Heat-resistant millable fluorosilicone rubber composition
The fluorosilicone rubber composition addresses heat resistance and colorability issues by incorporating specific components, achieving high-temperature durability and flexible color options.
Patent Information
- Application Number
- JP2023500916
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-02-18
- Filing Date
- 2022-02-17
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2042-02-17
AI Technical Summary
Existing fluorosilicone rubber compositions do not provide sufficient heat resistance at temperatures of 200°C or higher, particularly 250°C or higher, and are difficult to color to desired appearances due to additives like iron oxide causing coloration issues.
A millable fluorosilicone rubber composition containing organopolysiloxane with specific surface area and fluoroalkyl groups, reinforcing silica, titanium oxide modified with transition metal oxide, and calcium carbonate, along with a curing agent, to enhance heat resistance and allow easy coloration.
The composition achieves excellent heat resistance at high temperatures while suppressing hardness increases and enables easy coloration with pigments, maintaining mechanical properties.
Smart Images

Figure 0007580564000001 
Figure 0007580564000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a millable type fluorosilicone rubber composition which provides a silicone rubber having good heat resistance. [Background technology]
[0002] Silicone rubber has excellent weather resistance, electrical properties, low compression set, heat resistance, cold resistance, etc., and is therefore widely used in various fields, including electrical equipment, automobiles, construction, medicine, and food. In particular, fluorosilicone rubber compositions, which are based on fluorosilicone raw rubber, whose main chain of the base polymer is essentially composed of a repeating structure of (3,3,3-trifluoropropyl)methylsiloxane units having 3,3,3-trifluoropropyl groups as side chain substituents, have excellent solvent resistance, and are widely used as diaphragms, O-rings, oil seal materials, etc., as transportation equipment parts and petroleum-related equipment parts. Currently, the demand for silicone rubber is increasing, and the development of silicone rubber with excellent properties is desired.
[0003] It is known that additives such as cerium oxide, cerium hydroxide, iron oxide, carbon black, etc. can be blended to further improve the heat resistance of silicone rubber. However, in the case of fluorosilicone rubber, the heat resistance of silicone rubber under high temperature conditions of 200°C or higher is insufficient, and silicone rubber that exhibits excellent heat resistance under such conditions is required.
[0004] Patent Document 1 (JP Patent Publication No. 2016-518461) describes how adding 0.1% by mass or more of titanium oxide and iron oxide to silicone rubber can improve the heat resistance of the silicone rubber, but it only measures the amounts of formaldehyde, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, and dodecamethylcyclohexasiloxane generated when heated at 300°C for 1 hour, and makes no mention of changes in physical properties. Iron oxide is also well known as a colorant for silicone rubber, and even a small amount will color silicone rubber red, making it difficult to color it in a color other than red if desired.
[0005] Patent Document 2 (JP 2014-031408 A) describes that the heat resistance of silicone rubber can be improved by adding hydrous cerium oxide and / or hydrous zirconium oxide to the silicone rubber, and measures the physical properties after placing the material in a dryer at 225°C for 72 hours, but the physical properties decrease under higher temperature conditions.
[0006] Patent Document 3 (JP 2006-021991 A) and Patent Document 4 (WO 2010 / 140499) disclose titanium oxide doped with metal ions (metal salts) of transition metals or the like, but only disclose applications that utilize its optical properties, such as mid-infrared filters and photocatalysts. Patent Document 5 (WO2018 / 079376) claims that heat resistance can be improved by adding titanium oxide doped with 0.01 to 5 mass% transition metal oxide and cerium oxide and / or cerium hydroxide to millable silicone rubber, but this was not sufficient in the case of fluorosilicone rubber. Patent Document 6 (WO2008 / 154319) introduces a technology for improving heat resistance by adding carbon black, calcium carbonate, iron oxide, and optionally zinc oxide to fluorosilicone rubber, but it is difficult to impart the desired color appearance by adding carbon or iron oxide. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Special Publication No. 2016-518461 [Patent Document 2] JP 2014-031408 A [Patent Document 3] JP 2006-021991 A [Patent Document 4] WO2010 / 140499 [Patent Document 5] WO2018 / 079376 [Patent Document 6] WO2008 / 154319 Summary of the Invention [Problem to be solved by the invention]
[0008] Accordingly, an object of the present invention is to provide a millable type fluorosilicone rubber composition which gives a fluorosilicone rubber (cured product) that has excellent heat resistance at temperatures of 200°C or higher, particularly 250°C or higher. [Means for solving the problem]
[0009] As a result of intensive research conducted by the inventors in order to achieve the above-mentioned object, they discovered that by blending 0.01 to 5 mass % of titanium oxide modified with a transition metal oxide and calcium carbonate into a fluorosilicone rubber composition, the heat resistance of the fluorosilicone rubber obtained from the composition is significantly improved, which led to the completion of the present invention.
[0010] That is, the present invention provides (A) 100 parts by mass of an organopolysiloxane having at least two alkenyl groups bonded to silicon atoms in each molecule and having at least one fluoroalkyl group, the number of which is 40% or more of the total number of siloxane units, and the organopolysiloxane having an average degree of polymerization of 100 or more, (B) Specific surface area 50m 2 / g or more, 5 to 100 parts by mass of reinforcing silica, (C) 0.01 to 10 parts by mass of titanium oxide modified with a transition metal oxide, the titanium oxide containing 0.01 to 5% by mass of the transition metal oxide, (D) Calcium carbonate 0.01 to 10 parts by mass and (E) Hardener 0.1 to 50 parts by mass The present invention provides a millable type fluorosilicone rubber composition containing the above-mentioned compound, and a cured product of the composition. Effect of the Invention
[0011] The fluorosilicone rubber composition of the present invention can provide a fluorosilicone rubber (cured product) with excellent heat resistance. That is, the fluorosilicone rubber obtained by the present invention exhibits excellent heat resistance at temperatures of 200°C or higher, particularly at temperatures of 250°C or higher. In addition, an increase in the hardness of the fluorosilicone rubber can be suppressed. Furthermore, since the fluorosilicone rubber composition of the present invention is white, it can be easily colored to a desired color with a coloring agent such as a pigment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The composition of the present invention will be described in detail below. In this specification, the specific surface area is a value measured by the BET method. The millable composition means a composition that is a non-liquid composition with high viscosity that does not have self-flowability at room temperature (25°C) and can be uniformly kneaded under shear stress with a kneading machine such as a roll mill (e.g., two-roll or three-roll).
[0013] [(A) Organopolysiloxane] Component (A) is an organopolysiloxane that is the main component (base polymer) of the composition, and is an organopolysiloxane that has at least two alkenyl groups bonded to silicon atoms in each molecule, and contains siloxane units having at least one fluoroalkyl group in a proportion of 40% or more of the total number of all siloxane units, and has an average degree of polymerization of 100 or more. It contains at least two, and preferably 2 to 10,000, alkenyl groups bonded to silicon atoms in each molecule.
[0014] The organopolysiloxane (A) has an average degree of polymerization of 100 or more (usually 100 to 100,000), and preferably has an average degree of polymerization in the range of 1,000 to 100,000, more preferably 2,000 to 50,000, and particularly preferably 2,000 to 20,000. If the average degree of polymerization is less than the lower limit, the silicone rubber composition of the present invention will not satisfy the properties required for millable rubber, and roll kneading properties and the like will be significantly deteriorated, which is not preferable. In the present invention, the average degree of polymerization is based on the weight average molecular weight in terms of polystyrene in GPC (gel permeation chromatography) analysis measured under the following conditions.
[0015] [Measurement conditions] Developing solvent: THF ·Flow rate: 1mL / min Detector: Refractive index detector (RI) Column: 4 TSKGEL SUPERMULTIPORE HZ-H (Tosoh Corporation) Column temperature: 25℃ Sample injection volume: 10 μL (0.1% by mass in THF solution) In the present invention, component (A) is preferably a non-liquid organopolysiloxane gum that has a high degree of polymerization (high viscosity) and has no self-flowability at room temperature (25° C.).
[0016] The (A) component has 40% or more, preferably 45% or more, of the total number of siloxane units having at least one fluoroalkyl group. The upper limit is not particularly limited as long as it is 100% or less, preferably less than 100%, more preferably 99.8% or less, and may be 98% or less. By having siloxane units having a fluoroalkyl group in the above range, it is also possible to include copolymers containing siloxane units having a fluoroalkyl group and siloxane units having a dimethyl group.
[0017] The component (A) is preferably represented by the following average composition formula (1). R 1 nSiO (4-n) / 2 (1) In the above formula (1), R 1 are each independently a monovalent hydrocarbon group having 1 to 20 carbon atoms or a fluoroalkyl group having 1 to 20 carbon atoms, and n is a positive number of 1.95 to 2.04.
[0018] In the above average composition formula (1), R 1 are each independently a monovalent hydrocarbon group having 1 to 20 carbon atoms, preferably 1 to 12, more preferably 1 to 8 carbon atoms, or a fluoroalkyl group having 1 to 20 carbon atoms, preferably 1 to 10, more preferably 1 to 6 carbon atoms. Examples of the monovalent hydrocarbon group include alkyl groups such as methyl, ethyl, propyl, and butyl groups, cycloalkyl groups such as cyclohexyl groups, alkenyl groups such as vinyl, allyl, butenyl, and hexenyl groups, aryl groups such as phenyl and tolyl groups, and aralkyl groups such as β-phenylpropyl groups. Among these, methyl, vinyl, and phenyl groups are preferred, and methyl and vinyl groups are more preferred. Examples of the fluoroalkyl group include 3,3,3-trifluoropropyl groups, 3,3,4,4,5,5,5-heptafluorobutyl groups, and 3,3,4,4,5,5,6,6,6-nonafluorohexyl groups. Among these, 3,3,3-trifluoropropyl groups are preferred.
[0019] In the above average composition formula (1), n is a positive number of 1.95 to 2.04, and preferably a positive number of 1.98 to 2.02. If n is outside the range of 1.95 to 2.04, the resulting cured product may not exhibit sufficient rubber elasticity.
[0020] The organopolysiloxane (A) must have two or more alkenyl groups in one molecule. 1 Of the total moles, it is preferable that 0.001 to 10 mol %, particularly 0.01 to 5 mol % are alkenyl groups. The alkenyl groups are preferably vinyl groups and allyl groups, and particularly preferably vinyl groups.
[0021] The structure of the organopolysiloxane of component (A) is not particularly limited, but it is preferable that the main chain contains a diorganosiloxane unit (R 1 2 SiO 2 / 2 ) repeating units, and both ends of the molecular chain are triorganosiloxy groups (R 1 3 SiO 1 / 2 It is preferable that the diorganopolysiloxane is a linear diorganopolysiloxane terminated with R 1 is as described above. It is preferable that both molecular chain terminals are blocked with a trimethylsiloxy group, a dimethylvinylsiloxy group, a dimethylhydroxysiloxy group, a methyldivinylsiloxy group, a trivinylsiloxy group, etc. These organopolysiloxanes may be used alone or in combination of two or more types having different degrees of polymerization or molecular structures.
[0022] In the fluorosilicone rubber composition of the present invention, the content of component (A) is preferably 43 to 96 mass %, more preferably 50 to 90 mass %, and even more preferably 60 to 80 mass %.
[0023] [(B) Reinforcing Silica] The reinforcing silica of component (B) acts as a filler that imparts excellent mechanical properties to the resulting silicone rubber composition. The reinforcing silica may be precipitated silica (wet silica) or fumed silica (dry silica), and has a large number of silanol groups on its surface. In the present invention, the reinforcing silica (B) has a specific surface area of 50 m2 or less as measured by the BET method. 2 / g or more. Preferably, it is 100 to 400m 2 / g. This specific surface area is 50m 2 If it is less than 1 / g, the reinforcing effect of the silicone rubber imparted by component (B) will be insufficient.
[0024] The reinforcing silica of component (B) may be used in an untreated state, or may be surface-treated, as necessary, with an organosilicon compound such as organopolysiloxane, organopolysilazane, chlorosilane, alkoxysilane, etc. The reinforcing silica may be used alone or in combination of two or more types.
[0025] The amount of (B) reinforcing silica blended is 5 to 100 parts by mass, preferably 10 to 80 parts by mass, and more preferably 20 to 70 parts by mass, per 100 parts by mass of the organopolysiloxane of component (A). If the amount of component (B) blended is above the above upper limit or below the above lower limit, not only will the processability of the resulting silicone rubber composition decrease, but the mechanical properties such as tensile strength and tear strength of the silicone rubber cured product obtained by curing the silicone rubber composition will be insufficient.
[0026] [(C) Titanium oxide containing transition metal oxide] The component (C) is titanium oxide modified with a transition metal oxide, containing 0.01 to 5% by mass of the transition metal oxide, and is a component that significantly improves the heat resistance of silicone rubber. In the present invention, the titanium oxide modified with a transition metal oxide is, more specifically, titanium oxide doped with a transition metal oxide. The term "doped" refers to a form in which the transition metal oxide exists in the lattice of titanium oxide. The amount of the transition metal oxide contained in the titanium oxide is an amount that is 0.01 to 5% by mass relative to the mass of the modified (particularly doped) titanium oxide, and is preferably more than 0.01% by mass, preferably 0.05% by mass or more, more preferably 0.1% by mass or more, and even more preferably 1% by mass or more. The upper limit is 5% by mass or less, preferably 4.5% by mass or less, and more preferably 4% by mass or less. When the titanium oxide contains the transition metal oxide within the range, the heat resistance of the resulting fluorosilicone rubber can be effectively improved.
[0027] In the present invention, the transition metal oxide refers to a transition metal oxide other than titanium oxide, which is the side to be modified. Examples of the transition metal oxide include manganese oxide, iron oxide, cobalt oxide, nickel oxide, copper oxide, zinc oxide, zirconium oxide, etc., and among them, iron oxide (FeO, Fe 2 O 3 ) is preferred. By using titanium oxide modified with iron oxide, particularly titanium oxide doped with iron oxide, it is possible to suppress red coloration due to iron oxide and improve the heat resistance of silicone rubber. Titanium oxide modified with transition metal oxide, particularly titanium oxide doped with transition metal oxide, is produced by a known production method. For example, JP2010-013484A describes a method of doping iron oxide into crystalline titanium dioxide of 80% anatase type and 20% rutile type using titanium tetrachloride and iron trichloride.
[0028] The amount of component (C) is 0.01 to 10 parts by mass, preferably 0.1 to 5 parts by mass, and more preferably 0.5 to 3 parts by mass, per 100 parts by mass of organopolysiloxane (A). If the amount of component (C) is less than the lower limit, the heat resistance of the silicone rubber will not improve. If the amount exceeds the upper limit, the mechanical properties of the silicone rubber may be significantly reduced.
[0029] The content of the transition metal oxide in the fluorosilicone rubber composition is preferably 0.005 to 1.0 mass%, more preferably 0.01 to 1.0 mass%, and even more preferably 0.01 to 0.5 mass%, based on the total amount of the composition. If the content is equal to or more than the lower limit, the effect of the transition metal oxide contained in the titanium oxide can be sufficiently obtained, and if the content is equal to or less than the upper limit, the effect on coloring is small, which is preferable.
[0030] [(D) Calcium carbonate] The component (D) is calcium carbonate, which, in combination with the component (C), significantly improves the heat resistance of the silicone rubber. Commercially available calcium carbonate includes Silver W, Hakuenka CCR (manufactured by Shiraishi Kogyo Co., Ltd.), and Whiten SSB (manufactured by Bihoku Funka Kogyo Co., Ltd.). The amount of calcium carbonate in the fluorosilicone rubber composition is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, and more preferably 0.5 to 3 parts by mass, per 100 parts by mass of the component (A). If it is less than the lower limit, the heat resistance of the silicone rubber will not improve. If it exceeds the upper limit, the mechanical properties of the silicone rubber may be significantly reduced. There is no particular restriction on the particle size of the calcium carbonate, and it may be, for example, an average particle size of 0.1 to 50 μm.
[0031] The blending ratio of the components (C) and (D) is preferably 1:100 to 100:1, and more preferably 1:50 to 50:1, by mass ratio.
[0032] [(E) Hardener] The curing agent (E) is not particularly limited as long as it can cure the silicone rubber composition used in the present invention. The component (E) may be used alone or in combination of two or more. Examples of the component (E) include an organic peroxide curing agent (E-1), an addition reaction type curing agent (E-2), and a combination of the component (E-1) and the component (E-2). The amount of the component (E) is 0.1 to 50 parts by mass, preferably 0.1 to 40 parts by mass, and more preferably 0.2 to 10 parts by mass, based on 100 parts by mass of the organopolysiloxane (A).
[0033] (E-1) Organic peroxide curing agent Examples of the (E-1) organic peroxide curing agent include benzoyl peroxide, 2,4-dichlorobenzoyl peroxide, p-methylbenzoyl peroxide, o-methylbenzoyl peroxide, 2,4-dicumyl peroxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, di-t-butyl peroxide, t-butyl perbenzoate, and 1,6-hexanediol-bis-t-butylperoxycarbonate.
[0034] The amount of organic peroxide curing agent is preferably 0.1 to 10 parts by mass, and more preferably 0.2 to 5 parts by mass, per 100 parts by mass of component (A). If the amount is too small, curing may be insufficient, while if the amount is too large, the cured silicone rubber may turn yellow due to decomposition residues of the organic peroxide.
[0035] (E-2) Addition reaction curing agent As the addition reaction curing agent (E-2), it is preferable to use an organohydrogenpolysiloxane in combination with a hydrosilylation catalyst. As long as the organohydrogenpolysiloxane contains 2 or more, preferably 3 or more, more preferably 3 to 200, and even more preferably about 4 to 100 hydrogen atoms bonded to silicon atoms in one molecule (i.e., hydrosilyl groups), the structure may be linear, cyclic, branched, or a three-dimensional network structure, and the hydrosilyl groups may be located at the molecular chain terminals, in the middle of the molecular chain, or both.
[0036] The organohydrogenpolysiloxane may be any organohydrogenpolysiloxane known as a crosslinking agent for addition reaction curing type silicone rubber compositions. For example, an organohydrogenpolysiloxane represented by the following average composition formula (2) can be used. R 2 p H q SiO (4-p-q) / 2 (2)
[0037] In the above average composition formula (2), R 2They are each independently a monovalent hydrocarbon group having 1 to 12 carbon atoms, preferably 1 to 8 carbon atoms, which may be substituted or unsubstituted, and preferably has no aliphatic unsaturated bond. Specifically, examples include alkyl groups such as methyl group, ethyl group, and propyl group, cycloalkyl groups such as cyclohexyl group, aryl groups such as phenyl group and tolyl group, aralkyl groups such as benzyl group, 2-phenylethyl group, and 2-phenylpropyl group. Note that some or all of the hydrogen atoms of these groups may be substituted with halogen atoms or the like, and examples include 3,3,3-trifluoropropyl group.
[0038] In the above average composition formula (2), p satisfies 0 < p < 3, preferably 0.5 ≤ p ≤ 2.2, more preferably 1.0 ≤ p ≤ 2.0, q satisfies 0 < q ≤ 3, preferably 0.002 ≤ q ≤ 1.1, more preferably 0.005 ≤ q ≤ 1, and p + q is a positive number satisfying 0 < p + q ≤ 3, preferably 1 ≤ p + q ≤ 3, more preferably 1.002 ≤ p + q ≤ 2.7.
[0039] The organohydrogenpolysiloxane preferably has a viscosity of 0.5 to 10,000 mPa·s, particularly 1 to 300 mPa·s at 25°C. In the present invention, the viscosity is measured at 25°C using a rotational viscometer by the method described in JIS K 7117-1:1999. The organohydrogenpolysiloxane preferably has an average degree of polymerization of 1 to 1,000, particularly preferably in the range of 3 to 150, and particularly preferably in the range of 3 to 80. The average degree of polymerization is based on the weight-average molecular weight in terms of polystyrene in GPC (gel permeation chromatography) analysis measured under the above-described conditions.
[0040] Examples of organohydrogenpolysiloxanes include 1,1,3,3-tetramethyldisiloxane, 1,3,5,7-tetramethylcyclotetrasiloxane, tris(hydrogendimethylsiloxy)methylsilane, tris(hydrogendimethylsiloxy)phenylsilane, methylhydrogencyclopolysiloxane, methylhydrogensiloxane-dimethylsiloxane cyclic copolymer, methylhydrogenpolysiloxane blocked at both ends with trimethylsiloxy groups, dimethylsiloxane-methylhydrogensiloxane copolymer blocked at both ends with trimethylsiloxy groups, dimethylpolysiloxane blocked at both ends with dimethylhydrogensiloxy groups, dimethylsiloxane blocked at both ends with dimethylhydrogensiloxy groups, and dimethylsiloxane blocked at both ends with dimethylhydrogensiloxy groups. copolymer of methylsiloxane and methylhydrogensiloxane, copolymer of methylhydrogensiloxane and diphenylsiloxane both ends blocked with trimethylsiloxy groups, copolymer of methylhydrogensiloxane, diphenylsiloxane and dimethylsiloxane both ends blocked with trimethylsiloxy groups, copolymer of methylhydrogensiloxane, methylphenylsiloxane and dimethylsiloxane both ends blocked with trimethylsiloxy groups, copolymer of methylhydrogensiloxane, dimethylsiloxane and diphenylsiloxane both ends blocked with dimethylhydrogensiloxy groups, copolymer of methylhydrogensiloxane, dimethylsiloxane and methylphenylsiloxane both ends blocked with dimethylhydrogensiloxy groups, (CH 3 ) 2 HSiO 1 / 2 Units and (CH 3 ) 3 SiO 1 / 2 Units and SiO 4 / 2 A copolymer consisting of (CH 3 ) 2 HSiO 1 / 2 Units and SiO 4 / 2 A copolymer consisting of (CH 3 ) 2 HSiO 1 / 2 Units and SiO 4 / 2 Units and (C 6 H 5 ) 3 SiO 1 / 2and copolymers consisting of these units, and compounds in which part or all of the methyl groups in the above exemplary compounds have been substituted with other alkyl groups, phenyl groups, or the like.
[0041] The amount of the organohydrogenpolysiloxane is preferably 0.1 to 40 parts by mass per 100 parts by mass of component (A). The ratio of the number of hydrogen atoms bonded to silicon atoms (hydrosilyl groups) to one alkenyl group of component (A) is preferably in the range of 0.5 to 10, and more preferably 0.7 to 5. If the amount is less than the lower limit, crosslinking may be insufficient and sufficient mechanical strength may not be obtained, while if the amount is more than the upper limit, the physical properties after curing may decrease, and in particular the heat resistance of the silicone rubber may become poor or the compression set may become large.
[0042] The hydrosilylation catalyst is a catalyst that causes a hydrosilylation addition reaction between the alkenyl group of the (A) component and the silicon-bonded hydrogen atom (SiH group) of the organohydrogenpolysiloxane. Examples of the hydrosilylation catalyst include platinum group metal catalysts. There are simple platinum group metals and their compounds, and any catalyst for addition reaction curing type silicone rubber compositions that is known in the art may be used. For example, platinum catalysts such as particulate platinum metal adsorbed on a carrier such as silica, alumina, or silica gel, platinic chloride, chloroplatinic acid, and alcohol solutions of chloroplatinic acid hexahydrate, palladium catalysts, and rhodium catalysts may be used, with platinum or platinum compounds (platinum catalysts) being preferred.
[0043] The amount of catalyst added may be any amount that can promote the addition reaction. Usually, the catalyst is used in the range of 1 ppm by mass to 1% by mass, and preferably 10 to 500 ppm by mass, relative to the organopolysiloxane of component (A) in terms of the amount of platinum group metal. If the amount of catalyst is less than the lower limit, the addition reaction is not sufficiently promoted, and curing may be insufficient. If the amount of catalyst exceeds the upper limit, the effect on reactivity is small, and it may be uneconomical. It is also possible to prepare a co-vulcanization type silicone rubber composition that combines addition reaction curing and organic peroxide curing by blending the above-mentioned components (E-1) and (E-2) with the component (A) in the above-mentioned ranges of blending amounts.
[0044] [(F) Dispersants for fillers] In addition to the components (A) to (E), the silicone rubber composition of the present invention may further contain a dispersant for fillers, particularly a dispersant for inorganic fillers or silica. A dispersant for silica is preferred. By further containing the dispersant, the reinforcing silica described above can be well dispersed in the composition. The dispersant may be, for example, a low molecular weight organosilicon compound having an alkoxy group or a silanol group or a hydrolyzate thereof. More specifically, various alkoxysilanes, particularly phenyl group-containing alkoxysilanes and their hydrolyzates, diphenylsilanediol, carbon functional silane, and silanol group-containing low molecular weight siloxane may be used. Among them, the use of diphenylsilanediol is preferred because it further improves the heat resistance of the silicone rubber, and the use of diphenylsilanediol in combination with an alkylalkoxysilane or its hydrolyzate further improves the dispersibility of the filler, which is more preferred.
[0045] The amount of component (F) is preferably 0.1 to 50 parts by mass, and particularly preferably 1 to 20 parts by mass, per 100 parts by mass of component (A). If the amount of the organopolysiloxane capped at both ends with silanol groups used is too small, the effect of adding it will not be observed, whereas if the amount is too large, the plasticity of the composition will be too low, and roll adhesion will occur in kneading means such as a roll mill, which may deteriorate roll workability.
[0046] -Other ingredients- In addition to the above components, the silicone rubber composition used in the present invention may contain other components, such as fillers other than component (B) (crushed quartz, diatomaceous earth, etc.), colorants (pigments), tear strength improvers, flame retardancy improvers (platinum compounds, etc.), acid acceptors, thermal conductivity improvers (alumina, boron nitride, etc.), release agents, reaction regulators, and other known fillers and additives for thermosetting silicone rubber compositions, as long as the effects of the present invention are not impaired. The other components may be used alone or in combination of two or more. The amount of each may be appropriately adjusted as long as the effects of the present invention are not impaired.
[0047] -Method of manufacturing the composition- The millable silicone rubber composition of the present invention can be obtained by mixing the components constituting the composition with a known kneading machine such as a kneader, a Banbury mixer, or a two-roll mill. When using a composition containing the above-mentioned (A) to (E) components as the silicone rubber composition, it is preferable to mix (A) organopolysiloxane, (B) reinforcing silica, (C) titanium oxide doped with a transition metal oxide, and (D) calcium carbonate, and then add (E) a curing agent to the mixture obtained. When the composition containing the above-mentioned (A) to (E) components further contains other components, it is preferable to mix the (A), (B), (C), (D) and other components to obtain a mixture, and then add the (E) component to the mixture.
[0048] -Silicone rubber moldings- The molding method may be selected from known methods depending on the shape and size of the desired molded product, such as casting, compression molding, injection molding, calendar molding, and extrusion molding.
[0049] -Cured product- The curing conditions may be those known for the molding method used, and are generally from a few seconds to a day at a temperature of 60 to 450° C. In addition, for the purposes of reducing the compression set of the obtained cured product, reducing the low molecular weight siloxane components remaining in the obtained silicone rubber, and removing decomposition products of organic peroxides in the silicone rubber, a post cure (secondary cure) may be performed in an oven at 200° C. or higher, preferably 200 to 250° C., for 1 hour or more, preferably 1 to 70 hours, and more preferably 1 to 10 hours. EXAMPLES
[0050] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0051] In the present examples and comparative examples, the evaluations were carried out as follows.
[0052] [Heat resistance] Using a test sheet prepared by curing the silicone rubber composition, the initial values of hardness (Durometer A), tensile strength (MPa), and elongation at break (%) were measured according to JIS K 6249:2003. The test sheet was placed in a dryer at 225°C for 7 days or in a dryer at 260°C for 3 days, after which the hardness, tensile strength, and elongation at break were measured. The results are shown in Tables 1 and 2.
[0053] [Pigmentation] To 100 parts by mass of the silicone rubber composition prepared in the following Examples and Comparative Examples, 0.5 parts by mass of a yellow pigment (product name: KE-COLOR-Y-064, manufactured by Shin-Etsu Chemical Co., Ltd.) was added using a twin roll, and the color tone of the composition before and after mixing was visually confirmed. The results are shown in Tables 1 and 2.
[0054] The organopolysiloxanes (A) used in the examples and comparative examples are as follows: In the following, the mole percentage of each siloxane unit refers to the ratio of the number of each siloxane unit to the total number of siloxane units. Organopolysiloxane raw rubber (A1): Organopolysiloxane raw rubber consisting of 99.825 mol% 3,3,3-trifluoropropylmethylsiloxane units, 0.125 mol% methylvinylsiloxane units, and 0.05 mol% dimethylvinylsiloxy units, with an average degree of polymerization of 4,000 (alkenyl groups per molecule: 7, corresponding to n=2.0005 in the average composition formula (1) above). Organopolysiloxane raw rubber (A2): Organopolysiloxane raw rubber consisting of 40 mol% 3,3,3-trifluoropropylmethylsiloxane units, 59.825 mol% dimethylsiloxane units, 0.125 mol% methylvinylsiloxane units, and 0.05 mol% dimethylvinylsiloxy units, with an average degree of polymerization of 4,000 (alkenyl groups per molecule: 7, corresponding to n=2.0005 in the average composition formula (1) above).
[0055] The component (C) used in the examples and comparative examples was 3% by mass of iron oxide (Fe 2 O 3 ), and titanium oxide doped with said iron oxide (aeroxide TiO 2 PF2, manufactured by Nippon Aerosil Co., Ltd. In Comparative Example 3, titanium oxide not modified with iron oxide (AEROXIDE TiO 2 P25, manufactured by Nippon Aerosil Co., Ltd.) was used. Tables 1 and 2 show the iron oxide content (mass %) in the silicone rubber compositions in the following examples and comparative examples.
[0056] [Example 1] Organopolysiloxane raw rubber (A1) 100 parts by mass, BET specific surface area 200 m 2 40 parts by mass of fumed silica (Aerosil 200, manufactured by Nippon Aerosil Co., Ltd.) having a molecular weight of 1.0 g / g, 5 parts by mass of diphenylsilanediol, and 1.0 part by mass of 3,3,3-trifluoropropylmethylpolysiloxane having silanol groups at both ends, an average degree of polymerization of 4, and a viscosity of 15 mPa s at 25°C were added, and the mixture was heated under mixing in a kneader at 150°C for 2 hours to prepare a base compound (1). Compound (A) was prepared by adding 1.0 part by mass of (C) the above-mentioned titanium oxide containing iron oxide and 1.0 part by mass of (D) calcium carbonate (Silver W, manufactured by Shiraishi Kogyo Co., Ltd.) to 100 parts by mass of organopolysiloxane raw rubber using a twin roll mill. To the compound (A), 0.6 parts by mass of 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane as a curing agent (E) was added per 100 parts by mass of organopolysiloxane raw rubber using a two-roll mill, and the mixture was mixed uniformly to obtain a raw rubber-like silicone rubber composition.
[0057] The silicone rubber composition was subjected to a pressure of 165°C and 70 kgf / cm 2 The test sheet was then post-cured for 4 hours in an oven at 200° C. The cured product was subjected to the above-mentioned heat resistance test.
[0058] [Example 2] A silicone rubber composition was prepared and a cured product was obtained by repeating Example 1, except that the amount of (C) titanium oxide containing iron oxide added was 2.0 parts by mass in Example 1. The obtained cured product was subjected to the heat resistance test described above.
[0059] [Example 3] A silicone rubber composition was prepared and a cured product was obtained by repeating Example 1, except that diphenylsilanediol was not added and 6.0 parts by mass of dimethylpolysiloxane having silanol groups at both ends, an average degree of polymerization of 4, and a viscosity of 15 mPa s at 25°C was used. The heat resistance test described above was performed on the resulting cured product.
[0060] [Example 4] To 100 parts by mass of organopolysiloxane raw rubber, 0.5 parts by mass of a methylhydrogenpolysiloxane blocked with trimethylsiloxy groups at both ends and having hydrosilyl groups on the side chains as a curing agent (degree of polymerization 8, hydrosilyl groups 0.014 mol / g (8 per molecule), corresponding to p=1.4, q=0.8 in the average composition formula (2) above) was added, 0.07 parts by mass of ethynylcyclohexanol as a reaction inhibitor, and 0.15 parts by mass of a platinum catalyst (Pt concentration 1% by mass) were added using a twin roll and mixed uniformly to produce a raw rubber-like silicone rubber composition. The composition was then heated at 150° C. and 70 kgf / cm 2 The test sheet was then post-cured for 4 hours in an oven at 200° C. The cured product was subjected to the above-mentioned heat resistance test.
[0061] [Example 5] A silicone rubber composition was prepared and a cured product was obtained by repeating Example 1, except that the organopolysiloxane raw rubber (A1) was replaced with 100 parts by mass of organopolysiloxane raw rubber (A2). The obtained cured product was subjected to the heat resistance test described above.
[0062] [Comparative Example 1] A silicone rubber composition was prepared and a cured product was obtained by repeating Example 1, except that (D) calcium carbonate was not added in Example 1. The obtained cured product was subjected to the heat resistance test described above.
[0063] [Comparative Example 2] A silicone rubber composition was prepared and a cured product was obtained by repeating Example 1, except that component (C) was not added. The obtained cured product was subjected to the heat resistance test described above.
[0064] [Comparative Example 3] A silicone rubber composition was prepared by repeating Example 1, except that 1.0 part by mass of titanium oxide not modified with iron oxide (AEROXIDE TiO2 P25, manufactured by Nippon Aerosil Co., Ltd.) and 0.03 part by mass of iron oxide (red iron oxide SR-570, manufactured by Tone Sangyo Co., Ltd.) were added per 100 parts by mass of organopolysiloxane raw rubber instead of component (C) in Example 1, and a cured product was obtained. The heat resistance test described above was performed on the obtained cured product.
[0065] [Comparative Example 4] A silicone rubber composition was prepared and a cured product was obtained by repeating Example 4, except that neither component (C) nor component (D) was added. The obtained cured product was subjected to the heat resistance test described above.
[0066] [Comparative Example 5] A silicone rubber composition was prepared and a cured product was obtained by repeating Example 1, except that neither component (C) nor component (D) was added. The obtained cured product was subjected to the heat resistance test described above.
[0067] [Comparative Example 6] Example 1 was repeated, except that component (D) was not added and 1 part by mass of cerium oxide (product name: Cerium Oxide SN-2 (manufactured by Nikki Co., Ltd.) was added instead, to prepare a silicone rubber composition and obtain a cured product. The heat resistance test described above was performed on the obtained cured product.
[0068] [Comparative Example 1] A base compound (2) was prepared by repeating Example 1, except that the organopolysiloxane gum (A1) in Example 1 was replaced with 3,3,3-trifluoropropylmethylpolysiloxane, both ends of which were capped with dimethylvinylsiloxy groups and had an average degree of polymerization of 90. The base compound (2) was in a liquid state and could not be kneaded with a two-roll mill (not shown in Table 1).
[0069] [Table 1]
[0070] [Table 2]
[0071] As shown in Comparative Examples 1 and 2 in Table 2 above, fluorosilicone rubber obtained from a composition containing only either (C) titanium oxide containing iron oxide or (D) calcium carbonate is poor in long-term heat resistance at 225°C and 260°C. In addition, fluorosilicone rubber obtained from a fluorosilicone rubber composition containing titanium oxide containing iron oxide and cerium oxide is also poor in long-term heat resistance at high temperatures (Comparative Example 6). In addition, as shown in Comparative Example 3, silicone rubber obtained from a composition to which titanium oxide and iron oxide are added separately has good long-term heat resistance, but the silicone rubber is colored red even though only a small amount of iron oxide is blended, and coloring with a pigment is impossible. In contrast, as shown in Table 1 above, silicone rubber (cured product) obtained from the fluorosilicone rubber composition of the present invention has excellent heat resistance even under high-temperature long-term storage, can maintain good mechanical properties, and can suppress an increase in hardness of the silicone rubber. Furthermore, since the fluorosilicone rubber composition of the present invention is white, it can be easily colored with a colorant to a desired color. [Industrial Applicability]
[0072] The fluorosilicone rubber composition of the present invention can provide a fluorosilicone rubber (cured product) with excellent heat resistance. That is, the fluorosilicone rubber obtained by the present invention exhibits excellent heat resistance at temperatures of 200°C or higher, particularly at temperatures of 250°C or higher. In addition, an increase in the hardness of the fluorosilicone rubber can be suppressed. Furthermore, since the fluorosilicone rubber composition of the present invention is white, it can be easily colored to a desired color with a coloring agent such as a pigment.
Claims
1. (A) An organopolysiloxane having at least two alkenyl groups bonded to silicon atoms in each molecule, and having siloxane units having at least one fluoroalkyl group in a number of 40% or more based on the total number of siloxane units, and having an average degree of polymerization of 100 or more. 100 parts by mass, (B) Specific surface area 50m 2 / g or more 5 to 100 parts by mass, (C) 0.01 to 10 parts by mass of titanium oxide modified with a transition metal oxide, the titanium oxide containing 0.01 to 5% by mass of the transition metal oxide, (D) Calcium carbonate 0.01 to 10 parts by mass and (E) Hardener 0.1 to 50 parts by mass A millable type fluorosilicone rubber composition comprising:
2. 2. The millable-type fluorosilicone rubber composition according to claim 1, wherein the amount of said transition metal oxide relative to the total mass of said millable-type fluorosilicone rubber composition is 0.005 to 1.0 mass %.
3. 3. The millable type fluorosilicone rubber composition according to claim 1, wherein said transition metal oxide is iron oxide.
4. The millable type fluorosilicone rubber composition according to any one of claims 1 to 3, further comprising (F) 0.1 to 50 parts by mass of a dispersant for fillers.
5. The millable type fluorosilicone rubber composition according to any one of claims 1 to 4, wherein component (A) is a linear organopolysiloxane having an average degree of polymerization of 1,000 to 100,000.
6. 6. The millable type fluorosilicone rubber composition according to claim 1, wherein component (E) is an organic peroxide curing agent, and the amount of component (E) is 0.1 to 10 parts by mass.
7. The millable type fluorosilicone rubber composition according to any one of claims 1 to 5, wherein component (E) is an addition reaction type curing agent, which is a combination of 0.1 to 40 parts by mass of an organohydrogenpolysiloxane and a catalytic amount of a platinum group metal catalyst.
8. 5. The millable type fluorosilicone rubber composition according to claim 4, wherein said component (F) is a dispersant for silica.
9. A cured product of the millable type fluorosilicone rubber composition according to any one of claims 1 to 8.
Citation Information
Patent Citations
High-thermal-conductivity silicone rubber and preparation process thereof
CN105754353A
High-strength, room temperature-curable polyorganosiloxane composition
JP1991149259A
Method for producing metal doped titanium oxide particulate
JP2006021991A
Thermosetting silicone rubber composition
JP2014031408A
Heat resistant silicone rubber composition
JP2016518461A