Amorphous Polyester Resin

The amorphous polyester resin, formulated with specific repeating units, addresses high processing temperature issues in liquid crystal polyester resins by enhancing low-temperature processability and mechanical strength, suitable for low-temperature applications and polymer alloys.

JP7578505B2Active Publication Date: 2024-11-06UENO PHARMA CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021027631
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-24
Publication Date
2024-11-06
Estimated Expiration
2041-02-24

AI Technical Summary

Technical Problem

Existing liquid crystal polyester resins face challenges with high processing temperatures, limiting their low-temperature processability and compatibility with low-melting-point thermoplastic resins, leading to thermal decomposition.

Method used

An amorphous polyester resin is developed through condensation polymerization of specific repeating units, with a composition ratio of p:q:r:s:t:u = 35-65:15-45:5-15:5-15:0-10:0-10, and a glass transition temperature of 180°C or lower, enhancing low-temperature processability and mechanical properties.

Benefits of technology

The amorphous polyester resin exhibits improved low-temperature processability and mechanical strength, suitable for applications requiring low-temperature processing and as a polymer alloy material with other thermoplastic resins.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578505000001
    Figure 0007578505000001
  • Figure 0007578505000002
    Figure 0007578505000002
  • Figure 0007578505000003
    Figure 0007578505000003
Patent Text Reader

Abstract

To provide an amorphous polyester resin that is improved in low-temperature workability and has excellent mechanical properties.SOLUTION: This invention relates to an amorphous polyester resin containing repeat units represented by formulae (I)-(VI).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an amorphous polyester resin having low-temperature processability and good mechanical properties. [Background technology]

[0002] Thermotropic liquid crystal polyester resin (hereinafter referred to as liquid crystal polyester resin or LCP) is excellent in heat resistance, mechanical properties such as rigidity, chemical resistance, dimensional accuracy, etc., and therefore its use is expanding not only for molded products but also for various applications such as fibers and films. Particularly in the information and communication field such as personal computers and mobile phones, the integration density, miniaturization, thinning, and low height of parts are rapidly increasing, and there are many cases where very thin parts of 0.5 mm or less are formed, so the use of LCP has increased significantly by taking advantage of its excellent moldability, i.e., good fluidity and no flash, which are characteristics not found in other resins.

[0003] As described above, liquid crystal polyester resins have various excellent properties, but due to their high heat resistance, their processing temperature is significantly higher than that of other engineering plastics such as polyethylene terephthalate, polybutylene terephthalate, polycarbonate, etc. For this reason, depending on the application, the high processing temperature may become an obstacle.

[0004] In addition, polyester resins have been found to have the effect of modifying the physical properties of other thermoplastic resins, and demand for them as polymer alloy materials is increasing, so there has been a demand for polyester resins that have excellent low-temperature processability while retaining the good mechanical properties of liquid crystal polyester resins.

[0005] As a low-temperature processable polyester resin, for example, Patent Document 1 proposes a liquid crystal polyester resin that is composed of specific repeating units and has a melting point of 190 to 250° C. as measured by a differential scanning calorimeter. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2005-105232 A Summary of the Invention [Problem to be solved by the invention]

[0007] The liquid crystal polyester resin described in Patent Document 1 has excellent low-temperature processability compared to conventional liquid crystal polyester resins, but in recent years, there has been an increasing demand for polyester resins with even improved processability at low temperatures.

[0008] In addition, in order to blend a liquid crystal polyester resin with a low melting point thermoplastic resin such as polypropylene or polyethylene, which has a melting point below 200°C, it is necessary to melt-knead the resin at a temperature equal to or higher than the melting point of the liquid crystal polyester resin. This poses the problem that the thermoplastic resin is thermally decomposed, making it impossible to obtain the original physical properties.

[0009] An object of the present invention is to provide an amorphous polyester resin having improved low temperature processability and good mechanical properties. [Means for solving the problem]

[0010] In view of the above problems, the present inventors conducted intensive research and discovered that an amorphous polyester resin having improved low-temperature processability and good mechanical properties can be obtained by condensation polymerization of a monomer that gives a specific repeating unit, thereby completing the present invention.

[0011] That is, the present invention includes the following preferred embodiments. [1] Formulas (I) to (VI) [ka] In the formula, p, q, r, s, t, and u each represent a composition ratio (mol %) of each repeating unit in the amorphous polyester resin and satisfy the following formula: 35≦p≦65, 15≦q≦45, 5≦r≦15, 5≦s≦15, 0 ≤ t ≤ 10, and 0≦u≦10] An amorphous polyester resin comprising a repeating unit represented by the formula: [2] The amorphous polyester resin according to [1], further satisfying p>q. [3] The amorphous polyester resin according to [1] or [2], further satisfying p+q+r+s+t+u=100. [4] The amorphous polyester resin according to any one of [1] to [3], which has a bending strength of 140 MPa or more. [5] The amorphous polyester resin according to any one of [1] to [4], which has a glass transition temperature of 180° C. or lower as measured by a differential scanning calorimeter. [6] An amorphous polyester resin composition comprising 100 parts by mass of the amorphous polyester resin according to any one of [1] to [5] and 0.1 to 200 parts by mass of a fibrous, plate-like or granular filler. [7] A molded article comprising the amorphous polyester resin according to any one of [1] to [5] or the amorphous polyester resin composition according to [6]. Effect of the Invention

[0012] The amorphous polyester resin of the present invention has improved low-temperature processability and good mechanical properties, and is therefore useful in applications requiring low-temperature processability or as a polymer alloy material with other thermoplastic resins. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] In this specification and claims, "amorphous polyester resin" means a polyester resin which does not show a crystalline melting temperature in differential scanning calorimetry at a heating rate of 20°C / min and which softens near the glass transition temperature.

[0014] The amorphous polyester resin of the present invention contains aromatic oxycarbonyl repeating units represented by formula (I) and formula (II) as repeating units.

[0015] [ka]

[0016] In the amorphous polyester resin of the present invention, the composition ratio p of the repeating unit represented by formula (I) to the amorphous polyester resin is 35 to 65 mol%, preferably 35 to 60 mol%, more preferably 40 to 60 mol%, and the composition ratio q of the repeating unit represented by formula (II) to the amorphous polyester resin is 15 to 45 mol%, preferably 20 to 45 mol%, more preferably 20 to 40 mol%.

[0017] In the amorphous polyester resin of the present invention, the repeating units represented by formula (I) and formula (II) preferably satisfy the relationship p>q, with p / q being more preferably 1.01 to 2.0, even more preferably 1.03 to 1.9, and particularly preferably 1.08 to 1.8.

[0018] Examples of monomers which provide the repeating unit represented by formula (I) include 4-hydroxybenzoic acid and its ester-forming derivatives such as acylation products, ester derivatives and acid halides.

[0019] Examples of monomers which provide the repeating unit represented by formula (II) include 6-hydroxy-2-naphthoic acid and its ester-forming derivatives such as acylation products, ester derivatives and acid halides.

[0020] The amorphous polyester resin of the present invention also contains an aromatic dioxy repeat unit represented by formula (III).

[0021] [ka]

[0022] In the amorphous polyester resin of the present invention, the composition ratio r of the repeating unit represented by formula (III) to the amorphous polyester resin is 5 to 15 mol %, preferably 5 to 12 mol %, and more preferably 5 to 10 mol %.

[0023] Examples of monomers which provide the repeating unit represented by formula (III) include 4,4'-dihydroxybiphenyl and its acylated and other ester-forming derivatives.

[0024] Additionally, the amorphous polyester resin of the present invention contains aromatic dicarbonyl repeat units represented by formula (IV).

[0025] [ka]

[0026] In the amorphous polyester resin of the present invention, the composition ratio s of the repeating unit represented by formula (IV) to the amorphous polyester resin is 5 to 15 mol %, preferably 5 to 12 mol %, and more preferably 5 to 10 mol %.

[0027] Examples of monomers which provide the repeating unit represented by formula (IV) include isophthalic acid and its ester-forming derivatives such as ester derivatives and acid halides.

[0028] From the standpoint of heat resistance, strength, electrical properties, etc., the amorphous polyester resin of the present invention may further contain repeating units represented by formula (V) and / or formula (VI) as aromatic dicarbonyl repeating units.

[0029] [ka]

[0030] In the amorphous polyester resin of the present invention, the composition ratio t of the repeating unit represented by formula (V) to the amorphous polyester resin is 0 to 10 mol%, and when it is contained, it is preferably 1 to 10 mol%, more preferably 2 to 7 mol%, and even more preferably 3 to 5 mol%. Also, the composition ratio u of the repeating unit represented by formula (VI) to the amorphous polyester resin is 0 to 10 mol%, and when it is contained, it is preferably 1 to 10 mol%, more preferably 2 to 6 mol%, and even more preferably 3 to 4 mol%.

[0031] Examples of monomers which provide the repeating unit represented by formula (V) include 2,6-naphthalenedicarboxylic acid and its ester-forming derivatives such as ester derivatives and acid halides.

[0032] Examples of monomers which provide the repeating unit represented by formula (VI) include terephthalic acid and its ester-forming derivatives such as ester derivatives and acid halides.

[0033] In the amorphous polyester resin of the present invention, the total composition ratio of the repeating units [p+q+r+s+t+u] is preferably 100 mol %, but other repeating units may be further contained within a range that does not impair the object of the present invention.

[0034] Examples of monomers that provide other repeating units constituting the amorphous polyester resin of the present invention include other aromatic hydroxycarboxylic acids, other aromatic diols, other aromatic dicarboxylic acids, aromatic hydroxyamines, aromatic hydroxydicarboxylic acids, aromatic diamines, aromatic aminocarboxylic acids, aromatic mercaptocarboxylic acids, aromatic dithiols, aromatic mercaptophenols, and combinations thereof.

[0035] The proportion of repeating units provided by these other monomer components is preferably 10 mol % or less in the total repeating units.

[0036] The method for producing the amorphous polyester resin of the present invention will be described below.

[0037] The method for producing the amorphous polyester resin of the present invention is not particularly limited, and any known polyester polycondensation method for forming an ester bond between the above-mentioned monomer components, such as a melt acidolysis method or a slurry polymerization method, can be used.

[0038] The molten acidolysis process is the preferred method for producing the amorphous polyester resins of the present invention. In this process, the polymerizable monomers are first heated to form a molten solution of the reactants, and then the polycondensation reaction is continued to obtain a molten polymer. A vacuum may be applied to facilitate removal of volatile by-products (e.g., acetic acid, water, etc.) produced during the final stage of condensation.

[0039] A slurry polymerization process is a process in which polymerizable monomers are reacted in the presence of a heat exchange fluid, resulting in a solid product suspended in the heat exchange medium.

[0040] In both the melt acidolysis method and the slurry polymerization method, the polymerizable monomer component used in producing the amorphous polyester resin can be subjected to the reaction in a modified form in which the hydroxyl group is acylated, that is, as a lower acylated product. The lower acyl group preferably has 2 to 5 carbon atoms, more preferably has 2 or 3 carbon atoms. Particularly preferred is a method in which an acetylated product of the monomer component is used in the reaction.

[0041] The lower acylated product of the polymerizable monomer may be one which has been previously synthesized by separate acylation, or may be produced in the reaction system by adding an acylating agent such as acetic anhydride to the monomer during the production of the amorphous polyester resin.

[0042] In either the molten acidolysis method or the slurry polymerization method, the polycondensation reaction is generally carried out at a temperature of 150 to 400° C., preferably 250 to 370° C., under normal pressure and / or reduced pressure, and a catalyst may be used as necessary.

[0043] Specific examples of catalysts include organotin compounds such as dialkyltin oxides (e.g., dibutyltin oxide) and diaryltin oxides; titanium dioxide; antimony trioxide; organotitanium compounds such as alkoxytitanium silicates and titanium alkoxides; alkali and alkaline earth metal salts of carboxylic acids (e.g., sodium acetate, potassium acetate); and gaseous acid catalysts such as Lewis acids (e.g., boron trifluoride) and hydrogen halides (e.g., hydrogen chloride).

[0044] The catalyst is usually used in an amount of 10 to 1000 ppm, preferably 20 to 200 ppm, based on the total amount of monomers.

[0045] The amorphous polyester resin of the present invention thus obtained does not show a crystal melting temperature by a differential scanning calorimeter (DSC) as described below, but does show a glass transition temperature. The amorphous polyester resin of the present invention has a glass transition temperature of preferably 180°C or less, and is excellent in low-temperature processability. The amorphous polyester resin of the present invention has a glass transition temperature of more preferably 160°C or less, further preferably 140°C or less, and particularly preferably 120°C or less. The lower limit of the glass transition temperature is not particularly limited, but is, for example, 70°C.

[0046] In the present specification and claims, the "crystal melting temperature" is determined from the temperature at which an endothermic peak due to crystal melting is observed when measured at a heating rate of 20°C / min using a differential scanning calorimeter (hereinafter abbreviated as DSC). More specifically, after observing the endothermic peak temperature (Tm1) observed when a resin sample is measured under a heating condition of 20°C / min from room temperature, the sample is held at a temperature 20 to 50°C higher than Tm1 for 10 minutes, and then cooled to room temperature under a temperature drop condition of 20°C / min, and then measured again under a heating condition of 20°C / min. The temperature showing the peak top is taken as the crystal melting temperature of the resin. For example, a DSC7020 manufactured by Hitachi High-Tech Science Corporation can be used as a measuring instrument.

[0047] In the present specification and claims, the "glass transition temperature" is measured using a differential scanning calorimeter under the condition of a temperature rise of 20°C / min from room temperature.

[0048] The amorphous polyester resin of the present invention has a melt viscosity measured with a capillary rheometer of preferably 1 to 1000 Pa·s, more preferably 5 to 300 Pa·s.

[0049] In addition, the amorphous polyester resin of the present invention has a bending strength of preferably 140 MPa or more, more preferably 145 MPa or more, and even more preferably 150 MPa or more in a bending test using a rectangular test piece (length 65 mm x width 12.7 mm x thickness 2.0 mm). The upper limit of the bending strength is not particularly limited, but is, for example, 300 MPa.

[0050] The bending strength can be measured at a span distance of 40.0 mm and a compression speed of 1.3 mm / min.

[0051] The present invention further provides an amorphous polyester resin composition obtained by blending one or more fibrous, plate-like or granular fillers with the amorphous polyester resin of the present invention. The filler may be appropriately selected from substances known to be used in resin compositions depending on the purpose and application of the amorphous polyester resin composition.

[0052] Examples of fibrous fillers include glass fibers, silica alumina fibers, alumina fibers, carbon fibers, aramid fibers, etc. Among these, glass fibers are preferred because of their excellent balance between physical properties and costs.

[0053] Examples of the plate-like or granular filler include talc, mica, graphite, wollastonite, calcium carbonate, dolomite, clay, glass flakes, glass beads, barium sulfate, titanium oxide, etc. Among these, talc is preferred because of its excellent balance between physical properties and cost.

[0054] In the amorphous polyester resin composition containing the filler, the total amount of the filler is usually 0.1 to 200 parts by mass, and preferably 10 to 100 parts by mass, per 100 parts by mass of the amorphous polyester resin. If the amount of the filler exceeds 200 parts by mass, the molding processability of the resin composition tends to decrease, and wear of the cylinder and mold of the molding machine tends to increase.

[0055] In addition, the amorphous polyester resin of the present invention may contain one or more of the following additives that are known to be used in resin compositions, such as release improvers such as higher fatty acids, higher fatty acid esters, higher fatty acid amides, higher fatty acid metal salts, polysiloxanes, and fluororesins; colorants such as dyes and pigments; antioxidants; heat stabilizers; ultraviolet absorbers; antistatic agents; and surfactants, in a range that does not impair the effects of the present invention, depending on the purpose and use of the resin composition.

[0056] As for substances having an external lubricant effect, such as higher fatty acids, higher fatty acid esters, higher fatty acid metal salts, and fluorocarbon surfactants, they may be attached to the pellets in advance at the time of molding.

[0057] The amorphous polyester resin composition of the present invention can be prepared by blending all of the components, such as the filler and additives, with an amorphous polyester resin, and melt-kneading the blend at a temperature ranging from near the glass transition temperature of the amorphous polyester resin to the glass transition temperature + 100°C using a Banbury mixer, kneader, single-screw or twin-screw extruder, or the like.

[0058] The amorphous polyester resin and amorphous polyester resin composition of the present invention thus obtained can be processed into molded articles such as injection molded articles, films, sheets, and nonwoven fabrics by conventional molding methods such as injection molding, compression molding, extrusion molding, and blow molding.

[0059] The amorphous polyester resin and the amorphous polyester resin composition of the present invention are suitably used as electrical and electronic parts, mechanical parts such as camera modules, automobile parts, etc. In particular, the amorphous polyester resin of the present invention is useful in applications requiring low-temperature processability and as a polymer alloy material with other thermoplastic resins. EXAMPLES

[0060] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto.

[0061] In the examples, the following abbreviations represent the following compounds. POB: 4-hydroxybenzoic acid BON6: 6-hydroxy-2-naphthoic acid BP: 4,4'-dihydroxybiphenyl IPA: Isophthalic acid NDA: 2,6-naphthalenedicarboxylic acid TPA: Terephthalic acid HQ: Hydroquinone

[0062] <Measurement of crystal melting temperature and glass transition temperature> Measurement was performed using a differential scanning calorimeter (DSC7020 manufactured by Hitachi High-Tech Science Corporation). The resin samples of the examples and comparative examples were measured under conditions of a temperature rise of 20°C / min from room temperature, and after observing the endothermic peak temperature (Tm1), the sample was held at a temperature 20 to 50°C higher than Tm1 for 10 minutes. Next, the sample was cooled to room temperature under a temperature drop condition of 20°C / min, and then the endothermic peak was observed when measured again under a temperature rise condition of 20°C / min. The temperature showing the peak top was taken as the crystalline melting temperature of the resin sample, and the midpoint at which the DSC curve changed stepwise was taken as the glass transition temperature of the resin sample.

[0063] <Bending strength> Using an injection molding machine (MINIMAT M26 / 15 manufactured by Sumitomo Heavy Industries, Ltd.), rectangular test pieces with a length of 65 mm, a width of 12.7 mm, and a thickness of 2.0 mm were molded at a cylinder temperature of 20 to 40°C above the crystal melting temperature or 60 to 80°C above the glass transition temperature and a mold temperature of 70°C, and their bending strength was measured. The bending strength was measured at a span distance of 40.0 mm and a compression speed of 1.3 mm / min.

[0064] Example 1 POB, BON6, BP and IPA were charged in a reaction vessel equipped with a stirrer with a torque meter and a distillation tube in a total amount of 6.5 moles in the composition ratio shown in Table 1, and acetic anhydride was further charged in an amount of 1.03 times the moles of the hydroxyl groups (moles) of all monomers, and deacetic acid polymerization was carried out under the following conditions.

[0065] The temperature was raised from room temperature to 150°C in 1 hour under a nitrogen gas atmosphere, and the temperature was maintained for 30 minutes. Next, the temperature was raised quickly to 210°C while distilling off the by-product acetic acid, and the temperature was maintained for 30 minutes. After that, the temperature was raised to 340°C over 4 hours, and the pressure was reduced to 10 mmHg over 80 minutes. The polymerization reaction was terminated when a predetermined torque was indicated, and the contents of the reaction vessel were taken out and crushed to obtain the resin pellets of Example 1. The amount of acetic acid distilled during polymerization was almost the theoretical value.

[0066] Examples 2 to 5 and Comparative Examples 1 to 5 (Example 5 is a reference example) Resin pellets were obtained in the same manner as in Example 1, except that the monomer composition ratio was changed to the composition ratio shown in Table 1. The amount of acetic acid distilled during polymerization was approximately the theoretical value.

[0067] The crystal melting temperature, glass transition temperature and bending strength of the resin pellets of Examples 1 to 5 and Comparative Examples 1 to 5 are shown in Table 1.

[0068] In Examples 1 to 5, since no endothermic peak temperature (Tm1) was observed in any of them, the samples were held at 260°C for 10 minutes, cooled to room temperature at a temperature decreasing rate of 20°C / min, and then heated again at a temperature increasing rate of 20°C / min, but no endothermic peak was observed. In addition, for Comparative Examples 1 to 5, a stepwise change in DSC curve could not be confirmed, so it was difficult to identify the glass transition temperature.

[0069] [Table 1]

[0070] As is clear from Table 1, in all of the amorphous polyester resins of Examples 1 to 5 composed of specific repeating units, no crystalline melting temperature was observed in differential scanning calorimetry at a heating rate of 20°C / min, and the resins had low-temperature processability.

[0071] On the other hand, the liquid crystal polyester resins of Comparative Examples 1 to 5 were all confirmed to have a crystalline melting temperature higher than the glass transition temperature of the amorphous polyester resins of Examples 1 to 5, and were inferior in low-temperature processability.

Claims

1. Formulas (I) to (VI) [Formula 1] [In the formula, p, q, r, s, t, and u each represent a composition ratio (mol %) of each repeating unit in the amorphous polyester resin, and satisfy the following formula: 35≦p≦65, 15≦q≦45, 5≦r≦15, 5≦s≦15, 0≦t≦10, and 0≦u≦10] The repeating unit is represented by p>q, and p+q+r+s+t+u=100; The glass transition temperature measured by a differential scanning calorimeter is 70° C. or higher and 110.6° C. or lower. Amorphous polyester resin.

2. 2. The amorphous polyester resin according to claim 1, having a bending strength of 140 MPa or more.

3. 3. An amorphous polyester resin composition comprising 100 parts by mass of the amorphous polyester resin according to claim 1 and 0.1 to 200 parts by mass of a fibrous, plate-like or granular filler.

4. A molded article comprising the amorphous polyester resin according to any one of claims 1 to 2 or the amorphous polyester resin composition according to claim 3.

Citation Information

Patent Citations

  • Composition and method for producing stretchable polymer, and plastic article molded therefrom

    JP2001200034A

  • Method for producing amorphous anisotropic melt- forming polymer having high elasticity and polymer produced by the method

    JP2001226471A

  • Amorphous wholly aromatic polyester amide

    JP2004217890A

  • Liquid crystal polyester resin

    JP2005105232A

  • Blow molding process and blow molded article

    JP2005305810A