Manufacturing method of container member, and container member with thread and its manufacturing method
A two-layered manufacturing method using supercritical fluid forming and injection molding addresses appearance defects in plastic molded products, resulting in lightweight, aesthetically pleasing containers with enhanced structural integrity and recyclability.
Patent Information
- Application Number
- JP2020182342
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-30
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2040-10-30
AI Technical Summary
Supercritical fluid forming in plastic molded products often results in appearance defects such as sink marks and foam marks, limiting its application to larger industrial products and hindering the use of lightweight, aesthetically pleasing consumer items.
A manufacturing method involving two-layered structure with a foam layer and a dense layer, where the foam layer is formed using supercritical fluid and the dense layer covers external defects through injection molding, ensuring a lightweight and aesthetically appealing product.
The method produces a lightweight container member or cap with improved appearance by hiding external defects and promoting resin recycling, while maintaining structural integrity and aesthetic appeal.
Smart Images

Figure 0007577970000001 
Figure 0007577970000002 
Figure 0007577970000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a container member, a manufacturing method thereof, and a container cap. [Background technology]
[0002] In recent years, plastic molded products are used in all kinds of daily necessities and industrial products around us. The demand for plastic molded products is increasing as their quality improves and costs go down, making them more versatile. On the other hand, attention has been focused on the impact of microplastics on the environment, as seen in the problem of marine plastic waste, and there is a growing trend to move away from plastic and to refrain from using plastic products.
[0003] Regarding disposable plastic containers for food and daily necessities, there is a growing demand from users to reduce the amount of petroleum-based plastic used. In response to such demands, efforts are being made to reduce the amount of plastic used by using plant-based resins as part of the raw materials, utilizing recycled plastic materials, and improving dimensions and shapes.
[0004] Foam molding is known as a means for reducing the weight of plastic molded products. Foam molding can be broadly divided into chemical foam molding and physical foam molding. Chemical foam molding uses a foaming agent, while physical foam molding uses a fluid in a supercritical state (hereinafter referred to as "supercritical fluid molding"). Chemical foam molding has concerns about the negative impact of the foaming agent on the environment and issues such as mold contamination. Supercritical fluid molding does not have such concerns. Supercritical fluid molding has traditionally been applied to relatively large industrial products such as automobile part molding and office equipment. In recent years, with the improvement of supercritical fluid generation technology and resin composition kneading technology, the application of supercritical fluid molding to high-cycle injection molding has been considered. Patent Documents 1 to 3 disclose food containers manufactured by supercritical fluid molding. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 6085729 [Patent Document 2] Patent No. 6430684 [Patent Document 3] JP 2020-040690 A Summary of the Invention [Problem to be solved by the invention]
[0006] In order to broaden the scope of application of supercritical fluid molding, the inventors carried out supercritical fluid molding using various dies under various conditions. As a result, they found that as the degree of foaming increases, appearance defects such as minute sink marks and foaming marks (swirl marks) tend to occur on the surface of the molded product.
[0007] The present disclosure provides a container member and a manufacturing method thereof, which are lightweight due to foaming and have an excellent appearance. The present disclosure also provides a container cap, which are lightweight due to foaming and have an excellent appearance. [Means for solving the problem]
[0008] One aspect of the present disclosure relates to a method for producing a container member, which includes the steps of (A) injecting a first molten resin composition containing a resin material and a supercritical fluid into a cavity of a mold, (B) foaming the first molten resin composition in the cavity by reducing the pressure, and (C) injecting a second molten resin composition containing a resin material into the cavity of the mold while the foamed molded article obtained through the step (B) is placed in the cavity, and the container member obtained through the step (C) has a foamed layer made of a cured product of the first molten resin composition and having a plurality of voids derived from the supercritical fluid, and a dense layer made of a cured product of the second molten resin composition.
[0009] According to the above-mentioned manufacturing method, even if the surface of the foamed molded body (foam layer) obtained through step (B) has appearance defects such as sink marks or foaming marks caused by foaming, a dense layer can be provided by injection molding (e.g., two-color molding and insert molding) to cover the defects, thereby producing a container member having an excellent appearance.
[0010] The container member according to the present disclosure includes a foamed layer made of a first resin material and having a plurality of voids derived from a supercritical fluid, and a dense layer made of a second resin material. As described above, even if the surface of the foamed layer has appearance defects such as sink marks or foaming marks caused by foaming, these defects can be hidden by the dense layer. Therefore, the container member is lightweight due to foaming and has an excellent appearance. It is preferable that the dense layer is exposed on the surface of the container composed of the container member and other members.
[0011] In the present disclosure, the dense layer is in contact with at least a part of the surface of the foam layer, and it is preferable that the interface between the dense layer and the foam layer has irregularities. Appearance defects such as sink marks and foaming marks can be said to be fine irregularities on the surface of the foam layer. The irregularities at the interface between these layers can contribute to improving the adhesion between these layers. The interface may be intentionally provided with irregularities.
[0012] An example of a container member according to the present disclosure is a cap for a container for storing cosmetics, etc. The container cap according to the present disclosure includes a top surface portion and a side surface portion extending from the peripheral portion of the top surface portion in a direction away from the top surface portion, and includes a foamed layer made of a first resin material and having a plurality of voids derived from a supercritical fluid and constituting the inner surface of the container cap, and a dense layer made of a second resin material and constituting the outer surface of the container cap. This container cap is lightweight due to the foaming, and has an excellent appearance.
[0013] In the present disclosure, the foam layer and the dense layer are preferably made of the same type of resin material, which allows the container member and the container cap to be made of a mono-material, thereby contributing to the promotion of recycling of the resin material. Effect of the Invention
[0014] According to the present disclosure, a container member and a manufacturing method thereof are provided, which are lightweight due to foaming and have an excellent appearance. Also, according to the present disclosure, a container cap is provided, which is lightweight due to foaming and has an excellent appearance. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a schematic diagram of one embodiment of a container cap according to the present disclosure. [Diagram 2] FIG. 2 is a cross-sectional view that typically illustrates the interface between a foamed layer and a dense layer in the container cap illustrated in FIG. [Diagram 3] FIG. 3 is a cross-sectional view that illustrates another example of the interface between a foamed layer and a dense layer in a container cap. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, an embodiment of the present disclosure will be described in detail. Here, a container cap (screw cap) will be described as an example of a container member. Note that the present invention is not limited to the following embodiment.
[0017] <Container cap and manufacturing method thereof> 1 is a cross-sectional view showing a schematic diagram of a container cap according to the present embodiment. The container cap 10 shown in this figure (hereinafter sometimes simply referred to as "cap 10") is manufactured through the following steps. (A) A step of injecting a first molten resin composition containing a resin material and a supercritical fluid into a cavity of a mold. (B) foaming the first molten resin composition in the cavity by reducing the pressure. (C) A process of injecting a second molten resin composition containing a resin material into a cavity of a mold while the foam-molded article obtained through the process (B) is placed in the cavity. The cap 10 produced by this method includes a foamed layer L1 made of a cured product of a first molten resin composition (first resin material) and having a plurality of voids derived from a supercritical fluid, and a dense layer L2 made of a cured product of a second molten resin composition (second resin material). Note that a series of steps from (A) to (B) can be carried out, for example, using a MuCell injection molding machine ("MuCell" is a registered trademark of Trexel Co. Ltd) (see Patent Documents 1 and 2).
[0018] The cap 10 is called a screw cap. The cap 10 comprises a top surface portion 1 and a side surface portion 2 hanging down from the peripheral portion of the top surface portion 1. An inner ring portion 1a that fits into the inside of the opening of the container body is provided on the inner surface of the top surface portion 1. A screw thread 2a that corresponds to the screw thread (not shown) of the opening of the container body is provided on the inside of the side surface portion 2.
[0019] The thickness of the cap 10 is, for example, 1 to 2 mm. The thickness of the cap 10 here means the sum of the thickness of the foamed layer L1 (excluding the part where the inner ring part 1a and the screw thread 2a are provided) and the thickness of the dense layer L2. The thickness of the foamed layer L1 (excluding the part where the inner ring part 1a and the screw thread 2a are provided) is, for example, 0.3 to 1.7 mm, and may be 0.4 to 1.6 mm or 0.5 to 1.5 mm. When the foamed layer L1 has such a thickness, the effect of weight reduction by foaming can be sufficiently obtained. The thickness of the dense layer L2 is, for example, 0.3 to 0.7 mm, and may be 0.4 to 0.6 mm. When the dense layer L2 has such a thickness, the strength of the cap 10 can be sufficiently secured. Note that, when the thickness of the cap 10 is made thicker than 2 mm, the foamed layer L1 and the dense layer L2 may be made thicker than the above upper limit value.
[0020] FIG. 2 is a cross-sectional view showing a schematic diagram of the interface between the foam layer L1 and the dense layer L2 in the cap 10. As shown in FIG. 2, the interface F between the foam layer L1 and the dense layer L2 has irregularities. The irregularities are caused by foaming in the foam layer L1, and may be defects in appearance such as sink marks or foaming marks. The irregularities at the interface F can contribute to improving the adhesion (welding strength) between the foam layer L1 and the dense layer L2. Furthermore, by covering the foam layer L1 with the dense layer L2, it is possible to suppress a decrease in strength caused by foaming.
[0021] Fig. 3 is a cross-sectional view showing another example of the interface between the foamed layer L1 and the dense layer L2. The interface G shown in Fig. 3 has unevenness provided on each of the foamed layer L1 and the dense layer L2. Such unevenness can be formed by intentionally providing a rib shape on the foamed layer L1 or the dense layer L2, or by applying an embossing process to the mold surface. By increasing the surface area of the interface G, the adhesion (welding strength) between the foamed layer L1 and the dense layer L2 can be further improved.
[0022] The foam layer L1 and the dense layer L2 may be made of the same resin material or different resin materials. From the viewpoint of promoting recycling of the cap 10, it is preferable that the foam layer L1 and the dense layer L2 are made of the same resin material. That is, when the material of the foam layer L1 is PET (polyethylene terephthalate), it is preferable that the material of the dense layer L2 is also PET. When the material of the foam layer L1 is PP (polypropylene), it is preferable that the material of the dense layer L2 is also PP. When the material of the foam layer L1 is PE (polyethylene), it is preferable that the material of the dense layer L2 is also PE. Note that the color of the dense layer L2 may be different from the color of the foam layer L1 by two-color molding. In addition, when it is assumed that the cap is applied to a cap for a cosmetic container, PET may be used as the resin material of the dense layer L2, or an elastomer may be blended into the dense layer L2 to give it a glossy feel or texture.
[0023] Each step of the method for manufacturing the cap 10 will now be described.
[0024] [(A) Process] First, a molten resin composition containing a resin material and a supercritical fluid is prepared. Examples of the resin material include polypropylene resin and polyethylene resin. Examples of the supercritical fluid include carbon dioxide, nitrogen, argon, and helium. According to the study by the present inventors, when the supercritical fluid is carbon dioxide, the molten resin composition is prepared by adding preferably 1 to 4 parts by mass, more preferably 2 to 3 parts by mass of carbon dioxide in a supercritical state to 100 parts by mass of the resin material. When the carbon dioxide content of the molten resin composition is 1 part by mass or more, it is easy to form a sufficiently uniform foam layer over the entire top surface portion 1, and weight reduction by foaming tends to be realized. On the other hand, when the carbon dioxide content of the molten resin composition is 4 parts by mass or less, excessive foaming tends to be suppressed.
[0025] When the supercritical fluid is nitrogen, the molten resin composition is prepared by adding preferably 0.1 to 1.2 parts by mass, more preferably 0.3 to 0.7 parts by mass, of supercritical nitrogen per 100 parts by mass of the resin material. When the nitrogen content of the molten resin composition is 0.5 parts by mass or more, it is easy to form a sufficiently uniform foamed layer over the entire foamed layer L1, and weight reduction by foaming tends to be realized. On the other hand, when the nitrogen content of the molten resin composition is 1.0 part by mass or less, excessive foaming tends to be suppressed.
[0026] When the resin material used is a polypropylene resin, the temperature of the molten resin composition (screw cylinder temperature) is preferably about 210 to 230° C. When the resin material used is a polyethylene resin, this temperature is preferably about 220 to 240° C. When this temperature is equal to or higher than the lower limit, the resin easily flows in the cavity, while when the temperature is equal to or lower than the lower limit, for example, scorching of the resin tends to be suppressed.
[0027] The molten resin composition may contain components other than the resin material and the supercritical fluid. That is, the molten resin composition may further contain, for example, a filler, a colorant, an antistatic agent, an antioxidant, etc., as necessary. According to this embodiment, since the top surface portion 1 can be made white by the voids resulting from foaming, the molten resin composition may contain a white pigment of 2 mass% or less based on the mass of the molten resin composition, or may not contain a white pigment.
[0028] The molten resin composition prepared as described above is injected into the cavity through the gate of the mold. When the molten resin composition is introduced into the cavity, the pressure is reduced, and the cells grow, so that independent bubbles are generated in the resin composition. The injection speed is preferably 100 to 300 mm / sec, and more preferably 150 to 200 mm / sec. When the injection speed is 100 mm / sec or more, the resin can easily reach the end of the flow, and the occurrence of short shots tends to be suppressed. On the other hand, when the injection speed is 300 mm / sec or less, the occurrence of burr defects in the cap 10 tends to be suppressed. According to the study by the present inventors, when the resin material is a polyethylene resin and the supercritical fluid is nitrogen, it is preferable to set the injection speed in multiple stages. That is, it is more preferable to set the initial injection speed to 250 to 300 mm / sec, and to reduce the second-stage injection speed to 150 to 200 mm / sec.
[0029] In this embodiment, from the viewpoint of sufficiently promoting foaming in the cavity, it is not necessary to carry out a step of applying pressure to the cavity (pressure holding) after filling the cavity with the molten resin composition. In this embodiment, from the viewpoint of obtaining a sufficiently thin foamed molded product, it is preferable not to carry out a step called "core back" for reducing the pressure in the cavity. Core back is Cavity Before the molten resin filled in the mold finishes solidifying, the movable part of the mold is moved. Cavity (See Patent Document 1.) In this embodiment, as described above, foaming can be caused in the cavity by a pressure reduction that accompanies the introduction of the molten resin composition into the cavity.
[0030] When the temperature of the foamed molded body drops to about 30 to 60°C, the foamed molded body is recovered from the mold. Since voids resulting from foaming are formed in the foamed molded body, the weight is reduced and the amount of plastic material used is reduced. Since voids are formed, it is preferable that the weight is reduced by 3% by mass or more compared to a molded body without voids (a normal injection molded body).
[0031] [(C) Process] A dense layer L2 is formed so as to cover a part of the surface of the foamed molded product (foam layer L1) obtained through the above step (B). This step can be performed by insert molding. When forming a dense layer L2 of a different color from the foamed molded product, it can be performed by two-color molding. By covering the outside of the foamed layer L1 with an unfoamed dense layer L2, defects in the appearance of the outside of the foamed layer L1 can be hidden. In addition, it is possible to give the cap 10 a glossy appearance and to achieve a beautiful finish by coloring it with good color development.
[0032] Although the embodiments of the present disclosure have been described above, the present invention is not limited to the above embodiments. For example, in the above embodiments, a container cap is given as an example of a container member, but the present invention is not limited thereto. For example, packaging containers such as stoppered caps, trays, and cups may be manufactured by the manufacturing method according to the above embodiment. The contents of the packaging container may be food or non-food.
[0033] In the above embodiment, the container cap has a two-layer structure of the foamed layer L1 and the dense layer L2, but if a glossy appearance is required for only a part (e.g., the upper surface) of the top surface 1, only that part may have a two-layer structure of the foamed layer L1 and the dense layer L2. The other part may be a foamed resin body having a plurality of voids derived from the supercritical fluid, and further weight reduction effects can be obtained. [Explanation of symbols]
[0034] 1...top surface portion, 1a...inner ring portion, 2...side surface portion, 2a...screw thread, 10...container cap (container member), F, G...interface, L1...foamed layer, L2...dense layer.
Claims
1. (A) injecting a first molten resin composition containing a resin material and a supercritical fluid into a cavity of a mold; (B) foaming the first molten resin composition in the cavity by a reduction in pressure caused by the introduction of the first molten resin composition into the cavity, and maintaining the volume of the cavity without expanding until the first molten resin composition filled in the cavity is solidified; (C) a step of injecting a second molten resin composition containing a resin material into a cavity of a mold while the foamed molded article obtained through the step (B) is placed in the cavity; Including, A method for manufacturing a container member, wherein the container member obtained through the (C) step comprises a foamed layer made of a cured product of the first molten resin composition and having a plurality of voids derived from a supercritical fluid, and a dense layer made of a cured product of the second molten resin composition.
2. a foamed layer made of a first resin material and having a plurality of voids derived from a supercritical fluid; a dense layer made of a second resin material; Equipped with A threaded container member having threads defined by said foam layer.
3. The threaded container component is a container cap, A top surface portion and A side surface portion extending from a peripheral portion of the top surface portion in a direction away from the top surface portion; Equipped with the foam layer constitutes an inner surface of the container cap and the dense layer constitutes an outer surface of the container cap, The screw thread is provided on the inside of the side surface, Further comprising an inner ring portion provided on an inner surface of the top surface portion, 3. The threaded container component of claim 2, wherein the foam layer defines the threads and the inner ring portion.
4. 4. The threaded container member according to claim 2 or 3, wherein the dense layer is exposed on a surface of a container constituted by the threaded container member and another member.
5. the dense layer is in contact with at least a portion of a surface of the foam layer, 5. The threaded container member according to claim 2, wherein the interface between the dense layer and the foam layer has irregularities.
6. 6. The threaded container member according to claim 2, wherein the foam layer and the dense layer are made of the same type of resin material.
7. A method for manufacturing a threaded container member according to any one of claims 2 to 6, comprising the steps of: (A) injecting a first molten resin composition containing a resin material and a supercritical fluid into a cavity of a mold; (B) foaming the first molten resin composition in the cavity by a reduction in pressure caused by the introduction of the first molten resin composition into the cavity, and maintaining the volume of the cavity without expanding until the first molten resin composition filled in the cavity is solidified; (C) forming the dense layer by injecting a second molten resin composition containing a resin material into a mold cavity while the foamed layer obtained through the (B) process is placed in the mold cavity; Including, The method for producing a threaded container member, wherein the foamed layer obtained through the step (B) is provided with the threads.
Citation Information
Patent Citations
Stopper structure of vessel
JP1983001658A
Apparatus for measuring viscoelastic property of skin
JP1985085729A
Automatic fruit selector
JP1989030684A
Skin integrated molded product
JP1993200893A
Foam cap for polyethylene terephthalate-made bottle type container and method for manufacturing it