Polyol composition, foamable polyurethane composition, and polyurethane foam

By using a high boiling point hydrofluoroolefin and a catalyst system, the polyol composition stabilizes against boiling, enabling controlled reactions and enhancing the properties of polyurethane foam.

JP7579082B2Active Publication Date: 2024-11-07SEKISUI CHEMICAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020134231
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-06
Publication Date
2024-11-07
Estimated Expiration
2040-08-06

AI Technical Summary

Technical Problem

The polyol composition used in polyurethane foam production can boil before mixing with polyisocyanate, especially in high temperatures, leading to uncontrollable reactions and unsatisfactory application.

Method used

Incorporating a high boiling point hydrofluoroolefin blowing agent with a boiling point of 30°C or higher, along with a catalyst system including a trimerization catalyst and metal catalyst, to stabilize the polyol composition and facilitate controlled reaction with polyisocyanate.

Benefits of technology

The solution effectively suppresses boiling, allows for easier handling and controlled reaction, resulting in improved foamability and thermal conductivity of the polyurethane foam.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579082000001
    Figure 0007579082000001
  • Figure 0007579082000002
    Figure 0007579082000002
Patent Text Reader

Abstract

To provide a polyol composition that prevents the boiling of the polyol composition and facilitates the control of reaction with a polyisocyanate.SOLUTION: The present invention discloses a polyol composition that is reacted with a polyisocyanate to make a polyurethane foam, the polyol composition containing a polyol, a foamer, and a catalyst, the foamer containing a hydrofluoroolefin with a boiling point of 30°C or higher.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyol composition, a foamable polyurethane composition containing the polyol composition, and a polyurethane foam formed from the foamable polyurethane composition. [Background technology]

[0002] Due to its excellent heat insulating properties and adhesive properties, polyurethane foam is used as a heat insulating material for buildings such as apartment complexes, detached houses, various school facilities, commercial buildings, etc. Polyurethane foam is obtained by mixing a polyol composition and a polyisocyanate and foaming the mixture. There are various types of blowing agents, and hydrofluoroolefins (hereinafter sometimes referred to as "HFOs") have been proposed, which do not pose environmental problems such as global warming and ozone layer destruction (see, for example, Patent Document 1).

[0003] The application method is to mix the polyol composition and the polyisocyanate at the application site, react them, foam them, and spray them, etc. Therefore, the polyol composition and the polyisocyanate are stored separately in containers, drums, etc., and mixed just before application (for example, see Patent Document 2).

[0004] When the polyol composition contains a filler, the polyol composition may be stirred immediately before application in order to disperse the filler. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2018-21199 A [Patent Document 2] JP 2016-145360 A Summary of the Invention [Problem to be solved by the invention]

[0006] As described above, the polyol composition and the polyisocyanate are stored in a drum or the like before application, but the polyol composition may boil before mixing with the polyisocyanate, particularly in summer. Also, the polyol composition may boil due to stirring for dispersing fillers and the like in the polyol composition. The boiling of the polyol composition makes it difficult to control the reaction with the polyisocyanate, resulting in a problem of insufficient application.

[0007] In view of the above-mentioned problems, the present invention aims to provide a polyol composition capable of suppressing boiling of the polyol composition, a foamable polyurethane composition containing the polyol composition, and a polyurethane foam formed from the foamable polyurethane composition. [Means for solving the problem]

[0008] As a result of intensive research into solving the above problems, the present inventors have found that the cause of the boiling is the low-boiling point blowing agent contained in the polyol composition, and that the above problems can be solved by using a blowing agent with a high boiling point, and have completed the present invention. That is, the present invention provides the following [1] to

[12] .

[0009] [1] A polyol composition for use in reacting with a polyisocyanate to obtain a polyurethane foam, the polyol composition comprising a polyol, a blowing agent, and a catalyst, the blowing agent comprising a hydrofluoroolefin having a boiling point of 30°C or higher. [2] The polyol composition according to the above [1], wherein the blowing agent further contains a hydrofluoroolefin having a boiling point of less than 30°C. [3] The polyol composition according to the above [1] or [2], further comprising a filler. [4] The polyol composition according to any one of the above [1] to [3], wherein the catalyst comprises a trimerization catalyst. [5] The polyol composition according to the above [4], wherein the trimerization catalyst comprises a quaternary ammonium salt. [6] The polyol composition according to any one of the above [1] to [5], wherein the catalyst contains a metal catalyst containing at least one selected from the group consisting of bismuth and tin. [7] The polyol composition according to any one of the above [1] to [6], wherein the catalyst comprises an imidazole derivative. [8] The polyol composition according to any one of the above [1] to [7], wherein the hydrofluoroolefin having a boiling point of 30° C. or higher is 1,1,1,4,4,4-hexafluoro-2-butene. [9] The polyol composition according to any one of the above [2] to [8], wherein the hydrofluoroolefin having a boiling point of less than 30° C. is trans-1-chloro-3,3,3-trifluoropropene.

[10] A foamable polyurethane composition comprising the polyol composition according to any one of the above [1] to [9] and a polyisocyanate.

[11] The foamable polyurethane composition according to the above

[11] , having an isocyanate index of 200 or more.

[12] A polyurethane foam obtained by reacting and foaming the foamable polyurethane composition according to the above

[10] or

[11] . Effect of the Invention

[0010] According to the present invention, it is possible to provide a polyol composition that can suppress boiling of the polyol composition and facilitate control of the reaction with a polyisocyanate, thereby enabling favorable application, a foamable polyurethane composition containing the polyol composition, and a polyurethane foam formed from the foamable polyurethane composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] <Polyol composition> The polyol composition of the present invention comprises a polyol, a blowing agent, and a catalyst, and is characterized in that the blowing agent contains a hydrofluoroolefin having a boiling point of 30° C. or higher. The present invention will be described in detail below.

[0012] The polyol composition of the present invention contains a polyol as a raw material for polyurethane foam. Examples of the polyol used in the present invention include polylactone polyols, polycarbonate polyols, aromatic polyols, alicyclic polyols, aliphatic polyols, polyester polyols, polymer polyols, polyether polyols, etc. Polyols are usually liquid at room temperature (23° C.) and normal pressure (1 atm).

[0013] Examples of the polylactone polyol include polypropiolactone glycol, polycaprolactone glycol, and polyvalerolactone glycol. Examples of polycarbonate polyols include polyols obtained by dealcoholization reaction of hydroxyl group-containing compounds such as ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, octanediol, and nonanediol with ethylene carbonate, propylene carbonate, and the like.

[0014] Examples of aromatic polyols include bisphenol A, bisphenol F, phenol novolac, and cresol novolac. Examples of the alicyclic polyol include cyclohexanediol, methylcyclohexanediol, isophoronediol, dicyclohexylmethanediol, and dimethyldicyclohexylmethanediol. Aliphatic polyols include, for example, alkanediols such as ethylene glycol, propylene glycol, butanediol, pentanediol, and hexanediol.

[0015] Examples of polyester polyols include polymers obtained by dehydration condensation of polybasic acids and polyhydric alcohols, and condensates of hydroxycarboxylic acids and the above-mentioned polyhydric alcohols. Examples of polybasic acids include adipic acid, azelaic acid, sebacic acid, isophthalic acid (m-phthalic acid), terephthalic acid (p-phthalic acid), and succinic acid, etc. Examples of polyhydric alcohols include bisphenol A, ethylene glycol, 1,2-propylene glycol, 1,4-butanediol, diethylene glycol, 1,6-hexane glycol, and neopentyl glycol, etc. Examples of hydroxycarboxylic acids include castor oil and reaction products of castor oil and ethylene glycol.

[0016] Examples of the polymer polyol include polymers obtained by graft polymerizing an ethylenically unsaturated compound such as acrylonitrile, styrene, methyl acrylate, or methacrylate with an aromatic polyol, an alicyclic polyol, an aliphatic polyol, or a polyester polyol, or polybutadiene polyol, or hydrogenated products thereof.

[0017] Examples of polyether polyols include polymers obtained by ring-opening polymerization of at least one alkylene oxide such as ethylene oxide, propylene oxide, and tetrahydrofuran in the presence of at least one low molecular weight active hydrogen compound having two or more active hydrogens. Examples of low molecular weight active hydrogen compounds having two or more active hydrogens include diols such as bisphenol A, ethylene glycol, propylene glycol, butylene glycol, and 1,6-hexanediol, triols such as glycerin and trimethylolpropane, tetrahydric to octahydric alcohols such as pentaerythritol, sorbitol, mannitol, sorbitan, diglycerin, and dipentaerythritol, sucrose, glucose, mannose, fructose, methyl glucoside, and derivatives thereof, and amines such as ethylenediamine and butylenediamine.

[0018] The polyol used in the present invention is preferably at least one selected from the group consisting of polyester polyols and polyether polyols. From the viewpoint of foaming property and reactivity, polyester polyols are more preferable. Also, polyols having two hydroxyl groups are preferable. Among them, from the viewpoint of improving flame retardancy, aromatic polyester polyols, which are polyester polyols having aromatic rings, are preferable. As the aromatic polyester polyol, aromatic polyester polyols obtained by dehydration condensation of polybasic acids having aromatic rings such as isophthalic acid (m-phthalic acid) and terephthalic acid (p-phthalic acid) with dihydric alcohols such as bisphenol A, ethylene glycol, and 1,2-propylene glycol are more preferable. The use of aromatic polyester polyols makes it easier to improve flame retardancy.

[0019] The hydroxyl value of the polyol is preferably 20 to 350 mgKOH / g, more preferably 50 to 300 mgKOH / g, and even more preferably 100 to 250 mgKOH / g. When the hydroxyl value of the polyol is equal to or less than the upper limit, the viscosity of the polyol composition is likely to decrease, which is preferable from the viewpoint of handling, etc. On the other hand, when the hydroxyl value of the polyol is equal to or more than the lower limit, the crosslink density of the polyurethane foam increases, thereby increasing the strength. The hydroxyl value of the polyol can be measured in accordance with JIS K 1557-1:2007.

[0020] The content of the polyol in the polyol composition of the present invention is preferably 15 to 80% by mass, more preferably 20 to 70% by mass, and even more preferably 25 to 60% by mass. When the content of the polyol is equal to or more than the lower limit, it is preferable because the polyol and the polyisocyanate are easily reacted. On the other hand, when the content of the polyol is equal to or less than the upper limit, it is preferable from the viewpoint of handling because the viscosity of the polyol composition does not become too high.

[0021] <Foaming agent> The polyol composition of the present invention contains a hydrofluoroolefin having a boiling point of 30° C. or more (hereinafter, may be referred to as "high-boiling HFO") as a blowing agent. By containing a high-boiling HFO, the polyol composition of the present invention suppresses boiling and makes it easier to control the reaction with polyisocyanate. In addition, it is easier to reduce the thermal conductivity of the resulting polyurethane foam. Furthermore, HFO has high stability as a blowing agent, its catalytic activity is less likely to decrease, and its environmental load is also low. The high-boiling HFO is not particularly limited as long as it has a boiling point of 30° C. or more, and examples of such high-boiling HFO include fluoroalkenes having about 3 to 6 carbon atoms. In addition, the HFO may be a hydrochlorofluoroolefin having a chlorine atom, and therefore may be a chlorofluoroalkene having about 3 to 6 carbon atoms. Examples of high-boiling point HFOs include tetrafluoropropene and hexafluorobutene. More specifically, examples include cis-1,3,3,3-tetrafluoropropene (HFO-1234ze(Z), boiling point: 39° C.) and 1,1,1,4,4,4-hexafluoro-2-butene (HFO-1336mzz, boiling point: 33° C.), with HFO-1336mzz being particularly preferred. The upper limit of the boiling point of the high-boiling point HFO is not particularly limited, but from the viewpoint of obtaining good foamability, it is preferably 50°C or less, more preferably 45°C or less, and even more preferably 40°C or less. These high-boiling point HFOs may be used alone or in combination of two or more.

[0022] In addition, the polyol composition of the present invention may use only a high-boiling HFO as the hydrofluoroolefin, but it is preferable to use a high-boiling HFO in combination with an HFO having a boiling point of less than 30° C. (hereinafter sometimes referred to as a "low-boiling HFO"). By mixing a high-boiling HFO and a low-boiling HFO, the boiling point of the blowing agent can be controlled, and a better foam can be obtained.

[0023] The low-boiling-point HFO is not particularly limited as long as it has a boiling point of less than 30° C., and examples thereof include fluoroalkenes having about 3 to 6 carbon atoms. The HFO may also be a hydrochlorofluoroolefin having a chlorine atom, and therefore may be a chlorofluoroalkene having about 3 to 6 carbon atoms. Examples of low-boiling point HFOs include trifluoropropene, tetrafluoropropenes such as HFO-1234, pentafluoropropenes such as HFO-1225, chlorodifluoropropene, chlorotrifluoropropenes such as HFO-1233, and chlorotetrafluoropropene. More specifically, 3,3,3-trifluoropropene (HFO-1243zf, boiling point: -18°C), trans-1,3,3,3-tetrafluoropropene (HFO-1234ze(E), boiling point: -19°C), cis-1,3,3,3-tetrafluoropropene (HFO-1234ze(Z), boiling point: 10°C), 2,3,3,3-tetrafluoropropene (HFO-1234yf, boiling point: -29°C), 1,1,3,3-tetrafluoropropene (boiling point: 4°C), trans-1,2,3,3,3-tetrafluoropropene (HFO-1234yf, boiling point: -29°C), 1,1,3,3,3-pentafluoropropene (HFO-1225ye(E), boiling point: -10°C), cis-1,2,3,3,3-pentafluoropropene (HFO-1225ye(Z), boiling point: -19°C), 1,1,3,3,3-pentafluoropropene (HFO-1225zc, boiling point: -21°C), 1,1,2,3,3-pentafluoropropene (HFO-1225yc, boiling point: 2°C), trans-1-chloro-3,3,3-trifluoropropene (HFO-1233zd(E), boiling point: 19°C), etc. Among these, HFO-1233zd(E) is preferred. These low-boiling point HFOs may be used alone or in combination of two or more.

[0024] The lower limit of the boiling point of the low-boiling point HFO is not particularly limited, but is preferably 0° C. or higher from the viewpoint of easy handling. Therefore, the low-boiling point HFO according to the present invention preferably has a boiling point of 0 to 30° C. Furthermore, from the viewpoints of suppressing boiling of the polyol composition and achieving good handleability, the boiling point of the low-boiling point HFO is more preferably in the range of 10 to 25° C.

[0025] As described above, the high-boiling point HFO is preferably 1,1,1,4,4,4-hexafluoro-2-butene (HFO-1336mzz, boiling point: 33° C.), and the low-boiling point HFO is preferably trans-1-chloro-3,3,3-trifluoropropene (HFO-1233zd(E), boiling point: 19° C.), with a combination of these being most preferred.

[0026] The mixing ratio (mass ratio) of high-boiling point HFO to low-boiling point HFO is preferably high-boiling point HFO:low-boiling point HFO=10:0 to 1:9, more preferably 8:2 to 2:8, even more preferably 7:3 to 3:7, and particularly preferably 6:4 to 4:6. A high-boiling point HFO alone, or a high ratio of high-boiling point HFO, will provide excellent thermal conductivity, and a high content of low-boiling point HFO will provide suitable foamability.

[0027] The content of the hydrofluoroolefin is preferably 20 to 70 parts by mass, more preferably 25 to 60 parts by mass, and even more preferably 30 to 50 parts by mass, relative to 100 parts by mass of the polyol. When the content of the hydrofluoroolefin is equal to or more than the lower limit, foaming is promoted, the foamability is improved, and the density of the obtained polyurethane foam can be reduced. On the other hand, when the content of the hydrofluoroolefin is equal to or less than the upper limit, excessive foaming can be suppressed.

[0028] The polyol composition of the present invention may also contain a blowing agent other than hydrofluoroolefin. Examples of blowing agents other than hydrofluoroolefin include water, organic physical blowing agents, and inorganic physical blowing agents. Examples of organic physical blowing agents include low-boiling hydrocarbons such as propane, butane, pentane, hexane, heptane, cyclopropane, cyclobutane, cyclopentane, cyclohexane, and cycloheptane, chlorinated aliphatic hydrocarbon compounds such as dichloroethane, propyl chloride, isopropyl chloride, butyl chloride, isobutyl chloride, pentyl chloride, and isopentyl chloride, and ether compounds such as dimethyl ether and diisopropyl ether. Examples of inorganic physical blowing agents include nitrogen gas, oxygen gas, argon gas, and carbon dioxide gas. Among these, water, oxygen gas, and carbon dioxide gas are preferred from the viewpoint of handling, and water is more preferred from the viewpoint of adjusting the isocyanate index and from the viewpoint of ease of handling.

[0029] The content of the blowing agent other than HFO is preferably 0.01 to 25 parts by mass, more preferably 0.1 to 20 parts by mass, and even more preferably 0.5 to 15 parts by mass, based on 100 parts by mass of the polyol. When the content of the blowing agent is equal to or more than the lower limit, foaming is promoted, and the density of the resulting polyurethane foam can be reduced. On the other hand, when the content of the blowing agent is equal to or less than the upper limit, excessive foaming can be suppressed.

[0030] <Catalyst> Metal catalyst (resinized metal catalyst) The catalyst used in the polyol composition of the present invention preferably contains a metal catalyst containing at least one selected from the group consisting of bismuth and tin. This metal catalyst is generally called a resinified metal catalyst. In the present invention, the inclusion of the metal catalyst promotes the reaction between the polyol and the polyisocyanate. In addition, when a certain amount or more of a filler described later is contained, the reactivity of the polyurethane foam is inhibited and the foamability is likely to decrease, but the inclusion of a metal catalyst makes it easier to maintain good foamability of the polyurethane foam. From the viewpoint of foamability, it is more preferable that the metal catalyst contains bismuth.

[0031] The resinified metal catalyst is preferably a metal salt selected from bismuth and tin, more preferably a bismuth salt. The metal salt is preferably an organic acid metal salt, more preferably a metal salt of a carboxylic acid having 5 or more carbon atoms. The carboxylic acid has 5 or more carbon atoms, and thus has good stability against a blowing agent, particularly hydrofluoroolefin. In addition, the number of carbon atoms of the carboxylic acid is preferably 18 or less, more preferably 12 or less, from the viewpoint of catalytic activity. The carboxylic acid is preferably an aliphatic carboxylic acid, more preferably a saturated aliphatic carboxylic acid. The carboxylic acid may be linear or may have a branched structure, but preferably has a branched structure. Specific examples of carboxylic acids include octyl acid, lauric acid, versatic acid, pentanoic acid, and acetic acid, and among these, octyl acid is preferred. That is, the transition metal salt is preferably a metal salt of octyl acid. These carboxylic acids may be linear as described above, but may also have a branched structure. An example of an octyl acid having a branched structure is 2-ethylhexanoic acid. As the metal salt of carboxylic acid, bismuth salt of carboxylic acid and tin salt of carboxylic acid are preferable, and among them, bismuth salt of octylic acid is preferable. In addition, the metal salt of carboxylic acid may be a carboxylate of an alkyl metal. For example, the tin salt of carboxylic acid may be a dialkyltin carboxylate, and preferably is a dioctyltin carboxylate. Specific examples of metal salts of carboxylic acids include bismuth trioctate, dioctyltin versatate, dibutyltin dilaurate, dioctyltin dilaurate, tin dioctylate, etc., and are preferably bismuth trioctate or dioctyltin versatate, and more preferably bismuth trioctate.

[0032] The content of the metal catalyst in the polyol composition is preferably 0.1 to 10 parts by mass, more preferably 1 to 8 parts by mass, even more preferably 1.5 to 6 parts by mass, and even more preferably 2 to 5 parts by mass, relative to 100 parts by mass of the polyol. When the content of the metal catalyst is equal to or more than the lower limit, the curing reaction speed of the foamable polyurethane composition is improved and the foamability is good. On the other hand, when the content of the metal catalyst is equal to or less than the upper limit, the reaction is easily controlled.

[0033] <Imidazole derivatives> The catalyst used in the polyol composition of the present invention preferably contains a resinified amine catalyst, and more preferably contains an imidazole derivative as the resinified amine catalyst. The imidazole derivative is less susceptible to the influence of hydrofluoroolefin, and enhances the stability of the polyol composition while facilitating the reaction between the polyol and the polyisocyanate. Therefore, by containing the imidazole derivative in addition to the above-mentioned metal catalyst, the polyol composition enhances the reactivity between the polyol and the isocyanate, and the foaming property is further improved. The imidazole derivative is preferably an imidazole substituted at the 1- and 2-positions with an alkyl group having 8 or less carbon atoms, and the alkyl group preferably has 6 or less carbon atoms, more preferably has 4 or less carbon atoms. A specific example of a suitable imidazole derivative is represented by the following general formula (1).

[0034] [ka] (In general formula (1), R 1 and R 2each independently represents an alkyl group having 1 to 8 carbon atoms or an alkenyl group having 2 to 8 carbon atoms.

[0035] R in general formula (1) 1 and R 2 each independently represents an alkyl group having 1 to 8 carbon atoms or an alkenyl group having 2 to 8 carbon atoms. The alkyl group and the alkenyl group may each be linear or have a branched structure. Specific examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a pentyl group, a neopentyl group, an isopentyl group, a sec-pentyl group, a hexyl group, a heptyl group, and an octyl group. Specific examples of the alkenyl group include a vinyl group, a 1-propenyl group, an allyl group, an isopropenyl group, a 1-butenyl group, a 2-butenyl group, a pentenyl group, a hexenyl group, a heptenyl group, and an octenyl group. R 1 and R 2 When the number of carbon atoms in the alkyl group or alkenyl group in R is equal to or greater than the lower limit, steric hindrance increases and the copolymer is less susceptible to the effects of blowing agents such as hydrofluoroolefins, which is preferable. 1 and R 2 When the number of carbon atoms in the alkyl group is equal to or less than the upper limit, the steric hindrance is not extremely large, so that the reaction between the polyol and the polyisocyanate can proceed quickly, and the foaming properties are also good. From these perspectives, R 1 and R 2 are each independently preferably an alkyl group having 1 to 6 carbon atoms, more preferably an alkyl group having 1 to 4 carbon atoms, and further preferably a methyl group.

[0036] The imidazole derivative represented by general formula (1) includes 1,2-dimethylimidazole, 1-ethyl-2-methylimidazole, 1-methyl-2-ethylimidazole, 1,2-diethylimidazole, and 1-isobutyl-2-methylimidazole, among which, from the viewpoint of improving the activity of the catalyst in the presence of hydrofluoroolefin and from the viewpoint of rapidly proceeding the reaction, 1,2-dimethylimidazole and 1-isobutyl-2-methylimidazole are preferred.Moreover, from the viewpoint of further increasing stability, 1,2-dimethylimidazole is even more preferred.

[0037] The content of the imidazole derivative in the polyol composition is preferably 0.1 to 30 parts by mass, more preferably 1 to 20 parts by mass, further preferably 2 to 15 parts by mass, and particularly preferably 3 to 10 parts by mass, relative to 100 parts by mass of the polyol. When the content of the imidazole derivative is equal to or more than the lower limit, the formation of a urethane bond is easily caused, the reaction proceeds quickly, and the foaming property is good. On the other hand, when the content of the imidazole derivative is equal to or less than the upper limit, the reaction rate is easily controlled, which is preferable.

[0038] 《Trimerization catalyst》 The polyol composition of the present invention preferably further contains a trimerization catalyst. The trimerization catalyst is a catalyst that reacts the isocyanate groups contained in the polyisocyanate to trimerize them and promote the formation of isocyanurate rings. The inclusion of the trimerization catalyst has the advantage that a good foam can be obtained by completing the reaction of unreacted isocyanate groups. Examples of the trimerization catalyst include metal catalysts and ammonium salts. The metal catalyst (trimerization metal catalyst) used as the trimerization catalyst includes potassium organic acids, and preferably potassium carboxylates having 2 to 8 carbon atoms, such as potassium octylate such as potassium 2-ethylhexanoate, potassium acetate, potassium propionate, potassium butanoate, and potassium benzoate. As the ammonium salt, tertiary ammonium salts such as triethylammonium salts and triphenylammonium salts, and quaternary ammonium salts such as tetramethylammonium salts, tetraethylammonium salts and tetraphenylammonium salts can be used, among which quaternary ammonium salts are preferred. The ammonium salt is, for example, an ammonium salt of a carboxylic acid. As the carboxylic acid in the ammonium salt, for example, a saturated fatty acid having 1 to 10 carbon atoms, preferably 2 to 8 carbon atoms, can be mentioned. The saturated fatty acid may have a hydrocarbon group that is linear or branched, but preferably has a branched group. Specific examples of the carboxylic acid include 2-ethylhexanoic acid, 2,2-dimethylpropanoic acid, acetic acid, and formic acid, among which 2,2-dimethylpropanoic acid is preferred. The trimerization catalyst may be used alone or in combination of two or more kinds. When using two or more kinds in combination, it is preferred to use a quaternary ammonium salt in combination with a metal catalyst.

[0039] The content of the trimerization catalyst in the polyol composition is preferably 0.4 to 30 parts by mass, more preferably 1 to 25 parts by mass, even more preferably 2 to 20 parts by mass, and even more preferably 4 to 18 parts by mass, relative to 100 parts by mass of the polyol. When the content of the trimerization catalyst is equal to or more than the lower limit, there is no significant difference in activity between resinification and trimerization, and foaming can be suppressed from becoming two-stage, resulting in good foamability. On the other hand, when the content of the trimerization catalyst is equal to or less than the upper limit, the resinification reaction proceeds actively, and the activity of trimerization can be promoted by the heat of the resinification reaction, resulting in good foamability and allowing the formation of a good foam.

[0040] <Filler> The polyol composition of the present invention preferably contains a filler. The filler is a solid component contained in the polyol composition, and is generally a component present in the polyol composition in the form of particles or powder. In the present invention, by containing a filler, various physical properties such as flame retardancy and mechanical properties of the resulting polyurethane foam can be easily improved. Furthermore, when the polyol composition contains a filler, it may be stirred to disperse the filler before mixing with the polyisocyanate. When the outside temperature is high, such as in summer, boiling is likely to occur during stirring, but since the polyol composition of the present invention contains a high-boiling point HFO as described above, boiling is unlikely to occur even when stirred before mixing with the isocyanate, and the reaction with the polyisocyanate is easily controlled.

[0041] The filler may be any component that is solid at room temperature (23° C.) and normal pressure (1 atm) and does not dissolve in the polyol composition. From the viewpoint of reducing the water absorption rate of the polyurethane foam, the filler is preferably one that does not have hygroscopicity or deliquescent properties. As the filler, it is preferable to use a solid flame retardant that is solid at room temperature (23°C) and normal pressure (1 atm). The solid flame retardant is preferably at least one selected from red phosphorus-based flame retardants, phosphate-containing flame retardants, bromine-containing flame retardants, boric acid-containing flame retardants, antimony-containing flame retardants, chlorine-containing flame retardants, metal hydroxides, and the like. By using a solid flame retardant as a filler, the flame retardancy of the urethane foam is improved. The solid flame retardants may be used alone or in combination of two or more. In addition, inorganic fillers other than the solid flame retardant may be used as the filler. From the viewpoint of flame retardancy, it is preferable to use the inorganic fillers other than the solid flame retardant in combination with the solid flame retardant, but the inorganic fillers other than the solid flame retardant may be used alone as the filler. Of course, the solid flame retardant may be used alone.

[0042] (Red phosphorus flame retardant) The red phosphorus-based flame retardant used as a filler may be made of red phosphorus alone, may be red phosphorus coated with a resin, a metal hydroxide, a metal oxide, or the like, or may be red phosphorus mixed with a resin, a metal hydroxide, a metal oxide, or the like. The resin that coats the red phosphorus or mixes with the red phosphorus is not particularly limited, but examples thereof include thermosetting resins such as phenol resins, epoxy resins, unsaturated polyester resins, melamine resins, urea resins, aniline resins, and silicone resins. As the compound to be coated or mixed, a metal hydroxide is preferred from the viewpoint of flame retardancy. The metal hydroxide may be appropriately selected from those described below and used.

[0043] (Phosphate-containing flame retardants) Examples of phosphate-containing flame retardants include phosphates consisting of salts of various phosphoric acids and at least one metal or compound selected from metals in Groups IA to IVB of the periodic table, ammonia, aliphatic amines, aromatic amines, and heterocyclic compounds containing nitrogen in the ring. The term "various phosphoric acids" is a concept that includes not only phosphoric acid, but also phosphorous acid, hypophosphorous acid, and the like. Examples of metals in Groups IA to IVB of the periodic table include lithium, sodium, calcium, barium, iron (II), iron (III), and aluminum. Examples of aliphatic amines include methylamine, ethylamine, diethylamine, triethylamine, ethylenediamine, piperazine, etc. Examples of aromatic amines include aniline, o-triidine, 2,4,6-trimethylaniline, anisidine, 3-(trifluoromethyl)aniline, etc. Examples of heterocyclic compounds containing nitrogen in the ring include pyridine, triazine, melamine, etc.

[0044] Specific examples of the phosphate-containing flame retardant include monophosphates, polyphosphates, etc. Examples of the monophosphates include, but are not limited to, ammonium salts such as ammonium phosphate, ammonium dihydrogen phosphate, and diammonium hydrogen phosphate; sodium salts such as monosodium phosphate, disodium phosphate, trisodium phosphate, monosodium phosphite, disodium phosphite, and sodium hypophosphite; potassium salts such as monopotassium phosphate, dipotassium phosphate, tripotassium phosphate, monopotassium phosphite, dipotassium phosphite, and potassium hypophosphite; lithium salts such as monolithium phosphate, dilithium phosphate, trilithium phosphate, monolithium phosphite, dilithium phosphite, and lithium hypophosphite; barium salts such as barium dihydrogen phosphate, barium hydrogen phosphate, tribarium phosphate, and barium hypophosphite; magnesium salts such as monohydrogen magnesium phosphate, magnesium hydrogen phosphate, trimagnesium phosphate, and magnesium hypophosphite; calcium salts such as calcium dihydrogen phosphate, calcium hydrogen phosphate, tricalcium phosphate, and calcium hypophosphite; and zinc salts such as zinc phosphate, zinc phosphite, and zinc hypophosphite. Here, the polyphosphate is not particularly limited, but examples thereof include ammonium polyphosphate, piperazine polyphosphate, melamine polyphosphate, ammonium amide polyphosphate, and aluminum polyphosphate. The phosphate-containing flame retardants may be used alone or in combination of two or more of the above-mentioned compounds.

[0045] (Bromine-containing flame retardants) The bromine-containing flame retardant is not particularly limited as long as it contains bromine in its molecular structure and is a solid at room temperature (23°C) and normal pressure (1 atm), and examples thereof include brominated aromatic ring-containing aromatic compounds. Examples of the brominated aromatic ring-containing aromatic compound include monomeric organic bromine compounds such as hexabromobenzene, pentabromotoluene, hexabromobiphenyl, decabromobiphenyl, decabromodiphenyl ether, octabromodiphenyl ether, hexabromodiphenyl ether, bis(pentabromophenoxy)ethane, ethylene bis(pentabromophenyl), ethylene bis(tetrabromophthalimide), and tetrabromobisphenol A.

[0046] In addition, the brominated aromatic ring-containing aromatic compound may be a bromine compound polymer.Specific examples include brominated polycarbonates such as polycarbonate oligomers produced from brominated bisphenol A as a raw material, copolymers of this polycarbonate oligomer and bisphenol A, and diepoxy compounds produced by the reaction of brominated bisphenol A and epichlorohydrin.Furthermore, examples include brominated epoxy compounds such as monoepoxy compounds obtained by the reaction of brominated phenols and epichlorohydrin, brominated phenol condensates of brominated polyphenylene ether, brominated bisphenol A and cyanuric chloride, and uncrosslinked or crosslinked brominated polystyrene. In addition, compounds other than brominated aromatic ring-containing aromatic compounds such as hexabromocyclododecane may also be used. These bromine-containing flame retardants may be used alone or in combination of two or more.

[0047] (Boron-containing flame retardants) The boron-containing flame retardant used in the present invention includes borax, boron oxide, boric acid, borate, etc. Examples of boron oxide include diboron trioxide, boron trioxide, diboron dioxide, tetraboron trioxide, and tetraboron pentoxide. Examples of borates include borates of alkali metals, alkaline earth metals, elements of Groups 4, 12, and 13 of the periodic table, and ammonium. Specific examples include alkali metal borates such as lithium borate, sodium borate, potassium borate, and cesium borate, alkaline earth metal borates such as magnesium borate, calcium borate, and barium borate, zirconium borate, zinc borate, aluminum borate, and ammonium borate. The boron-containing flame retardants may be used alone or in combination of two or more kinds. The boron-containing flame retardant used in the present invention is preferably a borate, more preferably zinc borate.

[0048] (Antimony-containing flame retardants) Examples of antimony-containing flame retardants include antimony oxide, antimony salts, and pyroantimony salts. Examples of antimony oxide include antimony trioxide and antimony pentoxide. Examples of antimony salts include sodium antimonate and potassium antimonate. Examples of pyroantimonate include sodium pyroantimonate and potassium pyroantimonate. The antimony-containing flame retardant may be used alone or in combination of two or more kinds. The antimony-containing flame retardant used in the present invention is preferably antimony oxide.

[0049] <Chlorine-containing flame retardants> Chlorine-containing flame retardants include those commonly used in polyurethane foams, such as polychlorinated naphthalenes, chlorendic acid, and dodecachlorododecahydrodimethanodibenzocyclooctene, sold under the trade name "Dechlorane Plus."

[0050] (metal hydroxide) Examples of the metal hydroxides used in the present invention include magnesium hydroxide, calcium hydroxide, aluminum hydroxide, iron hydroxide, nickel hydroxide, zirconium hydroxide, titanium hydroxide, zinc hydroxide, copper hydroxide, vanadium hydroxide, and tin hydroxide. The metal hydroxides may be used alone or in combination of two or more. As the metal hydroxide, aluminum hydroxide is preferred.

[0051] (Needle filler) Examples of needle-like fillers include potassium titanate whiskers, aluminum borate whiskers, magnesium-containing whiskers, silicon-containing whiskers, wollastonite, sepiolite, zonolite, elestadite, boehmite, rod-shaped hydroxyapatite, glass fibers, carbon fibers, graphite fibers, metal fibers, slag fibers, gypsum fibers, silica fibers, alumina fibers, silica alumina fibers, zirconia fibers, boron nitride fibers, boron fibers, and stainless steel fibers. These needle-like fillers can be used alone or in combination of two or more. The aspect ratio (length / diameter) of the needle-like filler used in the present invention is preferably in the range of 5 to 50, and more preferably in the range of 10 to 40. The aspect ratio can be determined by observing the needle-like filler with a scanning electron microscope and measuring its length and width.

[0052] As the filler, inorganic fillers other than the flame retardants described above may be used. As such inorganic fillers, alumina, titanium oxide, calcium oxide, magnesium oxide, iron oxide, tin oxide, ferrites, basic magnesium carbonate, calcium carbonate, magnesium carbonate, zinc carbonate, barium carbonate, dawsonite, hydrotalcite, calcium sulfate, barium sulfate, calcium silicate, talc, mica, montmorillonite, bentonite, activated clay, imogolite, sericite, glass beads, aluminum nitride, boron nitride, silicon nitride, various metal powders, magnesium sulfate, lead zirconate titanate, molybdenum sulfide, silicon carbide, various magnetic powders, fly ash, etc. may be appropriately used. These inorganic fillers may be used alone or in combination of two or more. These fillers may be used alone or in combination of two or more kinds.

[0053] The content of the filler in the polyol composition is, for example, preferably 10 parts by mass or more, more preferably 30 parts by mass or more, even more preferably 40 parts by mass or more, and particularly preferably 50 parts by mass or more, relative to 100 parts by mass of the polyol. By making the content of the filler equal to or more than the above lower limit, it becomes easier to impart various properties such as flame retardancy to the polyurethane foam. In addition, the content of the filler is preferably 120 parts by mass or less, more preferably 100 parts by mass or less, even more preferably 100 parts by mass or less, and particularly preferably 90 parts by mass or less, relative to 100 parts by mass of the polyol. By making the content of the filler equal to or less than these upper limits, it becomes easier to obtain good foamability without decreasing reactivity.

[0054] <Phosphate ester> The polyol composition of the present invention may contain a flame retardant other than the solid flame retardant described above. Such flame retardants include flame retardants that are liquid at room temperature (23°C) and normal pressure (1 atm), specifically, phosphate esters. By using the phosphate ester, it becomes easier to improve the flame retardancy of the urethane foam without decreasing the fluidity of the polyol composition.

[0055] As the phosphate ester, monophosphate ester, condensed phosphate ester, etc. can be used. The monophosphate ester is a phosphate ester having one phosphorus atom in the molecule. Examples of the monophosphate ester include trialkyl phosphates such as trimethyl phosphate, triethyl phosphate, tributyl phosphate, and tri(2-ethylhexyl)phosphate, halogen-containing phosphate esters such as tris(β-chloropropyl)phosphate, trialkoxy phosphates such as tributoxyethyl phosphate, aromatic ring-containing phosphate esters such as tricresyl phosphate, trixylenyl phosphate, tris(isopropylphenyl)phosphate, cresyl diphenyl phosphate, and diphenyl(2-ethylhexyl)phosphate, and acidic phosphate esters such as monoisodecyl phosphate and diisodecyl phosphate.

[0056] Examples of the condensed phosphate ester include aromatic condensed phosphate esters such as trialkyl polyphosphate, resorcinol polyphenyl phosphate, bisphenol A polycresyl phosphate, and bisphenol A polyphenyl phosphate. Commercially available condensed phosphate esters include, for example, "CR-733S", "CR-741", and "CR747" manufactured by Daihachi Chemical Industry Co., Ltd., and "ADEKA STAB PFR" and "FP-600" manufactured by ADEKA Corporation.

[0057] The phosphoric acid ester may be used alone or in combination of two or more of the above-mentioned. Among them, from the viewpoint of easily adjusting the viscosity of the polyol composition to an appropriate value and from the viewpoint of improving the flame retardancy of the polyurethane foam, monophosphate ester is preferred, and halogen-containing phosphoric acid ester such as tris(β-chloropropyl)phosphate is more preferred. The content of the phosphoric acid ester in the polyol composition is preferably from 5 to 100 parts by mass, more preferably from 12 to 90 parts by mass, further preferably from 20 to 75 parts by mass, and even further preferably from 30 to 60 parts by mass, relative to 100 parts by mass of the polyol.

[0058] <Foam stabilizer> The polyol composition of the present invention may contain a foam stabilizer. By containing a foam stabilizer, the foamability of the polyurethane foam can be improved, and for example, foaming can be promoted when reacting with a polyisocyanate during spraying. The foam stabilizer may be specifically a surfactant, more specifically a nonionic surfactant, a cationic surfactant, an anionic surfactant, etc. Specific examples of nonionic surfactants include polyoxyalkylene foam stabilizers such as polyoxyalkylene alkyl ethers, silicone foam stabilizers such as organopolysiloxanes, etc. The foam stabilizer used in the present invention is not particularly limited, but silicone foam stabilizers are preferred from the viewpoint of foaming properties. The foam stabilizer may be used alone or in combination of two or more kinds.

[0059] The content of the foam stabilizer in the polyol composition of the present invention is preferably 0.1 to 12 parts by mass, more preferably 1 to 10 parts by mass, and even more preferably 2 to 8 parts by mass, based on 100 parts by mass of the polyol. When the content of the foam stabilizer is equal to or more than the lower limit, the mixture of the polyol composition and the polyisocyanate is easily foamed, so that a homogeneous polyurethane foam can be obtained. When the content of the foam stabilizer is equal to or less than the upper limit, the balance between the production cost and the obtained effect is optimal.

[0060] <Other ingredients> The polyol composition may contain, as necessary, one or more selected from additives such as phenol-based, amine-based, and sulfur-based antioxidants, heat stabilizers, metal inhibitors (metal deactivators), antistatic agents, stabilizers, crosslinking agents, lubricants, softeners, pigments, and tackifying resins, tackifiers such as polybutene and petroleum resins, etc., within the scope of the present invention.

[0061] <Method of producing polyol composition> The method for producing the polyol composition of the present invention is not particularly limited, and the composition can be produced, for example, by stirring each component at about 20 to 40° C. for about 30 seconds to 20 minutes using a homodisper or the like.

[0062] [Foamable polyurethane composition and polyurethane foam] The foamable polyurethane composition of the present invention contains the above-mentioned polyol composition and a polyisocyanate, and is obtained by mixing them. The polyurethane foam of the present invention is a reaction product obtained by reacting and foaming the foamable polyurethane composition.

[0063] <Polyisocyanate> Examples of the polyisocyanate include aromatic polyisocyanates, alicyclic polyisocyanates, and aliphatic polyisocyanates. Examples of aromatic polyisocyanates include phenylene diisocyanate, tolylene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate, dimethyldiphenylmethane diisocyanate, triphenylmethane triisocyanate, naphthalene diisocyanate, and polymethylene polyphenyl polyisocyanate (polymeric MDI).

[0064] Examples of the alicyclic polyisocyanate include cyclohexylene diisocyanate, methylcyclohexylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, and dimethyldicyclohexylmethane diisocyanate.

[0065] Examples of the aliphatic polyisocyanate include methylene diisocyanate, ethylene diisocyanate, propylene diisocyanate, tetramethylene diisocyanate, and hexamethylene diisocyanate.

[0066] Among these, from the viewpoints of ease of use and availability, aromatic polyisocyanates are preferred, and diphenylmethane diisocyanate, polymeric MDI, or a mixture thereof is more preferred. The polyisocyanates may be used alone or in combination of two or more. Furthermore, the polyisocyanate may be appropriately mixed with known additives that are mixed with polyisocyanates before being mixed with the polyol composition.

[0067] The polyol composition and the polyisocyanate mixed in the polyol composition preferably have substantially the same volume. Specifically, the volume ratio of the polyisocyanate to the polyol composition is preferably 0.8 to 1.2, more preferably 0.9 to 1.1, and further preferably 0.95 to 1.05.

[0068] The content of the filler in the foamable polyurethane composition is, for example, 4 parts by mass or more, preferably 6 parts by mass or more, more preferably 8 parts by mass or more, and even more preferably 10 parts by mass or more, relative to 100 parts by mass of the urethane resin. By making the content of the filler in the foamable polyurethane composition equal to or more than the above lower limit, the proportion of the filler in the polyurethane foam becomes sufficient, the water absorption rate of the polyurethane foam can be reduced, and hydrolysis can be suppressed well. In addition, the content of the filler is preferably 30 parts by mass or less, more preferably 25 parts by mass or less, and even more preferably 20 parts by mass or less, relative to 100 parts by mass of the urethane resin. By making it equal to or less than these upper limits, it becomes easier to obtain a polyurethane foam having good foamability. The urethane resin means the total amount of the polyol and polyisocyanate blended in the foamable polyurethane composition.

[0069] <Isocyanate Index> The isocyanate index in the foamable polyurethane composition of the present invention is not particularly limited, but is preferably 200 or more. If the isocyanate index is equal to or more than the lower limit, the amount of polyisocyanate relative to the polyol becomes excessive, and isocyanurate bonds due to the trimerization of the polyisocyanate are easily formed, resulting in improved flame retardancy of the polyurethane foam. It is also possible to impart non-flammability. Furthermore, if the isocyanate index is equal to or more than the lower limit, it is easy to produce a polyurethane foam having sufficient isocyanurate bonds, that is, a polyurethane foam having both flame retardancy and heat insulation at a high level, in combination with the use of the various catalysts described above. From these viewpoints, the isocyanate index is more preferably 250 or more, more preferably 300 or more, even more preferably 350 or more, and particularly preferably 400 or more. The isocyanate index is preferably not more than 1,000, more preferably not more than 800, and even more preferably not more than 600. When the isocyanate index is not more than the upper limit, flame retardancy that is sufficiently commensurate with the production costs can be obtained.

[0070] The isocyanate index can be calculated by the following method. Isocyanate Index = equivalents of polyisocyanate ÷ (equivalents of polyol + equivalents of water) × 100 Here, each equivalent number can be calculated as follows: Equivalent number of polyisocyanate = Amount of polyisocyanate used (g) × NCO content (mass%) / Molecular weight of NCO (mol) × 100 Equivalent weight of polyol = OHV × amount of polyol used (g) ÷ molecular weight of KOH (mmol) OHV is the hydroxyl value of the polyol (mg KOH / g). Equivalents of water = amount of water used (g) / molecular weight of water (mol) × number of OH groups in water In the above formulas, the molecular weight of NCO is 42 (mol), the molecular weight of KOH is 56,100 (mmol), the molecular weight of water is 18 (mol), and the number of OH groups in water is 2.

[0071] <Method of manufacturing polyurethane foam> Although there is no particular limitation on the method for producing the polyurethane foam, it is preferable to produce the polyurethane foam by mixing the polyol composition with the polyisocyanate in a foaming machine or the like, and reacting and foaming the resulting mixed liquid (foamable polyurethane composition). As the foaming machine, it is preferable to use a spray device having a spray gun or the like. The polyol composition is preferably fed to a foaming machine and mixed by collision inside the foaming machine with a polyisocyanate fed from another container, etc. Then, the mixed liquid (foamable polyurethane composition) is preferably discharged from a discharge port of a spray gun, etc., and a polyurethane foam is formed from the discharged foamable polyurethane composition.

[0072] In the present production method, the polyol composition contains a high-boiling point HFO, so that even when the outside temperature is high (e.g., about 30 to 40°C), such as in summer, boiling does not occur before mixing with the polyisocyanate, making it easier to control the reaction with the polyisocyanate. The polyol composition may be stirred before mixing with the polyisocyanate in order to disperse ingredients such as fillers. Stirring the polyol composition makes it more likely to boil, but since the present invention contains a high-boiling point HFO, boiling during stirring can also be suppressed.

[0073] The method of stirring the polyol composition is not particularly limited as long as the compound such as the filler can be dispersed in the polyol composition, but it may be carried out by using a stirrer or by shaking the container, but it is preferable to use a stirrer. The stirrer is preferably equipped with a stirring blade, and the stirring blade is placed in the polyol composition and rotated to stir the polyol composition. More specifically, the agitator may be one that has a shaft and an agitator blade attached to the shaft and rotates around the shaft, and such an agitator can be inserted into a container such as a drum through its opening to place the agitator blade in the polyol composition. As the agitator, for example, a commercially available drum mixer may be used. The polyol composition is stirred depending on the stirring method, but as described above, when stirring is performed using a stirrer, it is advisable to stir the polyol composition after opening the container.

[0074] The present manufacturing method can be applied to, for example, spraying applications. Therefore, the mixed liquid discharged from the foaming machine is sprayed onto a target surface at a certain discharge pressure, and foamed to form a polyurethane foam on the target surface. In the present invention, the polyurethane foam may be obtained by mixing the polyisocyanate and the polyol composition, pouring the mixture into a container such as a mold or a frame, and curing the mixture.

[0075] <Applications of polyurethane foam> The uses of the polyurethane foam of the present invention are not particularly limited, but since it has excellent flame retardancy and heat insulation, it can be suitably used for the walls, ceilings, roofs, floors, etc. of buildings, and it is advisable to mold the polyurethane foam onto the target surfaces such as walls, ceilings, roofs, floors, etc. It can also be suitably used as a member for filling any openings that occur in buildings, including joints and holes that occur between structural materials of buildings. EXAMPLES

[0076] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these. [Materials used] <Polyol composition> [Polyol] p-Phthalic acid polyester polyol (Kawasaki Chemical Industries, Ltd., product name: Maximol RLK-087, hydroxyl value = 200 mg KOH / g)

[0077] 〔catalyst〕 Resinized amine catalyst, 1,2-dimethylimidazole (manufactured by Tosoh Corporation, product name: TOYOCAT (registered trademark)-DM70) concentration 65 to 75% by mass Resinized metal catalyst, bismuth trioctate (manufactured by Nitto Kasei, product name: Neostan U-600) concentration 55-58% by mass Resinized metal catalyst, dioctyltin versatate (manufactured by Nitto Kasei, product name: Neostan U-830) concentration: approx. 99% by mass Ammonium salt (trimerization catalyst), tetramethylammonium salt of 2,2-dimethylpropanoic acid (Air Products, product name: DABCO (registered trademark) TMR7) concentration 45 to 55 mass% Metal catalyst (trimerization catalyst), potassium 2-ethylhexanoate (manufactured by Air Products, product name: DABCO (registered trademark) K-15) concentration 70 to 80% by mass

[0078] [Foaming Agent] High boiling point hydrofluoroolefin (high boiling point HFO, manufactured by Mitsui Chemours Fluoroproducts Co., Ltd., product name: Formacel 1100, 1,1,1,4,4,4-hexafluoro-2-butene, boiling point 34°C) Low boiling point hydrofluoroolefin (low boiling point HFO, manufactured by Honeywell Japan, product name: Soltis LBA, trans-1-chloro-3,3,3-trifluoropropene, boiling point 19°C) ·water

[0079] [Flame retardant] Tris(β-chloropropyl)phosphate (manufactured by Daihachi Chemical Industry Co., Ltd., product name: TMCPP)

[0080] [Filler] Wollastonite (SiO 2 CaO) (Kinseimatec Co., Ltd., product name: SH-1250)

[0081] <Polyisocyanate> 4,4'-Diphenylmethane diisocyanate (4,4'-MDI) (manufactured by Manka Chemical Japan Co., Ltd., product name: PM200)

[0082] [Evaluation method] 1. Boiling The small opening of the drum in which the polyol composition was stored was opened, and a drum mixer ("Air-driven mixer for drums with three-stage blades, product number: NUE035B-1" manufactured by Japan Urethane Engineering Co., Ltd.) was set in the drum. Thereafter, the large opening of the drum was opened, and the drum was stirred for 30 minutes with the drum mixer, and the contents were visually observed to see whether they boiled up and overflowed from the large opening. The evaluation criteria were as follows: 〇: No overflow ×: Overflowing

[0083] 2.Heat Conduction The polyol composition and the polyisocyanate were reacted and foamed to prepare a polyurethane foam on the substrate. The polyurethane foam was peeled off from the substrate and cut to 20 cm x 20 cm x 5 mm (thickness), and the thermal conductivity was measured according to JIS-A-9526 using a thermal conductivity measuring device ("HC-074" manufactured by Eiko Seiki Co., Ltd.). The evaluation criteria were as follows. ◎: Less than 0.022W / mK ○: 0.022~0.026W / mK ×: More than 0.026W / mK

[0084] 3. Activity The polyol composition and the polyisocyanate were sprayed on a substrate (gypsum board) using a sprayer under the following conditions so that the urethane foam thickness was 1 mm or less, and the surface curing time (tack-free time) after spraying was measured. 1 The evaluation criteria were as follows: ◎:t 1 Less than 27 seconds 〇:t 1 Between 27 and 30 seconds ×:t 1 exceeds 30 seconds <Condition> Spray machine: Graco H-25 spray machine Settings (heater and pressure settings) Isocyanate heater: 38℃ Premix heater (for heating polyol composition): 38℃ Hose heater (for heating isocyanate and polyol composition before mixing): 38℃ Pressure: Adjust so that the mist becomes a wide circular shape. Base material: gypsum board (thickness 12.5 mm) ·Substrate temperature: 0℃±1℃ ·Environmental temperature: 0℃±1℃

[0085] Examples 1 to 12 and Comparative Examples 1 to 3 A polyol composition was prepared by mixing each component according to the formulation shown in Table 1. The polyol composition was placed in a drum and stored at 32° C. for 24 hours. Evaluation was performed according to Evaluation Method 1 described above. In addition, the polyol compositions and polyisocyanates shown in Table 1 were used to perform the evaluations according to the above evaluation methods 2 and 3. The results are shown in Table 1.

[0086] [Table 1]

[0087] As is clear from the results of the above examples and comparative examples, the polyol composition of the present invention containing a high-boiling point HFO as a blowing agent can suppress boiling, and also shows excellent effects in the evaluation of thermal conductivity. On the other hand, all polyol compositions not containing a high-boiling point HFO caused boiling. It can be seen that the content of water as a blowing agent has no effect on boiling, and the presence or absence of boiling is determined by whether or not the polyol composition contains a high-boiling point HFO. In terms of thermal conductivity, the high-boiling-point HFO alone, without the low-boiling-point HFO, shows better results, but in terms of activity evaluation, a mixture of high-boiling-point HFO and low-boiling-point HFO gives a higher rating.

Claims

1. A foamable polyurethane composition for spray application, comprising a polyol composition and a polyisocyanate, for forming a urethane foam by spraying onto a target surface of a building, comprising: The polyol composition comprises a polyol, a blowing agent, a filler, and a catalyst; the catalyst comprises a quaternary ammonium salt, a metal catalyst containing at least one selected from the group consisting of bismuth and tin, an imidazole derivative, and a potassium organic acid; A foamable polyurethane composition for spray application, characterized in that the foaming agent contains a hydrofluoroolefin having a boiling point of 30°C or higher and a hydrofluoroolefin having a boiling point of less than 30°C (excluding those containing an acrylic surface conditioner).

2. 2. The foamable polyurethane composition for spray application according to claim 1, wherein said hydrofluoroolefin having a boiling point of 30° C. or higher is 1,1,1,4,4,4-hexafluoro-2-butene.

3. 3. The foamable polyurethane composition for spray application according to claim 1, wherein the hydrofluoroolefin having a boiling point of less than 30° C. is trans-1-chloro-3,3,3-trifluoropropene.

4. The foamable polyurethane composition for spray application according to any one of claims 1 to 3, which has an isocyanate index of 200 or more.

5. A polyurethane foam obtained by reacting and foaming the foamable polyurethane composition for spray application according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Mixture containing 1,1,1,3,3,3-hexafluorobutene and 1-chloro-3,3,3-trifluoropropene

    JP2012140592A

  • Blowing agents, foamable compositions and foams

    JP2016145360A

  • Azeotrope-like compositions including cis-1-chloro-3,3,3-trifluoropropene

    JP2018021199A

  • Curable composition and polyurethane foam

    JP2019019302A

  • Urethane resin composition and thermal insulation method of architectural structure

    JP2020033461A