Polypropylene resin composition and injection molded article
A polypropylene resin composition with specific molecular and compositional requirements, combined with an α-crystal nucleating agent, achieves a balanced performance in gloss, rigidity, and impact resistance, addressing the limitations of existing polypropylene compositions and enhancing injection molded article properties.
Patent Information
- Application Number
- JP2021046354
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-03-19
AI Technical Summary
Existing polypropylene resin compositions fail to achieve a balanced combination of gloss, rigidity, and impact resistance, which are key properties that amorphous ABS resin possesses, leading to inferior performance in applications requiring these characteristics.
A polypropylene resin composition comprising 75 to 95 parts by mass of a polypropylene resin (A) and 5 to 25 parts by mass of high-density polyethylene (B), along with an α-crystal nucleating agent (C), where the polypropylene resin (A) meets specific molecular and compositional requirements, including melt flow rate, insoluble and soluble fractions, molecular weight ratios, and ethylene content, and the nucleating agent promotes α-crystal formation.
The composition results in an injection molded article with an excellent balance of gloss, rigidity, and impact resistance, enabling faster crystallization and improved molding properties, suitable for various applications including automobile and home appliance parts.
Smart Images

Figure 0007579728000001 
Figure 0007579728000002 
Figure 0007579728000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polypropylene resin composition and an injection molded article made thereof. [Background technology]
[0002] ABS resin is widely used for housing equipment components and housing materials for home appliances because it has an excellent balance between rigidity and impact resistance and is highly glossy. However, ABS resin is not only expensive to manufacture, but also has poor chemical resistance because it is an amorphous resin, and home appliances such as vanities and refrigerators made of ABS resin have been prone to cracking when exposed to oil or other substances.
[0003] In recent years, therefore, there have been studies on replacing ABS resin with crystalline polypropylene resin, which is a material that has excellent chemical resistance and is inexpensive. For example, Patent Document 1 proposes a polypropylene resin composition that has an excellent balance of high rigidity, high impact resistance, and high gloss, and is obtained by blending a modifier containing an ethylene-α-olefin copolymer with a propylene-based polymer.
[0004] Patent Document 2 proposes a polypropylene resin composition that has high gloss while ensuring sufficient impact resistance and rigidity, and contains a mixture of a propylene polymer and an ethylene-1-butene copolymer, and a nucleating agent.
[0005] Patent Documents 3 and 4 propose polypropylene compositions made of a propylene (co)polymer and an ethylene-propylene copolymer, which have a good balance between rigidity and cold impact resistance, as well as high flowability and high gloss. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 10-158440 [Patent Document 2] JP 2016-89176 A [Patent Document 3] JP 2019-218459 A [Patent Document 4] JP 2020-063386 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, although the invention of Patent Document 1 is excellent in impact resistance and gloss, it has a poor balance between rigidity and impact resistance, resulting in a problem of low rigidity. The invention disclosed in Patent Document 2 is excellent in rigidity and especially in gloss, but has a poor balance between rigidity and impact resistance, resulting in a problem of low impact resistance.
[0008] The inventions disclosed in Patent Documents 3 and 4 are excellent in impact resistance and gloss, but have a poor balance between rigidity and impact resistance, and as a result, have a problem in that the rigidity is not yet sufficiently high. As described above, the polypropylene resin composition having excellent gloss has an essential problem that it is inferior in balance between rigidity and impact resistance compared to ABS resin, and this problem remains unsolved.
[0009] In view of the above circumstances, an object of the present invention is to provide a polypropylene resin composition capable of forming a molded article, particularly an injection molded article, having a good balance of gloss, rigidity and impact resistance. [Means for solving the problem]
[0010] The present inventors have conducted extensive research to solve the above problems. As a result, they have found that the above problems can be solved by a polypropylene resin composition that satisfies the following requirements, and have completed the present invention. Examples of aspects of the present invention are shown below.
[0011] [1] A polypropylene resin composition comprising 75 to 95 parts by mass of a polypropylene resin (A) satisfying the following (A-1) to (A-6), 5 to 25 parts by mass of a high-density polyethylene (B) satisfying the following (B-1) to (B-2) (wherein the total amount of the polypropylene resin (A) and the high-density polyethylene (B) is 100 parts by mass), and 0.05 to 1.0 part by mass of an α-crystal nucleating agent (C). (A-1) Melt flow rate (230℃, 2.16kg load) is 2-100g / 10min. (A-2) It is composed of 85 to 97% by mass of a component insoluble in n-decane at room temperature and 3 to 15% by mass of a component soluble in n-decane at room temperature (the total amount of both is 100% by mass). (A-3) The mesopentad fraction (mmmm fraction) of the component insoluble in n-decane at room temperature is 94.0% or more. (A-4) The component insoluble in n-decane at room temperature has an Mw / Mn ratio of 8.0 to 15.0 and an Mz / Mw ratio of 7.0 to 12.0. (A-5) The intrinsic viscosity [η] of the component soluble in n-decane at room temperature is 1.5 to 5.0 dL / g. (A-6) The ethylene content of the component soluble in n-decane at room temperature is 35 to 46% by mass. (B-1) Melt flow rate (190℃, 2.16kg load) is 20-80g / 10min. (B-2) Density is 955kg / m 3 More than this
[0012] [2] The polypropylene resin composition according to [1], wherein the α crystal nucleating agent (C) is a phosphate metal salt-based nucleating agent.
[0013] [3] An injection molded article of the polypropylene resin composition according to [1] or [2] above. Effect of the Invention
[0014] The propylene polymer composition according to the present invention can be used to form a molded article, particularly an injection molded article, having an excellent balance of physical properties such as gloss, rigidity and impact resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The polypropylene resin composition according to the present invention and the injection molded article made thereof will be specifically described below. [Polypropylene resin composition] The polypropylene resin composition according to the present invention is characterized by comprising 75 to 95 parts by mass of a polypropylene resin (A) satisfying the requirements (A-1) to (A-6) described below, 5 to 25 parts by mass of a high-density polyethylene (B) satisfying the requirements (B-1) and (B-2) described below (wherein the total amount of the polypropylene resin (A) and the high-density polyethylene (B) is 100 parts by mass), and 0.05 to 1.0 part by mass of an α-crystal nucleating agent (C).
[0016] [Polypropylene resin (A)] The polypropylene resin composition according to the present invention contains a polypropylene resin (A) that satisfies the requirements (A-1) to (A-6) described below. The polypropylene resin (A) is a propylene-based block copolymer that contains a component mainly consisting of structural units derived from propylene and a component mainly consisting of structural units derived from propylene and ethylene.
[0017] [Requirement (A-1)] The requirement (A-1) is that the melt flow rate (hereinafter also referred to as "MFR") of the polypropylene resin (A) (ASTM D1238, 230°C, 2.16 kg load) is 2 to 100 g / 10 min. The MFR is preferably 5 to 80 g / 10 min, more preferably 10 to 60 g / 10 min, and even more preferably 10 to 40 g / 10 min.
[0018] If the MFR is less than 2 g / 10 min, the flowability of the polypropylene resin composition is low, making large-scale injection molding difficult and causing flow marks in the injection-molded article, whereas if the MFR is more than 100 g / 10 min, the impact resistance of the injection-molded article may decrease.
[0019] [Requirement (A-2)] Requirement (A-2) is that the polypropylene resin (A) is composed of 85 to 97 mass% of a component insoluble in n-decane at room temperature (i.e., 25°C; the same applies below) (hereinafter also referred to as "CDIS") and 3 to 15 mass% of a component soluble in n-decane at room temperature (hereinafter also referred to as "CDS") (wherein the total amount of CDIS and CDS is 100 mass%). The proportion of the CDIS is preferably 90 to 95 mass%, and the proportion of the CDS is preferably 5 to 10 mass%.
[0020] If the amount of the CDIS exceeds 97% by mass (i.e., if the amount of the CDS is less than 3% by mass), the impact resistance of the injection-molded article may decrease. If the amount of the CDIS is less than 85% by mass (i.e., if the amount of the CDS is more than 15% by mass), the rigidity of the injection-molded article may decrease.
[0021] [Requirement (A-3)] Requirement (A-3) is that the polypropylene resin (A) has a CDIS mesopentad fraction (hereinafter also referred to as "mmmm fraction") of 94.0% or more, measured under the conditions employed in the examples described below or under conditions equivalent thereto. The mmmm fraction is preferably 95.0% or more. The upper limit of the mmmm fraction may be, for example, 99.8%. If the mmmm fraction is less than 94.0%, the rigidity of the injection-molded article may decrease.
[0022] The mesopentad fraction (mmmm fraction) indicates the proportion of pentad isotactic structures in a molecular chain, and is the fraction of propylene structural units at the center of a chain in which five consecutive propylene monomer units have a meso structure. A propylene homopolymer that satisfies such requirements can be obtained, for example, by polymerizing propylene with an olefin polymerization catalyst that contains a known solid titanium catalyst component and an organometallic compound catalyst component, as described below, and an electron donor that is used as necessary.
[0023] [Requirement (A-4)] The requirement (A-4) is that the polypropylene resin (A) has a CDIS Mw (weight average molecular weight) / Mn (number average molecular weight) of 8.0 to 15.0 and Mz (z average molecular weight) / Mw (weight average molecular weight) of 7.0 to 12.0, as measured under the conditions employed in the examples described below or under conditions equivalent thereto. The Mw / Mn is preferably 9.0 to 13.0, and the Mz / Mw is preferably 8.0 to 10.0. If the Mw / Mn is less than 8.0, the rigidity of the injection molded article may decrease, and if it exceeds 15.0, the impact resistance of the injection molded article may decrease. If the Mz / Mw is less than 7.0, the rigidity of the injection molded article may decrease, and if it exceeds 12.0, the impact resistance of the injection molded article may decrease.
[0024] [Requirements (A-5)] The requirement (A-5) is that the CDS of the polypropylene resin (A) has an intrinsic viscosity [η] of 1.5 to 5.0 dL / g, as measured under the conditions employed in the examples described below or under conditions equivalent thereto. The intrinsic viscosity [η] is preferably 2.0 to 4.0 dL / g. If the [η] is less than 1.5 dL / g, the impact strength of the injection molded article may decrease, whereas if it exceeds 5.0 dL / g, the gloss of the injection molded article may decrease.
[0025] [Requirement (A-6)] The requirement (A-6) is that the ethylene content of the CDS in the polypropylene resin (A) (i.e., the proportion of structural units derived from ethylene in the total structural units of the CDS) is 35 to 46 mass%. The ethylene content is preferably 36 to 45 mass%, and more preferably 38 to 44 mass%.
[0026] If the ethylene content is less than 35% by mass, the impact resistance of the injection-molded article may decrease, and if the ethylene content exceeds 46% by mass, not only the impact resistance of the injection-molded article may decrease, but also the gloss may decrease.
[0027] (Production method of polypropylene resin (A)) The polypropylene resin (A) is obtained by copolymerizing propylene and ethylene in the presence of a metallocene catalyst or a Ziegler-Natta catalyst. In addition, a monomer other than propylene and ethylene may be further copolymerized within a range that does not impair the effects of the present invention.
[0028] The polymerization may be carried out by any of gas phase polymerization, bulk polymerization, and slurry polymerization. These polymerization methods are preferably carried out by a multi-stage polymerization method, and may be carried out by a multi-stage method using an apparatus in which a plurality of polymerization reaction vessels are connected in series, or each stage may be carried out by a different polymerization method. From an industrial and economical point of view, a continuous gas phase polymerization method or a bulk-gas phase polymerization method in which a bulk polymerization method and a gas phase polymerization method are carried out continuously is preferred. For example, it can be obtained by producing a propylene homopolymer component by a bulk polymerization method in a first polymerization step, and producing a propylene-ethylene copolymer component by a gas phase method in a second polymerization step.
[0029] Examples of catalysts used in the polymerization include Ziegler-Natta catalysts and metallocene catalysts. The use of such catalysts makes it possible to obtain a polypropylene resin (A) having a broad molecular weight distribution, and therefore Ziegler-Natta catalysts are preferred.
[0030] When a Ziegler-Natta catalyst is used, it is preferable to carry out the polymerization in the presence of an olefin polymerization catalyst comprising a solid titanium catalyst component (I), an organometallic compound (II) containing a metal atom selected from the group consisting of Groups 1, 2 and 13 of the periodic table, and, if necessary, an electron donor (III).
[0031] The olefin polymerization catalyst may form a prepolymerization catalyst, which is formed by polymerizing an olefin, for example, an α-olefin having 2 to 8 carbon atoms such as propylene, in the presence of an olefin polymerization catalyst containing a solid titanium catalyst component (I), an organometallic compound (II) containing a metal atom selected from the group consisting of Groups 1, 2, and 13 of the periodic table, and, if necessary, an electron donor (III).
[0032] Various conditions in the polymerization step (polymerization temperature, polymerization pressure, monomer concentration, catalyst input amount, polymerization time, etc. in each step (in the case of adopting a multistage polymerization method, each polymerization step in each stage)) may be appropriately determined depending on the target polypropylene resin (A). The fraction of each component (for example, the fraction of each of the propylene homopolymer component and the propylene-ethylene copolymer component produced by the multistage polymerization method) may be adjusted by the polymerization time of each stage.
[0033] Furthermore, a composition prepared by blending a propylene-based block copolymer with another propylene homopolymer or propylene-based block copolymer also falls within the scope of the polypropylene resin (A) of the present invention.
[0034] Next, the method for adjusting each of the physical properties in the requirements (A-1) to (A-6) will be described taking as an example the case where the polypropylene resin (A) is produced by a multistage polymerization method, unless otherwise specified. The physical properties in the requirements (A-1) to (A-3) and (A-5) to (A-6) can be achieved by appropriately selecting a known catalyst when producing the polypropylene resin (A) and adjusting conditions such as the hydrogen concentration, polymerization temperature, and polymerization time in the polymerization of the propylene homopolymer component in the first stage and adjusting the ethylene concentration, hydrogen concentration, polymerization temperature, and polymerization time in the polymerization of the propylene-ethylene copolymer component in the second stage.
[0035] Specifically, regarding the MFR in requirement (A-1), the MFR can be increased by increasing the proportion of the amount of hydrogen gas supplied as a chain transfer agent in the previous polymerization stage, and the MFR can be decreased by decreasing this proportion.
[0036] The amounts of CDIS and CDS in the requirement (A-2) can be adjusted by controlling the polymerization times in the first and second stages.
[0037] The mmmm fraction of CDIS in requirement (A-3) can be adjusted by using various known catalysts, for example, a catalyst comprising (a) a solid titanium catalyst component containing magnesium, titanium, a halogen, and an electron donor, (b) an organometallic compound catalyst component containing a metal atom selected from the group consisting of Groups 1, 2, and 13 of the periodic table, and (c) an organosilicon compound catalyst component (electron donor) having at least one group selected from the group consisting of a cyclopentyl group, a cyclopentenyl group, a cyclopentadienyl group, and derivatives thereof, and this catalyst can be produced by a known method, for example, the method described in paragraphs
[0078] to
[0094] of WO 2010 / 74001.
[0038] The Mw / Mn and Mz / Mw of the CDIS in the requirement (A-4) can be adjusted, for example, by the following method (i), (ii), or (iii). Method (i): In the first polymerization step, a high molecular weight propylene homopolymer is produced by a bulk polymerization method under conditions such as no hydrogen supply or a low hydrogen concentration, in the second polymerization step, a low molecular weight propylene homopolymer is produced by a bulk polymerization method under conditions such as a high hydrogen concentration, and in the third polymerization step, a propylene-ethylene copolymer component is produced by a gas phase polymerization method.
[0039] Method (ii): A propylene homopolymer composition is produced by the first and second polymerization stages of method (i) above, and the propylene homopolymer composition is melt-kneaded with another propylene-ethylene block copolymer.
[0040] Method (iii): Produced by melt-blending high molecular weight propylene homopolymer polymerized under low hydrogen concentration conditions with other propylene-ethylene block copolymers. Among these methods, methods (i) and (ii) are preferred since they do not cause fisheyes in the injection molded article.
[0041] The intrinsic viscosity [η] of CDS in the requirement (A-5) can be adjusted by the ratio of the amount of hydrogen gas supplied as a chain transfer agent in the polymerization stage of the propylene-ethylene copolymer component.
[0042] The ethylene content of the CDS in the requirement (A-6) can be adjusted by the ratio of the amount of ethylene fed in the polymerization stage of the propylene-ethylene copolymer component.
[0043] The content of the polypropylene resin (A) in the polypropylene resin composition of the present invention is 75 to 95 parts by mass, preferably 78 to 92 parts by mass, and more preferably 80 to 90 parts by mass, per 100 parts by mass of the total of the polypropylene resin (A) and the high-density polyethylene (B). If the content of polypropylene resin (A) is less than 75 parts by mass, the rigidity of the injection-molded article may decrease, whereas if it exceeds 95 parts by mass, the impact resistance of the injection-molded article may decrease.
[0044] [High density polyethylene (B)] The polypropylene resin composition of the present invention contains a high-density polyethylene (B) that satisfies the requirements (B-1) and (B-2) described below.
[0045] [Requirements (B-1)] The requirement (B-1) is that the MFR of the high-density polyethylene (B), measured at 190° C. under a load of 2.16 kg, is 20 to 80 g / 10 min. The MFR is preferably 20 to 60 g / 10 min. If the MFR of the high-density polyethylene (B) is less than 20 g / 10 min, the gloss of the injection-molded article may decrease, whereas if it exceeds 80 g / 10 min, the impact resistance of the injection-molded article may decrease.
[0046] [Requirements (B-2)] Requirement (B-2) is that the density of high-density polyethylene (B) is 955 kg / m 3 The density is preferably 960 kg / m or more. 3 The density of the high-density polyethylene (B) is 955 kg / m 3 If it is less than this, the rigidity of the injection molded article may decrease.
[0047] (Production method of high density polyethylene (B)) The high density polyethylene (B) can be produced by a conventional method. That is, it is obtained by polymerizing mainly ethylene using various known catalysts such as Ziegler catalyst, Phillips catalyst, metallocene catalyst, etc. In general, Ziegler catalysts consisting of a transition metal compound such as titanium and a magnesium compound, Phillips catalysts such as chromium oxide catalysts, and metallocene catalysts having at least one cyclopentadienyl group or substituted cyclopentadienyl group in a transition metal compound such as zirconium are used.
[0048] In the polymerization, ethylene is polymerized alone, or ethylene is copolymerized with one or more comonomers selected from α-olefins having 3 to 18 carbon atoms to a predetermined density. Representative examples of α-olefins to be copolymerized include propylene, 1-butene, and 1-hexene.
[0049] The MFR in requirement (B-1) can be adjusted by adjusting the ratio of the amount of hydrogen gas supplied as a chain transfer agent to the amount of monomer (i.e., ethylene in the case of ethylene homopolymerization, or ethylene and α-olefin in the case of copolymerization) supplied when producing high-density polyethylene (B) by polymerizing ethylene (or copolymerizing ethylene and α-olefin). That is, by increasing this ratio, the MFR can be increased, and by decreasing this ratio, the MFR can be decreased.
[0050] The density in requirement (B-2) can be adjusted by adjusting the ratio of the amount of α-olefin fed to the amount of ethylene fed when ethylene is polymerized (or ethylene and α-olefin are copolymerized) to produce the high-density polyethylene (B). That is, by increasing this ratio, the density can be lowered, and by decreasing this ratio, the density can be increased. Examples of commercially available products of such high density polyethylene (B) include Hi-Zex (registered trademark) 1810J and 1820J manufactured by Prime Polymer Co., Ltd.
[0051] The content of the high-density polyethylene (B) in the polypropylene resin composition of the present invention is 5 to 25 parts by mass, preferably 8 to 22 parts by mass, and more preferably 10 to 20 parts by mass, per 100 parts by mass of the total of the polypropylene resin (A) and the high-density polyethylene (B). If the content of the high density polyethylene (B) is less than 5 parts by mass, the gloss of the injection molded article may decrease, whereas if it exceeds 25 parts by mass, the rigidity of the injection molded article may decrease.
[0052] [α-crystal nucleating agent (C)] The polypropylene resin composition of the present invention contains an α-crystal nucleating agent (C). The α-crystal nucleating agent (C) is a nucleating agent that promotes the growth of α-crystals of polypropylene, and examples of such nucleating agents include metal phosphate nucleating agents, sorbitol nucleating agents, metal carboxylate nucleating agents, rosin nucleating agents, and fine talc. Here, the fine talc refers to talc having an average particle size (D50 value as determined by a laser diffraction / scattering method) of about 0.1 to 10 μm.
[0053] Among these, from the viewpoint of improving the rigidity of the injection molded article, the phosphate metal salt-based nucleating agent is particularly preferable. Examples of the phosphate metal salt-based nucleating agent include sodium bis(4-t-butylphenyl)phosphate, lithium bis(4-t-butylphenyl)phosphate, aluminum bis(4-t-butylphenyl)phosphate, sodium 2,2'-methylene-bis(4,6-di-t-butylphenyl)phosphate, lithium 2,2'-methylene-bis(4,6-di-t-butylphenyl)phosphate, and aluminum bis(4-t-butylphenyl)phosphate. Examples of such products include aluminum phosphate, 2,2'-methylidene-bis(4,6-di-t-butylphenyl)phosphate calcium salt, 2,2'-ethylidene-bis(4,6-di-t-butylphenyl)phosphate sodium salt, 2,2'-ethylidene-bis(4,6-di-t-butylphenyl)phosphate lithium salt, 2,2'-ethylidene-bis(4,6-di-t-butylphenyl)phosphate aluminum salt, and bis-(4-t-butylphenyl)phosphate calcium salt. Examples of such products on the market include "ADK STAB (registered trademark) NA-11", "ADK STAB NA-21", and "ADK STAB NA-27" sold by ADEKA CORPORATION.
[0054] The content of the α crystal nucleating agent (C) in the polypropylene resin composition of the present invention is 0.05 to 1.0 part by mass, preferably 0.1 to 0.8 part by mass, per 100 parts by mass of the total of the polypropylene resin (A) and the high-density polyethylene (B). If the content of the α-crystal nucleating agent (C) is less than 0.05 part by mass, the rigidity of the injection-molded article may decrease, whereas if it exceeds 1.0 part by mass, the effect of improving the rigidity of the injection-molded article may decrease.
[0055] [Additives (excluding nucleating agents)] The polypropylene resin composition of the present invention may contain any additive (excluding nucleating agents). The additives are preferably known antioxidants and neutralizing agents that can be generally blended into polypropylene resins. When an antioxidant is blended, the blending amount is usually 500 to 8000 ppm by mass, preferably 750 to 7500 ppm by mass, based on the polypropylene resin composition. On the other hand, the blending amount of a neutralizing agent that leads to film defects such as an increase in fish eyes and sticky components is usually 5 to 1000 ppm by mass, preferably 10 to 750 ppm by mass, more preferably 15 to 500 ppm by mass, based on the polypropylene resin composition.
[0056] As for additives other than the antioxidant and neutralizing agent, any known additive that can be blended with polypropylene resin can be used within the scope of the present invention, for example, ultraviolet absorbers, lubricants, flame retardants, antistatic agents, etc. Inorganic fillers or organic fillers other than fine talc reduce the gloss of the injection molded article, so the polypropylene resin composition of the present invention preferably does not contain these.
[0057] (Method of producing polypropylene resin composition) The polypropylene resin composition of the present invention can be produced by various known production methods, for example, by mixing the polypropylene resin (A), the high-density polyethylene (B), the α crystal nucleating agent (C), and, if necessary, the additives in desired amounts by a conventional method such as dry blending or melt kneading in an extruder. Examples of the mixing method include a method of kneading the above-mentioned various components using a conventional kneading device such as a Henschel mixer, ribbon blender, or Banbury mixer. The above-mentioned various components may also be melt kneaded at, for example, 190 to 280°C, preferably 210 to 250°C, using a conventional single-screw extruder or twin-screw extruder, Brabender, or roll, and pelletized. When a twin-screw extruder is used, if the rotation speed is high, the ultra-high molecular weight component contained in the CDIS of the polypropylene resin (A) may decompose, resulting in a decrease in Mw / Mn and Mz / Mw, so a single-screw extruder is more preferable.
[0058] [Injection molded product] The injection molded article according to the present invention is produced using the polypropylene resin composition described above. The polypropylene resin contained in the polypropylene resin composition satisfies the above-mentioned requirements (A-1) to (A-6) at the same time, and therefore has a good balance of gloss, rigidity, and impact resistance. Furthermore, due to its wide molecular weight distribution (requirement (A-4)), it has high melt fluidity and contains a large amount of high molecular weight polymers, and based on this, the high molecular weight polymers exert their effect as crystal nucleating agents, resulting in a fast crystallization rate. Due to these characteristics, it has the characteristics of high fluidity into a mold during molding, and further, a fast crystallization rate, which allows the molding cycle to be shortened.
[0059] Therefore, the injection molded article according to the present invention is not limited in its application, but can be suitably used for automobile exterior parts, automobile interior parts, other automobile parts, home appliance parts, food containers, beverage containers, medical containers, containers, etc. It is particularly suitable for parts of home appliances (rice cookers, vacuum cleaners, washing machines, refrigerators, electric fans, air conditioners, etc.) or parts of housing equipment (dressing tables, ventilation fans, toilet seats, toilet covers, etc., and accessories or housings). EXAMPLES
[0060] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these. 1.Measurement method (1) Flexural modulus The measurements were made in accordance with ISO178 at a test temperature of 23°C and a test speed of 2.0 mm / min (units are MPa). The test specimens were molded into flat plates (thickness 4 mm, width 10 mm, length 80 mm) at a molding temperature of 200°C and a mold temperature of 40°C using a Toshiba Machine EC40 injection molding machine.
[0061] (2) Charpy impact strength The measurements were made in accordance with JIS K7112 at a test temperature of 23°C (units are kJ / m 2The test specimens were prepared by molding flat plates (thickness 4 mm, width 10 mm, length 80 mm) at a molding temperature of 190°C and a mold temperature of 40°C using a Toshiba Machine EC40 injection molding machine.
[0062] (3) Impact energy The puncture energy (hereinafter also referred to as "impact energy") (unit: J) was measured at a test temperature of 23°C and a test speed of 3.0 m / sec in accordance with JIS K7211-2. Test specimens were prepared by molding flat plates (thickness 2 mm, width 120 mm, length 130 mm) at a molding temperature of 230°C and a mold temperature of 40°C using a NEX110IV injection molding machine manufactured by Nissei Plastic Industrial Co., Ltd.
[0063] (4) Gross The 60° surface gloss was measured using a Gloss Meter VG7000 (manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with ISO 2813. The 60° surface gloss corresponds to the specular gloss when the specular gloss of 0.1001 at an incident angle of 60°, specified for a glass surface with a refractive index of 1.567, is taken as 100%. The same flat plate as in (3) above was used as the test piece.
[0064] (5) Melt flow rate (MFR) The MFR of the polypropylene resin (A) and the polypropylene resin composition was measured in accordance with JIS K7210 at 230° C. under a load of 2.16 kg (unit: g / 10 min). The MFR of the high-density polyethylene (B) was measured in accordance with ASTM D1238 at 190° C. under a load of 2.16 kg (unit: g / 10 min).
[0065] (6) Amount of n-decane insolubles at room temperature (CDIS amount) and amount of n-decane solubles at room temperature (CDS amount) The amount of n-decane insoluble at room temperature and the amount of n-decane soluble at room temperature were determined by the following method. 200 ml of n-decane was added to 5 g of polypropylene resin (A), and the mixture was dissolved by heating at 145° C. for 30 minutes. The solution was then cooled to room temperature of 25° C. over about 2 hours, and allowed to stand at 25° C. for 30 minutes. The solution was filtered through a filter cloth with an opening of about 15 μm, and dried to obtain a room temperature n-decane insoluble portion. The mass of the room temperature n-decane insoluble portion was divided by the mass of polypropylene resin (A), which was 5 g, to obtain the amount of n-decane insoluble portion.
[0066] In addition, the solution after filtering out the room temperature n-decane insoluble part is placed in acetone in an amount about three times the amount of the solution, and the components dissolved in n-decane are precipitated to obtain a room temperature n-decane soluble part. Thereafter, the room temperature n-decane soluble part is filtered out with a glass filter (G2, mesh size about 100 to 160 μm), dried, and the mass of the room temperature n-decane soluble part is measured. The mass of the room temperature n-decane soluble part at this time is divided by 5 g, which is the mass of polypropylene resin (A), to obtain the amount of n-decane soluble part. Note that no residue was observed even when the filtrate side from which the room temperature n-decane soluble part was filtered out was concentrated and dried.
[0067] (7) Mesopentad fraction of CDIS (mmmm fraction) The mesopentad fraction (mmmm fraction) of CDIS is a value determined by the assignment given in Macromolecules, 8, 687 (1975) by A. Zambelli et al. 13 The measurement was performed by C-NMR under the following conditions. The mesopentad fraction is a value expressed by the following formula. Mesopentad fraction = (peak area at 21.7 ppm) / (peak area at 19-23 ppm)
[0068] <Measurement conditions> Equipment JNM-Lambada400 (product name, manufactured by JEOL Ltd.) Resolution 400MHz Measurement temperature 125℃ Solvent: 1,2,4-trichlorobenzene / deuterated benzene = 7 / 4 (mass ratio) Pulse width 7.8μsec Pulse interval: 5 seconds Accumulation count: 2000 times Shift standard TMS=0ppm Mode Single pulse broadband decoupling.
[0069] (8) Intrinsic viscosity of n-decane soluble part at room temperature [η] The intrinsic viscosity [η] (unit: dl / g) of the room temperature n-decane soluble portion was determined as follows. About 25 mg of the room temperature n-decane soluble portion was dissolved in 25 ml of decalin, and the specific viscosity ηsp was measured in an oil bath at 135 ° C. using an Ubbelohde viscometer. After diluting this decalin solution by adding 5 ml of decalin solvent, the specific viscosity ηsp was measured in the same manner. This dilution procedure was repeated two more times, and the value of ηsp / C when the concentration C was extrapolated to 0 (zero) was calculated as the limiting viscosity, which was the limiting viscosity [η] measured in decalin at 135 ° C.
[0070] (9) Ethylene content of n-decane soluble matter at room temperature The ethylene content in the n-decane soluble fraction at room temperature is 13 The values were determined by the following measurement and calculation based on the C-NMR measurement. The samples used were the precipitates (α) and (β) obtained when the ratios of Dinsol and Dsol were calculated. The precipitates (α) and (β) were used as samples and were subjected to the following conditions: 13 C-NMR measurements were performed.
[0071] < 13 C-NMR measurement conditions> Measurement equipment: JEOL LA400 type nuclear magnetic resonance spectrometer Measurement mode: BCM (Bilevel Complete decoupling) Observation frequency: 100.4MHz Observation range: 17006.8Hz Pulse width: C core 45° (7.8 μsec) Pulse repetition time: 5 seconds Sample tube: 5mmφ Sample tube rotation speed: 12Hz Accumulation count: 20,000 times Measurement temperature: 125℃ Solvent: 1,2,4-trichlorobenzene: 0.35 ml / heavy benzene: 0.2 ml Sample size: approx. 40 mg
[0072] From the spectrum obtained by the measurement, the ratio of monomer chain distribution (triad distribution) was determined according to the following literature (1), and the molar fraction (mol%) of the structural unit derived from ethylene (hereinafter referred to as E (mol%)) and the molar fraction (mol%) of the structural unit derived from propylene (hereinafter referred to as P (mol%)) in the room temperature n-decane soluble portion were calculated. The ethylene content (mass%) (hereinafter referred to as E (mass%)) in the room temperature n-decane soluble portion of the polypropylene resin was calculated by converting the calculated E (mol%) and P (mol%) into mass% according to the following (Equation 1).
[0073] Literature (1): Kakugo, M.; Naito, Y.; Mizunuma, K.; Miyatake, T., Carbon-13 NMR determination of monomer sequence distribution in ethylene-propylenecopolymers prepared with delta-titanium trichloride-diethylaluminumchloride. Macromolecules 1982, 15, (4), 1150-1152 E(mass%)=E(mol%)×28×100 / [P(mol%)×42+E(mol%)×28](Formula 1)
[0074] (10) Mw / Mn, Mz / Mw The measurements were performed under the following conditions, and the obtained chromatograms were analyzed by known methods to calculate the number average molecular weight Mn, weight average molecular weight Mw, and Z-average molecular weight Mz of the polypropylene resin (A), and the values were used to obtain Mw / Mn and Mz / Mw. The molecular weight was calculated by the universal calibration method, and the value was calculated in terms of polystyrene. The baseline of the GPC chromatogram was set to the retention time at which the elution curve rose, and the retention time corresponding to a molecular weight of 1000 was set to the end point.
[0075] Liquid chromatograph: Waters ALC / GPC150-Cplus (Differential refractometer detector integrated type) Column: Tosoh Corporation GMH6-HT x 2 and Two GMH6-HTLs were connected in series. Mobile phase medium: o-dichlorobenzene Flow rate: 1.0mL / min Measurement temperature: 140℃ Calibration curve creation method: Standard polystyrene samples were used Sample concentration: 0.10% (W / W) Sample volume: 500μL
[0076] (11) Density The density of high density polyethylene (B) is determined by ASTM D1505.
[0077] 2. Raw Materials (A) Polypropylene resin (1) Raw materials In order to obtain the polypropylene resin (A) used in the examples and comparative examples, the following polymers (a1) to (a7) were prepared. (a1) Prime Polypro (registered trademark) J-784HV (propylene-ethylene block copolymer obtained by two-stage polymerization) manufactured by Prime Polymer Co., Ltd. (MFR = 12 g / 10 min, CDS ratio = 13.5 mass%, ethylene content of CDS = 35.0 mass%, intrinsic viscosity [η] of CDS = 2.5 dL / g) (a2) Prime Polypro X860 (propylene-ethylene block copolymer obtained by two-stage polymerization) manufactured by Prime Polymer Co., Ltd. (MFR = 63 g / 10 min, CDS ratio = 23.0 mass%, ethylene content of CDS = 31.7 mass%, intrinsic viscosity of CDS [η] = 2.5 dL / g) (a3) Prime Polypro J108P (homo PP) (MFR = 45g / 10min) manufactured by Prime Polymer Co., Ltd. (a4) Prime Polypro J13B (homo PP) (MFR=220g / 10min) manufactured by Prime Polymer Co., Ltd. (a5) Prime Polypro H-50000 (homo PP) (MFR=500g / 10min), manufactured by Prime Polymer Co., Ltd. (a6) Prime Polypro VP103W (homo PP) (MFR = 3.0 g / 10 min), manufactured by Prime Polymer Co., Ltd. (a7) Homo PP produced in Production Example 1 below
[0078] (2) Manufacturing Example [Production Example 1] (Production of polymer (a7)) (1) Preparation of magnesium compounds A reaction vessel equipped with a stirrer (capacity 500 liters) was thoroughly purged with nitrogen gas, and 97.2 kg of ethanol, 640 g of iodine, and 6.4 kg of metallic magnesium were added and reacted under reflux conditions with stirring until no more hydrogen gas was generated from the system, yielding a solid reaction product. The reaction liquid containing this solid reaction product was dried under reduced pressure to obtain the desired magnesium compound (support for solid catalyst).
[0079] (2) Preparation of solid catalyst component In a reactor (capacity 500 liters) equipped with a stirrer that had been thoroughly purged with nitrogen gas, 30 kg of the magnesium compound (not crushed), 150 liters of purified heptane (n-heptane), 4.5 liters of silicon tetrachloride, and 5.4 liters of di-n-butyl phthalate were added. The system was kept at 90°C, and 144 liters of titanium tetrachloride was added while stirring, and the reaction was carried out at 110°C for 2 hours, after which the solid component was separated and washed with purified heptane at 80°C. Furthermore, 228 liters of titanium tetrachloride was added, and the reaction was carried out at 110°C for 2 hours, followed by thorough washing with purified heptane to obtain a solid catalyst component.
[0080] (3) Preparation of prepolymerization catalyst 10 mmol of triethylaluminum, 2 mmol of dicyclopentyldimethoxysilane, and 1 mmol of the solid catalyst component obtained in (2) in terms of titanium atom were added to 200 mL of heptane. The internal temperature was kept at 20°C, and propylene was continuously introduced while stirring. After 60 minutes, the stirring was stopped, and as a result, a prepolymerization catalyst in which 4.0 g of propylene was polymerized per 1 g of the solid catalyst component was obtained.
[0081] (4) Main Polymerization 336 L of propylene was charged into a 600 L autoclave and the temperature was raised to 60°C. Then, 8.7 mL of triethylaluminum, 11.4 mL of dicyclopentyldimethoxysilane, and 2.9 g of the prepolymerization catalyst obtained in (3) were charged to initiate polymerization. 75 minutes after the start of polymerization, the temperature was lowered to 50°C over 10 minutes (end of the first stage polymerization).
[0082] The propylene homopolymer (a71) polymerized under the same conditions as in the first stage had an intrinsic viscosity [η] of 11 dL / g. After lowering the temperature in the same polymerization tank as the first stage, hydrogen was continuously introduced so that the pressure was kept constant at 3.3 MPaG, and polymerization was carried out for 160 minutes. Then, the vent valve was opened, and unreacted propylene was purged via an integrating flow meter (end of second stage polymerization). Thus, polymerization was carried out in a batch manner to obtain 54.4 kg of a powdery propylene homopolymer (B1).
[0083] The MFR of the finally obtained propylene homopolymer (polymer (a7)) was 1.9 g / 10 min. The proportion of the propylene homopolymer (a71) produced in the first stage polymerization in the finally obtained propylene homopolymer (a7) calculated from the material balance was 24 mass%. The physical properties of VP103W (polymer (a6)) and the homo-PP (propylene homopolymer (polymer (a7))) obtained in Production Example 1 are shown in Table 1.
[0084] [Table 1]
[0085] [Production Example 2] (Production of Polypropylene Resin (A1)) Polymers (a1), (a5) and (a6) were dry-blended in proportions of 55.6 mass%, 22.2 mass% and 22.2 mass%, respectively, and granulated in a co-rotating twin-screw kneader (product number NR2-36, manufactured by Nakatani Machinery Co., Ltd., kneading temperature: 230 ° C., screw rotation speed 200 rpm) to obtain polypropylene resin (A1). Here, polymer (a5) was blended to adjust the MFR and CDS content of the polypropylene resin, and polymer (a6) was blended to adjust the Mw / Mn and Mz / Mw of the CDIS of the polypropylene resin. The physical properties of the obtained polypropylene resin (A1) are shown in Table 2.
[0086] [Production Example 3] (Production of polypropylene resin (A2)) Polymers (a1), (a4) and (a6) were dry-blended in proportions of 55.6 mass%, 34.4 mass% and 10.0 mass%, respectively, and produced in the same manner as in Production Example 2. Polymer (a4) was blended to adjust the MFR and CDS content of the polypropylene resin. The physical properties of the obtained polypropylene resin (A2) are shown in Table 2.
[0087] [Production Example 4] (Production of polypropylene resin (A3)) Polymers (a2), (a3) and (a6) were dry-blended in proportions of 55.6 mass%, 22.2 mass% and 22.2 mass%, respectively, and produced in the same manner as in Production Example 2. Polymer (a3) was blended to adjust the MFR and CDS content of the polypropylene resin. The physical properties of the obtained polypropylene resin (A3) are shown in Table 2.
[0088] [Production Example 5] (Production of polypropylene resin (A4)) Polymers (a1), (a5) and (a7) were dry blended in proportions of 55.6 mass%, 22.2 mass% and 22.2 mass%, respectively, and produced in the same manner as in Production Example 2. Here, polymer (a5) was blended to adjust the MFR and CDS content of the polypropylene resin, and polymer (a7) was blended to adjust the Mw / Mn and Mz / Mw of the CDIS of the polypropylene resin. The physical properties of the obtained polypropylene resin (A4) are shown in Table 2.
[0089] (B) High-density polyethylene High density polyethylene (B1): Prime Polymer Co., Ltd., Hi-Zex 1820J (MFR (190°C, 2.16 kg) = 32 g / 10 min, density = 963 kg / m 3 ) High density polyethylene (B2): Prime Polymer Co., Ltd., Hi-Zex 1700J (MFR (190°C, 2.16 kg) = 17 g / 10 min, density = 968 kg / m 3 )
[0090] (C) Alpha crystal nucleating agent Alpha crystal nucleating agent (C1): Adeka STAB NA-11 (product name, CAS number: 85209-91-2, manufactured by ADEKA)
[0091] [Example 1] 90% by mass of polypropylene resin (A1) and 10% by mass of high-density polyethylene (B1) were mixed so that 0.2 parts by mass of α-crystal nucleating agent (C1) was included per 100 parts by mass in total, and these were mixed and granulated in a same-rotation twin-screw kneader (product number NR2-36, manufactured by Nakatani Machine Co., Ltd., mixing temperature: 230 ° C., screw rotation speed 200 rpm) to obtain a polypropylene resin composition. Here, the nucleating agent (C1) was mixed in advance by dry blending when producing (granulating) the propylene-based block copolymer (A1), and the granules and high-density polyethylene (B1) were dry blended and melt-kneaded to obtain a polypropylene resin composition. The composition of the polypropylene resin composition and its physical properties are shown in Table 3.
[0092] [Examples 2 to 4 and Comparative Examples 1 to 6] A polypropylene resin composition was obtained in the same manner as in Example 1, except that the types and amounts of (A), (B) and (C) were changed as shown in Table 3. Here, the nucleating agent (C1) was previously mixed by dry blending when the propylene-based block copolymers (A1 to A4) were produced (granulated). The amount of the nucleating agent (C1) was set to 0.2 parts by mass per 100 parts by mass of the polypropylene resins (A1 to A4) and the high-density polyethylene in total. The physical properties are shown in Table 3.
[0093] In comparison with the Examples, Comparative Example 1 has a lower content of high-density polyethylene (B) than the specified amount, so that the gloss is inferior, and Comparative Example 2 has a higher content than the specified amount, so that the rigidity is low. Comparative Examples 3 and 4 have a lower MFR of high-density polyethylene (B) than the specified amount, so that the gloss is inferior. Comparative Example 5 has a lower Mw / Mn and Mz / Mw than the specified amount of polypropylene resin (A), so that the rigidity and gloss are inferior, and Comparative Example 6 has a lower ethylene content in the CDS of polypropylene resin (A) than the specified amount, so that the Charpy impact strength is inferior. As described above, the compositions of the Examples have an excellent balance of rigidity, impact resistance, and gloss.
[0094] [Table 2]
[0095] [Table 3]
Claims
1. The composition comprises 75 to 95 parts by mass of a polypropylene resin (A) satisfying the following (A-1) to (A-6), 5 to 25 parts by mass of a high-density polyethylene (B) satisfying the following (B-1) to (B-2) (wherein the total amount of the polypropylene resin (A) and the high-density polyethylene (B) is 100 parts by mass), and 0.05 to 1.0 part by mass of an α-crystal nucleating agent (C), The polypropylene resin (A) is either a propylene-based block copolymer containing a component mainly consisting of structural units derived from propylene and a component mainly consisting of structural units derived from propylene and ethylene, or a composition prepared by blending the propylene-based block copolymer with another propylene homopolymer or propylene-based block copolymer. Polypropylene resin composition. (A-1) Melt flow rate (230°C, 2.16 kg load) is 2 to 100 g / 10 min. (A-2) It is composed of 85 to 97% by mass of a component insoluble in n-decane at room temperature and 3 to 15% by mass of a component soluble in n-decane at room temperature (the total amount of both is 100% by mass). (A-3) The mesopentad fraction (mmmm fraction) of the component insoluble in n-decane at room temperature is 94.0% or more. (A-4) The component insoluble in n-decane at room temperature has an Mw / Mn of 8.0 to 15.0 and an Mz / Mw of 7.0 to 12.
0. (A-5) The intrinsic viscosity [η] of the component soluble in n-decane at room temperature is 1.5 to 5.0 dL / g. (A-6) The ethylene content of the component soluble in n-decane at room temperature is 35 to 46% by mass. (B-1) Melt flow rate (190°C, 2.16 kg load) is 20 to 80 g / 10 min. (B-2) Density is 955 kg / m 3 More than this
2. The polypropylene resin composition according to claim 1, wherein the α crystal nucleating agent (C) is a phosphate metal salt-based nucleating agent.
3. 3. An injection molded article of the polypropylene resin composition according to claim 1 or 2.
Citation Information
Patent Citations
Resin composition for facing member
JP1985177049A
Propylene polymer composition
JP1988039944A
Modifier for polypropylene resin and polypropylene resin composition
JP1998158440A
Resin composition
JP1998330579A
Resin composition for gas-assisted injection molding and preparation of resin molding, and resin molding
JP1999060887A