SUPERABSORBENT POLYMER COMPOSITION AND METHOD FOR PRODUCING SAME
The superabsorbent resin composition addresses odor issues by integrating a surface crosslinked layer with sulfur-containing amino acids and metal iodide salts, maintaining absorption and retention capabilities while effectively reducing malodors.
Patent Information
- Application Number
- JP2023554373
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-12-09
- Filing Date
- 2022-12-14
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-12-14
AI Technical Summary
Superabsorbent resins used in sanitary materials face challenges with odor control due to absorbed liquids, leading to deterioration in usability and a need for improved deodorizing properties without compromising absorption performance.
A superabsorbent resin composition is developed by incorporating a surface crosslinked layer with sulfur-containing amino acids and metal iodide salts, along with other additives, to enhance deodorizing capabilities while maintaining absorption and retention properties.
The composition effectively minimizes odor while preserving or enhancing absorption capacity and retention, offering improved deodorizing power without significant reduction in physical properties.
Smart Images

Figure 0007580853000001 
Figure 0007580853000002 
Figure 0007580853000003
Abstract
Description
[Technical field]
[0001] Cross-references to related applications (etc.) This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0182480 dated December 20, 2021 and Korean Patent Application No. 10-2022-0171681 dated December 9, 2022, and all contents disclosed in the Korean patent applications, etc. are incorporated herein by reference.
[0002] The present invention relates to a superabsorbent polymer composition and a method for producing the same. Specifically, the present invention relates to a superabsorbent polymer composition having deodorizing and antiodor properties and a method for producing the same. [Background technology]
[0003] Super absorbent polymer (SAP) is a synthetic polymeric material that can absorb 500 to 1,000 times its own weight in water, and different companies that develop it give it different names, such as SAM (Super Absorbency Material) or AGM (Absorbent Gel Material). Such super absorbent polymers started to be used as sanitary products, and are now widely used in sanitary products such as baby diapers, as well as in soil water retention agents for gardening, water stoppers for civil engineering and construction, seedling sheets, freshness retention agents in the food distribution field, and materials for sap.
[0004] In most cases, such superabsorbent polymers are widely used in the field of sanitary materials such as diapers and sanitary napkins. In such sanitary materials, the superabsorbent polymer is generally contained in a state of being spread in the pulp. However, in recent years, there have been ongoing efforts to provide sanitary materials such as diapers with thinner thicknesses, and as part of these efforts, the pulp content has been reduced or even so-called pulpless diapers, which do not use pulp at all, have been actively developed.
[0005] In the case of sanitary materials in which the pulp content is reduced or no pulp is used, the superabsorbent polymer is contained at a relatively high ratio, and such superabsorbent polymer particles are inevitably contained in multiple layers in the sanitary materials. In order for the superabsorbent polymer particles contained in the multiple layers as a whole to more efficiently absorb liquids such as urine, the superabsorbent polymer must basically exhibit high absorption performance and absorption speed. In addition, the absorbed liquid must not leak even under external pressure, and in addition, the superabsorbent polymer must have permeability to maintain its original shape well even when swollen after absorbing liquid.
[0006] Therefore, much research has been conducted into improving the basic absorbency and water retention of superabsorbent resins, such as by surface cross-linking.
[0007] However, the superabsorbent polymer may be used in sanitary materials, and in this case, there may be a problem that the feeling of use is deteriorated due to the bad odor of the absorbed liquid such as human and pet excrement. Therefore, there is an increasing demand for the suppression of bad odors as well as the basic physical properties of the superabsorbent polymer, namely, the absorption capacity and water retention capacity. Therefore, there is a need to produce a superabsorbent polymer with deodorizing power. Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention provides a highly water-absorbent polymer composition having a deodorizing or anti-odor ability, and a method for producing the same.
[0009] More specifically, the present invention provides a superabsorbent polymer composition having excellent deodorizing power and a manufacturing method thereof, which minimizes deterioration of the physical properties of the superabsorbent polymer by controlling the combination and mixing ratio of deodorizing substances. [Means for solving the problem]
[0010] In order to solve the above problems, the present invention provides the following superabsorbent resin composition.
[0011] a superabsorbent resin including a base resin containing a crosslinked polymer obtained by crosslinking an acrylic acid monomer having at least a partially neutralized acidic group with an internal crosslinking agent; and a surface crosslinked layer formed on a surface of the base resin, the crosslinked polymer being further crosslinked via a surface crosslinking agent; Contains sulfur-containing amino acids and metal iodide salts.
[0012] The present invention also provides the following method for producing a superabsorbent resin composition.
[0013] A step (step 1) of cross-linking and polymerizing an acrylic acid monomer having at least a partially neutralized acidic group in the presence of an internal cross-linking agent and a polymerization initiator to form a hydrogel polymer; A step (step 2) of producing a base resin containing a crosslinked polymer by drying and pulverizing the hydrogel polymer; A step (step 3) of mixing the base resin with a surface cross-linking liquid to produce a mixture; Step 4: heat-treating the mixture to produce a superabsorbent resin having a surface cross-linked layer formed on the surface of the base resin; (Step 5) mixing the superabsorbent resin with an aqueous solution containing a sulfur-containing amino acid and a metal iodide salt; Includes. Effect of the Invention
[0014] As described above, the present invention is characterized in that it provides a superabsorbent polymer composition having excellent deodorizing power by applying a deodorizing substance in an optimal ratio to the superabsorbent polymer, and a method for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless the context clearly indicates otherwise. In this specification, the terms "include", "comprise", "have" and the like are intended to specify the presence of an implemented feature, step, component, or combination thereof, and should be understood not to preclude the presence or additional possibility of one or more other features, steps, components, or combinations thereof.
[0016] Since the present invention can be modified in various ways and can have various forms, specific embodiments will be illustrated and described in detail below. However, this is not intended to limit the present invention to the specific disclosed forms, and it should be understood that the present invention includes all modifications, equivalents, and alternatives falling within the spirit and technical scope of the present invention.
[0017] Hereinafter, the superabsorbent polymer composition and the preparation method thereof will be described in more detail with reference to specific embodiments of the present invention.
[0018] Prior to that, the terminology used in this specification is merely for the purpose of referring to specific embodiments and is not intended to limit the present invention. Furthermore, the singular forms, etc., used herein also include the plural forms, etc., unless the phrases, etc., clearly indicate the opposite.
[0019] For reference, in this specification, the term "super absorbent polymer" can refer to either the super absorbent polymer itself depending on the context, or a polymer that has been subjected to additional processes such as surface crosslinking, fine powder reassembly, drying, pulverization, classification, etc. to be made into a state suitable for commercialization.
[0020] In addition, in the present specification, the term "base resin" or "base resin powder" refers to a polymer prepared by drying and pulverizing a polymer obtained by polymerizing an acrylic acid monomer into a particle or powder form, and means a polymer in a state in which the surface modification or surface crosslinking step described below has not been performed.
[0021] (Super absorbent resin composition) According to one embodiment of the present invention, a superabsorbent polymer composition is provided.
[0022] The superabsorbent resin composition includes a base resin including a crosslinked polymer obtained by crosslinking an acrylic acid monomer having at least a partially neutralized acidic group with an internal crosslinking agent, a superabsorbent resin including a surface crosslinked layer formed on the surface of the base resin and obtained by further crosslinking the crosslinked polymer via a surface crosslinking agent, a sulfur-containing amino acid, and a metal iodide salt.
[0023] The acrylic acid monomer may be any monomer commonly used in the manufacture of superabsorbent resins. Specifically, the acrylic acid monomer may be a compound represented by the following Chemical Formula 1:
[0024] [Chemical formula 1] R 1 -COOM 1
[0025] In the above Chemical Formula 1, R 1 is an alkyl group having 2 to 5 carbon atoms and containing an unsaturated bond, M 1 is a hydrogen atom, a monovalent or divalent metal, an ammonium group, or an organic amine salt.
[0026] Preferably, the acrylic acid monomer includes at least one selected from the group consisting of acrylic acid, methacrylic acid, and their monovalent metal salts, divalent metal salts, ammonium salts, and organic amine salts.
[0027] The acrylic acid monomer may have an acidic group, and at least a part of the acidic group may be neutralized. Preferably, the monomer may be partially neutralized with an alkaline substance such as sodium hydroxide, potassium hydroxide, or ammonium hydroxide.
[0028] At this time, the neutralization degree of the monomer may be 40 to 95 mol%, 40 to 80 mol%, or 45 to 75 mol%. The range of the neutralization degree may vary depending on the final properties, but if the neutralization degree is too high, the neutralized monomer is precipitated and polymerization is difficult to proceed smoothly, and conversely, if the neutralization degree is too low, the polymer may not only have a significantly reduced absorbency, but also exhibit elastic rubber-like properties that are difficult to handle.
[0029] Meanwhile, in order to improve the physical properties of the resin obtained by polymerization of the acrylic acid monomer, the polymerization is carried out in the presence of a crosslinking agent ("internal crosslinking agent"). The crosslinking agent is for internally crosslinking the hydrogel polymer, and may be used separately from the "surface crosslinking agent" described later.
[0030] As the internal crosslinking agent, any compound can be used as long as it enables the introduction of crosslinking bonds during polymerization of the acrylic acid monomer. Non-limiting examples of the internal crosslinking agent include N,N'-methylenebisacrylamide, trimethylolpropane tri(meth)acrylate, ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, butanediol di(meth)acrylate, butylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, hexanediol di(meth)acrylate, triethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, dipentaerythritol pentaacrylate, glycerin tri(meth)acrylate, pentaerythritol tetraacrylate, triallylamine, allyl (meth)acrylate, ethylene glycol diglycidyl ether, propylene glycol, glycerin, and ethylene carbonate. These crosslinking agents may be used alone or in combination.
[0031] The internal crosslinking agent may be added at a concentration of 0.001 to 1 wt%, or 0.01 to 0.8 wt%, or 0.1 to 0.7 wt% based on the monomer composition. That is, if the concentration of the internal crosslinking agent is too low, the absorption speed of the resin may be slowed and the gel strength may be weakened, which is not preferable. Conversely, if the concentration of the internal crosslinking agent is too high, the absorption power of the resin may be low, which may be unpreferable as an absorbent.
[0032] In addition, the base resin may further contain additives such as a thickener, a plasticizer, a storage stabilizer, and an antioxidant, if necessary.
[0033] The surface cross-linked layer is formed by further cross-linking a cross-linked polymer via a surface cross-linking agent. In this case, the surface cross-linking agent is not particularly limited as long as it is a surface cross-linking agent generally used for surface cross-linking of a highly water-absorbent resin and is a compound capable of reacting with a functional group of the polymer.
[0034] In order to improve the properties of the resulting superabsorbent resin, the surface crosslinking agent may be at least one selected from the group consisting of polyhydric alcohol compounds; epoxy compounds; polyamine compounds; haloepoxy compounds; condensation products of haloepoxy compounds; oxazoline compounds; mono-, di- or polyoxazolidinone compounds; cyclic urea compounds; polyvalent metal salts; and alkylene carbonate compounds.
[0035] Specifically, examples of the polyhydric alcohol compound include one or more selected from the group consisting of mono-, di-, tri-, tetra- or polyethylene glycol, monopropylene glycol, 1,3-propanediol, dipropylene glycol, 2,3,4-trimethyl-1,3-pentanediol, polypropylene glycol, glycerol, polyglycerol, 2-butene-1,4-diol, 1,4-butanediol, 1,3-butanediol, 1,5-pentanediol, 1,6-hexanediol, and 1,2-cyclohexanedimethanol.
[0036] In addition, as the epoxy compound, ethylene glycol diglycidyl ether, glycidol, etc. may be used, and as the polyamine compound, one or more selected from the group consisting of ethylenediamine, diethylenetriamine, triethylenetetraamine, tetraethylenepentamine, pentaethylenehexamine, polyethyleneimine, and polyamidepolyamine may be used.
[0037] As the haloepoxy compound, epichlorohydrin, epibromohydrin, and α-methylepichlorohydrin may be used, while as the mono-, di-, or polyoxazolidinone compound, for example, 2-oxazolidinone may be used.
[0038] As the alkylene carbonate compound, ethylene carbonate or the like may be used. These may be used alone or in combination with each other. On the other hand, in order to increase the efficiency of the surface cross-linking step, one or more of these surface cross-linking agents may be used containing one or more polyhydric alcohol compounds having 2 to 10 carbon atoms.
[0039] The content of the surface crosslinking agent to be added may be appropriately selected depending on the type of the surface crosslinking agent to be specifically added and the reaction conditions, and may be usually used in an amount of about 0.001 to about 5 parts by weight, preferably about 0.01 to about 3 parts by weight, and more preferably about 0.05 to about 2 parts by weight relative to 100 parts by weight of the polymer.
[0040] If the content of the surface cross-linking agent is too low, the surface cross-linking reaction hardly occurs, whereas if the content exceeds 5 parts by weight per 100 parts by weight of the polymer, the surface cross-linking reaction may proceed excessively, resulting in a decrease in absorption capacity and physical properties.
[0041] Meanwhile, the surface cross-linking agent may further include an inorganic material. As the inorganic material, one or more inorganic materials selected from the group consisting of silica, clay, alumina, silica-alumina composite, titania, zinc oxide, and aluminum sulfate may be used. The inorganic material may be used in a powder or liquid form, and in particular, alumina powder, silica-alumina powder, titania powder, or nanosilica solution may be used. Also, the inorganic material may be used in an amount of about 0.001 to about 1 part by weight based on 100 parts by weight of the base resin.
[0042] The surface cross-linking agent may further include a thickener. When the surface of the base resin powder is further cross-linked in the presence of the thickener, the deterioration of physical properties after pulverization can be minimized. Specifically, the thickener may be one or more selected from polysaccharides and hydroxy-containing polymers. As the polysaccharide, a gum-based thickener, a cellulose-based thickener, etc. may be used. Specific examples of the gum-based thickener include xanthan gum, gum arabic, karaya gum, tragacanth gum, ghatti gum, guar gum, locust bean gum, and psyllium seed gum, while specific examples of the cellulose-based thickener include hydroxypropylmethylcellulose, carboxymethylcellulose, methylcellulose, hydroxymethylcellulose, hydroxyethylcellulose, hydroxypropylcellulose, hydroxyethylmethylcellulose, hydroxymethylpropylcellulose, hydroxyethylhydroxypropylcellulose, ethylhydroxyethylcellulose, and methylhydroxypropylcellulose, while specific examples of the hydroxy-containing polymer include polyethylene glycol and polyvinyl alcohol.
[0043] The sulfur-containing amino acid and the metal iodide salt may be included in an amount of 0.1 to 1.5 parts by weight and 0.001 to 0.05 parts by weight, respectively, based on 100 parts by weight of the base resin. The sulfur-containing amino acid may be added to the superabsorbent resin to impart deodorizing properties. Specifically, the sulfur-containing amino acid may include one or more selected from the group consisting of cysteine, cystine, and methionine. More specifically, the sulfur-containing amino acid may include cysteine or methionine.
[0044] The metal iodide salt is a form in which one or more selected from the group consisting of CuI, NaI, and KI are dissolved in water together with I2. The metal iodide salt can also be added to the superabsorbent resin in the same manner as the sulfur-containing amino acid to impart deodorizing properties.
[0045] Sulfur-containing amino acids can capture malodorous substances by chemically reacting with them. Malodorous substances generally have small molecular weights, and when they react with sulfur-containing amino acids, the malodor is reduced or turned into a substance with no malodor, effectively removing the malodor. In particular, sulfur-containing amino acids are effective in reducing the malodor of aldehyde and ketone compounds.
[0046] Metal iodide salts remove malodorous substances by oxidizing them, and are generally effective as they act on most malodorous substances.
[0047] The sulfur-containing amino acid may be included in an amount of 0.1 to 1.5 parts by weight based on 100 parts by weight of the base resin. Specifically, the sulfur-containing amino acid may be included in an amount of 0.1 parts by weight or more, 0.13 parts by weight or more, or 0.15 parts by weight or more, and 1.5 parts by weight or less, 1.2 parts by weight or less, 1.0 parts by weight or less, 0.8 parts by weight or less, 0.6 parts by weight or less, 0.5 parts by weight or less, 0.4 parts by weight or less, 0.3 parts by weight or less, or 0.2 parts by weight or less.
[0048] The metal iodide salt may be included in an amount of 0.001 to 0.05 parts by weight based on 100 parts by weight of the base resin, specifically, the metal iodide salt may be included in an amount of 0.001 parts by weight or more, 0.005 parts by weight or more, 0.01 parts by weight or more, 0.015 parts by weight or more, or 0.02 parts by weight or more, and 0.05 parts by weight or less, 0.04 parts by weight or less, 0.03 parts by weight or less, or 0.025 parts by weight or less.
[0049] If the sulfur-containing amino acid is contained in an excessively small amount, the deodorizing properties may not be realized, and if it is contained in an excessively large amount, the inherent physical properties of the superabsorbent polymer may be deteriorated, and processing problems may occur due to incomplete dissolution.
[0050] In addition, if the amount of metal iodide salt is too small, the deodorizing properties may not be fully realized, while if the amount is too large, the inherent physical properties of the superabsorbent polymer may be reduced. In addition, since the superabsorbent polymer is supplied as a solution in the process, the amount of waste may increase, which may result in a decrease in the deodorizing power.
[0051] The sulfur-containing amino acid and the metal iodide are mixed with the superabsorbent resin in the form of an aqueous solution using water as a solvent, and are present in the superabsorbent resin in a state where they are mixed and physically trapped in the superabsorbent resin. The metal iodide solution may be a solution with a solids concentration of 1% or less.
[0052] In addition, the base resin further contains a polymerizable antibacterial monomer as a monomer in an amount of 5 parts by weight or less per 100 parts by weight of the acrylic acid monomer, thereby imparting antibacterial properties as well as deodorizing properties to the superabsorbent resin. The polymerizable antibacterial monomer may be in the form of a polymerizable quaternary ammonium salt represented by the following chemical formula 2.
[0053] [ka]
[0054] In the above formula 2, R and R are each a substituted or unsubstituted C 1-30 Alkylene, C 1-30 Alkoxylen, C 6-30 C containing at least one selected from the group consisting of arylene, N, O, and S 5-30 R and R may be substituted or unsubstituted C 1-30 Alkyl, C 1-30 Alkoxy, C 6-30 C containing one or more selected from the group consisting of aryl, N, O, and S 5-30 It may be heteroaryl.
[0055] Specifically, the polymerizable quaternary ammonium salt may be at least one selected from the group consisting of cetethyldimonium bromide, myristyl betaine, and octenidine HCl.
[0056] The polymerizable antibacterial monomer may be included in an amount of 0.5 parts by weight or more, 1 part by weight or more, 1.5 parts by weight or more, or 1.8 parts by weight or more, and 5 parts by weight or less, 4 parts by weight or less, 3 parts by weight or less, or 2 parts by weight or less, based on 100 parts by weight of the acrylic acid monomer. If antibacterial effect is not the objective, the polymerizable antibacterial monomer may not be included, but if too little polymerizable antibacterial monomer is mixed to obtain antibacterial effect, the effect cannot be obtained. On the other hand, if too much polymerizable antibacterial monomer is included, there may be a problem that the water retention and absorption ability that a superabsorbent resin should have is reduced.
[0057] Also, zirconium phosphate may be further included in an amount of 5.0 parts by weight or less based on 100 parts by weight of the base resin. In this case, zirconium phosphate may be mixed in advance in a dry manner in the drying and pulverizing step of the base resin. That is, zirconium phosphate may be mixed in a solid state in the base resin before surface crosslinking in a dry physical manner. Zirconium phosphate is a material that can physically adsorb malodorous substances. Therefore, further mixing zirconium phosphate into the base resin powder can provide a further deodorizing effect.
[0058] In this case, zirconium phosphate may be included in an amount of 5.0 parts by weight or less based on 100 parts by weight of the base resin. Zirconium phosphate is for further increasing the deodorizing power and may not be included, but when included, it may be specifically included in an amount of 0.5 parts by weight or more, 0.8 parts by weight or more, 1.0 parts by weight or more, 1.3 parts by weight or more, 1.5 parts by weight or more, or 1.8 parts by weight or more and 5.0 parts by weight or less, 4.0 parts by weight or less, 3.0 parts by weight or less, or 2.0 parts by weight or less. If too little zirconium phosphate is mixed, there is a problem that the deodorizing effect is negligible, and if too much is included, there may be a problem that the surface cross-linking is not performed well, resulting in a decrease in absorbency under pressure.
[0059] The surface cross-linked layer may further contain a solid content of tannin, which chemically bonds with volatile malodorous substances such as aldehydes and can impart deodorizing power to the highly water-absorbent resin.
[0060] The tannin solid content may be 0.05 parts by weight or less relative to 100 parts by weight of the base resin. Tannin is for imparting further deodorizing properties to the superabsorbent resin, so it may not be included, but if it is included, it may be specifically 0.005 parts by weight or more, 0.015 parts by weight or more, or 0.025 parts by weight or more, and 0.05 parts by weight or less, 0.04 parts by weight or less, or 0.03 parts by weight or less relative to 100 parts by weight of the base resin. If too little tannin is mixed, there is a problem that the deodorizing effect is negligible, and if too much is included, there may be a problem that the physical properties of the superabsorbent resin are reduced, such as reduced absorption capacity and absorbency under pressure.
[0061] (Method of producing superabsorbent resin composition) According to one embodiment of the present invention, there is provided a method for preparing a superabsorbent polymer composition.
[0062] The method for producing the superabsorbent resin composition includes the steps of: The method includes the steps of: forming a hydrogel polymer by crosslinking and polymerizing an acrylic acid monomer having at least a partially neutralized acidic group in the presence of an internal crosslinking agent and a polymerization initiator; producing a base resin containing a crosslinked polymer by pulverizing and drying the hydrogel polymer; mixing the base resin with a surface crosslinking liquid to produce a mixture; heat-treating the mixture to produce a superabsorbent resin having a surface crosslinked layer formed on the surface of the base resin; and mixing the superabsorbent resin with an aqueous solution containing a sulfur-containing amino acid and a metal iodide salt.
[0063] The method for producing superabsorbent resin mainly includes the steps of polymerizing acrylic acid monomers to produce a hydrogel polymer and pulverizing the polymer. In order to improve various properties of the superabsorbent resin, a method of crosslinking the surface of the produced superabsorbent resin is used.
[0064] The present invention aims to provide a superabsorbent polymer composition having deodorizing properties by mixing a deodorizing substance with the surface-crosslinked superabsorbent polymer.
[0065] The present invention will now be described in detail for each step.
[0066] (Step 1) Step 1 is a step of producing a hydrogel polymer, specifically, a step of cross-linking and polymerizing a monomer composition including an acrylic acid monomer having at least a partially neutralized acid group to form a hydrogel polymer.
[0067] The acrylic acid monomer may be any monomer commonly used in the manufacture of superabsorbent resins. Specifically, the acrylic acid monomer may be a compound represented by the following Chemical Formula 1:
[0068] [Chemical formula 1] R 1 -COOM 1
[0069] In the above Chemical Formula 1, R1 is an alkyl group having 2 to 5 carbon atoms and containing an unsaturated bond, M 1 is a hydrogen atom, a monovalent or divalent metal, an ammonium group, or an organic amine salt.
[0070] Preferably, the acrylic acid monomer includes at least one selected from the group consisting of acrylic acid, methacrylic acid, and their monovalent metal salts, divalent metal salts, ammonium salts, and organic amine salts.
[0071] The acrylic acid monomer may have an acidic group, and at least a part of the acidic group may be neutralized. Preferably, the monomer may be partially neutralized with an alkaline substance such as sodium hydroxide, potassium hydroxide, or ammonium hydroxide.
[0072] At this time, the neutralization degree of the monomer may be 40 to 95 mol%, 40 to 80 mol%, or 45 to 75 mol%. The range of the neutralization degree may vary depending on the final properties, but if the neutralization degree is too high, the neutralized monomer is precipitated and polymerization is difficult to proceed smoothly, and conversely, if the neutralization degree is too low, the polymer may not only have a significantly reduced absorbency, but also exhibit elastic rubber-like properties that are difficult to handle.
[0073] In addition, the present invention may further include a polymerizable antibacterial monomer in order to impart antibacterial properties as well as deodorizing properties to the superabsorbent resin. Specifically, the polymerizable antibacterial monomer may be included in an amount of 5 parts by weight or less based on 100 parts by weight of the acrylic acid monomer. The polymerizable antibacterial monomer may be in the form of a polymerizable quaternary ammonium salt represented by the following chemical formula 2.
[0074] [ka]
[0075] In the above formula 2, R and R are each a substituted or unsubstituted C 1-30 Alkylene, C 1-30 Alkoxylen, C 6-30C containing at least one selected from the group consisting of arylene, N, O, and S 5-30 R and R may be substituted or unsubstituted C 1-30 Alkyl, C 1-30 Alkoxy, C 6-30 C containing one or more selected from the group consisting of aryl, N, O, and S 5-30 It may be heteroaryl.
[0076] Specifically, the polymerizable quaternary ammonium salt may be cetethyldimonium bromide, myristyl betaine, and octenidine HCl.
[0077] The polymerizable antibacterial monomer may be included in an amount of 0.5 parts by weight or more, 1 part by weight or more, 1.5 parts by weight or more, or 1.8 parts by weight or more, and 5 parts by weight or less, 4 parts by weight or less, 3 parts by weight or less, or 2 parts by weight or less, based on 100 parts by weight of the acrylic acid monomer. If antibacterial effect is not the objective, the polymerizable antibacterial monomer may not be included, but if too little polymerizable antibacterial monomer is mixed to obtain antibacterial effect, the effect cannot be obtained. On the other hand, if too much polymerizable antibacterial monomer is included, there may be a problem that the water retention and absorption ability that a superabsorbent resin should have is reduced.
[0078] The monomer composition may contain a polymerization initiator that is generally used in the production of highly water-absorbent resins.
[0079] The polymerization initiator may be a thermal polymerization initiator or a photopolymerization initiator depending on the polymerization method. However, since a certain amount of heat is generated by irradiation with ultraviolet light, etc., even in the photopolymerization method, and a certain amount of heat is generated by the progress of an exothermic polymerization reaction, a thermal polymerization initiator may be further included.
[0080] The photopolymerization initiator may be one or more compounds selected from the group consisting of benzoin ether, dialkyl acetophenone, hydroxyl alkyl ketone, phenyl glyoxylate, benzyl dimethyl ketal, acyl phosphine, and alpha-aminoketone. Among them, a specific example of the acylphosphine may be commonly used lucirin TPO, i.e., 2,4,6-trimethyl-benzoyl-trimethylphosphine oxide. More various photopolymerization initiators are disclosed in Reinhold Schwalm's book "UV Coatings: Basics, Recent Developments and New Application" (Elsevier, 2007), page 115, which may be referred to.
[0081] The thermal polymerization initiator may be one or more compounds selected from the group consisting of persulfate initiators, azo initiators, hydrogen peroxide, and ascorbic acid. Specifically, the persulfate initiator may be sodium persulfate (Na2S2O8), potassium persulfate (K2S2O8), ammonium persulfate ((NH4)2S2O8), etc. In addition, the azo initiator may be 2,2-azobis(2-amidinopropane) dihydrochloride, 2,2-azobis-(N,N-dimethylene)isobutyramidine dihydrochloride, etc. dihydrochloride, 2-(carbamoylazo)isobutylonitril, 2,2-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 4,4-azobis-(4-cyanovaleric acid), etc. More various thermal polymerization initiators are disclosed on page 203 of "Principle of Polymerization" by Odian (Wiley, 1981), which can be referred to.
[0082] The polymerization initiator may be added at a concentration of 0.001 to 1% by weight, or 0.005 to 0.1% by weight, based on the monomer composition. That is, if the concentration of the polymerization initiator is too low, the polymerization rate is slowed down, and a large amount of residual monomer may be extracted in the final product, which is not preferable. Conversely, if the concentration of the polymerization initiator is too high, the polymer chains forming the network are shortened, the content of water-soluble components is increased, and the compression absorption capacity is reduced, which is not preferable, and thus the physical properties of the resin may be deteriorated.
[0083] Meanwhile, the polymerization of the monomer composition is carried out in the presence of a crosslinking agent ("internal crosslinking agent") in order to improve the physical properties of the resin obtained by the polymerization of the acrylic acid monomer. The crosslinking agent is for internally crosslinking the hydrogel polymer, and may be used separately from the "surface crosslinking agent" described below.
[0084] As the internal crosslinking agent, any compound can be used as long as it enables the introduction of crosslinking bonds during polymerization of the acrylic acid monomer. Non-limiting examples of the internal crosslinking agent include N,N'-methylenebisacrylamide, trimethylolpropane tri(meth)acrylate, ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, butanediol di(meth)acrylate, butylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, hexanediol di(meth)acrylate, triethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, dipentaerythritol pentaacrylate, glycerin tri(meth)acrylate, pentaerythritol tetraacrylate, triallylamine, allyl (meth)acrylate, ethylene glycol diglycidyl ether, propylene glycol, glycerin, and ethylene carbonate. These crosslinking agents may be used alone or in combination.
[0085] The internal crosslinking agent may be added at a concentration of 0.001 to 1 wt%, or 0.01 to 0.8 wt%, or 0.1 to 0.7 wt% based on the monomer composition. That is, if the concentration of the internal crosslinking agent is too low, the absorption speed of the resin may be slowed and the gel strength may be weakened, which is not preferable. Conversely, if the concentration of the internal crosslinking agent is too high, the absorption power of the resin may be low, which may be unpreferable as an absorbent.
[0086] In addition, the cross-linking polymerization of the monomer composition may be carried out in the presence of a foaming agent depending on the necessity and degree of improvement in the absorption rate. The foaming agent is decomposed during the cross-linking polymerization reaction to generate gas, which can form pores in the hydrogel polymer. As a result, when the foaming agent is additionally used, a more developed porous structure is formed in the superabsorbent resin, and the absorption rate of the superabsorbent resin can be further improved.
[0087] Non-limiting examples of the foaming agent include sodium bicarbonate, sodium carbonate, potassium bicarbonate, potassium carbonate, calcium bicarbonate, calcium carbonate, magnesium bicarbonate, magnesium carbonate, azodicarbonamide (ADCA), dinitroso pentamethylene tetramine (DPT), p,p'-oxybis(benzenesulfonyl hydrazide (OBSH), p-toluenesulfonyl hydrazide (TSH), sucrose stearate (SSC ... The composition may include one or more compounds selected from the group consisting of sucrose stearate, sucrose palmitate, and sucrose laurate.
[0088] The blowing agent may be present in the monomer composition in an amount of 1000 to 4000 ppmw, more specifically, in an amount of 1000 ppm or more, alternatively 1100 ppmw or more, alternatively 1200 ppmw or more; and 4000 ppmw or less, alternatively 3500 ppmw or less, alternatively 3000 ppmw or less.
[0089] In addition, the monomer composition may further contain additives such as a thickener, a plasticizer, a storage stabilizer, and an antioxidant, if necessary.
[0090] The monomer composition may be prepared in the form of a solution in which raw materials such as the acrylic acid monomer, the polymerization initiator, the internal crosslinking agent, and the foaming agent are dissolved in a solvent.
[0091] In this case, the solvent that can be used may be any solvent capable of dissolving the above-mentioned raw materials, without being limited in composition. For example, the solvent may be water, ethanol, ethylene glycol, diethylene glycol, triethylene glycol, 1,4-butanediol, propylene glycol, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, methyl ethyl ketone, acetone, methyl amyl ketone, cyclohexanone, cyclopentanone, diethylene glycol monomethyl ether, diethylene glycol ethyl ether, toluene, xylene, butyrolactone, carbitol, methyl cellosolve acetate, N,N-dimethylacetamide, or a mixture thereof.
[0092] The formation of the hydrogel polymer through polymerization of the monomer composition may be carried out by a conventional polymerization method, and the process is not particularly limited.
[0093] As a non-limiting example, the polymerization method can be largely divided into thermal polymerization and photopolymerization depending on the type of polymerization energy source. When the thermal polymerization is performed, it may be performed in a reactor having a stirring shaft such as a kneader, and when the photopolymerization is performed, it may be performed in a reactor equipped with a movable conveyor belt.
[0094] For example, the monomer composition is introduced into a reactor such as a kneader equipped with an agitator shaft, and hot air is supplied thereto or the reactor is heated to thermally polymerize the monomer composition to obtain a hydrogel polymer. Depending on the type of agitator shaft installed in the reactor, the hydrogel polymer is discharged from the outlet of the reactor in the form of particles of several millimeters to several centimeters in size. Specifically, the hydrogel polymer obtained is obtained in various forms depending on the concentration of the monomer composition injected and the injection speed, but the hydrogel polymer obtained usually has a (weight average) particle size of 2 to 50 mm.
[0095] As another example, when the photopolymerization of the monomer composition is carried out in a reactor equipped with a movable conveyor belt, a hydrogel polymer in the form of a sheet is obtained. In this case, the thickness of the sheet may vary depending on the concentration and injection speed of the monomer composition to be injected, but it is generally preferable to adjust the thickness to 0.5 to 10 cm in order to ensure the production speed while ensuring uniform polymerization of the entire sheet.
[0096] The hydrogel polymer formed in this manner may exhibit a water content of 40 to 80% by weight. Here, the water content is the weight of water in the total weight of the hydrogel polymer, and may be a value obtained by subtracting the weight of the polymer in a dry state from the weight of the hydrogel polymer. Specifically, it may be defined as a value calculated by measuring the weight loss due to evaporation of water in the polymer during the process of drying by increasing the temperature of the polymer through infrared heating. Here, the drying conditions may be a method of increasing the temperature to about 180°C from room temperature and then maintaining it at 180°C, and the total drying time may be set to 20 minutes, including a 5-minute temperature increase step.
[0097] (Step 2) Step 2 of the present invention is a step of drying, pulverizing and classifying the hydrogel polymer previously produced in step 1 to form a base resin powder.
[0098] Specifically, the method not only increases the drying efficiency of the hydrogel polymer, but also affects the morphology of the superabsorbent polymer and various physical properties of the superabsorbent polymer, including the absorption rate, and in particular, in order to improve the absorption rate of the superabsorbent polymer, the present invention may further include a step of coarsely pulverizing the hydrogel polymer before drying. Hereinafter, for the sake of convenience, the term "coarse pulverization" is used in this specification for pulverization before drying, in order to distinguish it from pulverization after drying.
[0099] The pulverizer used for the pulverization is not limited in structure, and may specifically include any one selected from the group of pulverizing devices consisting of a vertical pulverizer, a turbo cutter, a turbo grinder, a rotary cutter mill, a cutter mill, a disc mill, a shred crusher, a crusher, a chopper, and a disc cutter, but is not limited to the above examples.
[0100] In this case, the coarse pulverization step may be performed so that the hydrogel polymer has a particle size of about 2 mm to about 10 mm. It is technically difficult to pulverize the hydrogel polymer to a particle size of less than 2 mm due to the high water content of the hydrogel polymer, and the pulverized particles may aggregate with each other. On the other hand, if the hydrogel polymer is pulverized to a particle size of more than 10 mm, the effect of increasing the efficiency of the subsequent drying step may be insignificant.
[0101] The drying may be performed at a temperature of 120 to 250°C, 140 to 200°C, or 150 to 190°C. Here, the drying temperature may be defined as the temperature of the heat medium supplied for drying or the temperature inside the drying reactor containing the heat medium and the polymer in the drying process. If the drying temperature is low and the drying time is long, the process efficiency decreases, so in order to prevent this, the drying temperature is preferably 120°C or more. In addition, if the drying temperature is higher than necessary, the surface of the hydrogel polymer is excessively dried, which may increase the generation of fine powder in the subsequent pulverization step and deteriorate the physical properties of the final resin. In order to prevent this, the drying temperature is preferably 250°C or less.
[0102] At this time, the drying time in the drying step is not particularly limited, but may be adjusted to 20 to 90 minutes at the drying temperature in consideration of process efficiency and the physical properties of the resin.
[0103] The drying is carried out using a common medium, but may also be carried out by, for example, supplying hot air to the pulverized hydrogel polymer, irradiating it with infrared rays, ultrashort waves, or ultraviolet rays.
[0104] It is preferable that the drying is performed so that the dried polymer has a moisture content of 0.1 to 10% by weight. That is, if the moisture content of the dried polymer is less than 0.1% by weight, it is not preferable because excessive drying may cause an increase in manufacturing costs and degradation of the crosslinked polymer. If the moisture content of the dried polymer exceeds 10% by weight, it is not preferable because defects may occur in the subsequent process.
[0105] The dried hydrogel polymer may then be pulverized, a step to optimize the surface area of the base resin powder and the superabsorbent polymer, and the pulverization may be performed so that the particle size of the pulverized polymer is between 150 and 850 μm.
[0106] In this case, the pulverizer used may be a conventional one such as a pin mill, a hammer mill, a screw mill, a roll mill, a disc mill, or a jog mill.
[0107] In addition, in order to control the physical properties of the superabsorbent resin to be manufactured as a final product, a step of selectively classifying the polymer particles obtained through the pulverization step into particles having a particle size of 150 to 850 μm is carried out.
[0108] The base resin powder is obtained through the above classification steps. Such base resin powder has a particle size of 150 to 850 μm, and may contain 2% by weight or less, or 1% by weight or less of fine powder having a particle size of less than 150 μm.
[0109] Also, the method may further include a step of mixing zirconium phosphate after obtaining the base resin powder by drying and pulverization. In this case, zirconium phosphate may be mixed in advance by dry mixing. That is, zirconium phosphate may be mixed as a solid content in the base resin before surface crosslinking by a dry physical method. Zirconium phosphate is a material that can physically adsorb malodorous substances. Therefore, further mixing of zirconium phosphate into the base resin powder can provide a further deodorizing effect.
[0110] In this case, zirconium phosphate may be included in an amount of 5.0 parts by weight or less based on 100 parts by weight of the base resin. Zirconium phosphate is for further increasing the deodorizing power and may not be included, but when included, it may be specifically included in an amount of 0.5 parts by weight or more, 0.8 parts by weight or more, 1.0 parts by weight or more, 1.3 parts by weight or more, 1.5 parts by weight or more, or 1.8 parts by weight or more and 5.0 parts by weight or less, 4.0 parts by weight or less, 3.0 parts by weight or less, or 2.0 parts by weight or less. If too little zirconium phosphate is mixed, there is a problem that the deodorizing effect is negligible, and if too much is included, there may be a problem that surface cross-linking is not performed well and absorption capacity under pressure is reduced.
[0111] (Step 3) Step 3 of the present invention is a step of mixing the base resin powder produced in step 2 with a surface cross-linking liquid.
[0112] The surface cross-linking liquid used in step 3 contains a surface cross-linking agent. The surface cross-linking agent is not particularly limited as long as it is a surface cross-linking agent generally used for surface cross-linking of a superabsorbent resin and is a compound capable of reacting with a functional group possessed by the polymer.
[0113] Preferably, in order to improve the properties of the resulting superabsorbent resin, the surface crosslinking agent may be one or more selected from the group consisting of polyhydric alcohol compounds; epoxy compounds; polyamine compounds; haloepoxy compounds; condensation products of haloepoxy compounds; oxazoline compounds; mono-, di- or polyoxazolidinone compounds; cyclic urea compounds; polyvalent metal salts; and alkylene carbonate compounds.
[0114] Specifically, examples of the polyhydric alcohol compound include one or more selected from the group consisting of mono-, di-, tri-, tetra- or polyethylene glycol, monopropylene glycol, 1,3-propanediol, dipropylene glycol, 2,3,4-trimethyl-1,3-pentanediol, polypropylene glycol, glycerol, polyglycerol, 2-butene-1,4-diol, 1,4-butanediol, 1,3-butanediol, 1,5-pentanediol, 1,6-hexanediol, and 1,2-cyclohexanedimethanol.
[0115] In addition, as the epoxy compound, ethylene glycol diglycidyl ether, glycidol, etc. may be used, and as the polyamine compound, one or more selected from the group consisting of ethylenediamine, diethylenetriamine, triethylenetetraamine, tetraethylenepentamine, pentaethylenehexamine, polyethyleneimine, and polyamidepolyamine may be used.
[0116] As the haloepoxy compound, epichlorohydrin, epibromohydrin, and α-methylepichlorohydrin may be used, while as the mono-, di-, or polyoxazolidinone compound, for example, 2-oxazolidinone may be used.
[0117] As the alkylene carbonate compound, ethylene carbonate or the like may be used. These may be used alone or in combination with each other. On the other hand, in order to increase the efficiency of the surface cross-linking step, one or more of these surface cross-linking agents may be used containing one or more polyhydric alcohol compounds having 2 to 10 carbon atoms.
[0118] The content of the surface crosslinking agent to be added may be appropriately selected depending on the type of the surface crosslinking agent to be specifically added and the reaction conditions, and may be usually used in an amount of about 0.001 to about 5 parts by weight, preferably about 0.01 to about 3 parts by weight, and more preferably about 0.05 to about 2 parts by weight relative to 100 parts by weight of the polymer.
[0119] If the content of the surface cross-linking agent is too low, the surface cross-linking reaction hardly occurs, whereas if the content exceeds 5 parts by weight per 100 parts by weight of the polymer, the surface cross-linking reaction proceeds excessively, resulting in a decrease in absorption capacity and physical properties.
[0120] Meanwhile, the surface cross-linking liquid may further contain an inorganic material to perform a step of forming a surface cross-linked layer. As the inorganic material, one or more inorganic materials selected from the group consisting of silica, clay, alumina, silica-alumina composite, titania, zinc oxide, and aluminum sulfate may be used. The inorganic material may be used in a powder or liquid form, and in particular, alumina powder, silica-alumina powder, titania powder, or nanosilica solution may be used. Also, the inorganic material may be used in an amount of about 0.001 to about 1 part by weight based on 100 parts by weight of the base resin.
[0121] In addition, the surface cross-linking liquid may further include a thickener. In this way, when the surface of the base resin powder is further cross-linked in the presence of a thickener, it is possible to minimize the deterioration of physical properties even after pulverization. Specifically, the thickener may be one or more selected from polysaccharides and hydroxy-containing polymers. As the polysaccharide, a gum-based thickener, a cellulose-based thickener, etc. may be used. Specific examples of the gum-based thickener include xanthan gum, gum arabic, karaya gum, tragacanth gum, ghatti gum, guar gum, locust bean gum, and psyllium seed gum, while specific examples of the cellulose-based thickener include hydroxypropylmethylcellulose, carboxymethylcellulose, methylcellulose, hydroxymethylcellulose, hydroxyethylcellulose, hydroxypropylcellulose, hydroxyethylmethylcellulose, hydroxymethylpropylcellulose, hydroxyethylhydroxypropylcellulose, ethylhydroxyethylcellulose, and methylhydroxypropylcellulose, while specific examples of the hydroxy-containing polymer include polyethylene glycol and polyvinyl alcohol.
[0122] The surface cross-linking liquid may further contain a tannin solution in addition to the surface cross-linking agent. Tannin can chemically bind to volatile malodorous substances such as aldehydes and impart deodorizing power to the highly water-absorbent resin.
[0123] The tannin solution may be contained in an amount of 1.0 part by weight or less relative to 100 parts by weight of the base resin. Tannin is for imparting further deodorizing properties to the superabsorbent resin, so it may not be contained, but when it is contained, it may be specifically 0.1 part by weight or more, 0.3 parts by weight or more, or 0.5 parts by weight or more and 1.0 part by weight or less, 0.8 parts by weight or less, or 0.6 parts by weight or less relative to 100 parts by weight of the base resin. If too little tannin is mixed, there is a problem that the deodorizing effect is negligible, and if too much tannin is mixed, there may be a problem that the physical properties of the superabsorbent resin, such as the absorption capacity and the absorption capacity under pressure, are reduced. In this case, the solid content concentration of the tannin solution may be 0.1% by weight or more to 5% or less.
[0124] Specifically, the tannin solids content may be 0.005 parts by weight or more, 0.015 parts by weight or more, or 0.025 parts by weight or more, and 0.05 parts by weight or less, 0.04 parts by weight or less, or 0.03 parts by weight or less, based on 100 parts by weight of the base resin.
[0125] On the other hand, the method of mixing the surface cross-linking liquid with the base resin is not particularly limited as long as the method can uniformly mix the surface cross-linking liquid with the base resin, and any method may be appropriately selected and used.
[0126] For example, a method in which the surface crosslinking liquid is placed in a reaction tank and the base resin is mixed, a method in which the surface crosslinking liquid is sprayed onto the base resin, a method in which the base resin and the surface crosslinking liquid are continuously supplied to a continuously operated mixer and mixed, or the like may be used.
[0127] In this case, the surface crosslinking liquid may be a solution, and when the content of solids in the solution is 1 wt% or more, 3 wt% or more, 5 wt% or more, 10 wt% or more, or 50 wt% or less, 30 wt% or less, or 20 wt% or less, it is suitable for uniform dispersion in the base resin and can prevent the aggregation phenomenon of the base resin.
[0128] (Step 4) Step 4 is a step for reacting the base resin with the surface cross-linking liquid to form an interpenetrating polymer network on the surface of the cross-linked polymer contained in the base resin, thereby further improving the physical properties of the superabsorbent resin. A surface cross-linked layer is formed on the surface of the pulverized base resin particles by such surface modification.
[0129] The formation of the surface cross-linked layer may be performed by a conventional method for increasing the cross-linking density on the surface of the polymer particles, for example, by mixing the pulverized polymer with a surface cross-linking liquid containing a surface cross-linking agent and heat-treating the mixture to cause a cross-linking reaction.
[0130] The step 4 may be carried out at a temperature of about 80° C. to about 250° C. More specifically, the surface cross-linking process may be carried out at a temperature of about 100° C. to about 220° C., about 110° C. to about 200° C., or about 120° C. to about 190° C. for about 10 minutes to about 2 hours, or about 20 minutes to about 60 minutes. If the cross-linking reaction temperature is less than 80° C. or the reaction time is too short, the surface cross-linking reaction may not proceed properly, resulting in low permeability, and if it exceeds 200° C. or the reaction time is too long, a problem of reduced water retention may occur.
[0131] The temperature raising means for the surface crosslinking reaction is not particularly limited. Heating may be performed by supplying a heat medium or directly supplying a heat source. In this case, the type of heat medium that can be used may be a heated fluid such as steam, hot air, or hot oil, but the present invention is not limited thereto, and the temperature of the heat medium to be supplied may be appropriately selected in consideration of the means of the heat medium, the heating rate, and the target temperature of the heat raising. On the other hand, examples of the heat source to be directly supplied include heating by electricity and heating by gas, but the present invention is not limited to the above-mentioned examples.
[0132] (Step 5) The step 5 is a step of mixing a solution containing a sulfur-containing amino acid and a metal iodide salt with a superabsorbent resin having a surface cross-linked layer formed on a base resin. That is, the step 5 is a step of mixing a solution containing a sulfur-containing amino acid and a metal iodide salt with a superabsorbent resin to obtain a superabsorbent resin composition.
[0133] The sulfur-containing amino acid can be added to the superabsorbent resin to impart deodorizing properties. Specifically, the sulfur-containing amino acid may include one or more selected from the group consisting of cysteine, cystine, and methionine. More specifically, the sulfur-containing amino acid may include cysteine or methionine.
[0134] The metal iodide salt is a form in which one or more selected from the group consisting of CuI, NaI, and KI are dissolved in water together with I2. The metal iodide salt can also be added to the superabsorbent resin in the same manner as the sulfur-containing amino acid to impart deodorizing properties.
[0135] Sulfur-containing amino acids can capture malodorous substances by chemically reacting with them. Malodorous substances generally have small molecular weights, and when they react with sulfur-containing amino acids, the malodor is reduced or becomes a substance without malodor, so that the malodor can be effectively removed. In particular, sulfur-containing amino acids are effective in reducing the malodor of aldehyde and ketone compounds.
[0136] Metal iodide salts remove malodorous substances by oxidizing them, and are generally effective as they act on most malodorous substances.
[0137] The sulfur-containing amino acid may be included in an amount of 0.1 to 1.5 parts by weight based on 100 parts by weight of the base resin. Specifically, the sulfur-containing amino acid may be included in an amount of 0.1 parts by weight or more, 0.13 parts by weight or more, or 0.15 parts by weight or more, and 1.5 parts by weight or less, 1.2 parts by weight or less, 1.0 parts by weight or less, 0.8 parts by weight or less, 0.6 parts by weight or less, 0.5 parts by weight or less, 0.4 parts by weight or less, 0.3 parts by weight or less, or 0.2 parts by weight or less.
[0138] The metal iodide salt solution may be included in an amount of 0.1 to 5.0 parts by weight based on 100 parts by weight of the base resin. Specifically, the metal iodide salt solution may be included in an amount of 0.1 parts by weight or more, 0.5 parts by weight or more, 1.0 parts by weight or more, 1.5 parts by weight or more, or 2.0 parts by weight or more, and 5.0 parts by weight or less, 4.0 parts by weight or less, 3.0 parts by weight or less, or 2.5 parts by weight or less. The metal iodide salt solution may be a solution having a metal iodide salt concentration of 1% or less.
[0139] Specifically, the metal iodide salt may be included in an amount of 0.001 parts by weight or more, 0.005 parts by weight or more, 0.01 parts by weight or more, 0.015 parts by weight or more, or 0.02 parts by weight or more and 0.05 parts by weight or less, 0.04 parts by weight or less, 0.03 parts by weight or less, or 0.025 parts by weight or less, based on 100 parts by weight of the base resin.
[0140] If the sulfur-containing amino acid is contained in an excessively small amount, the deodorizing properties may not be realized, and if it is contained in an excessively large amount, the inherent physical properties of the superabsorbent polymer may be deteriorated, and processing problems may occur due to incomplete dissolution.
[0141] In addition, if the amount of metal iodide salt is too small, the deodorizing properties may not be fully realized, while if the amount is too large, the inherent physical properties of the superabsorbent polymer may be reduced. In addition, since the superabsorbent polymer is supplied as a solution in the process, the amount of waste may increase, which may result in a decrease in the deodorizing power.
[0142] The sulfur-containing amino acid and the metal iodide salt are mixed with the superabsorbent resin in the form of an aqueous solution using water as a solvent, and are present in the superabsorbent resin in a state in which they are mixed and physically embedded in the superabsorbent resin.
[0143] After the step of mixing the aqueous solution containing a sulfur-containing amino acid and a metal iodide salt with the superabsorbent resin having a surface cross-linked layer (the post-water addition step), a drying step may be further carried out.
[0144] Preferred examples are presented below for better understanding of the present invention. However, the following examples are merely for illustrating the present invention and are not intended to limit the present invention thereto.
[0145] Comparative Example 1 100 g of acrylic acid, 0.37 g of N,N'-methylenebisacrylamide as a crosslinking agent, 0.15 g of sodium persulfate (SPS) as a thermal initiator, 0.008 g of benzoin ether as a UV initiator, 40 g of caustic soda (NaOH), and 127 g of water were mixed to prepare an aqueous monomer solution composition having a monomer concentration of 45.8 wt%. The aqueous monomer solution composition was fed into the feed section of a polymerization machine equipped with a continuously moving conveyor belt, and then irradiated with ultraviolet light using a UV irradiation device (irradiation dose: 10 mW / cm) while maintaining the polymerization atmosphere temperature at 80°C. 2 ) and UV polymerization was carried out for 2 minutes to produce a hydrogel polymer.
[0146] The hydrogel polymer was transferred to a meat chopper and cut into pieces of 2 mm to 10 mm. The water content of the cut hydrogel polymer was 47% by weight. The hydrogel polymer was then dried in a hot air dryer at 170°C for 30 minutes, and the dried hydrogel polymer was pulverized in a pin mill pulverizer. The polymer was then classified into particles of 150 μm to 850 μm using a sieve to produce a base resin.
[0147] Then, 100 parts by weight of the prepared base resin was uniformly mixed with a surface cross-linking liquid (2.5 parts by weight of water, 0.1 parts by weight of ethylene glycol diglycidyl ether (EX-810), 0.1 parts by weight of aluminum sulfate 18 hydrate (Al-S), and 0.1 parts by weight of silica (Aerosil A200)), and the surface cross-linking reaction was carried out at 140°C for 30 minutes. After the surface treatment was completed, the mixture was classified using a sieve to obtain a superabsorbent resin with a particle size range of 150 to 850 μm.
[0148] Comparative Example 2 100 g of acrylic acid, 0.37 g of N,N'-methylenebisacrylamide as a crosslinking agent, 0.15 g of sodium persulfate (SPS) as a thermal initiator, 0.008 g of benzoin ether as a UV initiator, 40 g of caustic soda (NaOH), and 127 g of water were mixed to prepare an aqueous monomer solution composition having a monomer concentration of 45.8 wt%. The aqueous monomer solution composition was fed into the feed section of a polymerization machine equipped with a continuously moving conveyor belt, and then irradiated with ultraviolet light using a UV irradiation device (irradiation dose: 10 mW / cm) while maintaining the polymerization atmosphere temperature at 80°C. 2 ) and UV polymerization was carried out for 2 minutes to produce a hydrogel polymer.
[0149] The hydrogel polymer was transferred to a meat chopper and cut into pieces of 2 mm to 10 mm. The water content of the cut hydrogel polymer was 47% by weight. The hydrogel polymer was then dried in a hot air dryer at 170°C for 30 minutes, and the dried hydrogel polymer was pulverized in a pin mill pulverizer. The polymer was then classified into particles of 150 μm to 850 μm using a sieve to produce a base resin.
[0150] Then, 100 parts by weight of the prepared base resin was uniformly mixed with a surface cross-linking liquid (2.5 parts by weight of water, 0.1 parts by weight of ethylene glycol diglycidyl ether (EX-810), 0.1 parts by weight of aluminum sulfate 18 hydrate (Al-S), and 0.1 parts by weight of silica (Aerosil A200)), and the surface cross-linking reaction was carried out at 140°C for 30 minutes. After the surface treatment was completed, the mixture was classified using a sieve to obtain a superabsorbent resin with a particle size range of 150 to 850 μm.
[0151] The obtained superabsorbent resin was mixed with an aqueous cysteine solution (cysteine concentration: 13 wt%). At this time, the amount of cysteine mixed was 0.1 parts by weight based on 100 parts by weight of the base resin. Then, a drying step was performed at 80° C. for 25 minutes.
[0152] Comparative Example 3 100 g of acrylic acid, 0.37 g of N,N'-methylenebisacrylamide as a crosslinking agent, 0.15 g of sodium persulfate (SPS) as a thermal initiator, 0.008 g of benzoin ether as a UV initiator, 40 g of caustic soda (NaOH), and 127 g of water were mixed to prepare an aqueous monomer solution composition having a monomer concentration of 45.8 wt%. The aqueous monomer solution composition was fed into the feed section of a polymerization machine equipped with a continuously moving conveyor belt, and then irradiated with ultraviolet light using a UV irradiation device (irradiation dose: 10 mW / cm) while maintaining the polymerization atmosphere temperature at 80°C. 2 ) and UV polymerization was carried out for 2 minutes to produce a hydrogel polymer.
[0153] The hydrogel polymer was transferred to a meat chopper and cut into pieces of 2 mm to 10 mm. The water content of the cut hydrogel polymer was 47% by weight. The hydrogel polymer was then dried in a hot air dryer at 170°C for 30 minutes, and the dried hydrogel polymer was pulverized in a pin mill pulverizer. The polymer was then classified into particles of 150 μm to 850 μm using a sieve to produce a base resin.
[0154] Then, 100 parts by weight of the prepared base resin was uniformly mixed with a surface cross-linking liquid (2.5 parts by weight of water, 0.1 parts by weight of ethylene glycol diglycidyl ether (EX-810), 0.1 parts by weight of aluminum sulfate 18 hydrate (Al-S), and 0.1 parts by weight of silica (Aerosil A200)), and the surface cross-linking reaction was carried out at 140°C for 30 minutes. After the surface treatment was completed, the mixture was classified using a sieve to obtain a superabsorbent resin with a particle size range of 150 to 850 μm.
[0155] The obtained superabsorbent resin was mixed with an aqueous CuI solution (CuI concentration 1 wt%). At this time, CuI was mixed in such a way that the amount of CuI was 0.02 parts by weight based on 100 parts by weight of the base resin. Then, a drying step was performed at 80° C. for 25 minutes.
[0156] Comparative Example 4 100 g of acrylic acid, 0.37 g of N,N'-methylenebisacrylamide as a crosslinking agent, 0.15 g of sodium persulfate (SPS) as a thermal initiator, 0.008 g of benzoin ether as a UV initiator, 40 g of caustic soda (NaOH), and 127 g of water were mixed to prepare an aqueous monomer solution composition having a monomer concentration of 45.8 wt%. The aqueous monomer solution composition was fed into the feed section of a polymerization machine equipped with a continuously moving conveyor belt, and then irradiated with ultraviolet light using a UV irradiation device (irradiation dose: 10 mW / cm) while maintaining the polymerization atmosphere temperature at 80°C. 2 ) and UV polymerization was carried out for 2 minutes to produce a hydrogel polymer.
[0157] The hydrogel polymer was transferred to a meat chopper and cut into pieces of 2 mm to 10 mm. The water content of the cut hydrogel polymer was 47% by weight. The hydrogel polymer was then dried in a hot air dryer at 170°C for 30 minutes, and the dried hydrogel polymer was pulverized in a pin mill pulverizer. The polymer was then classified into particles of 150 μm to 850 μm using a sieve to produce a base resin.
[0158] Then, 100 parts by weight of the prepared base resin was uniformly mixed with a surface cross-linking liquid (2.5 parts by weight of water, 0.1 parts by weight of ethylene glycol diglycidyl ether (EX-810), 0.1 parts by weight of aluminum sulfate 18 hydrate (Al-S), and 0.1 parts by weight of silica (Aerosil A200)), and the surface cross-linking reaction was carried out at 140°C for 30 minutes. After the surface treatment was completed, the mixture was classified using a sieve to obtain a superabsorbent resin with a particle size range of 150 to 850 μm.
[0159] The obtained superabsorbent resin was dry-mixed with 1.0 part by weight of beta-cyclodextrin based on 100 parts by weight of the superabsorbent resin.
[0160] Comparative Example 5 100 g of acrylic acid, 0.37 g of N,N'-methylenebisacrylamide as a crosslinking agent, 0.15 g of sodium persulfate (SPS) as a thermal initiator, 0.008 g of benzoin ether as a UV initiator, 40 g of caustic soda (NaOH), and 127 g of water were mixed to prepare an aqueous monomer solution composition having a monomer concentration of 45.8 wt%. The aqueous monomer solution composition was fed into the feed section of a polymerization machine equipped with a continuously moving conveyor belt, and then irradiated with ultraviolet light using a UV irradiation device (irradiation dose: 10 mW / cm) while maintaining the polymerization atmosphere temperature at 80°C. 2 ) and UV polymerization was carried out for 2 minutes to produce a hydrogel polymer.
[0161] The hydrogel polymer was transferred to a meat chopper and cut into pieces of 2 mm to 10 mm. The water content of the cut hydrogel polymer was 47% by weight. The hydrogel polymer was then dried in a hot air dryer at 170°C for 30 minutes, and the dried hydrogel polymer was pulverized in a pin mill pulverizer. The polymer was then classified into particles of 150 μm to 850 μm using a sieve to produce a base resin.
[0162] Thereafter, zirconium phosphate was dry-mixed with the base resin powder before surface crosslinking, so that the amount of zirconium phosphate was 2.0 parts by weight per 100 parts by weight of the base resin powder.
[0163] Then, 100 parts by weight of the base resin mixed with the zirconium phosphate was uniformly mixed with a surface cross-linking liquid (2.5 parts by weight of water, 0.1 parts by weight of ethylene glycol diglycidyl ether (EX-810), 0.1 parts by weight of aluminum sulfate 18 hydrate (Al-S), and 0.1 parts by weight of silica (Aerosil A200)), and the surface cross-linking reaction was carried out at 140°C for 30 minutes. After the surface treatment was completed, the mixture was classified using a sieve to obtain a superabsorbent resin with a particle size range of 150 to 850 μm.
[0164] Comparative Example 6 100 g of acrylic acid, 0.37 g of N,N'-methylenebisacrylamide as a crosslinking agent, 0.15 g of sodium persulfate (SPS) as a thermal initiator, 0.008 g of benzoin ether as a UV initiator, 40 g of caustic soda (NaOH), and 127 g of water were mixed to prepare an aqueous monomer solution composition having a monomer concentration of 45.8 wt%. The aqueous monomer solution composition was fed into the feed section of a polymerization machine equipped with a continuously moving conveyor belt, and then irradiated with ultraviolet light using a UV irradiation device (irradiation dose: 10 mW / cm) while maintaining the polymerization atmosphere temperature at 80°C. 2 ) and UV polymerization was carried out for 2 minutes to produce a hydrogel polymer.
[0165] The hydrogel polymer was transferred to a meat chopper and cut into pieces of 2 mm to 10 mm. The water content of the cut hydrogel polymer was 47% by weight. The hydrogel polymer was then dried in a hot air dryer at 170°C for 30 minutes, and the dried hydrogel polymer was pulverized in a pin mill pulverizer. The polymer was then classified into particles of 150 μm to 850 μm using a sieve to produce a base resin.
[0166] Then, 100 parts by weight of the prepared base resin was mixed with a surface cross-linking solution (2.5 parts by weight of water, 0.1 parts by weight of ethylene glycol diglycidyl ether (EX-810), 0.1 parts by weight of aluminum sulfate 18 hydrate (Al-S), and 0.1 parts by weight of silica (Aerosil A200)) and a tannin solution, and the surface cross-linking reaction was carried out at 140°C for 30 minutes. The tannin solution was an aqueous solution, and had a solid content of 5 parts by weight based on 100 parts by weight of the solution. The tannin solution was mixed with 100 parts by weight of the base resin at a solid content of 0.05 parts by weight. After the surface treatment was completed, the resin was classified using a sieve to obtain a superabsorbent resin having a particle size range of 150 to 850 μm.
[0167] Example 1 100 g of acrylic acid, 0.37 g of N,N'-methylenebisacrylamide as a crosslinking agent, 0.15 g of sodium persulfate (SPS) as a thermal initiator, 0.008 g of benzoin ether as a UV initiator, 40 g of caustic soda (NaOH), and 127 g of water were mixed to prepare an aqueous monomer solution composition having a monomer concentration of 45.8 wt%. The aqueous monomer solution composition was fed into the feed section of a polymerization machine equipped with a continuously moving conveyor belt, and then irradiated with ultraviolet light using a UV irradiation device (irradiation dose: 10 mW / cm) while maintaining the polymerization atmosphere temperature at 80°C. 2 ) and UV polymerization was carried out for 2 minutes to produce a hydrogel polymer.
[0168] The hydrogel polymer was transferred to a meat chopper and cut into pieces of 2 mm to 10 mm. The water content of the cut hydrogel polymer was 47% by weight. The hydrogel polymer was then dried in a hot air dryer at 170°C for 30 minutes, and the dried hydrogel polymer was pulverized in a pin mill pulverizer. The polymer was then classified into particles of 150 μm to 850 μm using a sieve to produce a base resin.
[0169] Then, 100 parts by weight of the prepared base resin was uniformly mixed with a surface cross-linking liquid (2.5 parts by weight of water, 0.1 parts by weight of ethylene glycol diglycidyl ether (EX-810), 0.1 parts by weight of aluminum sulfate 18 hydrate (Al-S), and 0.1 parts by weight of silica (Aerosil A200)), and the surface cross-linking reaction was carried out at 140°C for 30 minutes. After the surface treatment was completed, the mixture was classified using a sieve to obtain a superabsorbent resin with a particle size range of 150 to 850 μm.
[0170] The obtained superabsorbent resin was mixed with an aqueous cysteine solution (cysteine concentration 13 wt%) and an aqueous CuI solution (CuI concentration 1 wt%). The mixture was adjusted so that the amount of cysteine was 0.1 parts by weight per 100 parts by weight of the base resin, and the amount of CuI was 0.02 parts by weight per 100 parts by weight of the base resin. Then, a drying step was performed at 80°C for 25 minutes.
[0171] Example 2 100 g of acrylic acid, 0.37 g of N,N'-methylenebisacrylamide as a crosslinking agent, 0.15 g of sodium persulfate (SPS) as a thermal initiator, 0.008 g of benzoin ether as a UV initiator, 40 g of caustic soda (NaOH), and 127 g of water were mixed to prepare an aqueous monomer solution composition having a monomer concentration of 45.8 wt%. The aqueous monomer solution composition was fed into the feed section of a polymerization machine equipped with a continuously moving conveyor belt, and then irradiated with ultraviolet light using a UV irradiation device (irradiation dose: 10 mW / cm) while maintaining the polymerization atmosphere temperature at 80°C. 2 ) and UV polymerization was carried out for 2 minutes to produce a hydrogel polymer.
[0172] The hydrogel polymer was transferred to a meat chopper and cut into pieces of 2 mm to 10 mm. The water content of the cut hydrogel polymer was 47% by weight. The hydrogel polymer was then dried in a hot air dryer at 170°C for 30 minutes, and the dried hydrogel polymer was pulverized in a pin mill pulverizer. The polymer was then classified into particles of 150 μm to 850 μm using a sieve to produce a base resin.
[0173] Then, 100 parts by weight of the prepared base resin was uniformly mixed with a surface cross-linking liquid (2.5 parts by weight of water, 0.1 parts by weight of ethylene glycol diglycidyl ether (EX-810), 0.1 parts by weight of aluminum sulfate 18 hydrate (Al-S), and 0.1 parts by weight of silica (Aerosil A200)), and the surface cross-linking reaction was carried out at 140°C for 30 minutes. After the surface treatment was completed, the mixture was classified using a sieve to obtain a superabsorbent resin with a particle size range of 150 to 850 μm.
[0174] The obtained superabsorbent resin was mixed with an aqueous cysteine solution (cysteine concentration 13 wt%) and an aqueous CuI solution (CuI concentration 1 wt%). The mixture was adjusted so that the amount of cysteine was 0.15 parts by weight per 100 parts by weight of the base resin, and the amount of CuI was 0.01 parts by weight per 100 parts by weight of the base resin. Then, a drying step was performed at 80°C for 25 minutes.
[0175] Example 3 100 g of acrylic acid, 0.37 g of N,N'-methylenebisacrylamide as a crosslinking agent, 0.15 g of sodium persulfate (SPS) as a thermal initiator, 0.008 g of benzoin ether as a UV initiator, 40 g of caustic soda (NaOH), and 127 g of water were mixed to prepare an aqueous monomer solution composition having a monomer concentration of 45.8 wt%. The aqueous monomer solution composition was fed into the feed section of a polymerization machine equipped with a continuously moving conveyor belt, and then irradiated with ultraviolet light using a UV irradiation device (irradiation dose: 10 mW / cm) while maintaining the polymerization atmosphere temperature at 80°C. 2 ) and UV polymerization was carried out for 2 minutes to produce a hydrogel polymer.
[0176] The hydrogel polymer was transferred to a meat chopper and cut into pieces of 2 mm to 10 mm. The water content of the cut hydrogel polymer was 47% by weight. The hydrogel polymer was then dried in a hot air dryer at 170°C for 30 minutes, and the dried hydrogel polymer was pulverized in a pin mill pulverizer. The polymer was then classified into particles of 150 μm to 850 μm using a sieve to produce a base resin.
[0177] Then, 100 parts by weight of the prepared base resin was uniformly mixed with a surface cross-linking liquid (2.5 parts by weight of water, 0.1 parts by weight of ethylene glycol diglycidyl ether (EX-810), 0.1 parts by weight of aluminum sulfate 18 hydrate (Al-S), and 0.1 parts by weight of silica (Aerosil A200)), and the surface cross-linking reaction was carried out at 140°C for 30 minutes. After the surface treatment was completed, the mixture was classified using a sieve to obtain a superabsorbent resin with a particle size range of 150 to 850 μm. The content of the superabsorbent resin having an average particle size of less than 150 μm was less than 2%.
[0178] The obtained superabsorbent resin was mixed with an aqueous cysteine solution (cysteine concentration 13 wt%) and an aqueous CuI solution (CuI concentration 1 wt%). The mixture was adjusted so that the amount of cysteine was 0.3 parts by weight per 100 parts by weight of the base resin, and the amount of CuI was 0.001 parts by weight per 100 parts by weight of the base resin. Then, a drying step was performed at 80°C for 25 minutes.
[0179] Example 4 100 g of acrylic acid, 1.0 g of cetethyldimonium bromide as an antibacterial polymerizable monomer, 0.37 g of N,N'-methylenebisacrylamide as a crosslinking agent, 0.15 g of sodium persulfate (SPS) as a thermal initiator, 0.008 g of benzoin ether as a UV initiator, 40 g of caustic soda (NaOH) and 127 g of water were mixed to prepare an aqueous monomer solution composition having a monomer concentration of 45.8 wt%. The aqueous monomer solution composition was fed into the feed section of a polymerization machine equipped with a continuously moving conveyor belt, and then irradiated with ultraviolet light (irradiation dose: 10 mW / cm) using a UV irradiation device while maintaining the polymerization atmosphere temperature at 80°C. 2 ) and UV polymerization was carried out for 2 minutes to produce a hydrogel polymer.
[0180] The hydrogel polymer was transferred to a meat chopper and cut into pieces of 2 mm to 10 mm. The water content of the cut hydrogel polymer was 47% by weight. The hydrogel polymer was then dried in a hot air dryer at 170°C for 30 minutes, and the dried hydrogel polymer was pulverized in a pin mill pulverizer. The polymer was then classified into particles of 150 μm to 850 μm using a sieve to produce a base resin.
[0181] Thereafter, zirconium phosphate was mixed into the base resin powder before surface crosslinking, so that the amount of zirconium phosphate was 2.0 parts by weight based on 100 parts by weight of the base resin powder.
[0182] Then, 100 parts by weight of the prepared base resin was mixed with a surface cross-linking solution (2.5 parts by weight of water, 0.1 parts by weight of ethylene glycol diglycidyl ether (EX-810), 0.1 parts by weight of aluminum sulfate 18 hydrate (Al-S), and 0.1 parts by weight of silica (Aerosil A200)) and a tannin solution, and the surface cross-linking reaction was carried out at 140°C for 30 minutes. The tannin solution was an aqueous solution, and had a tannin solid content of 5 parts by weight based on 100 parts by weight of the solution. The tannin solution was mixed with 100 parts by weight of the base resin at a solid content of 0.05 parts by weight. After the surface treatment was completed, the resin was classified using a sieve to obtain a superabsorbent resin having a particle size range of 150 to 850 μm.
[0183] The obtained superabsorbent resin was mixed with an aqueous cysteine solution (13 wt%) and an aqueous CuI solution (1 wt%). The mixture was adjusted so that the amount of cysteine was 0.15 parts by weight per 100 parts by weight of the base resin, and the amount of CuI was 0.01 parts by weight per 100 parts by weight of the base resin. Then, a drying step was performed at 80°C for 25 minutes.
[0184] Example 5 100 g of acrylic acid, 0.5 g of cetethyldimonium bromide as an antibacterial polymerizable monomer, 0.37 g of N,N'-methylenebisacrylamide as a crosslinking agent, 0.15 g of sodium persulfate (SPS) as a thermal initiator, 0.008 g of benzoin ether as a UV initiator, 40 g of caustic soda (NaOH) and 127 g of water were mixed to prepare an aqueous monomer solution composition having a monomer concentration of 45.8 wt%. The aqueous monomer solution composition was fed into the feed section of a polymerization machine equipped with a continuously moving conveyor belt, and then irradiated with ultraviolet light (irradiation dose: 10 mW / cm) using a UV irradiation device while maintaining the polymerization atmosphere temperature at 80°C. 2 ) and UV polymerization was carried out for 2 minutes to produce a hydrogel polymer.
[0185] The hydrogel polymer was transferred to a meat chopper and cut into pieces of 2 mm to 10 mm. The water content of the cut hydrogel polymer was 47% by weight. The hydrogel polymer was then dried in a hot air dryer at 170°C for 30 minutes, and the dried hydrogel polymer was pulverized in a pin mill pulverizer. The polymer was then classified into particles of 150 μm to 850 μm using a sieve to produce a base resin.
[0186] Thereafter, zirconium phosphate was mixed into the base resin powder before surface crosslinking, so that the amount of zirconium phosphate was 2.0 parts by weight based on 100 parts by weight of the base resin powder.
[0187] Then, 100 parts by weight of the prepared base resin was mixed with a surface cross-linking solution (2.5 parts by weight of water, 0.1 parts by weight of ethylene glycol diglycidyl ether (EX-810), 0.1 parts by weight of aluminum sulfate 18 hydrate (Al-S), and 0.1 parts by weight of silica (Aerosil A200)) and a tannin solution, and the surface cross-linking reaction was carried out at 140°C for 30 minutes. The tannin solution was an aqueous solution, and had a solid content of 5 parts by weight based on 100 parts by weight of the solution. At this time, the tannin solution was mixed with 100 parts by weight of the base resin at a solid content of 0.05 parts by weight. After the surface treatment was completed, the resin was classified using a sieve to obtain a superabsorbent resin having a particle size range of 150 to 850 μm.
[0188] The obtained superabsorbent resin was mixed with an aqueous cysteine solution (cysteine concentration 13 wt%) and an aqueous CuI solution (CuI concentration 1 wt%). The mixture was adjusted so that the amount of cysteine was 0.3 parts by weight per 100 parts by weight of the base resin, and the amount of CuI was 0.001 parts by weight per 100 parts by weight of the base resin. Then, a drying step was performed at 80°C for 25 minutes.
[0189] Example 6 100 g of acrylic acid, 0.37 g of N,N'-methylenebisacrylamide as a crosslinking agent, 0.15 g of sodium persulfate (SPS) as a thermal initiator, 0.008 g of benzoin ether as a UV initiator, 40 g of caustic soda (NaOH), and 127 g of water were mixed to prepare an aqueous monomer solution composition having a monomer concentration of 45.8 wt%. The aqueous monomer solution composition was fed into the feed section of a polymerization machine equipped with a continuously moving conveyor belt, and then irradiated with ultraviolet light using a UV irradiation device (irradiation dose: 10 mW / cm) while maintaining the polymerization atmosphere temperature at 80°C. 2 ) and UV polymerization was carried out for 2 minutes to produce a hydrogel polymer.
[0190] The hydrogel polymer was transferred to a meat chopper and cut into pieces of 2 mm to 10 mm. The water content of the cut hydrogel polymer was 47% by weight. The hydrogel polymer was then dried in a hot air dryer at 170°C for 30 minutes, and the dried hydrogel polymer was pulverized in a pin mill pulverizer. The polymer was then classified into particles of 150 μm to 850 μm using a sieve to produce a base resin.
[0191] Then, 100 parts by weight of the prepared base resin was uniformly mixed with a surface cross-linking liquid (2.5 parts by weight of water, 0.1 parts by weight of ethylene glycol diglycidyl ether (EX-810), 0.1 parts by weight of aluminum sulfate 18 hydrate (Al-S), and 0.1 parts by weight of silica (Aerosil A200)), and the surface cross-linking reaction was carried out at 140°C for 30 minutes. After the surface treatment was completed, the mixture was classified using a sieve to obtain a superabsorbent resin with a particle size range of 150 to 850 μm.
[0192] The obtained superabsorbent resin was mixed with an aqueous methionine solution (methionine concentration 13 wt%) and an aqueous CuI solution (CuI concentration 1 wt%). The methionine was mixed at 0.15 parts by weight per 100 parts by weight of the base resin, and the CuI was mixed at 0.01 parts by weight per 100 parts by weight of the base resin. Then, a drying step was performed at 80°C for 25 minutes.
[0193] Example 7 100 g of acrylic acid, 0.5 g of cetethyldimonium bromide as an antibacterial polymerizable monomer, 0.37 g of N,N'-methylenebisacrylamide as a crosslinking agent, 0.15 g of sodium persulfate (SPS) as a thermal initiator, 0.008 g of benzoin ether as a UV initiator, 40 g of caustic soda (NaOH) and 127 g of water were mixed to prepare an aqueous monomer solution composition having a monomer concentration of 45.8 wt%. The aqueous monomer solution composition was fed into the feed section of a polymerization machine equipped with a continuously moving conveyor belt, and then irradiated with ultraviolet light (irradiation dose: 10 mW / cm) using a UV irradiation device while maintaining the polymerization atmosphere temperature at 80°C. 2 ) and UV polymerization was carried out for 2 minutes to produce a hydrogel polymer.
[0194] The hydrogel polymer was transferred to a meat chopper and cut into pieces of 2 mm to 10 mm. The water content of the cut hydrogel polymer was 47% by weight. The hydrogel polymer was then dried in a hot air dryer at 170°C for 30 minutes, and the dried hydrogel polymer was pulverized in a pin mill pulverizer. The polymer was then classified into particles of 150 μm to 850 μm using a sieve to produce a base resin.
[0195] Thereafter, zirconium phosphate was mixed into the base resin powder before surface crosslinking, so that the amount of zirconium phosphate was 2.0 parts by weight based on 100 parts by weight of the base resin powder.
[0196] Then, 100 parts by weight of the prepared base resin was mixed with a surface cross-linking solution (2.5 parts by weight of water, 0.1 parts by weight of ethylene glycol diglycidyl ether (EX-810), 0.1 parts by weight of aluminum sulfate 18 hydrate (Al-S), and 0.1 parts by weight of silica (Aerosil A200)) and a tannin solution, and the surface cross-linking reaction was carried out at 140°C for 30 minutes. The tannin solution was an aqueous solution, and had a solid content of 5 parts by weight based on 100 parts by weight of the solution. At this time, the tannin solution was mixed with 100 parts by weight of the base resin at a solid content of 0.05 parts by weight. After the surface treatment was completed, the resin was classified using a sieve to obtain a superabsorbent resin having a particle size range of 150 to 850 μm.
[0197] The obtained superabsorbent resin was mixed with an aqueous cysteine solution (cysteine concentration 13 wt%) and an aqueous CuI solution (CuI concentration 1 wt%). The mixture was adjusted so that the amount of cysteine was 0.6 parts by weight per 100 parts by weight of the base resin, and the amount of CuI was 0.01 parts by weight per 100 parts by weight of the base resin. Then, a drying step was performed at 80°C for 25 minutes.
[0198] [Table 1]
[0199] Experimental Example The superabsorbent resin compositions prepared in the above Examples and Comparative Examples were measured for various physical properties by the following methods.
[0200] 1) Deodorizing power The deodorizing power was measured using an adsorption tube method. The odorous substances diacetyl, 3-methylbutanal, and dimethyltrisulfide (DMTS) were selected and tested for deodorizing power.
[0201] - Adsorption tube measurement method: 1g of superabsorbent resin was placed in a 500mL glass bottle, and 25mL of malodorous substances were poured in. After that, aging was carried out for 3 hours in a thermostatic chamber, and then collection was carried out for 20 minutes. The temperature of the thermostatic chamber was 35℃, and the N2 flow rate was 250mL / min. The pushed out malodorous substances were adsorbed in the connected adsorption tube, and this was repeated twice for the same sample. The collection results were analyzed by GC and the results were confirmed.
[0202] - Deodorizing power (%) = (malodor amount of reference sample (super absorbent polymer of Comparative Example 1) measured by GC - malodor amount of sample measured by GC) / malodor amount of reference sample (super absorbent polymer of Comparative Example 1) measured by GC × 100 (%)
[0203] 2) Centrifuge Retention Capacity (CRC) The water retention capacity of each resin in terms of its unloaded absorbency was measured according to the European Disposables and Nonwovens Association (EDANA) standard EDANA WSP 241.3.
[0204] Specifically, resins obtained from the examples and comparative examples were classified into a particle size range of 300 μm to 500 μm. Such resins W0(g) (approximately 0.2 g) were uniformly placed in a nonwoven fabric envelope, sealed, and then immersed in physiological saline (0.9 wt%) at room temperature. After 30 minutes, the envelope was dewatered for 3 minutes under conditions of 250 G using a centrifuge, and the mass W2(g) of the envelope was measured. The same operation was performed without using resin, and the mass W1(g) at that time was measured.
[0205] Using the obtained masses, the CRC (g / g) was calculated according to the following formula 1.
[0206] [Formula 1] CRC(g / g)={[W2(g)-W1(g)] / W0(g)}-1
[0207] 3) Absorbency under Pressure (AUP) The absorbency at a pressure of 0.7 psi of the superabsorbent resins of the above Examples and Comparative Examples was measured by EDANA method WSP 242.3.
[0208] First, when measuring the pressurized absorbency, the resin fraction used in the CRC measurement was used.
[0209] Specifically, a stainless steel 400 mesh iron net was attached to the bottom of a plastic cylinder with an inner diameter of 25 mm. Under conditions of room temperature and humidity of 50%, the superabsorbent resin W0 (g) was evenly spread on the iron net, and a load of 0.7 psi was evenly applied to the net. The piston had an outer diameter slightly smaller than 25 mm, had no gap with the inner wall of the cylinder, and was not hindered from moving up and down. At this time, the weight W3 (g) of the device was measured.
[0210] A glass filter with a diameter of 90 mm and a thickness of 5 mm was placed inside a Petri dish with a diameter of 150 mm, and physiological saline composed of 0.9 wt% sodium chloride was placed at the same level as the upper surface of the glass filter. A sheet of filter paper with a diameter of 90 mm was placed on top of it. The measuring device was placed on the filter paper, and the liquid was absorbed under a load for 1 hour. After 1 hour, the measuring device was lifted and its weight W4 (g) was measured. Using the obtained masses, the pressurized absorption capacity (g / g) was calculated according to the following formula 2.
[0211] [Formula 2] AUP(g / g)=[W4(g)-W3(g)] / W0(g)
[0212] The results of the deodorizing power experiment are shown in Table 2, and the centrifugal separation water retention capacity and pressure absorption capacity are shown in Table 3.
[0213] The values in Table 2 show the deodorizing efficiency relative to Comparative Example 1, with higher values indicating higher deodorizing efficiency.
[0214] [Table 2]
[0215] [Table 3]
[0216] It can be seen from Table 2 that Examples 1 to 7 have uniformly excellent deodorizing ability for the malodorous substances diacetyl, 3-methylbutanal, and dimethyl trisulfide, compared to Comparative Examples 1 to 6. Also, it can be seen from Table 3 that the absorption ability of Examples 1 to 7 is maintained at a similar level to Comparative Examples 1 to 6. Therefore, it can be seen that the superabsorbent resin of the present invention has improved deodorizing ability without decreasing absorption ability.
Claims
1. a superabsorbent resin including a base resin containing a crosslinked polymer obtained by crosslinking an acrylic acid monomer having at least a partially neutralized acidic group with an internal crosslinking agent; and a surface crosslinked layer formed on the surface of the base resin, the crosslinked polymer being further crosslinked via a surface crosslinking agent; A superabsorbent polymer composition comprising a sulfur-containing amino acid and a metal iodide salt.
2. For 100 parts by weight of base resin, the sulfur-containing amino acid is 0.1 to 1.5 parts by weight; The metal iodide salt is included in an amount of 0.001 to 0.05 parts by weight. The highly water-absorbent resin composition according to claim 1.
3. The sulfur-containing amino acid includes at least one selected from the group consisting of cysteine, cystine, and methionine. The highly water-absorbent resin composition according to claim 1.
4. The base resin further comprises a polymerizable antibacterial monomer as a monomer. The highly water-absorbent resin composition according to claim 1.
5. further comprising zirconium phosphate in an amount of up to 5.0 parts by weight based on 100 parts by weight of said base resin; The highly water-absorbent resin composition according to claim 1.
6. The surface cross-linked layer further contains a tannin solid content of 0.05 parts by weight or less per 100 parts by weight of the base resin. The highly water-absorbent resin composition according to claim 1.
7. Step 1: forming a hydrogel polymer by cross-linking and polymerizing an acrylic acid monomer having at least a partially neutralized acid group in the presence of an internal cross-linking agent and a polymerization initiator; A step (step 2) of preparing a base resin containing a crosslinked polymer by drying and pulverizing the hydrogel polymer; A step (step 3) of mixing the base resin with a surface cross-linking liquid to produce a mixture; Step 4: heat-treating the mixture to produce a superabsorbent resin having a surface cross-linked layer formed on the surface of the base resin; Step 5: mixing the superabsorbent resin with an aqueous solution containing a sulfur-containing amino acid and a metal iodide salt; A method for producing a superabsorbent resin composition comprising the steps of:
8. In the above (Step 5), for 100 parts by weight of the base resin, the sulfur-containing amino acid is 0.1 to 1.5 parts by weight; The metal iodide salt is mixed in an amount of 0.001 to 0.05 parts by weight. A method for producing the highly water-absorbent resin composition according to claim 7.
9. The sulfur-containing amino acid includes at least one selected from the group consisting of cysteine, cystine, and methionine. A method for producing the highly water-absorbent resin composition according to claim 7.
10. In the step (1), the composition further comprises a polymerizable antimicrobial monomer. A method for producing the highly water-absorbent resin composition according to claim 7.
11. After the step 2, the step of mixing zirconium phosphate is further included. A method for producing the highly water-absorbent resin composition according to claim 7.
12. The surface cross-linking liquid of (step 3) contains a tannin solution, A method for producing the highly water-absorbent resin composition according to claim 7.
13. The zirconium phosphate is mixed in an amount of 5.0 parts by weight or less per 100 parts by weight of the base resin. A method for producing the highly water-absorbent resin composition according to claim 11.
14. The tannin solution is contained in an amount of 1.0 part by weight or less per 100 parts by weight of the base resin. A method for producing the highly water-absorbent resin composition according to claim 12.
Citation Information
Patent Citations
Antimicrobial polyamide resin molding
JP1998292107A
Deodorizing super absorbent composition
JP2009515691A
Wiping sheet
JP2012024566A
Sterilization and / or antiviral compositions
JP2014208606A