Inorganic particle dispersion slurry composition and method for producing inorganic sintered body

The use of a binder resin with carboxylic acid anhydrides and (meth)acrylic resins in inorganic particle-dispersed slurry compositions addresses high-temperature processing challenges, ensuring reliable electronic components with low residual carbon and oxidation resistance.

JP7579483B2Active Publication Date: 2024-11-07SEKISUI CHEMICAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024517137
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-12-07
Filing Date
2023-12-04
Publication Date
2024-11-07
Estimated Expiration
2043-12-04

AI Technical Summary

Technical Problem

Existing inorganic particle-dispersed slurry compositions face challenges with high-temperature processing, solvent selectivity issues, and poor storage stability, leading to oxidation and residual carbon problems during binder removal, which affect the reliability of electronic components.

Method used

A slurry composition containing a binder resin with specific carboxylic acid anhydrides and (meth)acrylic resins, combined with a binder removal aid, allows for low-temperature debinding and improved storage stability, reducing oxidation and residual carbon.

Benefits of technology

The solution enables the production of highly reliable electronic components with excellent printability and sinterability, achieving low residual carbon and oxidation resistance even at low temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579483000001
    Figure 0007579483000001
  • Figure 0007579483000002
    Figure 0007579483000002
  • Figure 0007579483000003
    Figure 0007579483000003
Patent Text Reader

Abstract

The present invention provides an inorganic particle dispersed slurry composition which has excellent storage stability and printability, and is capable of promoting a binder removal process even at low temperatures, and suppressing oxidation of inorganic particles. This inorganic particle dispersed slurry composition exhibits excellent sinterability and has less residual carbon after firing, and enables the achievement of an electronic component that has high reliability. The present invention also provides a method for producing an inorganic sintered body, the method using this slurry composition. An inorganic particle dispersed slurry composition according to the present invention contains a binder resin (A), inorganic particles (B) and a solvent (C), while containing, as a binder removal assistant (D), a carboxylic acid anhydride that has a boiling point of 200°C or more and an oxygen atom content of 40% by weight or more.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an inorganic particle dispersion slurry composition and a method for producing an inorganic sintered body. [Background technology]

[0002] Inorganic particle dispersion slurry compositions in which inorganic particles such as ceramic powder and glass particles are dispersed in a binder resin are used in the production of various electronic components. These slurry compositions are formed into sheets through coating and drying processes, and are called green sheets. Ceramic green sheets made of inorganic particles and binder resin are laminated on top of which electrode layers are formed by screen printing or the like, and this laminate is heated in a firing furnace to decompose and remove the binder resin contained therein and sinter the inorganic particles, producing a variety of electronic components. Due to the increasing need for sustainable business processes in recent years, there is a demand for binder resins that can be debindered at lower temperatures and in shorter times. The ability to perform debindering at lower temperatures not only reduces the energy required for heating furnaces, but also makes it possible to prevent thermal and oxidative degradation of inorganic components in electronic components, resulting in the production of more reliable electronic components. In Patent Document 1, a low-temperature decomposable acrylic binder is used in the production of an all-solid-state battery, and degreasing is performed by increasing the temperature from room temperature to 500° C. at a rate of 20° C. / min in air and holding at 500° C. for 30 minutes. In addition, in Patent Document 2, a sealing material for electronic components is produced by using aliphatic polypropylene carbonate as a low-temperature decomposition binder in a low-melting glass paste. In this case, the temperature is raised to 430°C in a nitrogen atmosphere, and the baking temperature is maintained for 10 minutes, and then the glass paste is degreased by cooling to room temperature and then baked. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2018-77989 A [Patent Document 2] JP 2011-178606 A Summary of the Invention [Problem to be solved by the invention]

[0004] Acrylic binders have high solvent selectivity and resin strength can be easily adjusted, so that the method described in Patent Document 1 can provide a slurry composition for producing a green sheet. However, degreasing requires a high temperature of 500°C in an air atmosphere, and depending on the inorganic material used, there is a problem that performance degradation such as oxidation can easily occur. In addition, although the propylene carbonate described in Patent Document 2 has better decomposability under a nitrogen atmosphere than acrylic resin, it has poor solvent selectivity and the resin decomposes in environments other than neutral pH, resulting in problems with the storage stability of the inorganic particle dispersion slurry.

[0005] The present invention aims to provide an inorganic particle dispersion slurry composition that is excellent in storage stability and printability, can promote binder removal treatment even at low temperatures, can suppress oxidation of inorganic particles, has little residual carbon after firing, has excellent sinterability, and can obtain highly reliable electronic components. Another aim of the present invention is to provide a method for producing an inorganic sintered body using the slurry composition. [Means for solving the problem]

[0006] The present disclosure (1) is an inorganic particle dispersion slurry composition containing a binder resin (A), inorganic particles (B), and a solvent (C), and further containing, as a binder removal aid (D), a carboxylic acid anhydride having a boiling point of 200° C. or more and an oxygen atom content of 40% by weight or more. The present disclosure (2) relates to the inorganic particle dispersion slurry composition of the present disclosure (1), wherein the carboxylic acid anhydride is an anhydride of at least one carboxylic acid selected from the group consisting of succinic acid, maleic acid, citric acid, glutaric acid, diglycolic acid, methoxyacetic acid, itaconic acid, citraconic acid, trimellitic acid, cyclobutane tetracarboxylic acid, tricarballylic acid, butane tetracarboxylic acid, and cyclopentane tetracarboxylic acid. The present disclosure (3) is the inorganic particle dispersion slurry composition of the present disclosure (1) or (2), in which the content of the carboxylic acid anhydride is 5 parts by weight or more and 30 parts by weight or less based on 100 parts by weight of the binder resin (A). The present disclosure (4) is an inorganic particle dispersion slurry composition in which the binder resin (A) contains a (meth)acrylic resin and is any combination with any of the present disclosures (1) to (3). The present disclosure (5) relates to the inorganic particle dispersion slurry composition of the present disclosure (4), in which the (meth)acrylic resin contains 50% by weight or more of segments derived from a (meth)acrylic acid ester having an ester substituent with 4 or more carbon atoms and a branched structure in the ester substituent. The present disclosure (6) is a method for producing an inorganic sintered body, comprising: a step of drying an inorganic particle dispersion slurry composition according to any one of the present disclosures (1) to (5) to obtain an inorganic particle dispersion compact; and a step of degreasing the inorganic particle dispersion compact at 300° C. or lower. The present invention will be described in detail below.

[0007] As a result of intensive research, the present inventors have found that a slurry composition containing a binder resin and a binder removal aid having a specific structure has excellent storage stability and printability. In addition, when the slurry composition is used in the production of an inorganic sintered body, it is possible to promote binder removal treatment even at low temperatures, suppress oxidation of inorganic particles, and produce electronic components with excellent sinterability and low residual carbon after firing, and thus have completed the present invention.

[0008] <Binder resin (A)> The slurry composition contains a binder resin (A). Examples of the binder resin (A) include (meth)acrylic resin, polystyrene resin, polyvinyl acetate resin, polyacetal resin, polycarbonate resin, etc. Among these, (meth)acrylic resin is preferred because of its excellent low-temperature decomposability. In the above-mentioned slurry composition, by combining a (meth)acrylic resin with a carboxylic acid anhydride described later, the binder removal treatment can be carried out at a low temperature even in a nitrogen atmosphere without using oxygen in the binder removal treatment, and oxidation of the inorganic particles can be suppressed. Furthermore, by combining the (meth)acrylic resin with the other binder resins described above as the binder resin (A), the binder resin can have better low-temperature decomposition properties.

[0009] The weight average molecular weight (Mw) of the binder resin (A) is preferably 20,000 or more and 4,000,000 or less. When the Mw is 20,000 or more, the viscosity of the slurry composition is not too low, and the dispersibility of the inorganic particles can be improved.When the Mw is 4,000,000 or less, the coating strength can be increased, and the viscosity of the slurry composition is sufficiently high to improve storage stability and provide excellent printability. The Mw is preferably 30,000 or more, more preferably 40,000 or more, and is preferably 3 million or less, more preferably 2 million or less, even more preferably 1 million or less, and even more preferably 500,000 or less. The Mw is preferably 20,000 to 4 million, more preferably 30,000 to 3 million, even more preferably 40,000 to 2 million, even more preferably 40,000 to 1 million, and particularly preferably 40,000 to 500,000.

[0010] The glass transition temperature (Tg) of the binder resin (A) is preferably 20° C. or higher, more preferably 30° C. or higher, and even more preferably 40° C. or higher, and is preferably 80° C. or lower, more preferably 70° C. or lower, even more preferably 60° C. or lower, and even more preferably 50° C. or lower. The Tg is preferably 20 to 80° C., more preferably 30 to 70° C., even more preferably 40 to 60° C., and even more preferably 40 to 50° C. The glass transition temperature (Tg) can be measured, for example, by using a differential scanning calorimeter (DSC).

[0011] The content of the binder resin (A) in the slurry composition is not particularly limited, but is preferably 3% by weight or more, more preferably 4% by weight or more, even more preferably 5% by weight or more, even more preferably 6% by weight or more, preferably 30% by weight or less, more preferably 20% by weight or less, and even more preferably 12% by weight or less. The content of the binder resin (A) is preferably 3 to 30% by weight, more preferably 4 to 20% by weight, even more preferably 5 to 12% by weight, and even more preferably 6 to 12% by weight. By setting the content of the binder resin within the above range, a slurry composition that can be fired at a low temperature can be produced.

[0012] The binder resin (A) preferably contains a (meth)acrylic resin. The (meth)acrylic resin preferably has a segment derived from a (meth)acrylic acid ester having a branched structure in the ester substituent. A (meth)acrylic resin mainly composed of a (meth)acrylic acid ester having a branched structure in the ester substituent has a lower decomposition end temperature than a (meth)acrylic resin mainly composed of a (meth)acrylic acid ester having a linear ester substituent. In an environment exceeding the ceiling temperature, a (meth)acrylic resin undergoes a depolymerization reaction in which it is decomposed into monomers, but a (meth)acrylic acid ester having a branched structure in the ester substituent has a characteristic that it is difficult to polymerize again, and therefore has a low decomposition end temperature. For this reason, a (meth)acrylic resin having the above structure has excellent low-temperature decomposability.

[0013] Examples of the (meth)acrylic acid ester having a branched structure in the ester substituent include an alkyl (meth)acrylic acid ester having a branched alkyl group, and a polyalkylene glycol (meth)acrylate having an alkylene glycol unit having a branched structure. The number of carbon atoms in the ester substituent is preferably 3 or more, more preferably 4 or more, and is preferably 20 or less, more preferably 15 or less, even more preferably 12 or less, for example, 10 or less. The number of carbon atoms in the ester substituent is preferably 3 to 20, more preferably 4 to 15, even more preferably 4 to 12, and even more preferably 4 to 10.

[0014] Examples of the (meth)acrylic acid alkyl ester having a branched alkyl group include isopropyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, isopentyl (meth)acrylate, isohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, and isodecyl (meth)acrylate. Among these, isopropyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and isodecyl (meth)acrylate are preferred, and isopropyl methacrylate, isobutyl methacrylate, s-butyl methacrylate, 2-ethylhexyl methacrylate, and isodecyl methacrylate are more preferred, and isobutyl methacrylate and 2-ethylhexyl methacrylate are even more preferred.

[0015] The (meth)acrylic polyalkylene glycol having the alkylene glycol unit with the branched structure may have propylene glycol unit.The (meth)acrylic polyalkylene glycol having the alkylene glycol unit with the branched structure may have an alkoxy group at the end.The alkoxy group may be, for example, a methoxy group, an ethoxy group, a butoxy group, etc. The (meth)acrylate polyalkylene glycol having alkylene glycol units having a branched structure preferably has 3 or more alkylene glycol units, more preferably 4 or more alkylene glycol units, and preferably 10 or less, more preferably 8 or less alkylene glycol units. The number of alkylene glycol units is preferably 3 to 10, more preferably 4 to 8.

[0016] The content of the segment derived from a (meth)acrylic acid ester having a branched structure in the ester substituent in the (meth)acrylic resin is preferably 50% by weight or more. When the content is within the above range, a slurry composition having excellent low-temperature decomposition properties can be obtained. The content of the segment derived from the (meth)acrylic acid ester having a branched structure in the ester substituent is preferably 60% by weight or more, more preferably 70% by weight or more, and is preferably 100% by weight or less, more preferably 90% by weight or less. The content of the segment derived from the (meth)acrylic acid ester having a branched structure in the ester substituent is preferably 50 to 100% by weight, more preferably 60 to 100% by weight, and more preferably 70 to 90% by weight. The above content can be measured, for example, by pyrolysis GC-MS.

[0017] The (meth)acrylic resin preferably has an ester substituent having 4 or more carbon atoms, and the ester substituent preferably has a segment derived from a (meth)acrylic acid ester having a branched structure. By having the above-mentioned constitution, it is possible to obtain a slurry composition having excellent low-temperature decomposition properties.

[0018] In addition, the (meth)acrylic resin preferably has, as a segment derived from a (meth)acrylic acid ester having a branched structure in an ester substituent, at least one selected from the group consisting of a segment derived from isobutyl methacrylate, a segment derived from 2-ethylhexyl methacrylate, a segment derived from isodecyl methacrylate, and a segment derived from isononyl methacrylate. By having the above-mentioned constitution, it is possible to obtain a slurry composition having excellent low-temperature decomposition properties.

[0019] The (meth)acrylic resin preferably has an ester substituent with 4 or more carbon atoms, and the content of segments derived from a (meth)acrylic acid ester having a branched structure in the ester substituent is preferably 50% by weight or more. When the content is within the above range, a slurry composition having excellent low-temperature decomposition properties can be obtained. The content of the segment derived from the (meth)acrylic acid ester having 4 or more carbon atoms in the ester substituent and having a branched structure in the ester substituent is preferably 60% by weight or more, more preferably 70% by weight or more, and for example, 100% by weight or less, preferably 90% by weight or less, and more preferably 80% by weight or less. The content of the segment derived from the (meth)acrylic acid ester having 4 or more carbon atoms in the ester substituent and having a branched structure in the ester substituent is preferably 50 to 100% by weight, more preferably 60 to 90% by weight, and more preferably 70 to 80% by weight.

[0020] The (meth)acrylic resin may further contain other segments, such as a segment derived from a (meth)acrylic acid ester whose ester substituent is linear, or a segment derived from a (meth)acrylic acid ester whose ester substituent has a cyclic structure. The above-mentioned composition can increase the strength of the coating film. Examples of the (meth)acrylic acid ester in which the ester substituent is linear include (meth)acrylic acid alkyl ester having a linear alkyl group, and (meth)acrylic acid polyalkylene glycol having a linear alkylene glycol unit. The number of carbon atoms in the ester substituent is preferably 1 or more, more preferably 2 or more, and is preferably 10 or less, more preferably 6 or less. The number of carbon atoms in the ester substituent is preferably 1 to 10, more preferably 2 to 6.

[0021] Examples of the (meth)acrylic acid alkyl ester having the linear alkyl group include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, and n-hexyl (meth)acrylate. Among them, methyl (meth)acrylate, ethyl (meth)acrylate, and n-butyl (meth)acrylate are preferred, and methyl methacrylate, ethyl methacrylate, and n-butyl methacrylate are more preferred. In addition, since a slurry composition having excellent low-temperature decomposition properties can be obtained, it is preferable that the (meth)acrylic resin further has a segment derived from n-butyl methacrylate.

[0022] The (meth)acrylic polyalkylene glycol having the linear alkylene glycol unit may be one having an ethylene glycol unit or one having a trimethylene glycol unit. The (meth)acrylic polyalkylene glycol having the linear alkylene glycol unit may have an alkoxy group at the end. Examples of the alkoxy group include a methoxy group, an ethoxy group, and a butoxy group. The alkoxy group does not have a branched structure. Among them, the (meth)acrylic polyalkylene glycol having an ethylene glycol unit is preferred, and the (meth)acrylic methoxypolyethylene glycol is more preferred. The polyalkylene glycol (meth)acrylate having the linear alkylene glycol units preferably has 4 or more, more preferably 10 or more, and preferably has 23 or less, more preferably 20 or less. The number of the alkylene glycol units is preferably 4 to 23, more preferably 10 to 20.

[0023] Examples of the (meth)acrylic acid ester in which the ester substituent has a cyclic structure include (meth)acrylic acid esters having a cyclic alkyl group, such as cyclohexyl (meth)acrylate and isobornyl (meth)acrylate, and (meth)acrylic acid esters having a glycidyl group, such as glycidyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, and 3,4-epoxycyclohexylmethyl (meth)acrylate.

[0024] In particular, it is preferable to use a (meth)acrylic resin containing a large amount of oxygen as a monomer, and a (meth)acrylic acid polyalkylene glycol having a linear polyalkylene glycol unit has a large oxygen content, and it is preferable to have a segment derived from such a (meth)acrylic acid ester. The depolymerization reaction of (meth)acrylic resin is an endothermic reaction, and it is difficult to obtain the heat required for decomposition at low temperatures. By having segments derived from monomers containing a lot of oxygen as described above, the (meth)acrylic resin is decomposed by combustion using its own oxygen near the ceiling temperature even in a nitrogen atmosphere, which can further improve low-temperature decomposition properties. The (meth)acrylate polyalkylene glycol having the linear alkylene glycol unit preferably has an oxygen composition ratio of 30% by weight or more, more preferably 35% by weight or more.

[0025] The content of the segment derived from the (meth)acrylic acid ester in which the ester substituent is linear in the (meth)acrylic resin is, for example, 0% by weight or more, preferably 1% by weight or more, more preferably 5% by weight or more, even more preferably 10% by weight or more, preferably 40% by weight or less, and more preferably 30% by weight or less. The content of the segment derived from the (meth)acrylic acid ester in which the ester substituent is linear is preferably 0 to 40% by weight, more preferably 1 to 30% by weight, even more preferably 5 to 30% by weight, and even more preferably 10 to 30% by weight. By setting the content within the above range, handling properties such as printability are improved. The above content can be measured, for example, by pyrolysis GC-MS.

[0026] The total content of the segment derived from isobutyl methacrylate, the segment derived from n-butyl methacrylate, and the segment derived from 2-ethylhexyl methacrylate in the (meth)acrylic resin is preferably 70% by weight or more. By satisfying the above-mentioned requirements, a slurry composition having excellent low-temperature decomposition properties can be obtained. The total content is preferably 75% by weight or more, and more preferably 80% by weight or more. There is no particular upper limit, and it is, for example, 100% by weight or less, and more preferably 90% by weight or less. The total content is preferably 70 to 100% by weight, more preferably 75 to 90% by weight, and more preferably 80 to 90% by weight. The above content can be measured, for example, by pyrolysis GC-MS.

[0027] The (meth)acrylic resin may have a segment derived from a (meth)acrylic acid ester having a glycidyl group, a carboxyl group or a hydroxyl group. Examples of the (meth)acrylic acid ester having a glycidyl group include glycidyl (meth)acrylate, 4-hydroxybutyl acrylate glycidyl ether, and 3,4-epoxycyclohexylmethyl methacrylate. Examples of the (meth)acrylic acid ester having a hydroxyl group or a carboxyl group include 2-hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and (meth)acrylic acid.

[0028] The content of the segment derived from the (meth)acrylic acid ester having a glycidyl group, a carboxyl group or a hydroxyl group in the (meth)acrylic resin is preferably 1% by weight or more, more preferably 4% by weight or more, and is preferably 10% by weight or less, more preferably 7% by weight or less. The content of the segment derived from the (meth)acrylic acid ester having a glycidyl group, a carboxyl group or a hydroxyl group is preferably 1 to 10% by weight, more preferably 4 to 7% by weight. By setting the content within the above range, the low-temperature decomposition property can be further improved, and the toughness of the obtained inorganic particle-dispersed sheet can be improved.

[0029] The weight average molecular weight (Mw) of the (meth)acrylic resin is preferably 20,000 or more and 4,000,000 or less. When the Mw is 20,000 or more, the viscosity of the slurry composition is not too low, and the dispersibility of the inorganic particles can be improved.When the Mw is 4,000,000 or less, the coating strength can be increased, and the viscosity of the slurry composition is sufficiently high to improve storage stability and provide excellent printability. The Mw is preferably 30,000 or more, more preferably 40,000 or more, and is preferably 3 million or less, more preferably 2 million or less, even more preferably 1 million or less, and even more preferably 500,000 or less. The Mw is preferably 20,000 to 4 million, more preferably 30,000 to 3 million, even more preferably 40,000 to 2 million, even more preferably 40,000 to 1 million, and particularly preferably 40,000 to 500,000.

[0030] The ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the (meth)acrylic resin is usually 1 or more, preferably 1.5 or more, more preferably 2 or more, and preferably 5 or less, more preferably 3 or less. The Mw / Mn is preferably 1 to 5, more preferably 1.5 to 3, and even more preferably 2 to 3. By setting the content within the above range, the component with a low degree of polymerization is appropriately contained, so that the viscosity of the slurry composition falls within a suitable range, and productivity can be increased. The weight average molecular weight (Mw) and number average molecular weight (Mn) are average molecular weights calculated based on polystyrene standards, and can be obtained by GPC measurement using, for example, column LF-804 (manufactured by Showa Denko KK).

[0031] The glass transition temperature (Tg) of the (meth)acrylic resin is preferably 20° C. or higher, more preferably 30° C. or higher, and even more preferably 40° C. or higher, and is preferably 80° C. or lower, more preferably 70° C. or lower, even more preferably 60° C. or lower, and even more preferably 50° C. or lower. The Tg is preferably 20 to 80° C., more preferably 30 to 70° C., even more preferably 40 to 60° C., and even more preferably 40 to 50° C. The glass transition temperature (Tg) can be measured, for example, by using a differential scanning calorimeter (DSC).

[0032] The content of the (meth)acrylic resin in the binder resin (A) is preferably 10% by weight or more and preferably 100% by weight or less, more preferably 40% by weight or more and more preferably 50% by weight or less.

[0033] The content of the (meth)acrylic resin in the slurry composition is not particularly limited, but is preferably 3% by weight or more, more preferably 4% by weight or more, even more preferably 5% by weight or more, even more preferably 6% by weight or more, preferably 30% by weight or less, more preferably 20% by weight or less, and even more preferably 12% by weight or less. The content of the (meth)acrylic resin is preferably 3 to 30% by weight, more preferably 4 to 20% by weight, even more preferably 5 to 12% by weight, and even more preferably 6 to 12% by weight. By setting the content of the (meth)acrylic resin within the above range, a slurry composition that can be fired at a low temperature can be produced.

[0034] The method for producing the (meth)acrylic resin is not particularly limited. For example, a method may be mentioned in which an organic solvent or the like is added to a raw material monomer mixture containing a (meth)acrylic acid ester having a branched structure in an ester substituent to prepare a monomer mixture, and a polymerization initiator is added to the obtained monomer mixture to polymerize the monomer mixture to produce the (meth)acrylic resin. The polymerization method is not particularly limited, and examples thereof include emulsion polymerization, suspension polymerization, bulk polymerization, interfacial polymerization, solution polymerization, etc. Among these, solution polymerization is preferred.

[0035] Examples of the polymerization initiator include dilauryl peroxide, p-menthane hydroperoxide, diisopropylbenzene hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, cumene hydroxyperoxide, t-butyl hydroxyperoxide, cyclohexanone peroxide, disuccinic acid peroxide, potassium persulfate, and ammonium persulfate. Examples of commercially available products include Permenta H, Percumyl P, Perocta H, Percumyl H-80, Perloyl 355, Perbutyl H-69, Perhexa H, Perloyl SA, Perloyl L (all manufactured by NOF Corporation), Trigonox 27, and Trigonox 421 (all manufactured by Nouryon).

[0036] <Inorganic particles (B)> The slurry composition contains inorganic particles. Examples of the inorganic particles include ceramic powder, glass powder, phosphor particles, silicon oxide, and metal particles.

[0037] Examples of the ceramic powder include alumina, ferrite, zirconia, zircon, barium zirconate, calcium zirconate, titanium oxide, barium titanate, strontium titanate, calcium titanate, magnesium titanate, zinc titanate, lanthanum titanate, neodymium titanate, lead zirconate titanate, aluminum nitride, and the like. Mi, Examples of the material include silicon nitride, boron nitride, gallium nitride, boron carbide, barium stannate, calcium stannate, magnesium silicate, mullite, steatite, cordierite, and forsterite. Also, ITO, FTO, niobium oxide, vanadium oxide, tungsten oxide, lanthanum strontium manganite, lanthanum strontium cobalt ferrite, yttrium stabilized zirconia, gadolinium doped ceria, nickel oxide, lanthanum chromite, Sm2Fe 17 N3, Nd2Fe 14 B, MnAlC, L 10 FeNi, La 2 / 3-x Li 3x TiO3, La (1-x) / 3 Li x NbO3, LaGaO3, LaScO3, CaZrO3, (La 0.875 Sr 0.125 )MnO3, PbZrTiO3, SrBi2Ta2O9, BiFeO3, KNbO3, PbVO3, BiCo3, Bi(Zn 1 / 2 Ti 1 / 2 )3 etc. can also be used. The above ceramic powder can be suitably used as a slurry composition for ceramic green sheets.

[0038] Examples of the glass powder include glass powders such as bismuth oxide glass, silicate glass, lead glass, zinc glass, and boron glass, as well as glass powders of various silicon oxides such as CaO-Al2O3-SiO2, MgO-Al2O3-SiO2, and LiO2-Al2O3-SiO2. In addition, the glass powder may be a mixture of SnO-B2O3-P2O5-Al2O3, a mixture of PbO-B2O3-SiO2, a mixture of BaO-ZnO-B2O3-SiO2, a mixture of ZnO-Bi2O3-B2O3-SiO2, a mixture of Bi2O3-B2O3-BaO-CuO, a mixture of Bi2O3-ZnO-B2O3-Al2O3-SrO, a mixture of ZnO-Bi2O3-B2O3, a mixture of Bi2O3-SiO2, a mixture of P2O5-Na2O-CaO-BaO-Al2O3-B2O3, a mixture of P2O5-SnO, a mixture of P2O5-SnO-B2O3, a mixture of P2O5-Na2O-CaO-BaO-Al2O3 ... O5-SnO-SiO2 mixture, CuO-P2O5-RO mixture, SiO2-B2O3-ZnO-Na2O-Li2O-NaF-V2O5 mixture, P2O5-ZnO-SnO-R2O-RO mixture, B2O3-SiO2-ZnO mixture, B2O3-SiO2-Al2O3-ZrO2 mixture, SiO2-B2O3-ZnO-R2O-RO mixture, SiO2-B2O3-Al2O3-RO-R2O mixture, SrO-ZnO-P2O5 mixture, SrO-ZnO-P2O5 mixture, BaO-ZnO-B2O3-SiO2 mixture, etc. can also be used. R represents an element selected from the group consisting of Zn, Ba, Ca, Mg, Sr, Sn, Ni, Fe, and Mn. In particular, a glass powder of a PbO-B2O3-SiO2 mixture, or a lead-free glass powder such as a lead-free BaO-ZnO-B2O3-SiO2 mixture or a lead-free ZnO-Bi2O3-B2O3-SiO2 mixture is preferred.

[0039] The inorganic particles contain lithium, and thus can be suitably used as an electrolyte slurry composition for all-solid-state lithium-ion batteries. Specific examples of the inorganic particles containing lithium include low-melting glass such as LiO2·Al2O3·SiO2-based inorganic glass, lithium sulfur-based glass such as Li2S-MxSy (M=B, Si, Ge, P), lithium cobalt composite oxide such as LiCoO2, lithium manganese composite oxide such as LiMnO4, lithium nickel composite oxide, lithium vanadium composite oxide, lithium zirconium composite oxide, lithium hafnium composite oxide, and lithium silicophosphate (Li 3.5 S 0.5 P 0.5 O4), lithium titanium phosphate (LiTi2(PO4)3), lithium titanate (Li4Ti5O 12 ), Li 4 / 3 Ti 5 / 3 O4, lithium germanium phosphate (LiGe2(PO4)3), Li2-SiS glass, Li4GeS4-Li3PS4 glass, LiSiO3, LiMn2O4, Li2S-P2S5 glass and ceramics, Li2O-SiO2, Li2O-V2O5-SiO2, LiS-SiS2-Li4SiO4 glass, ionic conductive oxides such as LiPON, lithium oxide compounds such as Li2O-P2O5-B2O3 and Li2O-GeO2Ba, LixAlyTiz(PO4)3 glass, LaxLiyTiOz glass, LixGeyPzO4 glass, Li7La3Zr2O 12 Lithium-based glasses, LivSiwPxSyClz-based glasses, lithium niobium oxides such as LiNbO3, lithium alumina compounds such as Li-β-alumina, Li 14 Examples include lithium zinc oxides such as Zn(GeO4)4.

[0040] The phosphor particles are not particularly limited, and for example, a blue phosphor material, a red phosphor material, a green phosphor material, etc., which are conventionally known as phosphor materials for displays, can be used as the phosphor material. As the blue phosphor material, for example, MgAl 10 O 17 :Eu, Y2SiO5:Ce series, CaWO4:Pb series, BaMgAl 14 O23 :Eu series, BaMgAl 16 O 27 :Eu series, BaMg2Al 14 O 23 :Eu series, BaMg2Al 14 O 27 ZnS:Eu-based and ZnS:(Ag,Cd)-based materials are used. Red phosphor materials include, for example, Y2O3:Eu-based, Y2SiO5:Eu-based, Y3Al5O 12 :Eu system, Zn3(PO4)2:Mn system, YBO3:Eu system, (Y,Gd)BO3:Eu system, GdBO3:Eu system, ScBO3:Eu system, LuBO3:Eu system are used. As green phosphor material, for example, Zn2SiO4:Mn system, BaAl 12 O 19 :Mn-based, SrAl 13 O 19 :Mn-based, CaAl 12 O 19 :Mn series, YBO3:Tb series, BaMgAl 14 O 23 :Mn system, LuBO3:Tb system, GdBO3:Tb system, ScBO3:Tb system, Sr6Si3O3Cl4:Eu system are used. Others include ZnO:Zn system, ZnS:(Cu,Al) system, ZnS:Ag system, Y2O2S:Eu system, ZnS:Zn system, (Y,Cd)BO3:Eu system, BaMgAl 12 O 23 :Eu-based materials can also be used.

[0041] The metal particles are not particularly limited, and examples thereof include powders of iron, copper, nickel, palladium, platinum, gold, silver, aluminum, tungsten, and alloys thereof. In addition, metals such as copper and iron, which have good adsorption properties with carboxyl groups, amino groups, amide groups, etc. and are easily oxidized, can also be preferably used. These metal powders may be used alone or in combination of two or more kinds. In addition to metal complexes, various carbon blacks, carbon nanotubes, and the like may also be used.

[0042] The average particle size of the inorganic particles is preferably 0.1 μm or more, more preferably 0.5 μm or more, and is preferably 100 μm or less, more preferably 50 μm or less. The average particle size is preferably 0.1 to 100 μm, more preferably 0.5 to 50 μm. When the specific surface area of ​​the inorganic particles is within the above range, the specific surface area is not too large, and a dense molded product can be obtained by firing. The average particle size of the inorganic particles can be measured, for example, by observation using a transmission electron microscope or by a light scattering method for a dispersion liquid.

[0043] The content of the inorganic particles in the slurry composition is not particularly limited, but is preferably 40% by weight or more and 90% by weight or less. By setting the content within the above range, the density of the inorganic particles can be sufficiently increased. In addition, the dispersibility of the inorganic particles can be sufficiently increased to improve the moldability. The content of the inorganic particles is preferably 40 to 90% by weight.

[0044] <Solvent (C)> The slurry composition contains a solvent. The above-mentioned solvent is not particularly limited, but it is preferable to use a solvent that has excellent coating properties, drying properties, and inorganic particle dispersibility when producing an inorganic particle-dispersed sheet. Examples of the solvent include alcohols such as aliphatic alcohols, glycols, terpene alcohols, and aromatic alcohols, aromatic hydrocarbons, esters, ketones, and N-methylpyrrolidone. Examples of the aliphatic alcohols include ethanol and isopropanol. Examples of the glycols include ethylene glycol monobutyl ether, diethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoisobutyl ether, butyl carbitol, ethylene glycol monoethyl ether acetate, trimethylpentanediol monoisobutyrate, butyl carbitol acetate, Texanol, ethylene glycol monophenyl ether, propylene glycol monophenyl ether, ethylene glycol ethyl ether, and ethyl carbitol acetate. Examples of the terpene alcohols include terpineol, dihydroterpineol, terpineol acetate, and dihydroterpineol acetate. Examples of the aromatic alcohols include benzyl alcohol, ethylene glycol monophenyl ether, propylene glycol monophenyl ether, and cresol. The aromatic hydrocarbons include toluene and the like. Examples of the esters include ethyl acetate, butyl acetate, hexyl acetate, isoamyl acetate, butyl butyrate, methoxybutyl acetate, butyl lactate, dioctyl phthalate, and dioctyl adipate. Examples of the ketones include methyl ethyl ketone, methyl isobutyl ketone, and isophorone. Of these, butyl acetate, hexyl acetate, butyl butyrate, isoamyl acetate, methoxybutyl acetate, ethyl carbitol acetate, terpineol, terpineol acetate, dihydroterpineol, dihydroterpineol acetate, diethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoisobutyl ether, butyl carbitol, butyl carbitol acetate, and texanol are preferred, with butyl acetate, hexyl acetate, terpineol, and ethyl carbitol acetate being more preferred, and butyl acetate, terpineol, and benzyl alcohol being even more preferred. These organic solvents may be used alone or in combination of two or more thereof. In one embodiment of the present invention, the organic solvent is different from the binder removal assistant.

[0045] The boiling point of the solvent is preferably 90° C. or higher and 230° C. or lower, more preferably 120° C. or higher and more preferably 210° C. or lower. The boiling point is preferably 90 to 230° C. and more preferably 120 to 210° C. When the content is within the above range, evaporation does not occur too quickly, and drying can be easily performed using a fan oven, etc. Furthermore, printability can be improved, and a coated product with a smooth surface can be obtained.

[0046] The content of the solvent in the slurry composition is preferably 10% by weight or more and preferably 60% by weight or less, more preferably 20% by weight or more and more preferably 50% by weight or less. By setting the content within the above range, it is possible to further improve the coatability and the dispersibility of the inorganic particles.The content of the solvent is preferably from 10 to 60% by weight, and more preferably from 20 to 50% by weight.

[0047] <Debinding aid (D)> The slurry composition contains a debinding aid. The binder aid contains a carboxylic acid anhydride having a boiling point of 200° C. or higher and an oxygen atom content of 40% by weight or higher. The binder removal aid has a large amount of oxygen atoms in its molecule, and burns by consuming its own oxygen even in a nitrogen atmosphere, and when mixed with the binder resin, it assists the thermal decomposition of the binder resin. Therefore, it is possible to promote the binder removal process without increasing the oxygen partial pressure, significantly reduce sintering residues, and suppress the oxidation of inorganic particles, resulting in the production of highly reliable electronic components.

[0048] The content of oxygen atoms in the carboxylic acid anhydride is 40% by weight or more, preferably 45% by weight or more, and more preferably 48% by weight or more, from the viewpoint of binder removal property and inhibition of oxidation of inorganic particles. Also, from the viewpoint of solubility in a solvent, the content of oxygen atoms is preferably 55% by weight or less, and preferably 50% by weight or less. The content of oxygen atoms is preferably 40 to 55% by weight, more preferably 45 to 50% by weight, and even more preferably 48 to 50% by weight. The oxygen atom content is the content of oxygen atoms in one molecule and can be calculated based on the molecular weight of the binder removal aid and the atomic weight of oxygen. The oxygen atom content can be calculated assuming that the atomic weight of carbon is 12, the atomic weight of hydrogen is 1, and the atomic weight of oxygen is 16.

[0049] The boiling point of the carboxylic acid anhydride is 200° C. or higher. By setting the boiling point within the above range, when the slurry composition is coated and dried, it is possible to exhibit the effect of accelerating the binder removal treatment without evaporating together with the solvent. The boiling point is preferably 390° C. or lower, more preferably 250° C. or higher, more preferably 370° C. or lower, even more preferably 270° C. or higher, and even more preferably 350° C. or lower. The boiling point is preferably 200 to 390° C., more preferably 250 to 370° C., and even more preferably 270 to 350° C. The carboxylic acid anhydride having a boiling point of 270° C. or more functions as a plasticizer. By using such a carboxylic acid anhydride as a binder removal assistant, it becomes possible to reduce the amount of plasticizer added. In addition, since the above-mentioned carboxylic acid anhydrides start to burn at less than 200° C. in an air atmosphere, it is preferable to measure the boiling point under reduced pressure conditions. The method of converting the boiling point under reduced pressure conditions can be the method described in Science of Petroleum, Vol. II, p. 1281 (1938), etc.

[0050] Examples of the carboxylic acid anhydride include anhydrides of succinic acid, maleic acid, citric acid, glutaric acid, diglycolic acid, methoxyacetic acid, itaconic acid, citraconic acid, trimellitic acid, cyclobutanetetracarboxylic acid, tricarballylic acid, butanetetracarboxylic acid, cyclopentanetetracarboxylic acid, and malonic acid. Of these, anhydrides of succinic acid, maleic acid, citric acid, glutaric acid, diglycolic acid, methoxyacetic acid, itaconic acid, citraconic acid, trimellitic acid, cyclobutanetetracarboxylic acid, tricarballylic acid, butanetetracarboxylic acid, and cyclopentanetetracarboxylic acid are preferred, and anhydrides of succinic acid, maleic acid, citric acid, diglycolic acid, and methoxyacetic acid are more preferred. The above carboxylic acid anhydrides may be used alone or in combination of two or more. By using the above-mentioned carboxylic acid anhydride as a binder removal aid, it is possible to promote the binder removal process without increasing the oxygen partial pressure, thereby significantly reducing the sintering residue, and also to suppress the oxidation of inorganic particles, thereby producing highly reliable electronic components.

[0051] Specific examples of the carboxylic acid anhydride include succinic anhydride (boiling point 261° C., oxygen content 48.0% by weight), maleic anhydride (boiling point 202° C., oxygen content 49.0% by weight), citric anhydride (boiling point 520° C., oxygen content 55.2% by weight), glutaric anhydride (boiling point 283° C., oxygen content 42.1% by weight), diglycolic anhydride (boiling point 240° C., oxygen content 55.2% by weight), itaconic anhydride (boiling point 232° C., oxygen content 42.9% by weight), citraconic anhydride (boiling point 213° C., oxygen content 42.9% by weight), trimellitic anhydride (boiling point 393° C., oxygen content 42.9% by weight), and carboxylic acid anhydride (boiling point 413° C., oxygen content 42.9% by weight). 41.7% by weight), 1,2,3,4-cyclobutanetetracarboxylic dianhydride (boiling point 545°C, oxygen content 49.0% by weight), 2-methoxyacetic anhydride (boiling point 215°C, oxygen content 49.4% by weight), tricarballylic anhydride (boiling point 390°C, oxygen content 50.6% by weight), 1,2,3,4-butanetetracarboxylic dianhydride (boiling point 492°C, oxygen content 48.5% by weight), 1,2,3,4-cyclopentanetetracarboxylic dianhydride (boiling point 527°C, oxygen content 45.7% by weight), malonic anhydride (oxygen content 55.8% by weight), and the like. Among these, succinic anhydride, maleic anhydride, citric anhydride, diglycolic anhydride, itaconic anhydride, citraconic anhydride, trimellitic anhydride, 1,2,3,4-cyclobutanetetracarboxylic dianhydride, 2-methoxyacetic anhydride, tricarballylic anhydride, 1,2,3,4-butanetetracarboxylic dianhydride, and 1,2,3,4-cyclopentanetetracarboxylic dianhydride are preferred because they have the advantages of a high oxygen content and a high boiling point, and succinic anhydride, maleic anhydride, citric anhydride, diglycolic anhydride, and 2-methoxyacetic anhydride are more preferred.

[0052] The content of the carboxylic acid anhydride in the slurry composition is preferably 0.1% by weight or more, preferably 15% by weight or less, more preferably 0.2% by weight or more, more preferably 10% by weight or less, even more preferably 0.4% by weight or more, and even more preferably 5% by weight or less. By setting the content within the above range, the binder removal effect is sufficiently enhanced, and the binder removal aid does not precipitate in the slurry composition, resulting in excellent printability. The content of the carboxylic acid anhydride is preferably 0.1 to 15% by weight, more preferably 0.2 to 10% by weight, and even more preferably 0.4 to 5% by weight.

[0053] The content of the carboxylic acid anhydride in the slurry composition is preferably 5 parts by weight or more and 30 parts by weight or less based on 100 parts by weight of the binder resin (A). By setting the content within the above range, it is possible to sufficiently enhance the binder removal effect while preventing the binder removal aid from precipitating in the slurry composition, thereby providing a composition with excellent printability. The content of the carboxylic acid anhydride is preferably 8 parts by weight or more, and preferably 25 parts by weight or less, more preferably 10 parts by weight or more, and more preferably 20 parts by weight or less. The content of the carboxylic acid anhydride is preferably 5 to 30 parts by weight, more preferably 8 to 25 parts by weight, and even more preferably 10 to 20 parts by weight, relative to 100 parts by weight of the binder resin (A).

[0054] The binder removal aid (D) may contain other binder removal aids such as inorganic oxides, such as borate glass, in addition to the carboxylic acid anhydrides.

[0055] The content of the binder removal aid (D) in the slurry composition is preferably 0.1% by weight or more, preferably 15% by weight or less, more preferably 0.2% by weight or more, more preferably 10% by weight or less, even more preferably 0.4% by weight or more, and even more preferably 5% by weight or less. The content of the binder removal aid (D) is preferably 0.1 to 15% by weight, more preferably 0.2 to 10% by weight, and even more preferably 0.4 to 5% by weight. By setting the content within the above range, the binder removal effect can be sufficiently enhanced, and the binder removal aid does not precipitate in the slurry composition, resulting in excellent printability.

[0056] The content of the binder removal aid (D) in the slurry composition is preferably 5 parts by weight or more and 30 parts by weight or less based on 100 parts by weight of the binder resin (A). By setting the content within the above range, it is possible to sufficiently enhance the binder removal effect while preventing the binder removal aid from precipitating in the slurry composition, thereby providing a composition with excellent printability. The content of the carboxylic acid anhydride is preferably 8 parts by weight or more, and preferably 25 parts by weight or less, more preferably 10 parts by weight or more, and more preferably 20 parts by weight or less, relative to 100 parts by weight of the (meth)acrylic resin. The content of the carboxylic acid anhydride is preferably 5 to 30 parts by weight, more preferably 8 to 25 parts by weight, and even more preferably 10 to 20 parts by weight, relative to 100 parts by weight of the (meth)acrylic resin.

[0057] (Other additives) The slurry composition may contain other additives such as a plasticizer, a surfactant, a dispersant, etc., in addition to the binder resin (A), the inorganic particles (B), the solvent (C), and the binder removal aid (D) containing a carboxylic acid anhydride.

[0058] Examples of the plasticizer include di(butoxyethyl) adipate, dibutoxyethoxyethyl adipate, triethylene glycol dibutyl ether, triethylene glycol bis(2-ethylhexanoate), triethylene glycol dihexanoate, tributyl acetyl citrate, diethyl acetyl citrate, dibutyl acetyl citrate, dibutyl sebacate, triacetin, diethyl acetyloxymalonate, and diethyl ethoxymalonate. By using these plasticizers, it is possible to reduce the amount of plasticizer added compared to when using normal plasticizers. The plasticizer is different from the binder removal aid. In addition, since plasticizers having aromatic rings such as benzene rings in their structure tend to burn and turn into soot, it is preferable to use non-aromatic plasticizers, and it is more preferable to use plasticizers that contain components derived from adipic acid, triethylene glycol, or citric acid.

[0059] The above-mentioned plasticizer is preferably one having an alkyl group with 2 or more carbon atoms, such as an ethyl group or a butyl group, and more preferably one having an alkyl group with 4 or more carbon atoms. By containing an alkyl group having two or more carbon atoms, it is possible to suppress the absorption of moisture into the plasticizer, and prevent defects such as voids and blisters from occurring in the obtained inorganic particle-dispersed sheet. In particular, it is preferable that the alkyl group of the plasticizer is located at the molecular terminal. A plasticizer having a substituent with 2 carbon atoms such as an ethyl group at the molecular end is compatible with a segment derived from ethyl methacrylate, and a plasticizer having a substituent with 4 carbon atoms such as a butyl group at the molecular end is compatible with a segment derived from butyl methacrylate. Such a plasticizer is compatible with the above-mentioned (meth)acrylic resin and can improve the brittleness of the resin. Furthermore, a plasticizer having a butoxyethyl group is compatible with both a segment derived from ethyl methacrylate and a segment derived from butyl methacrylate, and can be preferably used.

[0060] The plasticizer preferably has a carbon:oxygen ratio of 5:1 to 3:1. By setting the carbon:oxygen ratio within the above range, the combustibility of the plasticizer can be improved, and the generation of residual carbon can be prevented. In addition, the compatibility with the (meth)acrylic resin can be improved, and even a small amount of the plasticizer can exert a plasticizing effect. Furthermore, high-boiling organic solvents having a propylene glycol skeleton or a trimethylene glycol skeleton can also be preferably used so long as they contain an alkyl group having 4 or more carbon atoms and have a carbon:oxygen ratio of 5:1 to 3:1.

[0061] The boiling point of the plasticizer is preferably 240°C or higher and less than 390°C. When the content is within the above range, the resin is easily evaporated in the drying step, and therefore, it is possible to prevent the resin from remaining in the molded body, and also to prevent the generation of residual carbon. The above boiling point refers to the boiling point at normal pressure.

[0062] The content of the plasticizer in the slurry composition is not particularly limited, but is preferably 0.1% by weight or more and 3.0% by weight or less. The content of the plasticizer is preferably 0.1 to 3.0% by weight. By setting the thickness within the above range, both sheet handling property and sintering property can be achieved.

[0063] Examples of the surfactant include cationic surfactants, anionic surfactants, and nonionic surfactants. The nonionic surfactant is not particularly limited, but is preferably a nonionic surfactant with an HLB value of 10 or more and 20 or less. Here, the HLB value is used as an index representing the hydrophilicity and lipophilicity of a surfactant, and several calculation methods have been proposed. For example, for an ester-based surfactant, the saponification value is S, the acid value of the fatty acid constituting the surfactant is A, and the HLB value is defined as 20 (1-S / A). Specifically, a nonionic surfactant having a polyethylene oxide in which an alkylene ether is added to an aliphatic chain is suitable, and specifically, for example, polyoxyethylene lauryl ether, polyoxyethylene cetyl ether, etc. are preferably used. The nonionic surfactant has good thermal decomposition properties, but if added in large quantities, the thermal decomposition properties of the inorganic particle dispersion slurry composition may decrease, so the preferred upper limit of the content is 5% by weight.

[0064] Suitable examples of the dispersant include fatty acids, aliphatic amines, alkanolamides, and phosphoric esters. Silane coupling agents may also be used. The fatty acid is not particularly limited, and examples thereof include saturated fatty acids such as behenic acid, stearic acid, palmitic acid, myristic acid, lauric acid, capric acid, caprylic acid, coconut fatty acid, etc., and unsaturated fatty acids such as oleic acid, linoleic acid, linolenic acid, sorbic acid, beef tallow fatty acid, and hardened castor fatty acid, etc. Among these, lauric acid, stearic acid, oleic acid, etc. are preferred. The aliphatic amine is not particularly limited, and examples thereof include laurylamine, myristylamine, cetylamine, stearylamine, oleylamine, alkyl(coconut)amine, alkyl(hardened beef tallow)amine, alkyl(beef tallow)amine, and alkyl(soybean)amine. The alkanolamide is not particularly limited, and examples thereof include coconut fatty acid diethanolamide, beef tallow fatty acid diethanolamide, lauric acid diethanolamide, and oleic acid diethanolamide. The phosphate ester is not particularly limited, and examples thereof include polyoxyethylene alkyl ether phosphate ester and polyoxyethylene alkyl allyl ether phosphate ester.

[0065] Since the slurry composition contains the carboxylic acid anhydride as the binder removal aid (D), it is preferable that the water content is low, preferably 1% by weight or less, and more preferably 0.1% by weight or less. The method for reducing the water content is not particularly limited, but examples thereof include a reduced pressure degassing method and a molecular sieve method.

[0066] The viscosity of the slurry composition is not particularly limited, but the preferred lower limit of the viscosity is 0.1 Pa s and the preferred upper limit is 100 Pa s when measured at 20° C. using a Brookfield viscometer with the probe rotation speed set to 5 rpm. The viscosity is preferably 0.1 to 100 Pa s. By setting the viscosity at 0.1 Pa s or more, it becomes possible for the obtained inorganic particle-dispersed sheet to maintain a predetermined shape after coating by die coat printing method, etc. Furthermore, by setting the viscosity at 100 Pa s or less, defects such as indelible die coating marks can be prevented, and excellent printability can be achieved.

[0067] The method for preparing the slurry composition is not particularly limited, and examples thereof include conventionally known stirring methods. Specific examples thereof include a method in which the binder resin (A), the inorganic particles (B), the solvent (C), the binder removal aid (D) containing the carboxylic acid anhydride, and other additives added as necessary are mixed and stirred with a three-roll mill or the like.

[0068] By using the above slurry composition, electronic components, magnets such as neodymium magnets, etc. can be produced.

[0069] Examples of the electronic components include die attach paste (ACP), die attach film (ACF), TSV, TGV via electrodes, touch panels, various circuits for RFID and sensor substrates, various die bonding agents, sealing agents for MEMS devices, solar cells, multilayer ceramic capacitors, LTCC, silicon capacitors, electrode materials for all-solid-state batteries, etc. In addition to the above electrode circuit applications, the material can also be used for piezoelectric elements, inductors, sintered magnets, antibacterial materials and electromagnetic wave shields, catalysts, fluorescent materials, etc.

[0070] For example, the above-mentioned slurry composition is applied onto a substrate and dried to produce an inorganic particle dispersion molding, and the obtained inorganic particle dispersion molding is further heat-treated to remove the binder (degreasing), and then heated to the sintering temperature of the inorganic particles and fired to obtain an inorganic sintered body. The present invention also provides a method for producing an inorganic sintered body, comprising the steps of drying the inorganic particle-dispersed slurry composition to obtain an inorganic particle-dispersed compact, and degreasing the inorganic particle-dispersed compact at 300° C. or lower.

[0071] The method for forming the inorganic particle dispersion slurry composition is not particularly limited, but may be a method of forming a coil shape by alternately applying a U-shaped opening to a screen plate from above and below, a method of directly printing on a substrate to form a laminate, or a method of dip-coating the inorganic particle dispersion slurry composition on a substrate. By using a solvent with a high boiling point, it is possible to form the composition using screen printing or the like.

[0072] The slurry composition is applied onto a support film having one side subjected to a release treatment, and the solvent is dried to obtain a sheet-like inorganic particle dispersion molding, whereby an inorganic particle dispersion sheet can be produced. The inorganic particle-dispersed sheet preferably has a thickness of 1 to 20 μm.

[0073] The coating method may be, for example, a coating method using a roll coater, a die coater, a squeeze coater, a curtain coater, or the like.

[0074] The drying method may be, for example, drying by heating. The drying temperature is preferably 80°C or higher and 130°C or lower.

[0075] The support film used in producing the inorganic particle-dispersed sheet is preferably a resin film having heat resistance, solvent resistance and flexibility. The flexibility of the support film allows the inorganic particle-dispersed slurry composition to be applied to the surface of the support film by a roll coater, a blade coater or the like, and the obtained inorganic particle-dispersed sheet-forming film can be stored and supplied in a rolled state.

[0076] Examples of the resin that forms the support film include polyethylene terephthalate, polyester, polyethylene, polypropylene, polystyrene, polyimide, polyvinyl alcohol, polyvinyl chloride, fluorine-containing resins such as polyfluoroethylene, nylon, cellulose, and the like. The thickness of the support film is preferably, for example, 20 to 100 μm. In addition, the surface of the support film is preferably subjected to a release treatment, which allows the support film to be easily peeled off in the transfer step.

[0077] The above-mentioned inorganic particle dispersion molded body is subjected to a degreasing step in which the molded body is heat-treated to remove the binder (degreasing), and then a firing step in which the molded body is heated to the sintering temperature of the inorganic particles and fired, thereby obtaining an inorganic sintered body.

[0078] The degreasing step is preferably carried out at 300° C. or lower. By using the above-mentioned slurry composition, the binder removal process can be carried out sufficiently even in a low-temperature environment of 300° C. or less. The above temperature is preferably 250°C or higher and 280°C or lower. The time for which the above temperature is maintained is preferably 0.1 hour or more and 1 hour or less. Furthermore, the temperature rise rate is preferably 20° C. / min or more and 100° C. / min or less. The degreasing step is preferably carried out in a nitrogen atmosphere if the inorganic particles used are susceptible to deterioration by oxygen in the air, and may be carried out in an air atmosphere if the inorganic particles used are relatively stable against oxygen in the air. When carried out in an air atmosphere, the binder removal treatment can proceed more quickly compared to a nitrogen atmosphere, and the amount of firing residue remaining in the sintered body can be reduced.

[0079] After the degreasing step, a firing step is carried out in which the mixture is heated to the sintering temperature of the inorganic particles. In this way, an inorganic sintered body can be obtained. The firing temperature is not particularly limited since it is appropriately set depending on the type of inorganic particles, but is, for example, 300° C. or higher and 1000° C. or lower. The temperature rise rate is preferably 20° C. / min or more and 100° C. / min or less. The firing step may be carried out in a nitrogen atmosphere, an air atmosphere, a vacuum, or a reducing atmosphere containing a trace amount of hydrogen gas.

[0080] By using ceramic powder as the inorganic particles (B) in the above slurry composition, a ceramic sintered body can be produced. The ceramic sintered body may be a ceramic laminate or a ceramic single layer body. The ceramic laminate can be used for laminated ceramic capacitors, laminated ceramic substrates, all-solid-state batteries, etc., and the ceramic single layer can be used for ceramic packages, low-temperature co-fired ceramics (LTCC), circuit boards such as alumina, ceramic heat dissipation substrates such as aluminum nitride and silicon nitride, electrostatic chucks, ceramic columns, temperature sensors, piezoelectric elements, various machine parts, etc. The slurry composition and the inorganic particle-dispersed sheet can be used as materials for the positive electrode, solid electrolyte, and negative electrode of an all-solid-state battery to produce an all-solid-state battery, and the slurry composition and the inorganic particle-dispersed sheet can be used as materials for a dielectric green sheet and an electrode paste to produce a multilayer ceramic capacitor.

[0081] The method for producing the all-solid-state battery preferably includes the steps of: preparing an inorganic particle-dispersed sheet using the slurry composition; preparing an electrode active material sheet by molding a slurry for an electrode active material layer containing an electrode active material and a binder for an electrode active material layer; laminating the electrode active material sheet and the inorganic particle-dispersed sheet to prepare a laminate; and firing the laminate.

[0082] The method for producing the multilayer ceramic capacitor preferably includes the steps of: preparing an inorganic particle-dispersed sheet using the slurry composition; printing and drying a conductive paste on the inorganic particle-dispersed sheet to prepare a dielectric sheet; and laminating the dielectric sheets.

[0083] The conductive paste contains a conductive powder. The material of the conductive powder is not particularly limited as long as it is a material having conductivity, and examples thereof include nickel, palladium, indium, platinum, gold, silver, copper, and alloys thereof, etc. These conductive powders may be used alone or in combination of two or more kinds.

[0084] The method for printing the conductive paste is not particularly limited, and examples thereof include screen printing, die coat printing, offset printing, gravure printing, and inkjet printing.

[0085] In the method for producing the multilayer ceramic capacitor, the dielectric sheet on which the conductive paste is printed and the electrode layer are laminated to obtain the multilayer ceramic capacitor.

[0086] An electronic component can be produced by laminating an inorganic particle-dispersed sheet containing the binder removal aid and a conductive paste composition, firing the green ceramic component to produce a fired ceramic component, and then providing external electrodes. The firing conditions are not particularly limited, but firing is preferably carried out in an inert gas or reducing gas atmosphere so as to prevent the transition metal used in the electrode layer from being oxidized. Furthermore, the binder removal step and the inorganic particle firing step may be maintained at a temperature suited to the purpose. The binder removal process involves holding the material at 250°C or higher and 350°C or lower for 1 to 3 hours in an inert gas atmosphere to reduce the content of organic substances such as binders and plasticizers to 20% or less, and then moving on to the inorganic particle firing process. In the inorganic particle firing process, the inorganic particles are sintered by increasing the temperature from 800°C to 1300°C in an inert gas atmosphere or a reducing gas atmosphere. The heating rate is preferably 5°C / min or higher and 100°C / min or lower.

[0087] An electronic component can be produced by providing external electrodes on the fired ceramic component. The composition and method of installation of the external electrodes are not particularly limited. Metal plating, thermosetting conductive resin, metal paste, etc. can be preferably used. Metals that can be used in the metal paste are preferably those that have high conductivity and can be sintered at low temperatures. Examples include copper, nickel, silver, and palladium.

[0088] For example, in the above slurry composition, the inorganic particles (B) are NdFe 14 When B is used, the above slurry composition is applied to a ferrite magnet substrate, dried, and then magnetically pressed. The magnetic force is aligned while the substrate is fired at about 300°C, thereby producing a neodymium magnet with reduced loss of magnetic force. For example, La 2 / 3-x Li 3x When using TiO3(LLTO), the above slurry composition is applied onto a negative electrode Li foil, dried, and then laminated with a positive electrode sheet consisting of LLTO as a positive electrode, acetylene black as a conductive additive, and lithium niobium oxide as a positive electrode active material, and then fired at about 300°C to produce a large-capacity all-solid-state battery. Furthermore, by combining a slurry composition using barium titanate as the inorganic particles (B) with a slurry composition using nickel particles as the inorganic particles (B), a multilayer ceramic capacitor can be produced. In addition, an inductor can be manufactured by combining a slurry composition using Ni-Zn-Cu ferrite as the inorganic particles (B) and a slurry composition using copper particles as the inorganic particles (B). When the sintering property of the inorganic particles (B) is insufficient at about 300° C., borosilicate, phosphate, or the like may be added as a sintering aid. Effect of the Invention

[0089] According to the present invention, it is possible to provide an inorganic particle dispersion slurry composition that is excellent in storage stability and printability, can promote binder removal treatment even at low temperatures, can suppress oxidation of inorganic particles, has little residual carbon after firing, is excellent in sinterability, and can obtain highly reliable electronic components. It is also possible to provide a method for producing an inorganic sintered body using the slurry composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0090] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0091] <Preparation of (meth)acrylic resin> (Synthesis Example 1) A 2L separable flask equipped with a stirrer, a cooler, a thermometer, a hot water bath, and a nitrogen gas inlet was prepared. 50 parts by weight of isobutyl methacrylate (iBMA) was added to the 2L separable flask. Furthermore, 50 parts by weight of n-butyl methacrylate (nBMA) was added. Furthermore, 100 parts by weight of terpineol was mixed as an organic solvent to obtain a monomer mixture. After removing dissolved oxygen by bubbling nitrogen gas into the monomer mixture, the flask was heated to 80°C in a hot water bath. Then, 2.0 parts by weight of lauryl peroxide as a polymerization initiator was added in several portions, and after 6 hours, the polymerization was terminated to obtain a composition containing a (meth)acrylic resin. The resin solid content was 50.0% by weight. The obtained composition containing the (meth)acrylic resin was dried and dissolved in tetrahydrofuran (THF) at a resin concentration of 0.1% by weight. The weight average molecular weight (Mw) in terms of polystyrene was measured by GPC using a SHODEX LF-804 column. The Mw was as shown in Table 1.

[0092] (Synthesis Example 2) A 2L separable flask equipped with a stirrer, a condenser, a thermometer, a hot water bath, and a nitrogen gas inlet was prepared. 60 parts by weight of isobutyl methacrylate (iBMA) and 20 parts by weight of 2-ethylhexyl methacrylate (2EHMA) were added to the 2L separable flask. Furthermore, 20 parts by weight of n-butyl methacrylate (BMA) was added. Furthermore, 10 parts by weight of butyl acetate was mixed as an organic solvent to obtain a monomer mixture. After removing dissolved oxygen by bubbling nitrogen gas into the monomer mixture, the flask was heated in a water bath until the temperature inside reached 80°C. 2.0 parts by weight of lauryl peroxide as a polymerization initiator was added in several portions, and the polymerization was terminated after 6 hours. The resin solid content was 90.9% by weight.

[0093] (Synthesis Example 3) A (meth)acrylic resin was prepared in the same manner as in Synthesis Example 1, except that the amount of iBMA added was 40 parts by weight and the amount of nBMA added was 60 parts by weight.

[0094] (Synthesis Example 4) A (meth)acrylic resin was prepared in the same manner as in Synthesis Example 2, except that the amount of iBMA added was 40 parts by weight, no 2EHMA was added, and the amount of nBMA added was 60 parts by weight.

[0095] Example 1 10.0 parts by weight of the (meth)acrylic resin obtained in Synthesis Example 1 as the binder resin (A), 2.0 parts by weight of succinic anhydride as the binder removal aid (D) and 38.0 parts by weight of terpineol as the solvent (C) were added and uniformly dissolved using a high-speed stirrer. 10 GeP2S 12 50.0 parts by weight of LGPS (average particle size 10 μm) was added, and the inorganic particles were dispersed using a three-roll mill to obtain an inorganic particle dispersion slurry composition.

[0096] The obtained slurry composition was used to print a 5 cm square image on a ceramic plate using a screen printer, and then dried for 30 minutes in a fan oven set at 120° C. to obtain a printed substrate. The obtained printed substrate was heat-treated for 60 minutes in an electric furnace whose inside temperature was set at 280° C. and whose inside was replaced with nitrogen gas, to complete degreasing and obtain a fired substrate.

[0097] Example 2 50.0 parts by weight of Li2S-P2S5 glass powder (average particle size 10 μm) as inorganic particles (B) and 38.0 parts by weight of butyl acetate as solvent (C) were mixed and the inorganic particles (B) were stirred for 2 hours using a closed bead mill device. Then, 10.0 parts by weight of the (meth)acrylic resin obtained in Synthesis Example 2 as binder resin (A) and 2.0 parts by weight of maleic anhydride as binder removal aid (D) were added, and the mixture was further stirred for 3 hours to obtain an inorganic particle dispersion slurry composition.

[0098] The obtained slurry composition was printed on an indium substrate using a die coater and dried for 30 minutes in a fan oven set at 120° C. to obtain a printed substrate. The obtained printed substrate was heat-treated for 60 minutes in an electric furnace whose inside temperature was set at 280° C. and whose inside was replaced with nitrogen gas, to complete degreasing and obtain a fired substrate.

[0099] (Examples 3 to 5, Comparative Examples 1, 3, 4, and 6) An inorganic particle dispersion slurry composition and a fired substrate were obtained in the same manner as in Example 1, except that the compositions shown in Table 1 were used. In addition, Nd2Fe 14 In Examples 3 to 5 and Comparative Example 3 using B (average particle size 5 μm), the inner temperature of the electric furnace was set to 300° C. for degreasing, and then the substrate was fired at 700° C. for 1 hour in a nitrogen atmosphere to obtain a fired substrate.

[0100] (Examples 6 to 8, Comparative Examples 2, 5, and 7) An inorganic particle dispersion slurry composition and a fired substrate were obtained in the same manner as in Example 2, except that the compositions shown in Table 1 were used. In addition, the inorganic particles (B) are Sm2Fe 17 In Examples 6 and 7 and Comparative Example 5 using N3 (average particle size 5 μm), the inner temperature of the electric furnace was set to 300° C. for degreasing, and then the substrate was fired at 400° C. for 1 hour in a nitrogen atmosphere to obtain a fired substrate. In Example 8 and Comparative Example 7, in which GaN (average particle diameter 3 μm) was used as the inorganic particles (B), the internal temperature of the electric furnace was set to 300° C. and degreasing was performed, and then the substrate was fired at 1100° C. for 2 hours in a nitrogen atmosphere to obtain a fired substrate.

[0101] Comparative Example 8 An inorganic fine particle dispersion slurry composition was obtained in the same manner as in Example 1, except that the composition shown in Table 3 was used. The obtained slurry composition was printed on an indium substrate using a die coater and dried for 30 minutes in a fan oven set at 120° C. to obtain a printed substrate. The obtained printed substrate was heat-treated for 60 minutes in an electric furnace with an internal temperature set at 300° C. and an atmosphere of dry air, to complete degreasing and obtain a fired substrate.

[0102] (Example 9, Comparative Example 9) Except for using the compositions shown in Table 3, the same procedures as in Example 2 were carried out to obtain inorganic particle dispersion slurry compositions and fired substrates.

[0103] (Example 10, Comparative Example 10) Except for using the compositions shown in Table 3, the same procedures as in Example 3 were carried out to obtain inorganic particle dispersion slurry compositions and fired substrates.

[0104] Comparative Example 11 An inorganic particle dispersion slurry composition and a fired substrate were obtained in the same manner as in Example 6, except that the compositions shown in Table 3 were used.

[0105] (evaluation) The obtained slurry composition and fired substrate were evaluated as follows, and the results are shown in Tables 2 and 4.

[0106] (1) Viscosity The viscosity of the obtained slurry composition was measured at 25°C immediately after preparation using a B-type viscometer. After leaving the composition to stand for 2 weeks after preparation, the viscosity was similarly measured at 25°C. Furthermore, the viscosity change rate was calculated using the viscosity immediately after preparation and the viscosity after 2 weeks according to the following formula, and evaluated according to the following criteria. It is to be noted that a smaller viscosity change rate indicates excellent storage stability. Viscosity change rate (%) = |(viscosity after 2 weeks - viscosity immediately after preparation) / (viscosity immediately after preparation)| x 100 ◯: Viscosity change rate was less than 20%. ×: The viscosity change rate was 20% or more.

[0107] (2) Printability The printed image on the printed substrate was visually observed and evaluated according to the following criteria. ◯: No scratches, bleeding, etc., and good. ×: Defects such as scratches and bleeding were observed.

[0108] (3) Carbon Residue The obtained sintered substrate was pulverized, and the residual carbon amount was measured from the CO amount and CO2 amount obtained by combustion in a high-frequency induction heating furnace and infrared absorption method, and was evaluated according to the following criteria. ○: The residual carbon content was 200 ppm or less. ×: The amount of residual carbon was more than 200 ppm.

[0109] (4) Oxygen content The amount of oxygen contained in the obtained fired substrate was measured using an oxygen / nitrogen analyzer EMGA-920, and the measurement was evaluated according to the following criteria. ◯: The oxygen content was less than 0.2% by weight. ×: The oxygen content was 0.2% by weight or more.

[0110] (5) Cross-section observation The cross-sections of the sintered substrates were observed using an SEM and rated according to the following criteria: Voids in the sintered substrate are believed to result from the decomposition of the resin, and it can be said that electronic components with higher reliability can be obtained when there are fewer voids. ○: No voids were observed. △: 1 to less than 10 voids were found. ×: 10 or more voids were found.

[0111] [Table 1]

[0112] [Table 2]

[0113] [Table 3]

[0114] [Table 4] [Industrial Applicability]

[0115] According to the present invention, it is possible to provide an inorganic particle dispersion slurry composition that is excellent in storage stability and printability, can promote binder removal treatment even at low temperatures, can suppress oxidation of inorganic particles, has little residual carbon after firing, is excellent in sinterability, and can obtain highly reliable electronic components. It is also possible to provide a method for producing an inorganic sintered body using the slurry composition.

Claims

1. Contains a binder resin (A), inorganic particles (B) and a solvent (C), Further, the binder removal aid (D) contains a carboxylic acid anhydride having a boiling point of 200° C. or more and an oxygen atom content of 40% by weight or more, The inorganic particle dispersion slurry composition, wherein the content of the carboxylic acid anhydride is 5 parts by weight or more and 30 parts by weight or less based on 100 parts by weight of the binder resin (A).

2. The inorganic particle dispersion slurry composition according to claim 1, wherein the carboxylic acid anhydride is an anhydride of at least one carboxylic acid selected from the group consisting of succinic acid, maleic acid, citric acid, glutaric acid, diglycolic acid, methoxyacetic acid, itaconic acid, citraconic acid, trimellitic acid, cyclobutane tetracarboxylic acid, tricarballylic acid, butane tetracarboxylic acid, and cyclopentane tetracarboxylic acid.

3. The inorganic particle dispersion slurry composition according to claim 1 , wherein the binder resin (A) comprises a (meth)acrylic resin.

4. 4. The inorganic particle dispersion slurry composition according to claim 3, wherein the (meth)acrylic resin contains 50% by weight or more of a segment derived from a (meth)acrylic acid ester having an ester substituent with 4 or more carbon atoms and a branched structure in the ester substituent.

5. 3. A method for producing an inorganic sintered body, comprising: a step of drying the inorganic particle dispersion slurry composition according to claim 1 to obtain an inorganic particle dispersion compact; and a step of degreasing the inorganic particle dispersion compact at 300° C. or less.

Citation Information

Patent Citations

  • Production of sintered ceramic

    JP1988319248A

  • Production of ceramic sintered body

    JP1989033054A

  • Ceramic green sheet and method of manufacturing the same

    JP2011173765A

  • Glass paste

    JP2011178606A

  • Laminate green sheet and all-solid type secondary battery

    JP2018077989A