Thermoplastic resin composition
A thermoplastic resin composition with a sea-island structure of low molecular weight polybutylene terephthalate, rubber-reinforced polystyrene, and epoxy group-containing elastomer addresses warpage and heat resistance issues, offering enhanced mechanical strength and heat shock resistance for automotive and electronic components.
Patent Information
- Application Number
- JP2020204749
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-10
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-12-10
AI Technical Summary
Existing thermoplastic polyester resin compositions, such as those containing polybutylene terephthalate and glass fibers, suffer from high warpage, anisotropy, and inadequate heat resistance and heat shock resistance, necessitating improvements for applications requiring high mechanical strength and chemical resistance.
A thermoplastic resin composition comprising a blend of low molecular weight polybutylene terephthalate, rubber-reinforced polystyrene or polystyrene, and an epoxy group-containing elastomer, with glass fibers, forming a sea-island structure that enhances heat shock resistance and reduces warpage.
The composition achieves low warpage, excellent heat resistance, and improved mechanical strength, making it suitable for applications with metal inserts and demanding environments like automotive and electronic components.
Smart Images

Figure 0007581822000003 
Figure 0007581822000004 
Figure 0007581822000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermoplastic resin composition, and more particularly to a thermoplastic resin composition which achieves low warpage, heat resistance, and heat shock resistance all at high levels in a well-balanced manner. [Background technology]
[0002] Thermoplastic polyester resins, typified by polybutylene terephthalate and polyethylene terephthalate, are excellent in mechanical strength, chemical resistance, electrical insulation, and the like, and are therefore widely used in electrical and electronic equipment parts, automotive interior and exterior parts, other electrical parts, machine parts, and the like.
[0003] However, since polybutylene terephthalate resin is a crystalline resin, it has a large molding shrinkage rate, and when reinforced fillers such as glass fiber are mixed, the anisotropy tends to increase, and molded products may warp. Therefore, in order to reduce warping, a method of mixing various amorphous resins has been proposed.
[0004] Patent Document 1 describes an invention in which a polyester resin composition is prepared by blending (A) resin consisting of (a) 50-96% by weight of polyester resin, (b) 35-3% by weight of rubber-modified polystyrene resin, and (c) 15-1% by weight of aromatic polycarbonate resin and / or styrene-maleic anhydride copolymer, (B) glass fiber to which a sizing agent containing an amino-silane coupling agent and a novolac-type epoxy resin is attached, and (C) an epoxy compound, and the polyester resin composition has excellent flowability, dimensional accuracy, and heat resistance. However, further improvements are required in terms of heat resistance and low warpage of such polyester resin compositions.
[0005] Patent Document 2 also describes that a thermoplastic polyester resin composition containing 10-80% by weight of (A) thermoplastic polyester resin, 1-15% by weight of (B) epoxy group-containing vinyl copolymer, 1-15% by weight of (C) ABS resin, 1-20% by weight of (D) two or more resins selected from (d-1) maleic anhydride-modified polystyrene resin, (d-2) rubber-modified polystyrene resin, and (d-3) polycarbonate resin, 0-50% by weight of (E) glass fiber, 3-20% by weight of (F) halogenated epoxy bromine-based flame retardant, and 1-10% by weight of (G) antimony compound is excellent in flame retardancy, high impact resistance, high strength, low warpage, as well as heat cycle resistance, dimensional stability after annealing treatment, and heat resistance and rigidity. However, heat resistance and low warpage are required at an extremely high level these days, and the thermoplastic polyester resin composition described in Patent Document 2 is still insufficient in terms of heat resistance and low warpage.
[0006] The present inventors proposed in Patent Document 3 that by combining a low molecular weight polyalkylene terephthalate resin and a high molecular weight polystyrene resin, with a small amount of polyalkylene terephthalate resin and a large amount of polystyrene resin, a resin composition that exhibits high heat resistance, which is a characteristic of polyalkylene terephthalate, and also has excellent low warpage properties, despite being rich in polystyrene resin. However, although this resin composition is excellent in the above points, it was found that there was a problem with heat shock resistance. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2006-16559 A [Patent Document 2] JP 2007-314619 A [Patent Document 3] International Publication No. WO2020 / 111011 Summary of the Invention [Problem to be solved by the invention]
[0008] An object (object) of the present invention is to provide a thermoplastic resin composition which is excellent in low warpage, heat resistance, and heat shock resistance, as well as in mechanical strength and chemical resistance. [Means for solving the problem]
[0009] As a result of intensive research into solving the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by combining a small amount of a low molecular weight polybutylene terephthalate resin with a large amount of a polystyrene-based resin, and further combining it with an epoxy group-containing elastomer, thereby completing the present invention. The present invention relates to the following thermoplastic resin composition and molded article.
[0010] 1. A composition comprising 15 to 50 parts by mass of (A) polybutylene terephthalate resin having an intrinsic viscosity of 0.3 to 0.8 dl / g and 50 to 85 parts by mass of (B) rubber-reinforced polystyrene or polystyrene, for a total of 100 parts by mass, 12 to 35 parts by mass of (C) elastomer, and 5 to 150 parts by mass of (D) glass fiber, wherein the (C) elastomer contains (C-1) an epoxy group-containing olefin-based elastomer or an epoxy group-containing acrylic-based elastomer, and the (B) rubber-reinforced polystyrene or polystyrene is heated at 250°C for 912 sec. -1 A thermoplastic resin composition having a melt viscosity in the range of 70 to 300 Pa·s. 2. The thermoplastic resin composition according to 1 above, wherein the (C) elastomer further contains (C-2) a styrene-based elastomer. 3. The thermoplastic resin composition according to the above item 2, wherein the mass average molecular weight of the styrene-based elastomer (C-2) is 150,000 to 500,000. 4. A thermoplastic resin composition as described in 2 or 3 above, wherein the mass ratio (C-1) / (C-2) of the contents of (C-1) and (C-2) is 0.2 or more.
[0011] 5. The thermoplastic resin composition according to any one of 1 to 4 above, further comprising 1 to 30 parts by mass of a polycarbonate resin (E) per 100 parts by mass of the total of (A) and (B). 6. A thermoplastic resin composition according to any one of 1 to 5 above, wherein (C-1) the epoxy group-containing olefin-based elastomer or the epoxy group-containing acrylic elastomer is copolymerized with glycidyl methacrylate and contains 3 to 15 mass % of structural units derived from glycidyl methacrylate. 7. A molded article made of the thermoplastic resin composition according to any one of 1 to 6 above. 8. The molded product according to claim 7, which is a molded product having a metal insert. 9. The molded product according to claim 7 or 8, which is an in-vehicle housing part. Effect of the Invention
[0012] Although the thermoplastic resin composition of the present invention is a system in which the (A) polybutylene terephthalate resin is low and the (B) rubber-reinforced polystyrene or polystyrene is rich, the (A) polybutylene terephthalate resin having a low molecular weight forms a sea (matrix) of a sea-island structure or a sea of a co-continuous structure, and the (B) rubber-reinforced polystyrene or polystyrene having a high melt viscosity forms islands. Furthermore, the (C) epoxy group-containing olefin-based elastomer or epoxy group-containing acrylic elastomer has a thickening effect, which causes the islands of the (B) rubber-reinforced polystyrene or polystyrene to further aggregate, resulting in high heat shock resistance, excellent low warpage, excellent heat resistance, and excellent mechanical strength, appearance, and chemical resistance. In addition, by containing (D) glass fibers, the resin phase of the (A) polybutylene terephthalate resin becomes continuous through the glass fibers, which makes it easy to form a matrix (sea), resulting in excellent low warpage, heat shock resistance, and heat resistance. In addition, by further containing a polycarbonate resin, the strength and appearance can be further improved. Therefore, the thermoplastic resin composition of the present invention is also suitable for insert moldings in which metal is inserted. The thermoplastic resin composition of the present invention can also be suitably used as parts for various electric and electronic devices, interior and exterior parts for automobiles, and housing parts for automobiles. [Brief description of the drawings]
[0013] [Figure 1] FIG. 2 is a schematic diagram of a rectangular parallelepiped iron insert used in the evaluation of heat shock resistance in the examples. [Diagram 2] FIG. 2 is a cross-sectional view of a mold cavity with an insert supported by a support pin. [Diagram 3] This is a schematic diagram of an insert molding product with two weld lines occurring at the support pin marks. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The thermoplastic resin composition of the present invention contains 15 to 50 parts by mass of (A) a polybutylene terephthalate resin having an intrinsic viscosity of 0.3 to 0.8 dl / g and 50 to 85 parts by mass of (B) a rubber-reinforced polystyrene or polystyrene, for a total of 100 parts by mass, 12 to 35 parts by mass of (C) an elastomer, and 5 to 150 parts by mass of (D) a glass fiber, the (C) elastomer containing (C-1) an epoxy group-containing olefin-based elastomer or an epoxy group-containing acrylic-based elastomer, and the (B) rubber-reinforced polystyrene or polystyrene is melt-melted at 250° C. for 912 sec. -1 It is characterized in that the melt viscosity is in the range of 70 to 300 Pa·s.
[0015] Hereinafter, the embodiments of the present invention will be described in detail. The following description may be based on embodiments and specific examples, but the present invention should not be interpreted as being limited to such embodiments or specific examples. In this specification, the symbol "to" is used to mean that the numerical values before and after it are included as the lower limit and upper limit.
[0016] [(A) Polybutylene terephthalate resin] The thermoplastic resin composition of the present invention contains (A) a polybutylene terephthalate resin having an intrinsic viscosity (IV) of 0.3 to 0.8 dl / g. By using a resin composition having a low intrinsic viscosity (IV) of 0.3 to 0.8 dl / g in combination with (B) rubber-reinforced polystyrene or polystyrene, the resin composition has excellent heat shock resistance, low warpage, and heat resistance, as well as excellent mechanical strength and chemical resistance. (A) Polybutylene terephthalate resin is preferably one having high rigidity. A polybutylene terephthalate resin having high rigidity is characterized by having a rigidity of 1500 MPa or more in terms of flexural modulus according to ISO 178. If an intrinsic viscosity (IV) of less than 0.3 dl / g is used, the heat resistance of the polybutylene terephthalate is not expressed, and the mechanical strength is likely to be low. If the intrinsic viscosity (IV) is more than 0.8 dl / g, the above-mentioned sea-island structure is difficult to form, and the (B) rubber-reinforced polystyrene or polystyrene is likely to become a sea, the heat shock resistance and low warpage properties are deteriorated, and the flowability of the resin composition is poor, and moldability is likely to be deteriorated. The intrinsic viscosity (IV) is preferably 0.4 dl / g or more, more preferably 0.5 dl / g or more, and even more preferably 0.55 dl / g or more, and of these, 0.6 dl / g or more is preferable, and 0.75 dl / g or less is preferable.
[0017] In the present invention, the intrinsic viscosity of the (A) polybutylene terephthalate resin is a value measured at 30° C. in a mixed solvent of tetrachloroethane and phenol in a 1:1 (mass ratio).
[0018] (A) Polybutylene terephthalate resin is a polyester resin having a structure in which terephthalic acid units and 1,4-butanediol units are ester-bonded, and includes, in addition to polybutylene terephthalate resin (homopolymer), polybutylene terephthalate copolymers containing other copolymerization components other than terephthalic acid units and 1,4-butanediol units, and mixtures of homopolymers and the copolymers.
[0019] The (A) polybutylene terephthalate resin may contain a dicarboxylic acid unit other than terephthalic acid. Specific examples of the other dicarboxylic acids include aromatic dicarboxylic acids such as isophthalic acid, orthophthalic acid, 1,5-naphthalenedicarboxylic acid, 2,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, biphenyl-2,2'-dicarboxylic acid, biphenyl-3,3'-dicarboxylic acid, biphenyl-4,4'-dicarboxylic acid, bis(4,4'-carboxyphenyl)methane, anthracenedicarboxylic acid, and 4,4'-diphenyletherdicarboxylic acid; alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid and 4,4'-dicyclohexyldicarboxylic acid; and aliphatic dicarboxylic acids such as adipic acid, sebacic acid, azelaic acid, and dimer acid.
[0020] The diol unit may contain other diol units in addition to 1,4-butanediol, and specific examples of other diol units include aliphatic or alicyclic diols having 2 to 20 carbon atoms, bisphenol derivatives, etc. Specific examples include ethylene glycol, propylene glycol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, decamethylene glycol, cyclohexanedimethanol, 4,4'-dicyclohexylhydroxymethane, 4,4'-dicyclohexylhydroxypropane, and ethylene oxide adduct diol of bisphenol A. In addition to the above-mentioned bifunctional monomers, a small amount of a trifunctional monomer such as trimellitic acid, trimesic acid, pyromellitic acid, pentaerythritol, or trimethylolpropane may be used in combination to introduce a branched structure, or a monofunctional compound such as a fatty acid may be used in combination to adjust the molecular weight.
[0021] As described above, the (A) polybutylene terephthalate resin is preferably a polybutylene terephthalate homopolymer obtained by polycondensation of terephthalic acid and 1,4-butanediol, but may also be a polybutylene terephthalate copolymer containing, as carboxylic acid units, one or more dicarboxylic acids other than the above-mentioned terephthalic acid and / or, as diol units, one or more diols other than the above-mentioned 1,4-butanediol, within a range that does not impair the crystallinity of the (A) polybutylene terephthalate resin. When the (A) polybutylene terephthalate resin is a polybutylene terephthalate resin modified by copolymerization, specific preferred copolymers include polyester ether resins copolymerized with polyalkylene glycols, particularly polytetramethylene glycol, dimer acid copolymerized polybutylene terephthalate resins, and isophthalic acid copolymerized polybutylene terephthalate resins. These copolymers refer to those in which the copolymerization amount is 1 mol% or more and less than 50 mol% in the total segments of the polybutylene terephthalate resin. In particular, the copolymerization amount is preferably 2 mol% or more and less than 50 mol%, more preferably 3 to 40 mol%, and particularly preferably 5 to 20 mol%. By setting the copolymerization ratio in this range, fluidity and toughness tend to be easily improved, which is preferable.
[0022] The amount of terminal carboxyl groups in the polybutylene terephthalate resin (A) is preferably 0.1 to 30 eq / ton. If it exceeds 30 eq / ton, the hydrolysis resistance and alkali resistance are likely to decrease, and gas is likely to be generated during melt molding of the resin composition. The amount of terminal carboxyl groups is more preferably 3 eq / ton or more, and even more preferably 5 eq / ton or more, more preferably 25 eq / ton or less, and even more preferably 20 eq / ton or less.
[0023] The amount of terminal carboxyl groups in the polybutylene terephthalate resin is a value measured by dissolving 0.5 g of the polybutylene terephthalate resin in 25 mL of benzyl alcohol and titrating it with a 0.01 mol / l benzyl alcohol solution of sodium hydroxide. The amount of terminal carboxyl groups can be adjusted by any conventional method, such as adjusting the polymerization conditions such as the raw material charge ratio during polymerization, the polymerization temperature, and the pressure reduction method, or by reacting a terminal blocking agent.
[0024] (A) Polybutylene terephthalate resin can be produced by batch or continuous melt polymerization of a dicarboxylic acid component mainly composed of terephthalic acid or an ester derivative thereof and a diol component mainly composed of 1,4-butanediol. In addition, after producing a low molecular weight polybutylene terephthalate resin by melt polymerization, the degree of polymerization (or molecular weight) can be increased to a desired value by further solid-phase polymerization under a nitrogen gas flow or reduced pressure. The (A) polybutylene terephthalate resin is preferably one obtained by a production method in which a dicarboxylic acid component mainly composed of terephthalic acid and a diol component mainly composed of 1,4-butanediol are subjected to continuous melt polycondensation.
[0025] The catalyst used in carrying out the esterification reaction may be a conventionally known catalyst, and examples thereof include titanium compounds, tin compounds, magnesium compounds, calcium compounds, etc. Among these, titanium compounds are particularly preferred. Specific examples of titanium compounds as esterification catalysts include titanium alcoholates such as tetramethyl titanate, tetraisopropyl titanate, and tetrabutyl titanate, and titanium phenolates such as tetraphenyl titanate.
[0026] [(B) Rubber-reinforced polystyrene or polystyrene] The thermoplastic resin composition of the present invention contains (B) rubber-reinforced polystyrene or polystyrene, and is heat-treated at 250° C. for 912 sec. -1The melt viscosity of the rubber-reinforced polystyrene or polystyrene is in the range of 70 to 300 Pa·s.
[0027] (B) rubber-reinforced polystyrene or polystyrene is preferably amorphous. Here, amorphous refers to a property in which no clear melting point or melting peak is detected when a sample is measured using a differential scanning calorimeter (DSC) or the like. Conversely, crystalline refers to a property in which the molecules tend to be regularly arranged in a crystal structure, and which has a melting point and a melting peak when measured using a differential scanning calorimeter (DSC) or the like. Syndiotactic polystyrene, in which benzene rings are regularly arranged alternately in the polymer main chain, is crystalline, and is preferably excluded from (B) rubber-reinforced polystyrene or polystyrene.
[0028] The polystyrene resin may be a homopolymer of styrene or a copolymer of other aromatic vinyl monomers such as α-methylstyrene, paramethylstyrene, vinyltoluene, vinylxylene, etc. in an amount of, for example, 50% by mass or less.
[0029] The rubber-reinforced polystyrene resin is preferably a copolymer or blend of a butadiene rubber component, and the amount of the butadiene rubber component is usually 1 mass % or more and less than 50 mass %, preferably 3 to 40 mass %, more preferably 5 to 30 mass %, and further preferably 5 to 20 mass %. As the rubber-reinforced polystyrene resin, high impact polystyrene (HIPS) is particularly preferable.
[0030] In the present invention, (B) rubber-reinforced polystyrene or polystyrene is subjected to a process of 250° C., 912 sec. -1 The melt viscosity at η is 70 to 300 Pa·s. BBy blending (B) rubber-reinforced polystyrene or polystyrene in an amount of 15 to 50 parts by mass of (A) polybutylene terephthalate resin and 50 to 85 parts by mass of (B) rubber-reinforced polystyrene or polystyrene [based on a total of 100 parts by mass of (A) and (B)], and further blending (C) elastomer together, (A) polybutylene terephthalate resin becomes dominant in terms of physical properties, and as a result, high heat resistance, low warpage, and heat shock resistance can be achieved. If the melt viscosity is 70 Pa·s or more, heat resistance can be improved. Also, if the melt viscosity is 300 Pa·s or less, excellent production stability and flowability can be provided.
[0031] (B) Melt viscosity of rubber-reinforced polystyrene or polystyrene (η B ) is preferably 80 Pa·s or more, more preferably 90 Pa·s or more, even more preferably 100 Pa·s or more, of which 110 Pa·s or more, and particularly preferably 120 Pa·s or more. The upper limit is preferably 250 Pa·s or less, more preferably 220 Pa·s or less, even more preferably 200 Pa·s or less, of which 180 Pa·s or less, and particularly preferably 160 Pa·s or less. The melt viscosity can be measured using a capillary rheometer and a slit die rheometer in accordance with ISO 11443. Specifically, the melt viscosity can be calculated from the stress when a piston is pressed into a furnace body with an inner diameter of 9.5 mm heated to 250°C at a piston speed of 75 mm / min using an orifice with a capillary diameter of 1 mm and a capillary length of 30 mm.
[0032] As described above, the content of the polybutylene terephthalate resin (A) is 15 to 50 parts by mass, and the content of the rubber-reinforced polystyrene or polystyrene (B) is 50 to 85 parts by mass, based on 100 parts by mass of the total of (A) and (B), but preferably (A) is 20 parts by mass or more, more preferably 25 parts by mass or more, even more preferably 30 parts by mass or more, and preferably 47 parts by mass or less, more preferably 45 parts by mass or less. Preferably, (B) is 80 parts by mass or less, more preferably 75 parts by mass or less, even more preferably 70 parts by mass or less, and preferably 53 parts by mass or more, more preferably 55 parts by mass or more. (B) When the content of rubber-reinforced polystyrene or polystyrene is within such range, the heat shock resistance and low warpage can be further improved.
[0033] [(C) Elastomer] The thermoplastic resin composition of the present invention contains an elastomer (C), and the elastomer (C) contains an epoxy group-containing olefinic elastomer or an epoxy group-containing acrylic elastomer (C-1). By containing the epoxy group-containing olefinic or acrylic elastomer (C-1), high heat shock resistance is achieved, whereas elastomers not containing epoxy groups have insufficient heat shock resistance.
[0034] [(C-1) Epoxy group-containing olefin-based elastomer or epoxy group-containing acrylic elastomer] The component (C-1) is an olefin-based elastomer or an acrylic-based elastomer containing an epoxy group, and is an elastomer obtained by introducing a glycidyl group into an olefin-based elastomer or an acrylic-based elastomer. There is no limitation on the method for introducing the glycidyl group, and any known method can be adopted. Specifically, for example, a method of copolymerizing a vinyl monomer having an epoxy group, such as a glycidyl ester compound of an α,β-unsaturated acid such as glycidyl acrylate, glycidyl methacrylate, glycidyl ethacrylate, or glycidyl itaconate, with an olefin-based or acrylic monomer, which is an elastomer raw material, a method of polymerizing an elastomer polymer using a polymerization initiator or chain transfer agent having an epoxy group, a method of grafting an epoxy compound onto an elastomer, and the like can be mentioned.
[0035] The content of the glycidyl group, in the case of a glycidyl methacrylate group, is usually 1 to 20 mass %, preferably 3 to 15 mass %, more preferably 3 to 12 mass %, and particularly preferably 4 to 8 mass %.
[0036] Preferred examples of the olefin-based elastomer include polybutadiene, polyisoprene, styrene-butadiene random copolymers and block copolymers, hydrogenated products of the block copolymers, diene-based elastomers such as butadiene-isoprene copolymers, ethylene-propylene random copolymers and block copolymers, ethylene-butene random copolymers and block copolymers, copolymers of ethylene and α-olefins, ethylene-propylene non-conjugated diene terpolymers such as ethylene-propylene-hexadiene copolymers, and butylene-isoprene copolymers.
[0037] An acrylate-based elastomer is a rubber-like elastic material obtained by polymerization of an acrylic acid ester or copolymerization mainly containing the acrylic acid ester. For example, there is a rubber-like polymer obtained by graft polymerizing a graft-polymerizable monomer such as methyl methacrylate to a polymer obtained by polymerizing an acrylic acid ester such as butyl acrylate with a small amount of a crosslinkable monomer such as butylene diacrylate.
[0038] Examples of the acrylic acid ester include, in addition to butyl acrylate, methyl acrylate, ethyl acrylate, propyl acrylate, hexyl acrylate, 2-ethylhexyl acrylate, etc. Examples of the crosslinkable monomer include, in addition to butylene diacrylate, esters of polyols and acrylic acid or methacrylic acid such as butylene dimethacrylate and trimethylolpropane trimethacrylate, vinyl compounds such as vinyl acrylate and vinyl methacrylate, allyl acrylate, allyl methacrylate, diallyl maleate, diallyl fumarate, diallyl itaconate, monoallyl maleate, monoallyl fumarate, etc.
[0039] Examples of the graft polymerizable monomer include, in addition to methyl methacrylate, methacrylic acid esters such as ethyl methacrylate, butyl methacrylate, hexyl methacrylate, 2-ethylhexyl methacrylate, and lauryl methacrylate, styrene, and acrylonitrile. Further examples include acrylates having a glycidyl group, such as glycidyl methacrylate. A part of the graft polymerizable monomer can be copolymerized by being coexisted when the acrylic acid ester and the crosslinkable monomer are polymerized to produce a polymer.
[0040] As the olefin-based elastomer or the acrylic-based elastomer, a copolymer in which the above-mentioned olefin-based monomer and the above-mentioned acrylate-based monomer are combined is also preferred.
[0041] The epoxy group-containing olefin elastomer or epoxy group-containing acrylic elastomer (C-1) is preferably a copolymer of glycidyl methacrylate, and particularly preferably contains 3 to 15 mass % of structural units derived from glycidyl methacrylate.
[0042] [(C-2) Styrene-based elastomer] It is preferable that the (C) elastomer further contains (C-2) a styrene-based elastomer. As the (C-2) styrene-based elastomer, a block copolymer consisting of a polymer block having a vinyl aromatic compound as a polymerization component and a polymer block having a conjugated diene as a polymerization component, and a hydrogenated product thereof are preferable.
[0043] Examples of vinyl aromatic compounds constituting the vinyl aromatic hydrocarbon polymer block include styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, pt-butylstyrene, 1,3-dimethylstyrene, lower alkyl-substituted styrene, vinylnaphthalene, vinylanthracene, and other styrene or derivatives thereof. These can be used alone or in combination of two or more.
[0044] Examples of the conjugated diene constituting the conjugated diene block include butadiene, isoprene, 1,3-pentadiene, and 2,3-dimethyl-1,3-butadiene.
[0045] The (C-2) styrene-based elastomer is preferably a block copolymer consisting of at least two polymer blocks P mainly composed of a vinyl aromatic compound and at least one polymer block Q mainly composed of butadiene and / or isoprene, and represented by the formula (PQ)nP (n is an integer of 1 or more), or a triblock or higher block copolymer, and more preferably a block copolymer in which the polymer block P accounts for 20 to 60 mass % or a hydrogenated block copolymer obtained by hydrogenating the block copolymer. In the above, "mainly" means more than 50% by mass, preferably 55% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, of which 80% by mass or more, and particularly preferably 90% by mass or more.
[0046] Block copolymers such as triblock copolymers represented by the formula (PQ)nP are preferred because they provide a high thickening effect in proportion to the molecular weight, and the islands of (B) rubber-reinforced polystyrene or polystyrene, which become the islands in the sea-island structure formed by the resulting resin composition, are more likely to aggregate and provide a higher improvement in heat shock resistance. In the case of PQ-type diblock copolymers, the fluidity is too good, so the thickening effect is reduced, and the improvement in heat shock resistance tends to be small.
[0047] Specific preferred examples of the (C-2) styrene-based elastomer include styrene-butadiene-styrene block copolymer (SBS), hydrogenated styrene-butadiene-styrene block copolymer (SEBS), styrene-isoprene-styrene block copolymer (SIS), hydrogenated styrene-isoprene-styrene block copolymer (SEPS), and the like.
[0048] (C-2) styrene-based elastomers having a high molecular weight are preferred because they have a high thickening effect and the islands of (B) rubber-reinforced polystyrene or polystyrene are more likely to aggregate, resulting in a high improvement in heat shock resistance, and the above effect is more pronounced when the mass-average molecular weight is in the range of 150,000 to 500,000. The mass-average molecular weight is more preferably 200,000 or more, even more preferably 250,000 or more, and particularly preferably 300,000 or more, more preferably 450,000 or less, and even more preferably 400,000 or less.
[0049] The content of the (C) elastomer is 12 to 35 parts by mass, preferably 14 parts by mass or more, more preferably 15 parts by mass or more, even more preferably 16 parts by mass or more, and preferably 30 parts by mass or less, more preferably 27 parts by mass or less, even more preferably 25 parts by mass or less, and particularly preferably 23 parts by mass or less, relative to 100 parts by mass of the total of 15 to 50 parts by mass of the (A) polybutylene terephthalate resin and (B) rubber-reinforced polystyrene or polystyrene. The content of the (C) elastomer in such a range can further improve heat shock resistance in particular.
[0050] The content of the (C-2) styrene-based elastomer is preferably 0 to 25 parts by mass, more preferably 2 parts by mass or more, even more preferably 5 parts by mass or more, and preferably 23 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 18 parts by mass or less, relative to 100 parts by mass of the total of (A) and (B). By including the (C-2) styrene-based elastomer in such an amount, a higher level of heat shock resistance can be achieved.
[0051] The mass ratio (C-1) / (C-2) of the content of the epoxy group-containing olefin or acrylic elastomer (C-1) to the styrene elastomer (C-2) is preferably 0.2 or more, more preferably 0.3 or more, even more preferably 0.5 or more, more preferably 5 or less, and even more preferably 3 or less. By setting the mass ratio in this manner, it is possible to impart particularly high heat shock resistance and excellent flowability.
[0052] [(D) Glass fiber] The thermoplastic resin composition of the present invention contains (D) glass fibers. As the glass fiber, any known glass fiber can be used as long as it is one that is usually used in thermoplastic polyester resins, regardless of the form of the glass fiber when blended, such as A glass, E glass, alkali-resistant glass composition containing a zirconia component, chopped strands, roving glass, master batch of thermoplastic resin and glass fiber, etc. Among them, as the glass fiber used in the present invention, alkali-free glass (E glass) is preferable for the purpose of improving the thermal stability of the thermoplastic resin composition of the present invention.
[0053] The (D) glass fiber may have a circular cross section in the longitudinal direction, and is also preferably a glass fiber having an irregularity ratio of 2 to 6 in the longitudinal cross section. The irregularity ratio in the longitudinal cross section is the ratio of the major axis to the minor axis when a rectangle of the smallest area circumscribing a cross section perpendicular to the longitudinal direction of the glass fiber is assumed, and the length of the long side of this rectangle is the major axis and the length of the short side is the minor axis. By including glass fibers having an irregularity ratio of 2 to 6, the glass fibers exhibit a bridging function connecting the phases of the (A) polybutylene terephthalate resin in which the glass fibers are oriented, and the polybutylene terephthalate resin is easily made into a matrix (sea), so that the heat resistance is specifically improved, and it is also possible to obtain a glass fiber having low warpage and excellent appearance. Furthermore, when the glass fibers are present in a state surrounded by the (A) polybutylene terephthalate resin phase, the bridging effect of the glass fibers between the (A) polybutylene terephthalate resin phases is enhanced, and in addition, the bulky glass fibers act as an extender for the (A) polybutylene terephthalate resin, which further improves heat resistance.
[0054] In the case of glass fibers having a modified cross section, the modification ratio is more preferably 2.5 or more, even more preferably 3 or more, and more preferably 5.5 or less, even more preferably 5 or less. The shape of the longitudinal cross section is particularly preferably approximately rectangular. The cross-sectional area of the glass fiber in the longitudinal direction is 180 μm 2 Ultra 300μm 2 With such a cross-sectional area, the polybutylene terephthalate resin is likely to become a matrix, and as a result, the heat resistance is likely to be improved. The cross-sectional area is more preferably 180 μm 2 Super 250μm 2 Less than 180 μm, more preferably 2 Super 200μm 2 The following is the result. The thickness of the glass fiber is not particularly limited, but it is preferable that the minor axis is about 2 to 20 μm and the major axis is about 5 to 50 μm.
[0055] The (D) glass fiber may be treated with a sizing agent or a surface treatment agent. In addition, during the production of the resin composition of the present invention, a sizing agent or a surface treatment agent may be added separately from the untreated glass fiber to perform surface treatment.
[0056] Examples of the sizing agent include resin emulsions such as vinyl acetate resin, ethylene / vinyl acetate copolymer, acrylic resin, epoxy resin, polyurethane resin, and polyester resin. Examples of the surface treatment agent include aminosilane compounds such as γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, and γ-(2-aminoethyl)aminopropyltrimethoxysilane; chlorosilane compounds such as vinyltrichlorosilane and methylvinyldichlorosilane; alkoxysilane compounds such as vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriacetoxysilane, and γ-methacryloxypropyltrimethoxysilane; epoxysilane compounds such as β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane and γ-glycidoxypropyltrimethoxysilane; acrylic compounds, isocyanate compounds, titanate compounds, and epoxy compounds. These sizing agents and surface treatment agents may be used in combination of two or more kinds, and the amount used (adhering amount) is usually 10 mass % or less, preferably 0.05 to 5 mass %, based on the mass of the (D) glass fiber. By keeping the adhering amount to 10 mass % or less, a necessary and sufficient effect can be obtained.
[0057] Two or more kinds of (D) glass fibers may be used in combination depending on the required characteristics, and the content is 5 to 150 parts by mass relative to 100 parts by mass of the total of (A) polybutylene terephthalate resin and (B) rubber-reinforced polystyrene or polystyrene, preferably 10 parts by mass or more, more preferably 20 parts by mass or more, even more preferably 30 parts by mass or more, particularly preferably 40 parts by mass or more, and preferably 120 parts by mass or less, more preferably 100 parts by mass or less, among which 80 parts by mass or less, particularly preferably 60 parts by mass or less. By containing it in such a range, high heat resistance can be achieved, and the strength and shrinkage rate reduction effect of the obtained molded body can be improved.
[0058] In the resin composition of the present invention, in the cross-sectional structure of a molded article of the resin composition observed under an electron microscope, it is preferable that the (D) glass fiber is present in a state surrounded by the (A) polybutylene terephthalate resin phase. It is also preferable that the (A) polybutylene terephthalate resin forms a sea (matrix) of a sea-island structure, or forms a co-continuous phase with the (B) rubber-reinforced polystyrene or polystyrene. By having such a morphological structure, it is possible to specifically improve heat resistance, and furthermore, to obtain a product with excellent low warpage and excellent appearance.
[0059] The thermoplastic resin composition of the present invention preferably contains carbon fiber or other inorganic fillers in a plate-like, granular or amorphous form in addition to the above-mentioned (D) glass fiber. The plate-like inorganic filler exhibits a function of reducing anisotropy and warpage, and examples thereof include talc, glass flakes, mica, kaolin, and metal foil. Among the plate-like inorganic fillers, glass flakes are preferred. Other particulate or amorphous inorganic fillers include ceramic beads, clay, zeolites, barium sulfate, titanium oxide, silicon oxide, aluminum oxide, magnesium hydroxide, zinc sulfide, and the like. As the other inorganic filler, talc, titanium oxide, and zinc sulfide are preferable, and talc is particularly preferable.
[0060] When other inorganic fillers are contained, the content thereof is preferably 0.1 to 30 parts by mass, more preferably 0.5 parts by mass or more, even more preferably 1 part by mass or more, and more preferably 20 parts by mass or less, relative to 100 parts by mass of the total of (A) polybutylene terephthalate resin and (B) rubber-reinforced polystyrene or polystyrene.
[0061] [(E) Polycarbonate resin] The resin composition of the present invention preferably further contains (E) a polycarbonate resin. The inclusion of (E) a polycarbonate resin promotes the compatibility of (A) polybutylene terephthalate resin with (B) rubber-reinforced polystyrene or polystyrene, thereby reducing the dispersed particle size of (B) rubber-reinforced polystyrene or polystyrene dispersed in the (A) polybutylene terephthalate resin phase and increasing the interfacial strength, thereby further improving the mechanical strength and making it easier to obtain an excellent appearance.
[0062] Polycarbonate resins are thermoplastic polymers or copolymers, which may be branched, obtained by reacting a dihydroxy compound or a small amount of a polyhydroxy compound with phosgene or a carbonic acid diester. The method for producing the polycarbonate resin is not particularly limited, and polycarbonate resins produced by the conventionally known phosgene method (interfacial polymerization method) or melting method (ester exchange method) can be used.
[0063] The dihydroxy compound as the raw material is one that does not substantially contain bromine atoms, and is preferably an aromatic dihydroxy compound.Specific examples include 2,2-bis(4-hydroxyphenyl)propane (i.e., bisphenol A), tetramethylbisphenol A, bis(4-hydroxyphenyl)-p-diisopropylbenzene, hydroquinone, resorcinol, 4,4-dihydroxydiphenyl, and the like, and preferably bisphenol A.Also, a compound in which one or more tetraalkylphosphonium sulfonates are bonded to the above aromatic dihydroxy compound can be used.
[0064] As the polycarbonate resin, among the above, an aromatic polycarbonate resin derived from 2,2-bis(4-hydroxyphenyl)propane (i.e., bisphenol A) or an aromatic polycarbonate copolymer derived from 2,2-bis(4-hydroxyphenyl)propane and another aromatic dihydroxy compound is preferable. In addition, it may be a copolymer mainly composed of an aromatic polycarbonate resin, such as a copolymer with a polymer or oligomer having a siloxane structure. Furthermore, two or more of the above polycarbonate resins may be mixed and used.
[0065] In order to adjust the molecular weight of the polycarbonate resin, a monovalent aromatic hydroxy compound may be used, for example, m- and p-methylphenol, m- and p-propylphenol, p-tert-butylphenol, p-long-chain alkyl-substituted phenol, and the like.
[0066] The viscosity average molecular weight (Mv) of the polycarbonate resin is preferably 14000 or more, more preferably 15000 or more, and even more preferably 15500 or more, and is preferably 60000 or less, more preferably 40000 or less, and even more preferably 35000 or less. By using one having a viscosity average molecular weight within the above range, the obtained resin composition is preferably free from a decrease in mechanical strength such as impact resistance, and the fluidity of the resin composition is not decreased and the moldability is not deteriorated.
[0067] In the present invention, the viscosity average molecular weight (Mv) of a polycarbonate resin is a value calculated from the intrinsic viscosity ([η]) obtained by measuring the viscosity of a methylene chloride solution of the polycarbonate resin at 25° C. using an Ubbelohde viscometer, and then calculating the viscosity from the following Schnell viscosity formula: [η]=1.23×10 -4 Mv 0.83
[0068] The method for producing the polycarbonate resin is not particularly limited, and polycarbonate resins produced by either the phosgene method (interfacial polymerization method) or the melting method (ester exchange method) can be used. In addition, polycarbonate resins produced by the melting method and then subjected to post-treatment to adjust the amount of OH groups at the terminals are also preferred.
[0069] The content of the (E) polycarbonate resin is preferably 1 to 30 parts by mass, more preferably 3 parts by mass or more, even more preferably 5 parts by mass or more, of which 8 parts by mass or more, particularly preferably 10 parts by mass or more, and more preferably 25 parts by mass or less, even more preferably 20 parts by mass or less, of which 17 parts by mass or less, particularly preferably 15 parts by mass or less, relative to 100 parts by mass in total of the (A) polybutylene terephthalate resin and the (B) rubber-reinforced polystyrene or polystyrene.
[0070] [Stabilizer] The thermoplastic resin composition of the present invention preferably contains a stabilizer, which has the effect of improving thermal stability and preventing deterioration of mechanical strength, transparency, and color. As the stabilizer, phosphorus-based stabilizers, sulfur-based stabilizers, and phenol-based stabilizers are preferred.
[0071] Examples of phosphorus-based stabilizers include phosphorous acid, phosphoric acid, phosphorous acid esters (phosphites), trivalent phosphoric acid esters (phosphonites), pentavalent phosphoric acid esters (phosphates), and the like. Among these, phosphites, phosphonites, and phosphates are preferred.
[0072] The organic phosphate compound is preferably a compound represented by the following general formula: (R 1 O) 3-n P(=O)OH n (In the formula, R 1 are alkyl groups or aryl groups, which may be the same or different, and n is an integer of 0 to 2. More preferably, R 1and long-chain alkyl acid phosphate compounds having 8 to 30 carbon atoms. Specific examples of the alkyl group having 8 to 30 carbon atoms include an octyl group, a 2-ethylhexyl group, an isooctyl group, a nonyl group, an isononyl group, a decyl group, an isodecyl group, a dodecyl group, a tridecyl group, an isotridecyl group, a tetradecyl group, a hexadecyl group, an octadecyl group, an eicosyl group, and a triacontyl group.
[0073] Examples of long-chain alkyl acid phosphates include octyl acid phosphate, 2-ethylhexyl acid phosphate, decyl acid phosphate, lauryl acid phosphate, octadecyl acid phosphate, oleyl acid phosphate, behenyl acid phosphate, phenyl acid phosphate, nonylphenyl acid phosphate, cyclohexyl acid phosphate, phenoxyethyl acid phosphate, and alkoxypolyethylene glycol acid phosphate. Examples of suitable acid phosphates include bisphenol A acid phosphate, dimethyl acid phosphate, diethyl acid phosphate, dipropyl acid phosphate, diisopropyl acid phosphate, dibutyl acid phosphate, dioctyl acid phosphate, di-2-ethylhexyl acid phosphate, dioctyl acid phosphate, dilauryl acid phosphate, distearyl acid phosphate, diphenyl acid phosphate, bisnonylphenyl acid phosphate, etc. Among these, octadecyl acid phosphate is preferred, and this is commercially available under the trade name "ADEKA STAB AX-71" from ADEKA Corporation.
[0074] The organic phosphite compound is preferably a compound represented by the following general formula: R 2 OP(OR 3 )(OR 4 ) (In the formula, R 2 , R 3 and R 4 are each a hydrogen atom, an alkyl group having 1 to 30 carbon atoms, or an aryl group having 6 to 30 carbon atoms, and R2 , R 3 and R 4 At least one of the groups is an aryl group having 6 to 30 carbon atoms.) Examples of the compound include compounds represented by the following formula:
[0075] Examples of the organic phosphite compound include triphenyl phosphite, tris(nonylphenyl)phosphite, dilauryl hydrogen phosphite, triethyl phosphite, tridecyl phosphite, tris(2-ethylhexyl)phosphite, tris(tridecyl)phosphite, tristearyl phosphite, diphenyl monodecyl phosphite, monophenyl didecyl phosphite, diphenyl mono(tridecyl)phosphite, tetraphenyl dipropylene glycol diphosphite, tetraphenyl tetra(tridecyl)pentaerythritol tetraphosphite, hydrogenated bisphenol A phenol phosphite polymer, diphenyl hydrogen phosphite, 4,4'-butylidene-bis(3-methyl-6-tert-butylphenyl di(tridecyl)phosphite), tetra(tridecyl) 4,4'-isopropyl phosphite, tetraphenyl di ... Examples of the phosphite include propylidenediphenyl diphosphite, bis(tridecyl)pentaerythritol diphosphite, bis(nonylphenyl)pentaerythritol diphosphite, dilauryl pentaerythritol diphosphite, distearyl pentaerythritol diphosphite, tris(4-tert-butylphenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite, hydrogenated bisphenol A pentaerythritol phosphite polymer, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, 2,2'-methylenebis(4,6-di-tert-butylphenyl)octyl phosphite, and bis(2,4-dicumylphenyl)pentaerythritol diphosphite. Among these, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite is preferred.
[0076] The organic phosphonite compound is preferably a compound represented by the following general formula: R 5 -P(OR 6 )(OR 7 ) (In the formula, R 5 , R 6 and R 7 are each a hydrogen atom, an alkyl group having 1 to 30 carbon atoms, or an aryl group having 6 to 30 carbon atoms, and R 5 , R 6 and R 7 At least one of the groups is an aryl group having 6 to 30 carbon atoms.) Examples of the compound include compounds represented by the following formula:
[0077] The organic phosphonite compounds include tetrakis(2,4-di-isopropylphenyl)-4,4'-biphenylene diphosphonite, tetrakis(2,4-di-n-butylphenyl)-4,4'-biphenylene diphosphonite, tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenylene diphosphonite, tetrakis(2,4-di-tert-butylphenyl)-4,3'-biphenylene diphosphonite, and tetrakis(2,4-di-tert-butylphenyl)-3,3'-biphenylene diphosphonite. tetrakis(2,6-di-iso-propylphenyl)-4,4'-biphenylene diphosphonite, tetrakis(2,6-di-n-butylphenyl)-4,4'-biphenylene diphosphonite, tetrakis(2,6-di-tert-butylphenyl)-4,4'-biphenylene diphosphonite, tetrakis(2,6-di-tert-butylphenyl)-4,3'-biphenylene diphosphonite, and tetrakis(2,6-di-tert-butylphenyl)-3,3'-biphenylene diphosphonite.
[0078] As the sulfur-based stabilizer, any conventionally known sulfur atom-containing compound can be used, among which thioethers are preferred.Specific examples include didodecylthiodipropionate, ditetradecylthiodipropionate, dioctadecylthiodipropionate, pentaerythritol tetrakis(3-dodecylthiopropionate), thiobis(N-phenyl-β-naphthylamine), 2-mercaptobenzothiazole, 2-mercaptobenzimidazole, tetramethylthiuram monosulfide, tetramethylthiuram disulfide, nickel dibutyldithiocarbamate, nickel isopropylxanthate, and trilauryltrithiophosphite.Among these, pentaerythritol tetrakis(3-dodecylthiopropionate) is preferred.
[0079] Examples of phenol-based stabilizers include pentaerythritol tetrakis(3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate), octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, thiodiethylenebis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), pentaerythritol tetrakis(3-(3,5-di-neopentyl-4-hydroxyphenyl)propionate), etc. Among these, pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate) and octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate are preferred.
[0080] The stabilizer may be contained alone or in any combination and ratio of two or more kinds.
[0081] The content of the stabilizer is preferably 0.001 to 2 parts by mass relative to 100 parts by mass of the total of (A) polybutylene terephthalate resin and (B) rubber-reinforced polystyrene or polystyrene. If the content of the stabilizer is less than 0.001 parts by mass, it is difficult to expect improvement in the thermal stability and compatibility of the resin composition, and a decrease in molecular weight and deterioration in hue during molding are likely to occur, while if it exceeds 2 parts by mass, the amount becomes excessive, and silver generation and deterioration in hue tend to occur more easily. The content of the stabilizer is more preferably 0.01 to 1.5 parts by mass, and even more preferably 0.1 to 1 part by mass.
[0082] [Release agent] The thermoplastic resin composition of the present invention preferably contains a release agent. As the release agent, known release agents that are usually used for polyester resins can be used, but among them, polyolefin compounds and fatty acid ester compounds are preferred in terms of good alkali resistance, and polyolefin compounds are particularly preferred.
[0083] The polyolefin-based compound may be a compound selected from paraffin wax and polyethylene wax, and among them, those having a weight average molecular weight of 700 to 10,000, more preferably 900 to 8,000, are preferred.
[0084] Examples of fatty acid ester compounds include fatty acid esters such as saturated or unsaturated monovalent or divalent aliphatic carboxylic acid esters, glycerin fatty acid esters, sorbitan fatty acid esters, and partially saponified products thereof, etc. Among these, mono- or di-fatty acid esters composed of a fatty acid having 11 to 28 carbon atoms, preferably 17 to 21 carbon atoms, and an alcohol are preferred.
[0085] Examples of fatty acids include palmitic acid, stearic acid, caproic acid, capric acid, lauric acid, arachic acid, behenic acid, lignoceric acid, cerotic acid, melissic acid, tetralinic acid, montanic acid, adipic acid, azelaic acid, etc. The fatty acid may also be alicyclic. Examples of the alcohol include saturated or unsaturated monohydric or polyhydric alcohols. These alcohols may have a substituent such as a fluorine atom or an aryl group. Among these, monohydric or polyhydric saturated alcohols having 30 or less carbon atoms are preferred, and aliphatic saturated monohydric or polyhydric alcohols having 30 or less carbon atoms are more preferred. Here, the term "aliphatic" also includes alicyclic compounds. Specific examples of such alcohols include octanol, decanol, dodecanol, stearyl alcohol, behenyl alcohol, ethylene glycol, diethylene glycol, glycerin, pentaerythritol, 2,2-dihydroxyperfluoropropanol, neopentylene glycol, ditrimethylolpropane, and dipentaerythritol. The above ester compound may contain an aliphatic carboxylic acid and / or an alcohol as an impurity, and may be a mixture of a plurality of compounds.
[0086] Specific examples of fatty acid ester compounds include glycerin monostearate, glycerin monobehenate, glycerin dibehenate, glycerin-12-hydroxymonostearate, sorbitan monobehenate, pentaerythritol monostearate, pentaerythritol distearate, stearyl stearate, and ethylene glycol montanic acid ester.
[0087] The content of the release agent is preferably 0.1 to 3 parts by mass, more preferably 0.2 to 2.5 parts by mass, and even more preferably 0.3 to 2 parts by mass, based on 100 parts by mass of the total of (A) polybutylene terephthalate resin and (B) rubber-reinforced polystyrene or polystyrene. If it is less than 0.1 part by mass, the surface properties tend to deteriorate due to poor release during melt molding, while if it exceeds 3 parts by mass, the workability of kneading the resin composition tends to deteriorate and the surface of the molded product tends to become cloudy.
[0088] [Carbon black] The thermoplastic resin composition of the present invention preferably contains carbon black. The carbon black is not limited in type, raw material, or production method, and any of furnace black, channel black, acetylene black, ketjen black, etc. is usable. There is no particular limit to the number average particle size, but it is preferably about 5 to 60 nm.
[0089] The carbon black is preferably blended in advance with a thermoplastic resin, preferably a polyalkylene terephthalate resin, particularly a polybutylene terephthalate resin, as a master batch.
[0090] The carbon black content is preferably 0.1 to 4 parts by mass, more preferably 0.2 to 3 parts by mass, based on 100 parts by mass of the total of (A) polybutylene terephthalate resin and (B) rubber-reinforced polystyrene or polystyrene. If it is 0.1 part by mass or more, the effect of obtaining the desired color is enhanced, and the effect of improving weather resistance can be expected. If it is 4 parts by mass or less, the deterioration of mechanical properties can be suppressed.
[0091] [Other ingredients] The thermoplastic resin composition of the present invention may contain other thermoplastic resins than the above-mentioned (A) polybutylene terephthalate resin, (B) rubber-reinforced polystyrene or polystyrene, and (E) polycarbonate resin, within a range that does not impair the effects of the present invention. Specific examples of other thermoplastic resins include polyacetal resins, polyamide resins, polyphenylene oxide resins, polyphenylene sulfide resins, polysulfone resins, polyethersulfone resins, polyetherimide resins, polyetherketone resins, and polyolefin resins. However, when other resins are contained, the content is preferably 20 parts by mass or less per 100 parts by mass of the total of (A) polybutylene terephthalate resin and (B) rubber-reinforced polystyrene or polystyrene, more preferably 10 parts by mass or less, even more preferably 5 parts by mass or less, and particularly preferably 3 parts by mass or less.
[0092] The thermoplastic resin composition of the present invention may contain various additives other than those described above. Examples of such additives include flame retardants, flame retardant assistants, anti-dripping agents, ultraviolet absorbers, antistatic agents, anti-fogging agents, anti-blocking agents, plasticizers, dispersants, antibacterial agents, colorants, and dyes and pigments.
[0093] [Production of thermoplastic resin composition] The thermoplastic resin composition of the present invention can be produced according to a conventional method for preparing a resin composition. That is, (A) polybutylene terephthalate resin, (B) rubber-reinforced polystyrene or polystyrene, and (C) elastomer, excluding (D) glass fiber, as well as other resin components and various additives added as desired, are mixed together thoroughly and then melt-kneaded in a single-screw or twin-screw extruder. It is also possible to prepare a resin composition by not mixing each component in advance, or by mixing only a part of each component in advance, feeding the components to an extruder using a feeder, and melt-kneading the components. It is also possible to blend a part of the components in a master batch form and melt-knead the mixture. Furthermore, it is also possible to feed a mixture in which each component is mixed in advance to a molding machine such as an injection molding machine without melt-kneading the mixture, and produce various molded bodies. It is preferable to side-feed (D) glass fiber using a side feeder.
[0094] The heating temperature during melt kneading can usually be appropriately selected from the range of 220 to 300°C. If the temperature is too high, decomposition gas is likely to be generated, which may cause poor appearance. Therefore, it is desirable to select a screw configuration that takes into consideration shear heat generation, etc. In order to suppress decomposition during kneading and molding in the subsequent process, it is desirable to use an antioxidant or heat stabilizer.
[0095] [Molded body] The method for producing a molded article using the thermoplastic resin composition of the present invention is not particularly limited, and any molding method generally used for thermoplastic resin compositions can be used. Examples include injection molding, ultra-high speed injection molding, injection compression molding, two-color molding, gas-assisted hollow molding, molding using a heat-insulating mold, molding using a rapid heating mold, foam molding (including supercritical fluid), insert molding, IMC (in-mold coating molding) molding, extrusion molding, sheet molding, thermoforming, rotational molding, lamination molding, press molding, blow molding, etc. Among these, injection molding and insert molding are particularly preferred, and are particularly suitable for insert molding in which a metal member is inserted.
[0096] The obtained molded article has low warpage, excellent heat shock resistance, and heat resistance, and is excellent in mechanical strength and chemical resistance, and is therefore suitable for use as electrical and electronic equipment parts, interior and exterior parts for automobiles, and other electrical equipment parts for which these properties are strictly required. Specific examples of electrical and electronic equipment parts include housing parts for induction cookers, button cases, grill handles, coil peripheral members, rice cooker protective frames, relay cases, smart meter housings, industrial breaker housings, inverter cases, mobile phone housings, heating equipment housings, battery separators, battery cases, electronic component transport trays, battery transport trays, and automotive charging equipment. As for interior and exterior parts for automobiles, they can be particularly suitably used for on-board housing parts, on-board battery cases, on-board battery covers, on-board battery separators, various motor cases, sensor cases, camera cases, holder parts, air conditioner air direction control plates, door mirror stays, housings for head-up displays installed inside automobiles, housings for engine control units (ECUs), and electrical connector parts for automobiles. In particular, since the polyester resin composition of the present invention has high heat shock resistance, it is suitable as a molded product with a metal member inserted therein, such as an insert molded product such as an electrical appliance part, an in-vehicle electrical equipment part, or an in-vehicle housing part. EXAMPLES
[0097] The present invention will be described in more detail below with reference to examples, but the present invention should not be construed as being limited to the following examples.
[0098] (Examples 1 to 4, Comparative Examples 1 to 5) The components used are as shown in Table 1 below.
[0099] [Table 1]
[0100] Of the components shown in Table 1 above, the components except for (D) glass fiber were uniformly mixed in a tumbler mixer in the ratios shown in Table 2 below (all parts by mass). The resin composition was then melt-kneaded using a twin-screw extruder ("TEX30α" manufactured by The Japan Steel Works, Ltd., L / D=42) while feeding (D) glass fiber using a side feeder under conditions of a cylinder set temperature of 260°C, a discharge rate of 40 kg / h, and a screw rotation speed of 200 rpm. The resin composition was then quenched in a water tank and pelletized using a pelletizer to obtain pellets of a thermoplastic resin composition.
[0101] [Tensile strength at break, tensile elongation at break] The pellets obtained above were dried at 120°C for 5 hours, and then injection molded into ISO multipurpose test pieces (4 mm thick) using an injection molding machine manufactured by Japan Steel Works (clamping force 85T) under conditions of a cylinder temperature of 250°C and a mold temperature of 80°C. In accordance with ISO527, the tensile breaking strength (unit: MPa) and tensile breaking elongation (unit: %) were measured using the above-mentioned ISO multipurpose test piece (4 mm thick). [Maximum bending strength, bending modulus] In accordance with ISO178, the maximum bending strength (unit: MPa) and bending modulus (unit: MPa) were measured at a temperature of 23°C using the above ISO multipurpose test piece (4 mm thick). [Notched Charpy impact strength] In accordance with ISO179, the notched Charpy impact strength (unit: kJ / m) was measured at 23°C for the above ISO multipurpose test piece (4mm thick) with a notch. 2 ) was measured.
[0102] [Heat shock resistance] After drying the obtained pellets at 120°C for 6 hours, a rectangular parallelepiped iron (SUS) insert 1 (length 16mm x width 33mm x thickness 3mm) shown in Figure 1 was inserted into the mold cavity 4 with a support pin 2 as shown in Figure 2 using a Nissei Plastic Industrial Co., Ltd. TH60 R5VSE vertical injection molding machine at a cylinder temperature of 250°C and a mold temperature of 80°C (inserted iron piece 3). An insert molded product (length 18mm x width 35mm x thickness 5mm) shown in Figure 3 was produced by insert molding. The thickness of the resin part of this insert molded product is 1mm. Two weld lines 6 are generated at the support pin marks 5 in the insert molded product. A heat shock test was performed using this insert molded product with a heat shock tester TSA-102ES made by ESPEC. The heat shock test conditions were a cycle of -40°C for 60 minutes followed by 150°C for 60 minutes. The minimum and average number of cycles (number of cycles) at which cracks occurred at the weld lines in a total of 10 locations on the five molded products were indicated. From the minimum and average number of cycles obtained above, the heat shock resistance was evaluated and judged according to the following criteria. ◎: The minimum number of cycles is 200 or more. 〇: The minimum number of cycles is between 50 and 200, and the average number is 200 or more. ×: None of the above criteria are met
[0103] [Deflection temperature under load and heat resistance assessment] Using the above ISO multipurpose test piece (4 mm thick), the deflection temperature under load was measured under a load of 1.80 MPa in accordance with ISO75-1 and ISO75-2. The heat resistance was judged according to the following criteria. ○: Deflection temperature under load is 150℃ or higher ×: Deflection temperature under load is less than 150℃
[0104] [Warpage amount and warpage judgment] Using an injection molding machine (Nissei Plastic Industrial Co., Ltd.'s "NEX80"), a cylinder temperature of 260°C, a mold temperature of 80°C, and an injection time of 0.5 seconds, a disk with a diameter of 100 mm and a thickness of 1.6 mm was molded using a side gate mold, and the amount of warping of the disk (unit: mm) was measured. The warpage was evaluated according to the following criteria. ◎: Warpage is less than 1.0 mm ○: Warpage is 1.0mm to 1.5mm ×: Warpage is over 1.5 mm The results are shown in Table 2 below.
[0105] [Table 2] [Industrial Applicability]
[0106] INDUSTRIAL APPLICABILITY The thermoplastic resin composition of the present invention is excellent in low warpage, heat shock resistance, and heat resistance, as well as in mechanical strength, chemical resistance, and flame retardancy, and can therefore be suitably used for electrical appliance parts, in-vehicle electrical parts, in-vehicle housing parts, and the like, which are strictly required to have these properties.
Claims
1. The composition contains 12 to 35 parts by mass of (C) an elastomer and 5 to 150 parts by mass of (D) glass fiber relative to a total of 100 parts by mass of 15 to 50 parts by mass of (A) a polybutylene terephthalate resin having an intrinsic viscosity of 0.3 to 0.8 dl / g and 50 to 85 parts by mass of (B) a rubber-reinforced polystyrene or polystyrene, the elastomer (C) containing an epoxy group-containing olefin-based elastomer or an epoxy group-containing acrylic-based elastomer, and the rubber-reinforced polystyrene or polystyrene has a viscosity of 250° C., 912 sec. -1 The thermoplastic resin composition has a melt viscosity in the range of 70 to 300 Pa·s.
2. The thermoplastic resin composition according to claim 1, wherein the elastomer (C) further comprises a styrene-based elastomer (C-2).
3. The thermoplastic resin composition according to claim 2, wherein the mass average molecular weight of the styrene-based elastomer (C-2) is 150,000 to 500,000.
4. The thermoplastic resin composition according to claim 2 or 3, wherein the mass ratio (C-1) / (C-2) of the contents of (C-1) and (C-2) is 0.2 or more.
5. The thermoplastic resin composition according to any one of claims 1 to 4, further comprising 1 to 30 parts by mass of a polycarbonate resin (E) per 100 parts by mass of the total of (A) and (B).
6. The thermoplastic resin composition according to any one of claims 1 to 5, wherein the epoxy group-containing olefin-based elastomer (C-1) or the epoxy group-containing acrylic elastomer is obtained by copolymerizing glycidyl methacrylate and contains 3 to 15 mass% of a structural unit derived from glycidyl methacrylate.
7. A molded article made of the thermoplastic resin composition according to any one of claims 1 to 6.
8. 8. The molded product according to claim 7, which is a molded product having a metal insert.
9. 9. The molded product according to claim 7, which is an in-vehicle housing part.
Citation Information
Patent Citations
Resin composition for molding
JP1996259772A
Resin composition and molding
JP2003206396A
Glass fiber reinforced polyester resin composition and molding
JP2006016559A
Polybutylene terephthalate resin composition
JP2006111693A
Hydrolysis-resistant polyester resin composition weldable by laser