Process for preparing catalysts and catalyst compositions
Chemically modified clay support activators, formed by combining colloidal smectite clay with cationic polymetalates, address the complexity and cost of traditional catalysts, offering high-yield, cost-effective, and active catalysts for polyolefin production.
Patent Information
- Application Number
- JP2022544670
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-01-27
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2040-01-27
AI Technical Summary
The preparation of heterogeneous polymerization catalysts for polyolefin production is complex and expensive, requiring costly cocatalysts like MAO and arylboranes, which are inefficient and time-consuming to synthesize, and existing support activators face challenges such as low recovery yields and difficult isolation processes.
The use of chemically modified clay support activators, specifically smectite heteroadducts formed by contacting colloidal smectite clay with cationic polymetalates, which are easily prepared, recoverable in high yields, and require minimal washing, providing superior activity to traditional activators.
This approach simplifies the preparation and recovery of support activators, reducing costs and enhancing catalyst activity, making them suitable for metallocene-based polyolefin production without the need for expensive cocatalysts like MAO and arylboranes.
Smart Images

Figure 0007578702000014 
Figure 0007578702000015 
Figure 0007578702000016
Abstract
Description
[Technical Field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS none
[0002] The present disclosure relates to catalyst compositions comprising support activators for producing polyethylene and processes for their preparation and use. [Background technology]
[0003] Compounds such as methylaluminoxane (MAO) and arylboranes are commonly used as metallocene catalyst activators or cocatalysts for the polymerization of olefins. Because industrial-scale production of polyolefin resins can utilize gas-phase or slurry reactor platforms rather than solution-phase conditions, heterogeneous catalyst systems are used for these polymerization systems. The preparation and use of these heterogeneous polymerization catalysts can be complex and expensive. For example, when treating inorganic metal oxide supports such as silica or alumina with the catalyst, the additional use of cocatalysts or activators such as MAO and arylboranes is often required, which can be time-consuming and expensive. The synthesis of MAO and arylboranes themselves can be atom-inefficient, requiring multiple steps and inert conditions, which can increase the cost of using such activators.
[0004] Various support activators have been investigated to attempt to reduce the high costs of aluminoxanes, arylboranes, and other expensive activators or cocatalysts. For example, U.S. Patent Nos. 6,107,230 and 9,670,296 to McDaniel et al. address the use of amorphous alumina and silica-alumina derivatives as both supports and cocatalysts to provide metallocene polymerization activity. U.S. Patent Nos. 6,632,894 and 7,041,753 to McDaniel et al. also describe the use of clay minerals in sol-gel matrices that can serve as support activators for metallocenes, but which are themselves costly to manufacture. Other approaches include the use of chemically modified clay minerals, such as those found in U.S. Patent No. 5,973,084 to Suga et al., U.S. Patent No. 6,531,552 to Nikano et al., U.S. Patent No. 9,751,961 to Murase et al., and U.S. Patent No. 5,202,295 to McCauley. These approaches involve process limitations such as low catalyst recovery yields, excessive preparation steps, difficulty in separating the modified clay minerals, or narrow preparation conditions under which the clay can be modified and isolated.
[0005] Thus, there remains a need to improve the ease and economics of preparation of support activators. This need is evident when chemically modified clay support activators with sufficient activity are desired for producing metallocene-based polyolefins, such as high-transparency film resins. It would be desirable to develop clay support activators that eliminate the need for aluminoxanes and other expensive activators, are convenient and economical to prepare and recover in high yields, and / or exhibit relatively high activity with polymerization catalysts, such as metallocene compounds. Summary of the Invention
[0006] Aspects of the present disclosure provide new support activators and processes for their preparation, new catalyst compositions containing the support activators, methods for producing the catalyst compositions, and processes for polymerizing olefins. In one aspect, the chemically modified clay support activators can easily activate metallocene compounds for olefin polymerization, and can be surprisingly easily and inexpensively prepared and recovered in high yields. In particular, the processes and support activators of the present disclosure can largely avoid previous difficulties in isolating the chemically modified clay support activators, for example, from digestion of the clay particles during the activation process and leaching of the clay's octahedral alumina layer into solution, which makes standard filtration very difficult as the clay particle size decreases.
[0007] It has been unexpectedly discovered that contacting a colloidal smectite clay, such as a dioctahedral smectite clay, with a heterocoagulation reagent comprising at least one cationic polymetallate in a liquid carrier (also referred to as a "diluent"), using the heterocoagulation reagent in an amount relative to the colloidal smectite clay within a specific range, synthesizes a support activator containing an isolated smectite heteroadduct. By limiting the amount of heterocoagulation reagent relative to the colloidal smectite clay described herein, the smectite heteroadduct, also referred to as heterocoagulated smectite, can be easily isolated from the resulting slurry by conventional filtration processes. This isolation process was often difficult with previous chemically modified clay support activators, which could require days of filtration or multiple washing and centrifugation steps. Furthermore, the smectite heteroadduct support activator isolated according to the present disclosure can be used with little or no washing steps, further enhancing the usefulness, ease, and economy of preparation and use.
[0008] The smectite heteroadducts prepared in this manner can be used in conjunction with cocatalysts such as alkylaluminum compounds to provide highly active support activators for metallocene olefin polymerization, especially when compared with traditional MAO-SiO2 or borane-derived support activators. The heteroadducts used in this process can be very inexpensive and can be used with cocatalysts such as alkylaluminum compounds, even compared with aluminoxane and borane-based activators.
[0009] Furthermore, isolation of the smectite heteroadducts can be performed using conventional filtration, without the need for centrifugation or extensive dilution of the reaction mixture, and without extensive washing of the resulting solids. This process provides solid clay heteroadducts that exhibit superior activity to the corresponding untreated clays, and activity equivalent to or superior to that of the more difficult to prepare pillared clay supports, thereby filling a need.
[0010] Furthermore, unlike pillared clays, the hetero-coagulated clay materials of the present disclosure are amorphous solids. The preparation of hetero-coagulated clays provides a three-dimensional structure, but it is non-pillared, non-crystalline, and amorphous. Without intending to be bound by theory, it is believed that the regular crystalline structure of the starting smectite is not simply expanded upon contact with the cationic polymetallate, but is disrupted during the preparation of the clay hetero-adduct, providing a non-crystalline, non-layered, amorphous material.
[0011] Accordingly, in one aspect, the present disclosure provides a support activator comprising an isolated smectite heteroadduct, the smectite heteroadduct comprising the contact product in a liquid carrier of [1] colloidal smectite clay and [2] a heterocoagulation reagent comprising at least one cationic polymetallate and in an amount sufficient to provide a slurry of smectite heteroadduct having a zeta potential in the range of about positive 25 mV (+25 millivolts) to about negative 25 mV (-25 millivolts).
[0012] The present disclosure also provides, in another aspect, a method for producing a support activator comprising a smectite heteroadduct, the method comprising: a) providing a colloidal smectite clay; b) contacting the colloidal smectite clay in a liquid carrier with a heterocoagulation reagent in an amount sufficient to provide a slurry of smectite heteroadducts comprising at least one cationic polymetallate and having a zeta potential in the range of about positive 25 millivolts (mV) to about negative 25 mV; c) isolating the smectite heteroadduct from the slurry.
[0013] According to a further aspect, the present disclosure provides a catalyst composition for olefin polymerization, the catalyst composition comprising: a) at least one metallocene compound; b) optionally at least one co-catalyst; c) at least one supported activator comprising a calcined smectite heteroadduct, the smectite heteroadduct comprising the contact product of: (1) colloidal smectite clay; and (2) a heterocoagulation reagent in a liquid carrier, the heterocoagulation reagent comprising at least one cationic polymetallate, in an amount sufficient to provide a slurry of the smectite heteroadduct having a zeta potential in the range of about positive 25 millivolts (mV) to about negative 25 mV.
[0014] The present disclosure also provides, in another aspect, a method for producing an olefin polymerization catalyst, the method comprising, in any order: a) at least one metallocene compound; b) optionally at least one co-catalyst; c) contacting at least one support activator comprising a calcined smectite heteroadduct, the smectite heteroadduct comprising the contact product of [1] colloidal smectite clay and [2] a heterocoagulation reagent in a liquid carrier in an amount sufficient to provide a slurry of the smectite heteroadduct having a zeta potential in the range of about positive 25 mV (millivolts) to about negative 25 mV.
[0015] In one aspect, for example, the optional co-catalyst may be an alkylating agent, which may or may not be necessary to initiate efficient olefin polymerization, depending on the particular metallocene compound used to prepare the olefin polymerization catalyst.
[0016] In a further aspect, a process for polymerizing olefins is provided, the process comprising contacting at least one olefin monomer and a catalyst composition under polymerization conditions to form a polyolefin, the catalyst composition comprising: a) at least one metallocene compound; b) optionally at least one co-catalyst; c) at least one supported activator comprising a calcined smectite heteroadduct, the smectite heteroadduct comprising the contact product of: (1) colloidal smectite clay; and (2) a heterocoagulation reagent in a liquid carrier, the heterocoagulation reagent comprising at least one cationic polymetallate, in an amount sufficient to provide a slurry of the smectite heteroadduct having a zeta potential in the range of about positive 25 mV (+25 millivolts) to about negative 25 mV (-25 millivolts).
[0017] These and other aspects, features, and embodiments of the compositions, including the support activator and catalyst compositions, methods for making the compositions, and polymerization processes and related methods, are more fully described in the detailed description, drawings, examples, and claims provided herein. [Brief explanation of the drawings]
[0018] [Figure 1] A schematic diagram of an embodiment of the present disclosure is provided illustrating a method for preparing, washing, and isolating a support activator comprising the calcined smectite heteroadduct of the present disclosure, and contrasting this process with a method for preparing, washing, and isolating pillared clay. [Figure 2] Figure 1 provides powder XRD (X-ray diffraction) patterns for a series of calcined products combining aluminum chlorhydrate (ACH) and Volclay® HPM-20 montmorillonite. All samples were prepared according to the method of the present invention by example (see Examples 18, 20-21, and 23), except for the starting clay itself in the 6.4 mmol Al / g clay sample (top), which represents a typically prepared Al13 pillared clay (Comparative Example 5), and the 0 mmol Al / g clay sample (Comparative Example 3). [Figure 3] Figure 1 shows a zeta potential titration of a 2.5 wt% (wt%) aqueous solution of aluminum chlorohydrate (ACH, measured density 1.075 g / mL) into a 0.62 wt% aqueous dispersion of Volclay® HPM-20 bentonite. The measured zeta potential is plotted against the titration volume (mL). The titration setting was 0.5 mL per titration point, followed by a 30-second equilibration delay. The titration volume indicates the cumulative volume of aqueous aluminum chlorohydrate solution added. See also Table 4. [Figure 4] The plot in Figure 3 is converted to zeta potential versus aluminum-to-clay mass ratio. In particular, Figure 4 shows the zeta potential titration of a 2.5 wt. % aqueous solution of aluminum chlorohydrate (ACH, measured density 1.075 g / mL) in a 0.62 wt. % Volclay® HPM-20 bentonite dispersion, plotting the measured zeta potential versus Al content (mmol Al / g clay). The titration amount represents the cumulative mmol of aluminum in the added aqueous ACH solution. [Figure 5]Figure 1 shows the zeta potential titration of a 4.58 wt% aqueous solution of UltraPAC® 290 polyaluminum chloride (empirically Al2(OH)2.5Cl3.5) added by volume to a 1 wt% aqueous dispersion of Volclay® HPM-20 bentonite. The measured zeta potential is plotted against the titration volume (mL). The titration setting was 1 mL per titration point, followed by a 30-second equilibration delay. The titration volume indicates the cumulative volume of aqueous UltraPAC® 290 polyaluminum chloride solution added. See also Table 5. [Figure 6] Figure 1 shows a zeta potential titration (adjusted) for a volumetric addition of 10 wt% NYACOL® AL27 colloidal alumina aqueous dispersion into 0.75 wt% Volclay® HPM-20 bentonite aqueous dispersion. The measured zeta potential is plotted against the titration volume (mL). The titration settings were 1 mL per titration point from 0 to 27 mL and 3 mL per titration point thereafter, with an equilibration delay of 60 seconds. The titration volume indicates the cumulative volume of NYACOL® AL27 colloidal alumina aqueous solution added. See Example 11 and Table 6. [Figure 7] 1 shows the zeta potential titration of a 5 wt. % aqueous dispersion of AEROSIL® 200 fumed silica with a volumetric addition of 2.5 wt. % aqueous aluminum chlorohydrate (ACH). The measured zeta potential is plotted against the titration volume (mL). The titration setting was 1 mL per titration point, with an equilibration delay of 60 seconds. The titration volume indicates the cumulative volume of aqueous ACH solution added. See Example 37. [Figure 8] The plot of Figure 7 is converted to zeta potential versus aluminum to clay mass ratio. Specifically, Figure 8 shows the zeta potential titration of a 5 wt. % AEROSIL® 200 fumed silica aqueous dispersion with 2.5 wt. % aluminum chlorohydrate (ACH) in water, plotting the measured zeta potential versus Al content (mmol Al / g clay). The titration amount represents the cumulative mmol of aluminum in the added ACH solution. [Figure 9] This figure provides adjusted zeta potential titrations for the volumetric addition of aluminum chlorohydrate (ACH) solution-treated AEROSIL® 200 fumed silica aqueous dispersion, containing 5 wt. % silica, to 1 wt. % Volclay® HPM-20 bentonite aqueous dispersion. The titration settings were 0.2 mL per titration point from 0 to 1.2 mL, and 0.5 mL per titration point thereafter, with a 30-second equilibration delay. Because the titrant is a colloidal species, the zeta potential was adjusted using the method described in Example 11 to obtain the plot in Figure 9. See Example 38. [Figure 10]
[0023] Figure 1 shows the results of a nitrogen adsorption / desorption BJH (Barrett, Joyner, and Halenda) pore volume analysis of the aluminum chlorhydrate (ACH) hetero-coagulated clay of Example 18, providing a plot of pore diameter (Angstroms, Å) versus cumulative pore volume (cubic centimeters per gram, cc / g) for the hetero-adduct. The recipe for the preparation of this hetero-adduct slurry used 1.76 mmol Al / g clay. [Figure 11]
[0023] Figure 1 provides the results of a nitrogen adsorption / desorption BJH pore volume analysis of a comparative sheared and then azeotroped sample of Volclay® HPM-20 bentonite, but without further processing, per Comparative Example 3, showing a value for V3-10nm that is greater than 55% of the cumulative pore volume V3-30nm. [Figure 12]
[0023] Figure 1 provides the results of a nitrogen adsorption / desorption BJH pore volume analysis of an untreated sample of Volclay® HPM-20 bentonite that was suspended in water, evaporated, and calcined, but without further treatment, per Comparative Example 1, showing a value for V3-10nm that is greater than 55% of the cumulative pore volume V3-30nm. [Figure 13] 1H NMR spectrum of 7-phenyl-2-methyl-indene in CDCl3, with peaks for contaminants CH2Cl2 and water identified and peak integrals shown. [Figure 14]1H NMR spectrum of rac-dimethylsilylenebis(2-methyl-4-phenylindenyl)zirconium dichloride in CDCl3 with peak integrations shown. DETAILED DESCRIPTION OF THE INVENTION
[0019] In order to more clearly define the terms and phrases used herein, the following definitions are provided. To the extent that a definition or usage provided by any document incorporated herein by reference conflicts with a definition or usage provided herein, the definition or usage provided herein controls.
[0020] A. Definitions and Explanations of Terms Polymetallates. The term "polymetallate" and similar terms, such as "polyoxometallate," are used interchangeably in this disclosure to refer to water-soluble polyatomic cations containing two or more metal atoms (e.g., aluminum, silicon, titanium, zirconium, or other metals) with at least one bridging ligand between the metals, such as an oxo, hydroxy, and / or halide ligand. The specific ligand may depend on the precursor and other factors, such as the process for producing the polymetallate, solution pH, etc. For example, polymetallates of the present disclosure may be hydrated metal oxides, hydrated metal oxyoxides, etc., including combinations thereof. Bridging ligands, such as oxo ligands, bridging two or more metals may occur in these species, but polymetallates may also contain terminal oxo, hydroxyl, and / or halide ligands.
[0021] While many known polymetallate species are anionic, and the suffix "-ate" is often used to reflect anionic species, the polymetallate (polyoxometallate) species used in accordance with the present disclosure are cationic. These materials may be referred to as compounds, species, or compositions, although those skilled in the art will understand that multiple species may be contained in a suitable carrier, such as an aqueous solution, depending, for example, on the solution pH, concentration, starting precursors from which the polymetallate is generated in the aqueous solution, etc. For clarity and convenience, these multiple species will be collectively referred to as "polymetallates" or "polyoxometalates," regardless of whether the composition includes or is primarily composed of cationic polyoxometalates, polyhydroxymetalates, polyoxohydroxymetalates, or mixtures of species or compounds containing other ligands, such as halides. Examples of polymetallates include, but are not limited to, polyaluminum oxyhydroxychloride, aluminum chlorohydrate, polyaluminum chloride, or aluminum sesquichlorohydrate compositions, and may include linear, cyclic, or cluster compounds. These compositions are collectively referred to as polymetallates, although the terms "polymetallate" or "polyoxometallate" are also used to describe compositions containing substantially a single species.
[0022] Both isopolymetallates containing a single type of metal and heteropolymetallates containing two or more types of metals (or electropositive atoms, such as phosphorus) are included under the general terms polymetallate or polyoxometallate. For example, aluminum polymetallates, such as those provided by aluminum chlorhydrate (ACH) or polyaluminum chloride (PAC), are examples of isopolymetallates. In a further example, the polymetallates of the present disclosure can be prepared from a first metal oxide that is subsequently treated with a second metal oxide, metal halide, metal oxyhalide, or combination thereof, in an amount sufficient to provide a colloidal suspension of the heteropolymetallate. For example, the first metal oxide can include silica, alumina, zirconia, etc., including fumed silica, alumina, or zirconia, and the second metal oxide, metal halide, or metal oxyhalide can be obtained from an aqueous solution or suspension of a metal oxide, hydroxide, oxyhalide, or halide, such as ZrOCl2, ZnO, NbOCl3, B(OH)3, AlCl3, or combinations thereof. Thus, when different metals are used in the preparation, the resulting species is considered a heteropolymetallate. Both isopolymetallates and heteropolymetallates may be referred to simply as "polymetallates."
[0023] In a further aspect, polymetallates according to the present disclosure can be non-alkylated with respect to transition metal compounds, such as metallocene compounds, i.e., the subject polymetallates can be free of direct metal-carbon bonds, as found in aluminoxanes or other organometallic species.
[0024] Because the size and number or metal ions in polymetallate species can vary considerably, polymetallates can be considered to encompass both oligomeric and polymeric species. When polymetallates are described as "comprising," "consisting," "consisting essentially of," or "selected from" particular materials, such as polyaluminum chloride or aluminum sesquichlorohydrate, it should be understood that the polymetallate species formed when these materials are contacted with water, aqueous base, or the like, are described according to the precursors from which they are produced. Thus, for convenience and for the sake of certainty and clarity in accordance with 35 U.S.C. § 112, polymetallates may be described herein according to the precursor materials or compositions from which cationic polymetallates are produced to provide heterocoagulation reagents.
[0025] In one embodiment, the polymetallate according to the present disclosure can be at least one aluminum polymetallate. Examples include those of the general formula Al n Cl 3n-m (OH) m These polymetallate species include, but are not limited to, aluminum chlorhydrate (ACH), also known as aluminum chlorohydrate, which encompasses multiple water-soluble aluminum species typically considered to have the formula [Al oxyhydroxychloride]. These polymetallate species are sometimes referred to as aluminum oxyhydroxychloride compounds or compositions. Another polymetallate that can be used in accordance with the present disclosure is polyaluminum chloride (PAC), which is not a single species but an assembly of multiple aluminum polymeric species that can include linear, cyclic, or cluster compounds, examples of which can contain from 2 to about 30 aluminum atoms, oxo, chloride, and hydroxyl groups. Other examples of aluminum polymetallates include those having the general formula [Al oxyhydroxychloride], such as aluminum oxychlorohydrate. m O n (OH) x Cl y ] zH2O compounds and cluster-type species such as Keggin ions, e.g., "Al 13 It is sometimes called "-mer" polycation [AlO4Al12 (OH) 24 (H2O) 12 ] 7+ ●7[Cl] - Examples of aluminum species include, but are not limited to, aluminum chlorhydrate (ACH), aluminum chlorhydrate (ACH), and aluminum chloride (PAC). For example, polyaluminum chloride (PAC) can be produced by combining aqueous hydroxide with AlCl, resulting in a mixture of aluminum species with varying basicity. Aluminum chlorhydrate (ACH) is generally considered the most basic, while polyaluminum chloride (PAC) is considered the least basic.
[0026] Clay heteroadducts or clay heterocoagulates according to the present disclosure include the contact product of [1] a colloidal smectite clay, such as a dioctahedral smectite clay, and [2] a heterocoagulation reagent comprising at least one cationic polymetallate in a liquid carrier, such as an aqueous carrier, in an amount sufficient to provide a slurry of smectite heteroadduct having a zeta potential in the range of about +25 mV to about -25 mV. Once isolated, the smectite heteroadduct can be heated, dried, and calcined to form the support activator described herein. Upon calcination, additional reaction of the polymetallate initially intercalated into or associated with the smectite can occur, e.g., water can be driven from the intercalated polymetallate to form additional oxo groups. In this aspect, the term "polyoxometallate" can be particularly useful for irradiating the calcined product. In any event, the terms "polymetallate" and "polyoxometallate" are used interchangeably to describe compositions used to contact colloidal smectite.
[0027] Polymetallates of the present disclosure may also be referred to as "polycations" and may include both homopolycations and heteropolycations, depending on whether the polycation contains a single type of metal or two or more types of metals. For example, hydrotalcite is a heteropolycation according to the present disclosure [MgAl(OH) 16 ]CO3●4H2O.
[0028] Other examples of polymetallates, provided by way of example only, include the ε-Keggin cation [ε-PMo 12 O 36 (OH)4{Ln(H2O)4}4] 5+ (wherein Ln can be La, Ce, Nd, or Sm). See, for example, Angew. Chem., Int. Ed. 2002, 41, 2398. Other examples include compounds of the general formula [LnV 12 O 32 Lanthanide-containing cationic heteropolyoxovanadium clusters having the formula (H2O)8{Cl}]Cl, where Ln can be Eu, Gd, Dy, Tb, Ho, or Er. See, for example, RSC Adv. 2013, 3, 6299-6304.
[0029] Finally, reference to "at least one" cationic polymetallate is used to refer to one or more sources of the cationic polymetallate used to prepare the heterocoagulation reagent. That is, even if a single source of cationic polymetallate is used to prepare the heterocoagulation reagent in aqueous solution and multiple species may result, these multiple species may be collectively referred to as a single or single type of cationic polymetallate. Thus, reference to multiple or more cationic polymetallates is intended to refer to one or more precursor compositions or sources of the cationic polymetallate used to prepare the heterocoagulation reagent.
[0030] Heterocoagulation Reagents. The terms "heterocoagulation reagent," "heterocoagulant," and the like are used herein to describe compositions containing any positively charged oligomeric or polymeric metal oxide-containing species present in solution or as a colloidal suspension that, when combined with a colloidal clay dispersion in the appropriate ratio, forms a readily filterable solid (as defined herein). "Heterocoagulation reagent" may be used interchangeably with the terms "polymetallate" or "polyoxometallate" to refer to any positively charged oligomeric or polymeric metal oxide-containing species that function to form clay heteroadducts. Thus, "heterocoagulation reagent" emphasizes that a composition comprising one or more cationic polymetallate species in a liquid carrier forms a readily filterable solid when used in an amount sufficient to provide a slurry having a zeta potential in the range of about +25 mV to about -25 mV when contacted with colloidal smectite clay. "Heterocoagulation" is a term used in the art and is described by Lagaly in Ullmann's Encyclopedia of Chemistry 2012. In the context of the present disclosure, "heterocoagulation" is defined as the process of combining negatively charged colloidal clay particles with positively charged species of a heterocoagulation reagent to form a readily filterable solid, unless otherwise specified.Heterocoagulation may also be referred to as heteroaggregation in the art and herein, as described, for example, by Cerbelaud et al. Advances in Physics: X, 2017, vol. 2, 35-53.
[0031] Heteroadducts or Heteroconducts. Clay heteroadducts or clay heteroconducts, and similar terms such as "heteroconducted clay" or "smectite heteroadduct," refer to the contact product obtained from the combination of a heteroconducting reagent and a colloidal clay. That is, the aggregates formed when negatively charged colloidal clay particles are attracted to positively charged species in the heteroconducting reagent are referred to as "heteroadducts." See U.S. Patent No. 8,642,499 to Wu Cheng et al., which is incorporated herein by reference. In one aspect, these terms refer to the "easily filterable" contact product of a heteroconducting reagent and a colloidal clay, as defined herein. These terms are used to distinguish between easily filterable heteroconducting reagents and contact products of a heteroconducting reagent and a colloidal clay combined in a ratio that provides a product that is not easily filterable, such as the product formed when a pillared clay synthesis recipe is followed. In the case of a pillared clay recipe, the contact product is not easily filterable, and centrifugation is typically required to separate the pillared clay product.
[0032] When describing the formation of heterocoagulated clays using aluminum-containing heterocoagulation reagents, and unless otherwise specified, the ratio of pillaring reagent, such as aluminoxychloride (also referred to as heterocoagulation reagent), to clay is expressed as mm (mmol or millimole) Al / g clay, indicating the number of millimoles of Al per gram of clay in the pillaring or heterocoagulation reagent. See Gu et al., Clay and clay minerals, 1990, 38(5), 493-500, which is incorporated herein by reference. Unless otherwise specified, when the pillaring or aluminoxychloride heterocoagulation reagent is present as a soluble solution, millimoles of Al are calculated based on the weight % Al or weight % AlO content provided by the manufacturer. Alternatively, unless otherwise specified, when starting from a solid form of pillaring or heterocoagulation reagent dispersed in solution, millimoles of Al are determined by the weight used in the recipe and the empirical formula provided by the manufacturer.
[0033] Easily filterable. Terms such as "readily filterable," "readily filtered," "easily filterable," "easily filtered or separated," and the like, are used herein to describe compositions according to the present disclosure in which solids in a mixture containing a liquid phase can be separated from the liquid phase by filtration without centrifugation of less than about 2% by weight solids, ultracentrifugation, or dilute solutions, long settling times followed by decanting the liquid from the solids, and other such techniques. These terms are generally used herein to describe clay heteroadducts that are the contact product of colloidal smectite clay and heterocoagulation reagents under specific conditions according to the present disclosure and do not require isolation by centrifugation, high dilution and settling or settling tanks, or ultrafiltration. Thus, the readily filterable clay heteroadducts can be isolated or separated in good yield from the soluble salts and by-products of the synthesis in a time period of a few minutes or less, or less than about an hour, by passing a slurry containing the heteroadduct through conventional filtration materials such as sintered glass, metal or ceramic frits, paper, natural or synthetic matte fibers, under gravity or vacuum filtration conditions.
[0034] The present disclosure provides several specific experimental and quantitative methods for evaluating filterability. For example, a specific method for quantifying the filterability of a heteroadduct slurry is provided, which indicates that the slurry is easily filterable or can be considered to be easily filtered when prepared according to the methods of the present disclosure. Colloids or suspensions described by Lagaly in Ulmmann's Encyclopedia of Chemistry 2012, which require long settling times or ultrafiltration, are not considered "filterable" in the context of the present disclosure. Easily filterable suspensions or slurries of the present disclosure can produce clear filtrates upon filtration, while "non-easily filterable" suspensions that require substantially longer filtration times can contain particulate matter observable with the naked eye as a cloudy or opaque filtrate, indicative of a colloidal clay dispersion. When a support activator according to the present disclosure is prepared to provide a slurry of smectite heteroadducts having a zeta potential near the upper (positive) boundary of about +25 mV (millivolts) or near the lower (negative) boundary of about −25 mV, upon filtering the heteroadduct, some cloudiness may be observed in the filtrate, which is dark because the smectite heteroadducts are prepared using a ratio of colloidal smectite clay and heterocoagulation reagent that provides a slurry with a zeta potential near or close to 0 mV.
[0035] Colloids. "Colloid," "colloidal clay," "colloidal solution," "colloidal suspension," and similar terms are used as defined by Gerhard Lagaly in Ullmann's Encyclopedia of Industrial Chemistry, published January 15, 2007, in the chapter entitled "Colloids." These terms are used interchangeably.
[0036] Catalyst Compositions and Catalyst Systems. The terms "catalyst composition," "catalyst mixture," "catalyst system," and the like are used to refer to the combination of recited components that ultimately form, or are used to form, an active catalyst according to the present disclosure. The use of these terms is independent of any particular contacting step, contacting sequence, whether any reactions may occur between or among the components, or any products that may be formed from any contacting of any or all of the recited components. The use of these terms is also independent of the nature of the active catalyst sites or the fate of any cocatalyst, metallocene compound, or support activator after contacting or combining any of these components in any order. Thus, these and similar terms encompass the combination of the initially recited or starting components of the catalyst composition and any products that may result from contacting these initially recited starting components, regardless of whether the catalyst composition is heterogeneous or homogeneous or includes soluble and insoluble components. The terms "catalyst" and "catalyst system" or "catalyst composition" can be used interchangeably, and such use will be apparent to those skilled in the art from the context of this disclosure.
[0037] Catalyst Activity. Unless otherwise specified, the terms "activity," "catalyst activity," "catalyst composition activity," and the like refer to the polymerization activity of a catalyst composition comprising a dried or calcined clay heteroadduct as disclosed herein, typically expressed as the weight of polymer polymerized per weight of catalyst clay support activator alone, in the absence of any transition metal catalyst component such as a metallocene compound, any cocatalyst such as an organoaluminum compound, or any cocatalyst such as an aluminoxane, per hour of polymerization. In other words, the weight of polymer produced divided by the weight of calcined clay heteroadduct per hour, expressed in units of g / g / hr (grams / grams / hr).
[0038] The activity of a reference or comparative catalyst composition refers to the polymerization activity of a catalyst composition, including a comparative catalyst composition, based on the weight of the comparative ion-exchanged or pillared clay used to prepare the clay heteroadduct or the weight of the clay component itself. Terms such as "increased activity" or "improved activity" describe the activity of a catalyst composition according to the present disclosure that is greater than the activity of a comparative catalyst composition that uses the same catalyst components, such as a metallocene compound and cocatalyst, except that the comparative catalyst composition typically utilizes a different support activator or activator, such as a pillared clay, or the clay component used in the catalytic reaction is not a heterocoagulated clay. For example, an increased or improved activity according to the present disclosure includes an activity based on calcined clay heteroadduct of about 300 grams of polyethylene polymer per gram of calcined heterocoagulated clay per hour (g / g / hr) or more, using a standard set of ethylene homopolymerization conditions. In this embodiment, the standard set of ethylene homopolymerization conditions includes the following: A 2 L stainless steel reactor equipped with a ship-type impeller was set at about 500 rpm, and the slurry polymerization conditions included a 1 L purified isobutane diluent, a 90° C. polymerization temperature, 450 psi total ethylene pressure, a run length typically of 30 or 60 minutes, a metallocene catalyst composition comprising (1-Bu-3-MeCp)ZrCl with triethylaluminum (TEAL) cocatalyst, optionally using the metallocene as a stock solution containing TEAL, and a metallocene-to-clay ratio of about 7×10. -5 The amount loaded was such that it provided mmol of metallocene / mg of calcined clay. Typically, one alkylaluminum cocatalyst was used in the polymerization runs, usually selected from TEAL or triisobutylaluminum (TIBAL).
[0039] Contact Products. The term "contact product" is used herein to describe compositions in which components are combined or "contacted" together in any order, unless a specific order is described, required, or implied in any manner and at any length by the context of this disclosure. While a "contact product" can include a reaction product, the individual components need not react with each other, and the term is used regardless of whether or not it may result from contacting the listed components. For example, to form a contact product, the listed components can be contacted by blending or mixing, or the components can be contacted by adding the components in any order or simultaneously to a liquid carrier. Furthermore, contacting of any component can occur in the presence or absence of any other component of the compositions described herein, unless otherwise stated, required, or implied by the context in which the term is used. Combining or contacting the listed components or any additional materials can be carried out by any suitable method. Thus, the term "contact product" includes a mixture, blend, solution, slurry, reaction product, etc., or combinations thereof. Similarly, the term "contacting" is used herein to refer to materials that may be blended, mixed, slurried, dissolved, reacted, treated, or otherwise contacted in any way.
[0040] Pore size (pore size). Nitrogen adsorption / desorption measurements were used to determine pore size and pore volume distribution using the BJH method. Based on the International Union of Pure and Applied Chemistry (IUPAC) system for classifying porous materials (see Pure & Appl. Chem., 1994, 66, 1739-1758) and Klobes et al., National Institute of Standards and Technology Special Publication 960-17, pore size is defined as follows: "Micropore" and "microporous," as used herein, refer to pores present in a catalyst or catalyst support produced according to the process of the present disclosure that have a diameter of less than 20 Å. "Mesopore" and "mesoporous," as used herein, refer to pores present in a catalyst or catalyst support produced according to the process of the present disclosure that have a diameter ranging from 20 Å to less than 500 Å (i.e., 2 nm to <50 nm). "Macropores" and "macroporous," as used herein, refer to pores present in a catalyst or catalyst support produced according to the processes of the present disclosure having a diameter of 500 Å (50 nm) or greater.
[0041] Each of the above definitions of micropores, mesopores, and macropores are considered distinct and non-overlapping so that no pore is counted twice when summing the percentages or values in the distribution of pore sizes (pore size distribution) for any given sample.
[0042] "d50" refers to the median pore diameter measured by pore size measurement. Thus, "d50" corresponds to the median pore diameter calculated based on the pore size distribution, and is the pore diameter at which half of the pore diameters have a larger diameter. The d50 values reported herein are based on nitrogen desorption using the well-known calculation method described by E.P. Barrett, L.G. Joyner and P.P.H. Alenda ("B.J.H."), "The Determination of Pore Volume and Area Distributions in Porous Substances. I. Calculations from Nitrogen Isotherms," J.Am.Chem.Soc., 1951, 73(1), pp. 373-380.
[0043] "Median pore diameter" (MPD) can be calculated, for example, based on volume, surface area, or based on pore size distribution data. A median pore diameter calculated by volume refers to the pore diameter at which half of the total pore volume is present. A median pore diameter calculated by surface area refers to the pore diameter at which more than half of the total pore surface area is present. Similarly, a median pore diameter calculated based on pore size distribution refers to the pore diameter at which half of the pores have a larger diameter according to the pore size distribution determined elsewhere herein, for example, through derivation from nitrogen adsorption-desorption isotherms.
[0044] Transition metal catalyst. "Transition metal catalyst" refers to a transition metal compound or composition that functions as or can be converted into an active olefin polymerization catalyst when contacted with a support activator of the present disclosure, either in its present form or when contacted with a cocatalyst that can transfer or impart a polymerization-activating ligand to the transition metal catalyst. The use of the term "catalyst" is not intended to reflect any particular mechanism, or that the "transition metal catalyst" itself, when activated or when imparted with a polymerization-activatable ligand, represents an active site for catalytic polymerization. The transition metal catalyst is described according to the transition metal compound or compounds used in the process for preparing the polymerization catalyst, and can include metallocene compounds and related compounds as defined herein.
[0045] Cocatalyst. The term "cocatalyst" is used herein to refer to a chemical reagent, compound, or composition capable of providing a ligand to a metallocene that can initiate polymerization when the metallocene is otherwise activated with a support activator. In other words, the term "cocatalyst" is used herein to refer to a chemical reagent, compound, or composition capable of providing a polymerization-activatable ligand to a metallocene compound. Polymerization-activatable ligands include, but are not limited to, alkyl, such as methyl or ethyl; aryl and substituted aryl; substituted aryl, such as phenyl or tolyl; substituted alkyl, such as benzyl or trimethylsilylmethyl (-CH2SiM3); and hydrocarbyl substituents, such as hydride, silyl, and trimethylsilyl. Thus, in one aspect, the cocatalyst can be an alkylating agent, a hydriding agent, a silylating agent, or the like. There is no limitation on the mechanism by which the cocatalyst provides the polymerization-activatable ligand to the metallocene compound. For example, the cocatalyst can participate in a metathesis reaction to exchange an exchangeable ligand, such as a halide or alkoxide, on the metallocene compound for a polymerization-activating / initiating ligand, such as a methyl or hydride. In one embodiment, the cocatalyst is an optional component of the catalyst composition, for example, when the metallocene compound already includes a polymerization-activating / initiating ligand, such as a methyl or hydride. In another embodiment, as will be understood by those skilled in the art, even when the metallocene compound includes a polymerization-activatable ligand, the cocatalyst can be used for other purposes, such as to remove water from the polymerization reactor or process. According to a further embodiment, as the context requires or permits, the term "cocatalyst" may refer to an "activator" or may be used synonymously with the "cocatalyst" described herein.
[0046] Activator. As used herein, "activator" generally refers to a substance capable of converting a metallocene component into an active catalyst system capable of polymerizing olefins, and is intended to be independent of the mechanism by which such activation occurs. An "activator" can convert, for example, the contact product of a metallocene component and a component that provides an activatable ligand (such as an alkyl or hydride) to the metallocene into a catalyst system capable of polymerizing olefins, when the metallocene compound does not already contain such a ligand. This term is used regardless of the actual activation mechanism. Exemplary activators may include, but are not limited to, support activators, aluminoxanes, organoboron or organoborate compounds, ionizing compounds such as ionizing ionic compounds, and the like. Aluminoxanes, organoboron or organoborate compounds, and ionizing compounds may be referred to as "activators" or "co-activators" when used in a catalyst composition in which a support activator is present, but the catalyst composition is supplemented with one or more aluminoxanes, organoborons, organoborates, ionizing compounds, or other co-activators.
[0047] Support activators. The term "support activators," as used herein, refers to solid forms of activators, such as ion-exchanged clays, proton-acid-treated clays, or pillared clays, and similar insoluble supports that also function as activators. When the support activators are combined with a cocatalyst that can provide a metallocene and an activatable ligand, or optionally a metallocene and an activatable ligand, they provide a catalyst system capable of polymerizing olefins.
[0048] Ion-exchanged clays. As used herein, the term "ion-exchanged clays" refers to clays in which the exchangeable ions of naturally occurring or synthetic clays have been replaced with or exchanged for other selected ions (also referred to as "monoionic" or "monocationic" clays). Ion exchange can occur by treating natural or synthetic clays with a source of selected cations, usually from a concentrated ion solution such as a 2N aqueous solution of the cation, involving multiple exchange steps, e.g., three exchange steps. The exchanged clays can then be washed several times with deionized water to remove excess ions generated in the treatment steps, as described, for example, in Sanchez, et al., Colloids and Surfaces A: Physicochemical and Engineering Aspects, 2013, 423, 1-10, and Kawamura et al., Clay and Clay Minerals, 2009, 57(2), 150-160. Centrifugation is typically used to isolate the clay from the solution between ion treatment and washing.
[0049] Metallocene Compounds. The terms "metallocene" or "metallocene compound," as used herein, refer to any metallocene compound, regardless of the particular bonding mode, e.g., a metallocene compound in which the cycloalkadienyl-type ligand or the alkadienyl-type ligand is bonded to an η 5 -,η 3 -, or η 1 -bonding modes, and whether or not one or more of these bonding modes are accessible by the ligand. In this disclosure, the term "metallocene" refers to a transition metal or lanthanide metal compound that contains at least one substituted or unsubstituted cycloalkadienyl-type ligand or alkadienyl-type ligand, including heteroatom analogs thereof. 3The term "metallocene" is also used to refer to compounds containing at least one π-bonded allylic ligand, where the -allyl is not part of a cycloalkadienyl or alkadienyl ligand, and which may be used as the transition metal compound component of the catalyst compositions described herein. Thus, "metallocene" refers to a compound containing a substituted or unsubstituted η 3 ~η 5 -cycloalkadienyl type and η 3 ~η 5 -alkadienyl type ligands, including heteroatom analogues thereof, and cyclopentadienyl ligands, indenyl ligands, fluorenyl ligands, η 3 -η, including, but not limited to, allyl ligands, pentadienyl ligands, boratabenzenyl ligands, 1,2-azaborolyl ligands, 1,2-diaza-3,5-diborolyl ligands, substituted analogs thereof, and partially saturated analogs thereof 3 -allylic ligands. Partially saturated analogs include compounds with partially saturated η 5 cycloalkadienyl-type ligands are included, examples of which include, but are not limited to, tetrahydroindenyl, tetrahydrofluorenyl, octahydrofluorenyl, partially saturated indenyl, partially saturated fluorenyl, substituted analogs thereof, and the like. In some contexts, the metallocene is simply referred to as the "catalyst," and in much the same way, the term "cocatalyst" is used herein to refer to, for example, an organoaluminum compound. Thus, in this disclosure, metallocene ligands can be considered to include at least one substituted or at least one unsubstituted cyclopentadienyl, indenyl, fluorenyl, tetrahydroindenyl, tetrahydrofluorenyl, octahydrofluorenyl, pentadienyl, allyl, boratabenzenyl, 1,2-azaborolyl, or 1,2-diaza-3,5-diborolyl ligand, including substituted analogs thereof. For example, optional substituents can be halides, C1-C 20 Hydrocarbyl, C1-C 20 Heterohydrocarbyl, C1-C 20 Organoheteryl, fused C4-C 12a carbocyclic moiety or a fused C-C ring with at least one heteroatom independently selected from nitrogen, oxygen, sulfur, or phosphorus; 11 The heterocyclic moieties may be independently selected from:
[0050] Organoaluminum Compounds and Organoboron Compounds. The terms organoaluminum compounds and organoboron compounds, as used herein, include neutral compounds such as AlMe3 and BEt3, as well as anionic complexes such as LiAlMe4, LiAlH4, NaBH4, and LiBEt4. Thus, unless otherwise specified, aluminum and boron hydride compounds are included in the definition of organoaluminum compounds and organoboron compounds, respectively, regardless of whether the compounds are neutral or anionic.
[0051] Pillared clays. In this disclosure, "pillared clays" are defined as clay species having ordered layers with basal spacings substantially greater than 9 Å to 13 Å. When powdered clay samples are analyzed using an X-ray diffractometer capable of scanning 2θ angles of 2° or greater, species containing such pillared ordering are typically observed to have substantial peaks at 2θ values between 2° and 9°. These are typically prepared by the introduction of a pillaring agent, e.g., an oxygen-containing inorganic cation such as an oxygen-containing cation of lanthanum, aluminum, or iron. Aluminum-pillared clays are often prepared by contacting the pillaring agent with the clay in an amount ranging from about 5 mmol Al / g clay or 6 mmol Al / g clay, up to about 30 mmol Al / g clay. Typical pillared clay formulations can be contrasted with the preparation of support activators according to the present disclosure, in which the support activators disclosed herein can be prepared using about 2.0 mmol Al / g clay or less, about 1.7 mmol Al / g clay or less, about 1.5 mmol Al / g clay or less, about 1.3 mmol Al / g clay or less, or about 1.2 mmol Al / g clay or less, but greater than about 0.75 mmol Al / g clay, or greater than about 1.0 mmol Al / g clay. Thus, in one embodiment, the pillaring agent used to form the pillared clay can be selected from the same hetero-coagulation reagents used to form the hetero-coagulated clays of the present disclosure. As described herein, even during the preparation of the smectite hetero-adducts disclosed herein, some pillared clay species can be formed.
[0052] Intercalated. The terms "intercalated" or "intercalation" are terms of the art that refer to the insertion of a material between the layers of a clay substrate. These terms are used herein, unless otherwise noted, in a manner understood by those skilled in the art and as described in U.S. Pat. No. 4,637,992.
[0053] Basal Spacing. The terms "basal spacing," "basal d001 spacing," or "d001 spacing," when used in the context of smectite clays such as montmorillonite, typically refer to the distance, expressed in angstroms or nanometers, between similar planes of adjacent layers within the clay structure. Thus, for example, in the 2:1 family of smectite clays, including montmorillonite, the basal spacing is the distance from the top of a tetrahedral sheet to the top of the next tetrahedral sheet in an adjacent 2:1 layer, regardless of whether it is modified or pillared, including any intervening octahedral sheets. Basal spacing values are measured using X-ray diffraction analysis (XRD) of the d001 plane. For example, natural montmorillonite, found in ventronite, has a basal spacing ranging from about 12 Å to about 15 Å. (See, for example, Fifth National Conference on Clays and Clay Minerals, National Academy of Sciences, National Research Council, Publication 566, 1958: Proceedings of the Conference: "Heterogeneity In Montmorillonite", J.L. McAtee, Jr., pp. 279-88 and Table 1 at p. 282.) XRD test methods for determining basal spacing are described in Pillared Clays and Pillared Layered Solids, R.A. Schoonheydt et al., Pure Appl. Chem., 71(12), 2367-2371, (1999), and U.S. Pat. No. 5,202,295 (McCauley) at column 27, lines 22-43.
[0054] Zeta Potential. The term "zeta potential," as used herein, refers to the difference in electrical potential between the junction of the Stern layer (a layer of tightly attached counterions formed to neutralize the surface charge of colloidal particles) and the diffusion layer (a cloud of loosely attached ions that resides further from the particle surface than the Stern layer) and the bulk solution or slurry. This property is expressed in units of voltage, e.g., millivolts (mV). Zeta potential can be obtained by quantifying the "electrokinetic acoustic amplitude effect" (ESA), which is the generation of ultrasound waves as a result of applying an electrical potential across a colloidal suspension, as described in U.S. Pat. No. 5,616,872, incorporated herein by reference.
[0055] Hydrocarbyl Groups. As used herein, the term "hydrocarbyl group" is used in accordance with the art-recognized IUPAC definition as a monovalent, straight-chain, branched, or cyclic group formed by removing a monovalent hydrogen atom from a parent hydrocarbon compound. Unless otherwise specified, hydrocarbyl groups can be aliphatic or aromatic, saturated or unsaturated, and can contain straight-chain, cyclic, branched, and / or fused ring structures, unless any of these are specifically excluded. IUPAC Compendium of Chemical Terminology, 2 nd See Ed (1997) at 190. Examples of hydrocarbyl groups include, but are not limited to, aryl, alkyl, cycloalkyl, alkenyl, cycloalkenyl, cycloalkadienyl, alkynyl, aralkyl, aralkenyl, and aralkynyl groups.
[0056] Heterohydrocarbyl groups. The term "heterohydrocarbyl" is used in this disclosure to encompass monovalent, straight-chain, branched, or cyclic groups formed by removing a single hydrogen atom from a carbon atom of a parent "heterohydrocarbon" molecule, where at least one carbon atom is replaced with a heteroatom. The parent heterohydrocarbon can be aliphatic or aromatic. Examples of "heterohydrocarbyl" groups include halide, nitrogen, phosphorus, silicon, oxygen, and sulfur-substituted hydrocarbyl groups in which a hydrogen has been removed to form a carbon atom, resulting in a free valence. Examples of heterohydrocarbyl groups include, but are not limited to, -CH2OCH3, -CH2SPh, -CH2NHCH3, -CH2CH3NMe2, -CH2SiMe3, -CMe2SiMe3, -CH2(C6H4-4-OMe), -CH2(C6H4-4-NHMe), -CH2(C6H4-4-PPh2), -CH2CH3PEt2, -CH2Cl, -CH2(2,6-C6H3Cl2), and the like.
[0057] Heterohydrocarbyl encompasses both heteroaliphatic groups (including saturated and unsaturated groups) and heteroaromatic groups. Thus, heteroatom-substituted vinyl groups, heteroatom-substituted alkenyl groups, heteroatom-substituted dienyl groups, etc. are all encompassed by heterohydrocarbyl groups.
[0058] Organoheteryl group. The term "organoheteryl" group is also used in accordance with the art-recognized IUPAC definition as a monovalent group containing carbon, and therefore organic, but having its free valence at an atom other than carbon. IUPAC Compendium of Chemical Terminology, 2 ndSee Ed (1997) at 284. Organoheteryl groups can be linear, branched, or cyclic and include common groups such as alkoxy, aryloxy, organothio (or organylthio), organogermanium (or organylgermanium), acetamido, acetonylacetanato, alkylamido, dialkylamido, arylamido, diarylamido, trimethylsilyl, and groups such as -OMe, -OPh, -S(tolyl), -NHMe, -NMe2, -N(aryl)2, -SiMe3, -PPh2, -OS(CH4)Me, -OCF2CF3, -OC(alkyl), -OC(aryl), -N(alkyl)CO(alkyl), -N(aryl)CO(aryl), -N(alkyl)C(O)N(alkyl), hexafluoroacetonylacetanato, and the like.
[0059] Organyl Group. Organyl group is used in this disclosure to refer to any organic substituent, regardless of functional type, that has one free valence at a carbon atom according to the IUPAC definition, such as CH3CH2-, ClCH2C-, CH3C(=O)-, 4-pyridylmethyl, etc. Organyl groups may be linear, branched, or cyclic, and the term "organyl" may be used in conjunction with other terms, such as organylthio- (e.g., MeS-) and organyloxy.
[0060] Heterocyclyl group. The IUPAC Compendium compares organyl groups with other groups such as heterocyclyl and organoheteryl groups. These terms are listed in the IUPAC Compendium of Chemical Terminology, 2 ndEd (1997) states the following, which illustrates the practice of associating the "-yl" suffix with the portion of a molecule or group that derives its valence from a missing hydrogen: A heterocyclyl group is thus defined as a monovalent group formed by removing a hydrogen atom from any ring atom of a heterocyclic compound. For example, both the piperidin-1-yl and piperidin-2-yl groups shown below, in which the line drawn from the nitrogen or carbon atom represents the free valence, are heterocyclyl groups, not methyl groups: [Table 1]
[0061] However, a piperidin-1-yl group is also considered an organoheteryl group, and a piperidin-2-yl group is also considered a heterohydrocarbyl group. Thus, the valency of a "heterocyclyl" can occur at any suitable ring atom, but the valency of an "organoheteryl" occurs at a heteroatom, and the valency of a heterohydrocarbyl occurs at a carbon atom.
[0062] Hydrocarbylene and hydrocarbylidene groups. The "hydrocarbylene" group is also included in the IUPAC Compendium of Chemical Terminology, 2 nd As described in Ed (1997), a hydrocarbylene group is defined according to its common and customary meaning as a divalent group formed by removing two hydrogen atoms from a hydrocarbon, with its free valences not participating in a double bond. Examples of hydrocarbylene groups include 1,2-phenylene, 1,3-phenylene, 1,3-propanediyl (-CH2CH2CH2-), cyclopentylidene (=CC4H8), or a bridge (-CH2-) with a methylene that does not form a double bond. Hydrocarbylene groups, with their free valences not participating in a double bond, are distinguished from hydrocarbylidene groups, such as alkylidene groups.
[0063] A "hydrocarbylidene" group is a divalent group formed from a hydrocarbon by removing two hydrogen atoms from the same carbon atom, with its free valence being part of a double bond. An alkylidene group is an exemplary hydrocarbylidene, defined as a divalent group formed from an alkane by removing two hydrogen atoms from the same carbon atom, with its free valence being part of a double bond. Examples of alkylidene groups include =CHMe, =CHEt, =CMe2, =CHPh, or methylene, where the methylene carbon forms a double bond (=CH2).
[0064] Heterohydrocarbylene and Heterohydrocarbylidene Groups. The term "heterohydrocarbylene" group, analogous to a hydrocarbylene group, is used to refer to a divalent group formed by removing two hydrogen atoms from a parent heterohydrocarbon molecule, the free valences of which are not engaged in a double bond. The hydrogen atoms can be removed from two carbon atoms, two heteroatoms, or one carbon and one heteroatom, such that the free valences are not engaged in a double bond. Examples of "heterohydrocarbylidene" groups include, but are not limited to, -CHOCH, -CHNPhCH, -SiMe(1,2-CH)SiMe, -CMeSiMe, -CHNCMe, -CHCHPMe, -CH[1,2-CH(4-OMe)]CH, and the like.
[0065] Analogous to hydrocarbylidene, a "heterohydrocarbylidene" group is a divalent group formed from a heterohydrocarbon by removing two hydrogen atoms from the same carbon atom, the free valence of which is part of a double bond. Examples of heterohydrocarbylidene groups include, but are not limited to, groups such as =CHNMe2, =CHOPh, =CMeNMeCH2Ph, =CHSiMe3, and =CHCH2Cl.
[0066] Halides and Halogen. The terms "halide" and "halogen" are used herein to refer to fluorine, chlorine, bromine, or iodine ions or atoms, individually or in any combination, as context and chemistry permit or dictate. These terms may be used interchangeably regardless of the charge or bonding mode of these atoms.
[0067] Polymer. The term "polymer" is generally used herein to include olefin homopolymers, copolymers, terpolymers, and the like. Copolymers are derived from an olefin monomer and one olefin comonomer, while terpolymers are derived from an olefin monomer and two olefin comonomers. Thus, "polymer" encompasses copolymers, terpolymers, and the like derived from any olefin monomer and comonomer disclosed herein. Similarly, ethylene polymers include ethylene homopolymers, ethylene copolymers, ethylene terpolymers, and the like. Thus, an olefin copolymer, such as an ethylene copolymer, can be derived from ethylene and a comonomer such as propylene, 1-butene, 1-hexene, or 1-octene. When the monomer and comonomer are ethylene and 1-hexene, respectively, the resulting polymer is classified as an ethylene / 1-hexene copolymer. Similarly, the term "polymerization" includes homopolymerization, copolymerization, terpolymerization, and the like. For example, a copolymerization process involves contacting one olefin monomer, such as ethylene, with one olefin comonomer, such as 1-hexene, to produce a copolymer. Well-known abbreviations for polyolefin types may be used herein, such as "HDPE" for high density polyethylene.
[0068] Where the context permits or requires, the term "polymer" is used herein to refer to the inorganic composition used to prepare and form pillars in modified clays. For example, pillars are known to be formed in smectite clays based on the use of polymeric cationic hydroxymetal complexes of metals such as aluminum, zirconium, and / or titanium, e.g., aluminum chlorhydrate complexes (also known as "salt hydrates" or "chlorine hydrates"). Inorganic copolymers containing the complexes are also known. See, for example, U.S. Pat. Nos. 4,176,090 and 4,248,739. Furthermore, unless expressly stated otherwise, the term polymer is not limited by molecular weight and thus encompasses both low-molecular-weight polymers, sometimes referred to as oligomers, and high-molecular-weight polymers.
[0069] Procatalyst: The term "procatalyst," as used herein, means a compound, whether Lewis or Bronsted, that is capable of polymerizing, oligomerizing, or hydrogenating olefins when activated with an aluminoxane, borane, borate, or other acidic activator, or when activated with a support activator as disclosed herein.
[0070] Additional Explanations of Terms The following additional explanations of terms are provided in fully disclosed aspects and claims of this disclosure.
[0071] Unless otherwise specified or unless the context requires otherwise, the chemical formulas of the polymetallates used as heterocoagulants disclosed herein are empirical formulas, thus: (Al,Mg)2SiO 10 Formulas such as (OH)2(H2O)8 are empirical polymetallate formulas that can be considered to encompass oligomeric or polymeric species, and FeO x (OH) y (H2O) z ] n+ Formulas such as may also be considered to encompass oligomers or polymers where the variable subscripts are not required to be integers.
[0072] Several types of numerical ranges are disclosed herein, including, but not limited to, numerical ranges of atomic numbers, basal spacings, weight ratios, molar ratios, percentages, temperatures, etc. When disclosing or claiming any type of range, it is the intention of the applicant to separately disclose or claim each number that such range may reasonably encompass, including the endpoints of the range, and any subranges and combinations of subranges encompassed therein, consistent with the written description and context. For example, if the applicant were to disclose or claim a range of C1 to C12 (or C1 to C12), the applicant would not be limited to the ranges C1 to C12. 12 When disclosing or claiming a chemical moiety having a certain number of carbon atoms, such as an alkyl group, or alternative language having 1 to 12 carbon atoms, Applicant's intent is to refer to moieties including alkyl groups having 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, or 12 carbon atoms, independently selectable from any range between those two numbers (e.g., C1-C6 alkyl groups), and any combination of ranges between those two numbers (e.g., C2-C4 and C6-C8 alkyl groups). Applicant reserves the right to exclude or omit individual members of any such ranges or groups, including any subranges or combinations of subranges within groups, that may be claimed in a range or similar manner if for any reason Applicant chooses to claim less than the full measure of the disclosure, for example, in light of references that Applicant is not aware of at the time of filing.
[0073] In another aspect, any range of numbers set forth in the specification or claims, as representing a particular set of properties, units of measurement, conditions, physical states, or percentages, is intended to expressly incorporate herein by reference or otherwise any number falling within that range, including any subset of numbers within such stated range. For example, when a numerical range with a lower limit, R, and an upper limit, R, is disclosed, any number R falling within that range is specifically disclosed. In particular, the following numbers R within the range are specifically disclosed: R = RL + k (RU - RL), where k is a variable ranging from 1% to 100% in 1% increments, e.g., k is 1%, 2%, 3%, 4%, 5%, 50%, 51%, 52%, 95%, 96%, 97%, 98%, 99%, or 100%. Additionally, any numerical range represented by any two values of R, as calculated above, is also specifically disclosed.
[0074] For any particular compound disclosed herein, any presented general or specific structure also encompasses all stereoisomers, regioisomers, and stereoisomers that can arise from a particular set of substituents, unless otherwise indicated. Similarly, unless otherwise indicated, a general or specific structure also encompasses enantiomers, diastereomers, and other optical isomers (in either enantiomeric or racemic form), as well as mixtures of stereoisomers, as recognized by those skilled in the art.
[0075] Unless otherwise stated, values or ranges can be expressed in this disclosure using the term "about," for example, "about" the stated value, greater than or less than "about" the stated value, or ranging from "about" one value to "about" another value. When such values or ranges are expressed, other disclosed embodiments include the specific recited value, ranges between the specific recited values, and other values near the specific recited values. In one aspect, use of the term "about" means ±15% of the stated value, ±10% of the stated value, ±5% of the stated value, or ±3% of the stated value. For example, when the term "about" is used as a modifier to or in connection with a variable, property, or condition, it is intended to convey that the numerical values, ranges, properties, and conditions disclosed herein are sufficiently flexible that practice of the present disclosure by one of ordinary skill in the art using temperatures, rates, times, concentrations, amounts, contents, properties such as basal spacing, sizes including pore size, pore volume, surface area, and the like that may deviate somewhat from the stated ranges or differ from a single stated value can arrive at the desired results described herein, such as the preparation of porous catalyst support particles having the defined properties and their use in the preparation of active olefin polymerization catalysts and olefin polymerization processes using such catalysts.
[0076] The terms "a," "an," "the," etc. (e.g., "this") are intended to include plural alternatives, such as at least one, unless otherwise specified. For example, disclosure of a "support activator," an "organoaluminum compound," or a "metallocene compound" is intended to encompass mixtures or combinations of one or more catalyst support activators, organoaluminum compounds, or metallocene compounds, respectively.
[0077] The term "comprising" and its variations, such as "comprise," "comprised of," "having," and "including," are inclusive and open-ended, as recited in the transitional phrase or specification, and do not exclude additional, unrecited elements or method steps. The transitional phrase "consisting of" and its variations exclude any element, step, or ingredient not specified in the claim. The transitional phrase "consist essentially of" limits the scope of the claim to the specified ingredients or steps, as well as ingredients or steps that do not materially affect the basic and novel characteristics of the claimed invention. Unless otherwise indicated, describing a compound or composition as "consisting essentially of" should not be construed as "comprising," as this phrase is intended to describe the recited ingredients, including materials that do not materially alter the composition or method to which the term is applied. For example, a precursor or catalyst component can consist essentially of a material that, when prepared by a particular procedure, may contain impurities commonly present in commercially produced samples of the material. When a claim includes different features and / or feature classes (e.g., method steps, feedstock features, and / or product features, among other possibilities), it is possible for a transitional term to include, consist essentially of, and consist of only the feature class utilized, with different transitional terms or phrases utilized with different features within the claim. For example, a method may include several recited steps (and other unrecited steps), but utilize a catalyst system preparation that consists of specific, or alternatively essentially, specific steps, but utilizes a catalyst system that includes recited components and other unrecited components. When compositions and processes are described in terms of "comprising" various components or steps, the compositions and processes can also "consist essentially of" or "consist of" the various components or process steps.
[0078] Unless otherwise defined with respect to a particular property, characteristic, or variable, the terms "substantial" and "substantially" as applied to any criterion, such as a property, characteristic, or variable, mean meeting the stated criterion to a sufficient extent that one skilled in the art would understand that a benefit is achieved or a desired condition or property value is met. For example, the term "substantially" can be used to describe a metallocene catalyst or catalyst system that is substantially free of or substantially absent aluminoxane, borate activator, proton acid-treated clay, or pillared clay. In other words, the terms "substantially" and "substantially" serve to reasonably describe the subject matter, the scope of which is understood by those skilled in the relevant art, and to distinguish the claimed subject matter from any prior art. In one aspect, "substantially free" can be used to describe a composition in which the composition is substantially free of listed components, with only impurity amounts present, such as amounts resulting from purity limits of other components or amounts produced as by-products. In further embodiments, when a composition is said to be "substantially free" of a particular component, the composition may have less than 20% by weight of the component, less than 15% by weight of the component, less than 10% by weight of the component, less than 5% by weight of the component, less than 3% by weight of the component, less than 2% by weight of the component, less than 1% by weight of the component, less than 0.5% by weight of the component, or less than 0.1% by weight of the component.
[0079] The terms "optionally," "optional," and the like, with respect to a claim element are intended to mean that the subject element is required, or alternatively, that it is not required; both alternatives are intended to be within the scope of the claim, and it is contemplated that the claim may encompass either or both alternatives.
[0080] References to the periodic table or groups of elements within the periodic table refer to the Periodic Table of Elements published by the International Union of Pure and Applied Chemistry (IUPAC) and published online at http: / / old.iupac.org / reports / periodic_table / (February 19, 2010 edition). References to "groups" or "groups" of the periodic table as reflected in the Periodic Table of Elements, using the IUPAC system for numbering groups of elements as groups 1 through 18. To the extent that any group is identified by Roman numerals according to the Periodic Table of Elements published in, for example, "Hawley's Condensed Chemical Dictionary" (2001) (the "CAS" system), we will further identify one or more elements of that group to avoid confusion and provide a cross-reference to the numerical IUPAC identifier.
[0081] Various patents, publications, and documents are disclosed and referenced herein. Each reference cited in this disclosure, whether a patent, publication, or other document, is incorporated herein by reference in its entirety unless otherwise noted.
[0082] References that may provide some background information related to the present disclosure include, for example, U.S. Pat. Nos. 3,962,135, 4,367,163, 5,202,295, 5,360,775, 5,753,577, 5,973,084, 6,107,230, 6,531,552, 6,559,090, 6,632,894, 6,943,224, 7,041,753, 7,220,695, 9,751,961, and U.S. Patent Application Publication Nos. 2018 / 0142047 and 2018 / 0142048, each of which is incorporated by reference in its entirety. Additional publications that may provide some background information related to this disclosure include: Gu, B.; Doner, HE, Clay and Clay Minerals, 1991, 38(5), 493-500, Covarrubias et al.,Applied Catalysis A:General,347(2),15 September 2008,223-233、 Tayano et al.,Clay Science,2016,20,49-58、 Tayano et al.,Macromolecular Reaction Engineering,2017(11),201600017、 Journal of Molecular Catalysis A:Chemical,2016,420,228-236、 Clay Science,2016,20,49-58、 Finevich et al.,Russian Journal of General Chemistry 2007,77(12),2265-2271、 Bibi,Singh,and Silvester,Applied Geochemistry,2014,51,170-183、 Sharma et al.,Journal of Material Science,2018,53,10095-10110、 Okada et al.,Clay Science,2003,12,159-163、 Sucha et al.,Clay Minerals,1996,31,333-335、 Vlasova et al.,Science of Sintering,2003,35,155-166、 Kline and Fogler,Industrial&Engineering Chemistry Fundamentals,1981,20(2),155-161、 Ocelli,Clay and Clay Minerals,2000,48(2),304-308、 Kooli,Microporous and Mesoporous Materials;2013,167,228-236、 Pergher and Bertella,Materials,2017,10,712,and Tsvetkov et al.,Clay and Clay Minerals,1990,38(4),380-390, and the like, each of which is incorporated herein by reference in its entirety.
[0083] B. Overview The support activator of the present disclosure can be formed by starting with a slurry of expanded clay in a liquid carrier, such as a smectite or dioctahedral smectite clay, and contacting the clay in the slurry with a heterocoagulation reagent containing at least one cationic polymetallate prepared under the conditions specified herein. The heterocoagulated clay form can be very conveniently isolated by filtration, then dried and calcined to provide a support activator useful for supporting and activating metallocene catalysts for olefin polymerization. Formation of the clay heteroadduct in good yield can be achieved by controlling the ratio or amount of heterocoagulation reagent used relative to the clay, as determined by zeta potential measurement of the slurry in which the clay heteroadduct is formed. Thus, the clay heteroadduct comprises the product of contact, in a liquid, of [1] a smectite clay, such as a colloidal smectite clay, with [2] a sufficient amount of heterocoagulation reagent containing at least one cationic polymetallate to provide a slurry of the resulting clay heteroadduct having a zeta potential in the range of about positive 25 mV (millivolts) to about negative 25 mV.
[0084] When smectite clay is contacted with a heterocoagulation reagent in a liquid carrier using a cationic polymetallate, such as aluminum chlorhydrate (ACH), in a concentration greater than the moles per gram of clay specified immediately above, such that the resulting slurry has a zeta potential greater than about +25 mV, resulting from a reaction between the cationic polymetallate and the colloidal smectite clay. For example, using a recipe with a concentration of greater than about 2.3 mmol Al / g clay, greater than about 2.5 mmol Al / g clay, greater than about 2.7 mmol Al / g clay, or greater than about 3.0 mmol Al / g clay (millimoles of Al per gram of clay), correspondingly large amounts of pillared clay can be formed. The desired smectite heteroadduct slurry can contain some corresponding pillared clay, as observed by powder X-ray diffraction (XRD). While the formation of some pillared clay is secondary or incidental to support-activator formation, a concentration of pillared clay that is too high relative to the clay heteroadduct results in an immediate loss of filterability of the slurry, as the ease of separation of the support-activator is compromised. When smectite clay is contacted with a heterocoagulation reagent in a liquid carrier using fewer cationic polymetallates per gram of clay so that the resulting slurry has a zeta potential of less than about -25 mV, less than about 0.5 mmol Al / g clay, less than about 0.6 mmol Al / g clay, or less than about 0.8 mmol Al / g clay, or in some cases less than about 1.0 mmol Al / g clay (mmol Al per gram of clay) can be formed when using cationic polymetallate aluminum chlorhydrate (ACH) and colloidal smectite clay, and a significant amount of colloidal smectite clay can remain.
[0085] It has also been unexpectedly discovered that, in contrast to pillared clay support activators and similar clay-based activators used to support and activate metallocene catalysts, the clay heteroadduct support activators of the present disclosure require little or no subsequent washing steps after isolation by filtration. That is, the isolated heteroadduct support activator can be used directly in catalyst formation with a metallocene, and a cocatalyst such as an aluminum alkyl, if desired, without extensive or time-consuming purification, washing, or other such purification steps commonly used with other clay-based supports. This advantage can provide substantial economic benefits and enhanced ease of use when preparing olefin polymerization catalysts.
[0086] Thus, in one aspect, the present disclosure provides a support activator comprising an isolated smectite heteroadduct, the smectite heteroadduct comprising the contact product, in a liquid, of: [1] colloidal smectite clay; and [2] a heterocoagulation reagent in an amount sufficient to provide a slurry of smectite heteroadducts, the heteroadduct comprising at least one cationic polymetallate, the heterocoagulation reagent having a zeta potential in the range of about positive 25 millivolts (mV) to about negative 25 mV.
[0087] The present disclosure also provides, in another aspect, a method for producing a support activator comprising a smectite heteroadduct, the method comprising: a) providing a colloidal smectite clay; b) contacting the colloidal smectite clay with a hetero-coagulation reagent in a liquid carrier in an amount sufficient to provide a slurry of smectite hetero-adducts comprising at least one cationic polymetallate and having a zeta potential in the range of about positive 25 mV (millivolts) to about negative 25 mV.
[0088] The method may further include the step of c) isolating the smectite heteroadduct from the slurry.
[0089] According to a further aspect, the present disclosure provides a catalyst composition for olefin polymerization, the catalyst composition comprising: a) at least one transition metal catalyst, such as a metallocene compound; b) optionally at least one co-catalyst; c) at least one supported activator comprising a calcined smectite heteroadduct, the smectite heteroadduct comprising the contact product of: (1) colloidal smectite clay; and (2) a heterocoagulation reagent in a liquid carrier, the heterocoagulation reagent comprising at least one cationic polymetallate, in an amount sufficient to provide a slurry of the smectite heteroadduct having a zeta potential in the range of about positive 25 millivolts (mV) to about negative 25 mV.
[0090] In yet a further aspect, a method for producing an olefin polymerization catalyst, the method comprising, in any order: a) at least one transition metal catalyst, such as a metallocene compound; b) optionally at least one co-catalyst; c) contacting the support with at least one support activator comprising a calcined smectite heteroadduct as described in accordance with the present disclosure.
[0091] Yet another aspect of the present disclosure is a process for polymerizing olefins comprising contacting at least one olefin monomer and a catalyst composition under polymerization conditions to form a polyolefin, wherein the catalyst composition comprises: a) at least one transition metal catalyst, such as a metallocene compound; b) optionally at least one co-catalyst; c) at least one support activator comprising a calcined smectite heteroadduct, as described herein.
[0092] For detailed information on various aspects and embodiments, see the examples, data, and aspects of this written description that describe making and using the support activators and catalyst compositions described herein. The following sections provide specific details of some of the components used to prepare the catalyst compositions and to polymerize olefins using the catalyst compositions.
[0093] C. Colloidal smectite clay In addition to the definitions section, the following disclosure provides additional information related to smectite clays.
[0094] Expanded clays, such as smectites or 2:1 dioctahedral smectite clays, or combinations of expanded clays, can be used to prepare the support activators described herein. These expanded clays can be described as phyllosilicates or phyllosilicate clays, as they are specific members of the phyllosilicate clay mineral group. Suitable starting clays can include layered, naturally occurring, or synthetic smectites. Starting clays can also include dioctahedral smectite clays. Additionally, suitable starting clays can include clays such as montmorillonite, sauconite, nontronite, hektronite, beidellite, saponite, bentonite, or any combination thereof. Smectites are 2:1 layered clay minerals that carry a lattice charge and can expand upon solvation with water and alcohol. Therefore, suitable starting clays include, for example, monoion-exchanged dioctahedral smectites, such as lithium-exchanged clays, sodium-exchanged clays, or potassium-exchanged clays, or combinations thereof.
[0095] Water can also be coordinated to the layered clay structural units, either associated with the clay structure itself or coordinated to cations as hydration shells. When dehydrated, 2:1 layered clays have a repeat distance or d001 basal spacing of about 9 Å to about 12 Å in powder X-ray diffraction (XRD), or alternatively, a range of about 10 Å to about 12 Å in powder X-ray diffraction (XRD).
[0096] Layered smectite clays are also referred to as 2:1 clays because their structure is a "sandwich" structure containing two outer sheets of tetrahedral silicate and an inner sheet of octahedral alumina sandwiched between the silica sheets. Therefore, these structures are also referred to as "TOT" (tetrahedron-octahedron-octahedron) structures. These sandwich structures are stacked one on top of the other to produce clay particles. This configuration provides a repeating structure approximately every 9 and a half angstroms (Å), providing greater spacing between the natural clay layers compared to pillared or intercalated clays produced by inserting "pillars" of inorganic oxide material between these layers.
[0097] In one embodiment, the clay used to prepare the support activator can be colloidal smectite clay. Thus, the smectite clay can have an average particle size of less than about 10 μm (microns), less than about 5 μm, less than about 3 μm, less than 2 μm, or less than 1 μm, and the average particle size is greater than about 15 nm, greater than about 25 nm, greater than about 50 nm, or greater than about 75 nm. That is, any range of clay particle size between these listed numbers is disclosed. Clays that cannot form colloidal suspensions can be used, but they are less preferred than colloidal clays.
[0098] In one embodiment, the clay used to prepare the support activator can be devoid of divalent or trivalent ion-exchanged smectite, such as Mg-exchanged montmorillonite or Al-ion-exchanged montmorillonite, as described in U.S. Patent No. 6,531,552. In another embodiment, the clay used to prepare the support activator can be devoid of mica or synthetic hectorite, as described in U.S. Patent Nos. 6,531,552 and 5,973,084. In a further embodiment, the clay used to prepare the support activator can be devoid of trihedral smectite or vermiculite.
[0099] In one embodiment, the smectite clay also has the following formula: (M A IV)8(M B VI) p O 20 (OH)4(in the formula, a)M A IV is tetracoordinated Si 4+ and Si 4+ But Si 4+ Optionally, partially substituted by a tetracoordinate cation that is not (e.g., Si 4+ The cation that is not 3+ , Fe 3+ , P 5+ , B 3+ , Ge 4+ , Be 2+ , Sn 4+ can be selected independently from b)M B VI is hexacoordinated Al 3+ or Mg 2+ and Al 3+ or Mg 2+ But, Al 3+ or Mg 2+ Optionally partially substituted by a hexacoordinate cation that is not (e.g., Al 3+ or Mg 2+ The cation that is not 3+ , Fe 2+ , Ni 2+ , Co 2+ , Li+ , Zn 2+ , Mn 2+ , Ca 2+ , Be 2+ can be selected independently from c) p is 4 for a cation with a +3 formal charge, or p is 6 for a cation with a +2 formal charge; d) M A Si in IV 4+ Any charge deficiency resulting from partial substitution of a cation other than M B Al in VI 3+ or Mg 2+ The structural units can be characterized in that any charge deficit resulting from partial substitution of a cation other than 1 is balanced by cations intercalated between the structural units (e.g., the cations intercalated between the structural units can be selected from monocations, dications, trications, other multications, or any combination thereof).
[0100] The Examples, Data, and Aspects of the Disclosure section provide additional details of various aspects and embodiments of smectite clays.
[0101] D. Cationic polymetalates used in heterocoagulation reagents In addition to the "Definitions" section and aspects of the present disclosure, the following additional information further describes cationic polymetallates.
[0102] As explained in the Definitions section, the term "polymetallate" and similar terms such as "polyoxometallate" refer to polyatomic cations containing two or more metals (e.g., aluminum, silicon, titanium, zirconium, or other metals) with at least one bridging ligand between the metals, such as an oxo, hydroxy, and / or halide ligand. For example, polymetallates can be hydrated metal oxides, hydrated metal oxyoxides, etc., and can include bridging ligands such as oxo ligands that can bridge two or more metals in these species, and can also include terminal oxo, hydroxyl, and / or halide ligands. While many polymetallate species are anionic and the suffix "-ate" is often used to reflect anionic species, the polymetallate (polyoxometallate) compounds used in accordance with the present disclosure are cationic.
[0103] The heterocoagulation reagents of the present disclosure can be positively charged species that, when combined in the appropriate ratio with a clay colloidal suspension, form an easily filterable, easily washed coagulum. Positively charged species include soluble polyoxometalates, polyhydroxylmetalates, and polyoxohydroxymetallate cations, as well as related cations with partial halide substitution, such as polyaluminum oxyhydroxychloride, aluminum chlorohydrate, or polyaluminum chloride species, which are linear, cyclic, or cluster compounds. These compounds are collectively referred to as polymetalates. The latter aluminum compounds can contain from about 2 to about 30 aluminum atoms.
[0104] Useful heterocoagulation reagents also include any colloidal species characterized by a positive zeta potential when dispersed in aqueous or mixed aqueous and organic solvents (e.g., alcohol). For example, useful dispersions of heterocoagulation reagents can exhibit a zeta potential greater than (>) +20 mV (positive 20 mV >), a zeta potential greater than +25 mV, or a zeta potential greater than +30 mV. The starting colloidal clay may contain monovalent ions or species such as protons, lithium ions, sodium ions, or potassium ions, but at least a portion, some, most, substantially all, or all of these ions are replaced by the heterocoagulation reagent during the formation of the readily filterable clay heteroadduct. As discussed below, protons, lithium ions, sodium ions, potassium ions, or the like do not provide the filterability afforded by the cationic polymetallates of the present disclosure. This characteristic can be observed by the long filtration times encountered when preparing and attempting to isolate hydrochloric acid-treated support activators, such as those in Examples 40 and 41.
[0105] Furthermore, unlike processes that use strong, concentrated acids to leach Al ions from montmorillonite, the formation of clay heteroadducts does not leach Al ions from the clay. When using aluminum-containing heterocoagulation reagents such as ACH or PAC, the aluminum content of the support activator, although much less than that of the corresponding pillared clay, actually increases over that of the starting clay.
[0106] In one embodiment, the heterocoagulation reagent can include a colloidal suspension of bohemian (aluminum oxide hydroxide) or a metal oxide, such as a fumed metal oxide, which imparts a positive zeta potential (e.g., fumed alumina). In another embodiment, the heterocoagulation reagent can include a chemically modified or treated metal oxide, such as fumed silica treated with aluminum chlorhydrate, such that when in suspension, the chemically treated metal oxide imparts a positive zeta potential, as described below. In a further embodiment, the heterocoagulation reagent is produced by treating a metal oxide or metal oxide hydroxide, etc., with the reagent in a fluidized bed, resulting in a positive zeta potential when the reagent is dispersed in suspension. The heterocoagulation reagent can exhibit a positive value of greater than +20 mV before combination with the phyllosilicate clay component.
[0107] In one embodiment, the cationic polymetallate can include a first metal oxide that is chemically treated with a second metal oxide, a metal halide, a metal oxyhalide, or a combination thereof, in an amount sufficient to provide a colloidal suspension of the chemically treated first metal oxide having a positive zeta potential, e.g., a zeta potential greater than 20 millivolts (mV). That is, the chemically treated first metal oxide is the contact product of the first metal oxide with [1] a second metal oxide, i.e., another, different metal oxide, [2] a metal halide, [3] a metal oxyhalide, or [4] a combination thereof. For example, the chemically treated first metal oxide can include fumed silica, fumed alumina, fumed silica-alumina, fumed magnesia, fumed zinc oxide, fumed titania, fumed zirconia, fumed ceria, or the like, or any combination thereof. The second metal oxide, metal halide, or metal oxyhalide can be obtained from an aqueous solution or suspension of a metal oxide, hydroxide, oxyhalide, or halide, such as ZrOCl2, ZnO, NbOCl3, B(OH)3, AlCl3, or a combination thereof. For example, the treatment can consist of dispersing the fumed oxide in a solution of aluminum chlorhydrate. In the case of fumed silica, which can exhibit a negative zeta potential in suspension, after treatment with aluminum chlorhydrate, the suspension of the chemically treated fumed silica exhibits a positive zeta potential of greater than about +20 mV.
[0108] In another embodiment, the cationic polymetallate composition can include or be selected from: [1] fumed silica, fumed alumina, fumed silica-alumina, fumed magnesia, fumed zinc oxide, fumed titania, fumed zirconia, fumed ceria, or any combination thereof; and [2] chemically treated with polyaluminum chloride, aluminum chlorhydrate, aluminum sesquichlorohydrate, polyaluminum oxyhydroxychloride, or any combination thereof. For example, the cationic polymetallate composition can include or be selected from aluminum chlorhydrate-treated fumed silica, aluminum chlorhydrate-treated fumed alumina, aluminum chlorhydrate-treated fumed silica-alumina, or any combination thereof.
[0109] While not intending to be bound by theory, it is believed that the treated metal oxide may form a core-shell structure of a positively charged shell and a negative core, or a continuous structure of mixed negative and positive regions or atoms, such that the surface exhibits a positive zeta potential of greater than about +20 mV. Some fumed metal oxides, such as fumed alumina, may already exhibit a positive zeta potential before chemical treatment. Nevertheless, fumed metal oxides that do not have a zeta potential or have a positive zeta potential of less than about +20 mV may be chemically treated with species such as aluminum chlorohydrate to obtain a colloidal suspension with a zeta potential of greater than about +20 mV after treatment.
[0110] In another embodiment, the heterocoagulation reagent can include a fuming process or a mixture of metal oxides formed after the fuming process that exhibit a positive zeta potential due to their composition. An example of this type of fumed oxide is fumed silica alumina.
[0111] In another embodiment, the heterocoagulation reagent can include any colloidal inorganic oxide particles, such as colloidal ceria or colloidal zirconia, as described by Lewis et al., U.S. Pat. No. 4,637,992, incorporated herein by reference, or any positively charged colloidal metal oxide disclosed therein. In another aspect, the heterocoagulation reagent can include magnetite or ferrihydrite. For example, the cationic polymetallate can include or be selected from bohemian, fumed silica alumina, colloidal ceria, colloidal zirconia, magnetite, ferrihydrite, any positively charged colloidal metal oxide, or any combination thereof.
[0112] In another embodiment, the heterocoagulation reagent can include a cationic oligomeric or polymeric aluminum species in solution, such as aluminum chlorohydrate, also known as aluminum chlorhydrate (ACH), polyaluminum chloride (PAC), aluminum sesquichlorohydrate, or any combination or mixture thereof. For example, a cationic polymetallate heterocoagulation reagent can have the following empirical formula: Al2(OH) n Cl m (H2O) x , The aluminum species may comprise or be selected from any combination of species having the formula: wherein n+m=6 and x is a number from 0 to about 4.
[0113] In one embodiment, the cationic polymetallate has the formula [AlO(Al 12 (OH) 24 (H2O) 20 ] 7+ The aluminum species may include or be selected from, which have the following structure: 13 -mer" polycation, Al 13 It is thought to be a precursor of pillared clay.
[0114] When using aluminum chlorhydrate as a heterocoagulation or chemical treatment reagent for treating other metal oxides, commercially available aluminum chlorhydrate (ACH) solutions or solid powders are available. Aluminum chlorhydrate solutions, also known as polymeric cationic hydroxyaluminum complexes or aluminum chlorohydroxides, refer to polymers formed from monomer precursors with the general empirical formula 0.5[Al(OH)Cl(H0)]. Preparation of aluminum chlorhydrate solutions is described in U.S. Patent Nos. 2,196,016 and 4,176,090, both of which are incorporated herein by reference, and involves treating an amount of aluminum metal with hydrochloric acid to produce a composition having the above formula.
[0115] Alternatively, aluminum chlorhydrate solutions can be obtained using a variety of aluminum sources, such as alumina (Al2O3), aluminum nitrate, aluminum chlorhydrate or other aluminum salts, and treatment with acid or base. There are numerous species that can be present in such solutions, including tridecameric [AlO4(Al 12 (OH) 24 (H2O) 20 ] 7+ (Al 13 (-mer) polycations are described in Perry and Shafran, Journal of Inorganic Biochemistry, 2001, 87, 115-124, which is incorporated herein by reference. The species disclosed in this work, either individually or in combination, present in such solutions can be used as cationic polymetalates for heterocoagulation of smectite clays.
[0116] In one embodiment, aqueous aluminum chlorhydrate solutions used in accordance with the present disclosure can have an aluminum content, calculated or expressed as weight percent of Al2O3, in the range of about 15 wt% to about 55 wt%, although more dilute concentrations can be used. The use of more dilute solutions can involve adjustments to other reaction conditions, such as time and temperature, as would be understood by one of ordinary skill in the art. Alternative aluminum concentrations, expressed as weight percent Al2O3, in aqueous solutions of aluminum polymetalates, such as aqueous solutions of aluminum chlorhydrate, can include about 0.1 wt% to about 55 wt% Al2O3, about 0.5 wt% to about 50 wt% Al2O3, about 1 wt% to about 45 wt% Al2O3, about 2 wt% to about 40 wt% Al2O3, about 3 wt% to about 37 wt% Al2O3, about 4 wt% to about 35 wt% Al2O3, about 5 wt% to about 30 wt% Al2O3, or about 8 wt% to about 25 wt% Al2O3, with each range including all individual concentrations expressed to one-tenth (0.1) of a weight percent subsumed therein and including any subranges therein. For example, a description of about 0.1 wt% to about 30 wt% Al2O3 includes a description of 10.1 wt% to about 26.5 wt% Al2O3. Conveniently, a solid polymetallate such as solid aluminum chlorhydrate can be used and added to the colloidal clay slurry when preparing the heterocoagulant. Therefore, the concentrations disclosed above are exemplary rather than limiting.
[0117] In one embodiment, the cationic polymetallate can comprise or be selected from oligomers prepared by copolymerizing (co-oligomerizing) a soluble rare earth salt with a cationic metal complex of at least one additional metal selected from aluminum, zirconium, chromium, iron, or a combination thereof, in accordance with U.S. Pat. No. 5,059,568, which is incorporated herein by reference, and wherein the at least one rare earth metal can be cerium, lanthanum, or a combination thereof. In one embodiment, the heterocoagulation reagent comprises a lanthanide and Al complex as described by McCauley in U.S. Pat. No. 5,059,568. 13The calcined clay heteroadducts prepared using McCauley-type polymetallates, however, do not provide uniform intercalation structures with basal spacings greater than 13 Å (angstroms). Without wishing to be bound by theory, it is believed that this observation may result from the much lower ratio of Ce-Al heterocoagulation reagent to colloidal clay used in accordance with the present disclosure. This lower ratio results from conditions that contact the smectite clay with the heterocoagulation reagent in an amount sufficient to provide a slurry of smectite heteroadducts with a zeta potential ranging from about +25 mV (millivolts) to about -25 mV.
[0118] In a further aspect, exemplary polymetallates of the present disclosure include: [1] ε-Keggin cation [ε-PMo 12 O 36 (OH)4{Ln(H2O)4}4] 5+ where Ln can be La, Ce, Nd or Sm, and [2] the general formula [LnV 12 O 32 (H2O)8{Cl}]Cl, where Ln can be Eu, Gd, Dy, Tb, Ho, or Er.
[0119] In another embodiment, the heterocoagulant can be a layered double hydroxide, such as that described in Abend et al., Colloid Polym. Sci. 1998, 276, 730-731, or synthetic hematite, hydrotalcite, or other positively charged layered double hydroxides, including, but not limited to, those described in U.S. Pat. No. 9,616,412, incorporated herein by reference. Thus, the cationic polymetallate used as the heterocoagulant can be a layered double hydroxide or a mixed metal layered hydroxide. For example, the mixed metal layered hydroxide can be selected from Ni-Al, Mg-Al, or Zn-Cr-Al types, which have positive layer charges. In another embodiment, the layered double hydroxide or mixed metal layered hydroxide can be selected from aluminum magnesium hydroxide nitrate, aluminum magnesium hydroxide sulfate, aluminum magnesium hydroxide chloride, Mg x (Mg,Fe)3(Si,Al)4O 10 (OH)2(H2O)4 (where x is a number between 0 and 1, e.g., about 0.33 for ferrosaponite), (Al,Mg)2SiO 10 (OH)2(H2O)8, synthetic hematite, zinc oxide (basic zinc carbonate) Zn5(OH)6(CO3)2, hydrotalcite [Mg6Al2(OH) 16 ]CO3●4H2O, taconite [Ni6Al2(OH)6]CO3●4H2O, hydrocalumite [Ca2Al(OH)6]OH●6H2O, mag-aldorate [Mg 10 Al5(OH) 31 ](SO4)2●mH2O, pyroaurite [Mg6Fe2(OH) 16 ]CO3●4.5H2O, Ettringite [Ca6Al2(OH) 12 ](SO4)3●26H2O, or any combination thereof.
[0120] In still further embodiments, the heterocoagulation reagent can comprise an aqueous solution of Fe polycations as described by Oades, Clay and Clay Minerals, 1984, 32(1), 49-57, or as described by Cornell and Schwertmann in "The Iron Oxides: Structure, Properties, Reactions, Occurrences and Uses", 2003, Second Edition, Wiley VCH. The thionic polymetallate has the empirical formula FeO x (OH) y (H2O) z ] n+ wherein 2×+y is (<) 3, z is a number from 0 to about 4, and n is a number from 1 to 3.
[0121] The use of cations such as protons, lithium ions, sodium ions, or potassium ions, as described in Examples 40 and 41, does not result in clay heteroadducts like those provided by the cationic polymetallates of the present disclosure; for example, these acid-treated clays are generally not easily filterable. Without wishing to be bound by theory, it is believed that monovalent ions, such as protons from HCl or H2SO4 in aqueous solutions, as described in U.S. Patent No. 6,531,552 to Nakano et al. and references therein, incorporated herein by reference, are unable to form stable, easily filterable heterocoagulated clay adducts, even when using dilute or concentrated acids. Colloidal dispersions of smectites, such as ventronite or montmorillonite, possess a permanent negative charge and therefore exhibit a permanently negative zeta potential, even at low pH. Again, without being bound by theory, at high acid concentrations at low pH (<3), smectite colloidal dispersions become less negative, potentially even approaching a negative zeta potential of approximately 30 mV (-30 mV). (See Duran et al., Journal of Colloid and Interface Science, 2000, 229, p 107-117, which is incorporated herein by reference.) However, it is believed that before the colloidal clay approaches a neutral or nearly neutralized surface charge, the clay structure itself is disrupted by peptidation of the octahedral alumina layers. (See Tayano et al., Macromolecular Reaction Engineering, 2017, 11, 201600017 and Clay Science 2016, 20, 49-58, each of which is incorporated herein by reference.Leaching of the octahedral alumina layers from the TOT structure and dissolution of clays in strongly acidic solutions are described, for example, in U.S. Pat. No. 3,962,135, Bibi, Singh, and Silvester, “Dissolution kinetics of kaolinite, illite, and montmorillonite under acid-sulfate conditions: a comparative study,” prepared for Clay Minerals, Chapter 4 (manuscript reviewed at https: / / ses.library.usyd.edu.au / bitstream / handle / 2123 / 8647 / Chapter%204_Dissolution%20of%20illite,%20kaolinite,%20montmorillonite.pdf?sequence=5), and also in https: / / pdfs.semanticscholar.org / 6836 / 3c9c293dfd4255f9ad88678e1770c63384d3.pdf, and Dudkin et al. al., Chemistry for Sustainable Development, 2004, 12, 327-330, and Okada, et al., Clay Science, 2003, 12, 159-165, each of which is incorporated herein by reference.
[0122] Without wishing to be bound by theory, it has been observed that the addition of other aprotic monovalent cations, such as lithium, sodium, or potassium ions, to the point where coagulation of colloidal smectite particles can occur through their respective salts is believed to be due to shielding and reducing columbic repulsion between smectite particles. The concentration of monocation at which coagulation occurs is referred to as the critical coagulation concentration, and the concentration of monovalent cations required to achieve coagulation is generally significantly higher than that required when using divalent or trivalent cations. Again, without wishing to be bound by theory, monovalent cation clay products are difficult to filter and may require isolation by centrifugation or high dilution and settling tanks. Without washing and removing the monovalent ion salts, the coagulated clay will not yield a metallocene-support-activator catalyst with sufficient practical activity. Furthermore, to the extent that simple ion intercalations, such as sodium-exchanged montmorillonite or aluminum-exchanged montmorillonite, may be evident in the powder XRD of the calcined clay heteroadducts, it is believed that these materials arise as undesirable by-products or result from incomplete reaction of the colloidal clay with the polymetallate.
[0123] In another embodiment, the colloidal smectite clay can include or be selected from colloidal montmorillonite, such as Volclay® HPM-20 ventronite. The heterocoagulation reagent can include or be selected from aluminum chlorohydrate, polyaluminum chloride, or aluminum sesquichlorohydrate.
[0124] According to one embodiment, the cationic polymetallate has the following formula: [M(II) 1-x M(III) x (OH)2]A x / n mL (I) [LiAl2(OH)6]A 1 / n mL (II) (In the formula, M(II) is at least one divalent metal ion; M(III) is at least one trivalent metal ion; A is at least one inorganic anion; L is an organic solvent or water, n is the valence of the inorganic anion A, or in the case of several anions A, the average valence thereof; x is a number between 0.1 and 1, and m is a number from 0 to 10), the compound may comprise or be selected from a compound of Formula I or Formula II, or any combination of compound of Formula I or Formula II.
[0125] In this embodiment, M(II) can be zinc, calcium, strontium, barium, iron, cobalt, nickel, cadmium, manganese, copper, or magnesium; independently, M(III) can be iron, chromium, manganese, bismuth, cerium, or aluminum; A can be, for example, hydrogen carbonate (bicarbonate), sulfate, nitrate, nitrite, phosphate, chloride, bromide, fluoride, hydroxide, or carbonate; n can be, for example, a number from 1 to 3; and L can be, for example, methanol, ethanol, or isopropanol, or water. In addition to this embodiment, the cationic polymetallate is selected from a complex of formula I, where M(II) is magnesium, M(III) is aluminum, and A can be carbonate.
[0126] In one embodiment, the cationic polymetallate can include polyaluminum chloride, aluminum chlorohydrate, aluminum sesquichlorohydrate, or polyaluminum oxyhydroxychloride, or a combination thereof. In a further embodiment, the cationic polymetallate can include linear, cyclic, or cluster aluminum compounds containing, for example, 2 to 30 aluminum atoms. The ratio of millimoles (mmol) of aluminum (Al) in polyaluminum chloride, aluminum chlorohydrate, aluminum sesquichlorohydrate, or polyaluminum oxyhydroxychloride to grams (g) of colloidal smectite clay in a recipe for preparing a smectite heteroadduct can be in the range of, for example, from about 0.75 mmol Al / g clay to about 2.0 mmol Al / g clay, from about 0.8 mmol Al / g clay to about 1.9 mmol Al / g clay, from about 1.0 mmol Al / g clay to about 1.8 mmol Al / g clay, from about 1.1 mmol Al / g clay to about 1.8 mmol Al / g clay, or from about 1.1 mmol Al / g clay to about 1.7 mmol Al / g clay. Alternatively, the millimoles (mmol) of aluminum (Al) in the polyaluminum chloride, aluminum chlorohydrate, aluminum sesquichlorohydrate, or polyaluminum oxyhydroxychloride per gram (g) of colloidal smectite clay in a recipe for preparing a smectite heteroadduct can be, for example, about 0.75 mmol Al / g clay, about 0.8 mmol Al / g clay, about 0.9 mmol Al / g clay, about 1.0 mmol Al / g clay, about 1.1 mmol Al / g clay, about 1.2 mmol Al / g clay, about 1.3 mmol Al / g clay, about 1.4 mmol Al / g clay, about 1.5 mmol Al / g clay, about 1.6 mmol Al / g clay, about 1.7 mmol Al / g clay, about 1.8 mmol Al / g clay, about 1.9 mmol Al / g clay, or about 2.0 mmol Al / g clay, including any combination of these ratios or subranges therebetween.
[0127] In further embodiments, the ratio of millimoles (mmol) of aluminum (Al) in the polyaluminum chloride, aluminum chlorohydrate, aluminum sesquichlorohydrate, or polyaluminum oxyhydroxychloride to grams (g) of isolated or calcined smectite heteroadduct of colloidal smectite clay can be about 90% or less, about 80% or less, about 70% or less, about 60% or less, about 50% or less, about 45% or less, about 40% or less, or about 35% or less of the comparable ratio of millimoles of aluminum to grams of colloidal clay used to prepare a pillared clay using the same colloidal smectite clay and heterocoagulation reagent.
[0128] In this embodiment, the ratio of aluminum intake to clay in the pillaring recipe is expressed as mmol Al / g clay, which refers to the number of millimoles of Al in the aluminum chlorhydrate reagent and the number of grams of clay in the recipe. Specifically, this ratio reflects the ratio used in the synthesis recipe, not the ratio in the final pillared clay product. For example, see the Al 13 Considering the Keggin type ion, the amount of Al used in the pillared clay preparation far exceeds the amount of Al ultimately intercalated between the layers in the pillared clay solid. The use of excess aluminum reagent is used to maximize the pillar content in the final product and to obtain the desired porosity and surface area of the final fired material. Kooli in Microporous and Mesoporous Materials; 2013, 167, 228-236 discloses that a recipe typically requires approximately 6 mmol Al / gram clay to optimize pillaring. Al 13 Recent scale-up studies and optimization of Keggin ionic columnar viscosity, Pergher and Bertella in Materials, 2017, 10, 712, disclose that 15 mmol Al / g clay and approximately 1 wt% diluted dispersion are required to obtain columns with the desired basal spacing and surface area.
[0129] E. Preparation and Properties of Clay Heteroadducts (Heterosolidified Clays) Unlike pillared clays, the hetero-coagulated clays of the present disclosure are amorphous solids. Thus, the preparation of hetero-coagulated clays provides a three-dimensional structure, but it is a non-pillared, non-crystalline, and amorphous structure. Without intending to be bound by theory, it is believed that the regular crystalline structure of the starting smectite is not simply expanded upon contact with the cationic polymetallate as described, but is disrupted during the preparation of the clay hetero-adduct, providing a non-crystalline, non-ordered, non-layered amorphous material. Factors that can affect the formation of an amorphous three-dimensional structure include reaction time, reaction temperature, purity and clay particle size of the starting clay, drying method, etc., which can be easily determined for each hetero-coagulated reagent and clay system, as described herein.
[0130] In preparing the clay heteroadduct, the heterocoagulant may be added to a slurry of colloidal clay, the colloidal clay may be added to a slurry or solution of the heterocoagulant, or the heterocoagulant and colloidal clay may be added to a liquid carrier simultaneously or during overlapping periods. Alternatively, the heterocoagulant and colloidal clay may be added simultaneously to the heel of the heteroadduct product, such as by adding the heterocoagulant and clay as either a solid or a suspension to a vessel or reactor containing water or a water-containing heel.
[0131] In one embodiment, the liquid carrier in which the clay heteroadduct is prepared can be water or a water-based system to which additional components such as alcohol and / or at least one surfactant can be added. Suitable surfactants can include anionic surfactants, cationic surfactants, or nonionic surfactants. Specific examples of liquid carriers or "diluents" and specific examples of surfactants are provided in the Disclosure Aspects section.
[0132] As described, the ratio of heterocoagulant to clay used in the recipe is defined as the ratio that results in a coagulation product mixture, such as a slurry, with a zeta potential ranging from approximately positive (+) 25 mV (millivolts) to approximately negative (-) 25 mV. Therefore, the amount of heterocoagulant to be added to a known clay sample, i.e., the ratio of cationic polymetallate (heterocoagulant) to clay, is determined by titrating the clay with the heterocoagulant. For example, if the heterocoagulant contains a cationic polymetallate of aluminum, the ratio of heterocoagulant to clay can be reported in millimoles (mmol) of aluminum (Al) in the cationic polymetallate to grams (g) of clay. The actual amount of cationic polymetalate used to form the clay heteroadduct, i.e., the ratio of heterocoagulant to clay, may depend on factors such as the degree of positive charge of the cationic polymetalate and the zeta potential of the clay. The heterocoagulant and clay are combined, resulting in a slurry (dispersion) of heterocoagulated clay exhibiting a zeta potential ranging from approximately +25 mV to approximately -25 mV. Alternatively, the hetero-coagulation reagent and clay are combined in a ratio such that the resulting dispersion of hetero-coagulated clay exhibits a zeta potential in the range of about +22 mV to about −22 mV, about +20 mV to about −20 mV, about +18 mV to about −18 mV, about +15 mV to about −15 mV, about +10 mV to about −10 mV, about +5 mV to about −5 mV, or about 0 mV.
[0133] As described in the Examples, a Colloidal Dynamic Zeta Probe Analyzer™ was used for zeta potential measurements, which involved dynamically tracking the evolving zeta potential during the titration of colloidal clay dispersions with cationic polymetallate titrants. Exemplary results from zeta potential titrations are illustrated in the figures and described in the Examples, and data are presented, for example, in Tables 4-6. For example, Figure 3 plots the zeta potential of a series of dispersions formed during the titration of Volclay® HPM-20 montmorillonite with aluminum chlorhydrate (ACH), plotting the cumulative titrated volume (x) of added aqueous ACH solution versus the zeta potential (mV, (y)) of the dispersions. Similarly, Figure 4 plots the cumulative mmol Al / g clay versus the zeta potential (mV) of the dispersions for the same titrations. Samples of several solid products formed during this zeta potential titration of HPM-20 clay with ACH were collected. Figure 2 shows powder XRD patterns for a series of calcined products collected during this zeta potential titration of HPM-20 clay with ACH. The results compared and correlated mmol Al / g clay with zeta potential and the filterability of the resulting products. This analysis unexpectedly revealed that when clay and a heterocoagulation reagent containing at least one cationic polymetallate were contacted in a liquid carrier in amounts or ratios that provided slurries of smectite heteroadducts with zeta potentials ranging from about 25 mV to about 25 mV, the resulting products were readily filterable and could be used as support activators with no or minimal washing, imparting high polymerization activity to supported metallocene catalysts.
[0134] In synthesis reactions or titrations using cationic polymetalates, calculating the ratio of millimoles of metal atoms in the polymetalate per mass of clay provides a useful metric for comparison between polymetalates. For example, in zeta potential titrations using aluminum cationic polymetalates as heterocoagulation reagents, the ratio of millimoles of aluminum per mass of clay allows for a more direct comparison of different Al-containing heterocoagulation reagents, as shown in the titration curves in Figure 4. This value is derived by obtaining the aluminum weight percent of the heterocoagulant, which is typically provided directly from the manufacturer or as an aluminum oxide (e.g., Al2O3) equivalent percent. In the latter case, the aluminum weight percent can be derived by multiplying the weight fraction of aluminum in the empirical formula by the aluminum oxide weight percent. From this aluminum weight percent, the molar amount of the aluminum heterocoagulation reagent can be determined, and the molar aluminum / clay mass ratio can be obtained.
[0135] For example, Figure 4 shows that the ratio of aluminum chlorohydrate (ACH) to clay in Volclay® HPM-20, expressed in mmol Al / g of clay, within the desired zeta potential range is 1.76 mmol Al / g clay. The actual ratio may vary slightly depending on the aluminum chlorhydrate lot, preparation method, contamination or age, and / or the specific batch of Volclay® HPM-20. Figure 2 shows the zeta potential titration of American Colloid Company's Volclay® HPM-20 with 22 wt% aluminum chlorhydrate from GEO Specialty Chemicals. Thus, mmol Al / g clay can be determined as the point at which the zeta potential of the colloidal species in the mixture is less than +25 mV and greater than -25 mV, e.g., about +10 mV to -10 mV, providing a heterogeneously coagulated solid that is easily isolated by conventional filtration methods, such as using filter paper, as described in detail below. Thus, ready filtration of the resulting clay heteroadduct can be carried out with or without vacuum assistance, belt filters, and the like.
[0136] The resulting heterocoagulated clay dispersions exhibit zeta potentials in the disclosed range centered around zero, providing easily isolable (easily filterable) heteroadducts. While not limiting the zeta potential ranges disclosed and claimed herein and without wishing to be bound by theory, it is possible to obtain excellent yields and filterability of clay heteroadducts when the amount of heterocoagulation reagent combined with colloidal smectite (such as the dioctahedral smectite described herein) provides a particle dispersion with a zeta potential close to zero, such that the particles in the dispersion have little or no electrophoretic mobility. This zero zeta potential point can be considered the nominal target ratio of cationic polymetallate to colloidal clay. Electrophoretic mobility aspects are described, for example, in Gu, et al., Clay and Clay Minerals, 1990, 38(5), 493-500.
[0137] The experimentally derived ratio of heterocoagulant (cationic polymetallate) to colloidal clay can be determined by dispersing the colloidal clay in water, adding the dispersion to a zeta potential measurement vessel, and measuring the initial zeta potential of the clay dispersion. A solution of the selected heterocoagulant is prepared and added in portions to the dispersion, measuring the zeta potential of the dispersion after each addition. The ratio of cationic polymetallate to colloidal clay used to prepare an easily filterable clay heteroadduct is calculated by determining the ratio of heterocoagulant required to achieve a zero or essentially zero zeta potential from the resulting zeta potential titration curve.
[0138] In a further embodiment, when the zeta potential titration curve is not well-defined or has a discontinuity at or near zero potential (mV), extrapolation of the point closest to zero zeta potential can be used to estimate the crossing point where the zeta potential curve crosses from negative to positive zeta potential, thus accounting for the nominal target ratio. In another embodiment, when the zeta potential titration curve is discontinuous near zero and remains discontinuous at or near a zeta potential boundary (e.g., ±20 mV or ±25 mV), linear extrapolation between points on the titration curve immediately before and after the discontinuity can be used to estimate the heterocoagulation reagent-to-clay ratio useful for achieving the desired zeta potential. Examples of zeta probe (zeta potential) titration and determining the nominal target ratio of heterocoagulation reagent to clay are provided in the Figures and Examples sections of this disclosure. See, e.g., Figures 2-8, Examples 8-12, and Example 38.
[0139] The ratio of aluminum (mmol Al) of aluminum chlorohydrate to grams of Volclay® HPM-20 colloidal montmorillonite used to prepare the clay heteroadducts can be significantly lower, sometimes by less than an order of magnitude, than the ratio of mmol Al / g clay used to prepare pillared HPM-20 clay with aluminum chlorohydrate. That is, pillared clays are formed using the same cationic polymetallate and colloidal clay but with a mmol Al / g clay ratio that exceeds the range defined by the zeta potential of about +25 mV to about -25 mV for the clay heteroadduct dispersion. Thus, the ratio of cationic polymetallate to colloidal clay to form the clay heteroadducts of the present disclosure differs from that used, for example, in U.S. Patent Application Publications 2018 / 0142047 and 2018 / 0142048 to W.R. Grace, which use lanthanide-containing -Al pillared clays as support activators.
[0140] Conversely, if the ratio of heterocoagulation reagent to clay in a recipe is too low to produce a clay heteroadduct, the resulting contact product cannot be readily filtered by conventional filtration means. This characteristic is exemplified in Example 19, where a 0.30 mmol Al / g clay recipe for preparing a clay heteroadduct using aluminum chlorhydrate (ACH) and HPM-20 clay predicts a zeta potential of -44 mV as derived from the zeta potential titration in Figure 2. Filtration of the resulting contact product was difficult, and sample isolation and preparation required centrifugation to isolate the product. For convenience, products such as these may be referred to herein as "heteroadducts," even though they are outside the zeta potential range for readily filterability. Similarly, in Example 26, using a 0.30 mmol Al / g clay recipe with powdered ALOXICOLL® 51P aluminum chlorhydrate (Parchem Fine and Specialty Chemicals) resulted in a contact product heteroadduct that was difficult to process and isolate, requiring centrifugation to isolate the product.
[0141] The starting clay particles, such as montmorillonite, are formed by the isomorphous substitution of ions into one of the "TOT" layers, e.g., Al in the octahedral alumina layer, which imparts a negative charge. 3+ Mg 2+ The starting clay carries a permanent negative charge due to the substitution of cations. Thus, the starting clay forms a dispersion or suspension in water as the negatively charged clay particles repel each other and are stabilized in the polar aqueous environment. Without wishing to be bound by theory, it is believed that contact of cations, such as the cationic polymetallates disclosed herein, with the negatively charged colloidal clay initially promotes the coagulation of the colloidal clay through Coulomb attraction of the opposing charges and neutralization of the clay surface. This neutralization causes the clay heteroadducts to precipitate from the polar aqueous carrier as large, easily filterable aggregates or coagulated particles. Because additional cationic polymetallates are added in excess to the coagulation composition, such as when preparing ion-exchanged, protonic acid-treated, or pillared clays, some or all of the aggregated surfaces are "recharged" as positively charged species, thereby allowing them to be resuspended in a polar carrier such as water. This resuspension is difficult to filter, providing a dispersion of highly charged species that clog the filtration medium. It is believed that the clay heteroadducts of the present disclosure form at these high ratios, thereby avoiding repacking and resuspension of the clay heteroadducts. Thus, the near-zero zeta potential surface of the clay heteroadduct provides an easily filterable product and, coincidentally, substantially avoids clay pillaring and the homogeneously intercalated clay structure of the pillared clay and starting clay. Surprisingly, even in the absence of pillars, these structures form thermally stable, strong structures that can serve as highly active support activators for metallocenes.
[0142] In one embodiment, Figure 1 provides a schematic overview of a practical and desirable method for preparing neutral or weakly charged dispersions with low size, near-zero, or zero zeta potential. Filtration of clay heteroadducts with these properties proceeds rapidly, typically requiring multiple successive filtrations to produce supports with the desired surface area, porosity, and polymerization activity. In contrast, highly charged dispersions, such as those obtained from the preparation of pillared clays, are not readily filterable and must be processed using relatively expensive and cumbersome methods to yield useful support activators.
[0143] Also, in contrast to other materials, such as those described by Jensen et al. in U.S. Patent Application Publication Nos. 2018 / 0142047 and 2018 / 0142048, assigned to W.R. Grace, the clay adducts of the present disclosure can exhibit no, or substantially no, d001 peaks below 10 degrees 2θ (2θ) in powder XRD scans after filtering and calcining at 300°C or higher. This feature is illustrated in the examples in Figure 2, which presents powder XRD (X-ray diffraction) patterns for a series of calcined products combining aluminum chlorhydrate (ACH) and Volclay® HPM-20 montmorillonite, each sample differing by the amount of cationic polymetallate used to prepare the hetero-coagulated clay. These samples were prepared according to Examples 18, 20-21, 23, and 25, except as noted below. The sample marked as derived from the 6.4 mmol Al / g clay sample (top) contains 10 mmol Al. 13 This represents a typical preparation of pillared clay (see Example 5). The XRD of the starting clay itself (bottom) is marked as coming from a 0 mmol Al / g clay sample (see Example 3).
[0144] Referring again to Figure 2 and the examples for preparing these samples, Examples 12 through 30 provide preparation methods for forming ACH clay heteroadducts ranging from 0 mmol Al / g clay to 6.4 mmol Al / g clay, including several comparative examples. As the XRD patterns below approximately 10 degrees 2θ shown in Figure 2 demonstrate, there are two main peak changes as the proportion of cationic polymetallate increases in the preparation recipe. First, the XRD peak at approximately 9 degrees 2θ (2θ), corresponding to the starting clay, disappears, and as the proportion of cationic polymetallate increases, the peaks from approximately 9 degrees 2θ to approximately 10 degrees 2θ gradually increase. The disappearance of the 9 degree 2θ peak appears to indicate the progression of the reaction to form a mostly amorphous hetero-coagulated clay, and the subsequent 9-10 degree 2θ peaks indicate the presence of Al. 3+ This likely represents simple ion intercalation and is characterized by a smaller basal spacing than the initial ion-exchanged clay. As more polymetallate is added to the slurry, a peak develops from approximately 4° (2θ) to approximately 6° (2θ), with the TIS peak representing the main product at 6.4 mmol Al / g clay. This 4-6° (2θ) peak likely corresponds to the Keggin ion-interaction pillar structure that forms as the concentration of added polymetallate increases. Because the clay concentrations in these experiments were not highly dilute (i.e., greater than 1 wt.% clay), the 6.4 mmol Al / g clay product could not be easily isolated by simple filtration; instead, it had to be isolated and washed using multiple centrifugation and decanting steps. Additionally, the starting clay colloidal clay, used as a comparative sample, was also not easily filtrable.
[0145] In one embodiment, when aluminum chlorhydrate (ACH) was the heterocoagulation reagent and Volclay® HPM-20 montmorillonite was the colloidal clay, zeta potential data and XRD data showed that a zeta potential range of ±25 mV corresponded to a range of approximately 1 mmol Al / g clay to 1.8 mmol Al / g clay. Similarly, a zeta potential range of ±15 mV, where the clay heteroadducts had more charge, corresponded to a range of approximately 1.3 mmol Al / g clay to 1.7 mmol Al / g clay. These data also showed that a zeta potential of 0 mV, where the clay heteroadducts were close to zero charge, corresponded to approximately 1.5 mmol Al / g clay. Figure 2 shows that at 1.52 mmol Al / g clay, the powder XRD shows little or virtually no pillaring (XRD pattern between 4.8 degrees 2θ and 5.2 degrees 2θ) and little or virtually no simple ion-exchanged clay (XRD pattern between 9 degrees 2θ and 10 degrees 2θ) for mineral impurities present in the starting colloidal clay in the range of 20 to 30 degrees 2θ.
[0146] Without wishing to be bound by theory, it is believed that when using aluminum chlorhydrate and colloidal smectite, the near-zero charge of the heteroadduct provided by the 1.5 mmol Al / g clay recipe is indeed due to the Al 13This corresponds to less than half of the amount (proportion) of aluminum that can be incorporated into pillared smectites and a much smaller portion of the aluminum used in pillar recipes. For example, as described in Schoonheydt et al., Clay and Clay Minerals 1994, 42(5), 518-525, this amount is actually incorporated at about 3-4 mmol Al / g clay. As noted above, the amount of heteroadduct coagulation reagent that results in a zeta potential of 0 mV, which can be considered a preferred amount of about 1.5 mmol Al / g clay, is less than the amount used in the optimized pillar recipe of 15 mmol Al / g clay. The clay heteroadducts of the present disclosure are characterized by the absence or substantial absence of regularly intercalated pillar structures. Furthermore, it has been surprisingly discovered that clay heteroadducts provide comparable and even greater activity as metallocene support activators than pillared clays.
[0147] The clay heteroadducts of the present disclosure are not regularly intercalated pillar structures as described in U.S. Patent Application Publications 2018 / 0142047 and 2018 / 0142048 to Jensen et al. Specifically, the clay heteroadducts of the present disclosure are not microporous catalyst components comprising layered colloidal clays with various pillars intercalated between extended molecular layers of clay, or substantially regularly complex ion intercalations ("non-orderly intercalated"). Thus, the clay heteroadducts of the present disclosure are not regularly arranged and do not have the Al structure as described in U.S. Patent Application Publications 2018 / 0142047 and 2018 / 0142048. 13 Keggin ion or lanthanide-centered polyAl 13There is no evidence of consistent pillaring and / or consistent ordering imparted by layers of intercalated aluminum oxide or hydroxide, as would be expected from pillars. However, in some examples, particularly those that have been multiply washed and filtered, powder XRD peaks indicative of some pillaring can be detected. For example, the XRD pattern of the 1.76 mmol Al / g clay sample corresponds approximately to a zeta potential of +23 mV, but the intensity of the peak is substantially lower than that of a pillared recipe using, for example, 6.4 mmol Al / g clay.
[0148] Thus, in a further aspect, the calcined clay heteroadducts of the present disclosure do not exist in ordered domains, as evidenced by the absence of XRD peaks between 0 and 12 degrees 2θ. This observation highlights one difference between simple monoatomic ion exchange processes, where sodium ions (e.g., in the starting sodium montmorillonite) are exchanged for divalent, trivalent, or polyvalent ions obtained after drying, or complex polyatomic ion exchange processes, where the size or Al of the simple monoatomic ions is not significantly different. 13 This reflects the size of polyatomic ions such as Keggin ions or other columnar species as evidenced by the associated d001 basal spacing in XRD.
[0149] In one embodiment, the isolated clay heteroadducts are collected, for example, by filtration, and are not washed. In another embodiment, the isolated clay heteroadducts are washed minimally with a suitable washing solution, such as water, for example, only enough to provide some purification benefits. Without wishing to be bound by theory, for example, Schoonheydt et al., Clay and Clay Minerals 1994, 42(5), 518-525, which is incorporated herein by reference, has been observed to facilitate pillar washing. Thus, washing to the extent that pillar formation occurs appears to result in the formation of undesirable pillared clay by-products at the expense of the isolated, desirable clay heteroadducts.
[0150] In another aspect of the present disclosure, in further contrast to the regularly intercalated ion-exchanged clays disclosed in U.S. Patent Application Publication Nos. 2018 / 0142047 and 2018 / 0142048 to Jensen et al., extensive washing of the solid clay heteroadducts of the present disclosure until the wash water exhibits a negative AgNO test (chloride test) is not necessary to impart high polymerization activity to the clay heteroadducts. In contrast, a single filtration of an immediate heteroadduct mixture containing approximately 5 wt.% solids without the use of a dilution solution results in good polymerization activity in the final catalyst mixture. This feature is demonstrated, for example, in Examples 22, 24, 29-31, 33, and 35-36. For example, the difference in the preparation of the ACH clay heteroadduct between Example 22 and Example 23 is whether the product was prepared using one filtration or two filtrations, the latter including a single wash between each filtration. Thus, in the preparation of clay heteroadduct Example 22 using a single filtration, the filtrate obtained by filtering the slurry was characterized by a conductivity of 1988 μS / cm. In contrast, clay heteroadduct Example 23 using two filtrations provided a conductivity of 87 μS / cm, and a wash between filtrates characterized by a nearly 23-fold difference. However, the polymerization activity of catalysts prepared using these support activators varied by only 10%, which one skilled in the art would recognize as being within the range of variable bench-scale polymerization testing.
[0151] Similarly, polymerizations using the support activator of Example 24 versus Example 25 further demonstrate the economically beneficial aspects of the support activator, with single filtration versus double filtration of the clay heteroadduct again resulting in essentially the same polymerization activity. Specifically, the catalyst formed from the single-filtered support activator exhibited an activity of 3581 g / g / h compared to 3547 g / g / h observed for the catalyst formed from the double-filtered support activator. The conductivity of the slurry of the single-filtered product (Example 24) was 1500 μS / cm, and the conductivity of the final slurry of the double-filtered product (Example 25) was 180 μS / cm. Thus, it was unexpectedly discovered that extensive washing of the clay heteroadduct was not necessary for good polymerization activity (again, in comparison with U.S. Patent Application Publication Nos. 2018 / 0142047 and 2018 / 0142048).
[0152] Samples made according to Example 28 (additional washing step) and Example 29 (single filtration) using 1.52 mmol Al / g clay provided catalytic activities of 1404 g / g / hr and 1513 g / g / hr, respectively. In this comparison, the single-filtered heteroadduct slurry of Example 29, having a conductivity of 1750 μS / cm, actually provided higher activity than the Example 28 sample, which was washed and filtered twice after the initial filtration and had a slurry conductivity of 169 μS / cm. In another aspect, and in further contrast to the supported activators of U.S. Patent Application Publication Nos. 2018 / 0142047 and 2018 / 0142048, the clay heteroadduct slurry of the present disclosure does not need to be aged at room temperature or elevated temperature for at least 10 days before isolation and use. Rather, the clay heteroadduct slurry of the present disclosure can be immediately filtered and then dried or calcined, thus providing a much more efficient synthesis of supported activators.
[0153] The formation of the heterocoagulant has not been found to be very temperature sensitive, in that clays form heteroadducts with the heterocoagulant over a wide range of temperatures. For example, the formation of clay heteroadducts proceeds in the range of about 20°C to about 30°C, but temperatures ranging from about 0°C to the boiling point of the slurry containing the clay heteroadduct can be used.
[0154] The pH of the solution containing the heterocoagulant can be adjusted to provide a minimum zeta potential for the heterocoagulated product, which can be easily determined experimentally, as described by Goldberg, et al., Clay and Clay Minerals, 1987, 35, 220-270. The resulting heteroadduct isolated by this method can also be used with metallocenes for olefin polymerization. Furthermore, this method for adjusting the zeta potential can be used when the ratio of heterocoagulant to clay does not itself result in a zeta potential between the ±25 mV (or alternatively, ±22 mV, ±20 mV, etc.) range disclosed herein. However, this pH adjustment method requires additional steps in the synthesis and isolation of the clay heteroadduct, and it has been observed that this method does not guarantee filterability or optimal final polymerization activity. Without wishing to be bound by theory, it is believed that pH adjustment in such cases may result in protonated or hydroxylated clay, heterocoagulant, and / or clay heteroadduct, which may affect the properties and ultimate catalytic activity of the clay heteroadduct.
[0155] In another aspect, the present disclosure provides for the removal of salts and small amounts of non-coagulated colloidal material formed during the preparation of the heterocoagulated product. For example, soluble by-products such as sodium chloride, in addition to small amounts of colloidal material, are easily removed from the heterocoagulated product by simply filtering the product after washing with water. Washing can be accomplished by resuspending the isolated heterocoagulated product in water with mechanical stirring or shaking to form a slurry, which can then be refiltered. This method contrasts with pillaring processes, which generally require multiple washing and separation steps using high-speed centrifugation, decantation, pH changes in the pillaring clay solution, or large dilution and settling tanks for the isolation of the pillared clay product. Such additional steps add time and cost to separate and wash the pillared or chemically treated clay mineral adduct from its starting components, impurities such as nano- or micro-sized quartz, and other inorganic metal oxides. Conversely, filtration of the clay heterocoagulation product can be performed in bulk through sintered glass frits, metal frits, common filter paper, felt, or other filtration media, or continuously using a moving belt filter. Filtration is practical because it is fast; for example, filtration can be completed in as little as 1 minute or less, about 5 minutes or less, about 10 minutes or less, about 15 minutes or less, about 30 minutes or less, about 1 hour or less, about 2 hours or less, about 5 hours or less, about 8 hours or less, or about 24 hours or less.
[0156] The conductivity of the clay heteroadduct filtrate or slurry can be monitored using a commercially available conductance meter. In one embodiment, the clay heteroadduct slurry can be characterized by a conductivity in the range of about 100 μS / cm (0.1 mS / cm) to about 50,000 μS / cm (50 mS / cm), about 250 μS / cm to about 25,000 μS / cm, or about 500 μS / cm to about 15,000 μS / cm, alternatively about 1,000 μS / cm (1 mS / cm) to about 10,000 μS / cm (10 mS / cm) when the slurry concentration is in the range of about 1 wt% to about 10 wt% solids, about 2.5 wt% to about 10 wt% solids, or about 5 wt% to about 10 wt% solids.
[0157] The hetero-coagulated solid may optionally be dried by azeotropic methods, as implemented in some examples. Azeotropic drying is believed to preserve pore volume and surface area during drying compared to simply heating the hetero-coagulated solid. For example, filtered smectite hetero-adducts can be resuspended in a slurry with a solvent that lowers the boiling point of the water present in the hetero-coagulated product. This water lost during drying can be characterized as free water or chemically bound water. That is, the water lost during drying can come from free water located in the pores or exterior surfaces of the hetero-adducts and chemically bound water generated from dehydrated surface hydroxyls during the drying and calcination process. Various alcohols are useful as azeotropic agents, including, but not limited to, 1-butanol, 1-hexanol, isopentanol, ethanol, and the like, including any combination thereof.
[0158] Freeze drying, flash drying, fluidized bed drying, or any combination thereof can also be used to remove water from the clay heteroadduct. Whether used alone or in combination during water removal, these methods can help maintain pore volume and surface area during the drying process. In another embodiment, spray drying of a suspension of the clay heteroadduct can be used to control the support activator and supported catalyst particle morphology. For example, a suspension of the clay heteroadduct in an aqueous or organic solvent, or a combination of aqueous and organic solvents, can be spray dried. Dry or wet milling and sieving can be used to refine the morphology, size, and size distribution of the heteroadduct. These methods can be used individually or in combination to achieve the desired support activator particle morphology, particle size, and particle size distribution of the clay heteroadduct. Spray drying and / or sieving of the clay heteroadduct can be used, as can other methods known to those skilled in the art for removing fines or larger particles that may be problematic for transporting or using the heteroadduct as a support activator.
[0159] The hetero-coagulated solid can be calcined or heated in a fluidized bed, for example, at a temperature ranging from about 100°C to about 900°C. For example, the hetero-coagulated smectite clay can be calcined or heated in a fluidized bed at a temperature ranging from about 100°C to about 900°C, from about 200°C to about 800°C, from about 250°C to about 600°C, or from about 300°C to about 500°C. Calcination can be carried out in ambient atmosphere (air), for example, in dry air at a temperature ranging from at least 110°C, for example, from about 200°C to about 800°C, and for a time ranging from about 1 minute to about 100 hours. For example, the smectite heteroadduct can be calcined using any one of the following conditions: a) a temperature ranging from about 110°C to about 600°C for a time ranging from about 1 hour to about 10 hours, b) a temperature ranging from about 150°C to about 500°C for a time ranging from about 1.5 hours to about 8 hours, or c) a temperature ranging from about 200°C to about 450°C for a time ranging from about 2 hours to about 7 hours.
[0160] The clay heteroadduct may also be calcined at a temperature of about 225°C to about 700°C for a time ranging from about 1 hour to about 10 hours, most preferably at a temperature of about 250°C to about 500°C for a time ranging from about 1 hour to about 10 hours. Alternatively, calcination in air can be carried out at a temperature ranging from 200°C to 750°C, 225°C to 700°C, 250°C to 650°C, 225°C to 600°C, 250°C to 500°C, 225°C to 450°C, or 200°C to 400°C. As indicated, any single temperature or calcination temperature selected from a range of two temperatures, e.g., temperatures at least 10°C (i.e., 10°C) apart in the range of 110°C to 800°C, can be used to develop the final catalytic activity.
[0161] Heat treatments such as calcination can be carried out in ambient atmosphere or under other such conditions that facilitate water removal; for example, calcination can be carried out in a carbon monoxide atmosphere. The use of such an atmosphere can more efficiently remove surface hydroxyls at lower temperatures compared to those used in ambient air calcination processes, thus maintaining a greater pore volume and surface area during surface dehydration. After calcination, the hetero-solidified product may be described as a continuous, amorphous combination of clay particles and inorganic oxide particles, which are referred to herein as activator-support or support-activator.
[0162] Determination of the total porosity, pore volume distribution, and surface area of the activator support of the present disclosure can be accomplished by any method known in the art, such as analysis using nitrogen gas adsorption / desorption measurements. Adsorption or desorption isotherms plot the volume of gas (in this case, nitrogen) adsorbed onto or desorbed from the surface of the analyte (clay heteroadduct) as the pressure increases or decreases, respectively, at a constant temperature. Isothermal data can be analyzed using the BJH method to determine total pore volume and generate a pore size distribution, as described below, and isothermal data can be analyzed using the BET method to determine surface area.
[0163] The heteroadduct of smectite clay can provide an activator support with substantial porosity and exhibit catalytic activation properties when combined with metallocenes or other organotransition metal compounds capable of polymerizing olefins. In one embodiment, the calcined clay heteroadduct can exhibit a BJH porosity ranging from about 0.2 cc / g to about 3.0 cc / g, from about 0.3 cc / g to about 2.5 cc / g, or from about 0.5 cc / g to about 1.8 cc / g. The calcined clay heteroadduct can also exhibit a BJH porosity of 0.5 cc / g or greater. Calcined clay heteroadducts having porosities as low as about 0.2 cc / g can be used, e.g., heteroadducts exhibiting BJH porosities ranging from about 0.2 cc / g to about 0.5 cc / g, although clay heteroadducts having porosities less than about 0.2 cc / g can exhibit lower polymerization activity, e.g., <200 g PE / g support activator / hr, when combined with metallocenes such as bis(1-butyl-3-methylcyclopentadienyl)zirconium dichloride to make catalyst systems. In this disclosure, the term "g support activator" refers to grams of calcined clay heteroadduct used to make the catalyst.
[0164] A comparison of the BJH porosity of clay and clay heteroadducts is shown in Figures 10, 11, and 12. The BJH pore volume analysis of the starting montmorillonite, which was calcined but otherwise non-zeotropic and untreated with the heterocoagulant, is shown in Figure 11 (Example 1). The pore volume analysis of the starting montmorillonite, which was sheared, then azeotroped and calcined but otherwise untreated with the heterocoagulant, is shown in Figure 12 (Example 3). Finally, the pore volume analysis of the aluminum chlorhydrate (ACH) heterocoagulated clay (1.76 mmol Al / g clay) from Example 18 is shown in Figure 10. Thus, in the absence of a heterocoagulant, a calcined smectite, such as bentonite, can have a BJH porosity of about 0 cc / g to about 0.2 cc / g.
[0165] The cumulative pore volume between specific pore size boundaries can be determined using the BJH method-derived pore volume distribution. X nm (nanometers) to Y nm (V X-YnmThe cumulative pore volume for a pore size of 0 nm to 10 nm (X nm is the lower pore size limit and Y is the upper pore size limit) is determined by subtracting the total cumulative pore volume for pore sizes of 0 nm to X nm from the total cumulative pore volume for pore sizes of 0 nm to Y nm. In situations where the total cumulative pore volume for either the upper or lower pore size limits is not available, this pore size is estimated by linear interpolation between the two nearest pore size points for which cumulative pore size data is available.
[0166] In one embodiment of the calcined clay heteroadduct, the diameter of the calcined clay heteroadduct is 3 to 10 nm (V 3-10nm , or "small mesopores") is the total or cumulative pore volume of pores between 3 and 30 nm (V 3-30nm In a further embodiment, V 3-10nm is the cumulative pore volume V 3-30nm or alternatively, V 3-10nm is the cumulative pore volume V 3-30nm This feature is exemplified by the data in Figure 10, which shows the BJH pore volume analysis of the smectite heteroadduct of Example 18, where V 3-10nm The value is approximately 0.33(V 3-30nm This pore volume analysis contrasts with the BJH pore volume analysis of both the untreated non-azeotropic clay (Example 1, Figure 11) and the azeotropic clay (Example 3, Figure 12), both of which showed a V 3-10nm is 0.55(V 3-30nm ) is characterized by being larger than
[0167] These pore volume characteristics of the clay heteroadducts of Figure 10 of the present disclosure contrast with the pore volume characteristics of the acid-treated clays of Murase et al., U.S. Pat. No. 9,751,961, which range from 2 nm to 10 nm (V 2~10nm (See Figure 1 and Table 1 in U.S. Pat. No. 9,751,961). Specifically, Murase et al. disclose that smaller mesopores of 2 nm to 10 nm account for the majority of the total mesopore volume (2 nm to 50 nm), and the total mesopore volume is, for example, V 2-10nm +V10-30nm +V 30-50nm In contrast, the clay heteroadducts of the present disclosure have a V 10-30nm Smaller mesopores exceed V alone 3-10nm While not wishing to be bound by theory, it is believed that the increased proportion of larger mesopores relative to the share of total porosity in the present disclosure facilitates the diffusion and accessibility of the metallocene compound to the ionization sites on the clay heteroadduct surface. This is in contrast to smaller mesopores, which may impede or prevent the diffusion of the metallocene to surfaces containing ionization sites, particularly for metallocenes with radii of gyration that exceed the smallest end of the mesopore diameter.
[0168] Furthermore, as shown, for example, by Uchino et al., U.S. Patent No. 6,677,411, the pore size distribution determined by the BJH method can be shown by plotting dV(logD) against pore diameter. The diameter at which this function has its maximum value is referred to as the D M This is considered to be the most frequently occurring pore size, i.e., D M is the diameter corresponding to the highest value of DV (logD) in the pore diameter range of 30 Å to 500 Å. M The ordinal value of is D VM In one embodiment, this logarithmic differential pore volume distribution typically has a local maximum at about 30 Å to about 40 Å (Angstroms). This local maximum intensity is also expressed as a global maximum D VM In one embodiment, D VM The intensity at dV(logD) can be up to about 200% of the intensity of the maximum value of dV(logD) between 200 Å and 500 Å. Alternatively, D VM The intensity at 200 Å to 500 Å can be up to about 120% of the intensity of the maximum value of dV(logD). VMThe intensity at 200 Å to 500 Å can be up to about 100% of the intensity of the maximum dV(logD) between 200 Å and 500 Å. In another aspect, the maximum dV(logD) between 200 Å and 500 Å exceeds all values of dV(logD) between 30 Å and 200 Å. This is in contrast to, for example, the acid-treated clays described in U.S. Patent No. 6,677,411 to Uchino et al., which is incorporated herein by reference, and in which the maximum D observed in the log differential pore size distribution of desired embodiments is 0.01. VM The values are the associated diameters D between 60 Å and 200 Å. M It has.
[0169] Similarly, the treated clay activators described by Casty et al. in U.S. Pat. No. 7,220,695 have a maximum D VM Diameter D M defines a preferred embodiment in which the pore diameter D is between 60 Å and 200 Å (Angstroms). In contrast, the most frequently occurring pore diameter D of the clay heteroadducts of the present disclosure is M is either in the range of 30 Å to 40 Å or in the range of 200 Å to 500 Å.
[0170] Furthermore, the differential logarithmic pore volume distribution in U.S. Pat. No. 6,677,411 exhibits substantially lower intensity in the 200 Å to 500 Å range compared to the 60 Å to 200 Å range. The maximum dV(logD) in the 200 Å to 500 Å range is typically less than 10% of the maximum dV(logD) in the 60 Å to 200 Å range. In contrast, the clay heteroadducts of the present disclosure can provide a maximum dV(logD) in the 200 Å to 500 Å range, which is typically greater than 100% of the maximum dV(logD) in the 60 Å to 200 Å range. Without wishing to be bound by theory, it is believed that the presence of a greater proportion of larger mesopores in the clay heteroadducts of the present disclosure is desirable due to easier metallocene diffusion to the ionization sites of the support activator.
[0171] F. Filterability of smectite heteroadducts Clay heteroadducts prepared in slurry form within the zeta potential range according to the present disclosure have unexpectedly demonstrated improved ease of separation compared to similar pillared clays prepared using the same smectite clay and heterocoagulation reagent. Specifically, the clay heteroadducts, unlike pillared clays, can be readily isolated by filtration. This enhanced filterability has been observed and quantified, for example, by comparing the settling velocity of the clay heteroadduct slurries with the settling velocity of similar pillared clays prepared using the same clay and slurries containing the same amount of clay.
[0172] A comparison of the slurry settling rates of pillared clay and hetero-coagulated clay, each prepared with 5 wt. % HPM-20 clay aqueous dispersion, is shown in Table 1. Each slurry was prepared as described in the referenced examples and added to a graduated cylinder, and settling rate was measured over time by observing the volume of the cloud-free, substantially transparent layer of colloidal particles visible on top of the slurry. In this comparison, the settling rate of the hetero-coagulated clay was significantly faster, e.g., 5 times faster on a volumetric basis. Without wishing to be bound by theory, it is believed that the increased particle size of the hetero-coagulated clay dispersion, which has a zeta potential in a relatively narrow range around 0 mV, e.g., within about ±10 mV, favors coagulation relative to the pillared clay particles, which, in contrast, tend to remain dispersed. [Table 2]
[0173] Thus, one way the filterability of a hetero-coagulated clay slurry can be assessed as "easily filterable" is by examining the settling rate of the slurry compared to the settling rate of a pillared clay slurry. In one aspect, a composition such as a clay hetero-adduct is easily or readily filterable if the settling rate of a 2.5 wt.% aqueous hetero-adduct slurry (as described herein) is 3, 3.5, 4, 4.5, 5, 6, 7, 8, 9, or 10 times or more the settling rate of a 2.5 wt.% aqueous pillared clay slurry prepared using the same colloidal smectite clay, the same hetero-coagulation reagent, and the same liquid carrier, and the settling rates are compared at about 12, 18, 24, 30, 36, 48, 72, 95, 96, or 100 hours or more from the start of the settling test.
[0174] Further evidence of filterability was observed by quantifying the filtration rate, or filtration rate, of the clay slurries, as shown in Table 2. When pillared and hetero-coagulated clay slurries, each containing 5 g of clay, were prepared to a total mass of 250 g and filtered, the hetero-coagulated clay slurry filtered quickly and the filtrate water separated quickly, while the filtration rate of the pillared clay slurry was over 80% slower. Again, without wishing to be bound by theory, it is believed that the increased particle size of the coagulated hetero-coagulated clay allows for easier separation of the hetero-coagulated clay particles from the water, while the smaller particle size of the pillared clay leads to filter paper blockage, slowing separation and requiring replacement of the blocked filter paper, resulting in longer filtration times and continuous filtration. [Table 3]
[0175] Thus, in one aspect, the present disclosure provides another method for quantifying the filterability of a heteroadduct slurry, demonstrating that the slurry is readily filterable and can be readily filtered. In one aspect, a composition such as a clay heteroadduct is characterized in that the slurry exhibits the following filtration behavior: [a] When the 2.0 wt. % aqueous heteroadduct slurry is filtered within a time period of 0 to 2 hours after contacting step b) (i.e., after the initial formation of the heteroadduct slurry), the percentage of filtrate obtained in a 10 minute filtration time using either vacuum filtration or gravity filtration, based on the weight of the liquid carrier in the smectite heteroadduct slurry, is within the range of: (1) about 50 wt. % to about 100 wt. % of the liquid carrier in the slurry of the water weight before filtration, i.e., the initial slurry weight; (2) about 60 wt. % to about 100 wt. % of the liquid carrier in the slurry; (3) about 70 wt. % to about 100 wt. % of the liquid carrier in the slurry; or (4) about 80 wt. % to about 100 wt. % of the liquid carrier in the slurry before filtration; [b] The filtrate from the heteroadduct slurry is readily or easily filterable when it is evaporated to obtain a solid containing less than 20%, less than 15%, or less than 10% of the initial combined weight of clay and heterocoagulant.
[0176] Some non-heteroadduct slurries, including some pillared clay slurry compositions, are characterized for filtration within 0-2 hours after initial formation, as the slurry can be more easily filtered after allowing an initial settling period of several days.
[0177] In the examples used to generate the data in Table 2, the heteroadduct slurry and pillared clay slurry were filtered using a 20-micron filter a few minutes after the contact step between the colloidal clay and the polymetallate. The water from the heteroadduct slurry had essentially filtered by the 10-minute mark after vacuum filtration began, while the water from the pillared clay slurry had not filtered by 10 minutes after vacuum filtration began. By using a combination of the two characteristics listed above to evaluate "easily filterable," it is not necessary to specify either the filter spacing (e.g., 20 μm) or whether filtration was performed by gravity filtration or vacuum filtration. That is, filters with a specified opening size can be easily identified by those skilled in the art; for example, the 20 μm filter used in the examples allows the clay heteroadduct to meet both of these criteria, but neither filter size allows the pillared clay to meet both of these criteria.
[0178] As an example of applying this "easily filterable" test, if a filter with too large openings between filter media is used, such that a pillared clay filter meets the requirements of part [a] of the above criteria, it will fail part [b] and will not be considered readily filterable. When using such a large filter size, the clay heteroadduct will also fail part [b], but by reducing the filter size (e.g., to about 20 μm), the clay heteroadduct can meet both criteria [a] and [b], whereas the pillared clay will fail part [a] when the filter size is reduced. This is because the filter becomes clogged and little or no liquid carrier is filtered.
[0179] Similarly, either gravity filtration or vacuum filtration can be used in the "easily filterable" test, because at a specified time point in the filtrate measurements (10 minutes after filtration begins), an appropriate filter size can be readily identified by a person of appropriate skill that will allow the clay heteroadduct to meet both criteria [a] and [b], while the pillared clay will fail at least one of criteria [a] and [b].
[0180] In another aspect, another method of quantifying filterability is as follows: A composition such as a clay heteroadduct is characterized in that the slurry exhibits the following filtration behavior: [a] filtering a 2.0 wt. % aqueous heteroadduct slurry within a time period of 0 hours to 2 hours after the contacting step b) to provide a first filtrate, the weight ratio of the second filtrate to the first filtrate is less than 0.25, less than 0.20, less than 0.10, less than 0.15, less than 0.10, less than 0.5, or about 0.0, and the second filtrate is obtained from the filtration of a 2.0 wt. % slurry of pillared clay prepared using colloidal smectite clay, a heterocoagulation reagent, and a liquid carrier, and the weight of the first filtrate and the weight of the second filtrate are measured after identical filtration times of 5 minutes, 10 minutes, or 15 minutes; [b] A filtrate from a heteroadduct slurry can be considered readily filterable or easily filtered if it is characterized by: upon evaporation, obtaining a solid containing less than 20%, less than 15%, or less than 10% of the initial combined weight of clay and heterocoagulant.
[0181] Thus, this test compares the filtrate collected from the heteroadduct slurry to the column viscosity, while the previous test compares the filtrate collected from the heteroadduct slurry to the aqueous carrier of the initial slurry.
[0182] G. Metallocene Compounds The calcined clay heteroadducts can be used as substrates or catalyst support activators for one or more suitable polymerization catalyst precursors, such as metallocenes, other organometallic compounds, and / or organoaluminum compounds, or other catalyst components, to prepare olefin polymerization catalyst compositions. Thus, in one aspect, when the clay heteroadducts are prepared as disclosed herein and combined with an organobase metal, such as an alkylaluminum compound, and a Group 4 organotransition metal compound, such as a metallocene, an active olefin polymerization catalyst or catalyst system is provided.
[0183] The support activators of the present disclosure can be used with metallocene compounds (also referred to herein as metallocene catalysts) and cocatalysts such as organoaluminum compounds, and the resulting compositions exhibit catalytic polymerization activity in the absence or substantial absence of ion exchange, proton acid treatment, or pillared clay, or aluminoxane or borate activators. Previously, it was believed that activators such as aluminoxane or borate activators were necessary to achieve polymerization catalytic activity in metallocene or single-site or coordination catalyst systems. However, when desired to provide an activatable alkyl ligand to the metallocene, the combination of a heteroadduct support activator, metallocene, and cocatalyst such as an aluminum alkyl compound provides an active catalyst that would otherwise require other activators, such as aluminoxane or borate activators.
[0184] Metallocene compounds are well understood in the art, and one of ordinary skill in the art will recognize that any metallocene can be used with the support activators described herein, including, for example, both unbridged (non-ansa) metallocene compounds or bridged (ansa) metallocene compounds, or combinations thereof. Thus, one, two, or more metallocene compounds can be used with the clay heteroadduct support activators of the present disclosure.
[0185] In one embodiment, the metallocene can be a metallocene containing a Group 3-6 transition metal, or a metallocene containing a lanthanide metal or a combination of two or more metallocenes. For example, the metallocene can contain a Group 4 transition metal (titanium, zirconium, or hafnium). In a further embodiment, the metallocene compounds each independently have the formula: (X 1 )(X 2 )(X 3 )(X 4 )M(in the formula, a) M is selected from titanium, zirconium, or hafnium; b) X 1 is selected from substituted or unsubstituted cyclopentadienyl, indenyl, fluorenyl, pentadienyl, allyl, boratabenzenyl, 1,2-azaborolyl, or 1,2-diaza-3,5-diborolyl, and any of the substituents is selected from halide, C-C 20 Hydrocarbyl, C1-C 20 Heterohydrocarbyl, C1-C 20 Organoheteryl, fused C4-C 12 a carbocyclic moiety or a fused C-C ring with at least one heteroatom independently selected from nitrogen, oxygen, sulfur, or phosphorus; 11 are independently selected from heterocyclic moieties, c) X 2 is selected from [1] substituted or unsubstituted cyclopentadienyl, indenyl, fluorenyl, pentadienyl, or allyl, and the optional substituents are halide, C1-C 20 Hydrocarbyl, C1-C 20 Heterohydrocarbyl, or C1-C 20 [2] organoheteryls, or selected from halides, hydrides, C1-C 20 Hydrocarbyl, C1-C 20 Heterohydrocarbyl, C1-C 20 Organoheteryl, fused C4-C 12 a carbocyclic moiety or a fused C-C ring with at least one heteroatom independently selected from nitrogen, oxygen, sulfur, or phosphorus; 11 heterocyclic moiety; d) X 1 and X 2 is optionally bridged by at least one linker substituent having 2 to 4 bridging atoms independently selected from C, Si, N, P, or B, and each available non-bridging valence of each bridging atom is unsubstituted (bonded to H) or substituted, and any substituent is selected from halide, C-C 20 Hydrocarbyl, C1-C 20 Heterohydrocarbyl, or C1-C 20 and organoheteryl, and any hydrocarbyl, heterohydrocarbyl, or organoheteryl substituent is independently selected from the group consisting of bridging atoms and X 1 Or X 2 and can form a saturated or unsaturated cyclic structure, e)[1]X 3 and X 4 However, halides, hydrides, C1-C 20 Hydrocarbyl, C1-C 20 Heterohydrocarbyl, or C1-C 20 [2][GX A k X B 4-k ] - wherein G is B or Al, k is a number from 1 to 4, and X A is independently selected from H or a halide, and X in each occurrence B But C1-C 12 Hydrocarbyl, C1-C 12 Heterohydrocarbyl, C1-C 12 and [3]X 3 and X 4 But together with C4-C 20 Polyene or [4]X 3 and X 4 together with M form an unsubstituted or unsubstituted, saturated or unsaturated C3-C6 metallacycle moiety, and any substituents on the metallacycle moiety are selected from the group consisting of halide, C1-C 20 Hydrocarbyl, C1-C 20Heterohydrocarbyl, or C1-C 20 The compound or combination of compounds may comprise, consist of, consist essentially of, or be selected from a compound or combination of compounds having a hydroxyl group, independently selected from organoheteryl.
[0186] According to a further aspect, optionally, X 1 and X 2 teeth, a)>EX 5 2, -EX 5 2EX 5 2-, -EX 5 2EX 5 EX 5 2-, or >C=CX 5 2, wherein E at each occurrence is independently selected from C or Si; b)-BX 5 -, -NX 5 - or -PX 5 ,or c) [-SiX 5 2(1,2-C6H4)SiX 5 2-], [-CX 5 2(1,2-C6H4)CX 5 2-], [-SiX 5 2(1,2-C6H4)CX 5 2-], [-SiX 5 2(1,2-C2H2)SiX 5 2-], [-CX 5 2(1,2-C6H4)CX 5 2-] or [-SiX 5 2(1,2-C6H4)CX 5 2-] where X at each occurrence 5 H, halides, C1-C 20 Hydrocarbyl, C1-C 20 Heterohydrocarbyl, or C1-C 20 independently selected from organoheteryl, Any X selected from hydrocarbyl, heterohydrocarbyl, or organoheteryl substituents 5 If the substituent is a bridging atom, another X 5 Substituent, X1 , or X 2 and (capable of forming a saturated or unsaturated cyclic structure).
[0187] X 1 and X 2 Examples of suitable linker substituents capable of bridging include C1-C 20 Hydrocarbylene group, C1-C 20 Hydrocarbylene group, C1-C 20 Heterohydrocarbyl groups, C1-C 20 Heterohydrocarbylene group, C1-C 20 Heterohydrocarbylene group, or C1-C 20 heterohydrocarbylidene groups. For example, X 1 and X 2 is the expression >EX 5 2, -EX 5 2EX 5 2-, or -BX 5 wherein E is independently C or Si, and X in each occurrence 5 But halides, C1-C 20 Aliphatic group, C6-C 20 Aromatic group, C1-C 20 heteroaliphatic group, C4-C 20 Heteroaromatic groups, or C1-C 20 The alkylene group is bridged by at least one substituent having an alkyl group (independently selected from organoheteryl groups).
[0188] The Aspects of the Disclosure section is: X 1 and X 2 Regarding the connection part with X 5 and with respect to the specific linker substituent or X 5 Additional descriptions and options for the substituents are listed below.
[0189] The aspects section of the present disclosure also includes X 1 and X 2 X, including the above specific substituents 1 and X 2 Additional explanations and options are listed below.
[0190] The aspects section of the present disclosure also includes X 3 and X 4 X, including the above specific substituents 3 and X 4 Additional explanations and options are listed below.
[0191] The embodiments section of this disclosure also provides some specific examples of metallocene compounds useful in combination with the support activators of this disclosure.
[0192] Metallocene compounds are understood by those skilled in the art, and those skilled in the art will recognize and appreciate how to make and use metallocenes in olefin polymerization catalyst systems. Many metallocenes and processes for making metallocenes and organotransition metal compounds are disclosed in U.S. Patent Nos. 4,939,217, 5,210,352, 5,436,305, 5,401,817, 5,631,335, 5,571,880, 5,191,132, 5,480,848, 5,399,636, 5,565,592, 5,347,026, 5,594,078, 5,498,581, and 5,496,781. Nos. 5,563,284, 5,554,795, 5,420,320, 5,451,649, 5,541,272, 5,705,478, 5,631,203, 5,654,454, 5,705,579, 5,668,230, 9,045,504, and 9,163,100, and 2017 / 0342175, which are incorporated herein by reference in their entireties.
[0193] H.Cocatalyst According to one aspect, the present disclosure provides a catalyst composition for olefin polymerization, the catalyst composition comprising: a) at least one metallocene compound; b) optionally, at least one cocatalyst; and c) at least one support activator as described herein. Cocatalysts include compounds such as trialkylaluminum, which are believed to provide a ligand to the metallocene that can initiate polymerization when the metallocene is otherwise activated with the support activator. The cocatalyst may be considered optional, for example, in scenarios where the metallocene may already contain a polymerization-activating / initiating ligand (such as methyl or hydride). It will be understood that even when the metallocene compound contains a polymerization-activating / initiating ligand, the cocatalyst can be used for other purposes, such as removing water from the polymerization reactor or process. Thus, the cocatalyst can include or be selected from, for example, an alkylating agent, a hydridinating agent, or a silylating agent. The metallocene compound, the support activator, and the cocatalyst can be contacted in any order.
[0194] The co-catalyst can include or be selected from organoaluminum compounds, organoboron compounds, organozinc compounds, organomagnesium compounds, organolithium compounds, or any combination thereof.
[0195] The Aspects section of this disclosure lists additional descriptions and options for each of the organoaluminum compounds, organoboron compounds, organozinc compounds, organomagnesium compounds, and organolithium compounds.
[0196] In one embodiment, for example, the cocatalyst is a compound of the formula Al(X A ) n (X B ) m , M x [AlX A 4], Al(X C ) n (X D ) 3-n , M x [AlX C4] (i.e., it may be a neutral molecular compound or an ionic compound / salt of aluminum), where each of the variables in these formulas is defined in the Aspects section of this disclosure. For example, the cocatalyst may comprise, consist essentially of, or be selected from any combination of trimethylaluminum, triethylaluminum (TEA), tripropylaluminum, tributylaluminum, trihexylaluminum, trioctylaluminum, ethyl-(3-alkylcyclopentadiyl)aluminum, diethylaluminum ethoxide, diisobutylaluminum hydride, triisobutylaluminum (TIBAL), diethylaluminum chloride, ethyl-(3-alkylcyclopentadiyl)aluminum, and the like.
[0197] In another embodiment, for example, the cocatalyst is a compound of formula B(X E ) q (X F ) 3-q or M y [BX E4] (i.e., it may be a neutral molecular compound or an ionic compound / salt of boron), where each of the variables in these formulas is defined in the Aspects section of this disclosure. For example, the cocatalyst may comprise, consist essentially of, or be selected from trimethylboron, triethylboron, tripropylboron, tributylboron, trihexylboron, trioctylboron, diethylboron ethoxide, diisobutylboron hydride, triisobutylboron, diethylboron chloride, di-3-pinanylborane, pinacolborane, catecholborane, lithium borohydride, lithium triethylborohydride, etc., Lewis base adducts thereof, or combinations or mixtures thereof. In another embodiment, the co-catalyst can include or be a halogenated organoboron compound, such as a fluorinated organoboron compound, examples of which include tris(pentafluorophenyl)boron, tris[3,5-bis(trifluoromethyl)phenyl]boron, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, triphenylcarbenium tetrakis(pentafluorophenyl)borate, lithium tetrakis-(pentafluorophenyl)borate, N,N-dimethylanilinium tetrakis[3,5-bis(trifluoro-methyl)phenyl]borate, triphenylcarbenium tetrakis[3,5-bis(trifluoromethyl)-phenyl]borate, and any combination or mixture thereof.
[0198] In yet another embodiment, for example, the cocatalyst is of formula M C (X G ) r (X H ) 2-rwherein each variable in this formula is defined in the Aspects section of this disclosure. For example, the cocatalyst can comprise, consist essentially of, or be selected from any combination of dimethylzinc, diethylzinc, diisopropylzinc, dicyclohexylzinc, diphenylzinc, butylethylmagnesium, dibutylmagnesium, n-butyl-sec-butylmagnesium, dicyclopentadienylmagnesium, ethylmagnesium chloride, butylmagnesium chloride, and the like.
[0199] In yet another embodiment, for example, the cocatalyst is a compound of the formula Li(X J ), where each variable in this formula is defined in the Aspects section of this disclosure. For example, the co-catalyst can comprise, consist essentially of, or be selected from methyllithium, ethyllithium, propyllithium, butyllithium (including n-butyllithium and t-butyllithium), hexyllithium, isobutyllithium, and the like, or any combination thereof.
[0200] I. Optional Co-activators In one aspect, if desired, other activators in addition to the calcined smectite heteroadduct activator support can be used in the catalyst compositions of the present disclosure. These are referred to as co-activators, and examples of optional co-activators include, but are not limited to, ion-exchanged clays, protonated acid-treated clays, pillared clays, aluminoxanes, borate activators, aluminate activators, ionizing ionic compounds, solid oxides treated with electron-withdrawing anions, or any combination thereof.
[0201] The Aspects section of this disclosure lists additional descriptions and options for each of these optional co-activators.
[0202] Aluminoxanes. Aluminoxanes (also referred to as poly(hydrocarbyl aluminum oxides) or organoaluminoxanes) can be used, for example, to contact other catalyst components in any solvent that is substantially inert to the reactants, intermediates, and products of the activation step, such as a saturated hydrocarbon solvent or toluene. The catalyst composition thus formed may be isolated, if desired, or the catalyst composition may be introduced into a polymerization reactor without isolation.
[0203] As will be appreciated by those skilled in the art, aluminoxanes are oligomers, and aluminoxane compounds can include linear, cyclic, or cage structures, or mixtures thereof. For example, aluminoxanes of the formula (R-Al-O) n wherein R can be a linear or branched alkyl having from 1 to about 12 carbon atoms, and n can be an integer from 3 to about 12. (AlRO) n The moiety also constitutes a repeating unit in linear aluminoxanes, e.g., of the formula: R(R-Al-O) n The organoaluminoxanes have the formula AlR2, where R can be a linear or branched alkyl having from 1 to about 12 carbon atoms, and n can be an integer from 1 to about 75. For example, the R group can be a linear or branched C1-C8 alkyl, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, or octyl, and n can represent an integer from 1 to about 50. Depending on how the organoaluminoxane is prepared, stored, and used, the value of n can be variable within a single sample of the aluminoxane, and a combination or population of such organoaluminoxane species will typically be present in any given sample.
[0204] Organoaluminoxanes can be prepared by various procedures known in the art; for example, organoaluminoxane preparations are disclosed in U.S. Patent Nos. 3,242,099 and 4,808,561, each of which is incorporated herein by reference in its entirety. In one embodiment, aluminoxanes can be prepared by reacting water present in an inert organic solvent with an aluminum alkyl compound, such as AlR3, to form the desired organoaluminoxane compound. Alternatively, organoaluminoxanes can be prepared by reacting an aluminum alkyl compound, such as AlR3, with a hydrated salt, such as hydrated copper sulfate, in an inert organic solvent.
[0205] In one embodiment, the aluminoxane compound can be methylaluminoxane, ethylaluminoxane, n-propylaluminoxane, isopropylaluminoxane, n-butylaluminoxane, t-butylaluminoxane, sec-butylaluminoxane, isobutylaluminoxane, 1-pentylaluminoxane, 2-pentylaluminoxane, 3-pentylaluminoxane, isopentylaluminoxane, neopentylaluminoxane, or a combination thereof. In one aspect, methylaluminoxane (MAO), ethylaluminoxane (EAO), or isobutylaluminoxane (IBAO) can be used as an optional cocatalyst, and these aluminoxanes can be prepared from trimethylaluminum, triethylaluminum, or triisobutylaluminum, respectively. These compounds can be complex compositions and are sometimes referred to as poly(methylaluminum oxide), poly(ethylaluminum oxide), and poly(isobutylaluminum oxide), respectively. In another embodiment, the aluminoxanes can be used in combination with trialkylaluminums such as those disclosed in US Pat. No. 4,794,096, which is incorporated herein by reference in its entirety.
[0206] In preparing catalyst compositions containing an optional aluminoxane, the molar ratio of aluminum present in the aluminoxane to the metallocene compound in the composition can be lower than the typical molar ratio used in the absence of the support activator of the present disclosure. In the absence of the support activator of the present disclosure, the amount of aluminoxane can be, for example, from about 1:10 mol Al / mol metallocene (mol Al / mol metallocene) to about 100,000:1 mol Al / mol metallocene, or from about 5:1 mol Al / mol metallocene to about 15,000:1 mol Al / mol metallocene. When used in conjunction with the disclosed support activators, the relative amount of aluminoxane can be reduced. For example, the amount of any aluminoxane added to the polymerization zone can be less than previously typical amounts in the range of about 0.01 mg / L to about 1000 mg / L, about 0.1 mg / L to about 100 mg / L, or about 1 mg / L to about 50 mg / L. Alternatively, the aluminoxane can be used in amounts commonly used in the prior art, but with the additional use of a support activator of the present disclosure to obtain the added benefits of such a combination.
[0207] Organoboron Compound. The catalyst composition of the present disclosure can also optionally include an optional organoboron co-activator in addition to the listed components (support activator, metallocene, and optional cocatalyst). In one aspect, the organoboron compound can include or be selected from a neutral boron compound, a borate salt, or a combination thereof. For example, the organoboron compound can include or be selected from a fluoroorganoboron compound, a fluoroorganoborate compound, or a combination thereof, and any such fluorinated compound known in the art can be utilized.
[0208] Thus, the term fluorocarbon boron compounds is used herein to refer to neutral compounds of the form BY3, and the term fluorocarbon borate compounds is used herein to refer to neutral compounds of the form [cationic] +[BY4]- is used herein to refer to monoanionic salts of fluoroorganoboron compounds, where Y represents a fluorinated organic group. For convenience, fluoroorganoboron compounds and fluoroorganoborate compounds are typically referred to collectively by the organoboron compound, or by either name as the context requires.
[0209] In one embodiment, examples of fluoroborate compounds that can be used as co-activators include, but are not limited to, tris(pentafluorophenyl)borane, tris[3,5-bis(trifluoromethyl)phenyl]borane, and the like (including mixtures thereof). Examples of fluoroborate compounds that can be used as optional co-activators include, but are not limited to, fluorinated arylborates, such as N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, triphenylcarbenium tetrakis(pentafluorophenyl)borate, lithium tetrakis(pentafluorophenyl)borate, N,N-dimethylanilinium tetrakis[3,5-bis(trifluoromethyl)phenyl]borate, triphenylcarbenium tetrakis[3,5-bis(trifluoromethyl)phenyl]borate, and the like, including mixtures thereof.
[0210] The Aspects section of this disclosure lists additional descriptions and options for optional fluoroorganoboron and fluoroorganoborate compound co-activators.
[0211] Without intending to be bound by theory, it is believed that these fluoroorganoborates and fluoroorganoboron compounds form weakly coordinating anions when combined with metallocene compounds, as disclosed in U.S. Pat. No. 5,919,983, the entirety of which is incorporated herein by reference.
[0212] Generally, any amount of organoboron compound can be utilized as an optional co-activator. For example, in one embodiment, the molar ratio of organoboron compound to metallocene compound in the composition can range from about 0.1:1 moles of organoboron compound or organoborate compound per mole of metallocene (mol / mol) to about 10:1 mole / mol, or from about 0.5 mol / mol to about 10 mol / mol (moles of organoboron compound or organoborate compound per mole of metallocene), or alternatively, from about 0.8 mol / mol to about 5 mol / mol (moles of organoboron compound or organoborate compound per mole of metallocene). However, it should be understood that the amount can be reduced or adjusted downward in the presence of a clay heteroadduct support activator.
[0213] Ionizing compounds. In a further embodiment, any co-activator that may be used in addition to the listed components of the catalyst composition of the present disclosure may include or be selected from ionizing compounds. Examples of ionizing compounds are disclosed in U.S. Patent Nos. 5,576,259 and 5,807,938, each of which is incorporated herein by reference in its entirety.
[0214] The Aspects section of this disclosure lists additional descriptions and options for optional ionizing compound co-activators.
[0215] The term "ionizing compound" is a term used in the art and refers to a compound, particularly an ionic compound, that can enhance the activity of the catalyst composition. In one aspect, the fluoroorganoborate compounds described herein as any organic boron coactivator can also be considered and function as an ionizing compound coactivator. However, since compounds such as fluoroorganoaluminates are included in the ionizing compound, the scope of the ionizing compound is broader than that of the fluoroorganoborate compounds.
[0216] While not intending to be bound by theory, it is believed that the ionizing compound can interact or react with the metallocene compound, converting the metallocene to a cationic or initial cationic metallocene compound, activating the metallocene for polymerization activity. Again, without intending to be bound by theory, the ionizing compound can interact or react with the metallocene, particularly the metallocenes of formula (X 1 )(X 2 )(X 3 )(X 4 )M or (X 3 ) or (X 4 It is believed that an ionizing compound may function by fully or partially abstracting an anionic ligand from a non-alkadienyl ligand, such as X, to form a cationic or initial cationic metallocene. However, the ionizing compound can function as an activator (co-activator) regardless of the mechanism by which it functions. For example, the ionizing compound may ionize the metallocene and react with X in such a way as to form an ion pair. 3 or X 4 Extracting the Ligand and Metal-X 3 or Metal-X 4 Weaken the bond, or simply X 3 or X 4 It may be coordinated to a ligand or any other mechanism by which activation can occur. Furthermore, it is not necessary for the ionizing compound to activate (co-activate) only the metallocene, as the activating function of the ionizing compound is evident in the improved activity of the overall catalyst composition compared to a catalyst composition containing any ionizing compound that does not contain the optional ionizing compound.
[0217] Examples of ionizing compounds include, but are not limited to, the list of compounds provided in the Aspects section of this disclosure.
[0218] Optional Support Activators. In a further aspect, optional co-activators that may be used in addition to the listed components of the catalyst compositions of the present disclosure may include or be selected from other support activators, sometimes referred to as activator supports. These are referred to as co-activator supports when used in the catalyst compositions described herein. Examples of optional co-activator supports are disclosed in U.S. Patent Nos. 6,107,230, 6,653,416, 6,992,032, 6,984,603, 6,833,338, and 9,670,296, each of which is incorporated herein by reference in its entirety.
[0219] For example, the optional coactivator support can include or be selected from silica, alumina, silica-alumina, or silica-coated alumina treated with at least one electron-withdrawing anion. For example, the silica-coated alumina, in this embodiment, can have an alumina-to-silica weight ratio ranging from about 1:1 to about 100:1, or from about 2:1 to about 20:1. The at least one electron-withdrawing anion can include or be selected from fluoride, chloride, bromide, phosphate, triflate, bisulfate, sulfate, or the like, or combinations thereof.
[0220] In one aspect, the optional co-activator support can be selected from, for example, fluorinated alumina, chlorinated alumina, brominated alumina, sulfated alumina, fluorinated silica-alumina, chlorinated silica-alumina, brominated silica-alumina, sulfated silica-alumina, fluorinated silica-zirconia, chlorinated silica-zirconia, brominated silica-zirconia, sulfated silica-zirconia, fluorinated silica-titania, and the like, any or any combination of which can be used in the catalyst compositions disclosed herein. Alternatively, or additionally, the co-activator support can comprise or be selected from solid oxides treated with electron-withdrawing anions, such as fluorinated silica-alumina, or sulfated alumina.
[0221] Examples of co-activator supports can include, but are not limited to, those listed in the Aspects section of this disclosure.
[0222] J. Preparation of the Catalyst Composition In the catalyst system, 1 )(X 2 )(X 3 )(X 4 The relative concentration or ratio of metallocenes, such as Group 4 metallocenes with M, to calcined clay heteroadduct can be expressed as moles of M (metal) per gram of calcined clay heteroadduct (mol M / g heteroadduct). In one embodiment, it has been found that the molar ratio of M per gram of calcined clay heteroadduct can range from about 0.025 mol M / g heteroadduct to about 0.000000005 mol M / g heteroadduct. In another embodiment, moles of M per gram of calcined clay heteroadduct can range from about 0.0005 mol M / g heteroadduct to about 0.00000005 mol M / g heteroadduct, or alternatively, from about 0.0001 mol M / g heteroadduct to 0.000001 mol M / g heteroadduct. As with all ranges disclosed herein, these recited ranges include the endpoints, as well as intermediate values and subranges within the recited ranges. These ratios reflect the catalyst recipe, ie, they are based on the amounts of components combined to obtain the catalyst composition, regardless of what the ratios are in the final catalyst.
[0223] In a catalyst system, the relative concentration or ratio of cocatalyst to calcined clay heteroadduct can be expressed as moles of cocatalyst (e.g., organoaluminum compound) per gram of calcined clay heteroadduct (mol cocatalyst / g heteroadduct). In one embodiment, it has been found that the ratio of moles of cocatalyst, such as organoaluminum compound, per gram of calcined clay heteroadduct can range from about 0.5 mol cocatalyst / g heteroadduct to about 0.000005 mol cocatalyst / g heteroadduct. In another embodiment, the molar ratio of cocatalyst per gram of calcined clay heteroadduct can be used in the range of about 0.1 mol cocatalyst / g heteroadduct to about 0.00001 mol cocatalyst / g heteroadduct, or alternatively, in the range of about 0.01 mol cocatalyst / g heteroadduct to about 0.0001 mol cocatalyst / g heteroadduct.
[0224] The catalyst composition can be prepared by contacting a transition metal compound, such as a metallocene, a calcined clay heteroadduct, and a cocatalyst, such as an organoaluminum compound, under suitable conditions. Contacting can occur in any number of ways, such as blending, contacting in a carrier liquid, feeding each component separately, or feeding the components to the reactor in any order or combination. For example, various combinations of components or compounds can be contacted with each other before further contacting with the remaining compounds or components in the reactor. Alternatively, all three components or compounds can be contacted together before being introduced into the reactor. With regard to additional optional components that may be used in the catalyst systems disclosed herein, such as co-activators, ionizing ionic compounds, etc., the contacting step with these optional components can occur in any way and in any order.
[0225] In one embodiment, the catalyst composition can be prepared by first contacting a transition metal compound, such as a metallocene, with a cocatalyst, such as an organoaluminum compound, for a time period from about 1 minute to about 24 hours, or alternatively from about 1 minute to about 1 hour, at a contact temperature ranging from about 10° C. to about 200° C., alternatively from about 12° C. to about 100° C., alternatively from about 15° C. to about 80° C., or alternatively from about 20° C. to about 80° C., to form a first mixture, which can then be contacted with the calcined clay heteroadduct to form the catalyst composition.
[0226] In another embodiment, the metallocene, cocatalyst, such as an organoaluminum compound, and calcined clay heteroadduct can be pre-contacted before being introduced into the reactor. For example, the pre-contacting step can occur for a period of from about 1 minute to about 6 months. In one embodiment, for example, the pre-contacting step can occur at a temperature of from about 10° C. to about 200° C., or from about 20° C. to about 80° C., for a period of from about 1 minute to about 1 week to provide an active catalyst composition. Additionally, any subset of the final catalyst components can be pre-contacted in one or more pre-contacting steps, each with its own pre-contacting period.
[0227] After pre-contacting any or all of the catalyst system components, the catalyst composition can be said to contain the contacted components. For example, the catalyst composition can contain a contacted metallocene, a contacted cocatalyst such as an organoaluminum compound, and a contacted calcined clay heteroadduct component. In the field of catalyst technology, it is not uncommon for the specific and detailed nature of the active catalyst site, as well as the specific nature and fate of each component used to create the active catalyst, to be unknown. While not intending to be bound by theory, a majority of the weight of the catalyst composition, based on the relative weights of the individual components, can be considered to contain the contacted calcined clay heteroadduct. Because the nature of the active site and the contacted components is not precisely known, the catalyst composition can be simply described according to its components or referred to as containing the contacted compound or component.
[0228] The polymerization activity of the catalyst composition can be expressed as the weight of polymer per weight of support-activator containing the calcined smectite heteroadduct per unit time, e.g., grams polymer / gram (calcined) support-activator / hour (g / g / hr). That is, activity can be calculated based on the support-activator alone, in the absence of any metallocene or cocatalyst components. This measurement allows for comparison of various activator-supports, including those with other activators, where the metallocene, cocatalyst, and other conditions are the same or substantially the same. Unless otherwise specified, activity values disclosed in the examples were measured under slurry polymerization conditions, using isobutane as the diluent, at polymerization temperatures of about 50°C to about 150°C (e.g., at a temperature of 90°C), and a combined ethylene and isobutane pressure ranging from about 300 psi to about 800 psi, e.g., 450 psi for the combined total of ethylene and isobutane. Activity data is reported as the weight of polymer produced divided by the weight of the calcined clay heteroadduct per hour.
[0229] The catalytic activity can be a function of the metallocene and the calcined clay heteroadduct, as well as other ingredients and conditions. Under the conditions described above, the activity based on the weight of the calcined clay heteroadduct can be greater than about 1,000 grams per hour per gram of calcined clay heteroadduct (g PE / g heteroadduct / hr, or simply g / g / hr). In another embodiment, the activity based on the weight of the calcined clay heteroadduct can be greater than about 2,000 g / g / hr, greater than about 4,000 g / g / hr, greater than about 6,000 g / g / hr, greater than about 8,000 g / g / hr, greater than about 10,000 g / g / hr, greater than about 15,000 g / g / hr, greater than about 25,000 g / g / hr, or greater than about 50,000 g / g / hr. The upper limit for each of these activities can be about 70,000 g / g / hr, so that activities can range above these disclosed values and below about 75,000 g / g / hr.
[0230] For example, in one embodiment, using the conditions described herein, the activator support may be oxidized at a rate of about 500 g / g / hr, about 750 g / g / hr, about 1,000 g / g / hr, about 1,250 g / g / hr, about 1,500 g / g / hr, about 1,750 g / g / hr, about 2,000 g / g / hr, about 2,500 g / g / hr, about 3,500 g / g / hr, about 5,000 g / g / hr, about 7,500 g / g / hr, about 10,000 g / g / hr, about The polymerization activation activity may be about 12,500 g / g / hr, about 15,000 g / g / hr, about 17,500 g / g / hr, about 20,000 g / g / hr, about 25,000 g / g / hr, about 30,000 g / g / hr, about 35,000 g / hr, about 40,000 g / hr, about 50,000 g / g / hr, about 60,000 g / hr, about 70,000 g / hr, or about 75,000 g / hr, including any range therebetween. Higher values of polymerization activity may be associated with clay supports having extremely high site densities, and these activity values may also depend on the metallocene. Thus, by applying the teachings herein, activity levels within a range between two of the recited values can be achieved; for example, activity levels within the range of 500 to 75,000 g / g / hr, as well as within the ranges of 1,000 to 50,000 g / g / hr, 2,000 to 40,000 g / g / hr, or 2,500 to 20,000 g / g / hr can be obtained. The activities in the examples and data tables were measured under slurry homopolymerization conditions using isobutane as the diluent, a polymerization temperature of 90°C, a combined ethylene and isobutane pressure of 450 psi, and (1-n-butyl-3-methylcyclopentadienyl)ZrCl and triethylaluminum catalyst compositions.
[0231] In one embodiment, no aluminoxane, such as methylaluminoxane, was required to activate the metallocene and form the catalyst composition. Methylaluminoxane (MAO) is an expensive activator compound that can significantly increase polymer production costs. Furthermore, in another embodiment, no organoboron compounds, such as borate compounds, or ionizing compounds were required to activate the metallocene and form the catalyst composition. Furthermore, ion-exchange, proton acid treatment, or pillared clay, which also require multi-step preparations that increase costs, were also not required to activate the metallocene and form the catalyst composition. Thus, the active heterogeneous catalyst composition can be easily and inexpensively produced and used to polymerize olefin monomers, including comonomers, if desired, in the absence of any aluminoxane compounds, boron compounds, borate compounds, ion-exchanged, proton acid-treated, or pillared clays. MAO or other aluminoxanes, boron or borate compounds, ion-exchanged clays, protonated clays, or pillared clays are not required in the disclosed catalyst systems, although these compounds may be used in reduced or typical amounts in accordance with other aspects of the present disclosure.
[0232] K. Polyolefins and Polymerization Processes In one aspect, the present disclosure describes a process for producing at least one polymer (polyolefin) by contacting at least one olefin monomer with the disclosed catalyst composition. The term "polymer" is used herein to include polymers of more than two olefin monomers, such as homopolymers, copolymers of two olefin monomers, and terpolymers. For convenience, polymers of two or more olefin monomers are simply referred to as copolymers. Thus, the catalyst composition can be used to polymerize at least one monomer to produce a homopolymer or a copolymer.
[0233] In one embodiment, the homopolymers are composed of monomer residues having from 2 to about 20 carbon atoms per molecule, preferably from 2 to about 10 carbon atoms per molecule. The olefin monomers can include or be selected from ethylene, propylene, 1-butene, 3-methyl-1-butene, 1-pentene, 3-methyl-1-pentene, 4-methyl-1-pentene, 1-hexene, 3-ethyl-1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, and mixtures thereof. In one embodiment, homopolymers of ethylene, homopolymers of propylene, and homopolymers of other olefins are encompassed by the present disclosure. In another embodiment, copolymers of ethylene and at least one comonomer, and copolymers of two less common non-ethylene copolymers are encompassed by the present disclosure.
[0234] When copolymers are desired, each monomer may have from about 2 to about 20 carbon atoms per molecule. Comonomers for ethylene may include, but are not limited to, aliphatic 1-olefins having 3 to 20 carbon atoms per molecule, such as propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-octene, styrene, vinylcyclohexane, and other olefins, as well as conjugated or non-conjugated diolefins such as 1,3-butadiene, isoprene, piperylene, 2,3-dimethyl-1,3-butadiene, 1,4-pentadiene, 1,7-hexadiene, and other such diolefins and mixtures thereof. In a further embodiment, ethylene may be copolymerized with at least one comonomer comprising or selected from 1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, or 1-decene. An amount of comonomer can be introduced into the reactor zone sufficient to produce a copolymer that incorporates from about 0.01% to about 10% by weight of comonomer, or can exceed this range, based on the total weight of monomer and comonomer in the copolymer; alternatively, from about 0.01% to about 5% by weight of comonomer can be introduced; alternatively, from about 0.1% to about 4% by weight of comonomer can be introduced; or alternatively, any amount of comonomer can be introduced into the reactor zone that provides the desired copolymer.
[0235] Typically, the catalyst composition can be used to homopolymerize ethylene or propylene, or to copolymerize ethylene with a comonomer, or to copolymerize ethylene and propylene. In another aspect, several comonomers may be polymerized with the monomer in the same or different reactor zones to achieve desired polymer properties.
[0236] Other useful comonomers include polar vinyl, conjugated and non-conjugated dienes, acetylene and aldehyde monomers, which may be included in minor amounts in the terpolymer composition, for example. For example, non-conjugated dienes useful as comonomers may be linear, hydrocarbon diolefins, or cycloalkenyl-substituted alkenes having 6 to 15 carbon atoms. Suitable unconjugated dienes include, for example, (a) straight-chain acyclic dienes such as 1,4-hexadiene and 1,6-octadiene; (b) branched-chain acyclic dienes such as 5-methyl-1,4-hexadiene, 3,7-dimethyl-1,6-octadiene, and 3,7-dimethyl-1,7-octadiene; (c) monocyclic alicyclic dienes such as 1,4-cyclohexadiene, 1,5-cyclooctadiene, and 1,7-cyclododecadiene; (d) tetrahydroindene, norbornadiene, methyl-tetrahydroindene, dicyclopentene (DCPD), bicyclo-(2.2.1)-hepta-2,5-diene, alkenyl, alkyl, polycyclic alicyclic fused and bridged cyclic dienes such as cyclohexene, cycloaliphatic fused and bridged cyclic dienes such as cyclohexene, cycloalkenyl and cycloalkylidene norbornenes such as 5-methylene-2-norbornene (MNB), 5-propenyl-2-norbornene, 5-isopropylidene-2-norbornene, 5-(4-cyclopentenyl)-2-norbornene, 5-cyclohexylidene-2-norbornene, and 5-vinyl-2-norbornene (VNB); and (e) cycloalkenyl-substituted alkenes such as vinylcyclohexene, allylcyclohexene, vinylcyclooctene, 4-vinylcyclohexene, allylcyclodecene, and vinylcyclododecene. Particularly useful non-conjugated dienes include dicyclopentadiene, 1,4-hexadiene, 5-methylene-2-norbornene, 5-ethylidene-2-norbornene, and tetracyclo-(.Δ.-11,12)-5,8-dodecene. Particularly useful diolefins include 5-ethylidene-2-norbornene (ENB), 1,4-hexadiene, dicyclopentadiene (DCPD), norbornadiene, and 5-vinyl-2-norbornene (VNB). It should be noted that throughout this description, the terms "non-conjugated diene" and "diene" are used interchangeably.
[0237] The catalyst compositions can be used to polymerize olefins to produce oligomeric and polymeric materials for use in a wide range of densities, for example, from about 0.66 g / mL (also, g / cc) to about 0.96 g / mL, for use in numerous applications. The catalyst compositions disclosed herein are particularly useful for producing copolymers. For example, copolymer resins can have densities of 0.960 g / cc or less, preferably 0.952 g / cc or less, and more preferably 0.940 g / cc or less. According to certain embodiments of the present disclosure, densities below 0.91 g / cc are achievable, and as low as 0.860 g / cc. When densities are described as being less than a particular density, one lower limit for such densities can be about 0.860 g / cc. The copolymer resins can contain at least about 65 weight percent (wt%) ethylene units, i.e., the weight percent of ethylene monomer actually incorporated into the copolymer resin. In another aspect, the copolymer resins of the present disclosure can contain at least about 0.5 wt. % α-olefin (α-olefin), e.g., 0.5 wt. % to 35 wt. % α-olefin, referring to the weight % of α-olefin comonomer actually incorporated into the copolymer resin.
[0238] The catalyst compositions prepared according to the present disclosure are also useful for preparing: (a) ethylene / propylene copolymers, including "random copolymers" in which the comonomers are randomly distributed along the polymer backbone or chain; (b) "propylene random copolymers," random copolymers of propylene and ethylene, containing about 60% by weight of the polymer derived from propylene units; and (c) "impact copolymers," meaning two or more polymers in which one polymer is dispersed in other polymers, typically one polymer comprising a matrix phase and the other comprising an elastomeric phase. The catalyst compositions described herein can also be used to prepare polyalphaolefins having monomers containing more than three carbons. Such oligomers and polymers are particularly useful, for example, as lubricants.
[0239] Any number of polymerization methods or processes can be used with the catalyst compositions of the present disclosure. For example, slurry polymerization, gas-phase polymerization, and solution polymerization, including multiple reactor combinations, can be used. The multiple reactor combinations can be configured in series or parallel configurations, or combinations thereof, depending on the desired polymerization sequence. Examples of reactor systems and combinations include, for example, dual slurry loops in series, multiple slurry tanks in series, or a slurry loop combined with a gas phase, or a combination of multiple of these processes in which ethylene, propylene, and α-olefin polymerizations can be carried out separately or together. In another aspect, the gas-phase reactor can include a fluidized bed reactor or a tubular reactor, the slurry reactor can include a vertical loop or a horizontal loop or a stirred tank, and the solution reactor can include a stirred tank or an autoclave reactor. Thus, any polymerization zone known in the art capable of producing polyolefins, such as polyethylene, polypropylene, ethylene and α-olefin-containing polymers, including ethylene α-olefin copolymers, and more generally substituted olefins, such as vinylcyclohexane, can be utilized. In one aspect, for example, a stirred reactor can be utilized for a batch process, and the reaction can then be carried out continuously in a loop reactor, or in a continuous stirred reactor, or in a gas phase reactor.
[0240] The catalyst composition containing the listed components can polymerize olefins in the presence of a diluent or liquid carrier, and these two terms are used interchangeably herein, even if the catalyst components are not soluble in the diluent or liquid carrier. Suitable diluents for use in slurry and solution polymerizations are known in the art and include hydrocarbons that are liquid under reaction conditions. Furthermore, the term "diluent" as used in this disclosure does not necessarily mean that the material is inert, as the diluent may contribute to polymerization, such as bulk polymerization with propylene.
[0241] Suitable hydrocarbon diluents may include, but are not limited to, cyclohexane, isobutane, n-butane, propane, n-pentane, isopentane, neopentane, and n-hexane, as well as high-boiling solvents such as ISOPAR™. Isobutane works well as a diluent in slurry polymerization. Examples of such slurry polymerization techniques can be found in U.S. Pat. Nos. 4,424,341, 4,501,885, 4,613,484, 4,737,280, and 5,597,892, the entire disclosures of which are incorporated herein by reference. When polymerizing propylene or other α-olefins, the propylene or α-olefin itself may contain a solvent, known in the art as bulk polymerization.
[0242] In various aspects and embodiments, a polymerization reactor suitable for use with a catalyst system can include at least one feed system, at least one feed system for catalyst or catalyst components, at least one reactor system, at least one polymer recovery system, or any suitable combination thereof. Suitable reactors can further include any or a combination of a catalyst storage system, an extrusion system, a cooling system, a diluent recycle system, a monomer recycle system, and a comonomer recycle system or control system. Such reactors can optionally include continuous takeoff and direct recycle of catalyst, diluent, monomer, comonomer, inert gas, and polymer. In one aspect, a continuous process can include continuous introduction of monomer, comonomer, catalyst, if desired, cocatalyst, and diluent into a polymerization reactor, and continuous removal of a suspension containing polymer particles and diluent from the reactor.
[0243] In one embodiment, the polymerization method can be carried out over a wide temperature range. For example, the polymerization temperature can be in the range of about 50°C to about 280°C. In another embodiment, the polymerization reaction temperature can be in the range of about 70°C to about 110°C. The polymerization reaction pressure can be any pressure that does not terminate the polymerization reaction. In one embodiment, the polymerization pressure can be from about atmospheric pressure to about 30,000 psig. In another embodiment, the polymerization pressure can be from about 50 psig to about 800 psig.
[0244] The polymerization reaction can be carried out in an inert atmosphere, i.e., an atmosphere substantially free of molecular oxygen, and under substantially anhydrous conditions, thus in the absence of water at the start of the reaction. Thus, a dry, inert atmosphere, such as dry nitrogen or dry argon, is typically used in the polymerization reactor.
[0245] In one embodiment, hydrogen can be used in the polymerization process to control polymer molecular weight. In another embodiment, the method of deactivating the catalyst by adding carbon monoxide to the polymerization zone described in U.S. Patent No. 9,447,204, incorporated herein by reference, can be used to reduce or stop uncontrolled or runaway polymerization.
[0246] For the catalyst systems of the present disclosure, the polymerizations disclosed herein are typically carried out using a loop reaction zone or a batch process, or a slurry polymerization process in a gas phase zone utilizing a fluidized bed or stirred bed.
[0247] Slurry Loop. In one aspect, a typical polymerization method is a slurry polymerization process (also known as a "particle form process"), such as that disclosed in U.S. Pat. No. 3,248,179, incorporated herein by reference. Other polymerization methods for slurry processes can be used, including loop reactors of the type disclosed in U.S. Pat. No. 3,248,179, and those utilizing multiple stirred reactors, either in series, parallel, or a combination thereof.
[0248] The polymerization reactor system can include at least one loop slurry reactor, which can be a vertical loop or a horizontal loop, or a combination that can be independently selected from a single loop or a series of loops. Multiple loop reactors can include both vertical and horizontal loops. Slurry polymerization can be carried out in an organic solvent as a carrier or diluent. Examples of suitable solvents include propane, hexane, cyclohexane, octane, isobutane, or combinations thereof. The olefin monomer, carrier, catalyst system components, and optional comonomer can be continuously fed to the loop reactor where polymerization occurs. The reactor effluent can be flash evaporated to separate the solid polymer particles.
[0249] Gas phase. In one embodiment, the method for producing polyolefin polymers according to the present disclosure is a gas-phase polymerization process, for example, using a fluidized bed reactor. This type of reactor and means for operating it are described, for example, in U.S. Patent Nos. 3,709,853, 4,003,712, 4,011,382, 4,302,566, 4,543,399, 4,882,400, 5,352,749, 5,541,270, EP-A-0802202, and 839,380, each of which is incorporated herein by reference. These patents disclose gas-phase polymerization processes in which the polymerization medium is mechanically agitated or fluidized by a continuous flow of gaseous monomer and diluent.
[0250] Gas-phase polymerization systems can employ a continuous recycle stream containing one or more monomers continuously circulated through a fluidized bed in the presence of a catalyst under polymerization conditions. The recycle stream can be withdrawn from the fluidized bed and recycled back to the reactor. Simultaneously, polymer product can be removed from the reactor and fresh monomer can be added to replace the polymerized monomer. Such gas-phase reactors can include processes for the multistage gas-phase polymerization of olefins, in which olefins are polymerized in the gas phase in at least two independent gas-phase polymerization zones, while catalyst-containing polymer formed in the first polymerization zone is fed to the second polymerization zone.
[0251] Other gas phase processes contemplated by the disclosed polymerization process include sequential or multi-stage polymerization processes. In one aspect, gas phase processes that can be used in accordance with the present disclosure include those described in U.S. Patent Nos. 5,627,242, 5,665,818, and 5,677,375, and European publications EP-A-0794200, EP-B1-0649992, EP-A-0802202, and EP-B-634421, all of which are incorporated herein by reference.
[0252] In one embodiment of gas-phase polymerization according to the present disclosure, the ethylene partial pressure can be varied within a range suitable for providing practical polymerization conditions, such as from 10 psi to 250 psi, e.g., from 65 psi to 150 psi, from 75 psi to 140 psi, or from 90 psi to 120 psi. In another embodiment, the molar ratio of comonomer to ethylene in the gas phase can also be varied within a range suitable for providing practical polymerization conditions, such as from 0.0 to 0.70, from 0.0001 to 0.25, more preferably from 0.005 to 0.025, or from 0.025 to 0.05. According to one embodiment, the reactor pressure can be maintained within a range suitable for providing practical polymerization conditions, such as from 100 psi to 500 psi, from 200 psi to 500 psi, or from 250 psi to 350 psi.
[0253] According to a further aspect, in a fluidized gas bed process used to produce polymers, a gas stream containing one or more monomers can be continuously cycled through the fluidized bed in the presence of a catalyst under reactive conditions. The gas stream can be withdrawn from the fluidized bed and returned to the reactor, and simultaneously, polymer product can be withdrawn from the fluidized bed and withdrawn from the reactor, and fresh monomer can be added to replace the polymerized monomer. See, e.g., U.S. Pat. Nos. 4,543,399, 4,588,790, 5,028,670, 5,317,036, 5,352,749, 5,405,922, 5,436,304, 5,543,471, 5,462,999, 5,616,661, and 5,668,228, each of which is incorporated herein by reference in its entirety.
[0254] In another embodiment, the antistatic compound can be fed into the polymerization zone simultaneously with the finished catalyst. Alternatively, the antistatic compound can be used as described in U.S. Patent Nos. 7,919,569, 6,271,325, 6,281,306, 6,140,432 and 6,117,955, the entire contents of which are incorporated herein by reference. For example, the clay heteroadduct can be contacted with one or more antistatic compounds or impregnated with one or more antistatic compounds. The antistatic compound can be added at any time, for example, they can be added at any time after calcination, including after contacting the final catalyst preparation.
[0255] In another embodiment, so-called "self-limiting" compositions can be added to the clay heteroadduct to prevent chunking, contamination, or uncontrollable or runaway reactions in the polymerization zone. For example, U.S. Patent Nos. 6,632,769, 6,346,584, and 6,713,573, each of which is incorporated herein by reference, disclose additives that can release catalyst poisons above a threshold temperature. Typically, such compositions can be added at any time after calcination to limit or stop polymerization activity above a desired temperature.
[0256] Solution. The polymerization reactor can also include a solution polymerization reactor in which the monomer is contacted with the catalyst composition by suitable agitation or other means. Solution polymerization can be carried out batchwise or continuously. An inert organic diluent or carrier containing excess monomer can be used, and the polymerization zone is maintained at a temperature and pressure that results in the formation of a polymer solution in the reaction medium. Agitation can be used during polymerization to obtain better temperature control and maintain a homogeneous polymerization mixture throughout the polymerization zone, and appropriate means for dissipating the heat of polymerization are utilized. The reactor can also include a series of at least one separator that uses high and low pressures to separate the desired polymer.
[0257] Tubular reactors and high-pressure LDPE. In yet another embodiment, the polymerization reactor can include a tubular reactor, which can produce polymers by free radical initiation or, alternatively, by using the disclosed catalyst. The tubular reactor can have several zones into which fresh monomer, initiator, or catalyst and cocatalyst are added. For example, the monomer can be contained in an inert gas stream and introduced into one zone of the reactor, while the initiator, catalyst composition, and / or catalyst components can be contained in a gas stream and introduced into another zone of the reactor. These gas streams can then be mixed for polymerization, and the heat and pressure can be appropriately adjusted to obtain optimal polymerization reaction conditions.
[0258] Coupled or Multiple Reactors. In a further aspect, the catalysts and processes of the present disclosure are not limited by the type of reactor or combination of reactor types considered. For example, the disclosed catalysts and processes can be used in a multiple reactor system that can include coupled or connected reactors or multiple unconnected reactors to carry out polymerization. Polymer can be polymerized in one reactor under one set of conditions, and then the polymer can be transferred to a second reactor for polymerization under different conditions.
[0259] In this embodiment, the polymerization reactor system can include a combination of two or more reactors. The production of polymer in multiple reactors can include several stages in at least two separate polymerization reactors interconnected by a transfer device to transfer the polymer from the first polymerization reactor to the second reactor, with different polymerization conditions in the individual reactors. Alternatively, the polymerization in multiple reactors can include manually transferring the polymer from one reactor to a subsequent reactor to continue the polymerization. Such reactors can include any combination, including, but not limited to, multiple loop reactors, multiple gas reactors, a combination of a loop reactor and a gas reactor, a combination of an autoclave reactor or a solution reactor with a gas or loop reactor, multiple solution reactors, or multiple autoclave reactors.
[0260] Polymers produced using the disclosed catalysts and processes. The catalyst compositions used in this process are capable of producing high-quality polymer particles without substantial reactor fouling. When the catalyst compositions are used in a loop reactor zone under slurry polymerization conditions, the particle size of the calcined hetero-coagulated product can range from about 10 microns (μm) to about 1000 microns, from about 25 microns to about 500 microns, from about 50 microns to about 200 microns, or from about 30 microns to about 100 microns to provide good control of polymer particle production during polymerization.
[0261] When the catalyst composition is used in a gas phase reactor zone, the particle size of the calcined hetero-coagulated product can range from about 1 micron to about 1000 microns, from about 5 to about 500 microns, or from about 10 microns to about 200 microns, or from about 15 microns to about 60 microns to provide good control of the polymer particles and the polymerization reaction.
[0262] The preferred particle size in other polymerization reactor systems may be a function of whether the system is single or multiple, the total catalyst productivity, and the optimal particle size and particle size distribution of the final polymer-catalyst composite particles. For example, the optimal size and size distribution may be determined by the polymerization reactor system, such as whether the particles are easily fluidizable in a gas-phase system, but large enough not to be trapped in the fluidizing gas and clog downstream filters. Similarly, the optimal size and size distribution in a polymerization system may be balanced against the ease with which the catalyst-polymer composite particles can be transported or handled in a storage silo or extrusion facility when melted and extruded into pellets.
[0263] Polymers produced using the catalyst compositions of the present disclosure can be formed into a variety of articles, such as, for example, household containers and appliances, film products, car bumper components, drums, fuel tanks, pipes, geomembranes, and liners. In one aspect, additives and modifiers can be added to the polymer to provide desired effects, such as a desired combination of physical, structural, and flow properties. It is believed that by using the methods and materials described herein, articles can be produced at a lower cost while maintaining the desired polymer properties obtained for polymers produced using the transition metal or metallocene catalyst compositions disclosed herein.
[0264] Specific Embodiments. In more specific embodiments of the present disclosure, a process for producing a catalyst composition is provided, the process comprising: (1) contacting a suitable dioctahedral phyllosilicate clay with a heterocoagulant to form a solid that is easily filtered and washed to a conductivity of less than 10 mS / cm, or less than 5 mS / cm, or 1 mS / cm to 50 μS / cm, or 500 μS / cm to 50 μS / cm; (2) dehydrating and dehydroxylating the washed clay heteroadduct at a temperature of about -10°C to about 500°C, or within that range, to produce a calcined hetero-coagulated clay adduct composition that exhibits no or substantially no d001 peak below 8 degrees 2θ, preferably no or substantially no d001 peak below 10 degrees 2θ. If there are peaks in the region below 10 degrees 2θ, the dominant peak should be above 4 degrees 2θ, or greater in intensity than the peak that the clay mineral itself would exhibit after calcination at 300°C, e.g., in the range of 8 degrees 2θ to 12 degrees 2θ. (3) mixing the calcined hetero-coagulated clay additive composition with, for example, bis(1-butyl-3-methylcyclopentadienyl)zirconium dichloride at a temperature ranging from 15°C to 100°C to form a mixture; (4) after 1 minute to 1 hour, combining the mixture in part (3) with a trialkylaluminum, e.g., triethylaluminum, trioctylaluminum, or triisobutylaluminum, to produce (optionally, "consisting essentially of," or "consisting of") a catalyst composition.
[0265] A specific alternative embodiment to that described immediately above is to reverse the order of addition of the metallocene and trialkylaluminum in steps (1)-(4) immediately above. [Example]
[0266] The foregoing description is intended to illustrate, but not limit, the scope of the present disclosure, which is further illustrated by the following examples. The examples should not be interpreted as imposing limitations on the scope of the present disclosure. Rather, it should be understood that various other embodiments, aspects, modifications, and equivalents thereof that may suggest themselves to those skilled in the art in light of the written description can be pursued without departing from the spirit of the present invention or the scope of the appended claims. Therefore, the following examples are presented to provide more detailed disclosure and explanation to those skilled in the art.
[0267] Reagents and general procedures Unless otherwise stated, all reagents used to prepare the clay heteroadducts of the present disclosure were obtained from the commercial sources indicated and used "as is."
[0268] Volclay® HPM-20 aqueous bentonite dispersion (montmorillonite) from American Colloid Company was obtained from McCullough & Associates and is also referred to simply as HPM-20 or HPM-20 clay. 50% aluminum chlorhydrate aqueous solution (abbreviated as "ACH") and UltraPAC® 290 (polyaluminum chloride, empirically Al(OH) 2.5 Cl 3.5 ) were obtained from GEO Specialty Chemicals. Aluminum chlorhydrate powder (ALOXICOLL® 51P, empirically Al2Cl(OH)5) and aluminum sesquichlorohydrate solution (ALOXICOLL® 31L) were obtained from Parchem Fine and Specialty Chemicals. Fumed silica (AEROSIL® 200) and fumed aluminum oxide aqueous dispersion (AERODISP® W400) were obtained from Evonik Industries AG. An aqueous dispersion of colloidal alumina (NYACOL® AL27) was obtained from Nano Technologies, Inc.
[0269] Unless otherwise noted, clay dispersions, clay heteroadducts, pillared clays, and other compositions herein and in the Examples may be prepared using a dual-speed Conair™ Waring™ Commercial Lab Blender Model 7010G equipped with a timer. Blender speeds may be referred to as "low" speed blends versus "high" speed blends as follows: The Model 7010G blender was connected to a Staco Energy Variable Transformer (Model Number 3PN1010B), and blender speed was adjusted by changing the transformer settings. In the Examples and the Specification, "low" speed blends were achieved by setting the transformer between 0 and 50, and "high" speed blends were achieved by setting the transformer between 50 and 100.
[0270] Conductivity was measured using a Eutech PCSTestr 35 or a radiometer analytical conductivity meter according to the instrument's instruction manual and the references provided with each instrument. Solution or slurry pH measurements were performed using a Eutech PCSTestr 35 or a Beckmann φ 265 laboratory pH meter.
[0271] Deionized water, referred to herein as Milli-Q® water, was obtained by first pretreating the water using a Prepak 1 pretreatment pack and then further purifying the water using a Millipore Milli-Q® Advantage A10 water purification system. This water was typically used within two hours of collection.
[0272] Hexane, heptane, toluene, and dichloromethane were dried over activated molecular sieves and degassed with nitrogen before use. Instrument-grade isobutane, used as a solvent for ethylene homopolymerization, was purchased from Airgas and purified by passage through columns of activated carbon, alumina, and 13× molecular sieves. Finally, ultra-high-purity grade ethylene and hydrogen were obtained from Airgas via an OxyClear™ gas purifier, model number RGP-R1-500, from Diamond Tool and Die, Inc. UHP (ultra-high-purity) ethylene was further purified by passage through columns of activated carbon, alumina, 13× molecular sieves, and an OxyClear™ gas purifier, model number RGP-R1-500. UHP hydrogen was purified by passage through an OxyClear™ gas purifier, model number RGP-R1-500. Purified propylene was obtained as a slipstream from a commercial polypropylene plant.
[0273] All preparations involving the handling of organometallic compounds were carried out under a nitrogen (N2) atmosphere using Schlenk techniques or in a glove box.
[0274] Zeta potential measurement The zeta potential of the colloidal suspensions disclosed herein was derived from measuring the electroacoustic effect when an electric field was applied to the suspension. The instrument used to perform these measurements was a Colloidal Dynamic Zeta Probe Analyzer™. For example, zeta potential measurements were used to determine the dispersed clay concentration in 0.5 wt% to 1 wt% Volclay® HPM-20 / water dispersions as follows: A 250 g to 300 g sample of the dispersion to be measured was transferred to a measurement vessel containing an axial bottom stirrer. The stirring speed was set fast enough to prevent settling or substantial settling of the dispersion, but slow enough to allow the electroacoustic probe to be fully immersed in the mixture when fully lowered. Typically, the stirring speed was set at 250 rpm to 350 rpm, often 300 rpm.
[0275] The Colloid Dynamic Zeta Probe Analyzer™ measurement parameters used were: 5 readings at 1 reading / min, particle density of 2.6 g / cc, dielectric constant of 4.5. Initial estimated colloid weight percentage (concentration) of 0.7 wt% to 1.0 wt%. 推定値 ) was typically entered into the Zeta Probe Analyzer™ software. A 5 wt % Volclay® HPM-20 / water dispersion measured a zeta potential of -46 mV. In the equations below, where the final dispersed clay concentration is referred to as "concentration (conc)," the final dispersed clay concentration can be calculated from the initial estimated concentration according to the following equation: concentration = concentration 推定値 *(Measured Zeta Potential / (-46))
[0276] A Zeta Probe Analyzer™ was also used to dynamically track the evolving zeta potential during titration of clay dispersions, either colloidal or non-colloidal. Typically, cationic polymetallate titrants (or other cationic titrants) were added to 0.5 wt% to 5.0 wt% Volclay® HPM-20 / water dispersions at 0.25 mL to 2.0 mL per titration point, with an equilibration delay of 30 to 120 seconds.
[0277] The Zeta Probe software calculates the zeta potential using the colloid particle weight percentage not included in the colloid titrant. Therefore, when the titrant is a colloidal species, the measured zeta potential was adjusted to reflect the excess colloidal content of the solution measured by the following method: Initially, the weights of the titrated clay and titrated cationic species were calculated using the following formula: * is determined by multiplication, W is weight, and V is volume. W 滴定剤 =V 滴定剤 *density 滴定剤 *solid% 滴定剤 W 粘土 =V 合計 * density 滴定剤 * particle concentration 測定
[0278] The density of a 5% aqueous dispersion of Volclay® HPM-20 (titrant) was determined to be approximately 1.03 g / mL. The titration weight was scaled according to its particle density relative to the particle density of titrated Volclay® HPM-20 (montmorillonite) to determine the effective titration weight (W 有効 ) was obtained, and in this example, it was calculated as follows: W 有効 =W 滴定剤 *Particle density 滴定剤 / particle density 滴定剤
[0279] The effective colloid particle weight percentage (wt% ) was then calculated to provide an estimate of the relative increase in colloid content compared to an equivalent titration using a non-colloidal titrant. 有効 ) was calculated. The reciprocal of this value was then multiplied by the measured zeta potential to determine the adjusted zeta potential as follows: weight% 有効 =(W 有効 +W 粘土 ) / V t A=weight% 測定値 / weight% 有効 ZP 調整値 =ZP 測定値 *A
[0280] During zeta potential titrations of clay dispersions with cationic polymetalates, such as the titration of Volclay® HPM-20 montmorillonite with aluminum chlorhydrate (ACH), the zeta potential was measured before and during the titration as a function of titration volume and mmol Al / g clay. Samples of the solid material formed at various points during the titration (e.g., 0 mmol Al / g clay, 1.17 mmol Al / g clay, 1.52 mmol Al / g clay, etc.) were taken, and each sample was dried, calcined, and analyzed by powder XRD (X-ray diffraction).
[0281] As an example of a zeta potential titration, Figure 3 plots the zeta potential of a series of dispersions obtained by titrating Volclay® HPM-20 montmorillonite with aluminum chlorhydrate (ACH), plotting titration volume versus dispersion zeta potential (mV), and Figure 4 plots mmol Al / g clay versus dispersion zeta potential (mV) for the same titration. Figure 2 provides powder XRD patterns of a series of calcined products collected during this zeta potential titration of HPM-20 clay with ACH.
[0282] Powder X-ray diffraction (XRD) studies Powder X-ray patterns of the clay and clay heteroadducts were obtained using standard X-ray powder diffraction techniques on a Bruker D8 daVinci instrument, using a backloading holder and a Bragg Brentano geometry with a "θ-θ" scan type, zeroing the background silicon chip. The detector used was a linear silicon strip (LynxEYE) PSD detector. The test sample was placed in the sample holder of two circular goniometers enclosed in a radiation-safe enclosure. The X-ray source was a 2.0 kW Cu X-ray tube maintained at 40 kV and 25 mA operating current. The X-ray optics were in standard Bragg Brentano focusing mode, with X-rays diverging from the tube's DS slit (0.6 mm) to strike the sample and then converging on a position-sensitive X-ray detector (Lynx-Eye, Bruker-AXS). The two circular goniometers, each 250 mm in diameter, were computer-controlled with independent stepping motors and optical encoders. Flat, pressed powder samples were scanned at 0.8°(2θ) / min (2–30°2θ over 35 min). The software suite for data collection and evaluation was Windows-based. Data collection was automated using the Commander program by employing BSML files, and data were analyzed by the program DIFFRAC.EVA.
[0283] The XRD test method applied to the calcined clay heteroadducts disclosed herein to determine basal spacing is described, for example, by McCauley in U.S. Patent No. 5,202,295 (e.g., column 27, lines 22-43). The Bragg equation or law applied to clays is nλ=2d sinθ, where n is the repeat number, λ is 1.5418, d is the d001 spacing, and θ is the angle of incidence.
[0284] Pore volume and pore volume distribution The pore volume of the clay heteroadduct is calculated as cc / g (cm) of all pores identifiable by nitrogen desorption. 3 / g, cumulative volume (cubic centimeters per gram). For catalyst support or carrier particles such as alumina powder, as well as the clays and clay heteroadducts of the present disclosure, pore size distribution and pore volume are calculated by reference to nitrogen desorption isotherms (assuming cylindrical pores) by the BET (or BET) technique as described by S. Brunauer, P. Emmett, and E. Teller in the J. Am. Chem. Soc., 1939, 60, 309; see also ASTM D 3037, which identifies a procedure for determining surface area using the nitrogen BET method.
[0285] Pore volume distributions can be useful in understanding catalyst performance, and various attributes of the pore volume distribution, such as pore volume (total pore volume), the proportion of pores in various size ranges, and the "pore modes" describing the pore diameters corresponding to local maxima in the dV(logD) vs. pore diameter distribution, were derived from nitrogen adsorption-desorption isotherms based on the method described by E.P. Barrett, L.G. Joyner, and P.P. Halenda ("B.J.H."), "The Determination of Pore Volume and Area Distributions in Porous Substances. I. Computations from Nitrogen Isotherms," J. Am. Chem. Soc., 1951, 73(1), pp. 373-380.
[0286] surface area Determine surface area by nitrogen adsorption using the BET (or BET) technique described by S. Brunauer, P. Emmett, and E. Teller in the J. Am. Chem. Soc., 1939, 60, 309, nitrogen adsorption-desorption isotherm (assuming cylindrical pores) and see also ASTM D 3037, which identifies procedures for determining surface area using the nitrogen BET method. Pore volume (PV) (cc / g, cubic centimeters per gram) or surface area (SA) (m 2 All morphological properties related to weight, such as % wt. / g, meters squared per gram, were normalized to a "metal-free basis" according to procedures well known in the art. However, unless otherwise specified, morphological properties reported herein are on a "measured" basis without correction for metal content.
[0287] Polymerization reaction Ethylene homopolymerization was carried out in a dry 2-liter stainless steel Parr autoclave reactor using 1 liter of isobutane diluent. Table 3A reports the properties and polymerization data for the comparative support and the hetero-coagulated clay support of the present invention using (1-n-butyl-3-methylcyclopentadienyl)ZrCl2 and triethylaluminum (AlEt3) as the metallocene and cocatalyst. The selected pressure and temperature in the reactor for calculating the activity reported in Table 3A were 450 total psi and 90°C, maintained electronically by an ethylene mass flow controller or, alternatively, manually using a jacketed temperature controller. Table 3B reports the surface area and porosity properties of the comparative support and the hetero-coagulated clay support of the present invention.
[0288] Polymerization data using support activators of the present disclosure and comparative catalyst systems are presented in Table 3A. Polymerization runs are labeled P1 through P39, and the specific example number of the support used in each run is listed.
[0289] When hydrogen was used, a premixed gas supply tank of purified hydrogen and ethylene was used to maintain the desired total pressure in the supply tank with enough pressure to not significantly change the ethylene to hydrogen ratio in the reactor feed. The addition of hydrogen can affect the melt index of the polymer obtained with any given catalyst.
[0290] Before conducting a polymerization run, moisture was first removed from the reactor interior by preheating the reactor to at least 115°C under a dry nitrogen stream, which was maintained for at least 15 minutes. Agitation was provided, for example, by an impeller with a set point of 600 rpm and a Magnadrive™. The metallocene catalyst for the polymerization runs in Table 3A was (1-n-butyl-3-methylcyclopentadienyl)ZrCl2. Triethylaluminum (AlEt3 or TEA) was used as the cocatalyst or alkylating agent; 1.8 mmol of AlEt3 (3 mL of a 0.6 M solution of TEA in hexane) was typically used for the polymerization runs in this table. The post-contact catalyst components, i.e., a composition containing all listed catalyst system components previously contacted to form a composition, were prepared in an inert atmosphere glovebox and transferred to a catalyst charging tube or vessel. The contents of the catalyst charging vessel were then charged to the reactor by flushing with 1 L of isobutane. The reactor temperature control system was then turned on and allowed to reach a temperature a few degrees below the temperature setpoint, which typically took about 7 minutes. The reactor was brought to operating pressure by opening the ethylene manual feed valve, and the polymerization run continued for the time reported in Table 3A, e.g., 30 or 60 minutes. [Table 4] [Table 5]
[0291] Alternatively, the contents of the catalyst charging tube could be forced into the reactor with ethylene at a temperature approximately 10°C below the setpoint temperature, a few degrees below the run's setpoint temperature. In this method, two charging tubes were used. When the run pressure was reached, the reactor pressure was controlled by a mass flow controller. Ethylene consumption and temperature were monitored electronically. During the course of the polymerization, the reactor temperature was maintained at the setpoint temperature ±2°C, except for the initial catalyst charging during the first few minutes of operation. After 60 minutes or the specified run time, the polymerization was stopped by shutting off the ethylene inlet valve and venting isobutane. The reactor was allowed to return to ambient temperature. The polymer produced in the reaction was then removed from the reactor and dried, and the polymer weight was used to calculate the activity of a particular polymerization. Polymer melt indices, specifically the melt index (MI) and high-load melt index (HLMI), were obtained after stabilizing the polymer with butylated hydroxytoluene (BHT) according to ASTM procedures D618-05 and D1238-04C. Polymer density was measured according to ASTM D1505-03.
[0292] Catalyst and polymer characterization Metallocene compounds 1 H NMR spectra were collected at room temperature by placing 20 mg of the metallocene sample in a 10 mm NMR tube and adding 3.0 mL of CDCl3. 1 H NMR spectra were obtained on a Bruker AVANCE™ 400 NMR (400.13 MHz). Chemical shifts are reported in ppm (δ) relative to TMS or referenced to the chemical shifts of residual solvent proton resonances. Coupling constants are reported in Hertz (Hz).
[0293] NMR measurements of the isotactic pentad content in polypropylene were obtained by placing 400 mg of polymer sample in a 10 mm NMR tube, to which tetrachloroethane-d2 and 1.7 g of o-dichlorobenzene were added. 13C NMR spectra were obtained on a Bruker AVANCE™ 400 NMR (100.61 MHz, 90° pulse, 12 s delay between pulses). Approximately 5000 transients were stored for each spectrum, and the mmmm pentad peak (21.09 ppm) was used as the reference. Microstructure analysis was described in Busico, et al. Macromolecules, 1994, 27, 4521-4524.
[0294] Polypropylene melt flow rate (MFR) was determined at 230° C. under a load of 2.16 kg according to the ASTM D-1238 procedure.
[0295] The melting temperature, Tm, of polypropylene was obtained using a DSC and TA Instrument, Inc. Model: DSC Q1000 according to the procedure of ASTM D-3417.
[0296] Nitrogen adsorption / dissociation data for support activators and other materials were collected using an Anton Paar Autosorb iQ instrument. A typical measurement was performed as follows: 50 mg to 150 mg of calcined sample was weighed into a sample cell under an inert atmosphere and sealed with a stopper. The sample cell was inserted into the Autosorb iQ station and placed under vacuum. Liquid nitrogen was then used to cool the sample. Nitrogen adsorption / desorption isotherms were recorded at 77 K and relative pressures P / P = 0.05–1 (P = atmospheric pressure).
[0297] Example 1. Comparative Example of Preparation of Calcined Clay A 700 mg sample of Volclay® HPM-20 clay in its neat powder form was combined with 60 mL of deionized water. The mixture was vigorously stirred and rotary evaporated at 55 °C for 20-30 minutes. The resulting sample was then calcined at 300 °C for 6 hours, yielding 620 mg of a gray powder. The nitrogen adsorption / desorption BJH pore volume analysis is plotted in Figure 12.
[0298] Example 2. Comparative Example of Azeotropic Clay Preparation A 5.16 g sample of Volclay® HPM-20 clay powder was placed in a round-bottom flask and combined with 40 mL to 60 mL of n-butyl alcohol. The mixture was vigorously stirred and then rotary evaporated to dryness at 45°C. The drying process was stopped immediately after the alcohol had visibly evaporated. The odor of n-butyl alcohol was typically noticeable from the sample after this process. A 5.39 g sample of wet clay was obtained, and 4.46 g of this material was then calcined at 300°C for 6 hours, yielding 3.3 g of a black powder.
[0299] Example 3. Comparative Example of Preparation of Azeotropic Clay After Shearing A 133 g sample of a 5 wt % HPM-20 / water dispersion, prepared by slowly adding HPM-20 clay to deionized water in a Waring® blender with stirring, was first rotary evaporated at 45°C to 55°C to remove most of the water, after which 50 mL of n-butanol was added. Rotary evaporation at 45°C was continued, and drying was stopped immediately after the alcohol had visibly evaporated. A 3.2 g sample of this material was then calcined at 300°C for 6 hours, yielding 2.6 g of a gray powder. A BJH pore volume analysis of this material is shown in Figure 11.
[0300] Example 4. Preparation of colloidal clay dispersion A Waring® blender was charged with 570 g of deionized water, and 30.0 grams of HPM-20 was added in small portions while stirring. The mixture was stirred at a high rate (revolutions per minute, rpm) to obtain a 5 wt. % dispersion of the HPM-20 suspension that was substantially free of lumps or clumps. A 4.8 wt. % dispersion of Volclay® HPM-20 clay was prepared using 20 g of HPM-20 and 394 g of water and, when stirred using a Waring® blender at high rpm to obtain a clump-free dispersion, the dispersion was characterized by a conductivity of 908 μS / cm and a pH of 9.39.
[0301] Example 5. Aluminum chlorhydrate (Al) using aluminum chlorhydrate solution (6.4 mmol Al / g clay) 13Comparative Example of Preparation of Keggin-Ion Pillared Clay A Waring® blender was charged with 100 g of the colloidal clay dispersion prepared according to Example 4, followed by 6.9 g of a 50% GEO aluminum chlorhydrate solution, reported to have a basicity of 83.47%, while stirring. After the aluminum chlorhydrate was added, the mixture was stirred at high rpm for an additional 3 minutes. The pH of the mixture was measured as 4.23. Attempts to filter the resulting mixture through Fisherbrand® P8 filter paper failed. Therefore, two aliquots of the mixture were transferred to 50 milliliter plastic centrifuge tubes, and the samples were centrifuged at 3600 rpm in a Beckmann Coulter Allegra 6 centrifuge for a total of 140 minutes. The resulting clear supernatant was decanted from each tube and replaced with deionized water. The samples were shaken to resuspend the solids and centrifuged again. This process was repeated multiple times (typically 4-8 times) until the supernatant of one centrifuged sample had a conductivity of 67 μS / cm and a pH of 6.0. The supernatant was then decanted, and the solid was transferred to an Erlenmeyer flask with approximately 70 mL of n-butanol using a minimum of deionized water. Rotary evaporation yielded 2.11 g of an off-white powder. A 437 mg sample of this powder was placed in a porcelain bowl and placed in a 300 °C oven for 6 hours, yielding 0.301 grams of a dark gray powder.
[0302] Example 6. Aluminum chlorhydrate (Al) using aluminum chlorhydrate solution (6.4 mmol Al / g clay) 13 Reproducibility of the preparation of Keggin (Ionic) pillared clays: While stirring, 30 g of HPM-20 clay was slowly added over 1-2 minutes to a Waring® blender containing 570 g of deionized Milli-Q® water and stirred at low speed to obtain a gray colloidal dispersion that was free or substantially free of visible lumps or clumps. After the addition was complete, the resulting dispersion was blended at high speed for 5-10 minutes to obtain a slightly viscous mixture of a 5 wt% aqueous dispersion of HPM-20 clay.
[0303] A 150 g portion of this 5 wt% HPM-20 aqueous dispersion was transferred to a Waring® blender, and 9.35 g of a 50 wt% aqueous solution of GEO aluminum chlorohydrate was pipetted into a vial and added to the dispersion all at once. The mixture was blended at high speed for 5 minutes, then divided into four 50 mL centrifuge tubes and centrifuged at 3000-3500 rpm for 30-60 minutes. The pH and conductivity of the supernatant were measured (Eutech PCSTestr 35). The supernatant was decanted, and the remaining wet solid was resuspended in deionized Milli-Q® water. The centrifugation process (centrifugation, supernatant pH / conductivity measurement, supernatant removal, and resuspension in deionized Milli-Q® water) was repeated until the supernatant reached a conductivity of 100-300 μS / cm. A total of six centrifugations were performed, at which point the supernatant was discarded for the final time. To the remaining wet solid, 200 mL of 1-butanol was added, and after rotary evaporation at 45° C., 9.75 g of wet solid was obtained. The wet solid was then crushed with a pestle and mortar, and 4.28 g of this solid was transferred to a porcelain crucible and calcined at 300° C. for 6 hours to obtain 1.65 g of a gray-black powder.
[0304] Example 7. Aluminum chlorhydrate (Al 13 Comparative Example of the Preparation of Keggin-Ion Pillared Clay Using Powdered Aluminum Chlorohydrate (6.4 mg Al / g Clay) While stirring, a 30 g sample of HPM-20 clay was slowly added over 1-2 minutes to a Waring® blender containing 570 g of deionized Milli-Q® water and stirred at low speed to obtain a gray colloidal dispersion containing no or substantially no visible lumps or clumps. After addition was complete, the dispersion was blended at high speed for 5-10 minutes to obtain a slightly viscous mixture of a 5 wt% aqueous dispersion of HPM-20 clay.
[0305] A 100 g sample of this 5 wt% HPM-20 aqueous dispersion was transferred to a Waring® blender, and 3.42 g of Parchem ALOXICOLL® 51P powder was weighed into a vial, diluted with 35-40 g of deionized Milli-Q® water, and then added all at once to the dispersion. The mixture was blended at high speed for 5 minutes, then divided into four 50 mL centrifuge tubes and centrifuged at 3000-3500 rpm for 30-60 minutes. The pH and conductivity of the supernatant were measured (Eutech PCSTestr 35). The supernatant was decanted, and the remaining wet solid was resuspended in deionized Milli-Q® water. The centrifugation process (centrifugation, supernatant pH / conductivity measurement, supernatant removal, and resuspension in deionized Milli-Q® water) was repeated until the supernatant conductivity reached 100-300 μS / cm (a total of six centrifugations were performed at a final supernatant pH of 4.25 and a conductivity of 225 μS / cm), at which point the supernatant was discarded for the final time. The remaining wet solid was combined with 100-200 mL of 1-butanol in a round-bottom flask and rotary evaporated at 45 °C to yield 5.54 g of wet solid, which was then crushed with a pestle and mortar. A 1.8 g portion of this solid was transferred to a porcelain crucible and calcined at 300 °C for 6 hours to yield 1.2 g of a gray-black powder.
[0306] Example 8. Gravimetric Determination of Colloidal Clay Content of 1% Volclay® HPM-20 Aqueous Dispersions A 60 g sample of the 5 wt% HPM-20 clay dispersion in water was combined with 240 g of Milli-Q® deionized water to yield 300 g of a 1 wt% HPM-20 aqueous dispersion. Upon standing for 30 minutes to 1 hour, a significant amount of settled clay was observed in this diluted dispersion. The colloidal portion was decanted, and the settled portion was collected, dried, and weighed. This process provided 900 mg of collected HPM-20 clay, corresponding to a 0.7% colloidal content of the diluted dispersion. In a repeat of this experiment using 280–290 g of this 1% HPM-20 dispersion, 630 mg and 910 mg of solid clay were isolated, respectively, yielding colloidal content values of 0.77 and 0.69 wt% for the diluted dispersion.
[0307] Example 9. Zeta potential measurements of aluminum chlorhydrate / Volclay® HPM-20 ratios in clay heteroadducts While stirring, 30 g of HPM-20 clay was slowly added over several minutes to a Waring® blender containing 570 g of Milli-Q® deionized water to obtain a gray colloidal dispersion with no or substantially no visible lumps or clumps. After the addition was complete, the dispersion was stirred at high speed for 5-10 minutes to obtain a slightly viscous mixture of a 5 wt% aqueous dispersion of HPM-20 clay. A 42 g portion of this 5 wt% HPM-20 aqueous dispersion was combined with 258 g of Milli-Q® deionized water to obtain a 0.7 wt% aqueous dispersion of HPM-20. 280 g of this 0.7 wt% colloidal dispersion was then transferred to a Colloidal Dynamic Zeta Probe Analyzer™ measurement vessel containing an axial bottom stirrer. The stirring speed was set at 250 rpm to 350 rpm.
[0308] Following the procedures outlined in the Colloid Dynamic Zeta Probe Analyzer™ manual provided with the instrument, zeta potential measurements were performed on this diluted HPM-20 aqueous dispersion using an initial colloid content estimate of 0.7 wt% to determine the actual colloid content of the clay dispersion. Measurement of a 5 wt% HPM-20 aqueous dispersion yields a zeta potential measurement of -46 mV (negative 46 millivolts). The initial colloid content estimate was adjusted to match this zeta potential. In this case, the HPM-20 colloid content of the dispersion was determined to be 0.62%. Colloid Dynamic Zeta Probe measurement parameters were as follows: 5 readings, 1 reading / min, particle density of 2.6 g / cc, and dielectric constant of 4.5.
[0309] A 2.5 wt% aqueous solution of aluminum chlorohydrate (ACH) was obtained by dilution of a 50 wt% aluminum chlorohydrate solution (GEO). A volumetric titration of the 2.5 wt% ACH solution in a 0.7 wt% HPM-20 aqueous dispersion was then performed. The titration setting was 0.5 mL per titration point, with a 30-second equilibration delay. After adding 0.5 mL of the ACH solution, a 30-second delay was performed to allow equilibration before measuring the zeta potential.
[0310] Figure 3 and Table 4 report the results of this zeta potential titration for the volumetric addition of 2.5 wt% aluminum chlorohydrate (ACH) aqueous solution into a 0.7 wt% HPM-20 aqueous dispersion. The measured zeta potential is plotted against the titration volume (mL). The titration volume indicates the cumulative volume of aluminum chlorohydrate aqueous solution added. The amount of ACH solution and the measured density of the ACH solution, 1.075 g / mL, as well as the ACH molar aluminum / clay mass ratio used to achieve -20 mV, neutral, and +20 mV zeta potentials, are summarized in Table 4. [Table 6]
[0311] Example 10. Zeta potential measurements of polyaluminum chloride UltraPAC® 290 / Volclay® HPM-20 ratios in clay heteroadducts While stirring, 30 g of HPM-20 clay was slowly added over 1-2 minutes to a Waring® blender containing 570 g of Milli-Q® deionized water and stirred at low speed to obtain a gray colloidal dispersion that was free or substantially free of visible lumps or clumps. After addition was complete, the dispersion was stirred by blending at high speed for 5-10 minutes to obtain a slightly viscous mixture of a 5 wt% aqueous dispersion of HPM-20 clay.
[0312] A 60 g portion of this 5 wt% HPM-20 aqueous dispersion was combined with 240 g of Milli-Q® deionized water to obtain a 1 wt% HPM-20 aqueous dispersion. Approximately 280 g of the 1 wt% colloidal dispersion was transferred to a Colloid Dynamic Zeta Probe Analyzer™ measurement vessel containing an axial bottom stirrer. The stirring speed was set as described above.
[0313] Zeta potential measurements were performed on this diluted HPM-20 aqueous dispersion using an initial colloid content estimate of 1 wt% to determine the actual colloid content of the clay dispersion. Measurements on a 5 wt% HPM-20 aqueous dispersion yield a zeta potential measurement of -46 mV. The initial colloid content estimate is adjusted to match this zeta potential. In this case, the HPM-20 colloid content of the dispersion was estimated to be 0.67%. Colloid dynamic zeta probe measurement parameters were as follows: 5 readings, 1 reading / min, particle density of 2.6 g / cc, and dielectric constant of 4.5.
[0314] A 4.58 g sample of polyaluminum chloride (abbreviated as "PAC") UltraPAC® 290 (17.1% Al2O3 content) was diluted into a 100 mL volumetric flask using Milli-Q® deionized water. A volumetric titration of this 4.58 wt% UltraPAC® 290 solution in the aforementioned 1 wt% HPM-20 clay dispersion was then performed. The titration settings were 1 mL per titration point, with an equilibration delay of 30 seconds.
[0315] Figure 5 and Table 5 report the results of these zeta potential measurements, where titration volume indicates the cumulative volume of 4.58 wt% UltraPAC® 290 aqueous solution added, and the measured zeta potential is plotted against titration volume (mL). The amounts of UltraPAC® 290 dispersion used to achieve zeta potentials of -20 mV, neutral, and +20 mV are summarized in Table 5. [Table 7]
[0316] Example 11. Zeta Potential Measurements of NYACOL® AL27 Colloidal Alumina / Volclay® HPM-20 Ratios in Clay Heteroadducts A 1 wt% HPM-20 clay dispersion was prepared by adding approximately 60 g of a 5 wt% HPM-20 aqueous dispersion to 240 g of Milli-Q® water. A 285-300 g portion of the 1 wt% dispersion was transferred to a Zeta Probe measurement vessel and an initial zeta potential measurement was performed to estimate the true particle weight percent of the solution.
[0317] Zeta potential measurements were performed on this diluted HPM-20 aqueous dispersion to determine the actual colloid content of the clay dispersion. Measurement of a 5 wt% HPM-20 aqueous dispersion results in a zeta potential measurement of -44.2 mV. The initial colloid content estimate is adjusted to match this zeta potential. In this case, the HPM-20 clay colloid content of the dispersion was determined to be 0.92%. Colloid dynamic zeta probe measurement parameters were as follows: 5 readings, 1 reading / min, particle density of 2.6 g / cc, and dielectric constant of 4.5.
[0318] A 100 g sample of commercially available NYACOL® AL27 colloidal alumina dispersion (20 wt % Al2O3) was combined with 100 g of Milli-Q® deionized water to obtain a 10 wt % Al2O3 dispersion of NYACOL® AL27. A volumetric titration of this 10 wt % dispersion in the previously described 1 wt % HPM-20 clay dispersion was then performed. (The 1 wt % HPM-20% concentration designation is based on the recipe rather than the zeta potential estimate, which was determined to be approximately 0.92 wt %, because not all of the clay was colloidal upon dilution.) The titration settings were as follows: 1 mL per titration point from 0 mL to 27 mL and 3 mL per subsequent titration point, with a 60-second equilibration delay.
[0319] Figure 6 and Table 6 report the results of these measurements, with the titration volume indicating the cumulative volume of NYACOL® AL27 alumina dispersion added. In this example, the titrant is also a colloidal species. The zeta potential was adjusted using the method previously described and the dates are provided in Figure 6. The amounts of NYACOL® AL27 dispersion used to achieve zeta potentials of -20 mV, neutral, and +20 mV are summarized in Table 6. [Table 8]
[0320] Example 12. Preparation of aluminum chlorhydrate clay heteroadduct (1.76 mmol Al / g clay) A Waring® blender was charged with 475.22 grams of deionized water. While stirring, 25.09 grams of HPM-20 clay from American Colloid was slowly added. After the clay addition was complete, the mixture was stirred at elevated temperature for 5 minutes to obtain a lump-free, homogeneous suspension. Then, 9.53 grams of a 50% by weight aqueous solution of aluminum chlorhydrate (GEO) was added with stirring, and stirring was continued for 9 minutes. The mixture was poured into a high-density polyethylene bottle. The Waring® flask was rinsed with 42.5 grams of deionized Milli-Q® water, and the rinse water was transferred to the bottle. The bottle was shaken to thoroughly mix the contents, and the conductivity of the slurry was measured at 4.03 mS / cm, with a pH of 5.89.
[0321] A second batch of aluminum chlorhydrate clay heteroadduct was prepared in the same manner using 380.26 grams of deionized Milli-Q® water, 20.03 grams of HPM-20 clay, and 7.70 grams of a 50 wt. % aluminum chlorhydrate aqueous solution (GEO). The conductivity of this batch was measured at 3.64 mS / cm, and the pH was 5.58. The contents of the second batch, along with 30 grams of deionized water, were transferred to the bottle containing the remaining slurry from the first batch. The bottle was shaken to obtain a gray slurry with no visible lumps. The final conductivity of the combined batch was 3.84 mS / cm, and the final pH was 5.87.
[0322] Example 13. Comparative Example of Preparation of Aluminum Sesquichlorohydrate-Clay Heteroadduct Using Powdered Aluminum Sesquichlorohydrate (ASCH, 6.4 mmol Al / g Clay) In this comparative example, the synthesis of an aluminum sesquichlorohydrate clay heteroadduct using powdered aluminum sesquichlorohydrate (ASCH) demonstrates the need to use multiple washes and centrifugations to isolate the product, as compared to the procedures and products of Examples 31 and 32.
[0323] While stirring, 30 g of HPM-20 clay was slowly added over 1-2 minutes to a Waring® blender containing 570 g of deionized Milli-Q® water and stirred at low speed to obtain a gray colloidal dispersion that was free or substantially free of visible lumps or clumps. After addition was complete, the dispersion was blended at high speed for 5-10 minutes to obtain a slightly viscous mixture of a 5 wt% aqueous dispersion of HPM-20 clay.
[0324] A 100 g portion of this 5 wt% HPM-20 clay aqueous dispersion was transferred to a Waring® blender. A separate vial was charged with 3.53 g of ALOXICOLL® 31P powder and 35-40 mL of deionized Milli-Q® water, and this mixture was poured into the stirred dispersion all at once. The mixture was blended at high speed for 5 minutes, then divided into four 50 mL centrifuge tubes and centrifuged at 3000-3500 rpm for 30-60 minutes. The pH and conductivity of the supernatant were measured (Eutech PCSTestr 35); the pH was 4.0 and the conductivity was 7300 μS / cm. The supernatant was decanted, and the remaining wet solid was resuspended in deionized Milli-Q® water. The centrifugation process (centrifugation, supernatant pH / conductivity measurement, supernatant removal, and resuspension in deionized Milli-Q® water) was repeated until the supernatant reached a conductivity of 100-300 μS / cm. Achieving this conductivity required a total of six centrifugations, with a final supernatant pH of 4.3 and a conductivity of 286 μS / cm. At this point, the supernatant was discarded for the final time, and the remaining wet solid was combined with 100-200 mL of 1-butanol in a round-bottom flask and rotary evaporated at 45 °C to yield 5.82 g of wet solid, which was then crushed with a pestle and mortar. A 2.1 g sample of this solid was transferred to a porcelain crucible and calcined at 300 °C for 6 hours to yield 1.1 g of a gray-black powder.
[0325] Example 14. Spray Drying, Screening, and Calcination of Unwashed Aluminum Chlorohydrate Clay Heteroadduct Retained on a 325 Mesh Screen (1.76 mmol Al / g Clay) A portion of the aluminum chlorhydrate clay heteroadduct (1.76 mmol Al / g clay) mixture (slurry) prepared according to Example 12 was spray dried using a Buchi B290 laboratory spray dryer. A portion of the spray-dried clay heteroadduct was screened through a 325 mesh screen. Two grams of the material retained on the 325 mesh screen was loaded into a 300°C oven and heated in air for six hours. While still hot, the material was transferred to a vacuum chamber and allowed to cool to room temperature under vacuum.
[0326] Example 15. Spray drying, screening, and calcination of unwashed aluminum chlorhydrate clay heteroadduct passing through a 325 mesh screen (1.76 mmol Al / g clay) A portion of the aluminum chlorhydrate clay heteroadduct (1.76 mmol Al / g clay) mixture (slurry) prepared according to Example 12 was spray dried using a Buchi B290 laboratory spray dryer. A portion of the spray-dried clay heteroadduct was screened through a 325 mesh screen. Two grams of the screened material was loaded into a 300°C oven and heated in air for six hours. While still hot, the material was transferred to a vacuum chamber and allowed to cool to room temperature under vacuum.
[0327] Example 16. Spray-dried and calcined washed aluminum chlorohydrate clay heteroadduct (1.76 mmol Al / g clay) A portion of the aluminum chlorohydrate clay heteroadduct (1.76 mmol Al / g clay) slurry prepared according to Example 12 was filtered through Fisherbrand™ P8 filter paper using a Buchner funnel and vacuum. 158 grams of the filter cake was then transferred to an HDPE bottle and resuspended in approximately 1.2 liters of deionized water by shaking. The resulting slurry had a conductivity of 114 μS / cm and a pH of 6.25. The slurry was again filtered through Fisherbrand™ P8 filter paper and left on the filter overnight under vacuum to yield 109.03 grams of a gray solid. A 97.07 gram sample of this solid was loaded into an HDPE bottle with 452 g of deionized water and shaken until no lumps were visible in the slurry. The conductivity of the slurry was 112 μS / cm and the pH was 6.33. A portion of this aluminum chlorhydrate clay heteroadduct slurry was spray dried using a Buchi B290 laboratory spray dryer. A 1.77 gram sample of the spray-dried material was loaded into a 300°C oven and calcined in air for 6 hours. While still hot, the material was then transferred to a vacuum chamber and allowed to cool to room temperature under vacuum.
[0328] Example 17. Single-Filtered, Azeotroped, and Calcined Aluminum Chlorohydrate Clay Heteroadduct (1.76 mmol Al / g Clay) A 543 gram portion of the aluminum chlorhydrate clay heteroadduct (1.76 mmol Al / g clay) slurry prepared according to Example 12 was vacuum filtered through Fisherbrand™ brand P8 filter paper. The resulting filter cake was then resuspended in approximately 1 L of deionized water, resulting in a slurry with a conductivity of 114 μS and a pH of 6.25. This slurry was then vacuum filtered through Fisherbrand™ brand P8 paper, and 11.5 grams of the clay heteroadduct filter cake retained on the filter paper was loaded into an Erlenmeyer flask equipped with a stir bar. 200 mL of n-butanol was then added, and the mixture was stirred until a slurry without visible lumps or clumps was obtained. The stir bar was removed, and the Erlenmeyer was rotary evaporated from a 45°C bath. The off-white powder, containing some flakes and clumps, was very gently ground to a uniform powder and 1.04 grams was loaded into a porcelain crucible that was fired in air at 300° C. for 6 hours. The fired material was cooled under vacuum and 0.867 grams was transferred to an inert atmosphere glove box.
[0329] Example 18. Reproducibility of a single filtration, azeotrope, and calcination of an aluminum chlorhydrate clay heteroadduct (1.76 mmol Al / g clay) according to Example 17 While stirring, 30 g of HPM-20 clay was slowly added over 1-2 minutes to a Waring® blender containing 570 g of deionized Milli-Q® water and stirred at low speed to obtain a gray colloidal dispersion that was free or substantially free of visible lumps or clumps. After addition was complete, the dispersion was blended at high speed for 5-10 minutes to obtain a slightly viscous mixture of a 5 wt% aqueous dispersion of HPM-20 clay.
[0330] A 100 g portion of this 5 wt% HPM-20 clay aqueous dispersion was transferred to a Waring® blender, and 1.91 g of a 50 wt% aqueous solution of GEO aluminum chlorohydrate was pipetted into a vial and added all at once to the dispersion. The mixture rapidly solidified, and 70 mL of deionized Milli-Q® water was added to facilitate mixing. The mixture was then blended at high speed for 5 minutes before being vacuum filtered through Fisher P8 qualitative grade filter paper (coarse porosity). After 15-30 minutes of filtration, the filtrate pH and conductivity were measured (Eutech PCSTestr 35) and found to be pH 6.1 and conductivity 1516 μS / cm. The filtrate was discarded, and the remaining wet solid was resuspended in 50-100 mL of deionized Milli-Q® water.
[0331] The filtration process (suspension of the wet solid in deionized Milli-Q® water, vacuum filtration, and filtrate pH / conductivity measurement) was repeated again. The remaining wet solid was resuspended in 150-200 mL of 1-butanol and rotary evaporated at 45 °C. The resulting solid was then crushed with a pestle and mortar to yield 5.18 g of a light gray powder. A 1.90 g portion of this solid was transferred to a porcelain crucible and calcined at 300 °C for 6 hours to yield 0.9 g of a gray-black powder. The powder XRD (X-ray diffraction) pattern of this sample is displayed in Figure 2, and the BJH pore volume analysis of this sample is plotted in Figure 10.
[0332] Example 19. Comparative Example of Preparation of Aluminum Chlorohydrate (ACH) Ion-Exchanged Clay (0.3 mmol Al / g Clay) While stirring, 30 g of HPM-20 clay was slowly added over 1-2 minutes to a Waring® blender containing 570 g of deionized Milli-Q® water and stirred at low speed to obtain a gray colloidal dispersion that was free or substantially free of visible lumps or clumps. After addition was complete, the dispersion was blended at high speed for 5-10 minutes to obtain a slightly viscous mixture of a 5 wt% aqueous dispersion of HPM-20 clay.
[0333] A 100 g portion of this 5 wt% HPM-20 clay aqueous dispersion was transferred to a Waring® blender. A 0.325 g sample of the GEO ACH aqueous dispersion (50 wt%) was pipetted into a vial, combined with 20 mL of deionized Milli-Q® water, and then poured all at once into the clay dispersion. The resulting mixture was then blended at high speed for 5 minutes and then vacuum filtered through Fisher P8 qualitative-grade filter paper (coarse porosity). Filtration was slow (<1 drop / sec). After filtration continued for 15-30 minutes, the filtrate pH and conductivity were measured (Eutech PCSTestr 35) and found to be pH 7.3 and conductivity 487 μS / cm. The filtrate was discarded, and the remaining wet solid was resuspended in 50 mL of deionized Milli-Q® water and centrifuged once at 3000-3500 rpm for 30-60 minutes. After removing the supernatant (measured conductivity 180 μS / cm), the remaining wet solid was resuspended in 50–100 mL of 1-butanol and rotary evaporated at 45 °C. The resulting solid was then ground with a pestle and mortar, and 1.7 g of the powdered solid was transferred to a porcelain crucible and calcined at 300 °C for 6 h to yield 0.8 g of a gray-black powder.
[0334] Example 20. Preparation of aluminum chlorohydrate (ACH) clay heteroadduct (1.17 mmol Al / g clay) While stirring, 30 g of Volclay® HPM-20 clay was slowly added over 1-2 minutes to a Waring® blender containing 570 g of deionized Milli-Q® water and stirred at low speed to obtain a gray colloidal dispersion containing no or substantially no visible lumps or clumps. After addition was complete, the dispersion was blended at high speed for 5-10 minutes to obtain a slightly viscous mixture of a 5 wt% aqueous dispersion of HPM-20 clay.
[0335] A 100 g portion of this 5 wt% HPM-20 clay aqueous dispersion was transferred to a Waring® blender. Then, 1.27 g of a 50 wt% aqueous solution of GEO aluminum chlorohydrate was pipetted into a vial and added to the dispersion all at once. The mixture rapidly coagulated, and 70 mL of deionized Milli-Q® water was added to facilitate mixing. The mixture was then blended at high speed for 5 minutes, after which it was vacuum filtered through Fisher P8 qualitative grade filter paper (coarse porosity). After 15-30 minutes of filtration, the filtrate pH and conductivity were measured (Eutech PCSTestr 35) and found to be pH 6.25 and conductivity 1166 μS / cm, respectively. The filtrate was discarded, and the remaining wet solid was resuspended in 50-100 mL of deionized Milli-Q® water.
[0336] The filtration process (suspension of wet solid in deionized Milli-Q® water, vacuum filtration, filtrate pH / conductivity measurement) was repeated until the conductivity of the resuspended slurry reached 100-300 μS / cm. In this case, one additional filtration was performed, resulting in a slurry with a pH of 6.2 and a conductivity of 188 μS / cm. The remaining wet solid was resuspended in 150-200 mL of 1-butanol and rotary evaporated at 45 °C. The solid was then crushed with a pestle and mortar to yield 2.97 g of a light gray powder. A 1.7 g portion of this solid was transferred to a porcelain crucible and calcined at 300 °C for 6 hours to yield 1.0 g of a gray-black powder. The powder XRD (X-ray diffraction) pattern of this sample is shown in Figure 2.
[0337] Example 21. Preparation of Aluminum Chlorohydrate (ACH) Clay Heteroadduct (1.52 mmol Al / g Clay) While stirring, 30 g of Volclay® HPM-20 clay was slowly added over 1-2 minutes to a Waring® blender containing 570 g of deionized Milli-Q® water and stirred at low speed to obtain a gray colloidal dispersion containing no or substantially no visible lumps or clumps. After addition was complete, the dispersion was blended at high speed for 5-10 minutes to obtain a slightly viscous mixture of a 5 wt% aqueous dispersion of HPM-20 clay.
[0338] A 100 g portion of this 5 wt% HPM-20 clay aqueous dispersion was transferred to a Waring® blender. A 1.66 g sample of a 50 wt% aqueous solution of GEO aluminum chlorohydrate was pipetted into a vial and added all at once to the dispersion. The resulting mixture rapidly coagulated, and 80 mL of deionized Milli-Q® water was added to facilitate mixing. The mixture was then blended at high speed for 5 minutes before being vacuum filtered through Fisher P8 qualitative-grade filter paper (coarse porosity). After 15-30 minutes of filtration, the filtrate pH and conductivity were measured (Eutech PCSTestr 35) and found to be pH 6.2 and conductivity 1518 μS / cm. The filtrate was discarded, and the remaining wet solid was resuspended in 50-100 mL of deionized Milli-Q® water.
[0339] This filtration process (suspension of wet solid in deionized Milli-Q® water, vacuum filtration, filtrate pH / conductivity measurement) was repeated until the conductivity of the resuspended slurry reached 100-300 μS / cm. In this case, one additional filtration was performed, resulting in a slurry with a pH of 6.1 and a conductivity of 199 μS / cm. The remaining wet solid was resuspended in 150-200 mL of 1-butanol and rotary evaporated at 45 °C. The resulting solid was then crushed with a pestle and mortar to yield 3.19 g of a light gray powder. A 1.65 g sample of this solid was transferred to a porcelain crucible and calcined at 300 °C for 6 hours, yielding 0.9 g of a gray-black powder. The powder XRD pattern of this sample is shown in Figure 2.
[0340] Example 22. Preparation of Aluminum Chlorohydrate (ACH) Clay Heteroadduct (2.5 mmol Al / g Clay) and Comparative Example of Single Filtration While stirring, 30 g of HPM-20 clay was slowly added over 1-2 minutes to a Waring® blender containing 570 g of deionized Milli-Q® water and stirred at low speed to obtain a gray colloidal dispersion that was free or substantially free of visible lumps or clumps. After addition was complete, the dispersion was blended at high speed for 5-10 minutes to obtain a slightly viscous mixture of a 5 wt% aqueous dispersion of HPM-20 clay.
[0341] A 100 g portion of this 5 wt% HPM-20 clay aqueous dispersion was transferred to a Waring® blender. A 2.71 g sample of a 50 wt% aqueous solution of GEO aluminum chlorohydrate was pipetted into a vial and added all at once to the dispersion. The mixture quickly became viscous, and 100 mL of deionized Milli-Q® water was added to facilitate stirring. The mixture was then blended at high speed for 5 minutes and then vacuum filtered through Fisher P8 qualitative grade filter paper (coarse porosity). After 15-30 minutes of filtration, the filtrate pH and conductivity were measured (Eutech PCSTestr 35) and found to be 4.72 and 1988 μS / cm, respectively. A portion of the wet solid filter cake was resuspended in 50-100 mL of 1-butanol and rotary evaporated at 45°C. The dried solid was then crushed with a pestle and mortar, yielding 0.66 g of a light gray powder. A 0.64 g portion of this solid was transferred to a porcelain crucible and fired at 300° C. for 6 hours to yield 0.5 g of a gray-black powder.
[0342] Example 23. Comparative Example of Preparation of Aluminum Chlorohydrate (ACH) Clay Heteroadduct and Additional Washing / Filtration Compared to Example 22 (2.5 mmol Al / g Clay) While stirring, 30 g of HPM-20 clay was slowly added over 1-2 minutes to a Waring® blender containing 570 g of deionized Milli-Q® water and stirred at low speed to obtain a gray colloidal dispersion that was free or substantially free of visible lumps or clumps. After addition was complete, the dispersion was blended at high speed for 5-10 minutes to obtain a slightly viscous mixture of a 5 wt% aqueous dispersion of HPM-20 clay.
[0343] A 100 g portion of this 5 wt% HPM-20 clay aqueous dispersion was transferred to a Waring® blender. A 2.71 g sample of a 50 wt% aqueous solution of GEO aluminum chlorohydrate was pipetted into a vial and added all at once to the dispersion. The mixture quickly became viscous, and 100 mL of deionized Milli-Q® water was added to facilitate stirring. The mixture was then blended on high speed for 5 minutes and then vacuum filtered through Fisher P8 qualitative-grade filter paper (coarse porosity). After 15-30 minutes of filtration, the filtrate pH and conductivity were measured (Eutech PCSTestr 35). The filtrate was discarded, and the remaining wet solid was resuspended in 50-100 mL of deionized Milli-Q® water.
[0344] The filtration process (suspension of the wet solid in deionized Milli-Q® water, vacuum filtration, filtrate pH / conductivity measurement) was repeated until the conductivity of the resuspended slurry reached 100-300 μS / cm. In this case, one additional filtration was performed, resulting in a slurry with a pH of 4.67 and a conductivity of 87 μS / cm. The remaining wet solid was resuspended in 50-100 mL of 1-butanol and rotary evaporated at 45 °C. The dried solid was then crushed with a pestle and mortar to yield 3.73 g of a light gray powder. A 1.37 g portion of this solid was transferred to a porcelain crucible and calcined at 300 °C for 6 hours to yield 0.6 g of a gray-black powder. The powder XRD pattern of this sample is shown in Figure 2.
[0345] Example 24. Preparation of Aluminum Chlorohydrate (ACH) Clay Heteroadduct (3.5 mmol Al / g Clay) and Comparative Example of Single Filtration While stirring, 30 g of HPM-20 clay was slowly added over 1-2 minutes to a Waring® blender containing 570 g of deionized Milli-Q® water and stirred at low speed to obtain a gray colloidal dispersion that was free or substantially free of visible lumps or clumps. After addition was complete, the dispersion was blended at high speed for 5-10 minutes to obtain a slightly viscous mixture of a 5 wt% aqueous dispersion of HPM-20 clay.
[0346] A 100 g portion of this 5 wt% HPM-20 clay aqueous dispersion was transferred to a Waring® blender. A 3.80 g sample of a 50 wt% aqueous solution of GEO aluminum chlorohydrate was pipetted into a vial and added all at once to the dispersion. 20 mL of deionized Milli-Q® water was added to facilitate mixing. The mixture was then blended at high speed for 5 minutes and then vacuum filtered through Fisher P8 qualitative grade filter paper (coarse porosity). After 15-30 minutes of filtration, the filtrate pH and conductivity were measured (Eutech PCSTestr 35) and found to be 4.34 and 1500 μS / cm, respectively. A portion of the wet solid was resuspended in 50-100 mL of 1-butanol and rotary evaporated at 45°C. The dried solid was then crushed with a pestle and mortar to yield 0.74 g of a light gray powder. A 0.62 g portion of this solid was transferred to a porcelain crucible and fired at 300° C. for 6 hours to yield 0.5 g of a gray-black powder.
[0347] Example 25. Comparative Example of Preparation of Aluminum Chlorohydrate (ACH) Clay Heteroadduct and Additional Washing / Filtration Compared to Example 24 (3.5 mmol Al / g Clay) While stirring, 30 g of HPM-20 clay was slowly added over 1-2 minutes to a Waring® blender containing 570 g of deionized Milli-Q® water and stirred at low speed to obtain a gray colloidal dispersion that was free or substantially free of visible lumps or clumps. After addition was complete, the dispersion was blended at high speed for 5-10 minutes to obtain a slightly viscous mixture of a 5 wt% aqueous dispersion of HPM-20 clay.
[0348] A 100 g portion of this 5 wt% HPM-20 clay aqueous dispersion was transferred to a Waring® blender. A 3.80 g sample of a 50 wt% aqueous solution of GEO aluminum chlorohydrate was pipetted into a vial and added all at once to the dispersion. The mixture quickly became viscous, and 20 mL of deionized Milli-Q® water was added to facilitate stirring. The mixture was then blended on high speed for 5 minutes and then vacuum filtered through Fisher P8 qualitative-grade filter paper (coarse porosity). After 15-30 minutes of filtration, the filtrate pH and conductivity were measured (Eutech PCSTestr 35). The filtrate was discarded, and the remaining wet solid was resuspended in 50-100 mL of deionized Milli-Q® water.
[0349] The filtration process (suspension of wet solid in deionized Milli-Q® water, vacuum filtration, filtrate pH / conductivity measurement) was repeated until the conductivity of the resuspended slurry reached 100-300 μS / cm. In this case, one additional filtration was performed, yielding a slurry with a pH of 4.5 and a conductivity of 180 μS / cm. The remaining slurry was resuspended in 50-100 mL of 1-butanol and rotary evaporated at 45 °C. The dried solid was then crushed with a pestle and mortar to yield 4.33 g of a light gray powder. A 1.36 g portion of this solid was transferred to a porcelain crucible and calcined at 300 °C for 6 hours to yield 0.6 g of a gray-black powder. The powder XRD pattern of this sample is shown in Figure 2.
[0350] Example 26. Comparative Example of Preparation of Aluminum Chlorohydrate (ACH) Clay Heteroadduct Using Powdered ACH Reagent (0.3 mmol Al / g Clay) While stirring, 30 g of HPM-20 clay was slowly added over 1-2 minutes to a Waring® blender containing 570 g of deionized Milli-Q® water and stirred at low speed to obtain a gray colloidal dispersion that was free or substantially free of visible lumps or clumps. After addition was complete, the dispersion was blended at high speed for 5-10 minutes to obtain a slightly viscous mixture of a 5 wt% aqueous dispersion of HPM-20 clay.
[0351] A 100 g portion of this 5 wt% HPM-20 clay aqueous dispersion was transferred to a Waring® blender. A separate vial was charged with 0.160 g of ALOXICOLL® 51P powder and 20 mL of deionized Milli-Q® water. This mixture was poured into the stirred dispersion in one go, and 40 mL of deionized Milli-Q® water was added to facilitate mixing. The mixture was then blended on high speed for 5 minutes and then vacuum filtered through Fisherbrand™ P8 qualitative grade filter paper (coarse porosity). Filtration was slow (<1 drop / sec). After 15-30 minutes of filtration, the filtrate pH and conductivity were measured (Eutech PCSTestr 35) and found to be pH 6.5 and conductivity 780 μS / cm. The filtrate was discarded, and the remaining wet solid was resuspended in 50 mL of deionized Milli-Q® water and centrifuged once at 3000-3500 rpm for 30-60 minutes. After removing the supernatant (conductivity 180 μS / cm), the remaining wet solid was resuspended in 50-100 mL of 1-butanol and rotary evaporated. The resulting solid was then crushed with a pestle and mortar, then transferred to a porcelain crucible and calcined at 300°C for 6 hours to yield a gray-black powder.
[0352] Example 27. Comparative Example of Preparation of Aluminum Chlorohydrate (ACH) Clay Heteroadduct Using Powdered ACH Reagent (0.6 mmol Al / g Clay) While stirring, 30 g of HPM-20 clay was slowly added over 1-2 minutes to a Waring® blender containing 570 g of deionized Milli-Q® water and stirred at low speed to obtain a gray colloidal dispersion that was free or substantially free of visible lumps or clumps. After addition was complete, the dispersion was blended at high speed for 5-10 minutes to obtain a slightly viscous mixture of a 5 wt% aqueous dispersion of HPM-20 clay.
[0353] A 100 g portion of this 5 wt% HPM-20 clay aqueous dispersion was transferred to a Waring® blender. A separate vial was charged with 0.4 g of ALOXICOLL® 51P powder and 20 mL of deionized Milli-Q® water. This mixture was poured into the stirred dispersion all at once. 40 mL of deionized Milli-Q® water was added to facilitate mixing. The mixture was then blended at high speed for 5 minutes and then vacuum filtered through Fisher P8 qualitative-grade filter paper (coarse porosity). After 15-30 minutes of filtration, the filtrate pH and conductivity were measured (Eutech PCSTestr 35) and found to be pH 7.2 and conductivity 180 μS / cm. The filtrate was discarded, and the remaining wet solid was resuspended in 50 mL of deionized Milli-Q® water and centrifuged once at 3000-3500 rpm for 30-60 minutes. After removing the supernatant (conductivity 180 μS / cm), the remaining wet solid was resuspended in 50–100 mL of 1-butanol and rotary evaporated at 45°C. The resulting solid was then ground with a pestle and mortar to obtain 2 g of a gray powder, which was then transferred to a porcelain crucible and calcined at 300°C for 6 h to obtain a gray-black powder.
[0354] Example 28. Preparation of Aluminum Chlorohydrate (ACH) Clay Heteroadduct Using Powdered ACH Reagent and Additional Washing Compared to Example 29 (1.52 mmol Al / g Clay) While stirring, 30 g of HPM-20 clay was slowly added over 1-2 minutes to a Waring® blender containing 570 g of deionized Milli-Q® water and stirred at low speed to obtain a gray colloidal dispersion that was free or substantially free of visible lumps or clumps. After addition was complete, the dispersion was blended at high speed for 5-10 minutes to obtain a slightly viscous mixture of a 5 wt% aqueous dispersion of HPM-20 clay.
[0355] A 100 g portion of this 5 wt% HPM-20 clay aqueous dispersion was transferred to a Waring® blender. A separate vial was charged with 0.812 g of ALOXICOLL® 51P powder and 20 mL of deionized Milli-Q® water. This mixture was poured into the stirred dispersion all at once. To facilitate mixing, 20–40 mL of deionized Milli-Q® water was added. The mixture was then blended on high speed for 5 minutes and then vacuum filtered through Fisher P8 qualitative-grade filter paper (coarse porosity). After 15–30 minutes of filtration, the filtrate pH and conductivity were measured (Eutech PCSTestr 35). The remaining wet solid was resuspended in 50–100 mL of deionized Milli-Q® water.
[0356] The filtration process (suspension of the wet solid in deionized Milli-Q® water, vacuum filtration, filtrate pH / conductivity measurement) was repeated until the supernatant reached a conductivity of 100-300 μS / cm. In this case, two filtrations were performed, yielding a filtrate with a pH of 6.3 and a conductivity of 169 μS / cm. The remaining wet solid was resuspended in 150-200 mL of 1-butanol and rotary evaporated at 45 °C. The solid was then crushed with a pestle and mortar to yield 3.44 g of a light gray powder. A 1.5 g portion of this solid was transferred to a clay crucible and calcined at 300 °C for 6 hours to yield 1.0 g of a gray-black powder.
[0357] Example 29. Preparation of Aluminum Chlorohydrate (ACH) Clay Heteroadduct Using Powdered ACH Reagent and Single Filtration Compared to Example 28 (1.52 mmol Al / g Clay) While stirring, 30 g of HPM-20 clay was slowly added over 1-2 minutes to a Waring® blender containing 570 g of deionized Milli-Q® water and stirred at low speed to obtain a gray colloidal dispersion that was free or substantially free of visible lumps or clumps. After addition was complete, the dispersion was blended at high speed for 5-10 minutes to obtain a slightly viscous mixture of a 5 wt% aqueous dispersion of HPM-20 clay.
[0358] A 100 g portion of this 5 wt% HPM-20 clay aqueous dispersion was transferred to a Waring® blender. A separate vial was charged with 0.812 g of ALOXICOLL® 51P powder and 20 mL of deionized Milli-Q® water. This mixture was poured into the stirred dispersion in one go, and 20-40 mL of deionized Milli-Q® water was added to facilitate mixing. The mixture was then blended at high speed for 5 minutes and then vacuum filtered through Fisherbrand® P8 qualitative grade filter paper. After 15-30 minutes of filtration, the filtrate pH and conductivity were measured (Eutech PCSTestr 35) and found to be pH 5.8 and conductivity 1750 μS / cm. A portion of the remaining wet solid was resuspended in 50-100 mL of 1-butanol and rotary evaporated at 45°C. The solid was then crushed with a pestle and mortar to give 1 g of a grey powder, which was then transferred to a porcelain crucible and fired at 300° C. for 6 hours to give 0.6 g of a grey-black powder.
[0359] Example 30. Preparation of Aluminum Chlorohydrate (ACH) Clay Heteroadduct Using Powdered ACH Reagent (1.76 mmol Al / g Clay) While stirring, 30 g of HPM-20 clay was slowly added over 1-2 minutes to a Waring® blender containing 570 g of deionized Milli-Q® water and stirred at low speed to obtain a gray colloidal dispersion that was free or substantially free of visible lumps or clumps. After addition was complete, the dispersion was blended at high speed for 5-10 minutes to obtain a slightly viscous mixture of a 5 wt% aqueous dispersion of HPM-20 clay.
[0360] A 100 g portion of this 5 wt% HPM-20 clay aqueous dispersion was transferred to a Waring® blender. A separate vial was charged with 0.940 g of ALOXICOLL® 51P powder and 20 mL of deionized Milli-Q® water. This mixture was poured into the stirred dispersion all at once. 20-40 mL of deionized Milli-Q® water was added to facilitate mixing. The mixture was then blended at high speed for 5 minutes, then vacuum filtered through Fisherbrand™ P8 qualitative grade filter paper and washed with 100 mL of deionized Milli-Q® water. After 15-30 minutes of filtration, the filtrate pH and conductivity were measured (Eutech PCSTestr 35) and found to be pH 6.1 and conductivity 1799 μS / cm. A portion of the remaining wet solid was resuspended in 50-100 mL of 1-butanol and rotary evaporated at 45°C. The solid was then crushed with a pestle and mortar to give 1.07 g of a gray powder, which was then transferred to a porcelain crucible and fired at 300° C. for 6 hours to give 0.9 g of a gray-black powder.
[0361] Example 31. Preparation of aluminum sesquichlorohydrate clay heteroadduct (1.52 mmol Al / g clay) While stirring, 30 g of HPM-20 clay was slowly added over 1-2 minutes to a Waring® blender containing 570 g of deionized Milli-Q® water and stirred at low speed to obtain a gray colloidal dispersion that was free or substantially free of visible lumps or clumps. After addition was complete, the dispersion was blended at high speed for 5-10 minutes to obtain a slightly viscous mixture of a 5 wt% aqueous dispersion of HPM-20 clay.
[0362] A 100 g portion of this 5 wt% HPM-20 clay aqueous dispersion was transferred to a Waring® blender. A 1.30 g sample of ALOXICOLL® 31L solution was weighed into a vial and added to the dispersion along with enough deionized Milli-Q® water to facilitate stirring. The mixture was then blended at high speed for 5 minutes, and the conductivity was measured (Eutech PCSTestr 35), yielding a conductivity of 2600 μS / cm. The mixture was then vacuum filtered through Fisherbrand™ P8 qualitative grade filter paper and briefly washed with 100 mL of deionized Milli-Q® water. After 15-30 minutes of filtration, a portion of the remaining wet solid was resuspended in 50-100 mL of water and the conductivity was measured again; typical conductivities ranged from 100 μS / cm to 500 μS / cm (in this case, the conductivity was 70 μS / cm). The suspension was then combined with 100–200 mL of 1-butanol and rotary evaporated at 45° C. The solid was then crushed with a pestle and mortar to obtain 6.2 g of a gray powder, and 1.8 g of this solid was then transferred to a porcelain crucible and calcined at 300° C. for 6 h to obtain 0.9 g of a gray-black powder.
[0363] Example 32. Comparative Example of the Preparation of Aluminum Sesquichlorohydrate Clay Heteroadduct (2.5 mmol Al / g Clay) While stirring, 30 g of HPM-20 clay was slowly added over 1-2 minutes to a Waring® blender containing 570 g of deionized Milli-Q® water and stirred at low speed to obtain a gray colloidal dispersion that was free or substantially free of visible lumps or clumps. After addition was complete, the dispersion was blended at high speed for 5-10 minutes to obtain a slightly viscous mixture of a 5 wt% aqueous dispersion of HPM-20 clay.
[0364] A 100 g portion of this 5 wt% HPM-20 clay aqueous dispersion was transferred to a Waring® blender. A 2.79 g sample of ALOXICOLL® 31L solution was weighed into a vial and added to the dispersion along with enough deionized Milli-Q® water to facilitate stirring. The mixture was then blended at high speed for 5 minutes, and the conductivity was measured (Eutech PCSTestr 35), yielding a conductivity of 2800 μS / cm. The mixture was then vacuum filtered through Fisherbrand™ P8 qualitative grade filter paper and briefly washed with 100 mL of deionized Milli-Q® water. After 15-30 minutes of filtration, a portion of the remaining wet solid was resuspended in 50-100 mL or water, and the conductivity was measured again (320 μS / cm), with typical conductivities in the 100-500 μS / cm range. This suspension was then combined with 100–200 mL of 1-butanol and rotary evaporated at 45° C. The solid was then crushed with a pestle and mortar to obtain 5.57 g of a gray powder, and 1.7 g of this solid was then transferred to a porcelain crucible and calcined at 300° C. for 6 hours to obtain 1 g of a gray-black powder.
[0365] Example 33. Comparative Example of Preparation of Polyaluminum Chloride (PAC)-Clay Heteroadduct (0.5 mmol Al / g Clay) A 177.28 gram sample of a 5.0 wt. % Volclay® HPM-20 suspension prepared according to the procedure of Example 4 was loaded into a Waring® blender. While stirring, 1.32 g of UltraPAC® 290 solution (GEO) was added to the HPM-20 clay slurry, followed by stirring at elevated temperature for 9 minutes. The gray heteroadduct viscous mass was then transferred in two portions to an HDPE poly bottle along with 210 grams of deionized water. The gray heteroadduct slurry was then shaken by hand for approximately 1 minute, resulting in a pH of 4.31 and a conductivity of 1672 μS / cm. The slurry was filtered through Fisherbrand® P8 coarse filter paper, resulting in a 28.03 g wet cake, which was transferred to an HDPE bottle and then charged with 308 g of deionized water. The bottle was shaken to eliminate lumps in the slurry, and the pH was 4.76 and the conductivity was 200 μS / cm. The slurry was filtered through Fisherbrand™ P8 filter paper to yield 22.30 g of wet cake, which was transferred to an Erlenmeyer with a stir bar along with 200 mL of n-butanol and stirred until the clamps were no longer visible. The stir bar was removed, and the mixture was rotary evaporated from a 45°C bath to yield 9.49 g of an off-white powder that was lightly ground to a fine powder using a mortar and pestle. 1.10 grams of the off-white powder was charged into a porcelain crucible and then into a 300°C oven and fired for 6 hours to yield 0.8960 grams of a dark gray powder. The powder was cooled to ambient temperature under vacuum and then transferred to an inert atmosphere glove box.
[0366] Example 34. Preparation of polyaluminum chloride (PAC)-clay heteroadduct (1.01 mmol Al / g clay) A 201.23 gram sample of the 5.0 wt. % HPM-20 clay suspension prepared in Example 4 was loaded into a Waring® blender. While stirring, 3.036 g of UltraPAC® 290 solution (GEO) was added to the HPM-20 slurry. The resulting thick mass could not be agitated by the Waring® blender and was transferred to an HDPE bottle with two crushes of deionized water totaling 185 g. The bottle was shaken by hand to eliminate any visible clumps or lumps. The resulting slurry had a pH of 3.8 and a conductivity of 26 mS / cm. The slurry was filtered through Fisherbrand® coarse filter paper No. 8, and the clear filtrate yielded a conductivity of 5.2 mS / cm. A 61 g portion of the filter cake was then transferred to the original polymer bottle and resuspended in 328 g of deionized water by shaking until no lumps were visible. The resulting conductivity was 1116 μS / cm and pH was 3.93. The slurry was then filtered through Fisherbrand™ P8 filter paper. The clear filtrate had a conductivity of 1200 μS / cm. A 9.95 g sample of the filter cake was transferred to an Erlenmeyer flask. The remaining filter cake was resuspended in 281 g of deionized water in a new HDPE bottle with shaking, resulting in a slurry with a pH of 4.11 and a conductivity of 150 μS / cm. After standing overnight, the slurry was filtered through Fisherbrand™ P8 paper and 18.25 g of filter cake was transferred to an Erlenmeyer flask along with 100 mL of n-butanol. The flask was shaken to break up chunks, then rotary evaporated from a 40°C bath to yield 9.08 g of an off-white powder. A 2.384 g sample of the off-white powder was charged into a porcelain crucible and placed in a 300°C oven for 6 hours, yielding 1.72 g of a gray powder, which was placed under vacuum to cool to ambient temperature and then placed in an inert atmosphere glove box.
[0367] Example 35. Comparative Example of Preparation of Polyaluminum Chloride (PAC)-Clay Heteroadduct (1.46 mmol Al / g Clay) A 199.31 g sample of the 5.0 wt % HPM-20 clay suspension prepared in Example 4 was loaded into a Waring® blender. While stirring, 4.36 g of GEO Specialty Chemicals' UltraPAC® 290 solution was added to the HPM-20 clay slurry. The flask was removed from the blender and swirled using the blender until the viscous gray mass could be agitated, followed by vigorous stirring for 9 minutes. The viscous mass was then poured into an HDPE polymer bottle along with two portions of 85 grams of deionized water to yield a total of 275 g of gray heteroadduct slurry, which was then shaken by hand for approximately 1 minute, resulting in a slurry pH of 3.73 and a conductivity of 6.79 mS / cm. The slurry was filtered through Fisherbrand® P8 coarse filter paper, and the filter cake was subsequently resuspended in approximately 200 mL of deionized water to yield a slurry conductivity of 1 mS / cm. The slurry was filtered, and a 34 g portion of the filter cake was transferred to a 500 mL Erlenmeyer tube with a stir bar along with 200 mL of n-butanol. The mixture was stirred overnight to break up any solid clumps. The stir bar was then removed, and the mixture was rotary evaporated from a 45 °C bath to yield 10.78 g of an off-white powder that was lightly ground to a fine powder using a mortar and pestle. A 1.07 g portio...
Claims
1. 1. A support activator comprising an isolated smectite heteroadduct, the smectite heteroadduct comprising the contact product in a liquid carrier of: (1) a colloidal smectite clay; and (2) a heterocoagulation reagent, the heterocoagulation reagent being at least one cationic polymetallate, in an amount sufficient to provide a slurry of the smectite heteroadduct having a zeta potential, as quantified from an electrokinetic sonic amplitude (ESA) effect, in the range of positive (+) 25 mV (millivolts) to negative (-) 25 mV.
2. 2. The support activator of claim 1, wherein the smectite clay comprises montmorillonite, sauconite, nontronite, hectorite, beidellite, saponite, bentonite, or any combination thereof.
3. 2. The support activator of claim 1, wherein the cationic polymetalate comprises a cationic polyaluminate selected from polyaluminum chloride, aluminum chlorohydrate, aluminum sesquichlorohydrate, or polyaluminum oxyhydroxychloride, or any combination thereof.
4. 2. The support activator of claim 1, wherein the cationic polymetallate comprises a cationic polyaluminate selected from polyaluminum chloride, aluminum chlorohydrate, aluminum sesquichlorohydrate, polyaluminum oxyhydroxychloride, or any combination thereof, and the ratio of millimoles (mmol) of aluminum (Al) in the cationic polyaluminate to grams (g) of colloidal smectite clay is in the range of 0.2 mmol Al / g clay to 2.5 mmol Al / g clay.
5. 2. The support activator of claim 1, wherein the cationic polymetallate comprises a chemically-treated first metal oxide with a second metal oxide, a metal halide, a metal oxyhalide, or a combination thereof, in an amount sufficient to provide a colloidal suspension of the chemically-treated first metal oxide having a zeta potential greater than positive (+) 20 mV (millivolts).
6. 2. The support activator of claim 1, wherein the cationic polymetallate comprises fumed silica, fumed alumina, fumed silica-alumina, fumed magnesia, fumed zinc oxide, fumed titania, fumed zirconia, fumed ceria, or any combination thereof, that is chemically treated with polyaluminum chloride, aluminum chlorhydrate, aluminum sesquichlorohydrate, polyaluminum oxyhydroxychloride, or any combination thereof.
7. 2. The support activator of claim 1, wherein the slurry of the smectite heteroadduct is characterized by a conductivity in the range of 2 mS / cm to 10 μS / cm when the concentration of the slurry is in the range of 1 wt % to 10 wt % solids (as measured using a Eutech PCS Testr 35), and the isolated smectite heteroadduct is calcined.
8. The smectite heteroadduct is calcined and has a BJH porosity in the range of 0.2 cc / g to 3.0 cc / g and a total cumulative pore volume (V 3-30nm ) is less than 55% of the total cumulative pore volume (V 3-10nm 2. The support activator of claim 1, wherein
9. 2. The support activator of claim 1, wherein the colloidal smectite clay and the heterocoagulation reagent are contacted in an amount sufficient to provide a slurry of the smectite heteroadduct having a zeta potential in the range of positive (+) 20 mV (millivolts) to negative (-) 20 mV.
10. 2. The support activator of claim 1, wherein the colloidal smectite clay and the heterocoagulation reagent are contacted in amounts sufficient to provide a slurry of the smectite heteroadduct having a zeta potential in the range of positive (+) 15 mV (millivolts) to negative (-) 15 mV.
11. 2. The support activator of claim 1, wherein the smectite heteroadduct is isolated from the slurry by filtration without the use of ultrafiltration, centrifugation, or a settling tank, and the isolated smectite heteroadduct is [1] optionally washed with water, and [2] dried and / or calcined.
12. Providing a slurry of said smectite heteroadduct having the following filtration behavior: (a) when filtering a 2.0 wt. % aqueous slurry of said smectite hetero-adduct within a time period of 0 to 2 hours after contacting step b), the percentage of filtrate obtained in a 10 minute filtration time using either vacuum filtration or gravity filtration, based on the weight of said liquid carrier in said smectite hetero-adduct slurry, is in the range of 50% to 100% by weight of said liquid carrier in said slurry before filtration; (b) the filtrate from the smectite heteroadduct slurry, when evaporated, yields solids that constitute less than 20% of the initial combined weight of clay and heteroadhesive coagulant.
13. A catalyst composition for olefin polymerization comprising: a) at least one metallocene compound; b) optionally at least one cocatalyst; c) at least one supported activator comprising a calcined smectite heteroadduct, said calcined smectite heteroadduct comprising the contact product of (1) a colloidal smectite clay and (2) a heterocoagulation reagent which is at least one cationic polymetallate in a liquid carrier and in an amount sufficient to provide a slurry of said calcined smectite heteroadduct having a zeta potential in the range of positive (+) 25 mV (millivolts) to negative (-) 25 mV, as quantified from the electrokinetic sonic amplitude (ESA) effect.
14. The at least one metallocene compound has the formula: (X 1 )(X 2 )(X 3 )(X 4 )M(where, a) M is selected from titanium, zirconium, or hafnium; b) X 1 is selected from substituted or unsubstituted cyclopentadienyl, indenyl, fluorenyl, pentadienyl, allyl, boratabenzenyl, 1,2-azaborolyl, or 1,2-diaza-3,5-diborolyl, and the optional substituents are halide, C 1 -C 20 Hydrocarbyl, C 1 -C 20 Heterohydrocarbyl, C 1 -C 20 Organoheteryl, condensed C 4 -C 12 a carbocyclic moiety or a fused C having at least one heteroatom independently selected from nitrogen, oxygen, sulfur, or phosphorus; 4 -C 11 are independently selected from heterocyclic moieties, c) X 2 is selected from [1] substituted or unsubstituted cyclopentadienyl, indenyl, fluorenyl, pentadienyl, or allyl, and any of the optional substituents is selected from halide, C 1 -C 20 Hydrocarbyl, C 1 -C 20 Heterohydrocarbyl, or C 1 -C 20 or [2] a halide, a hydride, C 1 -C 20 Hydrocarbyl, C 1 -C 20 Heterohydrocarbyl, C 1 -C 20 Organoheteryl, condensed C 4 -C 12 a carbocyclic moiety or a fused C having at least one heteroatom independently selected from nitrogen, oxygen, sulfur, or phosphorus; 4 -C 11 heterocyclic moiety; d) X 1 and X 2 is optionally bridged by at least one linker substituent having 2-4 bridging atoms independently selected from C, Si, N, P, or B, each available non-bridging valence of each bridging atom being unsubstituted (bonded to H) or substituted, and any substituent being selected from halide, C 1 -C 20 Hydrocarbyl, C 1 -C 20 Heterohydrocarbyl, or C 1 -C 20 and any hydrocarbyl, heterohydrocarbyl, or organoheteryl substituent is independently selected from the group consisting of bridging atoms and X. 1 Or X 2 and can form a saturated or unsaturated cyclic structure, e) [1]X 3 and X 4 However, halides, hydrides, C 1 -C 20 Hydrocarbyl, C 1 -C 20 Heterohydrocarbyl, or C 1 -C 20 [2] [GX A k X B 4-k ] - wherein G is B or Al, k is a number from 1 to 4, and X A is independently selected from H or a halide; X B But, C 1 -C 12 Hydrocarbyl, C 1 -C 12 Heterohydrocarbyl, C 1 -C 12 and [3] X is independently selected from organoheteryl. 3 and X 4 But together C 4 -C 20 or [4]X 3 and X 4 M is unsubstituted or unsubstituted, saturated or unsaturated C 3 -C 6 forming a metallacycle moiety, wherein any substituent on said metallacycle moiety is a halide, C 1 -C 20 Hydrocarbyl, C 1 -C 20 Heterohydrocarbyl, or C 1 -C 20 14. The catalyst composition of claim 13, wherein the aryl group is independently selected from organoheteryls.
15. X 1 and X 2 but, a) >EX 5 2 , -EX 5 2 EX 5 2 -, -EX 5 2 EX 5 EX 5 2 - or >C=CX 5 2 wherein E at each occurrence is independently selected from C or Si; b) -BX 5 -, -NX 5 - or -PX 5 ,or c)[-SiX 5 2 (1,2-C 6 H 4 )SiX 5 2 -]、[-CX 5 2 (1,2-C 6 H 4 )CX 5 2 -]、[-SiX 5 2 (1,2-C 6 H 4 )CX 5 2 -]、 [-SiX 5 2 (1,2-C 2 H 2 ) SiX 5 2 -], [-CX 5 2 (1,2-C 6 H 4 ) C.X. 5 2 -] or [-SiX 5 2 (1,2-C 6 H 4 ) C.X. 5 2 -] (wherein X in each occurrence 5 H, halide, C 1 -C 20 Hydrocarbyl, C 1 -C 20 Heterohydrocarbyl, or C 1 -C 20 independently selected from organoheteryl, Any X selected from hydrocarbyl, heterohydrocarbyl, or organoheteryl substituents; 5 The substituent is a bridging atom, another X 5 Substituent, X 1 , or X 2 14. The catalyst composition of claim 13, wherein the linker substituents are selected from the group consisting of:
16. 14. The catalyst composition of claim 13, wherein the cocatalyst comprises an alkylating agent, a hydrogenating agent, or a silylating agent.
17. 14. The catalyst composition of claim 13, wherein the co-catalyst comprises an organoaluminum compound, an organoboron compound, an organozinc compound, an organomagnesium compound, an organolithium compound, or any combination thereof.
18. 1. A process for the polymerization of olefins comprising contacting at least one olefin monomer and a catalyst composition under polymerization conditions to form a polyolefin, said catalyst composition comprising: a) at least one metallocene compound; b) optionally at least one cocatalyst; c) a process for the polymerization of olefins comprising at least one supported activator comprising a calcined smectite heteroadduct, the calcined smectite heteroadduct comprising the contact product of: (1) a colloidal smectite clay; and (2) a heterocoagulation reagent which is at least one cationic polymetallate in a liquid carrier and in a sufficient amount to provide a slurry of the calcined smectite heteroadduct having a zeta potential in the range of positive 25 (+) mV (millivolts) to negative (-) 25 mV, as quantified from an electrokinetic sonic amplitude (ESA) effect.
19. 20. The process for polymerization of olefins according to claim 18, wherein the at least one olefin monomer is selected from [a] ethylene or propylene, or [b] ethylene in combination with at least one comonomer selected from propylene, 1-butene, 2-butene, 3-methyl-1-butene, 1-pentene, 2-pentene, 3-methyl-1-pentene, 4-methyl-1-pentene, 1-hexene, 3-ethyl-1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1,3-butadiene, isoprene, piperylene, 2,3-dimethyl-1,3-butadiene, 1,4-pentadiene, 1,7-hexadiene, vinylcyclohexane, or any combination thereof.
20. 20. The process for the polymerization of olefins according to claim 18, wherein the polymerization process comprises polymerization in a gas phase reactor, a slurry loop, dual slurry loops in series, multiple slurry tanks in series, a slurry loop in combination with a gas phase reactor, a continuously stirred reactor in a batch process, or a combination thereof.
21. 1. A method for producing a support activator, the method comprising the steps of: a) providing a colloidal smectite clay; b) contacting the colloidal smectite clay with a heterocoagulation reagent in a liquid carrier in an amount sufficient to provide a slurry of smectite heteroadducts, the heteroadduct being at least one cationic polymetallate and having a zeta potential, as quantified from an electrosonic amplitude (ESA) effect, in the range of positive (+) 25 mV (millivolts) to negative (-) 25 mV; c) isolating said smectite heteroadduct from said slurry.
22. 22. The method of claim 21, wherein the colloidal smectite clay and the heterocoagulation reagent are contacted in amounts sufficient to provide a slurry of smectite heteroadducts having a zeta potential in the range of positive (+) 20 mV (millivolts) to negative (-) 20 mV.
23. 22. The method of claim 21, wherein the colloidal smectite clay and the heterocoagulation reagent are contacted in amounts sufficient to provide a slurry of smectite heteroadducts having a zeta potential in the range of positive (+) 15 mV (millivolts) to negative (-) 15 mV.
24. The support activator of claim 1, wherein the liquid carrier comprises water, an alcohol, an ether, a ketone, an ester, or any combination thereof.
25. The support activator of claim 1, wherein the liquid carrier comprises a surfactant.
26. The support activator of claim 1, wherein the liquid carrier comprises an anionic surfactant, a cationic surfactant, or a nonionic surfactant.
27. The support activator of claim 26, wherein the anionic surfactant is selected from sulfates, sulfonates, phosphates, carboxylates, dialkylsulfocarboxylates, alkylarylsulfonates, alkylsulfonates, sulfosuccinates, alkali metal salts of fatty acids, polycarboxylates, polyoxyethylene alkyl ether phosphate esters, or alkylnaphthalenesulfonates, and unless otherwise specified, each salt contains a cation selected from alkali metals, alkaline earth metals, ammonium, or hydrocarbyl ammonium.
28. The support activator of claim 26, wherein the cationic surfactant is selected from a primary amine, a secondary amine, or a tertiary amine, or a primary ammonium compound, a secondary ammonium compound, a tertiary ammonium compound, or a quaternary ammonium compound.
29. The support activator of claim 26, wherein the nonionic surfactant is selected from an ethoxylate, a glycol ether, a fatty alcohol polyglycol ether, or a combination thereof.
30. The catalyst composition of claim 13, wherein the liquid carrier comprises water, an alcohol, an ether, a ketone, an ester, or any combination thereof.
31. The catalyst composition of claim 13, wherein the liquid carrier comprises a surfactant.
32. The catalyst composition of claim 13, wherein the liquid carrier comprises an anionic surfactant, a cationic surfactant, or a nonionic surfactant.
33. The catalyst composition of claim 32, wherein the anionic surfactant is selected from sulfates, sulfonates, phosphates, carboxylates, dialkylsulfocarboxylates, alkylarylsulfonates, alkylsulfonates, sulfosuccinates, alkali metal salts of fatty acids, polycarboxylates, polyoxyethylene alkyl ether phosphate esters, or alkylnaphthalenesulfonates, and unless otherwise specified, each salt contains a cation selected from alkali metals, alkaline earth metals, ammonium, or hydrocarbylammonium.
34. The catalyst composition of claim 32, wherein the cationic surfactant is selected from a primary amine, a secondary amine, or a tertiary amine, or a primary ammonium compound, a secondary ammonium compound, a tertiary ammonium compound, or a quaternary ammonium compound.
35. The catalyst composition of claim 32, wherein the nonionic surfactant is selected from an ethoxylate, a glycol ether, a fatty alcohol polyglycol ether, or a combination thereof.
36. The process for polymerizing olefins as described in claim 18, wherein the liquid carrier comprises water, an alcohol, an ether, a ketone, an ester, or any combination thereof.
37. The process for polymerizing olefins as described in claim 18, wherein the liquid carrier comprises a surfactant.
38. The olefin polymerization process of claim 18, wherein the liquid carrier comprises an anionic surfactant, a cationic surfactant, or a nonionic surfactant.
39. The process for polymerizing olefins according to claim 38, wherein the anionic surfactant is selected from sulfates, sulfonates, phosphates, carboxylates, dialkylsulfocarboxylates, alkylarylsulfonates, alkylsulfonates, sulfosuccinates, alkali metal salts of fatty acids, polycarboxylates, polyoxyethylene alkyl ether phosphates, or alkylnaphthalenesulfonates, and unless otherwise specified, each salt contains a cation selected from alkali metals, alkaline earth metals, ammonium, or hydrocarbylammonium.
40. The process for polymerization of olefins described in claim 38, wherein the cationic surfactant is selected from a primary amine, a secondary amine, or a tertiary amine, or a primary ammonium compound, a secondary ammonium compound, a tertiary ammonium compound, or a quaternary ammonium compound.
41. The process for polymerization of olefins described in claim 38, wherein the nonionic surfactant is selected from an ethoxylate, a glycol ether, a fatty alcohol polyglycol ether, or a combination thereof.
Citation Information
Patent Citations
Molecular sieve catalyst composition, its manufacture, and its use in conversion methods
JP2004537398A
Highly-concentrated bentonite water dispersion
JP2018111613A
Process for producing modified clays, produced modified clays and uses thereof
JP2018520078A
Process for producing modified clays, supported metallocene polymerization catalysts, produced catalysts and uses thereof
JP2018520225A