to the silanol group on the surface of the fine particle silica. Examples of commercially available products of such fumed silica include "AEROSIL (registered trademark)" R972 (average diameter of primary particles: about 16 nm, manufactured by Nippon Aerosil Co., Ltd.), "AEROSIL (registered trademark)" R812 (average diameter of primary particles: about 7 nm, manufactured by Nippon Aerosil Co., Ltd.), "AEROSIL (registered trademark)" RY200S (average diameter of primary particles: about 16 nm, manufactured by Nippon Aerosil Co., Ltd.), and "AEROSIL (registered trademark)" R805 (average diameter of primary particles: about 12 nm, manufactured by Nippon Aerosil Co., Ltd.).

[0062] In the towpreg of the present invention, it is preferable that the towpreg contains 0.5 to 2 parts by mass of particles that are insoluble in epoxy resin at 25°C and have a primary particle diameter of 0.5 to 150 μm per 100 parts by mass of epoxy resin, and the Rc is 20 to 28%. By satisfying such conditions, a better balance can be achieved between the effect of suppressing winding tightening during unwinding and the spreadability of the tow during filament winding molding. Here, the particles that are insoluble in epoxy resin at 25°C can be used without any particular limitation, and examples thereof include particles of latent curing agents such as dicyandiamide and diaminodiphenylsulfone, organic particles such as thermoplastic resins, and inorganic particles such as silica and carbon. The primary particle diameter of such particles can be measured by a laser diffraction / scattering method or the like.

[0063] In the present invention, the particles that are insoluble in epoxy resin at 25° C. and have a primary particle size of 0.5 to 150 μm preferably contain dicyandiamide. Among the particles, dicyandiamide has the property of dissolving during the curing process and acting as an epoxy resin curing agent, and since solid content is unlikely to remain as defects in the cured product, it is possible to obtain an epoxy resin composition for towpregs that provides a fiber-reinforced composite material with excellent mechanical properties.

[0064] The primary particle diameter of dicyandiamide is preferably 0.5 to 150 μm, more preferably 0.5 to 100 μm, and even more preferably 0.5 to 10 μm. By setting the primary particle diameter in this range, it becomes easy to adjust the interlayer friction coefficient to an appropriate range, and the mechanical properties of the resin cured product can be improved. Here, the primary particle diameter of dicyandiamide refers to the volume-based particle size distribution, and it is preferable that D10 is equal to or greater than the lower limit of the preferred range of the primary particle diameter, and D90 is equal to or less than the upper limit of the preferred range of the primary particle diameter. The primary particle diameter of dicyandiamide can be measured by a laser diffraction / scattering method or the like.

[0065] The epoxy resin composition for use in the towpreg of the present invention can be prepared by various known methods, for example, by kneading using a machine such as a kneader, planetary mixer, mechanical stirrer, dissolver, or three-roll mill, or by hand mixing using a beaker and spatula, etc.

[0066] The towpreg of the present invention can be manufactured by various known methods. That is, the epoxy resin composition used in the towpreg of the present invention can be heated without using an organic solvent to reduce the viscosity, and the reinforcing fiber bundle is immersed in the epoxy resin composition and impregnated therewith; the epoxy resin composition having a low viscosity at room temperature or the epoxy resin composition having a low viscosity by heating is coated on a rotating roll or release paper, and then transferred to one or both sides of the reinforcing fiber bundle, and then the reinforcing fiber bundle is pressed and impregnated by passing through a bending roll or a pressure roll. Since a high-quality towpreg can be manufactured, the manufacturing method of the towpreg of the present invention preferably includes a step of contacting a rotating roll coated with an epoxy resin composition with at least one side of the reinforcing fiber bundle. The towpreg is usually supplied in a bobbin shape wound around a paper tube with hundreds to thousands of meters.

[0067] The fiber-reinforced composite material of the present invention can be obtained by heat curing the towpreg of the present invention. The intermediate substrate of the present invention can be used in many fields such as aerospace, automobiles, railway vehicles, ships, civil engineering and construction, and sporting goods, and can be particularly suitably used for manufacturing hollow containers such as pressure vessels, and cylinders. EXAMPLES

[0068] The present invention will be described in detail below with reference to examples. However, the scope of the present invention is not limited to these examples. The unit "parts" in the composition ratio means parts by mass unless otherwise noted. Furthermore, the measurements of various characteristics (physical properties) were performed in an environment of a temperature of 23°C and a relative humidity of 50%, with the number of measurements being 1, unless otherwise noted.

[0069] <Materials used in the Examples and Comparative Examples> (1) Carbon fiber bundle Carbon fiber manufactured by Toray Industries, Inc. (fineness: 1645g / 1000m, arithmetic mean roughness (Ra): 2.1nm of single fiber surface).

[0070] (2) Epoxy resin "jER (registered trademark)" 807 (liquid bisphenol F type epoxy resin, manufactured by Mitsubishi Chemical Corporation) "jER (registered trademark)" 828 (liquid bisphenol A type epoxy resin, manufactured by Mitsubishi Chemical Corporation) "Sumiepoxy (registered trademark)" ELM-434VL (glycidylamine type epoxy resin, tetraglycidyldiaminodiphenylmethane, manufactured by Sumitomo Chemical Co., Ltd.) "EPICLON (registered trademark)" HP-7200L (dicyclopentadiene type epoxy resin, manufactured by DIC Corporation).

[0071] (3) Hardener "jER Cure (registered trademark)" DICY7 (dicyandiamide (D10: 0.9 μm, D90: 7.4 μm), manufactured by Mitsubishi Chemical Corporation) Accelerator DY 9577 (boron trichloride amine complex, Huntsman Japan Co., Ltd.) "DYHARD®" Fluid 111 (cyanamide, manufactured by AlzChem) "KAYAHARD (registered trademark)" AA (liquid aromatic amine, 3,3'-diethyl-4,4'-diaminodiphenylmethane, liquid at 25°C, manufactured by Nippon Kayaku Co., Ltd.) "jER Cure (registered trademark)" WA (liquid aromatic amine, diethyltoluenediamine, liquid at 25°C, manufactured by Mitsubishi Chemical Corporation).

[0072] (4) Additives "AEROSIL (registered trademark)" RY200S (hydrophobic fumed silica, average primary particle diameter: approx. 16 nm, manufactured by Nippon Aerosil Co., Ltd.) "Kane Ace (registered trademark)" MX-150 (liquid bisphenol A type epoxy resin masterbatch containing 40% polybutadiene rubber type core-shell rubber particles (particle diameter: 100 nm), manufactured by Kaneka Corporation) "Kane Ace (registered trademark)" MX-267 (liquid bisphenol F type epoxy resin masterbatch containing 37% polybutadiene rubber type core-shell rubber particles (particle diameter: 100 nm), manufactured by Kaneka Corporation) "Hypro (registered trademark)" 1300X13 (carboxyl-terminated butadiene nitrile rubber, manufactured by CVC Thermoset Specialties) "Vinylec" K (polyvinyl formal resin, manufactured by JNC Corporation).

[0073] <Method of measuring the arithmetic mean roughness (Ra) of a single fiber surface> The carbon fibers were cut to a length of a few mm and fixed on a substrate (silicon wafer) using silver paste, and then an atomic force microscope (AFM) was used to obtain an image of the three-dimensional surface shape at the center of each single fiber. The atomic force microscope used was a Digital Instruments NanoScope IIIa with a Dimension 3000 stage system. The observation conditions were as follows: Scanning mode: Tapping mode Tip: Silicon cantilever Scanning range: 0.6μm×0.6μm Scanning speed: 0.3Hz -Pixel count: 512 x 512 Measurement environment: Room temperature, in air For each sample, the roundness of the fiber cross section was approximated by a cubic curve for the images obtained by observing one point from each single fiber, and the arithmetic mean roughness (Ra) was calculated for the entire image. The average value of the values ​​obtained for five single fibers was used.

[0074] <Method for preparing epoxy resin composition> After the components other than the curing agent were put into a beaker, the components were heated to 100°C and stirred until uniform. When fumed silica was used, the heated and stirred epoxy resin was cooled to 25-40°C and dispersed using a three-roll mill. Next, the temperature of the epoxy resin was adjusted to 25-60°C, and the curing agent was added and stirred until uniform to obtain an epoxy resin composition. When a toughening agent compatible with the epoxy resin at 25°C was used, compatibility was confirmed by visual observation. The component content ratios of the examples and comparative examples are shown in Tables 1-3.

[0075] <Method for measuring viscosity of epoxy resin composition at 25°C> According to the "Viscosity measurement method using a cone-plate type rotational viscometer" in JIS Z8803 (2011), measurements were taken using an E-type viscometer (TVE-30H, manufactured by Toki Sangyo Co., Ltd.) equipped with a standard cone rotor (1°34' x R24) at a rotation speed of 5 to 20 revolutions per minute. The temperature inside the sample cup was adjusted to the measurement temperature (25°C), and the epoxy resin composition was poured in, and the value was read when the displayed value stabilized after 1 minute or more had elapsed.

[0076] <η 0.1 / η 10 Measurement method> In accordance with JIS K 7244-10 (2005), the frequency dependence of the viscosity of the epoxy resin composition was measured under the conditions shown below, and the complex shear viscosity (η 0.1 ) complex shear viscosity (η 10) was calculated. Equipment: ARES-G2 (TA Instruments) Plate composition: Aluminum φ40mm disposable plate Aluminum φ42mm disposable pull cup Gap: 1.0mm Temperature: 25℃ Measurement frequency: 0.1~10Hz Distortion: 10%.

[0077] <How to make a resin cured plate> The epoxy resin composition was degassed in a vacuum and then poured into a mold set to a thickness of 2 mm or 6 mm using a Teflon (registered trademark) spacer. The epoxy resin composition was then cured by increasing the temperature from room temperature to 150°C at a rate of 2.5°C per minute in a hot air oven and maintaining the temperature for 4 hours. The epoxy resin composition was then cooled to room temperature and removed from the mold to produce a cured resin plate.

[0078] <Method of measuring glass transition temperature> A test piece 12.7 mm wide and 45 mm long was cut out from a 2 mm thick resin cured plate, and DMA measurements were performed in the temperature range of 30 to 250°C using a viscoelasticity measuring device (ARES, manufactured by TA Instruments) under conditions of a torsional vibration frequency of 1.0 Hz and a heating rate of 5.0°C / min. The glass transition temperature (Tg) was defined as the temperature at the intersection of the tangent in the glassy state and the tangent in the transition state on the storage modulus G' curve.

[0079] <Method for measuring fracture toughness of cured resin> The test was conducted in accordance with the SENB (Single Edge Notched Bend) test method in accordance with ASTM D5045. A test piece 60 mm long and 12.7 mm wide was cut out from a 6 mm thick resin-cured plate, and a pre-crack was then introduced. Then, using an Instron universal testing machine (Instron Corporation), the span was set to 50.8 mm, the crosshead speed was set to 10 mm / min, and the number of samples was set to n=6, and the fracture toughness value (K IC ) was measured.

[0080] <How to make towpregs> Using a towpreg manufacturing device equipped with a creel, kiss roll, nip roll, and winder, an epoxy resin composition adjusted to a temperature of 20 to 60°C was applied to one side of a carbon fiber bundle, and then the bundle was passed through a nip roll to impregnate the inside of the reinforced fiber bundle with the epoxy resin composition, thereby obtaining a towpreg. The towpreg bobbin was wound up to 2300 m on a cardboard tube with an initial tension of 600 to 1000 gf and a wind ratio of 6 to 10, to form a cylindrical shape with a winding width of 230 to 260 mm.

[0081] <Method of measuring Rc of towpreg> The Rc of the towpreg is the mass of the towpreg bobbin (W A ), the mass of the paper tube (W B ), the mass per unit length of carbon fiber (W C ), the length of the towpreg wound on the bobbin (W D ) according to equation (1).

[0082]

number

[0083] <Method for measuring interlayer friction coefficient> The interlayer friction coefficient was measured by carrying out the following operations (a), (b), and (c) in this order. (a) First, as shown in FIG. 1, a first layer towpreg 4 cut to a length of 150 mm was placed on a release paper 2 having a width of 40 mm and a length of 150 mm, and a second layer towpreg 3 cut to the same size was laminated on top of it so as to overlap by a length of 60 mm. Next, a towpreg for spacer 5 having a length of 20 mm was laminated on the first layer towpreg 4 so as to contact the overlapping portion of the second layer, and a third layer towpreg 4 having a length of 150 mm was laminated on top of it so as to overlap with the first layer to produce a towpreg laminate. Next, in order to prevent the towpreg laminate from being deformed more than necessary due to a vertical load, a spacer 6 having a thickness equivalent to that of the towpreg laminate was laminated with cellophane tape and placed so as to contact the side of the towpreg laminate. Finally, a release paper 2 having a width of 40 mm and a length of 150 mm was attached so as to overlap with the release paper 2 of the lowest layer to produce a test sample. (b) The test sample was placed in a sample chamber with a temperature of 25°C and a humidity of 50% RH, and a constant vertical load of 20.6 N was applied using pressure plate 1 to the area ranging from 60 mm of the overlap portion to 10 mm in the center of the spacer (area 10 mm wide and 70 mm long). (c) 10 minutes after applying the vertical load, the second layer towpreg 3 was pulled out in the fiber direction at a tensile speed of 1 mm / min, and the pull-out load was measured. The maximum value of the pull-out load that appears after the start of pulling was taken as the static friction force, and the static friction coefficient was calculated according to the following formulas (2) to (6). At this time, since the area of ​​the overlap part where the second layer towpreg receives the vertical load decreases with pulling, the pull-out displacement at the time when the pull-out load becomes maximum is subtracted from the initial overlap part length, and the value obtained by dividing the pull-out load by twice the vertical load received by the area of ​​the overlap part was taken as the static friction coefficient. In addition, at this time, since the towpreg 3 has slack immediately after the start of measurement, the pull-out displacement at the time when the pull-out load becomes maximum was corrected by subtracting the displacement until the slack was eliminated. The interlaminar friction coefficient in the present invention was calculated by measuring this static friction coefficient three times and using the average value.

[0084]

number

[0085] Here, the symbols in the formulas (2) to (6) have the following meanings. F: Maximum pull-out load (static friction force) N: Vertical load applied to the overlapping part of towpreg 3 and towpreg 4 at maximum load P: Vertical pressure applied to the overlapping portion of towpreg 3 and towpreg 4 at maximum load A 34 : Area of ​​overlap between towpreg 3 and towpreg 4 under maximum load A s : Area of ​​spacer 5 W: Towpreg width L 34 : Length of overlap between towpreg 3 and towpreg 4 at maximum load L0: Initial overlap length L1: Displacement until the initial slack of towpreg 3 is eliminated L t : Pull-out displacement at maximum load.

[0086] <Method of measuring coverage> First, the towpreg was cut into a length of 10 mm and placed on a sample stage so that the surface coated with the epoxy resin composition could be observed. The surface of the towpreg was imaged at a magnification of 200 times using a Keyence digital microscope VHX-5000 while illuminating with a ring light, and a digital image as shown in FIG. 2 was obtained. By illuminating with a ring light, the reflection of light by the epoxy resin was canceled, and an image in which the solid components not dissolved in the epoxy resin were emphasized was obtained. The obtained digital image was then binarized using image analysis software ImageJ, and the parts covered by the solid components not dissolved in the epoxy resin were recognized and their area was calculated. The area of ​​the parts covered by the solid components not dissolved in the epoxy resin obtained by the above method was divided by the area actually captured, and the value expressed as a percentage was used as the coverage rate.

[0087] <Method for evaluating towpreg slippage> The towpreg bobbin obtained according to the above <Towpreg manufacturing method> was adjusted to 25°C, then placed so that the longitudinal direction of the paper tube was perpendicular to the surface of the workbench and left to stand for 10 minutes, and the amount of movement of the cylindrical bobbin bottom end was measured. When there was no movement of 10 mm or more and the shape stability of the bobbin was good, it was ranked as A, when the above abnormalities occurred infrequently but were tolerable, as B, and when the above abnormalities occurred frequently and were unacceptable, as C. The evaluation ranking was A was the best and C was the worst.

[0088] <Method for measuring towpreg tightening speed> First, the towpreg bobbin obtained according to the above <Towpreg manufacturing method> was rewound with a tension of 7N to make the winding tension constant, and then a 5 kg weight was hung from the end of the towpreg using the device shown in FIG. 5. Next, the displacement of the weight after hanging was recorded with a displacement meter (laser reading type) to create a displacement curve (displacement vs. elapsed time). The tightening speed (mm / s) was calculated from the initial slope of the displacement curve. In the present invention, the tightening speed was the average value of four measurements. It can be said that the smaller this average value, the more difficult it is to tighten the towpreg.

[0089] <Method for evaluating towpreg spreadability> First, a helical layer (±45°) was wound around a cylindrical liner (made of aluminum) with an outer diameter of 146 mm and a total length of 250 mm, using one towpreg obtained according to the above <Towpreg manufacturing method>, with a creel tension of 30 N. Next, as shown in FIG. 6, the yarn width of the towpreg in the trunk and head portions of the second and subsequent helical layers was measured with a vernier caliper. The value obtained by dividing the yarn width of the head portion of the helical layer by the yarn width of the trunk portion of the helical layer was taken as the towpreg width expansion ratio. In the present invention, the yarn width was measured at seven points while changing the measurement points, and the average value of the calculated towpreg width expansion ratios was adopted. It can be said that the closer this average value is to 1.0, the better the spreadability is.

[0090] Example 1 An epoxy resin composition was prepared according to the above <Method for preparing epoxy resin composition> using 100 parts by mass of "jER (registered trademark)" 828 as the epoxy resin and 1.0 part by mass of Accelerator DY 9577 as the curing agent. The viscosity of this resin composition at 25°C was 17 Pa s. The cured resin obtained according to the above <Method for preparing cured resin plate> had a glass transition temperature of 108°C and a fracture toughness value (K IC ) is 0.7MPa m 0.5 It was.

[0091] Next, a towpreg was obtained using this epoxy resin composition according to the above-mentioned <Towpreg Production Method>. The Rc of this towpreg was 26.3 mass%, the coverage was 0%, and the interlaminar friction coefficient was 0.049. As a result of evaluating this towpreg, the slippage was rated B, the expansion ratio was 0.86, and the tightening speed was 18, and good results were obtained in all tests.

[0092] (Examples 2 to 3) Epoxy resin compositions and towpregs were prepared and evaluated in the same manner as in Example 1, except that the formulation of the epoxy resin composition was changed as shown in Table 1. The evaluation results were the viscosity of the resin composition at 25°C, the glass transition temperature of the cured resin, and the fracture toughness value (K IC ), Rc, coverage, interlayer friction coefficient, slippage, expansion ratio, and tightening speed all showed good results.

[0093] In Example 3, where the viscosity of the resin composition was relatively high, it was necessary to heat the epoxy resin composition during towpreg production to reduce the viscosity to an easy-to-coat level and to control the temperature so as to prevent an increase in viscosity due to the progress of the curing reaction. However, in Example 2, since the viscosity was lower than 50 Pa s, only simple temperature control was required, and operability was excellent.

[0094] (Examples 4 to 6) Epoxy resin compositions and towpregs were prepared and evaluated in the same manner as in Example 1, except that the formulation of the epoxy resin composition was changed as shown in Table 1. The evaluation results were the viscosity of the resin composition at 25°C, the glass transition temperature of the cured resin, and the fracture toughness value (KIC ), Rc, coverage, interlayer friction coefficient, slippage, expansion ratio, and tightening speed all showed good results.

[0095] All of Examples 4 to 6 contained a toughening agent having a primary particle size of 50 nm to 1 μm, and therefore showed excellent toughness values. 0.1 / η 10 Since the value was 1.5 or more, the slip-down property was rated A, which was a better result than that of Example 1.

[0096] Furthermore, in Example 6, which contains 3 to 5 parts by mass of fumed silica having a primary particle diameter of 5 to 50 nm per 100 parts by mass of epoxy resin, a better balance was achieved between the effect of suppressing tight winding during unwinding and the spreadability of the tow during filament winding molding.

[0097] (Examples 7 to 10) Except for changing the composition of the epoxy resin composition as shown in Table 2 and using a liquid aromatic amine that is liquid at 25°C as the curing agent, the epoxy resin composition and towpreg were prepared and evaluated in the same manner as in Example 1. The evaluation results were the viscosity of the resin composition at 25°C, the glass transition temperature of the cured resin, and the fracture toughness value (K IC ), Rc, coverage, interlayer friction coefficient, slippage, expansion ratio, and tightening speed all showed good results.

[0098] In Examples 7 to 10, by using a liquid aromatic amine that is liquid at 25°C, the coverage rate could be controlled to be small, and even when a solid epoxy ("EPICLON (registered trademark)" HP-7200L) that is prone to increasing viscosity or a large amount of a toughening agent was used, it was easy to adjust the interlayer friction coefficient to within the appropriate range of the present invention.

[0099] Moreover, Examples 7 to 9 had higher Tg and better heat resistance than Example 10. Furthermore, since Examples 8 and 9 contain a glycidylamine type epoxy resin, the viscosity increase ratio after 24 hours at 25°C was smaller than that of Example 7, and the storage stability was excellent.

[0100] (Examples 11 to 13) Except for changing the composition of the epoxy resin composition as shown in Table 2, the epoxy resin composition and towpreg were prepared and evaluated in the same manner as in Example 1. The evaluation results were the viscosity of the resin composition at 25°C, the glass transition temperature of the cured resin, and the fracture toughness value (K IC ), Rc, coverage, interlayer friction coefficient, slippage, expansion ratio, and tightening speed all showed good results.

[0101] Even when a solid component is included, the interlayer friction coefficient can be controlled within an appropriate range by setting the coverage rate to 0% or more and less than 2.5%. In addition, in Examples 11 and 13, which contain 0.5 to 2 parts by mass of particles that are insoluble in epoxy resin at 25°C and have a primary particle diameter of 0.5 to 150 μm per 100 parts by mass of epoxy resin and have an Rc of 20 to 28%, the effect of suppressing winding tightness during unwinding and the spreadability of the tow during filament winding molding are better balanced than in Example 12.

[0102] (Comparative Example 1 and Comparative Example 2) Except for changing the composition of the epoxy resin composition as shown in Table 3, epoxy resin compositions and towpregs were prepared and evaluated in the same manner as in Example 1. As a result of the evaluation, Comparative Example 1 and Comparative Example 2, in which the coverage was 2.5% or more, had a large interlayer friction coefficient of 0.10 or more, and therefore had a small expansion ratio, resulting in insufficient results.

[0103] Comparative Example 3 An epoxy resin composition and a towpreg were prepared and evaluated in the same manner as in Example 1, except that the formulation of the epoxy resin composition was changed as shown in Table 3 and the viscosity at 25°C was lowered to less than 5 Pa s. The evaluation results showed that the interlaminar friction coefficient was 0.021, which was smaller than 0.04, and therefore the expansion ratio was 0.93, which was good, but the slippage was rated C and the tightening speed was 89 mm / sec, which were unsatisfactory results.

[0104] Comparative Example 4 An epoxy resin composition and a towpreg were prepared and evaluated in the same manner as in Example 1, except that the formulation of the epoxy resin composition was changed as shown in Table 3 and the viscosity at 25°C was increased to more than 150 Pa s. As a result of the evaluation, the interlaminar friction coefficient was 0.11, which was greater than 0.10, so the slippage property was rated A, and the tightening speed was 4.9 mm / sec, which was good, but the expansion ratio was 0.70, which was unsatisfactory.

[0105] Comparative Example 5 An epoxy resin composition and a towpreg were produced and evaluated in the same manner as in Example 1, except that the composition of the epoxy resin composition was changed as shown in Table 3 and Rc was set to 18.9%, which is smaller than 20%. As a result of the evaluation, the interlaminar friction coefficient was 0.64, which was larger than 0.10, so the slippage property was rated A, and the tightening speed was 0.5 mm / sec, which was good, but the expansion ratio was 0.61, which was unsatisfactory.

[0106] Comparative Example 6 An epoxy resin composition and a towpreg were produced and evaluated in the same manner as in Example 1, except that the composition of the epoxy resin composition was changed as shown in Table 3, and Rc was increased to 42.5%, which is greater than 40%. As a result of the evaluation, the interlaminar friction coefficient was 0.033, which was smaller than 0.04, and although the expansion ratio was good at 0.97, the slippage was rated C and the tightening speed was 45 mm / sec, which was an insufficient result. In addition, because Rc was large, there was a lot of seepage of the resin composition from the towpreg bobbin and a lot of scattering of the resin composition during the filament winding molding process, and the processability was insufficient.

[0107] [Table 1]

[0108] [Table 2]

[0109] [Table 3]

[0110] The compositions in the table are expressed in parts by mass. [Explanation of symbols]

[0111] 1: Pressure plate 2:Release paper 3: 2nd layer towpreg 4: 1st and 3rd towpreg layers 5: Towpreg for spacers 6: Cellophane tape spacer 7: Towpreg 8:Paper tube 9: Weight 10: Movable frustum 11: Displacement gauge 12: Towpreg 13: Liner 14: Width of the helical layer 15: Thread width of the mirror part of the helical layer

Claims

1. An epoxy resin composition containing as an epoxy resin a glycidylamine type epoxy resin selected from a glycidylaniline type, a diaminodiphenylmethane type, a diaminodiphenylsulfone type, an aminophenol type, or a metaxylenediamine type, and containing as a curing agent an aromatic amine which is liquid at 25°C and compatible with the epoxy resin, and having a viscosity at 25°C of 5 to 150 Pa·s, A towpreg impregnated with a carbon fiber bundle having a fineness of 30 to 4000 g / 1000 m, The content of the glycidylamine type epoxy resin is 10 to 60 parts by mass in 100 parts by mass of the epoxy resin, The liquid aromatic amine contains a compound represented by the following chemical formula (1): The resin content (Rc) of the towpreg is 20 to 40 mass%; and when the surface of the towpreg is observed at a magnification of 200 times using an optical microscope, the ratio of the area of ​​the portion covered by the solid component not dissolved in the epoxy resin to the area of ​​the field of view (coverage rate) is 0% or more and less than 2.5%. Furthermore, a towpreg is provided in which three layers of the towpreg are laminated in the same direction, and the central towpreg is pulled out under conditions of a temperature of 25° C., a humidity of 50% RH, a speed of 1 mm / min, and a normal load of 20.6 N, and the interlayer friction coefficient is measured to be 0.04 or more and less than 0.

10. 【Chemistry 1】 In the formula, R 1 , R 2 and R 3 are any one of hydrogen, an alkyl group having 1 to 4 carbon atoms, an alkoxy group and an alkylthio group, and R 1 , R 2 and R 3 may be the same or different.

2. The towpreg as described in claim 1, wherein the content of the glycidyl amine type epoxy resin is 20 to 60 parts by mass per 100 parts by mass of the epoxy resin.

3. The epoxy resin composition contains a toughening agent that is compatible with epoxy resins at 25°C and / or a toughening agent having a primary particle size of 50 nm to 1 µm, and the toughness value KIc of a cured product obtained by curing the epoxy resin composition at 150°C for 4 hours is 1.0 to 3.0 MPa m 0.5 The towpreg according to claim 1 or 2.

4. The epoxy resin composition was measured using a parallel plate oscillatory rheometer at 25° C. and a frequency of 0.1 Hz to determine the ratio (η) of the complex shear viscosity (η) measured using a parallel plate oscillatory rheometer at 25° C. and a frequency of 10 Hz. 0.1 / 10 4. The towpreg according to claim 1, wherein the ratio of the tensile strength to the welded strength is 1.5 or more.

5. The towpreg according to claim 4, comprising 3 to 5 parts by mass of fumed silica having a primary particle diameter of 5 to 50 nm per 100 parts by mass of the epoxy resin.

6. A towpreg as described in any one of claims 1 to 5, wherein the content of the aromatic amine is an amount such that the active hydrogen is 0.7 to 2.0 equivalents relative to the epoxy groups of the epoxy resin.

7. A towpreg as described in any one of claims 1 to 6, further comprising a bisphenol F type epoxy resin.

8. A fiber-reinforced composite material obtained by curing the towpreg according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Two-component curable composition

    JP2007514009A

  • Prepreg and golf club shaft

    JP2009074009A

  • Method of manufacturing composite container

    JP2010234658A

  • Epoxy resin composition for tow prepreg and tow prepreg

    JP2011157491A

  • Method for manufacturing tow prepreg and tow prepreg

    JP2015098556A