Perfluoroether fluororubber and its manufacturing method and application

The multi-stage polymerization method addresses non-uniform vulcanization in perfluoroether fluororubber production, achieving high-strength, low-hardness rubber with improved processability and media resistance, enhancing industrial efficiency and sustainability.

JP7581493B2Active Publication Date: 2024-11-12ZHONGHAO CHENGUANG RES INST OF CHEMICALINDUSTRY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023515689
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-09-09
Filing Date
2021-05-12
Publication Date
2024-11-12
Estimated Expiration
2041-05-12

AI Technical Summary

Technical Problem

Existing perfluoroether fluororubber manufacturing methods face challenges with non-uniform dispersion of vulcanization point monomers, leading to high hardness, poor processability, and extended polymerization times, which affect industrial efficiency and environmental sustainability.

Method used

A multi-stage polymerization method is employed, ensuring uniform distribution of tetrafluoroethylene and vulcanization point monomers, using a three-stage process with controlled pressures and monomer ratios, followed by peroxide vulcanization, to produce a perfluoroether fluororubber with an A-B-A block structure, enhancing flexibility and processability.

Benefits of technology

The method significantly reduces polymerization time from 90 hours to 4 hours or less, resulting in perfluoroether fluororubber with high tensile strength, low hardness, and excellent media resistance, facilitating efficient industrial production and processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581493000001
    Figure 0007581493000001
  • Figure 0007581493000002
    Figure 0007581493000002
Patent Text Reader

Abstract

The present invention provides perfluoroether fluoroelastomer and its manufacturing method and application, said perfluoroether fluoroelastomer is manufactured by multi-stage polymerization, wherein the polymerization monomers in each polymerization stage all comprise tetrafluoroethylene and perfluoroalkyl vinyl ether.The manufacturing method of perfluoroether fluoroelastomer provided by the present invention can shorten the polymerization time, improve manufacturing efficiency, and the finally obtained perfluoroether fluoroelastomer has good processing performance, high strength, low hardness and compression deformation, and good medium resistance.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention belongs to the technical field of fluorine-containing elastomers, and relates to a perfluoroether fluororubber and its production method and application, and more particularly to a copolymer composition of tetrafluoroethylene and perfluoroalkyl vinyl ether and its production method and application. [Background technology]

[0002] Perfluoroether fluoroelastomer is mainly made by copolymerizing tetrafluoroethylene (TFE) and perfluoroalkyl vinyl ether (PAVE) as the main copolymerization monomers, and usually further includes vulcanization point monomers such as perfluorobromine, iodine, and cyano-containing compounds, etc. After vulcanization, the product of perfluoroether fluoroelastomer has excellent high temperature resistance and medium resistance, which is favored by industries such as petrochemical industry and semiconductor industry.

[0003] CN107868163A discloses a method for producing low-temperature resistant perfluoroether elastomers, in which the vulcanization point monomer cannot be uniformly dispersed in the elastomer segments, and the activity of TFE is high, resulting in an increase in the TFE homosegment, which in turn results in poor vulcanization performance and high hardness of the vulcanized rubber, making it difficult to process.

[0004] CN1120343A discloses a method for producing a low-temperature perfluoroether elastomer. This patent application uses high molecular weight perfluoropolyether and perfluoroelastomer to blend them to produce a modified perfluoroether elastomer. Since the modifying monomer perfluoropolyether is added during the polymerization process, the activity of the polymer system is weakened, which lengthens the polymerization time, which is disadvantageous for industrialized production. At the same time, after the polymerization is completed, the perfluoropolyether remaining in the polymer system cannot be recovered and treated, which is disadvantageous for environmental protection.

[0005] Therefore, in order to meet the application requirements, it is necessary to develop perfluoroether fluoroelastomers that have a short manufacturing process time and excellent processability after vulcanization. Summary of the Invention

[0006] The present invention aims to provide perfluoroether fluororubber and its preparation method and application. The preparation method of perfluoroether fluororubber provided by the present invention can shorten the polymerization time, improve the preparation efficiency, and the finally obtained perfluoroether fluororubber has good processing performance, high strength, low hardness and compression deformation, and good medium resistance.

[0007] To achieve the objective, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a method for producing a perfluoroether fluororubber, the perfluoroether fluororubber being produced by a multi-stage polymerization method, Here, the polymerization monomers in each polymerization reaction stage all contain tetrafluoroethylene and perfluoroalkyl vinyl ether.

[0009] Compared with the one-step polymerization method (one-pot method), the present invention adopts a multi-stage polymerization method, which can ensure uniform distribution of tetrafluoroethylene and has fewer homopolymerized segments of tetrafluoroethylene in the segments, so that the final perfluoroether fluororubber has lower hardness and is less subject to compressive deformation.

[0010] In the present invention, the polymerizable monomers in each step of the polymerization reaction further include a vulcanization point monomer, and preferably, the vulcanization point monomer is a perfluoroiodoolefin, more preferably, I(CF2)2OCF=CF2.

[0011] In the multi-stage polymerization method of the present invention, a part of vulcanization point monomer is added in each polymerization stage, which can ensure the uniform distribution of vulcanization point monomer, and further improve the vulcanization performance and processing performance of the final rubber.

[0012] By introducing vulcanization point monomer into polymer, perfluoroether fluoroelastomer can adopt peroxide vulcanization system to carry out crosslinking vulcanization, and at the same time, iodine atom is very easy to deradicalize under the action of radical, which is helpful for peroxide vulcanization. This vulcanization point monomer can improve the processing performance of perfluoroether fluoroelastomer to a certain extent.

[0013] As a preferred technical solution of the present invention, the multi-stage polymerization process is a three-stage polymerization process, and the preparation process comprises: (1) performing a pre-polymerization reaction on a pre-polymerization monomer composed of a vulcanization point monomer, tetrafluoroethylene, and a perfluoroalkyl vinyl ether; (2) adding again a middle-stage polymerization monomer composed of a vulcanization point monomer, tetrafluoroethylene and a perfluoroalkyl vinyl ether to carry out a middle-stage polymerization reaction; (3) adding again a post-polymerization monomer composed of a vulcanization point monomer, tetrafluoroethylene and a perfluoroalkyl vinyl ether to carry out a polymerization reaction, and collecting the reaction product.

[0014] In the present invention, the molar ratio of the vulcanization point monomer, tetrafluoroethylene and perfluoroalkyl vinyl ether in the pre-polymerization monomer is (1-3):(60-70):(30-40).

[0015] In the present invention, the 1-3 may be 1.5, 2, 2.5, etc., the 60-70 may be 62, 64, 65, 68, etc., and the 30-40 may be 32, 34, 35, 36, 38, etc.

[0016] The molar ratio of the vulcanization point monomer, tetrafluoroethylene and perfluoroalkyl vinyl ether in the middle-stage polymerization monomer is (0.1-1):(35-55):(40-65).

[0017] In the present invention, the 0.1-1 may be 0.2, 0.4, 0.5, 0.6, 0.8, etc., the 35-55 may be 38, 40, 42, 45, 48, 50, 52, etc., and the 40-65 may be 42, 45, 48, 50, 52, 55, 58, 60, 62, etc.

[0018] The molar ratio of the vulcanization point monomer, tetrafluoroethylene and perfluoroalkyl vinyl ether in the latter stage polymerization monomer is (1-3):(60-70):(30-40).

[0019] In the present invention, the 1-3 may be 1.5, 2, 2.5, etc., the 60-70 may be 62, 64, 65, 68, etc., and the 30-40 may be 32, 34, 35, 36, 38, etc.

[0020] The perfluoroether fluororubber obtained by the multi-stage polymerization method of the present invention has an ABA block structure, and the A blocks on both sides are terpolymerization vulcanization point monomer / TFE / PAVE (vulcanization point monomer / tetrafluoroethylene / perfluoroalkyl vinyl ether), and the content of perfluoroalkyl vinyl ether in the B block is high, which can ensure that the final perfluoroether fluororubber has good flexibility, which is useful for the processing application of the product. The distribution of the vulcanization point monomer and tetrafluoroethylene in the perfluoroether fluororubber provided by the present invention is uniform, so that its hardness and compression deformation are low, and its processability is good.

[0021] In the preferred technical solution of the present invention, when the total mole number of the pre-polymerization monomer is taken as 100%, the content of the vulcanization point monomer is 1-3%, for example, 1.5%, 2%, 2.5%, etc., the content of the tetrafluoroethylene is 60-70%, for example, 62%, 64%, 65%, 68%, etc., and the content of the perfluoroalkyl vinyl ether is 30-40%, for example, 32%, 34%, 35%, 36%, 38%, etc.

[0022] When the total mole number of the middle-stage polymerization monomers is 100%, the content of the vulcanization point monomer is 0.1-1%, for example, 0.2, 0.4, 0.5, 0.6, 0.8, etc., the content of the tetrafluoroethylene is 35-55%, for example, 38, 40, 42, 45, 48, 50, 52, etc., and the content of the perfluoroalkyl vinyl ether is 40-65%, for example, 42, 45, 48, 50, 52, 55, 58, 60, 62, etc.

[0023] When the total mole number of the latter-stage polymerization monomers is taken as 100%, the content of the vulcanization point monomer is 1-3%, for example, 1.5%, 2%, 2.5%, etc., the content of the tetrafluoroethylene is 60-70%, for example, 62%, 64%, 65%, 68%, etc., and the content of the perfluoroalkyl vinyl ether is 30-40%, for example, 32%, 34%, 35%, 36%, 38%, etc.

[0024] In the present invention, the mass ratio of the first-stage polymerization monomer, the middle-stage polymerization monomer, and the second-stage polymerization monomer is (20-35):(30-60):(20-35).

[0025] The 20-35 may be 22, 25, 28, 30, 32, etc., the 30-60 may be 35, 40, 45, 50, 55, etc., the 20-35 may be 22, 25, 28, 30, 32, etc.

[0026] In the preferred technical solution of the present invention, the first-stage polymerization monomer accounts for 20-35% of the total mass of the polymerization monomers, such as 22%, 24%, 25%, 28%, 30%, 32%, etc., the middle-stage polymerization monomer accounts for 30-60% of the total mass of the polymerization monomers, such as 35%, 40%, 45%, 50%, 55%, etc., and the second-stage polymerization monomer accounts for 20-35% of the total mass of the polymerization monomers, such as 22%, 24%, 25%, 28%, 30%, 32%, etc.

[0027] In the preferred technical solution of the present invention, the mass of the second-stage polymerized monomer is the same as the mass of the first-stage polymerized monomer.

[0028] In a preferred technical solution of the present invention, the ratio of each component in the second-stage polymerization monomer is the same as that in the first-stage polymerization monomer.

[0029] In the preferred technical solution of the present invention, the total polymerization time of the multi-stage polymerization method is 2-4h, for example, 2.2h, 2.5h, 2.8h, 3.0h, 3.2h, 3.5h, 3.8h, etc.

[0030] By adopting the production method of the present invention, the reaction time can be significantly shortened from the conventional 90 hours or more to 4 hours or less, and production efficiency can be significantly improved.

[0031] In the present invention, the polymerization pressure of the first-stage polymerization reaction and the second-stage polymerization reaction are independently selected from 2.8-3.5 MPa, for example, 2.9 MPa, 3.0 MPa, 3.1 MPa, 3.2 MPa, 3.3 MPa, 3.4 MPa, etc., and the polymerization pressure of the middle-stage polymerization reaction is 1.6-2.5 MPa, for example, 1.7 MPa, 1.8 MPa, 1.9 MPa, 2.0 MPa, 2.2 MPa, 2.4 MPa, etc.

[0032] In the present invention, the reaction temperatures of the first, middle and second polymerization reactions are independently selected from 60-95°C, for example, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, etc.

[0033] Due to the large difference in reactivity ratio during the copolymerization process between tetrafluoroethylene monomer and perfluoroalkylvinylether monomer, the present invention controls the use of different polymerization processes at different polymerization stages, so that the polymerization pressure is high in the first and second polymerization stages, and the polymerization pressure is reduced during the middle polymerization stage, so that the hardness is prevented from being too high, and the amount of perfluoroalkylvinylether, which is a flexible monomer, introduced into the polymer segment is increased, thereby increasing the flexibility of the material. Therefore, the vulcanization point monomer and tetrafluoroethylene in the perfluoroether fluororubber provided by the present invention are uniformly distributed, so that it has excellent tensile strength, and at the same time, its hardness and compression deformation are low, and it has good medium resistance and processability.

[0034] In the present invention, if the polymerization pressure of the first and second stages is low, the perfluoroalkyl vinyl ether content of both sides of the polymer increases, the fluorine content decreases, which is unfavorable to the medium resistance performance and good strength of the polymer.If the polymerization pressure of the middle stage is high, the tetrafluoro content of the middle part of the polymer increases, the rigidity of the polymer increases, and the hardness index of the polymer increases, which is unfavorable to the processing application of the polymer.

[0035] As a preferred technical solution of the present invention, the unreacted pre-stage polymerization monomer is recovered before the addition of the middle-stage polymerization monomer, and preferably the unreacted middle-stage polymerization monomer is recovered before the addition of the second-stage polymerization monomer.

[0036] A preferred technical solution of the present invention further includes recovering the unreacted post-stage polymerization monomer in the reaction product obtained in step (3) to obtain an emulsion containing a perfluoroether fluorine-containing rubber.

[0037] In the preferred technical solution of the present invention, the dispersion medium in the multi-stage polymerization process is water.

[0038] In the present invention, the system of the first-stage polymerization reaction further includes an initiator, and preferably the initiator is any one or a combination of at least two of ammonium persulfate, potassium persulfate, or potassium permanganate. Preferably, based on 100 parts by weight of the aqueous medium, the amount of the initiator used is 0.0001-8 parts by weight, for example, 0.1 parts by weight, 0.5 parts by weight, 1 part by weight, 2 parts by weight, 3 parts by weight, 4 parts by weight, 5 parts by weight, 6 parts by weight, 7 parts by weight, etc.

[0039] In the present invention, the system of the first-stage polymerization reaction further contains a perfluorooctanoate salt as an emulsifier, and preferably, based on 100 parts by weight of the aqueous medium, the amount of the emulsifier used is 0.01-5 parts by weight, for example, 1 part by weight, 2 parts by weight, 3 parts by weight, 4 parts by weight, etc.

[0040] In the present invention, the system of the first-stage polymerization reaction further comprises a chain transfer agent, which is preferably any one or a combination of at least two of 1,2-diiodoperfluoroethane, 1,3-diiodoperfluoropropane, or 1,4-diiodoperfluorobutane, and the amount of the chain transfer agent used is preferably 0.01-5%, such as 0.1%, 0.5%, 1%, 2%, 3%, 4%, etc., based on the total mass of the polymerization monomers.

[0041] The present invention provides a specific embodiment, wherein the manufacturing method includes: (1) adding deionized water to a reactor, evacuating the reactor to an oxygen content of ≦30 ppm, adding an emulsifier, and heating the reactor to 60-95° C.; (2) adding a pre-stage polymerization monomer, increasing the pressure of the reactor to 2.8-3.5 MPa, then adding an initiator and a chain transfer agent to carry out a pre-stage polymerization reaction, and recovering unreacted monomer when the amount of the pre-stage polymerization monomer added reaches 20-35% of the total mass of the polymerization monomer; (3) adding a middle-stage polymerization monomer, then reducing the pressure to 1.6-2.5 MPa to carry out a middle-stage polymerization reaction, and recovering unreacted monomer when the amount of the middle-stage polymerization monomer added reaches 30-85% of the total mass of the polymerization monomer; (4) adding a second-stage polymerization monomer, then increasing the pressure to 2.8-3.5 MPa to carry out a second-stage polymerization reaction, and when the amount of the second-stage polymerization monomer added reaches 20-35% of the total mass of the polymerization monomers, recovering the unreacted monomer to obtain an emulsion containing a perfluoroether fluorine rubber; (5) subjecting the emulsion to coagulation, washing and drying to obtain the perfluoroether fluorine-containing rubber.

[0042] The processes of flocculation, washing and drying for the emulsion of the present invention are all common processes in the art, and therefore the description thereof is omitted here.

[0043] In a second aspect, the present invention provides a perfluoroether fluoro-rubber produced by the process according to the first aspect.

[0044] The perfluoroether fluororubber obtained by the method provided by the present invention has high tensile strength, which can reach 20 MPa or more, and elongation at break, which can reach 200%, and has low hardness and compressive deformation, and has good medium resistance and processability.

[0045] In a third aspect, the present invention provides an application of the perfluoroether fluororubber according to the second aspect in petrochemical industrial materials and semiconductor materials.

[0046] Compared with the prior art, the present invention has the following beneficial effects: (1) The present invention adopts the method of multi-stage polymerization to ensure that tetrafluoroethylene and vulcanization point monomers in the segments are distributed uniformly, and the final material has low hardness and good vulcanization performance. (2) The final rubber produced by the method of the present invention has an ABA block morphology, and the rubber obtained has a specific structure, which ensures that the rubber has high tensile strength, low hardness, and good processability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0047] The technical solutions of the present invention are further described below through the embodiments for carrying out the invention. Those skilled in the art should understand that the above embodiments are merely for aiding in the understanding of the present invention, and are not intended to specifically limit the present invention.

[0048] Example 1 The perfluoroether fluorine rubber is produced by the following method. (1) 30 L of deionized water is added to a 50 L reactor, and when the oxygen content becomes ≦30 ppm after exhaust treatment, 35 g of ammonium perfluorooctanoate is added and the contents of the reactor are heated to 85°C. (2) A first-stage polymerization monomer composed of I(CF2)2OCF=CF2, TFE, and perfluoromethylvinylether in a molar ratio of 1:60:39 is added, the pressure in the reactor is increased to 3.0 MPa, 15 g of potassium persulfate and 25 g of 1,2-diiodoperfluoroethane are added to start the first-stage polymerization reaction, and when the amount of the first-stage polymerization monomer added reaches 2.5 kg, the unreacted monomer is recovered. (3) A middle-stage polymerization monomer composed of I(CF2)2OCF=CF2, TFE, and perfluoromethylvinylether in a molar ratio of 0.1:35:64.9 is introduced into the reactor, the polymerization pressure is adjusted to 2.0 MPa, and the middle-stage polymerization reaction is carried out. When the amount of the middle-stage polymerization monomer added reaches 3.3 kg, the unreacted monomer is recovered. (4) Then, a second-stage polymerization monomer composed of I(CF2)2OCF=CF2, TFE, and perfluoromethylvinylether in a molar ratio of 1:60:39 is added to the reactor, the pressure in the reactor is increased to 3.0 MPa, and when the amount of the second-stage polymerization monomer added reaches 2.5 kg, the reaction is terminated, the unreacted monomer is recovered, and an emulsion containing perfluoroether fluorine rubber is obtained. (5) The emulsion is mechanically coagulated, washed, and vacuum dried at 100°C to obtain about 7.5 kg of perfluoroether fluororubber product.

[0049] Example 2 The perfluoroether fluorine rubber is produced by the following method. (1) 30 L of deionized water is added to a 50 L reactor, and when the oxygen content becomes ≦30 ppm after exhaust treatment, 50 g of ammonium perfluorooctanoate is added and the contents of the reactor are heated to 90°C. (2) A first-stage polymerization monomer composed of I(CF2)2OCF=CF2, tetrafluoroethylene, and perfluoropropyl vinyl ether in a molar ratio of 3:67:30 is added, the pressure in the reactor is increased to 3.5 MPa, 40 g of potassium persulfate and 50 g of 1,4-diiodoperfluorobutane are added to start the first-stage polymerization reaction, and when the amount of the first-stage polymerization monomer added reaches 3.5 kg, the unreacted monomer is recovered. (3) A middle-stage polymerization monomer composed of I(CF2)2OCF=CF2, TFE, and perfluoropropyl vinyl ether in a molar ratio of 1:55:44 is introduced into the reactor, the polymerization pressure is adjusted to 2.5 MPa, and the middle-stage polymerization reaction is carried out. When the amount of the middle-stage polymerization monomer added reaches 3.0 kg, the unreacted monomer is recovered. (4) Subsequently, a second-stage polymerization monomer composed of I(CF2)2OCF=CF2, TFE, and perfluoropropyl vinyl ether in a molar ratio of 3:67:30 is added to the reactor, the pressure in the reactor is increased to 3.5 MPa, and when the amount of the second-stage polymerization monomer added reaches 3.5 kg, the reaction is terminated, the unreacted monomer is recovered, and an emulsion containing perfluoroether fluorine rubber is obtained. (5) The emulsion is mechanically coagulated, washed, and vacuum dried at 100°C to obtain a perfluoroether fluorine rubber product.

[0050] Example 3 The difference from Example 1 is that in this comparative example, the pressure of the middle-stage polymerization reaction in step (3) is 3.0 MPa.

[0051] Example 4 The difference from Example 1 is that in this comparative example, the pressure in the first-stage polymerization reaction in step (2) and the second-stage polymerization reaction in step (4) are both 2.0 MPa.

[0052] Example 5 The difference from Example 1 is that in this comparative example, the molar ratio of I(CF2)2OCF=CF2, TFE, and perfluoromethylvinylether introduced in step (3) is 0.1:50:49.9.

[0053] Comparative Example 1 The perfluoroether fluorine rubber is produced by the following method. (1) 30 L of deionized water is added to a 50 L reactor, and when the oxygen content becomes ≦30 ppm after exhaust treatment, 35 g of ammonium perfluorooctanoate is added and the contents of the reactor are heated to 85°C. (2) I(CF2)2OCF=CF2, TFE, and perfluoromethylvinylether are added in a molar ratio of 1:45:55, and the total amount of polymerization monomers added is 8.3 kg. The pressure of the reactor is increased to 3.0 MPa, and 15 g of potassium persulfate and 25 g of 1,2-diiodoperfluoroethane are added to start the polymerization reaction. When the solid content reaches about 21%, the unreacted monomers are recovered to obtain an emulsion containing perfluoroether fluorine rubber. (5) The emulsion is mechanically coagulated, washed, and vacuum dried at 100°C to obtain about 8.0 kg of a perfluoroether fluororubber product.

[0054] Performance Testing The raw rubber (perfluoroether fluorine rubber product) produced in Example 1 and Comparative Example 1 was subjected to vulcanization treatment. The vulcanization compounding components are as shown in Table 1.

[0055] [Table 1]

[0056] The raw rubber and the vulcanized samples were subjected to performance tests to test their Mooney viscosity, fluorine content, mechanical properties (tensile strength and elongation at break), hardness and compression deformation. The test results are shown in Table 2.

[0057] [Table 2]

[0058] As can be seen from the examples and performance tests, the perfluoroether fluororubber produced by the production method provided by the present invention has excellent tensile strength and elongation at break, and at the same time, has low hardness and compressive deformation, and has good processing performance.

[0059] As can be seen from the comparison between Example 1 and Example 1-2, the pressure of the multi-stage polymerization reaction of the present invention must be within the limited range of the present invention, and only in this case can the rubber have excellent tensile strength and at the same time its hardness and compression deformation are low, and the medium resistance and processability are good. As can be seen from the comparison between Example 1 and Example 3, the raw material input ratio during the middle-stage polymerization reaction must be within the limited range of the present invention. As can be seen from the comparison between Example 1 and Comparative Example 1, the perfluoroether fluororubber obtained by the multi-stage polymerization method has lower hardness and pressure deformation performance, good vulcanization performance, and good processability.

[0060] The applicant declares that the present invention has been described in the above examples for the perfluoroether fluorine rubber of the present invention and its preparation method and application, but the present invention is not limited to the above detailed methods, that is, it does not mean that the present invention cannot be carried out without relying on the above detailed methods. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of each raw material of the product of the present invention and addition of auxiliary components, selection of specific methods, etc. are all within the protection scope and disclosure scope of the present invention.

Claims

1. A method for producing a perfluoroether fluorine rubber, the perfluoroether fluorine rubber being produced by a multi-stage polymerization method, wherein the polymerization monomers in each polymerization step include tetrafluoroethylene and perfluoroalkyl vinyl ether; The polymerization monomer in each step of the polymerization reaction further comprises a vulcanization point monomer, the vulcanization point monomer being a perfluoroiodoolefin; The multi-stage polymerization method is a three-stage polymerization method, and the production method includes the steps of: (1) performing a pre-polymerization reaction on a pre-polymerization monomer composed of a vulcanization point monomer, tetrafluoroethylene, and a perfluoroalkyl vinyl ether; (2) adding again a middle-stage polymerization monomer composed of a vulcanization point monomer, tetrafluoroethylene and a perfluoroalkyl vinyl ether to carry out a middle-stage polymerization reaction; (3) adding a second stage polymerization monomer composed of a vulcanization point monomer, tetrafluoroethylene and a perfluoroalkyl vinyl ether again to carry out a polymerization reaction, and collecting the reaction product; the molar ratio of the vulcanization point monomer, tetrafluoroethylene and perfluoroalkyl vinyl ether in the pre-polymerization monomer is (1-3):(60-70):(30-40); the molar ratio of the vulcanization point monomer, tetrafluoroethylene and perfluoroalkyl vinyl ether in the middle-stage polymerization monomer is (0.1-1):(35-55):(40-65); the molar ratio of the vulcanization point monomer, tetrafluoroethylene, and perfluoroalkyl vinyl ether in the latter-stage polymerization monomer is (1-3):(60-70):(30-40); When the total mole number of the pre-stage polymerization monomers is taken as 100%, the content of the vulcanization point monomer is 1-3%, the content of the tetrafluoroethylene is 60-70%, and the content of the perfluoroalkyl vinyl ether is 30-40%, When the total mole number of the middle-stage polymerization monomers is taken as 100%, the content of the vulcanization point monomer is 0.1-1%, the content of the tetrafluoroethylene is 35-55%, and the content of the perfluoroalkyl vinyl ether is 40-65%, A method for producing perfluoroether fluororubber, characterized in that, when the total molar number of the second-stage polymerization monomers is taken as 100%, the content of the vulcanization point monomer is 1-3%, the content of the tetrafluoroethylene is 60-70%, and the content of the perfluoroalkyl vinyl ether is 30-40%.

2. The method according to claim 1, wherein the mass ratio of the first-stage polymerization monomer, the middle-stage polymerization monomer and the second-stage polymerization monomer is (20-35):(30-60):(20-35).

3. The manufacturing method described in claim 1, characterized in that the first stage polymerization monomer accounts for 20-35% of the total mass of the polymerization monomers, the middle stage polymerization monomer accounts for 30-60% of the total mass of the polymerization monomers, and the second stage polymerization monomer accounts for 20-35% of the total mass of the polymerization monomers.

4. The method according to claim 2 , wherein the mass of the second-stage polymerized monomer is the same as the mass of the first-stage polymerized monomer.

5. The manufacturing method described in claim 2, characterized in that the ratio of each component in the second-stage polymerization monomer is the same as the ratio of each component in the first-stage polymerization monomer.

6. The total polymerization time of the multi-stage polymerization method is 2-4 h; and / or the polymerization pressure of the first-stage polymerization reaction and the second-stage polymerization reaction are each independently selected from 2.8-3.5 MPa, and the polymerization pressure of the middle-stage polymerization reaction is 1.6-2.5 MPa; and / or the reaction temperatures of the first polymerization reaction, the middle polymerization reaction and the second polymerization reaction are each independently selected from 60° C. to 95° C.; and / or recovering unreacted first-stage polymerization monomer before adding the middle-stage polymerization monomer; And / or, the method according to any one of claims 1 to 5, further comprising recovering unreacted second-stage polymerization monomer in the reaction product obtained in step (3) to obtain an emulsion containing a perfluoroether fluorine-containing rubber.

7. A method for producing a polymerizable composition according to any one of claims 1 to 5, characterized in that unreacted middle-stage polymerization monomer is recovered before adding the second-stage polymerization monomer.

8. The dispersion medium in the multi-stage polymerization method is water, And / or the system of the pre-stage polymerization reaction further contains an initiator, and / or the system of the first-stage polymerization reaction further contains a perfluorooctanoate as an emulsifier; And / or, the system of the first-stage polymerization reaction further contains a chain transfer agent.

9. The manufacturing method described in claim 8, characterized in that the initiator is any one or a combination of at least two of ammonium persulfate, potassium persulfate, or potassium permanganate.

10. The method according to claim 8, wherein the amount of the initiator used is 0.0001-8 parts by weight based on 100 parts by weight of the aqueous medium.

11. The method according to claim 8, wherein the amount of the emulsifier used is 0.01 to 5 parts by weight based on 100 parts by weight of the aqueous medium.

12. The method of claim 8, characterized in that the chain transfer agent is any one or a combination of at least two of 1,2-diiodoperfluoroethane, 1,3-diiodoperfluoropropane, and 1,4-diiodoperfluorobutane.

13. The method of claim 8, wherein the amount of the chain transfer agent used is 0.01-5% based on the total mass of the polymerized monomers.

14. The manufacturing method includes: (1) adding deionized water to a reactor, evacuating the reactor to an oxygen content of ≦30 ppm, then adding an emulsifier and heating the reactor to 60-95° C.; (2) adding a pre-stage polymerization monomer, increasing the pressure of the reactor to 2.8-3.5 MPa, then adding an initiator and a chain transfer agent to carry out a pre-stage polymerization reaction, and recovering unreacted monomer when the amount of the pre-stage polymerization monomer added reaches 20-35% of the total mass of the polymerization monomer; (3) adding a middle-stage polymerization monomer, then reducing the pressure to 1.6-2.5 MPa to carry out a middle-stage polymerization reaction, and recovering unreacted monomer when the amount of the middle-stage polymerization monomer added reaches 30-85% of the total mass of the polymerization monomers; (4) adding a second-stage polymerization monomer, then increasing the pressure to 2.8-3.5 MPa to carry out a second-stage polymerization reaction, and when the amount of the second-stage polymerization monomer added reaches 20-35% of the total mass of the polymerization monomers, recovering unreacted monomers to obtain an emulsion containing a perfluoroether fluorine-containing rubber; The method according to claim 1, further comprising the step of: (5) subjecting the emulsion to coagulation, washing, and drying to obtain the perfluoroether fluorine-containing rubber.

15. A perfluoroether fluororubber produced by the method according to any one of claims 1 to 14.

16. A method for using the perfluoroether fluorine-containing rubber according to claim 15 in a petrochemical industrial material, an automobile industrial material, a semiconductor material, an aerospace material, or an instrument material.

Citation Information

Patent Citations

  • Fluoroelastomer capable of being vulcanized by peroxide and preparation method thereof

    CN110818825A

  • Process for producing fluoroelastomers with bromine or iodine atom cure sites

    JP2009513795A

  • Methods of making fluoropolymers using polyiodides, compositions and articles thereof

    JP2016501311A

  • Highly fluorinated elastomer

    JP2016540088A

  • Process for the manufacture of fluoroelastomers having bromine or lodine atom cure sites