Process oil for rubber processing and rubber composition containing same
A process oil with liquid olefin copolymer, polyisobutylene, and alkylated phosphonium phosphate compounds enhances rubber compounding processability and mechanical properties, addressing viscosity and aging issues in rubber compounding.
Patent Information
- Application Number
- JP2023054603
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-05-04
- Filing Date
- 2023-03-30
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2043-03-30
AI Technical Summary
Existing rubber compounding processes face challenges in achieving improved processability and mechanical properties without significantly increasing oil input, which can lead to viscosity issues, separation of rubber, and oil diffusion, resulting in degraded mechanical properties and aging.
A process oil comprising a base oil with additives such as a liquid olefin copolymer, polyisobutylene, and alkylated phosphonium phosphate or butylhydroxybenzene compounds is used, balancing oil content to enhance processability and mechanical properties.
The solution improves rubber compounding processability and mechanical properties, reduces oil diffusion, and suppresses aging, while maintaining desired product dimensions and reducing manufacturing defects.
Smart Images

Figure 0007580515000001 
Figure 0007580515000002 
Figure 0007580515000003
Abstract
Description
[Technical Field]
[0001] The present invention relates to a process oil for rubber processing and a rubber composition containing the same. [Background technology]
[0002] EPDM (Ethylene-Propylene Diene Monomer) / SEBS (Styrene-Ethylene / Butylene-Styrene) are types of rubber used throughout industry. EPDM is produced by copolymerizing ethylene and propylene and adding ENB (Ethylene Norbonene) to allow for the inclusion of double bonds that can be crosslinked. Because of its excellent weather resistance and ozone resistance, it is often used in automotive weather strips and is widely used in rubber parts for home appliances and machinery.
[0003] To make rubber products using EPDM / SEBS, the composition must be designed to have the desired mechanical properties, and then semi-finished rubber products must be made through a compounding process. The compounded rubber manufacturing process typically involves the use of reinforcing agents, oils, antioxidants, activators, crosslinking agents, accelerators, tackifiers, and processing aids. The compounded rubber is then molded into a specific shape through processes such as extrusion or rolling, and the molded rubber is then crosslinked under heat and pressure to produce the final rubber product.
[0004] Rubber products have the unique ability to return to their original shape after deformation, and are therefore used in a variety of ways across industries, such as supporting bridges and buildings to dampen vibrations and being used between moving machinery to prevent noise and vibration.
[0005] A large amount of filler is used to satisfy the mechanical properties of rubber, which is widely used in this field. However, if reinforcing agents such as carbon black or silica are added to rubber in excess of a certain amount, the viscosity increases too much, making compounding difficult. In addition, the rubber may break apart due to lack of wetting, making it difficult to satisfy the mechanical properties of the rubber.
[0006] In this case, using an appropriate amount of oil makes compounding easier, but the amount cannot be increased infinitely.Adding too much oil makes compounding easier, but it can reduce the mechanical properties of the rubber, resulting in deviations from the designed properties, which affects product performance.
[0007] In addition, since the molecular weight of oil is smaller than that of rubber, it can be released into the air and diffuse to surrounding areas with low oil content, causing the amount of oil remaining in the rubber to decrease over time, which causes changes in the mechanical properties of rubber and is a type of rubber aging.
[0008] Therefore, there is a need to develop a technology that can improve rubber compounding processability, extrusion and rolling processability, increase the mechanical properties of rubber, and suppress the oil reduction phenomenon without significantly increasing the amount of oil input. Meanwhile, Korean Patent Publication No. 10-1363718 has been cited as a similar prior art document. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Korean Patent Publication No. 10-1363718 (February 10, 2014) Summary of the Invention [Problem to be solved by the invention]
[0010] An object of the present invention is to provide a process oil for rubber processing, which can improve rubber compounding processability, improve the mechanical properties of rubber, and suppress oil loss without significantly increasing the amount of oil added, and a rubber composition containing the same. [Means for solving the problem]
[0011] One aspect of the present invention relates to a process oil for rubber processing, comprising: a base oil; a liquid olefin copolymer dissolved in the base oil and produced by copolymerizing ethylene with an alpha-olefin having 3 to 20 carbon atoms; polyisobutylene; and one or more additives selected from alkylated phosphonium phosphate compounds and butylhydroxybenzene-based compounds.
[0012] In one embodiment, the process oil for rubber processing may contain 1 to 80% by weight of a base oil, 1 to 80% by weight of a liquid olefin copolymer, 10 to 50% by weight of polyisobutylene, and 0.01 to 3% by weight of an additive.
[0013] In the above-mentioned embodiment, the liquid olefin copolymer may be composed of 40 to 60 mol % of ethylene units and 60 to 40 mol % of alpha-olefin units having 3 to 20 carbon atoms.
[0014] In the above-mentioned embodiment, the polyisobutylene may have a number average molecular weight of 500 to 6,000 g / mol.
[0015] In one embodiment, the alkylated phosphonium phosphate compound may satisfy the following Chemical Formula 1: [Chemical formula 1] TIFF0007580515000001.tif28170 (In the formula, R1 to R6 are each independently a linear or branched alkyl group having 1 to 20 carbon atoms.)
[0016] In the one embodiment, the alkylated phosphonium phosphate compound may be one or more selected from tetraoctylphosphonium bis(2-ethylhexyl)phosphate, tributyltetradecylphosphonium bis(2-ethylhexyl)phosphate, tetraethylphosphonium bis(2-ethylhexyl)phosphate, and tributyltetradecylphosphonium bis(2-ethylhexyl)phosphate.
[0017] In the above-described embodiment, the butylhydroxybenzene-based compound may be one or more selected from N,N'-(hexane-1,6-diyl)bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propanamide], pentaerythritol tetrakis(3,5-di-t-butyl-4-hydroxyhydrocinnamate), alkyl-t-butylhydroxyhydrocinnamate, alkyl-3,5-di-t-butyl-4-hydroxyhydrocinnamate, and t-butylhydroanisole. Another aspect of the present invention relates to a rubber composition containing the above-mentioned process oil for rubber processing. In the other embodiment, the rubber composition can contain 80 to 200 parts by weight of process oil per 100 parts by weight of rubber.
[0018] In another embodiment, the rubber composition may further include a diene-based rubber, and the diene-based rubber may be at least one selected from ethylene propylene diene rubber (EPDM), butadiene rubber, natural rubber, isoprene rubber, styrene butadiene rubber (SBR), nitrile rubber (NBR), isobutene-isoprene rubber (IIR), and chloroprene rubber (CR). [Effects of the Invention]
[0019] The process oil of the present invention is a base oil to which a liquid olefin copolymer, polyisobutylene, and one or more additives selected from alkylated phosphonium phosphate compounds and butylhydroxybenzene compounds are added. This is advantageous in improving processing lines and improving the mechanical properties of the rubber, even though the process oil is added in the same amount as in the past when compounding rubber. DETAILED DESCRIPTION OF THE INVENTION
[0020] The advantages and features of the embodiments of the present invention, and methods for achieving them, will become clearer with reference to the embodiments described below in detail in conjunction with the accompanying drawings. However, the present invention is not limited to the embodiments disclosed below, and can be realized in various different forms. However, the present embodiments are provided to complete the disclosure of the present invention and to fully convey the scope of the invention to those skilled in the art, and the present invention is defined only by the scope of the claims. The same reference numerals refer to the same elements throughout the specification.
[0021] In describing embodiments of the present invention, if it is determined that a detailed description of a known function or configuration may unnecessarily obscure the gist of the present invention, the detailed description will be omitted. The terms described below are defined in consideration of the functions in the embodiments of the present invention, and may vary depending on the intentions or practices of users or operators. Therefore, the definitions should be based on the contents of the entire specification.
[0022] One aspect of the present invention relates to a process oil for rubber processing, comprising: a base oil; a liquid olefin copolymer dissolved in the base oil and produced by copolymerizing ethylene with an alpha-olefin having 3 to 20 carbon atoms; polyisobutylene; and one or more additives selected from alkylated phosphonium phosphate compounds and butylhydroxybenzene-based compounds.
[0023] As described above, the process oil of the present invention is a base oil to which one or more additives selected from a liquid olefin copolymer, polyisobutylene, and an alkylated phosphonium phosphate compound or a butylhydroxybenzene-based compound have been added. This is advantageous in improving processability and in improving the mechanical properties of the rubber, even though the process oil is added in the same amount as in the past when compounding rubber.
[0024] To achieve this, it is advisable to appropriately adjust the content of each component of the process oil. The process oil for rubber processing can contain 1 to 80 wt% base oil, 1 to 80 wt% liquid olefin copolymer, 10 to 50 wt% polyisobutylene, and 0.01 to 3 wt% additives. Preferably, it contains 5 to 60 wt% base oil, 20 to 80 wt% liquid olefin copolymer, 12 to 40 wt% polyisobutylene, and 0.05 to 2 wt% additives. Most preferably, it contains 20 to 45 wt% base oil, 35 to 45 wt% liquid olefin copolymer, 15 to 35 wt% polyisobutylene, and 0.1 to 1.5 wt% additives. When rubber is compounded within these ranges, excellent processability improvement effects can be achieved while also improving the mechanical properties of the rubber. On the other hand, if the content falls outside the above ranges, the processability improvement effects are negligible or the mechanical properties of the compounded rubber may be reduced.
[0025] The process oil according to an embodiment of the present invention will be described in more detail below. First, the base oil according to one example of the present invention may differ in viscosity characteristics, heat resistance, oxidation stability, and other properties depending on the production method, refining method, etc., but any base oil commonly used in the art may be used without any particular limitations, and the American Petroleum Institute (API) generally classifies base oils into five groups: I, II, III, IV, and V. These API categories are defined in API Publication 1509, 15th Edition, Appendix E, April 2002, as shown in Table 1 below.
[0026] [Table 1]
[0027] The base oil may be any of API Category Groups I to V. Base oils suitable for the present invention belong to API Category I and III. The term "saturated hydrocarbons" refers to paraffinic and naphthenic compounds. Paraffinic compounds may be branched or linear, and naphthenic compounds may be cyclic saturated hydrocarbons, i.e., cycloparaffins. Saturated hydrocarbons with cyclic structures are typically derivatives of cyclopentane or cyclohexane. Naphthenic compounds contain a single ring structure (mononaphthene), two isolated ring structures (isolated dinaphthenes), two fused ring structures (fused dinaphthenes), or three or more fused ring structures (polycyclic naphthenes or polynaphthenes). A liquid olefin copolymer according to one embodiment of the present invention facilitates wetting of reinforcing agents during rubber compounding, ensuring that the shear force of the compounding machine is transmitted to the rubber, ensuring thorough mixing of the rubber and reinforcing agents. Liquid olefin copolymers produced by copolymerizing ethylene with an alpha olefin having 3 to 20 carbon atoms exhibit different properties from conventionally used mineral oils such as naphthenic oil and paraffin oil. However, their similarity to EPDM / SEBS rubber makes them more miscible with rubber than mineral oils and they are advantageous for lowering the viscosity of compounded rubber. This reduces electricity consumption during the extrusion or rolling process and is advantageous for producing rubber products with dimensions closer to the desired. The improved dimensional stability of rubber products can also be expected to reduce the reject rate and lower production costs.
[0028] The liquid olefin copolymer is prepared by copolymerizing ethylene and an alpha-olefin monomer in the presence of a single-site catalyst system so that the alpha-olefin units are uniformly distributed in the copolymer chain. Preferably, the liquid olefin copolymer can be prepared by reacting ethylene and an alpha-olefin monomer in the presence of a single-site catalyst system containing a bridged metallocene compound, an organometallic compound, and an ionic compound that reacts with the bridged metallocene compound to form an ion pair.
[0029] The alpha-olefin monomer used with ethylene in producing the liquid olefin copolymer includes an aliphatic olefin having 3 to 20 carbon atoms, specifically, one or more selected from propylene, 1-butene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3-methyl-1-pentene, 1-heptene, 1-octene, 1-decene, 1-dodecene, and 1-tetradecene, including, but not limited to, isomers. Preferably, the alpha-olefin monomer is one or more alpha-olefins having 3 to 6 carbon atoms, most preferably propylene.
[0030] Preferably, the liquid olefin copolymer suitable for the present invention may be one that contains 40 to 60 mol% of ethylene units and 60 to 40 mol% of alpha-olefin units having 3 to 20 carbon atoms. Using a liquid olefin copolymer having such a content range is effective for improving processability and mechanical properties. On the other hand, if the ethylene unit content is less than 40 mol% or more than 60 mol%, the effect of improving processability may be insignificant, or the mechanical properties of the compounded rubber may be reduced.
[0031] The liquid olefin copolymer may have a number average molecular weight (Mn) of 500 to 10,000 g / mol, a molecular weight distribution (Mw / Mn, where Mw is the weight average molecular weight) of 3 or less, and a kinematic viscosity at 100°C of 30 to 5,000 cSt.
[0032] Polyisobutylene according to one embodiment of the present invention is a polymer with an isobutylene backbone. When the liquid olefin copolymer and polyisobutylene are added together to a base oil, the breaking strength and elongation of the rubber can be improved simultaneously. While EPDM / SEBS rubber can often suffer from wear, where smooth metal surfaces are stripped away by repeated stress, adding a process oil containing a liquid olefin copolymer and polyisobutylene according to the present invention during rubber compounding can improve both the breaking strength and elongation of the rubber, contributing to improved wear performance. Furthermore, by preventing oil from being released into the air or diffusing into surrounding rubber, the reduction in the amount of oil remaining in the compounded rubber can be suppressed. This prevents rubber aging due to oil loss and permanent deformation that cannot be recovered from repeated deformation.
[0033] The polyisobutylene suitable for the present invention preferably has a number average molecular weight of 500 to 6,000 g / mol, preferably 1,000 to 4,000 g / mol, and most preferably 1,500 to 3,000 g / mol, and a molecular weight distribution (PI) of 1 to 5, preferably 1 to 3. The kinematic viscosity at 100°C may be 2 to 10,000 cSt, preferably 100 to 5,000 cSt, and most preferably 1,000 to 3,000 cSt.
[0034] The additive according to one example of the present invention is added for friction-reducing effects and antioxidant effects, and may be one or more selected from the group consisting of alkylated phosphonium phosphate compounds and butylhydroxybenzene-based compounds, as described above.
[0035] The alkylated phosphonium phosphate compound may satisfy the following Chemical Formula 1, and a more specific example may be one or more selected from tetraoctylphosphonium bis(2-ethylhexyl)phosphate, tributyltetradecylphosphonium bis(2-ethylhexyl)phosphate, tetraethylphosphonium bis(2-ethylhexyl)phosphate, and tributyltetradecylphosphonium bis(2-ethylhexyl)phosphate. [Chemical formula 1] TIFF0007580515000003.tif28170 (In the formula, R1 to R6 are each independently a linear or branched alkyl group having 1 to 20 carbon atoms.)
[0036] The butylhydroxybenzene compound is a compound containing a butylhydroxybenzene group, and specifically may be one or more compounds selected from, for example, N,N'-(hexane-1,6-diyl)bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propanamide], pentaerythritol tetrakis(3,5-di-t-butyl-4-hydroxyhydrocinnamate), alkyl-t-butylhydroxyhydrocinnamate, alkyl-3,5-di-t-butyl-4-hydroxyhydrocinnamate, and t-butylhydroanisole, where the alkyl is an alkyl group having 1 to 20 carbon atoms and may be linear or branched.
[0037] Another aspect of the present invention relates to a rubber composition containing the above-mentioned process oil for rubber processing. Specifically, the rubber composition may contain rubber, process oil for rubber processing, and a filler.
[0038] The rubber composition may contain 80 to 200 parts by weight of process oil per 100 parts by weight of rubber, and more preferably 100 to 180 parts by weight of process oil. Within this range, the processability is excellently improved, and the mechanical properties of the compounded rubber are also effectively improved.
[0039] Meanwhile, the rubber according to an embodiment of the present invention may be any rubber commonly used in the art, and is not particularly limited thereto. Specifically, the diene rubber may be at least one selected from ethylene propylene diene rubber (EPDM), butadiene rubber, natural rubber, isoprene rubber, styrene butadiene rubber (SBR), nitrile rubber (NBR), isobutene-isoprene rubber (IIR), and chloroprene rubber (CR). Derivatives of such rubbers, such as tin compound-modified polybutadiene rubber, or epoxy-modified, silane-modified, or maleic acid-modified rubber, may also be used alone or in combination.
[0040] The filler according to one embodiment of the present invention may be silica, carbon black, white carbon, carbon nanotubes, clay, talc, or a mixture thereof, and more preferably carbon black. The amount of the filler may be 10 to 150 parts by weight, preferably 30 to 120 parts by weight, and most preferably 50 to 100 parts by weight, per 100 parts by weight of rubber.
[0041] In addition, the rubber composition may further contain one or more compounding components selected from a vulcanizing agent, a vulcanization accelerator, zinc oxide, stearic acid, and the like commonly used in the rubber industry, depending on the application and needs. Examples of the vulcanizing agent may be one or more selected from sulfur (free sulfur), amine disulfide, polymeric polysulfide, and sulfur olefin adducts, and the vulcanization accelerator may be one or more selected from benzothiazole-based accelerators such as 2-mercaptobenzothiazole, dibenzothiazyl disulfide, sodium-2-mercaptobenzothiazole, zinc salt-2-mercaptobenzothiazole, cyclohexylamine salt 2-mercaptobenzothiazole, N-cyclohexyl-2-benzothiazole sulfenamide, N-tert-butyl-2-benzothiazole sulfenamide, and N-oxydiethylene-2-benzothiazole sulfenamide, and thiuram-based accelerators such as tetramethylthiuram monosulfide, tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetrabutylthiuram disulfide, and dipentamethylenethiuram disulfide. The compounding components can be added in an amount of 0.1 to 10 parts by weight per 100 parts by weight of rubber, but are not limited to this amount.
[0042] The present invention will be described in detail below with reference to examples and comparative examples. The following examples are merely provided to aid in understanding the present invention, and the scope of the present invention is not limited by the following examples. In the present invention, "%" not specifically stated may mean "% by weight."
[0043] [Production Examples 1 to 15 and Comparative Production Examples 1 to 16] A process oil was prepared by mixing paraffin oil, naphthenic oil, liquid olefin copolymer (number average molecular weight (Mn) 7800 g / mol, ethylene content 50 mol%), polyisobutylene (PIB) (manufactured by Delim Co., Ltd., PB2000, Mn 2180 g / mol, kinematic viscosity at 100°C 2200 to 2400 cSt) and additives according to the amounts (wt %) listed in Table 2 below. The abbreviations for additives used in Table 2 are as follows:
[0044] TPEP:tetraoctylphosphonium bis(2-ethylhexyl)phosphate TBPEHP:tributyltetradecylphosphonium bis(2-ethylhexyl)phosphate TEPEHP:tetraethylphosphonium bis(2-ethylhexyl)phosphate BHC:Octyl-3,5-di-tert-butyl-4-hydroxyhydrocinnamate BHPPA:N,N'- (hexane-1,6-diyl) bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propanamide]
[0045] [Table 2]
[0046] [Examples 1 to 15 and Comparative Examples 1 to 16] Process oil, EPDM (KEP980N, manufactured by Kumho Polychem Corporation, ethylene content 71 wt%, ENB content 4.5 wt%, Mooney viscosity (ML(1+8)@125°C) 58), carbon black (CB), zinc oxide (ZnO), stearic acid (SA), sulfur, tetramethylthiuram disulfide (TMTD), and 2,2'-dibenzothiazyl disulfide (MBTS) were mixed in the amounts (wt%) shown in Table 3 below to produce a compounded rubber.
[0047] [Table 3] TIFF0007580515000006.tif55170
[0048] [Characteristics evaluation] Each property is tested by the following method, and the results of the Rheo test, Mooney viscosity and tensile properties are expressed as an index, with the higher the index number, the more advantageous the physical property. 1) Rheo test (Rheo (@160°C)): Measured based on ASTM D5289.
[0049] 2) Mooney viscosity (ML(1+4)@100°C): Measured according to ASTM D1646. Mooney viscosity is an index that indicates the viscosity of rubber; the higher the value, the lower the viscosity and the better the processability.
[0050] 3) Compression set (CSET) (%): Measured according to ASTM D395. Compression set indicates the mechanical strength of rubber, and the lower the value, the less deformation caused by compression.
[0051] 4) Tensile properties: Breaking strength and breaking elongation were measured according to ASTM D412. Tensile properties indicate the mechanical strength of rubber, and the higher the index number, the better the mechanical strength.
[0052] [Table 4]
[0053] Referring to Tables 2 to 4, in the examples in which the process oil prepared by mixing a base oil with one or more additives selected from a liquid olefin copolymer, polyisobutylene, and an alkylated phosphonium phosphate compound or a butylhydroxybenzene compound according to the present invention was blended with rubber, it was confirmed that the processability and mechanical properties of the rubber were generally improved compared to the comparative examples in which one or more of the liquid olefin copolymer and polyisobutylene were not added.
[0054] However, in the case of Examples 10, 11 and 15, the amount of liquid olefin copolymer or polyisobutylene added was somewhat small, so the effects of improving processability and mechanical properties were slight or reduced.
[0055] [Manufacturing Example 16] A process oil was prepared by mixing 36.68 wt% paraffin oil, 21.51 wt% naphthenic oil, 26.00 wt% liquid olefin copolymer (number average molecular weight (Mn) 7800 g / mol, ethylene content 35 mol%), 15.7 wt% polyisobutylene (PIB) (manufactured by Delim Co., Ltd., PB2000, Mn 2180 g / mol, kinematic viscosity at 100°C 2200-2400 cSt), and 0.11 wt% BHC.
[0056] [Manufacturing Example 17] A process oil was prepared by mixing 37.76 wt% paraffin oil, 16.52 wt% naphthenic oil, 25.50 wt% liquid olefin copolymer (number average molecular weight (Mn) 7800 g / mol, ethylene content 75 mol%), 20.1 wt% polyisobutylene (PIB) (manufactured by Delim Co., Ltd., PB2000, Mn 2180 g / mol, kinematic viscosity at 100°C 2200-2400 cSt), and 0.12 wt% BHC.
[0057] [Manufacturing Example 18] A process oil was prepared by mixing 67.63 wt% paraffin oil, 25.00 wt% liquid olefin copolymer (number average molecular weight (Mn) 7800 g / mol, ethylene content 70 mol%), 7.25 wt% polyisobutylene (PIB) (manufactured by Delim Co., Ltd., PB2000, Mn 2180 g / mol, kinematic viscosity at 100°C 2200-2400 cSt), and 0.12 wt% BHC.
[0058] [Manufacturing Example 19] A process oil was prepared by mixing 42.68 wt% paraffin oil, 23.35 wt% naphthenic oil, 26.54 wt% liquid olefin copolymer (number average molecular weight (Mn) 7800 g / mol, ethylene content 30 mol%), 7.32 wt% polyisobutylene (PIB) (manufactured by Delim Co., Ltd., PB2000, Mn 2180 g / mol, kinematic viscosity at 100°C 2200-2400 cSt), and 0.11 wt% BHC.
[0059] [Table 5]
[0060] [Examples 16 to 19] According to the addition amounts (wt %) shown in Table 6 below, process oil, EPDM (KEP980N, manufactured by Kumho Polychem Corporation, ethylene content 71 wt %, ENB content 4.5 wt %, Mooney viscosity (ML(1+8)@125°C) 58), carbon black (CB), zinc oxide (ZnO), stearic acid (SA), sulfur, tetramethylthiuram disulfide (TMTD), and 2,2'-dibenzothiazyl disulfide (MBTS) were mixed to produce compounded rubber.
[0061] [Table 6]
[0062] [Characteristics evaluation] The rheological test, Mooney viscosity, permanent compression and tensile properties were evaluated using the methods described above, and the results are shown in Table 7 below.
[0063] [Table 7] The above-mentioned Example 8 and Examples 16 to 19 are experimental examples in which liquid olefin copolymers with different ethylene contents were added.
[0064] Among them, Example 8, which used a liquid olefin copolymer with an ethylene content of 40 to 60 mol%, not only exhibited excellent processability, but also had excellent mechanical properties, with a permanent compression rate of 10.22% and a tensile strength index of 157.
[0065] On the other hand, in Examples 16 to 19, it was confirmed that the effects of improving processability and mechanical properties were negligible or decreased due to the addition of a liquid olefin copolymer having an ethylene content of more than 40 to 60 mol%.
Claims
1. Base oil and a liquid olefin copolymer dissolved in the base oil and produced by copolymerizing ethylene with an alpha-olefin having 3 to 20 carbon atoms; Polyisobutylene, and one or more additives selected from an alkylated phosphonium phosphate compound and a butylhydroxybenzene compound.
2. The process oil for rubber processing according to claim 1, comprising 1 to 80% by weight of a base oil, 1 to 80% by weight of a liquid olefin copolymer, 10 to 50% by weight of polyisobutylene, and 0.01 to 3% by weight of an additive.
3. 2. The process oil for rubber processing according to claim 1, wherein the liquid olefin copolymer contains 40 to 60 mol % of ethylene units and 60 to 40 mol % of alpha-olefin units having 3 to 20 carbon atoms.
4. The process oil for rubber processing according to claim 1, wherein the polyisobutylene has a number average molecular weight of 500 to 6,000 g / mol.
5. The process oil for rubber processing according to claim 1 , wherein the alkylated phosphonium phosphate compound satisfies the following chemical formula 1: [Chemical formula 1] (In the formula, R 1 ~R 6 are each independently a linear or branched alkyl group having 1 to 20 carbon atoms.
6. The alkylated phosphonium phosphate compound is The process oil for rubber processing according to claim 5, which is one or more selected from the group consisting of tetraoctylphosphonium bis(2-ethylhexyl)phosphate, tetraethylphosphonium bis(2-ethylhexyl)phosphate, and tributyltetradecylphosphonium bis(2-ethylhexyl)phosphate.
7. 2. The process oil for rubber processing according to claim 1, wherein the butyl hydroxybenzene-based compound is at least one selected from the group consisting of N,N'-(hexane-1,6-diyl)bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propanamide], pentaerythritol tetrakis(3,5-di-t-butyl-4-hydroxyhydrocinnamate), alkyl-t-butyl hydroxyhydrocinnamate, alkyl-3,5-di-t-butyl-4-hydroxyhydrocinnamate, and t-butyl hydroanisole.
8. A rubber composition comprising the process oil for rubber processing according to any one of claims 1 to 7.
9. The rubber composition according to claim 8, wherein the rubber composition comprises 80 to 200 parts by weight of a process oil for rubber processing per 100 parts by weight of rubber.
10. The rubber composition according to claim 8 , further comprising a diene rubber.
11. The diene rubber is at least one selected from ethylene propylene diene rubber (EPDM), butadiene rubber, natural rubber, isoprene rubber, styrene butadiene rubber (SBR), nitrile rubber (NBR), isobutene-isoprene rubber (IIR) and chloroprene rubber (CR). The rubber composition according to claim 10.
Citation Information
Patent Citations
Laminate of thermoplastic elastomer
JP1993004307A
Star-wise branched rubber / thermoplastic elastomer vulcanizate
JP2000072924A
Plasticized functionalized propylene copolymer adhesive composition
JP2008546890A
Thermoplastic elastomer composition, foam and method for producing foam
JP2009235241A
Vulcanizable rubber composition
JP2018501344A