Integrated composite of metal and resin and its manufacturing method
A chemical conversion treatment on aluminum alloys, combined with a specific polyamide resin composition, enhances bonding strength and durability in metal-resin composites, addressing the challenges of high temperature, humidity, and shock resistance for automotive applications.
Patent Information
- Application Number
- JP2020176274
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-20
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2040-10-20
AI Technical Summary
Existing technologies face challenges in achieving high bonding strength and durability of integrated metal and resin composites, particularly with aluminum alloys and polyamide resin compositions, under conditions of high temperature, humidity, and temperature shock, which are critical for applications in mobile machinery like automobiles.
The integration of aluminum alloys with a polyamide resin composition involves a chemical conversion treatment creating a rough surface with ultra-fine unevenness, combined with a resin composition containing semi-aromatic polyamide and aliphatic polyamide, reinforced with short glass fibers, to achieve a shear bond strength of 45 MPa or more, and withstand continuous external forces and temperature shocks.
The method results in a composite with high temperature and humidity resistance, maintaining bonding strength even after exposure to severe conditions, and supports high productivity through insert injection molding.
Smart Images

Figure 0007578968000004 
Figure 0007578968000005 
Figure 0007578968000006
Abstract
Description
[Technical field]
[0001] The present invention relates to an integrated composite of metal and resin, which is an integrated composite of metal and resin, and a method for producing the same. More specifically, the present invention relates to an integrated composite of metal and resin, which is an integrated composite of metal and resin, in which a polyamide resin composition, which is a highly crystalline thermoplastic resin, is integrated by injection joining with various aluminum alloys that have been subjected to a specific chemical conversion treatment, and a method for producing the same. [Background technology]
[0002] Technology for strongly bonding metal and synthetic resin is required not only in the parts manufacturing industry for automobiles, home appliances, industrial equipment, etc., but also in a wide range of industrial fields, and many adhesives have been developed for this purpose. Such bonding technology (lamination technology) is a core technology in all manufacturing industries. Meanwhile, bonding methods that do not use adhesives have also been researched and various proposals have been made. Among them, the technology that had a great impact on the technical field of bonding metal and resin by injection molding was developed and named by the inventors of the present invention (hereinafter referred to as the inventors). Below, the background of the present invention and the history of the development of this technology will be explained in order to make it easier to understand.
[0003] NMT is a joining technique between a piece of aluminum alloy (hereinafter also referred to as "Al alloy") that has been subjected to a certain chemical conversion treatment and a resin composition. The method involves injecting molten crystalline thermoplastic resin into an Al alloy piece that has been inserted into an injection mold in advance to form a resin part, and at the same time strongly joining the molded product (the resin part) and the Al alloy piece. New NMT is a similar joining technique between a resin composition and all commonly used metals, including Al alloys, by expanding the metal type. The difference from NMT is that both are performed before inserting into an injection mold, but the basic theory (chemical conversion treatment method) regarding the surface treatment method for metals is different. The inventor has named the technique of joining a solid object such as a metal material and a thermoplastic resin in an injection mold using an injection molding machine as "injection joining" or "injection joining technology".
[0004] (NMT) The inventors have stipulated the following four or five conditions as necessary for the establishment of NMT, an injection joining technology using aluminum alloys. First, the following (1) and (2) are necessary conditions for the aluminum alloy side. The chemical conversion treatment of the aluminum alloy surface to satisfy these two conditions is called "NMT treatment." (1) The entire surface is covered with ultrafine recesses with diameters of 20 to 50 nm. (2) A water-soluble amine compound is chemically adsorbed onto the surface layer. Next, the following two or three points are necessary conditions for the resin composition to be injected. (3) The resin composition used is a resin composition containing a highly crystalline thermoplastic resin as a main component. (4) The highly crystalline thermoplastic resin undergoes a chemical reaction with amine molecules at high temperatures. (5) The resin composition contains, as a minor resin, a resin that is compatible with the main component resin, or a resin that is not compatible with the main component resin but can become compatible or partially compatible with the main component resin by adding a third component resin. The above (1) to (4) are essential requirements, and the addition of the above (5) will further increase the injection joining strength. The NMT carried out by the applicant for a composite of an Al alloy housing of a mobile phone device or the like and a resin satisfies the above (1) to (5) requirements and selects hydrazine hydrate as the amine compound in (2).
[0005] (NMT2, NMT5~NMT8) As described above, the present inventors discovered that a strong bonding strength can be obtained by injection bonding a PBT (polybutylene terephthalate) resin composition to an NMT-treated Al alloy. Then, the present inventors discovered that a PPS resin composition can be injection bonded to an Al alloy similarly subjected to NMT (Patent Document 1). Next, as described in Patent Document 1, the inventors developed an "NMT2" treatment method by improving the surface treatment method of an Al alloy, and discovered that the injection bonding strength between this treated product and the above-mentioned PBT resin and PPS resin is improved. In particular, the inventors discovered that the shear bonding strength of the Al alloy and the PPS resin composition is about 40 MPa, and that even if the injection bonded product is exposed to a temperature of 85°C and a humidity of 85% for 6,000 to 8,000 hours or more, the shear bonding strength is maintained at 37 to 40 MPa, and that an integrated product of metal and resin with the highest degree of wet heat resistance can be obtained. The inventors named this technology NMT2.
[0006] At the time of the invention, the inventor considered NMT2 to be the highest level of injection bonding technology between Al alloys and PPS-based resin compositions, but problems emerged in subsequent experiments. If an Al alloy is treated with NMT2 and then stored for one week or more before the injection bonding process of the PPS-based resin composition is performed, the wet heat resistance of the shear bonding strength tends to decrease. The applicant carried out NMT2 on a large scale in the manufacture of an Al alloy body for an Al alloy smartphone. At this time, it was found that if an Al alloy treated with NMT2 is stored for one week or more, the desired bonding strength cannot be obtained, or more precisely, the shear bonding strength is obtained, but the heat resistance over a long period of time decreases. As a countermeasure, the inventor improved the NMT2 treatment method and developed successively improved chemical treatment methods for various Al alloys, called NMT5, NMT7, NMT8 treatment methods, etc.
[0007] When these new treatment methods are used, the above-mentioned effective storage period is 4 weeks or more. In addition, when new NMT treatment methods such as NMT5-Oxy, NMT7-Oxy, NMT5-Ano, and NMT7-Ano treatment methods, which are named and developed by the present inventor and described later, are applied to various Al alloys, the above-mentioned effective storage period is several months or more, and the weakness of NMT2 is completely eliminated. In addition, the present inventor has studied the shape of an injection-bonded product of an Al alloy surface-treated as described in Patent Document 4 and a PPS-based resin composition, and has found a shape (laminate) in which the bonding strength is not adversely affected at the bonded part even after a temperature shock test of 3,000 cycles (a type of creep test) of -50°C / +150°C in a certain specific shape. Patent Document 5 discloses an example of this structure.
[0008] (New NMT) The present inventors have invented a new NMT (short for New nano molding technology) that can injection-bond various metal materials with resin compositions, and have proposed and disclosed its basic processing method for each type of metal (Patent Documents 5 to 9). These have been proposed and disclosed as injection bonding technologies that are compatible with almost all types of practical metals that are widely used and supplied on the market, such as Mg alloys, Al alloys, copper, stainless steel, general steel materials (Patent Document 11), and special steel plates. The highly crystalline thermoplastic resin used here is the same as the injection bonding resin for NMT described above.
[0009] The conditions for the establishment of "New NMT" are the following five necessary conditions. Of these, the following three are necessary conditions for the metal materials used. And chemically treating the surface so as to satisfy these three points ((i) to (iii) below) is called "New NMT treatment". That is, (i) the metal material has a rough surface with a period of 0.8 to 10 μm; (ii) the rough surface has an ultrafine uneven surface shape with a period of 5 to 300 nm (preferably 50 to 100 nm); and (iii) the surface layer is covered with a thin layer of a hard ceramic material such as a metal oxide or metal phosphate; The following two points are necessary for the injected resin: (iv) using a resin composition containing a highly crystalline thermoplastic resin as a main component; and (v) The above resin composition contains, in addition to the highly crystalline thermoplastic resin as the main component, a minor resin which is either a resin that is compatible with the main component resin, or a third resin which is incompatible with the main component resin but is at least partially compatible with the main component resin.
[0010] New NMT was developed for all metal types, but the most technical results were confirmed for Al alloys. As mentioned above, for Al alloys, chemical conversion treatment methods called NMT5-Oxy, NMT7-Oxy, NMT5-Ano, NMT7-Ano treatment methods, etc. were improved, developed, and proposed. After NMT treatment, hydrogen peroxide water treatment is performed as the final step to destroy the adsorbed substances of hydrazine hydrate, which is called NMT5-Oxy, NMT7-Oxy treatment methods, etc. (...Oxy). The process of creating this ultra-fine uneven surface, which is immersed in an aqueous solution of amine molecules, is replaced by an anodizing process, which is called NMT5-Ano and NMT7-Ano treatment methods, etc. (...Ano). Injection-bonded products with PPS resin compositions treated with these improved treatment methods have very high moist heat resistance at the bonded parts between the metal and resin, and the specified quality can be obtained even if the storage time of the intermediate material from surface treatment until injection bonding is several months, half a year, or a year, rather than the 1-2 weeks of NMT2 (Patent Document 4).New NMT treatment methods have been invented for titanium alloys, austenitic stainless steel, ferritic stainless steel, and general steel, and these have been improved to further increase bonding strength, so that high shear bonding strength can be obtained in injection bonding using PBT and PPS resins.
[0011] (Polyamide resin) The initial development of injection joining technology using polyamide resin composition in the resin part was started by the aforementioned NMT, and the initial development was a resin composition that selected and combined main and sub-component resins from the group of Al alloy and aliphatic polyamide resin, i.e. PA6 (nylon 6 resin), PA66 (nylon 66 resin), and other aliphatic polyamides. Injection joining was possible, but the shear joining strength was only about 20 MPa at most, and the joining force was weak. This clearly indicated that the crystallization speed of polyamide resin during rapid cooling was too fast. Even if a different polymer was mixed with this polyamide resin to slow down the crystallization speed, the cooling was too fast to keep up. This means that the crystallization of the molten resin progressed before the injected resin penetrated into the deepest part of the ultrafine concaves on the ultrafine uneven surface of the metal piece inserted into the mold, and as a result, the viscosity rose sharply and the molten resin hardened before penetrating the bottom of the ultrafine concaves. Naturally, this composite has low joining force.
[0012] Therefore, semi-aromatic polyamides PA6T (alternating copolymer of hexamethylenediamine and terephthalic acid) and PA6I (alternating copolymer of hexamethylenediamine and isophthalic acid) were mixed in ratios of "8:2" and "2:8" to create a composite. All of the mixtures were resin compositions using semi-aromatic polyamide resins, and when they were subjected to an injection bonding test, the shear bonding strength of the resulting injection bonded product improved to 40 MPa. However, in this injection bonding experiment, this high bonding strength could not be obtained unless the pressure was maintained for about one minute after the molten resin was injected. If the time from the injection of the molten resin to the release of the molded product was short, the molten resin could not be completely cured, the bonding strength was low, and the shape of the molded product changed when the resin part was strongly gripped by hand. From the phenomenon that this resin composition cures slowly, it is estimated that the crystallization speed during quenching is abnormally slow.
[0013] Therefore, we explored whether the crystallization rate during quenching could be optimized so that it was neither too slow nor too fast by making the main component in this resin either a semi-aromatic polyamide or an aliphatic polyamide, and making the sub-component the opposite. Furthermore, we speculated on what would happen if we tried to make a block polymer in which the combination (mixture) exists in one polymer. The resin created in the process is a block polymer containing 17% PA6I component, 77% PA66 component, and 6% PA6 component. 50 parts of GF (Glass Fiber) were added to 100 parts of polyamide-based resin containing this semi-aromatic polyamide and compounded to obtain a polyamide-based resin composition. The shear joint strength of the injection joint made from the NMT-treated A5052Al alloy and this resin composition was 26 MPa. The injection molding conditions were a dwell time of about several tens of seconds, and molding was possible without the need to maintain it longer than usual (Patent Document 2).
[0014] The injection-bonded product, which showed a shear joint strength of 26 MPa, has a joint strength sufficient to withstand the specifications when used in home appliances, miscellaneous goods for indoor use, etc. This was a new finding for the inventor, who had initially thought that it was impossible to manufacture a practical injection-bonded product using a polyamide resin composition. However, since a previously developed injection-bonded product between a PPS resin composition and an NMT-treated Al alloy had a stable shear joint strength of about 40 MPa, the inventor concluded that polyamide resin compositions basically have low joint strength and are inferior to PPS resin compositions in joint strength. As a result, the inventor temporarily stopped research and development of polyamides using NMT and new NMT.
[0015] On the other hand, problems such as those mentioned above were found with NMT2 involving PPS-based resin compositions, which were improved to NMT5, NMT7, NMT8, etc., and injection-bonded products consisting of Al alloys and PPS-based resin compositions were able to obtain nearly perfect resistance to moisture and heat. Furthermore, the new NMT involving Al alloys was developed from the method of forming irregularities using the anodizing method (see Patent Document 6) that forms regular irregularities, and chemical conversion treatment methods named NMT5-Ano and NMT7-Ano treatment methods were developed and proposed. Furthermore, chemical conversion treatment methods called NMT5-Oxy and NMT7-Oxy treatment methods, which are improvements on this method, were proposed. Injection-bonded products of Al alloys and PPS-based resin compositions using these treatment methods not only obtained high injection bonding strength and the resistance of that bonding strength to moisture and heat, but also obtained high resistance to temperature shock of 3,000 cycles as mentioned above (Patent Documents 4 and 5).
[0016] In short, it was expected that these composites would be used not only in the field of electronic and electrical machines such as home appliances and smartphones, but also in the field of mobile machines such as automobiles, aircraft, and mobile robots, due to the bonding strength of the resulting injection-bonded products. However, the metal materials used in the automotive field are basically steel or Al alloy materials, and polyamide-based resin compositions are preferred and used as high-strength resin materials (crystalline thermoplastic resins). Therefore, there is a demand to hasten the development of injection-bonded products (composites) that are expected to be practical, not only by injection-bonded products made of PPS-based resin compositions and Al alloys (Patent Document 12), but also by combinations of polyamide-based resin compositions and steel materials, and polyamide resins and Al alloys (Patent Document 12). This was the starting point for resuming the development and research of injection bonding technology using the polyamide-based resin composition of the present invention.
[0017] In the automotive field, research and development of high-tensile steel sheets (hi-ten) that can reduce the weight of steel materials has progressed, and the adoption of these steel materials has led to the weight reduction of steel materials for automobile bodies, panels, etc. However, there are still issues to be addressed in order to further reduce the weight of steel materials while using them in various parts. In addition, the practical application of a method for producing shale oil from shale layers, mainly in the United States, has erased the prediction of a sharp rise in crude oil prices around the world, and it seems that the future of automobiles equipped with engines will not disappear all at once. As automobile manufacturers, we still need to research and develop the weight reduction of car bodies with an eye to the future, but we are no longer in a hurry to change the body made of steel to Al alloy materials all at once, like aircraft. It is still too early to use Al alloy materials for the main structural materials such as chassis, and it is now thought that the overall weight should be reduced by using them for the main parts.
[0018] In order to meet this demand, the present inventors have resumed research into optimal new polyamide-based resin compositions, starting from polyamide mixtures (compositions) containing PA6I, PA66, and PA6, which showed a shear bonding strength of 26 MPa, and block polymers of similar composition, as disclosed in Patent Document 2. They treated Al alloys using the newly obtained new NMT treatment methods for Al alloys, which they named NMT2 to NMT8 treatments and NMT5-Ano treatment, which showed good bonding strength in injection bonding with the above-mentioned PPS-based resin composition, and searched for polyamide-based resin compositions containing semi-aromatic polyamides that would be most strongly injection bonded to these surface-treated Al alloys.
[0019] Fortunately, during the ten-odd years since these proposals, many improved grades of polyamide resin compositions have been put on the market, and nylon resin manufacturers have developed grades that are not listed in the general product catalogs. In short, these products are the results of manufacturers' development for various users, and although they are commercially available, some of them are not listed in the general product catalogs because there are too many types. Therefore, we requested manufacturers of polyamide resin compositions to collect commercially available improved polyamide resin compositions while imagining a composition that includes "a wide variety of mixed compositions that include standard polyamides such as PA6 and PA66 but also semi-aromatic polyamides, or such copolymer polyamides," and searched for a polyamide resin composition that would be most strongly injected and bonded to the above-mentioned surface-treated Al alloys.
[0020] In short, the test piece shown in Figure 1 was created by injection joining Al alloy pieces that had been subjected to NMT7 and NMT8 processing, which showed the best performance in the injection joining with the PPS resin composition, and several types of polyamide resin compositions, such as commercially available products and developed products from each of the resin manufacturers mentioned above. The shear joining strength of these test pieces was measured to search for polyamide resin compositions that showed a shear joining strength of about 30 MPa or more, and five types remained. One of them was the commercially available "CM3506G50 (manufactured by Toray Industries, Inc. (headquarters: Tokyo, Japan))" which showed a surprising injection joining strength of 45 to 54 MPa in shear joining strength even when the type of Al alloy was changed to standardized Al alloy pieces such as A5052, A2017, A7075, A1100, etc., when the NMT8-treated product was used. In addition, among the above-mentioned "CM3500" series products that were commercially available as copolymer nylon made by the same company, there were some that showed a shear joining strength of 30 MPa or more. However, through the above experiments, we determined that the "CM3506G50" was the most suitable for injection joining technology. The only other remaining product was a type made by a certain company.
[0021] The bond strength of the injection-bonded specimen (test piece) of one type of polyamide resin composition manufactured by a certain company and A5052Al alloy was about 50 MPa, but when the shear bond strength of 10 pairs of the same injection-bonded specimens was measured in a retest for confirmation, the bond strength varied between 20 and 55 MPa, and of the 10 pairs of injection-bonded specimens, only one pair showed 55 MPa, while the rest showed 20 to 25 MPa, which was a fairly low bond strength. The inventors repeated the injection bonding work by changing various injection bonding conditions, but were unable to find a way to eliminate the bond strength variation. It is presumed that the resin manufacturer who manufactured this probably mixed some kind of compound that is effective in suppressing the crystallization rate. However, the amount of the compound or the dispersion process of the crystallization rate inhibitor may have been inappropriate for the present invention. Of course, the resin of the resin manufacturer does not adjust the resin components, etc., according to the intended use of the composite of the present invention, so it is inevitable that such cases occur. The present inventor approached a certain company that sells this resin to conduct joint development research, but the proposal was unsuccessful. In the end, the inventor decided that the aforementioned "CM3506G50" was the most suitable resin to be used in the present invention at that time.
[0022] Therefore, the commercially available "CM3506G50" was analyzed by pyrolysis GC mass spectrometry, and it was found that the main components were PA66, PA6, and semi-aromatic polyamide. However, the chart of the gas chromatography mass spectrometer (GC-MS) revealed that the semi-aromatic polyamide was a copolymer of phthalic acid and hexamethylenediamine, but it was not possible to determine whether it was PA6I or PA6T. In addition, it was not possible to determine whether it was a compound (mixture) of these polyamides or a block polymer made by copolymerization. However, as mentioned above, the present inventor has previously conducted joint research and development on injection joining technology with Toray Industries, Inc., the manufacturer of the above-mentioned "CM3506G50," and as a result, proposed a resin composition that was a block polymer containing 17% of the above-mentioned PA6I component, 77% of the PA66 component, and 6% of the PA6 component, and that added 50 parts of GF to 100 parts of resin. As mentioned above, it has been found that the injection joint with the NMT-treated A5052Al alloy exhibits a shear joint strength of 26 MPa (Patent Document 2).
[0023] Therefore, according to the inventor's aforementioned NMT theory, a compound resin containing 10% or more of semi-aromatic polyamide and 90% or less of a mixture of PA66 and PA6, or a linked block polymer thereof, is basically effective as a polyamide-based resin composition suitable for injection joining. In terms of the quantitative relationship (mixture) of each component, it is a mixed resin composition in which the main component is a mixed resin component of PA66 and PA6, and the sub-component is a semi-aromatic polyamide resin component. In this resin composition, if the ratio of the sub-component is increased, the crystallization rate during quenching decreases, and if the ratio of the sub-component is decreased, the crystallization rate during quenching increases. Based on this knowledge, the mixing ratio of the resin composition can be adjusted to produce an injection-joined product of optimal quality. In other words, the resin composition has a main component of PA66 resin and a minor component of a mixed component of PA6 and semi-aromatic polyamide. If the PA6 component in the minor component resin is increased while keeping the minor component ratio at around 25%, the crystallization rate during quenching increases, whereas if the semi-aromatic component in the minor component resin is increased, the crystallization rate during quenching decreases. Based on this knowledge, it is possible to adjust the resin composition ratio to obtain an injection-bonded product of the highest quality.
[0024] According to the catalog published by the manufacturer, the above "CM3506G50" has excellent heat resistance with a melting point of 228°C and HDT (Heat Distortion Temperature) of 240°C, a tensile strength of 245MPa, and a tensile elongation at break of 0.2%, making it a hard and rigid resin. It contains a large amount of GF (33.3%) compared to the entire resin composition, but has a good appearance (GF is not exposed on the surface). This published technical document also states that the purpose of this resin is to be used for injection molding, and that it is a compound resin that contains a large amount of GF, is hard and rigid, has a good appearance, and is intended to be a glossy and durable structural resin. Generally, resins with a high GF content tend to have exposed GF ends and do not have a good appearance. However, there is no description of injection joining technology for this resin. What can be said from these characteristics is that the resin has a good appearance because the crystallization speed during quenching is suppressed, and the GF ends are also wrapped, resulting in a smooth appearance of the molded product. In short, the block polymer containing 17% PA6I component, 77% PA66 component, and 6% PA6 component shown in Patent Document 2 is a polyamide-based resin composition that corresponds to the above-mentioned NMT theory, and is a resin composition whose main component is a mixed resin component of PA66 and PA6 and whose minor component is a semi-aromatic polyamide resin component.
[0025] On the other hand, the shape (test piece) shown in FIG. 1, which is obtained by injection joining the above-mentioned "CM3506G50" and an Al alloy that has been subjected to the above-mentioned chemical conversion treatments such as NMT7 treatment, NMT8 treatment, and NMT5-Ano treatment, showed a high joining strength of 50 MPa or more when the shear joining strength between the resin part and the metal part was measured. This test piece also showed a strong shear joining tackiness value (described later) of 38 MPa or more, and was judged to be the optimal resin for injection joining as a polyamide-based resin composition. Just to be sure, when the above-mentioned "CM3506G50" was analyzed by pyrolysis gas mass, it was found that the resin contained at least 10% or more of semi-aromatic polyamide components, and the rest was composed of aliphatic polyamide components mainly consisting of aliphatic polyamide components such as PA6 and PA66. This satisfies the above-mentioned "resin composition whose main component is a mixed resin component of PA66 and PA6 and whose minor component is a semi-aromatic polyamide resin component", and the polyamide resin composition disclosed in Patent Document 2, "CM3506G50", satisfies the composition range conditions of polyamide resin proposed by the present inventors themselves.
[0026] In short, the exact resin composition structure of the above "CM3506G50" is only outlined, but the details are completely unknown, and it was not possible to determine whether the detailed composition is close to or far from the "block polymer containing 17% PA6I, 77% PA66, and 6% PA6" shown in Patent Document 2, or even whether PA6I or PA6T is used. In any case, the resin composition that can be used in the present invention is one that "contains at least 10% or more of semi-aromatic polyamide in the resin content, and the rest is composed of aliphatic polyamide components mainly consisting of aliphatic polyamide components such as PA6 and PA66," as described below, and is defined as usable if the injection joining strength with various NMT7-treated Al alloys is 45 MPa or more in shear joining strength and 38 MPa or more in shear joining viscosity.
[0027] In conclusion, it is the composition ratio between several types of polyamides, namely PA66, PA6, and semi-aromatic polyamide, that constitute the resin, and several dozen types are created based on the composition ratio of Patent Document 2. Whether the created product is a compound or a block polymer, the resulting resin is used to create an injection-bonded product with an Al alloy, which is then subjected to tensile breaking to select the strongest one. As the inventor of the present invention, the greatest achievement is that an injection-bonded product is created between an Al alloy that has been subjected to NMT7 treatment or the like and a polyamide-based resin, and the bonding strength is about 50 MPa, which is a high-performance bonding strength that has not been obtained in the past. Even if the resin that demonstrates this is only one type of the above-mentioned "CM3506G50", after this discovery, by disclosing this invention to the above-mentioned manufacturers, it should become easier to manufacture improved resins that show higher injection bonding strength for new NMT-treated products of Al alloys and other metal materials, and this is the reason for disclosing the details of the development process of this invention here.
[0028] In short, the polyamide resin composition is a composition that is broadly considered to be the resin composition of the above-mentioned "CM3506G50", that is, the resin component contains at least 10% or more of a semi-aromatic polyamide component as a minor component, and the rest is a composition in which the aliphatic polyamide component in PA6 and PA66 accounts for the main components. This composition contains 25 to 35% by weight of GF as a whole. On the premise of using such a polyamide resin composition, the surface treatment (chemical conversion treatment) of the Al alloy pieces in the integrated composite of the present invention is a conversion of the joining technology of "for example, 'SGX120' (manufactured by Tosoh Corporation (headquarters: Tokyo, Japan))" (hereinafter referred to as "SGX120"), which is a polyphenylene sulfide resin (hereinafter referred to as "PPS")-based resin composition. The present invention was developed based on the determination that by applying a surface treatment technology for aluminum alloys that gives the surface shape of the alloy the highest level of mechanical properties through injection joining of a PPS resin composition with an aluminum alloy, it is possible to provide an optimal integrated metal-resin product for use as a part or component for automobiles, aircraft, mobile robots, other outdoor equipment, and machines. [Prior art documents] [Patent documents]
[0029] [Patent Document 1] WO2004 / 041532 [Patent Document 2] Patent Publication No. 2007-182071 [Patent Document 3] WO2012 / 070654 [Patent Document 4] Patent Publication 2019-188651 [Patent Document 5] Patent Publication No. 2019-217704 [Patent Document 6] Patent Publication No. 2007-050630 [Patent Document 7] WO2008 / 069252 [Patent Document 8] WO2008 / 081933 [Patent Document 9] WO2008 / 047811 [Patent Document 10] WO2008 / 078714 [Patent Document 11] WO2009 / 011398 [Patent Document 12] Patent Publication No. 2006-315398 [Patent Document 13] Patent Publication No. 2010-064496 Summary of the Invention [Problem to be solved by the invention]
[0030] In a joint in which metal and resin are integrally joined, if the lack of moisture resistance of the resin composition can be compensated for by applying an oil or painting, it is possible to use a polyamide resin, which is inexpensive and remains hydrophilic, instead of using expensive super engineering plastics such as PPS. Therefore, if an injection joint is obtained in which steel or Al alloy material is used as the metal material and a polyamide resin composition is used as the resin material, and the joint strength between the metal and resin in the integrated product is sufficiently high, it is necessary to apply an oil or paint to the injection joint and, considering the environment in which the injection joint is used, to perform a high temperature and high humidity test and, at the same time, a severe temperature shock test of 3,000 cycles to find a product that can withstand both. When using aluminum or steel materials that are prone to rust in moving machines such as automobiles, it is common practice to apply an oil or paint to the metal materials, etc., so we tried to expand the range of injection joints that can be used under the assumption of this surface treatment, with this condition. In short, the present invention relates to an Al alloy material and a polyamide resin composition. The present invention was invented in light of the above-mentioned development history and background, and achieves the following objects.
[0031] The object of the present invention is to provide an integrated composite of metal and resin in which an aluminum alloy and a polyamide resin composition are directly bonded to each other, which has high resistance to high temperatures and high humidity as well as high temperature shock, and a method for producing the same. Another object of the present invention is to provide an integrated composite of metal and resin in which an aluminum alloy and a polyamide-based resin composition are directly bonded to each other, which can be produced by injection joining, which is a highly productive insert molding method, and a method for producing the same. [Means for solving the problem]
[0032] The present invention provides the following means to solve the above problems. The integrated composite of metal and resin according to the present invention 1 is An integrated composite of metal and resin, comprising an aluminum alloy piece having a surface to be joined that has been chemically treated, and a polyamide-based resin composition directly bonded to the surface to be joined by injection bonding, The bonding surface is such that an uneven surface with a period of several tens of μm is clearly observed when observed at a magnification of 1,000 with an electron microscope, a fine uneven surface with a period of 0.8 to 5 μm is observed when observed at a magnification of 10,000, and an ultrafine uneven surface with a period of 30 to 100 nm is observed when observed at a magnification of 100,000, The polyamide-based resin composition contains 10% or more of a semi-aromatic polyamide component as a minor component in the resin content, with the remainder being mainly an aliphatic polyamide component, and contains 25 to 35% by weight of short glass fibers as a whole; The joining surface is characterized in that the shear joint strength is 45 MPa or more, a shear external force of 75% or more of the shear joint strength can be applied continuously 300 times without breaking, and the maximum shear external force value at which the shear joint does not break even when an external force is applied continuously 300 times, and the shear joint tackiness value is 38 MPa or more.
[0033] The integrated composite of metal and resin according to the second aspect of the present invention is the integrated composite of metal and resin according to the first aspect of the present invention, wherein the integrated composite of metal and resin is a test piece specified in the international standard (ISO19095), and the test piece is subjected to a durability test in which paint or oil is applied to the entire test piece and the test piece is exposed to an environment set at a temperature of 85° C. and a humidity of 85% for 1,000 hours, and the bonding surface In the measurement of the shear bond strength, the test specimen has a moist heat resistance of 75% or more of the value before the test, and has a temperature shock resistance capable of withstanding a temperature shock test of 3,000 cycles at -50°C / +150°C.
[0034] The integrated composite of metal and resin of Invention 3 is the integrated composite of metal and resin of Invention 1 or 2, characterized in that the aluminum alloy piece is a long member (2) that is a long plate material having an L-shaped, U-shaped, or semicircular cross section, and the aluminum alloy piece and the polyamide-based resin composition are integrally joined to each other by a structure (5) in which the polyamide-based resin composition fills a groove-like recess (3) in the long member (2) to increase the mechanical strength of the groove-like recess (3).
[0035] The metal and resin integrated composite of the fourth invention is the metal and resin integrated composite of the third invention, characterized in that a through hole penetrating the aluminum alloy piece is formed in the groove-shaped recess (3) of the metal, and the through hole is filled with the polyamide-based resin composition.
[0036] The integrated composite of metal and resin of the present invention 5 is the integrated composite of metal and resin according to the present invention 1 or 2, surface the resin molding is characterized in that it comprises a resin molding central portion (14, 15) which is the polyamide-based resin composition forming the central portion of the resin molding, a resin intermediate portion (16) which surrounds the resin molding central portion and has a thickness thinner than that of the resin molding central portion, and a thin-walled resin portion (17) which substantially surrounds the entire periphery of the resin molding central portions (14, 15) and the resin intermediate portion (16) and has a width of 5 mm or more, the thin-walled resin portion (17) having a thickness of 0.5 to 1.5 mm, and the resin intermediate portion (16) having a thickness of 1.0 to 3.0 mm.
[0037] The metal and resin integrated composite of Invention 6 is the metal and resin integrated composite of Invention 1 or 2, and the metal and resin integrated composite (30, 40) is characterized in that the aluminum alloy pieces are two plate materials (31, 35), the polyamide-based resin composition (32) is sandwiched between the two plate materials (31, 35) and bonded together, and the polyamide-based resin composition (32) has a thickness of 1.0 to 2.0 mm.
[0038] The metal and resin integrated composite of Invention 7 is the metal and resin integrated composite of Invention 6, characterized in that one or more heat conductive rods (34) made of an aluminum alloy are connected between the two plate materials (31, 35) so as to reduce the temperature difference between the two plate materials (31, 35).
[0039] The manufacturing method of an integrated composite of metal and resin of Invention 8 is a manufacturing method of an integrated composite of Inventions 1 to 7, characterized in that the integrated composite of metal and resin is manufactured by inserting the aluminum alloy pieces that have been subjected to a chemical conversion treatment into an injection molding die, and then injecting the polyamide-based resin composition to integrate the aluminum alloy pieces and the polyamide-based resin composition.
[0040] The reasons and background for the above-mentioned configuration and manufacturing method of the present invention will be described below. [Aluminum alloy flakes (Al alloy flakes) and their surface treatment] The Al alloy pieces used in the present invention are all types of Al alloys classified as wrought Al alloys and casting Al alloys and specified by JIS (Japanese Industrial Standards) and the like. Wrought Al alloys are specified by the JIS from the 1000s to the 8000s, and are similarly specified by corresponding alloy numbers in countries other than Japan, so that Al alloy materials with almost the same composition are available worldwide. On the other hand, the number of classifications of casting Al alloys is also specified by JIS, although it is fewer than the wrought Al alloy types, and these are also included in the Al alloys of the present invention. However, about 90% of the casting Al alloys are ADC12. At least for ADC12, an optimal surface treatment method has already been proposed, and will be shown in the examples described below.
[0041] The chemical conversion treatment method for the surface of the Al alloy pieces can be the above-mentioned NMT treatment method shown in Patent Documents 1 and 2, the NMT2 treatment method shown in Patent Document 3, and the NMT5, NMT7, and NMT8 treatment methods shown in Patent Document 4. In addition, there is the NMT-Ano treatment method described in Patent Document 13 as a new NMT type treatment method, and its improved form is the NMT5-Oxy, NMT7-Oxy, NMT5-Ano, and NMT7-Ano treatment methods shown in Patent Document 4. The chemical conversion treatment method for the surface of the Al alloy can be any of the surface treatment methods developed and proposed by the inventor of the present invention. The appearance of the surface chemically treated by these methods is usually a matte surface when observed visually. As a substitute for the integrated composite of metal and resin of the present invention, an injection joint having the shape (test piece) shown in Figure 1 was used for the test. The test piece was set in a tensile breaking machine and the shear joint strength was measured. From these measured values, the treatment method that showed the highest value for each Al alloy was selected and this was determined as the optimal treatment method.
[0042] The reason is that the surface treatment method proposed for each metal type was developed by the inventor while mainly using the above-mentioned "SGX120", which is a PPS-based resin composition. When this PPS-based resin composition is replaced with a polyamide-based resin composition containing a semi-aromatic polyamide of the present invention, the surface shape formed by this treatment method does not necessarily have the same tendency as when PPS is used. Therefore, the optimal chemical conversion treatment method for polyamide-based resin compositions was judged to be good or bad by test pieces that had undergone all the chemical conversion treatments already proposed by the inventor of the present invention. Furthermore, if the resin is so hydrophilic that it is subjected to a high temperature and high humidity test, it may peel off within a few weeks. For example, if there is a product that shows a shear bonding strength of 50 MPa at the beginning, it will become weak and cannot be used as a product if it is subjected to an extremely severe accelerated test of a high temperature and high humidity test at a temperature of 85°C and a humidity of 85% for 1,000 hours.
[0043] However, it was estimated that a composite that meets the durability test could be made if the composite was protected from air and moisture by painting the entire test piece with an epoxy-based baking paint or applying an oil such as engine oil. Although it is a different material, the above test piece was placed in a box filled with dry air as a preliminary test, and placed in a drawer of a work desk for one year (spring, summer, fall, and winter) in the same factory (Ota City, Gunma Prefecture, Japan) where the test of the present invention was performed. The bonding strength did not decrease. In short, even parts for mobile machines may be used in dry air as described above, and it was determined that the standards for high temperature and high humidity resistance that are too strict would narrow the industrial field to which the present invention can be applied. If we dare to say it, in the present invention, it is sufficient for a material to meet the high temperature and high humidity resistance to pass the temperature shock test of several thousand cycles (described later) proposed in the present invention.
[0044] [Polyamide resin composition] The polyamide resin composition of the present invention is a composition containing 10% or more of semi-aromatic polyamide components in the resin content, the remainder being mainly aliphatic polyamide components, and containing 25 to 35% by weight of short glass fibers. The polyamide resin composition will be described below. As described in the previous section, the procedure for selecting the injection-bonded product of the Al alloy and the polyamide synthetic resin composition is clear. The polyamide resin composition preferably usable in the present invention may be the above-mentioned "CM3506G50" in the commercially available products, or a semi-aromatic polyamide resin composition commercially available as a subsidiary component, or another resin that exhibits performance equal to or higher than that of the above-mentioned "CM3506G50" among polyamide resin compositions containing semi-aromatic polyamides. Alternatively, one or more types of polymers used in the resin composition of the above-mentioned "CM3506G50" are determined, and then a composition is prepared by replacing and mixing several suitable similar substances with the polymers, and an injection-bonded product is prepared with the composition, and various tests are performed to search for effective resin composition components.
[0045] The idea behind this search is to first take measures to suppress the crystallization rate during quenching by combining two aliphatic polyamides, and then add an appropriate semi-aromatic polyamide to further slow down the crystallization rate. This was explored through experiments using the combination of three polyamides, PA6, PA66, and PA6I, as shown in Patent Document 2, but the desired bonding strength could not be obtained before the development of the chemical conversion treatment methods for NMT7 and NMT8 described above. Therefore, the polyamide-based resin composition that can be preferably used in the present invention is the above-mentioned "CM3506G50), and it was estimated that the polyamide-based resin composition to be further improved would be a composition based on the above-mentioned "CM3506G50" with the ratio of each polyamide constituting the composition slightly changed.
[0046] (Linear expansion coefficient of polyamide resin composition) On the other hand, the above "CM3506G50" contains 50 parts by weight of GF as a reinforcing fiber, with the total resin content being 100 parts by weight. This means that 33.3% of the total resin composition is GF. The reason for selecting the above "CM3506G50" is that it showed high injection bonding strength as mentioned above, but the fact that it contains more than 33% GF is also a very important factor for injection bonding technology. The driving force for obtaining injection bonding strength is the crystallinity of the resin content, and more specifically, in relation to the injection molding time, a hardening speed that matches the crystallization speed during quenching is required. Simply put, if the content of GF contained as a reinforcing fiber is too high, the resin content will naturally decrease and the injection bonding strength will decrease. On the other hand, if the GF content is zero, that is, if a resin composition containing only resin content is used, a high injection bonding strength can be obtained, but the linear expansion coefficient is 8 to 10 x 10 -5 K -1 The linear expansion coefficient of Al alloy is very high at 2.3×10 -5 K -1 Therefore, the difference in linear expansion coefficient is large, which leads to a decrease in the joining strength.
[0047] Therefore, the injection-bonded product (test piece) of the shape shown in FIG. 1 obtained from both of them shows high shear bond strength between the metal and the resin, but when the test piece of FIG. 1 is subjected to a temperature shock tester of -50℃ / +150℃, it breaks by itself in about 100 cycles. In short, the result of this temperature shock test shows that in order to reduce the difference in linear expansion coefficient between the metal material and the resin and to withstand severe temperature changes (temperature shock), the GF content is better to be high, and the higher the GF content, the higher the mechanical strength of the resin itself. In the end, the balance between the GF content and the resin content is important, but in the case of the PBT-based resin composition and the PPS-based resin composition, the actual shear bond strength was highest when the GF content was 15 to 25% of the total. The GF content of the above-mentioned "CM3506G50", which is a polyamide-based resin composition, is 33.3%, which seemed to be too high compared to the PPS-based resin composition, but the actual measurement of the injection bond strength showed that it maintained a high shear bond strength. The reason for this is presumably due to the high adhesive strength between the resin and GF, which is believed to be due to the high affinity between the peptide bond portion of the polyamide and glass.
[0048] When the GF content increases to about 33%, the linear expansion coefficient drops significantly to about 2.5×10 -5 K -1 On the other hand, the linear expansion coefficient of Al alloys is 2.3×10 -5 K -1 Therefore, the linear expansion coefficient of the above-mentioned "CM3506G50" containing GF is very close to that, and the injection-bonded product of these two has the advantage of being able to withstand several thousand cycles in a temperature shock test without any problems. Furthermore, even if the GF content is reduced from 33% to nearly 20%, the linear expansion coefficient will only be equivalent to that of the above-mentioned "SGX120", and the shape shown as the injection-bonded product that can withstand 3,000 cycles in the -50℃ / +150℃ temperature shock test described in Patent Document 5 (the model is shown in Figures 4 and 5) is "CM3506G50" with a GF content of 33.3%, and it can easily withstand that temperature shock.
[0049] [Injection joining and annealing processes] In the present invention, there are some points to be noted as resin molding conditions during injection joining operation using an injection molding machine, compared to normal injection molding. The mold temperature, pre-injection time, and pressure dwell time should be noted, and the mold temperature is basically set to a high level, although there is a temperature range specified by the resin manufacturer. That is, if the temperature of the injection molding mold is low, it becomes difficult for the resin to penetrate into the ultra-fine recesses on the metal surface inserted into the injection molding mold. Specifically, when using the above-mentioned "CM3506G50", the mold temperature is preferably around 140°C. The pre-injection time during this molding refers to the time until the Al alloy piece is injected from the insert into the mold, but in the present invention, the pre-injection time can be ignored if the Al alloy piece to be inserted is small. However, for example, if a large item weighing 1 kg is used, the pre-injection time must be set to 1 to 1.5 minutes, otherwise the temperature of the insert will not rise to near the mold temperature, and the expected injection joining force cannot be secured. In addition, the time from the start of injection to the end of dwelling is estimated to be a little slow in the case of the above-mentioned "CM3506G50" in consideration of the ideal time required for the crystallization speed during quenching, so it is advisable to open the injection mold after about 20 to 30 seconds and proceed with the demolding operation. In the examples described later, the time from the start of injection to the opening of the injection mold was always 30 seconds.
[0050] The injection-bonded product obtained after being released from the injection mold should not be left to cool as it is to be used as the final product, but should be subjected to a heat treatment (annealing treatment) of about 150°C for 1 hour, preferably within a few hours, to sufficiently advance resin crystallization before completing the entire injection bonding process. In the experiment of the present invention, the total time of the injection time and the pressure holding time was set to 20 to 30 seconds, and many test pieces shown in Figure 1 were made to determine the minimum required pressure holding time, but after this, the injection-bonded product (composite) should be further annealed and left to cool to be used as the final product.
[0051] [Measurement of shear joint strength and shear joint viscosities] ISO19095 specifies the method of measuring the tensile lap-shear strength and tensile strength between the metal part and the resin molded part in the injection-bonded product. According to this specification, the test piece shown in FIG. 1 is tensile broken by a tensile tester to measure the shear bond strength, and the test piece shown in FIG. 2 is tensile broken by a tensile tester to measure the tensile bond strength. This shear bond strength measurement method was used by the present inventor in Patent Documents 6 to 10, and the tensile bond strength measurement method was started by the present inventor from around 2015 after various experiences. In either case, accurate measurement was not possible using the conventional methods specified in JISK6849, JISK6850, etc., which were conventional methods for measuring adhesive strength and bond strength, so the present applicant (Taisei Plus Co., Ltd.) proposed a new specification, which was considered by government agencies in Japan based on this proposal, and was approved as ISO19095 after deliberation by ISO-related government agencies of various countries.
[0052] Based on this premise, the inventor further devised a new method for measuring the joining strength, called the "shear joint tackiness" value, in addition to the shear joint strength, and placed more importance on this "shear joint tackiness" value than on the shear joint strength value. This is based on the experience of producing an injection joint (shape shown in FIG. 1) using the PPS resin composition "SGX120" and measuring its resistance to shear external forces. In this case, the shear joint strength is at most 40 to 42 MPa, and values above that are basically not observed. In short, when an injection joint (FIG. 1) is obtained using a certain injection joint resin, even if the type of metal used, the chemical surface treatment method, etc. are changed, if a fracture test is performed on the test piece shown in FIG. 1 and improvements are made, it will arrive at something that seems to be an upper limit value. Therefore, even if the surface treatment method of a certain type of metal alloy piece is further improved, it becomes difficult to tell from the shear joint strength value whether an improvement has been made or not and the warping has deteriorated when the shear joint strength approaches about 40 MPa. Therefore, the inventors decided to measure a new value called "shear joint tackiness" and to judge that a better surface treatment method has been achieved if the value is higher. From the same perspective, the injection joint using the above-mentioned "CM3506G50" was subjected to a tensile tester.
[0053] From the above, the term "shear joint toughness" in the present invention refers to the results obtained by the following experimental method. When measuring the shear joint toughness, the "shear joint strength" is measured in advance using a test piece (shaped as shown in FIG. 1) in a tensile tester. Then, a test is conducted in which a tensile force of about 75% of the "shear joint strength" is repeatedly applied 300 times to the same test piece made at the same time. The way in which the load is applied by the tensile tester in this test method is set by the operating software of the control device of the tester. This setting is such that the maximum tensile force is about 75% of the "shear joint strength" value, the minimum tensile force is about 2 / 3 of the maximum tensile force, and the tensile speed is ±10 mm / min as one cycle, and 300 cycles of repeated continuous operation are performed. If there is no shear fracture under this repeated tensile load, the maximum tensile load is increased by about 2 MPa, and a test is conducted in which the same repeated load is applied. If the test piece still does not break, a further 2 MPa is applied and the same procedure is repeated until the test piece shown in Figure 1 breaks. If the test piece breaks, the maximum tensile force before the break is used as the force in kg / 0.5 cm of the tester in the present invention. 2 The value was converted to MPa, and in the present invention, this was taken as the "shear joint toughness" value.
[0054] [High humidity resistance test of injection-bonded products] The maximum humidity that an automobile receives from the global environment is estimated to be, for example, when it rains in a tropical region at about 40°C between the rainy and dry seasons (humidity 100%). In such an area, if the composite of the present invention is used as an automobile component, the actual highest temperature and humidity in the automobile occurs when rainwear, clothing, etc. that are wet from the rain are brought into the automobile, and then the doors are closed with these left in the automobile, leaving the automobile unoccupied, and strong sunlight shines into the automobile, causing the temperature inside the automobile to reach a high temperature. In such a case, the temperature inside the automobile is estimated to be a maximum of 60°C if the amount of moisture brought in is very large, and as high as 100°C if the amount of moisture is small. Based on this assumption, the maximum humidity inside the automobile is estimated to be about 95% humidity at a temperature of 60°C. However, although these temperature and humidity values can certainly be used as a high humidity test for a test method for covering materials for automobile seats, they are not suitable for a high humidity resistance test of the integrated composite of metal and resin of the present invention. Assuming that an automobile is used for a maximum of 20 years, how long should the test time be under such high temperature and humidity? As there are no standards in this field, no one can give a clear answer. Therefore, in the end, it was decided to evaluate the automobile by exposing it to the commonly used temperature of 85°C and humidity of 85% for 1,000 hours. In other words, it is an accelerated test in which the automobile is exposed to extremely severe high temperature and humidity away from the environment in which it is actually used. Therefore, the inventor hesitated as to whether 1,000 hours was an appropriate time, but based on the experience from the experiment described in Patent Document 4, the inventor decided that 1,000 hours (42 days) was sufficient for the present invention to determine whether problems would occur or not.
[0055] The following also includes other injection-bonded products (composite of metal and resin). We made injection-bonded products (test pieces in Fig. 1) of various Al alloys, steels (SPCC was used), stainless steels, titaniums, etc., which were surface-treated for injection bonding, and the above-mentioned "CM3506G50". We tested these test pieces, or those that were painted and oiled, at 85℃ and 85% humidity for 1,000 hours. In these experiments, without oiling, the SPCC (cold-rolled steel plate) rusted heavily in just one day, and the aluminum alloy pieces also showed a color change that seemed to be caused by rusting in the exterior parts. Even in the oiled parts, the SPCC showed coloring and rust patterns in small places after about 3 days, as if the oil had peeled off. Furthermore, in the oiled Al alloys, stainless steels such as SUS304 and SUS430, and Ti alloy metal pieces, no abnormalities were observed in appearance even after 100 hours in the test exposed to high temperature and high humidity. In short, among the metals that are injection-bonded with hydrophilic polyamide resin compositions, the ones that will definitely rust if left in water are Al alloys and ferritic stainless steel SUS430. However, when these were oiled in this experiment, no change was observed in appearance. Therefore, in terms of bonding strength, if the product was oiled, it was presumed that the bonding strength between the metal and resin of the injection-bonded product had moisture and heat resistance.
[0056] As for the oil-treated product in which a commercially available engine oil was applied to an injection-bonded product of an Al alloy and the above-mentioned "CM3506G50", after completing the 1,000-hour test under high temperature and high humidity as described above, a drying process was performed at 80°C for 48 hours, and in addition to this drying, a high-temperature drying process was performed at 150°C for 4 hours to determine the shear bond strength. After this two-stage drying process, the shear bond strength was compared with the value shown by the initial injection-bonded product, and if there was a small decrease, it was judged that the bond strength of the injection-bonded product was substantially resistant to moist heat. The reason for performing the drying process in two stages in this way is that the test at 85°C and 85% humidity is merely an accelerated test, and is an environment of high temperature and high humidity that is not practically possible. In this environment, if a polyamide-based resin composition, which has a small amount of water absorption, is subjected to the drying process, the resin molded product itself absorbs the maximum amount of water and remains stable. This is because it was judged necessary to heat the material to about 80°C to volatilize the easily mobile moisture, and then expel the water molecules that had been incorporated into the polyamide and were somewhat stable at 150-170°C, restoring the material to its original polyamide-based resin composition. The results of this experiment are shown in the examples below, but many of the Al alloys treated with NMT7 and NMT8 had high injection joining strength with the above-mentioned "CM3506G50," and these had high humidity resistance that was deemed sufficient for practical use.
[0057] [-50℃ / +150℃ temperature shock test of injection-bonded parts, 3,000 cycles] The above-mentioned "CM3506G50" used is a resin composition containing 33.3% by weight of GF. Therefore, its linear expansion coefficient is (8 to 10) x 10 of a typical resin composition that does not contain reinforcing fibers. -5 ℃ -1 Much lower than 2.5×10 -5 K -1 On the other hand, the Al alloy material is 2.3×10 -5 K -1The linear expansion coefficients of the two are very close to each other. However, the semi-aromatic polyamide resin composition used in the present invention is not limited to the above-mentioned "CM3506G50". What is defined and limited in the present invention is the shear joint strength when the injection joint is made into the test piece shown in FIG. 1, and the height of the shear joint tackiness value. Therefore, if the GF content of the polyamide resin composition mainly composed of a semi-aromatic polyamide that satisfies this condition is in the range of 20 to 35%, it can provide a sufficiently high shear joint strength.
[0058] In other words, if a polyamide resin composition consisting of semi-aromatic polyamide and aliphatic polyamide contains 20 to 35% GF, its average linear expansion coefficient is (4.0 to 2.5) x 10 -5 K -1 In this case, the difference in linear expansion coefficient with Al alloy is (1.7~0.2)×10 -5 K -1 Therefore, if it is put into a temperature shock tester at -50℃ / +150℃ and there is a temperature change of 200℃ between the upper and lower temperatures, it will be 200℃×(1.7~0.2)×10 -5 K -1 =(3.4~0.4)×10 -3 A difference in length of 0.34%~0.04% occurs between the two materials with each temperature change. Although 0.04% is small, 0.34% is a sufficient value to cause the joint surface between the resin and the Al alloy material to break or become weak.
[0059] The bond between the resin and the Al alloy material is maintained near the bonding surface by the strong bonding force between them, and in the test piece of the injection-bonded product shown in Figure 1, the lower layer of the resin part (the resin layer near the bonding surface) is forced to expand and contract with the Al alloy material. If the temperature change is not an artificial temperature shock but a gradual change in temperature such as seasonal temperature changes, the resin part will deform slightly and the internal stress caused by the difference in linear expansion coefficient will be within the allowable elastic limit, but in the temperature shock cycle test, it will not be within the allowable elastic limit. However, in the case of the smallest temperature change of 0.04% mentioned above, as long as the injection-bonded product actually used is large and the thickness of the resin material does not exceed 3 mm, there is no problem regardless of the shape of the injection-bonded product. If there is one thing to be noted in the design, it is that when the temperature rises or cools rapidly, the Al alloy material has good heat conductivity and reaches the environmental temperature faster than the resin part, so the effect of this should be addressed. The key is to always strive to keep the temperature difference between the two materials small by making the resin part thin or by using a structural design that consciously creates a thermal corridor (thermal conduction).
[0060] On the other hand, when the GF content is low at about 20%, that is, when the difference in elongation in length is at its maximum of 0.34%, it goes without saying that care must be taken in the structural design of the injection-bonded product. For example, even in a small composite with a bonding area of 10 mm x 5 mm, as in the test piece shown in Figure 1, the longest part of the bonding surface is 11.2 mm, and 0.34% of that is 0.038 mm. Even with this slight difference in length, if subjected to a temperature shock test of 3,000 cycles at -50°C / +150°C, there is a good chance that peeling will occur at the edges of the four corners of the weakest bonding surface. In the test piece shown in Figure 1, the resin part is 3 mm thick, and the thicker the resin part is, the more likely it is that peeling will occur starting from the four corners of the bonding surface in a temperature shock test of several thousand cycles. Conversely, the thinner the resin part is, the more likely it is that the resin part will not peel off from the metal plate at all, even if the temperature shock is applied for more than several thousand cycles, because the resin part will follow the expansion and contraction of the metal.
[0061] In order to prove the effect of reducing the thickness of the resin part, the inventors used a router to cut the resin part of the joint of the injection-jointed test piece shown in Figure 1, which was 3 mm thick, to prepare pieces with a thickness of 2 mm and 1 mm, as described in Patent Document 5, and subjected these to the above-mentioned temperature shock 3,000 cycle test. The injection-jointed material in this case was an Al alloy and a PPS-based resin composition "SGX120," and the difference in linear expansion coefficient between the metal and the resin was 1.7 x 10 -5 ℃ -1 However, no peeling was observed at all in the case of a resin thickness of 1 mm, and even in the case of a resin thickness of 2 mm, only very small peeling was observed in one or two of the four corners. Based on this, the composite described in Patent Document 5 states that if the resin thickness of the PPS resin composition is 1.5 mm or less, even if the joining area is infinite (a practical area), the injection-joined product of the Al alloy piece and the above-mentioned "SGX120" can withstand the temperature shock 3,000 cycle test.
[0062] From the results described in the above Patent Document 5, the linear expansion coefficient difference in the injection-jointed product (composite) of the present invention is at most 1.7 × 10 -5 K -1 From this alone, it is similar to the injection-bonded product (composite) of Al alloy and PPS resin composition "SGX120", and the design method of the injection-bonded product is presumed to be similar to the structure shown in Patent Document 5. In any case, since the injection bonding strength of the above-mentioned "CM3506G50" is sufficiently high even with a GF content of 33.3%, there is no need to intentionally reduce the GF content. Reducing the GF content reduces the tensile strength of the resin itself and increases water absorption, which is not desirable for a resin composition. Effect of the Invention
[0063] The integrated composite of metal and resin and the manufacturing method thereof of the present invention can provide a joint in which an aluminum alloy and a polyamide resin composition are directly bonded, which has high resistance to high temperatures and high humidity as well as high temperature impact resistance. In addition, the manufacturing method of this integrated composite of metal and resin is insert injection molding, so that the productivity is high. [Brief description of the drawings]
[0064] [Figure 1] FIG. 1 is an external view showing the shape of an injection-bonded product (test piece) for the purpose of measuring the "shear bond strength" between a metal part and a resin part, which is an integrated metal and resin bonded product as specified in ISO19095. [Diagram 2] FIG. 2 is an external view of an injection-bonded product (test piece) that is an integrated metal-resin bond as specified in ISO19095 and is used to measure the "tensile bond strength" between the metal part and the resin part. [Diagram 3] FIG. 3 is a view showing the external appearance of an auxiliary jig used when measuring the shear joint strength of the test piece in FIG. 1, which is an integrated joint of metal and resin as specified in ISO19095. [Figure 4] Figure 4 shows a test piece in Figure 1 above, where the upper part of the resin joint surface was machined off, thinning the original thickness of 3 mm to 2 mm. [Diagram 5] Figure 5 shows a test piece in Figure 1 above, where the upper part of the resin joint surface was machined off, thinning the original thickness of 3 mm to 1 mm. [Figure 6] Figure 6 shows electron microscope photographs of the A5052Al alloy that was subjected to NMT7 treatment, with Figure 6(a) being magnified 1,000 times, Figure 6(b) being magnified 10,000 times, and Figure 6(c) being magnified 100,000 times. [Figure 7] FIG. 7 is an external view showing an example of the structure of an integrated composite of metal and resin according to the present invention, in which a long aluminum alloy member having an L-shaped cross section is lined with a resin composition for reinforcement. [Figure 8] FIG. 8 is an external view showing a modified example of the structure of the integrated composite body of metal and resin according to the present invention shown in FIG. [Figure 9] FIG. 9 shows an example of the structure of an integrated metal and resin composite of the present invention, in which a boss made of a resin composition is erected on a rigid Al alloy plate and the outer periphery is reinforced with a thin-walled resin composition, with FIG. 9(a) being a plan view and FIG. 9(b) being a front view. [Figure 10]FIG. 10 is an external view showing an example of the structure of an integrated composite of metal and resin according to the present invention, in which a resin composition is bonded between two aluminum alloy plate members to integrate them. [Figure 11] FIG. 11 shows an example of the structure of an integrated composite of metal and resin according to the present invention, which is a modified example of the one shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0065] Hereinafter, the embodiment of the present invention will be described with reference to a specific injection-jointed product. The integrated composite of metal and resin (hereinafter referred to as "composite") 1 shown in FIG. 7 is an example in which a polyamide-based resin composition 4 is joined by insert molding to strengthen an L-shaped angle material 2, which is an equal-leg or unequal-leg angle steel. The angle material 2 generally does not have a very high cross-sectional performance (section modulus) and the cross-sectional performance decreases depending on the direction of the load. Therefore, this is an example in which a polyamide-based resin composition 4 is integrally joined along an inner corner (recess) 3 of the L-shaped angle material 2 made of an Al alloy. This integrated composite of metal and resin 1 has a reinforcing wall 5 inserted at an angle, so it is resistant to bending, twisting, etc. and has high cross-sectional performance.
[0066] The composite 10 shown in FIG. 8 has the same basic structure and molding method as the metal and resin integrated composite 1 shown in FIG. 7. The difference is that a plurality of through holes 6 are opened in the inner corners 3 of an angle bar 2 made of an Al alloy, and a polyamide resin composition 4 is poured into the through holes 6, which have a circular cross-sectional shape, by insert molding. This integrated composite 10 of metal and resin has increased rigidity so that it can maintain its shape when an external force such as a bending moment or a torsional moment is applied to it. Note that the cross section of the through holes 6 is not limited to a circle, but may be rectangular, etc., and the position is not limited to the corners of the angle bar 2 and may be other positions.
[0067] FIG. 9 shows an example of a composite 20 formed by injection molding a resin body 13, which is a columnar protrusion, on an aluminum alloy plate 12. The composite 20 is composed of a metal rectangular plate 12 made of an Al alloy plate, and a resin molded body 13 integrally joined thereto. In this example, the metal rectangular plate 12 is 100 mm long and wide and 3 mm thick. The resin body 13 has a cylindrical portion (boss, bearing, etc.) 14 at its center, and four ribs 15 are erected at equal angles along the cylindrical portion 14 on its outer periphery so as to support it. The outer periphery of the resin molded body 13 is supported by a rectangular central pedestal 16 having a thickness of 1.5 to 3.0 mm and a side length of 50 mm. Furthermore, a rectangular peripheral pedestal 17 is formed so as to surround the outer periphery of the central pedestal 16. The peripheral pedestal 17 is formed in a rectangle having a width of 5 to 10 mm, a thickness of 0.8 to 1.5 mm, and a side length of 70 mm. That is, in order to maintain the joining force between the central columnar portion 14 and ribs 15, and the rectangular metal plate 12, the composite body 20 is formed with a central pedestal 16 and a thinner peripheral pedestal 17. The molten resin is injected from the rear surface of the rectangular metal plate 12 through a pin gate 18. This composite body 20 has different thicknesses, with the central pedestal 16 having a thickness of about 2 mm at the center and the peripheral pedestal 17 having a thickness of about 1 mm at the periphery, and is thus able to absorb the difference in linear expansion coefficient between the resin and the metal.
[0068] FIG. 10 is a perspective view of a composite 30 showing an example in which two plate members are joined with a polyamide resin composition. A polyamide resin composition 32 is sandwiched between two aluminum alloy plate members 31 and 35. The polyamide resin composition 32 is injected from a gate 33 opened as a through hole in the plate member 31. The molten resin injected from the gate 33 flows into the gap between the two plate members 31 and 35 and solidifies. The thickness of the polyamide resin composition 32 is about 1.0 to 2.0 mm. The composite 40 shown in FIG. 11 has basically the same structure as the composite 30 shown in FIG. 10. A thermal conductor 34 is disposed to reduce the temperature difference between the two plate members 31 and 35 when the composite 40 is heated from one side. The thermal conductor 34 is cylindrical in shape and is fixed to the two plate members 31 and 35 by an interference fit like a rivet. When the plate member 31 or the plate member 35 is heated, the heat is conducted through the thermal conductor 34, so that the temperatures of the two plate members 31, 35 are averaged. The thermal conductor 34 in this example uses an aluminum alloy JISA6063, but copper or the like may be used as long as it has excellent thermal conductivity. EXAMPLES
[0069] Examples of the present invention will be described in detail below. (a) Electron microscope observation An electron microscope was used mainly to observe the surface of the substrate. The electron microscope used was a scanning electron microscope (SEM) "SSM-7000F (product name)" (manufactured by JEOL Ltd., Tokyo, Japan), and observations were performed at 1 to 2 kV. (b) Measurement of bonding strength In this example, the breaking force when the injection-bonded product (test piece in FIG. 1) is tensile broken by a tensile tester is taken as the shear adhesive strength. An auxiliary jig with a shape shown in FIG. 3 is used to measure this shear bond strength. This measurement method is regulated by ISO19095. In this example, the breaking force when the injection-bonded product (test piece in FIG. 2) is tensile broken by a tensile tester is taken as the tensile bond strength. The tensile tester used was "AG-500N / 1kN (manufactured by Shimadzu Corporation (headquarters: Kyoto, Japan)"), and measurements were taken at a tensile speed of 10 mm / min.
[0070] (c) Measurement of shear joint toughness value The "shear joint tenacity value" in the present invention refers to a value obtained by the following test. The above tensile tester does not tensilely break the injection joint (test piece shown in FIG. 1), but rather measures the tensile joint strength of the test piece in advance and applies a force of about 75% of the force (shear joint strength) 300 times continuously. The operating software mode of the tensile tester is set so that this operation can be performed, and the maximum tensile force is set to the above force, the minimum tensile force is set to about 2 / 3 of the maximum tensile force, and the tensile speed is set to ±10 mm / min, and the test is performed for 300 continuous cycles. If the test piece does not break under this load, a test is performed in which a load of about 2 MPa is added to the maximum tensile force and the same load is applied 300 times repeatedly. If the test piece does not break under this load, another load of about 2 MPa is applied and the same operation is repeated until the test piece shown in FIG. 1 breaks. When the specimen breaks, the maximum tensile force before the break is measured and expressed in MPa, which is the "shear adhesive toughness" value. The tensile tester used is the "AG-500N / 1kN" mentioned above.
[0071] (d) Temperature shock cycle test The temperature shock cycle test was conducted using a temperature shock cycle tester, the "Small Thermal Shock Apparatus TSE-12-A (manufactured by Espec Corporation (Head Office: Osaka, Japan))." Standard conditions for the temperature shock cycle test were cold room temperature -50°C, hot room temperature +150°C, 30 minutes in each room, and approximately 5 minutes for the indoor air temperature to stabilize when moving. The temperature shock cycle time was 65 minutes per cycle, excluding the automatic shutdown of the cooling system to prevent ice block growth. (e) High temperature and humidity test The high temperature and humidity test was carried out by placing the injection-bonded product (such as the test piece shown in Figure 1) in a high temperature and humidity environment of 85℃ and 85% humidity, usually for 1,000 hours. The high temperature and humidity tester used was Model "1H400" (manufactured by Yamato Scientific Co., Ltd. (head office: Tokyo, Japan)).
[0072] [Experimental Example A] Surface treatment of each material [Experimental Example A1-1] Surface treatment (NMT treatment) of JIS standard A5052 aluminum alloy (hereinafter, "aluminum alloy" will be referred to as "Al alloy"): Reference example A 1.5 mm thick A5052 Al alloy plate was obtained and cut into 45 mm x 18 mm to obtain an Al alloy piece. In an immersion tank, an aqueous solution containing 10% aluminum degreaser "NA-6 (manufactured by Meltex Inc. (headquarters: Tokyo, Japan))" (hereinafter referred to as "NA-6") was heated to 60°C, and the Al alloy piece was immersed for 5 minutes, and then rinsed with tap water (rinsing with public tap water from Ota City, Gunma Prefecture, hereinafter simply referred to as "rinsing"). Next, in another immersion tank, a 1% concentration hydrochloric acid aqueous solution at 40°C was prepared, and the Al alloy piece was immersed in this for 1 minute, and then rinsed with water.
[0073] Next, in another immersion tank, a 1.5% concentration caustic soda solution at 40°C was prepared, and the Al alloy pieces were immersed in this for 4 minutes, and then washed with water. Next, in another immersion tank, a 3% concentration nitric acid solution at 40°C was prepared, and the Al alloy pieces were immersed in this for 3 minutes, and then washed with water. Next, in another immersion tank, a 3.5% concentration hydrazine hydrate solution at 60°C was prepared, and the Al alloy pieces were immersed in this for 1 minute, and then in another immersion tank, a 0.5% concentration hydrazine hydrate solution at 33°C was immersed for 0.5 minutes, and then washed with water. Next, the Al alloy pieces that had been subjected to the above treatment were placed in a hot air dryer set at 67°C for 15 minutes to dry, and then wrapped in clean aluminum foil and stored.
[0074] [Experimental Example A1-2] Surface treatment of A5052 Al alloy (NMT7 treatment) A 1.5 mm thick A5052 Al alloy plate was obtained and cut into 45 mm x 18 mm to prepare an Al alloy piece. In an immersion tank, an aqueous solution containing 10% aluminum degreaser "NA-6" was heated to 60°C, and the Al alloy piece was immersed for 5 minutes, and then rinsed with water. Next, in another immersion tank, a 10% aqueous caustic soda solution was prepared at 40°C, and the Al alloy piece was immersed in this for 1 minute, and then rinsed with water. Next, in another immersion tank, an aqueous solution containing 1% aluminum chloride hydrate and 5% hydrochloric acid at 40°C was prepared, and the Al alloy piece was immersed in this for 6 minutes, and then rinsed with water.
[0075] Next, in another immersion tank, an aqueous solution containing 2% ammonium difluoride and 10% sulfuric acid at 40°C was prepared, and the Al alloy pieces were immersed in this for 4 minutes, and then washed with water. Next, in another immersion tank, a 1.5% caustic soda aqueous solution at 40°C was prepared, and the Al alloy pieces were immersed in this for 1 minute, and then washed with water. Next, in another immersion tank, a 3% nitric acid aqueous solution at 40°C was prepared, and the Al alloy pieces were immersed in this for 1.5 minutes, and then washed with water. Next, in another immersion tank, a 3.5% hydrazine hydrate aqueous solution at 60°C was prepared, and the Al alloy pieces were immersed in this for 1 minute, and then in another immersion tank, a 0.5% hydrazine hydrate aqueous solution at 33°C was immersed for 6 minutes, and then washed with water. Next, the Al alloy pieces that had been subjected to the above chemical conversion treatment were placed in a hot air dryer set to a temperature of 67°C for 15 minutes to dry, and then wrapped in clean aluminum foil and stored.
[0076] The surface of the Al alloy piece obtained by the chemical conversion treatment, the NMT7 treatment, was observed with an electron microscope. The electron microscope photograph at 1,000 times magnification is shown in Figure 6 (a), the electron microscope photograph at 10,000 times magnification is shown in Figure 6 (b), and the electron microscope photograph at 100,000 times magnification is shown in Figure 6 (c). The electron microscope photograph at 1,000 times magnification revealed that the small mountains were connected in a mountain range, and that the mountain range and the plain parts were observed to have a large uneven surface with a period of several tens of μm. In fact, when the appearance of the Al alloy piece chemically treated with the NMT7 treatment was visually observed, a matte surface, which is generally called a matte finish, was observed, and this matte surface was caused by the presence of the rough surface chemically treated with the NMT7 treatment. The electron microscope photograph at 10,000 times magnification showed the presence of a fine uneven surface with a period of several μm, which was a depression as if the grain boundary of the metal crystal had been eroded. What was revealed in the 100,000-times magnification electron microscope photograph was an ultra-fine uneven surface with a period of 30 to 100 nm. Ultimately, the surface after NMT7 treatment had a triple uneven surface shape overall.
[0077] [Experimental Example A1-3] Surface treatment of A5052 Al alloy (NMT8 treatment) A 1.5 mm thick A5052 Al alloy plate was obtained and cut into 45 mm x 18 mm to obtain an Al alloy piece. After that, the same chemical conversion treatment as in the above-mentioned Experimental Example A1-1 was performed, and the following treatment process was added at the end. That is, the piece was immersed in a 0.5% concentration hydrazine hydrate aqueous solution at 33°C for 6 minutes, and then washed with water. Furthermore, the NMT8 treatment was performed by adding the following chemical conversion treatment. That is, the piece was immersed in a 1.5% concentration hydrogen peroxide solution in another immersion tank for 1 minute, and then thoroughly washed with water. Next, a 0.2% concentration triethanolamine aqueous solution at 40°C was prepared in another immersion tank, and the Al alloy piece after the above treatment was immersed in this for 4 minutes, and then thoroughly washed with water. Next, the Al alloy piece after the above chemical conversion treatment was dried in a hot air dryer set at 67°C for 15 minutes, and then wrapped in clean aluminum foil and stored.
[0078] [Experimental Example A2] Surface treatment of A6061Al alloy (NMT8 treatment) A 1.5 mm thick A6061 Al alloy plate of a different material from that of the above-mentioned experimental example A1-3 was obtained and cut into 45 mm x 18 mm to obtain an Al alloy piece. An aqueous solution containing 10% aluminum degreaser "NA-6" at 60°C was prepared in an immersion tank, and the Al alloy piece was immersed for 5 minutes and then rinsed with water. Next, a 10% caustic soda aqueous solution at 40°C was prepared in another immersion tank, and the Al alloy piece was immersed for 1 minute and then rinsed with water. Next, a 1% aqueous solution containing hydrated aluminum chloride and 5% hydrochloric acid at 40°C was prepared in another immersion tank, and the Al alloy piece was immersed for 1 minute and then rinsed with water. Next, a 2% aqueous solution containing ammonium difluoride and 10% sulfuric acid at 40°C was prepared in another immersion tank, and the Al alloy piece was immersed for 1 minute and then rinsed with water.
[0079] Next, in another immersion tank, a 1.5% concentration caustic soda solution at 40°C was prepared, and the Al alloy pieces were immersed in this for 2 minutes, and then washed with water. Next, in another immersion tank, a 3% concentration nitric acid solution at 40°C was prepared, and the Al alloy pieces were immersed in this for 1.5 minutes, and then washed with water. Next, in another immersion tank, a 3.5% concentration hydrazine hydrate solution at 60°C was prepared, and the Al alloy pieces were immersed in this for 1 minute, and then in another immersion tank, a 0.5% concentration hydrazine hydrate solution at 33°C was immersed for 4.5 minutes, and then washed with water. Next, a 1.5% concentration hydrogen peroxide solution was prepared, and the Al alloy pieces were immersed in this for 1 minute, and then washed with water. Next, in another immersion tank, a 0.2% concentration triethanolamine solution at 40°C was prepared, and the Al alloy pieces were immersed in this for 5 minutes, and then washed with water. Next, the Al alloy pieces that had been subjected to the above treatment were placed in a hot air dryer set at 67° C. for 15 minutes to dry, and then wrapped together in clean aluminum foil and stored.
[0080] [Experimental Example A3] Surface treatment of A2017Al alloy (NMT8 treatment) A 1.5 mm thick A2017 Al alloy plate of a different material from the above Experimental Example A2 and the above Experimental Example A1-3 was obtained and cut into 45 mm x 18 mm to obtain an Al alloy piece. In an immersion tank, an aqueous solution containing 10% aluminum degreaser "NA-6" was heated to 60°C, and the Al alloy piece was immersed for 5 minutes, and then washed with water. Next, in another immersion tank, a 10% caustic soda aqueous solution at 40°C was prepared, and the Al alloy piece was immersed for 1 minute, and then washed with water. Next, in another immersion tank, an aqueous solution containing 1% hydrated aluminum chloride and 5% hydrochloric acid at 40°C was prepared, and the Al alloy piece was immersed for 1 minute, and then washed with water. Next, in another immersion tank, an aqueous solution containing 2% ammonium difluoride and 10% sulfuric acid at 40°C was prepared, and the Al alloy piece was immersed for 4 minutes, and then washed with water.
[0081] Next, in another immersion tank, a 1.5% concentration caustic soda solution at 40°C was prepared, and the Al alloy pieces were immersed in this for 2 minutes, and then washed with water. Next, in another immersion tank, a 3% concentration nitric acid solution at 40°C was prepared, and the Al alloy pieces were immersed in this for 2.5 minutes, and then washed with water. Next, in another immersion tank, a 3.5% concentration hydrazine hydrate solution at 60°C was prepared, and the Al alloy pieces were immersed in this for 1 minute, and then in another immersion tank, a 0.5% concentration hydrazine hydrate solution at 33°C was immersed for 3 minutes, and then washed with water. Then, after immersing in a 1.5% concentration hydrogen peroxide solution for 1 minute, it was washed with water. Next, in another immersion tank, a 0.2% concentration triethanolamine solution at 40°C was prepared, and the Al alloy pieces were immersed in this for 4 minutes, and then washed with water. Next, the Al alloy pieces that had been subjected to the above chemical conversion treatment were placed in a hot air dryer set at 67° C. for 15 minutes to dry, and then the pieces were wrapped together in clean aluminum foil and stored.
[0082] [Experimental Example A4] Surface treatment of A2024Al alloy (NMT8 treatment) Similarly, a 1.5 mm thick A2024 Al alloy plate of a different material from the above experimental example was obtained and cut to 45 mm x 18 mm to obtain an Al alloy piece. In an immersion tank, an aqueous solution containing 10% aluminum degreaser "NA-6" was heated to 60°C, and the Al alloy piece was immersed for 5 minutes, and then rinsed with water. Next, in another immersion tank, a 10% caustic soda aqueous solution at 40°C was prepared, and the Al alloy piece was immersed for 1 minute, and then rinsed with water. Next, in another immersion tank, an aqueous solution containing 1% hydrated aluminum chloride and 5% hydrochloric acid at 40°C was prepared, and the Al alloy piece was immersed for 1 minute, and then rinsed with water. Next, in another immersion tank, an aqueous solution containing 2% ammonium difluoride and 10% sulfuric acid at 40°C was prepared, and the Al alloy piece was immersed for 3 minutes, and then rinsed with water.
[0083] Next, in another immersion tank, a 1.5% concentration caustic soda solution at 40°C was prepared, and the Al alloy pieces were immersed in this for 2 minutes, and then washed with water. Next, in another immersion tank, a 3% concentration nitric acid solution at 40°C was prepared, and the Al alloy pieces were immersed in this for 2.5 minutes and washed with water. Next, in another immersion tank, a 3.5% concentration hydrazine hydrate solution at 60°C was prepared, and the Al alloy pieces were immersed in this for 1 minute, and then in another immersion tank, a 0.5% concentration hydrazine hydrate solution at 33°C was prepared, and then washed with water. Then, after immersing in a 1.5% concentration hydrogen peroxide solution for 1 minute, it was washed with water. Next, in another immersion tank, a 0.2% concentration triethanolamine solution at 40°C was prepared, and the Al alloy pieces were immersed in this for 4 minutes, and then thoroughly washed with water. Next, the Al alloy pieces that had undergone the above treatment were placed in a hot air dryer set at 67° C. for 15 minutes to dry, and then wrapped together in clean aluminum foil and stored.
[0084] [Experimental Example A5] Surface treatment of A7075Al alloy (NMT8 treatment) A 1.5 mm thick A7075Al alloy plate was obtained and cut into 45 mm x 18 mm to obtain an Al alloy piece. In an immersion tank, an aqueous solution containing 10% aluminum degreaser "NA-6" was heated to 60°C, and the Al alloy piece was immersed for 5 minutes, and then rinsed with water. Next, in another immersion tank, a 10% aqueous caustic soda solution was prepared at 40°C, and the Al alloy piece was immersed for 1 minute, and then rinsed with water. Next, in another immersion tank, an aqueous solution containing 1% hydrated aluminum chloride and 5% hydrochloric acid at 40°C was prepared, and the Al alloy piece was immersed for 2 minutes, and then rinsed with water. Next, in another immersion tank, an aqueous solution containing 2% ammonium difluoride and 10% sulfuric acid at 40°C was prepared, and the Al alloy piece was immersed for 1 minute, and then rinsed with water.
[0085] Next, in another immersion tank, a 1.5% concentration caustic soda solution at 40°C was prepared, and the Al alloy pieces were immersed in this for 2 minutes, and then washed with water. Next, in another immersion tank, a 3% concentration nitric acid solution at 40°C was prepared, and the Al alloy pieces were immersed in this for 1 minute, and then washed with water. Next, in another immersion tank, a 3.5% concentration hydrazine hydrate solution at 60°C was prepared, and the Al alloy pieces were immersed in this for 1 minute, and then in another immersion tank, a 0.5% concentration hydrazine hydrate solution at 33°C was immersed for 2.5 minutes, and then washed with water. Furthermore, in another immersion tank, the pieces were immersed in a 1.5% concentration hydrogen peroxide solution for 1 minute, and then washed with water. Next, in another immersion tank, a 0.2% concentration triethanolamine solution at 40°C was prepared, and the Al alloy pieces were immersed in this for 10 minutes, and then washed with water. Next, the Al alloy pieces that had been subjected to the above chemical conversion treatment were placed in a hot air dryer set at 67° C. for 15 minutes to dry, and then the pieces were wrapped together in clean aluminum foil and stored.
[0086] [Experimental Example A6] Surface treatment of ADC12Al alloy (NMT5' treatment) A cast ADC12Al alloy piece was obtained and used as a plate-shaped piece of Al alloy piece of 45mm x 18mm x 1.5mm. In an immersion tank, an aqueous solution containing 10% aluminum degreaser "NA-6" was set at 60°C, and the Al alloy piece was immersed for 5 minutes, and then rinsed with water. Next, a 10% aqueous caustic soda solution at 40°C was prepared for another immersion, and the Al alloy piece was immersed for 1 minute, and then rinsed with water. Next, an aqueous solution containing 1% hydrated aluminum chloride and 5% hydrochloric acid at 40°C was prepared for another immersion tank, and the Al alloy piece was immersed for 2 minutes, and then rinsed with water. Next, an aqueous solution containing 2% ammonium difluoride and 10% sulfuric acid at 40°C was prepared for another immersion tank, and the Al alloy piece was immersed for 0.5 minutes, and then rinsed with water. Next, in another immersion tank, a 1.5% caustic soda solution at 40°C was prepared, and the Al alloy pieces were immersed in this for 4 minutes, and then washed with water. Next, in another immersion tank, a 3% nitric acid solution at 40°C was prepared, and the Al alloy pieces were immersed in this for 3 minutes.
[0087] Next, the pieces were placed in a water washing tank equipped with an ultrasonic oscillation terminal for 5 minutes to separate the smut on the surface of the Al alloy pieces, and then in another immersion tank, a 3% concentration nitric acid aqueous solution at 40°C was prepared, the Al alloy pieces were immersed in this for 0.5 minutes, and then washed with water. Next, in another immersion tank, a 3.5% concentration hydrazine hydrate aqueous solution at 60°C was prepared and the pieces were immersed in this for 2 minutes, and then in another immersion tank, a 0.5% concentration hydrazine hydrate aqueous solution at 33°C was prepared and then washed with water. Then, the pieces were immersed in a 1.5% concentration hydrogen peroxide solution for 1 minute, and then washed with water. Then, the pieces were dried in a hot air dryer set at 67°C for 15 minutes, and further heat-treated in a hot air dryer set at 100°C for 15 minutes, and then placed in a water washing tank equipped with an ultrasonic oscillation terminal for 7 minutes to separate the smut. The mixture was then dried in a hot air dryer set at 67° C. for 15 minutes, wrapped in clean aluminum foil, and stored.
[0088] [Experimental Example B] Measurement of injection joining force [Experimental Example B1] Measurement of shear joint strength in various injection-molded joints For the measurement of shear bond strength, various Al alloy pieces having a size of 45 mm x 18 mm x 1.5 mm, which had been subjected to the chemical conversion treatment described in the above-mentioned Experimental Examples A1 to A6, were bonded by injection with a polyamide resin composition to form a composite (test piece shown in FIG. 1). The test piece molded using the above-mentioned "CM3506G50" as the polyamide resin composition was used as the injection bonded product (composite in the present invention) of this experimental example. The injection bonding conditions were a mold temperature of 140°C and an injection temperature of 280°C. What was noted in this experiment was that the pressure retention time was extended from that of normal molding, and the time from injection to release was 30 seconds. The test piece, which was the release product, was placed in a hot air dryer set at a temperature of 150°C within a few hours, heated for 1 hour, and then allowed to cool. The shear bond strength was measured the next day with a tensile tester, and the results are shown in Table 1. As can be seen from the shear bonding strength shown in Table 1, the adhesive strength of all the metal pieces was 50 MPa or more, except for Experimental Example A1-1 (Reference Example), and the bonding strength was strong.
[0089] [Experimental Example B2] Measurement of shear joint viscosity values for various injection-molded joints Using various Al alloy pieces that had been subjected to the same chemical conversion treatment as in the above-mentioned Experimental Examples A1-2 to A6, and using the above-mentioned polyamide resin "CM3506G50", test pieces having the shape shown in Figure 1 were injection-joined. The shear joint strength and the shear joint tackiness values are shown in Table 1. [Table 1]
[0090] The values in Table 1 are expressed in kg (gravity unit) for the tensile tester. The bonded area of the test piece shown in Figure 1 is 0.5 cm2, 10 mm x 5 mm. 2 Therefore, kg / 0.5cm 2 This tensile tester applies a continuous repeated load 300 times, and the strength is gradually increased by about 2 MPa, but in reality it is 10 kg / 0.5 cm. 2 (1.96MPa). Therefore, the shear joint ductility value was also 10kg / 0.5cm. 2The shear joint toughness is approximately 220 kg / 0.5 cm for six types of Al alloys. 2 With the exception of the reference example (A1-1), the strength was surprisingly high, at approximately 80% of the shear joint strength.
[0091] [Experimental Example C] Temperature shock 3000 cycle test The above-mentioned NMT8-treated Al alloy was injection-bonded with the polyamide resin composition "CM3506G50," and generally showed high injection bonding strength. Therefore, in Table 1, the shear bonding viscosity value was 210 kg / 0.5 cm 2 An injection-bonded product (test piece shown in Figure 1) was created again from the above, and after applying oil (commercially available engine oil "30W10" (SAE standard)), it was subjected to a temperature shock test of 3,000 cycles at -50℃ / +150℃. The results are shown in Table 2. However, for this test, the operation of the temperature shock cycle test machine was temporarily stopped at the factory and research center, which were closed on Fridays in April and May 2020, on Saturdays and Sundays every week, during the summer vacation, the New Year's holiday statutory in Japan, the May consecutive holidays, and in addition, due to the COVID-19 pandemic.
[0092] In addition, an operation (operation) was added near the -60℃ cooling system in the test machine to prevent accidents of the mechanical operating mechanism due to the progress of ice adhesion. Therefore, this temperature shock cycle test was performed in a fully automatic operation method, including continuous operation for one cycle of 65 minutes and automatic shutdown of the cooling system to prevent ice growth. The operation was stopped for many days for this reason, and these tests took nearly a year. However, since the temperature shock cycle test machine was left in a room in a factory where the temperature is maintained at about 23℃ all year round, it is estimated that the environment of the sample box during the operation stoppage during the above-mentioned holiday period was in an environment of 10 to 20℃ and about 90% humidity. The amount of water molecules that penetrated into the Al alloy surface facing the resin part during this test machine stoppage period was judged to have had no significant effect on the test results, since the oil coating was originally applied to the outer periphery of the metal-resin joint surface. [Table 2]
[0093] [Experimental Example D] High temperature and humidity test for 1000 hours In Table 1, the shear joint viscosity value is 210 kg / 0.5 cm 2 The above-mentioned injection-bonded joints (test pieces shown in Figure 1) using the NMT7 and 8 treated products were prepared again, and oil (commercially available engine oil "10W30" (SAE standard)) was applied to them, and they were subjected to a durability test in which they were placed in a high-temperature, high-humidity tester at 85°C and 85% humidity for 1,000 hours. The results are shown in Table 3. In Table 3, two pairs of test pieces were taken out of the high-temperature, high-humidity tester, and after drying at a temperature of 80°C for 24 hours, one pair was broken in a tensile test to measure the shear bond strength, and the remaining pair was further dried at a temperature of 150°C for only 4 hours to expel water molecules that were dispersed in the resin and settled (contained) in the polyamide resin. The shear bond strength was then measured. From the experimental results, it was determined that the shear bond strength was 80-88% of the shear bond strength before the test, and that the bond strength was sufficiently maintained even when exposed to high temperature and high humidity. [Table 3] [Industrial Applicability]
[0094] The integrated composite of metal and resin of the present invention is suitable for use as parts and members of moving machines such as automobiles and aircraft that are exposed to heat and high humidity, such as driving machines such as engines and motors, light emitters, various batteries, electric machines, etc. In short, the present invention can be used for machines, equipment, etc. for various purposes that are exposed to harsh natural environments, and can also be used for those used outdoors. [Explanation of symbols]
[0095] 1, 10, 20, 30, 40...Metal and resin integrated composite (composite) 2...Angle iron 4...Polyamide resin composition 5…Reinforced wall 6...Through hole 12...Metal rectangular plate 13...Resin molded body 14…Cylindrical part 15…Rib 16…Center pedestal 17...Outer pedestal 31, 35...Plate member 33…Gate 34…Heat conductor
Claims
1. An integrated composite of metal and resin, comprising an aluminum alloy piece having a surface to be joined that has been chemically treated, and a polyamide-based resin composition directly bonded to the surface to be joined by injection bonding, The bonding surface is one in which an uneven surface with a period of several tens of μm is clearly observed when observed at a magnification of 1,000 with an electron microscope, a fine uneven surface with a period of 0.8 to 5 μm is observed when observed at a magnification of 10,000, and an ultrafine uneven surface with a period of 30 to 100 nm is observed when observed at a magnification of 100,000, The polyamide-based resin composition contains 10% or more of a semi-aromatic polyamide component as a minor component in the resin content, with the remainder being mainly an aliphatic polyamide component, and contains 25 to 35% by weight of short glass fibers as a whole, The bonding surface has a shear bonding strength of 45 MPa or more, a maximum shear external force value that does not break even when a shear external force of 75% or more of the shear bonding strength is continuously applied 300 times, and a shear bonding viscosity value of 38 MPa or more. An integrated composite of metal and resin.
2. The integrated composite of metal and resin according to claim 1, The integrated composite of metal and resin is a test piece specified in the international standard (ISO19095), and a durability test is performed in which the entire test piece is coated with paint or oil and the test piece is exposed to an environment set at a temperature of 85°C and a humidity of 85% for 1,000 hours. In the measurement of the shear bonding strength of the bonding surface, the integrated composite of metal and resin has a moist heat resistance that is 75% or more of the value before the test, and is observed to have a temperature shock resistance that can withstand a temperature shock test of 3,000 cycles at -50°C / +150°C. An integrated composite of metal and resin.
3. The integrated composite of metal and resin according to claim 1 or 2, The aluminum alloy piece is a long member (2) having an L-shaped, U-shaped, or semicircular cross section, which is a long plate material, and the aluminum alloy piece and the polyamide-based resin composition are integrally joined by a structure (5) in which the polyamide-based resin composition fills a groove-like recess (3) in the long member (2) to increase the mechanical strength of the groove-like recess (3). An integrated composite of metal and resin.
4. The integrated composite of metal and resin according to claim 3, A through hole penetrating the aluminum alloy piece is formed in the groove-like recess (3) of the metal, and the through hole is filled with the polyamide-based resin composition. An integrated composite of metal and resin.
5. The integrated composite of metal and resin according to claim 1 or 2, The integrated composite of metal and resin is A resin molding central portion (14, 15) which is the polyamide-based resin composition forming the central portion of the joining surface; a resin intermediate portion (16) surrounding the resin central portion of the resin molding and having a thickness thinner than that of the resin central portion; and a thin-walled resin portion (17) having a width of 5 mm or more, which substantially surrounds the entire periphery of the resin molding central portion (14, 15) and the resin intermediate portion (16); The thin resin portion (17) has a thickness of 0.5 to 1.5 mm, and the intermediate resin portion (16) has a thickness of 1.0 to 3.0 mm. An integrated composite of metal and resin.
6. The integrated composite of metal and resin according to claim 1 or 2, In the integrated composite (30, 40) of metal and resin, the aluminum alloy pieces are two plate materials (31, 35), and the polyamide-based resin composition (32) is sandwiched between the two plate materials (31, 35) and bonded together, and the thickness of the polyamide-based resin composition is 1.0 to 2.0 mm. An integrated composite of metal and resin.
7. The integrated composite of metal and resin according to claim 6, Between the two plates (31, 35), one or more rods (34) made of an aluminum alloy for heat conduction are connected so as to reduce the temperature difference between the two plates (31, 35). An integrated composite of metal and resin.
8. A method for producing an integrated composite of metal and resin according to any one of claims 1 to 7, comprising the steps of: The integrated composite of metal and resin is prepared by inserting the aluminum alloy pieces that have been subjected to chemical conversion treatment into an injection molding die, and then injecting the polyamide-based resin composition into the aluminum alloy pieces to integrate the aluminum alloy pieces with the polyamide-based resin composition. A method for producing an integrated composite of metal and resin.
Citation Information
Patent Citations
Composite of aluminum alloy and resin, and its manufacturing method
JP2006315398A
Complex and its manufacturing method
JP2007050630A
Composite of aluminum alloy and resin and production method thereof
JP2007182071A
Composite and method for manufacturing the same
JP2010064496A
Production method of composite of metal and frtp and the composite
JP2016060051A
Cited By
Integrated composite of metal and resin and manufacturing method of the same
JP2022187378A
Method of manufacturing composite of CFRP and metal materials and the composite
JP2023025546A
Manufacturing method of composite of CFRP and metal material and the composite