Polyol Compositions, Mixing Systems, and Polyurethane Foams

A polyol composition with hydrofluoroolefin and a low-boiling compound maintains adequate pressure for effective discharge and mixing, addressing the issue of insufficient initial discharge in HFO-based polyurethane aerosols, enhancing foam formation and flame retardancy.

JP7579135B2Active Publication Date: 2024-11-07SEKISUI CHEMICAL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020213982
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-23
Publication Date
2024-11-07
Estimated Expiration
2040-12-23

AI Technical Summary

Technical Problem

The use of hydrofluoroolefins (HFO) as a blowing agent in two-component polyurethane aerosols results in insufficient initial discharge due to low vapor pressure, leading to inadequate mixing of polyol and isocyanate liquids, which affects the formation of polyurethane foam and reduces flame retardancy.

Method used

A polyol composition containing hydrofluoroolefin and a low-boiling compound with a boiling point of 10°C or less, along with specific catalysts and fillers, is used to maintain an internal pressure of 0.3 to 1.0 MPa, ensuring adequate discharge and mixing.

Benefits of technology

The solution ensures good discharge properties and effective mixing of polyol and isocyanate, resulting in a polyurethane foam with improved flame retardancy and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579135000002
    Figure 0007579135000002
  • Figure 0007579135000001
    Figure 0007579135000001
Patent Text Reader

Abstract

To provide a polyol composition that demonstrates excellent dischargeability even when the polyol composition uses HFO as a foamer.SOLUTION: A polyol composition contains a polyol, a catalyst, a hydrofluoroolefin, and a low-boiling compound. The low-boiling compound is a low-boiling compound having a boiling point of 10°C or lower, but excluding hydrofluoroolefins. The polyol composition is charged into a container so that the internal pressure becomes 0.3-1.0 MPa at 35°C.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyol composition, a mixing system employing the polyol composition, and polyurethane foams obtained by the mixing system. [Background technology]

[0002] Conventionally, polyurethane foams have been used as heat insulating materials in vehicles such as automobiles, railroad cars, and ships, buildings, etc. They are also used as repair agents for filling defects in vehicles, buildings, etc. Recently, there has been an increasing need to impart flame retardancy to these heat insulating materials and repair agents.

[0003] A two-component polyurethane foam is widely used, in which a polyol liquid and an isocyanate liquid filled in separate containers are mixed to form the foam. Two-component polyurethanes are sometimes used in aerosol containers because each component can be discharged from a container with a relatively simple structure and mixed. When two-component polyurethanes are used in aerosol containers, one container is filled with a polyol compound and a low-boiling compound, and the other container is filled with a polyisocyanate compound and a low-boiling compound. The polyol liquid and polyisocyanate liquid are discharged from each container by the vapor pressure of the low-boiling compound, and polyurethane foam is formed by mixing them.

[0004] The low boiling point compounds used in aerosol containers include hydrofluorocarbons (HFCs), hydrochlorofluorocarbons (HCFCs), dimethyl ether (DME), liquefied petroleum gas (LPG), etc. Furthermore, because HFCs and HCFCs have a high global warming potential, there is a demand for alternative compounds to replace them. For example, Patent Document 1 describes a two-liquid aerosol composition for rigid polyurethane foam that contains a specific amount of a low-boiling point compound, and describes that by using liquefied petroleum gas (LPG), dimethyl ether (DME), etc. as the low-boiling point compound, there is no adverse effect on global warming. Furthermore, hydrofluoroolefins (hereinafter sometimes referred to as "HFOs") that do not pose environmental problems such as global warming and ozone layer destruction have been proposed (see, for example, Patent Document 2). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2006-169474 A [Patent Document 2] JP 2018-21199 A Summary of the Invention [Problem to be solved by the invention]

[0006] In two-component polyurethane aerosols, when the polyol liquid and isocyanate liquid are discharged from each container, a certain initial discharge amount is required. If the initial discharge amount is insufficient, the polyol liquid and the isocyanate liquid will not mix well, polyurethane foam will not be formed properly, and various performances such as flame retardancy will be reduced. As mentioned above, HFO is environmentally friendly and suitable as a foaming agent, but there is a problem that the initial discharge amount is insufficient because the vapor pressure cannot be guaranteed to be sufficient.

[0007] In recent years, due to the increasing awareness of disaster prevention, polyurethane foams used as heat insulating materials are required to have high flame retardant performance, and the use of flame retardants with high flame retardant effects has been considered. However, most flame retardants with high flame retardant effects are solid, and when mixed with polyol, for example, the fluidity of the polyol liquid is reduced. As a result, the initial discharge amount of the polyol liquid in the aerosol becomes even more insufficient, and problems such as the polyol liquid not being mixed sufficiently with the isocyanate liquid occur, resulting in a problem that the flame retardancy cannot be sufficiently improved.

[0008] Therefore, an object of the present invention is to provide a polyol composition that exhibits good dischargeability even when the polyol composition uses an HFO as a foaming agent. [Means for solving the problem]

[0009] Means for Solving the Problems The present inventors have conducted intensive studies to solve the above-mentioned problems, and as a result have found that the above-mentioned problems can be solved by using a low-boiling point compound in addition to an HFO, thereby completing the present invention. That is, the present invention is as follows.

[0010] [1] A polyol composition containing a polyol, a catalyst, a hydrofluoroolefin, and a low-boiling compound, wherein the low-boiling compound is a low-boiling compound other than a hydrofluoroolefin having a boiling point of 10°C or less, and the polyol composition is filled into a container so that the internal pressure at 35°C is 0.3 to 1.0 MPa. [2] The polyol composition according to the above [1], having a non-volatile content of 80 to 99 mass %. [3] The polyol composition according to the above [1] or [2], wherein the low-boiling point compound is at least one selected from nitrogen and carbon dioxide. [4] The polyol composition according to any one of the above [1] to [3], wherein the hydrofluoroolefin is at least one selected from trans-1,3,3,3-tetrafluoropropene and trans-1-chloro-3,3,3-trifluoropropene. [5] The polyol composition according to any one of the above [1] to [4], further comprising a phosphoric acid ester. [6] The polyol composition according to any one of the above [1] to [5], further comprising a filler. [7] A mixing system comprising a first container filled with the polyol composition according to any one of [1] to [6] above, and a second container filled with an isocyanate composition, the mixing system mixing the polyol composition discharged from the first container with the isocyanate composition discharged from the second container, wherein the internal pressures of the first container and the second container are each in the range of 0.3 to 1.0 MPa. [8] A polyurethane foam obtained by mixing and foaming a polyol composition and an isocyanate composition in the mixing system described in [7] above. Effect of the Invention

[0011] According to the present invention, it is possible to provide a polyol composition that uses an HFO as a foaming agent and that exhibits good dischargeability. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a conceptual diagram showing one embodiment of a mixing system of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] [Polyol composition] The polyol composition of the present invention contains a polyol, a catalyst, a hydrofluoroolefin, and a low-boiling compound. <Polyol> Examples of the polyol used in the present invention include polylactone polyols, polycarbonate polyols, aromatic polyols, alicyclic polyols, aliphatic polyols, polyester polyols, polymer polyols, and polyether polyols.

[0014] Examples of the polylactone polyol include polypropiolactone glycol, polycaprolactone glycol, and polyvalerolactone glycol. Examples of polycarbonate polyols include polyols obtained by dealcoholization reaction of hydroxyl group-containing compounds such as ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, octanediol, and nonanediol with ethylene carbonate, propylene carbonate, and the like.

[0015] Examples of aromatic polyols include bisphenol A, bisphenol F, phenol novolac, and cresol novolac. Examples of alicyclic polyols include cyclohexanediol, methylcyclohexanediol, isophoronediol, dicyclohexylmethanediol, and dimethyldicyclohexylmethanediol. Examples of the aliphatic polyol include ethylene glycol, propylene glycol, butanediol, pentanediol, and hexanediol.

[0016] Examples of polyester polyols include polymers obtained by dehydration condensation of polybasic acids and polyhydric alcohols, polymers obtained by ring-opening polymerization of lactones such as ε-caprolactone and α-methyl-ε-caprolactone, and condensates of hydroxycarboxylic acids and the above-mentioned polyhydric alcohols. Examples of polybasic acids include adipic acid, azelaic acid, sebacic acid, isophthalic acid (m-phthalic acid), terephthalic acid (p-phthalic acid), and succinic acid, etc. Examples of polyhydric alcohols include bisphenol A, ethylene glycol, 1,2-propylene glycol, 1,4-butanediol, diethylene glycol, 1,6-hexane glycol, and neopentyl glycol, etc. Examples of hydroxycarboxylic acids include castor oil and reaction products of castor oil and ethylene glycol.

[0017] Examples of the polymer polyol include polymers obtained by graft polymerizing an ethylenically unsaturated compound such as acrylonitrile, styrene, methyl acrylate, or methacrylate with an aromatic polyol, an alicyclic polyol, an aliphatic polyol, or a polyester polyol, or polybutadiene polyol, or hydrogenated products thereof.

[0018] Examples of polyether polyols include polymers obtained by ring-opening polymerization of at least one alkylene oxide (hereinafter also referred to as "AO") in the presence of at least one low molecular weight active hydrogen compound having two or more active hydrogens. Examples of AO include ethylene oxide (hereinafter also referred to as "EO"), 1,2-propylene oxide (hereinafter also referred to as "PO"), 1,3-propylene oxide, 1,2-butylene oxide, and 1,4-butylene oxide. Examples of AO include PO, EO, and 1,2-butylene oxide, and more preferably PO and EO. When two or more AOs are used (for example, PO and EO), the addition method may be block addition or random addition, or a combination of these. Examples of low molecular weight active hydrogen compounds having two or more active hydrogens include diols such as ethylene glycol, propylene glycol, butylene glycol, and 1,6-hexanediol; triols such as glycerin and trimethylolpropane; tetrahydric to octahydric alcohols such as pentaerythritol, sorbitol, mannitol, sorbitan, diglycerin, and dipentaerythritol; sucrose, glucose, mannose, fructose, methyl glucoside, and derivatives thereof; phloroglucinol, cresol, etc. Examples of suitable polyols include aromatic polyols such as pyrogallol, catechol, hydroquinone, bisphenol A, bisphenol F, bisphenol S, 1,3,6,8-tetrahydroxynaphthalene, and 1,4,5,8-tetrahydroxyanthracene; polyfunctional polyols such as castor oil polyol, (co)polymers of hydroxyalkyl (meth)acrylates, and polyvinyl alcohol; condensates of phenol and formaldehyde (novolaks), amines such as ethylenediamine, and butylenediamine.

[0019] The polyol used in the present invention is preferably a polyester polyol or a polyether polyol. The polyol may be a polyester polyol, but may be used in combination with a polyol other than the polyester polyol, such as a polyether polyol. A polyol having two hydroxyl groups is also preferred. Among them, polyester polyols obtained by dehydration condensation of a polybasic acid having an aromatic ring, such as isophthalic acid (m-phthalic acid) or terephthalic acid (p-phthalic acid), with a dihydric alcohol, such as bisphenol A, ethylene glycol, or 1,2-propylene glycol, are more preferred. From the viewpoint of improving flame retardancy, out of 100 parts by mass of polyol, it is preferable that the polyester polyol be 20 parts by mass or more, more preferably 50 parts by mass or more, even more preferably 80 parts by mass or more, and particularly preferably 100 parts by mass.

[0020] The hydroxyl value of the polyol is preferably 20 to 300 mgKOH / g, more preferably 30 to 250 mgKOH / g, and even more preferably 50 to 220 mgKOH / g. When the hydroxyl value of the polyol is equal to or less than the upper limit, the viscosity of the polyol composition is likely to decrease, which is preferable in terms of handleability, etc. On the other hand, when the hydroxyl value of the polyol is equal to or more than the lower limit, the crosslink density of the polyurethane foam increases, thereby increasing the strength. The hydroxyl value of the polyol can be measured in accordance with JIS K 1557-1:2007.

[0021] The content of the polyol in the polyol composition of the present invention is preferably 10 to 80% by mass, more preferably 20 to 75% by mass, and even more preferably 25 to 70% by mass. When the content of the polyol is equal to or more than the lower limit, the polyol and the polyisocyanate are easily reacted. On the other hand, when the content of the polyol is equal to or less than the upper limit, the viscosity of the polyol composition does not become too high, and the handling property is improved.

[0022] <Catalyst> The polyol composition of the present invention preferably contains at least a trimerization catalyst as a catalyst, and more preferably contains both a resinification catalyst and a trimerization catalyst. (Resinification catalyst) The resinification catalyst is a catalyst that promotes the reaction between a polyol compound and a polyisocyanate compound. Examples of the resinification catalyst include amine-based catalysts such as imidazole compounds and piperazine compounds, and metal-based catalysts. Examples of the imidazole compound include tertiary amines in which the secondary amine at the 1-position of the imidazole ring is substituted with an alkyl group, an alkenyl group, or the like. Specific examples include N-methylimidazole, 1,2-dimethylimidazole, 1-ethyl-2-methylimidazole, 1-methyl-2-ethylimidazole, 1,2-diethylimidazole, and 1-isobutyl-2-methylimidazole. In addition, examples include imidazole compounds in which the secondary amine in the imidazole ring is substituted with a cyanoethyl group. Furthermore, examples of the piperazine compound include tertiary amines such as N-methyl-N'N'-dimethylaminoethylpiperazine and trimethylaminoethylpiperazine. Examples of the amine catalyst include, in addition to imidazole compounds and piperazine compounds, various tertiary amines such as pentamethyldiethylenetriamine, triethylamine, N-methylmorpholinebis(2-dimethylaminoethyl)ether, N,N,N',N",N"-pentamethyldiethylenetriamine, N,N,N'-trimethylaminoethyl-ethanolamine, bis(2-dimethylaminoethyl)ether, N,N-dimethylcyclohexylamine, diazabicycloundecene, triethylenediamine, tetramethylhexamethylenediamine, and tripropylamine.

[0023] Examples of the metal catalyst include metal salts of lead, tin, bismuth, copper, zinc, cobalt, nickel, etc., and preferably organic acid metal salts of lead, tin, bismuth, copper, zinc, cobalt, nickel, etc. More preferred are organic acid tin salts such as dibutyltin dilaurate, dioctyltin dilaurate, dioctyltin versatate, and organic acid bismuth salts such as bismuth trioctate, bismuth tris(2-ethylhexanoate), and among these, organic acid bismuth salts are preferred. The resinification catalyst may be used alone or in combination of two or more. Among the above, imidazole compounds are preferred.

[0024] The content of the resinification catalyst (the total when two or more kinds are contained) is preferably 1 to 30 parts by mass, more preferably 3 to 25 parts by mass, and even more preferably 5 to 20 parts by mass, relative to 100 parts by mass of the polyol. When the content of the resinification catalyst is equal to or more than the lower limit, urethane bonds are easily formed and the reaction proceeds quickly. On the other hand, when the content is equal to or less than the upper limit, the reaction rate is easily controlled. In the polyol composition of the present invention, a substance containing impurities (e.g., diluent, etc.) other than the resinification catalyst component functioning as a resinification catalyst may be blended together with the resinification catalyst. In this case, the mass of only the resinification catalyst component excluding the impurities from the substance is the "content of the resinification catalyst".

[0025] (trimerization catalyst) The polyol composition of the present invention preferably contains a trimerization catalyst. The trimerization catalyst is a catalyst that reacts the isocyanate group contained in the polyisocyanate to trimerize it and promote the formation of an isocyanurate ring. The inclusion of the trimerization catalyst improves the flame retardancy of the polyurethane foam. As the trimerization catalyst, nitrogen-containing aromatic compounds such as tris(dimethylaminomethyl)phenol, 2,4-bis(dimethylaminomethyl)phenol, and 2,4,6-tris(dialkylaminoalkyl)hexahydro-S-triazine, alkali metal salts of carboxylic acids such as potassium acetate, potassium 2-ethylhexanoate, and potassium octylate, tertiary ammonium salts such as trimethylammonium salts, triethylammonium salts, and triphenylammonium salts, and quaternary ammonium salts such as tetramethylammonium salts, tetraethylammonium salts, tetraphenylammonium salts, triethylmonomethylammonium salts, and quaternary ammonium salts of carboxylic acids can be used. These may be used alone or in combination of two or more.

[0026] Among the above, one or more carboxylates selected from the group consisting of alkali metal carboxylates and quaternary ammonium carboxylates are preferred. Among these, quaternary ammonium carboxylates are more preferred. With these carboxylate trimerization catalysts, the reaction proceeds immediately from the start of the trimerization reaction, and the amount of unreacted isocyanate can be reduced. As a result, the flame retardancy of the polyurethane foam can be improved.

[0027] The content of the trimerization catalyst (the total when two or more types are contained) is preferably 0.5 to 20 parts by mass, more preferably 1 to 15 parts by mass, and even more preferably 2 to 10 parts by mass, based on 100 parts by mass of the polyol. When the content of the trimerization catalyst is equal to or more than the lower limit, trimerization of the polyisocyanate occurs easily, and the flame retardancy of the obtained polyurethane foam is improved. On the other hand, when the content of the trimerization catalyst is equal to or less than the upper limit, the reaction can be easily controlled. In the polyol composition of the present invention, a substance containing impurities other than the trimerization catalyst component that functions as a trimerization catalyst may be blended together with the trimerization catalyst. In this case, the mass of only the trimerization catalyst component, excluding the impurities, from the substance is the "content of the trimerization catalyst."

[0028] The total content of the trimerization catalyst and the resinification catalyst in the polyol composition of the present invention is not particularly limited, but is preferably 1 to 40 parts by mass, more preferably 5 to 35 parts by mass, and even more preferably 10 to 30 parts by mass, relative to 100 parts by mass of the polyol. When the total content of both catalysts in the polyol composition of the present invention is equal to or more than these lower limits, the formation of urethane bonds and trimerization proceed appropriately, and the flame retardancy of the polyurethane foam tends to be good. When the total content of both catalysts in the polyol composition of the present invention is equal to or less than these upper limits, the urethane formation and trimerization reactions are easily controlled.

[0029] In the polyol composition of the present invention, the trimerization catalyst content / resinification catalyst content is preferably in the range of 1 / 10 to 1 / 1, more preferably 1 / 5 to 1 / 1, and even more preferably 1 / 3 to 1 / 1. When the trimerization catalyst content / resinification catalyst content is equal to or greater than the lower limit, the formation of urethane bonds and trimerization proceed appropriately, and the flame retardancy of the polyurethane foam tends to be good. On the other hand, when the trimerization catalyst content / resinification catalyst content is equal to or less than the upper limit, the contents of the resinification catalyst and trimerization catalyst can be reduced.

[0030] <Foaming agent> The polyol composition of the present invention contains a hydrofluoroolefin as a blowing agent. Hydrofluoroolefins (HFOs) are highly stable as blowing agents, are less likely to reduce catalytic activity, and can also reduce the environmental impact. Examples of hydrofluoroolefins include fluoroalkenes having about 3 to 6 carbon atoms. The hydrofluoroolefins may also be hydrochlorofluoroolefins having chlorine atoms, and therefore may be chlorofluoroalkenes having about 3 to 6 carbon atoms. Preferred hydrofluoroolefins are fluoroalkenes having 3 or 4 carbon atoms, and more preferred hydrofluoroolefins are fluoroalkenes having 3 carbon atoms.

[0031] More specifically, 3,3,3-trifluoropropene (HFO-1243zf), trans-1,3,3,3-tetrafluoropropene (HFO-1234ze(E)), cis-1,3,3,3-tetrafluoropropene (HFO-1234ze(Z)), 2,3,3,3-tetrafluoropropene (HFO-1234yf), 1,1,3,3-tetrafluoropropene, trans-1,2,3,3,3-pentafluoropropene (HFO-1225y e(E)), cis-1,2,3,3,3-pentafluoropropene (HFO-1225ye(Z)), 1,1,3,3,3-pentafluoropropene (HFO-1225zc), 1,1,2,3,3-pentafluoropropene (HFO-1225yc), trans-1-chloro-3,3,3-trifluoropropene (HFO-1233zd(E)), 1,1,1,4,4,4-hexafluorobut-2-ene (HFO-1336mzz), and the like. Among these HFOs, trans-1,3,3,3-tetrafluoropropene (HFO-1234ze(E), cis-1,3,3,3-tetrafluoropropene (HFO-1234ze(Z)) and trans-1-chloro-3,3,3-trifluoropropene (HFO-1233zd(E)) are particularly preferred, with trans-1,3,3,3-tetrafluoropropene and trans-1-chloro-3,3,3-trifluoropropene being particularly preferred. The hydrofluoroolefins may be used alone or in combination of two or more kinds.

[0032] The content of HFO in the polyol composition is preferably 1 to 100 parts by mass, more preferably 10 to 90 parts by mass, further preferably 20 to 70 parts by mass, and particularly preferably 30 to 50 parts by mass, relative to 100 parts by mass of polyol. When the content is equal to or more than the lower limit, foaming is promoted, foamability is improved, and the density of the obtained polyurethane foam can be reduced. On the other hand, when the content is equal to or less than the upper limit, excessive foaming can be suppressed.

[0033] The polyol composition of the present invention may contain a blowing agent other than hydrofluoroolefin. Examples of the blowing agent other than hydrofluoroolefin include water, organic physical blowing agent, inorganic physical blowing agent, etc., but the organic physical blowing agent and the inorganic physical blowing agent are preferably low-boiling compounds as described below, and in the present invention, they are described below as low-boiling compounds. The polyol composition of the present invention may contain water as a blowing agent from the viewpoint of adjusting the isocyanate index and ease of handling.

[0034] <Low boiling point compounds> The polyol composition of the present invention contains a low-boiling point compound other than hydrofluoroolefin. Here, the low-boiling point compound refers to a compound having a boiling point of 10°C or less. In this specification, the boiling point means the boiling point at 1 atmospheric pressure. In addition, it means the boiling point of the low-boiling point compound alone, and does not mean, for example, the boiling point of the azeotropic low-boiling point compound with another compound. The polyol composition of the present invention contains a low-boiling point compound in addition to HFO, so that the discharge is stable and the dischargeability is good. When the boiling point of the low-boiling compound exceeds 10° C., it becomes difficult to extrude the polyol composition, particularly the polyol composition containing a filler. From the viewpoint of making the polyol composition easier to extrude, the boiling point of the low-boiling compound is preferably 0° C. or lower, more preferably −10° C. or lower, even more preferably −15° C. or lower, particularly preferably −20° C. or lower, even more preferably −70° C. or lower, and particularly preferably −180° C. or lower.

[0035] The low boiling point compound used in the present invention is not particularly limited as long as it has a boiling point of 10° C. or less, and examples thereof include hydrocarbons having 2 to 5 carbon atoms, dimethyl ether (DME, boiling point: −24° C.), hydrofluorocarbons (HFCs), air (compressed air), carbon dioxide (boiling point: −78.5° C.), inert gases, etc. Examples of inert gases include nitrogen (boiling point: −195.8° C.), argon (boiling point: −185.8° C.), and helium (boiling point: −268.9° C.). Specific examples of hydrocarbons having 2 to 5 carbon atoms include propane (boiling point: -42°C), isobutane (boiling point: -11.7°C), normal butane (boiling point: -0.5°C), etc. Also, a mixture of dimethyl ether and propane, isobutane, or normal butane may be used, or LPG (liquefied petroleum gas) containing propane and butanes as main components may be used. Specific examples of hydrofluorocarbons (HFCs) include trifluoromethane (HFC-23, boiling point: about -82°C), difluoromethane (HFC-32, boiling point: about -51.7°C), and 1,1,1,2-tetrafluoroethane (HFC-134a, boiling point: about -26.2°C).

[0036] Among these, it is preferable to use an inert gas such as air, carbon dioxide, or nitrogen. By using air, carbon dioxide, or an inert gas, the low boiling point compound does not become flammable, and the flame retardancy of the polyurethane foam is easily improved. In addition, from the viewpoint of handling, it is more preferable that the low boiling point compound contains at least one selected from carbon dioxide and nitrogen, and nitrogen is particularly preferable because it has a lower boiling point and is less compatible with other compounds constituting the polyol composition. Therefore, in the present invention, a combination of HFO and nitrogen is most preferable.

[0037] The content of the low boiling point compound is preferably 0.01 to 10 parts by mass, more preferably 0.02 to 5 parts by mass, still more preferably 0.03 to 3 parts by mass, and particularly preferably 0.03 to 1 part by mass, relative to 100 parts by mass of the polyol. When the content of the low boiling point compound is equal to or more than the lower limit, a sufficient initial discharge amount can be ensured, and a good polyurethane foam can be formed. On the other hand, when the content of the low boiling point compound is equal to or less than the upper limit, the initial discharge amount is not excessive, the foam density is not too low, and appropriate physical properties can be obtained.

[0038] <Phosphate ester> The polyol composition of the present invention may contain a phosphoric acid ester. When the polyol composition of the present invention contains a phosphoric acid ester, the flame retardancy of the polyurethane foam can be improved. The phosphoric acid ester is preferably a liquid flame retardant that is liquid at room temperature (23° C.) and normal pressure (1 atm.) By including a phosphoric acid ester, which is a liquid flame retardant, the flame retardancy of the polyurethane composition of the present invention can be improved without substantially decreasing the discharge flow rate and mixability of the polyol composition of the present invention.

[0039] As the phosphoric acid ester, it is preferable to use monophosphoric acid ester, condensed phosphoric acid ester, etc. As the monophosphoric acid ester, for example, trialkyl phosphate such as trimethyl phosphate, triethyl phosphate, tributyl phosphate, tri(2-ethylhexyl)phosphate, halogen-containing phosphoric acid ester such as tris(β-chloropropyl)phosphate, trialkoxy phosphate such as tributoxyethyl phosphate, aromatic ring-containing phosphoric acid ester such as tricresyl phosphate, trixylenyl phosphate, tris(isopropylphenyl)phosphate, cresyl diphenyl phosphate, diphenyl(2-ethylhexyl)phosphate, monoisodecyl phosphate, diisodecyl phosphate, and other acidic phosphoric acid esters are listed. Among them, halogen-containing phosphoric acid ester, particularly tris(β-chloropropyl)phosphate, etc. are preferable.

[0040] Examples of the condensed phosphate ester include aromatic condensed phosphate esters such as trialkyl polyphosphate, resorcinol polyphenyl phosphate, bisphenol A polycresyl phosphate, and bisphenol A polyphenyl phosphate. Commercially available condensed phosphate esters include, for example, "CR-733S", "CR-741", and "CR747" manufactured by Daihachi Chemical Industry Co., Ltd., and "ADEKA STAB PFR" and "FP-600" manufactured by ADEKA Corporation.

[0041] Among these, from the viewpoint of reducing the viscosity of the mixture of the polyol composition and the isocyanate composition of the present invention to facilitate the production of a polyurethane foam, and from the viewpoint of improving the flame retardancy of the polyurethane foam, monophosphate esters are preferred, and tris(β-chloropropyl) phosphate is more preferred.

[0042] When a phosphoric acid ester is contained, the content of the phosphoric acid ester in the polyol composition is preferably 5 to 90 parts by mass, more preferably 15 to 80 parts by mass, and even more preferably 25 to 70 parts by mass, based on 100 parts by mass of the polyol. By making the content of the phosphoric acid ester equal to or more than these lower limits, the effect of containing the phosphoric acid ester is easily exhibited. In addition, by making the content equal to or less than the upper limits, the foaming of the polyurethane foam is not inhibited by the phosphoric acid ester.

[0043] <Filler> The polyol composition of the present invention preferably contains a filler. By including a filler, various properties such as flame retardancy of the polyurethane foam can be easily improved. The filler preferably contains a flame retardant. By using a flame retardant as a filler, high flame retardancy can be imparted to the polyurethane foam. The flame retardant used as the filler is a solid flame retardant. In the present invention, by using a solid flame retardant, the flame retardancy can be more effectively improved. The solid flame retardant is a flame retardant that becomes solid at room temperature (23°C) and normal pressure (1 atm). The solid flame retardant used in the present invention is preferably at least one selected from the group consisting of phosphate-containing flame retardants, red phosphorus-based flame retardants, bromine-containing flame retardants, boron-containing flame retardants, antimony-containing flame retardants, metal hydroxides, and needle-shaped fillers.

[0044] Examples of the phosphate-containing flame retardant include phosphates consisting of salts of various phosphoric acids and at least one metal or compound selected from metals in Groups IA to IVB of the periodic table, ammonia, aliphatic amines, aromatic amines, and heterocyclic compounds containing nitrogen in the ring. The phosphoric acid is not particularly limited, and may be a monophosphoric acid such as phosphorous acid or hypophosphorous acid, or may be pyrophosphoric acid, polyphosphoric acid, or the like. Examples of metals in Groups IA to IVB of the periodic table include lithium, sodium, calcium, barium, iron (II), iron (III), and aluminum. Examples of the aliphatic amine include methylamine, ethylamine, diethylamine, triethylamine, ethylenediamine, piperazine, etc. Examples of the aromatic amine include aniline, o-triidine, 2,4,6-trimethylaniline, anisidine, 3-(trifluoromethyl)aniline, etc. Examples of the heterocyclic compound containing nitrogen in the ring include pyridine, triazine, melamine, etc.

[0045] Specific examples of phosphate-containing flame retardants include monophosphates such as aluminum phosphite and aluminum triphosphate, pyrophosphates, polyphosphates, etc. Here, the polyphosphates are not particularly limited, but include, for example, ammonium polyphosphate, piperazine polyphosphate, melamine polyphosphate, ammonium amide polyphosphate, aluminum polyphosphate, etc. The phosphate-containing flame retardant may be one or more of the above-mentioned compounds. In the present invention, aluminum tertiary phosphate is preferred.

[0046] The red phosphorus-based flame retardant may be composed of red phosphorus alone, may be red phosphorus coated with a resin, a metal hydroxide, a metal oxide, or the like, or may be a mixture of red phosphorus and a resin, a metal hydroxide, a metal oxide, or the like. The resin that coats the red phosphorus or is mixed with the red phosphorus is not particularly limited, but examples thereof include thermosetting resins such as phenol resins, epoxy resins, unsaturated polyester resins, melamine resins, urea resins, aniline resins, and silicone resins. From the viewpoint of flame retardancy, metal hydroxides are preferred as the compound to be coated or mixed. The metal hydroxide to be used may be appropriately selected from those described below.

[0047] The bromine-containing flame retardant is not particularly limited as long as it contains bromine in its molecular structure and is a solid at room temperature and pressure. Examples of the bromine-containing flame retardant include brominated aromatic ring-containing aromatic compounds. Examples of the brominated aromatic ring-containing aromatic compound include monomeric organic bromine compounds such as hexabromobenzene, pentabromotoluene, hexabromobiphenyl, decabromobiphenyl, decabromodiphenyl ether, octabromodiphenyl ether, hexabromodiphenyl ether, bis(pentabromophenoxy)ethane, ethylene bis(pentabromophenyl), ethylene bis(tetrabromophthalimide), and tetrabromobisphenol A.

[0048] In addition, the brominated aromatic ring-containing aromatic compound may be a bromine compound polymer.Specific examples include brominated polycarbonates such as polycarbonate oligomers produced from brominated bisphenol A as a raw material, copolymers of this polycarbonate oligomer and bisphenol A, and diepoxy compounds produced by the reaction of brominated bisphenol A and epichlorohydrin.Furthermore, examples include brominated epoxy compounds such as monoepoxy compounds obtained by the reaction of brominated phenols and epichlorohydrin, poly(brominated benzyl acrylate), brominated phenol condensates of brominated polyphenylene ether, brominated bisphenol A, and cyanuric chloride, brominated (polystyrene), poly(brominated styrene), brominated polystyrene such as crosslinked brominated polystyrene, crosslinked or non-crosslinked brominated poly(-methylstyrene), and the like. In addition, compounds other than brominated aromatic ring-containing aromatic compounds such as hexabromocyclododecane may be used. These bromine-containing flame retardants may be used alone or in combination of two or more. Among the above, brominated aromatic ring-containing aromatic compounds are preferred, and among them, monomeric organic bromine compounds such as hexabromobenzene are preferred.

[0049] The boron-containing flame retardant used in the present invention includes borax, boron oxide, boric acid, borate, etc. Examples of boron oxide include diboron trioxide, boron trioxide, diboron dioxide, tetraboron trioxide, and tetraboron pentoxide. Examples of borates include borates of alkali metals, alkaline earth metals, elements of Groups 4, 12, and 13 of the periodic table, and ammonium. Specific examples include alkali metal borates such as lithium borate, sodium borate, potassium borate, and cesium borate, alkaline earth metal borates such as magnesium borate, calcium borate, and barium borate, zirconium borate, zinc borate, aluminum borate, and ammonium borate. The boron-containing flame retardants may be used alone or in combination of two or more kinds. The boron-containing flame retardant used in the present invention is preferably a borate, more preferably zinc borate.

[0050] Examples of antimony-containing flame retardants include antimony oxide, antimony salts, and pyroantimony salts. Examples of antimony oxide include antimony trioxide and antimony pentoxide. Examples of antimony salts include sodium antimonate and potassium antimonate. Examples of pyroantimonate include sodium pyroantimonate and potassium pyroantimonate. The antimony-containing flame retardants may be used alone or in combination of two or more. The preferred antimony-containing flame retardant for use in the present invention is antimony trioxide.

[0051] Examples of the metal hydroxides used in the present invention include magnesium hydroxide, calcium hydroxide, aluminum hydroxide, iron hydroxide, nickel hydroxide, zirconium hydroxide, titanium hydroxide, zinc hydroxide, copper hydroxide, vanadium hydroxide, and tin hydroxide. The metal hydroxides may be used alone or in combination of two or more. The preferred metal hydroxide used in the present invention is aluminum hydroxide.

[0052] Examples of needle-like fillers include potassium titanate whiskers, aluminum borate whiskers, magnesium-containing whiskers, silicon-containing whiskers, wollastonite, sepiolite, zonolite, elestadite, boehmite, rod-shaped hydroxyapatite, glass fibers, carbon fibers, graphite fibers, metal fibers, slag fibers, gypsum fibers, silica fibers, alumina fibers, silica alumina fibers, zirconia fibers, boron nitride fibers, boron fibers, and stainless steel fibers. These needle-like fillers can be used alone or in combination of two or more.

[0053] The aspect ratio (length / diameter) of the needle-like filler used in the present invention is preferably in the range of 5 to 50, and more preferably in the range of 10 to 40. The aspect ratio can be determined by observing the needle-like filler with a scanning electron microscope and measuring its length and width.

[0054] (Anti-settling agent) The polyol composition of the present invention may contain an anti-settling agent as a filler. By using the anti-settling agent, precipitation of the solid flame retardant dispersed in the polyol composition can be prevented. In addition, by using the anti-settling agent, the solid flame retardant can be easily dispersed uniformly. The anti-settling agent is generally solid at room temperature and normal pressure, and usually becomes a solid content (insoluble content) in the polyol composition.

[0055] The anti-settling agent is not particularly limited, but it is preferable to use one or more selected from, for example, carbon black, powdered silica, organic clay, etc., and among these, powdered silica is more preferable. The carbon black used in the anti-settling agent may be produced by a furnace method, a channel method, a thermal method, etc. The carbon black may be appropriately selected from commercially available products. As the powdered silica, fumed silica, colloidal silica, silica gel, etc. can be used. Of these, fumed silica is preferable. As the fumed silica, Aerosil (registered trademark) from Nippon Aerosil Co., Ltd. can be used.

[0056] The content of the anti-settling agent is not particularly limited, but is, for example, 0.5 to 20 parts by mass, preferably 1 to 15 parts by mass, more preferably 3 to 10 parts by mass, and further preferably 4 to 8 parts by mass, relative to 100 parts by mass of the polyol. By setting the content of the anti-settling agent within the above range, it is possible to prevent the settling of the solid flame retardant and improve its dispersibility without increasing the solid content more than necessary.

[0057] As the filler, inorganic fillers other than the above-mentioned solid flame retardant and anti-settling agent may be used. Examples of inorganic fillers include silica, diatomaceous earth, alumina, titanium oxide, calcium oxide, magnesium oxide, iron oxide, tin oxide, antimony oxide, ferrites, calcium carbonate, magnesium carbonate, zinc carbonate, barium carbonate, dawsonite, hydrotalcite, calcium sulfate, barium sulfate, calcium silicate, talc, clay, mica, montmorillonite, bentonite, activated clay, sepiolite, imogolite, sericite, glass beads, silica balloons, aluminum nitride, boron nitride, silicon nitride, carbon black, graphite, carbon balloons, charcoal powder, various metal powders, potassium titanate, magnesium sulfate, lead zirconate titanate, aluminum borate, molybdenum sulfide, silicon carbide, various magnetic powders, fly ash, silica alumina fiber, and zirconia fiber. These inorganic fillers may be used alone or in combination of two or more.

[0058] When the polyol composition of the present invention contains a filler, the content thereof is preferably 10 to 150 parts by mass, more preferably 30 to 130 parts by mass, even more preferably 50 to 120 parts by mass, and even more preferably 60 to 100 parts by mass, relative to 100 parts by mass of the polyol. When the content of the filler is equal to or more than the lower limit, the polyurethane foam produced using the polyol composition can be sufficiently imparted with performance such as flame retardancy. On the other hand, when the content of the filler is equal to or less than the upper limit, the flowability of the polyol is not reduced, the initial discharge amount of the polyol composition is sufficient, and the polyol composition can be sufficiently mixed with the isocyanate composition, making it possible to enhance various performances such as flame retardancy.

[0059] (Foam stabilizer) The polyol composition of the present invention may contain a foam stabilizer for the purpose of facilitating foaming of the mixture of the polyol composition and the isocyanate composition. Examples of the foam stabilizer include polyoxyalkylene-based foam stabilizers such as polyoxyalkylene alkyl ethers, and surfactants such as silicone foam stabilizers such as organopolysiloxanes. These foam stabilizers may be used alone or in combination of two or more.

[0060] The content of the foam stabilizer in the polyol composition of the present invention is preferably 0.1 to 10 parts by mass, more preferably 1 to 8 parts by mass, and even more preferably 1 to 5 parts by mass, based on 100 parts by mass of the polyol. When the content of the foam stabilizer is equal to or more than the lower limit, the mixture of the polyol composition and the isocyanate composition is easily foamed, so that a homogeneous polyurethane foam can be obtained. When the content of the foam stabilizer is equal to or less than the upper limit, the balance between the production cost and the obtained effect is optimal.

[0061] (Other ingredients) Furthermore, the polyol composition of the present invention may contain, as necessary, one or more selected from phenol-based, amine-based, sulfur-based and other antioxidants, heat stabilizers, metal inhibitors, antistatic agents, stabilizers, crosslinking agents, lubricants, softeners, pigments, and the like, within the scope of the object of the present invention.

[0062] <Non-volatile content> The non-volatile content of the polyol composition of the present invention is preferably 80 to 99% by mass, more preferably 82 to 98% by mass. If it is equal to or more than the lower limit, the drying speed of the polyurethane foam is fast and sufficient strength is obtained, and if it is equal to or less than the upper limit, the productivity is high and the foaming property and discharge property are likely to be good. The non-volatile content can be measured by the method described in the Examples.

[0063] The polyol composition of the present invention is filled into a container so that the internal pressure at 35°C is 0.3 to 1.0 MPa. If the internal pressure is less than 0.3 MPa, the injection pressure is low, and a sufficient initial discharge amount cannot be obtained, making it impossible to obtain a good polyurethane foam. On the other hand, if the internal pressure exceeds 1.0 MPa, it is necessary to use a container with high pressure resistance. Also, the initial discharge amount may be larger than necessary. From the above viewpoints, the internal pressure at 35°C is preferably in the range of 0.4 to 0.9 MPa, more preferably in the range of 0.5 to 0.8 MPa. The higher the vapor pressure of the low-boiling compound, the higher the internal pressure in the container, and the higher the compatibility with the polyol, the lower the internal pressure in the container. Therefore, the internal pressure in the container can be controlled by the vapor pressure and content of the low-boiling compound, the compatibility between the low-boiling compound and the polyol, etc.

[0064] (Method of producing polyol composition) The method for producing the polyol composition of the present invention is not particularly limited, and the composition can be produced, for example, by the following method. First, the components other than the low-boiling compound are stirred and mixed with a known stirring device, and then filled into a container such as an empty aerosol can. The aerosol can is sealed with a stem valve, and the low-boiling compound is injected from the stem valve to produce a polyol composition filled in the container.

[0065] [Mixed system] The outline of the mixing system of the present invention will be described with reference to Fig. 1. Fig. 1 is a schematic diagram showing the outline of the mixing system of the present invention. The mixing system 10 of the present invention includes a first container 11 filled with a polyol composition, a second container 12 filled with an isocyanate composition, and a static mixer (static mixer) 13 that mixes the polyol composition discharged from the first container and the isocyanate composition discharged from the second container. The internal pressure of the first container 11 and the second container 12 at 35°C is both in the range of 0.3 to 1.0 MPa. If the internal pressure is less than 0.3 MPa, the injection pressure is low and a sufficient initial discharge amount cannot be obtained. On the other hand, if the internal pressure exceeds 1.0 MPa, the container needs to be made highly pressure-resistant. From the above viewpoints, the internal pressure of the first container and the second container is both preferably in the range of 0.4 to 0.9 MPa, more preferably in the range of 0.5 to 0.8 MPa. The internal pressure of the first container and the second container may be the same or different.

[0066] The first and second containers 11 and 12 are preferably spray cans for aerosols, and are preferably sealed with stem valves. When using a stem valve, for example, after a composition other than the low boiling point compound is filled into the spray can, the container may be sealed with the stem valve, and then the low boiling point compound may be filled through the stem valve. In the first container 11, a part of the polyol composition may be vaporized to form a gas phase, and in the second container 12, a part of the isocyanate composition may be vaporized to form a gas phase. The polyol composition and the isocyanate composition discharged from the first and second containers 11, 12 are mixed while being foamed by a foaming agent or the like, and the isocyanate and the polyol react with each other to form a polyurethane foam (polyurethane composition).

[0067] The mixing system 10 also includes a static mixer (hereinafter, sometimes simply referred to as a "mixer") 13. The static mixer 13 is a mixer without a driving section, in which the fluids are mixed by passing through the inside of the tube. An example of the static mixer is one in which a mixer element 13B is arranged inside a tube 13A as shown in FIG. 1. The mixer element 13B may be one formed in a spiral shape or one formed with a plurality of baffle plates. In the mixing system 10 of the present invention, the outlets 11A, 12A of the first and second containers 11, 12 are connected to the mixer 13 via the supply lines 11B, 12B. The outlets 11A, 12A may be provided with valves such as stem valves. The polyol composition and the isocyanate composition discharged from the first and second containers 11, 12 are supplied to the mixer 13 via the supply lines 11B, 12B, respectively, and are mixed in the mixer 13. Here, it is preferable that the static mixer has an injection port divided into two holes, and the polyol composition and the isocyanate composition are preferably supplied to the mixer 13 separately from the injection ports of the two holes. This makes it possible to prevent the polyol composition and the isocyanate composition from coming into contact with each other before being injected into the mixer. The polyol composition and the isocyanate composition mixed in the mixer 13 are sprayed onto the surface to be applied by a sprayer or the like. The static mixer may also function as an injector. In that case, the mixture of the polyol composition and the isocyanate composition mixed inside the tube 13A may be injected from the tip 13C of the tube, as shown in FIG. 1.

[0068] The polyol composition and the isocyanate composition of the present invention each contain a low-boiling point compound having a boiling point of less than 10° C. The polyol composition is as described above, and the internal pressure of the first container filled with the polyol composition at 35° C. is controlled to 0.3 to 1.0 MPa by the low-boiling point compound. The preferred range of the internal pressure of the first container at 35° C. is also as described above. The internal pressure of the second container filled with the isocyanate composition at 35°C is also preferably controlled to 0.3 to 1.0 MPa by the low boiling point compound, and as described above, is preferably in the range of 0.4 to 0.9 MPa, and more preferably in the range of 0.5 to 0.8 MPa. If it is equal to or higher than the lower limit, the injection pressure is high and a sufficient initial discharge amount can be obtained. On the other hand, if it is equal to or lower than the upper limit, there is no need to use a pressure-resistant container, and the initial discharge amount does not become larger than necessary. The higher the vapor pressure of the low-boiling compound, the higher the internal pressure in the container, and the higher the compatibility with the isocyanate, the lower the internal pressure in the container. Therefore, the internal pressure in the container can be controlled by the vapor pressure and content of the low-boiling compound, the compatibility between the low-boiling compound and the isocyanate, etc. The low-boiling point compound in the polyol composition and the isocyanate composition expels the polyol composition and the isocyanate composition, and vaporizes during the expulsion to foam the polyurethane composition described below, i.e., it also functions as a foaming agent.

[0069] [Isocyanate composition] The isocyanate composition preferably contains a polyisocyanate, an HFO, and a low-boiling compound. The HFO and low-boiling compound may be the same as those used in the polyol composition. The polyisocyanate used in the isocyanate composition may be any known polyisocyanate compound used in the formation of polyurethane foams, such as aromatic polyisocyanates, alicyclic polyisocyanates, and aliphatic polyisocyanates. Examples of aromatic polyisocyanates include phenylene diisocyanate, tolylene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate, dimethyldiphenylmethane diisocyanate, triphenylmethane triisocyanate, naphthalene diisocyanate, and polymethylene polyphenyl polyisocyanate.

[0070] Examples of the alicyclic polyisocyanate include cyclohexylene diisocyanate, methylcyclohexylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, and dimethyldicyclohexylmethane diisocyanate.

[0071] Examples of the aliphatic polyisocyanate include methylene diisocyanate, ethylene diisocyanate, propylene diisocyanate, tetramethylene diisocyanate, and hexamethylene diisocyanate.

[0072] Among these, from the viewpoints of ease of use and availability, aromatic polyisocyanates are preferred, and diphenylmethane diisocyanate (MDI) and polymethylene polyphenyl polyisocyanate are more preferred. The polyisocyanate compounds may be used alone or in combination of two or more.

[0073] As described above, the isocyanate composition preferably contains HFO and a low boiling point compound. The HFO can be the same compound as that used in the polyol composition, and the preferred compounds are also the same. The HFO used in the polyisocyanate composition may be the same as or different from the HFO used in the polyol composition. The content of HFO in the polyisocyanate composition is preferably 1 to 30 parts by mass, more preferably 2 to 20 parts by mass, further preferably 2.5 to 15 parts by mass, and particularly preferably 3 to 10 parts by mass, relative to 100 parts by mass of polyisocyanate. When the content is equal to or more than the lower limit, foaming is promoted, foamability is improved, and the density of the obtained polyurethane foam can be reduced. On the other hand, when the content is equal to or less than the upper limit, excessive foaming can be suppressed.

[0074] As the low-boiling compound, any of the above-mentioned low-boiling compounds having a boiling point of 10° C. or less can be used without any particular limitation. The low-boiling compound used in the polyisocyanate composition may be the same as or different from the low-boiling compound used in the polyol composition. The content of the low-boiling compound contained in the polyisocyanate composition is preferably 0.01 to 5 parts by mass, more preferably 0.02 to 1 part by mass, and even more preferably 0.03 to 0.5 parts by mass, based on 100 parts by mass of the polyisocyanate. When the content of the low-boiling compound is equal to or more than the lower limit, a sufficient initial discharge amount can be ensured, and a good polyurethane foam can be formed. On the other hand, when the content of the low-boiling compound is equal to or less than the upper limit, the foam density does not become too low, and appropriate physical properties can be obtained. Furthermore, the isocyanate composition may appropriately contain known additives contained in polyisocyanate compounds.

[0075] The polyol composition and the isocyanate composition preferably have substantially the same volume. Specifically, the volume ratio of the isocyanate composition to the polyol composition is preferably 0.8 to 1.2, more preferably 0.9 to 1.1, and further preferably 0.95 to 1.05. Moreover, the first container and the second container can be manufactured in a similar manner as described above.

[0076] [Polyurethane composition] The polyurethane composition according to the present invention is formed from a mixture in which the polyol composition according to the present invention and the isocyanate composition are mixed in a static mixer or the like.

[0077] (Isocyanate Index) The isocyanate index of the polyurethane composition of the present invention is not particularly limited, but is preferably 200 or more. If the amount of the polyisocyanate compound relative to the polyol compound is excessive, a large amount of the trimerization catalyst is required, but in the present invention, a specific amount of the resinification catalyst is used together with the trimerization catalyst, so that the amount of the trimerization catalyst used can be reduced. If the isocyanate index is equal to or greater than the lower limit, the amount of the polyisocyanate compound relative to the polyol compound becomes excessive, which makes it easier to generate isocyanurate bonds due to the trimerization of the polyisocyanate compound, and as a result, the flame retardancy of the polyurethane foam is improved. In addition, it is possible to impart non-flammability. Furthermore, if the isocyanate index is equal to or greater than the above lower limit, it is easy to produce a polyurethane foam having an isocyanurate bond, i.e., a polyurethane foam having both flame retardancy and heat insulation at a high level. From these viewpoints, the isocyanate index is more preferably 250 or more, even more preferably 300 or more, and particularly preferably 350 or more. The isocyanate index is preferably not more than 1000, more preferably not more than 800, and particularly preferably not more than 500. When the isocyanate index is not more than the upper limit, the resulting polyurethane foam will have a good balance between flame retardancy and production costs.

[0078] The isocyanate index can be calculated by the following method. Isocyanate Index = number of equivalents of polyisocyanate compound ÷ (number of equivalents of polyol compound + number of equivalents of water) × 100 Here, each equivalent number can be calculated as follows: Equivalent number of polyisocyanate compound = Amount of polyisocyanate compound used (g) × NCO content (mass%) / Molecular weight of NCO (mol) × 100 Equivalent number of polyol compound = OHV × amount of polyol compound used (g) ÷ molecular weight of KOH (mmol) OHV is the hydroxyl value (mgKOH / g) of the polyol compound. Equivalents of water = amount of water used (g) / molecular weight of water (mol) × number of OH groups in water In the above formulas, the molecular weight of NCO is 42 (mol), the molecular weight of KOH is 56100 (mmol), the molecular weight of water is 18 (mol), and the number of OH groups in water is 2.

[0079] (Method of producing polyurethane composition) The method for producing the polyurethane composition of the present invention is not particularly limited, but the polyurethane composition is formed by mixing the polyol composition of the present invention and the isocyanate composition in a static mixer and discharging the mixture from a dispenser such as a caulking gun or spray. The method for forming the polyurethane composition of the present invention using a caulking gun is, for example, carried out as follows: The polyol composition of the present invention and the isocyanate composition are discharged from cartridge containers each filled with the two compositions, and mixed in a static mixer such as a static mixer, and the mixture is sprayed from a caulking gun to cause foaming. The method for forming the polyurethane composition of the present invention by spraying is, for example, carried out as follows: The polyol composition of the present invention and the isocyanate composition are discharged from pressure-resistant spray containers each filled with the composition, and the two compositions are mixed in a static mixer such as a static mixer, and the mixture is sprayed from the tip of the static mixer to cause foaming.

[0080] (Uses of polyurethane compositions) In the present invention, the polyurethane composition can be used in various applications, but is preferably used as a heat insulating material. The polyurethane composition preferably constitutes a polyurethane foam. By forming the polyurethane foam, the polyurethane foam has a large number of bubbles, which provides a heat insulating effect. The polyurethane composition is more preferably used as a heat insulating material for vehicles or buildings. Examples of vehicles include railroad cars, automobiles, ships, and aircraft. The polyurethane composition of the present invention has high flame retardancy by using the above-mentioned polyol composition. Therefore, from the viewpoint of disaster prevention and safety, it can be suitably used for applications in vehicles or buildings. The mixing system of the present invention is also suitable for use as a small device and is well suited for repair applications. EXAMPLES

[0081] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these.

[0082] The components used in the examples and comparative examples are shown below, and the content (parts by mass) of each component is shown in Table 1. 1) Polyol compound: phthalic acid polyester polyol (manufactured by Kawasaki Chemical Industries, Ltd., product name: Maximol RLK-087, hydroxyl value = 200 mg KOH / g) 2) Trimerization catalyst: quaternary ammonium carboxylate (concentration 45 to 55% by mass, diluted with ethylene glycol) (manufactured by Evonik Japan, product name: DABCO TMR-7) 3) Resinification catalyst: Imidazole derivative (concentration 65-75% by mass, Kao Corporation, product name: KL No. 390) 4) Liquid flame retardant (phosphate ester): Tris(β-chloropropyl)phosphate (manufactured by Daihachi Chemical Industry Co., Ltd., product name: TMCPP) 5) Solid flame retardants (fillers) Red phosphorus: manufactured by Rinkagaku Kogyo Co., Ltd. Product name: Nova Excel 140 Zinc borate: Hayakawa Shoji Co., Ltd., product name: FIREBREAK ZB Brominated flame retardant: Ethylenebis(pentabromophenyl), manufactured by Albemarle Corporation, product name: SAYTEX (registered trademark) 8010 6) Anti-settling agent: Fumed silica (manufactured by Nippon Aerosil Co., Ltd., product name: Aerosil R976S) 7) HFO: HFO-1234ze (trans-1,3,3,3-tetrafluoropropene): manufactured by Honeywell, product name: Solstice (registered trademark) GBA, boiling point: -19°C 8)Low boiling point compounds Nitrogen, boiling point: -195.8℃ 9) Polyisocyanate: Diphenylmethane-4,4'-diisocyanate (MDI), manufactured by Bayer, product name: DESMODUR (registered trademark) 44LV20

[0083] Examples 1 to 6 and Comparative Examples 1 to 2 The components other than the low boiling point compound were mixed in the amounts shown in Table 1, and the mixture was poured into an empty aerosol can. The aerosol can was then sealed with a stem valve. The low boiling point compound was poured through the stem valve to the mass shown in Table 1, to form a first container. Next, the polyisocyanate and HFO were poured into another empty aerosol can so that the masses thereof were as shown in Table 1, and the aerosol can was sealed with the stem valve. A low-boiling compound was poured into the stem valve so that the masses thereof were as shown in Table 1, to form a second container. The initial discharge amount, discharge ratio, internal pressure, and non-volatile content of the first and second containers were evaluated by the methods described below. The results are shown in Table 1.

[0084] (1)Initial discharge amount The masses of the first container (aerosol can) and the second container (aerosol can) prepared in each Example and Comparative Example were measured. Then, the stem valves of the two aerosol cans were pressed simultaneously to eject the polyol composition and the isocyanate composition for 10 seconds, and the masses of the aerosol cans were measured. The change in mass of the aerosol can before and after ejection was evaluated based on the following evaluation criteria. (Evaluation Criteria) ◎: Over 60g, under 90g ○: 30g or more, but less than 60g, or 90g or more, but less than 120g ×: Less than 30g, 120g or more

[0085] (2) Discharge ratio The masses of the first container (aerosol can) and the second container (aerosol can) prepared in each Example and Comparative Example were measured. Next, the stem valves of the two aerosol cans were pressed simultaneously to discharge the polyol composition and the isocyanate composition for 5 seconds, and the masses of the aerosol cans were measured. This operation was repeated, and when the amount discharged in 5 seconds became less than 10 g, the discharge test was terminated, and the total amount of each discharged composition was calculated. The value obtained by dividing the total amount by the initial content volume was defined as the discharge ratio. The evaluation criteria are as follows. (Evaluation Criteria) ◎: 60% or more, 100% or less ○: 30% or more, less than 60% ×: 0% or more, less than 30%

[0086] (3) Method for measuring internal pressure In each of the Examples and Comparative Examples, each container filled with the polyol composition and the polyisocyanate composition was immersed in a constant temperature water bath at 35°C for 90 minutes, and then the container was shaken up and down to homogenize the contents. A Bourdon tube pressure gauge was connected to the stem valve of the container to measure the internal pressure of each container. (4) Non-volatile content The liquid agent discharged from the aerosol can was placed in a 1000 ml beaker and stirred at 400 rpm for 12 hours on a hot plate at 40° C. to remove the volatile components. The weight of the aerosol can before discharge was W0, the weight of the aerosol can after discharge was W1, and the weight of the discharged material after volatilization was W2, and the non-volatile content (mass%) was calculated by {W2 / (W0-W1)}×100.

[0087] [Table 1] *The values ​​for the polyol composition and isocyanate composition are in parts by mass, and the units for the internal pressure are in MPa.

[0088] The examples showed good initial discharge amounts and good discharge ratios. On the other hand, in Comparative Example 1, in which no HFO was used as a foaming agent, the initial discharge amount of the polyol composition was insufficient and the discharge ratio was also poor. In Comparative Example 2, in which no low-boiling point compound was used in the polyol composition and the isocyanate composition, the internal pressure of both the first container and the second container was less than 0.3 MPa, the initial discharge amounts of the polyol composition and the isocyanate composition were insufficient and the discharge ratio was also poor. [Explanation of symbols]

[0089] 10 Mixed Systems 11 First Container 12 Second Container 11A, 12A outlet 11B,12B supply line 13 Static mixer 13A Body 13B Mixer Element 13C Tip

Claims

1. A polyol composition comprising a polyol, a catalyst, a hydrofluoroolefin, and a low-boiling compound, The low-boiling compound is at least one selected from nitrogen and carbon dioxide, A polyol composition filled into a container so that the internal pressure at 35°C is 0.3 to 1.0 MPa.

2. The polyol composition according to claim 1, having a non-volatile content of 80 to 99 mass %.

3. 3. The polyol composition according to claim 1, wherein the hydrofluoroolefin is at least one selected from the group consisting of trans-1,3,3,3-tetrafluoropropene and trans-1-chloro-3,3,3-trifluoropropene.

4. The polyol composition according to any one of claims 1 to 3, further comprising a phosphoric acid ester.

5. The polyol composition according to any one of claims 1 to 4, further comprising a filler.

6. A mixing system comprising a first container filled with the polyol composition according to any one of claims 1 to 5 and a second container filled with an isocyanate composition, the mixing system mixing the polyol composition discharged from the first container with the isocyanate composition discharged from the second container, wherein the internal pressures of the first container and the second container are each in the range of 0.3 to 1.0 MPa.

7. A polyurethane foam produced by mixing and foaming the polyol composition and the isocyanate composition in the mixing system according to claim 6.

Citation Information

Patent Citations

  • 2-pack type aerosol composition used for hard polyurethane foam

    JP2006169474A

  • Azeotrope-like compositions including cis-1-chloro-3,3,3-trifluoropropene

    JP2018021199A

  • Splay can, polyurethane composition, and mixing system

    JP2020186046A

  • Mixed liquid agent, polyurethane composition, polyurethane foam, spray can, and mixing system

    WO2020067139A1