Poly(butylene oxide) polyol-based polyurethane cast elastomers and methods for making polyurethane cast elastomers - Patents.com
A hydroxyl-containing copolymer of butylene oxide and ethylene oxide, combined with a one-shot process, addresses the slow reactivity of poly(butylene oxide) polyols, achieving faster curing and improved mechanical properties in polyurethane elastomers.
Patent Information
- Application Number
- JP2021515216
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-09-28
- Filing Date
- 2019-09-17
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2039-09-17
AI Technical Summary
Poly(butylene oxide) polyols used in polyurethane cast elastomers have slow reactivity due to slow-reacting terminal secondary hydroxyl groups, leading to long curing times and increased production costs.
A hydroxyl-containing copolymer of butylene oxide and ethylene oxide with a high percentage of primary hydroxyl groups and limited oxyethylene content is used, along with a one-shot process involving polyisocyanate, chain extender, and crosslinker, to enhance reactivity and maintain hydrophobicity.
The solution results in faster curing times and the production of highly hydrophobic polyurethanes with excellent mechanical properties, without sacrificing hydrophobicity or elongation.
Smart Images

Figure 0007579240000001 
Figure 0007579240000002 
Figure 0007579240000003
Abstract
Description
[Technical field]
[0001] The present invention relates to polyurethanes and methods for making such polyurethanes.
[0002] Polyurethane cast elastomers are typically segmented polymers with "soft" and "hard" segments. The soft segments are characterized by a low glass transition temperature, whereas the hard segments have a glass transition temperature much higher than room temperature. The differentiation into these segments comes from the raw materials used to make the elastomer. The soft segments are derived from polyols with hydroxyl equivalent weights of 350 or more. Polyether polyols are very commonly used in cast polyurethane formulations to produce the soft segments. The hard segments are derived from polyisocyanates and chain extenders.
[0003] Poly(butylene oxide) polyols are potentially good candidates for making polyurethane cast elastomer products, in part because they are very hydrophobic materials and impart hydrophobicity to elastomers. However, their use in industrial processes is very limited due to the slow reactivity of their terminal secondary hydroxyl groups. Poly(butylene oxide)-based cast elastomer formulations react very slowly, requiring long cure times. This reduces production rates, reduces equipment usage, and increases costs.
[0004] A common method of increasing the reactivity of poly(butylene oxide) is to cap the ends of the polymer chains with ethylene oxide. This introduces fast-reacting primary hydroxyl groups. Unfortunately, this has not proven to be an acceptable solution. Ethylene oxide only poses difficulties for secondary hydroxyl groups at the ends of poly(butylene oxide) chains. Conversely, ethylene oxide adds very rapidly to primary hydroxyl groups, such as those formed when another molecule of ethylene oxide is ring-opened. As a result, it is very difficult to add ethylene oxide to poly(butylene oxide) to obtain a high concentration of primary hydroxyl groups. What tends to happen is that when secondary hydroxyl groups are oxyethylated to form primary hydroxyl groups, further ethylene oxide polymerization occurs almost exclusively at those sites, rather than being distributed throughout all the chains. The result is that most chain ends do not have terminal (primary hydroxyl) oxyethylene groups, but some chain ends have long poly(ethylene oxide) chains. This is undesirable for two reasons: The molecular weight distribution broadens (due to the combination of short chains of poly(butylene oxide) terminating in secondary hydroxyl groups and long chains of poly(butylene oxide) capped with long poly(ethylene oxide) chains), and most of the hydroxyl groups in the product tend to be the slow-reacting secondary hydroxyl groups. The latter problem can be overcome to some extent by polymerizing large amounts of ethylene oxide into poly(butylene oxide). Gradually more and more chain ends are oxyethylated, but the overall content of oxyethylene groups becomes high, resulting in a loss of the desired hydrophobicity of the polyol and the resulting elastomer.
[0005] Thus, there is a need for poly(butylene oxide) polyols that are highly reactive while still maintaining high hydrophobicity. Similarly, there is also a need for a process for preparing cast polyurethane elastomers from poly(butylene oxide) polyols that produces hydrophobic elastomers while having a reasonably short cure time.
[0006] The invention in one aspect is a hydroxyl-containing copolymer of butylene oxide and ethylene oxide having a hydroxyl equivalent weight of at least 150, an average of 1.8 to 6 hydroxyl groups per molecule, of which at least 70% are primary hydroxyl groups, and an oxyethylene content of 10% by weight or less, based on the weight of the copolymer.
[0007] The copolymers are characterized by having faster reactivity than poly(butylene oxide) homopolymers of similar equivalent weight and hydroxyl functionality, while at the same time being hydrophobic.
[0008] In another aspect, the invention is a polyurethane that is the reaction product of at least one polyisocyanate, at least one chain extender and / or at least one crosslinker, and at least one hydroxyl-containing copolymer of butylene oxide and ethylene oxide having a hydroxyl equivalent weight of at least 150, an average of 1.8 to 6 hydroxyl groups per molecule, of which at least 70% are primary hydroxyl groups, and an oxyethylene content of 10% by weight or less, based on the weight of the copolymer.
[0009] Polyurethane is highly hydrophobic, as characterized by low water absorption according to the test method described below, and has very good mechanical properties.
[0010] In another aspect, the invention is a one-shot process for making polyurethanes comprising forming a reaction mixture comprising isocyanate-reactive materials including one or more polyisocyanates having a number average isocyanate equivalent weight of 200 or less, at least one chain extender and / or at least one crosslinker, and at least one hydroxyl-containing copolymer of butylene oxide and ethylene oxide, the copolymer of butylene oxide and ethylene oxide having a hydroxyl equivalent weight of at least 150, an average of 1.8 to 6 hydroxyl groups per molecule, of which at least 70% are primary hydroxyl groups, and an oxyethylene content of 10% by weight or less, based on the weight of the copolymer; and curing the reaction mixture in one step to form the polyurethane.
[0011] The process is characterized by reasonably short curing times and the production of hydrophobic polyurethanes with very good mechanical properties.
[0012] For purposes of this invention, a "one-shot" process is characterized in that i) the polyisocyanate has a number average isocyanate equivalent weight of 200 or less, and ii) the polyisocyanate, the chain extender and / or crosslinker, and the polyether polyol having a hydroxyl equivalent weight of at least 150 are all formed into a mixture and cured such that the chain extender and / or crosslinker and the polyether polyol all react simultaneously with the polyisocyanate.
[0013] The "prepolymer" process is characterized in that i) at least 50% by weight of a polyol having a hydroxyl equivalent weight of 150 or greater is first reacted with a polyisocyanate to form a urethane group-containing isocyanate-terminated prepolymer having an isocyanate content of 20% by weight or less, and then ii) the prepolymer is subsequently cured by reaction of a chain extender and the remaining polyol having a hydroxyl equivalent weight of 150 or greater to produce a polyurethane.
[0014] Each polyisocyanate(s) is an organic compound having two or more isocyanate groups per molecule. The polyisocyanates preferably have a number average of 4 or less isocyanate groups, more preferably 3 or less or 2.7 or less isocyanate groups per molecule. In some embodiments, the polyisocyanates have a number average of 2 to 2.5 or 2 to 2.3 isocyanate groups per molecule.
[0015] The polyisocyanate has a number average isocyanate equivalent weight up to 200, such as 80-200, 80-180, or 80-150.
[0016] Examples of useful polyisocyanate compounds include, for example, m-phenylene diisocyanate, toluene-2,4-diisocyanate, toluene-2,6-diisocyanate, naphthylene-1,5-diisocyanate, methoxyphenyl-2,4-diisocyanate, diphenylmethane-4,4'-diisocyanate, diphenylmethane-2,4'-diisocyanate, 4,4'-biphenylene diisocyanate, 3,3'-dimethoxy-4,4'-biphenyl diisocyanate, 3,3'-dimethyl-4-4'-biphenyl diisocyanate, 3,3'-dimethyldiphenylmethane-4,4'-diisocyanate, 4,4',4"-triphenylmethane triisocyanate, polymethylene polyphenylisocyanate (PMDI), toluene-2,4-diisocyanate, diphenylmethane-2,4'-diisocyanate, diphenylmethane-4,4'-diisocyanate, 4,4',4"-triphenylmethane triisocyanate, polymethylene polyphenylisocyanate (PMDI), Examples of aromatic polyisocyanates include aromatic polyisocyanates such as dimethyldiphenylmethane-2,2',5,5'-tetraisocyanate, ...
[0017] Further useful polyisocyanate compounds having an isocyanate equivalent weight of up to 200 include one or more aliphatic polyisocyanates, examples of which include cyclohexane diisocyanate, 1,3- and / or 1,4-bis(isocyanatomethyl)cyclohexane, 1-methyl-cyclohexane-2,4-diisocyanate, 1-methyl-cyclohexane-2,6-diisocyanate, methylene dicyclohexane diisocyanate, isophorone diisocyanate, and hexamethylene diisocyanate, any of which can be modified to include urethane, urea, biuret, carbodiimide, uretonimine, allophanate, or other groups formed by reaction of isocyanate groups.
[0018] A chain extender for purposes of the present invention is a compound having exactly two isocyanate-reactive groups per molecule and an equivalent weight per isocyanate-reactive group of less than 150. The isocyanate-reactive groups can be, for example, hydroxyl and / or primary and / or secondary amino groups.
[0019] Examples of hydroxyl group containing chain extenders include 1,2-ethanediol, 1,2- or 1,3-propanediol, 1,4-butanediol, diethylene glycol, triethylene glycol, dipropylene glycol, tripropylene glycol, neopentyl glycol and alkoxylates of any of the foregoing having a hydroxyl equivalent weight of less than 150.
[0020] Examples of diamine chain extenders include aliphatic polyamines such as ethylenediamine, piperazine, diethylenetriamine, triethylenetetraamine, tetraethylenepentaminepiperazine, N-(2-aminoethyl)piperazine, N,N'-bis(2-aminoethyl)piperazine, cyclohexanediamine (including one or more of the 1,2-, 1,3- and 1,4-isomers), bis(aminomethyl)cyclohexane (including one or more of the 1,2-, 1,3- and 1,4-isomers), and bis(2-aminoethyl)cyclohexane, as well as aromatic polyamines such as toluenediamine, diethyltoluenediamine, methylenediphenyldiaminephenylenediamine, and bis(aminomethyl)benzene.
[0021] Examples of crosslinkers include glycerin, trimethylolpropane, trimethylolethane, erythritol, pentaerythritol, triethanolamine, diethanolamine, and alkoxylates of any of the foregoing having a hydroxyl equivalent weight of less than 175. Amino alcohols such as monoethanolamine and diethanolamine are also useful crosslinkers.
[0022] At least 50% of the polyols having a hydroxyl equivalent weight of 150 or greater are one or more hydroxyl-containing copolymers of butylene oxide and ethylene oxide, these copolymers being characterized in that: a) they have a hydroxyl equivalent weight of at least 150; b) they have a number average of 1.8 to 6 hydroxyl groups per molecule; c) at least 70% of the hydroxyl groups are primary hydroxyl groups; and d) they have an oxyethylene content of 10% by weight or less, based on the weight of the copolymer.
[0023] The oxyethylene groups constitute no more than 10% of the total weight of the copolymer. The oxyethylene groups may constitute at least 2%, at least 3%, or at least 5% of the total weight of the copolymer. The -CH groups formed when butylene oxide is polymerized 2 -CH(CH 2 -CH 3The -O- groups preferably constitute at least 50%, or at least 65% by weight of the copolymer, and may, for example, constitute up to 98%, up to 95%, or up to 90% by weight of the copolymer.
[0024] Copolymers of butylene oxide and ethylene oxide may also contain oxypropylene groups, which, if present, may constitute at least 1%, at least 5%, or at least 10% of the weight of the copolymer, for example, up to 40%, up to 30%, or up to 25% of the weight of the copolymer.
[0025] The oxyethylene groups are preferably present in the form of a single unit or block at the end of the polymer chain to generate the desired primary hydroxyl groups.
[0026] The oxybutylene groups are preferably present in the form of one or more internal blocks and / or within blocks of randomly copolymerized butylene oxide and propylene oxide and / or ethylene oxide. When present, the oxypropylene groups may form one or more internal blocks and / or be present in one or more blocks of randomly copolymerized butylene oxide and ethylene oxide.
[0027] In some embodiments, the hydroxyl-containing copolymer of butylene oxide and ethylene oxide comprises one or more internal poly(butylene oxide) blocks and one or more terminal poly(ethylene oxide) blocks. In other embodiments, the hydroxyl-containing copolymer of butylene oxide and ethylene oxide comprises one or more internal poly(butylene oxide) blocks, one or more poly(butylene oxide) blocks exterior to the poly(propylene oxide) blocks, and one or more terminal poly(ethylene oxide) blocks exterior to the poly(butylene oxide) blocks.
[0028] The number average hydroxyl functionality of the hydroxyl-containing copolymers of butylene oxide and ethylene oxide may be at least 1.9 or at least 2.0, and may be up to 4.0, up to 3.2, up to 3.0, up to 2.5 or up to 2.2. For purposes of this invention, all hydroxyl functionalities are nominal functionalities equal to the number average hydroxyl groups per molecule of the starter used to prepare the polymer.
[0029] The hydroxyl equivalent weight may be at least 200, at least 400, at least 500, at least 700, or at least 800, such as up to 3000, up to 2500, up to 2000, up to 1750, up to 1500, or up to 1200. The hydroxyl equivalent weight is determined by measuring the hydroxyl number in mg KOH / g polyol using a titration method and converting the hydroxyl number to hydroxyl equivalent weight using the relationship equivalent weight=56,100÷hydroxyl number.
[0030] In some embodiments, at least 70% or at least 75% of the hydroxyl groups of the butylene oxide and ethylene oxide copolymers are primary. Typically, up to 95%, up to 90%, or up to 85% of the hydroxyl groups are primary. The primary hydroxyl content is determined by the trifluoroacetic anhydride derivative of the polyol. 9 It can be determined by F NMR analysis.
[0031] The hydroxyl-containing copolymers of butylene oxide and ethylene oxide preferably have a polydispersity (weight average molecular weight divided by number average molecular weight, in each case determined by gel permeation chromatography (GPC) against polyether polyol or polystyrene standards) of 1.75 or less. The polydispersity can be, for example, 1.00-1.16, 1.00-1.15, 1.00-1.12, 1.00-1.10, 1.00-1.08 or 1.00-1.06.
[0032] Hydroxyl-containing copolymers of butylene oxide and ethylene oxide preferably contain at most a small amount of acetals. Acetals can be formed in some alkylene oxide polymerization processes through the formation and subsequent reaction of aldehyde-containing species, as described, for example, in Raghuraman et al. in Macromolecules 2016, 49(18), pp. 6790-6798. Hydroxyl-containing copolymers of butylene oxide and ethylene oxide preferably contain at most 5 mol% acetals, more preferably 2 mol% or less, 1.5 mol% or less, or 1 mol% or less acetals, based on the moles of carbon atoms in the polymer. The acetal content can be determined by the inverse gated method. 13 The C NMR spectroscopy can be used to determine the C NMR spectroscopy. A suitable procedure is as follows: Samples are prepared as ∼90% solutions in DMSO-d6 in 10 mm NMR tubes. 13 C NMR data are acquired using a Bruker Avance 400-MHz spectrometer equipped with a cryoprobe or equivalent using at least 64 temporal scans and a relaxation delay of 30 seconds (optimized for quantitative measurements). Acquisition is performed using a spectral width of 25,000 Hz and a file size of 65,000 data points. Relative moles of acetal species are measured by integrating the area under the resonance from the acetal carbon.
[0033] Mole % acetal = 100% x relative moles of acetal carbons ÷ sum of relative moles of all carbon species in the spectrum
[0034] Hydroxyl-containing polymers of butylene oxide and ethylene oxide can be made by polymerizing these oxides in the presence of a Lewis acid catalyst having the general formula:
number
[0035] Fluoroalkyl-substituted phenyl group R 1 The at least one fluoroalkyl substituent may be, for example, a fluorine-substituted alkyl group having 1 to 5 carbon atoms. A fluorine-substituted methyl group is preferred. The alkyl group contains at least one fluorine substituent and may have many more up to the point of being perfluorinated. A preferred fluoroalkyl substituent is -CF 3 In some embodiments, a fluoroalkyl substituent is a -CF 3 It is.
[0036] Fluoroalkyl-substituted phenyl group R 1 can be substituted with 1 to 5 fluoroalkyl groups. The fluoroalkyl groups can occupy any position on the phenyl ring. In some embodiments, R 1 The group is substituted with two fluoroalkyl groups, which may be located at the 2 and 5 carbons or the 3 and 5 carbons. In certain embodiments, the fluoroalkyl-substituted phenyl group R 1 is 2,5- or 3,5-bis(trifluoromethyl)phenyl. In some embodiments, R 1 is optionally substituted with fluoro and / or chloro groups.
[0037] R 1may be substituted to include, in addition to at least one fluoroalkyl group, other groups, such as fluorine and / or chlorine atoms replacing at least one hydrogen of the phenyl group.
[0038] R 1 For fluoroalkyl-substituted phenyl groups, R 2 and R 3 is R 2 and R 3 At least one of the following is R 1 The condition is that it is different from R. 2 and / or R 3 Instead of or in addition to being fluoroalkyl substituted, the phenyl group R may be fluoro- and / or chloro-substituted. 2 or R 3 R may be substituted with 1 to 5 fluoroalkyl, fluorine atoms and / or chlorine atoms. 2 and R 3 Exemplary groups include, in addition to 2,5- or 3,5-bis(trifluoromethyl)phenyl, [ka]
[0039] Any R 4 The functional group or functional polymer group may be a Lewis base that complexes with a Lewis acid catalyst. By functional group or functional polymer group is meant a molecule that includes at least one of water, alcohol, alkoxy (including, for example, linear or branched ethers and cyclic ethers), linear or branched ethers, cyclic ethers, aldehydes, ketones, esters, organosilanes, organosiloxanes, oximes, and substituted analogs thereof. Each of the alcohols, linear or branched ethers, cyclic ethers, aldehydes, ketones, esters, alkoxys, organosilanes, organosiloxanes, and oximes may contain 2-20 carbon atoms, 2-12 carbon atoms, 2-8 carbon atoms, and / or 3-6 carbon atoms.
[0040] For example, the functional group or functional polymer group can be represented by the formula (OY m H) n where O is oxygen, H is hydrogen, Y is alkylene, m is 0 or 1, and n is an integer (e.g., an integer from 1 to 100). However, other known functional groups or functional polymer groups that can be combined with Lewis acid catalysts can be used. Exemplary cyclic ethers include tetrahydrofuran and tetrahydropyran.
[0041] Suitable R 4 Groups include diethyl ether, cyclopentyl methyl ether, methyl tertiary butyl ether, tetrahydrofuran, tetrahydropyran, 1,4-dioxane, acetone, methyl isopropyl ketone, isopropyl acetate, and isobutyl acetate.
[0042] Methods for making such catalysts are described, for example, in PCT / US2018 / 050995 and PCT / US2018 / 051001, filed Sep. 14, 2018.
[0043] Examples of suitable Lewis acid catalysts include (2,5-bis(trifluoromethyl)phenyl)bis(3,5-bis(trifluoromethyl)phenyl)borane, bis(2,5-bis(trifluoromethyl)phenyl)(3,5-bis(trifluoromethyl)phenyl)borane, bis(3,5-bis(trifluoromethyl)phenyl)(2,3,5,6-tetrafluoro-4-(trifluoromethyl)phenyl)borane, bis(3,5-bis(trifluoromethyl)phenyl)(pentachlorophenyl)borane, and the tetrahydrofuran (THF) adduct of bis(3,5-bis(trifluoromethyl)phenyl)(2,4,6-trifluorophenyl)borane.
[0044] The polyurethanes are made by reacting i) one or more polyisocyanates as described above with isocyanate-reactive materials, including ii) at least one chain and / or at least one crosslinker, iii) one or more polyols having a hydroxyl equivalent of at least 150, and iv) at least one urethane catalyst, where at least 50% by weight of iii) is a hydroxyl-containing copolymer of butylene oxide and ethylene oxide as described herein. The reaction mixture may also include one or more optional materials, as described below. The reaction can be carried out using either a prepolymer or one-shot process, although some particular advantages of the present invention are realized when the one-shot process is used.
[0045] In some embodiments, the relative amounts of isocyanate-reactive material, chain extender and / or crosslinker, and polyol are selected so that the polyurethane has a hard segment content of 15 to 60 weight percent. The hard segment content is calculated from the weight of the starting materials as follows:
[0046] Hard segment (%) = 100% × (wt イソシアネート +wt 鎖延長剤+架橋剤 )÷(wt イソシアネート +wt 鎖延長剤+架橋剤 +wt ポリオール ), where wt ポリオール includes the weight of all isocyanate-reactive materials having a hydroxyl equivalent weight greater than 150. The hard segment content may be at least 20%, at least 30%, or at least 35%, and may be up to 55% or up to 50%, by weight in all cases.
[0047] The reaction mixture may contain a variety of optional components. Among these are other isocyanate-reactive materials different from the chain extenders and / or crosslinkers, as well as hydroxyl-containing copolymers of butylene oxide and ethylene oxide as described above. These include, for example, one or more polyether polyols, one or more polyester polyols, polyalkylene carbonate polyols, hydroxyl-terminated diene rubbers, polyvinyl alcohols, and amine-terminated polyethers. The hydroxyl-containing polymers of butylene oxide and ethylene oxide constitute at least 50% of the total weight of all isocyanate-reactive materials having an equivalent weight of 150 or greater, and may constitute at least 70%, at least 80%, at least 90%, or at least 95% up to 100% thereof. Optional isocyanate-reactive materials, if present, preferably constitute no more than 10%, no more than 5%, no less than 3%, or no more than 1% of the combined weight of all polyisocyanates and all isocyanate-reactive components of the reaction mixture.
[0048] Other optional ingredients include, for example, particulate fillers, colorants, catalysts, surfactants, drying and / or water scavenging agents, antioxidants, preservatives, biocides, reinforcing fibers, thixotropic agents, and the like.
[0049] The reaction mixture preferably contains no more than 5 weight percent or less than 2 weight percent (and may even be absent) of solvent. A solvent, for purposes of this invention, is a material that has a boiling point of no more than 200° C. at standard pressure and is not isocyanate-containing and is not isocyanate-reactive (i.e., does not contain isocyanate-reactive groups).
[0050] Polyurethanes are made by first forming an isocyanate-terminated prepolymer containing urethane groups by reacting at least a portion of a polyol having a hydroxyl equivalent weight of at least 150 with a polyisocyanate, and then curing the prepolymer by reaction with a chain extender and / or crosslinker. A portion of the chain extender and / or crosslinker can be present during the prepolymer formation, as well as a portion of the polyol having an equivalent weight of 150 or greater during the curing step. The prepolymer can have an isocyanate content of at least 1%, at least 2%, at least 3%, or at least 4%, up to 20%, up to 15%, up to 12%, or up to 10%.
[0051] Polyurethanes are made in a one-shot process by forming a reaction mixture containing a polyisocyanate, a chain extender and / or crosslinker, and a polyol having an equivalent weight of 150 or greater, and curing them in one go.
[0052] The process of the present invention is particularly suitable for producing polyurethane elastomers, sealants and / or adhesives, and coatings.
[0053] Elastomers are generally characterized as being flexible materials having an elongation at break of at least 100% as measured according to ASTM D638. The elastomeric products of the present invention can be of the static or dynamic type, with static elastomers being products that do not deform periodically during use (such as gasket materials and certain types of rollers) and dynamic elastomers being products that deform periodically and repeatedly during use. The elastomers of the present invention are useful as rollers for many applications, such as, for example, gaskets and seals, tubes, coating rollers, nip rollers, drive belts, squeeze rollers, office machine rollers, pulleys, conveyor wheels, fork truck wheels, tricycles, wheels, caster wheels, industrial tires, rod wipers, snow plow blades, chute and cyclone liners, agitator blades, etc.
[0054] Elastomers can be non-porous, porous, or microporous. Porous or microporous elastomers can be formed by incorporating a physical and / or chemical blowing agent into the reaction mixture and curing the reaction mixture under conditions where the blowing agent produces a gas that becomes trapped in the cured material producing bubbles. Alternatively, or in addition, air, carbon dioxide, nitrogen, or other gases can be bubbled into the reaction mixture to form bubbles that are cured to form porous or microporous elastomers.
[0055] When making elastomers or other moldings or shaped articles, curing can be done in a mold or other form, which may be open or closed. It can be carried out on a belt or other device. The reaction mixture can be formed into a layer on a substrate and cured thereon to form a composite. A fibrous material can be impregnated with the reaction mixture and then the reaction mixture can be cured in place to form a fiber-reinforced composite.
[0056] Curing of the elastomers is generally carried out at elevated temperatures, suitable temperatures being, for example, at least 50°C, preferably at least 65°C, up to 130°C, preferably up to 110°C or 100°C.
[0057] When forming elastomers or other molded articles, curing is generally continued until the elastomer has sufficient green strength to be handled without permanent damage. Gel times (gel points), measured according to the methods described in the Examples, can be, for example, 5 to 20 minutes. Demold times can be, for example, 5 minutes to 1 hour. Elastomers can be post-cured at elevated temperatures as just described to further complete the cure and develop mechanical and other properties.
[0058] The coating is formed by applying the reaction mixture to the surface of the substrate to form a film and curing the film on the substrate to form an adherent coating. The application step is conveniently carried out by methods such as spraying, brushing, rolling, or dipping. Curing can be carried out at ambient or elevated temperatures. The present invention is particularly useful for producing thick protective coatings and / or for producing soft surfaces. The coating compositions can be formulated to include pigments, dyes and other colorants, as well as filler particles (which may also function as colorants), various types of rheology modifiers, and the like.
[0059] When the polyurethane is a sealant and / or adhesive, the reaction mixture is applied to a bond line, joint, crack or other opening between two substrates (or within a portion of a single substrate) and cured in place to adhere to the substrate, at least partially seal the opening, and / or bond the substrates together. Such adhesives or sealants can be formulated with, for example, one or more fillers and colorants used to impart desired rheological and / or aesthetic properties, as well as a urethane catalyst that promotes room temperature or other low temperature cure. Curing is typically carried out under ambient conditions, although elevated temperatures can also be used.
[0060] The following examples are provided to illustrate the invention but are not intended to limit the scope of the invention. All parts and percentages are by weight unless otherwise indicated.
[0061] Preparation of catalyst Catalyst 1 is (2,5-bis(trifluoromethyl)phenyl)bis(3,5-bis(trifluoromethyl)phenyl)borane, prepared as follows: n-butyllithium (6.0 mL, 2.46 M in hexane, 14.8 mmol) was dissolved in a cold (−78 °C, CO) solution of 1-bromo-2,5-bis(trifluoromethyl)benzene (4.32 g, 14.8 mmol) in diethyl ether (200 mL). 2(s) bath) solution over 30 min. The reaction mixture is stirred in a dry ice bath for 1 h, at which time a precipitate forms. Isopropoxybis(3,5-bis(trifluoromethyl)phenyl)borane (7.32 g, 14.8 mmol) in ether (20 mL) is added over 30 min. The reaction mixture is warmed to ambient temperature with stirring overnight to give a clear yellow solution. A solution of HCl in ether (15.0 mL, 2.0 M, 30 mmol) is added, at which time a colorless precipitate forms. The reaction mixture is filtered and the volatiles are removed under a stream of nitrogen with stirring overnight to give a pale yellow sticky solid. Add more ether (100 mL) (not all solids dissolve). Add additional HCl (5 mL, 10 mmol) and stir the mixture for 2 h. Filter the mixture and remove the volatiles under reduced pressure. Extract the residue with toluene, filter, and remove the volatiles under reduced pressure. The residue is extracted with hot hexane, filtered, and the resulting solution is concentrated until a solid begins to form even at 60° C. The mixture is cooled in a freezer overnight. The supernatant is decanted, the solid is washed with hexane, and the solid is dried under reduced pressure.
[0062] Catalyst 2, the THF adduct of bis(3,5-bis(trifluoromethyl)phenyl)(2,4,6-trifluorophenyl)borane, is prepared as follows: In the first step, 3.00 grams (14.2 mmol) of 1-bromo-2,4,6-trifluorobenzene is mixed with 200 mL of diethyl ether in a 250 mL Schlenk flask and cooled in a -78 °C bath. A 2.5 M solution of n-butyllithium in hexanes (5.8 mL, 14 mmol) is added to the cold solution via syringe. A solution of 7.05 grams of bis(3,5-bis(trifluoromethyl)phenyl)isopropoxyborane diethyl ether (25 mL) is poured into the cold mixture and stirred for 30 minutes. The reaction mixture is allowed to slowly warm to room temperature with stirring overnight. The next morning the solution is filtered and all volatiles are removed under vacuum to give a yellow solid. The solid is extracted with hexanes, the mixture is filtered and the volatiles are removed from the filtrate to give an off-white solid. The solid is triturated with hexanes, the mixture is filtered and the volatiles are removed from the filtrate under reduced pressure to give the product, lithium bis(diethyl ether)bis(3,5-bis(trifluoromethyl)phenyl)(2,4,6-trifluorophenyl)isopropoxyborate as a white solid.
[0063] In the second step, 8.00 g (10.2 mmol) of lithium bis(diethyl etherate)bis(3,5-bis(trifluoromethyl)phenyl)(2,4,6-trifluorophenyl)isopropoxyborate from step 1 is dissolved in 100 mL of diethyl ether to form a colorless solution. Chlorotrimethylsilane (3.2 mL, 2.7 g, 25 mmol) is added to the room temperature solution with stirring. The mixture is stirred overnight at room temperature and a large amount of precipitate forms. The reaction mixture is filtered through Celite to remove LiCl, and the volatiles are removed from the filtrate under reduced pressure. The residue is extracted with benzene, the solution is filtered, and the volatiles are removed from the filtrate under reduced pressure to give bis(3,5-bis(trifluoromethyl)phenyl)(2,4,6-trifluorophenyl)borane as a white powder.
[0064] In the third step, 4.45 g (7.82 mmol) of bis(3,5-bis(trifluoromethyl)phenyl)(2,4,6-trifluorophenyl)borane from step 2 is dissolved in ether (20 mL) and THF (2 mL) is added. The volatiles are removed under reduced pressure to give the product, bis(3,5-bis(trifluoromethyl)phenyl)(2,4,6-trifluorophenyl)borane THF adduct, as a white solid.
[0065] Preparation of polyether polyols Polyol A is a commercially available poly(butylene oxide) homopolymer having a number average molecular weight of 2000. Less than 2% of the hydroxyl groups are primary.
[0066] Polyol B is made by polymerizing butylene oxide to a 400 molecular weight poly(propylene oxide) diol starter in the presence of catalyst 1. 67.3 parts of the starter are combined in a pressurized reactor under nitrogen with a solution of the catalyst in tetrahydrofuran. After purging with nitrogen, the reactor vent is closed and 239.9 parts of butylene oxide are added at a rate of 1.25 parts / min at 55° C. The reaction mixture is digested for 20 minutes at the same temperature, after which the reactor is vented, purged with nitrogen at 90° C., and cooled. The product has a number average molecular weight of 2051, a hydroxyl equivalent weight of about 1025, a polydispersity of 1.06, with 54% of the hydroxyl groups being primary.
[0067] Polyol 1 is made by polymerizing butylene oxide to a 400 molecular weight poly(propylene oxide) diol starter in the presence of catalyst 2. 65 parts of starter and a solution of catalyst in tetrahydrofuran are combined under nitrogen in a pressurized reactor. After purging with nitrogen, the reactor vent is closed and 231.1 parts of butylene oxide are added at a rate of 1.25 parts / min at 55° C. The reaction mixture is digested for 20 minutes at the same temperature. 28.6 parts of ethylene oxide are added at a constant rate of 0.75 parts / min. The reaction mixture is digested again, this time at 55° C. for 45 minutes, followed by venting the reactor, purging with nitrogen at 90° C., and cooling. The product has a number average molecular weight of 1931, a hydroxyl equivalent weight of about 965, a polydispersity of 1.07, and 82% of the hydroxyl groups are primary. Polyol 1 contains 20% oxypropylene units, 8.8% oxyethylene units, and 71.2% oxybutylene units.
[0068] Preparation of Elastomer 1 and Comparative Samples A and B Elastomer Example 1 and Comparative Samples A and B are prepared in a "one shot" process by combining 9.57 parts of polyol with 0.81 parts of 1,4-butanediol and 0.2 parts of a commercial metal carboxylate catalyst (KKat® XK-604 from King Industries) in a laboratory mixer, followed by the addition of 4.6 parts of polyisocyanate and brief mixing. The resulting reaction mixture is poured into a 15.2 cm x 15.2 x 0.155 cm chase and cured in a press for 30 minutes at 80°C and approximately 1200 psi (8.3 MPa). The resulting elastomer is removed from the chase and post cured at 80°C for 16 hours. The amounts of components are selected to produce an elastomer with a hard segment content of 36% by weight for each of Example 1 and Comparative Samples A and B. No surfactants, solvents, or other materials are included in the reaction mixture.
[0069] The polyisocyanate is an equal weight mixture of 143 equivalents of a carbodiimide modified MDI product and 181 equivalents of a urethane group-containing MDI prepolymer, each having an isocyanate functionality of about 2 isocyanate groups per molecule.
[0070] Elastomer Example 1 and Comparative Samples A and B are made with Polyols 1, A, and B, respectively.
[0071] The formulations are evaluated for gel point on a parallel plate rheometer under conditions of 1 rad / sec frequency, 10 Pa stress, and 80°C isothermal temperature. An uncured portion of the reaction mixture is placed between the plates and the loss and storage moduli are measured as a function of time. The gel point is taken as the time at which the loss modulus is equal to the storage modulus.
[0072] Elastomers are evaluated for hardness according to ASTM D2240-15e1 at 22 °C and 50% relative humidity. Tensile properties are measured according to ASTM D638 using type V specimens at a speed of 50 mm / min under conditions of 22 °C and 50% relative humidity. Glass transition temperatures are measured by dynamic mechanical analysis at a temperature sweep from -80 °C to 200 °C at a strain of 0.05%, a frequency of 1 Hz, and a ramp rate of 5 °C per minute. Water aging is evaluated by immersing samples in 70 °C water for 7 days and measuring the weight gain. The results are shown in Table 1. [Table 1]
[0073] Example 1 exhibits faster reactivity and produces an elastomer with a significantly higher modulus at comparable elongation than either of the comparative samples. Little change in water absorption is observed, despite the presence of oxyethylene groups in the elastomer. This data demonstrates that faster reactivity and improved modulus can be obtained by preparing elastomers using the butylene oxide-ethylene oxide copolymers of the present invention, without sacrificing hydrophobicity.
[0074] Example 2 and Comparative Samples C and D Elastomer Example 2 and Comparative Samples C and D are prepared in the same manner as Example 1 and Comparative Samples A and B, respectively, but the amounts of components are selected in each case to produce elastomers with a hard segment content of 50% by weight. Thus, in each case, the amount of polyol is 8.7 parts, the amount of 1,4-butanediol is 1.3 parts, the amount of isocyanate is 6.2 parts, and the amount of catalyst is 0.15 parts. As already mentioned, the reaction mixture does not contain surfactants, solvents or other materials.
[0075] Elastomeric Example 2 and Comparative Samples C and D are made with Polyols 1, A and B, respectively.
[0076] The elastomer properties were determined as previously described and are shown in Table 2. [Table 2]
[0077] These results follow roughly the same trends as the data in Table 1. The inventive examples cure significantly faster than any of the comparisons, producing elastomers with very large increases in modulus, but very rarely, increases in elongation. Water absorption is comparable to the samples, again demonstrating that the benefits of reactivity and mechanical properties are not gained at the expense of hydrophobicity.
[0078] Preparation of Elastomer 3 and Comparative Samples E and F Example 3 and Comparative Samples E and F are made by the "prepolymer" process. 32.3 parts of polyol are reacted with 26.9 parts of polyisocyanate to form a prepolymer having an isocyanate content of about 9.5% by weight. 18.2 parts of the resulting prepolymer, 1.8 parts of 1,4-butanediol, and 0.01 parts of a metal carboxylate catalyst are combined in a laboratory mixer, poured into an open mold, and cured as previously described to produce an elastomer having a hard segment content of 50% by weight.
[0079] Elastomeric Example 3 and Comparative Samples E and F are made with Polyols 1, A, and B, respectively.
[0080] The elastomer properties were determined as previously described and are shown in Table 3. [Table 3]
[0081] As the data in Table 3 show, similar benefits in mechanical properties are seen when the elastomers are made using a prepolymer process: hardness and modulus are increased without loss of elongation and without loss of the desired hydrophobic behavior. The present application also relates to the following aspects: (1) A hydroxyl-containing copolymer of butylene oxide and ethylene oxide, said copolymer having a hydroxyl equivalent weight of at least 150, an average of 1.8 to 6 hydroxyl groups per molecule, at least 70% of which are primary hydroxyl groups, and an oxyethylene content of 10% by weight or less, based on the weight of the copolymer. (2) The hydroxyl-containing copolymer according to (1) above, having a hydroxyl equivalent weight of 400 to 2000, an average of 2 to 4 hydroxyl groups per molecule, and a polydispersity of 1 to 1.175. (3) The hydroxyl-containing copolymer according to (1) or (2) above, which contains 2 to 10% by weight of oxyethylene units, and the oxyethylene units are present as a single unit or block at the chain ends of the hydroxyl-containing copolymer. (4) The hydroxyl-containing copolymer according to any one of (1) to (3) above, which contains 1 to 30% by weight of oxypropylene units. (5) A hydroxyl-containing copolymer according to any one of (1) to (4) above, prepared by polymerizing butylene oxide and ethylene oxide in the presence of a Lewis acid catalyst having the following general formula:
number
Claims
1. hydroxyl-containing copolymers of butylene oxide and ethylene oxide, said copolymer of butylene oxide and ethylene oxide having a hydroxyl equivalent weight of 400-2000, an average of 1.8-6 hydroxyl groups per molecule, of which at least 70% are primary hydroxyl groups, a polydispersity of 1-1.175, a butylene oxide content of 65-95% by weight based on the weight of the copolymer, and an oxyethylene content of 2-10% by weight based on the weight of the copolymer, said oxyethylene units being present as single units or blocks at the chain ends of the hydroxyl-containing copolymer; A hydroxyl-containing copolymer made by polymerizing butylene oxide and ethylene oxide with a poly(propylene oxide) diol starter in the presence of a Lewis acid catalyst having the general formula: [0010] (wherein M is boron, aluminum, indium, bismuth or erbium; R 1 is a fluoroalkyl-substituted phenyl group; R 2 and R 3 are each a fluoroalkyl-substituted phenyl group, a fluoro-substituted phenyl group, a chloro-substituted phenyl group, or a fluoro- and chloro-substituted phenyl group, with the proviso that R 1 , R 2 and R 3 are not all the same, R 4 is a functional group or a functional polymer group 2. The hydroxyl-containing copolymer of claim 1 having an average of 2 to 4 hydroxyl groups per molecule and a polydispersity of 1 to 1.
175.
3. A hydroxyl-containing copolymer according to any one of claims 1 to 2, comprising 1 to 30% by weight of oxypropylene units.
4. A polyurethane that is the reaction product of at least one polyisocyanate with an isocyanate-reactive material comprising at least one chain extender and at least one hydroxyl-containing copolymer according to any one of claims 1 to 3.
5. 5. The polyurethane of claim 4, wherein the at least one polyisocyanate and the at least one chain extender together comprise from 15 to 60 percent of the total combined weight of the one or more polyisocyanates and the isocyanate-reactive materials.
6. 10. A one-shot process for making a polyurethane, comprising forming a reaction mixture comprising one or more polyisocyanates having a number average isocyanate equivalent weight of 200 or less, isocyanate-reactive materials comprising at least one chain extender and at least one hydroxyl-containing copolymer of any one of claims 1 to 3, and curing the reaction mixture in one step to form the polyurethane.
7. 7. The one-shot process of claim 6, wherein said one or more polyisocyanates and said at least one chain extender together comprise 15 to 60% of the total combined weight of said one or more polyisocyanates and isocyanate-reactive materials.
8. 8. The one-shot process of claim 6 or 7, wherein the reaction mixture is cured in the presence of 5% or less of a solvent based on the weight of the reaction mixture to form the polyurethane.
Citation Information
Patent Citations
Manufacture of polyurethane elastomers
GB1063278A
Molding method of polyurethane by reaction injection molding
JP1981133143A
Manufacture of polyurethane elastomer
JP1982042715A
Production of polymeric polyol and polyurethane resin
JP1984152912A
Urethane prepolymer
JP1988120722A