Polyurethane foam

A polyurethane foam with a high closed cell ratio and cell membrane pores addresses dimensional instability and flame retardance issues, ensuring effective insulation and fire resistance.

JP7579087B2Active Publication Date: 2024-11-07SEKISUI CHEMICAL CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2020142903
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-26
Publication Date
2024-11-07
Estimated Expiration
2040-08-26

AI Technical Summary

Technical Problem

Polyurethane foams with high closed cell ratios for improved insulation are prone to dimensional deformation due to temperature changes, leading to positional displacement and reduced flame retardance, and increasing density compromises handling and productivity.

Method used

A polyurethane foam with a closed cell ratio of 80% or more, featuring pores in at least a portion of the cell membranes, formed using a foamable urethane resin composition containing polyol, polyisocyanate, flame retardant, blowing agent, and catalyst, with optional cell openers and hydrofluoroolefin blowing agents.

Benefits of technology

The foam achieves excellent heat insulation, resistance to dimensional deformation, and effective flame retardance, preventing fire spread with controlled steel ball sinking and melting distances.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579087000003
    Figure 0007579087000003
  • Figure 0007579087000004
    Figure 0007579087000004
  • Figure 0007579087000001
    Figure 0007579087000001
Patent Text Reader

Abstract

To provide a polyurethane foam that has superior heat insulation performance and resists dimensional deformation.SOLUTION: A polyurethane foam has a plurality of cells. The closed-cell ratio is 80% or more. Each cell has a cell film including, at least partially, holes therein.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to polyurethane foams. [Background technology]

[0002] 2. Description of the Related Art Polyurethane foams, taking advantage of their excellent heat insulating properties, are used in practical applications for insulating and preventing condensation on ceilings, roofs, walls, and the like of buildings such as apartment complexes, detached houses, and commercial buildings. In polyurethane foam, heat insulation is one of the important physical properties, and various attempts have been made to improve heat insulation. For example, Patent Document 1 discloses an invention relating to a polyurethane foam (polyurethane foam) that is foamed with carbon dioxide gas, contains 0.2 to 7.0% by weight of one or more high-boiling compounds selected from cyclic carbonate esters and fatty acid esters, has a bubble size of 0.1 to 0.5 mm, and has a closed cell ratio of 90% or more. It is known that polyurethane foam with a closed cell ratio of a certain level or more has excellent heat insulation performance because the gas in the bubbles is less likely to be replaced by air. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2000-230066 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, when the closed cell ratio is increased to improve the heat insulating performance, the foam shape is easily changed by the change in the ambient temperature, and for example, the dimensions of the polyurethane foam are easily deformed at high temperatures such as during a fire, which may cause the polyurethane foam to shift from its designated position, or cause physical properties such as flame retardancy to deteriorate due to the position shift. There is also a problem that the foam is prone to dimensional changes such as shrinkage even at room temperature. One way to solve this problem is to increase the density of the foam, but this poses problems in terms of handling and productivity. Therefore, an object of the present invention is to provide a polyurethane foam which has excellent heat insulating performance, is relatively lightweight, and is resistant to dimensional deformation. [Means for solving the problem]

[0005] As a result of extensive research, the present inventors have found that the above-mentioned problems can be solved by a polyurethane foam having a certain level of closed cell ratio or more and in which pores are formed in at least parts of the cell membranes of the cells, and have thus completed the present invention. That is, the present invention provides the following [1] to [8]. [1] A polyurethane foam having a plurality of cells, the polyurethane foam having a closed cell ratio of 80% or more, and having holes formed in at least a portion of the cell membrane of the cells. [2] The polyurethane foam according to [1] above, which is formed from a foamable urethane resin composition comprising a polyol compound, a polyisocyanate compound, a flame retardant, a foaming agent, and a catalyst. [3] The polyurethane foam according to [2] above, wherein the foamable urethane resin composition contains a cell opener comprising at least one fine particle component selected from organic fine particles and inorganic fine particles. [4] The polyurethane foam according to [2] or [3] above, wherein the blowing agent comprises a hydrofluoroolefin. [5] Radiant heat intensity of 50kW / m2, in accordance with the ISO-5660 test method 2 When heated for 5 minutes, the total heat generated is 8MJ / m 2 The polyurethane foam according to any one of the above [1] to [4], which is: [6] Radiant heat intensity of 50kW / m2, according to the ISO-5660 test method. 2 The maximum heat generation rate when heated for 5 minutes is 200kW / m 2 The polyurethane foam according to any one of the above [1] to [5], which is: [7] The polyurethane foam according to any one of [1] to [6] above, wherein the sinking distance of a steel ball in the hot steel ball evaluation described below is 10 mm or less. (Hot steel ball evaluation) (1) Cut the polyurethane foam into a cube with sides of 50 mm to use as a test specimen. (2) Place a steel ball with a diameter of 10.0 mm and a weight of 4.15 g inside an electric furnace set to 800°C and heat it for more than 10 minutes. (3) In an atmosphere of 23°C, the steel ball heated in (2) above is immediately placed on the center of the upper part of the test piece in (1) above and left there until the steel ball has completely sunk in. Then, the cross section of the sufficiently cooled test piece is cut and the sinking distance of the steel ball and the fusion diameter distance are measured. [8] The polyurethane foam according to any one of the above [1] to [7], which is formed by spraying a foamable urethane resin composition comprising a polyol compound, a polyisocyanate compound, a flame retardant, a foaming agent, and a catalyst. Effect of the Invention

[0006] According to the present invention, it is possible to provide a polyurethane foam that has excellent heat insulating properties, is relatively lightweight, and is resistant to dimensional deformation. [Brief description of the drawings]

[0007] [Figure 1] 1 is a scanning electron microscope photograph of a polyurethane foam of the present invention having pores formed in some of the cell membranes. [Diagram 2] 1 is a scanning electron microscope photograph of a polyurethane foam in which no holes are formed in the cell membrane. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] [Polyurethane foam] The polyurethane foam of the present invention has a plurality of cells, has a closed cell ratio of 80% or more, and has pores formed in at least some of the cell membranes of the cells.

[0009] (Closed bubble rate) The polyurethane foam of the present invention has a closed cell ratio of 80% or more. If the closed cell ratio of the polyurethane foam is less than 80%, the thermal conductivity increases and the heat insulation decreases. From the viewpoint of improving the heat insulation, the closed cell ratio of the polyurethane foam is preferably 85% or more, more preferably 90% or more. The closed cell ratio means the ratio of the closed cells to the total cells. The closed cell ratio can be adjusted by adjusting the composition of the foamable urethane resin composition described below. For example, it can be adjusted by the type and amount of a foam stabilizer described below, a cell opener which is a fine solid particle, the molecular weight and number of functional groups of the polyol, a combination of different polyols, the type and amount of the catalyst, etc.

[0010] The closed cell ratio of a polyurethane foam is calculated from the open cell ratio by measuring the true density using a dry density measurement method using a constant volume expansion method and then calculating the open cell ratio using the following formula (1). Open cell rate (%) = {(true density [g / cm 3 ])-(Apparent density [g / cm 3 ])} / (true density[g / cm 3 ])×100 (1) Closed cell ratio (%) = 100 - open cell ratio calculated from formula (1) (2) For information on dry density measurement, please refer to the Shimadzu Corporation website (https: / / www.an.shimadzu.co.jp / powder / lecture / middle / m04.htm).

[0011] (pores in cell membrane) The polyurethane foam of the present invention has a plurality of cells, and pores are formed in at least a part of the cell membrane of the cells. The presence of pores in at least a part of the cell membrane improves the dimensional stability of the polyurethane foam at high temperatures and at room temperature. The pores formed in the cell membrane are confirmed by observation with a scanning electron microscope. Fig. 1 shows a photograph of the surface of the polyurethane foam of the present invention observed using a scanning electron microscope. In the photograph, a plurality of cells (11a to 11f) are confirmed. Each cell has an internal gas and a cell membrane that covers the internal gas, and in Fig. 1, the cell membrane of each cell is observed. The cell membrane is made of polyurethane. A hole 12a is observed in the cell membrane of cell 11a, a hole 12b in the cell membrane of cell 11b, and a hole 12f in the cell membrane of cell 11f. For example, when exposed to high temperatures by heating or the like, if no holes are formed, the internal gas is isolated from the outside of the system by the cell membrane and is likely to expand and deform, but when holes are formed in part of the cell membrane as in the present invention, the cells are partially connected to the outside of the system, thereby ensuring an escape route for the gas, which is thought to increase the dimensional stability of the polyurethane foam at high temperatures. It is also thought that the dimensional stability at room temperature is also increased for the same reason. The black region observed between cell 11a and cell 11d is a region 13 that was generated during sample preparation, specifically, when the cell was partially cut during sample preparation for scanning electron microscope observation. Therefore, region 13 is different from the hole in the present invention. In contrast, the hole confirmed on the cell membrane is determined to be a hole that was present before the sample was prepared.

[0012] It is not necessary that holes are formed in all of the cell membranes of the multiple cells, as long as holes are formed in a part of the cell membranes in the foam. The average pore size is not particularly limited, but is preferably 1 to 100 μm, more preferably 2 to 60 μm, and even more preferably 3 to 40 μm. The average pore size may be calculated, for example, as the average value of 10 pore sizes among the pores observed with a scanning electron microscope. The pore size is the maximum distance between any two points on the contour line of the pores observed with a scanning electron microscope.

[0013] The number of holes is not particularly limited, but is 1 mm 2The number of pores per unit area is preferably 1 to 100, and more preferably 2 to 50. When the number of pores is equal to or more than these lower limits, dimensional changes of the polyurethane foam at high temperatures and at room temperature are easily suppressed, and when the number of pores is equal to or less than these upper limits (or the pores are in a state of being coalesced and enlarged), the heat insulating properties are less likely to decrease. The method for forming pores in the cell membrane of a polyurethane foam is not particularly limited, but examples include increasing the heat of internal reaction by adjusting a catalyst, delaying the curing of the resin, using a cell opener containing a fine particle component (organic fine particles, inorganic fine particles), etc., and combining a long-chain polyol and a short-chain polyol.

[0014] In the polyurethane foam of the present invention, the sinking distance of a steel ball in the hot steel ball evaluation described below is 10 mm or less. (Hot steel ball evaluation) (1) Cut the polyurethane foam into a cube with sides of 50 mm to use as a test specimen. (2) A steel ball having a diameter of 10.0 mm and a weight of 4.15 g is placed inside an electric furnace with the temperature inside the furnace set to 800°C and heated for more than 10 minutes. (3) In an atmosphere of 23°C, the steel ball heated in (2) above is immediately placed on the center of the upper part of the test piece in (1) above and left there until the steel ball has completely sunk in. Then, the cross section of the sufficiently cooled test piece is cut and the sinking distance of the steel ball and the fusion diameter distance are measured. In this hot steel ball evaluation, a small programmable electric furnace (MMF-1) with furnace inner dimensions of 120mm x 150mm x 100mm was used as the electric furnace in (2) above, and SUS304 steel balls were used. After the steel balls were heated, they were immediately placed on the test specimen. Therefore, the temperature inside the electric furnace (800°C) can be considered to be the temperature of the steel balls when they were placed on the test specimen.

[0015] In the above hot steel ball evaluation, as long as the diameter and weight of the steel ball are within the range of 10.0±0.2 mm, 4.15±0.3 g, and the temperature inside the electric furnace is within the range of 795 to 805°C, and the other conditions are as described above, an equivalent hot steel ball evaluation will be obtained, so the evaluation may be performed within these ranges of diameter, weight, and temperature inside the electric furnace.

[0016] By setting the steel ball sinking distance in the hot steel ball evaluation of the polyurethane foam of the present invention within the above-mentioned predetermined range, the polyurethane foam can be made less susceptible to fire spread when exposed to fire or the like.

[0017] The polyurethane foam of the present invention preferably has a steel ball sinking distance of 10 mm or less in a hot steel ball test. If the steel ball sinking distance is 10 mm or less, the polyurethane foam is less likely to spread fire when exposed to a fire or the like, and the spread of fire can be effectively prevented. From the viewpoint of effectively preventing the spread of fire, the steel ball sinking distance is preferably 5 mm or less, more preferably 3 mm or less, and even more preferably 0 mm.

[0018] The polyurethane foam of the present invention preferably has a melt diameter distance of 20 mm or less in a hot steel ball test. If the melt diameter distance is 20 mm or less, the polyurethane foam is less likely to spread fire when exposed to a fire or the like, and the spread of fire can be effectively prevented. From the viewpoint of effectively preventing the spread of fire, the melt diameter distance is preferably 15 mm or less, more preferably 13 mm or less, and even more preferably 12 mm or less. The melt diameter distance is 0 mm or more.

[0019] The steel ball sinking distance and molten diameter distance can be adjusted to desired values ​​by adjusting the type of polyol compound contained in the foamable urethane resin composition described below, the isocyanate index, the water content, and the like.

[0020] In the hot steel ball evaluation, a cavity is formed in the test specimen from the top surface to the inside due to the sinking of the steel ball. The sinking distance of the steel ball means the maximum distance of the cavity in the direction perpendicular to the top surface of the test specimen. The melting diameter distance is the diameter of the hole formed by the heated steel ball on the top surface of the test specimen. If the shape of the hole formed on the top surface of the test specimen is circular, the diameter of the hole means the diameter of the circle, and if the shape of the hole is elliptical, the diameter of the hole means the major axis. If the shape of the hole is other than circular or elliptical, the maximum distance between any two points of the shape is the diameter of the hole. If the steel ball remains on the surface of the test specimen and the test specimen does not melt and no cavity is formed on the top surface, the diameter of the carbonized or discolored part is measured in the same manner as when a cavity is formed.

[0021] (Total heat generation) The polyurethane foam of the present invention has a radiant heat intensity of 50 kW / m2 according to the test method of ISO-5660. 2 When heated for 5 minutes, the total heat generated is 8MJ / m 2 The total calorific value is preferably 8MJ / m or less. 2 The polyurethane foam of the present invention has a predetermined flame retardancy when the steel ball sinking distance and the molten diameter distance are equal to or less than certain values ​​as described above. The polyurethane foam has both flame retardancy and the property of not spreading fire, and can more effectively prevent the spread of fire in the event of a fire. From the viewpoint of further improving the flame retardancy of the polyurethane foam, the total calorific value is set to 7.8 MJ / m 2 It is preferable that the concentration is less than 7.5 MJ / m 2 More preferably, it is 7.0 MJ / m or less. 2 It is even more preferable that:

[0022] (Maximum heat generation rate) The polyurethane foam of the present invention has a radiant heat intensity of 50 kW / m2 according to the test method of ISO-5660. 2 The maximum heat generation rate when heated for 5 minutes is 200kW / m 2 It is preferable that the maximum heat generation rate is 200 kW / m or less.2 The polyurethane foam of the present invention has a predetermined flame retardancy by being within the range described below. In addition, by adjusting both the maximum heat release rate and the total heat release amount as described above, the flame retardancy is further improved. By having a predetermined flame retardancy and, as described above, having the steel ball sinking distance and molten diameter distance below certain values, a polyurethane foam is obtained that has both flame retardancy and the property of not spreading fire, and can more effectively prevent the spread of fire in the event of a fire. From the viewpoint of further improving the flame retardancy of the polyurethane foam, the maximum heat generation rate is set to 150 kW / m 2 It is preferable that the maximum power consumption is 130 kW / m or less. 2 More preferably, it is 100 kW / m or less. 2 It is even more preferable that:

[0023] The total heat release amount and maximum heat release rate can be obtained by a cone calorimeter test, and specifically, can be measured by the method described in the Examples. Since the polyurethane foam of the present invention is resistant to dimensional deformation as described above, the polyurethane foam subjected to the test can be prevented from coming into contact with the spark igniter of the cone calorimeter during the cone calorimeter test.

[0024] The density of the polyurethane foam is not particularly limited, but is preferably 20 to 200 kg / m 3 It is preferable that the density is in the range of 200 kg / m 3 By setting the density to 20kg / m or less, the polyurethane foam becomes lighter and easier to apply to structures. 3 From these viewpoints, the density of the polyurethane foam is preferably 25 to 100 kg / m 3 More preferably, the range is 25 to 80 kg / m 3 It is more preferable that the density of the polyurethane foam is in the range of 9. The density of the polyurethane foam can be measured in accordance with JIS K7222.

[0025] [Foamable urethane resin composition] The polyurethane foam of the present invention is preferably formed from a foamable urethane resin composition containing a polyol compound, a polyisocyanate compound, a flame retardant, a blowing agent, and a catalyst. Specifically, the polyurethane foam can be formed by foaming and curing the foamable urethane resin composition. Each of these components will be described below.

[0026] (Polyol Compound) The polyol compound contained in the foamable urethane resin composition of the present invention is not particularly limited, but examples thereof include polyether polyols, polyester polyols, and polymer polyols. From the viewpoint of improving the flame retardancy of the polyurethane foam, the polyol compound preferably contains a polyester polyol, and more preferably contains a phthalic acid-based polyester polyol. Also, from the viewpoint of improving the flame retardancy, it is preferable to use a halogen-containing polyol or a phosphorus-containing polyol.

[0027] From the viewpoint of dimensional stability of the foam, the polyol compound may be a combination of a long-chain polyol and a short-chain polyol. In this specification, the long-chain polyol means a polyol having a functionality of 3 or less and a hydroxyl value of less than 150 mgKOH / g. Examples of the long-chain polyol include a long-chain polyether polyol and a long-chain polyester polyol. In addition, the short-chain polyol means a polyol compound other than the long-chain polyol. When these are used in combination, the amount of the long-chain polyol blended is preferably 0.5 to 30 parts by mass, more preferably 1 to 15 parts by mass, per 100 parts by mass of the short-chain polyol.

[0028] <Polyester polyol> Examples of polyester polyols include aromatic polyester polyols and aliphatic polyester polyols, but when considering the flame retardancy of the resulting polyurethane foam, it is preferable to use aromatic polyester polyols. The aromatic polyester polyol is preferably a condensate of an aromatic dicarboxylic acid such as o-phthalic acid (phthalic acid), m-phthalic acid (isophthalic acid), p-phthalic acid (terephthalic acid), or naphthalenedicarboxylic acid with a glycol. Among them, from the viewpoint of increasing the flame retardancy of the polyurethane foam, reducing the values ​​of the steel ball sinking distance and the melting diameter distance described above, and improving the flame-spreading performance, it is preferable that the polyol compound contains a phthalic acid-based polyester polyol, which is a condensate of phthalic acid and a glycol, and more preferably contains a p-phthalic acid-based polyester polyol, which is a condensate of p-phthalic acid and a glycol. The glycol is not particularly limited, but it is preferable to use low molecular weight aliphatic glycols known as components of polyester polyols, such as ethylene glycol, propylene glycol, and diethylene glycol.

[0029] From the viewpoint of reducing the above-mentioned steel ball sinking distance and molten diameter distance values ​​and improving fire spread prevention performance, the content of the phthalic acid-based polyester polyol based on the total amount of the polyol compounds is preferably 60 mass% or more, more preferably 70 mass% or more, and even more preferably 75 mass% or more.

[0030] The hydroxyl value of the polyester polyol is preferably from 100 to 400 mgKOH / g, and more preferably from 150 to 350 mgKOH / g. The hydroxyl value is a value measured in accordance with JIS K1557-1:2007.

[0031] <Polyether polyol> Polyether polyol is a polyoxyalkylene polyol obtained by ring-opening addition polymerization of an alkylene oxide to an initiator having two or more active hydrogen atoms. Specific examples of the initiator include aliphatic polyhydric alcohols (e.g., glycols such as ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, 1,4-butanediol, 1,3-butanediol, 1,6-hexanediol, neopentyl glycol, cyclohexylene glycol, and cyclohexanedimethanol, triols such as trimethylolpropane and glycerin, tetrafunctional alcohols such as pentaerythritol, and polyfunctionals such as sucrose and sorbitol), aliphatic amines (e.g., alkylenediamines such as ethylenediamine, propylenediamine, butylenediamine, hexamethylenediamine, and neopentyldiamine, and alkanolamines such as monoethanolamine and diethanolamine), and aromatic amines (e.g., aniline, tolylenediamine, xylylenediamine, diphenylmethanediamine, and Mannich condensation products), and the like. These may be used alone or in combination of two or more.

[0032] As the polyether polyol, from the viewpoint of improving moldability at the time of injection during urethane foaming and workability at the time of spraying, those which are expected to have self-reactive activity, such as tolylenediamine-based polyether polyols and Mannich-based polyether polyols, and from the viewpoint of improving flame retardancy, in addition to the above, sucrose-based polyether polyols and sorbitol-based polyether polyols are preferred.

[0033] The tolylenediamine-based polyether polyol is a polyether polyol obtained by using tolylenediamine as an initiator. The same applies to sucrose-based polyether polyol and sorbitol-based polyether polyol. The Mannich polyether polyol is a polyether polyol obtained by utilizing the Mannich reaction, which is a Mannich condensation product having two or more hydroxyl groups in the molecule, or an alkylene oxide added to such a Mannich condensation product. More specifically, it is a Mannich condensation product obtained by the Mannich reaction of at least one of phenol and its alkyl-substituted derivatives, formaldehyde and alkanolamine, or a polyether polyol obtained by ring-opening addition polymerization of at least one of ethylene oxide and propylene oxide to this compound.

[0034] The hydroxyl value of the polyether polyol is preferably from 200 to 1000 mgKOH / g, and more preferably from 300 to 600 mgKOH / g.

[0035] <Polymer polyol> Examples of polymer polyols include those containing polymer components such as polyacrylonitrile, acrylonitrile-styrene copolymers, etc., in addition to polyester polyols, polyether polyols, etc. Polymer components such as polyacrylonitrile (acrylonitrile polymers) and acrylonitrile-styrene copolymers correspond to organic fine particles described later.

[0036] (Cell opener) The foamable urethane resin composition of the present invention preferably contains a cell opener. By containing a cell opener, holes are easily formed in the cell membrane of the foam, gas escape is promoted at high temperatures, deformation such as expansion is suppressed, and dimensional stability at room temperature is improved. The cell opener is a material containing at least one type of fine particle component selected from organic fine particles and inorganic fine particles. Examples of the organic fine particles used as the cell opener include polymers of at least one monomer selected from the group consisting of acrylonitrile, methacrylonitrile, fluorinated acrylonitrile, α-ethyl acrylonitrile, styrene, vinyl acetate, and acrylic monomers, and silicone polymers. Examples of the inorganic fine particles include silicon-containing particles such as silica particles.

[0037] The cell opener may be composed of only at least one type of fine particle component selected from organic fine particles and inorganic fine particles, or may be a mixture of at least one type of fine particle component selected from organic fine particles and inorganic fine particles with a surfactant, etc. Also, a cell opener-containing polyol in which a polyol compound and a cell opener are mixed in advance may be used.

[0038] The content of the fine particle component in the cell opener is not particularly limited, but is, for example, 3 to 100% by mass, and preferably 15 to 100% by mass. The content of the cell opener in the cell opener-containing polyol is not particularly limited, but is, for example, 0.01 to 10% by mass, and preferably 0.05 to 5% by mass.

[0039] When a cell opener is used, the content of the cell opener in the foamable urethane resin composition is preferably 0.01 to 50 parts by mass, and more preferably 0.1 to 15 parts by mass, per 100 parts by mass of the polyol compound, from the viewpoint of maintaining a certain level or higher of the closed cell ratio.

[0040] (Polyisocyanate compounds) As the polyisocyanate compound contained in the foamable urethane resin composition, various polyisocyanate compounds having two or more isocyanate groups, such as aromatic, alicyclic, and aliphatic polyisocyanate compounds, can be used. It is preferable to use liquid diphenylmethane diisocyanate (MDI) because of its ease of handling, rapid reaction, excellent physical properties of the resulting polyurethane foam, and low cost. As the liquid MDI, crude MDI (also called polymeric MDI) can be mentioned. Specific examples of commercially available liquid MDI include "44V-10" and "44V-20" (manufactured by Sumika Covestro Urethane Co., Ltd.), and "Millionate MR-200" (Nippon Polyurethane Industry Co., Ltd.). In addition, uretonimine-containing MDI (for example, a commercially available product "Millionate MTL": manufactured by Nippon Polyurethane Industry Co., Ltd.) may also be used. In addition, a part of the isocyanate active group in the isopolycyanate compound may be reacted with a hydroxyl group-containing compound to enhance the affinity with polyol in advance. In addition to liquid MDI, other polyisocyanate compounds may be used in combination, and as the polyisocyanate compounds to be used in combination, any polyisocyanate compound known in the technical field of polyurethanes can be used without any limitations.

[0041] The isocyanate index of the foamable urethane resin composition of the present invention is preferably in the range of 150 to 700, more preferably 200 to 650, and further preferably 250 to 600. When the isocyanate index is in such a range, it becomes easy to adjust the sinking distance and molten diameter distance of the steel ball in the above-mentioned hot steel ball evaluation to the desired range. The isocyanate index (INDEX) is calculated as follows.

[0042] INDEX = equivalents of isocyanate ÷ (equivalents of polyol + equivalents of water) × 100 Where: Isocyanate equivalent number = number of parts of polyisocyanate used x NCO content (%) x 100 / NCO molecular weight Polyol equivalent number = OHV × number of parts of polyol used ÷ molecular weight of KOH, OHV is the hydroxyl value of polyol (mgKOH / g), Equivalents of water = parts of water used × number of OH groups in water / molecular weight of water In the above formula, the unit of the parts used is weight (g), the molecular weight of the NCO group is 42, the NCO content is the proportion of NCO groups in the polyisocyanate compound expressed as mass%, and for convenience of unit conversion in the above formula, the molecular weight of KOH is 56100, the molecular weight of water is 18, and the number of OH groups in water is 2.

[0043] (Flame retardant) The foamable urethane resin composition of the present invention preferably contains a flame retardant. Examples of the flame retardant include solid flame retardants and liquid flame retardants. By containing a flame retardant, the flame retardancy of the polyurethane foam obtained is improved, and the polyurethane foam is less likely to deform when exposed to heat. In particular, it is preferable to use a phosphate flame retardant, which will be described later, as the liquid flame retardant. Here, a solid flame retardant refers to a flame retardant that is solid at 23°C, and a liquid flame retardant refers to a flame retardant that is liquid at 23°C.

[0044] (Liquid flame retardant) The foamable urethane resin composition of the present invention preferably contains a liquid flame retardant at room temperature, which makes it easier to adjust the steel ball sinking distance and melt diameter distance to the desired range, and since the flame retardant is liquid, it is possible to suppress wear of the equipment used when using the foamable urethane resin composition. Examples of liquid flame retardants include phosphate flame retardants such as monophosphate and condensed phosphate. Examples of monophosphate esters include, but are not limited to, trimethyl phosphate, triethyl phosphate, tricresyl phosphate, cresyl diphenyl phosphate, and tris(β-chloropropyl) phosphate. The condensed phosphate ester is not particularly limited, but examples thereof include resorcinol polyphenyl phosphate (product name: CR-733S), bisphenol A polycresyl phosphate (product name: CR-741), and aromatic condensed phosphate ester (product name: CR747).

[0045] (Solid flame retardant) Examples of solid flame retardants include boron-containing flame retardants, red phosphorus, bromine-containing flame retardants, phosphate-containing flame retardants, antimony-containing flame retardants, phosphinic acid-based flame retardants, and metal hydroxide-based flame retardants, among which boron-containing flame retardants and bromine-containing flame retardants are preferred, and boron-containing flame retardants are more preferred. By using a solid flame retardant, in addition to increasing the flame retardancy, it becomes easier to suppress shape deformation when the polyurethane foam is exposed to heat.

[0046] <Boron-containing flame retardants> Specific examples of the boron-containing flame retardant include alkali metal borate such as lithium borate, sodium borate, potassium borate, and cesium borate, alkaline earth metal borate such as magnesium borate, calcium borate, and barium borate, zirconium borate, zinc borate, aluminum borate, and ammonium borate, etc. Among these, zinc borate is preferred.

[0047] <Brominated flame retardants> The brominated flame retardant is not particularly limited as long as it is a compound containing bromine in its molecular structure, and examples thereof include aromatic brominated compounds. Specific examples of the aromatic brominated compound include monomeric organic bromine compounds such as hexabromobenzene, pentabromotoluene, hexabromobiphenyl, decabromobiphenyl, hexabromocyclodecane, decabromodiphenyl ether, octabromodiphenyl ether, hexabromodiphenyl ether, bis(pentabromophenoxy)ethane, ethylene bis(pentabromophenyl), ethylene bis(tetrabromophthalimide), and tetrabromobisphenol A; polycarbonate oligomers produced using brominated bisphenol A as a raw material; and mixtures of the polycarbonate oligomers and bisphenols. Examples of the brominated epoxy compounds include brominated polycarbonates such as copolymers with brominated bisphenol A, diepoxy compounds produced by the reaction of brominated bisphenol A with epichlorohydrin, and monoepoxy compounds obtained by the reaction of brominated phenols with epichlorohydrin, and halogenated bromine compound polymers such as poly(brominated benzyl acrylate), brominated polyphenylene ether, brominated bisphenol A, condensates of cyanuric chloride and brominated phenol, brominated (polystyrene), poly(brominated styrene), brominated polystyrenes such as crosslinked brominated polystyrene, and crosslinked or non-crosslinked brominated poly(α-methylstyrene). Among these, ethylene bis(pentabromophenyl), ethylene bis(tetrabromophthalimide), hexabromobenzene, and the like are preferable.

[0048] <Phosphate-containing flame retardants> Examples of the phosphate-containing flame retardant include phosphates consisting of a salt of phosphoric acid and at least one metal or compound selected from metals of Groups IA to IVB of the periodic table, ammonia, aliphatic amines, and aromatic amines. The phosphoric acid is not particularly limited, and examples thereof include various phosphoric acids such as monophosphoric acid, pyrophosphoric acid, and polyphosphoric acid. Examples of the metals in Groups IA to IVB of the periodic table include lithium, sodium, calcium, barium, iron (II), iron (III), aluminum, etc. Examples of the aliphatic amines include methylamine, ethylamine, diethylamine, triethylamine, ethylenediamine, piperazine, etc. Examples of the aromatic amines include pyridine, triazine, melamine, etc. The above-mentioned phosphate-containing flame retardants may be subjected to a known water resistance improving treatment, such as treatment with a silane coupling agent or coating with a melamine resin.

[0049] Specific examples of phosphate-containing flame retardants include monophosphates, pyrophosphates, polyphosphates, and the like. The monophosphate salt is not particularly limited, and examples thereof include ammonium salts such as ammonium phosphate, ammonium dihydrogen phosphate, and diammonium hydrogen phosphate; sodium salts such as monosodium phosphate, disodium phosphate, trisodium phosphate, monosodium phosphite, disodium phosphite, and sodium hypophosphite; potassium salts such as monopotassium phosphate, dipotassium phosphate, tripotassium phosphate, monopotassium phosphite, dipotassium phosphite, and potassium hypophosphite; lithium salts such as monolithium phosphate, dilithium phosphate, trilithium phosphate, monolithium phosphite, dilithium phosphite, and lithium hypophosphite; barium salts such as barium dihydrogen phosphate, barium hydrogen phosphate, tribarium phosphate, and barium hypophosphite; magnesium salts such as monohydrogen magnesium phosphate, magnesium hydrogen phosphate, trimagnesium phosphate, and magnesium hypophosphite; calcium salts such as calcium dihydrogen phosphate, calcium hydrogen phosphate, tricalcium phosphate, and calcium hypophosphite; and zinc salts such as zinc phosphate, zinc phosphite, and zinc hypophosphite.

[0050] The polyphosphate is not particularly limited, but examples thereof include ammonium polyphosphate, piperazine polyphosphate, melamine polyphosphate, ammonium amide polyphosphate, and aluminum polyphosphate. Among these, it is preferable to use monophosphates, and it is more preferable to use ammonium dihydrogen phosphate, since this improves the self-extinguishing property of the phosphate-containing flame retardant. The phosphate-containing flame retardants may be used alone or in combination of two or more.

[0051] <Antimony-containing flame retardants> Examples of the antimony-containing flame retardant used in the present invention include antimony oxide, antimonates, and pyroantimonates. Examples of antimony oxides include antimony trioxide and antimony pentoxide. Examples of antimonate salts include sodium antimonate and potassium antimonate. Examples of pyroantimonate salts include sodium pyroantimonate and potassium pyroantimonate. Preferably, the antimony-containing flame retardant is antimony oxide. The antimony-containing flame retardants may be used alone or in combination of two or more.

[0052] <Phosphinic acid flame retardants> Examples of phosphinic acid flame retardants include phosphinic acid, dimethylphosphinic acid, methylethylphosphinic acid, methylpropylphosphinic acid, diethylphosphinic acid, dioctylphosphinic acid, phenylphosphinic acid, diethylphenylphosphinic acid, diphenylphosphinic acid, and bis(4-methoxyphenyl)phosphinic acid.

[0053] <Metal hydroxide flame retardants> Examples of metal hydroxide flame retardants include magnesium hydroxide, calcium hydroxide, aluminum hydroxide, iron hydroxide, nickel hydroxide, zirconium hydroxide, titanium hydroxide, zinc hydroxide, copper hydroxide, vanadium hydroxide, tin hydroxide, etc. The metal hydroxide flame retardants may be used alone or in combination of two or more.

[0054] Examples of solid flame retardants other than the above-mentioned solid flame retardants include phosphazenes, metal phosphinates, silicone-based flame retardants, and organic sulfonate-based flame retardants.

[0055] The content of the flame retardant is preferably 5 to 100 parts by mass, more preferably 10 to 80 parts by mass, and further preferably 20 to 70 parts by mass, based on 100 parts by mass of the polyol compound.

[0056] (Foam stabilizer) The flame-retardant urethane resin composition of the present invention may contain a foam stabilizer. For example, a compound having a polar portion and a non-polar portion in the molecule and having a surface active effect may be used as the foam stabilizer. Specific examples of the foam stabilizer include silicone foam stabilizers such as organopolysiloxane. In addition, the silicone foam stabilizer may include a graft copolymer of polydimethylsiloxane and polyethylene glycol.

[0057] (foaming agent) Specific examples of the blowing agent include water, low-boiling point hydrocarbons, chlorinated aliphatic hydrocarbon compounds, fluorine compounds, hydrochlorofluorocarbon compounds, hydrofluorocarbons, ether compounds, hydrofluoroolefins, etc. Further examples of the blowing agent include organic physical blowing agents such as mixtures of these compounds, and inorganic physical blowing agents such as nitrogen gas, oxygen gas, argon gas, and carbon dioxide gas. Examples of the low boiling point hydrocarbon include propane, butane, pentane, hexane, heptane, cyclopropane, cyclobutane, cyclopentane, cyclohexane, and cycloheptane. Examples of the chlorinated aliphatic hydrocarbon compounds include dichloroethane, propyl chloride, isopropyl chloride, butyl chloride, isobutyl chloride, pentyl chloride, and isopentyl chloride. Examples of the fluorine compound include CHF3, CH2F2, and CH3F. Examples of the hydrochlorofluorocarbon compounds include trichloromonofluoromethane, trichlorotrifluoroethane, and dichloromonofluoroethane (for example, HCFC141b (1,1-dichloro-1-fluoroethane), HCFC22 (chlorodifluoromethane), and HCFC142b (1-chloro-1,1-difluoroethane)). Examples of the hydrofluorocarbon include HFC-245fa (1,1,1,3,3-pentafluoropropane) and HFC-365mfc (1,1,1,3,3-pentafluorobutane). The ether compound may, for example, be diisopropyl ether. Examples of the hydrofluoroolefin include HFO-1233zd(E) (trans-1-chloro-3,3,3-trifluoropropene), HFO-1234yf (2,3,3,3-tetrafluoro-1-propene), HFO-1224yd(Z) (trans-1-chloro-2,3,3,3-tetrafluoropropene), HFO-1336mzz(Z) (cis-1,1,1,4,4,4-hexafluorobut-2-ene), and HFO-1224yd(Z).

[0058] In the present invention, from the viewpoint of reducing the environmental load, the foaming agent preferably contains hydrofluoroolefin (HFO), and more preferably contains hydrofluoroolefin (HFO) and water. As the water, for example, ion-exchanged water, distilled water, etc. can be appropriately used. The amount of water relative to 100 parts by mass of the polyol compound is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, even more preferably 0.1 parts by mass or more, and preferably 2.0 parts by mass or less, more preferably 1.5 parts by mass or less. When the water content is equal to or more than these lower limits, the foamable urethane resin composition is easily foamed, and the density is easily adjusted to a desired range. In addition, when the water content is equal to or less than these upper limits, the sinking distance and melting diameter distance of the steel ball in the hot steel ball evaluation of the polyurethane foam are easily adjusted to the desired ranges described above.

[0059] In the present invention, the blowing agent preferably contains a hydrofluoroolefin as described above, and more preferably contains both the hydrofluoroolefin and the water described above. The amount of the hydrofluoroolefin per 100 parts by mass of the polyol compound is preferably 10 to 60 parts by mass, more preferably 15 to 50 parts by mass, and even more preferably 25 to 45 parts by mass.

[0060] (catalyst) The foamable urethane resin composition of the present invention preferably contains a catalyst. The catalyst preferably contains a trimerization catalyst, and more preferably contains a urethanization catalyst in addition to the trimerization catalyst. Note that the catalyst contained in the foamable urethane resin composition does not correspond to the inorganic filler of the present invention.

[0061] A trimerization catalyst is a catalyst that promotes trimerization to form an isocyanurate bond. By promoting trimerization of a polyurethane resin, the flame retardancy of a polyurethane foam is improved. Examples of the trimerization catalyst that can be used include aromatic compounds such as tris(dimethylaminomethyl)phenol, 2,4-bis(dimethylaminomethyl)phenol, and 2,4,6-tris(dialkylaminoalkyl)hexahydro-S-triazine; alkali metal salts such as potassium acetate, sodium acetate, potassium 2-ethylhexanoate, sodium 2-ethylhexanoate, potassium octylate, potassium formate, and sodium octylate; aziridines such as 2-ethylaziridine; lead compounds such as lead naphthenate and lead octylate; alcoholate compounds such as sodium methoxide; phenolate compounds such as potassium phenoxide; tertiary ammonium salts such as trimethylammonium salts, triethylammonium salts, and triphenylammonium salts; and quaternary ammonium salts such as tetramethylammonium salts, tetraethylammonium, and tetraphenylammonium salts. The trimerization catalyst may be used alone or in combination of two or more kinds.

[0062] The amount of the trimerization catalyst is not particularly limited, but is preferably in the range of 0.3 to 15 parts by mass, more preferably in the range of 0.5 to 10 parts by mass, and even more preferably in the range of 1 to 8 parts by mass, relative to 100 parts by mass of the urethane resin. By setting the amount of the trimerization catalyst within the above range, isocyanurate bonds are appropriately formed, improving flame retardancy. In addition, it becomes easier to adjust the closed cell ratio to a desired range.

[0063] The urethane catalyst is a catalyst that accelerates the reaction between the polyol component and the polyisocyanate. Specific examples of the urethane catalyst include amino compounds, tin compounds, bismuth compounds, and metal salts of acetylacetone. Examples of the amino compound include imidazole compounds such as 1-methylimidazole, 1,2-dimethylimidazole, 1-isobutyl-2-methylimidazole, and imidazole compounds in which the secondary amine functional group in the imidazole ring is substituted with a cyanoethyl group, pentamethyldiethylenetriamine, triethylamine, N-methylmorpholinebis(2-dimethylaminoethyl)ether, bis(2-dimethylaminoethyl)ether, N,N,N',N",N"-pentamethyldiethylenetriamine, N,N,N'-trimethylaminoethyl-ethanolamine, bis(2-dimethylaminoethyl)ether, N-methyl-N',N'-dimethylaminoethylpiperazine, N,N-dimethylcyclohexylamine, diazabicycloundecene, triethylenediamine, tetramethylethylenediamine, guanidine derivatives, tetramethylhexamethylenediamine, trimethylaminoethylpiperazine, tripropylamine, and the like, and acid-blocked products thereof. Examples of tin compounds include stannous octoate, dibutyltin diacetate, dibutyltin dilaurate, etc. Examples of bismuth compounds include bismuth neodecanoate, bismuth octoate, etc. Examples of acetylacetone metal salts include acetylacetone aluminum, acetylacetone iron, acetylacetone copper, acetylacetone zinc, acetylacetone beryllium, acetylacetone chromium, acetylacetone indium, acetylacetone manganese, acetylacetone molybdenum, acetylacetone titanium, acetylacetone cobalt, acetylacetone vanadium, and acetylacetone zirconium. The urethane resin curing catalyst may be used alone or in combination of two or more kinds.

[0064] The amount of the urethane catalyst in the foamable urethane resin composition is not particularly limited, but is preferably in the range of 0.5 to 30 parts by mass, more preferably in the range of 1 to 20 parts by mass, and even more preferably in the range of 3 to 15 parts by mass, relative to 100 parts by mass of the urethane resin. By setting the amount within the above range, the reaction between the polyol compound and the polyisocyanate compound can be promoted at an appropriate reaction speed. In addition, the closed cell ratio can be easily adjusted to a desired range. Note that 100 parts by mass of the urethane resin means 100 parts by mass in total of the polyol compound and the polyisocyanate compound.

[0065] The total amount of all the above catalysts is preferably 0.5 to 15 parts by mass, more preferably 1 to 12 parts by mass, and even more preferably 2 to 10 parts by mass, per 100 parts by mass of the urethane resin, from the viewpoint of improving the curing speed of the urethane (particularly the balance between cell formation by foaming and the appearance of pores of the present invention) and flame retardancy.

[0066] The foamable urethane resin composition can contain, as additives, for example, phenol-based, amine-based, sulfur-based and other antioxidants, heat stabilizers, light stabilizers, metal damage inhibitors, antistatic agents, crosslinking agents, lubricants, softeners, pigments, dyes, tackifying resins, and the like, within the scope of not impairing the effects of the present invention.

[0067] The foamable urethane resin composition of the present invention is cured by the reaction of the polyol compound and the polyisocyanate compound, and therefore the viscosity of the composition changes with time. Therefore, before using the foamable urethane resin composition, the foamable urethane resin composition is divided into two or more portions to prevent the foamable urethane resin composition from reacting and curing. When using the foamable urethane resin composition, it is preferable to combine the two or more portions of the foamable urethane resin composition into one.

[0068] When the foamable urethane resin composition is divided into two or more components, each of the components of the foamable urethane resin composition divided into two or more components does not start curing alone, and each component may be divided so that the curing reaction starts after each component of the foamable urethane resin composition is mixed. Usually, the foamable urethane resin composition is divided into a polyol composition containing a polyol compound and a polyisocyanate composition containing a polyisocyanate compound.

[0069] The above-mentioned flame retardant, blowing agent, catalyst, and foam stabilizer may be contained in the polyol composition, may be contained in the polyisocyanate composition, or may be provided separately from the polyol composition and the polyisocyanate composition, but are preferably contained in the polyol composition.

[0070] The foam of the present invention is not particularly limited, but when it is divided into two or more parts, such as a two-liquid type foamable urethane resin composition, for example, a polyol composition and a polyisocyanate composition, which are prepared by mixing each component in advance, are prepared in two or more parts, and then mixed and foamed. The mixing and foaming of each component can be performed by a known method. For example, it can be obtained using a known device such as a high-pressure foaming machine, a low-pressure foaming machine, a spray foaming machine, or a hand mixer. In addition, in the case of a one-liquid type, a method of foaming a foamable urethane resin composition obtained by mixing each component constituting the foamable urethane resin composition by a known method can be mentioned.

[0071] (Viscosity of polyol composition) The viscosity of the polyol composition at 25°C is not particularly limited, but is preferably 2000 mPa·s or less, and more preferably 1500 mPa·s or less. By setting the viscosity of the polyol composition to the above upper limit or less, the fluidity of the foamable urethane resin composition is improved, and mixing defects can be suppressed. The viscosity of the polyol composition can be appropriately adjusted, for example, depending on the molecular weight of the polyol compound used and the type and amount of the powder component. The viscosity of the polyol composition was measured using a B-type viscometer at a temperature of 25°C.

[0072] (Application) The uses of the foamable urethane resin composition and polyurethane foam of the present invention are not particularly limited, and they can be used for filling cavities in structures such as buildings, furniture, automobiles, trains, and ships. The foamable urethane resin composition can also be used for spraying onto the structures. Among them, it is preferable to use the composition for spraying onto structures, that is, as a foamable urethane resin composition for spraying. A polyurethane foam is formed by spraying the foamable urethane resin composition. Spraying can be performed using a spraying device (e.g., A-25 manufactured by GRACO) and a spray gun (e.g., D gun manufactured by Gasmar). Spraying can be performed by adjusting the temperature of the polyol composition and the polyisocyanate composition contained in separate containers in the spraying device, mixing them by collision at the tip of the spray gun, and turning the mixed liquid into a mist using air pressure. The spraying device and spray gun are well known and commercially available products can be used. In addition, the temperature settings and pressure of the raw liquid can be the same as those for spraying general urethane foam. EXAMPLES

[0073] The present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples in any way.

[0074] Details of each component used in each example and comparative example are as follows. (1) Polyol compounds (i) Polyester polyol p-Phthalic acid-based polyester polyol (Kawasaki Chemical Industries, Ltd., product name: RFK-505, hydroxyl value = 250 mg KOH / g, short-chain polyol) (ii) Polyether polyol Mannich-based polyether polyol (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., product name: DK3776, hydroxyl value = 350 mg KOH / g, short-chain polyol) Ethylenediamine polyether polyol (AGC Corporation, product name: Exenol 750ED, hydroxyl value = 760 mg KOH / g, short-chain polyol) Long-chain polyether polyol (Mitsui Chemicals, product name: T-3000, hydroxyl value = 56 mg KOH / g, long-chain polyol) (iii) Polymer polyol (cell opener-containing polyol) Mannich-based polyether polyol containing 0.1-2 wt% acrylonitrile polymer Hydroxyl value = 315 mg KOH / g Short chain polyol

[0075] (2) Cell opener ·Organic particles·Acrylonitrile polymer · Inorganic fine particles · Silica fine particles (specific surface area 400m 2 / g or less fumed silica)

[0076] (3) Liquid flame retardants Phosphate ester flame retardant <Tris(β-chloropropyl)phosphate> (manufactured by Daihachi Chemical Industry Co., Ltd., product name: TMCPP) (4) Solid flame retardants Red phosphorus (manufactured by Rinkagaku Kogyo Co., Ltd., product name: Nova Excel 140) Brominated flame retardant (Manac Corporation, product name: HBB-b) (5) Foam stabilizer Silicone foam stabilizer (Toray Dow Corning, product name: SH-193) (6) Catalyst (i) Trimerization catalyst Quaternary ammonium salt (manufactured by Evonik Japan, product name: TMR-7), mixture with ethylene glycol (45-55% by mass of quaternary ammonium salt, 45-55% by mass of ethylene glycol) (ii) Urethane catalyst Imidazole compound (Kao Corporation, product name: KL No. 390), concentration 65-75% by mass Bismuth compound (manufactured by Nitto Kasei, product name: Neostan U-600), concentration 55-58% by mass (7) Foaming agent ·water HFO-1233zd <hydrofluoroolefin> (Honeywell product name: Solstice LBA) (8) Polyisocyanate compounds MDI (manufactured by Sumika Covestro Urethane Co., Ltd., product name: 44V-20)

[0077] The methods for measuring the various physical properties and characteristics are as follows. [Closed bubble rate] The polyurethane foams produced in each of the Examples and Comparative Examples were cut into 30 mm squares, and the weights were measured to determine the apparent densities. The true densities were determined by dry density measurement using a constant volume expansion method, and the open cell ratio was calculated using the following formula (1). For the measurements, a dry automatic densimeter (Shimadzu Corporation's "Accupyc II 1340 Series") was used. The true densities were determined by a gas phase displacement method (pycnometer). The purge pressure was 0.2 MPa. Open cell rate (%) = {(true density [g / cm 3 ])-(Apparent density [g / cm 3 ])} / (true density[g / cm 3 ])×100 (1) Closed cell ratio (%) = 100 - open cell ratio calculated from the result of formula (1) (2) A closed cell rate of 80% or more was rated as "good", and a rate of less than 80% was rated as "poor".

[0078] [With or without holes] The polyurethane foams prepared in the respective Examples and Comparative Examples were cut into pieces of a measurable size to prepare measurement samples. The surface of the measurement sample was observed with a scanning electron microscope (Hitachi "N-FE-SEM") to observe whether or not holes were formed in the cell membrane of the foam. The observation magnification was 50 to 300 times, and the accelerating voltage was 1.0 kV. Fig. 1 shows an example of the results of scanning electron microscopy of Example 2, in which holes were confirmed in the cell membrane, and Fig. 2 shows an example of the results of scanning electron microscopy of Comparative Example 1, in which no holes were confirmed in the cell membrane.

[0079] [Evaluation of storage stability] The polyol compositions prepared in each of the Examples and Comparative Examples were transferred to a glass container and stored for 24 hours at 23° C. After 24 hours, the polyol compositions were visually observed, and those in which slight separation was observed were marked with △, and those in which no separation was observed were marked with ○.

[0080] [Dimensional stability evaluation] The polyurethane foams obtained in each of the Examples and Comparative Examples were cut into pieces 10 cm long, 10 cm wide and 5 cm thick, and stored at room temperature for 7 days. At this time, the pieces were cut so as to include one skin layer inside. The length retention rate for each of the length and width was calculated using the following formula, and these were averaged to determine the shape retention rate and evaluate the dimensional stability. A shape retention rate of 100% means that there was no shrinkage at all. Each length was measured at its smallest point. An evaluation of "Good" means that the foam is resistant to shrinkage and has excellent dimensional stability. Retention rate = 100 × (length of one side after storage for 7 days) / (length of one side before storage). ○ Shape retention rate is 90% or more × Shape retention rate is less than 90%

[0081] [Hot steel ball evaluation] For the polyurethane foams produced in each of the Examples and Comparative Examples, the sinking distance and fusion diameter distance of the steel ball were measured by the following procedures (1) to (3). (1) The polyurethane foam was cut into a cube with sides of 50 mm to be used as a test specimen. (2) A steel ball (SUS304) with a diameter of 10.0 mm and a weight of 4.15 g was placed inside an electric furnace with the temperature inside the furnace set to 800°C and heated for 15 minutes. (3) In an atmosphere of 23°C, the steel ball heated in (2) above was immediately placed on the center of the upper part of the test piece in (1) above, and left there until the steel ball had completely sunk in. The test piece was then left at 23°C for 30 minutes to cool sufficiently, and the cross section was cut to measure the sinking distance and fusion diameter distance of the steel ball. From the obtained sinking distance and molten diameter distance of the steel ball, the quality of the flame-proof property was judged as follows.

[0082] <Hot steel ball evaluation criteria> ○ The steel ball sinking distance is 5mm or less and the fusion diameter distance is 15mm or less △: The steel ball sinking distance is 5mm or less and the fusion diameter distance is over 15mm. ×: Anything other than the above 〇 and △

[0083] [Maximum heat release rate, total heat release] The maximum heat release rate and total heat release amount of the polyurethane foams produced in each of the Examples and Comparative Examples were evaluated by the following cone calorimeter test. The polyurethane foams were produced by spraying onto gypsum board (12.5 mm) using a spraying device and a spray gun. The polyurethane foams adhered to the gypsum board as a base were cut into pieces 10 cm long, 10 cm wide and 3.25 cm thick (within the gypsum board being 12.5 mm) to prepare samples for the cone calorimeter test. The cone calorimeter test samples were subjected to a radiant heat intensity test of 50 kW / m in accordance with the ISO-5660 test method. 2 The maximum heat release rate and total heat release amount were measured when the polyurethane foam was heated for 5 minutes at 100°C. In addition to the above method, the polyurethane foam was also produced using a hand mixer, with similar results obtained.

[0084] [Dimensional change at high temperatures (evaluation of contact with the igniter)] In the above-mentioned cone calorimeter test, the polyurethane foams produced in each of the Examples and Comparative Examples were evaluated for contact with the igniter when heated. Cases where there was no contact (no contact) were evaluated as "◯", and cases where there was contact (contact) were evaluated as "×". Cases where there was no contact were judged to have excellent dimensional stability at high temperatures, and cases where there was contact were judged to have poor dimensional stability at high temperatures.

[0085] [Thermal Conductivity] The foamable urethane resin composition used in each of the examples and comparative examples was sprayed onto a structure using a spraying device and a spray gun to produce a polyurethane foam. Three days after producing the polyurethane foam, the foam was cut into a size of 200 mm x 200 mm x 25 mm (including the skin layer inside) and the thermal conductivity was measured. The thermal conductivity in the thickness direction of the polyurethane foam was measured. The device used to measure the thermal conductivity was HC-074 manufactured by Eiko Seiki Co., Ltd.

[0086] [Example 1] According to the formulation in Table 1, a foamable urethane resin composition containing a polyol compound, a cell opener, a liquid flame retardant, a foam stabilizer, a catalyst, and a blowing agent was sprayed onto a structure using a spraying device and a spray gun in accordance with JISA9526 to produce a polyurethane foam. Various evaluations were performed using the polyurethane foam. The results are shown in Table 1.

[0087] [Examples 2 to 6, Comparative Examples 1 to 2] A polyurethane foam was obtained in the same manner as in Example 1, except that the formulation was changed as shown in Table 1. Various evaluations were carried out using the polyurethane foam. The results are shown in Table 1.

[0088] [Table 1]

[0089] It was confirmed that the polyurethane foams of the examples satisfying the requirements of the present invention have excellent heat insulating properties due to their low thermal conductivity, and furthermore, it was found that they also have excellent dimensional stability at high temperatures and at room temperature. In contrast, the polyurethane foams of the comparative examples, which do not satisfy the requirements of the present invention, exhibited poor dimensional stability. [Explanation of symbols]

[0090] 11 Cell 12 holes 13. Areas that occurred during sample preparation

Claims

1. A polyurethane foam having a plurality of cells, the foam is formed from a foamable urethane resin composition containing a polyol compound, a polyisocyanate compound, a flame retardant, a foaming agent, and a catalyst; The foamable urethane resin composition contains a cell opener containing at least one kind of fine particle component selected from organic fine particles and inorganic fine particles (excluding solid flame retardants). ) , the inorganic fine particles are silica particles, the polyol compound contains a phthalic acid-based polyester polyol, and the content of the phthalic acid-based polyester polyol is 75 mass% or more based on the total amount of the polyol compound; The flame retardant contains a liquid flame retardant, The blowing agent contains a hydrofluoroolefin, the catalyst contains a quaternary ammonium salt, an imidazole compound, and a bismuth compound; According to the ISO-5660 test method, when heated for 5 minutes at a radiant heat intensity of 50 kW / m 2 , the total heat generation amount is 8 MJ / m 2 or less; A polyurethane foam having a closed cell ratio of 80% or more, and pores formed in at least a part of the cell membrane of the cells (excluding those containing thermally expandable fine particles and those containing a compound having a vinyl polymerizable functional group represented by the following general formula (I)). 【Chemistry 1】 [In general formula (I), R represents hydrogen, an alkyl group having 1 to 15 carbon atoms, or an aryl group having 6 to 21 carbon atoms.]

2. The polyurethane foam described in claim 1, wherein the foamable urethane resin composition has an isocyanate index of 250 to 600.

3. A polyurethane foam as described in claim 1 or 2, wherein the flame retardant contains a solid flame retardant.

4. Radiant heat intensity 50kW / m according to ISO-5660 test method 2 The maximum heat generation rate when heated for 5 minutes is 200 kW / m 2 The polyurethane foam according to any one of claims 1 to 3, wherein:

5. The polyurethane foam according to any one of claims 1 to 4, wherein a steel ball sinks a distance of 10 mm or less in the hot steel ball evaluation described below. (Hot steel ball evaluation) (1) The polyurethane foam is cut into a cube with sides of 50 mm to prepare a test specimen. (2) A steel ball having a diameter of 10.0 mm and a weight of 4.15 g is placed inside an electric furnace set to 800° C. and heated for 10 minutes or more. (3) In an atmosphere of 23° C., the steel ball heated in (2) above is immediately placed on the center of the upper part of the test piece in (1) above, and left there until the steel ball has completely sunk in. Then, the cross section of the sufficiently cooled test piece is cut, and the sinking distance and fusion diameter distance of the steel ball are measured.

6. 6. The polyurethane foam according to claim 1, which is formed by spraying a foamable urethane resin composition comprising a polyol compound, a polyisocyanate compound, a flame retardant, a blowing agent, and a catalyst.

Citation Information

Patent Citations

  • Production of rigid polyurethane foam composite material

    JP1992279619A

  • Rigid polyurethane foam

    JP1993001171A

  • Polyurethane foam and its production

    JP2000230066A

  • Polyol composition for rigid polyurethane foam and method for producing rigid polyurethane foam

    JP2007046043A

  • Polyol composition for producing polyurethane resin, and method for producing polyurethane resin using the same

    JP2013227519A