Manufacturing method of tailor welded blank using hot press steel sheet with Al-Fe intermetallic alloy layer formed
Patent Information
- Application Number
- JP2023530234
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-18
- Filing Date
- 2021-12-17
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2041-12-17
AI Technical Summary
The formation of ferrite during laser welding of steel plates coated with an aluminum-iron intermetallic alloy layer leads to weld rupture and loss of intended mechanical properties in tailor welded blanks, posing a risk of fracture under external forces.
A method involving the preparation of a base steel plate with an aluminum-based plating layer, heat treatment to form an Al-Fe intermetallic alloy layer, and subsequent removal of this layer in the welding area to prevent ferrite formation, using methods like brushing, grinding, or laser irradiation before butt welding.
Ensures high mechanical strength and resistance to weld rupture by preventing ferrite formation, maintaining the integrity of the tailor welded blanks for automotive applications.
Smart Images

Figure 0007578823000002 
Figure 0007578823000003 
Figure 0007578823000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a tailor welded blank using a steel sheet for hot press use formed with an Al-Fe-based intermetallic alloy layer, and more particularly to a method for manufacturing a tailor welded blank using a steel sheet for hot press use formed with an Al-Fe-based intermetallic alloy layer capable of preventing the formation of ferrite, which is a source of fracture in welded parts. [Background technology]
[0002] In order to ensure collision safety such as anti-intrusion during a car collision, it is required to use steel materials having high mechanical strength by having a martensite or bainite-martensite microstructure for bumpers, door reinforcement parts, B-pillar reinforcement parts, loop reinforcement parts, etc.
[0003] Patent Document 1 discloses a hot or cold rolled steel plate coated with aluminum or an aluminum alloy. The aluminum or aluminum alloy coated steel plate is heat treated at or above the Ac1 temperature and cooled under specific conditions so that it can have a tensile strength of more than 1500 MPa while being formed for a part of a required shape. During heat treatment in a furnace, the coating forms a surface alloy through interdiffusion between the steel and aluminum, preventing decarburization and oxidation of the metal, and making it possible to omit operations such as shot blasting that are performed during the manufacture of final parts.
[0004] Meanwhile, in the heat treatment for manufacturing a part using such a steel plate coated with aluminum or an aluminum alloy, unless the heating conditions are appropriately designed, for example, when rapid heating is applied, problems such as contamination and burning in transfer equipment may occur due to melting of the aluminum coated on the surface.
[0005] In order to solve these problems, a technology has been proposed that allows rapid heating and provides the same performance of the final parts as before, but involves hot- or cold-rolled steel plates having an aluminum plating layer whose surface plating layer is composed only of an intermetallic alloy layer, thereby enabling rapid heating during the manufacture of parts, improving manufacturing productivity and reducing costs.
[0006] On the other hand, to reduce the weight of automobiles, blank-like components have been developed in which steels of other alloy compositions or thicknesses are butt-welded. Such welded components are called "custom welded blanks" or "tailor welded blanks". Laser beam welding has been used as the preferred method for producing such components, which is advantageous in terms of process flexibility, quality and productivity. The blanks produced are then cold pressed to obtain parts with mechanical strength, pressability and shock absorption that vary within the component itself. Thus, the required properties can be provided in the right places without incurring high costs.
[0007] Aluminum coated steel plates comprised solely of the aluminum-iron intermetallic alloy layer described above can also be manufactured from such tailor welded blanks and, by hot pressing with heat and quenching, provided as one part with various thicknesses and unique mechanical properties that ideally meet local loading requirements.
[0008] However, when laser welding steel plates having a coating layer consisting only of the aluminum-iron intermetallic alloy layer, the coating layer is mixed into the molten zone formed during welding, and in particular the Al component, which promotes the formation of ferrite, is concentrated by the convection of the liquid metal and segregates between the dendrites where the liquid fraction with the highest concentration is located during solidification. Therefore, when an austenitization treatment (heating) is performed for the purpose of quenching the welded blank, the Al-rich zone is transformed into ferrite during subsequent cooling. That is, the weld metal part (molten zone) formed by laser welding has a mixed composition of martensite, which has the intended high hardness and strength, and soft ferrite, which is not intended. This causes the weld to break when an external force such as a crash situation is applied during the use of the final part, resulting in the loss of the intended function of the part.
[0009] Therefore, there is a need for a technology that can prevent the formation of ferrite in welded components, which is the source of fracture. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] European Patent Application Publication No. 0971044 Summary of the Invention [Problem to be solved by the invention]
[0011] The present invention aims to provide a method for manufacturing a tailor welded blank using a steel sheet for hot press use having an Al-Fe-based intermetallic alloy layer formed thereon, which can prevent the formation of ferrite, which is a source of fracture in welded parts. [Means for solving the problem]
[0012] The present invention provides a method for producing a tailor welded blank using a steel sheet for hot press use having an Al-Fe-based intermetallic alloy layer formed thereon, the method comprising the steps of: preparing a base steel sheet and a plated steel sheet having an aluminum-based plating layer formed on one or both sides of the base steel sheet; heat treating the plated steel sheet so that the aluminum-based plating layer becomes an Al-Fe-based intermetallic alloy layer; and butt welding the heat-treated plated steel sheet, characterized in that before the welding, a part or all of the Al-Fe-based intermetallic alloy layer located in a region where welding is to be performed is removed. Effect of the Invention
[0013] According to the present invention, it is possible to provide a method for manufacturing a tailor welded blank using a steel sheet for hot press use on which an Al-Fe-based intermetallic alloy layer is formed. [Brief description of the drawings]
[0014] [Figure 1] FIG. 2 is a schematic diagram showing that an aluminum-based plating layer formed on a base steel sheet becomes an Al-Fe-based intermetallic alloy layer by heat treatment. [Diagram 2] FIG. 2 is a schematic diagram showing that a partial region of an Al-Fe-based intermetallic alloy layer formed on a base steel sheet has been removed. [Diagram 3] FIG. 2 is a schematic diagram of a base steel sheet from which a partial region of the Al-Fe-based intermetallic alloy layer has been removed, after butt welding. [Figure 4] 1 is a photograph of a microstructure of a plated steel sheet having an Al-Fe-based intermetallic alloy layer formed thereon, the microstructure being observed with an optical microscope, the plated steel sheet being manufactured according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, a method for producing a tailor welded blank using a steel sheet for hot press use having an Al-Fe-based intermetallic alloy layer formed thereon according to the present invention will be described.
[0016] First, a plated steel sheet having a base steel sheet and an aluminum-based plating layer formed on one or both sides of the base steel sheet is prepared. The plated steel sheet is obtained by immersing the base steel sheet in an aluminum-based plating bath. In the present invention, the type of the base steel sheet is not particularly limited, and any type of steel sheet used in the technical field can be used. However, preferably, a steel sheet having a high strength of 1500 MPa or more after hot forming can be used. In addition, in the present invention, the composition of the aluminum-based plating layer is not particularly limited, and any type of aluminum-based plating layer used in the technical field can be used.
[0017] On the other hand, when the base steel sheet is immersed in an aluminum-based plating bath, intermetallic compounds of several μm in size are crystallized on the surface of the base steel sheet due to a very fast reaction. However, since such intermetallic compounds are relatively brittle, the aluminum-based plating bath may further contain Si as an inhibitor to suppress the growth of the intermetallic compounds. That is, the aluminum-based plating layer may further contain Si, and in this case, the content of Si may be 8 to 12 wt %.
[0018] Thereafter, the plated steel sheet is heat-treated so that the aluminum-based plating layer becomes an Al-Fe-based intermetallic alloy layer. FIG. 1 is a schematic diagram showing how the aluminum-based plating layer formed on the base steel sheet becomes an Al-Fe-based intermetallic alloy layer through heat treatment. As shown in FIG. 1, an aluminum-based plating layer 20 formed on a base steel sheet 10 changes into an Al-Fe-based intermetallic alloy layer 30 as Fe diffuses from the base steel sheet through heat treatment. Meanwhile, the Al-Fe-based intermetallic alloy layer can sometimes be composed of a first layer and a second layer, and in this case, the first layer is composed of FeAl and Fe 3 The second layer contains one or more of Fe and Al. 2 Al 5 The second layer can be present in the form of a layer or islands. When the aluminum-based plating layer contains Si and the Al-Fe-based intermetallic alloy layer also contains Si, the second layer can be present in the form of Al. 2 Fe3 S 3 It may further include:
[0019] The reason why the compositions of the first and second layers are different is due to the difference in the amount of Fe diffused from the base steel sheet. That is, the first layer, which is closer to the base steel sheet, has a higher Fe content than the second layer, which is relatively farther from the base steel sheet, because Fe diffuses more into the first layer. The thickness and structure of the first and second layers may vary depending on the heat treatment temperature and time, but the present invention does not particularly limit the specific conditions. However, it is preferable that the heat treatment temperature is less than Ac1, but if the heat treatment temperature is Ac1 or higher, problems may occur during processing in a coiled state due to changes in the microstructure of the steel sheet.
[0020] Meanwhile, the Al-Fe intermetallic alloy layer formed by the above heat treatment has the advantage of enabling rapid heating during hot forming in a later process, compared to an aluminum-based plating layer formed only by plating without heat treatment. In addition, since the Al-Fe intermetallic alloy layer is formed by the above heat treatment, the thickness of the overall plating layer increases, and the thickness of the aluminum-based plating layer can be reduced. That is, the amount of Al plating can be reduced, and thus the Al content is smaller than that of the existing Al-Si plating layer, making it possible to improve problems such as poor welding. Furthermore, the intermetallic alloy layer of the existing Al-Si plating layer is FeAl 3 and the above FeAl 3 The melting point of the Al-Fe alloy is 1160°C, whereas the first layer of the Al-Fe alloy of the present invention is made of FeAl and Fe 3 Aluminum, which has a higher melting point of 1310°C and has the advantage of providing better corrosion resistance in the heat-affected zone during welding.
[0021] Fig. 2 is a schematic diagram showing that a part of the Al-Fe intermetallic alloy layer formed on the base steel sheet is removed, and Fig. 3 is a schematic diagram showing the state after the base steel sheet from which a part of the Al-Fe intermetallic alloy layer is removed is butt-welded. As shown in Figs. 2 and 3, the present invention is characterized in that a part or all of the Al-Fe intermetallic alloy layer 30 located in the area where welding is performed is removed before the welding. This prevents Al contained in the Al-Fe intermetallic alloy layer from being mixed into the molten area during welding, so that the microstructure of the final product does not contain ferrite, thereby ensuring high strength. It is preferable to remove the Al-Fe intermetallic alloy layer entirely, but even if the Al-Fe intermetallic alloy layer remains after removing a part of it, it does not have a significant effect on ensuring the physical properties of the final product. However, after removing a portion of the Al-Fe-based intermetallic alloy layer, the remaining Al-Fe-based intermetallic alloy layer preferably has a thickness of 10 μm or less. If the thickness exceeds 10 μm, a large amount of Al component is mixed into the weld metal portion during welding, which may result in a decrease in the mechanical properties of the weld portion of the final part after hot forming and quenching.
[0022] In the present invention, the method for removing the Al-Fe intermetallic alloy layer is not particularly limited, and for example, methods such as brushing, grinding, cutting, laser irradiation, and chemical solution immersion can be used. The removal of the Al-Fe intermetallic alloy layer may be performed as a preparatory operation before the welding process, or may be performed immediately before the welding process. Meanwhile, the width W of the removed Al-Fe intermetallic alloy layer may be Wb / 2 to Wb (mm). Here, Wb means the average width of the weld metal part 40 of the tailor welded blank obtained after welding. If the width of the removed Al-Fe intermetallic alloy layer is smaller than Wb / 2, the Al component in the Al-Fe intermetallic alloy layer may be mixed into the weld metal part, and if it is larger than Wb, there is a risk that the corrosion resistance cannot be sufficiently ensured due to excessive removal of the Al-Fe intermetallic alloy layer. Furthermore, when steel plates of different thicknesses are welded, the melted regions of the steel plates may differ from each other, and therefore the widths of the Al-Fe-based intermetallic alloy layers removed from the steel plates may also differ from each other.
[0023] Thereafter, the heat-treated plated steel sheet can be butt-welded to produce a tailor-welded blank. In the present invention, the welding method is not particularly limited, and any method can be used as long as it meets the productivity and quality requirements. For example, laser beam welding, GTAW, plasma welding, GMAW, etc. can be used. According to the present invention, the Al-Fe-based intermetallic alloy layer present in the region where the welding is performed is removed in advance, so that the Al component does not mix with the molten part, and there is an advantage that the physical properties of the weld metal part of the final product obtained by the subsequent hot forming process (austenitizing heat treatment, forming / quenching) are excellent. Meanwhile, after the butt welding, the tailor welded blank obtained can be further subjected to a hot press forming process, so that the final product obtained can be preferably applied to automobile parts and the like.
[0024] The present invention will be described in more detail below with reference to examples. However, the following examples are merely illustrative for explaining the present invention in more detail, and are not intended to limit the scope of the present invention.
[0025] (Example) 22MnB5 steel, a boron steel with a tensile strength of 1500 MPa, which is widely used as a collision material for car bodies, was plated with 10% Si-Al to obtain a cold-rolled plated steel sheet. This cold-rolled plated steel sheet was heat-treated at 500°C to obtain the FeAl, Fe 3 Al, Fe 2 Al 5 , Al 2 Fe 3 S 3 An Al-Fe-based intermetallic alloy layer containing the above was formed. At this time, the thickness of the Al-Fe-based intermetallic alloy layer was about 40 μm based on one side. Thereafter, the above cold-rolled plated steel sheet was cut into a blank having a rectangular shape of 500 × 120 mm, and then a part of the above Al-Fe-based intermetallic alloy layer was removed by each of the methods described below, and the blanks were butt-welded by laser beam welding to produce tailor-welded blanks. The tailor-welded blank was then heated to 920°C and held at that temperature for 4 minutes, followed by hot forming and quenching. The tensile strength, elongation and fracture rate of the welded portion of the tailor-welded blank thus produced were measured and are listed in Table 1 below. Meanwhile, the tailor-welded blank produced above had an average tensile strength of 1470 MPa in the region corresponding to the base steel sheet. Tensile strength and elongation were measured by taking samples from the welded area, preparing five test pieces for each test in accordance with the KS standard, and then measuring the average values by tensile testing at a tensile test speed of 10 mm / min. The fracture rate of the welded joint was expressed as the percentage of specimens in which fracture occurred relative to the number of tensile test specimens during the tensile test.
[0026] In Example 1, the Al-Fe intermetallic alloy layer present at the portion to be welded was removed from both sides using a Q-Switch pulse laser, and the removed width of the Al-Fe intermetallic alloy layer was 1 mm. Then, butt welding was performed using laser beam welding. In Example 2, the Al-Fe intermetallic alloy layer present at the portion to be welded was partially removed from both sides using a Q-Switch pulse laser, the removed width of the Al-Fe intermetallic alloy layer was 1 mm, and the remaining thickness was 5 μm. Then, butt welding was performed using laser beam welding. In Example 3, the Al-Fe intermetallic alloy layer present at the portion to be welded was removed from both sides using grinding equipment, and the removed width of the Al-Fe intermetallic alloy layer was 1 mm. Then, butt welding was performed using laser beam welding.
[0027] In Comparative Example 1, butt welding was performed using laser beam welding without removing the Al-Fe intermetallic alloy layer. During welding with the above laser beam, the beam diameter at the focal distance is approximately 0.4 mm. 2 A laser welding machine was used, and 20 liters of He gas per minute was used as the shielding gas, with the laser power set to 6 kW and the welding speed set to 6 m / min.
[0028] [Table 1] As can be seen from Table 1 above, Examples 1 to 3 manufactured to meet the conditions of the present invention have strength and high elongation at a level similar to that of the base steel sheet, whereas Comparative Example 1, which does not meet the conditions of the present invention, is inferior in both strength and elongation. [Explanation of symbols]
[0029] 10, 10': Base steel plate 20: Aluminum-based plating layer 30, 30': Al-Fe intermetallic alloy layer 40: Welded metal parts
Claims
1. preparing a plated steel sheet having a base steel sheet and an aluminum-based plating layer formed on one or both sides of the base steel sheet; heat treating the plated steel sheet so that the aluminum-based plating layer becomes an Al-Fe-based intermetallic alloy layer; butt welding the heat treated plated steel sheet; the Al-Fe-based intermetallic alloy layer comprises a first layer and a second layer, The first layer contains at least one of FeAl and Fe 3 Al, the second layer comprises Fe 2 Al 5 ; A method for producing a tailor welded blank using a steel sheet for hot press use having an Al-Fe-based intermetallic alloy layer formed thereon, characterized in that, before the welding, a part or all of the Al-Fe-based intermetallic alloy layer located in an area where welding is to be performed is removed.
2. The method for manufacturing a tailor welded blank using a steel sheet for hot press having an Al-Fe-based intermetallic alloy layer formed thereon according to claim 1, wherein the aluminum-based plating layer further contains Si.
3. the Al-Fe-based intermetallic alloy layer comprises a first layer and a second layer, The first layer is made of FeAl and Fe 3 Al, The second layer is Fe 2 A 5 and Al 2 Fe 3 S 3 The method for producing a tailor welded blank using the steel plate for hot press use having an Al-Fe based intermetallic alloy layer formed thereon according to claim 2, characterized in that the steel plate contains one or more of the following:
4. The method for manufacturing a tailor welded blank using a steel plate for hot press use having an Al-Fe-based intermetallic alloy layer formed thereon according to claim 1, characterized in that the temperature during the heat treatment is lower than Ac1.
5. 2. The method for manufacturing a tailor welded blank using a steel sheet for hot press on which an Al-Fe-based intermetallic alloy layer has been formed, as set forth in claim 1, characterized in that after removing a portion of the Al-Fe-based intermetallic alloy layer, the remaining Al-Fe-based intermetallic alloy layer has a thickness of 10 μm or less.
6. The method for manufacturing a tailor welded blank using a steel plate for hot press use having an Al-Fe-based intermetallic alloy layer formed thereon according to claim 1, characterized in that a width of the Al-Fe-based intermetallic alloy layer to be removed is Wb / 2 to Wb (mm). (Wb means the average width of the weld metal part of the tailor welded blank obtained after welding.)
7. The method for manufacturing a tailor welded blank using a hot press steel plate having an Al-Fe-based intermetallic alloy layer formed thereon according to claim 1, further comprising a hot press forming process after the butt welding.
Citation Information
Patent Citations
Clad hot-rolled and cold-rolled steel sheet, presenting a very high resistance after thermal treatment
EP0971044A1
Method for manufacturing pre-coated metal sheets
JP2019505387A
Tailored blank and method for manufacturing steel plate for tailored blank
JP2020189336A
Process and System for Laser Welding Pre-Coated Sheet Metal Workpieces
US20170095886A1
Steel sheet plated with al-fe for hot press forming having excellent corrosion resistance and spot weldability, and manufacturing method thereof
WO2020111881A1