Polymerization Processes Including the Addition of Monofunctional Vinyl Monomers
The controlled addition of monomers during suspension polymerization addresses the non-uniformity in polymer beads, achieving targeted MHC levels with lower polyfunctional monomer usage, thereby optimizing ion exchange resin production.
Patent Information
- Application Number
- JP2020525895
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-11-10
- Filing Date
- 2018-10-24
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2038-10-24
AI Technical Summary
Existing suspension polymerization methods result in non-uniform polymer beads due to varying reactivity of monomers, leading to inefficient use of polyfunctional vinyl monomers and difficulty in achieving targeted water holding capacity (MHC) in ion exchange resins, often requiring excessive amounts of polyfunctional monomers that increase costs.
A method involving suspension polymerization with controlled monomer addition, where a monomer feed solution is added during polymerization, maintaining a lower ratio of polyfunctional to monofunctional vinyl monomers, and adjusting the degree of polymerization to achieve targeted MHC levels with reduced polyfunctional monomer usage.
This approach produces polymer beads with consistent MHC levels and reduced polyfunctional monomer content, enhancing efficiency and reducing production costs while minimizing interpenetrating network structures.
Smart Images

Figure 0007578489000001 
Figure 0007578489000002 
Figure 0007578489000003
Abstract
Description
[Background technology]
[0001] A useful method for producing polymer beads is suspension polymerization, a process in which monomer oil droplets are suspended in an aqueous medium, and then the monomers in the oil droplets are polymerized to form polymer beads. When a mixture of monomers is present in the monomer oil droplet, it is believed that the monomers may react at different rates, thus forming non-uniform polymer beads. For example, it is believed that one or more regions within the oil droplet may form a copolymer having a proportion of polymerized units of a more reactive monomer that is higher than the average proportion of the more reactive monomer present in the mixture of monomers in the entire oil droplet. Therefore, it is also believed that one or more regions within the oil droplet may form a copolymer having a proportion of polymerized units of a more reactive monomer that is lower than the average proportion of the more reactive monomer present in the mixture of monomers in the entire oil droplet. In general, some non-uniformity in the beads is expected to occur in many cases due to different reactivities of the monomers.
[0002] It would be desirable to provide a method for producing polymeric beads that involves the polymerization of a mixture of monomers and that can exert some control over the type of uniformity or non-uniformity that occurs in the resulting polymeric beads.
[0003] Many polymer beads have covalently attached ion exchange groups, such as sulfonic acid groups, carboxyl groups, tertiary amine groups, or quaternary amine groups. Such polymer beads with ion exchange groups are known as ion exchange resins. Often, to produce ion exchange resins, monomers lacking ion exchange groups are polymerized to form polymer beads lacking ion exchange functional groups, and the polymer beads are subjected to one or more chemical reactions to attach the desired ion exchange group or groups. An important property of ion exchange resins is the water holding capacity (MHC). MHC is measured by equilibrating the ion exchange resin with air at 100% humidity and then measuring the amount of water adsorbed by the polymer beads. For many ion exchange resins intended to be used for a particular purpose, there is a specific desired target range of MHC values, and ion exchange resins having MHC in that target range are considered to be particularly suitable for the intended purpose.
[0004] Many polymer beads that lack ion exchange groups are copolymers of one or more monofunctional vinyl monomers and one or more polyfunctional vinyl monomers. Another important characteristic of such polymer beads is the amount of polymerized units of polyfunctional vinyl monomers. In the past, it was often found that the MHC value of an ion exchange resin was largely determined by the amount of polymerized units of polyfunctional vinyl monomers. For example, in some cases, it was necessary to use unnecessarily large amounts of polyfunctional vinyl monomers to achieve the desired MHC value.
[0005] It would be desirable to produce ion exchange resins that have desired target MHC values and that have a lower amount of polymerized units of multifunctional vinyl monomers than previously required. Multifunctional vinyl monomers are typically more expensive than other monomers, so reducing the amount of multifunctional vinyl monomers would typically reduce the cost of producing the polymer beads. It would also be desirable to produce polymer beads that lack ion exchange groups and that can be converted into such desirable ion exchange resins.
[0006] US Patent No. 3,792,029 describes a suspension polymerization process in which during the suspension polymerization of a monomer mixture, an emulsion containing a more reactive monomer is added to the suspension while polymerization is occurring. Also, in the process of US Patent No. 3,792,029, the monomer added is a significant amount relative to the amount of starting monomer, and the concentration of multifunctional vinyl monomer in the monomer feed is higher than in the starting monomer. It is believed that the process of US Patent No. 3,792,029 will result in a different polymer composition profile compared to the process carried out without feeding monomer during polymerization. It is further believed that the process of US Patent No. 3,792,029 will result in an interpenetrating polymer network structure, which can have a significant effect on ion exchange resin performance. Summary of the Invention [Problem to be solved by the invention]
[0007] It would be desirable to provide a process having one or more of the following characteristics: neat monomer is added to the suspension polymerization process; the amount of monomer fed during polymerization is less than the amount of monomer present before the start of polymerization; the ratio of multifunctional vinyl monomer to monofunctional vinyl monomer in the feed is lower than the ratio of multifunctional vinyl monomer to monofunctional vinyl monomer present before the start of polymerization; and / or improved consistency and / or efficiency of monomer mass transfer of the monomer being fed into the monomer droplets. It is believed that these characteristics provide a process that is easier to perform than the process of U.S. Pat. No. 3,792,029. It is also believed that these characteristics will provide a process that is less prone to producing interpenetrating network structures than the process of U.S. Pat. No. 3,792,029. It would also be desirable to provide polymer beads having target MHC levels after conversion to ion exchange resins with lower levels of polymerized units of multifunctional vinyl monomer than previously required. [Means for solving the problem]
[0008] The following is a statement of the present invention.
[0009] A first aspect of the present invention is a method for producing a collection of polymer beads, the beads comprising: (i) 75 to 99.7% by weight of polymerized units of a monofunctional vinyl monomer based on the weight of the beads; (ii) 0.3 to 25% by weight of polymerized units of a polyfunctional vinyl monomer based on the weight of the beads; Including, The method further comprising: (a) providing an aqueous suspension of monomer oil droplets comprising an initiator, a multifunctional vinyl monomer, and a monofunctional vinyl monomer; (b) initiating polymerization of the monomers in the monomer oil droplets; (c) adding a monomer feed solution to the suspension while polymerization of the monomers in the monomer oil droplets is occurring, This addition begins when the degree of polymerization (EXTSTART) of the monomer in the monomer oil droplet is between 0% and 50%. This addition ends when the degree of polymerization of the monomer in the monomer oil droplet after EXTSTART (EXTSTOP) is between 5% and 100%; the feed solution comprises monomer in an amount of 90% to 100%, by weight, based on the weight of the feed solution; The feed solution comprises monofunctional vinyl monomers in an amount of 50% to 100% by weight based on the weight of the feed solution. Process The method includes: DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The following is a detailed description of the present invention.
[0011] As used herein, the following terms have the definitions specified unless the context clearly dictates otherwise.
[0012] A "polymer," as used herein, is a relatively large molecule composed of the reaction product of smaller chemical repeating units. Polymers may have structures that are linear, branched, star-shaped, looped, hyperbranched, crosslinked, or combinations thereof; polymers may have a single type of repeating unit ("homopolymers"), or they may have two or more types of repeating units ("copolymers"). Copolymers may have the various types of repeating units arranged randomly, in order, in blocks, in other arrangements, or in any mixture or combination thereof.
[0013] Molecules that can react with each other to form repeat units of a polymer are known herein as "monomers." The repeat units so formed are known herein as "polymerized units" of the monomer.
[0014] Vinyl monomers have the structure: [ka] (In the formula, R 1 , R 2 , R 3 , and R 4 each is independently hydrogen, a halogen, an aliphatic group (such as, for example, an alkyl group), a substituted aliphatic group, an aryl group, a substituted aryl group, other substituted or unsubstituted organic groups, or any combination thereof. Vinyl monomers can undergo free radical polymerization to form polymers. Some vinyl monomers have the formula R 1 , R 2 , R 3 , and R 4 such vinyl monomers are known herein as polyfunctional vinyl monomers. Vinyl monomers with exactly one polymerizable carbon-carbon double bond are known herein as monofunctional vinyl monomers.
[0015] Styrene monomers are R 1and R 2 are hydrogen and R 3 is hydrogen or alkyl; -R4 is structure [ka] (In the formula, R 5 , R 6 , R 7 , R 8 , and R 9 each is independently hydrogen, a halogen, an aliphatic group (such as, for example, an alkyl group or a vinyl group), a substituted aliphatic group, an aryl group, a substituted aryl group, other substituted or unsubstituted organic groups, or any combination thereof. It is a vinyl monomer having the formula:
[0016] The reaction between monomers to form one or more polymers is referred to herein as a polymerization process.
[0017] As used herein, an initiator is a molecule that is stable at ambient conditions but can generate one or more fragments with free radicals under certain conditions that can interact with monomers to initiate a free radical polymerization process. Conditions that generate fragments with free radicals include, for example, high temperatures, participating in oxidation-reduction reactions, exposure to ultraviolet light and / or ionizing radiation, or combinations thereof.
[0018] As used herein, the phrase "total monomers" refers to all of the monomers used to make a polymer, including all of the monomers present when the initiation of polymerization begins and those that may be added during the polymerization process.
[0019] A polymer is said herein to contain polymerized units of the monomers used to make the polymer, even if some or all of those polymerized units are modified after polymerization by the addition of one or more functional groups. For example, a copolymer made from styrene and DVB in a weight ratio of 90:10 styrene:DVB is said to have 90% by weight polymerized units of styrene. If that copolymer is then modified by reaction with sulfuric acid to replace some of the hydrogen atoms on the aromatic rings with sulfonic acid groups, the resulting functionalized polymer would still be said to have 90% by weight polymerized units of styrene.
[0020] As used herein, an inhibitor is a molecule that reacts with vinyl monomer radicals or with radicals on a growing vinyl polymer chain to form new radicals or to form chemical species that do not participate in vinyl polymerization.
[0021] A porogen is a compound that is soluble in the monomer or mixture of monomers used in the practice of the invention, i.e., at 25° C., 100 grams or more of porogen will dissolve in 100 grams of the monomer or mixture of monomers used in the practice of the invention. The polymer does not absorb significant amounts of porogen, i.e., at 25° C., the polymer formed in the practice of the invention absorbs 5 grams or less of porogen per 100 grams of polymer.
[0022] Macroporous polymer beads have a porous structure with an average pore size of 20 nm or more. The pore size is measured using the Brunauer-Emmett-Teller (BET) method using nitrogen gas. Macroporous polymer beads are usually produced by incorporating a porogen into monomer oil droplets. The porogen is soluble in the monomer, but the polymer is not, so that phase-separated domains of the porogen remain as the polymer forms. After polymerization, the porogen is removed by evaporation or by washing with a solvent. The porous structure of the polymer beads is the empty space left when the porogen is removed from its phase-separated domains.
[0023] Gel-type polymer beads are produced without the use of porogens. The pores in gel-type polymer beads are the free volume between the atoms in the entangled, possibly cross-linked polymer chains of the polymer beads. The pores in gel-type polymer beads are smaller than 20 nm. In some cases, the pores in gel-type resins are too small to be detected using the BET method.
[0024] As used herein, ion exchange is a process in which a solution is contacted with an ion exchange resin. Prior to contact with the solution, the ion exchange resin has functional groups of a certain charge and has ions of the opposite charge associated with the functional groups. When the solution contacts the ion exchange resin, some ions in the solution bind to the ion exchange resin by exchanging places with ions of the same charge that were associated with the functional groups on the ion exchange resin.
[0025] A compound is said to be water soluble herein if 5 grams or more of the compound form a stable solution in 100 ml of water at 25° C. In the case of some water soluble polymers, the water may need to be heated above 25° C. to dissolve the polymer, but after cooling to 25° C., the solution is stable when kept at 25° C.
[0026] A suspension is a composition having particles of one substance distributed throughout a liquid medium. The distributed particles may be liquid or solid; distributed liquid particles are called oil droplets. A medium is "aqueous" if it contains 90% or more water by weight, based on the weight of the medium. A suspension may or may not be stable; that is, the distributed particles may or may not have a tendency to settle to the bottom of the container or float to the top of the container, and mechanical agitation may or may not be required to keep the particles distributed in the medium.
[0027] Polymer beads are particles that contain 90% or more by weight of organic polymers, based on the weight of the particle. Polymer beads are spherical or nearly spherical. They are characterized by their radius. If the bead is not spherical, the radius of the bead is interpreted herein as the radius of a "reference sphere", an imaginary sphere having the same volume as the bead. The sphericity of a particle is evaluated by its "sphericity", represented by the Greek letter Ψ. For a particle with volume VP and major axes of lengths a (long), b (medium) and c (short), the sphericity is:
number
[0028] As used herein, "ambient temperature" is synonymous with "room temperature" and is approximately 23°C.
[0029] The particle aggregate has a harmonic mean diameter (HMD) defined as:
number
[0030] As used herein, a suspension polymerization process is a "seed" process if the process includes the following conditions (S1): the monomer droplets contain 80% or more by weight of monomer based on the weight of the droplets; the monomer droplets have not undergone polymerization; and the monomer droplets contain polymer in an amount of 1% or more by weight based on the weight of the droplets. In a seed process, after condition (S1), polymerization of the monomer in the monomer droplets is initiated. In a typical seed process, a suspension of polymer particles is provided, then monomer is added to the suspension, the monomer is absorbed into the polymer particles, and then polymerization of the monomer is initiated.
[0031] Ratios are characterized herein as follows. For example, when a ratio is said to be 5:1 or greater, it means that the ratio can be 5:1 or 6:1 or 100:1, but not 4:1. Stated generally, when a ratio is said to be X:1 or greater, it means that the ratio is Y:1, where Y is X or greater. Similarly, for example, when a ratio is said to be 2:1 or less, it means that the ratio can be 2:1 or 1:1 or 0.001:1, but not 3:1. Stated generally, when a ratio is said to be Z:1 or less, it means that the ratio is W:1, where W is Z or less.
[0032] The process of the present invention involves monomer droplets containing a vinyl monomer and an initiator. The following is a description of the monomer droplets as they exist prior to the start of polymerization.
[0033] The monomer oil droplets optionally further contain a porogen. It is useful to characterize the sum of the amount of monomer plus the amount of porogen as a weight percentage based on the weight of the monomer oil droplets. Preferably, the sum is 95% or greater; more preferably 97% or greater; more preferably 99% or greater.
[0034] Preferably, the porogen is either absent or, if present, is present in a relatively small amount. If porogen is present in the monomer oil droplets, preferably the amount of porogen is limited to an amount of 10% or less; more preferably 3% or less; more preferably 1% or less; more preferably 0.3% or less, by weight based on the weight of the monomer oil droplets. More preferably, no porogen is present in the monomer oil droplets at all.
[0035] The following is a description of the monomer oil droplets as they exist prior to the start of polymerization.
[0036] Preferably, the amount of monomer in the monomer droplets, by weight based on the weight of the droplets, is 95% or more; more preferably 97% or more; more preferably 99% or more.
[0037] Preferred vinyl monomers are styrenic monomers, acrylic monomers, and mixtures thereof. Preferably, all the monomers used are selected from styrenic monomers, acrylic monomers, and mixtures thereof. More preferably, all the monomers used are selected from styrenic monomers. The vinyl monomers include one or more monofunctional vinyl monomers. Preferred monofunctional vinyl monomers are acrylic and styrenic monofunctional monomers; more preferably, monofunctional styrenic monomers; more preferably, styrene. The vinyl monomers also include one or more multifunctional vinyl monomers. Preferred multifunctional vinyl monomers are multifunctional styrenic monomers; more preferably, divinylbenzene. As used herein, the term "divinylbenzene" or "DVB" refers to a mixture containing approximately 63% by weight pure chemical DVB and approximately 37% by weight ethylvinylbenzene (EVB), possibly with other chemicals totaling less than 1% by weight in total. Thus, for example, a composition said to contain 4% DVB would contain approximately 2.35% EVB in addition to the 4% DVB. Preferably, the amount of vinyl chloride, by weight based on the total weight of all monomers, is 0-0.1%, more preferably 0-0.01%; more preferably 0%.
[0038] Preferably, the amount of styrene monomer in the oil droplets before the start of polymerization is, by weight based on the weight of all monomers in the oil droplets, 50% or more; more preferably 75% or more; more preferably 88% or more; more preferably 94% or more; more preferably 97% or more; more preferably 100%.
[0039] The monofunctional vinyl monomer in the oil droplet before the start of polymerization is designated MONO1. Preferably, the amount of MONO1 is, by weight based on the weight of all monomers in the oil droplet, 75% or more; more preferably 85% or more; more preferably 90% or more; more preferably 94% or more. Preferably, the amount of MONO1 is, by weight based on the weight of all monomers in the oil droplet, 99.5% or less; more preferably 99% or less; more preferably 98.5% or less.
[0040] Preferably, the amount of polyfunctional vinyl monomer in the oil droplets before the start of polymerization is 0.5% or more, more preferably 1% or more, more preferably 1.5% or more, by weight based on the weight of all monomers in the oil droplets. Preferably, the amount of polyfunctional vinyl monomer in the oil droplets is 25% or less, more preferably 15% or less, more preferably 10% or less, more preferably 6% or less, by weight based on the weight of all monomers in the oil droplets.
[0041] ratio MONORATIO=100*(WMONOTOTAL-WMONO1) / WMONOTOTAL where WMONO1 is the weight of MONO1 (the monofunctional vinyl monomer present before the start of polymerization); WMONOTOTAL is the total weight of monofunctional vinyl monomer used in the entire polymerization process, including the monofunctional vinyl monomer present before initiation and the monofunctional vinyl monomer added after initiation. It is useful to characterize MONORATIO as follows: Preferably, MONORATIO is 0.05% or more; more preferably, 0.1% or more; more preferably, 0.2% or more; more preferably, 0.4% or more. Preferably, MONORATIO is 30% or less; more preferably, 25% or less; more preferably, 20% or less; more preferably, 15% or less. Preferably, MONORATIO is 2% or more; more preferably, 4% or more; more preferably, 6% or more; more preferably, 8% or more.
[0042] The method of the present invention involves the suspension of monomer oil droplets in an aqueous medium prior to the initiation of polymerization. Preferably, the total amount of monomer prior to the initiation of polymerization is 15% or more; more preferably 20% or more; more preferably 25% or more; more preferably 30% or more, by volume, based on the total volume of the suspension prior to the initiation of polymerization. Preferably, the total amount of monomer prior to the initiation of polymerization is 55% or less; more preferably 50% or less; more preferably 45% or less, by volume, based on the total volume of the suspension.
[0043] After polymerization is completed, the amount of polymeric beads in the suspension, by volume, based on the total volume of the suspension, is 18% or more; more preferably 23% or more; more preferably 28% or more. After polymerization is completed, the amount of polymeric beads in the suspension, by volume, based on the total volume of the suspension, is 58% or less; more preferably 53% or less; more preferably 48% or less.
[0044] The aqueous medium optionally contains one or more dissolved nitrites, derivatives of the nitrites, or combinations thereof. The nitrites are represented by the formula M(NO 2 ) v where M is an ammonium cation or an alkali metal cation or an alkaline earth cation; and where v is 1 when M is an ammonium cation or an alkali metal cation and v is 2 when M is an alkaline earth cation. When the nitrite salt dissolves in water, the nitrite ion undergoes a chemical reaction to form, for example, nitrous acid and / or a compound of the formula N x O yIt is believed that the nitrites and derivatives thereof form derivatives such as compounds of the formula: ##STR1## The amount of these derivatives is characterized by the amount of dissolved salt plus the amount of salt that would have to be dissolved to produce the amount of derivative present in the aqueous medium. The preferred amount of nitrites and derivatives thereof is 0.005% or more; more preferably 0.008% or more; more preferably 0.011% or more; more preferably 0.014% or more, by weight based on the weight of the aqueous medium. The preferred amount of nitrites and derivatives thereof is 0.5% or less; more preferably 0.4% or less; more preferably 0.3% or less; more preferably 0.2% or less, by weight based on the weight of the aqueous medium.
[0045] A preferred nitrite is sodium nitrite. Preferably, the nitrite derivative is a sodium nitrite derivative.
[0046] The monomer oil droplets preferably contain one or more initiators. Preferred initiators have a solubility of 1 gram or less in 100 mL of water at 25°C; more preferably 0.5 grams or less; more preferably 0.2 grams or less; more preferably 0.1 grams or less. Peroxide and hydroperoxide initiators are preferred; peroxide initiators are more preferred; benzoyl peroxide and its derivatives are more preferred; benzoyl peroxide is more preferred. Preferably, the weight ratio of initiator to total monomer is 0.0005:1 or more; more preferably 0.002:1 or more; more preferably 0.005:1 or more. Preferably, the weight ratio of initiator to total monomer is 0.02:1 or less; more preferably 0.01:1 or less; more preferably 0.007:1 or less.
[0047] The monomer oil droplets optionally contain one or more porogens. Preferably, little or no porogen is present. That is, preferably, porogens are absent or, if present, the amount of porogen is 1% or less by weight based on the weight of the monomer oil droplets; more preferably, 0.1% or less. More preferably, no porogen is present in the monomer oil droplets.
[0048] Monomers, as typically supplied by manufacturers, contain relatively small amounts of inhibitors to prevent unintended polymerization during storage. Common inhibitors are quinones (e.g., 1,4-benzoquinone) and hindered phenols (e.g., 4-tert-butylpyrocatechol, also known as 4-t-butylcatechol).
[0049] Preferably, prior to the start of polymerization, the monomer oil droplets contain either no polymer of any kind or only small amounts of polymer of any kind, i.e., if any polymer is present in the monomer oil droplets, the total amount of polymer is preferably 0.1% or less by weight based on the weight of the monomer oil droplets; more preferably, it is zero.
[0050] The aqueous medium preferably contains one or more water-soluble polymers. Preferred water-soluble polymers are water-soluble polyvinyl alcohol polymers, water-soluble derivatives of cellulose, quaternary ammonium polymers, gelatin, and mixtures thereof. More preferred water-soluble polymers are water-soluble polyvinyl alcohol polymers, water-soluble derivatives of cellulose, and mixtures thereof. Among the quaternary ammonium polymers, a polymer of diallyl ammonium chloride (DADMAC) is preferred. Among the water-soluble derivatives of cellulose, carboxymethyl methylcellulose is preferred. Among the polyvinyl alcohol polymers, those with a degree of hydrolysis of 80% to 90% are preferred. Preferably, the aqueous medium contains one or more water-soluble polyvinyl alcohol polymers and one or more water-soluble derivatives of cellulose.
[0051] When one or more water-soluble polymers are used, preferably the total amount of water-soluble polymers is, by weight based on the weight of the aqueous medium, 0.02% or more; more preferably 0.05% or more; more preferably 0.1% or more. When one or more water-soluble polymers are used, preferably the total amount of water-soluble polymers is, by weight based on the weight of water, 1% or less; more preferably 0.5% or less.
[0052] Other methods of stabilizing monomer oil droplets are also suitable, which can be used instead of or in addition to one or more water-soluble polymers.For example, solid particles smaller than the monomer oil droplets can be present on the surface of the oil droplets to stabilize the oil droplets.One example of such solid particles is colloidal silica particles.
[0053] The aqueous suspension of monomer oil droplets optionally contains one or more suspending aids. The suspending aids are believed to stabilize the monomer oil droplets. The suspending aids may be introduced by adding them to the aqueous phase or by adding them to the monomer oil droplets, or a combination thereof. Regardless of the manner in which the suspending aid is introduced, the preferred amount of suspending aid is 0.001% to 0.1%, by weight, based on the weight of the monomer oil droplets. A preferred suspending aid is 4-vinylphenylboronic acid.
[0054] Gelatin may or may not be present in the suspension. If gelatin is present, the amount is 2% or less; or 1% or less; or 0.5% or less, by weight based on the weight of water. Preferred embodiments have little or no gelatin. Preferably, the amount of gelatin is low enough that the amount of gelatin is 0-0.01%; more preferably 0-0.001%, by weight based on the weight of water. More preferably, the amount of gelatin is zero.
[0055] The nature of the step of initiating the polymerization depends to some extent on the nature of the initiator used. For example, if a thermal initiator is used, the initiation conditions include establishing a temperature above 25°C that is high enough for a significant portion of the initiator molecules to decompose and form free radicals. For another example, if a photoinitiator is used, the initiation conditions include exposing the initiator to radiation of a sufficiently low wavelength and high enough intensity for a significant portion of the initiator molecules to decompose and form free radicals. For another example, if the initiator is a redox initiator, the initiation conditions include the presence of both an oxidizing agent and a reducing agent in a sufficiently high concentration so that a significant number of free radicals are generated. Preferably, a thermal initiator is used. Preferably, the initiation conditions include a temperature of 65°C or higher, more preferably 70°C or higher. That is, preferably, the suspension is provided at a temperature below 40°C, and the initiator present does not generate a significant number of free radicals at that temperature. Then, preferably, step (b) includes increasing the temperature to the initiation conditions.
[0056] After step (b), at any instant while the polymerization is occurring, the degree of free radical polymerization in the vessel containing the suspension can be characterized as follows: Degree of polymerization=100*PM / TM where PM is the mass of polymer formed by the free radical polymerization process, and TM is the total mass of monomer added to the vessel up to that moment, including the monomer in the oil droplets prior to polymerization and the monomer added in the monomer feed solution up to that moment.
[0057] Prior to the start of the polymerization process, the oil droplets are in suspension, the oil droplets containing the vinyl monomer and the initiator. Preferably, the oil droplets are distributed throughout the aqueous medium. Preferably, the composition of the aqueous medium contains water in an amount of 90% or more; more preferably 95% or more; more preferably 98% or more, by weight based on the weight of the aqueous medium. Compounds dissolved in water are considered to be part of the continuous liquid medium. Preferably, the volume average particle size of the oil droplets is 50 μm to 1,500 μm.
[0058] In the process of the present invention, the feed solution is added to the suspension as soon as polymerization in the monomer droplets has begun. The act of adding monomer to the suspension after polymerization has begun is known herein as "gradual addition", or GA. The feed solution may be added at any rate. The rate of addition of the feed solution may be constant or may be faster at some times than at others. The addition of the feed solution may be accomplished in a single continuous addition (which may be done quickly or slowly), or the addition of the feed solution may be interrupted one or more times.
[0059] Addition of Feed Solution is initiated when the reaction progress is at a point denoted herein as "EXTSTART." EXTSTART is between 0% and 50%, inclusive. Preferably, EXTSTART is 40% or less; more preferably 30% or less; more preferably 20% or less; more preferably 10% or less.
[0060] The reaction progress "EXTSTOP" is the reaction progress at which the last of the feed solution is added to the suspension. No feed solution is added to the suspension after EXTSTOP. EXTSTOP is between 5% and 100%. Preferably, EXTSTOP is 85% or less. Preferably, the amount EXTDIFF=EXTSTOP-EXTSTART is 5% or more; more preferably 20% or more; more preferably 50% or more; more preferably 60% or more.
[0061] Preferably, the feed solution contains total vinyl monomers of all types in an amount, by weight based on the weight of the feed solution, of 75% or more; more preferably 85% or more; more preferably 95% or more; more preferably 99% or more.
[0062] The amount of monofunctional monomer in the feed solution is preferably, by weight based on the weight of the feed solution, 50% or more; preferably 60% or more; more preferably 70% or more; more preferably 80% or more; more preferably 90% or more; more preferably 95% or more; more preferably 99% or more.
[0063] For use in the feed solution, the preferred monofunctional vinyl monomers are the same as those described above as preferred for use in the monomer oil droplets. When multifunctional vinyl monomers are present in the feed solution, the preferred multifunctional vinyl monomers are the same as those described above as preferred for use in the monomer oil droplets.
[0064] It is useful to characterize the ratio of polyfunctional vinyl monomer to monofunctional vinyl monomer and compare the ratio in the oil droplet with the same ratio in the feed solution. WMONO1 is the total weight of monofunctional vinyl monomer in the oil droplet; WMULTI1 is the total weight of polyfunctional vinyl monomer in the oil droplet; WMONO2 is the total weight of monofunctional vinyl monomer in the feed solution; WMULTI2 is the total weight of polyfunctional vinyl monomer in the feed solution. The comparison ratio COMPRATIO is defined as the ratio of (WMULTI2 / WMONO2) to (WMULTI1 / WMONO1). Preferably, COMPRATIO is less than 1:1; more preferably 0.1:1 or less; more preferably 0.01:1 or less; more preferably 0:1.
[0065] Preferably, the feed solution contains either no initiator or contains initiator in an amount, in parts per million by weight, of 100 ppm or less; more preferably 10 ppm or less; more preferably 1 ppm or less.
[0066] Preferably, the feed solution either contains no water or contains water in an amount, by weight based on the weight of the feed solution, of 70% or less; more preferably 20% or less; more preferably 10% or less; more preferably 3% or less; more preferably 1% or less; more preferably 0.3% or less; more preferably 0.1% or less.
[0067] It is also useful to characterize the total amount of feed solution used throughout the process of the present invention. The total weight of all monomers in all of the feed solutions added to the reaction vessel is WFEED. The total weight of all monomers in the monomer droplets before the start of polymerization is WDROP. The amount % FEED is %FEED=100×WFEED / WDROP It is defined as follows.
[0068] Preferably, %FEED is 5% or more; more preferably, 8% or more, more preferably, 10% or more. Preferably, %FEED is 25% or less; more preferably, 20% or less; more preferably, 15% or less.
[0069] Preferably, the method is not a seed process.
[0070] Also envisioned are embodiments in which the feed solution is replaced with a feed composition that is a dispersion of monomer oil droplets in an aqueous medium ("dispersion feed" embodiments). Such a dispersion can be any type of dispersion, such as, for example, a suspension, an emulsion, a microemulsion, or a nanoemulsion. Such a dispersion optionally contains one or more water-soluble polymers, one or more surfactants, one or more dispersants, or mixtures thereof, as described above. Among the dispersion feed embodiments, emulsions are preferred. Among the emulsions, those that contain one or more anionic surfactants are preferred.
[0071] In a dispersive feed embodiment, the total amount of monomers in the feed composition, by weight based on the weight of the feed composition, is 5% or more; more preferably 10% or more; more preferably 20% or more; more preferably 40% or more. In a dispersive feed embodiment, the total amount of monomers in the feed composition, by weight based on the weight of the feed composition, is 60% or less; more preferably 55% or less.
[0072] In a dispersed feed embodiment, it is useful to characterize the amount of monofunctional vinyl monomer as a weight percentage of the monomer content of the feed composition. In dispersed embodiments, preferably the amount of monofunctional vinyl monomer is 98% to 100%; more preferably 99% to 100%, by weight based on the total weight of monomers in the feed composition.
[0073] In the dispersed feed embodiment, the suitable and preferred conditions for feeding during polymerization (such as reaction progress) are the same as those described above.
[0074] The present invention also includes a population of polymer beads. The population of polymer beads is preferably produced by the method of the present invention. The polymer beads contain a polymer. The polymer beads are particles that are solid at 25° C. and contain a polymer in an amount of 90% or more; more preferably 95% or more, by weight based on the weight of the polymer particles.
[0075] The polymer beads can be macroporous beads or gel beads, with gel beads being preferred.
[0076] Preferably, the polymer beads have a volume average particle size of 50 μm or more, more preferably 100 μm or more, more preferably 200 μm or more, more preferably 400 μm or more. Preferably, the polymer beads have a volume average particle size of 1,500 μm or less, more preferably 1,000 μm or less.
[0077] The preferred polymers in the polymer particles are those formed by free radical polymerization of the preferred vinyl monomers described above. Preferably, the polymer contains polymerized units of styrenic monomers in an amount of 5% or more; more preferably 25% or more; more preferably 50% or more; more preferably 75% or more; more preferably 85% or more; more preferably 95% or more, by weight based on the weight of the polymer. The types of monomers preferred as polymerized units of the polymer are the same as those described above as preferred for use in the polymerization process.
[0078] Preferred polymers have polymerized units of multifunctional vinyl monomers in an amount, by weight, based on the weight of the polymer, of 0.3% or more; more preferably 0.5% or more; more preferably 1% or more; more preferably 1.5% or more. Preferred polymers have polymerized units of multifunctional vinyl monomers in an amount, by weight, based on the weight of the polymer, of 25% or less; more preferably 15% or less; more preferably 11% or less; more preferably 6% or less.
[0079] Preferred polymers have polymerized units of monofunctional vinyl monomers in an amount, by weight, based on the weight of the polymer, of 99.7% or less; more preferably 99.5% or less; more preferably 99% or less; more preferably 98.5% or less. Preferred polymers have polymerized units of monofunctional vinyl monomers in an amount, by weight, based on the weight of the polymer, of 75% or more; more preferably 85% or more; more preferably 89% or more; more preferably 94% or more.
[0080] The polymeric beads preferably have an average sphericity of 0.8 or greater; more preferably 0.85 or greater; more preferably 0.9 or greater; more preferably 0.95 or greater.
[0081] A preferred use of the polymers produced by the free radical polymerization process of the present invention is in a conversion process to produce ion exchange resins. Ion exchange resins fall into the following categories: Weakly basic anion exchange resins have pendant amino groups that are primary, secondary, or tertiary. Strongly basic anion exchange resins have pendant quaternary amino groups. Weakly acidic cation exchange resins have pendant carboxylic acid groups. Strongly acidic cation exchange resins have pendant sulfonic acid groups. When any of these pendant functional groups are attached to a polymer bead, the bead is said to be a "functionalized resin."
[0082] Typically, in the preparation of weakly basic anion exchange resins from polymer beads such as crosslinked polystyrene beads, the beads are advantageously haloalkylated, preferably halomethylated, most preferably chloromethylated, and ionically active exchange groups are then attached to the haloalkylated copolymer. Typically, the haloalkylation reaction consists of swelling the crosslinked addition copolymer with a haloalkylating agent, preferably bromomethyl methyl ether, chloromethyl methyl ether, or a mixture of formaldehyde and hydrochloric acid, most preferably chloromethyl methyl ether, and then reacting the copolymer with the haloalkylating agent in the presence of a Friedel-Crafts catalyst such as zinc chloride, iron chloride, or aluminum chloride. Typically, weakly basic anion exchange resins are prepared by reacting the haloalkylated copolymer with ammonia, a primary amine, or a secondary amine. Typically, strongly basic anion exchange resins are prepared by reacting the haloalkylated copolymer with a tertiary amine.
[0083] Typically, in the preparation of strongly acidic cation exchange resins from polymer beads, such as crosslinked polystyrene beads, the beads are advantageously sulfonated. Generally, the beads are swollen using a suitable swelling agent, and the swollen beads are reacted with a sulfonating agent, such as sulfuric acid or chlorosulfonic acid or sulfur trioxide, or mixtures thereof.
[0084] It is believed that the polymer beads of the present invention will be useful for a variety of purposes. The functionalized polymer beads will be useful for many of the purposes for which ion exchange resins are useful. For example, it is expected that the functionalized polymer beads of the present invention will be useful as water purification resins or as catalysts.
[0085] Some of the benefits expected from the present invention are explained as follows: In the historical process of suspension polymerization (i.e., the process known before the present invention and which did not include feeding of monomer during the polymerization process as described in the present invention), the amount of multifunctional vinyl monomer determined both the MHC and other resin properties. To achieve the target MHC value, a sufficient amount of multifunctional vinyl monomer was used, and if that amount of multifunctional vinyl monomer caused deterioration of other resin properties, that deterioration had to be accepted as inevitable. In contrast, in the practice of the present invention, a lower amount of multifunctional vinyl monomer results in an MHC that previously could only be obtained using a higher amount of DVB. Therefore, by using the present invention, the target MHC can be reached while reducing the risk of property deterioration that may be caused by high levels of multifunctional vinyl monomer. Thus, the method of the present invention can be considered to make more efficient use of the multifunctional vinyl monomer present in the final beads by making it possible to reach the target properties while using a reduced amount of multifunctional vinyl monomer. EXAMPLES
[0086] The following are examples of the present invention.
[0087] The following terms, abbreviations, and ingredients were used: Jetting = Introducing monomer oil droplets into an aqueous medium using the jetting procedures described in U.S. Pat. Nos. 4,444,960 and 4,623,706. tBC = 4-t-butylcatechol, which is present in the grade of DVB used. DVB = divinylbenzene. The grade of DVB used was manufactured by Dow Chemical Company and was a mixture containing 63% pure divinylbenzene and approximately 37% ethylvinylbenzene (EVB) by weight. The percentages of DVB given herein refer to the amount of pure DVB. It is assumed that EVB will also be present in a weight ratio of DVB:EVB of approximately 63:37. CMMC = Carboxymethyl methylcellulose, manufactured by The Dow Chemical Company PVOH = SELVOL manufactured by Sekisui Specialty Chemicals TM 523 Polyvinyl alcohol SBA = Strongly basic anion exchange resin; a copolymer of styrene / DVB functionalized with quaternary ammonium groups SAC = Strong Acid Cation Exchange Resin; a copolymer of styrene / DVB functionalized with sulfonic acid groups. Tris = tris(hydroxymethyl)aminomethane, a 20% solution by weight in water VPBA = 4-vinylphenylboronic acid BPO = benzoyl peroxide, 75% purity by weight DI Water = Deionized Water GA=gradual addition MHC=water holding capacity Ambient temperature = approx. 23°C
[0088] In preparing the oil droplet mixture or the aqueous medium described below, some of the submixtures were sometimes heated above 25° C. to achieve good mixing. However, when the oil droplets were formed and suspended in the aqueous medium, the components were all at ambient temperature.
[0089] When the copolymers were converted to SAC resins, the conversion was carried out by a standard sulfonation process using sulfuric acid to achieve a degree of substitution such that 95 mole % or more of the aromatic rings of the polymerized units of the monofunctional vinyl monomer carried a sulfonate group.
[0090] The water holding capacity (MHC) was measured as follows. Briefly, excess water was removed from the resin under humid air to produce a dehydrated but moist resin. The moist resin was weighed, dried, and reweighed. The relative weight loss upon drying is the water holding capacity. In detail, 50 mL of resin particle aggregate was mixed with 50 mL of deionized (DI) water. The mixture was placed in a Buchner funnel on a vacuum flask, and the water was allowed to drain from the sample under gravity. The sample was capped with a rubber stopper connected to a hose supplying air with 100% relative humidity from a humidification tower. The vacuum flask was evacuated to provide an air flow of 4.0 L / min for 5 min. The result is a dehydrated moist resin. Then, 4-5 g of resin was weighed (Wm), then dried in an oven at 105 °C for 18 h, and then reweighed (Wd). The water holding capacity (MHC) was calculated as: MHC(%)=100*(Wm-Wd) / Wm Given by.
[0091] In all examples the weight ratio of oil droplet component to aqueous phase component was 0.61: 1. The oil droplets were formed by jetting as defined above.
[0092] Comparative A-1Comp and Example A-2d. The oil droplets were formed by jetting. The composition of the oil droplets in the following examples was as follows: Amounts are in weight percent based on the weight of the monomer oil droplets. The total weight of each monomer oil droplet composition was 100%. Samples with the suffix "Comp" are used in the comparative method. In all cases, the aqueous phase concentration of the stabilizer was such that the percentage of the beads having a sphericity of 0.8 or greater was 99% or greater, based on the total number of beads. In all cases, the aqueous or monomer phase concentration of the stabilizer coagent was such that the percentage of the beads having a sphericity of 0.8 or greater was 99% or greater, based on the total number of beads. In all cases, the aqueous phase concentration of the latex inhibitor was such that the weight percentage of the emulsion polymer at the end of the reaction was less than 0.5%, based on the total weight of the polymer beads. In all cases, the harmonic mean size of the final polymer particles was 430-470 microns.
[0093] [Table 1]
[0094] The compositions of the aqueous vehicles in the following examples were as follows:
[0095] [Table 2]
[0096] Aqueous suspension polymerization was carried out on the suspension as follows.
[0097] For A-1Comp, an aqueous suspension polymerization was carried out on the reaction mixture as follows: A combination of reaction temperature and BPO concentration was selected to give a degree of conversion of 80-85% within 330-390 minutes. As soon as the conversion to polymer was in the 80-85% range, the pH was adjusted by Tris addition to the reactor so that the final pH was in the 8-9 range. The reaction system was heated to 97°C. After 1 hour at 97°C, the system was cooled to ambient temperature and the beads were dehydrated, washed with water and dried at ambient temperature. Two identical polymerizations were carried out.
[0098] For Example A-2d, aqueous suspension polymerization was carried out on the reaction mixture as follows: A combination of reaction temperature and BPO concentration was selected to provide 80-85% conversion within 390-550 minutes. As soon as the reaction temperature was reached, a continuous feed of styrene to the reactor was started and maintained from 0% conversion to 56% conversion. The styrene feed rate was varied over time.
[0099] Once the conversion to polymer was in the range of 60-75%, Tris was added to the reactor so that the final pH was in the range of 8-9. Within 60 minutes of Tris addition, the reaction was heated to 97°C. After 1 hour, the reaction was cooled to ambient temperature and the beads were dehydrated, washed with water, and dried at ambient temperature.
[0100] The water holding capacity (MHC) of the sulfonated resins was as follows:
[0101] [Table 3]
[0102] The MHC values were essentially the same for the two samples, but Example A-2d only had 4.1% DVB while the comparative example had 4.65% DVB. Thus, the examples had the same MHC with 12% less DVB. (Aspect) (Aspect 1) 1. A method for producing a collection of polymer beads, comprising: (i) 75 to 99.7% by weight of polymerization units of a monofunctional vinyl monomer based on the weight of the beads; (ii) 0.3 to 25% by weight of a polymerized unit of a polyfunctional vinyl monomer based on the weight of the beads; Includes; The method further comprising: (a) providing an aqueous suspension of monomer oil droplets comprising an initiator, a multifunctional vinyl monomer, and a monofunctional vinyl monomer; (b) initiating polymerization of the monomer in the monomer oil droplets; (c) adding a monomer feed solution to the suspension while the polymerization of the monomers in the monomer oil droplets is occurring, The step of adding begins when the degree of polymerization (EXTSTART) of the monomer in the monomer oil droplet is 0% to 50%, and The adding step is terminated when the degree of polymerization (EXTSTOP) of the monomer in the monomer oil droplet is 5% to 100% after EXTSTART; the feed solution comprises monomer in an amount of 90% to 100% by weight based on the weight of the feed solution; The feed solution comprises a monofunctional vinyl monomer in an amount of 50% to 100% by weight based on the weight of the feed solution. Process The method includes: (Aspect 2) 2. The method of embodiment 1, wherein the amount EXTDIF=EXTSTOP-EXTSTART is greater than or equal to 5%. (Aspect 3) The method of embodiment 1, wherein the monofunctional vinyl monomer comprises styrene. (Aspect 4) 2. The method of claim 1, wherein the multifunctional vinyl monomer comprises divinylbenzene. (Aspect 5) 2. The method of embodiment 1, wherein the weight ratio of multifunctional vinyl monomer to monofunctional vinyl monomer in the feed solution is lower than the weight ratio of multifunctional vinyl monomer to monofunctional vinyl monomer in the monomer oil droplets.
Claims
1. 1. A method for producing a collection of polymer beads, comprising: (i) 75 to 99.7 weight percent polymerized units of a monofunctional vinyl monomer, based on the weight of the beads; (ii) 0.3 to 25% by weight of polymerized units of a polyfunctional vinyl monomer, based on the weight of the beads; Including; The method further comprising: (a) providing an aqueous suspension of monomer oil droplets comprising an initiator, said multifunctional vinyl monomer, and said monofunctional vinyl monomer; (b) initiating polymerization of the monomers in the monomer oil droplets; (c) adding a monomer feed solution to the suspension while the polymerization of the monomers in the monomer oil droplets is occurring, The step of adding begins when the degree of polymerization (EXTSTART) of the monomer in the monomer oil droplets is between 0% and 50%, and The step of adding ends when the degree of polymerization (EXTSTOP) of the monomer in the monomer oil droplet is 5% to 85% after EXTSTART; the feed solution comprises monomer in an amount of 90% to 100% by weight based on the weight of the feed solution; The feed solution comprises the monofunctional vinyl monomer in an amount of 50% to 100% by weight based on the weight of the feed solution. process Including, the monofunctional vinyl monomer comprises a styrenic monomer; The styrenic monomer has the structure: [Formula 1] [In the formula, R 1 and R 2 are hydrogen, and R 3 is hydrogen or alkyl; -R 4 But the structure [chemical 2] (In the formula, R 5 , R 6 , R 7 , R 8 , and R 9 each of which is independently hydrogen, a halogen, an aliphatic group, a substituted aliphatic group, an aryl group, a substituted aryl group, or any combination thereof; a weight ratio of said multifunctional vinyl monomer to said monofunctional vinyl monomer in said feed solution is lower than a weight ratio of said multifunctional vinyl monomer to said monofunctional vinyl monomer in said monomer oil droplets; The method wherein the multifunctional vinyl monomer comprises divinylbenzene.
2. The method of claim 1 , wherein the amount EXTDIF=EXTSTOP-EXTSTART is greater than or equal to 5%.
3. The method of claim 1 , wherein the monofunctional vinyl monomer comprises styrene.
Citation Information
Patent Citations
Manufacture of copolymer, product and use
JP1984018705A
Manufacture of bridged copolymer beads
JP1984098117A
Production of modified styrenic polymer beads for producing foamed cup
JP1987209154A
Acrylic polymer particle, its production and molding composition containing same
JP1990225508A
Preparation of crosslinked polymer fine particle
JP1992096902A