Method for manufacturing paramagnetic garnet-type transparent ceramics

The production of transparent ceramics with controlled oxygen content in the Tb oxide raw material addresses the issues of high absorption and scattering in existing garnet-based Faraday rotators, resulting in stable, high-power rotators for fiber lasers with reduced thermal lens effects.

JP7582168B2Active Publication Date: 2024-11-13SHIN ETSU CHEMICAL CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021196873
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-12-03
Publication Date
2024-11-13
Estimated Expiration
2041-12-03

AI Technical Summary

Technical Problem

Existing garnet-based Faraday rotators for high-power fiber lasers suffer from high optical absorption and scattering, leading to thermal lens effects that degrade laser quality, and there is a need for materials with lower absorption and higher Verdet constants that can be produced stably and cost-effectively.

Method used

A method for producing transparent ceramics using a sintered body of paramagnetic garnet-type composite oxide containing terbium, involving controlled oxygen content in the Tb oxide raw material, precise firing and cooling atmospheres, and additional processing steps to minimize absorption and scattering, resulting in a stable and transparent material suitable for high-power applications.

Benefits of technology

The method produces transparent ceramics with minimized light absorption and scattering, enabling their use as high-power Faraday rotators in optical isolators, effectively reducing thermal lens effects and maintaining laser quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582168000005
    Figure 0007582168000005
  • Figure 0007582168000001
    Figure 0007582168000001
  • Figure 0007582168000002
    Figure 0007582168000002
Patent Text Reader

Abstract

To produce, in a simple and stable quality manner, a transparent sintered compact of a Tb-containing paramagnetic garnet-type composite oxide, which minimizes absorption and scattering even at a mounting length and can be used as a Faraday rotator in a high-power fiber lasers.SOLUTION: This invention relates to a method for producing a transparent sintered compact of a Tb-containing paramagnetic garnet-type composite oxide, including: a step of mixing a sintered Tb oxide raw material powder for sintering, which consists of Tb2O3+a (0≤a≤0.2), with all of oxide raw material powders of other elements constituting the paramagnetic garnet-type composite oxide to form a forming raw material powder; a step of conducting forming by using the forming raw material powder; a step of degreasing the obtained compact at a degreasing temperature of 270°C or more and less than 400°C for a degreasing time of 1 hour or more; and a sintering step of sintering the degreased compact.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing transparent ceramics that can be used as magneto-optical materials, and more specifically to a method for producing terbium-containing transparent paramagnetic garnet-type ceramics that are suitable as magneto-optical materials that constitute magneto-optical devices such as optical isolators and can be used in high-power fiber lasers of 100 W or more. [Background technology]

[0002] In recent years, with the increasing power output of lasers, laser processing using fiber lasers has begun to gain popularity. In order to perform laser processing stably, it is necessary to remove external light from the laser light source and prevent its oscillation state from being disturbed. In particular, when light is reflected at the end surface of a fiber, the reflected light reaches the laser light source, resulting in significant oscillation disturbance. For this reason, a component called an isolator is installed at the boundary between fibers in regular fiber lasers to completely suppress reflected light.

[0003] An optical isolator consists of a Faraday rotator, a polarizer arranged on the light input side of the Faraday rotator, and an analyzer arranged on the light output side of the Faraday rotator. The Faraday rotator is used by applying a magnetic field parallel to the light's traveling direction. In this case, the polarization line of the light only rotates in a fixed direction whether it moves forward or backward through the Faraday rotator. Furthermore, the Faraday rotator is adjusted to a length that rotates the polarization line of the light exactly 45 degrees. Here, if the polarization planes of the polarizer and the analyzer are shifted 45 degrees in the direction of rotation of the forward light, the polarization of the forward light will be transmitted because it matches the polarizer position and the analyzer position. On the other hand, the polarization of the backward light will rotate 45 degrees in the opposite direction to the deviation angle of the polarization plane of the polarizer, which is shifted 45 degrees from the analyzer position. Then, the polarization plane of the return light at the polarizer position will be shifted 45 degrees - (-45 degrees) = 90 degrees from the polarization plane of the polarizer, and it cannot be transmitted through the polarizer. In this way, it functions as an optical isolator that transmits and emits forward light and blocks backward returning light.

[0004] Examples of materials that have been used for Faraday rotators include the garnet-based Tb3Ga5O 12 (hereinafter referred to as TGG) (JP Patent Publication 2009-143751 (Patent Document 1)) and C-type rare earth (Tb x Re (1-x) )2O3 (JP Patent Publication 2012-206935 (Patent Document 2)), and the fluoride KTb3F 10 (hereinafter referred to as KTF) (Laser Technik Journal 13 (2017): 18-21 (Non-Patent Document 1)). What these materials have in common is that they contain terbium, which has low light absorption at 1064 nm, which is used as a laser, and has a large Verdet constant (magneto-optical constant).

[0005] However, with the recent increase in the power output of fiber lasers, the characteristics required of Faraday rotators have also changed, and a small optical absorption coefficient is now required rather than a large Verdet constant. When a Faraday rotator absorbs laser light, the optical energy becomes heat, causing temperature unevenness on the inside and outer periphery of the Faraday rotator. The temperature unevenness directly causes refractive index unevenness, and the Faraday rotator has a refractive index distribution as if it were a lens. This is called the thermal lens effect, and deterioration of laser quality and fluctuation of focal length are observed. This thermal lens effect was not a problem with low-power lasers, but with high power, the Faraday rotator heats up to 40°C or more, and the thermal lens effect becomes noticeable. Therefore, a small optical absorption coefficient is required for high-power Faraday rotators.

[0006] TGG, which is commonly used as a Faraday rotator, has optical absorption and an output limit of 70 W. In addition, C-type rare earth materials have the advantage of being able to maximize the Verdet constant, but their optical absorption is more than twice that of TGG, and it is expected that their output limit is 30 W. On the other hand, the fluoride-based KTF has very little optical absorption and is thought to be capable of output of over 400 W. However, there are many unknowns about KTF in terms of crystal stability and manufacturing costs, and its Verdet constant is the same as that of TGG, so it is not expected that the Verdet constant will be improved any further. There is a demand for materials with lower absorption and a higher Verdet constant than TGG.

[0007] A material with lower absorption and a higher Verdet constant than TGG is TbAlO. 12 (hereinafter TAG) (JP Patent Publication 2004-131369 (Patent Document 3)), Tb3Sc2Al3O 12 (hereinafter referred to as TSAG) (JP Patent Publication No. 2015-000834 (Patent Document 4)), (Y x Tb 1-x )3AlO 12 (hereinafter referred to as YTAG) (J. Am. Ceram. Soc. 100 (2017), 4081-4087 (Non-Patent Document 2)). These have a Verdet constant about 1.4 times higher than TGG, while also having low optical absorption, so they are expected to be able to be installed in 100W level fiber lasers.

[0008] However, TAG is difficult to manufacture because it is unstable as a crystal, and TSAG contains a large amount of expensive Sc, which is disadvantageous in terms of cost. In contrast, YTAG, in which some of the Tb in TAG is replaced with Y, is a more stable crystal than TAG and does not use expensive elements, making it a promising material. However, Non-Patent Document 2 does not contain any information on thermal lensing in the high-power range, nor is there any information on optical absorption loss at the mounting length (14 mm or more). From the description in Non-Patent Document 2, it is unclear whether YTAG ceramics can be used as a high-power Faraday rotator.

[0009] In addition, International Publication No. 2018 / 193848 (Patent Document 5) describes a high-power Faraday rotator (Tb 1-x-y Sc x Ce y )3(Al 1-z Sc z )5O 12 This transparent ceramic material makes it possible to achieve easy manufacturing and low cost by complementing the disadvantages of TAG, which is difficult to manufacture, and TSAG, which is expensive, and also keeps the temperature rise to 20°C or less when irradiated with a 100W laser with a mounting length of 15mm, in other words, it makes it possible to suppress the thermal lens effect to a certain extent. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2009-143751 A [Patent Document 2] JP 2012-206935 A [Patent Document 3] JP 2004-131369 A [Patent Document 4] JP 2015-000834 A [Patent Document 5] International Publication No. 2018 / 193848

[0011] [Non-Patent Document 1] Laser Technik Journal 13(2017):18-21 [Non-Patent Document 2] J.Am.Ceram.Soc.100(2017),4081-4087 Summary of the Invention [Problem to be solved by the invention]

[0012] However, when the present inventors performed follow-up tests on the material of Patent Document 5, they found that it was difficult to manufacture and they were unable to obtain stable quality.

[0013] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a method for producing transparent ceramics in a simple manner with stable quality, which is a transparent sintered body of a terbium-containing paramagnetic garnet-type complex oxide, which minimizes absorption and scattering even at the mounting length and can be used as a Faraday rotator for a high-power fiber laser. [Means for solving the problem]

[0014] The present inventors conducted further tests on the materials in Non-Patent Document 2 and found that, although it was indeed possible to obtain Sc-free YTAG ceramics with high transmittance and low scattering, the probability of obtaining such ceramics was extremely low, and the majority of the ceramics contained a large number of bubbles. In addition, referring to Non-Patent Document 2, (Tb 1-x-y Y x Sc y )3(Al 1-z Sc z )5O 12 Although we tried to stabilize the crystals of the system, the Verdet constant became relatively small, and as a result, the mounting length became longer, and absorption due to oxygen vacancies or cation vacancies had a greater effect than ever before. At the same time, scattering due to bubbles and grain boundaries could no longer be ignored due to the longer mounting length, and we found that it was necessary to establish a manufacturing method for YTAG ceramics with lower scattering. In order to investigate the causes of these problems, we investigated the state of the raw materials (base raw materials) used for sintering these ceramics and found that the amount of oxygen contained in Tb oxide is important. Based on this knowledge, we conducted further research and applied Non-Patent Document 2 to find that by controlling the amount of oxygen contained in the Tb oxide of the base raw material, it is possible to stably control the amount of bubbles, and moreover, as an unexpected result, it was found that the transmittance can also be improved, which led to the present invention.

[0015] Therefore, the present invention provides the following method for producing a transparent ceramic. 1. A method for producing transparent ceramics made of a sintered body of a paramagnetic garnet-type composite oxide containing Tb, comprising the steps of: 3+a A method for producing a paramagnetic garnet-type transparent ceramic, comprising the steps of: mixing a sintered Tb oxide raw material powder consisting of (0≦a≦0.2) for sintering with all of the oxide raw material powders of the other elements that constitute a paramagnetic garnet-type composite oxide to obtain a raw material powder for molding; molding the raw material powder for molding; degreasing the obtained molded body at a degreasing temperature of 270°C or higher and lower than 400°C for a degreasing time of 1 hour or longer; and sintering the degreasing molded body. 2. The method for producing a paramagnetic garnet-type transparent ceramic according to 1, further comprising the steps of: firing a Tb oxide made of TbO under the following conditions: a firing temperature of 1000°C or higher and 1400°C or lower; an oxygen atmosphere during the heating process to the firing temperature and the holding process at the firing temperature; and an inert atmosphere, a reducing atmosphere, or a reduced pressure of 1000 Pa or lower during the cooling process from the firing temperature, to obtain the fired Tb oxide raw material for sintering. 3. 3. The method for producing a paramagnetic garnet-type transparent ceramic according to 1 or 2, further comprising a pressure sintering step of pressure sintering the sintered body after the sintering step. 4. 4. The method for producing a paramagnetic garnet-type transparent ceramic according to 3, further comprising subjecting the pressure-sintered body to an oxidation annealing treatment. 5. 5. The method for producing a paramagnetic garnet-type transparent ceramic according to any one of 1 to 4, wherein the garnet-type composite oxide is represented by the following formula (1): (T 1-x A 1 x )3B 1 5O 12 (1) (Wherein, 0≦x≦0.4, A 1 is at least one selected from Y, Sc and lanthanoid elements, and B 1 consists of at least one selected from the group 13 elements and Sc. Effect of the Invention

[0016] According to the present invention, it is possible to provide a transparent ceramic material that is made of a sintered body of a paramagnetic garnet-type composite oxide containing terbium (Tb), and that can be used as a high-output Faraday rotator in which the absorption and scattering of light with a wavelength of 1,064 nm at a mounting length of 23 mm is minimized. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of the configuration of an optical isolator using the paramagnetic garnet-type transparent ceramic produced according to the present invention as a Faraday rotator. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The method for producing the paramagnetic garnet-type transparent ceramics according to the present invention will now be described. The method for producing a paramagnetic garnet-type transparent ceramic of the present invention is a method for producing a transparent ceramic comprising a sintered body of a paramagnetic garnet-type composite oxide containing Tb, comprising the steps of: 3+a The method comprises the steps of: mixing a powder of a sintered Tb oxide raw material having a structure of (0≦a≦0.2) for sintering with all of the oxide raw material powders of the other elements that constitute the paramagnetic garnet-type composite oxide to obtain a raw material powder for molding; molding using the raw material powder for molding; degreasing the obtained molded body at a degreasing temperature of 270°C or higher and lower than 400°C for a degreasing time of 1 hour or longer; and sintering the degreasing molded body.

[0019] (Sintered Tb oxide raw material for sintering) In the present invention, TbO 3+a It is essential to use a sintered Tb oxide raw material having a structure of (0≦a≦0.2). The sintered Tb oxide raw material for sintering refers to a Tb oxide raw material that can be mixed with all the oxide raw materials of the other elements that make up the paramagnetic garnet-type composite oxide and sintering aids, molded, and degreased as necessary, without any further sintering treatment, to produce paramagnetic garnet-type transparent ceramics by sintering.

[0020] Tb is an element that can have either trivalent or tetravalent valences. In the case of Tb oxide, Tb2O3, which is an oxide of trivalent Tb (Tb(III)), is stable in high-temperature atmospheres of 1000°C or higher. However, at room temperature in air, Tb4O7, which contains an oxide of trivalent Tb (Tb(III)) and an oxide of tetravalent Tb (Tb(IV)) in a 1:1 ratio, is the most stable. Therefore, the commercially available Tb oxide raw material is Tb4O7 (Tb2O 3.5 However, the Tb oxide raw material commercially available as Tb4O7 is not preferred for the following two reasons.

[0021] First, there is no guarantee that commercially available oxides labeled Tb4O7 are truly made of Tb4O7. Tb oxides can have many compositions, for example Tb7O 11 or TbO 7.273 It has also been reported that commercially available Tb oxide raw materials labeled as Tb4O7 are weighed according to the target composition assuming that they are made of Tb4O7, but this may not result in the desired composition, and there is a risk that the expected quality will not be obtained. However, this problem can be addressed by confirming whether or not a commercially available product is truly made of Tb4O7 through composition analysis.

[0022] The second problem is that a large amount of oxygen is released during sintering of the Tb oxide raw material consisting of Tb4O7. When sintering a compact, if the atmosphere is under vacuum, oxygen is released from the Tb oxide raw material (Tb4O7), the degree of vacuum drops, and gas (oxygen) may be taken into the bubbles inside the sintered body. Once gas is taken into the sintered body as bubbles, it is not easy to remove it, and it will remain as a source of light scattering. In addition, if there is a large amount of released oxygen, it may accelerate the deterioration of the heater material of the vacuum sintering furnace. In most cases, the heat source of a vacuum sintering furnace is a metal heater such as Mo-W or a carbon heater. When oxygen is released from the compact, the Mo-W heater reacts with oxygen, and molybdenum oxide, which has a particularly high vapor pressure, fills the furnace as vapor, which results in accelerated deterioration of the heater material and, in some cases, extra contamination of the sintered body. This is also true for carbon heaters.

[0023] As a method for reducing the amount of oxygen released from the Tb oxide raw material, there is a method of mixing and molding the Tb oxide raw material consisting of Tb4O7 and the Al oxide raw material, and subjecting the molded body to a heat treatment at 1000°C or higher. When heat treatment is performed at 1000°C or higher, the Tb oxide and the Al oxide react to form a Tb-Al composite oxide in which trivalent Tb is stable, and the amount of tetravalent Tb is reduced or absent. Reducing or not having tetravalent Tb is synonymous with the fact that the Tb oxide has almost or no excess oxygen, which means that it is possible to reduce the amount of oxygen released during the subsequent sintering. However, in this method, the molded body is sintered at a high temperature of 1000°C or higher, so that densification progresses to a certain extent, and the bubbles inside the molded body become difficult to escape and may remain as a source of light scattering.

[0024] In the present invention, TbO has a low oxygen release rate. 3+a By using the calcined Tb oxide having the formula (0≦a≦0.2) as an essential raw material for sintering, many of the problems described above that arise with the Tb oxide raw material made of Tb4O7 can be solved.

[0025] TbO3+a In the above formula, a is 0 or more and 0.2 or less, preferably more than 0 and 0.2 or less, more preferably 0.01 or more and 0.2 or less, still more preferably 0.01 or more and 0.08 or less, and particularly preferably 0.01 or more and 0.05 or less.

[0026] In addition, TbO 3+a The value of a in the above formula can be determined by thermogravimetry (TG) analysis of the powder, weight comparison before and after re-firing at 1000°C in an atmosphere of 100 vol% oxygen, elemental analysis, thermal desorption spectrometry (TDS), etc. Among these, TG analysis of the powder is most preferable from the viewpoint of reproducibility. TG analysis is a method for measuring the weight change when a sample (powder) is heated and cooled at a constant rate in situ, and is an analytical method used to predict chemical and physical changes such as decomposition and adsorption of the sample. Specifically, a value of a can be calculated from the weight increase when a sample (Tb oxide powder sample) is set in a TG analyzer and heated in the atmosphere from room temperature (23°C ± 15°C) to 1000°C at a constant heating rate (for example, 15°C / min) and then cooled to room temperature. If the weight of the sample before heating (when set) is b (g) and the weight of the sample after TG analysis is c (g), a can be determined by the following formula (2). In addition, in this formula (2), the calculation is performed assuming that the composition of Tb oxide when heated to 1000°C and then cooled to room temperature is Tb4O7. a = 1-2 × 23.5 × {(cb) / c} (2)

[0027] Here, the Tb oxide consisting of Tb4O7 is used as a starting material, and is fired under the following conditions: firing temperature: 1000° C. to 1400° C., preferably 1000° C. to 1300° C.; atmosphere during the temperature rise to the firing temperature and the temperature hold: oxygen atmosphere; atmosphere during the temperature drop from the firing temperature: inert atmosphere, reducing atmosphere, or reduced pressure (vacuum) of 1000 Pa or less, to produce the above Tb2O 3+aIt is preferable to obtain a calcined Tb oxide raw material for sintering consisting of (0≦a≦0.2). The temperature increase rate during the temperature increase to the calcination temperature is preferably 50 to 400°C / hour, and the temperature decrease rate during the temperature decrease from the calcination temperature is preferably 50 to 400°C / hour. During the temperature decrease from the calcination temperature, it is preferable to decrease the temperature to at least 400°C, which is the phase transition temperature of Tb.

[0028] At this time, TbO 3+a As a starting material for obtaining a calcined Tb oxide raw material for sintering consisting of (0≦a≦0.2), a commercially available powder consisting of Tb4O7 or its precursor powder (the precursor is, for example, Tb(NO3)3) is used, and after calcining at 1000°C to 1400°C in an oxygen atmosphere, it is preferable to change the atmosphere to an inert atmosphere, a reducing atmosphere, or a reduced pressure of 1000 Pa or less when the temperature control program for the calcination process switches to a temperature decreasing mode.

[0029] If the firing temperature is less than 1000°C, the oxygen in Tb4O7 will not be completely removed, and a may not fall within the range of 0 to 0.2. If the firing temperature is higher than 1400°C, the sinterability of the resulting raw material powder will be poor, making it difficult to produce transparent ceramics.

[0030] The atmosphere during the temperature drop from the firing temperature is not particularly limited as long as it is an inert atmosphere (Ar, He, N2, etc.), a reducing atmosphere (Ar+2vol%H2, Ar+2vol%CO, etc.), or a reduced pressure of 1000 Pa or less and a is in the range of 0 to 0.2, but an inert atmosphere made of argon, nitrogen, or helium, or a reducing atmosphere (Ar+2vol%H2) made by adding 2vol% hydrogen to argon is preferred. Note that it is preferable to evacuate the atmosphere during the temperature drop from the firing temperature holding process to reduce the remaining oxygen as much as possible (for example, to less than 0.1vol%), and then use the above atmosphere during the temperature drop from the firing temperature.

[0031] The Tb oxide made of Tb4O7 used as the starting material is preferably in the form of a powder, and the primary particle size is not particularly limited as long as it is a powder that can be made transparent, and can be selected in a wide range from 50 nm to 50,000 nm. The same applies when using a precursor powder of Tb4O7, and the synthesis conditions are not particularly limited.

[0032] (Transparent ceramics) The transparent ceramics produced in the present invention are made of a sintered body of a paramagnetic garnet-type complex oxide containing Tb, and are preferably a transparent sintered body of a complex oxide represented by the following composition formula (1): The side where Tb is coordinated in the garnet crystal structure represented by composition formula (1), i.e., the side in parentheses in the first half of formula (1), is called the A site, and the side that is B in the second half of formula (1) is called the B site. (T 1-x A 1 x )3B 1 5O 12 (1) (Wherein, 0≦x≦0.4, A 1 is at least one selected from Y, Sc and lanthanoid elements, and B 1 consists of at least one selected from the group 13 elements and Sc.

[0033] In the A site of formula (1), Tb is the element with the largest Verdet constant among the paramagnetic elements except for iron (Fe), and has extremely low absorption in the 1064 nm region (wavelength band 0.9 μm to 1.1 μm) used in fiber lasers, making it the most suitable element for use as an optical isolator material in this wavelength range. However, trivalent Tb is easily oxidized to generate tetravalent Tb. This tetravalent Tb has light absorption properties, so it is desirable to eliminate it as much as possible. To eliminate this tetravalent Tb, it is most preferable to adopt a crystal structure in which tetravalent Tb is unstable, i.e., a garnet structure.

[0034] Although the sintered body can be made transparent by the coordination of Tb alone at the A site of formula (1), in order to make the sintered body more transparent, it is recommended to combine Tb with other elements (A 1) may be substituted. The element substituted for Tb to make it transparent is preferably at least one selected from the group of Y or lanthanoids, and Y, Lu or La are preferred from the viewpoint of extremely small absorption in the wavelength band used, and Y is the most preferred from the viewpoint of cost and stability. Y is an element that stabilizes the garnet structure, and the more it is substituted, the more stable it becomes and the easier it is to manufacture. However, if the Y content is excessive, the Verdet constant becomes too small, and the Verdet constant becomes smaller than that of TGG. Therefore, the Y content is preferably 0 mol% or more and 40 mol% or less with respect to Tb, and more preferably 10 mol% or more and 35 mol% or less.

[0035] The element that fits into the B site of formula (1) (B 1 As the group 13 element, excluding Sc, which will be described later, is preferable, and Al is particularly preferable. Ga, a group 13 element, is highly volatile and volatilizes during sintering, reducing the amount, so special measures are required, but Al does not volatilize during sintering and, when contained in the sintered body, increases the thermal conductivity, making it the most preferable.

[0036] Here, in a composite oxide whose constituent elements are only Tb, Y, a lanthanoid element, and a group 13 element, a garnet structure may not be obtained due to a slight weighing error of each raw material, and it is difficult to stably manufacture a transparent ceramic usable for optical applications. Therefore, in the present invention, it is preferable to eliminate the composition deviation due to a slight weighing error of each raw material by adding scandium (Sc) as a constituent element. Sc is a material having an intermediate ionic radius that can be dissolved in both the A site and the B site in an oxide having a garnet structure, and is a buffer material that can adjust the distribution ratio to the A site (rare earth site consisting of Tb, Y, and a lanthanoid element) and the B site (site consisting of a group 13 element) to exactly match the stoichiometric ratio and thereby minimize the energy of crystallite formation when the compounding ratio of the rare earth elements consisting of Tb, Y, and a lanthanoid element and the group 13 element deviates from the stoichiometric ratio due to the variation in weighing.

[0037] The Sc content is preferably 0 mol% or more and less than 0.08 mol% at the A site, and 0 mol% or more and less than 0.16 mol% at the B site. If high transparency can be achieved without adding Sc, there is no particular need to add it, but from the viewpoint of stable production, it is preferable to add a certain amount. On the other hand, if the content is above the upper limit, it will be easier to achieve transparency, but it will be undesirable because a large amount of expensive Sc will be used, which will not be cost-effective.

[0038] In formula (1), the range of x is 0≦x≦0.4, preferably 0.05≦x≦0.4, more preferably 0.1≦x≦0.4, and even more preferably 0.2≦x≦0.35. When x is in this range, the perovskite-type heterophase can be reduced to a level that is not detectable by X-ray diffraction (XRD) analysis. Furthermore, it is preferable because the number of perovskite-type heterophases (typically 1 to 1.5 μm in diameter and granular, light brown in color) present in a 150 μm×150 μm field of view observed under an optical microscope is 1 or less. In this case, the ratio of the perovskite-type heterophase to the garnet mother phase is 1 ppmv or less. Similarly, when x is in the above range, the number of pores (typically 0.5 to 2.0 μm in diameter, which become spherical voids when subjected to hot isostatic pressing (HIP)) remaining in the ceramic sintered body is preferably one or less in a 150 μm x 150 μm field of view observed under an optical microscope, and the proportion of pores in the garnet matrix at this time is 1 ppmv or less.

[0039] If x exceeds 0.4, the Verdet constant at 1064 nm will be less than 30 rad / (T m), which is not desirable. Furthermore, if the relative concentration of terbium is excessively diluted, the total length required to rotate the 1064 nm laser light by 45 degrees will exceed 25 mm, which is not desirable because it will be difficult to manufacture.

[0040] The method for producing the paramagnetic garnet-type transparent ceramics of the present invention comprises the steps of mixing the above-mentioned fired Tb oxide raw material powder for sintering with all of the oxide raw material powders of the other elements that constitute the paramagnetic garnet-type composite oxide to obtain a raw material powder for molding, a molding step using the raw material powder for molding, a step of degreasing the obtained molded body, and a sintering step of sintering the degreasing molded body.

[0041] (mixture) The above-mentioned sintered Tb oxide raw material powder and the oxide raw material powders of other elements constituting the paramagnetic garnet-type complex oxide are weighed out in predetermined amounts so as to obtain the composition of the above-mentioned target Tb-containing paramagnetic garnet-type complex oxide, preferably the composition corresponding to formula (1), and further mixed with a raw material serving as a sintering aid as necessary to obtain a raw material powder for molding. The purity of the above raw materials is preferably 99.9% by mass or more, and particularly preferably 99.99% by mass or more.

[0042] Other elements that compose the paramagnetic garnet-type complex oxide (i.e., elements that occupy the B site (B 1 ), or the element that enters the A site (A 1 ) and B 1 The oxide raw material of ) may be a composite oxide of these elements, but it is preferable to use an oxide of each of these elements as the raw material.

[0043] The primary particle size of the raw material powder is not particularly limited, but can be selected from a wide range of from 50 nm to 50,000 nm.

[0044] The raw material for the sintering aid is not particularly limited as long as it can be made transparent, such as SiO2 raw material, MgO raw material, etc., but is preferably SiO2 raw material such as tetraethyl orthosilicate (TEOS) or silicon oxide powder. The amount of tetraethyl orthosilicate (TEOS) added is an amount that is more than 0 ppm and less than 1,000 ppm (more than 0 mass% and less than 0.1 mass%) in terms of SiO2 in the entire raw material powder (raw material powder for garnet-type complex oxide + sintering aid), and the amount of silicon oxide powder (SiO2 powder) added is preferably an amount that is more than 0 ppm and less than 1,000 ppm (more than 0 mass% and less than 0.1 mass%) in terms of SiO2 in the entire raw material powder (raw material powder for garnet-type complex oxide + sintering aid). If the amount added is more than 1,000 ppm, there is a risk of slight light absorption occurring due to crystal defects caused by the excessive Si contained. In the case of silicon oxide powder (SiO2 powder), the primary particle size is not particularly limited, but can be selected from a wide range from 50 nm to 50,000 nm.

[0045] In addition, when no sintering aid is added, it is advisable to select the raw material powder for sintering (i.e., the raw material powder for the garnet-type composite oxide) to be used, which has a nano-sized primary particle size and has extremely high sintering activity. Such a selection may be made appropriately.

[0046] When mixing the raw material powders, it is preferable to perform slurrying by wet mixing in order to mix them uniformly. Dry mixing without using a dispersion medium is not suitable because the raw material powders do not mix uniformly. Examples of wet mixing include ball mills, bead mills, jet mills, ultrasonic irradiation, and homogenizer treatment, and are not particularly limited as long as they can be uniformly dispersed and mixed. Examples of dispersion media for wet mixing include lower alcohols and pure water, and are not particularly limited as long as they can be made transparent. In addition, if a raw material that serves as a sintering aid is added, it is preferable to add it at this timing.

[0047] In addition, an organic additive may be added as a dispersant to improve the dispersibility of the raw material powder, and examples of the dispersant include polyoxyethylene alkyl ether-based dispersants, dodecylbenzene sulfonic acid, and polyethylene glycol-based dispersants, but are not particularly limited thereto. In addition, when a binder is used to improve the shape retention of the molding, it is preferable to add it at this timing, and examples of the binder include polyvinyl alcohol-based, polyacrylic acid-based, polyvinyl acetate-based, and polyvinyl butyral-based binders, but are not particularly limited thereto as long as the shape retention can be maintained. In this manner, a molding raw material powder in which all of the raw material powders are uniformly mixed, preferably a molding raw material powder slurry, is obtained.

[0048] (molding) Next, the above-mentioned raw material powder for molding (raw material powder slurry for molding) is used to mold into a desired shape. There are wet and dry molding methods, but in the present invention, there is no particular limitation as long as it can be made transparent. Examples of wet molding include casting, centrifugal casting, extrusion molding, and tape molding, but there is no particular limitation as long as the desired shape can be obtained. In addition, in dry molding, granules are prepared from the raw material powder slurry, and uniaxial press molding is performed using a jig to obtain a desired shape. Examples of granulation methods include spray drying and sieving after vibration drying, but there is no particular limitation as long as the granule diameter is 2 μm or more and 1000 μm or less. If the granule diameter is less than 2 μm, each granule becomes light, and moldability may be poor. Also, if it exceeds 1000 μm, the voids between the granules after molding will be large, and there is a risk that they will remain as coarse bubbles inside the molded body. In both wet and dry molding, it is possible to further increase the molding density by performing cold isostatic pressing (CIP) after molding. The molding density is not particularly limited as long as the sintered body can be made transparent, and may be any value.

[0049] (Degreasing) Since the obtained green body still contains organic additives such as dispersants and binders, a degreasing process is carried out to remove these organic substances (organic additives).If the degreasing process is not carried out, CO2 gas and other substances will be generated during the subsequent sintering process, which will damage the sintered body and the sintering furnace.

[0050] The degreasing atmosphere may be oxygen or an oxygen-containing atmosphere of the air, and is not particularly limited as long as the organic matter (organic additives) in the compact is certainly decomposed and the amount of tetravalent Tb does not increase excessively. The degreasing temperature is preferably a low temperature at which the organic matter in the compact is certainly decomposed, specifically, 270°C or more and less than 400°C, and preferably 270°C or more and less than 350°C. If the degreasing temperature is less than 270°C, the organic matter remains, and if it is 400°C or more, a large amount of oxygen is taken into the Tb oxide, which is the sintered Tb oxide raw material for sintering in the compact (the amount of tetravalent Tb in the Tb oxide increases), and as described above, impurities from the heater of the vacuum sintering furnace are scattered during sintering, accelerating the deterioration of the heater material, and in some cases, extra contamination occurs in the sintered body.

[0051] The debinding time must be at least one hour, which is the time required to completely remove the organic matter in the compact. On the other hand, as for the upper limit of the debinding time, it is better not to make the debinding time longer than necessary, since a large amount of oxygen may be taken into the Tb oxide, which is the sintered Tb oxide raw material for sintering (the amount of tetravalent Tb in the Tb oxide may increase).

[0052] As a means for confirming the complete decomposition of organic substances (organic additives) and the amount of oxygen contained (i.e., the amount of tetravalent Tb in Tb oxide) in the obtained degreased compact, the above TbO 3+a As shown in the case of determining a in the above, TG analysis, TDS, and weight change measurement are included, among which TG analysis is the most preferable. In this case, TG analysis is preferably performed by performing thermogravimetry on a powder sample of a degreased molded body in the air during the process of heating it from room temperature to a predetermined temperature (e.g., 1000°C) at a constant heating rate (e.g., 15°C / min). Among these, complete decomposition of the organic matter (organic additives) can be judged from the weight loss due to the decomposition of the organic matter when heated from room temperature to 400°C, and if the organic matter (organic additives) remains, a weight loss of up to 3% is observed. In the present invention, it is preferable to judge that the organic matter (organic additives) has been completely decomposed to the extent that it does not adversely affect the obtained sintered body when the weight loss is 0.2% or less. The oxygen content of the degreased compact (amount of tetravalent Tb in Tb oxide) can be measured in the same manner as in the case of the calcined Tb oxide raw material for sintering, and can be compared as a relative value from the weight increase rate (derived from oxygen absorption) associated with the oxidation reaction that appears around 400°C. That is, in the case of a heating rate of 15°C / min in TG analysis, the weight increase associated with the oxidation reaction of Tb oxide is observed from around 350°C to around 450°C, but a mountain-shaped (upward convex) peak shape with a maximum point corresponding to the weight increase associated with the oxidation reaction is shown around 400°C. Here, looking at the base of the peak shape, the peak starts around 290°C and ends around 450°C, so the weight increase rate associated with the oxidation reaction can be calculated by integrating the area of ​​the peak over the entire range of 290 to 450°C. For example, the collected powder sample is heated at a heating rate of 15°C / min, the peak area in the range of 250 to 500°C is calculated from the temperature differential of the measured weight change rate, and the calculated value is rounded off to the nearest tenth to obtain the "weight increase rate associated with the oxidation reaction." In this case, it can be determined that the larger the weight increase rate, the smaller the oxygen content of the Tb oxide in the compact (i.e., the amount of tetravalent Tb in the Tb oxide). Conversely, when the weight increase rate is small (less than 0.2%), the oxygen content of the Tb oxide in the compact (i.e., the amount of tetravalent Tb in the Tb oxide) is large, and when it is 0%, it can be determined that the Tb4O7 is in a stable state at room temperature under air. In the present invention, when the "weight increase rate due to oxidation reaction" is 0.2% or more, it is judged that the oxygen content (tetravalent Tb content in Tb oxide) of the degreased molded body is suppressed to a level that does not adversely affect the obtained sintered body, and when it is less than 0.2%, it is judged that the oxygen content (tetravalent Tb content in Tb oxide) of the degreased molded body is contained to a level that adversely affects the sintered body. The upper limit of the "weight increase rate due to oxidation reaction" is not particularly limited, but is, for example, less than 0.6%.

[0053] (Sintering) The degreased green body obtained as described above is sintered to make it transparent. The sintering process may be carried out in a single sintering step until the sintered body reaches a transparent state (i.e., a relative density of approximately 100%), or the first sintering (pre-sintering) may be carried out to a relative density of 93% or more, and then the sintered body (HIP sintered body) may be made transparent by hot isostatic pressing (HIP). However, in order to produce a transparent sintered body with a good yield, a two-stage sintering process (pre-sintering-HIP process) in which HIP is performed after pre-sintering is preferred.

[0054] The sintering atmosphere for one sintering process or pre-sintering in a two-stage sintering process may be any of a vacuum (reduced pressure), an atmosphere containing 20 to 100 vol% oxygen, and air. From the viewpoint of removing bubbles in the sintered body, a vacuum (reduced pressure) atmosphere is most preferable. In this case, the degree of vacuum is 1×10 -1 Pa or less is preferable, and 1×10 -2 Pa or less is more preferable, and 1×10 -3 Pa or less is particularly preferred. The sintering temperature, sintering holding time, and heating rate are not particularly limited as long as they are within the conditions to obtain the desired relative density and average sintered grain size of the sintered body as described below.

[0055] In the case of a two-stage sintering process in which HIP is performed after pre-sintering, the relative density of the sintered body after pre-sintering (pre-sintered body) is preferably 93% or more, more preferably 95% or more. If the relative density is less than 93%, the inside and outside of the compact are often connected by air bubbles (open pores), and it is difficult to achieve transparency even if HIP treatment is performed in that state. There is no particular upper limit to the sintered density as long as the air bubbles can be removed by HIP.

[0056] The average sintered grain size in the sintered body after pre-sintering (pre-sintered body) is preferably 5 μm or less, more preferably 3 μm or less. If the average sintered grain size exceeds 5 μm, air bubbles are difficult to remove even by the subsequent HIP treatment, and tend to remain inside the sintered body. The lower limit of the average sintered grain size is not particularly limited as long as the relative density of the sintered body is 93% or more.

[0057] The average grain size of the sintered grains (average sintered grain size) is determined by measuring the grain size of the sintered grains of the target sintered body using a metallurgical microscope, and is determined in detail as follows. That is, for the preliminary sintered body, a metal microscope is used, and a reflection image of the surface of the sintered body is taken using a 50x objective lens in reflection mode. In detail, the entire optically effective area of ​​the target sintered body is photographed taking into account the effective image size of the objective lens, and the photographed images are subjected to analysis processing. At this time, a diagonal line is first drawn on each photographed image, and the total number of sintered particles that the diagonal line crosses is counted, and the value obtained by dividing the diagonal line length by this total count is defined as the average grain size of the sintered particles in the image. Furthermore, the average grain sizes of each photographed image read in the analysis processing are added up, and the value divided by the number of photographs is defined as the average grain size of the target sintered body. For HIP sintered bodies, the transmission mode of a metal microscope is used to take a transmission open Nicol image of a sintered body sample with both end faces polished using a 50x objective lens. In detail, the entire optically effective area of ​​the target sintered body is photographed taking into consideration the effective image size and effective focal depth of the objective lens, and the photographed images are subjected to analysis processing. At this time, a diagonal line is first drawn on each photographed image, and the total number of sintered particles that the diagonal line crosses is counted, and the value obtained by dividing the diagonal line length by this total count is defined as the average grain size of the sintered particles in the image. Furthermore, the average grain sizes of each photographed image read in the analysis processing are added up, and the value divided by the number of photographs is defined as the average grain size of the target sintered body.

[0058] The most preferable pressure medium for the HIP treatment is argon, and a small amount of oxygen may be contained to suppress oxygen deficiency. However, when oxygen is contained, the heater material used in the HIP furnace is preferably a material resistant to oxidation, and platinum is the most preferable. The temperature of the HIP treatment is not limited as long as it can be made transparent, but it is most preferable to set it within a range of ±100°C of the pre-sintering temperature. If the temperature is more than 100°C lower than the pre-sintering temperature, the effect of the HIP treatment is weak, and if the temperature is more than 100°C higher, the crystal grains grow and it becomes difficult to remove bubbles, which is inappropriate. The pressure of the HIP treatment is preferably 100 MPa or more and 200 MPa or less. If it is less than 100 MPa, the effect of the HIP treatment is weak, and if it is more than 200 MPa, it is inappropriate because of the limitations of the device. In addition, in order to block contaminants from the heater of the HIP treatment, it is preferable to place the pre-sintered body in a metal can such as Mo or W and perform the treatment.

[0059] In order to improve the uniformity of the sintered body obtained as described above, it is recommended to carry out re-sintering and re-HIP processing to set the average sintered grain size to 15 μm or more and 40 μm or less. If the average sintered grain size exceeds 40 μm, the ceramics are likely to fall out, which is not preferable. In this case, the re-sintering temperature may be set so as to obtain the desired grain size, and similarly, the re-HIP temperature may be set so as to obtain a highly transparent body, and neither the re-sintering temperature nor the re-HIP temperature is particularly limited.

[0060] (Oxidation annealing treatment) The sintered body (HIP sintered body) obtained by the above process may have oxygen deficiency or cation deficiency in the sintered body, resulting in a colored appearance. In such a case, it is preferable to carry out an oxidation annealing treatment (a treatment to restore oxygen deficiency or cation deficiency) to remove the coloration.

[0061] The oxidation annealing treatment is preferably a treatment in which the sintered body (HIP sintered body) is heated at 1300°C to 1500°C in an atmosphere containing 15 vol% or more of oxygen for 10 hours or more. If the oxygen content is less than 15 vol%, the amount of oxygen is not sufficient to recover oxygen deficiency (or cation deficiency). Furthermore, if the oxygen content is less than 1300°C, oxygen cannot diffuse into the ceramic. If the oxygen content is more than 1500°C, the bubbles crushed by the HIP treatment will expand again and become a scattering source, which is not preferable. Furthermore, if the annealing time is less than 10 hours, oxygen cannot diffuse into the ceramic, which is also inappropriate. There is no particular upper limit to the annealing time, but if it is too long, it will not be cost-effective, so it should be set to a time sufficient to remove coloring.

[0062] (Processing process) In the manufacturing method of the present invention, it is preferable that the paramagnetic garnet-type transparent ceramics that have undergone the above-mentioned series of manufacturing steps are ground to a predetermined length, and then both end faces on the optical axis to be used optically are optically polished. In this case, the optical surface accuracy is preferably λ / 8 or less, and particularly preferably λ / 10 or less, when the measurement wavelength λ=633 nm. It is also possible to further reduce optical loss by appropriately forming an anti-reflection film on the optically polished surface.

[0063] In this manner, a transparent ceramic material is obtained that is made of a sintered body of a paramagnetic garnet-type composite oxide containing terbium (Tb), and that can be used as a high-output Faraday rotator with minimal absorption and scattering of light with a wavelength of 1,064 nm at a mounting length of 23 mm.

[0064] [Magneto-optical devices] Furthermore, since the paramagnetic garnet-type transparent ceramic obtained by the present invention is assumed to be used as a magneto-optical material, it is preferable to apply a magnetic field parallel to the optical axis of the paramagnetic garnet-type transparent ceramic, and then set a polarizer and an analyzer so that their optical axes are shifted by 45 degrees from each other to form a magneto-optical device. That is, the magneto-optical material of the present invention is suitable for magneto-optical device applications, and is particularly suitable for use as a Faraday rotator for an optical isolator with a wavelength of 0.9 to 1.1 μm.

[0065] FIG. 1 is a schematic cross-sectional view showing an example of an optical isolator, which is an optical device having, as an optical element, a Faraday rotator made of the paramagnetic garnet-type transparent ceramic obtained according to the present invention. 1, an optical isolator 100 includes a Faraday rotator 110 made of the paramagnetic garnet-type transparent ceramic obtained in the present invention, and a polarizer 120 and an analyzer 130, which are polarizing materials, are provided in front of and behind the Faraday rotator 110. Moreover, it is preferable that the optical isolator 100 has the polarizer 120, the Faraday rotator 110, and the analyzer 130 arranged in this order on its optical axis, and that a magnet 140 is placed on at least one of the side surfaces of these elements.

[0066] The optical isolator 100 can be suitably used in industrial fiber laser devices, that is, to prevent the reflected light of the laser light emitted from the laser light source from returning to the light source, causing the oscillation to become unstable. EXAMPLES

[0067] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these.

[0068] [Example 1] (Examples 1-1 to 1-5, Comparative Example 1) (Sintered Tb oxide raw material (TbO 3+a Preparation of Commercially available Tb4O7 powder (Shin-Etsu Chemical Co., Ltd., purity 99.999 mass%, particle size 50-100 nm) was placed in an yttria container and set in a firing furnace capable of controlling the atmosphere. The firing was performed at a heating rate of 200°C / hour to the firing temperature and at a firing temperature of 900-1400°C (six levels: 900°C, 1000°C, 1100°C, 1200°C, 1300°C, and 1400°C) for a holding time of 3 hours. The atmosphere during the heating process to the firing temperature and the holding process at the firing temperature was 100 vol% oxygen, and the atmosphere during the temperature drop from the firing temperature was Ar. Note that evacuation was performed for 1 minute before the temperature drop process from the holding process of the firing temperature to the temperature drop process, and the atmosphere during the temperature drop from the firing temperature was switched to Ar after the remaining oxygen was reduced to less than 0.1 vol%. In addition, the temperature decreasing rate in the process of decreasing the temperature from the firing temperature was 100° C. / hour. If the actual temperature in the process of decreasing the temperature did not keep up with the program, the temperature was allowed to decrease naturally to room temperature. The obtained calcined Tb oxide was a white to ocher powder.

[0069] (Measurement of oxygen content in fired Tb oxide raw material for sintering) The calcined Tb oxide sample (TbO 3+a The oxygen content a of the above was measured by TG analysis in the atmosphere as follows. That is, a calcined Tb oxide sample with a sample weight (b) of 0.08000±0.0010 g before heating (when set) was placed in a platinum pan, set in a differential thermal / thermogravimetric simultaneous measurement device (TG / DTA analyzer, Rigaku Corporation, model name: Thermo plus EVO), heated to 1000°C at a heating rate of 15°C / min, and then cooled to room temperature at a rate of 15°C / h. The sample weight c (g) after TG analysis was measured, and the composition of the calcined Tb oxide sample, TbO, was calculated by applying the following formula (2): 3+a The reference sample was alumina. a = 1-2 × 23.5 × {(cb) / c} (2)

[0070] Using the fired Tb oxide sample obtained as described above, transparent ceramics were produced in the following manner. (Mixing process) The calcined Tb oxide sample (TbO 3+a ), Y2O3 (Shin-Etsu Chemical Co., Ltd., purity 99.999 mass%, particle size 50-100 nm), Al2O3 (Taimei Chemical Co., Ltd., purity 99.99 mass%, particle size 200 nm), and Sc2O3 (Shin-Etsu Chemical Co., Ltd., purity 99.99 mass%, particle size 3 μm) were each prepared to the target composition (Tb 0.64 Y 0.34 Sc 0.02 )3(Al 0.98 Sc 0.02 )5O 12 The weight was measured so that the weight of the powder was 1.5% by weight, but the weight was measured while taking into consideration the effect of the oxygen content of the sintered Tb oxide sample. The weighted raw powder for sintering was mixed with ethanol as a dispersion medium, 2 mm alumina balls as a mixing medium, and 900 ppm by mass of TEOS (120 ppm by mass in terms of SiO2) as a sintering aid, all of which were placed in a resin pot, sealed, and mixed in a ball mill for 20 hours with a roller rotating at 200 rpm. Next, 1.5% by mass of polyvinyl acetate binder was added to the obtained slurry as a binder relative to the powder amount, and ball mill mixing was performed for another 4 hours. The slurry and the alumina balls were separated and granulated by spray drying. (molding process) The granules obtained in the previous process were filled into a cylindrical mold with a diameter of 7 mm, and a compact with a diameter of 7 mm and a length of 35 mm was obtained by dry uniaxial press molding. The pressure of the dry uniaxial press was 50 MPa. The compact was then subjected to CIP treatment at 200 MPa for 1 minute. (Degreasing process) The CIP molded body obtained in the previous process was placed in a muffle furnace and subjected to atmospheric degreasing treatment at a degreasing temperature of 280°C for 3 hours. The temperature increase rate was 100°C / hour and the temperature decrease rate was 150°C / hour.

[0071] (Measurement of weight gain rate associated with oxidation reaction) A part of the degreased molded body sample obtained as described above was taken out and pulverized in a mortar. The pulverized powder was filled into a platinum pan, and the powder sample was collected using a differential thermobalance (TG-DTA) (Thermo plus Evo, manufactured by Rigaku Corporation) as a thermal analyzer. The temperature of the powder sample was increased from room temperature to 1000°C at a heating rate of 15°C / min in air, and the peak area in the range of 250 to 500°C was calculated from the temperature differential value of the measured weight change rate. The calculated value was rounded off to three decimal places to obtain the "weight increase rate associated with the oxidation reaction".

[0072] (Sintering process) The sintering process was carried out in two stages: preliminary sintering and HIP treatment. First, the degreased compact was placed in a vacuum sintering furnace and sintered at a vacuum of 1×10 -4 The pre-sintering process was carried out under the conditions of 1 Pa, heating rate of 100°C / hour, and sintering temperature of 1600°C, and holding for 2 hours. After pre-sintering, the relative density of all samples was 93% or more, and the average sintered grain size was 1μm. Next, in order to achieve transparency, the pre-sintered samples were subjected to HIP treatment under the conditions of 198 MPa pressure, Ar atmosphere, HIP temperature of 1600°C, and holding time of 3 hours. After HIP, the samples became transparent, but blackening due to oxygen deficiency was observed in all samples, so oxidation annealing treatment was carried out in air at 1450°C for 30 hours. After oxidation annealing, all samples became colorless and transparent. (polishing / processing process) The annealed HIP sintered sample was cylindrically ground to an outer diameter of 5 mm, and then optically polished to a length of 23 mm. The polished surface accuracy was set to λ / 8 (λ=633 nm).

[0073] The transparent ceramic samples obtained as described above were evaluated as follows. (Total light transmittance and diffuse transmittance) The total light transmittance and diffuse transmittance as transparency of the optically polished transparent ceramic samples were measured with reference to JIS K7136:2000. That is, an integrating sphere was installed in a spectrophotometer (JASCO Corporation, V-670), and a pinhole was provided so that the spot diameter of the irradiated light was 3 mm. A halogen lamp was used as the light source, and a photomultiplier tube (wavelength less than 750 nm) and a PdS photoelectric cell (wavelength 750 nm or more) were used as the detector, and the measurement was performed by the double beam method. In this case, an entrance opening and an exit opening through which light passes were provided in the integrating sphere, a sample was placed at the entrance opening, and a reflector was attached to the exit opening, so that all the light emitted from the sample could be detected by the integrating sphere. The reflector at the exit opening was removed to detect the light other than that in the light traveling direction among all the light rays, and the ratio of this detected light intensity to the intensity of the light incident on the sample (incident light intensity) was calculated as the diffuse transmittance. The ratio of the intensity of the emitted light detected without removing the reflector at the exit opening to the intensity of the incident light was calculated as the total light transmittance. The measurement wavelength was fixed at 1064 nm.

[0074] (Verde constant) Each of the obtained transparent ceramic samples was inserted into the center of a neodymium-iron-boron magnet with an outer diameter of 32 mm, an inner diameter of 6 mm, and a length of 40 mm, and polarizers were placed on both ends. A high-power laser beam with a wavelength of 1064 nm was then incident on both end faces using a high-power laser (beam diameter 1.6 mm) manufactured by IPG Photonics Japan Co., Ltd., to determine the Faraday rotation angle θ. The Faraday rotation angle θ was defined as the angle at which the maximum transmittance was observed when the polarizer on the output side was rotated. The Verdet constant was calculated based on the following formula: The magnitude (H) of the magnetic field applied to the sample was calculated by simulation from the dimensions of the measurement system, the residual magnetic flux density (Br), and the coercive force (Hc). θ=V×H×L (In the formula, θ is the Faraday rotation angle (rad), V is the Verdet constant (rad / (T m)), H is the magnitude of the magnetic field (T), and L is the length of the Faraday rotator (0.023 m in this case).) The above results are shown in Table 1.

[0075] [Table 1]

[0076] In preparing the sintered Tb oxide raw material, the sintered Tb oxide raw material samples (Examples 1-1 to 1-5) sintered in an Ar atmosphere at a sintering temperature range of 1000 to 1400°C had a value of a of 0.19 or less (i.e., the amount of oxygen contained in the Tb oxide was sufficiently reduced), and the transparent ceramics produced using these sintered Tb oxide raw materials had a total light transmittance of 84.1% or more and a diffuse transmittance of 0.24% or less. On the other hand, the sintered Tb oxide raw material sample (Comparative Example 1) sintered in an Ar atmosphere at a sintering temperature of 900°C had a value of a of 0.38 (i.e., the amount of oxygen contained in the Tb oxide was not sufficiently reduced), and the transparent ceramics produced using this sintered Tb oxide raw material had a total light transmittance of 83.5% or more and a diffuse transmittance of 0.42%. The reason why the total light transmittance in Comparative Example 1 was 83.5% lower than that in Examples 1-1 to 1-5 is presumed to be because oxygen was desorbed from the compact during the sintering stage, oxidizing the tungsten in the heater, and the resulting vapor was contained in the sintered compact sample. The reason why the diffuse transmittance in Comparative Example 1 was 0.42% higher than that in Examples 1-1 to 1-5 is presumed to be because the bubbles (oxygen molecules) in the sintered compact could not be sufficiently removed in the two-stage sintering process. The diffuse transmittance in Example 1-5 is slightly higher than that in the other Examples 1-1 to 1-4, but this is presumed to be because the activity of Tb was reduced as a result of the sintering temperature being set at a high temperature of 1400°C in the preparation of the sintered Tb oxide raw material for sintering.

[0077] [Example 2] (Examples 2-1 to 2-5, Comparative Examples 2-1 to 2-3) In Example 1-3, the atmosphere during the temperature drop process from the sintering temperature in the preparation of the sintered Tb oxide raw material for sintering was changed from Ar to Ar + 2 vol% H2, Ar + 2 vol% CO, He, N2, vacuum (1 x 10 Pa), Ar + 2 vol% O2, Ar + 0.1 vol% O2, and O2. Otherwise, the process from the preparation of the sintered Tb oxide raw material for sintering to the production of transparent ceramics was carried out in the same manner as in Example 1-3, and evaluation was performed in the same manner as in Example 1. The results are shown in Table 2.

[0078] [Table 2]

[0079] As a result of the above, transparent ceramics with high transparency were obtained even if the atmosphere during the temperature drop process from the firing temperature in the preparation of the fired Tb oxide raw material for sintering was a reducing atmosphere, an inert atmosphere other than Ar, or a vacuum (reduced pressure). On the other hand, as a result of the above, if the atmosphere during the temperature drop process from the firing temperature in the preparation of the fired Tb oxide raw material for sintering contains even a small amount of oxygen, a in the fired Tb oxide raw material for sintering becomes large (i.e., the amount of oxygen contained in the Tb oxide is not reduced), and TbO 3.5 (i.e., Tb4O7), and as a result, the total light transmittance of the transparent ceramics produced using this material decreased, while the diffuse transmittance increased.

[0080] [Example 3] (Examples 3-1 to 3-6, Comparative Examples 3-1 to 3-4) In Example 1-3, the degreasing temperature and the degreasing time were changed, and otherwise the same procedures as in Example 1-3 were carried out to prepare transparent ceramics, which were then evaluated in the same manner as in Example 1. The results are shown in Table 3.

[0081] [Table 3]

[0082] As a result, transparent ceramics with high transparency were obtained under the conditions of a degreasing temperature of 270 to 350°C and a degreasing time of 1 hour or more (Examples 3-1 to 3-6). On the other hand, when the degreasing temperature was 400°C or more (Comparative Examples 3-1 and 3-2), the total light transmittance decreased and the diffuse transmittance increased compared to Examples 3-1 to 3-6. At this time, the weight increase rate due to the oxidation reaction in the degreasing molded body was 0. Furthermore, when the degreasing temperature was 250°C (Comparative Example 3-3) or when the degreasing temperature was 270°C and the degreasing time was 0.1 hours (Comparative Example 3-4), the organic matter in the molded body was not sufficiently removed, and the transparency evaluation (total light transmittance and diffuse transmittance) of the finally obtained ceramic sample was devitrified.

[0083] [Example 4] In Example 1-3, the composition was changed and the raw material powders were mixed as follows, but otherwise the same procedures were followed to prepare transparent ceramics in the same manner as in Example 1-3, and the ceramics were evaluated in the same manner as in Example 1. Note that the measurement of the weight increase rate due to the oxidation reaction in the degreased molded body was omitted.

[0084] (Example 4-1) The calcined Tb oxide sample (TbO 3+a ) and Al2O3 (manufactured by Taimei Chemical Co., Ltd., purity 99.99 mass%, particle size 200 nm) were used to obtain the target composition Tb3Al5O 12 The weight was measured so that the weight of the powder was 1.5% by weight, but the weight was measured while taking into consideration the effect of the oxygen content of the sintered Tb oxide sample. The weighted raw powder for sintering was mixed with ethanol as a dispersion medium, 2 mm alumina balls as a mixing medium, and 900 ppm by mass of TEOS (120 ppm by mass in terms of SiO2) as a sintering aid, all of which were placed in a resin pot, sealed, and mixed in a ball mill for 20 hours with a roller rotating at 200 rpm. Next, 1.5% by mass of polyvinyl acetate binder was added to the obtained slurry as a binder relative to the powder amount, and ball mill mixing was performed for another 4 hours. The slurry and the alumina balls were separated and granulated by spray drying.

[0085] (Example 4-2) The calcined Tb oxide sample (TbO3+a ) and Ga2O3 (manufactured by Yamanaka Hutech Co., Ltd., purity 99.9 mass%, particle size 400 nm) were used to obtain the target composition Tb3Ga5O 12 The weight was measured so that the weight of the powder was 1.5% by weight, but the weight was measured while taking into consideration the effect of the oxygen content of the sintered Tb oxide sample. The weighted raw powder for sintering was mixed with ethanol as a dispersion medium, 2 mm alumina balls as a mixing medium, and 900 ppm by mass of TEOS (120 ppm by mass in terms of SiO2) as a sintering aid, all of which were placed in a resin pot, sealed, and mixed in a ball mill for 20 hours with a roller rotating at 200 rpm. Next, 1.5% by mass of polyvinyl acetate binder was added to the obtained slurry as a binder relative to the powder amount, and ball mill mixing was performed for another 4 hours. The slurry and the alumina balls were separated and granulated by spray drying.

[0086] (Example 4-3) The calcined Tb oxide sample (TbO 3+a ), Y2O3 (Shin-Etsu Chemical Co., Ltd., purity 99.999 mass%, particle size 50-100 nm), and Al2O3 (Taimei Chemical Co., Ltd., purity 99.99 mass%, particle size 200 nm) were each prepared with the target composition (Tb 0.6 Y 0.4 )3AlO 12 The weight was measured so that the weight of the powder was 1.5% by weight, but the weight was measured while taking into consideration the effect of the oxygen content of the sintered Tb oxide sample. The weighted raw powder for sintering was mixed with ethanol as a dispersion medium, 2 mm alumina balls as a mixing medium, and 900 ppm by mass of TEOS (120 ppm by mass in terms of SiO2) as a sintering aid, all of which were placed in a resin pot, sealed, and mixed in a ball mill for 20 hours with a roller rotating at 200 rpm. Next, 1.5% by mass of polyvinyl acetate binder was added to the obtained slurry as a binder relative to the powder amount, and ball mill mixing was performed for another 4 hours. The slurry and the alumina balls were separated and granulated by spray drying.

[0087] (Examples 4-4, 4-5, and 4-6) The calcined Tb oxide sample (TbO 3+a), Y2O3 (Shin-Etsu Chemical Co., Ltd., purity 99.999 mass%, particle size 50-100 nm), Al2O3 (Taimei Chemical Co., Ltd., purity 99.99 mass%, particle size 200 nm), and Sc2O3 (Shin-Etsu Chemical Co., Ltd., purity 99.99 mass%, particle size 3 μm) were each prepared to the target composition (Tb 0.8 Y 0.18 Sc 0.02 )3(Al 0.95 Sc 0.05 )5O 12 , (Tb 0.6 Y 0.34 Sc 0.06 )3(Al 0.93 Sc 0.07 )5O 12 , (Tb 0.6 Y 0.37 Sc 0.03 )3(Al 0.992 Sc 0.008 )5O 12 The weight was measured so that the weight of the powder was 1.5% by weight, but the weight was measured while taking into consideration the effect of the oxygen content of the sintered Tb oxide sample. The weighted raw powder for sintering was mixed with ethanol as a dispersion medium, 2 mm alumina balls as a mixing medium, and 900 ppm by mass of TEOS (120 ppm by mass in terms of SiO2) as a sintering aid, all of which were placed in a resin pot, sealed, and mixed in a ball mill for 20 hours with a roller rotating at 200 rpm. Next, 1.5% by mass of polyvinyl acetate binder was added to the obtained slurry as a binder relative to the powder amount, and ball mill mixing was performed for another 4 hours. The slurry and the alumina balls were separated and granulated by spray drying.

[0088] (Examples 4-7) The calcined Tb oxide sample (TbO 3+a ), Y2O3 (Shin-Etsu Chemical Co., Ltd., purity 99.999 mass%, particle size 50-100 nm), and Al2O3 (Taimei Chemical Co., Ltd., purity 99.99 mass%, particle size 200 nm) were each prepared with the target composition (Tb 0.01 Y 0.99 )3AlO 12The weight was measured so that the weight of the powder was 1.5% by weight, but the weight was measured while taking into consideration the effect of the oxygen content of the sintered Tb oxide sample. The weighted raw powder for sintering was mixed with ethanol as a dispersion medium, 2 mm alumina balls as a mixing medium, and 900 ppm by mass of TEOS (120 ppm by mass in terms of SiO2) as a sintering aid, all of which were placed in a resin pot, sealed, and mixed in a ball mill for 20 hours with a roller rotating at 200 rpm. Next, 1.5% by mass of polyvinyl acetate binder was added to the obtained slurry as a binder relative to the powder amount, and ball mill mixing was performed for another 4 hours. The slurry and the alumina balls were separated and granulated by spray drying. The above results are shown in Table 4.

[0089] [Table 4]

[0090] As a result of the above, in the case of garnet-type composite oxides containing Tb, a high level of transparency was achieved without any problems for any composition. At first glance, some samples appear to have low total light transmittance, but this is because the theoretical value differs depending on the composition. When an anti-reflection film is formed on the optical end face, all samples have a total light transmittance of 99% or more, which means that the transparency is sufficient.

[0091] Although the present invention has been described above using the above-mentioned embodiment, the present invention is not limited to this embodiment, and can be modified within the scope of what a person skilled in the art can imagine, such as other embodiments, additions, modifications, deletions, etc., and any aspect is within the scope of the present invention as long as it achieves the effects of the present invention. [Explanation of symbols]

[0092] 100 Optical isolator 110 Faraday Rotator 120 Polarizer 130 Analyzer 140 Magnet

Claims

1. A method for producing a transparent ceramics comprising a sintered body of a paramagnetic garnet-type composite oxide containing Tb, comprising the steps of: 2 O 3+a A method for producing a paramagnetic garnet-type transparent ceramic, comprising the steps of: mixing a powder of a fired Tb oxide raw material for sintering consisting of (0≦a≦0.2) with all of the oxide raw material powders of the other elements constituting a paramagnetic garnet-type composite oxide to obtain a raw material powder for molding; molding the raw material powder for molding; degreasing the obtained molded body at a degreasing temperature of 270° C. or higher and lower than 400° C. for a degreasing time of 1 hour or longer; and sintering the degreased molded body.

2. Tb 4 O 7 2. The method for producing a paramagnetic garnet-type transparent ceramic according to claim 1, wherein the Tb oxide raw material for sintering is obtained by firing the Tb oxide consisting of the above under the conditions of a firing temperature of 1,000° C. or higher and 1,400° C. or lower, an oxygen atmosphere during the heating process to the firing temperature and the holding process at the firing temperature, and an inert atmosphere, a reducing atmosphere, or a reduced pressure of 1,000 Pa or lower during the cooling process from the firing temperature.

3. 3. The method for producing a paramagnetic garnet-type transparent ceramic according to claim 1, further comprising a pressure sintering step of pressure sintering the sintered body after the sintering step.

4. 4. The method for producing paramagnetic garnet-type transparent ceramics according to claim 3, further comprising subjecting the pressure-sintered body to an oxidation annealing treatment.

5. The method for producing a paramagnetic garnet-type transparent ceramic according to any one of claims 1 to 4, wherein the garnet-type composite oxide is represented by the following formula (1): () 1-x A 1 x ) 3 B 1 5 O 12 () (Wherein, 0≦x≦0.4, A 1 is at least one selected from Y, Sc and lanthanoid elements, B 1 consists of at least one selected from the group 13 elements and Sc.

Citation Information

Patent Citations

  • Zirconium-doped terbium aluminum garnet magnetic light rotation transparent ceramic and preparation method thereof

    CN110386818A

  • JP1974003631A

  • Method for manufacturing terbium-aluminum-based paramagnetic garnet single crystal

    JP2004131369A

  • Translucent rare earth-gallium garnet sintered compact, its manufacturing method and magneto-optical device

    JP2009143751A

  • Transparent ceramic, method of manufacturing the same, and magneto-optical device

    JP2012206935A