Method for producing polyphenylene ether

A two-step drying process with controlled heating temperatures addresses scaling and fusion issues in PPE drying, improving efficiency and product quality by preventing contamination.

JP7580965B2Active Publication Date: 2024-11-12ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020132574
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-04
Publication Date
2024-11-12
Estimated Expiration
2040-08-04

AI Technical Summary

Technical Problem

Existing methods for drying polyphenylene ether (PPE) face challenges such as scaling and fusion on heat transfer surfaces, particularly during the drying of low molecular weight PPE, leading to inefficient drying processes and equipment contamination.

Method used

A method involving a two-step drying process with controlled heating temperatures and solvent content adjustment to prevent scaling and fusion, using a first dryer at a temperature between bl°C and (Tg-30)°C, and a second dryer at (bh+5)°C to (Tg-5)°C, where bl and bh are the boiling points of the lowest and highest solvents, respectively, and Tg is the glass transition temperature of PPE.

Benefits of technology

This approach enhances drying efficiency while minimizing scaling and fusion, ensuring high-quality PPE production without contamination from fused materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580965000005
    Figure 0007580965000005
  • Figure 0007580965000006
    Figure 0007580965000006
  • Figure 0007580965000001
    Figure 0007580965000001
Patent Text Reader

Abstract

To provide a method for producing PPE which can enhance drying speed while reducing problems of scaling and fusion in a dryer during drying.SOLUTION: A method for producing polyphenylene ether includes: a solid-liquid separation step of solid-liquid separating polyphenylene ether having a weight average molecular weight (Mw) of 2,500-6,000 and a glass transition temperature (Tg) of 100-200°C, and a slurry liquid containing a good solvent of polyphenylene ether and a poor solvent of polyphenylene ether, and obtaining wet polyphenylene ether; and a drying step of drying the wet polyphenylene ether, in which a liquid-containing ratio of the wet polyphenylene ether at the time of start of the drying step is equal to or less an upper limit of a liquid-containing ratio of preventing fusion at a heating temperature T1 set according to the following expression, and when a boiling point of a solvent having the lowest boiling point in the solvent component contained in the wet polyphenylene ether is represented by bl°C and a boiling point of the solvent having the highest boiling point is represented by bh°C, in the drying step, a heating temperature T1 until a content of the solvent component becomes a limit liquid-containing ratio or less is set at the following range: bl°C≤T1≤(Tg-30)°C, and a heating temperature T2 after the content of the solvent component becomes the limit liquid-containing ratio or less is set at the following range: (bh+5)°C≤T2≤(Tg-5)°C, and T2 is set to be higher than T1.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing polyphenylene ether, which includes a new drying step of drying wet polyphenylene ether. [Background technology]

[0002] Polyphenylene ether (hereinafter sometimes simply referred to as PPE) has excellent high-frequency characteristics, flame retardancy, and heat resistance, and is therefore widely used as a material in the electrical and electronic fields, the automotive field, and various other industrial materials fields. While taking advantage of these properties, PPE with a lower molecular weight and increased solubility in general-purpose solvents is being investigated for use in electronic materials, as composite materials and additives that can be combined with other resins to obtain excellent properties.

[0003] The polymerization process in the general industrial production of PPE is either precipitation polymerization or solution polymerization. In precipitation polymerization, the product is a slurry liquid at the end of polymerization, while in solution polymerization, the product is a solution at the end of polymerization, but is mixed with a poor solvent for PPE in a later process to become a slurry liquid. The slurry liquid obtained in either polymerization process is subjected to solid-liquid separation after post-treatment such as washing to obtain wet PPE. Wet PPE contains a good solvent and a poor solvent for PPE, and when dried in a state where the good solvent content is high, the PPE is highly adhesive. In particular, with low-molecular-weight PPE, if the liquid content of the good solvent and poor solvent is high, problems such as scaling on the drying device occur. In addition, if the temperature of the heat transfer surface in the dryer is raised to a high temperature to increase the drying efficiency, a fusion phenomenon occurs on the heat transfer surface, which can cause problems such as strong scaling and the fusion product being mixed in due to the detachment of scaling material. Therefore, various studies have been conducted on methods for drying wet PPE in the industrial production of PPE.

[0004] Patent Document 1 describes a method for producing low molecular weight PPE. There is no detailed description of the drying conditions during production. Patent Document 2 describes a method of using a rotary dryer with multiple heating tubes installed inside to dry wet PPE. The method is characterized in that the temperature of PPE in the drying zone, where a good solvent for PPE is present at 10% by weight or more, is set to 100°C or lower, but there is no description regarding the heating temperature of the heat transfer surface of the dryer. Patent Document 3 discloses a method in which a dried PPE resin heated to a temperature 40°C lower than the glass transition temperature of the PPE resin in a dry state and below the glass transition temperature is mixed, stirred, and granulated with a wet PPE resin. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 62-39628 [Patent Document 2] JP 2001-335632 A [Patent Document 3] JP 2006-241258 A Summary of the Invention [Problem to be solved by the invention]

[0006] Although an example of Patent Document 1 discloses vacuum drying at 70° C. as a method for drying PPE, this drying method is inferior in productivity and cannot be said to be suitable for industrial production.

[0007] In Patent Document 2, the temperature of the PPE in the drying zone where the amount of the good solvent for PPE is 10% by weight or more is near the boiling point of the lowest boiling point solvent contained in the PPE during drying. Therefore, for example, when the PPE contains methanol (boiling point: 64.7°C), a typical poor solvent, the temperature of the PPE is near 64.7°C, which is the boiling point of methanol, but if the heating temperature is increased to increase the drying efficiency while adjusting (maintaining) the temperature of the PPE at 100°C or less, the temperature of the heating surface may reach 100°C or more, and it may be impossible to avoid scaling or fusion on the heating surface. Furthermore, when the main component of the solvent remaining in the PPE becomes toluene (boiling point: 110°C), a typical good solvent, the temperature of the heating surface must be set to 100°C or less in order to keep the temperature of the PPE at 100°C or less. However, when drying wet PPE, the amount of heat supplied is important for the constant rate drying speed until the limit liquid content is reached, and drying efficiency is insufficient when the temperature of the heating surface is below 100°C.

[0008] In the examples of Patent Document 3, the presence or absence of fusion when dried in a mixed state is confirmed, and it is described that the fusion phenomenon during drying can be suppressed by the method of Patent Document 3. However, since the dried polyphenylene ether resin is mixed and dried, the drying device needs to be large, which increases the equipment cost and running cost and is not efficient. In addition, it is described that a part of the granules is melted, and there is a concern that the fused material will scale in the dryer, especially when low molecular weight PPE is dried by the method of Patent Document 3. Furthermore, low molecular weight PPE has a lower glass transition temperature than regular PPE. Therefore, if drying is performed under the same temperature conditions as regular PPE, the heating temperature of the heat transfer surface may reach close to the glass transition temperature, causing the low molecular weight PPE to melt, which can lead to problems such as strong scaling and fusion of the scaling material into the product.

[0009] As described above, methods for drying wet PPE efficiently while avoiding scaling and fusion have been investigated in the low molecular weight PPE manufacturing process, but such methods have not yet been developed.

[0010] The present invention has been made in consideration of the above-mentioned problems, and aims to provide a method for producing PPE that can increase the drying speed while reducing problems such as scaling and fusion in the dryer during drying. [Means for solving the problem]

[0011] As a result of intensive research by the present inventors, it was found that, when drying wet PPE, scaling and fusion can be suppressed by adjusting the heating temperature of the heat transfer surface with which the wet PPE comes into contact to a lower value until the content of the solvent component falls below the critical liquid content, and supplying the wet PPE to the dryer at a liquid content below the upper limit of the non-fusion liquid content at the lower drying temperature. Furthermore, it was found that, after the content of the solvent component falls below the critical liquid content, the drying efficiency of the wet PPE can be significantly improved by increasing the heating temperature of the heat transfer surface within a range in which the PPE does not melt, and this led to the present invention.

[0012] That is, the present invention is as follows. [1] a solid-liquid separation step of subjecting a slurry liquid containing polyphenylene ether having a weight average molecular weight (Mw) of 2500 to 6000 and a glass transition temperature (Tg) of 100 to 200° C., a good solvent for the polyphenylene ether, and a poor solvent for the polyphenylene ether to solid-liquid separation to obtain wet polyphenylene ether; a drying step of drying the wet polyphenylene ether, The liquid content of the wet polyphenylene ether at the start of the drying step is equal to or less than an upper limit of the liquid content at which fusion does not occur at a heating temperature T1 set according to the following formula (upper unfused liquid content limit), When the boiling point of the lowest boiling point solvent among the solvent components contained in the wet polyphenylene ether is bl° C. and the boiling point of the highest boiling point solvent is bh° C., In the drying step, The heating temperature T1 until the content of the solvent component becomes equal to or less than the limit liquid content is set in the following range: bl℃≦T1≦(Tg-30)℃ The heating temperature T2 after the content of the solvent component becomes equal to or lower than the limit liquid content is set in the following range: (bh+5)℃≦T2≦(Tg-5)℃ And set T2 to a temperature higher than T1. death, a liquid content adjusting step of adjusting the liquid content of the wet polyphenylene ether obtained in the solid-liquid separation step to a level equal to or lower than the unfused upper limit liquid content at the heating temperature: T1 set according to the formula before the drying step, The liquid content adjusting step is a step of aerating the wet polyphenylene ether, the liquid content of which has exceeded the unfused upper limit liquid content at the heating temperature T1, to reduce the liquid content to equal to or lower than the unfused upper limit liquid content at the heating temperature T1; A method for producing polyphenylene ether. [2] a solid-liquid separation step of subjecting a slurry liquid containing polyphenylene ether having a weight average molecular weight (Mw) of 2500 to 6000 and a glass transition temperature (Tg) of 100 to 200° C., a good solvent for the polyphenylene ether, and a poor solvent for the polyphenylene ether to solid-liquid separation to obtain wet polyphenylene ether; a drying step of drying the wet polyphenylene ether, The liquid content of the wet polyphenylene ether at the start of the drying step is equal to or less than an upper limit of the liquid content at which fusion does not occur at a heating temperature T1 set according to the following formula (upper unfused liquid content limit), When the boiling point of the lowest boiling point solvent among the solvent components contained in the wet polyphenylene ether is bl° C. and the boiling point of the highest boiling point solvent is bh° C., In the drying step, The heating temperature T1 until the content of the solvent component becomes equal to or less than the limit liquid content is set in the following range: bl℃≦T1≦(Tg-30)℃ The heating temperature T2 after the content of the solvent component becomes equal to or lower than the limit liquid content is set in the following range: (bh+5)℃≦T2≦(Tg-5)℃ And set T2 to a temperature higher than T1, a liquid content adjusting step of adjusting the liquid content of the wet polyphenylene ether obtained in the solid-liquid separation step to a level equal to or lower than the unfused upper limit liquid content at the heating temperature: T1 set according to the formula before the drying step, The liquid content adjusting step is the wet polyphenylene ether, the liquid content of which has exceeded the unmelted upper limit liquid content at the heating temperature T1, is dried at a temperature equal to or higher than the boiling point of a solvent having the lowest boiling point among the solvent components contained in the wet polyphenylene ether and equal to or lower than the temperature at which the liquid content becomes the unmelted upper limit liquid content at the heating temperature T1, so as to reduce the liquid content to the unmelted upper limit liquid content at the heating temperature T1 or lower. A method for producing polyphenylene ether. [ 3 ] The solvent contained in the wet polyphenylene ether includes a solvent having a boiling point of 50 to 150°C. [1] Or [2] 2. A method for producing the polyphenylene ether according to claim 1 . [ 4 ] A dryer including a first drying unit set at the heating temperature T1 and a second drying unit set at the heating temperature T2 is used, 3 13. A method for producing the polyphenylene ether according to any one of claims 1 to 12. [ 5 ] [1] to [2] use a drying device including a first dryer set to the heating temperature: T1 and a second dryer set to the heating temperature: T2, which are arranged in series. 4 13. A method for producing the polyphenylene ether according to any one of claims 1 to 12. Effect of the Invention

[0013] According to the present invention, it is possible to produce PPE by increasing the drying speed while reducing problems such as scaling and adhesion in the dryer during drying. [Brief description of the drawings]

[0014] [Figure 1]1 is a diagram showing an example of a drying curve when a wet PPE is dried, where the vertical axis indicates the liquid content of the wet PPE on a normal scale, and the horizontal axis indicates the drying time. [Diagram 2] 1 is a diagram showing an example of a drying curve when a wet PPE is dried, where the vertical axis indicates the liquid content of the wet PPE on a logarithmic scale, and the horizontal axis indicates the drying time. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, an embodiment of the present invention (hereinafter, referred to as the present embodiment) will be described in detail. Note that the present invention is not limited to the following embodiment, and can be practiced in various modifications within the scope of the gist of the present invention.

[0016] [PPE] The PPE of this embodiment will be described below. The PPE is a homopolymer and / or copolymer having a repeating unit structure represented by the following formula (1).

[0017] [ka]

[0018] In the above formula (1), a is an integer of 1 to 6, and n is an integer of 1 or greater. R 11 , R 12 , R 13 , R 14 are each independently a hydrogen atom, a saturated or unsaturated hydrocarbon group having 1 to 6 carbon atoms, or a saturated or unsaturated aryl group having 6 to 12 carbon atoms. R 11 , R 12 is preferably a hydrogen atom, a methyl group, an ethyl group, an n-propyl group, or the like, more preferably a hydrogen atom or a methyl group, and further preferably a hydrogen atom. R 13 , R 14As the alkyl group, a methyl group, an ethyl group, an n-propyl group, a vinyl group, an allyl group, an ethynyl group, a propargyl group, etc. are preferable, a methyl group and an ethyl group are more preferable, and a methyl group is further preferable. Here, the saturated or unsaturated hydrocarbon group having 1 to 6 carbon atoms and the saturated or unsaturated aryl group having 6 to 12 carbon atoms may each have a substituent. A is a hydrogen atom or any substituent, each of which preferably contains a carbon-carbon double bond and / or an epoxy bond. Z is a hydrogen atom or any hydrocarbon group when a is 1. When a is 2 to 6, Z is any linking group having a valence of a, and preferred examples of the linking group having a valence of 2 or more include phenol compounds represented by the following formula (2).

[0019] [ka]

[0020] In the above formula (2), The integers for a are the same as those in formula (1), and a is preferably the same as that in formula (1). k is an integer from 1 to 4. X is any a-valent linking group, and is not particularly limited, but examples thereof include hydrocarbon groups such as chain hydrocarbon groups and cyclic hydrocarbon groups; hydrocarbon groups containing one or more atoms selected from nitrogen, phosphorus, silicon, and oxygen; atoms such as nitrogen, phosphorus, silicon, oxygen, etc.; and groups combining these. Preferred examples of X include a hydrocarbon group, an oxygen atom, an alkylamino group, a carbonyl group, a thiocarbonyl group, a sulfinyl group, a sulfonyl group, and combinations of these groups. R 21are each independently any substituent, such as a hydrogen atom, a halogen, or a saturated or unsaturated hydrocarbon group having 1 to 12 carbon atoms. Here, the saturated or unsaturated hydrocarbon group having 1 to 12 carbon atoms may have a substituent. More preferred hydrocarbon groups are one or a combination of a plurality of groups selected from an alkyl group, an alkylthio group, and an alkyloxy group. Even more preferred hydrocarbon groups are alkyl groups having 1 to 8 carbon atoms, such as a methyl group, an ethyl group, and an n-propyl group.

[0021] From the viewpoints of high frequency characteristics, flame retardancy, heat resistance, and solubility in solvents, the weight average molecular weight Mw of the PPE of this embodiment is 2500 to 6000, preferably 2750 to 5750, and more preferably 3000 to 5500. When the weight average molecular weight Mw of the PPE is 2500 or more, the high frequency characteristics, flame retardancy, and heat resistance, which are inherent properties of the PPE, can be sufficiently ensured, and when it is 6000 or less, the solvent solubility can be sufficiently ensured when the PPE is used as an electronic material or composite material. The number average molecular weight Mn of the PPE of this embodiment is not particularly limited, but is preferably in a range that is soluble in a general-purpose solvent (e.g., toluene, dichloromethane, methyl ethyl ketone, etc.) and does not inhibit mixability with other resins, for use in electronic materials, etc. Therefore, the number average molecular weight Mn of the PPE is preferably 500 to 30,000, more preferably 700 to 15,000, and even more preferably 700 to 10,000. The molecular weight distribution Mw / Mn is preferably 1.1-5, more preferably 1.3-4, and further preferably 1.5-3. The weight average molecular weight Mw, number average molecular weight Mn, and molecular weight distribution Mw / Mn of the PPE can be measured using gel permeation chromatography (GPC), and specifically, are values ​​measured by the measurement method in the examples described later.

[0022] The glass transition temperature (Tg) of the PPE of this embodiment is 100°C to 200°C, preferably 100°C to 190°C, and more preferably 104°C to 175°C. The glass transition temperature of the PPE can be measured using a differential scanning calorimeter, and specifically, it is a value measured by the measurement method in the examples described later.

[0023] [Manufacturing method of PPE] There are two methods for manufacturing PPE: precipitation polymerization and solution polymerization. In both methods, phenols are oxidatively polymerized in the presence of a copper compound and amines in a good solvent for PPE or in a mixed solvent of a good solvent and a poor solvent for PPE. In the precipitation polymerization method, the PPE precipitates during the oxidative polymerization and becomes a slurry. On the other hand, in the solution polymerization method, PPE does not precipitate during oxidative polymerization. In the solution polymerization method, the PPE solution after polymerization is subjected to post-treatment such as concentration if necessary, and then mixed with a poor solvent for PPE to precipitate PPE and form a slurry. In both the precipitation polymerization method and the solution polymerization method, the obtained slurry liquid is washed with a poor solvent or the like, subjected to solid-liquid separation, and if necessary, further washing with a poor solvent for PPE and solid-liquid separation are repeated to obtain wet PPE (solid-liquid separation step). The resulting wet PPE is dried (drying step) to produce a PPE product powder.

[0024] Representative examples of good solvents for PPE include alcohols having 4 or more carbon atoms, such as chloroform (boiling point: 61.2°C), benzene (boiling point: 80.1°C), toluene (boiling point: 110.7°C), o-xylene (boiling point: 144.5°C), m-xylene (boiling point: 139.1°C), p-xylene (boiling point: 138°C), ethylbenzene (boiling point: 136°C), mixed xylenes (mixture of o-xylene, m-xylene, p-xylene, and ethylbenzene), methyl ethyl ketone (boiling point: 79.64°C), and 1-butanol (boiling point: 117.7°C). Among these, at least one selected from the group consisting of benzene, toluene, mixed xylenes, methyl ethyl ketone, and alcohols having 4 or more carbon atoms is preferable, and at least one selected from the group consisting of toluene, 1-butanol, and methyl ethyl ketone is more preferable.

[0025] Representative poor solvents for PPE include ketones such as acetone (boiling point: 56.5° C.), alcohols having 3 or less carbon atoms such as methanol (boiling point: 64.7° C.), ethanol (boiling point: 78.3° C.), 1-propanol (boiling point: 97.2° C.), water, etc. Among these, at least one selected from the group consisting of methanol, ethanol, isopropanol, acetone, and water is preferable, and at least one selected from the group consisting of methanol, ethanol, acetone, and water is more preferable.

[0026] In this embodiment, these good solvents and poor solvents can be used alone, or a combination of a plurality of good solvents and poor solvents can be used. In this embodiment, the good solvent and the poor solvent used in the polymerization may be included in the solvent component (described later) contained in the wet PPE. When the boiling point of the lowest boiling point solvent among the solvent components is taken as bl°C, it is preferable that 45°C≦bl≦120°C, more preferably 50°C≦bl≦115°C, and even more preferably 55°C≦bl≦110°C. Furthermore, when the boiling point of the solvent with the highest boiling point among the solvent components is bh°C, it is preferable that 80°C≦bh≦180°C, more preferably 90°C≦bh≦165°C, and even more preferably 100°C≦bh≦150°C. Furthermore, the difference between bh and bl is preferably 10°C≦(bh-bl)≦130°C, more preferably 20°C≦(bh-bl)≦110°C, and even more preferably 30°C≦(bh-bl)≦90°C. From the viewpoints of safety and production stability, the solvent component preferably contains a solvent having a boiling point of 50 to 150° C. If the boiling point is 50° C. or higher, the risk of the solvent igniting and exploding can be reduced even in a process where temperature is not actively controlled, and safety can be ensured. In addition, if the boiling point is 150° C. or lower, the PPE can be dried well at a set temperature lower than the glass transition temperature Tg of the PPE in the drying process described below, and therefore the PPE can be produced stably without softening.

[0027] [Solid-liquid separation process] The solid-liquid separation step is a step of obtaining wet polyphenylene ether by performing solid-liquid separation on a slurry liquid containing polyphenylene ether, a good solvent for polyphenylene ether, and a poor solvent for polyphenylene ether. The solid-liquid separation can be carried out using any known solid-liquid separator, including, but not limited to, a centrifuge (basket type, vibration type, screw type, decanter type, etc.), a vacuum filter (filter dryer, drum type filter, belt filter, rotary vacuum filter, Young filter, Nutsche filter, etc.), a filter press, a roll press, or the like.

[0028] [Wet PPE liquid content adjustment process] In this embodiment, the liquid content of the wet PPE supplied to the drying step is set to be equal to or lower than the upper limit of the unmelted liquid content, which is the upper limit of the liquid content at which no fusion occurs at the heating temperature T1 (described below) of the dryer heat transfer surface until the content of the solvent component falls to the limit liquid content or lower. If the liquid content of the wet PPE obtained in the solid-liquid separation process before the drying process exceeds the above-mentioned upper limit of the unmelted liquid content, the liquid content can be adjusted to below the above-mentioned upper limit of the unmelted liquid content through a liquid content adjustment process, thereby further suppressing fusion and scaling in the dryer. The unfused upper limit liquid content can be measured by a heating test using an autoclave and an oil bath, and specifically, it is a value measured by the measurement method in the examples described later.

[0029] Methods for adjusting the liquid content of the wet PPE to below the above-mentioned upper unfused liquid content limit include selecting a solid-liquid separator with high separation capacity in the solid-liquid separation process, drying at low temperature in advance using a dryer, air-drying the wet PPE by passing an inert gas (e.g., nitrogen gas) through it, and mixing a low-liquid content PPE with the wet PPE.

[0030] In the method of previously drying at a low temperature using a dryer or the like, the drying temperature is preferably set to a temperature equal to or higher than the boiling point bl°C of the solvent with the lowest boiling point among the solvent components contained in the wet PPE and equal to or lower than the temperature at which the liquid content becomes the above-mentioned upper limit of the unmelted liquid content. The drying time is not particularly limited and may be determined appropriately depending on the size of the device, the amount of raw material, etc.

[0031] In the method of passing an inert gas or the like through wet PPE and air-drying it, the conditions such as the supply rate of the inert gas or the like and the air-drying time are not particularly limited and may be determined appropriately depending on the shape and size of the equipment, the amount of raw materials, etc. The apparatus used for air drying is not particularly limited, and any known air drying apparatus can be used. Alternatively, air may be passed through the solid-liquid separator used in the solid-liquid separation step.

[0032] In the method of mixing low-liquid content PPE with wet PPE, the liquid content of the low-liquid content PPE is not particularly limited as long as the liquid content is lower than the above-mentioned unfused upper limit liquid content, but it is preferably 0.001 mass% or more and less than the unfused upper limit liquid content, and more preferably 0.01 mass% or more and less than the unfused upper limit liquid content. The amount of low liquid content PPE added is not particularly limited, but is preferably 1.0 to 30,000 mass %, and more preferably 3.5 to 28,000 mass %, relative to 100 mass % of wet PPE.

[0033] [Wet PPE drying process] As described above, the wet PPE of this embodiment is obtained by a solid-liquid separation step in the PPE production process, in which a slurry liquid containing the PPE, its good solvent, and a poor solvent is subjected to solid-liquid separation. Drying of wet PPE may exhibit a two-stage, and possibly three or more-stage drying behavior. Figures 1 and 2 show examples of drying curves when wet PPE is dried. In Figure 1, the vertical axis shows the liquid content of the wet PPE on a normal scale, and the horizontal axis shows the drying time. In Figure 2, the vertical axis shows the liquid content of the wet PPE on a logarithmic scale, and the horizontal axis shows the drying time. In FIG. 1, I indicates the material preheating period, II indicates the constant rate drying period, and III indicates the falling rate drying period. In FIG. 2, IIIA indicates the falling rate drying period 1, and IIIB indicates the falling rate drying period 2. The stage called the material preheating stage, indicated by I in Figure 1, is the stage in which the temperature of the wet PPE rises to near the boiling point (bl) of the solvent with the lowest boiling point among the solvent components, and the drying rate is slow during the temperature rise. The stage called constant rate drying, shown as II in FIG. 1, is the stage where the solvent components adhering to the surface of the PPE particles are vaporized and separated, and the drying speed is relatively fast. The stage called falling-rate drying, shown as III in Figure 1, is a stage in which the solvent components inside the PPE particles diffuse to the particle surface after the completion of constant-rate drying, and are evaporated and separated on the surface. The drying speed is slower than that of constant-rate drying. Falling-rate drying can also be divided into falling-rate drying period 1 and falling-rate drying period 2, which will be described later.

[0034] When drying wet PPE, the drying rate may further decrease depending on the solvent composition contained, etc. In this case, the falling-rate drying before the drying rate decrease is called falling-rate drying 1, and the falling-rate drying after the drying rate decrease is called falling-rate drying 2. In this case, the liquid content when switching from constant-rate drying to falling-rate drying 1 is sometimes called limit liquid content 1, and the liquid content when switching from falling-rate drying 1 to falling-rate drying 2 is sometimes called limit liquid content 2, and in this embodiment, limit liquid content 1 is taken as the limit liquid content. The limit liquid content is measured according to the method described in the Examples. The stage called falling-rate drying 1, shown as IIIA in Figure 2, is the stage where a large amount of solvent components are contained inside the particles, the flow path through which the solvent components diffuse onto the particle surface is wide, and the drying speed is fast among falling-rate drying stages. The stage called falling-rate drying 2, shown in IIIB in Figure 2, is the stage where the solvent content inside the particle is reduced, and the flow path through which the solvent content diffuses to the particle surface is narrow, so the drying speed is slow even among falling-rate drying stages. In this embodiment, the content of the solvent component in the wet PPE when switching from constant rate drying to falling rate drying is defined as the limit liquid content.

[0035] Here, the solvent component contained in the wet PPE refers to the solvent contained in the wet PPE to be subjected to the drying step, which is contained in an amount of 0.35 mass% or more relative to the wet PPE (100 mass%). The solvent component may include the above-mentioned good solvent or poor solvent.

[0036] Wet PPE contains solvent components, and when it is heated while the liquid content of the good solvent is high, the surface becomes highly adhesive, causing scaling on the walls of the drying device, or the particles themselves melt and become a hard, candy-like solid, resulting in fusion. Fusion is likely to occur at high temperatures, and is particularly likely to occur on the heat transfer surface with which the wet PPE comes into contact. If the fused material adheres to the heat transfer surface, heat transfer will decrease significantly. Furthermore, if the fused material adheres to the heat transfer surface and falls off and gets mixed into the product, it will become a foreign object, causing a decrease in the physical properties of the final product.

[0037] The inventors have found that when wet PPE contains solvent components at or above the critical liquid content, scaling and fusion are likely to occur when the wet PPE is heated to a high temperature (e.g., by increasing the temperature of the heat transfer surface in contact with the wet PPE), whereas when wet PPE contains solvent components at or below the critical liquid content, scaling and fusion are relatively unlikely to occur even when the wet PPE is heated to a high temperature (e.g., by increasing the temperature of the heat transfer surface in contact with the wet PPE).

[0038] In most cases, the boiling point of the good solvent for PPE is higher than that of the poor solvent for PPE. When drying and removing the low boiling point solvent on the particle surface in the constant rate drying region, the drying speed is highly dependent on the amount of heat supplied. Generally, a dryer with a sufficient heat transfer area is used, but another method is to increase the temperature of the dryer heat transfer surface. In this case, even if the dryer heat transfer surface temperature is set high during constant rate drying of wet PPE, the temperature of the wet PPE will once stabilize near the boiling point of the low-boiling poor solvent, and the low-boiling poor solvent will be preferentially removed, so the drying speed of the high-boiling good solvent will be slow. Therefore, if the dryer heat transfer surface temperature is increased, the high-boiling good solvent in the solvent adhering to the PPE particles will preferentially remain, and PPE particles with a large amount of remaining good solvent will come into contact with the dryer heat transfer surface heated to a high temperature, making it easy for fusion to occur near the heat transfer surface. The inventors have found that fusion can be further suppressed by measuring in advance the upper limit of the unfused liquid content at which fusion does not occur at the dryer heat transfer surface temperature set in the constant rate drying zone, and setting the liquid content of the wet PPE supplied to the dryer in the constant rate drying zone to a value equal to or lower than the upper limit of the unfused liquid content.

[0039] In this embodiment, the wet PPE is supplied to the dryer with its liquid content reduced to below the upper limit of the unfused liquid content, and the heating temperature of the wet PPE is increased after the solvent component content reaches the limit liquid content, thereby enabling the wet PPE to be dried efficiently without causing scaling or fusion.

[0040] When the wet PPE is dried, it is fed to the dryer in a state below the unfused upper limit liquid content, and the heating temperature T1 of the heat transfer surface of the dryer is set to bl° C. or higher and (Tg-30)° C. or lower, until the content of the solvent components in the wet PPE becomes below the limit liquid content, where the boiling point of the lowest boiling point solvent among the solvent components contained in the wet PPE is bl° C. and the glass transition temperature of the PPE is Tg° C. The above T1 is preferably (bl+5)° C. or higher and (Tg-33)° C. or lower, and more preferably (bl+10)° C. or higher and (Tg-36)° C. or lower. By setting the heating temperature: T1 to bl°C or higher, it is possible to dry at a good drying rate, and by setting the heating temperature: T1 to (Tg-30)°C or lower, it is possible to suppress the adhesion and melting of the particle surface and prevent scaling and fusion.

[0041] As the drying progresses and the content of the solvent components in the wet PPE falls below the critical liquid content, the heating temperature T2 of the heat transfer surface of the dryer is set to (bh+5)°C or higher and (Tg-5)°C or lower, where bh°C is the boiling point of the highest boiling point solvent among the solvent components contained in the wet PPE. The above T2 is preferably (bh+10)°C or higher and (Tg-8)°C or lower, and more preferably (bh+15)°C or higher and (Tg-10)°C or lower. By setting the heating temperature T2 of the dryer heat transfer surface to (bh+5)°C or higher, it is possible to dry at a good drying rate, and by setting the heating temperature T2 of the dryer heat transfer surface to (Tg-5)°C or lower, it is possible to suppress the adhesion and melting of particle surfaces and prevent scaling and fusion.

[0042] Here, the heating temperature T1 of the dryer heat transfer surface and the heating temperature T2 of the dryer heat transfer surface refer to the temperature of the drying atmosphere for the wet PPE, and may be the set temperature of the heat medium or electric heater, that is, the drying wall surface temperature. In addition, the heating temperature T1 of the dryer heat transfer surface may be the maximum (wall surface) temperature during the time period in which the wet PPE containing a solvent component at or above the critical liquid content is dried until the content of the solvent component in the wet PPE becomes below the critical liquid content, and the difference between the maximum (wall surface) temperature and the minimum (wall surface) temperature during this time period is preferably 20°C or less, and more preferably 15°C or less. The heating temperature T2 of the dryer heat transfer surface may be the maximum (wall surface) temperature during the period from when the content of the solvent component in the wet PPE becomes equal to or less than the limit liquid content until the dry PPE is obtained, and the difference between the maximum (wall surface) temperature and the minimum (wall surface) temperature during this period is preferably 20°C or less, and more preferably 15°C or less.

[0043] In this embodiment, the heating temperature T2 of the dryer heat transfer surface is set to a temperature higher than the heating temperature T1 of the dryer heat transfer surface. The difference between the heating temperature T1 of the dryer heat transfer surface and the heating temperature T2 of the dryer heat transfer surface is preferably 5°C to 85°C, more preferably 10°C to 70°C, and further preferably 15°C to 55°C.

[0044] In this embodiment, the limit liquid content is preferably 1 to 30 mass %, more preferably 2 to 20 mass %, and further preferably 3 to 15 mass %, relative to the wet PPE (100 mass %) supplied to the drying step.

[0045] [Drying equipment] In the present embodiment, one or more suitable drying devices may be used for the drying, and one or more dryers may be used for the drying device. In addition, each dryer may be provided with one or more drying units. Here, the drying unit may refer to a unit that divides the drying environment to which the wet PPE supplied to the drying process is exposed. In addition, between multiple drying units, the wet PPE being dried may be moved continuously or by being transferred.

[0046] The dryer may be either a continuous dryer or a batch dryer. In either case, the dryer is preferably a so-called indirect heating dryer that has a heat transfer surface that heats the wet PPE by conductive heat transfer and heats the wet PPE by conductive heat transfer from the heat transfer surface. Examples of the heat transfer surface include the surface of the jacket and the surface of the heating tube. Examples of continuous dryers that can be used in this embodiment include agitator dryers such as a paddle dryer, rotary dryers such as a steam tube dryer, fluidized bed dryers, and hopper dryers. Examples of the batch type dryer that can be used in this embodiment include a ribbon mixer dryer and a Nauta mixer. In addition, the above-mentioned continuous dryer can also be used as the batch type dryer. These methods can suppress the occurrence of scaling and fusion, and can efficiently reduce the liquid content (residual solvent).

[0047] [How to change the heating temperature] The continuous dryer used in this embodiment may be equipped with multiple heating units per dryer. For example, when the dryer is equipped with two heating units, it may be possible to set different heating temperatures in the front and rear stages. In this embodiment, for example, the heating temperature of the heat transfer surface of the front-stage dryer can be set to bl°C or higher and (Tg-30)°C or lower to dry to below the limit liquid content, and the heating temperature of the heat transfer surface of the rear-stage dryer can be set to (bh+5)°C or higher and (Tg-5)°C or lower to complete the drying.

[0048] In this embodiment, multiple continuous dryers are arranged in series. For example, when two dryers are provided, the heating temperature of the heat transfer surface of the upstream dryer of the continuous dryers can be set to bl°C or higher and (Tg-30)°C or lower, and the heating temperature of the heat transfer surface of the downstream dryer can be set to (bh+5)°C or higher and (Tg-5)°C or lower, to complete drying. In this case, it is also possible to select an upstream dryer equipped with multiple heating units and to set the temperature differently in the front and rear stages of the heating units. In this case, the heat transfer surface temperature of the heating unit in the front stage of the upstream dryer may be set to bl°C or higher and (Tg-30)°C or lower, the heat transfer surface temperature of the heating unit in the rear stage of the upstream dryer may be set to bl°C or higher and (Tg-5)°C or lower, the heat transfer surface temperature of the heating unit in the front stage of the downstream dryer may be set to bl°C or higher and (Tg-5)°C or lower, and the heat transfer surface temperature of the heating unit in the rear stage of the downstream dryer may be set to (bh+5)°C or higher and (Tg-5)°C or lower.

[0049] When a batch-type dryer is used in this embodiment, the heating temperature of the dryer heat transfer surface can be set to bl°C or more and (Tg-30)°C or less until the content of the solvent component falls below the critical liquid content, and after the content of the solvent component falls below the critical liquid content, the heating temperature of the dryer heat transfer surface can be set to (bh+5)°C or more and (Tg-5)°C or less to complete the drying. In this embodiment, two batch dryers are arranged in series, and, for example, the heating temperature of the heat transfer surface of the first batch dryer is set to be bl°C or higher and (Tg-30)°C or lower, and the heating temperature of the heat transfer surface of the second batch dryer is set to be (bh+5)°C or higher and (Tg-5)°C or lower. The PPE dried in the first batch dryer until the solvent component content falls below the limit liquid content can be loaded into the second batch dryer to complete the drying process.

[0050] In addition, if drying to below the critical liquid content is possible within the heating unit of each dryer, the material can also be dried at a heating temperature of bl°C or higher and (Tg-30)°C or lower until it is discharged from that heating unit, even if the material is below the critical liquid content.

[0051] [Residual solvent in PPE powder after drying] After drying, the PPE is usually in a powder state, and the solvent remains in the powder PPE. The liquid content (residual solvent content) in the dried PPE is preferably 0.35% by mass or less, more preferably 0.30% by mass or less, even more preferably 0.25% by mass or less, and still more preferably 0.20% by mass or less, based on 100% by mass of the dried PPE. By keeping the liquid content after drying to 0.35 mass % or less, it is possible to ensure the stability of the solvent dissolution during processing into a high frequency compatible board material. EXAMPLES

[0052] Hereinafter, the present embodiment will be specifically described with reference to examples and comparative examples, but the present embodiment is not limited to the following examples.

[0053] First, an example , reference example The methods for measuring the physical properties and characteristics used in the comparative examples are shown below.

[0054] (1) Measurement of weight average molecular weight (Mw) and weight average molecular weight (Mw) / number average molecular weight (Mn) A gel permeation chromatography System 21 manufactured by Showa Denko K.K. was used as the measuring device, and a calibration curve was prepared using standard polystyrene and ethylbenzene. Using this calibration curve, the weight average molecular weight (Mw) and number average molecular weight (Mn) of the obtained PPE were measured. The standard polystyrenes used had molecular weights of 3,650,000, 2,170,000, 1,090,000, 681,000, 204,000, 52,000, 30,200, 13,800, 3,360, 1,300, and 550. The columns used were two Showa Denko K-805L columns connected in series. The solvent used was chloroform, with a solvent flow rate of 1.0 mL / min and a column temperature of 40°C. A 1 g / L chloroform solution of PPE was prepared and used as the measurement sample. The UV wavelength of the detection unit was 254 nm for standard polystyrene and 283 nm for PPE. The weight average molecular weight and the weight average molecular weight / number average molecular weight measured above were used as data.

[0055] (2) Measurement of liquid content of wet PPE For the wet PPE in each state, when the PPE powder was dried in a vacuum for 1 hour at a temperature of 140°C and an absolute pressure of 0.013 kPa or less, the mass of the PPE powder was taken as Wd, and the mass of the wet PPE or dry PPE before the vacuum drying was taken as W. The liquid content (mass%) was calculated and quantified using the following formula. Liquid content = {(W-Wd) / W}×100 (mass%)

[0056] (3) Measurement of glass transition temperature The glass transition temperature of the PPE was measured using a differential scanning calorimeter (DSC Pyris-1 manufactured by Perkin-Elmer). In a nitrogen atmosphere, the sample was heated from room temperature to 280°C at a heating rate of 40°C per minute, then cooled to 50°C at a heating rate of 40°C per minute, and the glass transition temperature (°C) was measured at a heating rate of 40°C per minute.

[0057] (4) Judgment of scale and foreign matter After drying, the inside of the dryer was visually inspected and judged as follows: ◎: Only powder is attached, no scale, no adhesion, and no contamination of dried products △: Melted matter and lumpy aggregates adhere to the heat transfer surface, but are not mixed into the dried product, or there are no melted matter or lumpy aggregates on the heat transfer surface, but melted matter is mixed into the dried product. ×: Melted material and lumpy aggregates adhere to the heat transfer surface, etc., and are mixed into the dried product.

[0058] (5) Measurement of limit liquid content The wet PPE was loaded into the dryer to be used, and batch drying was carried out at a heating temperature of (bl+40)°C. During drying, the PPE in the dryer was sampled every 10 minutes, and the liquid content was quantified according to (2) Measurement of the liquid content of wet PPE above. The sampling time was plotted on the horizontal axis and the liquid content on the vertical axis, and two drying curves were created with the vertical axis on a normal scale and a logarithmic scale. After switching from the material preheating period, in which the temperature of the wet PPE rises to near bl, to the constant rate drying period, the inflection point on the shortest time side was taken as the point at which constant rate drying switches to falling rate drying (falling rate drying 1), and the liquid content at this inflection point was taken as the limit liquid content (mass%).

[0059] (6) Measurement of the upper limit of unfused liquid content 50 g of the wet PPE obtained in the manufacturing example described below was weighed and placed in an autoclave. After replacing the inside of the autoclave with nitrogen, it was immersed in an oil bath heated to a heating temperature of T1°C. After heating the autoclave in the oil bath for 30 minutes, the autoclave was removed from the oil bath and cooled to the outside temperature. The autoclave was opened and the presence or absence of fusion of the PPE was visually confirmed. When no fusion occurred, it was determined that the unfused upper limit liquid content was equal to or greater than the liquid content of the wet PPE after solid-liquid separation. If fusion occurred, the wet PPE was dried at a low temperature (a temperature at which fusion does not occur) to reduce the liquid content in 1% increments. The above heating test was performed again using the adjusted wet PPE. This process was repeated, and the highest liquid content at which fusion did not occur was determined as the upper limit of the unfused liquid content (mass%) at heating temperature T1.

[0060] (dryer 1) Nara Machinery Co., Ltd. Paddle dryer Model NPD-1.6W-12L-LG Effective volume: 12L The jacket is designed to be heated by a type of steam. (Dryer 2) Nara Machinery Co., Ltd. Paddle dryer Model NPD-1.6WG-SFG Usable volume: 77L The jacket is designed to be heated by a type of steam.

[0061] [Production Example 1] In a 400-liter jacketed reactor equipped with a sparger for introducing oxygen-containing gas at the bottom of the reactor, stirring turbine blades and baffles, and a reflux condenser on the vent gas line at the top of the reactor, 67.0 g of cupric chloride dihydrate, 245.0 g of 35% hydrochloric acid, 2558.3 ​​g of N,N,N',N'-tetramethylpropanediamine, 18.9 kg of n-butanol, 170.1 kg of methanol, and 48.0 kg of 2,6-dimethylphenol were placed. The composition weight ratio of the solvents used was n-butanol:methanol=10:90. Next, oxygen was introduced into the reactor from the sparger at a rate of 48.0 L / min while vigorously stirring, and at the same time, the polymerization temperature was adjusted by passing a heat medium through the jacket to maintain it at 45°C. The polymerization liquid gradually took on the form of a slurry. 120 minutes after the start of oxygen introduction, the aeration of the oxygen-containing gas was stopped, and a 50% aqueous solution of 346.7 g of ethylenediaminetetraacetic acid tripotassium salt (reagent manufactured by Dojindo Laboratories) was added to the polymerization mixture, followed by the addition of 432.0 g of hydroquinone (reagent manufactured by Wako Pure Chemical Industries, Ltd.) in small portions, and the reaction was carried out at 45 ° C for 1 hour until the slurry-like PPE turned white. After the reaction was completed, the mixture was filtered and washed three times with a quantity of washing solution (b) such that the mass ratio (b) / (a) of the methanol washing solution (b) to the PPE (a) to be washed was 4, and the mixture was subjected to solid-liquid separation under pressure using a filter dryer manufactured by Kobelco Eco Solutions Co., Ltd. to obtain wet polyphenylene ether. When cracks or cracks occurred in the wet polyphenylene ether wet cake layer during solid-liquid separation, the mixture was spread with the stirring blade attached to the filter dryer (an operation to level the wet cake surface and fill the cracks or cracks) and pressure was continued. Pressure was continued until the filtrate no longer came out completely. The filtration time was 68 minutes, the liquid content of the wet PPE was 27.8% by mass, the Mw after drying was 2897, the Mw / Mn was 1.9, the Tg was 149°C, the limit liquid content was 5.8% by mass, the upper limit of unfused liquid content at T1=125°C was 26.2% by mass, the upper limit of unfused liquid content at T1=120°C was 26.8% by mass, the upper limit of unfused liquid content at T1=118°C was 27.1% by mass, the upper limit of unfused liquid content at T1=109°C was 29.0% by mass, the upper limit of unfused liquid content at T1=70°C was greater than 27.8% by mass, the upper limit of unfused liquid content at T1=68°C was greater than 27.8% by mass, and the upper limit of unfused liquid content at T1=55°C was greater than 27.8% by mass.

[0062] [Production Example 2] The procedure was carried out in the same manner as in Production Example 1, except that the slurry after three washings was subjected to solid-liquid separation using a basket center manufactured by Tanabe Wiltec to obtain wet polyphenylene ether. The liquid content of the wet PPE was 45.2% by mass, the Mw after drying was 2897, the Mw / Mn was 1.9, the Tg was 149°C, the limit liquid content was 5.8% by mass, the upper limit of unfused liquid content at T1=125°C was 26.2% by mass, the upper limit of unfused liquid content at T1=120°C was 26.8% by mass, the upper limit of unfused liquid content at T1=118°C was 27.1% by mass, the upper limit of unfused liquid content at T1=109°C was 29.0% by mass, the upper limit of unfused liquid content at T1=70°C was greater than 45.2% by mass, the upper limit of unfused liquid content at T1=68°C was greater than 45.2% by mass, and the upper limit of unfused liquid content at T1=55°C was greater than 45.2% by mass.

[0063] [Production Example 3] PPE was obtained in the same manner as in Production Example 1, except that the solvents used were 56.8 kg of n-butanol and 132.5 kg of methanol, the composition weight ratio of the solvents used was n-butanol:methanol = 30:70, and the phenolic compound used was a mixture of 40.5 kg of 2,6-dimethylphenol and 7.5 kg of 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane. The liquid content of the wet PPE was 44.5 mass%, Mw after drying was 3727, Mw / Mn was 1.5, Tg was 140°C, the limit liquid content was 6.5 mass%, the unfused upper limit liquid content at T1 = 109°C was 30.0 mass%, and the unfused upper limit liquid content at T1 = 55°C was more than 44.5 mass%.

[0064] The evaluation results of the PPE obtained in Production Examples 1 to 3 are shown in Table 1. [Table 1]

[0065] [Example 1] The wet PPE obtained in Production Example 1 was weighed out at 5.0 kg and placed in the front-stage dryer 1, and nitrogen was supplied to the shaft seal at a flow rate of 20 L / min. After rotating the paddle at 30 rpm, steam of 0.14 MPa was supplied to the jacket. The heating temperature of the jacket surface was 109°C. The wet PPE was dried until the liquid content reached 5.0% by mass, and the drying time was 11 minutes. The pre-dryer 1 was opened to check the internal scale and fusion. Although there was a thin powdery deposit on the surface of the jacket, paddles, and paddle shaft of the pre-dryer 1, there was no scale or fusion. In addition, no fused foreign matter was mixed into the dried PPE. 3.1 kg of PPE dried to a liquid content of 5.0% by mass was placed in the rear dryer 1, in which 0.37 MPa steam had been previously supplied to the jacket and nitrogen had been supplied to the shaft seal at a flow rate of 20 L / min, and the paddle was rotated at 30 rpm. The heating temperature of the jacket surface was 139°C. After drying for 241 minutes, the liquid content of the PPE was 0.20% by mass. The rear-stage dryer 1 was opened to check the internal scale and fusion state. Although there was a thin powdery deposit on the surface of the jacket, paddles, and paddle shaft of the rear-stage dryer 1, there was no scale or fusion. In addition, no fused foreign matter was mixed into the dried PPE.

[0066] [Comparative Example 1] Pre-drying was carried out in the same manner as in Example 1 except that the drying time in the pre-dryer 1 was changed to 9 minutes, and the liquid content of the wet PPE after drying was 8.7% by mass. The pre-dryer 1 was opened to check the internal scale and fusion. Although there was a thin powdery deposit on the surface of the jacket, paddles, and paddle shaft of the pre-dryer 1, there was no scale or fusion. In addition, no fused foreign matter was mixed into the dried PPE. The wet PPE having a liquid content of 8.7% by mass was charged into the latter-stage dryer 1, and the latter-stage drying was carried out for 241 minutes in the same manner as in Example 1, whereupon the liquid content was found to be 0.31% by mass. The latter-stage dryer 1 was opened to check the internal scale and fusion state. Yellow colored candy-like fused material had scaled on the surfaces of the jacket, paddles, and paddle shaft of the latter-stage dryer 1. In addition, flake-like fused material was found mixed in the dried PPE as foreign matter. Furthermore, layers of scale had adhered to the surfaces of the jacket, paddles, and paddle shaft, which reduced the heat transfer efficiency and made it impossible to sufficiently reduce the liquid content.

[0067] [Comparative Example 2] Preliminary drying was performed in the same manner as in Example 1, except that the wet PPE obtained in Production Example 2 was used as the drying raw material. The wet PPE was dried until the liquid content was 5.0% by mass, and the drying time was 19 minutes. The pre-drying machine 1 was opened to check the internal scale and adhesion. Yellow, candy-like fused material had scaled on the surface of the jacket, paddles, and paddle shaft of the pre-drying machine 1. Yellow, candy-like fused material granules were found in the PPE after the pre-drying. The second stage drying was carried out in the same manner as in Example 1, except that the yellow, candy-like fused granules were removed from the PPE after the first stage drying. The rear-stage dryer 1 was opened to check the internal scale and fusion state. Although there was a thin powdery deposit on the surface of the jacket, paddles, and paddle shaft of the rear-stage dryer 1, there was no scale or fusion. No fused foreign matter was mixed into the dried PPE.

[0068] [Example 2] The same procedure as in Example 1 was carried out except that warm water was run through the front-stage dryer 1 so that the jacket surface temperature became 68°C, and the wet PPE obtained in Production Example 2 was used as the drying raw material. The drying times in the front-stage and rear-stage dryers 1 until the liquid content approached the target liquid content were 103 and 228 minutes, respectively. The PPE liquid content in the front-stage and rear-stage dryers 1 was 5.1% by mass and 0.22% by mass, respectively. After drying was completed, the front and rear dryers 1 were opened to check the internal scale and fusion. Although there was a thin powdery deposit on the surface of the jacket, paddle and paddle shaft of both dryers, there was no scale or fusion. In addition, there was no fused material or other foreign matter in the dried PPE.

[0069] [Example 3] 10 kg of the wet PPE with a liquid content of 45.2% by mass obtained in Production Example 2 was charged into a powder stirring tank, and nitrogen gas was supplied to the gas phase at 100 L / min while stirring. Hot water at 55°C was run through the jacket of the powder stirring tank, and after stirring for 12 minutes, the liquid content was measured and found to be 27.9% by mass. The same procedure as in Example 1 was carried out except that the wet PPE with a liquid content of 27.9% by mass was charged into the dryer 1. Steam of 0.14 / 0.37 MPa was supplied to the jackets of the front-stage and rear-stage dryers 1. The jacket surface temperatures of the front-stage and rear-stage dryers 1 were 109 / 139° C., respectively. The PPE liquid contents in the front-stage and rear-stage dryers 1 were 5.0% by mass and 0.21% by mass, respectively. After drying was completed, the front and rear dryers 1 were opened to check the internal scale and fusion. Although there was a thin powdery deposit on the surface of the jacket, paddle and paddle shaft of both dryers, there was no scale or fusion. In addition, there was no fused material or other foreign matter in the dried PPE.

[0070] [Example 4] In the solid-liquid separation using the basket centrifuge in Production Example 2, the operation of the basket centrifuge was continued for 40 minutes while supplying nitrogen gas at 100 L / min to the wet PPE after deliquescence. The liquid content of the obtained wet PPE was 26.8% by mass. The same procedure as in Example 1 was carried out except that the wet PPE having a liquid content of 26.8% by mass was charged into the dryer 1. Steam of 0.14 / 0.37 MPa was supplied to the jackets of the front-stage and rear-stage dryers 1. The jacket surface temperatures of the front-stage and rear-stage dryers 1 were 109 / 139° C., respectively. In the front-stage dryer 1, drying was possible until the PPE liquid content reached 5.0 mass % after 10 minutes of operation. In the rear-stage dryer 1, drying was possible until the PPE liquid content reached 0.23 mass % after 222 minutes of operation. The front and rear dryers 1 were opened to check the internal scale and fusion. Although there was a thin powdery deposit on the surface of the jacket, paddles and paddle shaft of the rear dryer 1, there was no scale or fusion. In addition, no fused foreign matter was mixed into the dried PPE.

[0071] [ reference Example 5] When 3.14 kg of the wet PPE obtained in Production Example 2 and 1.86 kg of dry PPE with a liquid content of 0.2% by mass were weighed and mixed by stirring, the liquid content of the mixed PPE was 28.5% by mass. The mixed PPE was charged into the front-stage dryer 1, and nitrogen gas was supplied to the shaft seal at a flow rate of 20 L / min. After rotating the paddle at 30 rpm, steam of 0.14 MPa was supplied to the jacket. The heating temperature of the jacket surface was 109°C. When the PPE was dried until the liquid content reached 5.0% by mass, the drying time was 11 minutes, and 3.8 kg of wet PPE was obtained after drying. 3.8 kg of PPE dried to a liquid content of 5.0% by mass was placed in the rear dryer 1, in which 0.37 MPa steam had been supplied to the jacket and nitrogen gas had been supplied to the shaft seal at a flow rate of 20 L / min, and the paddle was rotated at 30 rpm. The heating temperature of the jacket surface was 139°C. After drying for 222 minutes, the liquid content of the PPE was 0.23% by mass. After drying was completed, the front and rear dryers 1 were opened to check the internal scale and fusion. Although there was a thin powdery deposit on the surface of the jacket, paddle and paddle shaft of both dryers, there was no scale or fusion. In addition, there was no fused material or other foreign matter in the dried PPE.

[0072] [ reference Example 6] When 2.84 kg of the wet PPE obtained in Production Example 2 and 2.16 kg of the dry PPE with a liquid content of 0.2% by mass were weighed and mixed by stirring, the liquid content of the mixed PPE was 25.8% by mass. The mixed PPE was charged into the front-stage dryer 1, and nitrogen gas was supplied to the shaft seal at a flow rate of 20 L / min. After rotating the paddle at 30 rpm, steam of 0.18 MPa was supplied to the jacket. The heating temperature of the jacket surface was 117°C. When the PPE was dried until the liquid content reached 5.0% by mass, the drying time was 6 minutes, and 3.8 kg of the wet PPE after drying was obtained. Steam of 0.37 MPa was supplied to the jacket in advance, and nitrogen gas was supplied to the shaft seal at a flow rate of 20 L / min. In the rear-stage dryer 1, 4.0 kg of PPE dried to a liquid content of 5.0 mass% was placed and the paddle was rotated at 30 rpm. The heating temperature of the jacket surface was 139°C. After drying for 241 minutes, the liquid content of the PPE was 0.20 mass%. After drying was completed, the front and rear dryers 1 were opened to check the internal scale and fusion. Although there was a thin powdery deposit on the surface of the jacket, paddle and paddle shaft of both dryers, there was no scale or fusion. In addition, there was no fused material or other foreign matter in the dried PPE.

[0073] [Comparative Example 3] reference The wet PPE with a liquid content of 28.5% by mass prepared in Example 5 was charged into the pre-drier 1. reference The procedure was carried out in the same manner as in Example 6. In pre-dryer 1, drying was possible until the PPE liquid content reached 5.0% by mass after 10 minutes of operation. Pre-dryer 1 was opened to check the internal scale and fusion status. Yellow, candy-like fused material had scaled on the surfaces of the jacket, paddles, and paddle shafts of pre-dryer 1. Yellow, candy-like fused material granules were mixed into the PPE after pre-drying. After the first drying, the yellowish, candy-like fused granules were removed from the PPE, and the rest was added in the second drying period 1. referenceThe same procedure as in Example 6 was carried out. In the latter-stage dryer 1, the PPE was dried until the liquid content reached 0.23% by mass after 222 minutes of operation. The latter-stage dryer 1 was opened to check the internal scale and fusion state. Although there was a thin powdery deposit on the surface of the jacket, paddle, and paddle shaft of the latter-stage dryer 1, there was no scale or fusion. In addition, no fused foreign matter was mixed into the dried PPE.

[0074] [Example 7] Two dryers 2 were arranged in series, and 0.14 MPa steam was supplied to the front dryer 2 jacket. The temperature of the front dryer 2 jacket surface was 109 ° C. The temperature of the rear dryer 2 jacket surface was 139 ° C. Both the front and rear dryers 2 were supplied with 100 L / min of nitrogen gas from the discharge side, and the paddles were rotated at 30 rpm. The wet PPE obtained in Production Example 1 was supplied to the front dryer 2. The PPE discharged from the front dryer 2 was temporarily stored in a hopper heated to 109 ° C and supplied to the rear dryer 2. The residence times of the front and rear dryers 2 were adjusted to 11 / 241 minutes, which is the same as in Example 1. After six hours of operation, the liquid content of the PPE discharged from the front-stage and rear-stage dryers 2 stabilized at 5.1% by mass and 0.19% by mass, respectively. After operating for 9 hours, the front and rear dryers 2 were opened to check the internal scale and fusion. Although there was a thin powdery deposit on the surface of the jacket, paddle and paddle shaft of both dryers, there was no scale or fusion. Furthermore, there was no fused foreign matter mixed in with the dried PPE.

[0075] [Comparative Example 4] The same procedure as in Example 7 was carried out, except that the residence times in the front-stage and rear-stage dryers 2 were adjusted to 9 and 246 minutes, respectively. After six hours of operation, the liquid content of the PPE discharged from the front-stage and rear-stage dryers 2 stabilized at 8.7% by mass and 0.39% by mass, respectively. After operating for 9 hours, the front and rear dryers 2 were opened to check for internal scale and adhesion. Although there was a thin powdery deposit on the surface of the jacket, paddles and paddle shaft of the front-stage dryer 2, it had not progressed to the stage of scaling or fusion. In addition, there was no fused foreign matter mixed in with the dried PPE. Yellow, candy-like fused material was found scaling on the surfaces of the jacket, paddles, and paddle shafts of the rear-stage dryer 2. Yellow, candy-like fused material granules were found in the PPE after rear-stage drying.

[0076] [Comparative Example 5] The same procedure as in Example 7 was repeated except that the wet PPE obtained in Production Example 2 was used. After six hours of operation, the liquid content of the PPE discharged from the front-stage and rear-stage dryers 2 stabilized at 12.1% by mass and 0.58% by mass, respectively. After operating for 9 hours, the front and rear dryers 2 were opened to check the internal scale and adhesion. Both dryers had yellow, candy-like fused scaling on the surfaces of the jacket, paddles, and paddle shafts. In addition, yellow, candy-like fused granules were found in the PPE after drying in both dryers.

[0077] [Comparative Example 6] The same procedure as in Comparative Example 5 was carried out except that the residence time in the front-stage dryer 2 was 20 minutes. After six hours of operation, the liquid content of the PPE discharged from the front-stage and rear-stage dryers 2 stabilized at 5.2% by mass and 0.24% by mass, respectively. After operating for 9 hours, the front-stage and rear-stage dryers 2 were opened to check the internal scale and adhesion. For the front-stage dryer 2, yellow-colored, candy-like fused scaling was found on the surfaces of the jacket, paddles, and paddle shaft. Yellow-colored, candy-like fused granules were mixed in the PPE after the front-stage drying. For the rear-stage dryer 2, although there was a thin powdery deposit on the surfaces of the jacket, paddles, and paddle shaft, there was no scale or adhesion. Yellow-colored, candy-like fused granules were mixed in the PPE after the rear-stage drying.

[0078] [Example 8] The same procedure as in Example 7 was carried out, except that warm water was run through the front-stage dryer 2 so that the jacket surface temperature reached 68°C, the wet PPE with a liquid content of 45.2% by mass obtained in Production Example 2 was used as the drying raw material, and the drying time in the front-stage dryer 2 was set to a time at which the liquid content after the front stage was equal to or less than the limit liquid content. The drying times in the front-stage and rear-stage dryers 2 until the liquid content approached the target liquid content were 103 and 235 minutes, respectively. The PPE liquid contents in the front-stage and rear-stage dryers 2 were 5.3% by mass and 0.21% by mass, respectively. After drying was completed, the front and rear dryers 2 were opened to check the internal scale and fusion. Although there was a thin powdery deposit on the surface of the jacket, paddles and paddle shafts in both dryers, there was no scale or fusion. In addition, there was no fused material or other foreign matter in the dried PPE.

[0079] [Example 9] 10 kg of the wet PPE with a liquid content of 44.5% by mass obtained in Production Example 3 was placed in a powder stirring tank, and nitrogen gas was supplied to the gas phase at 100 L / min while stirring. Hot water at 55°C was run through the jacket of the powder stirring tank, and stirring was continued for 12 minutes. The liquid content was then measured and found to be 28.6% by mass. The same procedure as in Example 1 was carried out except that the above-mentioned wet PPE with a liquid content of 28.6% by mass was charged into the dryer 1. Steam of 0.14 / 0.30 MPa was supplied to the jackets of the front-stage and rear-stage dryers 1. The jacket surface temperatures of the front-stage and rear-stage dryers 1 were 109 / 133° C., respectively. The PPE liquid contents in the front-stage and rear-stage dryers 1 were 6.0% by mass and 0.22% by mass, respectively. After drying was completed, the front and rear dryers 1 were opened to check the internal scale and fusion. Although there was a thin powdery deposit on the surface of the jacket, paddle and paddle shaft of both dryers, there was no scale or fusion. In addition, there was no fused material or other foreign matter in the dried PPE.

[0080] Working Example , reference example The evaluation results of the comparative examples are shown in Table 2. [Table 2] [Industrial Applicability]

[0081] The present invention makes it possible to suppress the occurrence of scaling and fusion during drying of wet PPE, enabling efficient drying. It also makes it possible to provide PPE that does not experience deterioration in physical properties even when processed into final products such as molded products, without the inclusion of fused bodies in the product.

Claims

1. a solid-liquid separation step of subjecting a slurry liquid containing polyphenylene ether having a weight average molecular weight (Mw) of 2500 to 6000 and a glass transition temperature (Tg) of 100 to 200° C., a good solvent for the polyphenylene ether, and a poor solvent for the polyphenylene ether to solid-liquid separation to obtain wet polyphenylene ether; a drying step of drying the wet polyphenylene ether, The liquid content of the wet polyphenylene ether at the start of the drying step is equal to or less than an upper limit of the liquid content at which fusion does not occur at a heating temperature T1 set according to the following formula (upper unfused liquid content limit), When the boiling point of the lowest boiling point solvent among the solvent components contained in the wet polyphenylene ether is bl° C. and the boiling point of the highest boiling point solvent is bh° C., In the drying step, The heating temperature T1 until the content of the solvent component becomes equal to or less than the limit liquid content is set in the following range: bl℃≦T1≦(Tg-30)℃ The heating temperature T2 after the content of the solvent component becomes equal to or lower than the limit liquid content is set in the following range: (bh+5)℃≦T2≦(Tg-5)℃ Furthermore, T2 is set to a temperature higher than T1; a liquid content adjusting step of adjusting the liquid content of the wet polyphenylene ether obtained in the solid-liquid separation step to a level equal to or lower than the unfused upper limit liquid content at the heating temperature: T1 set in accordance with the formula before the drying step, The liquid content adjusting step includes: aeration of the wet polyphenylene ether, the liquid content of which has exceeded the unfused upper limit liquid content at the heating temperature T1, so as to reduce the liquid content to equal to or lower than the unfused upper limit liquid content at the heating temperature T1; A method for producing polyphenylene ether.

2. A solid-liquid separation step of obtaining wet polyphenylene ether by solid-liquid separation of a slurry liquid containing polyphenylene ether having a weight average molecular weight (Mw) of 2500 to 6000 and a glass transition temperature (Tg) of 100 to 200°C, a good solvent for the polyphenylene ether, and a poor solvent for the polyphenylene ether; a drying step of drying the wet polyphenylene ether, The liquid content of the wet polyphenylene ether at the start of the drying step is equal to or less than an upper limit of the liquid content at which fusion does not occur at a heating temperature T1 set according to the following formula (upper unfused liquid content limit), When the boiling point of the lowest boiling point solvent contained in the solvent components of the wet polyphenylene ether is bl° C. and the boiling point of the highest boiling point solvent is bh° C., In the drying step, The heating temperature T1 until the content of the solvent component becomes equal to or less than the limit liquid content is set in the following range, bl℃≦T1≦(Tg-30)℃ The heating temperature T2 after the content of the solvent component becomes equal to or lower than the limit liquid content is set in the following range: (bh+5)℃≦T2≦(Tg-5)℃ Furthermore, T2 is set to a temperature higher than T1; a liquid content adjusting step of adjusting the liquid content of the wet polyphenylene ether obtained in the solid-liquid separation step to a level equal to or lower than the unfused upper limit liquid content at the heating temperature: T1 set in accordance with the formula before the drying step, The liquid content adjusting step includes: a step of drying the wet polyphenylene ether having a liquid content exceeding the unmelted upper limit liquid content at the heating temperature T1 at a temperature equal to or higher than the boiling point of a solvent having the lowest boiling point among solvent components contained in the wet polyphenylene ether and equal to or lower than a temperature at which the liquid content becomes the unmelted upper limit liquid content at the heating temperature T1, so as to reduce the liquid content to the unmelted upper limit liquid content at the heating temperature T1 or lower. A method for producing polyphenylene ether.

3. 3. The method for producing polyphenylene ether according to claim 1, wherein the wet polyphenylene ether contains a solvent having a boiling point of 50 to 150°C.

4. The method for producing polyphenylene ether according to any one of claims 1 to 3, wherein a dryer including a first drying unit set at the heating temperature: T1 and a second drying unit set at the heating temperature: T2 is used.

5. The method for producing polyphenylene ether according to any one of claims 1 to 4, wherein a drying device is used that includes a first dryer set to the heating temperature: T1 and a second dryer set to the heating temperature: T2, which are arranged in series.

Citation Information

Patent Citations

  • Production of mono- and di- functional oligophenylene oxide

    JP1987039628A

  • Production method of polyphenylene ether

    JP2001335632A

  • Method for producing polyphenylene ether

    JP2004099681A

  • Method for producing granular polyphenylene ether resin

    JP2006241258A

  • Process for producing polyphenylene ether

    JP2017179009A