Polyamide resin foam particles

By optimizing crystallite size, heat of fusion, and closed cell ratio, the polyamide resin foam particles achieve enhanced in-mold moldability and heat resistance, enabling the production of lightweight, heat-resistant molded articles with improved surface properties and fusion characteristics.

JP7579059B2Active Publication Date: 2024-11-07JSP CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020025271
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-02-18
Publication Date
2024-11-07
Estimated Expiration
2040-02-18

AI Technical Summary

Technical Problem

Existing polyamide resin expanded particles exhibit limited in-mold moldability, particularly in thick or complex shapes, due to narrow moldability ranges and insufficient formability.

Method used

The polyamide resin foam particles are engineered with a crystallite size exceeding 8 nm, a total heat of fusion between 40 to 140 J/g, an apparent density of 10 to 300 kg/m³, and a closed cell ratio exceeding 90%, along with specific cell diameters and surface layer thicknesses, enhancing their in-mold moldability and heat resistance.

Benefits of technology

The engineered particles demonstrate excellent in-mold moldability, allowing for the production of lightweight, heat-resistant molded articles with improved surface properties and fusion characteristics, even in thick or complex designs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579059000001
    Figure 0007579059000001
  • Figure 0007579059000002
    Figure 0007579059000002
  • Figure 0007579059000003
    Figure 0007579059000003
Patent Text Reader

Abstract

To provide polyamide-based resin foam particles excellent in in-mold moldability.SOLUTION: Polyamide-based resin foam particles have a crystallite size measured by an X-ray diffraction method of more than 8 nm.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an expanded polyamide resin particle. [Background technology]

[0002] Polyamide resins are known as resins with high heat resistance and excellent abrasion resistance, chemical resistance, and the like. Since foamed molded products obtained by foaming this polyamide resin can be made lighter while maintaining these excellent properties, they are expected to be used in automobile parts and other applications. For this reason, various studies have been conducted on foamed molded products of polyamide resins for practical use in various applications. For example, Patent Document 1 discloses a polyamide resin foamed bead molded product that has a crystallite size of 10 nm or more and a crystallinity of 10 to 50%, which is obtained by filling a cavity of a mold with polyamide resin pre-expanded particles and subjecting the molded product to a process of heating the molded product in multiple stages using water vapor, with the aim of improving heat resistance and sound insulation. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2016 / 147582 Summary of the Invention [Problem to be solved by the invention]

[0004] Patent Document 1 discloses that a polyamide resin foamed bead molding having excellent heat resistance is provided. However, the foamed beads of Patent Document 1 have a narrow moldable range within a moldable area, and depending on the shape of the molded article, such as a thick article, the moldability within the moldable area is insufficient. An object of the present invention is to provide expanded polyamide resin beads which are excellent in moldability. [Means for solving the problem]

[0005] As a result of extensive investigations, the present inventors have found that the above-mentioned problems can be solved by adjusting the crystallite size of the expanded polyamide resin beads to a specific value.

[0006] That is, the present invention provides the following [1] to [8]. [1] Polyamide resin foam particles with a crystallite size exceeding 8 nm as measured by X-ray diffraction. [2] The expanded polyamide resin particles according to the above item [1], wherein the total heat of fusion in the DSC curve measured based on the heat flux differential scanning calorimetry method of JIS K7122-1987 by using the expanded polyamide resin particles as a test piece and heating the test piece from 30°C to a temperature 30°C higher than the end of the melting peak at a heating rate of 10°C / min is 40 to 140 J / g. [3] The apparent density of the polyamide resin foam particles is 10 to 300 kg / m 3 The expanded polyamide resin particles according to the above [1] or [2], [4] The expanded polyamide resin particles according to any one of the above [1] to [3], wherein the apex temperature of the melting peak in the DSC curve of the second heating obtained under the following condition 1 is 185 to 285°C. Condition 1 Based on the heat flux differential scanning calorimetry method of JIS K7121-1987, a polyamide resin foamed particle is used as a test piece, and is heated at a heating rate of 10°C / min from 30°C to a temperature 30°C higher than the end of the melting peak, and then maintained at that temperature for 10 minutes. The test piece is then cooled to 30°C at a cooling rate of 10°C / min, and is then heated again at a heating rate of 10°C / min to a temperature 30°C higher than the end of the melting peak. The DSC curve measured during this process is the DSC curve for the second heating. [5] The expanded polyamide resin particles according to any one of the above [1] to [4], wherein the expanded polyamide resin particles have a crystallite size of 10 nm or more as measured by X-ray diffraction. [6] The expanded polyamide resin particles according to any one of the above [1] to [5], wherein the expanded polyamide resin particles have a closed cell rate of more than 90%. [7] The expanded polyamide resin particles according to any one of the above [1] to [6], wherein the expanded polyamide resin particles have an average cell diameter of 20 to 200 μm. [8] The expanded polyamide resin particles according to any one of the above [1] to [7], wherein the expanded polyamide resin particles have a surface layer thickness of 5 to 50 μm. Effect of the Invention

[0007] According to the present invention, it is possible to provide expanded polyamide resin beads having excellent moldability in a mold. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The present invention relates to expanded polyamide resin particles having a crystallite size of more than 8 nm as measured by X-ray diffraction.

[0009] [Polyamide resin foam particles] <Crystallite size of expanded polyamide resin particles> The expanded polyamide resin beads of the present invention have a crystallite size of more than 8 nm as measured by X-ray diffraction. By having a crystallite size of more than 8 nm, the pressure range in which the beads can be molded in the mold is wide, and the beads have excellent moldability in the mold. The crystallite size measured by X-ray diffraction is more than 8 nm, and is preferably 9 nm or more, more preferably 10 nm or more, even more preferably 11 nm or more, and even more preferably 12 nm or more. There is no upper limit, but it is preferably 30 nm or less, and more preferably 20 nm or less. The reason why the expanded polyamide resin beads have excellent moldability in the mold when the crystallite size is in the above range is not clear, but it is thought that the large crystallite size improves the heat resistance of the expanded beads, and the beads can be stably molded under various conditions, such as when the desired molded product is thick, even at high temperatures during molding in the mold. The crystallite size is measured by X-ray diffraction, and specifically, it is measured by the method shown below. The X-ray diffraction (XRD) measurement of the expanded polyamide resin beads is performed by a transmission method using an X-ray scattering device. The X-ray diffraction profile obtained by the X-ray diffraction measurement is assumed to have a Gaussian function as the peak shape, and the peaks are separated into a diffraction peak derived from crystals and a diffraction peak derived from amorphous crystals. The full width at half maximum β (rad) of the peak having the narrowest peak width among the peaks obtained by the peak separation is calculated, and the crystallite size D of the expanded beads is calculated using the full width at half maximum β according to the following formula (2).

number

[0010] <Melting characteristics of polyamide resin foam particles> The expanded polyamide resin beads of the present invention preferably have the following melting characteristics. The expanded polyamide resin beads of the present invention preferably have a total heat of fusion of 40 to 140 J / g, more preferably 45 J / g or more, and even more preferably 50 J / g or more, in a DSC curve measured when the expanded polyamide resin beads are used as a test piece and heated at a heating rate of 10°C / min from 30°C to a temperature 30°C higher than the end of the melting peak, based on the heat flux differential scanning calorimetry method of JIS K7122-1987. Also, it is more preferably 120 J / g or less, and even more preferably 100 J / g or less. Since the DSC curve is obtained by first heating using the expanded polyamide resin beads as a test piece, the DSC curve is the DSC curve of the first heating. The larger the total heat of fusion of the DSC curve of the first heating, the more advanced the crystallization of the expanded beads is. The more advanced the crystallization of the expanded beads is, the more excellent the heat resistance is. If the total heat of fusion in the DSC curve in the first heating is within the above range, the expanded beads will have better heat resistance, which is preferable.

[0011] The total heat of fusion is calculated as follows. On the obtained DSC curve, a straight line is drawn connecting the point of 150°C on the DSC curve and the point showing the temperature at the end of the melting peak on the DSC curve. This straight line is the baseline, and the area surrounded by the baseline and the DSC curve on the endothermic side of the baseline corresponds to the endothermic energy of the melting peak, and the heat calculated from this is the total heat of fusion. When the DSC curve has multiple melting peaks, the total heat of fusion is the sum of all the heat amounts. The point showing the temperature at the end of the melting peak on the DSC curve refers to the temperature at the end of the melting peak of the highest temperature side. In this specification, a test piece that has been left to stand for 24 hours or more in an environment of 23°C and 50% relative humidity is used for measuring the DSC curve.

[0012] The expanded polyamide resin beads of the present invention preferably have a melting peak apex temperature of 185 to 285° C. in the DSC curve of the second heating obtained under the following condition 1. The melting peak apex temperature of the DSC curve of the second heating obtained here (hereinafter also referred to as the melting point of the expanded polyamide resin beads, and indicated by Tm1) corresponds to the melting point of the polyamide resin derived from the inherent crystal structure that the polyamide resin originally has. Condition 1 Based on the heat flux differential scanning calorimetry method of JIS K7121-1987, a polyamide resin foamed particle is used as a test piece, and is heated at a heating rate of 10°C / min from 30°C to a temperature 30°C higher than the end of the melting peak, and then maintained at that temperature for 10 minutes. The test piece is then cooled to 30°C at a cooling rate of 10°C / min, and is then heated again at a heating rate of 10°C / min to a temperature 30°C higher than the end of the melting peak. The DSC curve measured during this process is the DSC curve for the second heating.

[0013] The apex temperature of the melting peak of the DSC curve in the second heating is preferably 185 to 285° C., more preferably 188° C. or higher, and even more preferably 190° C. or higher. On the other hand, from the viewpoint of easy temperature control during foaming, the apex temperature of the melting peak of the second DSC curve is more preferably 280° C. or lower, even more preferably 260° C. or lower, still more preferably 230° C. or lower, and even more preferably 225° C. or lower. When the melting point of the expanded polyamide resin beads satisfies the above range, expanded polyamide resin beads having a low apparent density and excellent heat resistance are easily obtained, which is preferable.

[0014] <Other characteristics of polyamide resin foam beads> In addition to the above-mentioned melting properties, the expanded polyamide resin particles of the present invention preferably have the following properties. The apparent density of the expanded polyamide resin particles of the present invention is 10 to 300 kg / m 3 The apparent density of the expanded polyamide resin beads of the present invention is preferably 10 kg / m 3 More preferably, it is 30 kg / m 3 More preferably, it is 50 kg / m 3 More preferably, it is 100 kg / m or more. 3 The apparent density of the expanded polyamide resin particles is preferably 300 kg / m 3 More preferably, it is 250 kg / m or less. 3 More preferably, it is 200 kg / m or less. 3 and even more preferably 150 kg / m 3 When the apparent density of the expanded beads is within the above range, the expanded beads and the molded article made of the expanded beads are less likely to shrink, and it is easy to obtain a good expanded bead molded article. The apparent density of the expanded polyamide resin beads is measured by the following method. Prepare a measuring cylinder containing water at a temperature of 23°C. After leaving the measuring cylinder for 24 hours or more under the conditions of 50% relative humidity, 23°C, and 1 atm, the volume of the water is approximately 500 cm 3The mass W1 of the foamed beads is measured and submerged using a wire net. Taking into account the volume of the wire net, the volume V1 [cm3] of the foamed beads is read from the rise in the water level. 3 ] is measured, and the mass W1 [g] of the foamed particles is divided by the volume V1 (W1 / V1), and the unit is [kg / m 3 ], the apparent density of the expanded beads can be calculated.

[0015] The closed cell ratio of the expanded polyamide resin beads of the present invention is preferably 85% or more, more preferably 88% or more, and even more preferably more than 90%. When the closed cell ratio of the expanded beads satisfies the above range, expanded beads with low apparent density are easily obtained. In addition, the moldability of the expanded beads is good, and the expanded bead molding produced by molding the expanded beads in a mold has excellent surface properties and fusion properties. In this way, by using expanded beads with a large crystallite size and a closed cell ratio in the above range, a molding that is excellent in moldability and lightweight can be obtained. The closed cell ratio is the ratio of the volume of the closed cells to the volume of all the cells in the expanded beads, and can be determined using an air comparison type specific gravity meter based on ASTM-D2856-70.

[0016] The average cell diameter of the expanded polyamide resin beads of the present invention is preferably 20 μm or more, more preferably 30 μm or more, and even more preferably 50 μm or more. On the other hand, the average cell diameter of the expanded polyamide resin beads is preferably 200 μm or less, more preferably 150 μm or less, and even more preferably 140 μm or less. The average cell diameter of the expanded polyamide resin beads is measured by the following method. First, the expanded bead is divided into two parts along the center of the expanded bead, and the cut surface is photographed with a scanning electron microscope. Next, in the obtained cross-sectional photograph, lines are drawn at equal intervals in eight directions from the center of the expanded bead cut surface to the outermost surface of the expanded bead at 45° increments, and the number of bubbles that intersect with the lines is counted. The total length of the lines is divided by the number of bubbles counted, and the resulting value is the bubble diameter of the expanded beads. This operation is performed in the same manner for 10 or more expanded beads, and the arithmetic average value of the bubble diameters of each expanded bead is the average bubble diameter of the expanded beads.

[0017] The surface layer thickness of the polyamide resin expanded beads of the present invention is preferably 5 μm or more, more preferably 10 μm or more. On the other hand, the surface layer thickness of the polyamide resin expanded beads is more preferably 50 μm or less, and even more preferably 30 μm or less. When the surface layer thickness of the polyamide resin expanded beads is within the above range, internal pressure is applied to the bubbles when the expanded beads are pressurized, and the expanded beads can be made to have excellent surface properties in in-mold molding. In addition, the expanded beads are less likely to break when molded in a mold, and a molded product of expanded beads with a high ratio is easily obtained. Furthermore, the fusion between the expanded beads is excellent during molding in a mold, and molding can be performed without excessively increasing the molding steam pressure. In the present invention, since the crystallite size of the expanded beads is particularly large, expanded beads having excellent heat resistance and excellent moldability in a mold can be provided, and a molded product having light weight and excellent heat resistance can be obtained.

[0018] The surface layer thickness of the expanded polyamide resin beads can be measured as follows: For eight straight lines extending from near the center of the cut surface of the expanded beads obtained using the average bubble diameter of the expanded beads to the outermost surface of the expanded beads, the lengths (surface layer thickness) from the outermost surface of the expanded beads to the bubbles located at the outermost positions are measured, and the average surface layer thickness of the expanded beads is calculated by arithmetically averaging these values.

[0019] The expanded polyamide resin particles of the present invention preferably have a ratio [(Tm1-20°C compressive stress) / (23°C compressive stress)] of 5% compressive stress at 23°C (23°C compressive stress) at a temperature (Tm1-20°C) 20°C lower than the melting point (Tm1) of the expanded polyamide resin particles to 5% compressive stress at 23°C (23°C compressive stress) of 0.1 or more. The ratio [(Tm1-20°C compressive stress) / (23°C compressive stress)] is more preferably 0.15 or more, and even more preferably 0.2 or more. The upper limit is about 1. Expanded beads having a high ratio [(Tm1-20°C compressive stress) / (23°C compressive stress)] have a small decrease in compressive stress at high temperatures compared to the compressive stress at room temperature, and maintain a high compressive stress even at high temperatures, which means that they have excellent heat resistance. Expanded polyamide resin beads having a high value of the ratio [(Tm1-20°C compressive stress) / (23°C compressive stress)] can be suitably used for applications such as a filling material for composite molding. The reason for setting the temperature (Tm1-20°C) 20°C lower than the melting point of the expanded polyamide resin beads is to evaluate the compression properties at a temperature at which the crystals of the expanded beads do not melt.

[0020] The 5% compression stress at a temperature (Tm1-20°C) 20°C lower than the melting point of the polyamide resin foamed beads can be obtained by measuring the foamed beads in compression mode using a thermal analyzer (TMA; for example, "TMA7100" manufactured by Hitachi High-Tech Science Co., Ltd.). Specifically, one foamed bead is randomly selected, and the foamed bead is clamped in the short diameter direction with a compression probe under a load of 10 mN, and then heated to a temperature (Tm1-20°C) 20°C lower than the melting point of the polyamide resin foamed beads. Thereafter, the foamed bead is pressed at a speed of 1 mm / min while maintaining an isothermal temperature at a temperature (Tm1-20°C) 20°C lower than the melting point of the polyamide resin foamed beads, and the load of the probe is monitored. The stress at the point when the thickness of the foamed bead becomes 5% of the thickness of the foamed bead before compression is defined as the 5% compression stress of the foamed bead at Tm1-20°C. The 5% compression stress at 23°C can be determined by measuring the expanded beads in a compression mode using a thermal analyzer (TMA; for example, "TMA7100" manufactured by Hitachi High-Tech Science Corporation). Specifically, one expanded bead is randomly selected, and the expanded bead is clamped in the minor axis direction with a compression probe under a load of 10 mN, and then pressed at a speed of 1 mm / min at 23°C while monitoring the load of the probe. The stress at the point when the thickness of the expanded bead becomes 5% of the thickness of the expanded bead before compression is defined as the 5% compression stress at 23°C.

[0021] <Method of manufacturing polyamide resin foam beads> The expanded polyamide resin beads of the present invention may be produced by any method as long as the crystallite size measured by X-ray diffraction exceeds 8 nm. However, the following method is preferred.

[0022] The expanded polyamide resin beads of the present invention are preferably expanded beads produced by a process including a step of heating the resin beads in a state containing more moisture than the amount of water absorbed under normal conditions to increase the crystallite size.Specific examples of the expanded polyamide resin beads include a method of heating the resin beads in a state containing moisture to form resin particles with grown crystallites, impregnating the resin particles with a blowing agent and foaming to form expanded beads with grown crystallites, a method of impregnating the resin particles containing moisture with a blowing agent and heating to foam to form expanded beads with grown crystallites, and a method of impregnating the expanded beads with water and heating to form expanded beads with grown crystallites. Among the above, from the viewpoint of facilitating the enlargement of the crystallite size, the expanded polyamide resin beads of the present invention are preferably obtained by adding a blowing agent to polyamide resin beads containing water and expanding them by heating. Methods for incorporating moisture into polyamide-based resin particles or expanded polyamide-based resin particles include a method of immersing the resin particles or expanded particles in water, a method of leaving the resin particles or expanded particles in a high humidity atmosphere such as a relative humidity of 90% or more, a method of spraying water onto the resin particles or expanded particles with a spray, etc. Among the above, the method of incorporating moisture by immersion in water is preferred because it is easy to incorporate moisture into the particles. When the polyamide resin particles or expanded polyamide resin particles are heated in water, they are filled with water and can be considered to satisfy the above moisture content. The moisture content in the resin particles or expanded particles can be determined by a Karl Fischer moisture meter, and specifically, can be determined by the following method. After wiping off the water on the surface of the polyamide-based resin particles or expanded polyamide-based resin particles with a dry cloth, the polyamide-based resin particles or expanded polyamide-based resin particles are weighed, and then the polyamide-based resin particles or expanded polyamide-based resin particles are heated using a heating moisture vaporizer to vaporize the internal moisture, and the moisture content is measured by Karl Fischer titration (coulometric titration method) using a Karl Fischer moisture meter. The polyamide-based resin particles containing water or the moisture content of the polyamide-based resin particles is preferably 3% or more, more preferably 5% or more, and further preferably 7% or more.

[0023] Methods for heating polyamide-based resin particles or expanded polyamide-based resin particles include a method of immersing the resin particles or expanded particles in a medium such as water and heating the medium to heat the resin particles or expanded particles, a method of heating the resin particles or expanded particles by blowing hot air into the particles, etc. Among the above, the method of heating in a medium such as water is preferred because it allows uniform heating. The heating temperature when heating the polyamide-based resin particles or the expanded polyamide-based resin particles is preferably at least 90° C. lower than the melting point (Tm) of the polyamide-based resin (Tm-90° C.), more preferably at least Tm-80° C., and even more preferably at least Tm-70° C. On the other hand, the heating temperature is preferably at most 20° C. higher than the melting point (Tm) of the polyamide-based resin (Tm+20° C.), more preferably at most Tm+10° C., and even more preferably at most the melting point of the polyamide-based resin.

[0024] (Polyamide resin particles) The polyamide-based resin particles used in the production of the expanded polyamide-based resin particles contain a polyamide-based resin. The polyamide-based resin may be one type alone or a mixture of two or more types of the polyamide-based resin. The polyamide resin particles may contain other thermoplastic resins and thermoplastic elastomers within the scope of not impairing the objects and effects of the present invention. Examples of other thermoplastic resins and thermoplastic elastomers include polyethylene resins, polypropylene resins, polystyrene resins, vinyl acetate resins, thermoplastic polyester resins, acrylic acid ester resins, methacrylic acid ester resins, ethylene-propylene rubbers, ethylene-1-butene rubbers, propylene-1-butene rubbers, ethylene-propylene-diene rubbers, isoprene rubbers, neoprene rubbers, nitrile rubbers, and other rubbers, styrene-diene block copolymers, and hydrogenated styrene-diene block copolymers. From the viewpoint of obtaining polyamide-based resin expanded particles having excellent heat resistance, abrasion resistance, and chemical resistance, the content of other thermoplastic resins in the polyamide-based resin particles is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, even more preferably 10 parts by mass or less, still more preferably 5 parts by mass or less, and still more preferably, the polyamide-based resin particles are composed only of polyamide-based resin.

[0025] In addition to the polyamide resin, various additives such as commonly used bubble regulators, antistatic agents, conductive agents, lubricants, antioxidants, ultraviolet absorbers, flame retardants, metal deactivators, colorants (pigments, dyes, etc.), crystal nucleating agents, and fillers can be appropriately blended into the polyamide resin particles as necessary. Examples of the bubble regulator include inorganic bubble regulators such as talc, sodium chloride, calcium carbonate, silica, titanium oxide, gypsum, zeolite, borax, aluminum hydroxide, alum, and carbon, and organic bubble regulators such as phosphoric acid compounds, amine compounds, and polytetrafluoroethylene (PTFE). The amount of these various additives to be added varies depending on the purpose of use of the molded product, but is preferably 25 parts by mass or less with respect to 100 parts by mass of the polymer components constituting the polyamide resin particles. More preferably, it is 15 parts by mass or less, even more preferably, it is 10 parts by mass or less, and even more preferably, it is 5 parts by mass or less.

[0026] The average mass per polyamide resin particle is appropriately set depending on the size, apparent density, etc. of the targeted polyamide resin expanded particle, but is preferably 0.5 to 15.0 mg. If it is within the above range, the apparent density can be increased. From this viewpoint, the lower limit of the mass of the polyamide resin particle is more preferably 1.0 mg, and even more preferably 1.5 mg. On the other hand, the upper limit is more preferably 10.0 mg, even more preferably 7.0 mg, and even more preferably 5.0 mg.

[0027] The method for producing polyamide-based resin particles is not particularly limited, and can be obtained by known methods.For example, polyamide-based resin particles can be obtained by feeding polyamide-based resin and, if necessary, additives such as bubble adjuster and colorant into an extruder, kneading to obtain a melt-kneaded product, extruding the melt-kneaded product in a strand shape from the small hole of the die attached to the extruder tip, cutting the extruded strand to a predetermined mass with a pelletizer, hot cutting method cutting the melt-kneaded product immediately after extruding it into a gas phase, underwater cutting method (UWC method) cutting the melt-kneaded product immediately after extruding it into water, etc.

[0028] [Polyamide resin] In the present specification, examples of the polyamide resin include polyamide and polyamide copolymers, with polyamide copolymers being preferred. Polyamides include, for example, poly(6-aminohexanoic acid), also known as poly(caprolactam) (polycaproamide, nylon 6), poly(laurolactam) (nylon 12), poly(hexamethylene adipamide) (nylon 66), poly(7-aminoheptanoic acid) (nylon 7), poly(8-aminooctanoic acid) (nylon 8), poly(9-aminononanoic acid) (nylon 9), poly(10-aminodecanoic acid) (nylon 10), poly(11-aminounsodium EDTA) (nylon 11), poly(12-aminobutanoic acid) (nylon 12), poly(1 ... Examples of the homopolymers include poly(hexamethylene sebacamide) (nylon 11), poly(hexamethylene sebacamide) (nylon 610), poly(decamethylene sebacamide) (nylon 1010), poly(hexamethylene azelamide) (nylon 69), poly(tetramethylene adipamide) (nylon 46), poly(tetramethylene sebacamide) (nylon 410), poly(pentamethylene adipamide) (nylon 56), and poly(pentamethylene sebacamide) (nylon 510). The polyamide copolymer means a homopolymer having two or more kinds of repeating units, and at least a part of each repeating unit has an amide bond. Examples of polyamide copolymers include caprolactam / hexamethylenediaminoadipic acid (nylon 6 / 66), caprolactam / hexamethylenediaminoadipic acid / lauryl lactam (nylon 6 / 66 / 12), and caprolactam / lauryl lactam copolymer (nylon 6 / 12). The polyamide resin may be one of these polyamides and polyamide copolymers, or a combination of two or more of them. From the viewpoint of easily obtaining polyamide resin foam particles having high water absorption and large crystallite size, among the above polyamide resins, a polyamide resin selected from one or a combination of two or more of nylon 6, nylon 66, and nylon 6 / 66 is preferable, and nylon 6 / 66 is more preferable.

[0029] The polyamide copolymer may be a block copolymer in which a certain amount of amides of the same repeating unit are followed by a certain amount of amides of different types, or a random copolymer in which different types of amides are randomly repeated, but is preferably a random copolymer. If the polyamide copolymer is a random copolymer, it becomes possible to mold the expanded polyamide resin beads in a mold at a relatively low molding steam pressure.

[0030] The melting point (Tm) of the polyamide resin is preferably 180°C or higher, more preferably 185°C or higher, even more preferably 188°C or higher, and even more preferably 190°C or higher. On the other hand, the melting point (Tm) of the polyamide resin is preferably 280°C or lower, more preferably 260°C or lower, even more preferably 230°C or lower, and even more preferably 225°C or lower. If the polyamide resin satisfies the above melting point range, it is preferable because it is easy to obtain polyamide resin expanded particles having a low apparent density and is easy to obtain polyamide resin expanded particles having excellent heat resistance. In addition, the melting point of the polyamide resin refers to the melting point of the polyamide resin when one type of polyamide resin is used alone. When the polyamide resin is a mixture of two or more types of polyamide resins, or a mixture of a polyamide resin and another thermoplastic resin, it refers to the melting point of the kneaded product kneaded in advance with an extruder or the like.

[0031] The melting point (Tm) of a polyamide resin is a value determined by using a raw material polyamide resin as a test piece, leaving it for 24 hours in an environment at a temperature of 23°C and a relative humidity of 50%, and then determining the peak apex temperature of the melting peak of a second DSC curve obtained under the same conditions as those in Condition 1 above, except that the test piece is changed to a polyamide resin. When a DSC curve has multiple melting peaks, the peak apex temperature of the melting peak with the largest area is used as the melting temperature.

[0032] The polyamide resin in this specification has a flexural modulus of preferably 1000 MPa or more, more preferably 1200 MPa or more, and even more preferably 1500 MPa or more. If the flexural modulus of the polyamide resin is within the above range, it is preferable because the polyamide resin is less likely to shrink even when exposed to room temperature after foaming due to its high flexural modulus, and it is easy to obtain expanded beads with a high expansion ratio. In addition, the high flexural modulus is preferable because it has excellent moldability in a mold. The upper limit of the flexural modulus of the polyamide resin is about 3000 MPa.

[0033] The flexural modulus of a polyamide-based resin can be determined by measuring a test piece in accordance with JIS K7171:2016 after leaving the test piece at rest for 24 hours at a temperature of 23°C and a relative humidity of 50%.

[0034] The polyamide resin in this specification preferably has a density of 1.05 g / cm 3 More preferably, it is 1.1 g / cm 3 The density can be measured based on the method described in ISO 1183-3.

[0035] The polyamide resin used in the present invention is preferably a terminal-blocked polyamide resin in which the functional groups at the molecular chain ends are blocked, which can more reliably suppress hydrolysis during the production process of the expanded polyamide resin beads, and can more easily produce expanded polyamide resin beads that can withstand in-mold molding. Furthermore, the durability of the expanded polyamide resin bead molded article (hereinafter simply referred to as "expanded bead molded article" or "molded article") obtained by molding in a mold is improved. As the terminal blocking agent for blocking the molecular chain terminals, for example, a carbodiimide compound, an oxazoline compound, an isocyanate compound, an epoxy compound, etc. can be used. Among these, carbodiimide compounds are preferred. Specific examples include aromatic monocarbodiimides such as bis(dipropylphenyl)carbodiimide (e.g., "Stabaxol 1-LF" manufactured by Rhein Chemie), aromatic polycarbodiimides (e.g., "Stabaxol P", "Stabaxol P100", "Stabaxol P400" manufactured by Rhein Chemie), and aliphatic polycarbodiimides such as poly(4,4'-dicyclohexylmethanecarbodiimide) (e.g., "Carbodilite LA-1" manufactured by Nisshinbo Chemical Co., Ltd.). These end-capping agents may be used alone or in combination of two or more. The amount of the end blocking agent is preferably 0.1 to 5 parts by mass, and more preferably 0.3 to 3 parts by mass, based on 100 parts by mass of the polyamide resin. As described above, the polyamide-based resin used in the present invention is preferably a polyamide-based resin end-blocked with one or more end-blocking agents selected from a carbodiimide compound, an epoxy compound, an isocyanate compound, and the like, and more preferably a polyamide-based resin end-blocked with a carbodiimide compound.

[0036] The expanded polyamide resin beads of the present invention are preferably obtained by the method of heating and expanding the polyamide resin beads containing water as described above, but are preferably produced by the following methods 1 and 2.

[0037] Method 1 includes a step of dispersing polyamide-based resin particles in water in a sealed container to obtain a dispersion liquid; impregnating the polyamide-based resin particles in the dispersion with a foaming agent; maintaining the dispersion at a temperature lower than the melting point of the polyamide-based resin; and a step of setting the temperature of the dispersion just before foaming to a temperature lower than the melting point of the polyamide-based resin, and releasing the polyamide-based resin particles containing a foaming agent together with water from the sealed container to a pressure lower than the pressure inside the sealed container to foam the polyamide-based resin. Method 2 includes a step of making polyamide-based resin particles absorb moisture to obtain hydrous resin particles; impregnating the hydrous resin particles with a blowing agent in a sealed container; and heating the hydrous resin particles containing the foaming agent to foam them. Each method is explained below.

[0038] (Method of producing expanded polyamide resin beads (Method 1)) Method 1 includes a step of dispersing polyamide-based resin particles in water in a sealed container to obtain a dispersion liquid; impregnating the polyamide-based resin particles in the dispersion with a foaming agent; maintaining the dispersion at a temperature lower than the melting point of the polyamide-based resin; and expanding the polyamide-based resin particles impregnated with the blowing agent. Each step will be described below.

[0039] [Step of obtaining dispersion liquid] The step of obtaining a dispersion is a step of dispersing polyamide-based resin particles in water in a closed container to obtain a dispersion. The method for dispersing the polyamide-based resin particles in water is not particularly limited, and any known method can be used. For example, a dispersion can be obtained by adding the polyamide-based resin particles to water while stirring the water using a stirrer, and further stirring the water. In addition, it is preferable to add a dispersant such as an inorganic substance such as aluminum oxide, tricalcium phosphate, magnesium pyrophosphate, zinc oxide, kaolin, mica, talc, smectite, etc., or a dispersing aid such as an anionic surfactant such as sodium dodecylbenzenesulfonate, sodium alkanesulfonate, etc., to the dispersion liquid as needed. The mass ratio of the polyamide resin particles to the dispersing aid (resin particles / dispersing aid) is preferably 20 to 2000, more preferably 30 to 1000. In addition, the mass ratio of the dispersing agent to the dispersing aid (dispersing agent / dispersing aid) is preferably 1 to 500, more preferably 1 to 100.

[0040] [Step of impregnating foaming agent] The step of impregnating the foaming agent is a step of impregnating the polyamide resin particles in the dispersion with the foaming agent. In this step, the foaming agent can be impregnated and the polyamide resin particles can also absorb water. The method of impregnating the polyamide resin particles with the foaming agent is not particularly limited, but it is preferable to disperse the polyamide resin particles in water in a pressurizable closed container such as an autoclave and impregnate the polyamide resin particles with the foaming agent. In addition to pressurizing, it is preferable to heat the polyamide resin particles when impregnating them with the foaming agent, from the viewpoint of sufficiently impregnating the polyamide resin particles with the foaming agent in a short time.

[0041] The temperature during the impregnation under heating is preferably 50°C or higher, more preferably 80°C or higher, from the viewpoint of sufficiently impregnating the polyamide-based resin particles with the foaming agent in a short period of time, and is preferably the melting point (Tm(°C)) or lower of the polyamide-based resin particles, more preferably (Tm-20(°C)) or lower.

[0042] In addition, from the viewpoint of sufficiently impregnating the polyamide resin particles with the foaming agent in a short time, the pressure during impregnation under pressure (hereinafter also referred to as the impregnation pressure) is adjusted so that the pressure inside the sealed container is preferably 1.5 MPa (G) or more, more preferably 2.5 MPa (G) or more, and is preferably 7.0 MPa (G) or less, and more preferably 5.0 MPa (G) or less, by adding the foaming agent to the container containing the dispersion. Note that "1.5MPa(G)" means that the gauge pressure is 1.5 MPa.

[0043] From the step of dispersing the polyamide-based resin particles in water to obtain a dispersion liquid until the step of holding the dispersion liquid, the additive also plays a role of allowing the polyamide-based resin particles to absorb water. From the viewpoint of allowing the polyamide resin particles to sufficiently absorb water, the temperature increase rate is preferably 10° C. / min or less, more preferably 7° C. / min or less, whereas from the viewpoint of productivity of the expanded polyamide resin particles, the temperature increase rate is preferably 1° C. / min or more, more preferably 2° C. / min or more.

[0044] (foaming agent) A physical foaming agent can be used as the foaming agent. Examples of the physical foaming agent include organic physical foaming agents such as aliphatic hydrocarbons such as propane, butane, pentane, hexane, and heptane, alicyclic hydrocarbons such as cyclopentane and cyclohexane, halogenated hydrocarbons such as chlorofluoromethane, trifluoromethane, 1,1-difluoroethane, 1,1,1,2-tetrafluoroethane, methyl chloride, ethyl chloride, and methylene chloride, and dialkyl ethers such as dimethyl ether, diethyl ether, and methyl ethyl ether. Examples of the inorganic physical foaming agent include carbon dioxide, nitrogen, helium, argon, and air. Among the physical blowing agents, from the viewpoints of having little impact on the environment, being non-flammable and having excellent safety, inorganic physical blowing agents are preferred, carbon dioxide or nitrogen are more preferred, and carbon dioxide is even more preferred.

[0045] [Holding step] The maintaining step is a step of maintaining the dispersion at a temperature lower than the melting point of the polyamide-based resin. The maintaining step is a step of heating the polyamide-based resin particles in a water-containing state. From the viewpoint of increasing the crystallite size, the holding temperature of the dispersion in the holding step is preferably 90°C lower than the melting point (Tm) of the polyamide resin (Tm-90°C) or higher, more preferably 80°C lower than the melting point (Tm-80°C) or higher, even more preferably 70°C lower than the melting point (Tm-70°C) or higher, and even more preferably 65°C lower than the melting point (Tm-65°C). In addition, the holding temperature of the dispersion in the holding step is preferably less than 50°C lower than the melting point (Tm) of the polyamide resin (Tm-50°C), more preferably 55°C lower than the melting point (Tm-55°C), even more preferably 57°C lower than the melting point (Tm-57°C), and even more preferably 59°C lower than the melting point (Tm-59°C). It is believed that the polyamide resin particles are plasticized by the water used as the dispersion liquid, and by maintaining the temperature within a specific range, it becomes possible to produce expanded beads with a desired crystallite size.

[0046] The holding time in the holding step is preferably 5 minutes or more, more preferably 10 minutes or more, and even more preferably 20 minutes or more, from the viewpoint of facilitating the growth of crystallites in a specific range. The holding time in the holding step is preferably 60 minutes or less, more preferably 40 minutes or less. By holding for the above time, it is possible to obtain expanded polyamide resin particles having a large crystallite size. Furthermore, it is easy to obtain expanded particles having a low apparent density and a high closed cell ratio. The holding step can be set in multiple stages within the above temperature range, and it is also possible to slowly increase the temperature within the temperature range over a sufficient period of time. From the viewpoint of facilitating the growth of crystallites, it is preferable to set the temperature in one stage (constant holding temperature) within the above temperature range and hold for the above time.

[0047] The holding step is preferably carried out under pressure, from the viewpoint of allowing the polyamide resin to absorb moisture sufficiently and to uniformly impregnate the polyamide resin with the foaming agent, and is preferably maintained at the same pressure as the impregnation pressure. The pressure in the container containing the dispersion is preferably 1.5 MPa (G) or more, more preferably 2.5 MPa (G) or more. The pressure in the container containing the dispersion is preferably 7.0 MPa (G) or less, more preferably 5.0 MPa (G) or less.

[0048] [Foaming step] The foaming step is a step of foaming the polyamide resin particles impregnated with a foaming agent. The method for expanding the polyamide-based resin particles is not particularly limited, but a preferred method is a foaming method in which, following the holding step, the polyamide-based resin particles impregnated with a foaming agent are released together with water into a pressure atmosphere (usually atmospheric pressure) lower than the pressure inside the sealed container to cause foaming.

[0049] The temperature Te of the dispersion immediately before foaming (hereinafter also referred to as the foaming temperature) is preferably 90°C lower than the melting point (Tm) of the polyamide resin (Tm-90°C) or higher, more preferably 80°C lower than the melting point (Tm-80°C) or higher, even more preferably 70°C lower than the melting point (Tm-70°C) or higher, and even more preferably 65°C lower than the melting point (Tm-65°C) or higher, from the viewpoint of obtaining polyamide resin expanded particles having a low apparent density and a high closed cell ratio. The foaming temperature is preferably less than 50°C lower than the melting point (Tm) of the polyamide resin (Tm-50°C), more preferably 55°C lower than the melting point (Tm) of the polyamide resin (Tm-55°C), even more preferably 57°C lower than the melting point (Tm-57°C), and even more preferably 59°C lower than the melting point (Tm-59°C).

[0050] The pressure immediately before release in the foaming step (foaming pressure) is preferably 0.5 MPa (G) or more, more preferably 1.5 MPa (G) or more, and even more preferably 2.5 MPa (G) or more. The foaming pressure is preferably 10.0 MPa (G) or less, more preferably 7.0 MPa (G) or less, and even more preferably 5 MPa (G) or less.

[0051] In the foaming step, when the polyamide resin particles impregnated with the foaming agent are released together with water under a pressure lower than the pressure inside the sealed container, it is preferable to keep the temperature of the atmosphere at which they are released high. That is, in the manufacturing method of method 1, in the foaming step, the temperature of the dispersion immediately before foaming is set to a temperature lower than the melting point of the polyamide resin, and when the polyamide resin particles containing a foaming agent are released from a sealed container together with water under a pressure lower than the pressure inside the sealed container to foam, it is preferable to keep the atmospheric temperature high. Here, the atmospheric temperature refers to the temperature of the atmosphere with which the dispersion comes into contact immediately after the dispersion is released from the sealed container. As a method for keeping the atmospheric temperature high, a method of increasing the atmospheric temperature by steam is preferable, but a method of increasing the atmospheric temperature by high-temperature air may also be used. By keeping the temperature of the released atmosphere high, the growth of the crystallites of the resin particles can be promoted, and the obtained polyamide resin expanded particles can be expanded particles with a larger crystallite size. The atmospheric temperature is preferably 80 to 120°C. In addition, the pressure is preferably 0.05 to 0.3 MPa (G).

[0052] (Method of producing polyamide resin expanded beads (Method 2)) Method 2 includes a step of making polyamide-based resin particles absorb moisture to obtain hydrous resin particles; impregnating the resin particles with a blowing agent in a closed container; and heating the hydrous resin particles containing the foaming agent to foam them. Each step will be described below. The order of the step of obtaining water-containing resin particles and the step of impregnating the resin particles with a foaming agent is not particularly limited, and the step of impregnating the resin particles with a foaming agent may be performed after the step of obtaining water-containing resin particles, the step of obtaining water-containing resin particles may be performed after the step of impregnating the resin particles with a foaming agent, or the step of obtaining water-containing resin particles and the step of impregnating the resin particles with a foaming agent may be performed simultaneously.

[0053] [Step of Obtaining Water-Containing Resin Particles] The step of obtaining hydrous resin particles is a step of causing polyamide resin particles to absorb water. As a method for making the polyamide-based resin particles absorb water, a method of immersing the polyamide-based resin particles in water can be mentioned. The immersion conditions are not particularly limited as long as the polyamide-based resin particles can sufficiently absorb water. For example, it is preferable to place polyamide-based resin particles and an amount of water that completely immerses the polyamide-based resin particles in a container, and to carry out the immersion at the following temperature and time. The temperature during immersion is preferably 10° C. or higher, more preferably 15° C. or higher, and preferably 100° C. or lower, more preferably 80° C. or lower, from the viewpoint of sufficiently impregnating the polyamide resin particles with water in a short period of time. The immersion time is preferably 20 minutes or more, more preferably 40 minutes or more. From the viewpoint of shortening the production time, the upper limit of the immersion time is about 24 hours. The step of obtaining the hydrous resin particles may be performed under pressure.

[0054] [Step of impregnating foaming agent] In the step of impregnating the foaming agent, the method of impregnating the polyamide resin particles with the foaming agent is not particularly limited, but for example, it is preferable to place the polyamide resin particles in a pressurizable sealed container such as an autoclave and impregnate the polyamide resin particles with the foaming agent. When transferring the hydrous resin particles from the container (container 1) for the step of obtaining the hydrous resin particles to the container (container 2) for the step of impregnating the foaming agent, the hydrous resin particles may be taken out from the container 1 and put into the container 2 without removing the moisture on the surface of the resin particles.

[0055] The temperature during impregnation is preferably 0° C. or higher, more preferably 5° C. or higher, from the viewpoint of sufficiently impregnating the polyamide resin particles with the foaming agent in a short time, and is preferably 80° C. or lower, more preferably 60° C. or lower, from the viewpoint of preventing mutual adhesion between the water-containing resin particles.

[0056] In addition, from the viewpoint of sufficiently impregnating the polyamide resin particles with the foaming agent in a short time, the pressure during impregnation under pressure (impregnation pressure) is adjusted so that the pressure inside the pressure vessel containing the particles is preferably 1.5 MPa (G) or more, more preferably 2.5 MPa (G) or more, and is preferably 7.0 MPa (G) or less, and more preferably 5.0 MPa (G) or less, by adding the foaming agent to the pressure vessel.

[0057] The total time for the step of impregnating the foaming agent is preferably 30 minutes or more, more preferably 60 minutes or more, while from the viewpoint of productivity of the polyamide resin expanded beads, the time is preferably 300 minutes or less, more preferably 240 minutes or less.

[0058] After the foaming agent is applied, the pressure is gradually lowered to atmospheric pressure, thereby making it possible to obtain hydrous resin particles containing the foaming agent.

[0059] [Foaming step] The step of impregnating with a blowing agent is a step of heating the hydrous resin particles containing the blowing agent to expand the polyamide resin particles impregnated with the blowing agent. The foaming step is a step of heating the polyamide resin particles in a water-containing state. The method for expanding the polyamide-based resin particles is not particularly limited. For example, it is preferable to expand the water-containing polyamide-based resin particles impregnated with a blowing agent by heating them with a heat medium such as steam, hot air, or oil.

[0060] [Polyamide resin foamed bead molding] A polyamide resin expanded bead molding (expanded molded article) can be obtained by molding the expanded polyamide resin beads of the present invention in a mold. That is, the expanded molded article obtained here is obtained by molding the expanded polyamide resin beads of the present invention in a mold. The in-mold molding method can be a conventionally known method, but it is preferable to use heating with steam. The polyamide resin in the polyamide resin foamed beads is plasticized by absorbing water by steam, so that the molding steam pressure can be reduced. If the obtained molded product is dried, the polyamide resin returns to its original physical properties, resulting in a molded product with high heat resistance. The expanded polyamide resin beads of the present invention have excellent moldability in a molded body because the crystallites have grown large, and can be used to produce a good expanded bead molding. In addition, the expanded beads have excellent heat resistance, and therefore a molded body that is lightweight and has excellent heat resistance can be obtained. Specifically, excellent moldability in a molded body means that the surface is excellent when molding in a molded body, that the fusion property and recovery property are excellent, and that the moldable pressure range is wide. In addition, the expanded polyamide resin beads of the present invention have excellent moldability in a molded body, and therefore a good molded body can be obtained even if it is thick. The thick molded body is, for example, preferably 30 mm or more, more preferably 40 mm or more, and even more preferably 50 mm or more.

[0061] The density of the expanded polyamide resin bead molding of the present invention is preferably 20 kg / m 3 More preferably, it is 40 kg / m 3 More preferably, it is 50 kg / m 3 The density of the compact is preferably 300 kg / m 3 More preferably, it is 250 kg / m or less. 3 More preferably, it is 200 kg / m or less. 3 and even more preferably 150 kg / m 3 The following is the result. If the density of the molded article is within the above range, the balance between light weight and strength of the molded article is excellent. The density of the green body is measured by the following method. First, the expanded bead moldings are left to stand for 24 hours or more in an environment of 23°C and 50% relative humidity, and cut into rectangular samples of appropriate size (with the molding skin removed). The apparent volume of each sample is then calculated from the external dimensions of each sample, and the sum of these is taken as the apparent volume H of the sample. The molding density [kg / m 3 ] is required.

[0062] The closed cell ratio of the polyamide resin expanded bead molding of this specification is preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more. When the closed cell ratio of the expanded bead molding satisfies the above range, expanded beads with low apparent density are easily obtained. The closed cell ratio of the expanded bead molding means the ratio of the volume of the closed cells to the volume of the bubbles contained in the expanded beads constituting the expanded bead molding (the total volume of the closed cells and the open cells), and can be determined using an air comparison type specific gravity meter or the like in accordance with Procedure C described in ASTM-D2856-70. In this way, by using expanded polyamide resin particles having a large crystallite size, a molded article having a low apparent density and a high closed cell ratio can be obtained. EXAMPLES

[0063] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto.

[0064] Various physical properties of the polyamide resin and polyamide resin particles in each Production Example were measured by the following methods.

[0065] [Measurement of physical properties of polyamide resin and polyamide resin particles] [Melting point (Tm)] The melting point of the polyamide resin particles was measured by heat flux differential scanning calorimetry based on JIS K7121-1987. Under the condition of nitrogen inflow of 30 mL / min, the particles were heated from 30°C to a temperature 30°C higher than the end of the melting peak at a heating rate of 10°C / min (first temperature rise), then held at that temperature for 10 minutes, cooled to 30°C at a cooling rate of 10°C / min, and heated again to a temperature 30°C higher than the end of the melting peak at a heating rate of 10°C / min. The melting point was determined as the peak apex temperature of the melting peak of the second DSC curve. The measuring device used was a high-sensitivity differential scanning calorimeter "EXSTAR DSC7020" (manufactured by SII Nano Technology Co., Ltd.). For the measurement of the DSC curve, polyamide resin particles were used that had been left to stand for 24 hours or more in an environment of 23°C and 50% relative humidity.

[0066] 〔density〕 This is a catalog value determined based on the method described in ISO 1183-3.

[0067] [Flexural modulus] The flexural modulus of polyamide resin was determined by measurement in accordance with JIS K7171: 2016. The flexural modulus was measured by preparing a resin test piece having a thickness of 4 mm, a width of 10 mm, and a length of 80 mm, and leaving the test piece at rest for 72 hours at room temperature of 23°C and relative humidity of 50%, and then measuring the flexural modulus using an autograph AGS-10kNG (Shimadzu Corporation) testing machine under the conditions of a support distance of 64 mm, an indenter radius of 15.0 mm, a support table radius of 25.0 mm, a test speed of 2 mm / min, a room temperature of 23°C, and a relative humidity of 50%, and the average of the calculated values ​​(5 points) was used. The amide elastomer (Arkema, product name "PEBAX5533", melting point 159°C, density 1.01g / cm 3 The flexural modulus of elasticity of the above-mentioned polymer was measured by the above-mentioned method and was found to be 150 MPa.

[0068] [Production of polyamide resin particles] Manufacturing Example 1 A polyamide resin (5033B, details are shown in Table 1) was fed to an extruder, and 0.8000 parts by mass of "Talcan Powder PK-S" (manufactured by Hayashi Kasei Co., Ltd.) was added as a cell regulator relative to 100 parts by mass of the polyamide resin, and aromatic polycarbodiimide (Stabaxol P, manufactured by Rhein Chemie AG) was fed as an end-capping agent in an amount of 1 part by mass relative to 100 parts by mass of the polyamide resin, and melt-kneaded. The melt-kneaded product was extruded into strands with a circular cross section from the holes in the die attached to the tip of the extruder, and the extruded strands were water-cooled, then cut into an average mass of 2 mg using a pelletizer, and dried to obtain polyamide resin particles.

[0069] Manufacturing Example 2 Polyamide-based resin particles were obtained in the same manner as in Production Example 1, except that the polyamide-based resin was changed from 5033B to 1030B (details are shown in Table 1).

[0070] Production Example 3 Polyamide-based resin particles were obtained in the same manner as in Production Example 1, except that the polyamide-based resin was changed from 5033B to E2046 (details are shown in Table 1), and the end-capping agent was changed from Stabaxol P to aromatic polycarbodiimide (Stabaxol P100, manufactured by Rhein Chemie).

[0071] Production Example 4 Polyamide resin particles were obtained in the same manner as in Production Example 1, except that the end-capping agent (Stabaxol P) was not used.

[0072] [Table 1]

[0073] Various physical properties of the expanded polyamide resin particles in each of the Examples and Comparative Examples were measured by the following methods.

[0074] [Measurement of physical properties of polyamide resin foam particles] The various physical properties of the expanded polyamide resin beads other than the moisture content were measured after the following conditioning. First, the obtained expanded polyamide resin beads were placed in an environment at a temperature of 60°C for 24 hours, and then slowly cooled to room temperature (23°C). Next, the condition was conditioned by leaving them to stand in an environment at a temperature of 23°C, a relative humidity of 50%, and 1 atm for 24 hours.

[0075] [Moisture percentage] Polyamide resin expanded particles immediately after expansion were randomly selected, and the moisture on the surface of the expanded particles was wiped off with a dry cloth. Approximately 0.2 g of the expanded particles were then weighed and heated to 160°C using a heating moisture vaporizer to vaporize the moisture inside the expanded particles. The moisture content was then measured by Karl Fischer titration (coulometric titration method) using a Karl Fischer moisture meter (AQ-2200A, manufactured by Hiranuma Sangyo Co., Ltd.).

[0076] [Crystallite size] The crystallite size of the polyamide resin foamed particles was determined by the following method. The X-ray diffraction (XRD) measurement of the obtained polyamide resin foamed particles was performed by a reflection method using an X-ray scattering device "SmartLab SE" (manufactured by Rigaku Corporation). The detector used was a semiconductor one-dimensional detector D / teX Ultra 250. The sample used was a test piece in which randomly selected foamed particles were packed as densely as possible in a 24 mm diameter sample holder without overlapping. Empty cell scattering correction was also performed. The one-dimensional X-ray diffraction profile thus obtained was subjected to peak separation into a diffraction peak derived from crystals and a diffraction peak derived from amorphous crystals, assuming a Gaussian function as the peak shape, using software (product name: SmartLab Studio II). The full width at half maximum β (rad) of the peak with the narrowest peak width among the peaks obtained by peak separation was calculated, and the crystallite size D of the foamed particles was calculated according to the following formula (2) using the full width at half maximum β. The above measurement was performed on 10 test pieces, and the arithmetic average value thereof was taken as the crystallite size of the foamed particles.

[0077]

number

[0078] [Total heat of fusion in the DSC curve of the first heating] For the measurements, a high-sensitivity differential scanning calorimeter "EXSTAR DSC7020" (manufactured by SII NanoTechnology Inc.) was used. Polyamide resin foamed particles were used as test pieces and heated at a heating rate of 10°C / min from 30°C to a temperature 30°C higher than the end of the melting peak by heat flux differential scanning calorimetry based on JIS K7122-1987, and a DSC curve for the first heating was obtained. On the obtained DSC curve, a straight line was drawn connecting the point of 150°C on the DSC curve and the point on the DSC curve that shows the temperature at the end of the melting peak. This straight line was used as the baseline, and the amount of heat calculated from the area enclosed by the baseline and the DSC curve on the endothermic side of the baseline was used as the total heat of fusion of the DSC curve for the first heating.

[0079] [The apex temperature of the melting peak of the DSC curve of the second heating] For the measurements, a high-sensitivity differential scanning calorimeter "EXSTAR DSC7020" (manufactured by SII NanoTechnology Inc.) was used. Polyamide resin foamed particles were used as test pieces, and were heated from 30°C to a temperature 30°C higher than the end of the melting peak at a heating rate of 10°C / min according to heat flux differential scanning calorimetry based on JIS K7121-1987, and held at that temperature for 10 minutes. Thereafter, the sample was cooled to 30° C. at a cooling rate of 10° C. / min, and then heated again from 30° C. to a temperature 30° C. higher than the end of the melting peak at a heating rate of 10° C. / min to obtain a DSC curve for the second heating. In the obtained DSC curve, the apex (peak top) temperature of the maximum melting peak (endothermic peak) appearing on the DSC curve was taken as the apex temperature of the melting peak of the DSC curve of the second heating.

[0080] [Apparent density of expanded polyamide resin particles] A measuring cylinder containing water at a temperature of 23°C is prepared, and a volume of about 500 cm is added to the measuring cylinder. 3The mass W1 of the foamed beads was measured and submerged using a wire net. Taking into account the volume of the wire net, the volume V1 [cm3] of the foamed beads was calculated based on the rise in the water level. 3 ] is measured, and the mass W1 [g] of the foamed particles is divided by the volume V1 (W1 / V1), and the unit is [kg / m 3 The apparent density of the expanded beads was calculated by converting the density into the mass ratio (μm).

[0081] [Average bubble diameter] First, the expanded beads were divided into two parts along the center of the expanded beads, and the cut surface was photographed with a scanning electron microscope. Next, in the obtained cross-sectional photograph, lines were drawn at equal intervals in eight directions from the center of the expanded beads cut surface to the surface of the expanded beads at 45° increments, and the number of bubbles intersecting the lines was counted. The total length of the lines was divided by the number of bubbles counted to obtain the bubble diameter of the expanded beads. This operation was carried out for 30 expanded beads in the same manner, and the arithmetic mean value of the bubble diameters of each expanded bead was taken as the average bubble diameter of the expanded beads.

[0082] [Surface film thickness] The length from the outermost surface of the expanded beads to the outermost bubble of the expanded beads (thickness of the outermost surface layer) was measured on the straight line segments of the eight directions of the average bubble diameter, and the average thickness of the outermost surface layer of each expanded bead was calculated by arithmetically averaging the values. The average surface layer thickness of the expanded beads was then calculated by arithmetically averaging the values ​​of 30 expanded beads.

[0083] [Closed cell ratio of expanded polyamide resin particles] The true volume Vx of the foamed beads (the sum of the volume of the resin that constitutes the foamed beads and the total volume of the air bubbles in the closed cell part inside the foamed beads) was measured according to procedure C described in ASTM-D2856-70. To measure this true volume Vx, an air comparison specific gravity meter "930" manufactured by Toshiba Beckman Co., Ltd. was used. Next, the closed cell ratio was calculated according to the following formula (1), and the arithmetic average of the five measurement results was calculated. Closed cell ratio (%)=(Vx-W / ρ)×100 / (Va-W / ρ) (1) Vx: The true volume of the foam particles measured by the above method (cm 3 ) Va: Apparent volume of foam particles (cm 3 ) W: Mass of the sample for measuring foam particles (g) ρ: Density of the resin that composes the foamed particles (g / cm 3 )

[0084] [Evaluation of polyamide resin foam particles] [Heat resistance evaluation (ratio of 5% compressive stress at 20℃ lower than the melting point (Tm1-20℃) to 5% compressive stress at 23℃ of polyamide resin foam particles)] The expanded beads were measured in compression mode (diameter of the tip of the compression probe: 3.5 mm) using a thermal analyzer (TMA; Hitachi High-Tech Science Corporation, "TMA7100"). Specifically, one expanded bead was randomly selected, and the expanded bead was clamped in the short diameter direction with a compression probe under a load of 10 mN, and then the temperature was adjusted to a specified level. The expanded bead was then pressed at a speed of 1 mm / min while maintaining the temperature at the same temperature, and the load of the probe was monitored, and the stress at the point when the thickness of the expanded bead became 5% of the thickness of the expanded bead before compression was recorded. The above operation was performed three times, and the arithmetic average value was taken as the 5% compression stress. As shown in Table 2, the predetermined temperatures are a temperature (Tm1-20°C) that is 20°C lower than the melting point of the expanded polyamide resin particles used in the expanded polyamide resin particles, and 23°C. Furthermore, the ratio of the 5% compressive stress at a temperature (Tm1-20°C) 20°C lower than the melting point to the 5% compressive stress at 23°C of the expanded polyamide resin beads [(Tm1-20°C compressive stress) / (23°C compressive stress)] was calculated using the measured values ​​obtained by the above measurement. The above operation was performed for three expanded beads, and the arithmetic average value was taken as the ratio of the 5% compressive stress at a temperature (Tm1-20°C) 20°C lower than the melting point to the 5% compressive stress at 23°C of the expanded polyamide resin beads [(Tm1-20°C compressive stress) / (23°C compressive stress)]. The larger the ratio, the more excellent the heat resistance. Such expanded polyamide resin particles having excellent heat resistance are suitably used in applications requiring heat resistance, such as the manufacture of a composite by compounding with an uncured thermosetting resin by mixing or laminating the particles and curing the thermosetting resin.

[0085] [Production of expanded polyamide resin particles] Example 1 1 kg of the polyamide resin particles obtained in Production Example 1 and 3 liters of water as a dispersion liquid were charged into a 5-liter autoclave equipped with a stirrer, and further, 0.3 parts by mass of kaolin as a dispersant and 0.004 parts by mass of sodium alkylbenzene sulfonate as a surfactant were added to the dispersion liquid relative to 100 parts by mass of the polyamide resin particles. The contents in the autoclave were heated from room temperature (23°C) while stirring, and carbon dioxide as a foaming agent was injected into the autoclave until the pressure in the autoclave reached 4.0 MPa (G) (impregnation pressure) before reaching 136°C (impregnation temperature). At this time, the temperature rise time from room temperature (23°C) to the impregnation temperature was 40 minutes. Next, 136°C (holding temperature) and 4 MPa (G) (holding pressure) were held for 30 minutes. Thereafter, the polyamide-based resin particles impregnated with the foaming agent were released together with the dispersion liquid under atmospheric pressure (0.1 MPa). The foaming temperature (temperature Te of the dispersion liquid immediately before foaming) was 136° C. The obtained expanded polyamide-based resin particles were cured in an oven at 60° C. for 24 hours, and then slowly cooled to obtain expanded polyamide-based resin particles. The physical properties of the obtained polyamide-based resin expanded beads are shown in Table 2. The moisture content of the polyamide-based resin expanded beads immediately after foaming in Example 1 was measured to be 18%. The moisture content of the polyamide-based resin expanded beads is higher than the saturated water absorption of the polyamide-based resin. This is believed to be because the polyamide-based resin expanded beads are in a supersaturated water absorption state and therefore exhibit a higher value than the saturated water absorption of the polyamide-based resin. In addition, although it is difficult to measure the moisture content of the polyamide-based resin expanded beads in the autoclave, it is believed to be at least higher than that of the polyamide-based resin expanded beads immediately after foaming.

[0086] Example 2 Expanded polyamide resin particles were obtained in the same manner as in Example 1, except that the polyamide resin particles obtained in Production Example 2 were used and the impregnation temperature, holding temperature and expansion temperature were all set at 158°C.

[0087] Example 3 Expanded polyamide resin particles were obtained in the same manner as in Example 1, except that the polyamide resin particles obtained in Production Example 3 were used and the impregnation temperature, holding temperature and expansion temperature were all set at 175.5°C.

[0088] Example 4 Expanded polyamide resin particles were obtained in the same manner as in Example 1, except that the polyamide resin particles obtained in Production Example 4 were used.

[0089] Example 5 In this example, the polyamide-based resin particles impregnated with a blowing agent were produced in the same manner as in Example 1, except that the polyamide-based resin particles were released from the autoclave to atmospheric pressure while steam at a pressure of 0.1 MPa (G) was supplied to the outlet of the valve. The atmospheric temperature of the dispersion containing the polyamide-based resin particles and water at the portion where the dispersion contacted the steam was 100°C.

[0090] Example 6 3 kg of the polyamide resin particles obtained in Production Example 1 were completely immersed in 6 liters of water and allowed to stand for 1 hour. Next, the resin particles taken out from the water were placed in an autoclave, and carbon dioxide as a blowing agent was injected into the autoclave until the pressure inside the autoclave reached 4 MPa (G) (impregnation pressure). Next, the pressure was maintained at 10°C (impregnation temperature) and 4 MPa (G) for 3 hours. Thereafter, the polyamide-based resin particles impregnated with the blowing agent were removed from the autoclave and transferred to a foaming vessel filled with an oil medium heated to the temperature (foaming temperature) shown in Table 2, and the polyamide-based resin particles impregnated with the blowing agent were immersed in the oil medium to be foamed. The surfaces of the obtained expanded polyamide-based resin particles were washed with normal hexane to remove the oil, and the expanded polyamide-based resin particles were cured in an oven at 60°C for 24 hours and then slowly cooled to obtain expanded polyamide-based resin particles. The physical properties of the obtained expanded polyamide resin particles are shown in Table 2. The moisture content of the polyamide resin particles immediately before expansion was measured and found to be 6.2%.

[0091] Example 7 In this example, expanded polyamide resin particles were obtained in the same manner as in Example 1, except that the holding temperature was changed to 139°C and the expansion temperature was changed to 135°C.

[0092] Comparative Example 1 3 kg of the polyamide-based resin particles obtained in Production Example 1 was charged into an autoclave, and carbon dioxide as a foaming agent was injected into the autoclave until the pressure inside the autoclave reached 4 MPa (G) (impregnation pressure). Then, the temperature was maintained at 10°C (impregnation temperature) and 4 MPa (G) for 3 hours. Thereafter, the polyamide-based resin particles impregnated with the foaming agent were transferred to an expansion device, and air having a temperature (foaming temperature) shown in Table 2 was blown in for 20 seconds to obtain expanded polyamide-based resin particles. The obtained expanded polyamide-based resin particles were cured in an oven at 60°C for 24 hours, and then slowly cooled to obtain expanded polyamide-based resin particles. The physical properties of the resulting expanded polyamide resin particles are shown in Table 2. The moisture content of the polyamide resin particles immediately before expansion was measured and found to be 3.0%.

[0093] [Evaluation of moldability of expanded polyamide resin beads and molded bodies made from expanded polyamide resin beads] The moldability of the expanded polyamide resin beads in each of the Examples and Comparative Examples was evaluated by the following methods, and various physical properties of the obtained molded articles were measured by the following methods.

[0094] [Production of expanded polyamide resin bead moldings] First, the polyamide resin expanded beads obtained in Examples 1 to 7 and Comparative Example 1 were filled into a flat mold having a length of 300 mm, a width of 300 mm, and a thickness of 50 mm, and molding was performed in the mold by steam heating to obtain a plate-shaped expanded bead molding. The heating method was as follows: steam was supplied for 5 seconds with the drain valves of both sides of the mold open to perform preheating (exhaust process), then one-sided heating was performed at a pressure 0.04 MPa (G) lower than the molding steam pressure shown in Table 2, and one-sided heating was performed from the opposite direction at a pressure 0.02 MPa (G) lower than the molding steam pressure shown in Table 2, and then main heating was performed from both sides at the molding steam pressure shown in Table 2. After the heating was completed, the pressure was released, and the molded product was water-cooled until the surface pressure due to the expansion force of the molded product was reduced to 0.02 MPa (gauge pressure), and then the mold was opened and the molded product was removed from the mold. The obtained molded product was cured in an oven at 80°C for 12 hours, and then slowly cooled to room temperature. In this manner, a polyamide expanded bead molding was obtained. The moldability of the expanded beads was evaluated for the molded bodies at each molding steam pressure, and the physical properties of the molded bodies were also measured. The results are shown in Table 2.

[0095] [Evaluation of moldability of expanded polyamide resin beads] The polyamide resin expanded bead moldings obtained by the above-mentioned production method were measured for recovery, surface properties, and fusion properties, and the moldability of the polyamide resin expanded bead moldings was evaluated. The evaluation methods are shown below. (Recovery of foamed bead molded bodies) The thicknesses of the end (10 mm inside from the end) and center (part dividing the molded body into two equal parts in both the vertical and horizontal directions) of the expanded bead molding corresponding to the dimensions of the flat mold used in the in-mold molding were measured. The thickness ratio of the expanded bead molding (thickness of the center part of the molding / thickness of the end part of the molding×100(%)) was then calculated and evaluated as follows. The higher the thickness ratio, the better the recovery and moldability. ◯: Thickness ratio is 95% or more. ×: The thickness ratio is less than 95%.

[0096] (Surface properties of foamed bead molded bodies) The surface properties of the expanded bead moldings were evaluated as follows: The more the gaps between the expanded beads on the surface of the molding are filled, the more excellent the surface properties of the expanded beads and the better the moldability. ◯: Gaps between the foamed particles on the surface of the molded article are filled. ×: Gaps between the foamed particles on the surface of the molded article are not filled.

[0097] (Fusing property of foamed bead molded body) The fusion rate of the molded body was determined based on the ratio of the number of foamed beads that had been broken among the foamed beads exposed on the fracture surface when the foamed bead molded body was broken. Specifically, first, a test piece (100 mm long x 100 mm wide x thickness: thickness of the molded body) was cut out from the foamed bead molded body, and a cutter knife was used to make a cut of about 5 mm in the thickness direction of each test piece, and then the test piece was broken from the cut part. Next, the number of foamed beads (n) present on the fracture surface of the foamed bead molded body and the number of foamed beads that had been broken (b) were measured, and the ratio of (b) to (n) (material breakage on the fracture surface, b / n) was expressed as a percentage. The larger the value of material breakage on the fracture surface, the better the fusion adhesion of the foamed beads and the better the moldability.

[0098] [Measurement of physical properties of polyamide resin expanded bead molded bodies] The various physical properties of the expanded polyamide resin bead moldings shown below were measured after the expanded polyamide resin bead moldings were cooled slowly to room temperature and allowed to stand for 24 hours in an environment of 23° C. and 50% relative humidity. (Molded object density) A sample (length 100 mm × width 100 mm × thickness 30 mm) was cut out from the foamed bead molding, excluding the skin surface. The apparent volume of the sample was calculated from the outer dimensions of the sample, and this was taken as the apparent volume H of the sample. The total weight W of the sample was divided by the apparent volume H (W / H) to obtain the molding density [kg / m 3 ] was requested.

[0099] (Closed cell ratio of polyamide resin foamed beads) A sample (length 30 mm × width 30 mm × thickness 30 mm) excluding the skin surface was cut out from the foamed bead molding, and the true volume Vx of the foamed bead molding (the sum of the volume of the resin constituting the foamed bead molding and the total volume of the air bubbles in the closed cell part in the foamed bead molding) was measured according to procedure C described in ASTM-D2856-70. To measure this true volume Vx, an air comparison type specific gravity meter "930" manufactured by Toshiba Beckman Co., Ltd. was used. Next, the closed cell ratio was calculated using the following formula (3), and the arithmetic average of the five measurement results was calculated. Closed cell ratio (%)=(Vx-W / ρ)×100 / (Va-W / ρ) (3) Vx: The true volume (cm) of the foamed bead molding measured by the above method 3 ) Va: Apparent volume of foamed bead molding (cm 3 ) W: Mass of the foamed bead molded body measurement sample (g) ρ: Density of the resin constituting the foamed bead molding (g / cm 3 )

[0100] [Table 2]

[0101] From the results shown in Table 2, it is understood that the expanded polyamide resin beads of the Examples have excellent moldability in a mold. In addition, the expanded polyamide resin beads of the Examples also have excellent heat resistance.

Claims

1. The expanded polyamide resin particles have a crystallite size of more than 8 nm as measured by X-ray diffraction.

2. The expanded polyamide resin beads according to claim 1, wherein a total heat of fusion in a DSC curve measured by using the expanded polyamide resin beads as a test piece and heating the test piece from 30°C to a temperature 30°C higher than the end of the melting peak at a heating rate of 10°C / min based on heat flux differential scanning calorimetry according to JIS K7122-1987 is 40 to 140 J / g.

3. The apparent density of the polyamide resin foam particles is 10 to 300 kg / m 3 3. The expanded polyamide resin particles according to claim 1 or 2,

4. 4. The expanded polyamide resin beads according to claim 1, wherein the apex temperature of the melting peak in the DSC curve of the second heating obtained under the following condition 1 is 185 to 285° C. Condition 1 According to the heat flux differential scanning calorimetry method of JIS K7121-1987, a polyamide resin foamed particle is used as a test piece, and is heated at a heating rate of 10°C / min from 30°C to a temperature 30°C higher than the end of the melting peak, and then maintained at that temperature for 10 minutes. The test piece is then cooled to 30°C at a cooling rate of 10°C / min, and is then heated again at a heating rate of 10°C / min to a temperature 30°C higher than the end of the melting peak. The DSC curve measured during this process is taken as the DSC curve for the second heating.

5. 5. The expanded polyamide resin beads according to claim 1, wherein the expanded polyamide resin beads have a crystallite size of 9 nm or more as measured by X-ray diffraction.

6. 6. The expanded polyamide resin beads according to claim 1, wherein the expanded polyamide resin beads have a crystallite size of 10 nm or more as measured by X-ray diffraction.

7. 7. The expanded polyamide resin beads according to claim 1, wherein the expanded polyamide resin beads have a closed cell ratio of more than 90%.

8. 8. The expanded polyamide resin beads according to claim 1, wherein the expanded polyamide resin beads have an average cell diameter of 20 to 200 μm.

9. 9. The expanded polyamide resin beads according to claim 1, wherein the surface layer of the expanded polyamide resin beads has a thickness of 5 to 50 μm.

10. A polyamide-based resin foamed particle described in any one of claims 1 to 9, wherein the polyamide-based resin particles used in the production of the polyamide-based resin foamed particles contain a polyamide-based resin, and the polyamide-based resin is a polyamide copolymer.

Citation Information

Patent Citations

  • Polyamide prefoamed beads and foam therefrom and its production

    JP1986268737A

  • JPP6653049B

  • Polyamide microparticles, manufacturing method therefor, optical film using said polyamide microparticles, and liquid-crystal display device

    WO2011132680A1

  • Polyamide resin foam-molded article and method for producing polyamide resin foam-molded article

    WO2016147582A1