Aluminum alloy for die casting and manufacturing method of cast product using same

The aluminum alloy with tailored compositions and injection conditions addresses the lack of strength and toughness in die casting by refining crystallized substances, achieving high mechanical properties through T5 treatment.

JP7580215B2Active Publication Date: 2024-11-11AISIN KEIKINZOKU CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020121010
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-25
Filing Date
2020-07-15
Publication Date
2024-11-11
Estimated Expiration
2040-07-15

AI Technical Summary

Technical Problem

Existing aluminum alloys for die casting lack sufficient strength and toughness, particularly when using T5 treatment, due to insufficient Cu content and coarse crystallized substances, limiting their effectiveness in producing high-strength and high-toughness cast products.

Method used

An aluminum alloy composition with specific ranges of Si (7.0-9.0%), Mg (0.4-0.6%), Cu (0.4-0.7%), Cr (0.1-0.5%), Mn (0.5%), and optionally Ti (up to 0.2%), along with controlled injection conditions, to enhance strength and toughness through refined crystallized substances and laminar flow.

Benefits of technology

The alloy achieves tensile strength of 280 MPa, 0.2% proof stress of 180 MPa, and Charpy impact value of 3 J/cm² with 4% elongation, resulting in a die-cast product with high strength and toughness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580215000001
    Figure 0007580215000001
  • Figure 0007580215000002
    Figure 0007580215000002
  • Figure 0007580215000003
    Figure 0007580215000003
Patent Text Reader

Abstract

To provide an aluminum alloy suitable for obtaining a die-cast aluminum product having high strength and high toughness, and a method for producing a cast product using the same.SOLUTION: The aluminum alloy comprises, by mass%, Si: 7.0 to 9.0%, Mg: 0.4 to 0.6%, Cu: 0.4 to 0.7%, Cr: 0.1 to 0.5%, Mn: 0.5% or less, [Cr+Mn]: 0.1 to 0.8%, Fe: 0.10 to 0.25%, and Sr: 0.005 to 0.02%, the balance being Al and impurities.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an aluminum alloy suitable for die casting using a die casting machine and a method for producing a cast product by die casting using the same, which is particularly capable of achieving both high strength and high toughness. [Background technology]

[0002] Die casting is a casting method in which molten metal is filled into a mold cavity at high speed and under high pressure. It is highly productive and is widely used for automobile parts, machine parts, etc. For such die casting, aluminum alloys are used because of the requirement for good flowability into the mold. In recent years, however, there has been a demand for higher strength aluminum alloys due to the need for weight reduction. However, these alloys tend to have insufficient toughness, so there is a demand for aluminum alloys that are both high strength and tough.

[0003] Patent Document 1 discloses an aluminum alloy containing 3.5-7.5% Si, 0.45-0.8% Mg, 0.05-0.25% Cr, and 0-0.01% Cu, but states that heat treatment, known as T6 treatment, is required after solution treatment to obtain a tensile strength of 320 MPa or more. However, the T6 treatment is longer and less productive than the T5 treatment, and the Cu content is low at 0 to 0.01%, so it is presumed that sufficient strength cannot be obtained with the T5 treatment.

[0004] Patent Document 2 discloses an alloy containing 6.00-6.50% Si, 0.10-0.50% Mg, 0.30% or less Fe, 0.30-0.60% Mn, and 0.10-0.30% Cr for the purpose of obtaining high yield strength and high ductility, and further describes the inclusion of 30-200 ppm Sr, 1-50 ppm B, 0.05-0.20% Sb, and 0.05-0.30% Ti. However, since the Si content is low and there is a risk of poor melt flow, and since only a small amount of Cu is added, it is presumed that sufficient strength cannot be obtained by T5 treatment. [Prior art documents]

Patent Document

[0005]

Patent Document 1

Patent Document 2

Summary of the Invention

Problems to be Solved by the Invention

[0006] An object of the present invention is to provide an aluminum alloy suitable for obtaining a die-cast aluminum casting product having high strength and high toughness, and a method for manufacturing a casting product using the same.

Means for Solving the Problems

[0007] The aluminum alloy for die-casting according to the present invention contains, in all mass percentages below, Si: 7.0 to 9.0%, Mg: 0.4 to 0.6%, Cu: 0.4 to 0.7%, Cr: 0.1 to 0.5%, Mn: 0.5% or less, [Cr + Mn]: 0.1 to 0.8%, Fe: 0.10 to 0.25%, Sr: 0.005 to 0.02%, and the balance is Al and impurities. Furthermore, Ti may be contained in the range of 0.2% or less as necessary. Here, the impurities refer to inevitable impurities that may be mixed in during the manufacturing process.

[0008] In the present invention, the reasons for selecting the component ranges are explained. <Si Component> In die-casting, Si is required to be 7.0 mass% or more (hereinafter simply expressed as %) to ensure the fluidity of the molten metal. If it exceeds 9.0%, coarse primary Si is likely to precipitate, and the elongation may decrease. Therefore, the range of Si is set to 7.0 to 9.0%. Preferably, the range is Si: 7.10 to 8.50%. <Mg, Cu Components> Mg and Cu are components effective in improving the strength of the cast product. In the present invention, Mg: 0.4% or more and Cu: 0.4% or more are used so that high strength can be obtained by heat treatment (T5 treatment) after casting. However, in order to suppress the elongation from decreasing more than necessary, the range is set to Mg: 0.4 - 0.6% and Cu: 0.4 - 0.7%. <Cr, Mn, Fe components> In die-cast casting, the Fe component is one of the components that are easily mixed in. When Fe exceeds 0.25%, the crystals become coarser and the elongation decreases. Therefore, in the present invention, it is set in the range of Fe: 0.10 - 0.25%, and by adding Cr, the refinement of Fe-based crystals is achieved. If the Cr component exceeds 0.5%, there is a risk that coarser crystals will crystallize, so the range is set to Cr: 0.1 - 0.5%. In the present invention, the Fe-based crystals can also be refined by adding Mn. When adding Mn, it is preferably 0.5% or less. When Mn exceeds 0.5%, coarse crystals are likely to crystallize and the elongation decreases. Also, when adding both Cr and Mn, it is necessary to control the total value. The total of Cr and Mn [Cr + Mn] is preferably in the range of 0.1 - 0.8%. <Sr, Ti components> Adding a small amount of Sr is effective in refining eutectic Si, and the range is set to Sr: 0.005 - 0.02%. Also, Ti is not an essential component in the present invention, but when added, it is effective in refining the crystal grains of the aluminum alloy. When adding, the range of 0.01 - 0.2% is preferred.

[0009] The mold used for die-cast casting consists of a movable mold that is open / closed controlled with respect to a fixed mold. The molten aluminum alloy poured into the sleeve is injected into the cavity formed when the fixed mold and the movable mold are closed by a plunger under high-speed and high-pressure conditions for casting. This injection condition is preferably set so that the gate speed is 1 m / sec or less so that laminar flow filling occurs in the cavity of the mold. The mold used in the present invention is preferably a center gate type mold capable of radially injecting molten metal from the center.

[0010] When the aluminum alloy according to the present invention is used, a tensile strength of 280 N / mm can be achieved by performing heat treatment (T5 treatment) at 160°C to 200°C for 2 to 8 hours after die casting. 2 Above, 0.2% yield strength 180N / mm 2 or more, elongation 4% or more and Charpy impact value 3J / cm 2 Thus, a cast product having the above-mentioned high strength and high toughness can be obtained. In addition, when the average area of ​​the crystallized particles excluding eutectic Si in the metal structure of such a casting product is measured using an optical microscope, it is found to be 2 μm 2 It is as follows. Effect of the Invention

[0011] When the aluminum alloy according to the present invention is used for die casting, a die cast product having high strength and excellent toughness can be obtained by the subsequent T5 treatment. [Brief description of the drawings]

[0012] [Figure 1] The chemical composition of the aluminum alloy used in the evaluation is shown below. [Diagram 2] The evaluation results are shown. [Diagram 3] 1 shows optical microscope photographs of the metal structures of Example 1 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Molten aluminum alloys with the chemical compositions shown in the table in Figure 1 were prepared, and die-cast into cast products using a center-gate type mold. The casting conditions are molten metal temperature of approximately 700°C and injection gate speed of 0.8 m / see. After casting, heat treatment (T5) was performed at 190°C for 3 hours. FIG. 2 shows the measurement results of the mechanical properties and the average area (average area) of crystallized particles excluding eutectic Si. FIG. 3 shows examples of optical microscope photographs of Example 1 and Comparative Example 1.

[0014] The test items and test methods are as follows: <Tensile strength, 0.2% yield strength and elongation> Based on JIS-Z2241, JIS-4 test pieces were cut out from the castings, and tensile tests were carried out using a tensile testing machine conforming to the JIS standard to measure the tensile strength (MPa), 0.2% yield strength (MPa), and elongation (%). <Charpy impact test> Based on JIS-Z2242, JIS-4 Charpy impact test pieces were cut out from the castings and measured using a Charpy impact tester conforming to the JIS standard. <Average crystallized area> The cut surfaces of the castings were mirror-polished and observed and measured under an optical microscope. Measurement area at 1000x magnification: 0.166mm 2 Image processing was performed within the range, and the area of ​​the crystallized matter in the part excluding the eutectic Si was measured and the average value was calculated.

[0015] The chemical composition in FIG. 1 and the evaluation results in FIG. 2 reveal the following. In the present invention, the target is a high strength of tensile strength of 280 MPa or more, 0.2% yield strength of 180 MPa or more, and a Charpy impact value of 3 J / cm at an elongation of 4% or more. 2 The goal was to achieve even higher toughness. All of Examples 1 to 11 have alloy compositions within the set ranges, and meet all targets for T5 treatment. In contrast, in Comparative Example 1, the Cr content was 0.85%, exceeding 0.5%, so coarse Cr-based crystals were formed, the elongation was below the target, and the Charpy impact value also did not reach the target. On the other hand, in Comparative Example 2, since Cr was not added, Fe-based crystallized particles became coarse, resulting in a low elongation value. Comparative Example 3 had a low Cu content, Comparative Example 4 had a low Si content, and Comparative Example 5 had a low Mg content, so that the 0.2% yield strength of the tensile strength did not reach the target. Comparative Example 6 had a high Cu content, Comparative Example 7 had a high Mg content, and Comparative Example 8 had a high Fe content, resulting in low elongation. In Comparative Example 9, since Sr was not added, the elongation was poor. Comparative Examples 10 to 14 are made of F material and therefore have low strength. In Comparative Example 15, the total of [Cr+Mn] was 0.98%, exceeding 0.8%, so the crystallized particles became coarse and the average crystallized particle area was 5.6 μm 2 and 2 μm 2 This resulted in lower growth.

Claims

1. An aluminum alloy for die casting containing, by mass, Si: 7.0 to 9.0%, Mg: 0.4 to 0.6%, Cu: 0.4 to 0.7%, Cr: 0.1 to 0.5%, Mn: 0.5% or less, [Cr + Mn]: 0.1 to 0.8%, Fe: 0.10 to 0.25%, Sr: 0.005 to 0.02%, Ti: 0.01 to 0.2%, and the balance being Al and impurities, The die is filled with laminar flow at a gate speed of 1 m / sec or less by die casting. A method for manufacturing a cast product, comprising the steps of: after die casting, performing heat treatment at 160°C to 200°C for 2 to 8 hours.

2. Tensile strength: 280N / mm 2 Above, 0.2% yield strength 180N / mm 2 or more, elongation 4% or more and Charpy impact value 3 J / cm 2 2. The method for producing a casting product according to claim 1, wherein the casting product has the above-mentioned high strength and high toughness.

Citation Information

Patent Citations

  • Freezing method by reinforced frozen ground

    JP1980075028A

  • Breaking circuit for converter power source

    JP1982097360A

  • Aluminum alloy, rod-shape material, forging shaped article, machining shaped article, wear-resistant aluminum alloy having excellent hardness of anodically oxidized film using the same, sliding part, and their production method

    JP2004232087A

  • Aluminum alloy for die casting, and die-cast aluminum alloy using same

    WO2016166779A1

  • Aluminum alloy for die casting, and aluminum alloy die casting using same

    WO2018189869A1