Polyisocyanurate-containing foams with long cream time and fast cure properties

A reaction mixture with polyisocyanate compounds, trimerization catalysts, and low molecular weight polyols provides polyisocyanurate-containing foams with extended cream times and rapid curing, addressing the limitations of existing processes for composite honeycomb structures.

JP7581407B2Active Publication Date: 2024-11-12HUNTSMAN ICI CHEM LLC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023055576
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-01-16
Filing Date
2023-03-30
Publication Date
2024-11-12
Estimated Expiration
2038-10-05

AI Technical Summary

Technical Problem

Current techniques for producing polyisocyanurate-containing foams for composite honeycomb structures are limited by short cream times and/or long curing times, lacking sufficient process flexibility.

Method used

A reaction mixture comprising polyisocyanate compounds, a trimerization catalyst, low molecular weight polyols, and water-based blowing agents, with specific catalyst and polyol concentrations, achieves long cream times and fast curing properties.

Benefits of technology

The reaction mixture enables polyisocyanurate-containing foams with cream times over 35 seconds and curing times under 110 seconds, enhancing processing flexibility and reducing manufacturing cycle times.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581407000001
    Figure 0007581407000001
  • Figure 0007581407000002
    Figure 0007581407000002
  • Figure 0007581407000003
    Figure 0007581407000003
Patent Text Reader

Abstract

To provide a reaction mixture and a production method for producing, a polyisocyanurate-including foam comprising density in a range of 50 to 500 kg / m3.SOLUTION: A method comprises: mixing components of a reaction mixture at an isocyanate index of at least 200 for forming a foam. The reaction mixture includes: a polyisocyanate composition including at least one polyisocyanate compound; a catalyst composition including at least a trimerized catalyst compound by at least 50 mass% based on total weight of all catalyst compounds in the catalyst composition; and one or more foaming agents including at least a low molecular weight polyol having a molecular amount of less than 200 g / mol, by 2-20 mass% based on total weight of the isocyanate reactive composition, and including at least 50 mol% of water based on a total molar amount of the all foaming agents, in the reaction mixture, a cream time is greater than 35 seconds and a quick curable property is achieved.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to reaction mixtures for producing polyisocyanurate-containing cellular materials, and more particularly to polyisocyanurate-containing rigid foams for use in composite materials such as honeycomb structures.

[0002] The present invention further relates to a method for making said polyisocyanurate-containing materials that achieves long cream times and fast cure.

[0003] The invention further relates to polyisocyanurate-containing foams suitable for the production of composite materials. [Background technology]

[0004] However, current technology for producing polyisocyanurate-containing foams suitable for making composite honeycomb structures has several process problems, such as cream times that are too short and / or cure times that are too long.

[0005] One object of the present invention is to produce polyisocyanurate-containing composites, and to provide reaction mixtures which allow the preparation of polyisocyanurate-containing composites with better process flexibility, particularly with respect to cream time and fast cure.

[0006] U.S. Patent No. 6,602,927 discloses a method for producing a polyisocyanurate foam component. US Patent No. 6,602,927 provides an isocyanurate system comprising a polyisocyanate reactive component comprising a trimerization catalyst, a polyol, and a carboxylic acid (and optionally water as a co-blowing agent) and a polyisocyanate. The reaction system can be foamed with just the carboxylic acid to produce SRIM (structural reaction injection molded) articles that can be demolded with reduced mold hold times. However, US Patent No. 6,602,927 provides a method for the preparation of polyisocyanurate systems that are primarily water blown (using at least 50 mole % water based on the total molar amount of all blowing agents used), particularly for use with cleaners. It does not provide sufficient process flexibility in terms of cure time and fast cure.

[0007] U.S. Patent No. 5,109,031 deals with rigid cellular low density polymers prepared by reacting a polyol component comprising a polyester polyol having a free glycol content of less than about 7% by weight, based on the total weight of the polyester polyol, with an organic polyisocyanate in the presence of a blowing agent. The purpose of U.S. Patent No. 5,109,031 is to improve thermal insulation. However, U.S. Patent No. 5,109,031 states that Mainly water-blown (use at least 50 mol% water based on the total molar amount of all blowing agents used) For high density polyisocyanurate foam systems, especially with regard to cream time and fast cure does not provide sufficient process flexibility.

[0008] U.S. Pat. No. 6,207,725 further describes isocyanate reactions involving polyester polyols. This paper deals with a method for producing rigid polyurethane foams and rigid urethane-modified polyisocyanurate foams by reacting a polyurethane composition with an organic polyisocyanate composition in the presence of an amine catalyst.

[0009] The objective of U.S. Patent No. 6,207,725 is to achieve rapid foam rise. Thus, U.S. Patent No. 6,207,725 discloses a method for achieving long cream times and fast cure primarily through water foaming (using at least 50 mole percent water based on the total molar amount of all foaming agents used). It does not provide any such processing details. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] U.S. Patent No. 6,602,927 [Patent Document 2] U.S. Patent No. 5,109,031 [Patent Document 3] U.S. Patent No. 6,207,725 Summary of the Invention

[0011] It is an object of the present invention to improve the processing for producing polyisocyanurate foamed materials suitable for use in composite materials such as honeycomb structures. It is an object of the present invention to achieve the production of polyisocyanurate-containing foams while achieving a long cream time of at least 35 seconds and a fast cure. The fast cure provides a more efficient cure and therefore shorter cycle times, while the long cream time allows flexibility in handling times (e.g., for spraying the reaction mixture and / or for This allows enough time for the mold to fill before hardening.

[0012] Surprisingly, we have discovered reaction mixtures for producing polyisocyanurate-containing foams that lead to long cream times and fast cure.

[0013] The reaction mixture of the present invention provides increased cream time and fast cure, which allows easier processing on the laminator, and allows for the production of PIR foams that are not currently possible using state of the art reaction mixtures due to limitations imposed by the foaming kinetics of state of the art reaction mixtures. It is believed that molding is possible.

[0014] Summary of the Invention According to the first aspect, 50 to 500 kg / m 3 A reaction mixture for producing a polyisocyanurate (PIR)-containing foam having a density in the range of at least 200 and having an isocyanate index of at least ■ a polyisocyanate composition containing one or more polyisocyanate compounds; ■ a catalyst composition comprising at least a trimerized catalyst compound in an amount of at least 50 wt. %, based on the total weight of all catalyst compounds in the catalyst composition; At least a low molecular weight (MW) polyol having a molecular weight of less than 200 g / mol is added to an isocyanate. isocyanate-reactive compound in an amount of 0.1 to 30% by weight based on the total weight of the isocyanate-reactive composition composition; one or more blowing agents that contain at least 50 mol % water, based on the total molar amount of the blowing agents; and ■ Optionally, one or more surfactants, one or more flame retardants, one or more antioxidants, or Combinations of these; wherein the weight percent of the trimerization catalyst compound is [trimerization catalyst compound + polyisocyanate] The content of the component (I) in the composition is less than 0.5% by weight based on the total weight of the composition.

[0015] According to some embodiments, the weight percent of the trimerization catalyst compound is [catalyst composition + polyisocyanate]. The anate composition is preferably less than 0.5% by weight, more preferably less than 0.45% by weight, even more preferably less than 0.4% by weight, and most preferably less than 0.35% by weight, based on the total weight of the anate composition.

[0016] According to some embodiments, the weight percent of the trimerization catalyst compound is [catalyst composition + polyisocyanate]. The anate composition is less than 0.3% by weight based on the total weight of the anate composition.

[0017] According to some embodiments, the trimerization catalyst compound is selected from organic salts, preferably alkali metal organic salts, alkaline earth metal organic salts, and / or quaternary ammonium organic salts (e.g., acetic acid). Potassium hexanoate, potassium hexanoate, potassium ethylhexanoate, potassium octanoate, milk The salt is selected from potassium phosphate, N-hydroxypropyltrimethylammonium octanoate, N-hydroxypropyltrimethylammonium formate, and mixtures thereof.

[0018] According to some embodiments, the low molecular weight (MW) polyol is less than 150 g / mol, preferably has a molecular weight of less than 100 g / mol.

[0019] According to some embodiments, the low molecular weight (MW) polyol is selected from glycerol and / or ethylene glycol.

[0020] According to some embodiments, the amount of low molecular weight (MW) polyol is in the range of 1 to 25 weight percent, more preferably in the range of 2 to 20 weight percent, based on the total weight of the isocyanate-reactive composition.

[0021] According to some embodiments, the amount of trimerized catalyst compound is at least 75 wt %, and preferably at least 90 wt %, based on the total weight of all catalyst compounds in the catalyst composition.

[0022] According to some embodiments, the polyisocyanate compound is selected from toluene diisocyanate, methylene diphenyl diisocyanate, polyisocyanate compositions containing methylene diphenyl diisocyanate, or mixtures of such polyisocyanates.

[0023] According to some embodiments, the one or more isocyanate-reactive compounds in the reaction mixture are Additionally, the copolymers have an average nominal hydroxy functionality of 1 to 8 and a number average molecular weight in the range of 200 to 8000 g / mol. and the monool and / or polyol ( For example, polyether polyols, polyester polyols, mercaptans, polybasic acids and mixtures with carboxylic acids, amines, or polyamines such as phenylalanine, ...

[0024] According to some embodiments, the blowing agent is water, isobutene, dimethyl ether, methylene chloride, acetone, chlorofluorocarbons (CFCs), hydrofluorocarbons (HFCs), hydrochlorofluorocarbons (HCFCs), hydrofluoroolefins (HFOs), and / or carbon blacks. and 0.1 to 80 parts by weight per 100 parts by weight of one or more isocyanate-reactive compounds selected from hydrogen fluoride and It is present in an amount of 0.2 to 60 parts by weight (pbw), preferably in an amount of 0.2 to 60 pbw.

[0025] According to the second aspect, 50 to 500 kg / m 3 Polyisocyanurate-containing hardeners having densities in the range A method for producing a foam having a cream time of greater than 35 seconds and fast cure is disclosed, the method comprising combining and mixing ingredients of a reaction mixture according to a first aspect of the present invention at an Isocyanate Index of at least 200 to obtain a foam.

[0026] According to some embodiments, the cream time is greater than 45 seconds, more preferably greater than 55 seconds, and the fast cure is less than 110 seconds, preferably less than 90 seconds, more preferably less than 70 seconds.

[0027] According to some embodiments, the isocyanate index is greater than 220, preferably greater than 250.

[0028] According to a third aspect, a polyisocyanurate-containing material obtainable by the process according to the second aspect is disclosed.

[0029] According to some embodiments, the polyisocyanurate-containing material according to the present invention has a viscosity of 50 kg / m 3 ~500kg / m 3 in the range of 75 kg / m 3 ~300kg / m 3 in the range of 100 kg / m 3 ~200kg / m 3 The material has a free rise density (measured according to ISO 845) in the range of

[0030] According to a fourth aspect, the polyisocyanurate-containing material according to the invention is incorporated into a composite honeycomb structure. The use of the compound in an article is disclosed.

[0031] Particular and preferred features of the invention are set out in the independent and dependent claims. Features from the dependent claims may be combined with features of the independent claims or with features of other dependent claims as appropriate.

[0032] The above and other characteristics, features and advantages of the present invention will become apparent from the following detailed description, which is for illustrative purposes only and is not intended to limit the scope of the present invention.

[0033] Terms and their meanings In the context of the present invention, the following terms have the following meanings.

[0034] (1) "Isocyanate Index" (NCO Index or Index) It is the ratio of NCO groups to isocyanate-reactive hydrogen atoms present in a formulation, expressed as a percentage: [NCO] x 100 / [reactive hydrogen atoms].

[0035] In other words, the NCO index is a function of the amount of isocyanate-reactive hydrogens used in the formulation. It represents the percentage of isocyanate actually used in a formulation relative to the amount of isocyanate theoretically required to react.

[0036] It should be noted that the Isocyanate Index used herein is considered in terms of the actual polymerization process that produces a material that contains an isocyanate component and an isocyanate-reactive component. (including isocyanate derivatives such as those called prepolymers in Isocyanate groups consumed in the preliminary stage or in the preliminary stage (e.g., isocyanate The activity consumed in the reaction of esters with ethylene glycol to produce modified polyols and modified polyamines Hydrogen is not considered in the calculation of the Isocyanate Index: only free isocyanate groups and free isocyanate-reactive hydrogens (including water hydrogen atoms, if water is used) are considered.

[0037] (2) "Isocyanate-reactive compounds" and "isocyanate-reactive hydrogen atoms" This term is used herein to calculate the Isocyanate Index and represents the sum of the active hydrogen atoms in the hydroxyl and amine groups present in an isocyanate-reactive compound. This means that for the purposes of calculating the Isocyanate Index in an actual polymerization process, one hydroxyl group is considered to contain one reactive hydrogen and one The primary amine group is considered to contain one reactive hydrogen, and one water molecule contains two active This means that the compound is considered to contain hydrogen.

[0038] (3) "Reaction system" The polyisocyanate is maintained in one or more containers separate from the isocyanate-reactive components. A combination of compounds in the form of

[0039] (4) "Average Nominal Hydroxyl Functionality" (or simply "functionality"). The term is used herein to refer to the number average functionality (total number of active hydrogens per molecule) of the initiator used in the preparation of a polyol or polyol composition. It is used to indicate the number average functionality (number of hydroxyl groups per molecule) of In practice, however, it is often somewhat lower due to some terminal unsaturation.

[0040] (5) “Average” Unless otherwise stated, numbers represent averages.

[0041] (6) “Trimerization catalyst” As used herein, it refers to a catalyst that can catalyze (promote) the production of isocyanurate groups from polyisocyanates. This means that isocyanates react with other isocyanates to produce polymers with isocyanurate structures (polyisocyanates). This means that the reaction between isocyanate and polyol and between isocyanate and isocyanate may occur simultaneously. This process may occur in succession, resulting in the formation of a polymer containing urethane and isocyanurate structures (PIR-PUR).

[0042] (7) "Polyisocyanurate-containing materials" (form) It refers to a material composition containing urethane and isocyanurate structures (PIR-PUR) produced with an isocyanate index of 200 or greater, and more preferably with an isocyanate index of greater than 220.

[0043] (8) "Free-rise density" It represents the density measured according to ISO 845 for foam samples produced under atmospheric conditions (in the presence of a blowing agent).

[0044] (9) "Cream Time" It represents the time required for the reaction mixture to change from a liquid to a creamy state and subsequently begin to foam (expand).

[0045] (10) "snap cure behavior" or "rapid cure" This indicates that the difference between tack-free time and cream time is small or negligible. Cure time is often also called demold time. Tack-free time (TFT) is the time when the cure begins. The tack-free time is the time from when the foam is pressed to when the outer skin of the foam is no longer tacky. The tack-free time can be determined by pressing a polyethylene film against the surface and checking for the presence of any sticky material when the film is removed.

[0046] Detailed Description The present invention will be described with reference to certain embodiments. It should be noted that the term "comprising" used in the claims should not be interpreted as being limited to the means listed thereafter, nor does it exclude other elements or steps. It should therefore be interpreted as specifying the presence of the stated features, steps or components, but not excluding the presence or addition of one or more other features, steps, components or groups thereof. Therefore, the scope of the expression "a device comprising means A and B" should not be limited to a device consisting of only components A and B. It means that the most relevant components of the device in the context of the present invention are A and B.

[0047] Throughout this specification, the phrase "one embodiment" or "an embodiment" is used. Such a phrase indicates that a particular feature described in connection with that embodiment is included in at least one embodiment of the invention. Thus, throughout this specification, The appearances of the phrases "in one embodiment" or "in an embodiment" in various places throughout this specification are not necessarily all referring to the same embodiment (including, but not limited to, the same embodiment). In addition, as will be apparent to those skilled in the art, certain features Or features may be combined in any suitable manner in one or more embodiments. .

[0048] It should be understood that, while preferred embodiments and / or materials have been described for providing an embodiment in accordance with the present invention, various modifications and variations can be made without departing from the spirit and scope of the invention.

[0049] The present invention relates to such a reaction system in which both a long cream time (greater than 35 seconds) and a rapid cure (fast curing) are achieved. The present invention further relates to a method for producing polyisocyanurate-containing foams, and more particularly to a method for producing polyisocyanurate-containing rigid foams for use in composite materials (such as honeycomb structures) using the reaction system of the present invention. [1] 50-500kg / m 3 1. A reaction mixture for producing a polyisocyanurate (PIR)-containing foam having a density in the range of ■ a polyisocyanate composition containing one or more polyisocyanate compounds; ■ a catalyst composition comprising at least a trimerized catalyst compound in an amount of at least 50 wt. %, based on the total weight of all catalyst compounds in the catalyst composition; ■ an isocyanate-reactive composition comprising at least a low molecular weight (MW) polyol having a molecular weight of less than 200 g / mole in an amount of 0.1 to 30 wt. %, based on the total weight of the isocyanate-reactive composition; one or more blowing agents that contain at least 50 mol % water, based on the total molar amount of all blowing agents; and ■ Optionally, one or more surfactants, one or more flame retardants, one or more antioxidants, or combinations thereof; wherein the weight percent of the trimerization catalyst compound is less than 0.5 weight percent based on the total weight of the [trimerization catalyst compound + polyisocyanate composition]. [2] The reaction mixture of [1], wherein the trimerization catalyst compound is selected from organic salts, preferably alkali metal organic salts, alkaline earth metal organic salts, and / or quaternary ammonium organic salts, such as potassium acetate, potassium hexanoate, potassium ethylhexanoate, potassium octanoate, potassium lactate, N-hydroxypropyltrimethylammonium octanoate, N-hydroxypropyltrimethylammonium formate, and mixtures thereof. [3] The reaction mixture according to any one of [1] to [2], wherein the low molecular weight (MW) polyol has a molecular weight of less than 150 g / mol, preferably less than 100 g / mol. [4] The reaction mixture according to any one of [1] to [3], wherein the low molecular weight (MW) polyol is selected from glycerol and / or ethylene glycol. [5] The reaction mixture according to any one of [1] to [4], wherein the amount of low molecular weight (MW) polyol is in the range of 1 to 25% by weight, more preferably in the range of 2 to 20% by weight, based on the total weight of the isocyanate-reactive composition. [6] The reaction mixture according to any one of [1] to [5], wherein the amount of the trimerization catalyst compound is at least 75% by weight, preferably at least 90% by weight, based on the weight of all catalyst compounds in the catalyst composition. [7] The reaction mixture according to any one of [1] to [6], wherein the polyisocyanate compound is selected from toluene diisocyanate, methylene diphenyl diisocyanate, a polyisocyanate composition containing methylene diphenyl diisocyanate, or a mixture of such polyisocyanates. [8] The reaction mixture according to any one of [1] to [7], wherein the one or more isocyanate-reactive compounds further comprise mono-ols and / or polyols having an average nominal hydroxy functionality of 1 to 8 and a number average molecular weight in the range of 200 to 8000 g / mol, and mixtures of said mono-ols and / or polyols, such as polyether polyols, with polyester polyols, mercaptans, carboxylic acids such as polybasic acids, amines, or polyamines. [9] The reaction mixture according to any one of [1] to [8], wherein the blowing agent further contains, in addition to water, isobutene, dimethyl ether, methylene chloride, acetone, chlorofluorocarbons (CFCs), hydrofluorocarbons (HFCs), hydrochlorofluorocarbons (HCFCs), hydro(chloro)fluoroolefins (HFOs / HCFOs), and / or hydrocarbons.

[10] 50-500kg / m 3 The method for producing a polyisocyanurate-containing rigid foam having a density in the range of 1 to 30, the method comprising mixing together components of a reaction mixture according to any one of [1] to [9] above, the reaction mixture having a cream time of less than 35 seconds and a density of 30 to 300, the reaction mixture having a cream time of less than 35 seconds and a density of 30 to 300, and the reaction mixture having a cream time of less than 35 seconds and a density of 30 to 300, ...

[11] The method according to

[10] , wherein the cream time is more than 45 seconds, more preferably more than 55 seconds, and the fast setting time, defined as the difference between the tack-free time and the cream time, is less than 110 seconds, preferably less than 90 seconds, more preferably less than 70 seconds.

[12] The method according to any one of

[10] to

[11] , wherein the isocyanate index is greater than 220, preferably greater than 250.

[13] The method according to any one of

[10] to

[12] , wherein the weight percentage of the trimerization catalyst compound is preferably less than 0.45 weight%, more preferably less than 0.40 weight%, and most preferably less than 0.35 weight%, based on the total weight of the trimerization catalyst compound and the polyisocyanate composition.

[14] The method according to any one of

[10] to

[13] , wherein the weight percentage of the trimerization catalyst compound is less than 0.30 weight percent based on the total weight of the trimerization catalyst compound and the polyisocyanate composition.

[15] A polyisocyanurate-containing material obtained by the production method according to any one of

[10] to

[14] .

[16] 75kg / m 3 ~300kg / m 3 in the range of 100 kg / m 3 ~200kg / m 3 3. The polyisocyanurate-containing material according to claim 15, having a free rise density, measured in accordance with ISO 845, in the range of

[17] Use of the polyisocyanurate-containing material according to

[16] in a composite honeycomb structure.

[18] A composite material having a composite honeycomb structure having a core layer containing the polyisocyanurate-containing material according to any one of

[15] to

[16] . DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0050] According to the first aspect of the present invention, 50 to 500 kg / m 3 A reaction system for producing polyisocyanurate-containing foams having a free rise density (measured according to ISO 845) in the range of The reaction system comprises at least ■ a polyisocyanate composition containing one or more polyisocyanate compounds; ■ a catalyst composition comprising at least a trimerized catalyst compound in an amount of at least 50 wt. %, based on the total weight of all catalyst compounds in the catalyst composition; At least a low molecular weight (MW) polyol having a molecular weight of less than 200 g / mol is added to an isocyanate. isocyanate-reactive compound in an amount of 0.1 to 30% by weight based on the total weight of the isocyanate-reactive composition composition; ■ one or more blowing agents containing at least 50 mol % water, based on the total weight of the blowing agents; and ■ Optionally, one or more surfactants, one or more flame retardants, one or more antioxidants, or Combinations of these; wherein the weight percent of the trimerization catalyst compound is [trimerization catalyst compound + polyisocyanate] The content of the component (I) in the composition is less than 0.5% by weight based on the total weight of the composition.

[0051] According to some embodiments, the weight percent of the trimerization catalyst compound is [catalyst composition + polyisocyanate]. The anate composition is preferably less than 0.5% by weight, more preferably less than 0.45% by weight, even more preferably less than 0.4% by weight, and most preferably less than 0.35% by weight, based on the total weight of the anate composition.

[0052] According to some embodiments, the weight percent of the trimerization catalyst compound is [catalyst composition + polyisocyanate]. The anate composition is less than 0.3% by weight based on the total weight of the anate composition.

[0053] According to some embodiments, the low molecular weight (MW) polyol is less than 200 g / mol, preferably has a molecular weight of less than 150 g / mole, more preferably less than 100 g / mole.

[0054] The advantage of the reaction mixture of the present invention is that it can produce polyisocyanurate (PIR) with a long shelf life. The advantage of using 100% ethylene glycol is that it can be used to achieve both high build times and fast cure times. This combined effect translates into shorter manufacturing cycle times, for example in composite applications.

[0055] According to some embodiments, the catalyst composition comprises at least a trimerized catalyst compound in an amount of at least 75 weight percent, more preferably at least 90 weight percent, based on the total weight of all catalyst compounds in the catalyst composition.

[0056] According to a preferred embodiment of the first aspect of the present invention, the trimerization catalyst compound is selected from organic salts. Preferably, said organic salt is selected from alkali metal organic salts, alkaline earth metal organic salts, and / or quaternary ammonium organic salts. More preferably, said organic salt is selected from the group of carboxylates and alkoxides and mixtures thereof, carboxylates / alkoxides having 1 to 12 carbon atoms, and mixtures thereof. Preferred examples are potassium carboxylates, Sodium carboxylates, potassium alkoxides, and sodium alkoxides. Additionally, carboxylates / alkoxides with ring structures (e.g., sodium benzoate and potassium benzoate) are also suitable trimerization catalysts. The most preferred examples are potassium acetate, Potassium hexanoate, potassium ethylhexanoate, potassium octanoate, potassium lactate, N-hydroxypropyltrimethylammonium octanoate, N-hydroxypropyltrimethylammonium formate, and mixtures thereof. Suitable catalysts are commercially available, such as Catalyst LB available from Huntsman, Dabco® K2097 (containing potassium acetate) and Dabco K15 (containing potassium octanoate) available from Air Products.

[0057] According to some embodiments, a low molecular weight (MW) polyol having a molecular weight of less than 200 g / mole. is present in the reaction mixture in an amount of 0.1 to 30% by weight based on the total weight of the isocyanate-reactive composition. Preferably, it is present in an amount of from 1 to 25% by weight, more preferably from 2 to 20% by weight.

[0058] According to some embodiments, the one or more isocyanate-reactive compounds of low molecular weight are monoisocyanate-reactive compounds of low molecular weight. Suitable examples are monools selected from methanol, ethanol, propanol, butanol, phenol, cyclohexanol, and hydrocarbon monools (such as aliphatic monools and polyether monools) having a number average molecular weight of up to 200 g / mol, and / or monools selected from monoethylene glycol, diene monools, di ...

[0033] Examples of suitable glycerols include ethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, trimethylolpropane, sorbitol, glycerol, propanediol, butanediol, pentanediol, hexanediol, and glycerols having a molecular weight of less than 200 g / mol, preferably less than 150 g / mol, and more preferably less than 100 g / mol. The polyol is selected from aromatic and / or aliphatic polyols having a molecular weight of

[0059] According to some embodiments, the isocyanate-reactive composition comprises, in addition to a low molecular weight polyol, a polyol having a number average molecular weight of preferably 200 to 8000 and an average nominal functionality of preferably 1 to 8. Further included are high molecular weight polyols, which may be selected from polyether polyols, polyester polyols, mercaptans, carboxylic acids (e.g., polybasic acids), amines, polyamines having an average nominal hydroxy functionality of 1 to 8 and a number average molecular weight of up to 8000, and mixtures thereof. Examples of suitable polyols include Hoopol® 1000, ... TM F-1390 (a polyester polyol available from Synthesia) and Daltolac® R-166 (a polyether polyol available from Huntsman). Riolu.

[0060] According to a second aspect of the present invention, the reaction mixture of the present invention is used to prepare polyisocyanate-containing A method for producing a polystyrene foam is disclosed, which method accordingly comprises mixing together the components of a reaction mixture at an Isocyanate Index of at least greater than 200, preferably at an Isocyanate Index of 220 or greater.

[0061] According to some embodiments, the method of making polyisocyanate-containing foams of the present invention includes a cream time of greater than 35 seconds, preferably greater than 45 seconds, and more preferably greater than 55 seconds, and a cream time of less than 110 seconds. The curing rate is preferably less than 90 seconds, and more preferably less than 70 seconds.

[0062] There are many different orders for contacting or combining the compounds necessary to produce the polyisocyanurate-containing foams of the present invention, and as will be apparent to those skilled in the art, it is within the scope of the present invention to vary the order in which these compounds are added.

[0063] According to some embodiments, in the reaction mixture for producing the PIR-containing foam of the present invention, The polyisocyanate compounds used are aliphatic isocyanates (e.g. hexamethyl diisocyanate), more preferably aromatic isocyanates (e.g., m-phenylene diisocyanate, p-phenylene diisocyanate, tolylene-2,4-diisocyanate, triisocyanate, phenylene-2,6-diisocyanate, diphenylmethane-4,4'-diisocyanate, chlorophenylene-2,4-diisocyanate, naphthylene-1,5-diisocyanate, diphenylene-4,4'- Diisocyanate, 4,4'-diisocyanate-3,3'-dimethyldiphenyl, 3-methyldiphenyl phenylmethane-4,4'-diisocyanate, and diphenyl ether diisocyanate), alicyclic diisocyanates (e.g., cyclohexane-2,4-diisocyanate, cyclohexa 1-methylcyclohexyl-2,3-diisocyanate, 1-methylcyclohexyl-2,4-diisocyanate, 1-methylcyclohexyl-2,6-diisocyanate, and the above diisocyanates and bis-(isocyanate)s. tricyclohexyl)-methane], and triisocyanates (e.g., 2,4,6- Triisocyanatotoluene and 2,4,4'-triisocyanatodiphenyl ether) The isocyanate is selected from organic isocyanates having a plurality of isocyanate groups.

[0064] According to some embodiments, the polyisocyanate composition comprises a mixture of polyisocyanates, such as a mixture of tolylene diisocyanate isomers (e.g., a commercial mixture of the 2,4-isomer and the 2,6-isomer) and a mixture of diisocyanates and aniline / formaldehyde condensates. and mixtures with higher polyisocyanates obtained by phosgenation. Such mixtures are well known in the art and include crude phosgenation products which contain mixtures of methylene bridged polyphenyl polyisocyanates, including diisocyanates, triisocyanates, and higher polyisocyanates, together with by-products of phosgenation.

[0065] The preferred polyisocyanate compositions of the present invention are those in which the polyisocyanate is an aromatic diisocyanate or a polyisocyanate of higher functionality (especially diisocyanates). Polyisocyanates in the case of crude mixtures of methylene-bridged polyphenyl polyisocyanates containing isocyanates, triisocyanates, and polyisocyanates of higher functionality Methylene-bridged polyphenyl polyisocyanates (e.g., methylene diphenyl Methylene bridged polyphenyl diisocyanates (abbreviated as MDI) are well known in the art and have the general formula I, where n is 1 or more and, in the case of crude mixtures, represents an average value greater than 1. Crude mixtures of methylene bridged polyphenyl polyisocyanates are prepared by phosgenation of the corresponding mixtures of polyamines obtained by the condensation reaction of aniline with formaldehyde.

[0066] [ka] Other suitable polyisocyanate compositions include isocyanate-terminated prepolymers prepared by the reaction of an excess of a diisocyanate or a higher functionality polyisocyanate with a hydroxyl-terminated polyester or hydroxyl-terminated polyether, and polyisocyanate-based prepolymers prepared by the reaction of an excess of a diisocyanate or a higher functionality polyisocyanate with a polyol monomer or monomers (e.g., ethylene glycol, trimethylolpropane, or butanediol, etc. One preferred class of isocyanate-terminated prepolymers is diisocyanate, triisocyanate, The prepolymer is an isocyanate-terminated prepolymer obtained from a crude mixture of methylene bridged polyphenyl polyisocyanates, which contain isocyanates of higher functionality, and methylene bridged polyphenyl polyisocyanates.

[0067] According to some embodiments, the polyisocyanate compound in the polyisocyanate composition is selected from toluene diisocyanate, methylene diphenyl diisocyanate, a polyisocyanate composition comprising methylene diphenyl diisocyanate, or a mixture of such polyisocyanates.

[0068] According to some embodiments, the isocyanate index is greater than 200, preferably greater than 220, and more preferably greater than 250. The isocyanate index may be in the range of, for example, 200-1000, 200-600, or 200-400.

[0069] The use of reaction mixtures having an isocyanate index of greater than 200 (leading to the production of isocyanurates), for example in composite honeycomb applications, offers several advantages over reaction mixtures having an isocyanate index of about 100 (leading to the production of polyurethanes). For example, isocyanate indexes greater than 200 generally release more heat and therefore require lower mold temperatures to achieve resin cure (i.e., energy savings). The high aromatic content of the reaction mixture with ethylenediaminetetraacetate gives the final composite better flame properties and also a higher crosslink density, resulting in increased mechanical strength (higher Tg).

[0070] According to some embodiments, the blowing agent is preferably water, used alone or in combination with another blowing agent, such as isobutene, dimethyl ether, methylene chloride, acetone, chlorofluorocarbons (CFCs), hydrofluorocarbons, etc. The blowing agent may be selected from hydrocarbons such as benzene (HFC), hydrochlorofluorocarbons (HCFC), hydrofluoroolefins (HFO), and pentanes. The amount of blowing agent used may vary based on, for example, the intended use of the foam product and the desired foam stiffness and foam density. The blowing agent is present in an amount of 0.1 to 80 parts by weight (pbw) per 100 parts by weight of isocyanate-reactive compound (polyol), including the weight of the catalyst composition, more preferably in an amount of 0.2 to 60 pbw. You may.

[0071] According to some embodiments, one or more optional urethane catalyst compounds may be added to the reaction mixture. However, the trimerization catalyst compound must be present in an amount of more than 50% by weight based on the total weight of all catalyst compounds used. Suitable urethane catalysts for use herein include metal salt catalysts (e.g., organotin compounds), amine compounds (e.g., triethylenediamine (TEDA), N-methylimidazole, 1,2-dimethylimidazole, N-methylmorpholine, N-ethylmorpholine, triethylamine, N,N'-dimethylpiperazine, 1,3,5-tris(dimethylaminopropyl)hexahydrotriazine, 2,4,6 ... (ethyl)phenol, N-methyldicyclohexylamine, pentamethyldipropylenetriamine amine, N-methyl-N'-(2-dimethylamino)-ethyl-piperazine, tributylamine, pentaerythritol dimethyldiethylenetriamine, hexamethyltriethylenetetramine, heptamethyltetraethylenepentamine, dimethylaminocyclohexylamine, pentamethyldipropylene-triamine, triethanolamine, dimethylethanolamine, bis(dimethylaminoethyl)ether, tris(3-dimethylamino)propylamine, or its acid bromine and mixtures thereof.

[0072] The present invention further relates to polyisocyanurate-containing foams produced using the process of the present invention and utilizing the reaction mixtures disclosed in the present invention, and the use of said foams in, for example, composite materials, e.g., fast cycle automotive applications (e.g., parcel shelves, road floors, headlights, etc.). Fiber-reinforced honeycomb composite structures for containers, trays, semi-structural components, etc. It relates to the use of [construction].

[0073] According to some embodiments, the polyisocyanurate-containing material of the present invention has a viscosity of 50 kg / m 3 ~500 kg / m 3 in the range of 75 kg / m 3 ~300kg / m3 in the range of 100 kg / m 3 ~200kg / m 3 The material has a free rise density (measured according to ISO 845) in the range of

[0074] In accordance with a preferred embodiment, a composite material is disclosed having a composite honeycomb structure including a core layer comprising a polyisocyanurate-containing material produced in accordance with the present invention.

[0075] According to some embodiments, the reaction mixture of the present invention can be applied by spraying from a spray nozzle, for example onto a honeycomb structure or into a mold, after mixing with the required components at the exit point.

[0076] In some embodiments, the polyisocyanurate-containing foams of the present invention can be used, for example, in honeycomb structures. The polyisocyanurate-containing foams of the present invention can be prepared by allowing sufficient time for the reaction mixture to be sprayed evenly onto a substrate (e.g., fiberglass, honeycomb assemblies, etc.) and / or by inserting the reaction mixture into a heated compression mold, whereupon curing occurs (preferably fast curing so that cycle times are as short as possible). (b) meet all requirements that would enable the provision of sufficient time for the EXAMPLES

[0077] Chemicals used Hoopol (registered trademark) F-1390: polyester commercially available from Synthesia Terpolyol (OH value: 240mgKOH / g) Daltolac® R-166: Polyether polyol available from Huntsman (OH number: 165 mg KOH / g) Tegostab (registered trademark) B8490: A silicone surfactant commercially available from Evonik (OH value: 0 mgKOH / g) ■LB Catalyst: Potassium acetate PIR catalyst available from Huntsman (OH value: 865 mg KOH / g; potassium acetate 48.2 wt%, MEG 48.2 wt%, water 3.6 wt%) DETDA: Diethyltoluenediamine (OH value: 630 mgKOH / g) available from Lonza. Used as a chain extender DABCO® 33LV: A gelling catalyst available from Air Products (OH number: 560 mg KOH / g, 33 wt. % TEDA (triethylenediamine) in dipropylene glycol). ■ Jeffcat (registered trademark) PMDETA: Pentamethyldiethylenetriamine, a blowing catalyst commercially available from Huntsman (OH number: 0 mg KOH / g) Glycerol: Available from Huntsman (OH value: 1826 mg KOH / g) MEG: Monoethylene glycol (OH value: 1808 mg KOH / g) available from Sigma-Aldrich ■ Black Repitan (registered trademark) 90655: A polyether medium commercially available from REPI Carbon black dispersion (OH value: 30mgKOH / g) ■IMR VP063235: Internal release agent commercially available from KVS Eckert & Woelk ■ S2085: Suprasec (registered trademark) 2085 (polymeric MDI, NCO value: 30.5) available from Huntsman ■S5025: Supracek 5025 (polymeric MDI, NCO value: 31.0) available from Huntsman Examples 1 to 7 and Comparative Examples 1 to 2 All foams were produced by mixing the polyol blend (prepared in advance) and isocyanate using a high shear Heidolph mixer (approximately 4000 rpm) under free rise conditions on a cup scale (approximately 120 g) for 10 seconds. Foam density was measured according to standard test method ISO 845.

[0078] The amounts of ingredients used to make the foams of the present invention (Examples 1-7) and the comparative foams (Comparative Examples 1-2) are shown in Table 1, expressed in parts by weight (pbw).

[0079] Compared to Comparative Example 1 (without low molecular weight polyol), Examples 1 and 2 contain an increased amount of glycerol. As a result, the cream time became longer (55 seconds → 65 seconds → 70 seconds) and the hardening time became faster as can be seen from the decrease in Δt. In other words, the presence of glycerol improves the fast setting property while at the same time not decreasing the cream time (i.e., the cream time is long). hold the time).

[0080] Looking at Comparative Example 2 and Examples 4, 5, 6, and 7 (increasing amounts of MEG), a similar trend is observed (CT: 47 sec → 67 sec → 82 sec → 87 sec → 112 sec; Δt: 103 sec → 83 sec → 58 sec → 28 sec → 28 sec). This improves fast setting while not decreasing cream time.

[0081] Comparing Example 3 with Comparative Example 1, it can be seen that increasing the amount of PIR catalyst and low molecular weight polyol (glycerol in this particular case) can significantly improve the fast cure while maintaining a constant cream time (55 seconds in this particular case, i.e., no decrease). I understand.

[0082] Therefore, all these examples show that the presence of PIR catalysts and low molecular weight polyols results in long creatinine synthesis. It can be seen that the cure time can be maintained (greater than 35 seconds) and the fast cure properties can be improved (reduced Δt).

[0083] [Table 1] Examples 8 to 14 and Comparative Examples 3 to 4 The same foam manufacturing methods as in Examples 1-7 and Comparative Examples 1-2 were used.

[0084] The amounts of ingredients used to make the foams of the present invention (Examples 8-14) and the comparative foams The amounts of the components used to prepare the films (Comparative Examples 3-4) are shown in Table 1 in pbw (parts by weight).

[0085] From Comparative Examples 3 and 4, it can be seen that increasing the amount of PIR catalyst improves the fast curing property (Δt from 365 seconds to 166 seconds). sec), but in the absence of low molecular weight polyol, the cream time (CT) was also 55 sec. It can be seen that the curing time is significantly reduced from 50 to 32 seconds (which is undesirable) in Example 11. In Example 11, the presence of glycerol and a higher amount of PIR catalyst allows a similar CT (58 seconds) to Comparative Example 3 (55 seconds) to be achieved while at the same time achieving a much faster cure (Δt of 57 seconds vs. 365 seconds). seconds).

[0086] Compared to Comparative Example 4 (no low molecular weight polyol present), Examples 8, 9, 10, 11, and 12 As the amount of glycerol increased, the cream time became longer (32 seconds → 38 seconds → 42 seconds → 48 seconds → 58 seconds). It is clear that the presence of glycerol improves the fast setting properties (time from time t to time 65 seconds) and also improves the fast setting properties as seen by the decrease in Δt. In other words, the presence of glycerol improves the fast setting properties while at the same time not decreasing the cream time (i.e., maintaining a long cream time).

[0087] Looking at Comparative Example 4 and Examples 13 and 14 (increased amount of MEG), a similar trend is observed (Clean (Time: 32 sec → 40 sec → 45 sec; Δt: 166 sec → 40 sec → 20 sec). The presence of MEG improved the fast curing property. At the same time, the cream time does not decrease.

[0088] Therefore, all these examples show that the presence of PIR catalysts and low molecular weight polyols results in long creatinine synthesis. It can be seen that the cure time can be maintained (greater than 35 seconds) while the fast cure properties can be improved (reduced Δt).

[0089] The effect of PIR catalyst and / or low molecular weight polyol on foaming kinetics and fast cure properties using polyester (e.g. Hupol F-1390) and polyether (e.g. Daltrac R166) does not affect the trend.

[0090] [Table 2] Example 10 and Comparative Examples 5 to 10 The same foam manufacturing methods as in Examples 1-7 and Comparative Examples 1-2 were used.

[0091] The amounts of ingredients used to make the foam of the present invention (Example 10) and the comparative foam ( The amounts of components used to prepare Comparative Examples 5-10) are shown in Table 3 in pbw (parts by weight).

[0092] Example 10 is the same example shown in Table 2.

[0093] In comparison with Example 10, Comparative Examples 5, 6, 7, 8, 9, and 10 are polyurethane gelling catalysts and blowing catalysts. It is shown that when a large amount of is present, the cream time is significantly reduced to less than 35 seconds while the fast curing property is further deteriorated (Comparative Examples 6, 7, 9, and 10).

[0094] [Table 3] Example 3 and Comparative Examples 11 to 13 The same foam manufacturing methods as in Examples 1-7 and Comparative Examples 1-2 were used.

[0095] The amounts of ingredients used to make the foam of the present invention (Example 3) and the comparative foams (Comparative Examples 11, 12, and 13) are shown in Table 4 in parts by weight (pbw). vinegar.

[0096] Example 3 is the same example as shown in Table 1.

[0097] Compared to Example 3, Comparative Examples 11, 12, and 13 show that when the amount of PIR catalyst was too high (i.e., greater than 0.5 wt %), cream time dropped significantly to values ​​below 35 seconds, despite the presence of glycerol. This indicates that the

[0098] [Table 4]

Claims

1. 75-300kg / m 3 1. A method for producing a polyisocyanurate (PIR) containing foam having a density in the range of The method includes combining and mixing components of a reaction mixture at an Isocyanate Index of at least 200 to obtain a foam; wherein the reaction mixture comprises at least (iii) a polyisocyanate composition containing one or more polyisocyanate compounds; A catalyst composition comprising at least a trimerization catalyst compound in an amount of at least 50% by weight based on the total weight of all catalyst compounds in the catalyst composition; ■ an isocyanate-reactive composition comprising at least a low molecular weight (MW) polyol having a molecular weight of less than 200 g / mole in an amount of 2 to 20 wt. %, based on the total weight of the isocyanate-reactive composition; one or more blowing agents containing at least 50 mol % water based on the total molar amount of all blowing agents; and ■ Optionally, one or more surfactants, one or more flame retardants, one or more antioxidants, or combinations thereof; wherein the weight percent of the trimerization catalyst compound is less than 0.35 weight percent based on the total weight of the [trimerization catalyst compound + polyisocyanate composition], the low molecular weight polyol is selected from glycerol and / or ethylene glycol, the cream time is greater than 35 seconds, and the fast cure, defined as the difference between the tack-free time and the cream time, is less than 110 seconds.

2. The method of claim 1 , wherein the trimerization catalyst compound is selected from an organic salt.

3. The method of any of claims 1 to 2, wherein the low molecular weight (MW) polyol has a molecular weight of less than 150 g / mol.

4. The method according to any one of claims 1 to 3, wherein the low molecular weight (MW) polyol is selected from glycerol.

5. The method according to any one of claims 1 to 4, wherein the amount of the trimerization catalyst compound is 75 wt% or more, based on the weight of all catalyst compounds in the catalyst composition.

6. The polyisocyanate compound is Toluene diisocyanate, methylene diphenyl diisocyanate, A polyisocyanate composition comprising methylene diphenyl diisocyanate, or Mixtures of such polyisocyanates, The method according to any one of claims 1 to 5, wherein the method is selected from the group consisting of

7. 7. The method of any of claims 1 to 6, wherein the one or more isocyanate-reactive compounds comprise mono-ols and / or polyols or mixtures thereof having an average nominal hydroxy functionality of 1 to 8 and a number average molecular weight in the range of 200 to 8000 g / mol.

8. The method according to any one of claims 1 to 7, wherein the blowing agent further comprises, in addition to water, isobutene, dimethyl ether, methylene chloride, acetone, chlorofluorocarbons (CFCs), hydrofluorocarbons (HFCs), hydrochlorofluorocarbons (HCFCs), hydro(chloro)fluoroolefins (HFOs / HCFOs) and / or hydrocarbons.

9. The method of any one of claims 1 to 8, wherein the cream time is greater than 45 seconds.

10. The method of any one of claims 1 to 9, wherein the isocyanate index is greater than 220.

11. The method of any of claims 1 to 10, wherein the weight percent of the trimerization catalyst compound is less than 0.30 weight percent, based on the total weight of the trimerization catalyst compound and the polyisocyanate composition.

12. A polyisocyanurate-containing material obtainable by the method according to any one of claims 1 to 11.

13. Free rise density measured according to ISO 845 is between 100 and 200 kg / m 3 13. The polyisocyanurate-containing material of claim 12, wherein

14. 14. Use of the polyisocyanurate-containing material of claim 13 in a composite honeycomb structure.

15. 14. A composite material having a composite honeycomb structure having a core layer comprising the polyisocyanurate-containing material of claim 12 or 13.

Citation Information

Patent Citations

  • Production of heat-resistant urethane-modified polyisocyanurate foam

    JP1990248419A

  • Laminated light weight panel and manufacture thereof

    JP1997295364A

  • polyisocyanurate foam

    JP2002510730A

  • Raw material composition for rigid polyurethane foam and method for producing rigid polyurethane foam

    JP2004315745A

  • Method for producing rigid foam synthetic resin

    JP2011132520A