Processing aid and resin composition

A resin composition with high and low molecular weight polymers with specific glass transition temperatures addresses melt tension and flowability issues, enhancing molding processability and blocking resistance.

JP7581764B2Active Publication Date: 2024-11-13MITSUBISHI CHEM CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020174963
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-10-17
Filing Date
2020-10-16
Publication Date
2024-11-13
Estimated Expiration
2040-10-16

AI Technical Summary

Technical Problem

Existing methods to increase melt tension in resin compositions for improved molding face challenges such as increased melt viscosity and reduced processability, particularly with resins like vinyl chloride, leading to issues like uneven tension, stagnation, and blocking during processing.

Method used

A resin composition containing a high molecular weight polymer A with a low glass transition temperature and a lower molecular weight polymer B with a high glass transition temperature, in a specific ratio, to uniformly improve melt tension and powder flowability, enhancing molding processability and blocking resistance.

Benefits of technology

The composition achieves excellent melt tension, short gelation time, good processability, and improved powder flowability, resulting in homogeneous molded products with high expansion ratios and reduced blocking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581764000001
    Figure 0007581764000001
Patent Text Reader

Abstract

To provide a processing aid that improves homogeneously the molten tension of a resin composition, to improve the moldability or improve the powder flowability of the processing aid, thereby achieving excellent blocking resistance.SOLUTION: A processing aid has a polymer A with a weight average molecular weight of 2000,000 or more and with a glass transition temperature of 50°C or lower and a polymer B with a weight average molecular weight of 1500,000 or less and with a glass transition temperature of 70°C or higher. The content of the polymer A is higher than the content of the polymer B.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a processing aid that improves processability during resin molding, and a resin composition containing the same. [Background technology]

[0002] The melt tension of a resin during molding is a key factor in making the molding process successful. For example, high melt tension fixes the structure of foam cells in foam molding, resulting in homogeneous molded products with high expansion ratios. In profile extrusion, it becomes easier to pull the molten resin through a die or sizing, leading to improved productivity. In this way, increasing the melt tension of a resin provides many advantages in molding.

[0003] A method of using a matrix resin with a high molecular weight is known as a method of increasing the melt tension of a resin composition. However, when the molecular weight of the matrix resin is increased, the melt viscosity increases along with the melt tension, and processing may become difficult using a general molding device. In addition, for resins that take a long time to melt, such as vinyl chloride resins, increasing the molecular weight will further slow down the melting, significantly impairing processability.

[0004] In order to solve the above problems, a method of adding a high molecular weight processing aid to a resin composition is widely known (Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Special Publication No. 2019-502804 [Patent Document 2] U.S. Patent No. 3,833,686 Summary of the Invention [Problem to be solved by the invention]

[0006] Patent Document 1 discloses a method for lowering the glass transition temperature of a processing aid to improve dispersibility in resin and melt tension during processing. However, since powder particles of a processing aid with a low glass transition temperature tend to fuse easily, the powder flowability of the processing aid is low, and retention and blocking of the processing aid occur during the resin molding process, which is a factor in reducing the productivity of resin molded products.

[0007] Patent Document 2 discloses that by covering a polymer with a low glass transition temperature with a polymer with a high glass transition temperature, it is possible to prevent powder fusion and improve the powder flowability of the processing aid. However, since a polymer with a high glass transition temperature has low dispersibility in resin, the tension of the molten resin becomes uneven, adversely affecting uniform processing, and sufficient performance is not obtained as a processing aid.

[0008] The present invention is devised to solve the above-mentioned problems, and has an object to provide a processing aid that can uniformly improve the melt tension of a resin composition to improve molding processability, and can improve the powder fluidity of the processing aid to achieve excellent blocking resistance. [Means for solving the problem]

[0009] The present invention has the following aspects. [1] A processing aid comprising: a polymer A having a weight-average molecular weight of 2 million or more and a glass transition temperature of 50°C or less; and a polymer B having a weight-average molecular weight of 1.5 million or less and a glass transition temperature of 70°C or more, wherein the processing aid contains more polymer A than polymer B. [2] The processing aid according to [1], wherein the polymer A contains, as a structural unit thereof, one or more units of alkyl (meth)acrylate having an alkyl group having two or more carbon atoms. [3] The processing aid according to [1] or [2], wherein the polymer B contains, as a constituent unit thereof, one or more units selected from the group consisting of methyl (meth)acrylate, a copolymer of aromatic vinyl and vinyl nitrile, and a vinyl halide. [4] The processing aid according to any one of [1] to [3], wherein the proportion of polymer A is 55% by mass or more and 99% by mass or less, and the proportion of polymer B is 1% by mass or more and 45% by mass or less, relative to 100% by mass of the total mass of polymer A and polymer B. [5] The processing aid according to any one of [1] to [4], wherein the proportion of one or more alkyl (meth)acrylate units having an alkyl group having two or more carbon atoms relative to all structural units constituting the polymer A is from 20% by mass to 100% by mass, and the total proportion of methyl (meth)acrylate, a copolymer of aromatic vinyl and vinyl nitrile, and a vinyl halide unit is from 0% by mass to 80% by mass. [6] The processing aid according to any one of [1] to [5], wherein the proportion of one or more alkyl (meth)acrylate units having an alkyl group having two or more carbon atoms relative to all structural units constituting the polymer B is from 0% by mass to 45% by mass, and the total proportion of methyl (meth)acrylate, a copolymer of aromatic vinyl and vinyl nitrile, and a vinyl halide unit is from 55% by mass to 100% by mass. [7] The processing aid according to any one of [1] to [6], wherein a ratio of methyl methacrylate units to all structural units of the polymer A is from 1% by mass to 80% by mass. [8] The processing aid according to any one of [1] to [7], wherein a ratio of methyl methacrylate units to all structural units of the polymer B is 65% by mass or more and 100% by mass or less. [9] A resin composition comprising: a polymer A having a weight-average molecular weight of 2 million or more and a glass transition temperature of 50° C. or less; a polymer B having a weight-average molecular weight of 1.5 million or less and a glass transition temperature of 70° C. or more; and a matrix resin, wherein the polymer A is contained in a larger amount than the polymer B.

[10] The resin composition according to [9], wherein the total ratio of the polymer A and the polymer B per 100 parts by mass of the matrix resin is 0.1 parts by mass or more and 30 parts by mass or less.

[11] The resin composition according to [9] or

[10] , wherein the matrix resin is a vinyl chloride resin. Effect of the Invention

[0010] According to the present invention, it is possible to provide a processing aid that can uniformly improve the melt tension of a resin composition, thereby improving molding processability, and that can improve the powder fluidity of the processing aid, thereby achieving excellent blocking resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The following definitions of terms apply throughout the specification and claims. "(Meth)acrylate" means "acrylate" or "methacrylate".

[0012] The present invention will be described in detail below. <Processing aids> The processing aid of the present invention contains polymer A and polymer B, and may further contain a third component. Specifically, the processing aid contains at least polymer A having a weight-average molecular weight of 2 million or more and a glass transition temperature of 50° C. or less, and polymer B having a weight-average molecular weight of 1.5 million or less and a glass transition temperature of 70° C. or more, and further contains more polymer A than polymer B. Although the mechanism is not clear, when the resin composition contains the processing aid, the melt tension of the resin composition is uniformly improved, and the molding processability and the powder flowability of the processing aid are improved, thereby realizing excellent blocking resistance.

[0013] The ratio of polymer A to polymer B contained in the processing aid of the present invention is not particularly limited as long as, as described above, there is more polymer A than polymer B, that is, the proportion of polymer A relative to the total mass of polymer A and polymer B (100% by mass) is greater than 50% by mass. However, from the viewpoint of obtaining good processability and powder handleability, it is preferable that, with the total mass of polymer A and polymer B being 100% by mass, polymer A is 55% by mass or more and 99% by mass or less, and polymer B is 1% by mass or more and 45% by mass or less, more preferably polymer A is 70% by mass or more and 99% by mass or less, and polymer B is 1% by mass or more and 30% by mass or less, and particularly preferably polymer A is 75% by mass or more and 95% by mass or less, and polymer B is 5% by mass or more and 25% by mass or less.

[0014] From the viewpoint of obtaining good processability, the weight average molecular weight of the processing aid of the present invention is preferably 2 million or more, more preferably 3 million or more, and particularly preferably 4 million or more.

[0015] <Polymer A> The weight-average molecular weight of the polymer A of the present invention can be adjusted by changing the radical polymerization initiator, polymerization temperature, and polymerization time, and from the viewpoint of obtaining good processability, the lower limit is preferably 2 million or more, more preferably 3 million or more, particularly preferably 4 million or more, and most preferably 4.5 million or more, while the upper limit is preferably 10 million or less, more preferably 8 million or less, and particularly preferably 6 million or less. That is, it is preferable to select the upper and lower limits of the weight-average molecular weight of the polymer A within the above-mentioned range, and among them, it is preferably 4 million or more and 10 million or less, particularly preferably 4.5 million or more and 10 million or less, and most preferably 4.5 million or more and 8 million or less.

[0016] The glass transition temperature of the polymer A of the present invention can be adjusted by changing the monomer charge, and from the viewpoint of obtaining good processability, it is preferably 50°C or lower, more preferably 0°C or higher and 45°C or lower, and particularly preferably 15°C or higher and 40°C or lower.

[0017] The structural units of polymer A of the present invention preferably contain alkyl (meth)acrylate units having an alkyl group with 2 or more carbon atoms, and more preferably contain alkyl acrylate units having an alkyl group with 2 or more carbon atoms.

[0018] Examples of alkyl (meth)acrylates having an alkyl group having 2 or more carbon atoms include linear alkyl (meth)acrylates such as ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, and hexyl (meth)acrylate; branched alkyl (meth)acrylates such as isopropyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, isopentyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate; and cyclic alkyl (meth)acrylates such as cyclopropyl (meth)acrylate, cyclobutyl (meth)acrylate, cyclopentyl (meth)acrylate, and cyclohexyl (meth)acrylate. These may be used alone or in combination of two or more.

[0019] Among these, the number of carbon atoms in the alkyl (meth)acrylate having an alkyl group having 2 or more carbon atoms is preferably 2 to 14, and more preferably 2 to 10, in terms of obtaining good processability.

[0020] The ratio of alkyl (meth)acrylate units having an alkyl group having 2 or more carbon atoms to all structural units constituting polymer A is not particularly limited, but from the viewpoint of obtaining good processability, it is preferably from 20% by mass to 100% by mass, more preferably from 25% by mass to 90% by mass, and particularly preferably from 30% by mass to 80% by mass.

[0021] The structural units of the polymer A of the present invention may further include one or more units selected from the group consisting of methyl (meth)acrylate, a copolymer of aromatic vinyl and vinyl nitrile, and a vinyl halide. The ratio of these structural units to all structural units constituting the polymer A is not particularly limited, but from the viewpoint of obtaining good processability, it is preferably 0% by mass or more and 80% by mass or less, more preferably 10% by mass or more and 75% by mass or less, and particularly preferably 20% by mass or more and 70% by mass or less.

[0022] Examples of aromatic vinyls include styrene and α-methylstyrene, examples of vinyl nitriles include acrylonitrile and methacrylonitrile, and examples of vinyl halides include vinyl chloride.

[0023] When the polymer A contains methyl methacrylate units as a structural unit, the ratio of the methyl methacrylate units to all structural units constituting the polymer A is not particularly limited, but from the viewpoint of obtaining good processability, it is preferably 1% by mass or more and 80% by mass or less, more preferably 50% by mass or more and 75% by mass or less, and even more preferably 50% by mass or more and 70% by mass or less. In this case, the ratio of the alkyl (meth)acrylate units having an alkyl group having 2 or more carbon atoms to all structural units constituting the polymer A is preferably 20% by mass or more and 99% by mass or less, more preferably 25% by mass or more and 50% by mass or less, and even more preferably 30% by mass or more and 50% by mass or less.

[0024] As the polymer A, one type of polymer may be used, or two or more types of polymers may be used.

[0025] <Polymer B> The mass average molecular weight of polymer B of the present invention can be adjusted by changing the radical polymerization initiator, the polymerization temperature, and the polymerization time. From the viewpoint of obtaining good processability, the mass average molecular weight is preferably 1,500,000 or less, more preferably 1,000,000 or less, and particularly preferably 500,000 or less, while the mass average molecular weight is preferably 50,000 or more, more preferably 100,000 or more, and particularly preferably 120,000 or more.

[0026] The glass transition temperature of the polymer B can be adjusted by changing the amount of monomer charged, and is preferably 70° C. or higher, more preferably 80° C. or higher, and particularly preferably 90° C. or higher.

[0027] The structural units of polymer B may contain one or more types of alkyl (meth)acrylate units having an alkyl group having two or more carbon atoms.

[0028] Examples of alkyl (meth)acrylates having an alkyl group having 2 or more carbon atoms include linear alkyl (meth)acrylates such as ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, and hexyl (meth)acrylate; branched alkyl (meth)acrylates such as isopropyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, isopentyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate; and cyclic alkyl (meth)acrylates such as cyclopropyl (meth)acrylate, cyclobutyl (meth)acrylate, cyclopentyl (meth)acrylate, and cyclohexyl (meth)acrylate. These may be used alone or in combination of two or more.

[0029] Among these, the alkyl (meth)acrylate preferably has 2 to 14 carbon atoms, and more preferably has 2 to 10 carbon atoms, from the viewpoint of obtaining good processability.

[0030] The ratio of alkyl (meth)acrylate units having an alkyl group with 2 or more carbon atoms to all structural units constituting polymer B is not particularly limited, but from the viewpoint of obtaining good powder handleability, it is preferably from 0 to 45% by mass, more preferably from 0 to 20% by mass, and particularly preferably from 1 to 20% by mass.

[0031] The polymer B preferably contains at least one unit selected from the group consisting of methyl (meth)acrylate, a copolymer of aromatic vinyl and vinyl nitrile, and a vinyl halide as a structural unit. The ratio of these structural units to all structural units constituting the polymer B is not particularly limited, but from the viewpoint of obtaining good powder handling properties, it is preferably from 55% by mass to 100% by mass, more preferably from 80% by mass to 100% by mass, and can be set to from 80% by mass to 95% by mass.

[0032] Examples of aromatic vinyls include styrene and α-methylstyrene, examples of vinyl nitriles include acrylonitrile and methacrylonitrile, and examples of vinyl halides include vinyl chloride. Note that, since homopolymers of aromatic vinyls and vinyl nitriles are not compatible with PVC resins, etc., when used as a constituent component of polymer B, it is necessary to make them into copolymers of aromatic vinyls and vinyl nitrile.

[0033] When methyl methacrylate units are contained as structural units of polymer B, the ratio of methyl methacrylate units to all structural units constituting polymer B is preferably 65% ​​by mass or more and 100% by mass or less, more preferably 80% by mass or more and 100% by mass or less, and can be set to 80% by mass or more and 95% by mass or less, from the viewpoint of obtaining good processability and powder handling properties. In this case, the ratio of alkyl (meth)acrylate units having an alkyl group having 2 or more carbon atoms to all structural units constituting polymer B can be set in the range of 0% by mass or more and 35% by mass or less.

[0034] As the polymer B, one type of polymer may be used, or two or more types of polymers may be used.

[0035] As described above, the processing aid may contain a third component. The third component is not particularly limited, but may be any of known silica, talc, calcium carbonate, hydrotalcite, zeolite, etc. The proportion of the third component relative to the total mass of the processing aid is not particularly limited, but is preferably 0% by mass or more and 3% by mass or less.

[0036] <Method of manufacturing processing aids> The polymerization method for obtaining the processing aid of the present invention is not particularly limited and may be, for example, an emulsion polymerization method, a soap-free polymerization method, a mini-emulsion polymerization method, a suspension polymerization method, etc., but from the viewpoint of ease of structure control, an emulsion polymerization method and a soap-free polymerization method are preferred.

[0037] The polymerization initiator used in the production of the processing aid may be a water-soluble or oil-soluble single-system or redox-system polymerization initiator. Specifically, an inorganic polymerization initiator such as a normal persulfate may be used alone, or an inorganic polymerization initiator may be used in combination with a sulfite, hydrogen sulfite, thiosulfate, or the like as a redox-system initiator. Furthermore, organic peroxides such as t-butyl hydroperoxide, cumene hydroperoxide, benzoyl peroxide, lauroyl peroxide, and the like, azo compounds, or the like may be used alone, or these may be used in combination with sodium formaldehyde sulfoxylate, or the like as a redox-system initiator, but the present invention is not limited to these specific examples.

[0038] For example, when the processing aid is produced by emulsion polymerization, the emulsifier used in the emulsion polymerization may be anionic surfactants such as alkyl sulfonates, alkyl benzene sulfonates, alkyl phosphates, dialkyl sulfosuccinates, etc.; nonionic surfactants such as polyoxyethylene alkyl ethers, polyoxyethylene fatty acid esters, sorbitan acid fatty esters, glycerin fatty acid esters, etc.; cationic surfactants such as alkylamine salts, etc., but is not particularly limited thereto. Sulfonic acid-based anionic surfactants are preferred, and alkyl diphenyl ether disulfonates are more preferred. These emulsifiers may be used alone or in combination of two or more kinds.

[0039] The method for recovering the processing aid in powder form is not particularly limited, but for example, when the processing aid is produced by emulsion polymerization, the resulting copolymer latex is cooled, and then the copolymer is precipitated by acid coagulation or salting out with an acid such as sulfuric acid or hydrochloric acid, or an electrolyte such as a salt such as aluminum chloride, calcium chloride, magnesium sulfate, aluminum sulfate, calcium acetate, etc., and then the processing aid is obtained by filtering, washing, and drying. The processing aid can also be recovered in powder form by various methods such as spray drying and freeze drying.

[0040] The powder of the processing aid may be a powder of a copolymer latex produced in one pot, a powder of a blend of different latexes produced separately, or a blend of different polymers powdered separately.

[0041] The processing aid preferably has suitable blocking resistance, gelling properties and melt tension. Specifically, in order to improve the melt tension of the resin composition uniformly to improve molding processability, or to improve the powder fluidity of the processing aid to realize excellent blocking resistance, it is preferable that the blocking resistance is "good" in the evaluation and measurement method in the examples described later, the gelling property value is 700 sec or less, and the melt tension is 0.22 N or more at the same time.

[0042] <Resin composition> The resin composition contains at least a matrix resin and a processing aid. That is, the resin composition contains at least a matrix resin, a polymer A, and a polymer B, and contains more of the polymer A than the polymer B. The matrix resin may be a thermosetting resin or a thermoplastic resin, and is not particularly limited, but is preferably a thermoplastic resin, more preferably a vinyl halide resin, and particularly preferably a vinyl chloride resin.

[0043] The vinyl chloride resin is a homopolymer of a vinyl chloride monomer, or a copolymer containing units of a vinyl chloride monomer and units of one or more monomers selected from a group of monomers copolymerizable with a vinyl chloride monomer, and the content of the vinyl chloride monomer units in the copolymer is preferably 50% by mass or more and 99% by mass or less.

[0044] In the resin composition, the total proportion of polymer A and polymer B relative to 100 parts by mass of the matrix resin is not particularly limited, but in order to improve the melt tension, it is preferably 0.1 part by mass or more, more preferably 0.5 parts by mass or more, and particularly preferably 1 part by mass or more, while in order to improve processability, it is preferably 30 parts by mass or less, more preferably 15 parts by mass or less, even more preferably 10 parts by mass or less, and particularly preferably 8 parts by mass or less.

[0045] The resin composition of the present invention may contain other components, such as an impact modifier, a stabilizer, a lubricant, a plasticizer, a colorant, a filler, a foaming agent, etc., if necessary.

[0046] In the resin composition, the ratio of other components to 100 parts by mass of the matrix resin is not particularly limited, but is preferably 0.1% by mass or more, and more preferably 1% by mass or more, while in order not to impair the properties of the matrix resin, it is preferably 80% by mass or less, and more preferably 50% by mass or less.

[0047] The resin composition can be prepared by mixing various components and kneading them using a kneading machine such as a Banbury mixer, a kneader, a roll, a ribbon blender, a Henschel mixer, etc., at a temperature of, for example, 100° C. or higher and 250° C. or lower. The kneaded resin composition can then be molded into an appropriate shape by extrusion molding, blow molding, injection molding, calendar molding, vacuum molding, etc.

[0048] <Glass transition temperature> "Glass transition temperature" (Tg) refers to the temperature at which a glassy polymer begins (or stops) localized motion of polymer chains. The glass transition temperature of a copolymer can be estimated by the Fox equation (Bulletin of the American Physical Society, 1(3) Page 123 (1956)) as follows: 1 / Tg=w1 / Tg(1)+w2 / Tg(2) For copolymers, w1 and w2 refer to the weight fractions of the two comonomers, and Tg(1) and Tg(2) refer to the glass transition temperatures of the two corresponding homopolymers made from the monomers. For polymers containing three or more monomers, additional terms are added (wn / Tg(n)). The glass transition temperatures of homopolymers can be found, for example, in "Polymer Handbook," edited by J. Brandrup and EH Immergut, Interscience Publishers. EXAMPLES

[0049] <Analysis of processing aids> Processing aids can be separated by Gradient Polymer Elution Chromatography (GPEC) under the conditions shown below, and the copolymer composition and weight average molecular weight can be measured. [GPEC conditions] Apparatus: Agilent Technologies Infinity 1260 Detector: Thermo Fisher Scientific Corona VeoRS Column: TSKgel ODS-100V (4.6 x 150 mm, 5 μm) Column temperature: 40℃ Mobile phase: ATN / THF=100 / 0→0 / 100(10min)→0 / 100(15min) Flow rate: 1.0ml / min Concentration: 1000ppm (THF BHT included) Injection volume: 1μl

[0050] <Method for measuring copolymer composition> The copolymer composition of the polymer was determined by pyrolysis gas chromatography-mass spectrometry (PY-GC / MS) and nuclear magnetic resonance ( 1 Identification by H-NMR. [PY-GC / MS conditions] Measuring device: GC-7890A, MSD-5975C, EGA / PY-2020D Measurement conditions: PY / IF 600℃ / 320℃ Column: UA-5 (30 m, 0.25 mm, 0.25 μm) Carrier gas: Helium (1mL / min) Detector: MAD(EI) Oven temperature: 40℃ (2 min) → 20℃ / min heating → 320℃ (5 min) Inlet temperature: 320℃ Transfer temperature: 320℃ Mass spectrum range: 20~1000 Split ratio: 50 / 1

[0051] [ 1 H-NMR conditions] Equipment: JNM EX-270 manufactured by JEOL Ltd. Solvent: deuterated chloroform (7.26 ppm) Concentration: 20mg / 65ml Temperature: 23℃ Total: 64 times

[0052] <Weight average molecular weight measurement method> The weight average molecular weight of the polymer is identified by gel permeation chromatography (GPC) under the following conditions. [GPC conditions] Equipment: Tosoh HLC-8320 Separation columns: TSK-guardcolumn HHR(30) (7.5 mmφ×75 mm) and TSK-GEL GMHHR-H(20) (20 μm, 7.8 mmφ×300 mm) are connected in series. Column temperature: 40℃ Eluent: THF (contains stabilizer) Concentration: 10mg / 10ml Flow rate: 0.600ml / min Injection volume: 10μl Detector: RI (differential refractometer) Calibration curve: Monodisperse polystyrene Internal standard: Antage W400

[0053] <Method for evaluating blocking resistance of processing aids> 20g of the processing aid is weighed out and placed in a cylindrical mold with a diameter of 65mm. A 5kg weight is placed on top of the mold and heated at 60℃ for 2 hours. After heating, a test piece of the processing aid that has solidified into a cylindrical shape is removed and placed on a 12 mesh sieve, and vibration is applied for 10 minutes using dial 10 on a micro-type electromagnetic vibration sieve shaker (Tsutsui Rikagaku Kikai, M-2). The mass of the test piece remaining on the sieve after the test is measured, and the mass reduction rate relative to the original test piece is calculated. A mass reduction rate of 20% is used as the standard, and samples with a reduction rate of 20% or more are evaluated as having good blocking resistance and marked with "○", while samples with a reduction rate of less than 20% are evaluated as having poor blocking resistance and marked with "×".

[0054] <Method for evaluating gelling properties of resin composition> 60 g of the vinyl chloride resin composition was filled into a Plasticorder (manufactured by Brabender) heated to 160°C, and after holding for 3 minutes, the gelling characteristics were observed at a temperature of 160°C and a rotation speed of 30 rpm. The time required for the torque to exceed 30 N·m after the start of kneading was recorded as the gelling time. The shorter the gelling time, the more homogeneously the processing aid is dispersed and the better the processability. For example, in order to obtain a molded product with a homogeneous appearance by foam extrusion molding, the gelling time is preferably 700 sec or less, more preferably 680 sec or less, and even more preferably 675 sec or less.

[0055] <Method for evaluating melt tension of resin composition> 250 g of the vinyl chloride resin composition is kneaded for 3 minutes with a heated roll with a diameter of 8 inches heated to 185 ° C. to prepare a roll sheet, and the roll sheet is cut into a strip (5 mm × 80 mm × 0.5 mmt) to prepare a test piece. The test piece is placed in a twin capillary rheometer (manufactured by ROSAND, RH-7) set at 195 ° C., preheated for 5 minutes, extruded at a piston speed of 8.89 mm / min, and wound up at 6 m / min while measuring the melt tension. If the melt tension is high, the structure of the foam cells is fixed in the foam molding, and a homogeneous molded product with a high expansion ratio is obtained, but in order to obtain a molded product with a good expansion ratio, the melt tension is preferably 0.22 N or more, more preferably 0.24 N or more, and even more preferably 0.26 N or more.

[0056] (Production Example 1) (Production of resin composition) 100 parts by mass of a vinyl chloride resin having an average degree of polymerization of 1000 (manufactured by Shin-Etsu Chemical Co., Ltd., "TK-1000"), 4 parts by mass of a Ca-Zn-based stabilizer (manufactured by Nitto Kasei Kogyo Co., Ltd., "HT-547A"), 0.5 parts by mass of an ester-based lubricant (manufactured by Emery Oleochemicals Japan Co., Ltd., "LOXIOL VPN963") as a lubricant, 0.5 parts by mass of an ester-based lubricant (manufactured by Emery Oleochemicals Japan Co., Ltd., "LOXIOL G60") as a lubricant, 5 parts by mass of calcium carbonate (manufactured by Shiraishi Kogyo Co., Ltd., "μ-POWDER 3S") as a filler, and 4.5 parts by mass of titanium oxide (manufactured by Ishihara Sangyo Co., Ltd., "R-830") were mixed in a Henschel mixer and heated to 110°C to obtain a vinyl chloride resin composition.

[0057] Example 1 (Manufacturing of processing aids) A reaction vessel equipped with a stirrer and a reflux condenser was charged with 115 parts by mass of ion-exchanged water, to which 0.1 parts by mass of anhydrous sodium carbonate, 54.5 parts by mass of methyl methacrylate (MMA), and 30 parts by mass of n-butyl acrylate (BA) were added, and the atmosphere in the reaction vessel was replaced with nitrogen. Then, 1.7 parts by mass of sodium alkyl diphenyl ether disulfonate (manufactured by Kao Corporation, "Pelex SS-L") was added as an emulsifier, and the reaction vessel was heated to 50°C under stirring, and 0.13 parts by mass of potassium persulfate was added as a polymerization initiator to initiate the polymerization reaction, and the polymerization was terminated by heating and stirring for 4 hours, to obtain an emulsion containing polymer A. The obtained emulsion was heated to 80° C., and 0.04 parts by mass of potassium persulfate was added. Then, a mixed liquid of 15.5 parts by mass of methyl methacrylate (MMA) and 0.008 parts by mass of octyl mercaptan was added dropwise over 30 minutes, and the mixture was held for 1 hour after the dropwise addition to obtain an emulsion containing polymer A and polymer B. The obtained emulsion was spray-dried under the condition of hot air inlet temperature of 135°C to obtain a powder of the processing aid. The resulting processing aid was separated and the copolymer composition and weight average molecular weight (Mw) were measured. It was found to contain a polymer with Mw = 4.6 million and MMA / BA = 65% by mass / 35% by mass, and a polymer with Mw = 490,000 and MMA = 100% by mass, in a ratio of 85% by mass:15% by mass.

[0058] (Evaluation of Processing Aids and Resin Compositions) The obtained powder of the processing aid was evaluated for blocking resistance by the above-mentioned method for evaluating the blocking resistance of processing aids. In addition, 1 part by mass of the obtained processing aid was added to 114.5 parts by mass of the vinyl chloride resin composition obtained in Production Example 1 to evaluate gelling properties. Furthermore, 7 parts by mass of the obtained processing aid was added to 114.5 parts by mass of the vinyl chloride resin composition obtained in Production Example 1 to evaluate melt tension. These results are shown in Table 1.

[0059] (Examples 2 to 12, Comparative Examples 1 to 4) Except for changing the composition and molecular weight of the polymer as shown in Table 1, the processability was evaluated by measuring the gelling characteristics and melt tension, and the powder flowability was evaluated by testing the blocking resistance in the same manner as in Example 1. The results are shown in Table 1. In Table 1, "AN" stands for acrylonitrile, "St" stands for styrene, "BMA" stands for butyl methacrylate, and "k" in the weight average molecular weight (Mw) is 10 3 Shows.

[0060] [Table 1]

[0061] The results in Table 1 show that the processing aids and resin compositions obtained in each of Examples 1 to 12 had a blocking resistance of "good", a gelling characteristic value of 700 sec or less, and a melt tension of 0.22 N or more. These properties indicate that the processing aids and resin compositions obtained in each of Examples 1 to 12 have high melt tension, short gelling time, and good processability, as well as good powder fluidity and excellent blocking resistance.

Claims

1. A processing aid comprising: a polymer A having a weight-average molecular weight of 3,000,000 or more and a glass transition temperature of 50° C. or less; and a polymer B having a weight-average molecular weight of 1,500,000 or less and a glass transition temperature of 70° C. or more, wherein the polymer A is contained in a larger amount than the polymer B; As the structural unit of the polymer A, Contains at least a unit of butyl (meth)acrylate, further optionally containing one or more units selected from the group consisting of methyl (meth)acrylate units, copolymer units of aromatic vinyl and vinyl nitrile, and vinyl halide units; a ratio of butyl (meth)acrylate units to all structural units constituting the polymer A is 20% by mass or more and 100% by mass or less, and a total ratio of methyl (meth)acrylate units, units of a copolymer of aromatic vinyl and vinyl nitrile, and units of a vinyl halide is 0% by mass or more and 80% by mass or less, As the structural unit of the polymer B, The copolymer comprises at least one of a methyl methacrylate unit and a copolymer unit of an aromatic vinyl and a vinyl nitrile, and optionally further comprises one or more alkyl (meth)acrylate units having an alkyl group having two or more carbon atoms; A processing aid in which the total proportion of methyl methacrylate units and aromatic vinyl / vinyl nitrile copolymer units relative to all structural units constituting the polymer B is 55% by mass or more and 100% by mass or less, and the proportion of one or more alkyl (meth)acrylate units having an alkyl group having two or more carbon atoms is 0% by mass or more and 45% by mass or less.

2. The processing aid according to claim 1, wherein the proportion of the polymer A is 55% by mass or more and 99% by mass or less, and the proportion of the polymer B is 1% by mass or more and 45% by mass or less, relative to 100% by mass of the total mass of the polymer A and the polymer B.

3. The processing aid according to claim 1 or 2, wherein a ratio of methyl methacrylate units to all structural units of the polymer A is 1% by mass or more and 80% by mass or less.

4. A processing aid comprising: a polymer A having a weight-average molecular weight of 2,000,000 or more and a glass transition temperature of 50°C or less; and a polymer B having a weight-average molecular weight of 1,500,000 or less and a glass transition temperature of 70°C or more, wherein the polymer A is contained in a larger amount than the polymer B; As the structural unit of the polymer A, Contains butyl (meth)acrylate units and methyl methacrylate units, a ratio of butyl (meth)acrylate units to all structural units constituting the polymer A is 20% by mass or more and 99% by mass or less, and a ratio of methyl methacrylate units is 1% by mass or more and 80% by mass or less, As the structural unit of the polymer B, The copolymer comprises at least one of a methyl methacrylate unit and a copolymer unit of an aromatic vinyl and a vinyl nitrile, and optionally further comprises one or more alkyl (meth)acrylate units having an alkyl group having two or more carbon atoms; A processing aid in which the total proportion of methyl methacrylate units and aromatic vinyl / vinyl nitrile copolymer units relative to all structural units constituting the polymer B is 55% by mass or more and 100% by mass or less, and the proportion of one or more alkyl (meth)acrylate units having an alkyl group having two or more carbon atoms is 0% by mass or more and 45% by mass or less.

5. The processing aid described in claim 4, wherein the proportion of polymer A is 55% by mass or more and 99% by mass or less, and the proportion of polymer B is 1% by mass or more and 45% by mass or less, relative to the total mass of polymer A and polymer B (100% by mass).

6. The processing aid according to any one of claims 1 to 5, wherein the ratio of methyl methacrylate units to all structural units of the polymer B is 65% by mass or more and 100% by mass or less.

7. A resin composition comprising the processing aid described in any one of claims 1 to 6 and a matrix resin.

8. A resin composition comprising: a polymer A having a weight-average molecular weight of 3,000,000 or more and a glass transition temperature of 50° C. or less; a polymer B having a weight-average molecular weight of 1,500,000 or less and a glass transition temperature of 70° C. or more; and a matrix resin, the polymer A being contained in a larger amount than the polymer B, As the structural unit of the polymer A, Contains at least a unit of butyl (meth)acrylate, further optionally containing one or more units selected from the group consisting of methyl (meth)acrylate units, copolymer units of aromatic vinyl and vinyl nitrile, and vinyl halide units; a ratio of butyl (meth)acrylate units to all structural units constituting the polymer A is 20% by mass or more and 100% by mass or less, and a total ratio of methyl (meth)acrylate units, units of a copolymer of aromatic vinyl and vinyl nitrile, and units of a vinyl halide is 0% by mass or more and 80% by mass or less, As the structural unit of the polymer B, The copolymer comprises at least one of a methyl methacrylate unit and a copolymer unit of an aromatic vinyl and a vinyl nitrile, and optionally further comprises one or more alkyl (meth)acrylate units having an alkyl group having two or more carbon atoms; A resin composition, wherein the total ratio of methyl methacrylate units and aromatic vinyl / vinyl nitrile copolymer units to all structural units constituting the polymer B is 55% by mass or more and 100% by mass or less, and the ratio of one or more alkyl (meth)acrylate units having an alkyl group having 2 or more carbon atoms is 0% by mass or more and 45% by mass or less.

9. A resin composition described in claim 8, wherein the ratio of methyl methacrylate units to all structural units of polymer A is 1 mass% or more and 80 mass% or less.

10. A resin composition comprising: a polymer A having a weight-average molecular weight of 2,000,000 or more and a glass transition temperature of 50°C or less; a polymer B having a weight-average molecular weight of 1,500,000 or less and a glass transition temperature of 70°C or more; and a matrix resin, wherein the polymer A is contained in a larger amount than the polymer B, As the structural unit of the polymer A, Contains butyl (meth)acrylate units and methyl methacrylate units, a ratio of butyl (meth)acrylate units to all structural units constituting the polymer A is 20% by mass or more and 99% by mass or less, and a ratio of methyl methacrylate units is 1% by mass or more and 80% by mass or less, As the structural unit of the polymer B, The copolymer comprises at least one of a methyl methacrylate unit and a copolymer unit of an aromatic vinyl and a vinyl nitrile, and optionally further comprises one or more alkyl (meth)acrylate units having an alkyl group having two or more carbon atoms; A resin composition, wherein the total ratio of methyl methacrylate units and aromatic vinyl / vinyl nitrile copolymer units to all structural units constituting the polymer B is 55% by mass or more and 100% by mass or less, and the ratio of one or more alkyl (meth)acrylate units having an alkyl group having 2 or more carbon atoms is 0% by mass or more and 45% by mass or less.

11. A resin composition described in any one of claims 8 to 10, wherein the proportion of polymer A is 55 mass% or more and 99 mass% or less, and the proportion of polymer B is 1 mass% or more and 45 mass% or less, relative to the total mass of polymer A and polymer B (100 mass%).

12. A resin composition described in any one of claims 8 to 11, wherein the ratio of methyl methacrylate units to all structural units of polymer B is 65 mass% or more and 100 mass% or less.

13. The resin composition according to any one of claims 7 to 12, wherein the total ratio of the polymer A and the polymer B to 100 parts by mass of the matrix resin is 0.1 parts by mass or more and 30 parts by mass or less.

14. The resin composition according to any one of claims 7 to 13, wherein the matrix resin is a vinyl chloride resin.

Citation Information

Patent Citations

  • Lubricant for thermoplastic resin and thermoplastic resin composition containing the same

    JP1997221576A

  • Processing aid, vinyl, chloride-based resin composition using the same and production of molded article using the same composition

    JP2001031826A

  • Polymer composition for plastic additive

    JP2001323006A

  • Powdery resin composition being excellent in blocking resistance and in odor, and method for producing the same

    JP2009024069A

  • Polymeric composition having low glass transition temperature

    JP2011140657A