Substrate with resin molded body and method for producing substrate with resin molded body
The method of cold press molding with grooves and warpage suppressing sections addresses the high costs and warping issues in existing base material manufacturing by balancing thermal stresses, achieving a cost-effective and warp-resistant vehicle interior component.
Patent Information
- Application Number
- JP2021074155
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-04-26
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2041-04-26
AI Technical Summary
The existing methods for manufacturing vehicle interior base materials with plant fibers and resins require multiple heat treatments, leading to increased processing costs and cycle times, and result in warping due to thermal shrinkage mismatch between the resin and fiber components.
A method for manufacturing a base material with a resin molded body that involves cold press molding without reheating, using a configuration with grooves and warpage suppressing sections filled with thermoplastic resin to balance compressive stresses and reduce warping, by providing a resin molded body on one surface and a warpage suppressing portion on the other.
This approach reduces the number of heat treatments, lowers manufacturing costs, and effectively suppresses warping by balancing thermal contraction stresses, resulting in a durable and cost-effective base material.
Smart Images

Figure 0007582047000001 
Figure 0007582047000002 
Figure 0007582047000003
Abstract
Description
[Technical field]
[0001] The technology disclosed in this specification relates to a substrate having a resin molded body and a method for producing a substrate having a resin molded body. [Background technology]
[0002] Conventionally, substrates containing plant-based fibers and resins have been used as substrates for vehicle interiors. For example, Patent Document 1 discloses that a flat pre-board is prepared in advance by blending plant-based fibers and resin fibers and heat-molding them, and that the pre-board is reheated and cold-press molded at the required timing to give it a desired shape. It also discloses that a resin molded product is integrally provided on the substrate by subsequently subjecting the cold-press molded substrate to injection molding. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-157603 A Summary of the Invention [Problem to be solved by the invention]
[0004] In the manufacturing method of the substrate in Patent Document 1, the heat treatment is performed twice, when the pre-board is made and when the substrate is molded, which increases the processing cost and the cycle time, resulting in a problem of high manufacturing costs. Furthermore, in cold press molding, in addition to the press molding machine, it is necessary to have a means for reheating the pre-board, which also creates restrictions in terms of manufacturing equipment.
[0005] In order to solve such problems, it is conceivable to perform cold press molding without heating. Here, when the pre-board is reheated and cold press molding is performed, the resin in the pre-board is in a softened state, so that the pre-board can absorb and mitigate the shrinkage caused by solidification of the integrally injection-molded resin molding. However, when cold press molding is performed without reheating the pre-board, if the injection-molded resin molding shrinks on the surface of the substrate, a compressive stress is generated along the surface of the substrate, and a new problem occurs in that the substrate is warped.
[0006] The technology disclosed herein was developed based on the above circumstances, and aims to produce a substrate with a resin molding while reducing the number of heat treatments and suppressing warping. [Means for solving the problem]
[0007] The substrate with resin molding according to the technology disclosed herein comprises a plate-shaped substrate including fibers and a first thermoplastic resin and having a first surface and a second surface opposite the first surface, and a resin molding provided on the second surface of the substrate and extending along a first direction, wherein the first surface of the substrate is provided with a groove extending along the first direction, and the groove is provided with a warp suppression portion formed by filling the groove with a second thermoplastic resin.
[0008] The thermoplastic resin constituting the resin molded body generally undergoes thermal shrinkage when transformed from a molten state to a solidified state, and the thermal shrinkage rate is greater than that of a substrate in which fibers are solidified with a thermoplastic resin binder. Therefore, when the resin molded body is integrally formed with the substrate, if the substrate is also heated to integrally form the resin molded body, the warping of the substrate caused by the difference in thermal shrinkage rate can be alleviated. On the other hand, if the resin molded body is integrally formed without heating the substrate, the warping of the substrate caused by the difference in thermal shrinkage rate becomes noticeable. Therefore, according to the above configuration, a resin molded body is provided on one side of the substrate, and a warping suppressing portion is provided on the other side so as to follow the resin molded body. As a result, the compressive stress caused by the thermal shrinkage of the resin molded body and the compressive stress caused by the warping suppressing portion are balanced on the front and back plate surfaces of the substrate, and the warping of the substrate is suppressed.
[0009] In a preferred embodiment of the present technology, the warp suppression portion is provided at a position overlapping the resin molded body. According to the above configuration, a compressive stress acting on the first surface of the base material due to the resin molded body can be effectively offset by a compressive stress acting on the second surface of the base material due to the warp suppression portion.
[0010] In a preferred embodiment of the present technology, the groove includes a first groove and a second groove provided to sandwich the resin molded body in a second direction intersecting the first direction, and the warp suppressing portion includes a first warp suppressing portion and a second warp suppressing portion formed by filling the first groove and the second groove with the second thermoplastic resin. With the above configuration, it is possible to suppress a compressive stress caused by thermal contraction of the thermoplastic resin from acting locally on the base material.
[0011] In a preferred embodiment of the present technology, a cross-sectional area S1 of the warp suppression portion in a second direction intersecting with the first direction satisfies the following relationship with respect to a cross-sectional area S2 of the resin molded body in the second direction: 0.5×S2≦S1≦1.5×S2. With the above configuration, it is possible to effectively balance a compressive stress acting on the second surface of the base material due to the resin molded body and a compressive stress acting on the first surface of the base material due to the warp suppression portion.
[0012] In a preferred embodiment of the present technology, a dimension W1 of the warp suppression portion along a second direction intersecting with the first direction satisfies the following relationship with respect to a dimension W2 of the resin molded body along the second direction: 0.8×W2≦W1≦1.2×W2. According to the above configuration, when the height of the resin molded body from the plate surface of the base material is large, it is possible to effectively balance the compressive stress acting on the second surface of the base material due to the resin molded body and the compressive stress acting on the first surface of the base material due to the warp suppression portion.
[0013] In a preferred embodiment of the present technology, the dimension of the warp suppressing portion in the thickness direction of the base material is 50% or less of the thickness of the base material. With the above configuration, it is possible to suppress warping of the base material while avoiding a decrease in strength of the base material due to the provision of the warp suppressing portion.
[0014] In a preferred embodiment of the present technology, the base material includes a through hole penetrating the base material, and a continuous portion filled with the second thermoplastic resin is provided inside the through hole, and the resin molded body and the warp suppressing portion are continuous via the continuous portion. According to the above configuration, the base material can be easily manufactured, and can be provided as, for example, a low-cost base material.
[0015] In a preferred embodiment of the present technology, the substrate has a bent portion bent so that the first surface protrudes, the bent portion is continuous with the groove, and a corner portion continuous with the first surface of the bent portion is provided with a filling portion filled with the second thermoplastic resin. When the substrate is bent without heating, the substrate is bent without flexibility, and therefore the substrate may be torn on the outer surface of the bent portion, resulting in loss of surface smoothness or the substrate may become thin and lose strength. According to the above configuration, the bent portion has a resin portion continuous with the warp suppression portion, so that the resin portion can smooth the surface of the substrate and even out the plate thickness. This makes it possible to provide substrates of various shapes.
[0016] In another aspect, a method for manufacturing a substrate with a resin molding according to the technology disclosed herein includes a preparation step of preparing a substrate having a plate-like substrate comprising fibers and a first thermoplastic resin, the substrate comprising a first surface and a second surface opposite the first surface, the substrate having a groove extending in the first direction on the first surface so as to follow a resin molding extending in the first direction that is to be provided on the second surface; and a resin supply step of supplying a second thermoplastic resin for forming the resin molding on the second surface of the substrate at a temperature at which the first thermoplastic resin does not melt, and supplying a third thermoplastic resin into the groove on the first surface, thereby obtaining a substrate with a resin molding having a warp suppressing portion that has the resin molding on the second surface and in which the groove on the first surface is filled with the third thermoplastic resin.
[0017] According to the above-mentioned configuration, by forming a resin molded body on one surface of the substrate and providing a warp suppressing section on the other surface of the substrate so as to fit the resin molded body, a substrate with a resin molded body can be manufactured without heating the substrate. This makes it possible to balance the compressive stress caused by the thermal contraction of the thermoplastic resin and the compressive stress caused by the warp suppressing section on the front and back plate surfaces of the substrate, and a substrate with a resin molded body with warp suppressed can be manufactured without heating and without significantly increasing the number of steps.
[0018] In a preferred embodiment of the present technology, the preparation step includes a preboard preparation step of preparing a plate-shaped preboard without grooves, which includes the fiber and the first thermoplastic resin and has the first surface and the second surface but does not have the grooves, and a groove forming step of providing the grooves on the second surface of the preboard without grooves. The substrate in the present technology may be obtained with grooves formed in advance, or a preboard without grooves may be prepared and grooves may be formed in it. Here, a substrate with grooves formed in advance has the disadvantages of limited use and difficulty in responding to design changes in a short period of time. According to the above configuration, for example, the substrate disclosed herein can be manufactured using a preboard with no limited use.
[0019] In a preferred embodiment of the present technology, the second thermoplastic resin and the third thermoplastic resin are the same, and the preparation step includes a preboard preparation step of preparing a plate-shaped grooveless preboard that includes the fiber and the first thermoplastic resin and has the first surface and the second surface but does not include the groove, and a communication step of providing a through hole penetrating the preboard and making a cut to communicate the through hole with the groove, and in the resin supply step, the second thermoplastic resin for forming the resin molded body is supplied to the second surface of the preboard, and the second thermoplastic resin is fed to the first surface through the through hole and supplied to the groove. According to the above configuration, since the preboard has a through hole, by supplying the second thermoplastic resin to one surface, the second thermoplastic resin can be fed to the other surface through the through hole. This makes it possible to simplify the substrate manufacturing device and manufacture the substrate.
[0020] In a preferred embodiment of the present technology, the preparation step includes a preboard preparation step of preparing a plate-shaped grooveless preboard that includes the fiber and the first thermoplastic resin and has the first surface and the second surface but does not include the groove, a cutting step of making a cut at a predetermined position on the first surface of the preboard, and a press molding step of pressing the preboard with a molding surface of a mold at a temperature at which the first thermoplastic resin does not melt so as to bend the preboard along the cut and in a manner such that the first surface protrudes, thereby forming the cutout portion formed by opening the cutout, and in the resin supply step, the second thermoplastic resin is filled into the cutout portion. According to the above configuration, press molding of the substrate is also performed, and the defective shape of the substrate caused by press molding without heating is compensated for by filling the thermoplastic resin in the resin supply step. This makes it possible to efficiently manufacture substrates of various shapes without heating. Effect of the Invention
[0021] According to the technology disclosed in this specification, it is possible to produce a substrate with a resin molded body while reducing the number of heat treatments and suppressing warping. [Brief description of the drawings]
[0022] [Figure 1] FIG. 1 is a perspective view of a seat back board according to an embodiment, viewed from the front side; [Diagram 2] FIG. 2 is a plan view of the seat back board of FIG. 1 viewed from the back side. [Diagram 3] A cross-sectional view showing the state where a pre-board without grooves is pressed by a press die. [Figure 4] A perspective view of the pre-board from the front [Diagram 5] Cross-sectional view of the mold with the pre-board set (open state) [Figure 6] Cross-sectional view of the main part when the pre-board is set in the mold (open state) [Figure 7] Cross-sectional view including the groove when the pre-board is set in the mold (open state) [Figure 8] Cross-sectional view of the main part when the pre-board is pressed in the mold (closed state) [Figure 9] Another cross-sectional view of the main part showing the state where the pre-board is set in the forming mold and the slide mold is in the protruding state (closed state) [Figure 10] Cross-sectional view of the main part including the groove when the pre-board is set in the mold (closed state) [Figure 11] Another cross-sectional view of the main part showing the state in which the pre-board is set in the forming mold and the slide mold is moved to the retracted state (closed state) [Figure 12] FIG. 9 is a cross-sectional view of the main part of the mold shown in FIG. 8 after resin is injected into the mold (closed state). [Figure 13] FIG. 10 is another cross-sectional view of the main part (closed state) showing the state after the resin is injected into the molding die of FIG. [Figure 14] 11 is a cross-sectional view of the main part including the groove after the resin is injected into the mold of FIG. 10 (closed state). [Figure 15] FIG. 12 is a cross-sectional view (open state) showing a state in which the molding device is opened from the state shown in FIG. 11 to complete the seat back board. [Figure 16]FIG. 13 is a cross-sectional view of a main part showing a state in which the molding device is opened from the state shown in FIG. 12 to complete the seat back board (open state). [Figure 17] FIG. 14 is a cross-sectional view including the groove in a state where the molding device is opened from the state shown in FIG. 13 to complete the seat back board (open state). [Figure 18] FIG. 13 is a cross-sectional view of a main portion of a seat back board according to another embodiment of the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] <Embodiment 1> An embodiment of the present technology will be described with reference to Fig. 1 to Fig. 17. The substrate with a resin molded body and the manufacturing method of the substrate with a resin molded body of the present embodiment are preferably applied to a seat backboard 1 (one example of a substrate with a resin molded body) constituting a vehicle seat such as an automobile and its manufacturing. More specifically, the vehicle seat includes a seat cushion on which an occupant sits and a seat back which is a backrest portion, and the seat backboard 1 is a relatively hard and flat portion constituting the rear surface of the seat back. For example, when the seat back is folded down onto the seat surface, the seat backboard 1 becomes a flat and sturdy luggage platform or floor, etc., and heavy luggage and the like can be placed on it without hesitation.
[0024] In addition, an X-axis, a Y-axis, and a Z-axis are shown in a part of each drawing, and the X-axis and the Y-axis indicate two mutually intersecting directions along the surface of the seat back board 1, and the Z-axis corresponds to the thickness direction of the seat back board 1. In this embodiment, the X-axis, the Y-axis, and the Z-axis are perpendicular to each other. In addition, the upper side in FIG. 1 is the front side, and the lower side in the same drawing is the back side, and the direction along the X-axis corresponds to the first direction in this technology, and the direction along the Y-axis corresponds to the second direction in this technology. In the case of multiple identical parts, a reference symbol is attached to one part, and the reference symbol is omitted for the other parts.
[0025] <Seat back board> As shown in Figures 1 and 2, the seat back board 1 has a generally rectangular shallow dish shape as a whole. The seat back board 1 includes a base material 10 and a resin part 20 provided at a predetermined portion of the base material 10. The resin part 20 includes a resin molded body 21, a warp suppressing part 24, a filling part 27, and a resin corner part 28. Each part will be described below.
[0026] The base material 10 constitutes the main body of the seat backboard 1, and contains a binder made of fibers and a first thermoplastic resin. The fibers are bound by the first thermoplastic resin as a binder and integrated into a plate shape. Kenaf fibers can be used as the fibers contained in the base material 10. The type of fiber is not limited to this, and may be, for example, wood fibers, thermoplastic resin fibers, glass fibers, carbon fibers, etc. Any one of these may be used, or two or more may be used in combination. The first thermoplastic resin as a binder may have a higher softening point or melting point than the second thermoplastic resin described later. In addition, when the fibers are thermoplastic resin fibers, the thermoplastic resin fibers may have a higher softening point or melting point than the first thermoplastic resin and the second thermoplastic resin. Such a first thermoplastic resin may be, for example, a polyester-based resin such as polyethylene or polypropylene. The first thermoplastic resin may be partially or entirely fibrous. The ratio of the fibers to the first thermoplastic resin as a binder can be, for example, about 20:80 to 90:10, or about 50:50 to 80:20, in terms of the mass ratio of fibers:binder.
[0027] The base material 10 has roughly the same external shape as the seat back board 1. The base material 10 has a front surface 10A (an example of a first surface) arranged on the front side and a back surface 10B (an example of a second surface) arranged on the back side. As will be described in detail later, the base material 10 is formed by folding side walls 13P provided on the four peripheries of a flat pre-board 10P having a shape as shown in FIG. 4 when unfolded toward the back side. The base material 10 includes a flat main surface portion 11 constituting a design surface (front surface) arranged on the front side, a groove 12 provided in the main surface portion 11, a side wall portion 13 extending from the periphery of the main surface portion 11 toward the back side, a bent portion 14 connecting the main surface portion 11 and the side wall portion 13, and a through hole 16. The through hole 16 is an element additionally provided in this embodiment.
[0028] The main surface portion 11 is a substantially rectangular flat plate with rounded corners. The side wall portion 13 is a plate-like piece, and is provided so as to extend toward the back side at the four ends of the main surface portion 11 excluding the rounded corners (hereinafter referred to as "rounded corners"). Although not limited to this, the side wall portion 13 in this example is arranged so as to be substantially perpendicular to the main surface portion 11. The bent portion 14 is arranged between the main surface portion 11 and the side wall portion 13, and is a curved portion that smoothly connects the main surface portion 11 and the side wall portion 13. The bent portion 14 includes a notch portion 15 that is opened by bending a notch portion 15P described later provided on the front surface 10A of the preboard 10P. This notch portion 15 is thinner than the main surface portion 11 and the side wall portion 13.
[0029] The groove 12 is a concave groove provided on the surface of the main surface portion 11. The groove 12 in this example has a U-shaped cross section. The groove 12 is a mold for forming and accommodating the warpage suppression portion 24. The groove 12 extends generally along the arrangement direction of the resin molded body 21 provided on the back surface of the main surface portion 11. In this example, the grooves 12 are provided in two parts, a first groove 12A and a second groove 12B, parallel and spaced apart along the first direction so as to sandwich the resin molded body 21 extending along the first direction in the second direction. In addition, in this example, the grooves 12 are provided in two parts, a third groove 12C and a fourth groove 12D, parallel and spaced apart along the second direction so as to sandwich the resin molded body 21 extending along the second direction in the first direction.
[0030] The through hole 16 is a hole that penetrates the base material 10 and communicates between the front surface 10A and the back surface 10B. The through hole 16 is provided at a position overlapping at least one of the warp suppressing portion 24 and the compensation portion 27 so as to connect the resin molding 21 provided on the back surface 10B to the warp suppressing portion 24 and the compensation portion 27 provided on the front surface 10A. In this example, the through hole 16 is provided at a point where the resin molding 21 and the compensation portion 27 overlap. More specifically, the through hole 16 is provided at both ends of two first runner portions 23A, 23B (resin moldings 21) described later, at points where the through hole 16 overlaps with each of the four compensation portions 27 (the central portions in the longitudinal direction of each compensation portion 27).
[0031] Therefore, the pre-board 10P has a shape in which the main surface portion 11, the side wall portion 13, and the bent portion 14 are developed into a single flat plate. The pre-board 10P has a front surface 10AP (an example of a first surface) arranged on the front side, and a back surface 10BP (an example of a second surface) arranged on the back side. The pre-board 10P includes a main surface portion 11P corresponding to the main surface portion 11, a side wall portion 13P corresponding to the side wall portion 13, and a bent portion 14P corresponding to the bent portion 14 provided between the main surface portion 11P and the side wall portion 13P. The bent portion 14P is provided with a notch portion 15P corresponding to the notch portion 15. The notch portion 15P is formed as a V-groove having a V-shaped cross section on the front surface 10A of the bent portion 14P. A through hole 16P corresponding to the through hole 16 is provided in the central portion along the longitudinal direction of the four notch portions 15P. Further, the main surface portion 11P of the pre-board 10P is provided with grooves 12P (first groove 12AP to fourth groove 12DP) corresponding to the grooves 12 (first groove 12A to fourth groove 12D). The pre-board 10P is formed by forming the rounded corners of the main surface portion 11P and the side wall portions 13P of the pre-board, and removing the remaining portions (for example, by die-cutting) at the four corners of the approximately rectangular flat pre-board that is slightly larger than the main surface portion 11P. Since the pre-board 10P of this example is a stampable sheet before being subjected to three-dimensional molding, the dimension in the thickness direction of each portion can be larger than that of the base material 10 by the amount of compression ratio, and the density of each portion can be smaller than that of the base material 10 by the amount of compression ratio.
[0032] The resin part 20 is integrally formed with the base material 10. A part of the resin part 20 may be impregnated into the base material 10. As described above, the resin part 20 includes the resin molded body 21 provided on the back surface of the base material 10, the warp suppressing part 24 and the filling part 27 provided on the front surface of the base material 10, and the resin corner part 28 that smoothly connects between the four side wall parts 13 and the main surface part 11. The resin molded body 21 includes a clip seat 22, first runner parts 23A, 23B, a second runner part 23C, and a rib part 23D. These resin molded bodies 21 are formed of a thermoplastic resin (second thermoplastic resin) such as polypropylene.
[0033] The clip seat 22 is formed so as to protrude from the back surface 10B of the main surface portion 11 of the base material 10. In this example, for the sake of simplicity, one clip seat 22 is provided at the center of the main surface portion 11, but two or more clip seats 22 may be provided. The clip seat 22 is substantially cylindrical with a lid, and a clip (not shown) is fitted in a hole provided in the lid so as to protrude toward the back side. The clip seat 22 is formed by cooling and hardening molten resin filled in a cavity C2 for forming a clip seat provided in a molding die 50 (lower die 61) described later.
[0034] The rib portion 23D is a plurality of plate-shaped members connected to the main surface portion 11 and the side wall portion 13. The rib portion 23D is an element that bonds the side wall portion 13 to the main surface portion 11 and supports the attitude of the side wall portion 13 relative to the main surface portion 11. The rib portion 23D can be an element that assists the joining of the side wall portion 13 to the main surface portion 11 with a predetermined strength. The rib portion 23D is formed by cooling and hardening molten resin filled in a cavity C3 for forming the rib portion provided in a molding die 50 (lower die 61) described later.
[0035] The first runner portions 23A, 23B and the second runner portion 23C are formed by cooling and hardening the molten resin filled in the first runner 64 and the second runner 65 provided in the molding die 50 (lower die 61). Here, the first runner 64 and the second runner 65 are flow paths for sending the molten resin to the cavities C2, C3 for forming the clip seat 22 and the rib portion 23D. The first runner portions 23A, 23B are in the form of upright walls erected against the main surface portion 11, and extend in all four directions in the first and second directions from the clip seat 22 to the side wall portion 13. In this example, the portion extending along the first direction is represented as the first runner portion 23A, and the portion extending along the second direction is represented as the first runner portion 23B. The second runners are arranged along each of the joints between the main surface portion 11 and the four side wall portions 13, and are connected to both the main surface portion 11 and the side wall portions 13, as well as to the first runner portions 23A, 23B and the multiple rib portions 23D. The first runner portions 23A, 23B and the second runner portion 23C are formed to cross the main surface portion 11 along the first direction or the second direction, respectively.
[0036] The warp suppressing portion 24 is an element for reducing the compressive stress acting on the surface of the main surface portion 11 due to the manufacturing of the resin molded body 21 and suppressing the warp of the base material 10. In this example, the warp suppressing portion 24 is provided to suppress the warp caused by the first runner portions 23A, 23B of the resin molded body 21, which have a large dimension along the surface direction of the main surface portion 11. The warp suppressing portion 24 is formed by cooling and hardening the molten resin filled in the first groove 12A to the fourth groove 12D. The warp suppressing portion 24 is formed so that the surface of the main surface portion 11 recessed by the first groove 12A to the fourth groove 12D becomes flush. In this example, the warp suppressing portion 24 is provided in parallel along the first direction with a space therebetween, i.e., the first warp suppressing portion 24A and the second warp suppressing portion 24B, so as to sandwich the first runner portion 23A extending along the first direction in the second direction. In this example, the warp suppressing portion 24 includes a third warp suppressing portion 24C and a fourth warp suppressing portion 24D that are provided parallel to each other and spaced apart from each other along the second direction so as to sandwich the first runner portion 23B extending along the second direction in the first direction. The warp suppressing portion 24 is preferably provided over the range in which the first runner portions 23A and 23B extend.
[0037] Regarding the shape of the warp suppressing portion 24, for example, the cross-sectional area S1 (total value) of the first warp suppressing portion 24A and the second warp suppressing portion 24B along the second direction may satisfy the following relationship with the cross-sectional area S2 of the first runner portion 23A along the second direction: 0.5×S2≦S1≦1.5×S2;. Independently, the cross-sectional area S1 (total value) of the third warp suppressing portion 24C and the fourth warp suppressing portion 24D along the first direction may satisfy the following relationship with the cross-sectional area S2 of the first runner portion 23B along the first direction: 0.5×S2≦S1≦1.5×S2;. This allows the warp of the base material 10 caused by the first runner portions 23A and 23B to be suitably balanced with the warp suppressing force by the warp suppressing portions 24A, 24B, 24C, and 24D. These cross-sectional areas S1 and S2 preferably independently satisfy 0.7×S2≦S1≦1.3×S2, and more preferably satisfy 0.9×S2≦S1≦1.1×S2.
[0038] As for the shape of the warp suppressing portion 24, for example, the dimension W1 of the warp suppressing portion along the second direction intersecting with the first direction may satisfy the following relationship with respect to the dimension W2 of the resin molded body along the second direction: 0.8×W2≦W1≦1.2×W2;. Independently, the dimension W1 (total value) of the third warp suppressing portion 24C and the fourth warp suppressing portion 24D along the first direction may satisfy the following relationship with the dimension W2 of the first runner portion 23B along the first direction: 0.8×W2≦W1≦1.2×W2;. With this configuration, the warp of the base material 10 caused by the first runner portions 23A and 23B can be suitably balanced with the warp suppressing force of the warp suppressing portions 24A, 24B, 24C, and 24D. The dimensions L1 and L2 of the first runner portions 23A and 23B and the warp suppressing portion 24 may be the dimensions of the portions in contact with the base material. Moreover, the dimension of the warp suppressing portion 24 along the thickness direction of the base material 10 is 50% or less of the thickness of the base material 10 (about 20% in this example).
[0039] The filling portion 27 is provided on the surface 10A side of the cutout portion 15. The filling portion 27 is an element for filling the cutout portion 15, which is thinner than the main surface portion 11 and the side wall portion 13, in the bent portion 14, to smoothly connect the surface 10A of the main surface portion 11 and the surface 10A of the side wall portion 13. The filling portion 27 is also an element for increasing the rigidity of the base material 10 and the bonding strength between the main surface portion 11 and the side wall portion 13. The filling portion 27 in this example is formed so that its cross-sectional shape is a sector shape. The filling portion 27 is formed by cooling and hardening the molten resin filled in the portion (cavity C4) corresponding to the filling portion in the molding space C1 provided in the molding die 50 described later. In this example, a through hole 16 is provided at the point where the warp suppressing portion 24 of the base material 10 and the filling portion 27 are bonded (overlapping point). The filling portion 27 includes a portion (continuous portion) where the molten resin filled in the through hole 16 has cooled and hardened.
[0040] The resin corner part 28 is an element that smoothly connects between the four side wall parts 13 and the main surface part 11. The resin corner part 28 continuously connects between adjacent side wall parts 13 with a curved surface substantially perpendicular to the main surface part 11, and is formed to have a sector-shaped cross section and be smoothly continuous between the peripheries of the rounded corner parts of the main surface part 11 and between adjacent bent parts 14. The resin corner part 28 is formed by cooling and hardening the molten resin that is plastically filled in the part (cavity C5) corresponding to the resin corner part in the molding space C1 provided in the molding die 50 described later.
[0041] The above-described warpage suppression part 24, filling part 27, and resin corner part 28 are formed of a thermoplastic resin (third thermoplastic resin) such as polypropylene, for example. In the present embodiment, the thermoplastic resin (second thermoplastic resin) constituting the resin molded body 21 is the same as the thermoplastic resin (third thermoplastic resin) constituting the warpage suppression part 24, filling part 27, and resin corner part 28. When the second thermoplastic resin and the third thermoplastic resin are different, they are preferably compatible. Also, the second thermoplastic resin and the third thermoplastic resin are preferably compatible with the first thermoplastic resin as well.
[0042] The manufacturing method of such a seat back board 1 is not particularly limited, but a preferred manufacturing method of the seat back board 1 will be described below. The manufacturing method of this seat back board 1 generally includes the following steps. Each step will be described in order. S1. Preparation step of preparing a pre-board S1-1. Preparation step of a pre-board without grooves S1-2. Groove forming step S1-3. Communication step · Cutting step S2. Resin supply step S2-1. Cold press step (an example of a press molding step) S2-2. Resin injection step
[0043] <S1. Preparation step of preparing a pre-board> In step S1-1, a preboard without grooves is prepared. The preboard without grooves is a press molding substrate called a stampable sheet, which is made by homogeneously mixing the fibers (here, plant fibers) and thermoplastic resin fibers, which are the raw materials for the substrate, by a wet method (papermaking method) or a dry method (airlaying method) to form a fleece, and then repeatedly poking the fibers with a needle that moves up and down in the thickness direction to entangle the fibers, and then heating the fibers to bond them together. The heating in this step is performed to a temperature equal to or higher than the melting point or softening point of the thermoplastic resin fibers made of the first thermoplastic resin as a binder.
[0044] At this time, the groove-free preboard may be press-molded using a heated press platen as shown in FIG. 3. In the manufacturing method according to the present technology, a cold press without heating is used in the subsequent pressing process. The stampable sheet cannot be compressed to the desired board thickness and base material density by the subsequent cold press without heating using a low clamping force. Therefore, at this preparation process stage where the preboard is prepared, it is formed to have the targeted board thickness and base material density (i.e., a base material density higher than that of conventional preboards).
[0045] In step S1-2, as shown in FIG. 4, a groove 12P is provided in the press molding substrate. In step S1-3, as shown in FIG. 4, a cutout portion 15P and a through hole 16P are provided in the press molding substrate. These steps S1-2 and S1-3 may be performed after step S1-1, or may be performed so as to overlap with step S1-1. In addition, either step S1-2 or step S1-3 may be performed first, or the two may be performed in parallel. For example, the cutout portion 15P can be formed by performing a marking process (an example of a cutting process) on the fleece before the heating in the above step S1-1. In addition, the groove 12P and the through hole 16P can be formed by performing a die cutting process, a cutting process, a laser process, or the like before or after the first thermoplastic resin that has been softened or melted is hardened after the fleece is integrated by heating in the above step S1-1. In this way, a pre-board 10P is prepared.
[0046] <S2. Resin supply process> In step S2-1, the prepared pre-board 10P is cold-pressed by the forming surface of the mold 50 so as to be bent along the notch 15P and with the surface 10A protruding at a temperature at which the first thermoplastic resin does not melt. Thereby, the shape of the base material 10 of the sheet back board 1 is imparted to the pre-board 10P. At this time, the notch 15P is opened and the bent portion 14 is formed.
[0047] In cold pressing, for example, as shown in FIG. 5, it is preferable to use a base material manufacturing apparatus 40 including a mold 50 capable of performing cold pressing and resin injection molding simultaneously. The base material manufacturing apparatus 40 may be installed in an environment not provided with a heating device for heating the pre-board 10P which is an object to be molded around it. The base material manufacturing apparatus 40 includes, as shown in FIG. 5, an injection device 41 and a mold 50. The mold 50 includes an upper mold 51 which is a movable mold and a lower mold 61 which is a fixed mold. The injection device 41 is, for example, of a screw type and is provided in the lower mold 61 in the present embodiment.
[0048] The upper mold 51 is a movable mold that can be moved relative to the lower mold 61 by a driving device (for example, an electric motor, an air cylinder, a hydraulic cylinder, etc.) not shown. By moving the upper mold 51 closer to and away from the lower mold 61, the mold clamping and mold opening of the upper mold 51 and the lower mold 61 are possible.
[0049] The lower die 61 has a shape in which a die surface 61A, which is a surface facing the upper die 51, protrudes toward the upper die 51. The upper die 51 has a shape in which a die surface 51A, which is a surface facing the lower die 61, is recessed corresponding to the shape of the lower die 61. In a closed state in which the upper die 51 and the lower die 61 are closed, a molding space C1 corresponding to the outer shape of the target seat backboard 1 is formed between the upper die 51 and the lower die 61. That is, in a closed state, the die surface 51A and the die surface 61A are disposed opposite to each other with a distance equal to the plate thickness of the base material 10 (see FIG. 8, etc.). As a result, when the pre-board 10P is pressed by the upper die 51 and the lower die 61, the pre-board 10P is compressed into a shape corresponding to the shape of the molding space C1, and the base material 10 is molded. The thickness of the base material 10, that is, the distance between the upper die 51 and the lower die 61 in the closed state, is set to be smaller than the thickness of the pre-board 10P in accordance with the compression rate.
[0050] As shown in Figs. 5 to 7, the upper mold 51 includes an upper main mold 53 which is the main body of the upper mold 51, and a slide mold 52 which can be raised and lowered with respect to the upper main mold 53. The slide mold 52 can be displaced between a protruding state in which its mold surface 52A protrudes downward from the mold surface 53A of the upper main mold 53 and a retracted state (see Fig. 11) in which it is flush with the mold surface 53A of the upper main mold 53. The slide mold 52 in this example is formed by combining a plurality of elongated plate pieces, and in the protruding state, it is provided at a position corresponding to the groove 12P of the pre-board 10P, and can position the pre-board 10P with respect to the lower mold 61. The width (thickness of the plate piece) of the slide mold 52 is set to a dimension equal to or slightly smaller than the width of the groove 12P. When the pre-board 10P is placed on the lower mold 61 and the slide mold 52 is inserted into the groove 12P, a large gap is not created between the slide mold 52 and the groove 12P. On the other hand, when the slide mold 52 is inserted into the groove 12P in the protruding state and then the slide mold 52 is retracted, a cavity C6 (see FIG. 11, etc.) for forming the warp suppression portion 24 is formed between the slide mold 52 and the pre-board 10P.
[0051] In addition, between the molding die 50 in the closed state and the pre-board 10P, a cavity C4 (see FIGS. 8 and 10) for forming the filling portion 27 and a cavity C5 (see FIG. 5) for forming the resin corner portion 28 are formed. The cavities C4 and C5 are included in advance in the molding space C1.
[0052] A cavity C2 for molding the clip seat 22 described above is recessed so as to open to the mold surface 61A of the lower mold 61. The lower mold 61 is provided with a slide mechanism (not shown) for forming the clip seat 22 having an undercut structure.
[0053] In addition, a rib portion forming cavity C3 (see FIG. 5) for molding the rib portion 23D is recessed into the mold surface 61A of the lower mold 61 so as to open to the mold surface 61A. Furthermore, a first runner 64 and a second runner 65 for molding the first runner portions 23A and 23B and the second runner portion 23C are recessed into the mold surface 61A of the lower mold 61 in the form of grooves that open to the mold surface 61A.
[0054] The second runner 65 is provided so as to go around the end (corner) of the portion protruding upward from the lower mold 61. In other words, the second runner 65 extends to a position corresponding to the bent portion 14 of the positioned pre-board 10P. The first runner 64 extends in a direction intersecting the extending direction of the second runner 65 so as to connect between the clip seat molding recess and the second runner 65. The injection device 41 is provided with a gate 42, which is an injection port for injecting resin, so as to communicate with a position of the first runner 64 close to the second runner 65.
[0055] In such a substrate manufacturing apparatus 40, as shown in Figs. 8 to 10, the slide mold 52 is in a protruding state at a temperature at which the first thermoplastic resin does not melt (for example, room temperature (25°C)), and the pre-board 10P is positioned, and then the molding die 50 is closed. By adopting a positioning step in which the slide mold 52 is aligned with the groove 12, it is possible to more reliably suppress misalignment of the pre-board 10P relative to the lower die 61 during molding. As a result, while pressing the main surface portion 11P of the pre-board 10P, the side wall portion 13 can be folded toward the back side along the notch portion 15P and with the front surface 10AP protruding. At this time, the notch portion 15P of the pre-board 10P is opened, and the notch portion 15 is formed. In this example, the substrate 10 with a groove is thus formed.
[0056] In step S2-2, a second thermoplastic resin for forming the resin portion 20 is supplied to the front surface 10A and the back surface 10B of the base material 10. More specifically, as shown in FIG. 11, the molding die 50 is kept in a closed state, and the slide die 52 is in a retreated state. As shown in FIGS. 12 to 14, the injection device 41 injects the second thermoplastic resin in a molten state (hereinafter, referred to as molten resin) into the first runner 64 through the gate 42. This allows the molten resin to be supplied to the back surface 10B first. The molten resin injected into the first runner 64 is supplied to the cavity C2 for forming the clip seat, the cavity C3 for forming the rib portion, and the second runner 65, which are continuous with the first runner 64. Then, the molten resin supplied to the second runner 65 is supplied to the cavity C4 for forming the filling portion, the cavity C6 for forming the warp suppressing portion, and the cavity C5 for forming the resin corner portion through the through hole 16, which is continuous with the second runner 65. This allows the molten resin to be supplied also to the surface 10A.
[0057] The resin supplied to the first runner 64, the second runner 65, the through hole 16, and the cavities C2 to C6 is cooled and hardened, thereby forming the resin molded body 21 (i.e., the clip seat 22, the first runner portions 23A and 23B, the second runner portion 23C, and the rib portion 23D), the warp suppression portion 24, the filling portion 27 (including a continuous portion formed by hardening the molten resin supplied to the through hole 16), and the resin corner portion 28 integrally with the base material 10. Thereafter, as shown in Figs. 15 to 17, the molding die 50 is opened to manufacture the seat backboard 1 having the resin molded body 21 on the back surface 10B and the warp suppression portion 24 on the front surface 10A.
[0058] Next, the effect of this embodiment will be described. In the above embodiment, the seat backboard 1 (base material with resin molding) includes a plate-shaped base material 10 containing fibers and a first thermoplastic resin and having a front surface 10A (first surface) and a back surface 10B (second surface) opposite to the front surface 10A, and a first runner portion 23A (resin molding 21) provided on the back surface 10B of the base material 10 and extending along a first direction, and the front surface 10A of the base material 10 is provided with grooves 12A and 12B extending along the first direction, and the grooves 12A and 12B are provided with warp suppressing portions 24A and 24B formed by filling a second thermoplastic resin into the grooves. In addition, a first runner portion 23B (resin molding 21) is provided on the back surface 10B of the substrate 10 and extends along the second direction, and grooves 12C, 12D are provided on the front surface 10A of the substrate 10, extending along the second direction, and warp suppression portions 24C, 24D are provided in the grooves 12C, 12D by filling them with a second thermoplastic resin.
[0059] The thermoplastic resin constituting the resin molded body 21 generally undergoes thermal shrinkage when transformed from a molten state to a solidified state, and the thermal shrinkage rate is greater than that of the substrate 10. Therefore, when the resin molded body 21 is integrally formed with the substrate 10, if the substrate 10 is also heated to integrally form the resin molded body 21, the warping of the substrate 10 caused by the difference in thermal shrinkage rate can be alleviated, but if the resin molded body 21 is integrally formed without heating the substrate 10, the warping of the substrate 10 caused by the difference in thermal shrinkage rate becomes significant. In particular, the first runner portion 23A extending along the first direction generates a compressive stress along the first direction on the back surface 10B during the cooling and hardening process, and the first runner portion 23B extending along the second direction generates a compressive stress along the second direction on the back surface 10B during the cooling and hardening process. According to the above configuration, the first runner portions 23A, 23B (resin molded body 21) are provided on one surface of the base material 10, and the warp suppressing portions 24A-24D extending in the first and second directions, respectively, are provided on the other surface so as to follow the first runner portions 23A, 23B. As a result, on the front and back plate surfaces of the base material 10, a balance is achieved between the compressive stress caused by the thermal contraction of the resin molded body 21 and the compressive stress caused by the warp suppressing portions 24, thereby suppressing warping of the base material 10.
[0060] In the above embodiment, the groove 12 includes a first groove 12A and a second groove 12B provided to sandwich the first runner portion 23A (resin molded body 21) in a second direction intersecting with the first direction, and the warp suppressing portion 24 includes a first warp suppressing portion 24A and a second warp suppressing portion 24B formed by filling the first groove 12A and the second groove 12B with a second thermoplastic resin. The groove 12 also includes a third groove 12C and a fourth groove 12D provided to sandwich the first runner portion 23B (resin molded body 21) in a first direction intersecting with the second direction, and the warp suppressing portion 24 includes a third warp suppressing portion 24C and a fourth warp suppressing portion 24D formed by filling the third groove 12C and the fourth groove 12D with a second thermoplastic resin. With the above configuration, it is possible to suppress the compressive stress caused by the thermal contraction of the thermoplastic resin from acting locally on the base material.
[0061] In the above embodiment, the cross-sectional area S1 of the warp suppressing parts 24A and 24B in the second direction intersecting with the first direction satisfies the following relationship with respect to the cross-sectional area S2 of the first runner part 23A (resin molded body 21) in the second direction: 0.5×S2≦S1≦1.5×S2;. The cross-sectional area S1 of the warp suppressing parts 24C and 24D in the first direction intersecting with the second direction satisfies the following relationship with respect to the cross-sectional area S2 of the first runner part 23B (resin molded body 21) in the first direction: 0.5×S2≦S1≦1.5×S2;. With the above configuration, it is possible to effectively balance the compressive stress acting on the back surface 10B (second surface) of the base material due to the resin molded body and the compressive stress acting on the front surface 10A (first surface) of the base material due to the warp suppressing part 24.
[0062] In the above embodiment, the dimension W1 of the warp suppressing parts 24A, 24B along the second direction intersecting with the first direction satisfies the following relationship with respect to the dimension W2 of the first runner part 23A (resin molded body 21) along the second direction: 0.8×W2≦W1≦1.2×W2. Independently, the dimension W1 of the warp suppressing parts 24C, 24D along the first direction intersecting with the second direction satisfies the following relationship with respect to the dimension W2 of the first runner part 23B (resin molded body 21) along the first direction: 0.8×W2≦W1≦1.2×W2. According to the above configuration, when the height of the first runner portions 23A, 23B from the plate surface of the substrate 10 is high, for example, the compressive stress acting on the rear surface 10B (second surface) of the substrate 10 due to the first runner portions 23A, 23B and the compressive stress acting on the front surface 10A (first surface) of the substrate 10 due to the warp suppression portion can be effectively balanced.
[0063] In the above embodiment, the dimension (i.e., height) of the warp suppression section 24 along the thickness direction of the base material 10 is about 20% (one example of 50% or less) of the thickness of the base material 10. According to the above configuration, it is possible to prevent a decrease in strength of the base material 10 due to the provision of the warp suppression section 24, while suppressing warping of the base material 10.
[0064] In the above embodiment, the base material 10 is provided with a through hole 16, and a continuous portion (part of the filling portion 27) filled with a second thermoplastic resin is provided inside the through hole 16, and the resin molded body 21 and the warp suppressing portion 24 are continuous with each other through the continuous portion. According to the above configuration, the warp suppressing portion 24 and the like on the front surface 10A can be formed by supplying the second thermoplastic resin to the rear surface 10B of the base material, and this base material 10 can be easily manufactured, and can be provided as, for example, a low-cost base material. In addition, since gate marks and the like for forming the warp suppressing portion 24 and the like are not exposed on the front surface 10A, the design of the front surface 10A of the seat backboard 1 is improved.
[0065] In the above embodiment, the surface 10A (first surface) has a bent portion 14 (bent portion) bent so as to protrude, the bent portion 14 is continuous with the groove 12, and the corner portion of the bent portion 14 that is continuous with the first surface is provided with a filling portion filled with the second thermoplastic resin. When the substrate is bent without heating, the substrate is bent without flexibility, and therefore the substrate may be torn on the outer surface of the bent portion, resulting in loss of surface smoothness or the substrate may become thin and lose strength. According to the above configuration, the bent portion has a resin portion continuous with the warp suppression portion, so that the resin portion can smooth the surface of the substrate and even out the plate thickness. This makes it possible to provide substrates of various shapes.
[0066] In another aspect, a method for manufacturing a substrate with a resin molding according to the technology disclosed herein includes a preparation step of preparing a substrate having a plate-like substrate comprising fibers and a first thermoplastic resin, the substrate comprising a first surface and a second surface opposite the first surface, the substrate having a groove extending in the first direction on the first surface so as to follow a resin molding extending in the first direction that is to be provided on the second surface; and a resin supply step of supplying a second thermoplastic resin for forming the resin molding on the second surface of the substrate at a temperature at which the first thermoplastic resin does not melt, and supplying a third thermoplastic resin into the groove on the first surface, thereby obtaining a substrate with a resin molding having a warp suppressing portion that has the resin molding on the second surface and in which the groove on the first surface is filled with the third thermoplastic resin.
[0067] According to the above-mentioned configuration, by forming a resin molded body on one surface of the substrate and providing a warp suppressing section on the other surface of the substrate so as to fit the resin molded body, a substrate with a resin molded body can be manufactured without heating the substrate. This makes it possible to balance the compressive stress caused by the thermal contraction of the thermoplastic resin and the compressive stress caused by the warp suppressing section on the front and back plate surfaces of the substrate, and a substrate with a resin molded body with warp suppressed can be manufactured without heating and without significantly increasing the number of steps.
[0068] In the above embodiment, the preparation step includes a preboard preparation step of preparing a plate-shaped preboard without grooves, which includes the fiber and the first thermoplastic resin and has the first surface and the second surface but does not have the groove, and a groove forming step of providing the groove on the second surface of the preboard without grooves. The substrate in the present technology may be obtained with grooves formed in advance, or a preboard without grooves may be prepared and grooves may be formed in it. Here, a substrate with grooves formed in advance has the disadvantages that its use is limited and it is difficult to respond to design changes in a short period of time. According to the above configuration, for example, the substrate disclosed herein can be manufactured using a preboard with no use restrictions.
[0069] In the above embodiment, the second thermoplastic resin and the third thermoplastic resin are the same, and the preparation step includes a preboard preparation step of preparing a plate-shaped grooveless preboard that includes the fiber and the first thermoplastic resin and has the first surface and the second surface but does not have the groove, and a communication step of providing a through hole penetrating the preboard and making a cut to communicate the through hole with the groove, and in the resin supply step, the second thermoplastic resin for forming the resin molded body is supplied to the second surface of the preboard, and the second thermoplastic resin is fed to the first surface through the through hole and supplied to the groove. According to the above configuration, since the preboard has a through hole, by supplying the second thermoplastic resin to one surface, the second thermoplastic resin can be fed to the other surface through the through hole. This makes it possible to simplify the substrate manufacturing device and manufacture the substrate.
[0070] In the above embodiment, the preparation step includes a preboard preparation step of preparing a plate-shaped grooveless preboard that includes the fiber and the first thermoplastic resin and has the first surface and the second surface but does not include the groove, a cutting step of making a cut at a predetermined position on the first surface of the preboard, and a press molding step of pressing the preboard with a molding surface of a mold at a temperature at which the first thermoplastic resin does not melt so as to bend the preboard along the cut and in a manner such that the first surface protrudes, thereby forming the cutout portion formed by opening the cutout, and in the resin supply step, the second thermoplastic resin is filled into the cutout portion. According to the above configuration, press molding of the substrate is also performed, and the defective shape of the substrate caused by press molding without heating is compensated for by filling the thermoplastic resin in the resin supply step. This makes it possible to efficiently manufacture substrates of various shapes without heating.
[0071] <Other embodiments> The technology disclosed in this specification is not limited to the embodiments described above and illustrated in the drawings, and for example, the following embodiments are also included within the technical scope.
[0072] (1) In the above embodiment, two warp suppressing portions 24A-24B, 24C-24D are provided for each first runner portion 23A, 23B. However, the number of warp suppressing portions 24 provided for each first runner portion 23A, 23B is not limited. For example, as shown in FIG. 18, one warp suppressing portion may be provided for each runner portion. Also, three or more warp suppressing portions may be provided for each runner portion. From the viewpoint of reducing the installation area and resin amount of the warp suppressing portion to reduce weight, it is preferable to provide about one to three warp suppressing portions parallel to the runner portion.
[0073] (2) In the above embodiment 1, the second runner portion 23C was arranged on the back surface 10B so as to follow the joint portion between the main surface portion 11 and the side wall portion 13. However, the position of the second runner portion 23C is not limited to this, and the second runner portion 23C may be arranged so as to follow the back surface of the side wall portion 13 at a position slightly away from the side wall portion 13, and may be connected to the first runner portions 23A, 23B and the multiple rib portions 23D.
[0074] (3) In the above embodiment 1, the preboard is produced by combining the papermaking / air-laying method, the needle punching method, and the thermal bonding method. However, the method for producing the preboard is not limited to this, and may be a combination of various conventionally known methods such as the spunbonding method, the chemical bonding method, the water flow bonding method, and the lamination method.
[0075] (4) In the above embodiment, a through hole 16 is provided in the substrate 10, and molten resin is supplied only to the back surface 10B to form the front and back resin portions 20. However, it is not necessary to provide the through hole 16, and molten resin may be supplied to both the front surface 10A and the back surface 10B.
[0076] (5) In addition, in the above embodiment, the second thermoplastic resin and the third thermoplastic resin are the same thermoplastic resin, but they may be composed of different types of thermoplastic resins.
[0077] (6) In the above embodiment, one clip seat 22 is provided in the center of the seat backboard as one of the resin molded bodies, but multiple clip seats may be provided along the periphery of the seat backboard, or no clip seat may be provided. Accordingly, the shapes and arrangements of the first and second runners for feeding molten resin to the clip seats, ribs, etc. may be changed as desired.
[0078] (7) In the above embodiment, the planar shape of the slide mold 52 is designed to be the same as that of the groove 12. However, the planar shape of the slide mold 52 may be configured to press a part (e.g., four places) of the groove 12 to the extent that the pre-board can be positioned relative to the lower mold.
[0079] (8) In the above embodiment, the cuts in the pre-board are V-grooves having a V-shaped cross section. The shape of the cuts in the pre-board is not limited to this, and can be changed as appropriate to a U-shape, a C-shape, or the like.
[0080] (9) In the above embodiment, an example was disclosed in which the shape of the warp suppression part was determined based on the cross-sectional area in the direction intersecting the extension direction of the resin molded body, the dimension along the extension direction, or both. However, the shape of the warp suppression part may be determined based on the area of the joint between the extended resin molded body and the base material as one criterion. For example, the area S11 of the joint between the extended resin molded body and the base material may satisfy the relationship of 0.5×S12≦S11≦1.5×S12, and more preferably, the relationship of 0.8×S12≦S11≦1.2×S12, with respect to the area S12 of the joint between the warp suppression part and the base material. [Explanation of symbols]
[0081] 1...seat back board, 10...base material, 10A...surface, 10B...back surface, 12, 12A, 12B, 12C, 12D...groove, 13...side wall portion, 14...bending portion, 15...notch portion, 16...through hole, 20...resin portion, 23A, 23B...first runner portion (resin molded body), 24, 24A, 24B, 24C, 24D...warping suppression portion, 10P...pre-board, 10AP...surface, 10BP...back surface, 12P...groove, 14P...bending portion, 15P...notch portion, 16P...through hole
Claims
1. A plate-shaped substrate including fibers and a first thermoplastic resin and having a first surface and a second surface opposite to the first surface; a resin molded body provided on the second surface of the base material and extending along a first direction; Equipped with The first surface of the base material is provided with a groove extending along the first direction, and the groove is provided with a warp suppression portion formed by filling a second thermoplastic resin, The groove includes a first groove and a second groove provided so as to sandwich the resin molded body in a second direction intersecting the first direction, The warp suppressing portion includes a first warp suppressing portion and a second warp suppressing portion formed by filling the first groove and the second groove with the second thermoplastic resin.
2. A plate-shaped substrate including fibers and a first thermoplastic resin and having a first surface and a second surface opposite to the first surface; a resin molded body provided on the second surface of the base material and extending along a first direction; Equipped with The first surface of the base material is provided with a groove extending along the first direction, and the groove is provided with a warp suppression portion formed by filling a second thermoplastic resin, The first surface has a bent portion bent so as to protrude, The bent portion is continuous with the groove, The substrate with resin molding has a corner portion continuous with the first surface of the bent portion, the corner portion being provided with a filling portion filled with the second thermoplastic resin.
3. The substrate with resin molded body according to claim 1 , wherein the warpage suppressing portion is provided at a position overlapping the resin molded body.
4. The substrate with resin molding according to any one of claims 1 to 3, wherein a cross-sectional area S1 of the warp suppression portion in a second direction intersecting the first direction satisfies the following relationship with respect to a cross-sectional area S2 of the resin molding in the second direction: 0.5 x S2 ≦ S1 ≦ 1.5 x S2.
5. 5. The substrate with resin molding according to claim 1, wherein a dimension W1 of the warp suppression portion along a second direction intersecting the first direction satisfies the following relationship with respect to a dimension W2 of the resin molding along the second direction: 0.8×W2≦W1≦1.2×W2.
6. The substrate with resin molding according to any one of claims 1 to 5, wherein a dimension of the warp suppressing portion in a thickness direction of the substrate is 50% or less of a thickness of the substrate.
7. a through hole penetrating the base material, and a continuous portion filled with the second thermoplastic resin is provided inside the through hole, The resin molded body and the warp suppressing portion are continuous with each other via the continuous portion. The substrate with resin molded body according to any one of claims 1 to 6.
8. a preparation step of preparing a substrate comprising a plate-like substrate including fibers and a first thermoplastic resin, the plate-like substrate having a first surface and a second surface opposite to the first surface, the substrate including a first groove and a second groove extending along a first direction on the first surface so as to follow a resin molded body extending in the first direction to be provided on the second surface, the first groove and the second groove being provided so as to sandwich the resin molded body in a second direction intersecting the first direction; a resin supplying step of supplying a second thermoplastic resin for forming the resin molded body onto the second surface of the substrate at a temperature at which the first thermoplastic resin does not melt, and supplying a third thermoplastic resin into the first groove and the second groove on the first surface, thereby obtaining a substrate with a resin molded body that has the resin molded body on the second surface and that has a first warp suppressing portion and a second warp suppressing portion formed by filling the first groove and the second groove on the first surface with the third thermoplastic resin; The method for producing a substrate with a resin molded body comprising the steps of:
9. The preparation step includes: a preboard preparation step of preparing a plate-shaped grooveless preboard including the fibers and the first thermoplastic resin, the plate-shaped preboard having the first surface and the second surface but not including the groove; a groove forming step of providing the first groove and the second groove on the second surface of the grooveless preboard; The method for producing a substrate with a resin molded body according to claim 8 , comprising:
10. the second thermoplastic resin and the third thermoplastic resin are the same; The preparation step includes: a preboard preparation step of preparing a plate-shaped grooveless preboard including the fibers and the first thermoplastic resin, the plate-shaped preboard having the first surface and the second surface but not including the groove; a communication step of providing a through hole penetrating the preboard and making a cut to communicate the through hole with the groove; Including, 10. The method for manufacturing a substrate with a resin molding according to claim 8 or 9, wherein in the resin supplying process, the second thermoplastic resin for forming the resin molding is supplied to the second surface of the preboard, and the second thermoplastic resin is sent to the first surface through the through hole and supplied to the groove.
11. The preparation step includes: a preboard preparation step of preparing a plate-shaped grooveless preboard including the fibers and the first thermoplastic resin, the plate-shaped preboard having the first surface and the second surface but not including the groove; a cutting step of making a cut at a predetermined location on the first surface of the preboard; a press molding process in which the pre-board is pressed by a molding surface of a molding die at a temperature at which the first thermoplastic resin does not melt, so as to bend the pre-board along the incisions and in a manner such that the first surface protrudes, thereby forming a notch portion in which the incisions are opened; Including, The method for manufacturing a substrate with a resin molding according to any one of claims 8 to 10, wherein in the resin supplying step, the second thermoplastic resin is filled into the notch.
Citation Information
Patent Citations
JP1975134059A
Molding process of outsert
JP1987041009A
Moisture absorbing and discharging fiberboard and production thereof
JP1997193253A
Method for manufacturing resin molded article
JP2003053771A
Electronic component, and base material for electronic component and manufacturing method thereof
JP2011146350A