Ultra-high molecular weight propylene (co)polymer

Optimizing polymerization catalysts and conditions produces ultra-high molecular weight propylene polymers with high intrinsic viscosity, addressing the lack of such polymers in existing technologies, and enhancing their suitability for extrusion molded products and organic fillers.

JP7580375B2Active Publication Date: 2024-11-11SUNALLOMER LTD +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021528173
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-17
Filing Date
2020-06-12
Publication Date
2024-11-11
Estimated Expiration
2040-06-12

AI Technical Summary

Technical Problem

Existing technologies have not reported ultra-high molecular weight propylene polymers with intrinsic viscosity exceeding 20 dl/g when measured using tetralin as a solvent.

Method used

The production of ultra-high molecular weight propylene polymers is achieved by optimizing polymerization catalysts and conditions, specifically using a catalyst containing magnesium, titanium, halogen, and an electron donor compound, along with an organoaluminum compound, to produce propylene homopolymers or copolymers with intrinsic viscosities over 20 dl/g in tetralin, and adjusting ethylene content and melting point through a specific formula.

Benefits of technology

The resulting propylene polymers exhibit high molecular weight, excellent foamability, and improved melt tension, with enhanced crystallinity and powder fluidity, making them suitable for extrusion molded products and organic fillers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580375000001
    Figure 0007580375000001
  • Figure 0007580375000002
    Figure 0007580375000002
  • Figure 0007580375000003
    Figure 0007580375000003
Patent Text Reader

Abstract

Provided are: a propylene homopolymer; or a copolymer composed of propylene and at most 30 wt% of α-olefin having 2 or 4 to 8 carbon atoms, the homopolymer or the copolymer having an intrinsic viscosity of more than 20 dl / g as measured in a tetralin solvent at 135°C.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to ultra-high molecular weight propylene (co)polymers. [Background technology]

[0002] High molecular weight propylene polymers are particularly useful as resin components for extrusion molded products (general sheets, foam sheets, blow molded products, etc.), and various studies have been conducted on the production of high molecular weight propylene polymers. For example, Patent Document 1 discloses a crosslinked ultra-high molecular weight olefin polymer having an intrinsic viscosity [η] of 5 to 50 dl / g measured in a decalin solvent at 135°C. However, the olefin polymer specifically disclosed in the examples is only polyethylene. Patent Document 2 discloses an ultra-high molecular weight propylene homopolymer having an intrinsic viscosity [η] of 7 dl / g or more and less than 25 dl / g measured using a decalin solution. The examples of this document disclose a propylene polymer having [η] of 20.2 dl / g. Patent Document 3 discloses an ultra-high molecular weight polypropylene having an intrinsic viscosity [η] of at least 5 dl / g measured using a decalin solution. The examples of this document disclose a polypropylene having [η] of 20.25 dl / g. Patent Document 4 discloses polypropylene having an intrinsic viscosity [η] of 5 to 20 dl / g measured in a tetrahydronaphthalene (tetralin) solvent at 135° C. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 5979985 [Patent Document 2] Patent No. 5653761 [Patent Document 3] Patent No. 3023382 [Patent Document 4] Patent No. 6144045 Summary of the Invention [Problem to be solved by the invention]

[0004] Patent Document 1 does not specifically disclose a propylene polymer with a high [η]. Patent Documents 2 and 3 disclose a propylene polymer with an [η] of about 20 dl / g, but the viscosity is a value measured using decalin as a solvent. It is obvious to those skilled in the art that the value of [η] measured using decalin as a solvent is lower when converted to a value measured using tetralin as a solvent. Therefore, when the [η] described in Patent Documents 2 and 3 is converted to a value measured using tetralin as a solvent, it is less than 20 dl / g. From the above, no ultra-high molecular weight propylene polymer with an [η] measured using tetralin as a solvent exceeding 20 dl / g has been reported so far. In view of such circumstances, an object of the present invention is to provide an ultra-high molecular weight propylene polymer. [Means for solving the problem]

[0005] The inventors have found that the ultra-high molecular weight polypropylene polymer can be produced by optimizing the polymerization catalyst and polymerization conditions, and have completed the present invention. [1] A propylene homopolymer or a copolymer of propylene and 30% by weight or less of an α-olefin having 2 or 4 to 8 carbon atoms, having an intrinsic viscosity of more than 20 dl / g measured in tetralin solvent at 135°C. [2] The copolymer according to [1], wherein the α-olefin is ethylene. [3] The copolymer according to [2], wherein the intrinsic viscosity is 23 dl / g or more and the ethylene content is 3 to 30% by weight. [4] The melting point Tm (°C) of the copolymer measured at a heating rate of 10°C / min using DSC and the ethylene content C2 (wt%) in the copolymer satisfy the following formula (1); Tm ≧ -3.4×C2 + 162 …(1) The copolymer according to [2] or [3]. [5] (A) a solid catalyst comprising magnesium, titanium, a halogen, and an electron donor compound as essential components; (B) an organoaluminum compound, and A method for producing the polymer according to any one of [1] to [4], comprising preparing the polymer by polymerizing a corresponding monomer using a catalyst optionally containing (C) an external electron donor compound. [6] A composition comprising the polymer according to any one of [1] to [4] above, A polypropylene resin composition, the content of the polymer being 0.1 to 20% by weight based on the total weight of resin components constituting the composition. Effect of the Invention

[0006] The present invention provides an ultra-high molecular weight propylene polymer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] The present invention will be described in detail below. In the present invention, "X to Y" includes the extreme values ​​X and Y.

[0008] 1. Propylene (co)polymer (1) Intrinsic viscosity The propylene homopolymer or copolymer of propylene and 30% by weight or less of an α-olefin having 2 or 4 to 8 carbon atoms (hereinafter collectively referred to as "propylene (co)polymer") of the present invention has an intrinsic viscosity of more than 20 dl / g measured in a tetralin solvent at 135°C. The intrinsic viscosity is an index of molecular weight, and the propylene (co)polymer of the present invention has an extremely high molecular weight that has not been achieved in the past. A resin composition containing the propylene (co)polymer having a high intrinsic viscosity also has a high melt tension, and therefore gives, for example, an excellent foam. From this viewpoint, the lower limit of the intrinsic viscosity is preferably 23 dl / g or more. Also, from the viewpoint of ease of production, the upper limit of the intrinsic viscosity is preferably 50 dl / g or less.

[0009] (2) Amount of comonomer When the propylene (co)polymer of the present invention is a copolymer, the amount of the comonomer is 30% by weight or less. If the amount of the comonomer exceeds this value, the crystallinity of the copolymer decreases and the powder properties of the polymer deteriorate, making production difficult. From this viewpoint, the upper limit of the amount is preferably 25% by weight or less. On the other hand, the lower limit of the amount of the comonomer is not limited, and is preferably 3% by weight or more, more preferably 5% by weight or more. The amount of the comonomer is the amount of units derived from the monomer in the copolymer. The comonomer is an α-olefin having 2 or 4 to 8 carbon atoms. Among these, from the viewpoint of reactivity, the α-olefin having 2 carbon atoms, that is, ethylene, is preferable as the comonomer. The intrinsic viscosity of the propylene polymer can be further increased by copolymerizing ethylene. Thus, in one aspect, the propylene (co)polymer of the present invention is a copolymer having the intrinsic viscosity of 23 dl / g or more and an ethylene content (content ratio of ethylene-derived units) of 3 to 30% by weight.

[0010] (3)XI The propylene (co)polymer of the present invention has a xylene insoluble matter (XI) of preferably 40% by weight or more, more preferably 50% by weight or more, further preferably 60% by weight or more, particularly preferably 70% by weight or more. XI is a crystalline component in the propylene (co)polymer. The upper limit of XI is not particularly limited.

[0011] (4) Melting point The propylene (co)polymer of the present invention has a melting point (Tm) of preferably 100°C or higher, more preferably 120°C or higher, even more preferably 140°C or higher, and particularly preferably 150°C or higher. The melting point is the temperature at which the heat of fusion associated with melting observed by second scanning using DSC shows a maximum value. The second scan refers to a thermal analysis in which a sample (resin) is heated and melted, cooled to crystallize, held at room temperature for 5 minutes, and then heated a second time. Specifically, the sample is heated to a melting temperature or higher (230°C), held at that temperature for 5 minutes, cooled to 30°C at a temperature drop rate of 10°C / min, held for 5 minutes, and then heated to 230°C at a temperature rise rate of 10°C / min to perform thermal analysis.

[0012] The propylene copolymer of the present invention has a feature that it has a higher melting point than conventional copolymers when the type and content of the comonomer are the same. In particular, when the propylene copolymer of the present invention is a propylene-ethylene copolymer, it is preferable that the Tm (°C) and the ethylene content C2 (wt%) in the copolymer satisfy the formula (1). Equation (1): Tm ≧ -3.4×C2 + 162

[0013] (5) Properties etc. From the viewpoint of handling, the propylene (co)polymer of the present invention is preferably a powder. And the powder has more preferably a powder fluidity of 3.5 or less. Powder fluidity is the fluidity of the powder polymer produced in the polymerization reactor, and is an index of the production stability of the polymer. Specifically, the powder fluidity is a value that quantifies the ease of flow of the powder when a constant load is applied to the powder placed on a substrate at a constant temperature for a constant time, the load is removed, and the powder is made to flow by tilting the substrate, etc. The lower the powder fluidity value, the better the powder fluidity and the better the production stability. The powder fluidity of the propylene (co)polymer of the present invention is preferably 3.5 or less, more preferably 3.0 or less, and even more preferably 2.0 or less.

[0014] The powder flowability is measured by the following method. A frame with an opening measuring 5 cm long x 5 cm wide x 1 cm high is placed on the metal substrate (first substrate), and 5 g of a polymer sample is spread inside the frame. The pressure applied to the sample is uniformly 23 g / cm 2 The second substrate is placed on the frame so that the sample is in the shape of a square. After the sample in the frame is held at 70°C for 20 minutes, the frame and the second substrate are removed, and the first substrate on which the sample is placed is tilted to evaluate the degree of collapse of the sample according to the following criteria. 1. If tilted between 0° and 30°, the entire container will collapse. 2. If tilted at an angle between 30° and 50°, the entire container will collapse. 3. If tilted more than 50° but less than 70°, the entire contents will fall off. 4. If you tilt it more than 70 degrees but less than 90 degrees, the whole thing will fall apart. 5. Even if tilted over 90 degrees, the entire contents will not fall off The first and second substrates are preferably made of stainless steel from the viewpoints of heat transfer and rust resistance during repeated use. In addition, the first substrate preferably has a surface roughness (maximum roughness Ry) of 1 μm or less to eliminate the influence of friction with the powder.

[0015] 2. Manufacturing method The propylene (co)polymer of the present invention is preferably produced using a catalyst containing (A) a solid catalyst containing magnesium, titanium, a halogen, and an electron donor compound as essential components, (B) an organoaluminum compound, and, if necessary, (C) an external electron donor compound.

[0016] (1) Solid catalyst (component (A)) Component (A) can be prepared by a known method, for example, by contacting a magnesium compound, a titanium compound, and an electron donor compound with each other. The titanium compound used in the preparation of component (A) is represented by the general formula: Ti(OR) g X 4-g In the formula, R is a hydrocarbon group, X is a halogen, and 0≦g≦4. More specifically, the titanium compound is TiCl 4 , TiBr 4 , TiI 4 Titanium tetrahalides such as Ti(OCH 3 )Cl 3 , Ti(OC 2 H 5 )Cl 3 , Ti(O n -C 4 H 9 )Cl 3 , Ti(OC 2 H 5 )Br 3 , Ti(OisoC 4 H 9 )Br 3 Alkoxy titanium trihalides such as Ti(OCH 3 ) 2 Cl 2 , Ti(OC 2 H 5 )2 Cl 2 , Ti(O n -C 4 H 9 ) 2 Cl 2 , Ti(OC 2 H 5 ) 2 Br 2 Alkoxy titanium dihalides such as Ti(OCH 3 ) 3 Cl, Ti(OC 2 H 5 ) 3 Cl, Ti(O n -C 4 H 9 ) 3 Cl, Ti(OC 2 H 5 ) 3 Monohalogenated trialkoxy titanium such as Br; Ti(OCH 3 ) 4 , Ti(OC 2 H 5 ) 4 , Ti(O n -C 4 H 9 ) 4 Among these, preferred are halogen-containing titanium compounds, particularly titanium tetrahalides, and particularly preferred is titanium tetrachloride.

[0017] Examples of the magnesium compound include magnesium compounds having a magnesium-carbon bond or a magnesium-hydrogen bond, such as dimethylmagnesium, diethylmagnesium, dipropylmagnesium, dibutylmagnesium, diamylmagnesium, dihexylmagnesium, didecylmagnesium, ethylmagnesium chloride, propylmagnesium chloride, butylmagnesium chloride, hexylmagnesium chloride, amylmagnesium chloride, butylethoxymagnesium, ethylbutylmagnesium, butylmagnesium hydride, etc. These magnesium compounds can be used in the form of a complex compound with, for example, organoaluminum, etc., and may be in either liquid or solid form. Further preferred magnesium compounds include magnesium halides such as magnesium chloride, magnesium bromide, magnesium iodide, and magnesium fluoride; alkoxymagnesium halides such as methoxymagnesium chloride, ethoxymagnesium chloride, isopropoxymagnesium chloride, butoxymagnesium chloride, and octoxymagnesium chloride; aryloxymagnesium halides such as phenoxymagnesium chloride and methylphenoxymagnesium chloride; alkoxymagnesium such as ethoxymagnesium, isopropoxymagnesium, butoxymagnesium, n-octoxymagnesium, and 2-ethylhexoxymagnesium; dialkoxymagnesium such as dimethoxymagnesium, diethoxymagnesium, dipropoxymagnesium, dibutoxymagnesium, ethoxymethoxymagnesium, ethoxypropoxymagnesium, and butoxyethoxymagnesium; and aryloxymagnesium such as phenoxymagnesium and dimethylphenoxymagnesium.

[0018] The electron donor compound is generally called an “internal electron donor compound.” In the present invention, the internal electron donor compound is preferably a compound having an ester skeleton represented by formula (I).

[0019] [ka]

[0020] In the formula, R1 is independently a hydrogen atom or a hydrocarbon group having 1 to 15 carbon atoms. The hydrocarbon group may have a heteroatom such as halogen, P, S, N, O, or Si, and may form a ring. R2 is defined in the same way as R1, but R2 and R1 do not have to have the same structure. Furthermore, R1 and R2 may be linked to form a ring.

[0021] A is a divalent bridging group. The chain length between the bridging bonds is preferably 1 to 10 atoms. When A has a cyclic structure, the chain length refers to the number of atoms in the shortest sequence between the oxygen atoms to which A is bonded. A is preferably -(ZR 3 m ) n Z is preferably C, Si, Ge, O, N, S or P. 3 are each independently hydrogen or a hydrocarbon group having 1 to 20 carbon atoms, and may contain the heteroatom. 3 may be fused to form one or more rings. m is a number corresponding to the valence of Z, and n is an integer from 1 to 10. For example, R 3 can form an aromatic ring, a heterocyclic ring, or an alicyclic ring together with Z. -(ZR 3 m ) n When - includes O, S, and N, they are not directly attached to the oxygen atom of formula (I).

[0022] In the present invention, it is more preferable to use a carbamate compound as the internal electron donor compound. The carbamate compound is a compound having a carbamic acid ester skeleton and is represented by the formula (II). [ka]

[0023] In the formula, R4 is independently a hydrogen atom or a hydrocarbon group having 1 to 15 carbon atoms. The hydrocarbon group may have a heteroatom such as halogen, P, S, N, O, or Si, and two R4 may be linked to form a ring. R5 is defined in the same way as R4, but R4 and R5 do not have to have the same structure.

[0024] A is defined as above, and Z is preferably C or Si, more preferably C. In particular, compounds having the following combinations are preferred: A: a divalent aromatic group which may have a substituent. Examples of the aromatic group include a phenylene group and a naphthylene group. Examples of the substituent include a linear or branched alkyl group having 1 to 5 carbon atoms, such as a methyl group, an ethyl group, a propyl group, a butyl group, and a pentyl group. R4 and R5: a linear or branched alkyl group having 1 to 5 carbon atoms, such as a methyl group, an ethyl group, a propyl group, a butyl group, or a pentyl group. Specifically, the compound defined by formula (II) may be one described in US Patent Application Publication No. 2015 / 0266981.

[0025] (2) Organoaluminum compounds (component (B)) The organoaluminum compounds include the following: Trialkylaluminum such as triethylaluminum and tributylaluminum; Trikenylaluminum such as triisoprenylaluminum: Dialkylaluminum alkoxides such as diethylaluminum ethoxide and dibutylaluminum butoxide; Alkyl aluminum sesquialkoxides such as ethyl aluminum sesquiethoxide, butyl aluminum sesquibutoxide;

[0026] Partially halogenated alkylaluminums such as ethylaluminum dichloride, propylaluminum dichloride, butylaluminum dibromide, diethylaluminum chloride, dipropylaluminum chloride, dibutylaluminum chloride, etc.; Dialkylaluminum hydrides such as diethylaluminum hydride and dibutylaluminum hydride; partially hydrogenated alkylaluminums such as alkylaluminum dihydrides such as ethylaluminum dihydride and propylaluminum dihydride; Partially alkoxylated and halogenated alkylaluminums such as ethylaluminum ethoxychloride, butylaluminum butoxychloride, and ethylaluminum ethoxybromide.

[0027] (3) Electron donor compound (component (C)) The electron donor compound is also called an “external electron donor compound.” As the external electron donor compound, an organosilicon compound is preferable, and specific examples thereof include the following compounds. Trimethylmethoxysilane, trimethylethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, diisopropyldimethoxysilane, t-butylmethyldimethoxysilane, t-butylmethyldiethoxysilane, t-amylmethyldiethoxysilane, diphenyldimethoxysilane, phenylmethyldimethoxysilane, diphenyldiethoxysilane, bis-o-tolyldimethoxysilane, bis-m-tolyldimethoxysilane, bis-p-tolyldimethoxysilane, bis-p-tolyldiethoxysilane, bis-ethylphenyldimethoxysilane, dicyclopentyldimethoxysilane, dicyclohexyldimethoxysilane, cyclohexylmethyldimethoxysilane, cyclohexylmethyldiethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, vinyltrimethoxysilane, methyltrimethoxysilane, n-propyltriethoxysilane, decyltrimethoxysilane, decyltriethoxy Silane, phenyltrimethoxysilane, gamma-chloropropyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, vinyltriethoxysilane, t-butyltriethoxysilane, thexyltrimethoxysilane, n-butyltriethoxysilane, iso-butyltriethoxysilane, phenyltriethoxysilane, gamma-aminopropyltriethoxysilane, chlorotriethoxysilane, ethyltriisopropoxysilane, vinyltributoxysilane, cyclohexyltrimethoxysilane, cyclohexyltriethoxysilane, 2-norbornanetrimethoxysilane, 2-norbornanetriethoxysilane, 2-norbornanemethyldimethoxysilane, ethyl silicate, butyl silicate, trimethylphenoxysilane, methyltriallyloxysilane, vinyltris(β-methoxyethoxysilane), vinyltriacetoxysilane, dimethyltetraethoxydisiloxane, methyl(3,3,3-trifluoro-n-propyl)dimethoxysilane, cyclohexylethyldimethoxysilane, cyclopentyl-t-butoxydimethoxysilane, diisobutyldimethoxysilane, isobutylisopropyldimethoxysilane, n-propyltrimethoxysilane, di-n-propyldimethoxysilane, thexyltrimethoxysilane, t-butylethyldimethoxysilane, t-butylpropyldimethoxysilane, t-butyl-t-butoxydimethoxysilane, isobutyltrimethoxysilane, cyclohexylisobutyldimethoxysilane, di-sec-butyldimethoxysilane, isobutylmethyldimethoxysilane, bis(decahydroisoquinolin-2-yl)dimethoxysilane, diethylaminotriethoxysilane, dicyclopentyl-bis(ethylamino)silane, tetraethoxysilane, tetramethoxysilane, isobutyltriethoxysilane.,

[0028] (4) Composition ratio The composition ratio of components (A) to (C) is not limited, but the composition ratio of components (A) and (B) is adjusted so that the Al / Ti molar ratio is preferably 10 to 1000, more preferably 30 to 600. When component (C) contains silicon, the composition ratio of components (A) and (C) is adjusted so that the Si / Al molar ratio is preferably 0.01 to 1.5, more preferably 0.05 to 1.0.

[0029] (5) Polymerization The raw material monomer is polymerized by contacting it with the catalyst prepared as described above. At this time, prepolymerization may be performed using the catalyst. Prepolymerization is a process in which a polymer chain that serves as a foothold for the subsequent main polymerization of the raw material monomer is formed on a solid catalyst component. Prepolymerization can be performed by a known method. Prepolymerization is usually performed at 40°C or less, preferably 30°C or less, and more preferably 20°C or less. Then, the prepolymerized catalyst (prepolymerization catalyst) is introduced into a polymerization reaction system to perform the main polymerization of the raw material monomer. Polymerization may be performed in a liquid phase, a gas phase, or a liquid-gas phase. The polymerization temperature is preferably 0 to 90°C, more preferably 20 to 80°C. The polymerization pressure is preferably in the range of 0.8 to 6.0 MPa when performed in a liquid phase, and preferably in the range of 0.5 to 3.0 MPa when performed in a gas phase. In the present invention, a chain transfer agent (for example, hydrogen or ZnEt 2 A trace amount of a conventional molecular weight regulator known in the art, such as dimethylaminopropylamine, ...

[0030] A polymerization vessel having a gradient of monomer concentration or polymerization conditions may also be used. In such a polymerization vessel, for example, one having at least two polymerization zones connected thereto is used, and a monomer can be polymerized by gas phase polymerization. Specifically, in the presence of a catalyst, a monomer is supplied and polymerized in a polymerization zone consisting of an uprising tube, and a monomer is supplied and polymerized in a downcomer connected to the uprising tube, and a polymer product is recovered while circulating between the uprising tube and the downcomer. This method includes a means for completely or partially preventing the gas mixture present in the uprising tube from entering the downcomer. Also, a gas or liquid mixture having a composition different from that of the gas mixture present in the uprising tube is introduced into the downcomer. As the above polymerization method, for example, the method described in JP-A-2002-520426 can be applied.

[0031] 3.Applications Since the propylene (co)polymer of the present invention has an extremely high molecular weight, a composition containing this polymer has high melt tension and die swell. Therefore, the propylene (co)polymer of the present invention is useful for applications of extrusion molded products (general sheets, foam sheets, blow molded products, etc.) and injection molded products. In addition, the propylene (co)polymer of the present invention has a characteristic of being crystalline and difficult to melt, so it is also useful as an organic filler. Therefore, the propylene (co)polymer of the present invention can be used alone, but can also be used as an additive or additional component in combination with other resins to form a composition. The addition method can be a known method such as melt kneading, solution blending, or polymerization blending by multi-stage polymerization. Furthermore, the composition can be used as a master batch and combined with other polyolefins to form a secondary composition.

[0032] When a composition containing a small amount of the propylene (co)polymer of the present invention is obtained by polymerization blending, the propylene (co)polymer of the present invention may be polymerized in a prepolymerization stage. The content of the propylene (co)polymer of the present invention in the composition is preferably 0.1% by weight or more, more preferably 0.5% by weight or more, and even more preferably 1% by weight or more, based on the total weight of the resin components constituting the composition. The upper limit is preferably 20% by weight or less, more preferably 15% by weight or less, and even more preferably 10% by weight or less. If the content is less than 0.1% by weight, it is difficult to obtain the expected moldability and physical properties, and if it exceeds 20% by weight, the flowability of the composition may decrease. EXAMPLES

[0033] [Example 1] In a nitrogen-purged 300 mL four-neck round-bottom flask, 45 mL of toluene and 10.0 g of finely divided spherical Mg(OC 2 H 5 ) 2was introduced at 5°C. 28.7 ml of titanium tetrachloride was added dropwise over 10 minutes while stirring, and 11.3 mmol of 5(tertiarybutyl)-3-methyl-1,2-phenylenebis(diethylcarbamate) (hereinafter also referred to as compound a) was added. The temperature was raised to 110°C and maintained for 120 minutes. Then, stirring was stopped, the solid product was allowed to settle, and the supernatant liquid was siphoned off. It was then washed four times with toluene (75 mL) at 90°C.

[0034] 50 ml of toluene was added to the washed solid. 21 ml of titanium tetrachloride was added thereto, and the temperature was raised to 100°C and stirred for 90 minutes. Stirring was then stopped, the solid product was allowed to settle, and the supernatant liquid was sucked out. Next, the solid was washed six times with heptane (75 mL) at 40°C. The washed solid was dried under reduced pressure to obtain 7.6 g of solid catalyst component (A). The solid catalyst component contained 14.3 wt% of compound a, 14.0 wt% of Mg, and 4.0 wt% of Ti.

[0035] The inside of a 20L autoclave reactor equipped with a stirrer was thoroughly vacuum dried and replaced with nitrogen. 52.8 mg of the prepared solid catalyst, triethylaluminum (TEAL), and dicyclopentyldimethoxysilane (DCPMS) were added to the reactor in amounts such that the Al / Ti molar ratio was 150 and the Si / Al molar ratio was 0.2. Then, 5.6 kg of propylene was added, the temperature of the autoclave was raised to 40°C, and polymerization was carried out at 40°C for 30 minutes. After the polymerization reaction was completed, unreacted monomers were discharged, and 75 g of propylene homopolymer was obtained and evaluated. The results are shown in Table 1.

[0036] [Examples 2 and 3] Polymerization was carried out in the same manner as in Example 1, except that the Al / Ti molar ratio and the Si / Al molar ratio were changed, and a propylene homopolymer was obtained and evaluated. The results are shown in Table 1. The Al / Ti molar ratio was changed by adjusting the amount of TEAL used. In the following cases where the Al / Ti molar ratio was changed, the same procedure was followed.

[0037] [Example 4] Except for using triisobutylaluminum (TIBAL) instead of TEAL, polymerization was carried out in the same manner as in Example 1 to obtain a propylene homopolymer, which was then evaluated. The results are shown in Table 1.

[0038] [Examples 5 to 6] Except for changing the polymerization temperature and the Si / Al molar ratio, polymerization was carried out in the same manner as in Example 1, and an actual propylene homopolymer was obtained and evaluated. The results are shown in Table 1.

[0039] [Example 7] A propylene-ethylene copolymer was obtained and evaluated in the same manner as in Example 1, except that 5 kg of propylene was added to the reactor, ethylene gas was continuously supplied during the polymerization to adjust the ethylene partial pressure to a constant value, and the polymerization was carried out for 30 minutes at 40° C. The results are shown in Table 1.

[0040] [Examples 8 to 12] Polymerization was carried out in the same manner as in Example 7, except that the Al / Ti molar ratio and the Si / Al molar ratio were changed and the ethylene partial pressure was adjusted so that the ethylene content in the polymer had the value shown in Table 1, and a propylene-ethylene copolymer was obtained and evaluated. The results are shown in Table 1.

[0041] [Example 13] Except for using diisopropyldimethoxysilane (DIPMS) as an external electron donor compound and adjusting the ethylene partial pressure, polymerization was carried out in the same manner as in Example 10 to obtain a propylene-ethylene copolymer, which was then evaluated. The results are shown in Table 1.

[0042] [Example 14] The polymerization was carried out in the same manner as in Example 13, except that no external electron donor compound was used and the ethylene partial pressure was adjusted for polymerization, and a propylene-ethylene copolymer was obtained and evaluated. The results are shown in Table 1. [Example 15] Polymerization was carried out in the same manner as in Example 10, except that the polymerization temperature was set to 70° C. and the ethylene partial pressure was adjusted, to obtain a propylene-ethylene copolymer, which was then evaluated. The results are shown in Table 1. [Example 16] Polymerization was carried out in the same manner as in Example 10, except that 100 cc of hydrogen was introduced into the reactor as a chain transfer agent and the ethylene partial pressure was adjusted, to obtain a propylene-ethylene copolymer, which was then evaluated. The results are shown in Table 1.

[0043] [Comparative Example 1] A solid catalyst component was prepared according to the method described in Example 1 of EP 674991. The solid catalyst was MgCl 2 TiCl on top 4 (Titanium tetrachloride) was supported with diisobutyl phthalate as an internal electron donor by the method described in the above patent publication. Except for using this solid catalyst, polymerization was carried out in the same manner as in Example 5 to obtain a propylene homopolymer, which was then evaluated. The results are shown in Table 2.

[0044] [Comparative Example 2] The solid catalyst prepared in Comparative Example 1, TEAL and DCPMS were added to the reactor in such amounts that the Al / Ti molar ratio was 150 and the Si / Al molar ratio was 0.15. As in Example 16, 900 cc of hydrogen was introduced into the reactor, and ethylene was continuously supplied during the polymerization to adjust the ethylene partial pressure to a constant value. The polymerization temperature was 70°C, and the polymerization time was 60 minutes, and a propylene-ethylene copolymer was obtained and evaluated. The results are shown in Table 2.

[0045] [Comparative Example 3] A solid catalyst component was prepared as follows, with reference to the method described in the Examples of JP 2011-500907 A. Into a 500 mL four-neck round-bottom flask purged with nitrogen, 250 mL of titanium tetrachloride was introduced at 0° C. With stirring, 10.0 g of finely divided MgCl 2 1.8C 2 H 5 OH and 9.1 mmol of diethyl-2,3-(diisopropyl)succinate were added. 2 1.8C 2 H 5OH was prepared according to the method described in Example 2 of US Pat. No. 4,399,054, except that the rotation speed was changed from 10,000 rpm to 3,000 rpm.

[0046] The temperature in the flask was raised to 100° C. and maintained for 120 minutes. Then, stirring was stopped, the solid product was allowed to settle, and the supernatant liquid was siphoned off. The following procedure was then repeated twice. 250 mL of fresh titanium tetrachloride was added, the mixture was reacted for 60 minutes at 120° C., and the supernatant liquid was siphoned off. The solid was washed six times with anhydrous hexane (6×100 mL) at 60° C.

[0047] Except for using the above solid catalyst, polymerization was carried out under the same conditions as in Example 5 to obtain a propylene homopolymer. The results are shown in Table 2.

[0048] [Comparative Example 4] A propylene-ethylene copolymer was obtained and evaluated in the same manner as in Example 10, except that the catalyst prepared in Comparative Example 3 was used and the ethylene partial pressure was adjusted so that the ethylene content in the polymer had the value shown in Table 2. The results are shown in Table 2.

[0049] [Comparative Examples 5 to 8] Polymerization was carried out in the same manner as in Example 1, except that the polymerization conditions were changed as shown in Table 2, to obtain and evaluate a propylene homopolymer. The results are shown in Table 2.

[0050] [Comparative Example 9] A 6L autoclave equipped with a stirrer was thoroughly vacuum dried and purged with nitrogen. 97.8mg of titanium trichloride catalyst (manufactured by Tosoh Finechem Co., Ltd.) was added as a catalyst, and diethylaluminum chloride (DEAC) was added as an organoaluminum compound in an amount such that the Al / Ti molar ratio was 13. Then, 1.5kg of propylene was added, the temperature of the autoclave was raised to 60°C, and polymerization was carried out at 60°C for 30 minutes. After the polymerization reaction was completed, the unreacted monomer was purged, 250ml of isobutyl alcohol was added, and deashing treatment was carried out at 80°C for 1 hour. Then, the solid components were allowed to settle, and the supernatant liquid was sucked out. Then, the mixture was washed twice with heptane (300mL) at 80°C, and 73g of propylene homopolymer was obtained and evaluated. The results are shown in Table 2.

[0051] [Comparative Example 10] Polymerization was carried out in the same manner as in Comparative Example 9, except that the polymerization temperature was changed to 40° C., and a propylene homopolymer was obtained and evaluated. The results are shown in Table 2.

[0052] [Table 1-1] [Table 1-2]

[0053] [Table 2]

[0054] [Example 17] 1) Polypropylene resin composition Using the solid catalyst containing the compound a prepared in Example 1, polymerization was carried out as follows.

[0055] [Pre-stage polymerization] The inside of a 20L autoclave reactor equipped with a stirrer was thoroughly vacuum dried and replaced with nitrogen. 59.3 mg of the prepared solid catalyst component containing compound a, TEAL, and DCPMS were added in amounts such that the Al / Ti molar ratio was 150 and the Si / Al molar ratio was 1.0. Next, 5.6 kg of liquefied propylene was added to the reactor, and ethylene gas was continuously supplied during the polymerization to adjust the ethylene partial pressure to a constant level, and polymerization was carried out at 40°C for 10 minutes. The polymerization pressure was adjusted to obtain the propylene-ethylene copolymer of the present invention. Thereafter, unreacted monomers were purged, and the inside of the reactor was thoroughly replaced with nitrogen.

[0056] [Second-stage polymerization] Next, TEAL and DCPMS were added to the reactor in amounts such that the Al / Ti molar ratio was 400 and the Si / Al molar ratio was 0.05. 5.6 kg of liquefied propylene and hydrogen gas were added so that the hydrogen concentration in the liquid propylene was 0.7 mol%, and the temperature of the autoclave was raised to 70°C, and polymerization (polymerization of propylene) was carried out for 180 minutes. After the polymerization reaction was completed, unreacted monomers were purged to obtain 4.6 kg of a powdery composition. This composition was obtained by polymerizing and blending the propylene-ethylene copolymer of the present invention and polypropylene. The physical properties of this composition are shown in Table 3. However, the intrinsic viscosity, the content ratio of ethylene-derived units, and the melting point of the propylene-ethylene copolymer of the present invention are the results of analyzing the polymer obtained by carrying out only the first-stage polymerization under the same conditions. The ratio of the propylene-ethylene copolymer of the present invention in the composition was determined by the activity ratio with the first-stage polymerization.

[0057] To the composition obtained above, 0.2 phr of BASF B225 as an antioxidant and 0.1 phr of calcium stearate as a neutralizer made by Dannan Chemical Industry Co., Ltd. were added, and the mixture was obtained by stirring for 1 minute with a Henschel mixer. The mixture was then melt-kneaded using an extruder (manufactured by Technovel Co., Ltd., screw diameter 15 mm, same-rotation twin-screw extruder) with the screw temperature set to 230°C. The molten mixture was then discharged from the extruder, cooled to form strands, and the strands were cut to obtain a pellet-shaped polypropylene resin composition.

[0058] 2) Formation of foam To the polypropylene resin composition obtained as described above, 4 phr of Cellmic MB3064 manufactured by Sankyo Kasei Co., Ltd. was added as a foaming agent, and the mixture was dry-blended to obtain a foamable composition. Then, the foamable composition was used to form a foamed strand under the following conditions, and the obtained foam was evaluated. Extruder: Thermo Plastics Industry Co., Ltd. single screw extruder TP-15 Die shape: Strand die Tie part dimensions: 2mmφ Output: 500g / h Screw shape: Full flight screw Screw rotation speed: 40 rpm Cylinder temperature setting: 210℃ Die section temperature setting: 180℃

[0059] Similarly, 6 phr of Cellmike MB3064 manufactured by Sankyo Kasei Co., Ltd. was added as a foaming agent to the polypropylene resin composition obtained in 1) and dry-blended to obtain a foamable composition. The foamable composition was used to obtain a foam and evaluate it as described above.

[0060] Similarly, the polypropylene resin composition obtained in 1) was subjected to heat press molding at a temperature of 230° C. to obtain a non-foamable sheet (thickness: 500 μm). This was cut into test pieces, and the stiffness was measured. The results are shown in Table 3.

[0061] [Table 3]

[0062] The evaluation was carried out as follows. [Content of ethylene-derived units] A propylene (co)polymer sample was heat-pressed at 230 °C to produce a sheet with a thickness of 0.4 mm. The IR absorption spectrum of the sample versus air background was collected by Fourier transform infrared spectroscopy (FT-IR). The absorption spectrum was measured from 760 cm to 690 cm after correcting for the thickness of the sheet. -1 The content (wt%) of the ethylene-derived unit in the propylene (co)polymer was calculated using the peak area. The data collection parameters were as follows: Apodization: Cosine Resolution: 2cm -1

[0063] [Polymer XI] 0.1-0.5 g of polymer was dissolved in 250 mL of xylene at 135° C. with stirring. After 30 min, the solution was cooled to 25° C. with stirring and then allowed to stand for 30 min. The precipitate was filtered with filter paper, the solution was evaporated in a nitrogen stream, and the residue was dried at 80° C. under vacuum until a constant weight was reached. In this way, the weight percent of the polymer soluble in xylene at 25° C. was calculated. The amount of xylene insoluble matter (weight percent of the polymer insoluble in xylene at 25° C., XI) was calculated by subtracting 100 from the weight percent of the soluble polymer, and is considered to be the amount of crystalline components in the polymer.

[0064] [Intrinsic viscosity of polymer] A sample of propylene (co)polymer was dissolved in tetralin at 135° C. to obtain a solution with a concentration of 0.01% by weight. The intrinsic viscosity of the solution was measured using an automatic capillary viscosity measuring device (SS-780-H1, manufactured by Shibayama Scientific Instruments Co., Ltd.).

[0065] [Powder fluidity] A metal frame with an opening measuring 5 cm in length, 5 cm in width, and 1 cm in height was placed on the metal plate, and 5 g of polymer was spread inside the metal frame as a sample. The pressure applied to the sample was uniformly 23 g / cm 2 A 0.92g metal lid was placed inside the metal frame so that the sample in the metal frame was held at 70°C for 20 minutes, after which the metal frame and metal lid were removed, and the sample placed on the metal plate was tilted to perform the following 5-point evaluation four times and the average was calculated. 1. If tilted between 0° and 30°, the entire container will collapse. 2. If tilted at an angle between 30° and 50°, the entire container will collapse. 3. If tilted more than 50° but less than 70°, the entire contents will fall off. 4. If you tilt it more than 70 degrees but less than 90 degrees, the whole thing will fall apart. 5. Even if tilted over 90 degrees, the entire contents will not fall off The materials for the metal plate, metal frame, and metal cover were SUS304 stainless steel, and the metal plate used had a surface roughness (maximum roughness Ry) of 0.2 μm obtained by polishing the surface with #400 (sisal finish).

[0066] [Polymer melting point] The melting point of the polymer was measured by carrying out the second scan defined above using a Diamond DSC manufactured by PerkinElmer.

[0067] [MFR] The measurements were performed in accordance with JIS K7210-1 at a temperature of 230°C and a load of 2.16 kg.

[0068] [Melt tension] The resin composition was melted at a temperature of 200°C using a capillary rheometer (Capillograph 1D, manufactured by Toyo Seiki Seisakusho Co., Ltd.) equipped with a cylindrical orifice with a length of 8.0 mm and a diameter of 2.095 mm and a flat upper surface. The molten resin composition was extruded from the orifice at a resin extrusion speed of 15 mm / min to form a strand. The strand was taken up at a take-up speed of 6.5 m / min using a rotating take-up means, and the melt tension (unit: g force) was measured.

[0069] [Appearance of foam] The appearance of the foamed strands expanded to 3.0 to 3.4 times was evaluated according to the following criteria. A: The surface is smooth and the strands are straight. B: The surface is slightly uneven or wavy. C: The surface is uneven and the strands are wavy.

[0070] [Closed cell] A foamed strand that had been expanded 3.0 to 3.4 times its original size was cut with a razor to a length of 4 cm, and one end of the cut piece was immersed in an ethanol solution of the pigment for 30 seconds. The closed cell property was evaluated based on the distance from the cut surface to the interior where the ethanol had penetrated the most (maximum coloring distance). A: Maximum coloring distance is 2mm or less B: Maximum coloring distance is over 2mm and 20mm or less C: Maximum coloring distance exceeds 20 mm

[0071] [Stiffness] The non-foamed sheet was punched out to prepare five test pieces measuring 2.75 inches long and 1.5 inches wide. The stiffness of each test piece was measured according to JIS P8125 using a V-5 stiffness tester (model 150-B) manufactured by Taber Instrument Corporation at room temperature of 23° C. The measurement conditions were as follows: Measurement range: 50-500 Range weight: 500 units Curvature angle: 15° Measurement span: 5cm Scale factor: 5x Hold time 1 minute Measurement temperature: 23℃ The stiffness was calculated by reading the values ​​at a warp angle of 15° on both sides of each test piece and averaging them. The stiffness of the non-foamed sheet was then calculated using the following formula. E = 9.83 × T su / t 3 (E: sheet stiffness [MPa], T su : average stiffness [gf cm], t: thickness of test piece [mm]) A larger stiffness value means higher rigidity.

[0072] It is clear that, when the content of ethylene-derived units in the polymer is the same, the propylene-ethylene copolymers of the Examples having an intrinsic viscosity of more than 20 dl / g have superior powder flowability compared to the propylene-ethylene copolymers of the Comparative Examples having an intrinsic viscosity of 20 dl / g or less. It is also clear that the non-foamed sheets and foams obtained from the compositions containing the propylene (co)polymers of the present invention have excellent properties.

Claims

1. A copolymer of propylene and 30% by weight or less of ethylene, having an intrinsic viscosity of more than 20 dl / g measured in tetralin solvent at 135°C, The melting point Tm (°C) of the copolymer determined by DSC at a temperature increase rate of 10°C / min and the ethylene content C2 (wt%) in the copolymer satisfy the following formula (1): Tm ≧ -3.4×C2 + 162…(1) Here, the Tm is the temperature at which the heat of fusion accompanying melting shows a maximum value in the melting curve of DSC. Copolymer.

2. 2. The copolymer according to claim 1, wherein the intrinsic viscosity is 23 dl / g or more and the ethylene content is 3 to 30% by weight.

3. (A) a solid catalyst containing magnesium, titanium, a halogen, and an electron donor compound as essential components; (B) an organoaluminum compound, and 3. A method for producing the polymer according to claim 1 or 2, comprising preparing the polymer by polymerizing the corresponding monomer using a catalyst optionally containing (C) an external electron donor compound.

4. A composition comprising the polymer according to claim 1 or 2, A polypropylene resin composition, the content of said polymer being 0.1 to 20% by weight based on the total weight of the resin components constituting said composition.

Citation Information

Patent Citations

  • Refuse disposal machine

    JP1981053761A

  • Electric connector assembly

    JP1984079985A

  • Vehicle mirror housing drive device

    JP1986044045A

  • Manufacture of differential pressure forming crystalline polypropylene sheet

    JP1993293821A

  • Ultra-high-molecular-weight polypropylene composition

    JP1994057055A