Surface-treated steel foil for current collector and its manufacturing method

JP7578802B2Active Publication Date: 2024-11-06TOYO KOHAN CO LTD
5 Cites 0 Cited by

Patent Information

Application Number
JP2023517638
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-04-28
Filing Date
2022-04-28
Publication Date
2024-11-06
Estimated Expiration
2042-04-28

AI Technical Summary

Technical Problem

Bipolar batteries experience performance deterioration due to hydrogen permeation through the metal material used as a current collector, which affects the battery's hydrogen storage alloys, leading to voltage drops and gradual performance decline.

Method used

A surface-treated steel foil for current collectors is developed with an iron-nickel alloy layer on at least one side, having a thickness of 0.5 μm or more, to suppress hydrogen permeation and enhance electrolyte resistance, which includes a nickel layer and optional roughened nickel layer for improved adhesion and conductivity.

Benefits of technology

The surface-treated steel foil effectively suppresses hydrogen permeation, maintaining battery performance and preventing voltage drops, making it suitable for bipolar batteries and other hydrogen-containing battery environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578802000004
    Figure 0007578802000004
  • Figure 0007578802000005
    Figure 0007578802000005
  • Figure 0007578802000006
    Figure 0007578802000006
Patent Text Reader

Abstract

[Problem] To provide a surface treated steel foil which is for a current collector and which has hydrogen barrier properties suitable for a battery using a hydrogen occluding alloy. [Solution] This surface treated steel foil is for a current collector and has a first surface on which a hydrogen occluding alloy is disposed and a second surface positioned on the side opposite to the first surface. The surface treated steel foil is characterized by having nickel-iron alloy layers that are laminated on the first-surface side and / or the second-surface side on the side opposite to the first surface of a metal base material composed of steel foil and that minimize penetration or diffusion of hydrogen within said surface treated steel foil for a current collector, and is characterized in that at least one of the nickel-iron alloy layers has a thickness of at least 0.5 μm.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a surface-treated steel foil that is particularly suitable for use as a current collector for secondary batteries and the like, and a method for producing the same. [Background technology]

[0002] Conventionally, nickel-metal hydride batteries and lithium-ion batteries are known as secondary batteries that are used for in-vehicle applications, etc. Known types of electrode structures for these secondary batteries include monopolar electrodes in which a positive electrode layer or a negative electrode layer is formed on both sides of a current collector, and bipolar electrodes in which a positive electrode layer (positive electrode active material layer) and a negative electrode layer (negative electrode active material layer) are formed on both sides of a current collector.

[0003] A bipolar battery is constructed by stacking the bipolar electrodes described above with an electrolyte, a separator, etc., and housing them in a single battery case. This configuration allows the electrodes to be stacked in a series circuit, which is known to reduce the internal resistance of the battery and make it easier to increase the operating voltage and output. In addition to the battery performance, it is believed that the battery volume and weight can be reduced by omitting or reducing the number of components such as leads for extracting current through battery design compared to conventional batteries using monopolar electrodes, thereby improving the volume and weight energy density of the battery. For example, Patent Document 1 listed below discloses the use of a metal foil such as a nickel foil as a current collector for a bipolar battery. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2020-053401 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present inventors have been working hard to improve battery characteristics while promoting development of a metal foil such as a steel foil as a suitable metal material for a current collector, and have found that deterioration of battery performance can be reduced by suppressing hydrogen permeation through the metal material used as the current collector.

[0006] For example, in nickel-metal hydride batteries, hydrogen is used as the active material of the negative electrode, generally a hydrogen storage alloy. In the case of a conventional monopolar electrode, it was sufficient for the surface to have electrolyte resistance according to the type of battery, but in the case of the bipolar electrode described above, the phenomenon that hydrogen present on the negative electrode side moves through the metal material and permeates to the positive electrode side is likely to occur, and when such a permeation phenomenon occurs, the battery performance is likely to decrease.

[0007] The present invention has been made in consideration of solving such problems, and has an object to provide a surface-treated steel foil for a current collector that combines the hydrogen barrier property (performance of suppressing hydrogen permeation) required for bipolar batteries and the electrolyte resistance and other properties required for secondary batteries. [Means for solving the problem]

[0008] In order to solve the above-mentioned problems, a surface-treated steel foil for a current collector in one embodiment of the present invention is: (1) a surface-treated steel foil for a current collector having a first surface on which a hydrogen storage alloy is disposed and a second surface located opposite to the first surface, the surface-treated steel foil having an iron-nickel alloy layer laminated on at least one of the first surface side and the second surface side opposite to the first surface side of a metal base made of a steel foil, the iron-nickel alloy layer suppressing permeation or diffusion of hydrogen in the surface-treated steel foil for a current collector; the iron-nickel alloy layer is in a range between 2 / 10 of the maximum X-ray intensity of nickel and iron when a quantitative analysis of nickel and iron is performed in a thickness direction from a surface layer side of the first surface or the second surface in an analysis of a cross section of the surface-treated steel foil for a current collector by energy dispersive X-ray spectroscopy, At least one of the iron-nickel alloy layers has a thickness of 0.5 μm or more.

[0009] In the surface-treated steel foil for a current collector described in the above-mentioned (1), (2) it is preferable that an iron-nickel alloy layer is formed on both the first surface and the second surface of the surface-treated steel foil for a current collector, and the total thickness of the iron-nickel alloy layer on both surfaces is 0.7 μm or more.

[0010] In the surface-treated steel foil for a current collector of the above (1) or (2), (3) the metal substrate is preferably low carbon steel or ultra-low carbon steel.

[0011] In any one of the above surface-treated steel foils for current collectors (1) to (3), (4) the amount of nickel deposited in the iron-nickel alloy layer is 0.80 g / m 2 ~53.4g / m 2 It is preferable that:

[0012] In any one of the above surface-treated steel foils for current collectors (1) to (4), (5) it is preferable that the surface-treated steel foil for current collectors further comprises a metal layer formed on the iron-nickel alloy layer, and the metal layer is a nickel layer.

[0013] In the surface-treated steel foil for a current collector according to the above (5), (6) the metal layer is a nickel layer, and the total amount of nickel coating in the iron-nickel alloy layer and the nickel layer is 2.0 g / m 2 ~53.4g / m 2 It is preferable that:

[0014] In any one of the surface-treated steel foils for current collectors described above in (1) to (6), (7) a hydrogen permeation current density measured electrochemically is 20 μA / cm 2 Here, the hydrogen permeation current density is defined as the increase in oxidation current measured on the hydrogen detection side when a potential of -1.5 V is applied to the hydrogen generation side in an electrolyte at 65°C under the condition that the potential on the hydrogen detection side is +0.4 V. The reference electrodes for the potentials on the hydrogen detection side and hydrogen generation side are Ag / AgCl.

[0015] In any one of the above surface-treated steel foils for current collectors (1) to (7), (8) it is preferable that a roughened nickel layer is formed on the outermost surface of either the first surface side or the second surface side, and that the roughened nickel layer has a three-dimensional surface texture parameter Sa of 0.2 μm to 1.3 μm. Effect of the Invention

[0018] According to the present invention, it is possible to provide a surface-treated steel foil for a current collector that has both hydrogen barrier properties suitable for bipolar batteries and electrolyte resistance and other properties required for secondary batteries. [Brief description of the drawings]

[0019] [Figure 1(a)] FIG. 1 is a diagram illustrating a surface-treated steel foil for a current collector according to the present embodiment. [Figure 1(b)] FIG. 1 is a diagram illustrating a surface-treated steel foil for a current collector according to the present embodiment. [Figure 1(c)] FIG. 1 is a diagram showing a schematic diagram of a surface-treated steel foil for a current collector according to the present embodiment. [Figure 2(a)] FIG. 1 is a schematic diagram of an apparatus for measuring the hydrogen barrier property of the surface-treated steel foil 10 for a current collector of the present embodiment. [Figure 2(b)] FIG. 1 is a schematic diagram of an apparatus for measuring the hydrogen barrier property of the surface-treated steel foil 10 for a current collector of the present embodiment. [Figure 2(c)] FIG. 2 is an explanatory diagram of a method for measuring the hydrogen barrier property of the surface-treated steel foil 10 for a current collector of the present embodiment. [Figure 2(d)] FIG. 2 is an explanatory diagram of a method for measuring the hydrogen barrier property of the surface-treated steel foil 10 for a current collector of the present embodiment. [Figure 2(e)] FIG. 2 is an explanatory diagram of a method for measuring the hydrogen barrier property of the surface-treated steel foil 10 for a current collector of the present embodiment. [Diagram 3] FIG. 4 is a diagram for explaining a method for calculating the thickness of an iron-nickel alloy layer in the present embodiment. [Figure 4] FIG. 2 is a schematic diagram showing a surface-treated steel foil for a current collector according to another embodiment. [Figure 5(a)] FIG. 2 is a schematic diagram showing a surface-treated steel foil for a current collector according to another embodiment. [Figure 5(b)] FIG. 2 is a schematic diagram showing a surface-treated steel foil for a current collector according to another embodiment. [Figure 6] FIG. 2 is a schematic diagram showing a surface-treated steel foil for a current collector according to another embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] <Surface-treated steel foil for current collectors 10> Hereinafter, an embodiment for carrying out the surface-treated steel foil for a current collector of the present invention will be described. Fig. 1 is a schematic diagram showing one embodiment of a surface-treated steel foil 10 for a current collector of the present invention. The surface-treated steel foil 10 for a current collector of this embodiment can be used as a current collector for a bipolar battery, and can also be used as a current collector for a positive or negative electrode of a monopolar battery. The type of battery may be a secondary battery or a primary battery.

[0021] The surface-treated steel foil 10 for a current collector of this embodiment has a metal substrate 20 and an iron-nickel alloy layer 30. The surface-treated steel foil 10 for a current collector has a first surface 10a and a second surface 10b opposite to the first surface. A hydrogen storage alloy is disposed on the first surface 10a as a negative electrode material when assembled into a battery. On the other hand, in the case of a nickel-metal hydride battery with a bipolar electrode structure, for example, a positive electrode material is disposed on the second surface 10b.

[0022] The surface-treated steel foil 10 for a current collector of this embodiment is characterized by having an iron-nickel alloy layer 30 as described above. The iron-nickel alloy layer 30 may be disposed on the second surface 10b side as shown in Fig. 1(a), or may be disposed on either the first surface 10a side as shown in Fig. 1(b). Also, it may be disposed on both the first surface 10a side and the second surface 10b side as shown in Fig. 1(c). The iron-nickel alloy layer 30 may be disposed on the outermost surface of the surface-treated steel foil 10 for a current collector as shown in Figs. 1(a) to (c), or may be disposed inside (in the middle) of the surface-treated steel foil 10 for a current collector as shown in Fig. 4. The iron-nickel alloy layer 30 has a function of suppressing the permeation or diffusion of hydrogen within the surface-treated steel foil for current collector.

[0023] <Regarding the metal substrate 20> The steel foil of the metal substrate 20 used in the surface-treated steel foil 10 for current collector of this embodiment is preferably an iron-based metal substrate containing less than 1.0 wt% of Cr and other added metal elements. Specifically, low carbon steel (carbon content 0.01 to 0.15 wt%) such as low carbon aluminum-killed steel, ultra-low carbon steel with a carbon content of less than 0.01 wt%, or non-aging ultra-low carbon steel obtained by adding Ti, Nb, etc. to ultra-low carbon steel are preferably used.

[0024] The thickness of the metal substrate 20 used in the surface-treated steel foil 10 for current collector of this embodiment is preferably in the range of 0.01 mm to 0.5 mm. When used as a current collector for a battery that places importance on volumetric and weight energy density, the thickness is more preferably 0.01 mm to 0.3 mm, and even more preferably 0.025 mm to 0.1 mm, from the viewpoints of strength and desired battery capacity. The thickness of the metal substrate 20 is preferably measured by cross-sectional observation using an optical microscope or a scanning electron microscope (SEM). Furthermore, thickness measurement using a micrometer or the like can be used to measure the thickness before surface treatment, i.e., before nickel plating or iron-nickel alloy plating. Although a rolled steel foil is usually used for the metal substrate 20, it may be an electrolytic iron foil produced by electrolytic plating.

[0025] <About the iron-nickel alloy layer 30> The iron-nickel alloy layer 30 included in the surface-treated steel foil 10 for current collector of this embodiment is an alloy layer containing iron (Fe) and nickel (Ni), that is, a metal layer containing an alloy of iron and nickel (also referred to as "iron-nickel alloy" or "Fe-Ni alloy"). The state of the alloy of iron and nickel may be any one of a solid solution, a eutectoid / eutectic, or a compound (intermetallic compound), or they may coexist.

[0026] The iron-nickel alloy layer 30 included in the surface-treated steel foil 10 for current collector of this embodiment may contain other metal elements and inevitable impurities as long as the object of the present invention can be solved. For example, the iron-nickel alloy layer 30 may contain metal elements such as cobalt (Co) and molybdenum (Mo) and additive elements such as boron (B). The ratio of metal elements other than iron (Fe) and nickel (Ni) in the iron-nickel alloy layer 30 is preferably 10% by weight or less, more preferably 5% by weight or less, and even more preferably 1% by weight or less. Since the iron-nickel alloy layer 30 may be a binary alloy substantially composed of only iron and nickel, the lower limit of the content ratio of other metal elements except inevitable impurities is 0%. The types and amounts of other metal elements contained can be measured by known means such as an X-ray fluorescence (XRF) measuring device or GDS (glow discharge optical emission surface spectroscopy).

[0027] The iron-nickel alloy layer 30 contained in the surface-treated steel foil 10 for current collector of this embodiment is preferably formed by plating or a method involving plating and heat treatment, and examples of plating include electrolytic plating, electroless plating, hot-dip plating, dry plating, etc. Among these, electrolytic plating is particularly preferred from the viewpoints of cost, film thickness control, etc.

[0028] For example, there may be mentioned a method in which a Ni plating layer is formed on at least one surface of the metal base material 20 by a method such as electrolytic plating, and then iron (Fe) and nickel (Ni) in the metal base material 20 are diffused and alloyed by a thermal diffusion treatment or the like, or a method in which an alloy layer is formed by FeNi alloy plating. Details of these manufacturing methods will be described later.

[0029] Next, the hydrogen barrier property of the iron-nickel alloy layer 30 contained in the surface-treated steel foil 10 for a current collector of this embodiment will be described.

[0030] In the course of repeated experiments to improve battery performance, the inventors discovered that the phenomenon of voltage drop (self-discharge) of unknown causes occurs, and that suppressing hydrogen permeation through the surface-treated steel foil 10 for a current collector is effective in eliminating this phenomenon. The cause of hydrogen permeation and the reason why the suppression of hydrogen permeation in the surface-treated steel foil 10 for a current collector can suppress the occurrence of the above-mentioned voltage drop (self-discharge) phenomenon are still unclear, but the inventors make the following prediction.

[0031] That is, in this embodiment, when the surface-treated steel foil 10 for a current collector is used as an electrode of a bipolar battery, a hydrogen storage alloy used as a negative electrode material is disposed on at least one side of the surface-treated steel foil 10 for a current collector, and a positive electrode material is disposed on the opposite side. In this case, a hydrogen-rich environment (negative electrode) and a hydrogen-poor environment (positive electrode) exist on either side of the surface-treated steel foil 10 for a current collector, and a hydrogen concentration gradient occurs. It was expected that hydrogen would permeate and move through the surface-treated steel foil 10 for a current collector due to some trigger, and the permeated hydrogen would react at the positive electrode, causing the voltage drop (self-discharge) as described above. The voltage drop caused by such hydrogen permeation is considered to accelerate the reaction in the battery usage environment, and the time until the voltage drop occurs is shorter, that is, the battery performance is deteriorated faster. The condition for hydrogen to easily permeate is considered to be that the higher the hydrogen concentration gradient is, the easier it is to permeate. In addition to the hydrogen concentration gradient, the state in which voltage is applied to both sides of the surface-treated steel foil is considered to further promote hydrogen permeation. In other words, hydrogen permeation may be one of the factors that cause the gradual decrease in battery performance over time in batteries using hydrogen storage alloys, batteries with high concentration gradients such as nickel-metal hydride batteries, and secondary batteries with many charge and discharge cycles. On the other hand, the gradual decrease in battery performance is largely due to other factors, and the phenomenon of hydrogen permeation is difficult to grasp, so it has not been clarified in the use and development of conventional monopolar batteries. However, the present inventors have come up with the idea that the improvement of the hydrogen barrier property of the iron-nickel alloy layer contributes to the suppression of the deterioration of battery performance while repeating experiments in the development of surface-treated steel foil for bipolar battery current collectors. Therefore, the surface-treated steel foil of this embodiment is particularly suitable for use as a current collector in batteries that use hydrogen storage alloys, particularly bipolar batteries. However, even in batteries that do not use other hydrogen storage alloys, as long as the battery contains or generates hydrogen, it is believed that there may be a gradual deterioration in battery performance due to hydrogen permeation that has not been detected until now, and the surface-treated steel foil of this embodiment can be preferably used. In the following description, the hydrogen entry side is also referred to as the hydrogen generation side, and is the side where a hydrogen storage alloy is placed, i.e., the first surface 10a side of the surface-treated steel foil for current collector 10. The hydrogen detection side is the side opposite to the hydrogen entry side, and is the positive electrode side of the bipolar electrode structure, i.e., the second surface 10b side of the surface-treated steel foil for current collector 10.

[0032] Next, evaluation of hydrogen barrier properties will be described. When hydrogen permeates and moves through the surface-treated steel foil 10 for current collectors as described above, hydrogen atoms that reach the hydrogen detection side from the hydrogen entry side are oxidized to hydrogen ions. The value of the oxidation current at this time increases or decreases according to the amount of hydrogen that reaches the hydrogen detection surface, so it is possible to quantify and evaluate the hydrogen barrier properties of the surface-treated steel foil 10 for current collectors from the detected current value. (Mizunare Tohru, Tokyo Institute of Technology, Materials and Environment, 63, 3-9 (2014), Measurement of Hydrogen Entry and Permeation into Steel by Electrochemical Method) As a result of the above prediction, the inventors performed measurements and evaluations and concluded that in order to suppress the occurrence of the above-mentioned voltage drop (self-discharge) in this embodiment, the surface-treated steel foil 10 for a current collector of this embodiment must have a hydrogen permeation current density of 20 μA / cm, which is obtained from the oxidation current measured electrochemically. 2 It was concluded that the following is preferable. The conditions for measuring the hydrogen permeation current density in this embodiment are an electrolyte at 65° C., an Ag / AgCl (silver-silver chloride) reference electrode, a potential on the hydrogen generation side of −1.5 V, and a potential on the hydrogen detection side of +0.4 V. All of the potential values ​​used in the method for measuring the hydrogen permeation current density in this embodiment are based on an Ag / AgCl (silver-silver chloride) reference electrode.

[0033] As a specific example of a method for measuring the hydrogen permeation current density in this embodiment, a measuring device having a configuration as shown in Fig. 2(a) is used to detect the current value (current density), which makes it possible to quantify and evaluate the hydrogen barrier property of the surface-treated steel foil 10 for a current collector. The measuring device shown in Fig. 2(a) will be described below.

[0034] Two cells, a cell X for generating hydrogen and a cell Y for detecting permeated hydrogen, are prepared, and a test piece (sample) of the surface-treated steel foil for current collector 10 is placed between these two measurement cells. An alkaline electrolyte is contained in each measurement cell, and a reference electrode (RE1 and RE2) and a counter electrode (CE1 and CE2) are immersed in each cell. An Ag / AgCl electrode in a saturated KCl solution is used as the reference electrode, and platinum (Pt) is used as the counter electrode. The alkaline electrolyte is composed of KOH, NaOH, and LiOH, and the liquid temperature is 65°C. As shown in FIG. 2(b), the measurement diameter of the surface-treated steel foil for current collector 10 is φ20 mm (measurement area 3.14 cm). 2 )

[0035] A potentiostat is used for potential control and current measurement on the hydrogen entry side and hydrogen detection side as shown in Fig. 2(a). As a potentiostat, for example, the "Multi-electrochemical measurement system HZ-Pro" manufactured by Hokuto Denko Corporation can be used. The sample of the surface-treated steel foil 10 for current collector to be evaluated and the connections of each electrode can be made as shown in Fig. 2(a).

[0036] On the hydrogen generation side, the sample is polarized to the cathode (lower potential), hydrogen is generated on the sample surface, and hydrogen is absorbed. The potential is applied in stages of -0.7V, -1.1V, and -1.5V, and each potential is applied for 15 minutes. The reason for applying the potential in stages in this way is to suppress the effects of potential changes and obtain a stable plot. The measurement plot is taken every 5 seconds.

[0037] In general, in a nickel-hydrogen battery using a nickel hydroxide compound in the positive electrode and a hydrogen storage alloy in the negative electrode, the operating potential of the negative electrode in the charge and discharge reaction of the battery is around -1.1 V. In the above-mentioned measurement method applicable to this embodiment, as a method for confirming the effect of hydrogen barrier properties without using a hydrogen storage alloy, measurement conditions under which hydrogen is generated more significantly were examined. Then, the hydrogen permeation current density I (μA / cm 2 ) was calculated using the change in oxidation current when the applied potential on the hydrogen generation side was −1.5 V (hereinafter, also referred to as the oxidation current change).

[0038] When hydrogen atoms permeate from the hydrogen generation side, the hydrogen atoms are oxidized on the hydrogen detection side, generating an oxidation current that is measured by a potentiostat on the hydrogen detection side. This change in oxidation current therefore makes it possible to quantify and evaluate the hydrogen permeability of the surface-treated steel foil 10 for current collectors. Note that on the hydrogen detection side, a potential is applied and maintained to promote the oxidation of hydrogen atoms to hydrogen ions and clarify the peak of the oxidation current.

[0039] In nickel-metal hydride batteries, which use nickel hydroxide compounds in the positive electrode and hydrogen storage alloys in the negative electrode, the positive electrode operating potential in the charge and discharge reaction of the battery is generally around +0.4V. Therefore, in this measurement method, a potential of +0.4V was applied to the detection side and maintained during measurement. Note that before application to the hydrogen generation side, the hydrogen detection side was maintained at the aforementioned potential for 60 minutes to stabilize the current value. After the hydrogen generation application was completed, that is, after the application of -1.5V for 15 minutes was completed and the application to the hydrogen generation side was set to zero, the hydrogen detection side was maintained at +0.4V for 5 minutes to calculate the background. Measurement plots were made every 5 seconds. That is, as a preliminary step to the evaluation by the above measurement, first, +0.4 V is applied on the hydrogen detection side, and then the current value is stabilized by application for 60 minutes, after which application on the hydrogen generation side is started for the actual evaluation (15 minutes at each potential, a total of 45 minutes).

[0040] From the change in the oxidation current on the hydrogen detection side obtained by the above method, the hydrogen permeation current density I (μA / cm 2 The obtained oxidation current and hydrogen permeation current density I (μA / cm 2 The quantification image of () is shown in Figure 2(c) to Figure 2(e).

[0041] FIG. 2(c) is a diagram showing the overall current value measurement including the pre- and post-processes for evaluation. FIG. 2(d) is a diagram showing the change in current value for actual evaluation, and is an enlarged diagram showing the area from around 5300 seconds to around 6500 seconds in FIG. 2(c). FIG. 2(e) is a diagram shown for comparison with the present invention, showing the change in current value when a surface-treated steel foil having a thickness of 50 μm and a nickel plating layer of 1.0 μm is provided without heat treatment, that is, without an iron-nickel alloy layer, is used to perform a current value measurement similar to that in FIG. 2(c). According to FIG. 2(e), it can be confirmed that the detection side current value during application of −1.5 V for 15 minutes is clearly higher in the surface-treated steel foil having no iron-nickel alloy layer, which is a feature of the present invention, than the metal foil shown in FIG. 2(c).

[0042] In this embodiment, the hydrogen permeation current density I (μA / cm 2 ) can be calculated using the following formula based on the change in oxidation current when the applied potential on the hydrogen generation side is −1.5 V as shown in FIG. 2(d). Hydrogen permeation current density I (μA / cm 2 ) = ((average value of oxidation current from Ib to Ic) / S) - ((average value of Ia and Id) / S) where Ia (μA) is the oxidation current 5 seconds before application of -1.5 V, Ib (μA) is the oxidation current 155 seconds after the start of application of -1.5 V, Ic (μA) is the oxidation current at the end of application of -1.5 V, Id (μA) is the oxidation current 155 seconds after the end of application of -1.5 V, and S (cm 2 ) is the measurement area (evaluation area) of the test piece. The hydrogen permeation current density I (μA / cm) calculated from the above formula 2 ) is small, hydrogen permeation is suppressed, that is, the hydrogen barrier properties are high, and the hydrogen permeation current density I (μA / cm 2 ) is larger, it can be judged that hydrogen permeation is easier.

[0043] In this embodiment, the hydrogen permeation current density measured electrochemically as described above is 55 μA / cm 2From the viewpoint of hydrogen barrier properties in the surface-treated steel foil 10 for current collector, it was concluded that a current collector having a hydrogen barrier property of 20 μA / cm or less is suitable for a bipolar electrode. 2 However, the hydrogen permeation current density is the increase in oxidation current measured on the hydrogen detection side (anode side) when a potential of -1.5 V is applied to the hydrogen generation side (cathode side) under the condition that the potential on the hydrogen detection side is +0.4 V (vs Ag / AgCl) in an electrolyte at 65°C.

[0044] In general, it is known that metal materials have different hydrogen diffusion coefficients depending on the type, and metal materials that suppress hydrogen penetration may be required to suppress defects and hydrogen embrittlement caused by hydrogen in metals depending on the application of the metal material. For example, high alloy steel is used to suppress delayed fracture of high strength bolts, and titanium welded parts are used to suppress cracking of pressure reactor vessels. However, these materials and applications do not anticipate hydrogen penetration in an environment where the amount of hydrogen increases, such as when a hydrogen storage alloy is placed on the surface. The problem with these technologies is that hydrogen remains in the metal, affecting the mechanical properties of the metal itself, but there is no problem of hydrogen permeating the metal material and affecting the opposite surface. In addition, as for hydrogen permeation in battery components, it is known that, for example, hydrogen impermeability is required as gas impermeability in fuel cell separators. However, in fuel cells, hydrogen permeation is mainly a problem in the case of carbon separators, and it was thought that hydrogen permeation does not occur and is not a problem when stainless steel or aluminum separators are used. In addition, since corrosion resistance in a sulfuric acid atmosphere is essential for fuel cell separators and steel plates are difficult to apply, no issues were found assuming the application of steel plates. On the other hand, it was found that a current collector in a bipolar electrode structure in which one side of the current collector is a negative electrode active material layer and the other side is a positive electrode active material layer is more likely to cause hydrogen permeation than a fuel cell, and that this may affect the battery performance. It is thought that this issue was identified precisely because the battery structure, target parts, internal environment, etc. are different from those of fuel cells.

[0045] Next, the thickness of the iron-nickel alloy layer 30 will be described. From the viewpoint of suppressing hydrogen permeation as described above, the thickness of the iron-nickel alloy layer 30 included in the surface-treated steel foil 10 for current collector of this embodiment must be 0.5 μm or more in at least one layer, preferably 0.6 μm or more, and more preferably 0.7 μm or more. There is no particular upper limit, but if it is too thick, the ratio of hard layers in the surface-treated steel foil for current collector increases, and the surface-treated steel foil for current collector itself may be easily cracked, and the resistance increases, so that it is preferably 7.5 μm or less per side, more preferably 6 μm or less. The total thickness of both sides is preferably 15 μm or less, more preferably 12 μm or less, even more preferably 7 μm or less, and even more preferably 3.5 μm or less. In particular, when a continuous steel strip is used as the substrate, that is, when the surface-treated steel foil for current collector having the iron-nickel alloy layer of this embodiment is obtained by subjecting the continuous steel strip to surface treatment, it is preferably 6 μm or less per side, more preferably 3.5 μm or less, from the viewpoint of controlling the plating coverage and avoiding unevenness in heat treatment.

[0046] As described above, the entire surface-treated steel foil 10 for a current collector may be the iron-nickel alloy layer 30. In this case, since the metal substrate 20 is not included, the surface-treated steel foil 10 for a current collector can be manufactured, for example, by forming the iron-nickel alloy layer 30 on a support by electrolytic plating and then peeling it off. In this case, the thickness of the surface-treated steel foil 10 for a current collector is preferably 4 μm to 25 μm.

[0047] As described above, the iron-nickel alloy layer 30 may be disposed on both the first surface 10a and the second surface 10b as shown in FIG. 1(c). In that case, from the viewpoint of hydrogen barrier properties, the iron-nickel alloy layer 30 needs to have a thickness of 0.5 μm on at least one surface. From the viewpoint of further improving hydrogen barrier properties, the total thickness of the iron-nickel alloy layer on both surfaces is preferably 0.7 μm or more, and more preferably 0.8 μm or more. The thickness of the iron-nickel alloy layer on both surfaces may be the same or different, and it is sufficient that it is formed to a thickness of 0.5 μm or more on at least one surface.

[0048] In this embodiment, a method for calculating the thickness of the iron-nickel alloy layer 30 will be described. In this embodiment, the thickness of the iron-nickel alloy layer 30 can be calculated by quantitatively analyzing Ni and Fe at a depth of at least 10 μm from the surface layer side in the thickness direction by SEM-EDX (energy dispersive X-ray spectroscopy) analysis of the cross section of the surface-treated steel foil for current collector. When the diffusion layer thickness exceeds 10 μm, quantitative analysis is performed to the required depth.

[0049] An example of a method for obtaining the thickness of the iron-nickel alloy layer 30 from a graph obtained by SEM-EDX is shown below. In the graph of Fig. 3, the horizontal axis indicates the distance (μm) in the depth direction from the surface side, and the vertical axis indicates the X-ray intensity of Ni and Fe. The graph of Fig. 3 shows that the nickel content is high and the iron content is low in the shallower parts in the thickness direction. On the other hand, the iron content increases as the thickness direction progresses. In this embodiment, in the portion before and after the intersection of the nickel curve and the iron curve, the distance between 2 / 10 of the maximum values ​​of nickel and iron is taken as the iron-nickel alloy layer 30, and its thickness can be read from the graph. Even when a metal layer 40 or a roughened nickel layer 50 described below is formed on the iron-nickel alloy layer 30, the thickness of the iron-nickel alloy layer 30 can be obtained by the above method.

[0050] In this embodiment, the reason why the distance between 2 / 10 of the maximum values ​​of nickel and iron is set as the thickness of the iron-nickel alloy layer 30 is as follows. That is, in the present invention, it is preferable that the thickness of the iron-nickel alloy layer 30 is set to a predetermined value or more, but when the thickness of the iron-nickel alloy layer 30 is measured by SEM-EDX, it has been found that even in a sample that has not been subjected to heat treatment, that is, a sample in which iron is not diffused into nickel, the iron intensity at the position where the nickel intensity is at its peak is detected as a value of about 10% to 20% of the nickel intensity. Furthermore, after the nickel intensity has attenuated, that is, in the measurement of the metal base material 20 portion, the nickel intensity continues to be detected as a value of about 3 to 8% of the maximum nickel intensity. At this time, the nickel intensity is also about 2% of the iron intensity, and even if the measurement is continued for 2 μm or more after attenuation, it does not fall below 1%. In other words, it has been found that the nickel intensity and the iron intensity are influenced by each other in a trace range in the measurement by SEM-EDX. Therefore, in this specification, the range in which an intensity of 2 / 10 or more of the maximum intensity is detected is specified as the thickness of the alloy layer that is more reliably alloyed and can ensure hydrogen barrier properties.

[0051] In the surface-treated steel foil 10 for a current collector of this embodiment, the amount of nickel deposited in the iron-nickel alloy layer 30 is 0.80 g / m 2 ~53.4g / m 2 From the viewpoint of hydrogen barrier properties and electrolyte resistance suitable for a bipolar electrode, it is preferable that the thickness is 0.80 g / m. 2 ~26.7g / m 2The amount of nickel deposited in the iron-nickel alloy layer 30 can be measured by X-ray fluorescence analysis (XRF) or the like.

[0052] In the iron-nickel alloy layer 30 of this embodiment, from the viewpoint of hydrogen barrier properties, the crystallite diameter in the (200) plane of the iron-nickel alloy is preferably 3 nm or more, more preferably 8 nm or more. There is no particular upper limit, but it is usually 50 nm or less. When hydrogen permeates the iron-nickel alloy layer, it is not clear which path hydrogen moves through, but it is thought that grain boundaries and interfaces with large orientation differences are places where hydrogen can easily pass through. Therefore, in the case of a configuration in which the crystallite diameter is small and the grain boundaries are likely to be numerous, it is thought that there are many paths for hydrogen, the total amount of hydrogen permeation is likely to increase, and the hydrogen barrier properties are likely to deteriorate. On the other hand, in the case of a configuration in which the crystallite diameter is large, there are few grain boundaries and interfaces with large orientation differences, and it is thought that hydrogen permeation is unlikely to occur. In particular, when the iron-nickel alloy layer is formed by iron-nickel alloy plating, the grains become fine and the crystallite diameter is likely to be small, but by performing heat treatment after alloy plating, the crystallite diameter can be made 8 nm or more, and hydrogen barrier properties can be obtained more effectively. When the crystallite size exceeds 50 nm, it is assumed that the heat treatment has significantly promoted Fe diffusion from the iron of the base material to the outermost surface, and the Fe composition at the surface of the iron-nickel alloy layer 30 tends to be high, which is undesirable since it tends to cause Fe elution.

[0053] In the iron-nickel alloy layer 30 of this embodiment, the reason why it is preferable to specify the crystallite size in the (200) plane of the iron-nickel alloy as described above is that the iron-nickel alloy has a face-centered cubic structure, and the (200) plane is a plane that is easy to obtain strength from and allows the crystallite size of the iron-nickel to be measured more accurately, making it a suitable plane for control.

[0054] In the iron-nickel alloy layer 30 of this embodiment, the crystallite size of the (200) plane of the iron-nickel alloy is calculated from the peak half-width by X-ray diffraction using the following formula. The X-ray diffraction measurement is performed using, for example, a known X-ray diffraction device. The crystallite size is calculated using the peak of the (200) plane of the iron-nickel alloy that appears around 2θ=51°. D = K × λ / (β × cosθ) D: Crystallite diameter K: Scherrer constant (K = 0.94 is used) λ: wavelength of X-rays used β: Half-width of diffracted X-rays from crystallites θ: Bragg angle

[0055] Next, the overall thickness of the surface-treated steel foil 10 for a current collector in this embodiment will be described. Note that the "thickness of the surface-treated steel foil 10 for a current collector" in this embodiment can be measured by cross-sectional observation with a scanning electron microscope (SEM) or by thickness measurement with a micrometer. The total thickness of the surface-treated steel foil 10 for a current collector in this embodiment is preferably in the range of 0.01 to 0.5 mm when it does not have a roughened nickel layer 50 described later, and more preferably 0.01 to 0.3 mm, and even more preferably 0.025 to 0.1 mm, from the viewpoints of strength and desired battery capacity. On the other hand, when the surface-treated steel foil 10 for a current collector has a roughened nickel layer 50 on the outermost surface, the total thickness of the surface-treated steel foil 10 for a current collector in this embodiment is preferably in the range of 0.02 to 0.51 mm. From the viewpoints of strength and desired battery capacity, the thickness is more preferably 0.02 to 0.31 mm, and further preferably 0.035 to 0.11 mm. If the thickness exceeds the upper limit of the above range, this is not preferable from the viewpoint of the volume and weight energy density of the battery to be manufactured, and is particularly unfavorable when aiming at a thinner battery.On the other hand, if the thickness is below the lower limit of the above range, not only will it be difficult to provide sufficient strength against the effects of charging and discharging the battery, but there will also be a high possibility of the battery being torn, ripped, or wrinkled during manufacturing or handling.

[0056] The surface-treated steel foil 10 for current collector in this embodiment may further have a metal layer 40 formed on the iron-nickel alloy layer 30, as shown in FIG. 4. Examples of metal materials constituting the metal layer 40 include nickel, chromium, titanium, copper, cobalt, and alloys containing these. Among these, nickel or nickel alloys are particularly preferred because of their excellent electrolyte resistance and strength. The metal layer 40 may include a nickel layer formed on the iron-nickel alloy layer by not diffusing iron to the surface when performing heat treatment after electrolytic nickel plating to form the iron-nickel alloy layer 30. Nickel plating may also be performed on the nickel layer.

[0057] That is, in the surface-treated steel foil 10 for a current collector of this embodiment, the effect of forming the metal layer 40 on the iron-nickel alloy layer 30 includes the following points: By forming the metal layer 40 in addition to the iron-nickel alloy layer 30, the electrical conductivity, electrolyte resistance, strength, etc. of the surface-treated steel foil 10 for a current collector as a whole can be adjusted, and it becomes possible to produce a surface-treated steel foil for a current collector having desired properties as a current collector material.

[0058] In the surface-treated steel foil 10 for a current collector of this embodiment, when the metal layer 40 is a nickel layer, the total amount of nickel deposited in the iron-nickel alloy layer 30 and the metal layer 40 (nickel layer) is 2.0 g / m 2 ~53.4g / m 2 From the viewpoint of hydrogen barrier properties and electrolyte resistance suitable for a bipolar electrode, it is preferable that the thickness is 2.0 g / m. 2 ~26.7g / m 2 The amount of nickel deposited in the iron-nickel alloy layer 30 and the metal layer 40 can be measured by X-ray fluorescence analysis (XRF) or the like.

[0059] The thickness of the metal layer 40 is preferably 0.1 μm to 4.0 μm, more preferably 0.1 μm to 3.5 μm, even more preferably 0.1 to 3.0 μm, and particularly preferably 0.2 to 2.5 μm. In addition, the thickness ratio of the iron-nickel alloy layer 30 to the metal layer 40 in the surface-treated steel foil 10 for current collector, particularly when the metal layer 40 is a layer made of nickel, is preferably iron-nickel alloy layer 30:metal layer 40=3:10 to 60:1, more preferably iron-nickel alloy layer 30:metal layer 40=3:4 to 35:1, from the viewpoint of improving hydrogen barrier property and electrolyte resistance. As with the iron-nickel alloy layer 30, the thickness of the metal layer 40 can be measured by analyzing a cross section of the surface-treated steel foil for current collector with SEM-EDX (energy dispersive X-ray spectroscopy).

[0060] In the surface-treated steel foil 10 for a current collector of this embodiment, a roughened nickel layer 50 may be formed on the outermost surface as shown in Fig. 5. Note that a roughened nickel layer may be formed on the above-mentioned metal layer 40 as shown in Fig. 6.

[0061] The roughened nickel layer 50 may be formed on the second surface 10b of the surface-treated steel foil 10 for a current collector as shown in FIG. 5(a), or on the first surface 10a as shown in FIG. 5(b), or on both. The roughened nickel layer is described in, for example, the applicant's application (WO2021 / 020338, etc.), so details are omitted here. However, it is preferable that the three-dimensional surface property parameter Sa of the roughened nickel layer is 0.2 μm to 1.3 μm from the viewpoint of improving adhesion with the active material. More preferably, it is 0.36 to 1.2 μm.

[0062] In addition, when forming the roughened nickel layer 50, from the viewpoint of adhesion between the roughened nickel layer 50 and the layer below it, a base nickel layer may be formed before the roughened nickel plating, and then a coating nickel plating may be applied after the roughened nickel plating to form the roughened nickel layer. That is, the nickel plating applied as the metal layer 40 on the iron-nickel alloy layer may be used as the base nickel layer, and the roughened nickel layer 50 may be formed thereon. In addition, the metal layer 40 formed by further applying nickel plating to the nickel layer in which almost no iron has diffused during the heat treatment for forming the iron-nickel alloy layer is left on the iron-nickel alloy layer in the heat treatment for forming the iron-nickel alloy layer, and the metal layer 40 may be used as the base nickel layer, and the roughened nickel layer 50 may be formed thereon. In addition, the above-mentioned metal layer 40 may be described in the present specification as the "roughened nickel layer 50" in some cases including the coating nickel layer. The details of the base nickel layer, the roughened nickel layer, and the coating nickel layer will be described later.

[0063] When the roughened nickel layer 50 is formed, the total amount of nickel deposited in the iron-nickel alloy layer 30 and the roughened nickel layer 50 is 7.7 g / m 2 ~106g / m 2 and more preferably 9 g / m 2 ~70g / m 2 and more preferably 15 g / m 2 ~60g / m 2 It is. In the case where the roughened nickel layer 50 is formed and the roughened nickel layer 50 is formed on the metal layer 40 made of nickel, the total amount of nickel deposited in the iron-nickel alloy layer 30, the metal layer 40 and the roughened nickel layer 50 is 7.7 g / m 2 ~106g / m 2 and more preferably 9 g / m 2 ~70g / m 2 and more preferably 15 g / m 2 ~60g / m 2 It is. In addition, as a method for measuring the amount of nickel deposited on the roughened nickel layer 50, for example, the methods described in International Publication No. WO2020 / 017655 and International Publication No. WO2021 / 020338 can be appropriately adopted. That is, the total amount of nickel can be measured for the surface-treated steel foil 10 for a current collector using X-ray fluorescence analysis (XRF) or the like.

[0064] <Manufacturing method of surface-treated steel foil for current collector> The manufacturing method of the surface-treated steel foil 10 for a current collector of this embodiment will be described below. The manufacturing method of the surface-treated steel foil 10 for a current collector of this embodiment includes a step of forming an iron-nickel alloy layer 30 for suppressing the permeation or diffusion of hydrogen in the surface-treated steel foil for a current collector on at least one of a first surface 10a on which a hydrogen storage alloy is disposed and a second surface 10b opposite to the first surface 10a.

[0065] In this embodiment, after a nickel plating layer is formed by electrolytic plating on at least one surface of the steel foil serving as the metal substrate 20, the iron-nickel alloy layer 30 can be formed by thermal diffusion by carrying out a heat treatment. Alternatively, the iron-nickel alloy layer 30 may be formed on at least one surface of a steel foil serving as the metal substrate 20 by electrolytic plating using a plating bath containing iron ions and nickel ions. That is, the process for forming the iron-nickel alloy layer 30 includes (i-1) a process for forming a nickel plating layer on at least one side of a steel foil, and (i-2) a process for forming the iron-nickel alloy layer 30 by thermal diffusion through heat treatment of the nickel plating layer formed on the steel foil. Alternatively, the step of (ii) forming an iron-nickel alloy layer 30 on at least one surface of the steel foil using a plating bath containing iron ions and nickel ions can also be included.

[0066] In the manufacturing method of this embodiment, known plating conditions can be applied to the formation of the nickel plating layer or the iron-nickel alloy plating layer by electrolytic plating. Examples of plating conditions are shown below.

[0067] [An example of nickel plating bath (Watts bath) and plating conditions] ·Bath composition: Nickel sulfate hexahydrate: 200~300g / L Nickel chloride hexahydrate: 20-60g / L Boric acid: 10~50g / L Bath temperature: 40~70℃ pH: 3.0~5.0 Agitation: Air agitation or jet agitation Current density: 5~30A / dm 2 In addition to the Watts bath, the bath composition may be a known nickel sulfamate bath or a known citric acid bath. Furthermore, additives such as known brighteners may be added to the plating bath to produce bright nickel plating or semi-bright nickel plating.

[0068] [An example of iron-nickel alloy plating bath and plating conditions] ·Bath composition Nickel sulfate hexahydrate: 150~250g / L Iron sulfate heptahydrate: 5~100g / L Nickel chloride hexahydrate: 20~50g / L Boric acid: 20-50g / L Sodium citrate (or trisodium citrate) 1-15g / L Sodium saccharin: 1-10g / L ·Temperature: 25~70℃ pH: 2~4 Agitation: Air agitation or jet agitation ·Current density: 5~40A / dm 2

[0069] Regarding the bath temperature, if it is less than 25°C, the electrodeposition efficiency will decrease or deposition will be difficult, making it difficult to form the desired alloy layer, which is not preferred. It is also not preferred because there is a possibility that the layer will not be deposited. On the other hand, if it exceeds 70°C, it is also not preferred because the plating film will become hard and the probability of defects such as cracks occurring will increase. It is also not preferred because it will be difficult to control the composition of iron (Fe) and nickel (Ni).

[0070] If the pH is less than 2, nickel (Ni) becomes difficult to deposit, making it impossible to control the composition of the desired iron (Fe) and nickel (Ni), which is not preferred. It is also not preferred because the deposition efficiency of the plating decreases. On the other hand, if the pH exceeds 4, iron (Fe) becomes difficult to deposit, making it impossible to control the composition of the desired iron (Fe) and nickel (Ni), which is not preferred. It is also not preferred because there is a possibility that sludge will be entrained in the resulting iron-nickel alloy layer.

[0071] The current density is 5A / dm 2 If the current density is less than 40 A / dm, the stress of the coating becomes too high, which is undesirable since it is prone to cause defects such as cracks in the plating coating. In addition, there is a risk of a decrease in production efficiency, which is undesirable. 2 If it exceeds this value, plating fading may occur, which is not preferable. Also, a suitable amount of a pitting inhibitor may be added.

[0072] In the manufacturing method of this embodiment, the nickel coating weight in the nickel plating layer or iron-nickel alloy plating layer formed on the steel foil is 0.80 g / m per side. 2 ~53.4g / m 2 It is preferable that the coating weight is 53.4 g / m 2 If the coating weight exceeds 0.80 g / m, the operability of electrolytic plating decreases, and the cost increases significantly. 2 If the nickel content is less than 0.80 g / m per side, the nickel coating amount on the steel foil after alloy plating or after the heat treatment described below is more preferably 0.80 g / m per side from the viewpoints of cost and electrolyte resistance. 2 ~26.7g / m 2 The total amount of adhesion on both sides is 1.6 g / m 2 ~53.5g / m 2 It is even more preferable that:

[0073] Next, the conditions of the heat treatment in the above-mentioned step (i-2) will be described. The conditions of the heat treatment step in this embodiment can be the following conditions. The heat treatment in this embodiment can be continuous annealing or batch annealing (box annealing). The heat treatment after iron-nickel alloy plating, not after nickel plating, can be performed under the same conditions, and the crystallite size can be set to a more preferable range by performing the heat treatment after iron-nickel alloy plating.

[0074] In the case of continuous annealing, the temperature and time are preferably within the range of 650°C to 950°C and the soaking time is preferably within the range of 15 seconds to 150 seconds. If the temperature is lower or the time is shorter than this range, it may not be possible to obtain a sufficient iron-nickel alloy layer 30, which is not preferable. On the other hand, if the temperature is higher or the time is longer than the above heat treatment range, the mechanical properties of the steel foil, which serves as the base material, change significantly, resulting in a significant decrease in strength, or it is not preferable from the viewpoint of cost.

[0075] For example, the temperature and time for batch annealing (box annealing) are preferably within the range of 450°C to 690°C, a soaking time of 1.5 hours to 20 hours, and a total time including the heating, soaking, and cooling times of 4 hours to 80 hours. If the temperature is lower or the time is shorter than this range, it is not preferable because a sufficient iron-nickel alloy layer 30 may not be obtained. On the other hand, if the temperature is higher or the time is longer than the above heat treatment range, the mechanical properties of the steel foil, etc., which serves as the base material, may change significantly, resulting in a significant decrease in strength, or it is not preferable from the viewpoint of cost.

[0076] In the manufacturing method of the surface-treated steel foil 10 for a current collector of this embodiment, when a nickel layer is further formed as a metal layer on the iron-nickel alloy layer 30, it can be formed using a known nickel bath such as the above-mentioned Watts bath, nickel sulfamate bath, or citric acid bath. In this case, it is preferable to carry out a known strike nickel plating treatment immediately before forming the nickel layer. After the metal layer is formed using nickel plating, it is preferable not to carry out a heat treatment from the viewpoint of adhesion with the roughened nickel layer described below.

[0077] In the manufacturing method of the surface-treated steel foil 10 for current collector of the present embodiment, the roughened nickel layer 50 can be formed on the outermost surface. The plating bath for forming the roughened nickel layer has a chloride ion concentration of preferably 3 to 90 g / L, more preferably 3 to 75 g / L, and even more preferably 3 to 50 g / L, a ratio of nickel ions to ammonium ions in terms of the weight ratio of "nickel ions / ammonium ions" of preferably 0.05 to 0.75, more preferably 0.05 to 0.60, even more preferably 0.05 to 0.50, and even more preferably 0.05 to 0.30, and a bath conductivity at 50°C of preferably 5.00 to 30.00 S / m, more preferably 5.00 to 20.00 S / m, and even more preferably 7.00 to 20.00 S / m. When the chloride ion concentration is 10 g / L or more, a good roughened plating state is easily obtained even if the amount of adhesion in the roughened nickel plating is small. The method for adjusting the chloride ion concentration, the ratio of nickel ions to ammonium ions, and the bath conductivity of the plating bath to be within the above ranges is not particularly limited, but an example of the method includes a method in which the plating bath contains nickel sulfate hexahydrate, nickel chloride hexahydrate, and ammonium sulfate, and the amounts of these ingredients are appropriately adjusted. An example of the plating conditions is as follows.

[0078] <An example of roughening nickel plating conditions> bath composition Nickel sulfate hexahydrate 10-100g / L, nickel chloride hexahydrate 1-90g / L, ammonium sulfate 10-130g / L pH 4.0~8.0 Bath temperature 25~70℃ Current density 4~40A / dm 2 Plating time: 10 seconds to 150 seconds Agitation: Air agitation or jet agitation The addition of ammonia to the nickel plating bath may be performed using ammonia water or ammonium chloride instead of ammonium sulfate. The ammonia concentration in the plating bath is preferably 6 to 35 g / L, more preferably 10 to 35 g / L, further preferably 16 to 35 g / L, and even more preferably 20 to 35 g / L. In order to control the chloride ion concentration, a basic nickel carbonate compound, hydrochloric acid, sodium chloride, potassium chloride, or the like may be used.

[0079] As disclosed in International Publication WO2020 / 017655, a roughened nickel layer may be formed by applying a coated nickel plating as a subsequent step to the roughened nickel plating. Since the contents disclosed in International Publication WO2020 / 017655 can be applied to the coated nickel plating conditions, detailed description thereof will be omitted here.

[0080] As described above, the three-dimensional surface texture parameter Sa of the roughened nickel layer 50 is preferably 0.2 μm to 1.3 μm. In order to set the numerical value of the three-dimensional surface texture parameter Sa of the roughened nickel layer 50 within this range, for example, it can be achieved by controlling the surface roughness of the metal substrate 20, adjusting the roughened nickel plating conditions and thickness, adjusting the undercoat nickel plating conditions and thickness, adjusting the coating nickel plating conditions and thickness, etc.

[0081] Example The present invention will be described in more detail below with reference to examples. First, the measurement methods used in the examples will be described.

[0082] [Method for measuring thickness of iron-nickel alloy layer after heat treatment] The thickness of the iron-nickel alloy layer was calculated by SEM-EDX (energy dispersive X-ray spectroscopy) (device names: Hitachi High-Technologies SU8020 and AMETEK EDAX), and elemental analysis of Ni and Fe was performed by line analysis from the surface to a depth of 15 μm in the thickness direction. The measurement conditions were acceleration voltage: 15 kV, observation magnification: 5000 times, and measurement step: 0.1 μm. As shown in Figure 3, the horizontal axis is the distance in the depth direction from the surface (μm), and the vertical axis is the X-ray intensity of Ni and Fe. The distance between 2 / 10 of the maximum values ​​of nickel and iron in the part before and after the intersection of the nickel curve and the iron curve was taken as the iron-nickel alloy layer 30, and its thickness was read from the graph.

[0083] [Method for measuring hydrogen permeation current density] Using the apparatus shown in FIG. 2, the evaluation sample was used as the working electrode, the reference electrode was Ag / AgCl, and the potential of the hydrogen generation side (cathode side) was -1.5V, and the potential of the hydrogen detection side (anode side) was +0.4V. The detailed measurement method was performed using the apparatus shown in FIG. 2(a) as described above. As the electrolyte, an alkaline aqueous solution consisting of KOH, NaOH, and LiOH, containing 6 mol / L of KOH as the main component at 65°C, and having a total concentration of 7 mol / L of KOH, NaOH, and LiOH, was used. As the potentiostat, the "Multi Electrochemical Measurement System HZ-Pro" manufactured by Hokuto Denko Corporation was used. First, a potential of +0.4V was applied to the hydrogen detection side and held for 60 minutes to stabilize the current value. The hydrogen detection side was continued to be held at the same potential. Next, the potential of the hydrogen entry side was applied stepwise to -0.7V, -1.1V, and -1.5V, and each potential was applied for 15 minutes. The change in oxidation current when the potential on the hydrogen entry side is −1.5 V is defined as the hydrogen permeation current density, and is the subject of evaluation in this embodiment and comparative example. The measurement diameter is φ20 mm, and the measurement area is 3.14 cm 2 It was decided. The hydrogen permeation current density I (μA / cm) obtained by the following formula (1) 2 ) are shown in Table 1. Hydrogen permeation current density I (μA / cm 2) = ((average value of oxidation current from Ib to Ic) / S) - ((average value of Ia and Id) / S) (1) where Ia (μA) is the oxidation current 5 seconds before application of -1.5 V, Ib (μA) is the oxidation current 155 seconds after the start of application of -1.5 V, Ic (μA) is the oxidation current at the end of application of -1.5 V, Id (μA) is the oxidation current 155 seconds after the end of application of -1.5 V, and S (cm 2 ) is the measured area (evaluated area).

[0084] [Crystallite size measurement] To measure the crystallite size, X-ray diffraction was performed using an X-ray diffractometer (Rigaku Corporation, fully automatic multipurpose horizontal X-ray diffractometer SmartLab). <Device configuration> ·X-ray source: CuKα Goniometer radius: 300nm ·Optical system: Concentration method (Inlet slit system) Solar slit: 5° Length limit slit: 5mm Divergence slit: 2 / 3° (Light receiving slit system) Scattering slit: 2 / 3° Solar slit: 5° Receiving slit: 0.3 mm Monochromatization method: Counter monochromator method Detector: Scintillation counter <Measurement parameters> Tube voltage-tube current: 45kV 200mA ·Scanning axis: 2θ / θ (concentration method) Scanning mode: Continuous Measurement range: 2θ 40~100° Scanning speed: 10° / min Step: 0.02°

[0085] The sample was placed on a sample stage for measurement, and the iron-nickel alloy layer was subjected to X-ray diffraction measurement by reflection method in the range of X-ray diffraction angle 2θ = 40 to 100 °. After that, the crystallite size was calculated from the obtained measured values ​​according to the following formula using the integrated powder X-ray analysis software PDXL manufactured by Rigaku Corporation. Specifically, the half-width at the 51.05° peak originating from the (200) plane of the iron-nickel alloy was calculated in the obtained measurement chart to obtain the crystallite diameter of the (200) plane of the iron-nickel alloy. If there is a peak near 51.85° originating from the nickel (200) plane, it is possible to perform peak separation. When performing data processing using the above-mentioned X-ray analysis software, the peak optimization process is performed in the range of X-ray diffraction angles 2θ = 48 to 54°, with only the angles fixed at 2θ (FeNi (200)) = 51.05 ° and 2θ (Ni (200)) = 51.85 °, and the other settings are set automatically, so that it is possible to separate the peaks of each component and calculate the crystallite diameter. The optimization process conditions can be such that the peak shape is a split pseudo-Voigt function. D = K × λ / (β × cosθ) D: Crystallite diameter K: Scherrer constant (K = 0.94 is used) λ: wavelength of X-rays used β: Half-width of diffracted X-rays from crystallites θ: Bragg angle

[0086] <Example 1> First, a cold-rolled foil (thickness: 50 μm) of low-carbon aluminum-killed steel having the chemical composition shown below was prepared as the metal substrate 20 . C: 0.04% by weight, Mn: 0.32% by weight, Si: 0.01% by weight, P: 0.012% by weight, S: 0.014% by weight, balance: Fe and unavoidable impurities

[0087] Next, the prepared metal substrate was electrolytically degreased and pickled by immersion in sulfuric acid, and then nickel-plated on both sides of the steel foil under the following conditions to achieve a nickel coating weight of 4.45 g / m at a target thickness of 0.5 μm. 2 The nickel plating layer was formed under the following conditions. (Ni plating conditions) Bath composition: Nickel sulfate hexahydrate: 250g / L Nickel chloride hexahydrate: 45g / L Boric acid: 30g / L Bath temperature: 60℃ pH: 4.0~5.0 Agitation: Air agitation or jet agitation Current density: 10A / dm 2

[0088] The amount of nickel attached was measured using an X-ray fluorescence analyzer (Rigaku Corporation ZSX100e), and the obtained values ​​are shown in Table 1. The specific measurement method is the same as the method described in International Publication WO2020 / 017655, so detailed explanation is omitted here.

[0089] Next, the steel foil having the nickel plating layer formed above was heat-treated by box annealing under the conditions of a heat treatment temperature of 640°C, a soaking time of 2 hours (total of heating time, soaking time, and cooling time: 6 hours) in a reducing atmosphere. This heat treatment yielded a surface-treated steel foil having iron-nickel alloy layers on both sides, with the iron-nickel alloy layer on one side being 1.4 μm thick (total thickness of the iron-nickel alloy layers on both sides: 2.8 μm). A nickel film for measurement was formed on both sides of the obtained surface-treated steel foil. Then, the hydrogen permeation current density was measured. The "nickel film for measurement" was formed under the following plating conditions in order to avoid the influence of the difference in surface state between each example and comparative example on the measurement conditions and the measured value (oxidation current). The results obtained are shown in Table 1.

[0090] <Nickel plating conditions for measurement> Bath composition: Nickel sulfate hexahydrate 250g / L, Nickel chloride hexahydrate 45g / L, Boric acid 30g / L pH 4.0~5.0 Bath temperature 60℃ Current density 10A / dm 2 The target thickness of the nickel layer to be measured was 1.0 μm on each side.

[0091] <Example 2> The same procedure as in Example 1 was carried out except that the target thickness of the nickel plating layer formed on the steel foil was set to 1.5 μm. The results are shown in Table 1.

[0092] <Example 3> The same procedure as in Example 1 was carried out except that the target thickness of the nickel plating layer formed on the steel foil was set to 3.0 μm. The results are shown in Table 1.

[0093] <Example 4> The same procedure as in Example 1 was carried out except that the target thickness of the nickel plating layer formed on the steel foil was set to 1.0 μm. The results are shown in Table 1. In addition, the crystallite diameter of the (200) plane of the iron-nickel alloy layer was measured before and after the formation of the nickel film for measurement. It was 12 nm before the formation of the nickel film for measurement and 10.9 nm after the formation of the nickel film for measurement.

[0094] <Example 5> The target thickness of the nickel plating layer formed on the steel foil was 1.5 μm, and the heat treatment conditions for the box annealing were a heat treatment temperature of 560° C. and a soaking time of 6 hours (total of heating time, soaking time, and cooling time: 10 hours). Other than that, the same procedure as in Example 1 was carried out. The results are shown in Table 1.

[0095] <Example 6> The same procedure as in Example 5 was carried out except that the target thickness of the nickel plating layer formed on the steel foil was set to 2.0 μm. The results are shown in Table 1.

[0096] <Example 7> The same procedure as in Example 5 was carried out except that the target thickness of the nickel plating layer formed on the steel foil was 0.5 μm. The results are shown in Table 1.

[0097] <Example 8> The same procedure as in Example 5 was carried out except that the target thickness of the nickel plating layer formed on the steel foil was 1.0 μm. The results are shown in Table 1.

[0098] <Example 9> The same procedure as in Example 5 was carried out except that the target thickness of the nickel plating layer formed on the steel foil was 3.0 μm. The results are shown in Table 1.

[0099] <Example 10> The same procedures as in Example 1 were carried out except that the target thickness of the nickel plating layer formed on the steel foil was 3.0 μm, the heat treatment was performed by continuous annealing, the ultimate temperature was 900° C., and the soaking time was 120 seconds.

[0100] <Example 11> The same procedures as in Example 1 were carried out except that the target thickness of the nickel plating layer formed on the steel foil was 0.7 μm, the heat treatment was performed by continuous annealing, the ultimate temperature was 900° C., and the soaking time was 120 seconds.

[0101] <Example 12> The same procedures as in Example 1 were carried out except that the target thickness of the nickel plating layer formed on the steel foil was 0.7 μm, the heat treatment was performed by continuous annealing, the ultimate temperature was 900° C., and the soaking time was 30 seconds.

[0102] <Example 13> The same procedures as in Example 1 were carried out except that the target thickness of the nickel plating layer formed on the steel foil was 1.0 μm, and the heat treatment was performed by continuous annealing, with the ultimate temperature being 900° C. and the soaking time being 20 seconds.

[0103] <Example 14> A metal substrate was subjected to iron-nickel alloy plating under the following conditions to obtain a surface-treated steel foil having an iron-nickel alloy layer with a target thickness of 5.0 μm on both sides. (Iron-nickel alloy plating conditions) ·Bath composition Nickel sulfate hexahydrate: 200g / L Iron sulfate heptahydrate: 50g / L Nickel chloride hexahydrate: 45g / L Boric acid: 30g / L Trisodium citrate: 10g / L Sodium saccharin: 5g / L Anti-pitting agent: 1ml / L ·Temperature: 60℃ pH: 2.5~3.0 Agitation: Air agitation ·Current density: 15A / dm 2 No heat treatment was performed after plating. Other than that, the procedure was the same as in Example 1. The results are shown in Table 1. In addition, after forming the nickel film for measurement, the crystallite diameter of the (200) plane of the iron-nickel alloy layer was obtained and was found to be 5.3 nm.

[0104] <Example 15> The metal substrate was subjected to iron-nickel alloy plating under the same conditions as in Example 14 to obtain a surface-treated steel foil having an iron-nickel alloy layer with a target thickness of 1.0 μm on both sides. No heat treatment was performed after plating. The rest was the same as in Example 1. The results are shown in Table 1. In addition, the crystallite diameter of the (200) plane of the iron-nickel alloy layer was measured before and after the formation of the nickel film for measurement. It was 5.0 nm before the formation of the nickel film for measurement and 5.3 nm after the formation of the nickel film for measurement.

[0105] <Example 16> The metal substrate was subjected to iron-nickel alloy plating under the same conditions as in Example 14 to obtain a surface-treated steel foil having an iron-nickel alloy layer with a target thickness of 1.0 μm on both sides. The heat treatment after plating was performed by continuous annealing, with the ultimate temperature of 900° C. and the soaking time of 120 seconds. The rest of the procedure was the same as in Example 1. The results are shown in Table 1. In addition, before the formation of the nickel film for measurement, the crystallite diameter of the (200) plane of the iron-nickel alloy layer was measured and found to be 11.7 nm.

[0106] <Example 17> The same procedure as in Example 5 was repeated, except that the target thickness of the nickel plating layer formed on the steel foil was 0.25 μm on one side and 0.1 μm on the other side. The hydrogen permeation current density was measured using the surface of the nickel plating layer with a target thickness of 0.1 μm as the detection surface. The results are shown in Table 2.

[0107] <Example 18> After the heat treatment by continuous annealing in Example 14, a nickel coating for measurement was not formed, and instead, a "nickel base layer and a roughened nickel layer" were formed on the iron-nickel alloy layer on one side under the following conditions, and only a nickel base layer was formed on the iron-nickel alloy layer on the other side. The roughened nickel layer was formed by roughening nickel plating and covering nickel plating.

[0108] <Conditions for nickel plating undercoat> Bath composition: Nickel sulfate hexahydrate 250g / L, Nickel chloride hexahydrate 45g / L, Boric acid 30g / L pH 4.0~5.0 Bath temperature 60℃ Current density 10A / dm 2 The target thickness of the nickel undercoat layer was as shown in Table 3.

[0109] <Roughened Nickel Plating Conditions> Nickel sulfate hexahydrate concentration in plating bath: 10g / L Nickel chloride hexahydrate concentration in plating bath: 10g / L Chloride ion concentration in plating bath: 3g / L Ratio of nickel ions to ammonium ions in the plating bath: nickel ions / ammonium ions (weight ratio) = 0.17 pH:6 Bath temperature: 50℃ Current density: 12A / dm 2 Plating time: 80 seconds

[0110] <Conditions for nickel plating> Bath composition: Nickel sulfate hexahydrate 250g / L, Nickel chloride hexahydrate 45g / L, Boric acid 30g / L pH: 4.0~5.0 Bath temperature: 60℃ Current density: 5A / dm 2 Plating time: 36 seconds

[0111] The total nickel coating weight of the iron-nickel alloy layer, the nickel base layer and the roughened nickel layer of the obtained surface-treated steel foil was 38.1 g / m 2 The hydrogen permeation current density was measured using the roughened nickel layer as the detection surface. In addition, if a roughened layer is formed on the test piece, the hydrogen permeation current density may not be measured normally due to electrolyte seepage from the gaps in the roughened layer. Therefore, in order to suppress the influence of electrolyte seepage from the gaps in the roughened layer, a piece of polypropylene resin cut out to a measurement diameter of Φ20 mm was attached to the surface on which the roughened layer was formed, aligned to the measurement position, and then the test piece was placed between the measurement cells. A polypropylene resin film with a thickness of 70 μm was used, and the film was bonded by thermocompression bonding at 170°C and 0.1 to 0.4 MPa for 3 seconds. The three-dimensional surface texture parameter Sa of the outermost surface of the surface-treated steel foil on which the roughened nickel layer was formed was measured and found to be 0.6 μm. The results are shown in Table 3. The three-dimensional surface texture parameter Sa was measured using a laser microscope (Olympus Corporation, 3D measuring laser microscope LEXT OLS5000) at a magnification of 100x for the OLS5000 objective lens.

[0112] <Example 19> After the heat treatment in Example 1, a nickel coating for measurement was not formed, and instead, a "base nickel layer and roughened nickel layer" were formed on the iron-nickel alloy layer on one side under the same conditions as in Example 18, and only a base nickel layer was formed on the iron-nickel alloy layer on the other side. The roughened nickel layer was formed by roughening nickel plating and coating nickel plating. The total amount of nickel attached was obtained in the same manner as in Example 18, and the hydrogen permeation current density and the three-dimensional surface property parameter Sa were measured. The results are shown in Table 3.

[0113] <Example 20> The same procedures as in Example 1 were carried out except that the thickness of the cold-rolled foil as the metal substrate 20 was 60 μm, the target thickness of the nickel plating layer formed on the steel foil was changed, the heat treatment conditions for forming the iron-nickel alloy layer were a heat treatment temperature of 560° C. and a soaking time of 8 hours (total of heating time, soaking time, and cooling time: 80 hours), and cold rolling was performed at a rolling reduction of 17.7% after the heat treatment. The nickel deposition amount was measured using a fluorescent X-ray device after the cold rolling. The results are shown in Table 1.

[0114] <Comparative Example 1> The same procedure as in Example 1 was carried out except that the steel foil having the nickel plating layer was not subjected to heat treatment. The results are shown in Table 1. Note that in Comparative Example 1, since no heat treatment was carried out, an iron-nickel alloy layer was actually formed, but in the measurement by SEM-EDX, the distance from 2 / 10 strength of iron to 2 / 10 strength of nickel was 0.3 μm.

[0115] <Comparative Example 2> The same procedure as in Comparative Example 1 was carried out except that the thickness of the nickel plating layer was changed as shown in Table 1. The results are shown in Table 1.

[0116] <Comparative Example 3> The same procedure as in Comparative Example 1 was carried out except that the thickness of the nickel plating layer was changed as shown in Table 1. The results are shown in Table 1.

[0117] <Reference example 1> Under the same Ni plating conditions as in Example 1, the target thickness on the titanium substrate was 26.0 μm and the nickel deposition amount was 231.4 g / m 2 An electrolytic nickel foil was prepared by forming a nickel layer on the foil and peeling it off. No heat treatment was performed. The hydrogen permeation current density was measured in the same manner as in Example 1. The results are shown in Table 1.

[0118] <Reference example 2> As in Reference Example 1, the target thickness was 50.0 μm and the nickel coating weight was 445.0 g / m 2 An electrolytic nickel foil was prepared by subjecting the foil to nickel plating of 1000g / g. The hydrogen permeation current density was measured in the same manner as in Reference Example 1. The results are shown in Table 1.

[0119] [Table 1]

[0120] [Table 2]

[0121] [Table 3]

[0122] It was confirmed that each of the examples had favorable hydrogen barrier properties. On the other hand, it was confirmed that the objective could not be achieved in terms of hydrogen barrier properties in Comparative Example 1 in which only a nickel layer was formed on the steel foil. In addition, in Comparative Examples 2 and 3, when the thickness of the nickel layer was increased, the hydrogen permeation current density tended to decrease, but the reduction was not sufficient, and it was confirmed that the objective could not be achieved in terms of hydrogen barrier properties. That is, in each example, a nickel film having a thickness of 1 μm was provided for measurement in order to standardize the surface condition in order to confirm the effect of the alloy layer thickness, but it was found that the effect of hydrogen barrier properties is not the effect of the nickel film but the effect of the alloy layer. Therefore, from the viewpoint of hydrogen barrier properties, the nickel film as plated on the surface is not essential in the actual form, but it was also found that the hydrogen barrier properties are not impaired even if a nickel plating layer of a preferred thickness is formed as an upper layer of the alloy layer for other purposes. Similarly, it was found in Examples 18 and 19 that even when a roughened nickel layer was formed, the hydrogen barrier properties were not impaired. Furthermore, in Example 20, it was found that the hydrogen barrier properties were not impaired even when rolling of 25% or less was performed after the iron-nickel alloy layer was formed.

[0123] In addition, in order to confirm the effect of the crystallite size on the (200) plane of the iron-nickel alloy in the iron-nickel alloy layer, it was found that better hydrogen barrier properties can be obtained when the crystallite size is 3 nm or more, preferably 8 nm or more. In particular, in Examples 15 and 16 in which the FeNi alloy layer was formed by alloy plating, it was confirmed that the crystallite size can be enlarged by carrying out heat treatment after alloy plating, and the hydrogen barrier properties can be improved more effectively.

[0124] In addition, in the hydrogen permeation current density measurement in a strong alkaline environment with a potential of +0.4 V applied to the hydrogen detection side, no peak indicating dissolution was observed and the background oxidation current was stable, so this embodiment can be said to also have electrolyte resistance. The tendency of the background oxidation current was similar even in the absence of the nickel coating for measurement.

[0125] From the above results, it is considered that the surface-treated steel foil of this embodiment has good hydrogen barrier properties, that is, it can suppress the voltage drop caused by hydrogen permeation, that is, the deterioration of the battery performance. The surface-treated steel foil of this embodiment maintains good battery performance for a long period of time by suppressing hydrogen permeation, and can improve battery performance over time, and can be suitably used as a current collector for bipolar secondary batteries.

[0126] The above-described embodiment and examples can be modified in various ways without departing from the spirit and scope of the present invention. In addition, the surface-treated steel foil for current collector in the above-mentioned embodiment and examples has been described as being used mainly as a current collector for a bipolar secondary battery. However, the surface-treated steel foil for current collector of the present invention is not limited to the current collector for a bipolar secondary battery, and can be applied to a current collector for a battery using a hydrogen storage alloy, and can be suitably used since it has effective hydrogen barrier properties even in harsh environments such as an in-vehicle battery. [Industrial Applicability]

[0127] As described above, the surface-treated steel foil for current collectors of the present invention can be applied to current collectors of various types of batteries that require hydrogen barrier properties, and when the surface-treated steel foil for current collectors of the present invention is used in in-vehicle batteries, it can particularly contribute to fuel efficiency. [Explanation of symbols]

[0128] 10. Surface-treated steel foil for current collectors 10a First Side 10b The second aspect 20 Metal substrate 30 Iron-nickel alloy layer 40 metal layer 50 Roughened nickel layer Ch1 Potentiostat Ch2 Potentiostat

Claims

1. A surface-treated steel foil for a current collector having a first surface on which a hydrogen storage alloy is disposed and a second surface located opposite to the first surface, an iron-nickel alloy layer is laminated on at least one of the first surface side and the second surface side opposite to the first surface side of a metal base made of a steel foil, the iron-nickel alloy layer suppressing permeation or diffusion of hydrogen in the surface-treated steel foil for a current collector; the iron-nickel alloy layer has a range of 2 / 10 of the maximum X-ray intensity of nickel and iron when a quantitative analysis of nickel and iron is performed in a thickness direction from a surface layer side of the first surface or the second surface in an analysis of a cross section of the surface-treated steel foil for a current collector by energy dispersive X-ray spectroscopy, The surface-treated steel foil for a current collector, wherein at least one of the iron-nickel alloy layers has a thickness of 0.5 μm or more.

2. 2. The surface-treated steel foil for a current collector according to claim 1, wherein an iron-nickel alloy layer is formed on both the first surface and the second surface of the surface-treated steel foil for a current collector, and a total thickness of the iron-nickel alloy layer on both surfaces is 0.7 μm or more.

3. The surface-treated steel foil for a current collector according to claim 1 or 2, wherein the metal substrate is a low carbon steel or an extremely low carbon steel.

4. The amount of nickel deposited in the iron-nickel alloy layer is 0.80 g / m 2 ~53.4g / m 2 The surface-treated steel foil for a current collector according to any one of claims 1 to 3.

5. The surface-treated steel foil for a current collector according to any one of claims 1 to 4, further comprising a metal layer formed on the iron-nickel alloy layer, the metal layer being a nickel layer.

6. The total nickel coating weight in the iron-nickel alloy layer and the nickel layer is 2.0 g / m 2 ~53.4g / m 2 The surface-treated steel foil for a current collector according to claim 5 ,

7. The hydrogen permeation current density measured electrochemically is 20 μA / cm 2 The surface-treated steel foil for a current collector according to any one of claims 1 to 6, wherein: The hydrogen permeation current density is the increase in oxidation current measured on the hydrogen detection side when a potential of −1.5 V is applied to the hydrogen generation side in an electrolyte at 65° C. under the condition that the potential on the hydrogen detection side is +0.4 V. The reference electrodes for the potentials on the hydrogen detection side and the hydrogen generation side are Ag / AgCl.

8. The surface-treated steel foil for current collectors according to any one of claims 1 to 7, wherein a roughened nickel layer is formed on an outermost surface of either the first surface side or the second surface side, and a three-dimensional surface texture parameter Sa of the roughened nickel layer is 0.2 μm to 1.3 μm.

Citation Information

Patent Citations

  • Battery can and its manufacturing method

    JP2007005092A

  • Ni-PLATED STEEL FOIL, BATTERY CONDUCTIVE MEMBER, AND MANUFACTURING METHOD OF Ni-PLATED STEEL FOIL

    JP2017047466A

  • Power storage device

    JP2020053401A

  • Nickel plating steel foil for nickel-hydrogen secondary battery current collector, nickel-hydrogen secondary battery current collector, and nickel-hydrogen secondary battery

    JP2021163639A

  • Steel foil and method for producing same

    WO2013157600A1