Liquid crystal polyester amide resin

A liquid crystal polyesteramide resin with specific repeating unit compositions addresses the mechanical weaknesses of fully aromatic polyester amides, providing enhanced tensile strength and impact resistance for electronic device applications.

JP7578507B2Active Publication Date: 2024-11-06UENO PHARMA CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021028899
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-25
Publication Date
2024-11-06
Estimated Expiration
2041-02-25

Smart Images

  • Figure 0007578507000001
    Figure 0007578507000001
  • Figure 0007578507000002
    Figure 0007578507000002
  • Figure 0007578507000003
    Figure 0007578507000003
Patent Text Reader

Abstract

To provide a liquid crystal polyester amide resin having excellent mechanical characteristics such as tensile strength and Izod impact strength, and a liquid crystal polyester amide resin composition, and a molding composed of the liquid crystal polyester amide resin or the resin composition.SOLUTION: This invention relates to a liquid crystal polyester amide resin containing repeat units represented by formulae (I)-(V).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a liquid crystal polyesteramide resin having excellent mechanical strength. [Background technology]

[0002] Liquid crystal polymers are widely used as high-performance engineering plastics because they have a good balance of excellent fluidity, mechanical strength, heat resistance, chemical resistance, electrical properties, etc. Known liquid crystal polymers include liquid crystal polyesters and liquid crystal polyester amides.

[0003] As a liquid crystal polyesteramide, for example, Patent Document 1 proposes a wholly aromatic polyesteramide that is composed of specific repeating units and is said to have a sufficient balance between a low melting point and heat resistance. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2020-41012 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the wholly aromatic polyesteramide described in Patent Document 1 has poor mechanical properties such as tensile strength and impact resistance, and has the problem that it is difficult to use it for parts of electronic devices such as mobile phones that are susceptible to shocks due to dropping during daily use.

[0006] An object of the present invention is to provide a liquid crystal polyesteramide resin having excellent mechanical properties such as tensile strength and Izod impact strength. [Means for solving the problem]

[0007] In view of the above problems, the present inventors conducted intensive research and discovered that a liquid crystal polyesteramide resin composed of specific repeating units has excellent mechanical properties such as tensile strength and Izod impact strength, thereby completing the present invention.

[0008] That is, the present invention includes the following preferred embodiments. [1] Formulas (I)~(V) [ka] In the formula, p, q, r, s and t each represent a composition ratio (mol %) of each repeating unit in the liquid crystal polyester amide resin, and satisfy the following formula: 25≦p≦60, 3≦q≦50, 5≦r≦30, 5≦s≦25, and 0≦t≦25] A liquid crystal polyester amide resin comprising a repeating unit represented by the formula: [2] The liquid crystal polyesteramide resin according to [1], further satisfying p+q≧50. [3] The liquid crystal polyesteramide resin according to [1] or [2], further satisfying p+q+r+s+t=100. [4] The liquid crystal polyesteramide resin according to any one of [1] to [3], which has a tensile strength of 190 MPa or more. [5] The liquid crystal polyesteramide resin according to any one of [1] to [4], which has an Izod impact strength according to ASTM D256 of 300 J / m or more. [6] A liquid crystal polyesteramide resin composition comprising 100 parts by mass of the liquid crystal polyesteramide resin according to any one of [1] to [5] and 0.1 to 200 parts by mass of a fibrous, plate-like or granular filler. [7] A molded article comprising the liquid crystal polyesteramide resin according to any one of [1] to [5] or the liquid crystal polyesteramide resin composition according to [6]. Effect of the Invention

[0009] The liquid crystal polyesteramide resin and the liquid crystal polyesteramide resin composition of the present invention have excellent mechanical properties such as tensile strength and Izod impact strength, and are therefore suitably used for applications such as electrical and electronic parts, such as housings and packages for various communication equipment and electronic devices. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] In this specification and claims, the term "liquid crystal polyesteramide resin" refers to a polyesteramide resin that forms an anisotropic molten phase, and is known in the art as a thermotropic liquid crystal polyesteramide resin.

[0011] The nature of the anisotropic molten phase can be confirmed by conventional polarized light examination using crossed polarizers. More specifically, the anisotropic molten phase can be confirmed by observing the sample placed on a Leitz hot stage under a nitrogen atmosphere at a magnification of 40 times using a Leitz polarizing microscope. The liquid crystal polyesteramide resin of the present invention is optically anisotropic, i.e., transmits light when examined between crossed polarizers. If the sample is optically anisotropic, polarized light will be transmitted even when it is stationary.

[0012] The liquid crystal polyesteramide resin of the present invention contains aromatic oxycarbonyl repeating units represented by formula (I) and formula (II) as repeating units.

[0013] [ka]

[0014] In the liquid crystal polyesteramide resin of the present invention, the composition ratio p of the repeating unit represented by formula (I) to the liquid crystal polyesteramide resin is 25 to 60 mol%, preferably 30 to 55 mol%, and the composition ratio q of the repeating unit represented by formula (II) to the liquid crystal polyesteramide resin is 3 to 50 mol%, preferably 4 to 40 mol%, more preferably 5 to 35 mol%.

[0015] In the liquid crystal polyesteramide resin of the present invention, the repeating units represented by formula (I) and formula (II) preferably satisfy the relationship p+q≧50, more preferably satisfy the relationship p+q≧55, even more preferably satisfy the relationship p+q≧60, and particularly preferably satisfy the relationship p+q≧65.

[0016] Specific examples of monomers that provide the repeating unit represented by formula (I) include 4-hydroxybenzoic acid and its ester-forming derivatives such as acylation products, ester derivatives and acid halides.

[0017] Specific examples of monomers that provide the repeating unit represented by formula (II) include 6-hydroxy-2-naphthoic acid and its ester-forming derivatives such as acylation products, ester derivatives and acid halides.

[0018] The liquid crystal polyesteramide resin of the present invention contains an aromatic oxyamino repeating unit represented by formula (III).

[0019] [ka]

[0020] In the liquid crystal polyesteramide resin of the present invention, the composition ratio r of the repeating unit represented by formula (III) to the liquid crystal polyesteramide resin is 5 to 30 mol %, preferably 7 to 28 mol %, and more preferably 10 to 25 mol %.

[0021] Specific examples of monomers which provide the repeating unit represented by formula (III) include 4-aminophenol and its amide-forming derivatives such as acylated products.

[0022] The liquid crystal polyesteramide resin of the present invention contains an aromatic dicarbonyl repeating unit represented by formula (IV).

[0023] [ka]

[0024] In the liquid crystal polyesteramide resin of the present invention, the composition ratio s of the repeating unit represented by formula (IV) to the liquid crystal polyesteramide resin is 3 to 25 mol %, preferably 5 to 23 mol %.

[0025] Specific examples of monomers that provide the repeating unit represented by formula (IV) include 2,6-naphthalenedicarboxylic acid and its ester-forming derivatives such as ester derivatives and acid halides.

[0026] The liquid crystal polyesteramide resin of the present invention may further contain a repeating unit represented by formula (V) as another aromatic dicarbonyl repeating unit.

[0027] [ka]

[0028] In the liquid crystal polyesteramide resin of the present invention, the composition ratio t of the repeating unit represented by formula (V) to the liquid crystal polyesteramide resin is 0 to 25 mol %, preferably 1 to 20 mol %, and more preferably 2 to 15 mol %.

[0029] Specific examples of monomers which provide the repeating unit represented by formula (V) include terephthalic acid and isophthalic acid, as well as ester-forming derivatives thereof, such as ester derivatives and acid halides.

[0030] That is, the repeating unit represented by formula (V) is preferably a repeating unit represented by formula (VI) and / or formula (VII).

[0031] [ka]

[0032] In the liquid crystal polyesteramide resin of the present invention, the total composition ratio of the repeating units [p+q+r+s+t] is preferably 100 mol %, but other repeating units may be further included as long as the object of the present invention is not impaired.

[0033] Examples of monomers that provide other repeating units constituting the liquid crystal polyesteramide resin of the present invention include other aromatic hydroxycarboxylic acids, other aromatic hydroxyamines, other aromatic dicarboxylic acids or aromatic diols, aromatic hydroxydicarboxylic acids, aromatic diamines, aromatic aminocarboxylic acids, aromatic mercaptocarboxylic acids, aromatic dithiols, aromatic mercaptophenols, and combinations thereof.

[0034] The proportion of repeating units provided by these other monomer components is preferably 10 mol % or less in the total repeating units.

[0035] The method for producing the liquid crystal polyesteramide resin of the present invention will be described below.

[0036] The method for producing the liquid crystal polyesteramide resin of the present invention is not particularly limited, and any known polyester or polyamide polycondensation method that forms an ester bond or amide bond between the above-mentioned monomer components, such as a melt acidolysis method or a slurry polymerization method, can be used.

[0037] The molten acidolysis method is a preferred method for producing the liquid crystal polyesteramide resin of the present invention. In this method, the polymerizable monomers are first heated to form a molten solution of the reactants, and then the polycondensation reaction is continued to obtain a molten polymer. A vacuum may be applied to facilitate removal of volatile by-products (e.g., acetic acid, water, etc.) produced at the final stage of condensation.

[0038] A slurry polymerization process is a process in which polymerizable monomers are reacted in the presence of a heat exchange fluid, resulting in a solid product suspended in the heat exchange medium.

[0039] In both the melt acidolysis method and the slurry polymerization method, the polymerizable monomer components used in producing the liquid crystal polyesteramide resin can be subjected to the reaction in a modified form in which the hydroxyl group and / or amino group is acylated, that is, as a lower acylated product. The lower acyl group preferably has 2 to 5 carbon atoms, more preferably has 2 or 3 carbon atoms. Particularly preferred is a method in which an acetylated product of the monomer component is used in the reaction.

[0040] The lower acylated product of the polymerizable monomer may be one which has been previously synthesized by separate acylation, or may be produced in the reaction system by adding an acylating agent such as acetic anhydride to the monomer during the production of the liquid crystal polyesteramide resin.

[0041] In either the molten acidolysis method or the slurry polymerization method, the polycondensation reaction is generally carried out at a temperature of 150 to 400° C., preferably 250 to 370° C., under normal pressure and / or reduced pressure, and a catalyst may be used as necessary.

[0042] Specific examples of catalysts include organotin compounds such as dialkyltin oxides (e.g., dibutyltin oxide) and diaryltin oxides; titanium dioxide; antimony trioxide; organotitanium compounds such as alkoxytitanium silicates and titanium alkoxides; alkali and alkaline earth metal salts of carboxylic acids (e.g., sodium acetate, potassium acetate); and gaseous acid catalysts such as Lewis acids (e.g., boron trifluoride) and hydrogen halides (e.g., hydrogen chloride).

[0043] The catalyst is usually used in an amount of 10 to 1000 ppm, preferably 20 to 200 ppm, based on the total amount of monomers.

[0044] The liquid crystal polyesteramide resin of the present invention thus obtained has a crystalline melting temperature of preferably 200° C. or higher, as measured by a differential scanning calorimeter (DSC) described below, and has excellent heat resistance. The crystalline melting temperature of the liquid crystal polyesteramide resin of the present invention is preferably 200° C. or higher, more preferably 210° C. or higher.

[0045] In the present specification and claims, the "crystal melting temperature" is determined from the temperature at which an endothermic peak due to crystal melting is observed when measured at a heating rate of 20°C / min using a differential scanning calorimeter (hereinafter abbreviated as DSC). More specifically, after observing the endothermic peak temperature (Tm1) observed when a sample of liquid crystal polyesteramide resin is measured under a heating condition of 20°C / min from room temperature, the sample is held at a temperature 20 to 50°C higher than Tm1 for 10 minutes, and then cooled to room temperature under a temperature drop condition of 20°C / min, and then measured again under a heating condition of 20°C / min. The temperature showing the peak top is taken as the crystal melting temperature of the liquid crystal polyesteramide resin. For example, a DSC7020 manufactured by Hitachi High-Tech Science Corporation can be used as a measuring instrument.

[0046] The liquid crystal polyesteramide resin of the present invention is subjected to a shear rate measurement of 1000 s using a capillary rheometer (Capillograph 1D manufactured by Toyo Seiki Co., Ltd.) with a capillary of 0.7 mmφ×10 mm. -1 The melt viscosity measured under the above conditions at a temperature 30° C. above the crystal melting temperature is preferably from 1 to 1000 Pa·s, and more preferably from 5 to 300 Pa·s.

[0047] In addition, the liquid crystal polyesteramide resin of the present invention preferably has a tensile strength of 190 MPa or more, more preferably 205 MPa or more, and further preferably 220 MPa or more, in a tensile test using a dumbbell-shaped test piece (length 63.5 mm x width 3.5 mm x thickness 2.0 mm). The upper limit of the tensile strength is not particularly limited, but is, for example, 350 MPa.

[0048] The tensile strength can be measured at a span distance of 25.4 mm and a tensile speed of 5.0 mm / min.

[0049] The liquid crystal polyesteramide resin of the present invention preferably has an Izod impact strength at 23° C. according to ASTM D256 of 300 J / m or more, more preferably 350 J / m or more, and even more preferably 400 J / m or more. The upper limit of the Izod impact strength is not particularly limited, but may be, for example, 1000 J / m It is.

[0050] The present invention further provides a liquid crystal polyesteramide resin composition obtained by blending one or more fibrous, plate-like or granular fillers with the liquid crystal polyesteramide resin of the present invention. The filler may be appropriately selected from substances known to be used in resin compositions depending on the purpose and application of the liquid crystal polyesteramide resin composition.

[0051] Examples of fibrous fillers include glass fibers, silica alumina fibers, alumina fibers, carbon fibers, aramid fibers, etc. Among these, glass fibers are preferred because of their excellent balance between physical properties and costs.

[0052] Examples of the plate-like or granular filler include talc, mica, graphite, wollastonite, calcium carbonate, dolomite, clay, glass flakes, glass beads, barium sulfate, titanium oxide, etc. Among these, talc is preferred because of its excellent balance between physical properties and cost.

[0053] In the liquid crystal polyesteramide resin composition containing the filler, the total amount of the filler is usually 0.1 to 200 parts by mass, and preferably 10 to 100 parts by mass, per 100 parts by mass of the liquid crystal polyesteramide resin. If the amount of the filler exceeds 200 parts by mass, the molding processability of the resin composition tends to decrease, and wear of the cylinder and mold of the molding machine tends to increase.

[0054] In addition, the liquid crystal polyesteramide resin of the present invention may further contain one or more of the following additives that are known to be used in resin compositions, such as release improvers such as higher fatty acids, higher fatty acid esters, higher fatty acid amides, higher fatty acid metal salts, polysiloxanes, and fluororesins; colorants such as dyes and pigments; antioxidants; heat stabilizers; ultraviolet absorbers; antistatic agents; and surfactants, in combination depending on the purpose and use of the resin composition, within a range that does not impair the effects of the present invention.

[0055] As for substances having an external lubricant effect, such as higher fatty acids, higher fatty acid esters, higher fatty acid metal salts, and fluorocarbon surfactants, they may be attached to the pellets in advance at the time of molding.

[0056] The liquid crystal polyesteramide resin composition of the present invention can be prepared by blending all of the components, such as fillers and additives, with a polyesteramide resin and melt-kneading the blend at a temperature ranging from near the crystalline melting temperature of the liquid crystal polyesteramide resin to the crystalline melting temperature + 100°C using a Banbury mixer, kneader, single-screw or twin-screw extruder, or the like.

[0057] The liquid crystal polyesteramide resin and liquid crystal polyesteramide resin composition of the present invention thus obtained can be processed into molded articles such as injection molded articles, films, sheets and nonwoven fabrics by conventional molding methods such as injection molding, compression molding, extrusion molding and blow molding.

[0058] The liquid crystal polyesteramide resin and the liquid crystal polyesteramide resin composition of the present invention have excellent mechanical properties such as tensile strength and Izod impact strength, and are therefore suitably used for applications such as electrical and electronic parts, such as housings and packages for various communication equipment and electronic devices. EXAMPLES

[0059] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto.

[0060] In the examples, the following abbreviations represent the following compounds. POB: 4-hydroxybenzoic acid BON6: 6-hydroxy-2-naphthoic acid BP: 4,4'-dihydroxybiphenyl PAP: 4-aminophenol NDA: 2,6-naphthalenedicarboxylic acid IPA: Isophthalic acid TPA: Terephthalic acid

[0061] Measurement of Crystal Melting Temperature Measurement was performed using a differential scanning calorimeter (DSC7020 manufactured by Hitachi High-Tech Science Corporation). The resin samples of the following examples and comparative examples were measured under conditions of a temperature rise of 20°C / min from room temperature, and after observing the endothermic peak temperature (Tm1), the sample was held at a temperature 20 to 50°C higher than Tm1 for 10 minutes. Next, the sample was cooled to room temperature under a temperature drop condition of 20°C / min, and then measured again under a temperature rise condition of 20°C / min to observe the endothermic peak, and the temperature showing the peak top was taken as the crystalline melting temperature of the resin sample.

[0062] Tensile strength Using an injection molding machine (MINIMAT M26 / 15 manufactured by Sumitomo Heavy Industries, Ltd.), a cylinder temperature of melting point +20 to 40°C and a mold temperature of 70°C were used to mold dumbbell-shaped tensile test pieces with a length of 63.5 mm, width of 3.5 mm, and thickness of 2.0 mm, and the tensile strength was measured. The tensile strength was measured at a span distance of 25.4 mm and a tensile speed of 5.0 mm / min.

[0063] <Izod impact strength> Injection molding machine: Using an injection molding machine (MINIMAT M26 / 15 manufactured by Sumitomo Heavy Industries, Ltd.), strip-shaped test pieces with a length of 65 mm, a width of 12.7 mm, and a thickness of 2.0 mm were molded at a cylinder temperature of melting point +20 to 40°C and a mold temperature of 70°C, and were measured in accordance with ASTM D256.

[0064] Example 1 A reaction vessel equipped with a stirrer with a torque meter and a distillation tube was charged with POB, BON6, PAP, NDA and IPA in a total amount of 6.5 moles in the composition ratio shown in Table 1, and 1.03 moles of acetic anhydride relative to the amount (moles) of hydroxyl groups in all monomers was further charged, and deacetic acid polymerization was carried out under the following conditions.

[0065] The temperature was raised from room temperature to 150°C in 1 hour under a nitrogen gas atmosphere, and the temperature was maintained for 30 minutes. Next, the temperature was raised quickly to 210°C while distilling off the by-product acetic acid, and the temperature was maintained for 30 minutes. After that, the temperature was raised to 345°C over 4 hours, and the pressure was reduced to 10 mmHg over 80 minutes. The polymerization reaction was terminated when a predetermined torque was reached, and the contents of the reaction vessel were removed and pellets of liquid crystal polyesteramide resin were obtained using a grinder. The amount of acetic acid distilled during polymerization was almost the theoretical value.

[0066] Examples 2 to 5 and Comparative Examples 1 to 4 Resin pellets were obtained in the same manner as in Example 1, except that the monomer composition ratio was changed to the composition ratio shown in Table 1. The amount of acetic acid distilled during polymerization was approximately the theoretical value.

[0067] Table 1 shows the crystalline melting temperature, tensile strength and Izod impact strength of the resins obtained in Examples 1 to 5 and Comparative Examples 1 to 4.

[0068] [Table 1]

[0069] As can be seen from Table 1, all of the liquid crystal polyesteramide resins of Examples 1 to 5, which were composed of specific repeating units, were excellent in mechanical properties such as tensile strength and Izod impact strength.

[0070] On the other hand, the resins of Comparative Examples 1 to 4 were all inferior to the liquid crystal polyesteramide resins of Examples 1 to 5 in mechanical properties such as tensile strength and Izod impact strength.

Claims

1. Formulas (I) to (V) [Formula 1] [In the formula, p, q, r, s and t each represent a composition ratio (mol %) of each repeating unit in the liquid crystal polyester amide resin, and satisfy the following formula: 25≦p≦60, 3≦q≦50, 5≦r≦30, 3≦s≦25, and 0≦t≦25] The repeating unit is represented by A liquid crystal polyesteramide resin that satisfies p+q+r+s+t=100.

2. The liquid crystal polyesteramide resin according to claim 1 , further satisfying p+q≧50.

3. The liquid crystal polyesteramide resin according to claim 1 or 2, which has a tensile strength of 190 MPa or more and 350 MPa or less.

4. The liquid crystal polyesteramide resin according to any one of claims 1 to 3, having an Izod impact strength according to ASTM D256 of 300 J / m or more and 1000 J / m or less.

5. A liquid crystal polyesteramide resin composition comprising 100 parts by mass of the liquid crystal polyesteramide resin according to any one of claims 1 to 4 and 0.1 to 200 parts by mass of a fibrous, plate-like or granular filler.

6. A molded article comprising the liquid crystal polyesteramide resin according to any one of claims 1 to 4 or the liquid crystal polyesteramide resin composition according to claim 5.

Citation Information

Patent Citations

  • Copolyester amide and its production

    JP1993170903A

  • Copolyester and its production

    JP1994263857A

  • Wholly aromatic polyester amide and method for producing the same

    JP2020041012A

  • Method of preparing aromatic liquid crystalline polyester amide resin and aromatic liquid crystalline polyester amide resin compound including the aromatic liquid crystalline polyester amide resin prepared by the method

    KR1020140074094A