Catalyst for olefin polymerization and method for producing olefin polymer
A catalyst system with a nitrogen-doped carbon material, organoaluminum compound, and transition metal compound addresses the challenge of dispersing carbon materials in polyolefins, achieving high polymerization activity and cost-effective dispersion in olefin polymers with enhanced conductivity.
Patent Information
- Application Number
- JP2020180631
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-28
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-10-28
AI Technical Summary
Existing methods for dispersing carbon materials in polyolefins face challenges in achieving high dispersibility while avoiding the use of expensive organoaluminum oxy compounds, which are typically required for effective polymerization catalysts.
A catalyst system comprising a specific carbon material with a nitrogen-doped graphene structure, an organoaluminum compound, and a transition metal compound is used, which allows for efficient dispersion and high polymerization activity without the need for expensive cocatalysts.
The catalyst system achieves high polymerization activity and efficient dispersion of carbon materials in olefin polymers, reducing production costs and enhancing thermal and electrical conductivity.
Smart Images

Figure 0007579672000007 
Figure 0007579672000001 
Figure 0007579672000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an olefin polymerization catalyst and a process for producing an olefin polymer using the olefin polymerization catalyst. [Background technology]
[0002] By blending carbon materials such as graphite, graphene, and carbon nanotubes (CNTs) with polyolefins, it is possible to impart high thermal conductivity, electrical conductivity, and weather resistance to the polyolefins (see, for example, Patent Document 1). However, there is a problem in that it is difficult to disperse these carbon materials in polyolefins.
[0003] In order to improve the dispersibility of carbon materials in polyolefins, methods have been proposed for producing composites of carbon materials and polyolefins by polymerization using a polymerization catalyst in which a metal complex is supported or impregnated on the carbon material (see, for example, Patent Documents 2 to 4). However, all of these methods use expensive organoaluminum oxy compounds such as methylaluminoxane (MAO) as co-catalysts, and there is a demand for reducing the production cost. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-071079 A [Patent Document 2] JP 2006-176601 A [Patent Document 3] JP 2007-161741 A [Patent Document 4] Special Publication No. 2005-506404 Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide an olefin polymerization catalyst which shows high polymerization activity without using an expensive organoaluminum oxy compound and is capable of producing an olefin polymer in which a carbon material is efficiently dispersed, and a method for producing an olefin polymer using the olefin polymerization catalyst. [Means for solving the problem]
[0006] The present inventors have conducted extensive research to solve the above problems, and as a result have found that the above problems can be solved by using a specific carbon material and a specific organoaluminum compound as a co-catalyst, thereby completing the present invention.
[0007] That is, the olefin polymerization catalyst according to the present invention is A carbon material (A) that satisfies the following requirements (AI) and (A-II); An organoaluminum compound (B) represented by the following general formula (BI), A transition metal compound (C) represented by the following general formula (CI): Includes. (AI) The nitrogen atom / carbon atom molar ratio as measured by X-ray photoelectron spectroscopy (XPS) is 0.003 or more and 0.300 or less; (A-II) A nitrogen-doped carbon material having a graphene structure in which nitrogen atoms are substituted or introduced; R a m Al(OR b ) n H p X q (BI) [In the general formula (BI), R a and R b represents a hydrocarbon group having 1 to 15 carbon atoms, which may be the same or different, X represents a halogen atom, m represents an integer of 1 to 3, n represents an integer of 0 to 2, p represents an integer of 0 to 2, q represents an integer of 0 to 2, and m+n+p+q=3. L m MX n ···(CI) [In formula (CI), M is an atom selected from the group consisting of atoms of groups 3, 4, 5, 6, 7, 8, 9, 10, and 11 of the periodic table, and lanthanide atoms; L is a ligand, and a plurality of L may be the same or different from each other, and a plurality of L may be connected by a substituent in L, but at least one L contains at least one atom selected from the group consisting of boron, nitrogen, oxygen, phosphorus, sulfur, and selenium, m is an integer of 2 or more, n is an integer of 1 to 4 that satisfies the valence of M; X is a leaving group selected from a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, a conjugated diene derivative group, and a neutral ligand capable of coordinating with a lone electron pair, and when n is 2 or more, multiple Xs may be the same or different from each other and may be bonded to each other to form a ring. Effect of the Invention
[0008] According to the present invention, it is possible to provide an olefin polymerization catalyst which shows high polymerization activity without using an expensive organoaluminum oxy compound and is capable of producing an olefin polymer in which a carbon material is efficiently dispersed, and a method for producing an olefin polymer using the olefin polymerization catalyst. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a schematic diagram showing an example of the configuration of an in-liquid plasma generator used in the production of carbon material (A). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described in detail below. [Olefin polymerization catalyst] The olefin polymerization catalyst of the present invention comprises A carbon material (A) that satisfies the following requirements (AI) and (A-II); An organoaluminum compound (B) represented by the following general formula (BI), A transition metal compound (C) represented by the following general formula (CI): The present invention is characterized by comprising:
[0011] (AI) The nitrogen atom / carbon atom molar ratio in X-ray photoelectron spectroscopy (XPS) is 0.003 or more and 0.300 or less. (A-II) Nitrogen-doped carbon materials having a graphene structure in which nitrogen atoms are substituted or introduced are included.
[0012] R a m Al(OR b ) n H p X q (BI) In the above general formula (BI), R a and R b represents a hydrocarbon group having 1 to 15 carbon atoms, which may be the same or different, X represents a halogen atom, m is an integer of 1 to 3, n is an integer of 0 to 2, p is an integer of 0 to 2, q is an integer of 0 to 2, and m+n+p+q=3.
[0013] L m MX n ···(CI) In the general formula (CI), M represents an atom selected from the group consisting of atoms of Groups 3, 4, 5, 6, 7, 8, 9, 10, and 11 of the periodic table, and lanthanide atoms; L represents a ligand, and a plurality of L may be the same or different from each other, and a plurality of L may be connected by a substituent in L, but at least one L contains at least one atom selected from the group consisting of boron, nitrogen, oxygen, phosphorus, sulfur, and selenium; and m is 2 or more. n is an integer of 1 to 4 satisfying the valence of M; X is a leaving group selected from the group consisting of hydrogen atoms, halogen atoms, hydrocarbon groups, halogen-containing groups, silicon-containing groups, oxygen-containing groups, sulfur-containing groups, nitrogen-containing groups, phosphorus-containing groups, boron-containing groups, aluminum-containing groups, conjugated diene derivative groups, and neutral ligands capable of coordinating with lone electron pairs; when n is 2 or more, multiple Xs may be the same or different and may be bonded to each other to form a ring.
[0014] Each component constituting the olefin polymerization catalyst of the present invention will be described below. <Carbon material (A)> The carbon material (A) used in the present invention satisfies the following requirements (AI) and (A-II).
[0015] (AI) The nitrogen atom / carbon atom molar ratio in X-ray photoelectron spectroscopy (XPS) is 0.003 or more and 0.300 or less, preferably 0.004 or more and 0.200 or less, and more preferably 0.005 or more and 0.100 or less.
[0016] The nitrogen atom / carbon atom molar ratio is a value obtained by X-ray photoelectron spectroscopy (XPS) measurement, specifically, the peaks of nitrogen atoms and carbon atoms in the spectrum obtained from the carbon material (A). strength The nitrogen atom / carbon atom molar ratio can be calculated from the above.
[0017] A higher nitrogen atom / carbon atom molar ratio is preferable because it promotes coordination to a cation generated from a transition metal compound (C) described later. However, if the nitrogen atom / carbon atom molar ratio is too high, the graphene structure in the carbon material (A) tends to decrease.
[0018] (A-II) Nitrogen-doped carbon materials having a graphene structure in which nitrogen atoms are substituted or introduced are included. The nitrogen-doped carbon material is a material in which nitrogen atoms are introduced into a carbon material, and typically has a structure in which nitrogen atoms are doped (substituted or introduced) into the positions of carbon atoms in a graphene structure. The carbon material (A) preferably contains this nitrogen-doped carbon material on at least a part of the surface of the carbon material.
[0019] The carbon material other than the nitrogen-doped carbon material in the carbon material (A) used in the present invention, and the carbon material to be doped with nitrogen atoms in the nitrogen-doped carbon material, can be used without any particular limitation as long as it has a graphene structure in at least a part of its structure. Such a carbon material may be either a carbonaceous material with relatively low crystallinity or a graphitic material with relatively high crystallinity. Examples of the carbon material include graphene, graphene flakes in which 1 to 10 sheets of graphene are stacked by van der Waals forces, graphite with a larger number of layers than graphene flakes, carbon nanotubes in which sheet-like graphene is rolled into a cylindrical shape, onion-like carbon in which multiple graphene sheets are closed in a concentric shell shape, carbon nanoscrolls in which sheet-like graphene is rolled into a spiral shape, carbon nanohorns in which sheet-like graphene is rolled into a horn shape, carbon nanocones in which sheet-like graphene is rolled into a cone shape, carbon nanowalls in which sheet-like graphene has grown vertically to a substrate with an arbitrary cross-sectional shape, and carbon black made of many graphite crystallites. The carbon material may be an aggregate in which many primary particles are gathered, or may be a strong aggregate (aggregate) in which the primary particles are strongly aggregated, or may be a weak aggregate in which the primary particles are weakly aggregated. These carbon materials can be manufactured by a conventionally known method, or commercially available products can be used.
[0020] The carbon material (A) may be a carbon material that has been subjected to a surface modification or modification treatment (for example, introduction of a functional group, oxidation treatment, or reduction treatment), may contain a metal or the like, or may have some of the carbon atoms substituted with other atoms.
[0021] Examples of methods for producing nitrogen-doped carbon materials having a graphene structure in which nitrogen atoms have been substituted or introduced include a method of subjecting a carbon material to plasma treatment in a nitrogen atmosphere, as exemplified in ACS NANO, 2010, 1790, etc., and a method of subjecting a cyclic compound having a chemical composition containing carbon and nitrogen and at least a ring structure in at least a part thereof, as exemplified in JP-A-2014-100617 and JP-A-2019-189495, etc.
[0022] A cyclic compound having a ring structure means a group of organic compounds in which constituent atoms are bonded in at least one ring in a chemical structure. That is, it is a general term for organic compounds having a ring structure based on a carbon skeleton. Therefore, the cyclic compound may be a monocyclic compound having one ring in one molecule, or a polycyclic compound having two or more rings, and may be various cyclic compounds such as a monocyclic compound having a ring constituted by one type of atom, or a heterocyclic compound having a ring constituted by two or more types of atoms. Furthermore, it may be an aromatic cyclic compound having a conjugated unsaturated ring structure (typically, an aromatic hydrocarbon), or an alicyclic compound containing one or more saturated or unsaturated carbon rings that do not have aromaticity. It is preferably a cyclic compound having at least one unsaturated bond. There is no limit to the number of atoms that constitute such a ring structure, and it may be, for example, a compound having a small ring, a medium ring, or a large ring, and typically, a cyclic compound having about 3 to 10 membered rings can be considered.
[0023] A preferred embodiment of the method for producing a nitrogen-doped carbon material is a method in which plasma is generated in a liquid containing the cyclic compound having a five-membered ring or a six-membered ring or both in its chemical structure.
[0024] The nitrogen-doped carbon material obtained by the above-mentioned method is considered to have a chemical structure in which several of the cyclic compounds, which are raw material compounds, are polymerized. For example, a 6-membered pyridine-type structure or a 5-membered pyrrole-type structure can be formed at the end of the graphene structure. Therefore, the raw material compound used in the present invention is preferably one having a 5-membered or 6-membered ring structure, since nitrogen atoms can be suitably introduced into the graphene structure. Such a cyclic compound may be a cyclic compound whose ring structure is composed of only carbon, or a heterocyclic compound whose ring structure contains atoms other than carbon. The cyclic compound may also contain atoms other than carbon and nitrogen. Specific preferred examples include pyrrole, pyrrolidine, imidazole, thiazole, piperidine, pyridine, 2-cyanopyridine, pyrazine, pyrimidine, triazine, quinoline, isoquinoline, xaquinoline, cinnoline, pteridine, indole, purine, aniline, 1-naphthylamine, 2-naphthylamine, phenylenediamine, and derivatives thereof, and these may be used alone or in combination of two or more.
[0025] The cyclic compound may have a substituent. Such a substituent may be various organic functional groups, and examples thereof include a hydrocarbon group, a hydroxy group, an aldehyde group, a carboxyl group, a carbonyl group, a halogeno group, a silicon-containing functional group, a sulfur-containing functional group, a nitrogen-containing functional group, and a phosphorus-containing functional group. More preferably, examples thereof include a hydrocarbon group represented by a linear, branched or cyclic alkyl group having 1 to 10 carbon atoms, a vinyl group, an aryl group, and the like; a hydroxy group, an aldehyde group, a carboxyl group, a carbonyl group, a halogeno group such as a fluoro group, a chloro group, or a bromo group; a silicon-containing functional group represented by an alkylsilyl group, and the like; a sulfur-containing functional group represented by a thiol group, a sulfo group, and the like; a nitrogen-containing functional group represented by an aldehyde group, a nitro group, and the like; and a phosphorus-containing functional group represented by a phosphonic acid group, and the like.
[0026] The cyclic compound may be one containing the above-mentioned cyclic compound as a part of its structure. For example, it may be a compound such as a bipyridine compound or a phenylpyridine compound containing pyridine as a part of its structure. It may also be a polymer such as polypyrrole or polythiophene in which multiple pyrroles or multiple thiophenes are bonded.
[0027] As is clear from the above, the raw material compounds may naturally contain hydrogen and oxygen, unless they are present as different elements. The raw material compound may be liquid at room temperature and normal pressure (typically 25° C., 1 atm, hereinafter the same). For this reason, a liquid consisting of 100% raw material compound can be used as a liquid (liquid phase) containing the raw material compound. Also, such a raw material compound may be diluted in a suitable solvent. In this case, the solvent is not particularly limited and may be water, an organic solvent such as alcohol or benzene, or a mixed solvent thereof. In addition, when the raw material compound is solid at room temperature and normal pressure, it may be in the form of a solution in which it is dissolved in a suitable solvent, or a dispersion in which the raw material compound is microscopically dispersed. The amount of raw material compound contained in the liquid can be appropriately adjusted.
[0028] A preferred embodiment of the method for producing a nitrogen-doped carbon material is a method in which a pair of linear electrodes is placed in the liquid containing the raw material compound, and the plasma is generated by applying a pulse voltage between the electrodes with a pulse width of 0.1 μs to 5 μs and a repetition frequency of 10 Hz to 150 Hz. With this configuration, most of the bubbles generated in the liquid by Joule heat generated between the linear electrodes can be maintained in a stable state in the liquid without floating up to the water surface, and plasma can be generated in the bubbles in a stable state. This makes it possible to produce a carbon-based catalyst more efficiently and stably.
[0029] In a preferred embodiment of the method for producing a carbon-based catalyst, the plasma is glow discharge plasma. The plasma generated in the liquid may be in the form of spark discharge, corona discharge, glow discharge, or arc discharge. Among them, glow discharge plasma is a more preferred form of in-liquid plasma that can be used in the production of the nitrogen-doped carbon material. This makes it possible to generate non-equilibrium low-temperature plasma, and to efficiently synthesize the nitrogen-doped carbon material without destroying the structure of the raw material compound.
[0030] By generating the plasma in the liquid containing the raw material compound, the action of active species such as positive and negative ions, electrons, and radicals that constitute the plasma causes a polymerization reaction of the raw material compound contained in the liquid and the formation of a carbon skeleton. Regardless of the specific composition and structure of the nitrogen-doped carbon material produced in this way, the liquid, which was almost colorless and transparent to the human eye, changes to brown and then to black as the treatment with plasma progresses, so that it can be confirmed that the raw material compound, which is typically organic, is converted to inorganic carbon. This phenomenon is similar to the change in appearance of organic polymer materials such as cellulose, in which oxygen and hydrogen are lost as carbonization progresses, the carbon concentration increases, and the appearance changes from brown to black.
[0031] As the carbon material (A) used in the present invention, the nitrogen-doped carbon material obtained by the plasma treatment may be used as it is, or may be used after filtering with a membrane filter or the like, drying by heating in an oven or the like, pulverizing in a mortar, etc. Alternatively, the carbon material in a solid state may be added to a liquid containing the raw material compounds, and then the plasma treatment may be performed, so that at least a part of the surface of the carbon material is covered with the nitrogen-doped carbon material and used as the carbon material (A).
[0032] <Organoaluminum Compounds (B)> The organoaluminum compound (B) used in the present invention is a compound represented by the following general formula (BI).
[0033] R a m Al(OR b ) n H p X q (BI) In formula (BI), R a and R b represents a hydrocarbon group having 1 to 15 carbon atoms, which may be the same or different, X represents a halogen atom, m is an integer of 1 to 3, n is an integer of 0 to 2, p is an integer of 0 to 2, q is an integer of 0 to 2, and m+n+p+q=3.
[0034] The hydrocarbon group having 1 to 15 carbon atoms is, for example, an alkyl group, a cycloalkyl group, or an aryl group, and specific examples thereof include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an isobutyl group, a pentyl group, a hexyl group, an octyl group, a cyclopentyl group, a cyclohexyl group, a phenyl group, and a tolyl group.
[0035] Specific examples of the organoaluminum compound (B) include trialkylaluminums such as trimethylaluminum, triethylaluminum, triisopropylaluminum, triisobutylaluminum, trihexylaluminum, trioctylaluminum, and tri-2-ethylhexylaluminum; dialkylaluminum halides such as dimethylaluminum chloride, diethylaluminum chloride, diisopropylaluminum chloride, and dimethylaluminum bromide; alkylaluminum sesquihalides such as methylaluminum sesquichloride, ethylaluminum sesquichloride, isopropylaluminum sesquichloride, butylaluminum sesquichloride, and ethylaluminum sesquibromide; methylaluminum dichloride, ethylaluminum dichloride, isopropylaluminum dichloride, and ethylaluminum sesquibromide. Examples of the aluminum dihalide include alkyl aluminum dihalides such as aluminum dichloride and ethyl aluminum dibromide; alkyl aluminum hydrides such as dimethyl aluminum hydride, diethyl aluminum hydride, dihydrophenyl aluminum hydride, diisopropyl aluminum hydride, di-n-butyl aluminum hydride, diisobutyl aluminum hydride, diisohexyl aluminum hydride, diphenyl aluminum hydride, dicyclohexyl aluminum hydride, di-sec-heptyl aluminum hydride and di-sec-nonyl aluminum hydride; and dialkyl aluminum alkoxides such as dimethyl aluminum ethoxide, diethyl aluminum ethoxide, diisopropyl aluminum methoxide and diisobutyl aluminum ethoxide.
[0036] Among the above, trimethylaluminum, triethylaluminum, triisobutylaluminum, trihexylaluminum, trioctylaluminum, diethylaluminum chloride, ethylaluminum sesquichloride, ethylaluminum dichloride, diisobutylaluminum hydride, and diethylaluminum ethoxide are particularly preferred.
[0037] <Transition metal compound (C)> The transition metal compound (C) used in the present invention is a compound represented by the following general formula (CI).
[0038] L m MX n ···(CI) In formula (CI), M is an atom selected from the group consisting of atoms of groups 3, 4, 5, 6, 7, 8, 9, 10, and 11 of the periodic table, and lanthanide atoms. It is preferably an atom of a transition metal of group 4 of the periodic table, specifically a titanium atom, a zirconium atom, or a hafnium atom.
[0039] L is a ligand, and multiple L may be the same or different from each other, and multiple L may be connected by a substituent in L, but at least one L contains at least one atom selected from the group consisting of boron, nitrogen, oxygen, phosphorus, sulfur, and selenium. Among them, it is preferable that at least one atom selected from the group consisting of boron, nitrogen, oxygen, phosphorus, sulfur, and selenium in L is covalently bonded or coordinately bonded to the M. Furthermore, it is particularly preferable that the atom bonded to the M is a nitrogen atom or an oxygen atom. m is an integer of 2 or more, and is preferably 2. n is an integer of 1 to 4 which satisfies the valence of M, and is preferably 1 or 2.
[0040] X is a leaving group selected from the group consisting of a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, a conjugated diene derivative group, and a neutral ligand capable of coordinating with a lone electron pair. When n is 2 or more, multiple Xs may be the same or different from each other, and may be bonded to each other to form a ring. Preferred are a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a silicon-containing group, an oxygen-containing group, or a conjugated diene derivative group. The halogen atom includes fluorine, chlorine, bromine, iodine, etc., and is preferably chlorine or bromine.
[0041] Examples of the hydrocarbon group include linear or branched alkyl groups such as a methyl group, an ethyl group, a 1-propyl group, a 1-butyl group, a 1-pentyl group, a 1-hexyl group, a 1-heptyl group, a 1-octyl group, an isopropyl group, a sec-butyl group (butan-2-yl group), a tert-butyl group (2-methylpropan-2-yl group), an isobutyl group (2-methylpropyl group), a pentan-2-yl group, a 2-methylbutyl group, an isopentyl group (3-methylbutyl group), a neopentyl group (2,2-dimethylpropyl group), a cyamyl group (1,2-dimethylpropyl group), an isohexyl group (4-methylpentyl group), a 2,2-dimethylbutyl group, a 2,3-dimethylbutyl group, a 3,3-dimethylbutyl group, a thexyl group (2,3-dimethylbut-2-yl group), and a 4,4-dimethylpentyl group; Vinyl group, allyl group, propenyl group (prop-1-en-1-yl group), iso-propenyl group (prop-1-en-2-yl group), allenyl group (prop-1,2-dien-1-yl group), but-3-en-1-yl group, crotyl group (but-2-en-1-yl group), but-3-en-2-yl group, methallyl group (2-methylallyl group), buta-1,3-dienyl group, pentaerythritol group, linear or branched alkenyl groups or unsaturated double bond-containing groups, such as ter-4-en-1-yl group, pent-3-en-1-yl group, pent-2-en-1-yl group, iso-pentenyl group (3-methylbut-3-en-1-yl group), 2-methylbut-3-en-1-yl group, pent-4-en-2-yl group, and prenyl group (3-methylbut-2-en-1-yl group); linear or branched alkynyl groups or unsaturated triple bond-containing groups, such as ethynyl, prop-2-yn-1-yl, and propargyl (prop-1-yn-1-yl); aromatic linear or branched alkyl groups and unsaturated double bond-containing groups, such as benzyl, 2-methylbenzyl, 4-methylbenzyl, 2,4,6-trimethylbenzyl, 3,5-dimethylbenzyl, cuminyl (4-isopropylbenzyl), 2,4,6-tri-isopropylbenzyl, 4-tert-butylbenzyl, 3,5-di-tert-butylbenzyl, 1-phenylethyl, benzhydryl (diphenylmethyl), and cumyl; cyclic saturated hydrocarbon groups such as a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, a cycloheptatrienyl group, a norbornyl group, a norbornenyl group, a 1-adamantyl group, and a 2-adamantyl group; Aromatic substituents (aryl groups) such as phenyl, tolyl (methylphenyl), xylyl (dimethylphenyl), mesityl (2,4,6-trimethylphenyl), cumenyl (isopropylphenyl), julyl (2,3,5,6-tetramethylphenyl), 2,6-diisopropylphenyl, 2,4,6-triisopropylphenyl, 4-tert-butylphenyl, 3,5-ditert-butylphenyl, naphthyl, biphenyl, terphenyl, binaphthyl, acenaphthalenyl, phenanthryl, anthracenyl, pyrenyl, and ferrocenyl. Among the above hydrocarbon groups, a methyl group, an iso-butyl group, a neopentyl group, a cyamyl group, a benzyl group, a phenyl group, a tolyl group, a xylyl group, a mesityl group, and a cumenyl group are preferable.
[0042] Examples of the halogen-containing group include a fluoromethyl group, a trifluoromethyl group, a trichloromethyl group, a pentafluoroethyl group, a 2,2,2-trifluoroethyl group, a fluorophenyl group, a difluorophenyl group, a trifluorophenyl group, a tetrafluorophenyl group, a pentafluorophenyl group, a trifluoromethylphenyl group, a bistrifluoromethylphenyl group, and a hexachloroantimonate anion. Among the halogen-containing groups, a pentafluorophenyl group is preferable.
[0043] Examples of the silicon-containing group include a trimethylsilyl group, a triethylsilyl group, a tri-isopropylsilyl group, a diphenylmethylsilyl group, a tert-butyldimethylsilyl group, a tert-butyldiphenylsilyl group, a triphenylsilyl group, a tris(trimethylsilyl)silyl group, a trimethylsilylmethyl group, etc. Among the silicon-containing groups, a trimethylsilylmethyl group is preferred.
[0044] Examples of the oxygen-containing group include alkoxy groups such as a hydroxyl group, a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an allyloxy group, an n-butoxy group, a sec-butoxy group, an isobutoxy group, a tert-butoxy group, a benzyloxy group, and a methoxymethoxy group; aryloxy groups such as a phenoxy group, a 2,6-dimethylphenoxy group, a 2,6-di-isopropylphenoxy group, a 2,6-di-tert-butylphenoxy group, a 2,4,6-trimethylphenoxy group, and a 2,4,6-tri-isopropylphenoxy group; a furyl group, a benzofuryl group, a tetrahydrofuryl group, a pyranyl group, a tetrahydropyranyl group, an acetoxy group, a pivaloyloxy group, a benzoyloxy group, a trifluoroacetoxy group, a perchlorate anion, and a periodate anion. Among the oxygen-containing groups, a methoxy group, an ethoxy group, an iso-propoxy group, and a tert-butoxy group are preferred.
[0045] Examples of the sulfur-containing group include mesyl group (methanesulfonyl group), phenylsulfonyl group, tosyl group (p-toluenesulfonyl group), triflyl group (trifluoromethanesulfonyl group), nonaflyl group (nonafluorobutanesulfonyl group), thiophenyl group, mesylate group (methanesulfonate group), tosylate group (p-toluenesulfonate group), triflate group (trifluoromethanesulfonate group), nonaflate group (nonafluorobutanesulfonate group), thiophene group, benzothiophene group, etc. Among the sulfur-containing groups, triflate (trifluoromethanesulfonate) is preferred.
[0046] Examples of the nitrogen-containing group include an amino group, a cyano group, a methylamino group, a dimethylamino group, an ethylamino group, a diethylamino group, an allylamino group, a diallylamino group, a benzylamino group, a dibenzylamino group, a nitro group, a pyrrolidinyl group, a piperidinyl group, a morpholyl group, a pyrrolyl group, a bistriflyl imide group, a pyridinyl group, a pyrimidinyl group, a quinolinyl group, a triazinyl group, an oxazoline group, an imidazole group, an indole group, a carbazole group, etc. Among the nitrogen-containing groups, a dimethylamino group, a diethylamino group, a pyrrolidinyl group, a pyrrolyl group, and a bistriflyl imide group are preferred.
[0047] The phosphorus-containing group may, for example, be a hexafluorophosphate anion. Examples of the boron-containing group include tetrafluoroborate anion, tetrakis(pentafluorophenyl)borate anion, (methyl)(tris(pentafluorophenyl))borate anion, (benzyl)(tris(pentafluorophenyl))borate anion, tetrakis((3,5-bistrifluoromethyl)phenyl)borate anion, and groups represented by BR4 (each R independently represents hydrogen, an alkyl group, an aryl group which may have a substituent, a halogen atom, or the like).
[0048] Examples of the aluminum-containing group include [ka] or [ka] A four-membered ring represented by (M represents M in the general formula [3] or [4].) Examples of the group include a group represented by AlR4 (R represents hydrogen, an alkyl group, an aryl group which may have a substituent, a halogen atom, or the like) which can form the following formula:
[0049] Examples of the conjugated diene derivative group include a 1,3-butadienyl group, an isoprenyl group (2-methyl-1,3-butadienyl group), a piperylenyl group (1,3-pentadienyl group), a 2,4-hexadienyl group, a 1,4-diphenyl-1,3-pentadienyl group, a cyclopentadienyl group, and a metallocyclopentene group.
[0050] Examples of neutral ligands capable of coordinating with lone electron pairs include ethers such as diethyl ether, tetrahydrofuran, dioxane, and 1,2-dimethoxyethane; amines such as triethylamine and diethylamine; heterocyclic compounds such as pyridine, picoline, lutidine, oxazoline, oxazole, thiazole, imidazole, and thiophene; and organic phosphorus compounds such as triphenylphosphine, tricyclohexylphosphine, and tri-tert-butylphosphine.
[0051] The hydrocarbon group, the halogen-containing group, the silicon-containing group, the oxygen-containing group, the sulfur-containing group, the nitrogen-containing group, the phosphorus-containing group, the boron-containing group, the aluminum-containing group, the conjugated diene-based divalent derivative group, and the neutral ligand capable of coordinating with a lone electron pair may be further substituted with another substituent.
[0052] Examples of such transition metal compounds (C) include those described in JP-A-2003-206310, JP-A-2020-117711, JP-T-2009-537656, JP-T-2017-520548, JP-A-2004-269825, JP-A-2011-127121, JP-T-2016-527182, and JP-T-2017-535518, and preferably include transition metal compounds represented by the following general formula (C-II):
[0053] [ka]
[0054] In the general formula (C-II), M represents a transition metal atom of Group 4 or Group 5 of the periodic table, specifically a titanium atom, a zirconium atom, a hafnium atom, a vanadium atom, a niobium atom, or a tantalum atom. It is preferably a transition metal atom of Group 4 of the periodic table, specifically a titanium atom, a zirconium atom, or a hafnium atom, and particularly preferably a titanium atom or a zirconium atom.
[0055] In the general formula (C-II), the dotted line connecting the nitrogen atom (N) and M generally indicates that the nitrogen atom (N) is coordinated to M, but in the present invention, it does not matter whether the nitrogen atom (N) is coordinated to M.
[0056] R 1 , R 2 , R 3 , R 4 and R 5 may be the same or different and represent a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, a germanium-containing group, or a tin-containing group, and two or more of these may be linked to each other to form a ring.
[0057] Specific examples of the halogen atom, hydrocarbon group, halogen-containing group, silicon-containing group, oxygen-containing group, sulfur-containing group, nitrogen-containing group, phosphorus-containing group, and boron-containing group include the same as those exemplified as X in the general formula (CI), and the germanium-containing group or tin-containing group includes groups in which the silicon of the silicon-containing group is substituted with germanium or tin. In addition, structures having the halogen-containing group, silicon-containing group, oxygen-containing group, sulfur-containing group, nitrogen-containing group, phosphorus-containing group, and boron-containing group as substituents in the hydrocarbon group are also included in R. 1 , R 2 , R 3 , R 4 , R 5 The following can be given as an example.
[0058] Examples of the hydrocarbon group include linear or branched alkyl groups having 1 to 30 carbon atoms, preferably 1 to 20 carbon atoms, such as a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a neopentyl group, and an n-hexyl group; aryl groups having 6 to 30 carbon atoms, preferably 6 to 20 carbon atoms, such as a phenyl group, a naphthyl group, a biphenyl group, a terphenyl group, a phenanthryl group, or an anthracenyl group; These aryl groups are preferably substituted with 1 to 5 substituents such as a halogen atom, an alkyl group or alkoxy group having 1 to 30 carbon atoms, preferably 1 to 20 carbon atoms, or an aryl group or aryloxy group having 6 to 30 carbon atoms, preferably 6 to 20 carbon atoms.
[0059] R 1 is preferably a group selected from a linear or branched hydrocarbon group having 1 to 20 carbon atoms, an alkyl group having 3 to 20 carbon atoms, and an aryl group having 6 to 20 carbon atoms, from the viewpoint of olefin polymerization catalyst activity and of providing a high-molecular-weight ethylene polymer.
[0060] R 6is selected from a hydrogen atom, a hydrocarbon group having 1 to 3 carbon atoms consisting only of primary or secondary carbon, an alkyl group having 4 or more carbon atoms, an aryl-substituted alkyl group, a monocyclic or bicyclic cyclic hydrocarbon group, an aryl group, and a halogen atom. Among these, from the viewpoint of olefin polymerization catalyst activity and from the viewpoint of providing a high molecular weight ethylene polymer, it is preferably a group selected from an alkyl group having 4 or more carbon atoms, an aryl-substituted alkyl group, a monocyclic or bicyclic cyclic hydrocarbon group, and an aryl group, and more preferably includes a branched alkyl group such as a tert-butyl group; an aryl-substituted alkyl group such as a benzyl group, a 1-methyl-1-phenylethyl group (cumyl group), a 1-methyl-1,1-diphenylethyl group, or a 1,1,1-triphenylmethyl group (trityl group); or a cyclic hydrocarbon group having a ring structure having 6 to 15 carbon atoms, such as a cyclohexyl group, an adamantyl group, a norbornyl group, or a tetracyclododecyl group.
[0061] X is a leaving group, and is a substituent selected from the group consisting of hydrogen atoms, halogen atoms, hydrocarbon groups, anionic ligands, and neutral ligands capable of coordinating with lone electron pairs, and the anionic ligand is a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, or a conjugated diene derivative group. When n is 2 or more, the multiple Xs may be the same or different from each other, and may be bonded to each other to form a ring. Preferred are hydrogen atoms, halogen atoms, hydrocarbon groups having 1 to 20 carbon atoms, silicon-containing groups, oxygen-containing groups, or conjugated diene derivative groups.
[0062] Specific examples of X include the same as those exemplified as X in the above general formula (CI). n is an integer of 1 to 4 satisfying the valence of M, and is preferably 1 or 2.
[0063] A carbon material (A) that satisfies the requirements (AI) and (A-II); An organoaluminum compound (B) represented by the general formula (BI), A transition metal compound (C) represented by the general formula (CI), The olefin polymerization catalyst of the present invention, which comprises the above compound, can produce an olefin polymer having a carbon material efficiently dispersed therein with high polymerization activity.
[0064] The reason why the present invention exhibits its effects is not entirely clear, but the inventors speculate as follows. In order for the transition metal compound (C) to exhibit catalytic activity, it is necessary to chemically extract the leaving group (X in formula (CI)) from the electronically neutral transition metal compound (C) to form a cation. However, when only the organoaluminum compound (B) is brought into contact with the transition metal compound (C), the equilibrium between the neutral and cations in the transition metal compound (C) is biased toward the neutral side, resulting in low catalytic activity, as shown in "Chem.Rev., 2000,100,1391" and the like. In order to bias this equilibrium toward the cation side, it is necessary to physically or electronically shield the cations generated from the transition metal compound (C). The carbon material (A) of the present invention is mainly formed of sp 2 It is presumed that the nitrogen atoms introduced into the two-dimensional sheet structure formed by the bonded carbon coordinate with the cations generated from the transition metal compound (C), thereby physically or electronically shielding the cations. In particular, in the transition metal compound (C) that has a heteroatom with high electronegativity, it is believed that the strengthened cationicity promotes the coordination of the nitrogen atoms in the carbon material (A).
[0065] <Method for preparing olefin polymerization catalyst> One of the preferred embodiments of the olefin polymerization catalyst of the present invention is a solid catalyst component (X) prepared by contacting the carbon material (A), the organoaluminum compound (B) and the transition metal compound (C).
[0066] It is preferable that the organoaluminum compound (B) and the transition metal compound (C) are diluted with an inert solvent if they are liquid, or dissolved in an inert solvent if they are solid, and then contacted with the carbon material (A). Examples of the inert solvent include aromatic hydrocarbons such as benzene, toluene, and xylene, aliphatic saturated hydrocarbons such as hexane, heptane, and decane, alicyclic hydrocarbons such as cyclohexane and methylcyclopentane, halogenated hydrocarbons such as ethylene chloride, chlorobenzene, and dichloromethane, and mixtures thereof.
[0067] The method for contacting the carbon material (A), the organoaluminum compound (B), and the transition metal compound (C) is not particularly limited as long as the effects of the present invention are achieved. For example, a method of adding an inert solvent containing the organoaluminum compound (B) or the transition metal compound (C) to the carbon material (A) and impregnating it into the pores of the carbon material (A), a method of immersing the carbon material (A) in an inert solvent containing the organoaluminum compound (B) or the transition metal compound (C) and leaving it to stand, a method of mixing the carbon material (A) with an inert solvent containing the organoaluminum compound (B) or the transition metal compound (C) by stirring or the like, a method of passing an inert solvent containing the organoaluminum compound (B) or the transition metal compound (C) through the carbon material (A), and the like may be used. The carbon material (A) may be physically or chemically fixed on a solid support (including powder, granulated particles, fibers, films, and the like), and a heating operation may be performed during the contact.
[0068] Among these, a method in which the carbon material (A) is mixed with an inert solvent containing the organoaluminum compound (B) or the transition metal compound (C) by stirring or the like is preferred. After the contact operation, if necessary, the contact liquid is left to stand and the supernatant is removed, or the inert solvent is removed by a method such as filtration, and if necessary, the mixture is washed with the inert solvent.
[0069] The temperature when the heating operation is performed varies depending on the solvent used, but is usually from the freezing point of the solvent to 200° C. or less, preferably 150° C. or less. The contact time varies depending on the contact method and temperature, but is usually from 30 seconds to 1,000 hours, preferably from 5 minutes to 120 hours.
[0070] In any step of the contact method, by adding component (G), fouling during the polymerization reaction can be suppressed to a higher degree and the particle properties of the resulting polymer can be further improved. As component (G), a compound having a polar functional group can be used, and a nonionic surfactant is preferable, and a polyalkylene oxide block, a higher aliphatic amide, a polyalkylene oxide, a polyalkylene oxide alkyl ether, an alkyldiethanolamine, a polyoxyalkylene alkylamine, a glycerin fatty acid ester, or an N-acyl amino acid is more preferable. These may be used alone or in combination of two or more kinds.
[0071] The order of contacting the carbon material (A), the organoaluminum compound (B) and the transition metal compound (C) is not particularly limited as long as the effects of the present invention can be obtained. A step (1-1) of contacting the carbon material (A) with the organoaluminum compound (B); a step (1-2) of contacting the contact product obtained in the step (1-1) with the transition metal compound (C) to obtain a solid catalyst component (X); A step (2-1) of contacting the transition metal compound (C) with the organoaluminum compound (B); a step (2-2) of contacting the contact product obtained in the step (2-1) with the carbon material (A) to obtain a solid catalyst component (X); A step (3-1) of contacting the carbon material (A) with the organoaluminum compound (B); A step (3-2) of contacting the transition metal compound (C) with the organoaluminum compound (B); and a step (3-3) of contacting the contact product obtained in the step (3-1) with the contact product obtained in the step (3-2) to obtain a solid catalyst component (X). In this case, the organoaluminum compound (B) used in the step (3-1) and the step (3-2) may be the same or different.
[0072] In the steps (1-1) and (3-1), the organoaluminum compound (B) can be used in an amount of preferably 0.1 mmol or more and 500 mmol or less, more preferably 0.2 mmol or more and 200 mmol or less, and even more preferably 0.5 mmol or more and 100 mmol or less, per 1 g of the carbon material (A).
[0073] In the steps (2-1) and (3-2), the organoaluminum compound (B) can be used in an amount of preferably 0.1 mmol or more and 3000 mmol or less, more preferably 0.5 mmol or more and 1000 mmol or less, and even more preferably 1 mmol or more and 500 mmol or less, per 1 mmol of the transition metal compound (C).
[0074] In the steps (1-2), (2-2) and (3-3), the transition metal compound (C) can be used in an amount of preferably 0.1 μmol to 1000 μmol, more preferably 0.5 μmol to 500 μmol, and even more preferably 1 μmol to 200 μmol, per 1 g of the carbon material (A).
[0075] In the production of olefin polymers, the solid catalyst component (X) may be used in a state of being suspended in an inert hydrocarbon or in a dried state, or may be used after being prepolymerized with an olefin which may be the same as or different from the olefin used in the production of the olefin polymer.
[0076] [Production method of olefin polymer] The process for producing an olefin polymer of the present invention is characterized by comprising a step of polymerizing an olefin in the presence of the above-mentioned olefin polymerization catalyst of the present invention. In the present invention, the term "polymerization" may include copolymerization such as random copolymerization and block copolymerization in addition to homopolymerization.
[0077] The olefins to be polymerized in the present invention include ethylene, α-olefins, and cyclic olefins. Among these, the α-olefin may be a linear or branched α-olefin having 3 to 30 carbon atoms, preferably 3 to 20 carbon atoms. More specifically, propylene, 1-butene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3-methyl-1-pentene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene are preferred. Among these, propylene, 1-butene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, and 3-methyl-1-pentene are preferred, and propylene, 1-butene, 1-hexene, and 4-methyl-1-pentene are more preferred.
[0078] Examples of the cyclic olefin include cyclic olefins having 3 to 30 carbon atoms, and preferably 3 to 20 carbon atoms. More specific examples include cyclopentene, cycloheptene, norbornene, 5-methyl-2-norbornene, tetracyclododecene, and 2-methyl-1,4,5,8-dimethano-1,2,3,4,4a,5,8,8a-octahydronaphthalene.
[0079] The step of polymerizing an olefin is preferably a step of homopolymerizing ethylene or a step of copolymerizing ethylene and an α-olefin having 3 to 20 carbon atoms in the presence of the solid catalyst component (X).
[0080] In the method for producing an olefin polymer of the present invention, the polymerization can be carried out by either a liquid phase polymerization method such as suspension polymerization or a gas phase polymerization method. Examples of the inert hydrocarbon medium used in the liquid phase polymerization method include aliphatic hydrocarbons such as propane, butane, pentane, hexane, heptane, octane, decane, dodecane, and kerosene; alicyclic hydrocarbons such as cyclopentane, cyclohexane, and methylcyclopentane; aromatic hydrocarbons such as benzene, toluene, and xylene; halogenated hydrocarbons such as ethylene chloride, chlorobenzene, and dichloromethane, and mixtures thereof, and the olefin itself can also be used as the solvent.
[0081] In the method of the present invention, the lower limit of the temperature for polymerizing the olefin is -20°C, preferably 0°C, more preferably 20°C, and particularly preferably 30°C, and the upper limit of the temperature for polymerizing the olefin is 200°C, preferably 150°C, more preferably 100°C, and particularly preferably 80°C.
[0082] The polymerization pressure in the method of the present invention is usually from atmospheric pressure to 10 MPa, preferably from atmospheric pressure to 5 MPa, and the polymerization reaction can be carried out in any of a batch system, a semi-continuous system, and a continuous system.
[0083] In the process for producing an olefin polymer of the present invention, the polymerization can be carried out by any of a batch system, a semi-continuous system, and a continuous system. The process for producing an olefin polymer of the present invention may be a so-called multi-stage polymerization process in which the polymerization reaction is carried out in two or more stages under different polymerization reaction conditions.
[0084] The molecular weight of the resulting olefin polymer can be adjusted by making hydrogen present in the polymerization system or by changing the polymerization temperature. In the step of polymerizing the olefin, the component (G) can be present in order to suppress adhesion (fouling) to a polymerization reactor or to improve particle properties.
[0085] <Olefin polymer> One embodiment of the olefin polymer obtained by the method for producing an olefin polymer of the present invention is an ethylene-based polymer containing ethylene-derived structural units in a range of preferably 90 mol% to 100 mol%, more preferably 95 mol% to 100 mol%. The ethylene-based polymer contains α-olefin-derived structural units having 3 to 20 carbon atoms in a total amount of preferably 0 mol% to 10 mol%, more preferably 0 mol% to 5 mol%, where the sum of the content of ethylene-derived structural units and the content of α-olefin-derived structural units having 3 to 20 carbon atoms is taken as 100 mol%.
[0086] Among these polymers, ethylene homopolymer, ethylene / propylene copolymer, ethylene / 1-butene copolymer, ethylene / propylene / 1-butene copolymer, ethylene / 1-octene polymer, ethylene / 1-hexene polymer, ethylene / 4-methyl-1-pentene polymer, ethylene / propylene / 1-octene polymer, ethylene / propylene / 1-hexene polymer, and ethylene / propylene / 4-methyl-1-pentene polymer are preferred. Also, so-called block copolymers (impact copolymers) obtained by mixing or continuously producing two or more types selected from these polymers may be used.
[0087] The olefin polymer obtained by the method for producing an olefin polymer contains the carbon material (A) in an amount of preferably 0.01% by weight to 25% by weight, more preferably 0.02% by weight to 10% by weight. The carbon material (A) is efficiently dispersed in the olefin polymer, and is expected to have high thermal conductivity, electrical conductivity, and weather resistance. EXAMPLES
[0088] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0089] [Carbon materials] The following carbon materials (A-1) to (A-4) and (A'-5) were used as the carbon materials. Each of the carbon materials was dried under reduced pressure at 100°C for 3 hours before use, and then cooled to room temperature under a nitrogen atmosphere before being used in the preparation of the solid catalyst component (X).
[0090] Carbon materials (A-1) to (A-4): Carbon materials obtained in the following Preparation Examples 1A to 4A Carbon material (A'-5): Graphene powder (1-5 layers thick x 0.5-5 microns wide, surface area 650-750m) purchased from STREM. 2 / g:Product code 06-0318)
[0091] <Preparation Example 1A> As a raw material compound, pyridine (Kanto Chemical Co., Ltd., special grade pyridine) was prepared and used as raw material compound-containing liquid 1-1.
[0092] Next, plasma was generated in the raw compound-containing liquid using the following device. FIG. 1 is a schematic diagram of a solution plasma generating device 10 for generating plasma in liquid. In this embodiment, the raw compound-containing liquid 1-1 prepared above is placed in a container 5 made of a glass beaker, and is stirred by a stirring device 7 made of a magnetic stirrer. A pair of electrodes 6 for generating plasma are disposed in the raw compound-containing liquid 1-1 at a predetermined interval and are held in the container 5 via an insulating member 9. In this embodiment, a needle-shaped electrode 6 capable of locally concentrating an electric field is used. The electrode 6 is made of a tungsten wire (manufactured by Nilaco Corporation) having a diameter of 1.0 mm, and the distance between the electrodes is set to 1.0 mm. In addition, only the tip (for example, about several mm) is exposed in order to suppress excess current that hinders the concentration of the electric field, and the remaining part is insulated by an insulating member 9 made of fluororesin. In this embodiment, the insulating member 9 is configured to fix the electrode 6 to the container 5 and also to serve as a stopper for keeping the electrode 6 and the container 5 watertight. The electrode 6 is connected to an external power source 8, and a pulse voltage of predetermined conditions is applied from this external power source 8. As the external power source 8, a bipolar pulse power source (MPP-HV04, power source for generating pulsed plasma in liquid, manufactured by Kurita Manufacturing Co., Ltd.) was used.
[0093] In this embodiment, the application conditions of the pulse voltage for generating solution plasma were secondary voltage: 1500 V, pulse width: 1.0 μs, and repetition frequency: 50 kHz, and under these conditions, solution plasma was generated in the raw material compound-containing liquid 1-1 for 15 minutes. The raw material compound-containing solution 1-1 was colorless and transparent, but immediately after the generation of the solution plasma, it turned yellowish, turned brown after about 5 minutes, and turned black and opaque after about 10 minutes.
[0094] After the solution plasma treatment, suction filtration was performed using a membrane filter (Merck Millipore, Omnipore(TM) membrane, maximum pore size 2.0 μm), and the obtained black powder was dried overnight in an oven at 80° C. to obtain 0.20 g of black powder. This powder was pulverized in a mortar to obtain a carbon material (A-1).
[0095] <Preparation example 2A> A solution plasma was generated in the same manner as in Preparation Example 1A, except that the application conditions of the pulse voltage were changed to secondary voltage: 1500 V, pulse width: 1.0 μs, and repetition frequency: 25 kHz.
[0096] After the solution plasma treatment, suction filtration was performed using a membrane filter (Merck Millipore, Omnipore(TM) membrane, maximum pore size 1.0 μm), and the obtained black powder was dried overnight in an oven at 80° C. to obtain 0.20 g of black powder. This powder was pulverized in a mortar to obtain a carbon material (A-2).
[0097] <Preparation example 3A> As raw material compounds, EMIM-DCA (1-Ethyl-3-methyl imidazolium dicyanamide ≧98.0% (metals basis) manufactured by ALDRICH) and aniline (special grade aniline manufactured by Kanto Chemical Co., Ltd.) were prepared, and these were mixed and stirred in a ratio of 5 mL of EMIM-DCA + 95 mL of aniline to be used as raw material compound-containing liquid 1-2. Except for this, solution plasma was generated in the same manner as in Preparation Example 1A. The raw material compound-containing solution 1-2 was transparent and light orange in color, but changed color to brown about 5 minutes after the generation of the solution plasma, and turned opaque and black about 10 minutes later.
[0098] After the solution plasma treatment, suction filtration was performed using a membrane filter (Merck Millipore, Omnipore(TM) membrane, maximum pore size 2.0 μm), and the obtained black powder was dried overnight in an oven at 80° C. to obtain 0.02 g of black powder. This powder was pulverized in a mortar to obtain a carbon material (A-3).
[0099] <Preparation example 4A> As raw material compounds, EMIM-DCA (1-Ethyl-3-methyl imidazolium dicyanamide ≧98.0% (metals basis) manufactured by ALDRICH) and aniline (special grade aniline manufactured by Kanto Chemical Co., Ltd.) were prepared, and these were mixed and stirred in a ratio of 10 mL EMIM-DCA + 90 mL aniline to be used as raw material compound-containing solution 1-3. Solution plasma was generated in the same manner as in Preparation Example 1A, except that the application conditions of the pulse voltage were changed to secondary voltage: 1500 V, pulse width: 1.5 μs, and repetition frequency: 30 kHz.
[0100] After the solution plasma treatment, suction filtration was performed using a membrane filter (Merck Millipore, Omnipore(TM) membrane, maximum pore size 1.0 μm), and the obtained black powder was dried overnight in an oven at 80° C. to obtain 0.02 g of black powder. This powder was pulverized in a mortar to obtain a carbon material (A-4).
[0101] ≪Nitrogen content≫ The nitrogen contents of the carbon materials (A-1) to (A-4) and (A'-5) were determined by X-ray photoelectron spectroscopy (XPS) (VersaProbe II, manufactured by ULVAC-PHI, Inc.). Narrow scan analysis was performed under the following analytical conditions, and the nitrogen atom concentration was determined from the peak intensity of the N1s narrow spectrum, and the carbon atom concentration was determined from the peak intensity of the C1s narrow spectrum, and the molar ratio of nitrogen atoms to carbon atoms was calculated. The results are shown in Table 1. (Analysis conditions) X-ray source: Mg-Kα radiation X-ray generation current: 1.7mA X-ray generation voltage: 25 kV
[0102] [Organoaluminum compounds] The organoaluminum compound used was the following organoaluminum compound (B-1). The organoaluminum compound (B-1) was used after diluting to 1.0 mol / L in decane solution. ·Organoaluminum compound (B-1): Tosoh Finechem Corporation, triisobutylaluminum (TIBAL)
[0103] [Transition metal compounds] As the transition metal compound, transition metal compounds (C-1) and (C'-2) represented by the following formulae (C-1) and (C'-2) were produced by a known method and used. [ka]
[0104] <Identification of transition metal compound (C)> The structure of the transition metal compound is 270MHz 1 The determination was made by measurement using a H-NMR (GSH-270 manufactured by JEOL Ltd.) according to a conventional method.
[0105] [Preparation of solid catalyst component (X)] <Preparation example 1X> In a Schlenk flask with a volume of 30 mL and thoroughly purged with nitrogen, 100 mg of carbon material (A-1) and 5 mL of toluene were added, and stirring was started using a rotor. 0.25 mL of a decane solution of organoaluminum compound (B-1) (0.25 mmol in terms of organoaluminum compound (B-1)) was added to this suspension, and stirring was continued at room temperature for 30 minutes. After that, 3.0 μmol of transition metal compound (C-1) was added as a toluene solution, and stirring was continued for another 30 minutes at room temperature to prepare a slurry of solid catalyst component (X-1) with a solid concentration of carbon material (A-1) of 10.0 g / L.
[0106] <Preparation example 2X~5X> Slurries of solid catalyst components (X-2) to (X-5) were prepared in the same manner as in Preparation Example 1X, except that carbon materials (A-2) to (A-4) and (A'-5) were used instead of the carbon material (A-1).
[0107] <Preparation example 6X> In a Schlenk flask with a volume of 30 mL and thoroughly purged with nitrogen, 100 mg of carbon material (A'-5), 30 μL of pyridine (Fujifilm Wako Pure Chemical Industries, pyridine (dehydrated) for organic synthesis), and 5 mL of toluene were added, and stirring was started using a rotor. 0.25 mL of a decane solution of organoaluminum compound (B-1) (0.25 mmol in terms of organoaluminum compound (B-1)) was added to this suspension, and stirring was continued at room temperature for 30 minutes. After that, 3.0 μmol of transition metal compound (C-1) was added as a toluene solution, and stirring was continued for another 30 minutes at room temperature to prepare a slurry of solid catalyst component (X-6) with a solid concentration of carbon material (A) of 10.0 g / L.
[0108] <Preparation Example 7X> Preparation example except that no organoaluminum compound (B-1) was used. 3 A slurry of a solid catalyst component (X-7) was prepared in the same manner as in X.
[0109] <Preparation example 8X> Preparation example except that transition metal compound (C'-2) was used instead of transition metal compound (C-1). 3 A slurry of a solid catalyst component (X-8) was prepared in the same manner as in X.
[0110] [Production of olefin polymers] <Example 1> In a nitrogen atmosphere, 500 milliliters of heptane was added to a SUS autoclave reactor with a capacity of 1 liter, which had been thoroughly substituted with nitrogen, and ethylene was then passed through to saturate the reactor with ethylene. Next, 0.375 mL of a decane solution of the organoaluminum compound (B-1) (0.375 mmol in terms of the organoaluminum compound (B-1)) and an amount of slurry equivalent to the amount shown in Table 1 as the solid content of the carbon material (A-1) were extracted from the slurry of the solid catalyst component (X-1) obtained in Preparation Example 1 and charged into the reactor. Then, the temperature and pressure were raised to 80°C and 0.8 MPaG with ethylene, and a polymerization reaction was carried out for 60 minutes at a rotation speed of 350 rpm. After the reaction was completed, the contents in the reactor were filtered and dried under reduced pressure at 80°C for 10 hours to obtain the amount of olefin polymer shown in Table 1.
[0111] <Examples 2 to 4> Polymerization reaction was carried out in the same manner as in Example 1, except that the slurries of the solid catalyst components (X-2) to (X-4) obtained in Preparation Examples 2X to 4X were used instead of the solid catalyst component (X-1), and the amounts shown in Table 1 were charged into the reactor as the solid content of the carbon material. After the reaction was completed, the contents in the reactor were filtered and dried under reduced pressure at 80°C for 10 hours, to obtain the amount of olefin polymer shown in Table 1.
[0112] <Comparative Examples 1 to 2> Polymerization reaction was carried out in the same manner as in Example 1, except that the slurries of the solid catalyst components (X-5) and (X-6) obtained in Preparation Examples 5X and 6X were used instead of the solid catalyst component (X-1), and the amounts shown in Table 1 were charged into the reactor as the solid content of the carbon material. After the reaction was completed, the contents in the reactor were filtered and dried under reduced pressure at 80°C for 10 hours, to obtain the amount of olefin polymer shown in Table 1.
[0113] <Comparative Example 3> A polymerization reaction was carried out in the same manner as in Example 1, except that no organoaluminum compound (B-1) was used, and the slurry of the solid catalyst component (X-7) obtained in Preparation Example 7X was used instead of the solid catalyst component (X-1), and the amount of the solid carbon material listed in Table 1 was charged into the reactor. After the reaction was completed, the contents in the reactor were filtered and dried under reduced pressure at 80°C for 10 hours, to obtain the amount of olefin polymer shown in Table 1.
[0114] <Comparative Example 4> A polymerization reaction was carried out in the same manner as in Example 1, except that the slurry of the solid catalyst component (X-8) obtained in Preparation Example 8X was used instead of the solid catalyst component (X-1), and the amount of the solid carbon material listed in Table 1 was charged into the reactor. After the reaction was completed, the contents in the reactor were filtered and dried under reduced pressure at 80°C for 10 hours, to obtain the amount of olefin polymer shown in Table 1.
[0115] [Table 1]
[0116] It can be seen that the carbon material (A) constituting the olefin polymerization catalyst of the Example has a high nitrogen content, and can obtain a larger amount of olefin polymer than the Comparative Example using a carbon material with a low nitrogen content. In addition, even if a nitrogen atom-containing compound not introduced into the graphene structure was separately added to the carbon material with a low nitrogen content, the polymer yield did not increase.
[0117] It is also seen that the examples using the organoaluminum compound (B) give a larger amount of olefin polymer than the comparative examples not using the organoaluminum compound (B). Furthermore, it is also seen that the examples using the transition metal compound (C-1) having a hetero atom as the transition metal compound give a larger amount of olefin polymer than the comparative examples using the transition metal compound (C'-2) not having a hetero atom. [Explanation of symbols]
[0118] 2 liquid (liquid phase) 4. Solution Plasma (Plasma Phase) 5 containers 6 electrodes 7 Mixing device 8 External power supply 9. Insulating materials 10 Solution plasma generator
Claims
1. A carbon material (A) that satisfies the following requirements (AI) and (A-II); An organoaluminum compound (B) represented by the following general formula (BI), A transition metal compound (C) represented by the following general formula (C-II): A catalyst for olefin polymerization comprising: (A-I) The nitrogen atom / carbon atom molar ratio measured by X-ray photoelectron spectroscopy (XPS) is 0.003 or more and 0.300 or less; (A-II) A nitrogen-doped carbon material having a graphene structure in which nitrogen atoms are substituted or introduced; R a m Al(OR b ) n H p X q ・・・(B-I) [In general formula (BI), R a and R b represents a hydrocarbon group having 1 to 15 carbon atoms, which may be the same or different from each other, X represents a halogen atom, m represents an integer of 1 to 3, n represents an integer of 0 to 2, p represents an integer of 0 to 2, q represents an integer of 0 to 2, and m+n+p+q=3. 【Chemistry 1】 [In general formula (C-II), M represents a transition metal atom of Group 4 or 5 of the periodic table, R 1 , R 2 , R 3 , R 4 , and R 5 may be the same or different and represent a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, a germanium-containing group, or a tin-containing group, two or more of which may be bonded to each other to form a ring; R 6 represents a hydrogen atom, a hydrocarbon group having from 1 to 3 carbon atoms and consisting only of primary or secondary carbon, an alkyl group having 4 or more carbon atoms, an aryl group-substituted alkyl group, a monocyclic or bicyclic cyclic hydrocarbon group, an aryl group, or a halogen atom; n is an integer of 1 to 4 that satisfies the valence of M; X is a leaving group selected from the group consisting of a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, a conjugated diene derivative group, and a neutral ligand capable of coordinating with a lone electron pair, and when n is 2 or more, multiple Xs may be the same or different from each other and may be bonded to each other to form a ring.
2. 2. The olefin polymerization catalyst according to claim 1, wherein M in the general formula (C-II) is a transition metal atom of Group 4 of the periodic table.
3. 3. The olefin polymerization catalyst according to claim 1, wherein the nitrogen atom / carbon atom molar ratio in the requirement (AI) is 0.005 or more and 0.100 or less.
4. A process for producing an olefin polymer, comprising a step of polymerizing an olefin in the presence of the olefin polymerization catalyst according to any one of claims 1 to 3.
5. The method for producing an olefin polymer according to claim 4, wherein the step of polymerizing an olefin is a step of homopolymerizing ethylene or a step of copolymerizing ethylene with a linear or branched α-olefin having 3 to 30 carbon atoms.
Citation Information
Patent Citations
Method for producing ultra-high-molecular-weight olefin-based polymer for high-tenacity fiber and ultra-high-molecular-weight olefin fiber
JP2005029775A
Metal complex composition and use of metal complex composition as catalyst for polydiene production
JP2005506404A
Polymerization catalyst, polymer obtained by using the same, and its polymer complex
JP2006176601A
Carbon nanotube-polyolefin composite
JP2007161741A
Method for producing carbon nanotube / polymer mixtures by gas-phase polymerization
JP2009545639A