Resin composition and molded article

The resin composition addresses low bio-based content and mixing issues by using a block copolymer with a high-biobased plasticizer, enhancing moldability and reducing environmental impact while preventing oil bleed.

JP7578863B2Active Publication Date: 2024-11-06KURARAY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024524977
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-09-30
Filing Date
2023-07-31
Publication Date
2024-11-06
Estimated Expiration
2043-07-31

AI Technical Summary

Technical Problem

Existing resin compositions using plant-derived plasticizers have low bio-based content and environmental impact reduction, and vegetable oils face mixing difficulties, leading to oil bleed issues.

Method used

A resin composition incorporating a block copolymer containing aromatic vinyl and conjugated diene compounds with a biomass-derived plasticizer having a biobased degree of 70% or more and specific kinematic viscosity, along with optional polyolefin resin and tackifier, to enhance moldability and reduce environmental load.

Benefits of technology

The composition achieves excellent moldability, reduced environmental impact, and minimizes oil bleed, providing a high biobased content suitable for various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578863000039
    Figure 0007578863000039
  • Figure 0007578863000001
    Figure 0007578863000001
  • Figure 0007578863000002
    Figure 0007578863000002
Patent Text Reader

Abstract

Provided are: a resin composition that exhibits an excellent moldability and contains material that can lessen the environmental impact; and a molded article that uses this resin composition. This resin composition comprises: (I) a block copolymer that contains a polymer block (a1) containing an aromatic vinyl compound-derived structural unit and a polymer block (a2) containing a conjugated diene compound-derived structural unit; and (II) a biomass-derived plasticizer that does not have the carboxy group. The biobased content of the plasticizer (II) is at least 70 mass%.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition and a molded article, and more particularly to a resin composition containing a material capable of reducing the environmental load and having excellent moldability, and a molded article made using the resin composition. [Background technology]

[0002] Thermoplastic resins are lightweight and have excellent moldability, and some of them also have excellent strength and heat resistance, etc., and therefore are widely used in various packaging materials, home appliances, machine parts, automobile parts, industrial parts, etc. In addition, due to growing environmental awareness, there is an increasing demand for using biomass-derived raw materials for these components. Technologies have been disclosed that use plant-derived plasticizers and vegetable oils (sunflower oil, linseed oil) as biomass-derived raw materials to impart various physical properties while being mindful of reducing the environmental burden (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Special Publication No. 2019-529688 Summary of the Invention [Problem to be solved by the invention]

[0004] However, when the plant-derived plasticizer described in Patent Document 1 is used, the bio-based degree is low and the reduction in environmental impact is insufficient. Furthermore, when vegetable oil is used, it is difficult to mix it with the resin component, and oil bleeding occurs.

[0005] Therefore, an object of the present invention is to provide a resin composition containing a material capable of reducing the environmental load and having excellent moldability, and a molded article obtained by using the resin composition. [Means for solving the problem]

[0006] As a result of intensive research aimed at solving the above problems, the present inventors have conceived the following invention and found that the above problems can be solved. That is, the present invention is as follows.

[0007] [1] A resin composition comprising: a block copolymer (I) including a polymer block (a1) containing a structural unit derived from an aromatic vinyl compound and a polymer block (a2) containing a structural unit derived from a conjugated diene compound; and a biomass-derived plasticizer (II) having no carboxy group, wherein the bio-based content of the plasticizer (II) is 70 mass% or more. [2] The resin composition according to the above [1], wherein the plasticizer (II) has a kinetic viscosity at 40°C of 100.0 cSt or less. [3] The resin composition according to the above [1] or [2], wherein the plasticizer (II) is at least one of a compound represented by the following general formula (1) and a compound represented by the following general formula (2): [ka] In the general formula (1), n 1 ~n 3 are each independently 1 or 3; R 1 ~R 6 are each independently a hydrogen atom or an unsubstituted hydrocarbon group; R 1 and R 2 The total number of carbon atoms is 14, and R 3 and R 4 The total number of carbon atoms is 14, and R 5 and R 6 The total number of carbon atoms is 14, and R 1 ~R 6 may have a branched structure. [ka] In the general formula (2), n 4 and n 5 are each independently 1 or 3; R 7 ~R 10are each independently a hydrogen atom or an unsubstituted hydrocarbon group; R 7 and R 8 The total number of carbon atoms is 14, and R 9 and R 10 The total number of carbon atoms is 14, and R 7 ~R 10 may have a branched structure. [4] The resin composition according to any one of the above [1] to [3], wherein the aromatic vinyl compound in the polymer block (a1) in the block copolymer (I) is at least one selected from the group consisting of styrene, α-methylstyrene, and 4-methylstyrene. [5] The resin composition according to any one of the above [1] to [4], wherein the content of the aromatic vinyl compound in the polymer block (a1) in the block copolymer (I) is 1 to 65 mass %. [6] The resin composition according to any one of the above [1] to [5], wherein the block copolymer (I) has a weight average molecular weight of 50,000 to 600,000 as calculated in terms of standard polystyrene by gel permeation chromatography. [7] The resin composition according to any one of the above [1] to [6], wherein the vinyl bond content in the polymer block (a2) of the block copolymer (I) is 1.0 to 40.0 mol %. [8] The resin composition according to any one of the above [1] to [7], wherein the hydrogenation rate of carbon-carbon double bonds in the structural units derived from the conjugated diene compound in the block copolymer (I) is 5.0 mol % or more. [9] The resin composition according to the above [8], wherein the hydrogenation rate of carbon-carbon double bonds in the structural units derived from the conjugated diene compound in the block copolymer (I) is 30.0 mol % or more.

[10] The resin composition according to the above [9], wherein the hydrogenation rate of carbon-carbon double bonds in the structural units derived from the conjugated diene compound in the block copolymer (I) is 70.0 mol % or more.

[11] The resin composition according to any one of the above [1] to

[10] , comprising 1 to 1,500 parts by mass of the plasticizer (II) per 100 parts by mass of the block copolymer (I).

[12] The resin composition according to any one of the above [1] to

[11] , comprising 1 to 200 parts by mass of a polyolefin resin (III) per 100 parts by mass of the block copolymer (I).

[13] The resin composition according to

[12] above, wherein the polyolefin resin (III) comprises polyethylene and / or polypropylene.

[14] The resin composition according to the above

[12] , wherein the polyolefin resin (III) is polypropylene.

[15] The resin composition according to the above

[12] , wherein the polyolefin resin (III) is polyethylene.

[16] The resin composition according to any one of the above [1] to

[15] , further comprising 1 to 300 parts by mass of a tackifier (IV) per 100 parts by mass of the block copolymer (I).

[17] The resin composition according to any one of the above [1] to

[16] , wherein the resin composition has a bio-based content of 15 mass % or more.

[18] A molded article obtained by using the resin composition according to any one of the above [1] to

[17] . Effect of the Invention

[0008] According to the present invention, it is possible to provide a resin composition containing a material capable of reducing the environmental load and having excellent moldability, and a molded article made using the resin composition. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is a diagram for explaining a tensile test (forward stress, return stress, stress relaxation) of a film as a molded article obtained by using the resin composition of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, the present invention will be described based on an example of an embodiment. However, the embodiment shown below is an example for embodying the technical idea of ​​the present invention, and the present invention is not limited to the following description. Any selected or combined embodiment of the items described in this specification is also included in the present invention. In this specification, preferred definitions may be selected arbitrarily, and combinations of preferred definitions may be considered more preferred. In this specification, the expression "XX to YY" means "at least XX and at most YY." In this specification, the lower limit and upper limit described in stages for the preferred numerical range (e.g., range of content, etc.) can be independently combined. For example, the description "preferably 10 to 90, more preferably 30 to 60" can be combined with the "preferable lower limit (10)" and the "more preferable upper limit (60)" to form "10 to 60."

[0011] In this specification, the term "bio-based content" is an index showing the content ratio of bio-derived materials in a target substance, as measured in accordance with ASTM D6866-21. For example, the term "bio-based content of a resin composition" refers to the content ratio of bio-derived raw materials in a resin composition, as measured in accordance with ASTM D6866-21. The term "bio-based content of a resin" refers to the content ratio of bio-derived raw materials in a resin, as measured in accordance with ASTM D6866-21.

[0012] <Resin composition> The resin composition of this embodiment contains a block copolymer (I) and a plasticizer (II), and further contains a polyolefin resin (III), a tackifier (IV), and additives, as necessary.

[0013] [Block copolymer (I)] The resin composition of this embodiment contains the block copolymer (I), and thus has good flexibility, which makes it easier to suppress deterioration of physical properties at low temperatures, and can exhibit excellent moldability. The block copolymer (I) contains a polymer block (a1) containing a structural unit derived from an aromatic vinyl compound, and a polymer block (a2) containing a structural unit derived from a conjugated diene compound (excluding the polymer block (a1)). The block copolymer (I) may be used alone or in combination of two or more kinds.

[0014] (Polymer block (a1)) The polymer block (a1) in the block copolymer (I) contains a structural unit derived from an aromatic vinyl compound. Examples of such aromatic vinyl compounds include styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 4-propylstyrene, 4-t-butylstyrene, 4-cyclohexylstyrene, 4-dodecylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 2,4,6-trimethylstyrene, 2-ethyl-4-benzylstyrene, 4-(phenylbutyl)styrene, 1-vinylnaphthalene, 2-vinylnaphthalene, vinylanthracene, N,N-diethyl-4-aminoethylstyrene, vinylpyridine, 4-methoxystyrene, monochlorostyrene, dichlorostyrene, and divinylbenzene. These aromatic vinyl compounds may be used alone or in combination of two or more. Among these, styrene, α-methylstyrene, and 4-methylstyrene are preferred, and styrene is more preferred.

[0015] The polymer block (a1) may contain a structural unit derived from a monomer other than an aromatic vinyl compound, for example, a monomer constituting the polymer block (a2) described below. However, the content of the structural unit derived from an aromatic vinyl compound in the polymer block (a1) is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, and particularly preferably 100% by mass.

[0016] The content of the polymer block (a1) in the block copolymer (I) is preferably 1 to 65% by mass, more preferably 5 to 60% by mass, even more preferably 5 to 50% by mass, even more preferably 10 to 40% by mass, and even more preferably 10 to 35% by mass. When the content is 1% by mass or more, the resin composition is likely to exhibit excellent moldability. When the content is 65% by mass or less, it is expected that the resin composition will exhibit tear strength, tensile properties, and the like while having sufficient flexibility. When the block copolymer (I) contains a plurality of polymer blocks (a1), the total amount of the plurality of polymer blocks (a1) is preferably within the above range.

[0017] (Polymer block (a2)) The polymer block (a2) in the block copolymer (I) is a polymer block containing a structural unit derived from a conjugated diene compound. Examples of the conjugated diene compound include isoprene, butadiene, farnesene, 2,3-dimethyl-butadiene, 2-phenyl-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, 1,3-octadiene, 1,3-cyclohexadiene, 2-methyl-1,3-octadiene, 1,3,7-octatriene, myrcene, chloroprene, etc. These may be used alone or in combination of two or more. Among these, isoprene, butadiene, farnesene, and myrcene are preferred, and isoprene, butadiene, and farnesene are more preferred.

[0018] The polymer block (a2) containing a structural unit derived from a conjugated diene compound may be composed of structural units derived from only one of these conjugated diene compounds, or may be composed of structural units derived from two or more of these conjugated diene compounds, and is particularly preferably composed of structural units derived from butadiene, isoprene, or farnesene, or structural units derived from butadiene and isoprene.

[0019] The farnesene may be either α-farnesene or β-farnesene represented by the following formula (1), but β-farnesene is preferred from the viewpoint of ease of production of the block copolymer (I). Note that α-farnesene and β-farnesene may be used in combination.

[0020] [ka]

[0021] The polymer block (a2) containing a structural unit derived from a conjugated diene compound is preferably a polymer block containing 70% by mass or more of the structural unit derived from a conjugated diene compound, more preferably 80% by mass or more of the structural unit, even more preferably 90% by mass or more of the structural unit, even more preferably 95% by mass or more of the structural unit, and particularly preferably 100% by mass of the structural unit. The polymer block (a2) may contain only the structural unit derived from a conjugated diene compound, but may also contain a structural unit derived from another copolymerizable monomer together with the structural unit, as long as it does not interfere with the present invention. Examples of the other copolymerizable monomer include styrene, α-methylstyrene, and 4-methylstyrene. When the polymer block (a2) contains a structural unit derived from another copolymerizable monomer, the proportion of the structural unit derived from the other copolymerizable monomer is preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less, based on the total amount of the structural unit derived from the conjugated diene compound and the structural unit derived from the other copolymerizable monomer.

[0022] (Polymer block (a3)) The block copolymer (I) may further contain a polymer block (a3) ​​containing a structural unit derived from a conjugated diene compound, in addition to the above-mentioned polymer block (a1) and polymer block (a2). It should be noted that the block (a2) and the block (a3) ​​are not the same polymer block.

[0023] Examples of the conjugated diene compound constituting the structural unit derived from a conjugated diene compound include the same conjugated diene compounds constituting the structural unit derived from a conjugated diene compound in the above-mentioned polymer block (a2), and preferred examples are also the same.

[0024] Furthermore, the polymer block (a3) ​​may contain structural units other than the structural units derived from the conjugated diene compound. The content of the structural unit derived from the conjugated diene compound in the polymer block (a3) ​​is preferably 70 to 100 mass%, more preferably 80 to 100 mass%, even more preferably 90 to 100 mass%, even more preferably 95 to 100 mass%, and particularly preferably 100 mass%.

[0025] (combined form) The block copolymer (I) is a block copolymer containing at least one polymer block (a1) and at least one polymer block (a2). The bonding form of the polymer block (a1) and the polymer block (a2) is not particularly limited and may be linear, branched, radial, or a combination of two or more thereof. Among these, a form in which each block is bonded linearly is preferred. As a linear bonding form, when the polymer block (a1) is represented by A and the polymer block (a2) is represented by B, the bond form is (AB). l , A-(BA) m , or B-(AB) n Here, the l, m and n each independently represent an integer of 1 or more. When the block copolymer (I) contains at least one each of the polymer block (a1) and the polymer block (a2), it is preferable that the block copolymer (I) is a triblock copolymer represented by ABA, having blocks in the order of the polymer block (a1), the polymer block (a2), and the polymer block (a1). That is, the block copolymer (I) is preferably a triblock copolymer represented by ABA, and the triblock copolymer may be either an unhydrogenated product or a hydrogenated product.

[0026] The block copolymer (I) may also be a block copolymer containing at least two polymer blocks (a1), at least one polymer block (a2), and at least one polymer block (a3).

[0027] When the block copolymer (I) contains the polymer block (a1), the polymer block (a2) and the polymer block (a3), the bonding form of the multiple polymer blocks is not particularly limited and may be linear, branched, radial or a combination of two or more thereof. Among these, a form in which each block is bonded linearly is preferred.

[0028] Here, in this specification, when the same type of polymer blocks are linearly bonded via a divalent coupling agent or the like, the entirety of the bonded polymer blocks is treated as one polymer block. Accordingly, a polymer block that should be strictly represented as AXA (X represents a coupling agent residue) is represented as A as a whole. In this specification, since this type of polymer block containing a coupling agent residue is treated as above, for example, a block copolymer containing a coupling agent residue and that should be strictly represented as BACXCAB is represented as BACAB and treated as an example of a pentablock copolymer.

[0029] In addition, the two or more polymer blocks (a1) in the block copolymer (I) may be polymer blocks consisting of the same structural units or different structural units. Similarly, when the block copolymer (I) has two or more polymer blocks (a2) or two or more polymer blocks (a3), each polymer block may be a polymer block consisting of the same structural units or different structural units. For example, in the two polymer blocks (a1) in a triblock copolymer represented by ABA, the types of aromatic vinyl compounds may be the same or different.

[0030] When the block copolymer (I) contains the polymer block (a1) and the polymer block (a2) but does not contain the polymer block (a3), the mass ratio of the polymer block (a1) to the polymer block (a2) [(a1) / (a2)] is preferably 1 / 99 to 65 / 35, more preferably 5 / 95 to 60 / 40, even more preferably 10 / 90 to 50 / 50, even more preferably 15 / 85 to 40 / 60, and even more preferably 15 / 85 to 35 / 65. When it is within the above range, a resin composition having excellent flexibility and even more excellent moldability can be obtained. When the block copolymer (I) contains the polymer block (a1), the polymer block (a2) and the polymer block (a3), the mass ratio of the polymer block (a1) to the polymer block (a2) [(a1) / (a2)] is preferably 1 / 99 to 70 / 30, more preferably 5 / 95 to 60 / 40, even more preferably 10 / 90 to 50 / 50, even more preferably 20 / 80 to 40 / 60, and even more preferably 25 / 75 to 35 / 65. When it is within the above range, a resin composition having excellent flexibility and even more excellent moldability can be obtained.

[0031] In the block copolymer (I), the mass ratio of the polymer block (a1) to the total amount of the polymer block (a2) and the polymer block (a3) ​​[(a1) / ((a2)+(a3))] is preferably 1 / 99 to 65 / 35. The mass ratio [(a1) / ((a2)+(a3))] is more preferably 5 / 95 to 60 / 40, even more preferably 10 / 90 to 40 / 60, even more preferably 10 / 90 to 30 / 70, and even more preferably 15 / 85 to 25 / 75.

[0032] When the block copolymer (I) contains the polymer block (a1) and the polymer block (a2) but does not contain the polymer block (a3), the total content of the polymer block (a1) and the polymer block (a2) in the block copolymer is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and even more preferably 100% by mass. One embodiment of the block copolymer (I) is, for example, a block copolymer consisting of at least one polymer block (a1) and at least one polymer block (a2). When the block copolymer (I) contains the polymer block (a1) and the polymer block (a2) but does not contain the polymer block (a3), examples of the block copolymer (I) include an (a1)-(a2) diblock copolymer, an (a1)-(a2)-(a1) triblock copolymer, an (a1)-(a2)-(a1)-(a2) tetrablock copolymer, an (a2)-(a1)-(a2)-(a1)-(a2) pentablock copolymer, an (a2)-(a1)-(a2)-(a1)-(a2)-(a1) hexablock copolymer, an ((a1)-(a2)) n -X (X represents a coupling agent residue, and n represents an integer of 2 or more), and a hyperbranched block copolymer represented by ((a2)-(a1)-(a2)) n Preferred embodiments include multi-branched block copolymers represented by -X (X represents a coupling agent residue, and n represents an integer of 2 or more), of which (a1)-(a2) diblock copolymers, (a1)-(a2)-(a1) triblock copolymers, (a1)-(a2)-(a1)-(a2) tetrablock copolymers, and (a2)-(a1)-(a2)-(a1)-(a2) pentablock copolymers are more preferred, (a1)-(a2) diblock copolymers, (a1)-(a2)-(a1) triblock copolymers, and (a1)-(a2)-(a1)-(a2) tetrablock copolymers are even more preferred, and (a1)-(a2)-(a1) triblock copolymers and (a1)-(a2)-(a1)-(a2) tetrablock copolymers are even more preferred. When the block copolymer (I) contains the polymer block (a1), the polymer block (a2) and the polymer block (a3), the total content of the polymer blocks (a1) to (a3) ​​in the block copolymer is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and even more preferably 100% by mass. One embodiment of the block copolymer (I) is, for example, a block copolymer consisting of at least one polymer block (a1), at least one polymer block (a2) and at least one polymer block (a3).

[0033] (Polymer blocks composed of other monomers) The block copolymer (I) may contain, in addition to the polymer block (a1), the polymer block (a2) and the polymer block (a3), a polymer block composed of another monomer, so long as the effect of the present invention is not impaired.

[0034] Examples of such other monomers include functional group-containing unsaturated compounds such as acrylic acid, methacrylic acid, methyl acrylate, methyl methacrylate, acrylonitrile, methacrylonitrile, maleic acid, fumaric acid, crotonic acid, itaconic acid, 2-acryloylethanesulfonic acid, 2-methacryloylethanesulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, 2-methacrylamido-2-methylpropanesulfonic acid, vinylsulfonic acid, vinyl acetate, and methyl vinyl ether. These may be used alone or in combination of two or more. When the block copolymer (I) has a polymer block constituted by another monomer, the content thereof is preferably 10% by mass or less, more preferably 5% by mass or less.

[0035] (Method for Producing Block Copolymer (I)) When the block copolymer (I) is, for example, a block copolymer containing polymer block (a1) and polymer block (a2), or a block copolymer containing polymer block (a1), polymer block (a2), and polymer block (a3), it can be suitably produced by a polymerization step of obtaining a block copolymer by anionic polymerization. Furthermore, when the block copolymer (I) is a hydrogenated block copolymer, it can be suitably produced by a step of hydrogenating a carbon-carbon double bond in a structural unit derived from a conjugated diene compound in the block copolymer.

[0036] ((Polymerization process)) The block copolymer (I) can be produced by a solution polymerization method or the methods described in JP-A-2012-502135 and JP-A-2012-502136, etc. Among these, the solution polymerization method is preferred, and known methods such as ionic polymerization methods such as anionic polymerization and cationic polymerization, and radical polymerization methods can be applied. Among these, the anionic polymerization method is preferred. In the anionic polymerization method, an aromatic vinyl compound and a conjugated diene compound are successively added in the presence of a solvent, an anionic polymerization initiator, and, if necessary, a Lewis base to obtain a block copolymer. Examples of the anionic polymerization initiator include alkali metals such as lithium, sodium, and potassium; alkaline earth metals such as beryllium, magnesium, calcium, strontium, and barium; lanthanoid rare earth metals such as lanthanum and neodymium; and compounds containing the alkali metals, alkaline earth metals, and lanthanoid rare earth metals. Among these, compounds containing an alkali metal or an alkaline earth metal are preferred, and organic alkali metal compounds are more preferred.

[0037] Examples of the organic alkali metal compound include organic lithium compounds such as methyl lithium, ethyl lithium, n-butyl lithium, sec-butyl lithium, t-butyl lithium, hexyl lithium, phenyl lithium, stilbene lithium, dilithiomethane, dilithionaphthalene, 1,4-dilithiobutane, 1,4-dilithio-2-ethylcyclohexane, and 1,3,5-trilithiobenzene; sodium naphthalene, and potassium naphthalene. Among these, organolithium compounds are preferred, n-butyllithium and sec-butyllithium are more preferred, and sec-butyllithium is even more preferred. The organoalkali metal compounds may be reacted with secondary amines such as diisopropylamine, dibutylamine, dihexylamine, and dibenzylamine to form organoalkali metal amides. The amount of the organic alkali metal compound used in the polymerization varies depending on the molecular weight of the block copolymer (I), but is usually in the range of 0.01 to 3 mass % based on the total amount of the aromatic vinyl compound and the conjugated diene compound.

[0038] The solvent is not particularly limited as long as it does not adversely affect the anionic polymerization reaction, and examples thereof include saturated aliphatic hydrocarbons such as n-pentane, isopentane, n-hexane, n-heptane, and isooctane; saturated alicyclic hydrocarbons such as cyclopentane, cyclohexane, and methylcyclopentane; and aromatic hydrocarbons such as benzene, toluene, and xylene. These may be used alone or in combination of two or more. There is no particular limit to the amount of the solvent used.

[0039] The Lewis base plays a role in controlling the microstructure of the structural unit derived from the conjugated diene compound. Examples of such Lewis bases include ether compounds such as dibutyl ether, diethyl ether, tetrahydrofuran, dioxane, and ethylene glycol diethyl ether; pyridine; tertiary amines such as N,N,N',N'-tetramethylethylenediamine and trimethylamine; alkali metal alkoxides such as potassium t-butoxide; and phosphine compounds. When using a Lewis base, the amount is usually preferably in the range of 0.01 to 1000 molar equivalents per mole of the anionic polymerization initiator.

[0040] The temperature of the polymerization reaction is usually in the range of about -80 to +150°C, preferably 0 to 100°C, and more preferably 10 to 90°C. The polymerization reaction may be carried out batchwise or continuously. The block copolymer (I) can be produced by continuously or intermittently supplying each monomer to the polymerization reaction liquid so that the amounts of the aromatic vinyl compound and the conjugated diene compound present in the polymerization reaction system are within a specific range, or by sequentially polymerizing each monomer in the polymerization reaction liquid so that the ratio of each monomer is specific. The polymerization reaction can be terminated by adding an alcohol such as methanol or isopropanol as a polymerization terminator. The block copolymer can be isolated by pouring the resulting polymerization reaction solution into a poor solvent such as methanol to precipitate the block copolymer, or by washing the polymerization reaction solution with water, separating it, and then drying it.

[0041] An example of a preferred embodiment of the block copolymer (I) is a structure having polymer block (a1), polymer block (a2), and polymer block (a1) in this order. Therefore, a process for obtaining block copolymer (I) by producing polymer block (a1), polymer block (a2), and polymer block (a1) in this order is preferred. In the case of a hydrogenated product, it is more preferred to produce hydrogenated block copolymer (I) by a method further including a process for hydrogenating the obtained block copolymer (I).

[0042] In producing the block copolymer (I), a coupling agent can be used from the viewpoint of efficient production. Examples of the coupling agent include divinylbenzene; polyfunctional epoxy compounds such as epoxidized 1,2-polybutadiene, epoxidized soybean oil, and tetraglycidyl-1,3-bisaminomethylcyclohexane; halides such as tin tetrachloride, tetrachlorosilane, trichlorosilane, trichloromethylsilane, dichlorodimethylsilane, and dibromodimethylsilane; methyl benzoate, ethyl benzoate, phenyl benzoate, diethyl oxalate, diethyl malonate, diethyl adipate, dimethyl phthalate, Examples of suitable silane compounds include ester compounds such as dimethyl terephthalate; carbonate compounds such as dimethyl carbonate, diethyl carbonate, and diphenyl carbonate; alkoxysilane compounds such as diethoxydimethylsilane, trimethoxymethylsilane, triethoxymethylsilane, tetramethoxysilane, tetraethoxysilane, tetrabutoxysilane, tetrakis(2-ethylhexyloxy)silane, bis(triethoxysilyl)ethane, and 3-aminopropyltriethoxysilane; and 2,4-tolylene diisocyanate.

[0043] ((Hydrogenation process)) The block copolymer (I) may be hydrogenated by subjecting the block copolymer obtained by the above-mentioned method to a hydrogenation process. One of the preferred embodiments of the block copolymer (I) is the hydrogenated block copolymer (I). The hydrogenation method may be a known method. For example, the hydrogenation reaction is carried out in the presence of a hydrogenation catalyst such as a Ziegler catalyst; a nickel, platinum, palladium, ruthenium or rhodium metal catalyst supported on carbon, silica, diatomaceous earth, or an organometallic complex having a cobalt, nickel, palladium, rhodium or ruthenium metal; in a solution of the block copolymer (I) dissolved in a solvent that does not affect the hydrogenation reaction. In the hydrogenation step, a hydrogenation reaction may be carried out by adding a hydrogenation catalyst to the polymerization reaction solution containing the block copolymer obtained by the above-mentioned method for producing the block copolymer (I). In the present invention, the hydrogenation catalyst is preferably palladium carbon in which palladium is supported on carbon. In the hydrogenation reaction, the hydrogen pressure is preferably 0.1 to 20 MPa, the reaction temperature is preferably 100 to 200° C., and the reaction time is preferably 1 to 20 hours.

[0044] The hydrogenation rate of the carbon-carbon double bonds in the structural units derived from the conjugated diene compound in the block copolymer (I) is preferably 5.0 mol% or more. From the viewpoint of heat resistance and weather resistance, the hydrogenation rate of the carbon-carbon double bonds in the structural units derived from the conjugated diene compound is more preferably 10.0 mol% or more, even more preferably 20.0 mol% or more, even more preferably 25.0 mol% or more, and particularly preferably 30.0 mol% or more. The hydrogenation rate of the carbon-carbon double bond in the structural unit derived from the conjugated diene compound in the block copolymer (I) is preferably 70.0 mol% or more. From the viewpoint of heat resistance and weather resistance, the hydrogenation rate of the carbon-carbon double bond in the structural unit derived from the conjugated diene compound is more preferably 75.0 mol% or more, even more preferably 80.0 mol% or more, even more preferably 85.0 mol% or more, and particularly preferably 90.0 mol% or more. In the case of an embodiment in which weather resistance is particularly important, the hydrogenation rate is preferably 93.0 mol% or more, more preferably 95.0% mol% or more, and even more preferably 97.0 mol% or more. There is no particular restriction on the upper limit of the hydrogenation rate, and a block copolymer having a hydrogenation rate of substantially 100.0 mol% can also be preferably used. From the viewpoint of selectively and stably hydrogenating only the carbon-carbon double bond in the structural unit derived from the conjugated diene compound in the block copolymer (I), the upper limit of the hydrogenation rate is preferably 99.7 mol% or less, and more preferably 99.5 mol% or less. The hydrogenation rate is the ratio of the block copolymer (I) before hydrogenation to the block copolymer (I) after hydrogenation. 1 It can be calculated by measuring H-NMR.

[0045] The above hydrogenation rate is the hydrogenation rate of the carbon-carbon double bonds in all structural units derived from the conjugated diene compound present in the block copolymer (I). An example of the carbon-carbon double bond in the structural unit derived from a conjugated diene compound present in the block copolymer (I) is a carbon-carbon double bond in the structural unit derived from a conjugated diene compound in the polymer block (a2). In this specification, although the polymer block (a2) and the polymer block (a3) ​​in the hydrogenated block copolymer (I) have been hydrogenated, they are referred to as "polymer block (a2)" and "polymer block (a3)" in the same manner as before hydrogenation.

[0046] In this embodiment, an unmodified block copolymer may be used, but a block copolymer modified as described below may also be used. In the case of a modified block copolymer, the block copolymer may be modified after the hydrogenation step. Examples of functional groups that can be introduced by modification include amino groups, alkoxysilyl groups, hydroxyl groups, epoxy groups, carboxy groups, carbonyl groups, mercapto groups, isocyanate groups, and acid anhydride groups. As a method for modifying the block copolymer, for example, a method in which the isolated and hydrogenated block copolymer is grafted with a modifying agent such as maleic anhydride can be mentioned. The block copolymer can also be modified before the hydrogenation step. A specific method includes adding a coupling agent such as tin tetrachloride, tetrachlorosilane, dichlorodimethylsilane, dimethyldiethoxysilane, tetramethoxysilane, tetraethoxysilane, 3-aminopropyltriethoxysilane, tetraglycidyl-1,3-bisaminomethylcyclohexane, 2,4-tolylenediisocyanate, a polymerization end modifier such as 4,4'-bis(diethylamino)benzophenone, N-vinylpyrrolidone, or other modifiers described in JP-A-2011-132298, which can react with the polymerization active terminal, before adding a polymerization terminator. The position where the functional group is introduced may be the polymerization terminal or the side chain of the block copolymer. The functional group may be one type or a combination of two or more types. The modifier is preferably used in an amount of 0.01 to 10 molar equivalents per mole of the anionic polymerization initiator.

[0047] (Weight average molecular weight and molecular weight distribution) The weight average molecular weight (Mw) of the block copolymer (I) is preferably from 50,000 to 600,000, more preferably from 100,000 to 500,000, and even more preferably from 150,000 to 300,000, from the viewpoint of moldability. The molecular weight distribution (Mw / Mn) of the block copolymer (I) is preferably from 1 to 6, more preferably from 1 to 4, even more preferably from 1 to 3, and even more preferably from 1 to 2. When the molecular weight distribution is within the above range, the viscosity of the block copolymer (I) varies little, making it easy to handle. In this specification, the weight average molecular weight (Mw) and the molecular weight distribution (Mw / Mn) are values ​​measured by the method described in the examples described later.

[0048] The total weight average molecular weight (Mw) of the polymer blocks (a1) in the block copolymer (I) is preferably from 2,000 to 100,000, more preferably from 4,000 to 80,000, even more preferably from 5,000 to 70,000, and even more preferably from 6,000 to 65,000, from the viewpoint of moldability.

[0049] When the structural unit constituting the polymer block (a2) in the block copolymer (I) is any one of an isoprene unit, a butadiene unit, and a mixed unit of isoprene and butadiene, the bonding form of each of the isoprene and butadiene can be a 1,2-bond or a 1,4-bond in the case of butadiene, and a 1,2-bond, a 3,4-bond or a 1,4-bond in the case of isoprene.

[0050] In the block copolymer (I), the total content of 3,4-bond units and 1,2-bond units in the polymer block (a2) (hereinafter, sometimes simply referred to as "vinyl bond content") is preferably 1.0 to 40.0 mol%, more preferably 1.0 to 35.0 mol%, even more preferably 1.0 to 30.0 mol%, and even more preferably 1.0 to 25.0 mol%, or may be 1.0 to 20.0 mol%, 1.0 to 15.0 mol%, or 1.0 to 10.0 mol%. If it is within the above range, it is suitable for suppressing deterioration of physical properties at low temperatures. Here, the vinyl bond content is the total content of 3,4-bond units and 1,2-bond units relative to the total amount of structural units derived from butadiene and isoprene in the polymer block (a2), and can be calculated according to the method described in the Examples. 1 This value was calculated by H-NMR measurement.

[0051] [Plasticizer (II)] The resin composition of this embodiment contains the plasticizer (II), and as a result, the moldability and flowability are improved. Furthermore, the resin composition of this embodiment has good durability (compression set) by containing the plasticizer (II). The mechanism of action of the good durability (compression set) by containing the plasticizer (II) is that the plasticizer (II) has a relatively low viscosity, but a high molecular weight, and contains few naphthene components and aromatic components, so it does not corrode the polymer block (a1) in the block copolymer (I), does not lower the glass transition point, and maintains durability at high temperatures. The content of the plasticizer (II) in the resin composition of this embodiment is not particularly limited, and is preferably 10% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more. In addition, the resin composition of this embodiment is sufficient as long as it contains the plasticizer (II), and may contain other plasticizers such as vegetable oils and synthetic plasticizers, but it is preferable that the other plasticizers are plasticizers that do not have a carboxy group. When the total amount of the plasticizer (II) and the other plasticizers is 100 parts by mass, the content of the plasticizer (II) is preferably 40 parts by mass or more, more preferably 60 parts by mass or more, even more preferably 80 parts by mass or more, even more preferably 90 parts by mass or more, particularly preferably 95 parts by mass or more, and most preferably 100 parts by mass.

[0052] The bio-based degree of the plasticizer (II) is not particularly limited as long as it is 70% by mass or more. From the viewpoint of further reducing the environmental load, however, it is preferably 80% by mass or more, more preferably 85% by mass or more, even more preferably 90% by mass or more, still more preferably 95% by mass or more, and most preferably 100% by mass.

[0053] The kinematic viscosity of the plasticizer (II) at 40°C is not particularly limited, but is preferably 100.0 cSt or less, more preferably 90.0 cSt or less, even more preferably 80.0 cSt or less, still more preferably 70.0 cSt or less, and even more preferably 60.0 cSt or less.

[0054] The melting point (pour point) of the plasticizer (II) is not particularly limited, but is preferably -70°C or higher, more preferably -60°C or higher, even more preferably -50°C or higher, and is preferably 20°C or lower, more preferably 10°C or lower, even more preferably 0°C or lower.

[0055] The plasticizer (II) is a biomass-derived plasticizer having no carboxy group, and is not particularly limited as long as it has a biobased content of 70% by mass or more, but suitable examples include compounds represented by the following general formula (1) and compounds represented by the following general formula (2). These may be used alone or in combination of two or more.

[0056] [ka] In the general formula (1), n 1 ~n 3are each independently 1 or 3; R 1 ~R 6 are each independently a hydrogen atom or an unsubstituted hydrocarbon group; R 1 and R 2 The total number of carbon atoms is 14, and R 3 and R 4 The total number of carbon atoms is 14, and R 5 and R 6 The total number of carbon atoms is 14, and R 1 ~R 6 may have a branched structure.

[0057] [ka] In the general formula (2), n 4 and n 5 are each independently 1 or 3; R 7 ~R 10 are each independently a hydrogen atom or an unsubstituted hydrocarbon group; R 7 and R 8 The total number of carbon atoms is 14, and R 9 and R 10 The total number of carbon atoms is 14, and R 7 ~R 10 may have a branched structure.

[0058] (Specific examples of compounds represented by formula (1)) Specific examples of the compound represented by general formula (1) include compounds represented by the following structural formulas (1-1) to (1-8).

[0059] [ka] (The compound represented by structural formula (1-1) is represented by the general formula (1), R 1 =H, R 2 =C 14 H 29 , R 3 =C 14 H 29 , R 4 =H, R 5=H, R 6 =C 14 H 29 , n 1 =1, n 2 =1, n 3 =1 compound.)

[0060] [ka] (The compound represented by structural formula (1-2) is represented by the general formula (1), R 1 =H, R 2 =C 14 H 29 , R 3 =C 14 H 29 (branch), R 4 =H, R 5 =H, R 6 =C 14 H 29 (branch), n 1 =1, n 2 =1, n 3 =1 compound.)

[0061] [ka] (The compound represented by structural formula (1-3) is represented by the general formula (1), R 1 =H, R 2 =C 14 H 29 (branch), R 3 =C 10 H 21 , R 4 =C4H9,R 5 =H, R 6 =C 14 H 29 , n 1 =3, n 2 =1, n 3 =1 compound.)

[0062] [ka]

[0063] (The compound represented by structural formula (1-4) is represented by the general formula (1), R 1 =H, R 2 =C 14 H 29 (branch), R 3 =C 11 H 23 (branch), R 4 =C3H7,R 5 =C3H7,R 6 =C 11 H 23 , n 1 =3, n 2 =1, n 3 =1 compound.) [ka] (The compound represented by structural formula (1-5) is represented by the general formula (1), R 1 =C6H 13 , R 2 =C8H 17 , R 3 =C3H7,R 4 =C 11 H 23 (branch), R 5 =C9H 19 , R 6 =C5H 11 , n 1 =1, n 2 =3, n 3 =1 compound.)

[0064] [ka] (The compound represented by structural formula (1-6) is represented by the general formula (1), R 1 =H, R 2 =C 14 H 29 , R 3 =C3H7,R 4 =C 11 H 23 (branch), R 5 =C 11 H 23 (branch), R 6 =C3H7,n 1=3, n 2 =3, n 3 =3 compound.)

[0065] [ka] (The compound represented by structural formula (1-7) is represented by the general formula (1), R 1 =C 10 H 21 , R 2 =C4H9,R 3 =C3H7,R 4 =C 11 H 23 , R 5 =C 11 H 23 , R 6 =C3H7,n 1 =3, n 2 =3, n 3 =3 compound.)

[0066] [ka] (The compound represented by structural formula (1-8) is represented by the general formula (1), R 1 =C9H 19 (branch), R 2 =C5H 11 , R 3 =C5H 11 , R 4 =C9H 19 , R 5 =C9H 19 , R 6 =C5H 11 , n 1 =3, n 2 =3, n 3 =3 compound.)

[0067] (Specific examples of compounds represented by formula (2)) Specific examples of the compound represented by general formula (2) include compounds represented by the following structural formulas (2-1) to (2-8).

[0068] [ka] (The compound represented by structural formula (2-1) is represented by the general formula (2), R 7 =C 14 H 29 , R 8 =H, R 9 =C 14 H 29 , R 10 =H, n 4 =1, n 5 =1 compound.)

[0069] [ka] (The compound represented by structural formula (2-2) is represented by the general formula (2), R 7 =C 14 H 29 (branch), R 8 =H, R 9 =C 14 H 29 (branch), R 10 =H, n 4 =1, n 5 =1 compound.)

[0070] [ka] (The compound represented by structural formula (2-3) is a compound represented by the general formula (2), R 7 =C 14 H 29 , R 8 =H, R 9 =C 10 H 21 , R 10 =C4H9,n 4 =1, n 5 =1 compound.)

[0071] [ka]

[0072] (The compound represented by structural formula (2-4) is represented by the general formula (2), R 7 =C 11 H 23 , R 8 =C3H7,R 9 =C 11 H 23 (branch), R 10 =C3H7,n 4 =1, n 5 =1 compound.) [ka] (The compound represented by structural formula (2-5) is represented by the general formula (2), R 7 =C5H 11 , R 8 =C9H 19 , R 9 =C3H7,R 10 =C 11 H 23 (branch), n 4 =1, n 5 =3 compound.)

[0073] [ka] (The compound represented by structural formula (2-6) is represented by the general formula (2), R 7 =C3H7,R 8 =C 11 H 23 (branch), R 9 =C3H7,R 10 =C 11 H 23 (branch), n 4 =3, n 5 =3 compound.)

[0074] [ka] (The compound represented by structural formula (2-7) is represented by the general formula (2), R 7 =C3H7,R 8 =C 11 H 23 , R9 =C3H7,R 10 =C 11 H 23 , n 4 =3, n 5 =3 compound.)

[0075] [ka] (The compound represented by structural formula (2-8) is represented by the general formula (2), R 7 =C5H 11 , R 8 =C9H 19 , R 9 =C5H 11 , R 10 =C9H 19 , n 4 =3, n 5 =3 compound.)

[0076] (vegetable oil) Examples of vegetable oils include castor oil, cottonseed oil, linseed oil, safflower oil, rapeseed oil, soybean oil, safflower oil, Japan wax, pine oil, corn oil, peanut oil, olive oil, palm oil, palm olein, palm stearin, and other plant-derived oils and fats, as well as interesterified oils, hydrogenated oils, and fractionated oils thereof. These oils and fats may be used alone or in combination of two or more. Among these, from the viewpoint of compatibility with the block copolymer (I), crude palm oil, refined palm oil, crude palm stearin, refined palm stearin, crude palm olein, refined palm olein, and hydrogenated products thereof are preferred, and hydrogenated products of refined palm stearin are more preferred.

[0077] The bio-based content of the vegetable oil is preferably 10% by mass or more, more preferably 30% by mass or more, even more preferably 50% by mass or more, still more preferably 70% by mass or more, and even more preferably 80% by mass or more.

[0078] (Synthetic plasticizer) Examples of synthetic plasticizers include oil-based softeners such as paraffinic, naphthenic, and aromatic process oils, mineral oils, and white oils; phthalic acid derivatives such as dioctyl phthalate and dibutyl phthalate; liquid cooligomers of ethylene and α-olefins; liquid paraffin; polybutene; low molecular weight polyisobutylene; liquid polydienes such as liquid polybutadiene, liquid polyisoprene, liquid polyisoprene / butadiene copolymers, liquid styrene / butadiene copolymers, and liquid styrene / isoprene copolymers; and hydrogenated or modified products thereof. These may be used alone or in combination of two or more.

[0079] Among these, from the viewpoint of compatibility with the block copolymer (I), paraffinic and naphthenic process oils; liquid cooligomers of ethylene and α-olefins; liquid paraffin; and low molecular weight polyisobutylene are preferred, with paraffinic and naphthenic process oils being more preferred.

[0080] [Polyolefin resin (III)] The resin composition of the present invention may further contain a polyolefin resin (III). In one embodiment of the resin composition of the present invention, the polyolefin resin (III) is preferably contained in an amount of 1 to 200 parts by mass, more preferably 5 to 150 parts by mass, even more preferably 15 to 150 parts by mass, and still more preferably 35 to 130 parts by mass, per 100 parts by mass of the block copolymer (I). Examples of the polyolefin resin (III) include polyethylene resins and polypropylene resins derived from biomass; homopolymers of olefins such as ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 3-methyl-1-butene, and 4-methyl-1-pentene; homopolymers of ethylene and propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, 1-hexene, 1-heptene, 6-methyl-1-heptene, isooctene, isooctane, decadiene, and the like. Examples of such elastomers include ethylene-α-olefin copolymers, which are copolymers with α-olefins having 3 to 20 carbon atoms such as ethylene-propylene-diene copolymers (EPDM); ethylene-vinyl acetate copolymers; ethylene-unsaturated carboxylic acid copolymers such as ethylene-acrylic acid copolymers and ethylene-methacrylic acid copolymers; polyolefin-based elastomers containing polyolefins such as polypropylene and polyethylene as hard segments and ethylene-propylene copolymer rubbers (EPM) and ethylene-propylene-diene copolymer rubbers (EPDM) as soft segments; and the like. These may be used alone or in combination of two or more. Among these, polypropylene (e.g., homopolypropylene, block polypropylene, random polypropylene) and biomass-derived polyethylene resins are preferred, biomass-derived low-density polyethylene (LDPE) and biomass-derived high-density polyethylene (HDPE) are more preferred, and biomass-derived high-density polyethylene (HDPE) is even more preferred.

[0081] The bio-based content of the polyolefin resin (III) is preferably 20% by mass or more, more preferably 50% by mass or more, and from the viewpoint of further reducing the environmental burden, is even more preferably 70% by mass or more, still more preferably 80% by mass or more, and even more preferably 90% by mass or more. The melt flow rate of the polyolefin resin (III) under conditions of a temperature of 190°C and a load of 2.16 kgf (21 N) is preferably 0.1 to 100 (g / 10 min), more preferably 0.5 to 80 (g / 10 min), and even more preferably 1 to 70 (g / 10 min), from the viewpoints of compatibility with the block copolymer (I), moldability, and flowability. The melt flow rate of the polypropylene at a temperature of 230° C. and a load of 2.16 kgf (21 N) is preferably 0.1 to 100 (g / 10 min), more preferably 0.5 to 80 (g / 10 min), and even more preferably 1 to 70 (g / 10 min), from the viewpoints of compatibility with the block copolymer (I), moldability, and flowability. The melt flow rate of the biomass-derived high density polyethylene (HDPE) at a temperature of 190°C and a load of 2.16 kgf (21 N) is preferably 1 to 100 (g / 10 min), more preferably 5 to 50 (g / 10 min), and even more preferably 10 to 30 (g / 10 min), from the viewpoints of compatibility with the block copolymer (I), moldability, and flowability.

[0082] [Tackifier (IV)] The resin composition of the present invention may further contain a tackifier (IV). The resin composition of the present invention includes an embodiment in which the tackifier (IV) is preferably contained in an amount of 1 to 300 parts by mass, more preferably 10 to 250 parts by mass, even more preferably 50 to 200 parts by mass, and even more preferably 100 to 180 parts by mass, per 100 parts by mass of the block copolymer (I). Examples of the tackifier (IV) include coumarone-based resins such as coumarone-indene resins; phenolic resins and terpene-based resins such as pt-butylphenol-acetylene resins, phenol-formaldehyde resins, terpene-phenolic resins, polyterpene resins, and xylene-formaldehyde resins; petroleum resins such as aromatic petroleum resins, aliphatic petroleum resins, alicyclic petroleum resins, aromatic petroleum resins, and modified alicyclic petroleum resins; rosin-based resins such as rosin esters represented by pentaerythritol ester of rosin and glycerol ester of rosin, hydrogenated rosin, methyl ester of hydrogenated rosin, pentaerythritol ester of polymerized rosin, hydrogenated rosin ester, high melting point ester-based resins, polymerized rosin, hardened rosin, and special rosin esters; etc. These may be used alone or in combination of two or more. Among these, terpene resins, petroleum resins, and rosin resins are preferred, and petroleum resins such as hydrogenated petroleum resin (product name: ARKON P100, manufactured by Arakawa Chemical Industries, Ltd.) are more preferred.

[0083] The softening point of the tackifier is preferably 70 to 160° C., more preferably 80 to 140° C., and even more preferably 85 to 120° C. If the softening point of the tackifier is 70° C. or higher, when the resin composition is used as a pressure-sensitive adhesive, the heat resistance tends to be high and bleeding out (exudation) onto the adherend tends to be reduced, whereas if the softening point is 160° C. or lower, the coatability and processability tend to be good.

[0084] [Additives] The resin composition of this embodiment may contain additives other than those described above, provided that the effects of the present invention are not impaired. Examples of additives include inorganic fillers, heat aging inhibitors, hindered phenol-based antioxidants (ADEKASTAB AO-60, manufactured by ADEKA CORPORATION), phosphorus-based antioxidants (IRGAFOS 168, manufactured by BASF Japan), and other antioxidants, light stabilizers, antistatic agents, release agents, flame retardants, foaming agents, pigments, dyes, and brighteners. These additives may be used alone or in combination of two or more. The content of the additive in the resin composition is preferably 15% by mass or less, more preferably 5% by mass or less, and even more preferably 1% by mass or less. The content of the additive in the resin composition can be, for example, 0.01% by mass or more.

[0085] [Content of each component in the resin composition] The resin composition of this embodiment is For 100 parts by mass of the block copolymer (I), Contains 1 to 1,500 parts by mass of plasticizer (II) This is one of the preferred embodiments.

[0086] In the resin composition of this embodiment, the content of the plasticizer (II) relative to 100 parts by mass of the block copolymer (I) is preferably 1 to 1500 parts by mass, more preferably 10 to 1000 parts by mass, even more preferably 15 to 500 parts by mass, and even more preferably 20 to 300 parts by mass.

[0087] In one preferred embodiment of the present invention, the resin composition comprises: For 100 parts by mass of the block copolymer (I), a plasticizer (II) in an amount of preferably 1 to 1500 parts by mass, more preferably 10 to 1000 parts by mass, even more preferably 15 to 500 parts by mass, and even more preferably 20 to 200 parts by mass; The polyolefin resin (III) is preferably contained in an amount of 1 to 200 parts by mass, more preferably 5 to 150 parts by mass, even more preferably 15 to 150 parts by mass, and still more preferably 35 to 130 parts by mass.

[0088] In one preferred embodiment of the present invention, the resin composition comprises: For 100 parts by mass of the block copolymer (I), A plasticizer (II) of preferably 1 to 1500 parts by mass, more preferably 10 to 1000 parts by mass, even more preferably 15 to 500 parts by mass, and still more preferably 20 to 100 parts by mass, An embodiment in which the tackifier (IV) is contained in an amount of preferably 1 to 300 parts by mass, more preferably 10 to 250 parts by mass, even more preferably 50 to 200 parts by mass, and even more preferably 100 to 180 parts by mass, can be mentioned.

[0089] The total content of the above (I) to (IV) in the resin composition of this embodiment is not particularly limited, but is preferably 85 to 100 mass %, more preferably 90 to 100 mass %, and even more preferably 95 to 100 mass %.

[0090] The resin composition of the present invention may be in the form of a pellet, a gel composition, or a pressure-sensitive adhesive, and examples of the embodiments include the following (1) to (3). (1) Pellets containing a block copolymer (I), a plasticizer (II), and a polyolefin resin (III): Such pellets have a high bio-based content, little oil bleeding and coloring, and have physical properties equivalent to those of paraffin-based process oil. (2) A gel composition containing a block copolymer (I) and a plasticizer (II): Such a gel composition has a high bio-based content, a low viscosity, and physical properties equivalent to those of paraffin-based process oil. (3) An adhesive comprising a block copolymer (I), a plasticizer (II), and a tackifier (IV): Such an adhesive has a high bio-based content, a low viscosity, and adhesive performance equivalent to that of paraffin-based process oil.

[0091] [Method of producing resin composition] The method for producing the resin composition of this embodiment is not particularly limited, and examples thereof include a method in which the above (I) to (II), and if necessary, the above (III) to (IV), and further additives are preblended and mixed together, and then melt-kneaded using a single-screw extruder, a multi-screw extruder, a Banbury mixer, a heating roll, various kneaders, etc. Also included is a method in which the above (I) to (II), and if necessary, the above (III) to (IV), and further additives are fed from separate feed ports and melt-kneaded. Examples of the preblending method include a method using a mixer such as a Henschel mixer, a high-speed mixer, a V blender, a ribbon blender, a tumbler blender, a conical blender, etc. The temperature during melt kneading can be arbitrarily selected preferably within the range of 150°C to 300°C.

[0092] The resin composition may be produced by the following method. First, the above (I) and (II) are premixed, and the premixed composition is melt-kneaded, extruded and cut to produce an oil-extended compound for dry blending (V). Next, the produced oil-extended compound for dry blending (V), the above (III), optionally the above (IV), and optionally other additives are mixed together to obtain a resin composition.

[0093] The gel composition (2) above can be produced by a production method well known in the art. For example, it can be produced by mixing the plasticizer (II), the block copolymer (I), and other components as necessary. The mixing can be carried out using a well-known mixing device. More specifically, it can be produced by mixing the plasticizer (II), the block copolymer (I), and other components as necessary at 100 to 200°C under air or nitrogen for 0.1 to 10 hours, and then cooling under vacuum as necessary.

[0094] [Bio-based ratio] The biobased content of the resin composition of this embodiment is preferably 15% by mass or more, and can be 30% by mass or more, 45% by mass or more, 50% by mass or more, 55% by mass or more, or 60% by mass or more. The biobased content is an index showing the petroleum dependency of the resin composition, and having a biobased content in the above range can reduce petroleum dependency. The biobased content (mass %) is calculated from the mass ratios of the block copolymer (I), the plasticizer (II) and the polyolefin resin (III) and the biobased content of each component according to the following formula: Biobased content (mass%) = (MI x XI / 100) + (MII x XII / 100) + (MIII x XIII / 100) In the above formula, MI represents the mass ratio (mass%) of the block copolymer (I) to the total mass of the resin composition, MII represents the mass ratio (mass%) of the plasticizer (II) to the total mass of the resin composition, and MIII represents the mass ratio (mass%) of the polyolefin resin (III) to the total mass of the resin composition. XI (mass%) represents the biobased degree of the block copolymer (I), XII (mass%) represents the biobased degree of the plasticizer (II), and XIII (mass%) represents the biobased degree of the polyolefin resin (III).

[0095] <Physical properties of resin composition> (Melt flow rate (MFR)) The resin composition of this embodiment has a melt flow rate (MFR) of preferably 200 (g / 10 min) or less, more preferably 160 (g / 10 min) or less, even more preferably 120 (g / 10 min) or less, and preferably 1 (g / 10 min) or more, more preferably 3 (g / 10 min) or more, even more preferably 5 (g / 10 min) or more. If the melt flow rate (MFR) is within the above range, the breaking strength is good and the moldability is also excellent. In this specification, the "melt flow rate (MFR)" is a value measured at a temperature of 230°C and a load of 2.16 kgf in accordance with JIS K7210:1999, as in the examples described later.

[0096] (hardness) The resin composition of this embodiment has a hardness according to JIS K 6253-2:2012 (Type A: 22°C: 0 seconds) of preferably 97 or less, and preferably 10 or more, more preferably 20 or more, and even more preferably 25 or more. If the A hardness is within the above range, the moldability is good and the flexibility is also excellent. In this specification, "hardness (Type A: 22°C: 0 seconds)" is a value measured under the same conditions as in the examples described later.

[0097] The resin composition of this embodiment has a hardness according to JIS K 6251:2010 (Type A: 22°C: 15 seconds) of preferably 97 or less, more preferably 93 or less, and even more preferably 90 or less. In addition, the hardness (Type A: 22°C: 15 seconds) is preferably 5 or more, more preferably 10 or more, and even more preferably 20 or more. If the A hardness is within the above range, the moldability is good and the flexibility is also excellent.

[0098] The resin composition of this embodiment has a hardness (type C: 23°C) according to JIS K 7312:1996 using an Asker rubber hardness tester type C of preferably 30 or less, more preferably 10 or less, and even more preferably 5 or less. If the hardness (type C: 23°C) is within the above range, the flexibility is good and the feel is excellent. In this specification, "hardness (Type C: 23° C.)" is a value measured under the same conditions as in the examples described later.

[0099] The resin composition of this embodiment has a hardness (type C: -20°C) according to JIS K 7312:1996 using an Asker rubber hardness tester type C of preferably 10 or less, more preferably 7 or less, and even more preferably 4 or less. If the hardness (type C: -20°C) is within the above range, the composition has good flexibility at low temperatures and exhibits little change in hardness over a wide temperature range. In this specification, "hardness (type C: -20°C)" is a value measured under the same conditions as in the examples described later.

[0100] (Tensile strength) The tensile strength of the resin composition of this embodiment can be evaluated according to JIS K6251:2010. The tensile strength is preferably 1 MPa or more, more preferably 2 MPa or more, and even more preferably 3 MPa or more. If the tensile strength is within the above range, the resin composition will have excellent durability.

[0101] (Tensile elongation) The resin composition of this embodiment can be evaluated for tensile elongation according to JIS K6251:2010. The tensile elongation is preferably 100% or more, more preferably 150% or more, and even more preferably 200% or more. If the tensile elongation is within the above range, the resin composition has excellent extensibility.

[0102] (Compression set) The resin composition of this embodiment can be evaluated for compression set (100°C x 22 hours) according to JIS K6262:2013. The compression set (100°C x 22 hours) is preferably 95% or less, more preferably 90% or less, and even more preferably 85% or less. If the compression set (100°C x 22 hours) is within the above range, the composition has excellent heat resistance.

[0103] (Storage modulus) The storage modulus (22°C) of the resin composition of this embodiment can be evaluated by viscoelasticity measurement. The storage modulus (22°C) is preferably 2.0 x 10 5 Pa or less, more preferably 1.5×10 5 Pa or less, more preferably 1.0×10 5 The storage modulus (22° C.) is preferably 1.0×10 4 Pa or more, preferably 2.0×10 4 Pa or more, more preferably 3.0×10 4 When the storage modulus (22° C.) is within the above range, the balance between flexibility and shape retention is excellent.

[0104] The storage modulus (−30° C.) of the resin composition of this embodiment can be evaluated by viscoelasticity measurement. The storage modulus (−30° C.) is preferably 3.0×10 5 Pa or less, more preferably 2.0×10 5 Pa or less, more preferably 1.5×10 5 If the storage modulus (-30°C) is within the above range, the flexibility at low temperatures will be excellent.

[0105] (Melt Viscosity) The melt viscosity (160°C) of the resin composition of this embodiment can be evaluated by a B-type viscometer. The melt viscosity (160°C) is preferably 2.0 x 10 5 mPa s or less, preferably 1.5×10 5 mPa s or less, more preferably 8.0×10 4 The melt viscosity (160°C) is preferably 1.0 x 10 3 mPa s or more, preferably 5.0×10 3 mPa s or more, more preferably 1.5×10 4 If the melt viscosity (160°C) is within the above range, the low-temperature coatability (formability) will be excellent.

[0106] The melt viscosity (180°C) of the resin composition of this embodiment can be evaluated by a B-type viscometer. The melt viscosity (180°C) is preferably 1.0 x 10 5 mPa s or less, preferably 8.0×10 4 mPa s or less, more preferably 5.0×10 4 The melt viscosity (180°C) is preferably 1.0 x 10 3 mPa s or more, preferably 5.0×10 3 mPa s or more, more preferably 1.5×10 4 If the melt viscosity (180°C) is within the above range, the coating property (formability) will be excellent.

[0107] (Compressive stress) The resin composition of this embodiment has a compressive stress (22°C) of preferably 0.500 MPa or less, more preferably 0.100 MPa or less, and even more preferably 0.035 MPa or less, and is also preferably 0.001 MPa or more, more preferably 0.005 MPa or more, and even more preferably 0.010 MPa or more. If the compressive stress (22°C) is within the above range, the composition has excellent flexibility and shape retention. In this specification, the "compressive stress (22°C)" is a value measured under the same conditions as in the examples described later.

[0108] (dropping point) The resin composition of this embodiment has a dropping point of preferably 175° C. or higher, more preferably 185° C. or higher, even more preferably 195° C. or higher, even more preferably 205° C. or higher, even more preferably 215° C. or higher, and even more preferably 220° C. or higher. If the dropping point is within the above range, the gel composition as a filler will not flow out from the protective tube or cable over a wide range of temperatures even if the protective tube is damaged. In this specification, the "dropping point" is a value measured under the same conditions as those in the examples described later.

[0109] (viscosity) The resin composition of this embodiment is 1s -1 The viscosity is preferably 200,000 mPa·s or less, more preferably 100,000 mPa·s or less, and even more preferably 50,000 mPa·s or less, and is preferably 10,000 mPa·s or more, more preferably 20,000 mPa·s or more, and even more preferably 30,000 mPa·s or more. -1 If the viscosity is within the above range, the gel composition can be easily filled into a protective tube or a cable during cable production, and the gel composition has excellent handleability. The resin composition of this embodiment is 6s -1 The viscosity is preferably 50,000 mPa·s or less, more preferably 30,000 mPa·s or less, and even more preferably 20,000 mPa·s or less, and is preferably 5,000 mPa·s or more, more preferably 8,000 mPa·s or more, and even more preferably 12,000 mPa·s or more. -1 If the viscosity is within the above range, the gel composition can be easily filled into a protective tube or a cable during cable production, and the gel composition has excellent handleability. The resin composition of this embodiment is 50s -1The viscosity is preferably 20,000 mPa·s or less, more preferably 10,000 mPa·s or less, and even more preferably 5,000 mPa·s or less, and is preferably 1,000 mPa·s or more, more preferably 2,000 mPa·s or more, and even more preferably 3,000 mPa·s or more. -1 If the viscosity is within the above range, the gel composition can be easily filled into a protective tube or a cable during cable production, and the gel composition has excellent handleability. In this specification, "1s -1 Viscosity”, “6s -1 Viscosity" and "50s -1 The "viscosity" is a value measured under the same conditions as in the examples described later.

[0110] (100℃ oil separation degree) The resin composition of this embodiment can be evaluated for 100°C oil separation rate according to JIS K 2220:2013. The resin composition of this embodiment has a 100°C oil separation rate of preferably 10.0% or less, more preferably 5.0% or less, and even more preferably 1.0% or less. If the 100°C oil separation rate is within the above range, it indicates that the composition of the gel composition is uniform, and the gel composition is difficult to separate.

[0111] (Worked Penetration) The worked penetration of the resin composition of this embodiment can be evaluated according to item 7 of JIS K 2220:2013. The worked penetration of the resin composition of this embodiment is preferably 3,000 or less, more preferably 1,500 or less, and even more preferably 1,000 or less, and is preferably 100 or more, more preferably 150 or more, and even more preferably 200 or more. If the worked penetration is within the above range, the gel composition as a filler does not flow out from the protective tube or cable under a wide range of temperatures even if the protective tube is damaged.

[0112] <Molded body> The molded article of the present invention is produced using the resin composition of the present invention. The shape of the molded product may be any shape that can be produced using the resin composition of the present invention. For example, the molded product may be molded into various shapes such as pellets, films, sheets, plates, pipes, tubes, rods, and granules. The method for producing the molded product is not particularly limited, and the molded product may be molded by various conventional molding methods such as injection molding, blow molding, foam molding, press molding, extrusion molding, and calendar molding. The resin composition of the present invention has excellent moldability and is therefore suitable for injection-molded or extrusion-molded articles, and in particular, injection-molded articles that have been embossed by injection molding can be obtained with good design.

[0113] The molded article of the present invention may have the following embodiments, for example. A film made of a resin composition containing a copolymer (I), a plasticizer (II), and a polyolefin resin (III): such a film has a high bio-based content and little orientation.

[0114] <Physical properties of molded products (especially films)> The resin composition of the present invention can provide a molded article with a high bio-based content, and in particular, when it is made into a film, it can provide a film with small differences in physical properties between MD and TD. By using the resin composition of the present invention, the MD / TD ratio at 100% elongation can be set to 0.1 to 2.8, 0.2 to 2.4, or even 0.3 to 2.1.

[0115] <Application> The resin composition of the present invention is expected to have a reduced environmental impact and excellent moldability. Therefore, the resin composition and molded article of the present invention can be suitably used as molded products such as sheets, films, tubes, hoses, and belts. Specifically, the present invention can be suitably used for various vibration-proof and vibration-damping members such as anti-vibration rubber, mats, sheets, cushions, dampers, pads, and mounting rubber; footwear such as sports shoes and fashion sandals; home appliance parts such as televisions, stereos, vacuum cleaners, and refrigerators; building materials such as sealing packings for building doors and window frames; interior and exterior parts of automobiles such as bumper parts, body panels, weather strips, grommets, skins for instrument panels, and airbag covers; grips of equipment used in sports and fitness such as drivers, golf clubs, tennis rackets, ski poles, bicycles, motorcycles, fishing gear, and water sports; grips of tools and electric tools such as hammers, drivers, pliers, and wrenches; grips of water-related products such as kitchen utensils, toothbrushes, interdental brushes, razors, and bathtub handrails; grips of writing instruments such as pens and scissors; grips used in the interior and exterior of automobiles such as shift levers and assist knobs; grips of bags; anti-slip mats such as anti-slip gloves and kitchen mats; toys; and tires such as automobile tires, bicycle tires, and motorcycle tires. The film can also be suitably used for food packaging materials such as food wrap films; medical devices such as infusion bags, syringes, and catheters; stoppers and cap liners for containers for storing food, beverages, medicines, etc.; stretch films; diapers; and the like. EXAMPLES

[0116] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these. β-Farnesene (purity: 97.6% by mass, biobased concentration (ASTM D6866-21): 99%, manufactured by Amyris, Inc.) was purified using 3 Å molecular sieves and distilled under a nitrogen atmosphere to remove hydrocarbon impurities such as zingiberene, bisabolene, farnesene epoxide, farnesol isomers, E,E-farnesol, squalene, ergosterol, and several dimers of farnesene, and was then used in the following polymerization.

[0117] The components used in the examples and comparative examples are as follows. <Block Copolymer (I)> Block copolymer (P-1) of Production Example 1 described below, biobased content (ASTM D6866-21): 0% by mass Block copolymer (P-2) of Production Example 2 described below, biobased content (ASTM D6866-21): 0% by mass Block copolymer (Q-1) of Production Example 3 described below, bio-based content (ASTM D6866-21): 0% by mass Block copolymer (R-1) of Production Example 4 described below, biobased content (ASTM D6866-21): 68% by mass Block copolymer (R-2) of Production Example 5 described below, biobased content (ASTM D6866-21): 80% by mass Block copolymer (T-1) of Production Example 6 described below, biobased content (ASTM D6866-21): 0% by mass Block copolymer (P-3) of Production Example 7 described below, biobased content (ASTM D6866-21): 0% by mass Block copolymer (P-4) of Production Example 8 described below, biobased content (ASTM D6866-21): 0% by mass Block copolymer (P-5) of Production Example 9 described below, biobased content (ASTM D6866-21): 0% by mass Block copolymer (P-6) of Production Example 10 described below, biobased content (ASTM D6866-21): 0% by mass Block copolymer (R-3) of Production Example 14 described later, biobased content (ASTM D6866-21): 80% by mass

[0118] <Plasticizer (II)> Plasticizer A: Product name: VIVA-B-FIX10227, manufactured by H&R, mixture having a structure represented by general formula (1), biobased content (ASTM D6866-21): 100% by mass Plasticizer B: Product name: VIVASPES10234, H&R Company, mixture having a structure represented by general formula (2), biobased content (ASTM D6866-21): 100% by mass <Plasticizers not covered by the present invention> Plasticizer C: Paraffin-based process oil (product name: Diana Process PW-90, manufactured by Idemitsu Kosan Co., Ltd.), bio-based content (ASTM D6866-21): 0% by mass Plasticizer D: Sunflower oil (product name: Olein Rich, manufactured by Showa Sangyo Co., Ltd.), biobased content (ASTM D6866-21): 95% by mass, contains carboxyl groups Plasticizer E: Linseed oil (product name: Linseed oil, manufactured by Nisshin Oillio Co., Ltd.), bio-based content (ASTM D6866-21): 95% by mass, containing carboxyl groups Plasticizer F: naphthenic oil (product name: SUNTHEN 450, manufactured by Nippon San Oil Co., Ltd.), biobased content (ASTM D6866-21): 0% by mass Plasticizer G: Product name: Krystol TM 550, Petro-Canada Lubricants Inc., Bio-based content (ASTM D6866-21): 0% by mass Plasticizer H: Product name: Renoil70-W, manufactured by DA Lubricants Company Inc., Bio-based content (ASTM D6866-21): 0% by mass Plasticizer I: Paraffin-based process oil (product name: PW-32, manufactured by Idemitsu Kosan Co., Ltd.), Bio-based content (ASTM D6866-21): 0% by mass Plasticizer J: Paraffin-based process oil (product name: KP0-50, manufactured by MORESCO Corporation), Bio-based content (ASTM D6866-21): 0% by mass

[0119] <Polyolefin resin (III)> Homo-PP: Homopolypropylene (product name: J107G, manufactured by Prime Polymer Co., Ltd., MFR: 30 g / 10 min (temperature 230°C, load 2.16 kg), bio-based content (ASTM D6866-21): 0% by mass) Block-PP: Block polypropylene (product name: J707, manufactured by Prime Polymer Co., Ltd., MFR: 30 g / 10 min (temperature 230°C, load 2.16 kg), bio-based content (ASTM D6866-21): 0% by mass) Bio-Block-PP: Bio-block polypropylene (product name: Circluen EP540P, manufactured by Lyondellbasell, melt flow rate: 15 g / 10 min (temperature 230°C, load 2.16 kg), bio-based content (ASTM D6866-21): 25% by mass) Bio-LDPE: Bio-LDPE polyethylene (product name: SPB608, manufactured by Braskem, melt flow rate: 30 g / 10 min (temperature 190°C, load 2.16 kg), bio-based content (ASTM D6866-21): 95% by mass) Bio-HDPE: Bio HDPE polyethylene (product name: SHA7260, manufactured by Braskem, melt flow rate: 20 g / 10 min (temperature 190°C, load 2.16 kg), bio-based content (ASTM D6866-21): 94% by mass)

[0120] <Tackifier (IV)> Tackifier resin A: Tackifier (product name: ARKON P100, manufactured by Arakawa Chemical Industries, Ltd.) Tackifying resin B: Manufactured by EASTMAN Chemical Company, product name: Regalite TM R1125 <Antioxidants> Hindered phenol antioxidant (ADEKASTAB AO-60, manufactured by ADEKA Corporation)

[0121] Details of the measurement methods for the block copolymer (I) obtained in the Production Examples are as follows. (1) Measurement of weight average molecular weight (Mw) and molecular weight distribution The weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) of the block copolymer (I) and the styrene block were determined in terms of standard polystyrene by gel permeation chromatography (GPC) using the following measuring device and conditions: Equipment: Tosoh Corporation GPC equipment "HLC-8320GPC" Separation column: Tosoh Corporation column "TSKgelSuperHZ4000" Eluent: Tetrahydrofuran ·Eluent flow rate: 0.7mL / min Sample concentration: 5mg / 10mL Column temperature: 40℃

[0122] (2) Measurement method for hydrogenation rate The block copolymer (I) before hydrogenation and the block copolymer (I) after hydrogenation were each dissolved in CDCl3, 1 H-NMR measurement [apparatus: "ADVANCE 400 Nano bay" (manufactured by Bruker), measurement temperature: 30°C] was performed. The hydrogenation rate of the carbon-carbon double bond in the structural unit derived from the conjugated diene compound in the block copolymer (I) before hydrogenation was calculated from the proton peak of the carbon-carbon double bond appearing at 4.5 to 6.0 ppm in the obtained spectrum according to the following formula. Hydrogenation rate (mol%)={1-(moles of carbon-carbon double bonds contained in 1 mole of block copolymer (I) after hydrogenation) / (moles of carbon-carbon double bonds contained in 1 mole of block copolymer (I) before hydrogenation)}×100

[0123] (3) Vinyl bond content of block copolymer (I) The details of the method for measuring the vinyl bond content in the block copolymer (I) obtained in the Production Examples are as follows. The block copolymer (I) before hydrogenation was dissolved in CDCl3, 1H-NMR measurement was performed [apparatus: "ADVANCE 400 Nano bay" (manufactured by Bruker), measurement temperature: 30°C]. The amount of vinyl bonds was calculated from the ratio of the peak area corresponding to the 3,4-bond unit and the 1,2-bond unit in the isoprene structural unit and the 1,2-bond unit in the butadiene structural unit to the total peak area of ​​the butadiene-derived structural unit, the isoprene-derived structural unit, or the butadiene and isoprene-derived structural units.

[0124] <Block Copolymer (I)> [Production Example 1] Block copolymer (P-1) A pressure vessel that had been purged with nitrogen and dried was charged with 50.0 kg of cyclohexane as a solvent and 0.0310 kg of sec-butyllithium (10.5 mass% cyclohexane solution) as an anionic polymerization initiator, and the vessel was heated to 50°C. After that, 1.32 kg of styrene (1) was added and polymerization was carried out for 1 hour, a mixed liquid of 2.73 kg of butadiene and 3.44 kg of isoprene was added and polymerization was carried out for 2 hours, and further 1.32 kg of styrene (2) was added and polymerization was carried out for 1 hour, thereby obtaining a reaction liquid containing a polystyrene-poly(butadiene / isoprene)-polystyrene triblock copolymer. Palladium carbon (palladium loading: 5% by mass) was added as a hydrogenation catalyst to the reaction solution in an amount of 5% by mass relative to the block copolymer, and the reaction was carried out for 10 hours under conditions of a hydrogen pressure of 2 MPa and 150° C. After cooling and depressurization, the hydrogenation catalyst was removed by filtration, and the filtrate was concentrated and further dried in vacuum to obtain a hydrogenated product of polystyrene-poly(butadiene / isoprene)-polystyrene triblock copolymer (block copolymer (P-1)). The above physical properties of the block copolymer (P-1) were measured, and the results are shown in Table 1.

[0125] [Manufacturing Examples 2-3] Block copolymer (P-2), block copolymer (Q-1) Block copolymer (P-2) and block copolymer (Q-1) were produced in the same manner as in Production Example 1, except that the raw materials and the amounts used were as shown in Table 1. However, in the production of block copolymer (Q-1), tetrahydrofuran was used as the Lewis base. The above physical properties of the resulting block copolymer (P-2) and block copolymer (Q-1) were measured, and the results are shown in Table 1.

[0126] [Production Example 4] Block copolymer (R-1) A pressure vessel that had been purged with nitrogen and dried was charged with 50.0 kg of cyclohexane as a solvent and 0.0155 kg of sec-butyllithium (10.5 mass% cyclohexane solution) as an anionic polymerization initiator, and the vessel was heated to 50°C. After that, 1.32 kg of styrene (1) was added and polymerization was carried out for 1 hour, followed by addition of 6.18 kg of β-farnesene and polymerization for 2 hours, and further addition of 1.32 kg of styrene (2) and polymerization for 1 hour, to obtain a reaction liquid containing a polystyrene-poly(β-farnesene)-polystyrene triblock copolymer. Palladium carbon (palladium loading: 5% by mass) was added as a hydrogenation catalyst to the reaction solution in an amount of 5% by mass relative to the block copolymer, and the reaction was carried out for 10 hours under conditions of a hydrogen pressure of 2 MPa and 150° C. After cooling and depressurization, the hydrogenation catalyst was removed by filtration, and the filtrate was concentrated and further dried in vacuum to obtain a hydrogenated product of polystyrene-poly(β-farnesene)-polystyrene triblock copolymer (block copolymer (R-1)). The bio-based content of the resulting block copolymer (R-1) was 68 mass % as measured in accordance with ASTM D6866-21. The above physical properties of the block copolymer (R-1) were measured, and the results are shown in Table 1.

[0127] [Production Example 5] Block copolymer (R-2) A block copolymer (R-2) was produced in the same manner as in Production Example 4, except that the raw materials and the amounts used were as shown in Table 1. The above physical properties of the resulting block copolymer (R-2) were measured, and the results are shown in Table 1.

[0128] [Production Example 14] Block copolymer (R-3) A pressure vessel that had been purged with nitrogen and dried was charged with 50.0 kg of cyclohexane as a solvent and 0.0413 kg of sec-butyllithium (10.5 mass% cyclohexane solution) as an anionic polymerization initiator, and the vessel was heated to 50°C. After that, 1.12 kg of styrene (1) was added and polymerization was carried out for 1 hour, followed by addition of 10.25 kg of β-farnesene and polymerization for 2 hours, and further addition of 1.12 kg of styrene (2) and polymerization for 1 hour, to obtain a reaction liquid containing a polystyrene-poly(β-farnesene)-polystyrene triblock copolymer. Palladium carbon (palladium loading: 5% by mass) was added as a hydrogenation catalyst to the reaction solution in an amount of 5% by mass relative to the block copolymer, and the reaction was carried out for 3 hours under conditions of a hydrogen pressure of 2 MPa and 150° C. After cooling and depressurization, the hydrogenation catalyst was removed by filtration, and the filtrate was concentrated and further dried in vacuum to obtain a hydrogenated product of polystyrene-poly(β-farnesene)-polystyrene triblock copolymer (block copolymer (R-3)). The bio-based content of the resulting block copolymer (R-3) was 80 mass % as measured in accordance with ASTM D6866-21. The above physical properties of the block copolymer (R-3) were measured, and the results are shown in Table 1.

[0129] [Production Example 6] Block copolymer (T-1) A pressure vessel that had been purged with nitrogen and dried was charged with 50.0 kg of cyclohexane as a solvent and 0.061 kg of sec-butyllithium (10.5 mass% cyclohexane solution) as an anionic polymerization initiator, and the vessel was heated to 50°C. After that, 0.81 kg of styrene (1) was added and polymerized for 1 hour, followed by addition of 10.87 kg of isoprene and polymerization for 2 hours, and further addition of 0.81 kg of styrene (2) and polymerization for 1 hour, to obtain a reaction liquid containing a styrene-isoprene-styrene triblock copolymer. Palladium carbon (palladium loading: 5% by mass) was added as a hydrogenation catalyst to this reaction liquid in an amount of 5% by mass relative to the block copolymer, and the reaction was carried out under conditions of a hydrogen pressure of 2 MPa and 150° C. for 10 hours. After cooling and releasing the pressure, the palladium carbon was removed by filtration, the filtrate was concentrated and further dried in vacuum to obtain a hydrogenated styrene-isoprene-styrene triblock copolymer (SEPS). Similarly to (SEPS), 50.0 kg of cyclohexane as a solvent and 0.420 kg (44.1 g of sec-butyllithium) as an anionic polymerization initiator were placed in a nitrogen-purged, dried pressure vessel, and the temperature was raised to 50°C. After that, 2.83 kg of styrene (1) was added and polymerized for 1 hour, and subsequently 19.81 kg of isoprene was added and polymerized for 2 hours to obtain a reaction liquid containing a styrene-isoprene diblock copolymer. This reaction mixture was hydrogenated in the same manner as for (SEPS), to obtain a hydrogenated product of styrene-isoprene diblock copolymer (SEP). The (SEPS) and (SEP) obtained above were melt-kneaded using a Coperion screw extruder ZSK26MagaCopounder (L / D=56) at a screw speed of 300 rpm and a kneading temperature of 200°C to obtain a block copolymer (T-1), which is a composition consisting of SEPS and SEP.

[0130] [Manufacturing Examples 7-8] Block copolymer (P-3), block copolymer (P-4) Block copolymers (P-3) and (P-4) were produced in the same manner as in Production Example 1, except that the raw materials and the amounts used were as shown in Table 1. The above physical properties of the resulting block copolymer (P-3) and block copolymer (P-4) were measured, and the results are shown in Table 1.

[0131] [Manufacturing Examples 9-10] Block copolymer (P-5), block copolymer (P-6) Block copolymers (P-5) and (P-6) were produced in the same manner as in Production Example 1, except that the raw materials and the amounts used were as shown in Table 1. The above physical properties of the resulting block copolymer (P-5) and block copolymer (P-6) were measured, and the results are shown in Table 1.

[0132] Block copolymer (S-1) SBS, styrene-butadiene-styrene block copolymer, Mw: 304,000 / 119,000 / 59,000=1.0 / 87 / 13, hydrogenation rate: 0 mol%, vinyl bond content: 11 mol% (product name: D-1102, manufactured by KRATON)

[0133] Block copolymer (U-1) SIS, styrene-isoprene-styrene block copolymer, Mw: 213,000 / 112,000=64 / 36, hydrogenation rate: 0 mol%, vinyl bond content: 7.0 mol% (product name: Quintac3421, manufactured by ZEON)

[0134] [Examples 11 to 13] <Table 9: Oil-extended compounds for dry blending (V)> Oil-extended compound for dry blending (T-2), Oil-extended compound for dry blending (T-3), Oil-extended compound for dry blending (T-4) The components were premixed according to the formulation shown in Table 9 below. Next, using a twin-screw extruder (Coperion's "ZSK26Mc"; number of cylinders: 14), the premixed composition was fed into a hopper under conditions of a cylinder temperature of 180°C and a screw rotation speed of 300 rpm. The mixture was then melt-kneaded, extruded into strands, and cut to produce pellets of the resin composition.

[0135] [Table 1]

[0136] The notations in Table 1 are as follows: [(a1) / (a2)]: The mass ratio of the content of polymer block (a1) to the content of polymer block (a2) is shown. Polymer backbone: St-(Bd / Ip)-St denotes a polystyrene-poly(butadiene / isoprene)-polystyrene triblock copolymer. St-Bd-St denotes a polystyrene-poly(butadiene)-polystyrene triblock copolymer. St-F-St denotes a polystyrene-poly(β-farnesene)-polystyrene triblock copolymer. St-Ip-St refers to a polystyrene-poly(isoprene)-polystyrene triblock copolymer. St-Ip denotes a polystyrene-poly(isoprene) diblock copolymer.

[0137] Details of each measurement method for the plasticizer (II) are as follows. (1) Measurement of kinetic viscosity The kinetic viscosities of plasticizers A to J were measured using an SVM dynamic viscometer (product name: SVM(TM)3001, manufactured by Oil Lubricant Communications Co., Ltd.) at 40° C. The results are shown in Table 2. (2) Melting point (pour point) measurement The melting points (pour points) of plasticizers A to J were measured using an automatic pour point tester (product name: RPP-303CML, manufactured by Rigo Co., Ltd.) under the conditions of JIS K2269: 1987. The results are shown in Table 2.

[0138] [Table 2]

[0139] (Examples 1 to 22, 29 to 31, and 69, Comparative Examples 1 to 14, and 17 to 20) <Table 3-1~4 and 7: Compound> According to the formulations shown in Tables 3-1 to 3-4 and 7, the components were premixed. Next, the premixed composition was fed into a hopper of a twin-screw extruder (Coperion's "ZSK26Mc"; number of cylinders: 14) under conditions of a cylinder temperature of 210° C. and a screw rotation speed of 300 rpm. The composition was then melt-kneaded, extruded into strands, and cut to produce pellets of the resin composition.

[0140] <Table 5: Oil extended compounds> The components were premixed according to the formulation shown in Table 5. Next, using a twin-screw extruder (Coperion's "ZSK26Mc"; number of cylinders: 14), the premixed composition was fed into a hopper under conditions of a cylinder temperature of 160°C and a screw rotation speed of 300 rpm. The mixture was then melt-kneaded, extruded into strands, and cut to produce pellets of the resin composition.

[0141] (Examples 23 to 28 and 70, Comparative Examples 15 to 16) <Table 6: Adhesive> According to the formulation shown in Table 6, a solution was prepared by dissolving each component in cyclohexane to a solids concentration of 25% by mass. For melt viscosity measurement The above solution was placed in a container and dried to obtain a resin composition. ·For adhesive force measurement The solution was applied to a substrate layer (PET film: thickness 50 μm) using an automatic film coater PI-1210 (manufactured by Tester Sangyo Co., Ltd.) with a Baker-type applicator SA-201 (manufactured by Tester Sangyo Co., Ltd.) set to 6 mil, and then dried at 60°C for 0.5 hours and at room temperature for 22 hours to obtain a laminate with an adhesive layer thickness of approximately 25 μm.

[0142] (Examples 32 to 34, Examples 67 to 68, Comparative Examples 21 to 22, Comparative Examples 29 to 30) <Table 8: Film> Each component was premixed according to the formula shown in Table 8. The premixed composition was then fed to a hopper of a twin-screw extruder (Coperion's "ZSK26Mc"; number of cylinders: 14) under kneading conditions of a cylinder temperature of 205° C. and a screw rotation speed of 300 rpm. The mixture was then melt-kneaded, extruded into strands, and cut to produce pellets of the resin composition. A film of the thermoplastic elastomer composition was then obtained under molding conditions using a Thermo Fisher 20 mm single screw machine set at a temperature of 220°C.

[0143] The notations in Table 8 are as follows: ·Tackifying resin B: Manufactured by EASTMAN Chemical Company, product name: Regalite TM R1125 Polyolefin elastomer: ExxonMobil Corporation, product name: Vistamaxx TM 6102 (Structural units derived from ethylene: 16% by mass) ·Polystyrene resin: Manufactured by INEOS Styrolution America LLC, product name: Styrolution PS3190 (weight average molecular weight: 250,000)

[0144] (Examples 35, 39, 41, 43, 45, 47, and 49) <Table 10-1: Pellets, injection sheets> Each component was premixed according to the formulation shown in Table 10-1. Next, using a twin-screw extruder (Coperion's "ZSK26Mc"; number of cylinders: 14), the premixed composition was fed into a hopper under conditions of a cylinder temperature of 210°C and a screw rotation speed of 300 rpm. The mixture was then melt-kneaded, extruded into strands, and cut to produce pellets of the resin composition. The pellets obtained above were injection molded using an injection molding machine "EC75SX" (manufactured by Toshiba Machine Co., Ltd.) at a cylinder temperature of 210°C, a mold temperature of 40°C, and an injection pressure of 80 MPa to produce an injection sheet with a length of 110 mm, a width of 110 mm, and a thickness of 2 mm.

[0145] (Examples 36, 37, 38, 40, 42, 44, 46, 48, and 50) <Table 10-1: Injection sheet (dry blend)> According to the formulation shown in Table 10-1, T-2 or T-3 was placed in a bag and premixed with polyolefin resin, and the mixture was then loaded into an injection molding machine "EC75SX" (manufactured by Toshiba Machine Co., Ltd.) and injection molded at a cylinder temperature of 210°C, a mold temperature of 40°C, and an injection pressure of 80 MPa to produce an injection sheet 110 mm long, 110 mm wide, and 2 mm thick.

[0146] (Examples 51 and 53) <Table 10-2: Pellets> Each component was premixed according to the formulation shown in Table 10-2. Next, using a twin-screw extruder (Coperion's "ZSK26Mc"; number of cylinders: 14), the premixed composition was fed into a hopper under conditions of a cylinder temperature of 210°C and a screw rotation speed of 300 rpm. The mixture was then melt-kneaded, extruded into strands, and cut to produce pellets of the resin composition. The pellets obtained above were molded into a ribbon sheet with a thickness of 1 mm and a width of 35 mm using a single-screw extruder (Freesia Macross "NV40mm"; L / D 36) under conditions of a barrel temperature of 180°C and a screw rotation speed of 30 rpm.

[0147] (Examples 52 and 54) <Table 10-2: Ribbon sheet (dry blend)> According to the formulation shown in Table 10-2, T-2 and polyolefin resin were premixed in a bag and fed into a single-screw extruder (Freesia Macross "NV40mm"; L / D 36) and molded into a ribbon sheet with a thickness of 1 mm and a width of 35 mm at a barrel temperature of 180°C and a screw rotation speed of 30 rpm.

[0148] (Comparative Examples 23 and 25) <Table 11: Pellets, injection sheets> Each component was premixed according to the formulation shown in Table 11. Next, using a twin-screw extruder (Coperion's "ZSK26Mc"; number of cylinders: 14), the premixed composition was fed into a hopper under conditions of a cylinder temperature of 210°C and a screw rotation speed of 300 rpm. The mixture was then melt-kneaded, extruded into strands, and cut to produce pellets of the resin composition. The pellets obtained above were injection molded using an injection molding machine "EC75SX" (manufactured by Toshiba Machine Co., Ltd.) at a cylinder temperature of 210°C, a mold temperature of 40°C, and an injection pressure of 80 MPa to produce an injection sheet with a length of 110 mm, a width of 110 mm, and a thickness of 2 mm.

[0149] Comparative Example 24 <Table 11: Injection Sheet (Dry Blend)> According to the formulation shown in Table 11, T-4 and polyolefin resin were premixed in a bag and then placed in an injection molding machine "EC75SX" (manufactured by Toshiba Machine Co., Ltd.) and injection molded at a cylinder temperature of 210°C, a mold temperature of 40°C, and an injection pressure of 80 MPa to produce an injection sheet 110 mm long, 110 mm wide, and 2 mm thick.

[0150] (Examples 55 to 65 and Comparative Examples 26 to 27) <Table 12: Resin composition (gel composition), sheet sample, cylindrical test piece> The components were premixed according to the formulation shown in Table 12, and left to absorb oil for 1.5 hours in a Safee Oven SPH-202 (manufactured by Espec Corp.) heated to 120°C. Next, the mixture was kneaded for 5 minutes using a Labo Plastomill (manufactured by Toyo Seiki Co., Ltd.) at a set temperature of 110°C and a rotation speed of 70 rpm to obtain a resin composition (gel composition). The obtained resin composition (gel composition) was compressed at 160°C and 100 kgf / cm using a compression press molding machine "NF-37" manufactured by Shindo Metal Industries Co., Ltd. and a Teflon (registered trademark) coated metal frame as a spacer. 2The sheet samples for the bending test were obtained by compression press molding at a load of 160°C for 3 minutes and then cooling. The pieces for the compression stress test and the compression set test were compressed at 160°C for 3 minutes to prepare cylindrical test pieces with a diameter of 13.0±0.5 mm and a thickness of 6.3±0.3 mm (d0).

[0151] (Example 66 and Comparative Example 28) Table 13: Gel composition According to the formulation shown in Table 13, the ingredients were mixed under nitrogen at 120° C. for 3 hours, placed under vacuum, and then cooled to obtain a gel composition.

[0152] The notations in Tables 10-1, 10-2 and 11 are as follows. Homo-PP A: Homo polypropylene (product name: J107G, manufactured by Prime Polymer, MFR: 30g / 10min (temperature 230℃, load 2.16kg) Homo-PP B: Homopolypropylene (product name: J106G, manufactured by Prime Polymer, MFR: 16g / 10min (temperature 230℃, load 2.16kg) Homo-PP C: Homo polypropylene (product name: J105G, manufactured by Prime Polymer, MFR: 9.0g / 10min (temperature 230℃, load 2.16kg) Homo-PP D: Homo polypropylene (product name: E-100GPL, manufactured by Prime Polymer, MFR: 0.9g / 10min (temperature 230℃, load 2.16kg) "Difference from pellet" is the "pellet value" - "dry blend value". The lower the value, the smaller the difference and the better. - "Percent change relative to pellet" is calculated as ("Pellet value" - "Dry blend value") / "Pellet value" * 100. The lower the value, the smaller the percent change and the better.

[0153] The notations in Table 12 are as follows. "Hardness change" is the value of "hardness at an ambient temperature of 23°C" - "hardness at an ambient temperature of -20°C". The lower the value, the smaller the change and the better the result.

[0154] <Measurement and Evaluation> The following measurements and evaluations were carried out using the resin compositions obtained in the above Examples and Comparative Examples. The results are shown in Tables 3-1 to 8 and 10-1 to 13. The results in Tables 3-1 to 8 and 10-1 to 13 are for groups having the same composition ratio (for example, (1) a group consisting of Examples 1 to 3 and Comparative Examples 1 to 5, (2) a group consisting of Examples 5, 6, and 8 and Comparative Examples 6 to 8, (3) a group consisting of Examples 9 to 11 and Comparative Examples 9 to 11, (4) a group consisting of Examples 12 to 14, (5) a group consisting of Examples 19 and 20 and Comparative Example 12, (6) a group consisting of Example 21 and Comparative Example 13, (7) a group consisting of Example 22 and Comparative Example 14, (8) a group consisting of Examples 23, 24, 26, and 28 and Comparative Examples 15 and 16, (9) a group consisting of Example 29 and Comparative Example 17, (10) a group consisting of Example 30 and Comparative Example 18, (11) a group consisting of Example 15 and Comparative Example 19, (12) a group consisting of Example 31 and Comparative Example 19, (13) a group consisting of Example 32 and Comparative Example 19, (14) a group consisting of Example 33 and Comparative Example 19, (15) a group consisting of Example 34 and Comparative Example 19, (16) a group consisting of Example 35 and Comparative Example 19, (17) a group consisting of Example 36 and Comparative Example 19, (18) a group consisting of Example 37 and Comparative Example 19, (19) a group consisting of Example 38 and Comparative Example 20, (20) a group consisting of Example 39 and Comparative Example 21, (21) a group consisting of Example 30 and Comparative Example 22, (22 It is preferable to compare those belonging to the following groups with each other: (1) the group consisting of Comparative Example 20, (13) the group consisting of Examples 32, 33, 67, and 68 and Comparative Examples 21, 29, and 30, (14) the group consisting of Example 34 and Comparative Example 22, (15) the group consisting of Examples 35 to 40, (16) the group consisting of Examples 41 to 44, (17) the group consisting of Examples 45 to 48, (18) the group consisting of Examples 49 to 50, (19) the group consisting of Examples 51 to 52, (20) the group consisting of Examples 53 to 54, (21) the group consisting of Comparative Examples 23 to 24, (22) the group consisting of Examples 55 to 59 and 65 and Comparative Example 26, (23) the group consisting of Examples 60 to 64 and Comparative Example 27, (24) the group consisting of Example 66 and Comparative Example 28, and (25) the group consisting of Examples 27 and 70. (1) Bio-based content of resin composition The biobased degree (mass%) of the resin composition was calculated from the mass ratio of the block copolymer (I), plasticizer (II) and polyolefin resin (III) used in the above Examples and Comparative Examples, and the biobased degree of each component, using the following formula. The results are shown in Tables 3-1 to 13. Biobased content (mass%) = (MI x XI / 100) + (MII x XII / 100) + (MIII x XIII / 100) In the above formula, MI represents the mass ratio (mass%) of the block copolymer (I) to the total mass of the resin composition, MII represents the mass ratio (mass%) of the plasticizer (II) to the total mass of the resin composition, and MIII represents the mass ratio (mass%) of the polyolefin resin (III) to the total mass of the resin composition. XI (mass%) represents the biobased degree of the block copolymer (I), XII (mass%) represents the biobased degree of the plasticizer (II), and XIII (mass%) represents the biobased degree of the polyolefin resin (III).

[0155] (2) Melt flow rate (MFR) The melt flow rate (MFR) of the resin compositions in Tables 3-1, 3-2, 4, 7, 8, and 10-1 to 11 was measured using a Melt Indexer L244 (manufactured by Techno Seven Co., Ltd.) under the following measurement conditions in accordance with JIS K7210:1999. The results are shown in Tables 3-1, 3-2, 4, 7, 8, and 10-1 to 11. (Measurement conditions) ·Temperature: 230℃ Load capacity: 2.16kg Die: Standard die (diameter: 2.095mm, length: 8.000mm) (3)Hardness (3-1) Preparation of resin composition sheet The pellets of the resin composition obtained in each example were injection molded using an injection molding machine "EC75SX" (manufactured by Toshiba Machine Co., Ltd.) at a cylinder temperature of 210°C, a mold temperature of 40°C, and an injection pressure of 80 MPa to produce an injection sheet with a length of 110 mm, a width of 110 mm, and a thickness of 2 mm. (3-2) Hardness measurement From the above-mentioned ejected sheet, a dumbbell No. 3 test piece (2 mm) was obtained using a punching blade conforming to JIS K 6251:2010. Three of the obtained test pieces were stacked and the hardness of a 6 mm thick piece was measured using a Type A durometer indenter at a room temperature of 22°C in accordance with JIS K 6253-3:2012 ((1) 22°C, 0 sec; (2) 22°C, 15 sec). The results are shown in Tables 3-1 to 5, 7, and 10-1 to 11.

[0156] (4) Tensile strength, (5) Tensile elongation Using the dumbbell No. 3 test pieces (2 mm) prepared in (3-2) above, the tensile strength and tensile elongation were measured in accordance with JIS K 6251:2010 in Tables 3-1 to 5, 7, 10-1, and 10-2 in the machine direction (TD), and in Table 11 in the MD direction. The higher the tensile strength and tensile elongation values, the better the tensile properties. The results are shown in Tables 3-1 to 5, 7, and 10-1 to 11.

[0157] (6) Compression set The thermoplastic elastomer compositions obtained in each of the Examples and Comparative Examples were compression molded at 160°C for 3 minutes to prepare cylindrical test pieces with a diameter of 13.0±0.5 mm and a thickness of 6.3±0.3 mm (d0). In accordance with JIS K6262:2013, the cylindrical test pieces were compressed and deformed by 25% using a spacer with a thickness of 4.8 mm (d1), and were held in an atmosphere at 70°C or 100°C for 22 hours, after which the compression was released. The thickness (d2: mm) of the cylindrical test pieces was then measured after leaving them in an atmosphere at 23°C and a relative humidity of 50% for 30 minutes, and the compression set (%) was calculated as 100×(d0-d2) / (d0-d1). The lower the value, the better the rubber elasticity. The results are shown in Tables 3-1 to 4, 7, and 10-1 to 11.

[0158] (7) Storage modulus A disk-shaped test piece with a diameter of 25 mm and a thickness of 2 mm was cut out from the sheet prepared in (3-1) above. Dynamic viscoelasticity measurements were performed on this test piece using an ARES-G2 rheometer (manufactured by TA Instruments) under the following conditions, and the storage modulus (G') at -22°C and +22°C was measured. The results are shown in Table 5. (Dynamic viscoelasticity measuring device and measurement conditions) Parallel plates: diameter 25mm Vibration mode: Torsional vibration Distortion: 0.1% Frequency: 1Hz ·Measurement temperature: -70~200℃ Heating rate: 3℃ / min

[0159] (8) Complex viscosity A disk-shaped test piece with a diameter of 25 mm and a thickness of 2 mm was cut out from the sheet prepared in (3-1) above. The complex viscosity of this test piece was measured under the following conditions using an ARES-G2 rheometer (manufactured by TA Instruments). If the complex viscosity is low in this frequency range, kneading with low shear is possible, resin heat generation can be reduced, and moldability is excellent. The results are shown in Table 5. Parallel plates: diameter 25mm Vibration mode: Torsional vibration Frequency: 0.25Hz Measurement temperature: 240°C (Example 21, Comparative Example 13) 250°C (Examples 19 and 20, Comparative Example 12), 270°C (Example 22, Comparative Example 14)

[0160] (9) Odor The sheet prepared in (3-1) above was left for 24 hours in an atmosphere of 23° C. and 50% relative humidity, and then the odor was evaluated according to the following evaluation criteria. The evaluation results are shown in Tables 3-1 to 5, 7, and 10-1 to 11. (Evaluation Criteria) 1: Odorless (good) 2: Slight odor (OK) 3: Odor (not acceptable)

[0161] (10) Oil bleed The sheet prepared in the above (3-1) was left for 24 hours in an atmosphere of 23° C. and 50% relative humidity, and then evaluated visually and by touch according to the following evaluation criteria. The evaluation results are shown in Tables 3-1 to 8 and 10-1 to 11. (Evaluation Criteria) 1: No bleeding, not visible to the naked eye, does not remain on hands (good) 2: Slight bleeding. Not visible to the naked eye, but slight bleeding remains on the hands (OK). 3: Bleeding is visible and remains on hands (not acceptable)

[0162] (11) Coloring The sheet prepared in the above (3-1) was left for 24 hours in an atmosphere of 23° C. and 50% relative humidity, and then visually evaluated according to the following evaluation criteria. The evaluation results are shown in Tables 3-1 to 5, 7, and 10-1 to 11. (Evaluation Criteria) 1: No coloring (good) 2: Slightly colored (acceptable) 3: Colored (not available)

[0163] (12) Melt Viscosity The solution prepared in the same manner as for the adhesive evaluation was air-dried at room temperature for 48 hours, then dried in a vacuum dryer at 60°C for 0.5 hours to remove the cyclohexane, and a cast film of 5cm x 5cm x approximately 0.1cm was prepared. The melt viscosity of a sample cut from this cast film was measured at 160°C and 180°C using a Brookfield DV-II+VISCMETER (manufactured by Brookfield). The smaller the value, the better the moldability. The results are shown in Table 6.

[0164] (13) Adhesive strength A smooth SUS304 (BA one side SG pasted, thickness 1.0 mm) or an acrylic resin plate (product name: Sumipex E, thickness 1.5 mm, manufactured by Sumitomo Chemical Co., Ltd.) was used as the adherend. The laminate for "adhesive strength measurement" described above was pasted to the adherend so that the adhesive layer was in contact with the adherend, and cut to a width of 25 mm to prepare a test piece. This test piece was rolled with a 2 kg rubber roller at a speed of 20 mm / min, and then left for 30 minutes in an atmosphere of 23±1°C and humidity of 50±5%. Thereafter, in accordance with JIS Z 0237:2009, the 180° peel strength was measured at a peel speed of 300 mm / min, and the peel strength (23°C) was determined. The peel strength (23°C) is preferably 10 N / 25 mm or more, more preferably 15 N / 25 mm or more. When the peel strength (23°C) is within the above range, the adhesive strength to the adherend is excellent. The results are shown in Table 6.

[0165] (14) Tensile test (forward stress, return stress, stress relaxation, stress difference) Using the thermoplastic elastomer compositions (MD, TD) molded into films of Examples 32-34, Examples 67-68, Comparative Examples 21-22, and Comparative Examples 29-30, tests were conducted in an atmosphere of 23°C in accordance with ASTM D882-18. Test pieces (6 pieces) were prepared by cutting into a size of 50.8 mm x 25.4 mm using a die, and the thickness (inches) at the center of each test piece was measured. The test results shown in Table 8 are the average values ​​of the 6 test pieces. The test pieces were inserted into the pneumatic grip of an Instron 5567 (manufactured by Instron) equipped with Bluehill 3 software and a 100 N load cell, and the crosshead was operated to stretch the test pieces at 250 mm / min until they reached 200% elongation, held at 200% elongation for 30 seconds, and then returned to 0% elongation in 60 seconds, and the stress relaxation property (%) was calculated by the following formula. A 100N load cell was used with a pneumatic film grip having a 12.7mm x 25.4mm grip on one side and a 25.4mm line grip on the other side. The results are shown in Table 8. Stress relaxation rate (%) = ["stress at 200% elongation" - "stress after 200% elongation and holding for 30 seconds"] / "stress at 200% elongation" x 100 The "stress relaxation property (%)" is represented, for example, by (3) or (6) in FIG. 1 described later, the "stress at 200% elongation" is represented, for example, by (2) or (5) in FIG. 1 described later, and the "stress after 200% elongation and holding for 30 seconds" is represented, for example, by (2-2) or (5-2) in FIG. 1 described later. (1) Stress during the first 100% elongation: Stress at 100% elongation when elongating from 0% to 200% under the above conditions ((1) in Figure 1) (2) Stress during the first 200% elongation: Stress at 200% elongation when elongating from 0% to 200% under the above conditions ((2) in Figure 1) (3) First stress relaxation: The stress reduction rate (%) after stretching from 0% to 200% under the above conditions and holding for 30 seconds (= [(stress at first 200% stretch) - (stress at first 200% stretch and holding for 30 seconds)] ((3) in Figure 1) / (stress at first 200% stretch) x 100) (4) Return stress after the first 30% elongation: The stress when the specimen is stretched from 0% to 200% under the above conditions, held for 30 seconds, and then returned to 30% ((4) in Figure 1) (5) Stress during the second 200% elongation: The stress at 200% elongation when the sample measured once is stretched again from 0% to 200% ((5) in Figure 1) (6) Second stress relaxation: The stress reduction rate (%) after stretching from 0% to 200% under the above conditions and holding for 30 seconds (= [(stress at the second 200% stretch) - (stress after the second 200% stretch and holding for 30 seconds)] ((6) in Figure 1) / (stress at the second 200% stretch) x 100) (7) Return stress at the second 30% elongation: The stress when the specimen is stretched from 0% to 200% under the above conditions, held for 30 seconds, and then returned to 30% ((7) in Figure 1). (8) Stress difference percentage (%): The percentage (%) of the stress difference ((8) in Figure 1) obtained by subtracting the "stress at the first 200% elongation ((5) in Figure 1)" from the "stress at the second 200% elongation ((2) in Figure 1)" to the "stress at the first 200% elongation ((2) in Figure 1)" (= [(stress at the first 200% elongation) - (stress at the second 200% elongation)] / (stress at the first 200% elongation) x 100)

[0166] (15) Compressive stress (22°C) The thermoplastic elastomer compositions obtained in each of the Examples and Comparative Examples were compression molded at 140°C for 3 minutes to prepare cylindrical test pieces with a diameter of 13.0±0.5 mm and a thickness of 6.3±0.3 mm (d0). The cylindrical test pieces were deformed using an AUTOGRAPH AGX-V (Shimadzu Corporation) at a compression speed of 1 mm / min and a compression width of 4 mm, and the stress was measured at an ambient temperature of 22°C. The lower the stress, the better the flexibility. The results are shown in Table 12.

[0167] (16) Hardness (23℃), Hardness (-20℃) The hardness was measured at 23° C. and −20° C. using an Asker rubber hardness tester type C in accordance with JIS K 7312:1996. The results are shown in Table 12.

[0168] (17) Dropping point of gel composition The dropping point of each of the obtained gel compositions was measured in accordance with JIS K 2220: 2013. The results are shown in Table 13.

[0169] (18) Viscosity of the gel composition The viscosity was measured using a rheometer (R / S+ RHEOMETER, manufactured by BROOKFIELD) at 25°C for 1s -1 , 6s -1 , and 50s -1 More specifically, about 30 mL of the gel composition was placed in a sample chamber (MB3-25F, manufactured by Brookfield Corporation), which was then attached to a rheometer body equipped with a spindle (CC3-25, manufactured by Brookfield Corporation), and the shear rate was set to 1 s at 25°C. -1 The measurement was then performed for 300 seconds at 1 s and stabilized. -1 From the 50s -1 After raising it for 120 seconds, -1 From 1s -1 (2) The shear rate was then reduced to 1 s over a period of 120 s. -1 From the 50s -1 After raising it for 120 seconds, -1 From 1s -1 (3) The shear rate was then reduced to 1 s over a period of 120 s. -1 From the 50s -1 After raising it for 120 seconds, -1 From 1s -1 The shear rate in (3) was reduced to 1 s over a period of 120 seconds. -1 From the 50s -1 The measurement was performed over a period of 120 seconds to obtain the value of 1s. -1 , 6s -1 , and 50s -1 The viscosity at the shear rate condition of 1s shown in Table 13 was used. -1 Viscosity, 6s -1 Viscosity, and 50s -1 The viscosity is 1s -1 , 6s -1 , and 50s -1The results are shown in Table 13.

[0170] (19) Oil Separation Rate of Gel Composition The degree of oil separation was measured according to JIS K 2220:2013. More specifically, 10 g of the gel composition was weighed into a wire cone filter (a cone filter made of stainless steel wire mesh with an opening of 250 μm (wire diameter 160 μm) as specified in JIS Z 8801-1:2013) and kept at 80° C. for 24 hours, after which the mass of the oil separated from the gel composition was measured and the degree of oil separation was calculated. The results are shown in Table 13.

[0171] (20) Worked consistency of gel composition The consistency (worked consistency) of each of the obtained gel compositions was measured in accordance with item 7 of JIS K 2220:2013. The results are shown in Table 13.

[0172] [Table 3-1]

[0173] [Table 3-2]

[0174] [Table 4]

[0175] [Table 5]

[0176] [Table 6]

[0177] [Table 7]

[0178] [Table 8]

[0179] [Table 9]

[0180] [Table 10-1]

[0181] [Table 10-2]

[0182] [Table 11]

[0183] [Table 12]

[0184] [Table 13]

[0185] The notations in Tables 3-1 to 13 are as follows. "Parts" in the resin composition refers to parts by mass in the resin composition. "%" in the resin composition means mass % of the resin composition.

[0186] It can be seen from Tables 3-1 to 3-7 that the resin compositions and molded articles of the examples contain materials that can reduce the environmental load, and that the resin compositions and molded articles obtained are excellent in moldability.

[0187] From Table 8, it can be seen that the films of the examples have a high bio-based content, small film orientation (small difference in physical properties between MD and TD), and a small stress difference ratio obtained by subtracting the stress at 0% to 200% elongation in the second pass from the stress at 0% to 200% elongation in the first pass. This makes the films of the examples suitable for use as stretch films, and it can be inferred that, for example, in adult diapers where film is used over the entire surface, a good fit can be obtained due to the small difference in stress between the length and width.

[0188] From Table 10-1, it can be seen that when comparing Examples 35 and 36, Examples 39 and 40, Examples 41 and 42, Examples 43 and 44, Examples 45 and 46, Examples 47 and 48, and Examples 49 and 50, which have the same components but different manufacturing methods, the hardness and compression set are equivalent. In addition, when Examples 36 to 38 in which the MFR values ​​of the polyolefin resins dry-blended at the same compounding ratio were changed were compared, it was found that the hardness and compression set were the same.

[0189] From Table 10-2, it can be seen that when comparing Examples 51 and 52, and Examples 53 and 54, which have the same components but are manufactured by different methods, the hardness and compression set are equivalent.

[0190] From Tables 10-1 and 11, when Example 35 is compared with Comparative Example 23, and Example 36 is compared with Comparative Example 24, which differ only in the plasticizer (II) used, it can be seen that the Examples are superior in tensile elongation, odor, coloring, and oil bleeding. Also, when Example 49 is compared with Comparative Example 25, which differs only in the plasticizer (II) used, it can be seen that the Examples are superior in biobased degree and compression set.

[0191] It was found that the resin compositions and molded articles of the examples in Table 12 were compositions with high flexibility and durability over a wide temperature range.

[0192] As can be seen from Table 13, Example 66 had higher biobased content, dropping point, and thixotropy (viscosity ratio) and lower viscosity than Comparative Example 28. In addition, as can be seen from Table 13, Example 66 and Comparative Example 28 had equivalent oil separation rate and worked penetration. [Industrial Applicability]

[0193] The resin composition of the present invention contains a material capable of reducing the environmental load and is expected to have excellent moldability. Therefore, the resin composition and molded article of the present invention can be suitably used as molded products such as sheets, films, tubes, hoses, and belts.

Claims

1. A block copolymer (I) including a polymer block (a1) containing a structural unit derived from an aromatic vinyl compound and a polymer block (a2) (excluding the polymer block (a1)) containing a structural unit derived from a conjugated diene compound; and A plasticizer (II) derived from biomass having no carboxy group, the hydrogenation rate of carbon-carbon double bonds in the structural units derived from the conjugated diene compound in the block copolymer (I) is 93.0 mol % or more; The amount of vinyl bonds in the polymer block (a2) of the block copolymer (I) is 1.0 to 40.0 mol %, The bio-based content of the plasticizer (II) is 70% by mass or more, The plasticizer (II) is at least one of a compound represented by the following general formula (1) and a compound represented by the following general formula (2), [Formula 1] In the general formula (1), n 1 ~n 3 are each independently 1 or 3; R 1 ~R 6 are each independently a hydrogen atom or an unsubstituted hydrocarbon group; R 1 and R 2 The total number of carbon atoms in R is 14, 3 and R 4 The total number of carbon atoms in R is 14, 5 and R 6 The total number of carbon atoms in R is 14, 1 ~R 6 may have a branched structure. [chemical 2] In the general formula (2), n 4 and n 5 are each independently 1 or 3; R 7 ~R 10 are each independently a hydrogen atom or an unsubstituted hydrocarbon group; R 7 and R 8 The total number of carbon atoms in R is 14, 9 and R 10 The total number of carbon atoms in R is 14, 7 ~R 10 may have a branched structure.

2. The resin composition according to claim 1, wherein the plasticizer (II) has a kinetic viscosity at 40°C of 100.0 cSt or less.

3. The aromatic vinyl compound in the polymer block (a1) in the block copolymer (I) is at least one selected from the group consisting of styrene, α-methylstyrene, and 4-methylstyrene. The resin composition according to claim 1.

4. The resin composition according to claim 1, wherein the content of the polymer block (a1) in the block copolymer (I) is 1 to 65 mass%.

5. 2. The resin composition according to claim 1, wherein the block copolymer (I) has a weight average molecular weight of 50,000 to 600,000 as calculated in terms of standard polystyrene by gel permeation chromatography.

6. 2. The resin composition according to claim 1, wherein the block copolymer (I) has a weight average molecular weight of 262,000 to 600,000 as calculated in terms of standard polystyrene by gel permeation chromatography.

7. The resin composition according to claim 1, comprising 1 to 1500 parts by mass of the plasticizer (II) relative to 100 parts by mass of the block copolymer (I).

8. The resin composition according to claim 7, comprising 450 to 1500 parts by mass of the plasticizer (II) per 100 parts by mass of the block copolymer (I).

9. The resin composition according to claim 1, comprising 1 to 200 parts by mass of a polyolefin resin (III) per 100 parts by mass of the block copolymer (I).

10. The resin composition according to claim 9, wherein the polyolefin resin (III) comprises polyethylene and / or polypropylene.

11. The resin composition according to claim 9, wherein the polyolefin resin (III) is polypropylene.

12. The resin composition according to claim 9, wherein the polyolefin resin (III) is polyethylene.

13. The resin composition of claim 1 further comprising a synthetic plasticizer.

14. The resin composition according to claim 1, comprising 1 to 300 parts by mass of a tackifier (IV) per 100 parts by mass of the block copolymer (I).

15. The resin composition according to claim 1 , wherein the resin composition has a bio-based content of 15% by mass or more.

16. The resin composition according to claim 1, wherein the resin composition has a hardness (type C: 23°C) of 10 or less according to JIS K 7312:1996 using an Asker rubber hardness tester type C.

17. A molded article obtained by using the resin composition according to any one of claims 1 to 16.

Citation Information

Patent Citations

  • Adherent sheet pack

    JP1980092306A

  • Bio-based polymer composition

    JP2019529688A

  • Resin composition and molded body

    WO2022163787A1

  • Thermoplastic elastomer composition and molded article thereof

    WO2023145927A1