Heat-resistant millable silicone rubber composition

A millable silicone rubber composition with yellow iron oxide, cerium oxide, and organic peroxide enhances heat resistance and mechanical properties at high temperatures, addressing the limitations of existing compositions.

JP7580251B2Active Publication Date: 2024-11-11SHIN ETSU CHEMICAL CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020188245
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-11
Publication Date
2024-11-11
Estimated Expiration
2040-11-11

AI Technical Summary

Technical Problem

Existing silicone rubber compositions exhibit poor heat resistance at high temperatures, particularly around 300°C, and there is a need for improved heat resistance and mechanical properties under such conditions.

Method used

A millable silicone rubber composition containing specific amounts of yellow iron oxide, cerium oxide, and organic peroxide, along with reinforcing silica and a silica dispersant, without epoxy resin, is formulated to enhance heat resistance and maintain mechanical properties.

Benefits of technology

The composition achieves excellent heat resistance at temperatures above 200°C, particularly up to 300°C, while suppressing hardness increase and maintaining good mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580251000001
    Figure 0007580251000001
  • Figure 0007580251000002
    Figure 0007580251000002
Patent Text Reader

Abstract

To provide a millable-type silicone rubber composition, which provides a silicone rubber (cured material) having more excellent heat resistance at a high temperature of 200°C or more, especially 300°C.SOLUTION: A millable-type silicone rubber composition comprises: (A) 100 pts.mass of organopolysiloxane with an average degree of polymerization of 1,000 or more, having 2 or more alkenyl groups bonded to silicon atoms in one molecule; (B) 5 to 100 pts.mass of reinforcing silica having a specific surface area of 50 m2 / g or more; (C) 0.01 to 10 pts.mass of yellow iron oxide; (D) 0.01 to 10 pts.mass of at least one selected from cerium oxide and cerium hydroxide; and (E) 0.1 to 10 pts.mass of an organic peroxide.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a millable type silicone rubber composition. [Background technology]

[0002] Silicone rubber has excellent weather resistance, electrical properties, low compression set, heat resistance, cold resistance, etc., and is therefore widely used in various fields, including electrical equipment, automobiles, construction, medicine, and food. For example, it is used in rubber contacts used as rubber contacts in remote controllers, typewriters, word processors, computer terminals, musical instruments, etc.; construction gaskets; various rolls such as copier rolls, developing rolls, transfer rolls, charging rolls, and paper feed rolls; anti-vibration rubbers for audio equipment, etc.; and packings for compact disks used in computers. Currently, the demand for silicone rubber is increasing, and the development of silicone rubber with excellent properties is desired.

[0003] It is known that additives such as cerium oxide, cerium hydroxide, iron oxide, carbon black, etc. can be blended to further improve the heat resistance of silicone rubber. However, the heat resistance of silicone rubber under high temperature conditions of 250°C or higher is insufficient, and silicone rubber that exhibits excellent heat resistance under such conditions is required.

[0004] Patent Document 1 describes how the heat resistance of silicone rubber can be improved by adding 0.1 mass % or more of titanium oxide and iron oxide (particularly diferric oxide) to silicone rubber. However, the document only measures the amounts of formaldehyde, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, and dodecamethylcyclohexasiloxane generated when heated at 300°C for one hour, and makes no mention of any changes in physical properties.

[0005] Patent Document 2 describes that the heat resistance of silicone rubber can be improved by adding hydrous cerium oxide and / or hydrous zirconium oxide to the silicone rubber, and measures the physical properties after placing the material in a dryer at 225°C for 72 hours. However, the heat resistance at higher temperatures is not sufficient.

[0006] Patent Documents 3 and 4 describe titanium oxide doped with metal ions (metal salts) of transition metals or the like, but only disclose applications that utilize its optical properties, such as mid-infrared filters and photocatalysts.

[0007] Patent Document 5 describes an addition reaction curing organopolysiloxane composition containing 0.1 to 50 parts by weight of yellow iron oxide fine powder, preferably yellow iron oxide solid-dissolved with aluminic acid or aluminate, per 100 parts by weight of an alkenyl group-containing organopolysiloxane, and describes that the composition cures by addition reaction to provide a cured product having excellent heat resistance in a high temperature range of 280° C. or higher. Patent Document 6 also describes that the heat resistance of silicone rubber is improved by blending 0.01 to 5% by weight of titanium oxide and cerium oxide and / or cerium hydroxide doped with a transition metal oxide into a silicone rubber composition. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Special Publication No. 2016-518461 [Patent Document 2] JP 2014-031408 A [Patent Document 3] JP 2006-021991 A [Patent Document 4] WO2010 / 140499 [Patent Document 5] Japanese Patent Application Publication No. 7-292256 [Patent Document 6] WO2018 / 079376 Summary of the Invention [Problem to be solved by the invention]

[0009] The addition reaction curing agent described in Patent Document 5 has a problem of poor heat resistance at high temperatures close to 300° C. The silicone rubber obtained from the silicone rubber composition described in Patent Document 6 also has poor long-term heat resistance at high temperatures. Therefore, an object of the present invention is to provide a millable type silicone rubber composition that gives a silicone rubber (cured product) with excellent heat resistance at high temperatures of 200° C. or higher, particularly 300° C. [Means for solving the problem]

[0010] As a result of intensive research conducted by the inventors in order to achieve the above object, they discovered that the heat resistance of silicone rubber can be improved by adding specific amounts of yellow iron oxide and cerium oxide, etc. to an organic peroxide-curing type silicone rubber composition, and thus completed the present invention.

[0011] That is, the present invention provides A millable type silicone rubber composition comprising the following components (A) to (F): (A) A compound having two or more alkenyl groups bonded to silicon atoms in one molecule and having a main chain of R 1 2SiO 2 / 2 It consists of repeating diorganosiloxane units represented by the formula: 1 3SiO 1 / 2 100 parts by mass of a linear diorganopolysiloxane having an average degree of polymerization of 1,000 or more and terminated with a triorganosiloxy group represented by the formula: (In the above formula, R 1 are each independently an unsubstituted group having 1 to 20 carbon atoms selected from an alkyl group, a cycloalkyl group, an alkenyl group, an aryl group, and an aralkyl group. (B) Specific surface area 50m 2 / g or more, 5 to 100 parts by mass of reinforcing silica, (C) 0.01 to 10 parts by mass of yellow iron oxide, (D) 0.01 to 10 parts by mass of cerium oxide, (E) 0.1 to 10 parts by mass of an organic peroxide, and (F) Silica dispersant 0.1 to 50 parts by mass and However, the composition 、 Titanium oxide doped with transition metal oxides does not contain, and The millable type silicone rubber composition does not contain an epoxy resin. to provide. Effect of the Invention

[0012] The millable silicone rubber composition of the present invention can provide silicone rubber with excellent heat resistance. That is, the silicone rubber obtained by curing the millable silicone rubber composition of the present invention exhibits excellent heat resistance at temperatures of 200° C. or higher, particularly at temperatures below 300° C. In addition, the increase in hardness of the silicone rubber (cured product) can be suppressed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] In this specification, the specific surface area is a value measured by the BET method. The millable composition means a composition that is a non-liquid composition with high viscosity that does not have self-flowability at room temperature (25°C) and can be uniformly kneaded under shear stress with a kneading machine such as a roll mill (e.g., two-roll or three-roll).

[0014] [(A) Organopolysiloxane] Component (A) is an organopolysiloxane that is the main component (base polymer) of the composition, and is characterized by having two or more alkenyl groups bonded to silicon atoms in each molecule, preferably 2 to 10,000 alkenyl groups bonded to silicon atoms.

[0015] Component (A) has an average degree of polymerization of 1 , 00 0 The average degree of polymerization is preferably in the range of 1,000 to 100,000, more preferably in the range of 3,000 to 50,000, and particularly preferably in the range of 4,000 to 20,000. Above lower limitIf the average polymerization degree is less than this, the silicone rubber composition of the present invention will not satisfy the properties required for millable rubber, and roll kneading properties will be significantly deteriorated, which is not preferable. The average polymerization degree is determined from the weight average molecular weight converted into polystyrene in GPC (gel permeation chromatography) analysis measured under the following conditions. [Measurement conditions] Developing solvent: Toluene ·Flow rate: 1mL / min Detector: Refractive index detector (RI) Column: KF-805L x 2 (Shodex) Column temperature: 25℃ Sample injection volume: 30 μL (0.2% by mass in toluene solution) In the present invention, component (A) is preferably a non-liquid organopolysiloxane gum that has a high degree of polymerization (high viscosity) and has no self-flowability at room temperature (25° C.).

[0016] The component (A) may be any alkenyl-containing organopolysiloxane that satisfies the above average degree of polymerization, and is preferably represented by the following average composition formula (1). R 1 n SiO (4-n) / 2 (1) (In formula (1), R 1 are each independently a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, and n is a positive number of 1.95 to 2.04.

[0017] In the above average composition formula (1), R 1is a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, preferably 1 to 12, more preferably 1 to 8. Examples of the monovalent hydrocarbon group include alkyl groups such as methyl, ethyl, propyl, and butyl groups, cycloalkyl groups such as cyclohexyl groups, alkenyl groups such as vinyl, allyl, butenyl, and hexenyl groups, aryl groups such as phenyl and tolyl groups, and aralkyl groups such as β-phenylpropyl groups. In addition, some or all of the hydrogen atoms bonded to the carbon atoms of these groups may be substituted with halogen atoms, and examples thereof include 3,3,3-trifluoropropyl groups. Among these, methyl, vinyl, phenyl, and trifluoropropyl groups are preferred, and more preferably methyl or vinyl groups. Among these, R in the above formula (1) is preferred. 1 Of the total moles of R, 50 mol % or more are methyl groups, more preferably 80 mol % or more are methyl groups, and further preferably all R other than alkenyl groups are 1 is preferably a methyl group. In addition, in the above formula (1), R 1 The alkenyl group preferably accounts for 0.001 to 10 mol %, particularly preferably 0.01 to 5 mol %, of the total moles of the above. The alkenyl group is preferably a vinyl group or an allyl group, particularly preferably a vinyl group.

[0018] In the above average composition formula (1), n ​​is a positive number of 1.95 to 2.04, and preferably a positive number of 1.98 to 2.02. If the n value is within the range of 1.95 to 2.04, the resulting cured product will exhibit sufficient rubber elasticity.

[0019] The structure of component (A) is not particularly limited, but the main chain is preferably a diorganosiloxane unit (R 1 2SiO 2 / 2 , R 1 The molecular chain is terminated at both ends with a triorganosiloxy group (R 1 3SiO 1 / 2It is preferable that both molecular chain terminals are blocked with a trimethylsiloxy group, a dimethylvinylsiloxy group, a dimethylhydroxysiloxy group, a methyldivinylsiloxy group, a trivinylsiloxy group, or the like, and it is particularly preferable that both molecular chain terminals are blocked with a siloxy group having at least one vinyl group. These organopolysiloxanes may be used alone or in combination of two or more types having different degrees of polymerization or molecular structures.

[0020] In the silicone rubber composition of the present invention, the content of component (A) is preferably 43 to 96 mass %, more preferably 50 to 90 mass %, and even more preferably 60 to 80 mass %.

[0021] [(B) Reinforcing Silica] The reinforcing silica (B) acts as a filler that imparts excellent mechanical properties to the resulting silicone rubber. The reinforcing silica may be precipitated silica (wet silica) or fumed silica (dry silica), and has a large number of silanol (SiOH) groups on its surface. In the present invention, the reinforcing silica (B) has a specific surface area of ​​50 m2 or less as measured by the BET method. 2 The upper limit of the specific surface area is not particularly limited, but it is preferably 400 m 2 / g or less, preferably 100 to 400m 2 / g. The specific surface area is 50m 2 If it is less than 1 / g, the reinforcing effect of the silicone rubber imparted by component (B) will be insufficient.

[0022] (B) Reinforcing silica may be used in an untreated state, or may be surface-treated with an organosilicon compound such as organopolysiloxane, organopolysilazane, chlorosilane, or alkoxysilane, as necessary. This organosilicon compound is different from the dispersant for (F) reinforcing silica, which will be described later. The reinforcing silica may be used alone or in combination of two or more kinds.

[0023] The amount of (B) reinforcing silica blended is 5 to 100 parts by mass, preferably 10 to 80 parts by mass, and more preferably 20 to 70 parts by mass, per 100 parts by mass of (A) organopolysiloxane. If the amount of (B) component blended is above the above upper limit or below the above lower limit, not only will the processability of the resulting silicone rubber composition decrease, but the mechanical properties such as tensile strength and tear strength of the silicone rubber cured product obtained by curing the silicone rubber composition will be insufficient.

[0024] [(C) Yellow iron oxide] (C) Yellow iron oxide significantly improves the heat resistance of silicone rubber when used in combination with the following component (D). The yellow iron oxide is a powder of iron oxyhydroxide, the main component of which (e.g., 85% or more) is represented by the formula α-FeOOH, and the particles are acicular in shape. There are no particular limitations on the particle size, and any ordinary yellow iron oxide will do. It is preferable that the residue on a 45 μm sieve is 0.01% or less. Commercially available yellow iron oxide products include the TAROX series (manufactured by Titanium Kogyo Co., Ltd.).

[0025] The amount of yellow iron oxide added is 0.01 to 10 parts by mass, preferably 0.1 to 8 parts by mass, and more preferably more than 0.5 to 5 parts by mass, per 100 parts by mass of the organopolysiloxane of component (A). If the amount added is less than the lower limit, the heat resistance of the silicone rubber will not improve, whereas if the amount added exceeds the upper limit, the mechanical properties of the silicone rubber may be significantly reduced.

[0026] The amount of yellow iron oxide in the composition is preferably 0.01 to 5 mass%, and more preferably 0.1 to 3 mass%. The silicone rubber composition of the present invention may contain a small amount of a transition metal oxide other than the component (C) and the component (D) described below, as long as the effect of the present invention is not impaired. The silicone rubber composition of the present invention also includes an embodiment that does not contain titanium oxide, red iron oxide, or titanium oxide doped with a transition metal oxide such as iron oxide.

[0027] [(D) Cerium oxide and / or cerium hydroxide] Component (D) is at least one selected from cerium oxide and cerium hydroxide, either of which can be used in combination with component (C) to significantly improve the heat resistance of the silicone rubber. Commercially available cerium oxide products include Showlox FL-2 (manufactured by Showa Denko K.K.), SN-2 (manufactured by Nikki Co., Ltd.), and Cerium Oxide S (manufactured by Anan Kasei Co., Ltd.). Commercially available cerium hydroxide products include cerium hydroxide (manufactured by Nikki Co., Ltd.) and Cerhydrate 90 (manufactured by Trybach Industrie AG).

[0028] The amount of the (D) component added is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, per 100 parts by mass of the (A) component organopolysiloxane. If the amount is less than the lower limit, the heat resistance of the silicone rubber is not improved, and if the amount is more than the upper limit, the mechanical properties of the silicone rubber may be significantly reduced. Cerium oxide and cerium hydroxide may be used alone or in combination. When cerium oxide and cerium hydroxide are used in combination, the total amount may be within the above range.

[0029] The blending ratio of the components (C) and (D) is preferably 1:100 to 100:1, and more preferably 1:50 to 50:1, by mass ratio.

[0030] [(E)Organic peroxide] (E) Organic peroxide is a curing agent capable of curing the silicone rubber composition of the present invention. Organic peroxides have excellent heat resistance at high temperatures of nearly 300°C, and can therefore further improve the high-temperature heat resistance of the silicone rubber composition. In contrast, addition reaction curing agents using organohydrogenpolysiloxane and platinum-based metal compound catalysts are not preferred because they have poor heat resistance at high temperatures of nearly 300°C.

[0031] Examples of organic peroxide curing agents include benzoyl peroxide, 2,4-dichlorobenzoyl peroxide, p-methylbenzoyl peroxide, o-methylbenzoyl peroxide, 2,4-dicumyl peroxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, di-t-butyl peroxide, t-butyl perbenzoate, and 1,6-hexanediol-bis-t-butyl peroxycarbonate. The amount of organic peroxide curing agent is preferably 0.1 to 10 parts by mass, particularly 0.2 to 5 parts by mass, per 100 parts by mass of component (A). If the amount is too small, curing may be insufficient, and if the amount is too large, the silicone rubber cured product may yellow due to the decomposition residue of the organic peroxide.

[0032] [(F) Dispersants for fillers] In addition to the components (A) to (E), the silicone rubber composition of the present invention may further contain a dispersant for fillers, particularly a dispersant for inorganic fillers or silica. A silica dispersant is preferred. By further containing the dispersant, the reinforcing silica described above can be well dispersed in the composition. The dispersant may be, for example, a low molecular weight organosilicon compound having an alkoxy group or a silanol group or a hydrolyzate thereof. More specifically, various alkoxysilanes, particularly phenyl group-containing alkoxysilanes and their hydrolyzates, diphenylsilanediol, carbon functional silane, silanol group-containing low molecular weight siloxane, etc. can be mentioned. Among them, diphenylsilanediol is preferred because it further improves the heat resistance of the silicone rubber. In addition, by using diphenylsilanediol in combination with an alkylalkoxysilane or its hydrolyzate, the dispersibility of the reinforcing silica is further improved, which is more preferred. As mentioned above, the component (F) is different from the organosilicon compound for surface-treating the reinforcing silica (B).

[0033] The amount of component (F) is preferably 0.1 to 50 parts by mass, and particularly preferably 1 to 20 parts by mass, per 100 parts by mass of component (A). If the amount of the organopolysiloxane capped at both ends with silanol groups used is too small, the effect of adding it will not be observed, whereas if the amount is too large, the plasticity of the composition will be too low, and roll adhesion will occur in kneading means such as a roll mill, which may deteriorate roll workability.

[0034] -Other ingredients- The silicone rubber composition used in the present invention may contain, in addition to the above components, other fillers and additives known in thermosetting silicone rubber compositions, as necessary, within the range that does not impair the effects of the present invention. For example, fillers other than component (B) (crushed quartz, diatomaceous earth, calcium carbonate, etc.), colorants (pigments), tear strength improvers, flame retardancy improvers (platinum compounds, etc.), acid acceptors, thermal conductivity improvers (alumina, boron nitride, etc.), release agents, and reaction control agents, etc. may be mentioned. The other components may be used alone or in combination of two or more. The blending amount may be appropriately adjusted within the range that does not impair the effects of the present invention.

[0035] -Method of manufacturing the composition- The millable silicone rubber composition of the present invention can be obtained by mixing the above-mentioned components with a known kneading machine such as a kneader, a Banbury mixer, or a two-roll mill. For example, when preparing a composition containing the above-mentioned components (A) to (E), it is preferable to mix the organopolysiloxane (A), the reinforcing silica (B), the yellow iron oxide (C), and the cerium oxide (D), and then add the organic peroxide (E) to the mixture obtained. When other components are further included, it is preferable to mix the components (A), (B), (C), and (D) with the other components, and then add the organic peroxide (E) to the mixture obtained.

[0036] The millable silicone rubber composition may be molded into the desired shape and size of the molded product by a known molding method, such as casting, compression molding, injection molding, calendar molding, and extrusion molding.

[0037] -Cured product- The curing conditions for the millable silicone rubber composition may be the known conditions for the molding method used, and are generally from a few seconds to a day at a temperature of 60 to 450° C. In addition, for the purpose of reducing the compression set of the obtained cured product, reducing the low molecular weight siloxane components remaining in the obtained silicone rubber, and removing decomposition products of organic peroxides in the silicone rubber, a post cure (secondary cure) may be performed in an oven at 200° C. or higher, preferably 200 to 250° C., for 1 hour or more, preferably 1 to 70 hours, and more preferably 1 to 10 hours. EXAMPLES

[0038] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0039] In the examples and comparative examples, the heat resistance test was carried out as follows. [Heat resistance] Using a test sheet prepared by curing the silicone rubber composition, the initial values ​​of hardness (Durometer A), tensile strength (MPa), and elongation at break (%) were measured according to JIS K 6249:2003. The test sheet was placed in a 300°C dryer for 3 days and 7 days, or in a 220°C dryer for 7 days, and then the hardness, tensile strength, and elongation at break were measured. The results are shown in Table 1.

[0040] [Example 1] It is composed of 99.85 mol% dimethylsiloxane units, 0.125 mol% methylvinylsiloxane units, and 0.025 mol% dimethylvinylsiloxy units, and has an average degree of polymerization of 8,000 100 parts by mass of organopolysiloxane raw rubber, BET specific surface area 200 m 240 parts by mass of fumed silica (Aerosil 200, manufactured by Nippon Aerosil Co., Ltd.) having a molecular weight of 1.0 to 1.2 g / g, 5 parts by mass of diphenylsilanediol, and 2 parts by mass of dimethylpolysiloxane having silanol groups at both ends, an average degree of polymerization of 4, and a viscosity of 15 mPa s at 25°C were added, and the mixture was heated under mixing in a kneader at 170°C for 2 hours to prepare base compound (1). 0.5 parts by mass of yellow iron oxide (TAROX-LL-XLO, needle-shaped powder containing 87.5% or more of α-FeOOH, manufactured by Titan Kogyo Co., Ltd.) and 0.5 parts by mass of cerium oxide (SN-2, manufactured by Nikki Co., Ltd.) were added to the base compound (1) using a two-roll mill to prepare compound (A). 0.6 parts by mass of 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane was added to compound (A) using a twin roll mill, and the mixture was mixed uniformly to obtain a millable type silicone rubber composition. The silicone rubber composition was subjected to a pressure of 165°C and 70 kgf / cm 2 The test sheet was then post-cured for 4 hours in an oven at 200° C. The cured product was subjected to the above-mentioned heat resistance test.

[0041] [Example 2] A silicone rubber composition was prepared by repeating Example 1, except that the amount of cerium oxide added was 1.5 parts by mass per 100 parts by mass of organopolysiloxane raw rubber, to obtain a cured product. The cured product was subjected to the heat resistance test described above.

[0042] [Example 3] A silicone rubber composition was prepared by repeating Example 2, except that the amount of yellow iron oxide added was 3.0 parts by mass per 100 parts by mass of the organopolysiloxane raw rubber, and a cured product was obtained. The cured product was subjected to the heat resistance test described above.

[0043] [ Reference example 4] A silicone rubber composition was prepared by repeating Example 3, except that the same amount of cerium hydroxide (Cerhydrate 90, manufactured by Treibach Industrie AG) was used instead of the cerium oxide, and a cured product was obtained. The cured product was subjected to the heat resistance test described above.

[0044] [Comparative Example 1] the above In Example 3, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane was replaced with 0.37 parts by mass of methylhydrogenpolysiloxane having SiH groups on the side chains (dimethylsiloxane-methylhydrogensiloxane copolymer capped with trimethylsiloxy groups at both ends, with a degree of polymerization of 38 and 0.0074 mol% SiH groups) per 100 parts by mass of organopolysiloxane raw rubber Using 0.07 parts by mass of ethynylcyclohexanol as a reaction inhibitor, and 0.15 parts by mass of a platinum catalyst (Pt concentration: 1% by mass) Use, The silicone rubber composition was mixed uniformly using a two-roll mill to produce a raw rubber-like silicone rubber composition. 2 The test sheet was then post-cured for 4 hours in an oven at 200° C. The cured product was subjected to the above-mentioned heat resistance test.

[0045] [Comparative Example 2] A silicone rubber composition was prepared by repeating Example 3, except that red iron oxide (red oxide SR-570, manufactured by Tone Sangyo Co., Ltd.) was used instead of the yellow iron oxide, and a cured product was obtained. The cured product was subjected to the heat resistance test described above.

[0046] [Comparative Example 3] A silicone rubber composition was prepared by repeating Example 3, except that the cerium oxide was not used, to obtain a cured product, which was then subjected to the heat resistance test described above.

[0047] [Comparative Example 4] A silicone rubber composition was prepared by repeating the procedure of Comparative Example 2, except that the cerium oxide was not used, to obtain a cured product, which was then subjected to the heat resistance test described above.

[0048] [Comparative Example 5] A silicone rubber composition was prepared by repeating Example 3, except that the amount of cerium oxide added was 3.0 parts by mass per 100 parts by mass of organopolysiloxane raw rubber and the yellow iron oxide was not used, to obtain a cured product. The cured product was subjected to the heat resistance test described above.

[0049] [Comparative Example 6] A silicone rubber composition was prepared and a cured product was obtained by repeating Example 2, except that 0.8 parts by mass of titanium oxide doped with 3% by mass of iron oxide (Fe2O3) (AEROXIDE TiO2PF2, manufactured by Nippon Aerosil Co., Ltd.) was used instead of the yellow iron oxide. The cured product was subjected to the heat resistance test described above.

[0050] [Table 1]

[0051] [Table 2]

[0052] As shown in Table 1 above, and as shown in Comparative Examples 3 and 5, silicone rubber with excellent heat resistance at 300°C cannot be obtained with a composition containing only yellow iron oxide and either cerium oxide or cerium hydroxide. In addition, as shown in Comparative Example 2, the use of red iron oxide in combination with cerium oxide cannot improve heat resistance at 300°C. In addition, even with a composition containing yellow iron oxide and cerium oxide, the addition reaction type silicone rubber composition has poor heat resistance at 300°C and deteriorated mechanical properties (Comparative Example 1). In addition, the mechanical properties of silicone rubber obtained from a silicone rubber composition containing titanium oxide doped with iron oxide and cerium oxide change significantly after storage at 220°C for 7 days and at 300°C for 7 days, and the silicone rubber has poor long-term high-temperature heat resistance (Comparative Example 6). In contrast, the silicone rubber (cured product) obtained from the silicone rubber composition of the present invention has excellent heat resistance and can maintain good mechanical properties even under high-temperature long-term storage at 300°C for 7 days, and can suppress an increase in the hardness of the silicone rubber.

Claims

1. A millable silicone rubber composition comprising the following components (A) to (F): (A) A polymer having two or more alkenyl groups bonded to silicon atoms in one molecule and a main chain of R 1 2 SiO 2/2 The diorganosiloxane unit is represented by the following formula: 1 3 SiO 1/2 100 parts by mass of a linear diorganopolysiloxane having an average degree of polymerization of 1,000 or more and terminated with a triorganosiloxy group represented by the formula: (In the above formula, R 1 are each independently an unsubstituted group selected from an alkyl group, a cycloalkyl group, an alkenyl group, an aryl group, and an aralkyl group having 1 to 20 carbon atoms. (B) Specific surface area 50m 2 / g or more, 5 to 100 parts by mass of reinforcing silica, (C) yellow iron oxide 0.01 to 10 parts by mass, (D) 0.01 to 10 parts by mass of cerium oxide, (E) 0.1 to 10 parts by mass of an organic peroxide, and (F) Silica dispersant 0.1 to 50 parts by mass and However, the millable type silicone rubber composition does not contain titanium oxide doped with a transition metal oxide, and does not contain an epoxy resin.

2. 2. The millable type silicone rubber composition according to claim 1, wherein said component (A) has an average degree of polymerization of 1,000 to 100,000.

3. 3. The millable silicone rubber composition according to claim 1, wherein the amount of component (C) is 0.01 to 5% by mass based on the total mass of the composition.

4. 4. The millable silicone rubber composition according to claim 1, wherein component (F) is a low molecular weight organosilicon compound having an alkoxy group or a silanol group, or a hydrolyzate thereof.

5. A cured product of the millable type silicone rubber composition according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Antibacterial and high-flame-retardant cable

    CN105741947A

  • Thermally stable fluorosilicone rubber composition

    JP1993186699A

  • Curable organopolysiloxane composition

    JP1995292256A

  • Silicone rubber composition

    JP2000212444A

  • Method for producing metal doped titanium oxide particulate