Container member and manufacturing method thereof, container cap and container body

The method enhances supercritical fluid forming by creating a dense foam layer with voids to address surface defects, achieving lightweight containers with excellent sealing and recyclable designs.

JP7581773B2Active Publication Date: 2024-11-13TOPPAN HOLDINGS INC
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020182421
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-30
Publication Date
2024-11-13
Estimated Expiration
2040-10-30

AI Technical Summary

Technical Problem

Supercritical fluid forming in container manufacturing leads to surface defects like minute sink marks and foam marks, which can cause liquid or air leakage, limiting its application in lightweight, high-sealing performance containers.

Method used

A manufacturing method involving injecting a first molten resin composition into a mold, followed by injecting a second molten resin composition with a supercritical fluid, and reducing pressure to foam the second composition, creating a dense foam layer with a foamed layer having voids, ensuring excellent sealing performance despite surface defects.

Benefits of technology

The method produces lightweight containers with excellent sealing performance and promotes recyclability by using a monomaterial design, addressing surface defects and enhancing adhesion through irregular interfaces and voids.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581773000001
    Figure 0007581773000001
  • Figure 0007581773000002
    Figure 0007581773000002
  • Figure 0007581773000003
    Figure 0007581773000003
Patent Text Reader

Abstract

To provide a method for manufacturing a member for a container which achieves reduction in the weight by foaming, and can achieve excellent sealing property.SOLUTION: A method for manufacturing a member for a container includes: a step (A) of injecting a first molten resin composition containing a resin material into a cavity of a mold; a step (B) of injecting a second molten resin composition containing a resin material and a supercritical fluid into the cavity in a state where the molded body obtained through the above step (A) is arranged in the cavity of the mold; and a step (C) of foaming the second molten resin composition in the cavity by lowering of pressure. The member for the container obtained through the above step (C) has a dense layer formed from a cured product of the first molten resin composition, and a foam layer that is formed from a cured product of the second molten resin composition and has a plurality of gaps derived from the supercritical fluid.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a container member and a manufacturing method thereof, as well as a container cap and a container body. [Background technology]

[0002] In recent years, plastic molded products are used in all kinds of daily necessities and industrial products around us. The demand for plastic molded products is increasing as their quality improves and costs go down, making them more versatile. On the other hand, attention has been focused on the impact of microplastics on the environment, as seen in the problem of marine plastic waste, and there is a growing trend to move away from plastic and to refrain from using plastic products.

[0003] Regarding disposable plastic containers for food and daily necessities, there is a growing demand from users to reduce the amount of petroleum-based plastic used. In response to such demands, efforts are being made to reduce the amount of plastic used by using plant-based resins as part of the raw materials, utilizing recycled plastic materials, and improving dimensions and shapes.

[0004] Foam molding is known as a means for reducing the weight of plastic molded products. Foam molding can be broadly divided into chemical foam molding and physical foam molding. Chemical foam molding uses a foaming agent, while physical foam molding uses a fluid in a supercritical state (hereinafter referred to as "supercritical fluid molding"). Chemical foam molding has concerns about the negative impact of the foaming agent on the environment and issues such as mold contamination. Supercritical fluid molding does not have such concerns. Supercritical fluid molding has traditionally been applied to relatively large industrial products such as automobile part molding and office equipment. In recent years, with the improvement of supercritical fluid generation technology and resin composition kneading technology, the application of supercritical fluid molding to high-cycle injection molding has been considered. Patent Documents 1 to 3 disclose food containers manufactured by supercritical fluid molding. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 6085729 [Patent Document 2] Patent No. 6430684 [Patent Document 3] JP 2020-040690 A Summary of the Invention [Problem to be solved by the invention]

[0006] In order to broaden the scope of application of supercritical fluid molding, the present inventors carried out various supercritical fluid moldings using various dies. As a result, they found that as the degree of foaming increases, defects such as minute sink marks and foaming marks (swirl marks) tend to occur on the surface of the molded body. If a container is constructed using a container member having surface defects, even if they are minute, liquid leakage or air leakage may occur depending on the type of content.

[0007] The present disclosure provides a container member and a manufacturing method thereof, which are lightweight due to foaming and capable of realizing excellent sealing properties. The present disclosure also provides a container cap and a container body, which are lightweight due to foaming and capable of realizing excellent sealing properties. [Means for solving the problem]

[0008] One aspect of the present disclosure relates to a method for producing a container member, which includes the steps of (A) injecting a first molten resin composition containing a resin material into a cavity of a mold, (B) injecting a second molten resin composition containing a resin material and a supercritical fluid into the cavity of the mold while the molded body obtained through the step (A) is placed in the cavity, and (C) foaming the second molten resin composition in the cavity by reducing the pressure, and the container member obtained through the step (C) has a dense layer made of a cured product of the first molten resin composition and a foamed layer made of a cured product of the second molten resin composition and having a plurality of voids derived from the supercritical fluid.

[0009] The container member obtained through step (C) constitutes a container together with other members. For example, when the container member is a container cap, the other members are a container body that contains the contents. When the container member is a container body with a flange portion provided on the periphery of the opening, the other members are a lid material that abuts against the flange portion.

[0010] The dense layer formed in the above step (A) has an abutment portion against other members that constitute the container together with the container member. This abutment portion is constituted by the dense layer. Therefore, even if the surface of the foamed layer formed through the step (C) has appearance defects such as sink marks or foaming marks due to foaming, excellent sealing properties can be achieved.

[0011] The dense layer is in contact with at least a part of the surface of the foam layer, and the interface between the dense layer and the foam layer preferably has irregularities. The irregularities at the interface between these layers can contribute to improving the adhesion between these layers. The interface may be intentionally provided with irregularities.

[0012] The foam layer may have a through hole penetrating in the thickness direction, and the through hole may be filled with a first resin material. By filling the through hole with the first resin material, a portion (dense layer) made of the first resin material can be partially exposed on the surface of the container member. For example, by forming the shape of the through hole in a plan view into a logo of a product, a logo or the like having a texture, gloss, or color different from that of the foam layer can be provided on the surface of the container member. In addition, the through hole in the foam layer and the first resin material filled therein can contribute to improving the adhesion between the dense layer and the foam layer.

[0013] An example of a container member according to the present disclosure is a cap for a container that contains liquid or the like. The container cap according to the present disclosure includes a top surface portion having an inner ring portion on the inner surface side, and a side surface portion extending from the peripheral portion of the top surface portion in a direction away from the top surface portion, and includes a dense layer made of a first resin material and including the inner ring portion, and a foam layer made of a second resin material and having a plurality of voids derived from a supercritical fluid. The inner ring portion is a portion that fits into the opening of the container body. Since the inner ring portion is made of a dense layer, excellent sealing performance can be achieved.

[0014] Another example of the container member according to the present disclosure is a container body that constitutes a container together with a lid. The container body according to the present disclosure includes an opening, a dense layer that constitutes a flange portion provided around the periphery of the opening and constitutes the inner surface of the container body, and a foam layer that is made of a second resin material, has a plurality of voids derived from a supercritical fluid, and constitutes the outer surface of the container body. The flange portion is a portion that the lid material abuts against. For example, the lid material is attached to the flange portion by heat sealing to ensure the sealing of the container. Since the flange portion is composed of a dense layer, excellent sealing can be achieved.

[0015] In the present disclosure, the foam layer and the dense layer are preferably made of the same type of resin material, which allows the container member, container cap, and container body to be made of a mono-material, thereby contributing to the promotion of recycling of the resin material. Effect of the Invention

[0016] According to the present disclosure, a container member and a manufacturing method thereof are provided, which are light-weighted by foaming and capable of realizing excellent sealing performance. Also, according to the present disclosure, a container cap and a container body are provided, which are light-weighted by foaming and capable of realizing excellent sealing performance. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a schematic diagram of one embodiment of a container cap according to the present disclosure. [Diagram 2] FIG. 2 is a cross-sectional view that typically illustrates the interface between a dense layer and a foam layer in the container cap illustrated in FIG. [Diagram 3] FIG. 3(a) is a plan view that shows a schematic diagram of another embodiment of a container cap according to the present disclosure, and FIG. 3(b) is a cross-sectional view taken along line bb in FIG. 3(a). [Figure 4] FIG. 4 is a cross-sectional view that illustrates a schematic diagram of one embodiment of a container body according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, an embodiment of the present disclosure will be described in detail. Here, a container cap (screw cap) will be described as an example of a container member. Note that the present invention is not limited to the following embodiment.

[0019] <Container cap and manufacturing method thereof> 1 is a cross-sectional view showing a schematic diagram of a container cap according to the present embodiment. The container cap 10 shown in this figure (hereinafter sometimes simply referred to as "cap 10") is manufactured through the following steps. (A) A step of injecting a first molten resin composition containing a resin material into a cavity of a mold. (B) A process of injecting a second molten resin composition containing a resin material and a supercritical fluid into a cavity of a mold while the molded body obtained through the process (A) is placed in the cavity. (C) foaming the second molten resin composition in the cavity by reducing the pressure. The cap 10 produced by this method includes a dense layer L1 made of a cured product of a first molten resin composition (first resin material) and a foamed layer L2 made of a cured product of a second molten resin composition (second resin material) and having a plurality of voids derived from a supercritical fluid. Note that a series of steps from (B) to (C) can be carried out, for example, using a MuCell injection molding machine ("MuCell" is a registered trademark of Trexel Co. Ltd) (see Patent Documents 1 and 2).

[0020] The cap 10 is called a screw cap. The cap 10 comprises a top surface portion 1 and a side surface portion 2 hanging down from the peripheral portion of the top surface portion 1. An inner ring portion 1a that fits into the inside of the opening of the container body is provided on the inner surface of the top surface portion 1. A screw thread 2a that corresponds to the screw thread (not shown) of the opening of the container body is provided on the inside of the side surface portion 2.

[0021] The thickness of the cap 10 is, for example, 1 to 2 mm. The thickness of the cap 10 here means the sum of the thickness of the dense layer L1 (excluding the part where the inner ring part 1a and the screw thread 2a are provided) and the thickness of the foamed layer L2. The thickness of the dense layer L1 (excluding the part where the inner ring part 1a and the screw thread 2a are provided) is, for example, 0.3 to 0.7 mm, and may be 0.4 to 0.6 mm. When the dense layer L1 has such a thickness, the strength of the cap 10 can be sufficiently ensured. The thickness of the foamed layer L2 is, for example, 0.3 to 1.7 mm, and may be 0.4 to 1.6 mm or 0.5 to 1.5 mm. When the foamed layer L2 has such a thickness, the effect of weight reduction by foaming can be sufficiently obtained. Note that, when the thickness of the cap 10 is made thicker than 2 mm, the dense layer L1 and the foamed layer L2 may be made thicker than the above upper limit value.

[0022] Fig. 2 is a cross-sectional view showing a schematic diagram of the interface between the dense layer L1 and the foam layer L2 in the cap 10. As shown in Fig. 2, the interface F between the dense layer L1 and the foam layer L2 may have irregularities. Such irregularities can be formed by intentionally providing a rib shape in the dense layer L1 or the foam layer L2, or by applying an embossing process to the surface of a mold. By increasing the surface area of ​​the interface F, the adhesion (welding strength) between the dense layer L1 and the foam layer L2 can be further improved.

[0023] The dense layer L1 and the foam layer L2 may be made of the same type of resin material or different types of resin materials. From the viewpoint of promoting recycling of the cap 10, it is preferable that the dense layer L1 and the foam layer L2 are made of the same type of resin material. That is, when the material of the dense layer L1 is PET (polyethylene terephthalate), it is preferable that the material of the foam layer L2 is also PET. When the material of the dense layer L1 is PP (polypropylene), it is preferable that the material of the foam layer L2 is also PP. When the material of the dense layer L1 is PE (polyethylene), it is preferable that the material of the foam layer L2 is also PE. Note that the color of the dense layer L1 may be different from the color of the foam layer L2 by two-color molding.

[0024] Each step of the method for manufacturing the cap 10 will now be described.

[0025] [(A) Process] A molded body is produced by injecting a first molten resin composition containing a resin material into a cavity of a mold. This molded body becomes the dense layer L1 in the cap 10. Step (A) can be carried out by normal injection molding.

[0026] [(B) Process] First, a molten resin composition containing a resin material and a supercritical fluid is prepared. Examples of the resin material include polypropylene resin and polyethylene resin. Examples of the supercritical fluid include carbon dioxide, nitrogen, argon, and helium. According to the study by the present inventors, when the supercritical fluid is carbon dioxide, the molten resin composition is prepared by adding preferably 1 to 4 parts by mass, more preferably 2 to 3 parts by mass of carbon dioxide in a supercritical state to 100 parts by mass of the resin material. When the carbon dioxide content of the molten resin composition is 1 part by mass or more, it is easy to form a sufficiently uniform foam layer over the entire top surface portion 1, and weight reduction by foaming tends to be realized. On the other hand, when the carbon dioxide content of the molten resin composition is 4 parts by mass or less, excessive foaming tends to be suppressed.

[0027] When the supercritical fluid is nitrogen, the molten resin composition is prepared by adding preferably 0.1 to 1.2 parts by mass, more preferably 0.3 to 0.7 parts by mass, of supercritical nitrogen per 100 parts by mass of the resin material. When the nitrogen content of the molten resin composition is 0.5 parts by mass or more, it is easy to form a sufficiently uniform foamed layer over the entire foamed layer L2, and weight reduction by foaming tends to be realized. On the other hand, when the nitrogen content of the molten resin composition is 1.0 part by mass or less, excessive foaming tends to be suppressed.

[0028] When the resin material used is a polypropylene resin, the temperature of the molten resin composition (screw cylinder temperature) is preferably about 210 to 230° C. When the resin material used is a polyethylene resin, this temperature is preferably about 220 to 240° C. When this temperature is equal to or higher than the lower limit, the resin easily flows in the cavity, while when the temperature is equal to or lower than the lower limit, for example, scorching of the resin tends to be suppressed.

[0029] The molten resin composition may contain components other than the resin material and the supercritical fluid. That is, the molten resin composition may further contain, for example, a filler, a colorant, an antistatic agent, an antioxidant, etc., as necessary. According to this embodiment, since the top surface portion 1 can be made white by the voids resulting from foaming, the molten resin composition may contain a white pigment of 2 mass% or less based on the mass of the molten resin composition, or may not contain a white pigment.

[0030] A foamed layer L2 is formed so as to cover a part of the surface of the molded body (dense layer L1) obtained through the above step (A). This step can be carried out by insert molding using a supercritical fluid. That is, with the molded body obtained through the above step (A) placed in the cavity of a mold, a molten resin composition is injected into the cavity through a gate of the mold.

[0031] When the molten resin composition is introduced into the cavity, the pressure is reduced, and the air bubble cells grow, so that independent air bubbles are generated in the resin composition. The injection speed is preferably 100 to 300 mm / sec, and more preferably 150 to 200 mm / sec. When the injection speed is 100 mm / sec or more, the resin can easily reach the flow end, and the occurrence of short shots tends to be suppressed. On the other hand, when the injection speed is 300 mm / sec or less, the occurrence of burr defects in the cap 10 tends to be suppressed. According to the study by the present inventors, when the resin material is a polyethylene resin and the supercritical fluid is nitrogen, it is preferable to set the injection speed in multiple stages. That is, it is more preferable to set the initial injection speed to 250 to 300 mm / sec, and to reduce the second-stage injection speed to 150 to 200 mm / sec.

[0032] In this embodiment, from the viewpoint of sufficiently promoting foaming in the cavity, it is not necessary to carry out a step of applying pressure to the cavity (pressure holding) after filling the cavity with the molten resin composition. In this embodiment, from the viewpoint of forming a sufficiently thin foam layer L2, it is preferable not to carry out a step called "core back" for reducing the pressure in the cavity. Core back is CavityBefore the molten resin filled in the mold finishes solidifying, the movable part of the mold is moved. Cavity (See Patent Document 1.) In this embodiment, as described above, foaming can be caused in the cavity by a pressure reduction that accompanies the introduction of the molten resin composition into the cavity.

[0033] When the temperature of the cap 10 drops to about 30 to 60°C, the cap 10 is removed from the mold. The foamed layer L2 having voids resulting from foaming is formed, thereby reducing the weight and the amount of plastic material used. The formation of voids preferably reduces the weight by 3% by mass or more compared to a molded body without voids (a normal injection molded body).

[0034] Although the embodiment of the present disclosure has been described above, the present invention is not limited to the above embodiment. For example, as shown in FIG. 3(a) and FIG. 3(b), the foam layer L2 may have through holes 5 penetrating in the thickness direction, and the through holes 5 may be filled with the first resin material constituting the dense layer L1. By filling the through holes 5 with the first resin material, the portion made of the first resin material (the dense layer L1) can be partially exposed on the surface of the container cap 20. As shown in FIG. 3(a), by forming the shape of the through holes 5a, 5b, and 5c in a plan view into a logo of the product ("ABC" in FIG. 3(a) indicates a logo), a logo having a texture, glossiness, or color different from that of the foam layer L2 can be provided on the surface of the container cap 20. In addition, the through holes 5 in the foam layer L2 and the first resin material filled therein may contribute to improving the adhesion between the dense layer L1 and the foam layer L2. As shown in FIGS. 3(a) and 3(b), from the standpoint of design, a logo (ABC) may be displayed on the surface of a recess 1b provided in the center of the top surface 1.

[0035] In the above embodiment, a container cap is given as an example of a container member, but the present invention is not limited thereto. For example, packaging containers such as stoppered caps, trays, and cups may be manufactured by the manufacturing method according to the above embodiment. The contents of the packaging container may be food or non-food. FIG. 4 is a cross-sectional view showing a cup (container body) that constitutes a container together with a lid material. The cup 30 shown in this figure is composed of a dense layer L1 and a foam layer L2. The dense layer L1 constitutes the flange portion 12 provided on the periphery of the opening 11 and also constitutes the inner surface of the cup 30. The foam layer L2 constitutes the outer surface of the cup 30. The flange portion 12 is an abutment portion against the lid material 15. Since the flange portion 12 is composed of the dense layer L1, excellent sealing performance can be achieved. The container composed of the cup 30 and the lid material 15 is sold in a state in which pudding, jelly, etc. are contained.

[0036] The thickness of the cup 30 is, for example, 1 to 2 mm. The thickness of the cup 30 here means the sum of the thickness of the dense layer L1 (excluding the flange portion 12) and the thickness of the foamed layer L2. The thickness of the dense layer L1 (excluding the flange portion 12) is, for example, 0.3 to 0.7 mm, and may be 0.4 to 0.6 mm. When the dense layer L1 has such a thickness, the strength of the cup 30 can be sufficiently ensured. The thickness of the foamed layer L2 is, for example, 0.3 to 1.7 mm, and may be 0.4 to 1.6 mm or 0.5 to 1.5 mm. When the foamed layer L2 has such a thickness, the effect of weight reduction by foaming can be sufficiently obtained. When the thickness of the cup 30 is made thicker than 2 mm, the dense layer L1 and the foamed layer L2 may be made thicker than the above upper limit value, and when the thickness of the cup 30 is made thinner than 1 mm, the dense layer L1 and the foamed layer L2 may be made thinner than the above lower limit value.

[0037] In the above embodiment, the container cap has a two-layer structure of the dense layer L1 and the foamed layer L2 as a whole, but for example, only the inner ring portion 1a and its periphery may have a two-layer structure of the dense layer L1 and the foamed layer L2. The other portions may be foamed resin bodies having a plurality of voids derived from the supercritical fluid, and further weight reduction effects can be obtained. [Explanation of symbols]

[0038] 1...top surface portion, 1a...inner ring portion, 1b...recess, 2...side portion, 2a...screw thread, 5a, 5b, 5c...through hole, 10, 20...container cap (container member), 11...opening, 12...flange portion, 15...lid material, 30...cup (container body, container member), F...interface, L1...dense layer, L2...foam layer.

Claims

1. (A) injecting a first molten resin composition containing a resin material into a cavity of a mold; (B) a step of injecting a second molten resin composition containing a resin material and a supercritical fluid into a cavity of a mold while the molded body obtained through the step (A) is placed in the cavity; (C) foaming the second molten resin composition in the cavity by a reduction in pressure caused by the introduction of the second molten resin composition into the cavity, and maintaining the volume of the cavity without expanding until the second molten resin composition filled in the cavity is solidified; Including, A method for manufacturing a container member, wherein the container member obtained through the (C) process comprises a dense layer consisting of a cured product of the first molten resin composition, and a foamed layer consisting of a cured product of the second molten resin composition and having a plurality of voids derived from a supercritical fluid.

2. a dense layer made of a first resin material; a foamed layer made of a second resin material and having a plurality of voids derived from a supercritical fluid; A container member comprising: the dense layer has an abutment portion for contacting another member constituting a container together with the container member, The foam layer has through holes penetrating in a thickness direction, The through hole is filled with the first resin material.

3. the dense layer is in contact with at least a portion of a surface of the foam layer, The container member according to claim 2 , wherein an interface between the dense layer and the foamed layer has irregularities.

4. 4. The container member according to claim 2, wherein the dense layer and the foamed layer are made of the same type of resin material.

5. A top surface portion having an inner ring portion on an inner surface side thereof; A side surface portion extending from a periphery of the top surface portion in a direction away from the top surface portion; A screw thread provided on the inside of the side surface; A container cap comprising: a dense layer made of a first resin material and including the inner ring portion; a foamed layer made of a second resin material and having a plurality of voids derived from a supercritical fluid; Equipped with The thread is formed by the dense layer, A container cap, wherein the dense layer constitutes an inner surface of the top surface portion, and the dense layer is exposed in a region of the inner surface of the top surface portion that is surrounded by the inner ring portion.

6. A container body that constitutes a container together with a lid material, An opening; a dense layer made of a first resin material, constituting the entire flange portion provided around the periphery of the opening and constituting the inner surface of the container body; a foam layer made of a second resin material, having a plurality of voids derived from the supercritical fluid, and constituting an outer surface of the container body; A container body comprising:

Citation Information

Patent Citations

  • Apparatus for measuring viscoelastic property of skin

    JP1985085729A

  • Cap made of resin and manufacture thereof

    JP1988012459A

  • Automatic fruit selector

    JP1989030684A

  • Skin integrated molded product

    JP1993200893A

  • Impeller for blower

    JP2005155437A