Epoxy resin compositions, cured products, and electrical and electronic parts

A tailored epoxy resin composition with controlled components and additives enhances optical and electrical properties, addressing the limitations of existing hydrogenated bisphenol-type epoxy resins by improving curability, crack resistance, and heat resistance for electronic applications.

JP7582194B2Active Publication Date: 2024-11-13MITSUBISHI CHEM CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2021540731
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-08-22
Filing Date
2020-08-07
Publication Date
2024-11-13
Estimated Expiration
2040-08-07

AI Technical Summary

Technical Problem

Existing hydrogenated bisphenol-type epoxy resins exhibit insufficient optical properties, curability, crack resistance, and heat resistance in cured products, failing to meet the stringent requirements of the electronics industry.

Method used

A specific epoxy resin composition comprising 89.0-99.9% of epoxy resin (1) and 0.1-11.0% of epoxy resin (2) or (3), with controlled chlorine content, epoxy equivalent weight, and low Hazen color number, combined with a curing agent, to enhance electrical and optical properties and improve crack resistance and heat resistance.

Benefits of technology

The composition achieves excellent electrical and optical properties, enabling cured products with superior curability, crack resistance, and heat resistance, suitable for electrical and electronic applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582194000001
    Figure 0007582194000001
  • Figure 0007582194000002
    Figure 0007582194000002
  • Figure 0007582194000003
    Figure 0007582194000003
Patent Text Reader

Abstract

An epoxy resin composition which contains: an epoxy resin (1) having a structure represented by formula (1); and an epoxy resin (2) having a structure represented by formula (2) and / or an epoxy resin (3) having a structure represented by formula (3). From 89.0% by mass to 99.9% by mass of the epoxy resin (1) and from 0.1% by mass to 11.0% by mass of the epoxy resin (2) and / or the epoxy resin (3) are contained in a total of 100% by mass of the epoxy resin (1) and the epoxy resin (2) and / or the epoxy resin (3).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an epoxy resin composition, a cured product, and an electric / electronic part. In particular, the present invention relates to an epoxy resin composition (A) having excellent electrical and optical properties, an epoxy resin composition (B) having excellent curability obtained by blending a curing agent with the epoxy resin composition (A), and a cured product having excellent crack resistance and heat resistance obtained by curing the epoxy resin composition (B), and an electric / electronic part. [Background technology]

[0002] Epoxy resins, when cured with various curing agents, generally become cured products with excellent mechanical properties, heat resistance, electrical properties, etc., and are therefore used in a wide range of fields, including adhesives, paints, and electrical and electronic materials. In particular, hydrogenated bisphenol-type epoxy resins, which are aromatic epoxy resins with hydrogen added, are widely used in the optical field.

[0003] Patent Document 1 describes a method for producing a glycidyl group-containing alicyclic compound having a low chlorine content in the presence of an ether group-containing alcohol, and a low-viscosity epoxy resin composition containing the glycidyl group-containing alicyclic compound and having excellent electrical insulation properties and weather resistance.

[0004] Patent Document 2 discloses a method for producing a hydrogenated bisphenol-type epoxy resin by cyclizing and hydrogenating a bisphenol A-type epoxy resin and a bisphenol F-type epoxy resin in the presence of a specific heterogeneous ruthenium catalyst supported on silicon dioxide.

[0005] Patent Document 3 describes a method for producing an alicyclic epoxy compound having an improved hue by selectively hydrogenating an aromatic ring of an aromatic epoxy compound in the presence of a hydrogenation catalyst, the reaction being carried out in the presence of a reaction solvent having an ester solvent content of 50 mass%.

[0006] [Patent Document 1] JP 2002-97251 A [Patent Document 2] Special Publication No. 2007-515276 [Patent Document 3] JP 2003-212955 A

[0007] With the remarkable development of the electronics industry in recent years, the levels required for optical materials in terms of electrical properties, optical properties, hardening properties, crack resistance, and heat resistance are becoming increasingly strict.

[0008] The hydrogenated bisphenol-type epoxy resins described in Patent Documents 1 to 3 were insufficient in terms of optical properties such as transparency, curability when formed into a cured product, crack resistance and heat resistance of the cured product, and the like. Summary of the Invention

[0009] The present invention aims to provide an epoxy resin composition (A) having excellent electrical and optical properties, an epoxy resin composition (B) containing the epoxy resin composition (A) and having excellent curing properties, and a cured product and an electric / electronic part obtained by curing the epoxy resin composition (B) having excellent crack resistance and heat resistance.

[0010] The present inventors have found that the above-mentioned problems can be solved by an epoxy resin composition (A) having a specific composition, and an epoxy resin composition (B) containing the epoxy resin composition (A) and a curing agent, and have thus completed the invention.

[0011] That is, the gist of the present invention lies in the following [1] to [9].

[0012] [1] An epoxy resin composition comprising an epoxy resin having a structure represented by the following formula (1) (hereinafter referred to as "epoxy resin (1)"), and an epoxy resin having a structure represented by the following formula (2) (hereinafter referred to as "epoxy resin (2)") and / or an epoxy resin having a structure represented by the following formula (3) (hereinafter referred to as "epoxy resin (3)"), wherein the epoxy resin composition (A) contains 89.0 to 99.9 mass% of the epoxy resin (1) and 0.1 to 11.0 mass% of the epoxy resin (2) and / or the epoxy resin (3) in a total of 100 mass% of the epoxy resin (1), the epoxy resin (2) and / or the epoxy resin (3).

[0013] [ka]

[0014] In the above formulas (1), (2), and (3), X is a divalent linking group selected from a direct bond, -SO2-, -O-, -CO-, -C(CF3)2-, -S-, or a hydrocarbon group having 1 to 20 carbon atoms. 1 are hydrogen atoms, hydrocarbon groups having 1 to 10 carbon atoms, or halogen atoms, and may be the same or different. Two R 1 may be bonded to each other to form a ring structure having 4 to 20 carbon atoms. n is an integer of 0 to 2.

[0015] [2] In the formulas (1) to (3), X is an isopropylidene group, and R 1 The epoxy resin composition (A) according to [1], wherein is a hydrogen atom, and n is 0.

[0016] [3] The epoxy resin composition (A) according to [1] or [2], having a total chlorine content (in accordance with JIS K7043-3) of 1000 ppm or less.

[0017] [4] The epoxy resin composition (A) according to any one of [1] to [3], having an epoxy equivalent of 176 to 186 g / equivalent.

[0018] [5] The epoxy resin composition (A) according to any one of [1] to [4], which has a Hazen color number value (APHA value: in accordance with ISO 6271-2:2004) of 12 or less.

[0019] [6] An epoxy resin composition (B) comprising 0.01 to 1,000 parts by mass of a curing agent based on 100 parts by mass of the epoxy resin composition (A) according to any one of [1] to [5].

[0020] [7] A cured product obtained by curing the epoxy resin composition (B) described in [6].

[0021] [8] An electric or electronic part obtained by curing the epoxy resin composition (B) described in [6].

[0022] [9] An optical component obtained by curing the epoxy resin composition (B) according to [6]. Effect of the Invention

[0023] According to the present invention, there are provided an epoxy resin composition (A) having excellent electrical and optical properties, an epoxy resin composition (B) containing the epoxy resin composition (A) and having excellent curing properties, and a cured product and an electric / electronic part obtained by curing the epoxy resin composition (B) having excellent crack resistance and heat resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] The following is a detailed description of an embodiment of the present invention. The following description is an example of an embodiment of the present invention, and the present invention is not limited to the following description as long as it does not deviate from the gist of the present invention. In this specification, when the expression "~" is used, it is used as an expression including the numerical values ​​or physical property values ​​before and after it.

[0025] [Epoxy resin composition (A)] The epoxy resin composition (A) of the present invention is an epoxy resin composition comprising an epoxy resin having a structure represented by the following formula (1) (hereinafter may be referred to as "epoxy resin (1)"), an epoxy resin having a structure represented by the following formula (2) (hereinafter may be referred to as "epoxy resin (2)"), and / or an epoxy resin having a structure represented by the following formula (3) (hereinafter may be referred to as "epoxy resin (3)"), characterized in that the epoxy resin composition (A) contains 89.0 to 99.9 mass% of the epoxy resin (1) and 0.1 to 11.0 mass% of the epoxy resin (2) and / or the epoxy resin (3) in a total of 100 mass% of the epoxy resin (1), the epoxy resin (2) and / or the epoxy resin (3).

[0026] Hereinafter, the proportion of epoxy resin (1) in the total of 100 mass% of epoxy resin (1) and epoxy resin (2) and / or epoxy resin (3) may be simply referred to as the "epoxy resin (1) content," and the proportion of epoxy resin (2) and / or epoxy resin (3) in the total of 100 mass% of epoxy resin (1) and epoxy resin (2) and / or epoxy resin (3) may be referred to as the "epoxy resin (2) / (3) content."

[0027] [ka]

[0028] In the above formulas (1), (2), and (3), X is a divalent linking group selected from a direct bond, -SO2-, -O-, -CO-, -C(CF3)2-, -S-, or a hydrocarbon group having 1 to 20 carbon atoms. 1 are hydrogen atoms, hydrocarbon groups having 1 to 10 carbon atoms, or halogen atoms, and may be the same or different. Two R 1 may be bonded to each other to form a ring structure having 4 to 20 carbon atoms. n is an integer of 0 to 2.

[0029] The epoxy resin composition (A) of the present invention is specified as an "epoxy resin composition" since it contains multiple components such as epoxy resin (1), epoxy resin (2) and / or epoxy resin (3). However, in the technical field of epoxy resins, an "epoxy resin" may be obtained as a "composition" consisting of multiple components other than a single component. Therefore, the epoxy resin composition (A) of the present invention may be expressed as an "epoxy resin" or sold as an "epoxy resin" in the industry and market. In addition, in the industry, an "epoxy compound (uncured)" is called an "epoxy resin".

[0030] In the above formulas (1) to (3), X is preferably a direct bond or a hydrocarbon group having 1 to 10 carbon atoms, more preferably a direct bond, a methylene group, or an isopropylidene group, and most preferably X is an isopropylidene group.

[0031] R 1 is preferably a hydrogen atom or a methyl group, and most preferably a hydrogen atom.

[0032] In the above formulas (1) to (3), n is preferably 0 to 1, and most preferably 0. As n becomes larger, the molecular weight becomes larger, and therefore the viscosity and softening temperature increase, which may deteriorate the handleability.

[0033] Multiple R in formula (1) 1 When n is 1 or more, the multiple X's may all be the same or different. However, it is preferable that they are the same, since different compounds have different boiling points during the distillation of the epoxy resin (1), making the distillation process difficult. 1 , and similarly for X. X and R in formulas (1) to (3) 1 Although n may be the same or different among the formulas (1) to (3), from the viewpoint of ease of adjusting the content of each component in the epoxy resin composition (A) and ease of production, X, R in each structural formula are 1 It is preferable that n is the same in formulas (1) to (3).

[0034] [Composition of epoxy resin composition (A)] The epoxy resin composition (A) of the present invention contains an epoxy resin (1), an epoxy resin (2) and / or an epoxy resin (3) from the viewpoint of obtaining excellent electrical properties, optical properties, and excellent curability, crack resistance and heat resistance as the epoxy resin composition (B) containing a curing agent, which will be described later, and is characterized in that the epoxy resin (1) is contained in an amount of 89.0 to 99.9 mass% and the epoxy resin (2) and / or the epoxy resin (3) is contained in an amount of 0.1 to 11.0 mass% in a total of 100 mass% of the epoxy resin (1), the epoxy resin (2) and / or the epoxy resin (3). The Hazen color number of the epoxy resin composition (A) tends to be lower as the content of the epoxy resin (1) increases and the content of the epoxy resin (2) and / or the epoxy resin (3) decreases, but when the epoxy resin composition (B) is prepared, the crosslink density increases and the linear expansion coefficient decreases, thereby improving the crack resistance, and the glass transition temperature increases, thereby improving the heat resistance. On the other hand, as the content of the epoxy resin (1) is smaller and the content of the epoxy resin (2) and / or the epoxy resin (3) is larger, the crack resistance and heat resistance of the resulting epoxy resin composition (B) tend to become worse.

[0035] From the viewpoint of more effectively obtaining the effects of the present invention by containing the epoxy resin (1) and the epoxy resin (2) and / or the epoxy resin (3), the content of the epoxy resin (1) is preferably 90.0 to 99.0 mass%, and the content of the epoxy resin (2) and / or the epoxy resin (3) is preferably 1.0 to 10.0 mass%, more preferably the content of the epoxy resin (1) is 92.0 to 98.0 mass%, the content of the epoxy resin (2) and / or the epoxy resin (3) is 2.0 to 8.0 mass%, and particularly preferably the content of the epoxy resin (1) is 95.0 to 98.0 mass%, and the content of the epoxy resin (2) and / or the epoxy resin (3) is 2.0 to 5.0 mass%.

[0036] In the epoxy resin composition (A) of the present invention, the ratio of the epoxy resin (2) and / or the epoxy resin (3) to the epoxy resin (1) is preferably 0.1 to 13 mass %, more preferably 1 to 12 mass %.

[0037] Since the epoxy resin (2) and the epoxy resin (3) have the same molecular weight and the same number of hydroxyl groups, and it is difficult to distinguish between them and analyze their contents, they are described as "epoxy resin (2) and / or epoxy resin (3)" in the present invention. The epoxy resin composition (A) of the present invention may contain only one of the epoxy resin (2) and the epoxy resin (3), or may contain both the epoxy resin (2) and the epoxy resin (3). According to the production method of the epoxy resin composition (A) of the present invention described below, an epoxy resin composition (A) containing both the epoxy resin (2) and the epoxy resin (3) is produced. Since it is difficult to separate the epoxy resin (2) and the epoxy resin (3) by purification or the like, when producing the epoxy resin composition (A) on an industrial scale, it is easier to analyze the content of "epoxy resin (2) and / or epoxy resin (3)" in the epoxy resin composition (A) than to analyze the contents of the epoxy resin (2) and the epoxy resin (3) separately.

[0038] The epoxy resin composition (A) of the present invention may usually contain other components in addition to the above epoxy resins (1) to (3).

[0039] The other components are chlorine impurities produced as by-products in the reaction process in the above formulas (1) to (3) during the production of the epoxy resin composition (A) of the present invention. The chlorine impurities are a general term for organic substances and compounds containing a chlorine atom (Cl), and are, for example, compounds containing a chlorine atom in their structural formula that are produced as by-products during the production of the epoxy resin composition (A).

[0040] The content of other components in the epoxy resin composition (A) of the present invention is preferably 3% by mass or less, more preferably 2% by mass or less, and further preferably 1% by mass or less. If the content of other components is high, the necessary content of the epoxy resins (1) to (3) cannot be ensured, and the effects of improving the electrical properties, optical properties, curability, crack resistance, and heat resistance of the epoxy resin composition (B) cannot be sufficiently obtained. In the epoxy resin composition (A) of the present invention, when other components are contained, the total of the epoxy resins (1) to (3) and the other components is 100 mass %.

[0041] The contents of the epoxy resins (1) to (3) and other components in the epoxy resin composition (A) of the present invention can be measured, for example, by gel permeation chromatography analysis (hereinafter, GPC analysis) under the following conditions. Equipment: Tosoh HLC-8220L GPC Detector: RI Mobile phase: Tetrahydrofuran (containing BHT) Flow rate: 0.8mL / min Column: Tosoh TSKgel G2000Hxl + G1000Hxl x 2 Column temperature: 40℃

[0042] [Epoxy equivalent] The epoxy resin composition (A) of the present invention preferably has an epoxy equivalent of 178 to 186 g / equivalent from the viewpoint of obtaining excellent curability, crack resistance, and heat resistance as the epoxy resin composition (B) containing a curing agent, and more preferably has an epoxy equivalent of 178 to 181 g / equivalent from the viewpoint of further improving the above properties. It is believed that by setting the epoxy equivalent within the above specific range, the above excellent properties can be obtained.

[0043] In the present invention, the "epoxy equivalent" is defined as "the mass of an epoxy resin containing one equivalent of an epoxy group" and can be measured in accordance with JIS K7236-1955.

[0044] [Hazen color number] In the epoxy resin composition (A) of the present invention, from the viewpoint of obtaining excellent optical properties as an epoxy resin, the Hazen color number is preferably 12 or less, and from the viewpoint of further improving the optical properties, this value is more preferably 9 or less, and particularly preferably 8 or less. It is considered that excellent optical properties can be obtained by making the Hazen color number equal to or less than the above upper limit. The lower the Hazen color number, the more preferable, and there is no particular restriction on the lower limit.

[0045] In the present invention, the "Hazen color number" can be measured in accordance with ISO 6271-2:2004.

[0046] [Total chlorine content] In the epoxy resin composition (A) of the present invention, from the viewpoint of obtaining excellent electrical reliability as an epoxy resin, the total chlorine content is preferably 1000 ppm (ppm by mass) or less, and from the viewpoint of further improving electrical reliability, the total chlorine content is more preferably 750 ppm or less, and particularly preferably 700 ppm or less. By making the total chlorine content below the above upper limit, it is possible to obtain a cured product having excellent electrical properties, optical properties, and curing properties when made into an epoxy resin composition (B) containing a curing agent, and excellent crack resistance and heat resistance. The lower the total chlorine content, the more preferable, and there is no particular restriction on the lower limit.

[0047] The "total chlorine content" refers to the content of chlorine atoms (Cl) contained in the epoxy resin composition (A). In the present invention, the "total chlorine content" can be measured in accordance with JIS K7243-3.

[0048] [Method for producing epoxy resin composition (A)] <Raw material aromatic epoxy resin> The method for producing the epoxy resin composition (A) of the present invention is not particularly limited, but it is preferable to produce the epoxy resin composition (A) of the present invention by using an aromatic epoxy resin as a raw material and carrying out a hydrogenation reaction, which makes it possible to efficiently obtain the epoxy resin composition (A) of the present invention.

[0049] A preferred aromatic epoxy resin used as a raw material is an epoxy resin having a structure represented by the following formula (4) (hereinafter, sometimes referred to as "aromatic epoxy resin (4)").

[0050] [ka]

[0051] In the above formula (4), R 1 , X and n are the same as those in formulas (1) to (3).

[0052] Specific examples of the aromatic epoxy resin (4) include bisphenol type epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, 3,3',5,5'-tetramethyl-4,4'-biphenol type epoxy resins, and 4,4'-biphenol type epoxy resins; bisphenol A novolac type epoxy resins; and naphthalene diol type epoxy resins. Among these, bisphenol A type epoxy resins are more preferred. These aromatic epoxy resins (4) may be used alone or in combination of two or more.

[0053] As the aromatic epoxy resin (4), it is preferable to use one having the following qualities, since it is suitable as a raw material prior to the hydrogenation reaction for efficiently obtaining the epoxy resin composition (A) of the present invention.

[0054] The epoxy equivalent of the aromatic epoxy resin (4) is preferably 165 to 194 g / equivalent, from the viewpoint of adjusting the content of the epoxy resin (1) in the epoxy resin composition (A) to the above-mentioned preferred range. The total chlorine content of the aromatic epoxy resin (4) is preferably 2000 ppm or less, particularly preferably 1500 ppm or less, from the viewpoint of keeping the total chlorine content of the epoxy resin composition (A) at 1000 ppm or less.

[0055] <Distillation of aromatic epoxy resin> The epoxy resin composition (A) of the present invention is preferably produced by carrying out a hydrogenation reaction of an aromatic epoxy resin (4). From the viewpoint of facilitating control of the ratios and contents of the epoxy resins (1) to (3) in the epoxy resin composition (A) and further the total amount of chlorine, it is preferred to previously distill the aromatic epoxy resin (4) before subjecting it to the hydrogenation reaction.

[0056] In this case, the time for distillation is not particularly limited, but is preferably 5 to 30 hours, more preferably 6 to 15 hours. The temperature and pressure during distillation are not particularly limited, but the temperature is preferably 130 to 240° C., more preferably 210 to 230° C. If the distillation temperature is too high, the aromatic epoxy resin (4) may decompose. If the distillation temperature is too low, the pressure must be reduced to a high vacuum, which is not an industrially advantageous method. The distillation pressure is preferably reduced to a degree of 0.001 to 1 Torr, and more preferably to a degree of 0.001 to 0.01 Torr.

[0057] The distillation is preferably carried out under conditions of a fraction of 70% or less, for example, 40 to 60%. If the distillation is carried out under conditions of a fraction of more than 70%, the amount of oligomer components in the aromatic epoxy resin (4) increases, and it tends to become difficult to control the content of each component of the epoxy resin composition (A) of the present invention within the above-mentioned preferred range.

[0058] The distillation method is not particularly limited, but distillation using a thin film still is preferred.

[0059] The properties of the aromatic epoxy resin (4) obtained by distillation are not particularly limited, but the epoxy equivalent is preferably 165 to 180 g / equivalent from the viewpoint of easily adjusting the content of the epoxy resin (1) in the epoxy resin composition (A) to the above-mentioned preferred range. The total chlorine content is preferably 1500 ppm or less, particularly preferably 1000 ppm or less.

[0060] <Hydrogenation reaction> The hydrogenation catalyst used in the hydrogenation reaction is preferably a catalyst containing a platinum group element as an active component. Among these, a rhodium catalyst or a ruthenium catalyst is preferred. The hydrogenation catalyst is preferably a catalyst in which an active component is supported on a carbon-based carrier. Examples of the carbon-based carrier include activated carbon, graphite, and carbon black. Among these, activated carbon or graphite called high surface area graphite is particularly preferred. The specific surface area of ​​the carbon-based carrier is usually 5 to 3,000 m. 2 / g, preferably 50 to 1500m 2 / g, and the particle size is usually 5 to 500 μm.

[0061] The hydrogenation catalyst may be prepared, for example, by the method described in JP-A-11-217379. The amount of catalytic metal component mixed into the obtained epoxy resin composition (A) varies depending on the hydrogenation catalyst preparation method, but the catalytic metal component can be removed in the purification step described below.

[0062] From the viewpoint of improving the color of the resulting epoxy resin composition (A), the hydrogenation reaction is preferably carried out in the presence of a reaction solvent having an ester solvent content of 50% by mass or more.

[0063] Examples of ester solvents include fatty acid esters, carbonates, lactones, etc., and fatty acid esters are particularly preferred. From the viewpoint of handling, fatty acid esters having a boiling point in the range of 50 to 180°C under normal pressure are preferred. Examples of such fatty acid esters include methyl acetate, ethyl acetate, propyl acetate, butyl acetate, amyl acetate, methyl propionate, propyl propionate, butyl propionate, methyl butyrate, ethyl butyrate, and methyl isovalerate. Among these, acetate and propionate are preferred. Specifically, ethyl acetate, propyl acetate, butyl acetate, and methyl propionate are preferred, and ethyl acetate is particularly preferred.

[0064] The ester solvent may be used in combination with an ether solvent, an alcohol solvent, or a paraffin solvent, which are widely used in the prior art. In this case, the ratio of the ester solvent to the mixed solvent is usually 50% by mass or more, preferably 90% by mass or more. It is preferable that the ether solvent is substantially free of the mixed solvent, and specifically, the content of the ether solvent is preferably 1% by mass or less.

[0065] The amount of reaction solvent used, expressed as a mass ratio to the raw material aromatic epoxy resin (4), is usually 0.05 to 10, preferably 0.1 to 3. If the amount of reaction solvent is too small, the viscosity of the raw material is generally high, which leads to poor diffusion of hydrogen, a decrease in reaction rate, and a decrease in the selectivity of the hydrogenation reaction. If the amount of reaction solvent is too large, the productivity decreases, which is economically disadvantageous.

[0066] The reaction temperature is usually 30 to 150° C., preferably 50 to 130° C. If the reaction temperature is too low, the reaction rate decreases, and a large amount of hydrogenation catalyst and a long time are required to complete the reaction. If the reaction temperature is too high, not only does the occurrence of side reactions such as hydrogenolysis of epoxy groups increase, but the amount of eluted catalyst metal components increases, resulting in a decrease in the quality of the obtained epoxy resin composition (A).

[0067] The reaction pressure is usually 1 to 30 MPa, preferably 3 to 15 MPa. If the reaction pressure is too low, the reaction rate decreases, and a large amount of hydrogenation catalyst and a long time are required to complete the reaction. If the reaction pressure is too high, the necessary equipment becomes large-scale, which is economically disadvantageous.

[0068] The reaction can be carried out in a liquid phase suspension reaction or a fixed bed reaction, with the liquid phase suspension reaction being particularly preferred.

[0069] Hydrogen may be introduced in a flow-through manner or in the amount to be consumed. Hydrogen may be introduced and dispersed in the liquid. Hydrogen may also be absorbed by entraining it in the liquid from the gas phase by stirring or other means. The end point of the reaction may be determined by monitoring hydrogen absorption or by sampling and analysis. The hydrogenation rate of the aromatic rings in the aromatic epoxy resin (4) is preferably 85% or more, and can be even higher.

[0070] After the reaction is completed, if necessary, the catalyst is separated from the reaction solution by an operation such as filtration or centrifugation, and then the reaction solvent is distilled off to obtain the target product. The reaction solvent is distilled off under reduced pressure, usually at 50 to 200°C, preferably 70 to 150°C. From the viewpoint of the impact on the environment during use, particularly odor, the remaining amount of the reaction solvent is usually 1 mass% or less, preferably 0.2 mass% or less. The lower limit of the remaining amount of the reaction solvent is usually 0.001 mass%. Distilling off the reaction solvent beyond this amount requires long-term heating, and there is a concern that the stability of the obtained epoxy resin composition (A) will decrease. To further reduce the remaining amount of the reaction solvent, it is effective to introduce an inert gas such as nitrogen.

[0071] The concentration of the catalytic metal component in the epoxy resin composition (A) obtained by such a hydrogenation reaction is usually 0.01 to 50 ppm. In addition to using an ester-based solvent as the solvent, the concentration of the catalytic metal component in the epoxy resin composition (A) can be made to be such a low concentration by selecting the preparation of the catalyst used in the hydrogenation reaction and the conditions of the hydrogenation reaction. Furthermore, in order to reliably further reduce the concentration of the catalytic metal component in the epoxy resin composition (A), it is more preferable to carry out a purification step using an adsorbent as described below.

[0072] <Purification process> Examples of adsorbents used in the purification process include activated carbon, activated clay, ion exchange resins, and synthetic adsorbents. Among these, activated carbon is preferred. There are no particular limitations on the type of activated carbon, and various types of activated carbon produced from various raw materials such as coconut shells, wood, and coal can be used. The specific surface area of ​​the activated carbon is 500 to 3000 m 2 / g range is preferred. The active surface of the adsorbent may be acidic, neutral or basic, but is preferably basic. Examples of such basic adsorbents include solid basic compounds such as magnesium oxide, and basic ion exchange resins.

[0073] The purification step may be carried out by either batch contact treatment using a powder adsorbent or flow treatment through a packed bed of granular adsorbent. As the powder adsorbent, an adsorbent having an average particle size of 1 to 1000 μm is preferable. As the granular adsorbent, an adsorbent having an average particle size of 1 to 10 mm is preferable.

[0074] The amount of the adsorbent used varies depending on the type of adsorbent, but is usually 0.01 to 100% by mass, preferably 0.1 to 20% by mass, and more preferably 0.2 to 10% by mass, based on the epoxy resin composition to be purified.

[0075] The temperature during the adsorption treatment is usually 0 to 100° C., preferably 10 to 80° C. The adsorption treatment is preferably carried out in a state containing a solvent, from the viewpoints of workability, recovery rate, adsorption efficiency, etc. The type of solvent is not particularly limited as long as it dissolves the epoxy resin.

[0076] The above purification step is usually carried out before concentrating the hydrogenation reaction liquid, so the reaction solvent is preferably used as it is during the adsorption treatment. The content of the solvent is usually 5 to 80 mass % as the concentration in the liquid to be subjected to the adsorption treatment. If the amount of the solvent is too small, the viscosity of the treatment liquid increases, and the adsorption efficiency decreases.

[0077] The adsorption treatment can also be carried out by adding an adsorbent to the reaction liquid after the hydrogenation reaction without separating the hydrogenation catalyst, mixing the reaction liquid with the adsorbent, and subjecting both the catalyst and the adsorbent to solid-liquid separation. This method has the following advantages.

[0078] That is, when the catalyst is subjected to solid-liquid separation without adding an adsorbent to the reaction liquid after the hydrogenation reaction, the solid-liquid separation property is reduced due to the stickiness of the organic matter attached to the catalyst surface. In contrast, when the catalyst is subjected to solid-liquid separation together with an adsorbent (especially activated carbon) according to the above method, the solid-liquid separation property is extremely good. Even with this method, the catalyst removal efficiency is hardly changed. When the catalyst is subjected to solid-liquid separation together with an adsorbent, the amount of the adsorbent used is preferably 1 to 30 times by mass relative to the catalyst.

[0079] The contents of the epoxy resins (1) to (3) in the epoxy resin composition (A) of the present invention can be controlled by carrying out the reaction in a combination of the respective requirements for the reaction conditions of the above-mentioned hydrogenation reaction.

[0080] [Epoxy resin composition (B)] The epoxy resin composition (B) of the present invention contains at least the above-mentioned epoxy resin composition (A) of the present invention and a curing agent. The epoxy resin composition (B) of the present invention may be appropriately blended with other epoxy resins than the epoxy resin composition (A) of the present invention (hereinafter, may be simply referred to as "other epoxy resins"), curing accelerators, inorganic fillers, coupling agents, etc., as necessary.

[0081] The epoxy resin composition (B) of the present invention, which contains the epoxy resin composition (A) of the present invention, is excellent in curing properties such as curability, and gives a cured product that fully satisfies various physical properties required for various applications. The epoxy resin composition (B) of the present invention, which has excellent curing properties, can realize improvement in productivity in application to various applications.

[0082] [Hardening agent] In the present invention, the curing agent refers to a substance that contributes to the crosslinking reaction and / or chain extension reaction between epoxy groups of an epoxy resin. In the present invention, even substances that are usually called "curing accelerators" are considered to be curing agents as long as they contribute to the crosslinking reaction and / or chain extension reaction between epoxy groups of the epoxy resin.

[0083] In the epoxy resin composition (B) of the present invention, the content of the curing agent is preferably 0.1 to 1000 parts by mass, more preferably 500 parts by mass or less, and further preferably 300 parts by mass or less, based on 100 parts by mass of the total epoxy resin components as solid contents. In the present invention, the term "solid content" refers to components excluding the solvent, and includes not only solid epoxy resins but also semi-solid and viscous liquid substances. The "total epoxy resin components" corresponds to the amount of epoxy resin contained in the epoxy resin composition (B) of the present invention. When the epoxy resin composition (B) of the present invention contains only the epoxy resin composition (A), the amount of epoxy resin in the epoxy resin composition (A) corresponds to this. When the epoxy resin composition (B) of the present invention contains the epoxy resin composition (A) and other epoxy resins, the amount of epoxy resin in the epoxy resin composition (A) corresponds to this.

[0084] The curing agent is not particularly limited, and any agent generally known as an epoxy resin curing agent can be used, such as phenol-based curing agents, amine-based curing agents such as aliphatic amines, polyether amines, alicyclic amines, and aromatic amines, acid anhydride-based curing agents, isocyanuric acid derivative-based curing agents, amide-based curing agents, tertiary amines, and imidazoles.

[0085] Among these, by including an acid anhydride curing agent, an isocyanuric acid derivative-based curing agent, or a phenol-based curing agent, the epoxy resin composition (B) of the present invention can obtain excellent curing properties, crack resistance, and heat resistance. Therefore, it is preferable that the curing agent includes an acid anhydride curing agent, an isocyanuric acid derivative-based curing agent, or a phenol-based curing agent. From the viewpoint of heat resistance, etc., it is preferable to contain an acid anhydride-based curing agent or an isocyanuric acid derivative-based curing agent. It is also preferable to use imidazoles from the viewpoint of sufficiently progressing the curing reaction and improving heat resistance.

[0086] The curing agent may be used alone or in combination of two or more. When two or more curing agents are used in combination, they may be mixed in advance to prepare a mixed curing agent and then used, or when mixing the components of the epoxy resin composition (B), each component of the curing agent may be added separately and mixed at the same time.

[0087] <Acid anhydride curing agent> Examples of the acid anhydride-based curing agent include acid anhydrides and modified products of acid anhydrides. Examples of acid anhydrides include phthalic anhydride, maleic anhydride, trimellitic anhydride, pyromellitic anhydride, benzophenone tetracarboxylic anhydride, dodecenylsuccinic anhydride, polyadipic anhydride, polyazelaic anhydride, polysebacic anhydride, poly(ethyloctadecanedioic) anhydride, poly(phenylhexadecanedioic) anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, hexahydrophthalic anhydride, methylhymic anhydride, and methylhexahydrophthalic anhydride. Acid anhydrides, trialkyltetrahydrophthalic anhydride, methylcyclohexene dicarboxylic anhydride, methylcyclohexene tetracarboxylic anhydride, ethylene glycol bistrimellitate dianhydride, HET anhydride, nadic anhydride, methylnadic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexane-1,2-dicarboxylic anhydride, 3,4-dicarboxy-1,2,3,4-tetrahydro-1-naphthalene succinic dianhydride, 1-methyl-dicarboxy-1,2,3,4-tetrahydro-1-naphthalene succinic dianhydride, glutaric anhydride, dimethylglutaric anhydride, diethylglutaric anhydride, succinic anhydride, and the like.

[0088] Of these acid anhydride curing agents, it is preferable to use phthalic anhydride, trimellitic anhydride, hexahydrophthalic anhydride, tetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, glutaric anhydride, dimethylglutaric anhydride, or diethylglutaric anhydride.

[0089] The modified acid anhydride may be, for example, the above-mentioned acid anhydride modified with glycol. Examples of glycols that can be used for modification include alkylene glycols such as ethylene glycol, propylene glycol, and neopentyl glycol, and polyether glycols such as polyethylene glycol, polypropylene glycol, and polytetramethylene ether glycol. Furthermore, copolymer polyether glycols of two or more of these glycols and / or polyether glycols may also be used.

[0090] In the case of modified acid anhydrides, the amount of glycol modified is 0.4 moles or less per mole of acid anhydride. When the amount of modification is not more than the above upper limit, the viscosity of the epoxy resin composition does not become too high, and the workability tends to be good, and the rate of the curing reaction with the epoxy resin also tends to be good.

[0091] The acid anhydride curing agents listed above may be used alone or in any combination of two or more in any amount.

[0092] When an acid anhydride curing agent is used, it is preferable to use it so that the equivalent ratio of the functional groups in the curing agent to the epoxy groups in all epoxy resin components in the epoxy resin composition (B) is in the range of 0.8 to 1.5. If it is within this range, it is preferable because unreacted epoxy groups and functional groups of the curing agent are less likely to remain.

[0093] <Isocyanuric acid derivative curing agent> Examples of the isocyanuric acid derivative curing agent include 1,3,5-tris(1-carboxymethyl)isocyanurate, 1,3,5-tris(2-carboxyethyl)isocyanurate, 1,3,5-tris(3-carboxypropyl)isocyanurate, and 1,3-bis(2-carboxyethyl)isocyanurate.

[0094] Of these isocyanuric acid derivative-based curing agents, it is preferable to use 1,3,5-tris(3-carboxypropyl)isocyanurate.

[0095] The isocyanuric acid derivative-based curing agents listed above may be used alone or in any combination of two or more in any amount.

[0096] When an isocyanuric acid derivative-based curing agent is used, it is preferable to use it so that the equivalent ratio of the functional groups in the curing agent to the epoxy groups in all epoxy resin components in the epoxy resin composition (B) is in the range of 0.8 to 1.5. If it is within this range, it is preferable because unreacted epoxy groups and functional groups of the curing agent are less likely to remain.

[0097] <Phenol-based hardener> Examples of phenol-based curing agents include novolak-type phenolic resins obtained by condensing or co-condensing phenols such as phenol, cresol, resorcin, catechol, bisphenol A, bisphenol F, phenylphenol, and aminophenol, and / or naphthols such as α-naphthol, β-naphthol, and dihydroxynaphthalene with compounds having an aldehyde group such as formaldehyde, benzaldehyde, and salicylaldehyde under an acidic catalyst; phenol-aralkyl resins synthesized from phenols and / or naphthols and dimethoxy-paraxylene or bis(methoxymethyl)biphenyl; and biphenylene-type phenolic resins. These include aralkyl-type phenolic resins such as phenol aralkyl resins and naphthol aralkyl resins; dicyclopentadiene-type phenolic resins such as dicyclopentadiene-type phenolic novolac resins and dicyclopentadiene-type naphthol novolac resins, which are synthesized by copolymerizing phenols and / or naphthols with dicyclopentadiene; triphenylmethane-type phenolic resins; terpene-modified phenolic resins; paraxylylene and / or metaxylylene-modified phenolic resins; melamine-modified phenolic resins; cyclopentadiene-modified phenolic resins; and phenolic resins obtained by copolymerizing two or more of these.

[0098] The amount of the phenol-based curing agent is preferably 0.1 to 1000 parts by mass, more preferably 500 parts by mass or less, further preferably 300 parts by mass or less, and particularly preferably 100 parts by mass or less, based on 100 parts by mass of all epoxy resin components in the epoxy resin composition (B).

[0099] <Amine-based hardener> Examples of amine-based hardeners (excluding tertiary amines) include aliphatic amines, polyamines, Examples of the amines include triether amines, alicyclic amines, and aromatic amines.

[0100] Examples of aliphatic amines include ethylenediamine, 1,3-diaminopropane, 1,4-diaminopropane, hexamethylenediamine, 2,5-dimethylhexamethylenediamine, trimethylhexamethylenediamine, diethylenetriamine, iminobispropylamine, bis(hexamethylene)triamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, N-hydroxyethylethylenediamine, and tetra(hydroxyethyl)ethylenediamine.

[0101] Examples of polyetheramines include triethylene glycol diamine, tetraethylene glycol diamine, diethylene glycol bis(propylamine), polyoxypropylene diamine, polyoxypropylene triamines, and the like.

[0102] Examples of alicyclic amines include isophoronediamine, methacenediamine, N-aminoethylpiperazine, bis(4-amino-3-methyldicyclohexyl)methane, bis(aminomethyl)cyclohexane, 3,9-bis(3-aminopropyl)-2,4,8,10-tetraoxaspiro(5,5)undecane, and norbornenediamine.

[0103] Examples of aromatic amines include tetrachloro-p-xylylenediamine, m-xylylenediamine, p-xylylenediamine, m-phenylenediamine, o-phenylenediamine, p-phenylenediamine, 2,4-diaminoanisole, 2,4-toluenediamine, 2,4-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 4,4'-diamino-1,2-diphenylethane, 2,4-diaminodiphenylsulfone, 4,4'-diaminodiphenylsulfone, m-aminophenol, m-aminobenzylamine, benzyldimethylamine, 2-(dimethylaminomethyl)phenol, triethanolamine, methylbenzylamine, α-(m-aminophenyl)ethylamine, α-(p-aminophenyl)ethylamine, diaminodiethyldimethyldiphenylmethane, and α,α'-bis(4-aminophenyl)-p-diisopropylbenzene.

[0104] The amine-based curing agents listed above may be used alone or in any combination of two or more in any blend ratio.

[0105] The amine-based curing agent is preferably used so that the equivalent ratio of the functional groups in the curing agent to the epoxy groups in all the epoxy resin components contained in the epoxy resin composition (B) is in the range of 0.8 to 1.5. If it is within this range, it is preferable because unreacted epoxy groups and functional groups of the curing agent are less likely to remain.

[0106] Examples of tertiary amines include 1,8-diazabicyclo(5,4,0)triethylenediamine7, triethylenediamine, benzyldimethylamine, triethanolamine, dimethylaminoethanol, tris(dimethylaminomethyl)phenol, dimethylaminomethylphenol, and the like.

[0107] The tertiary amines listed above may be used alone or in any combination of two or more kinds in any blend ratio.

[0108] The tertiary amine is preferably used so that the equivalent ratio of the functional group in the curing agent to the epoxy group in all epoxy resin components contained in the epoxy resin composition (B) is in the range of 0.8 to 1.5. If it is within this range, it is preferable because unreacted epoxy groups and functional groups of the curing agent are less likely to remain.

[0109] <Amide-based hardener> Examples of the amide-based curing agent include dicyandiamide and its derivatives, polyamide resins, and the like.

[0110] The amide-based curing agent may be used alone or in any combination and ratio of two or more kinds.

[0111] When an amide-based curing agent is used, it is preferable to use the amide-based curing agent in an amount of 0.1 to 20 mass % based on the total amount of all epoxy resin components and the amide-based curing agent in the epoxy resin composition (B).

[0112] <Imidazoles> Examples of imidazoles include 2-phenylimidazole, 2-ethyl-4(5)-methylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyano-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl- Examples include 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, and adducts of epoxy resins and the above-mentioned imidazoles. Since imidazoles have catalytic activity, they can generally be classified as curing accelerators, but in the present invention they are classified as curing agents.

[0113] The imidazoles listed above may be used alone or in any combination and ratio of two or more.

[0114] When imidazoles are used, the amount of the imidazoles is preferably 0.1 to 20% by mass based on the total amount of all epoxy resin components and imidazoles in the epoxy resin composition (B).

[0115] <Other hardeners> In addition to the above curing agents, other curing agents can be used in the epoxy resin composition (B) of the present invention. There are no particular limitations on the other curing agents that can be used in the epoxy resin composition (B) of the present invention, and any curing agent generally known as a curing agent for epoxy resins can be used. The other curing agents may be used alone or in combination of two or more.

[0116] [Other epoxy resins] The epoxy resin composition (B) of the present invention may further contain other epoxy resins in addition to the epoxy resin composition (A). By containing other epoxy resins, the heat resistance, stress resistance, moisture absorption resistance, flame retardancy, etc. of the epoxy resin composition (B) of the present invention can be improved.

[0117] The other epoxy resins that can be used in the epoxy resin composition (B) of the present invention include all epoxy resins other than the epoxy resins (mainly the epoxy resins (1) to (3)) contained in the epoxy resin composition (A). Specific examples include bisphenol A type epoxy resins, trisphenolmethane type epoxy resins, anthracene type epoxy resins, phenol-modified xylene resin type epoxy resins, bisphenolcyclododecyl type epoxy resins, bisphenoldiisopropylideneresorcin type epoxy resins, bisphenolF type epoxy resins, bisphenolAD type epoxy resins, hydroquinone type epoxy resins, methylhydroquinone type epoxy resins, dibutylhydroquinone type epoxy resins, resorcin type epoxy resins, methylresorcin type epoxy resins, biphenol type epoxy resins, tetramethylbiphenol type epoxy resins other than the epoxy resins (1) and (2) in the epoxy resin composition (A), tetramethylbisphenolF type epoxy resins, dihydroxydiphenylether type epoxy resins, epoxy resins derived from thiodiphenols, dihydroxynaphthalene type epoxy resins, dihydroxyanthracene type epoxy resins, dihydroxydihydroanthracene type epoxy resins, dicyclopentadiene type epoxy resins, dihydroxyxylene ... Examples of epoxy resins include epoxy resins derived from cystilbenes, phenol novolac type epoxy resins, cresol novolac type epoxy resins, bisphenol A novolac type epoxy resins, naphthol novolac type epoxy resins, phenol aralkyl type epoxy resins, naphthol aralkyl type epoxy resins, biphenyl aralkyl type epoxy resins, terpene phenol type epoxy resins, dicyclopentadiene phenol type epoxy resins, epoxy resins derived from a condensate of phenol and hydroxybenzaldehyde, epoxy resins derived from a condensate of phenol and crotonaldehyde, epoxy resins derived from a condensate of phenol and glyoxal, epoxy resins derived from co-condensation resins of heavy oil or pitches, phenols, and formaldehydes, epoxy resins derived from diaminodiphenylmethane, epoxy resins derived from aminophenols, epoxy resins derived from xylenediamine, epoxy resins derived from methylhexahydrophthalic acid, and epoxy resins derived from dimer acids. These may be used alone or in any combination of two or more in any blend ratio.

[0118] [Cure accelerator] The epoxy resin composition (B) of the present invention preferably contains a curing accelerator, which makes it possible to shorten the curing time and lower the curing temperature, and therefore makes it easier to obtain a desired cured product.

[0119] The curing accelerator is not particularly limited, but specific examples include organic phosphines, phosphorus compounds such as phosphonium salts, tetraphenylboron salts, organic acid dihydrazides, boron halide amine complexes, and the like.

[0120] Phosphorus compounds that can be used as curing accelerators include triphenylphosphine, diphenyl(p-tolyl)phosphine, tris(alkylphenyl)phosphine, tris(alkoxyphenyl)phosphine, tris(alkyl alkoxyphenyl)phosphine, tris(dialkylphenyl)phosphine, tris(trialkylphenyl)phosphine, tris(tetraalkylphenyl)phosphine, tris(dialkoxyphenyl)phosphine, tris(trialkoxyphenyl)phosphine, tris(tetraalkoxyphenyl)phosphine, trialkylphosphine, Examples of such organic phosphines include organic phosphines such as phosphine, dialkylarylphosphine, and alkyldiarylphosphine; complexes of such organic phosphines with organic borons; and compounds obtained by adding such organic phosphines to quinone compounds such as maleic anhydride, 1,4-benzoquinone, 2,5-toluquinone, 1,4-naphthoquinone, 2,3-dimethylbenzoquinone, 2,6-dimethylbenzoquinone, 2,3-dimethoxy-5-methyl-1,4-benzoquinone, 2,3-dimethoxy-1,4-benzoquinone, and phenyl-1,4-benzoquinone, and compounds such as diazophenylmethane.

[0121] Among the above-listed curing accelerators, organic phosphines and phosphonium salts are preferred, and organic phosphines are most preferred.

[0122] The curing accelerator may be used alone or in any combination and ratio of two or more of the above-listed curing accelerators.

[0123] The curing accelerator is used in an amount of 100 parts by mass of the total epoxy resin components in the epoxy resin composition (B). It is preferably used in the range of 0.1 to 20 parts by weight, more preferably 0.5 parts by weight or more, even more preferably 1 part by weight or more, more preferably 15 parts by weight or less, and even more preferably 10 parts by weight or less. When the content of the curing accelerator is equal to or more than the lower limit, a good curing acceleration effect can be obtained. When the content of the curing accelerator is equal to or less than the upper limit, the desired curing properties are easily obtained.

[0124] [Inorganic filler] The epoxy resin composition (B) of the present invention may contain an inorganic filler. Examples of inorganic fillers include fused silica, crystalline silica, glass powder, alumina, calcium carbonate, calcium sulfate, talc, boron nitride, titanium oxide, etc. These may be used alone or in any combination of two or more in any ratio.

[0125] When an inorganic filler is used in the epoxy resin composition (B) of the present invention, the inorganic filler is preferably blended in an amount of 60 to 95% by mass based on the total epoxy resin composition (B).

[0126] [Release agent] A mold release agent can be blended into the epoxy resin composition (B) of the present invention. Examples of the mold release agent include natural waxes such as carnauba wax, synthetic waxes such as polyethylene wax, higher fatty acids such as stearic acid and zinc stearate and their metal salts, and hydrocarbon-based mold release agents such as paraffin. These may be used alone or in any combination of two or more kinds in any blending ratio.

[0127] When a release agent is blended in the epoxy resin composition (B) of the present invention, the blending amount of the release agent is preferably 0.1 to 5.0 parts by mass, more preferably 0.5 to 3.0 parts by mass, based on 100 parts by mass of the total epoxy resin components in the epoxy resin composition (B). When the blending amount of the release agent is within the above range, it is preferable because good release properties can be exhibited while maintaining the curing characteristics of the epoxy resin composition (B).

[0128] [Coupling agent] It is preferable to blend a coupling agent in the epoxy resin composition (B) of the present invention. The coupling agent is preferably used in combination with an inorganic filler, and blending the coupling agent can improve the adhesion between the epoxy resin matrix and the inorganic filler.

[0129] The coupling agent includes a silane coupling agent, a titanate coupling agent, and the like.

[0130] Examples of the silane coupling agent include epoxy silanes such as γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; amino silanes such as γ-aminopropyltriethoxysilane, N-β(aminoethyl)γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropylmethyldimethoxysilane, γ-aminopropyltrimethoxysilane, and γ-ureidopropyltriethoxysilane; mercapto silanes such as 3-mercaptopropyltrimethoxysilane; vinyl silanes such as p-styryltrimethoxysilane, vinyltrichlorosilane, vinyltris(β-methoxyethoxy)silane, vinyltrimethoxysilane, vinyltriethoxysilane, and γ-methacryloxypropyltrimethoxysilane; and polymeric epoxy, amino, and vinyl silanes.

[0131] Examples of titanate coupling agents include isopropyl triisostearoyl titanate, isopropyl tri(N-aminoethyl aminoethyl) titanate, diisopropyl Examples of such titanates include pyribis(dioctylphosphate)titanate, tetraisopropylbis(dioctylphosphite)titanate, tetraoctylbis(ditridecylphosphite)titanate, tetra(2,2-diallyloxymethyl-1-butyl)bis(ditridecyl)phosphite titanate, bis(dioctylpyrophosphate)oxyacetate titanate, and bis(dioctylpyrophosphate)ethylene titanate.

[0132] These coupling agents may be used alone or in any combination and ratio of two or more kinds.

[0133] When a coupling agent is used in the epoxy resin composition (B) of the present invention, the amount of the coupling agent is preferably 0.1 to 3.0 parts by mass per 100 parts by mass of the total epoxy resin components. When the amount of the coupling agent is equal to or more than the lower limit, the effect of improving the adhesion between the epoxy resin matrix and the inorganic filler by adding the coupling agent tends to be improved. When the amount of the coupling agent is equal to or less than the upper limit, the coupling agent is less likely to bleed out from the obtained cured product.

[0134] [Other ingredients] The epoxy resin composition (B) of the present invention may contain components other than those described above (sometimes referred to as "other components" in the present invention). Examples of other components include flame retardants, plasticizers, reactive diluents, pigments, etc., and these may be appropriately added as needed. The epoxy resin composition (B) of the present invention does not in any way preclude the addition of components other than those listed above.

[0135] Examples of the flame retardant used in the epoxy resin composition (B) of the present invention include halogen-based flame retardants such as brominated epoxy resins and brominated phenol resins, antimony compounds such as antimony trioxide, phosphorus-based flame retardants such as red phosphorus, phosphate esters and phosphines, nitrogen-based flame retardants such as melamine derivatives, and inorganic flame retardants such as aluminum hydroxide and magnesium hydroxide.

[0136] [Cured product] The cured product of the present invention can be obtained by curing the epoxy resin composition (B) of the present invention. The cured product of the present invention obtained by curing the epoxy resin composition (B) of the present invention has excellent properties in terms of curability, crack resistance, and heat resistance.

[0137] The method for curing the epoxy resin composition (B) of the present invention is not particularly limited, but a cured product can usually be obtained by a thermosetting reaction caused by heating. During the thermosetting reaction, it is preferable to appropriately select the curing temperature depending on the type of curing agent used. For example, when an acid anhydride curing agent is used, the curing temperature is usually 80 to 250°C. It is also possible to lower the curing temperature by adding a curing accelerator to these curing agents.

[0138] The reaction time of the thermosetting reaction is preferably 1 to 20 hours, more preferably 2 to 18 hours, and further preferably 3 to 15 hours. If the reaction time is equal to or more than the lower limit, the curing reaction tends to proceed sufficiently, which is preferable. If the reaction time is equal to or less than the upper limit, deterioration due to heating and energy loss during heating are easily reduced, which is preferable.

[0139] A cured product using the epoxy resin composition (B) of the present invention has excellent curability, crack resistance and heat resistance.

[0140] The epoxy resin composition (B) of the present invention can give a cured product having a gel time of 34 minutes or less at 120°C, as measured preferably using a No. 153 gel time tester (magnetic type) manufactured by Yasuda Seiki Seisakusho Co., Ltd. The shorter the gel time of the cured product, the shorter the molding cycle for obtaining the cured product, which is preferable.

[0141] The epoxy resin composition (B) of the present invention can provide a cured product having α2 of 182 ppm or less and Tg of 125° C. or more when the second α2 (linear expansion coefficient after Tg) and Tg (glass transition temperature) are measured in compression mode, preferably with a thermomechanical analyzer (TMA: TMA / SS6100 manufactured by Seiko Instruments Inc.) at a first heating rate of 5° C. / min (from 30° C. to 200° C.), a first cooling rate of 10° C. / min (from 200° C. to 30° C.), and a second heating rate of 5° C. / min (from 30° C. to 200° C.). The smaller the α2 of the cured product, the smaller the thermal expansion at high temperatures, making it less likely to cause thermal stress and cracks. The higher the Tg, the smaller the change in physical properties at high temperatures, making it more preferable.

[0142] [Application] The epoxy resin composition (A) of the present invention has excellent electrical and optical properties. The epoxy resin composition (B) of the present invention containing the epoxy resin composition (A) of the present invention has excellent curing properties. The cured product of the epoxy resin composition (B) of the present invention has excellent crack resistance and heat resistance.

[0143] Therefore, the epoxy resin composition (A), the epoxy resin composition (B) and the cured product thereof of the present invention can be effectively used in any application where these physical properties are required. For example, they can be suitably used in the fields of coatings such as optical materials, electrocoating paints for automobiles, heavy-duty anticorrosive coatings for ships and bridges, and coatings for the inner surface of beverage cans; in the fields of electrical and electronics such as laminates, semiconductor encapsulants, insulating powder coatings, and coil impregnation; in the fields of civil engineering, construction, and adhesives such as earthquake-resistant reinforcement of bridges, concrete reinforcement, flooring materials for buildings, linings for water facilities, drainage and permeable pavements, and adhesives for vehicles and aircraft. Among these, they are particularly useful for applications in electrical and electronic parts and optical materials.

[0144] The epoxy resin composition (B) of the present invention may be used for the above-mentioned applications after curing, or may be cured during the production process for the above-mentioned applications. EXAMPLES

[0145] The present invention will be described in more detail below with reference to examples. The present invention is not limited to the following examples as long as it does not depart from the gist of the present invention.

[0146] [Production and evaluation of epoxy resin composition (A)] [Examples 1 to 3, Comparative Examples 1 to 7] The analytical methods and physical property measuring methods for the epoxy resin compositions obtained in Examples 1 to 3 and Comparative Examples 1 to 7 were as follows.

[0147] (1) Composition analysis of epoxy resin composition: The area percentages of "epoxy resin (1)," "epoxy resin (2) and / or epoxy resin (3)," and "other components" of the epoxy resin compositions produced in each Example and Comparative Example were analyzed under the following conditions, and the mass percentages were calculated from the area percentages. The other components are epoxy resins other than the epoxy resins (1) to (3). Equipment: Tosoh HLC-8220L GPC Detector: RI Mobile phase: Tetrahydrofuran (containing BHT) Flow rate: 0.8mL / min Column: Tosoh TSKgel G2000Hxl + G1000Hxl x 2 Column temperature: 40℃

[0148] (2) Total chlorine content: The total chlorine content was analyzed according to JIS K7243-3.

[0149] (3) Epoxy equivalent: The epoxy equivalent was analyzed according to JIS K7236-1955.

[0150] (4) Number of Hazen colors: Hazen color index was analyzed using a UV-Vis spectrophotometer according to ISO 6271-2:2004.

[0151] [Example 1] Mitsubishi Chemical Corporation's bisphenol A type epoxy resin "jER828EL" (wherein X=isopropylidene group, R 1 = hydrogen atom, n = 0, epoxy equivalent = 186 g / equivalent, total chlorine content = 1300 ppm) was collected over 6 hours using a centrifugal thin-film distillation apparatus at a temperature of 220°C and a reduced pressure of 0.003 Torr, and a 50% fraction (500 g) was collected over 6 hours to obtain a distilled bisphenol A type epoxy resin (epoxy equivalent = 171 g / equivalent, total chlorine content = 800 ppm).

[0152] In a 1L induction stirring autoclave, 400g of the previously obtained distilled bisphenol A type epoxy resin (epoxy equivalent = 171g / equivalent, total chlorine content = 800ppm), 100g of ethyl acetate, and 2.4g of 5 mass% rhodium / graphite catalyst (NE Chemcat Corporation) as a hydrogenation catalyst were charged, and the atmosphere in the autoclave was replaced with nitrogen and then with hydrogen. After that, the hydrogenation reaction was carried out at 110°C and a hydrogen pressure of 8MPa until hydrogen absorption almost stopped. The reaction time was 180 minutes. The hydrogenation catalyst was filtered from the reaction mixture using 5C filter paper. Next, the reaction solvent was distilled off under reduced pressure at 100° C. while blowing in a small amount of nitrogen, to obtain an epoxy resin composition (A) of Example 1.

[0153] [Example 2] An epoxy resin composition (A) of Example 2 was obtained in the same manner as in Example 1, except that the amount of the hydrogenation catalyst used was 1.2 g and the hydrogenation reaction time was 360 minutes.

[0154] [Example 3] An epoxy resin composition (A) of Example 3 was obtained in the same manner as in Example 1, except that the amount of the hydrogenation catalyst used was 4.8 g and the hydrogenation reaction time was 90 minutes.

[0155] In the following Comparative Example 1, a reaction was carried out in accordance with Example 1 of JP-A No. 2002-97251.

[0156] [Comparative Example 1] In a 500 ml stainless steel autoclave equipped with a magnetic stirrer, 40 g of bisphenol A diglycidyl ether "Epotohto YD-8125" (epoxy equivalent = 172 g / equivalent) manufactured by Tohto Kasei Co., Ltd., 120 g of propylene glycol monomethyl ether, and 1.0 g of 5 mass% rhodium / graphite catalyst (NE Chemcat Corporation) were charged, and the system was replaced with hydrogen. The mixture was then heated at 50°C with stirring under a hydrogen pressure of 4.9 MPa (50 kg / cm). 2 ) for 5 hours. After the reaction, the catalyst was filtered off, and the solvent was distilled off at 150° C. and 266 Pa (20 Torr) to obtain the epoxy resin composition of Comparative Example 1.

[0157] In the following Comparative Examples 2 to 4, the reactions were carried out according to Hydrogenation Examples 5, 6 and 7 using catalysts produced according to the examples in JP-A-2007-515276.

[0158] [Comparative Example 2] A 1.2-liter pressure-resistant autoclave equipped with a gas supply tube (700 rpm) and a sample collection tube was used. In an autoclave, 21 g of catalyst (catalyst D, Ru content 1.7 wt.%) was loaded into the catalyst cage and heated to 50° C. with 600 g of a 40 wt.% solution of low-oligomer bisphenol-A-bisglycidyl ether (distilled product, EEW=171 g / eq.) in THF with 4.5 wt.% water and hydrogenated at 250 bar hydrogen pressure. After a reaction time of 24 h, the autoclave was cooled to room temperature, depressurized and the reaction batch was removed. Mechanically fine fragments of the catalyst were filtered off. An aliquot of the colorless effluent was subjected to solvent removal by rotary evaporation (conditions: oil bath temperature 130° C., vacuum 5-10 mbar, 15 min) to obtain the epoxy resin composition of Comparative Example 2.

[0159] [Comparative Example 3] In a 1.2 liter pressure autoclave equipped with a gas supply (700 rpm) and a sampling tube, 21 g of catalyst (catalyst D, Ru content 2.0% by weight) were loaded into the catalyst cage and heated to 50° C. with 600 g of a 40% by weight solution of low-oligomer bisphenol-A-bisglycidyl ether (distilled product, EEW=171 g / eq.) in THF with 4.5% by weight of water and hydrogenated at 250 bar hydrogen pressure. After a reaction time of 11 h, 1 The aromatic conversion was complete according to H-NMR. The autoclave was cooled to room temperature, depressurized, and the reaction batch was removed. Mechanically fine catalyst debris was filtered off. An aliquot of the colorless effluent was subjected to solvent removal by rotary evaporation (conditions: oil bath temperature 130°C, vacuum 5-10 mbar, 15 min) to obtain the epoxy resin composition of Comparative Example 3.

[0160] [Comparative Example 4] In a 1.2 liter pressure autoclave equipped with a gas supply (700 rpm) and a sampling tube, 17.9 g of catalyst (catalyst D, Ru content 2.0% by weight) were loaded into the catalyst cage and heated to 50° C. with 600 g of a 40% by weight solution of low-oligomer bisphenol-A-bisglycidyl ether (distilled product, EEW=171 g / eq.) in THF with 4.5% by weight of water and hydrogenated at 250 bar hydrogen pressure. After a reaction time of 14 h, 1 The aromatic conversion was complete according to H-NMR. The autoclave was cooled to room temperature, depressurized, and the reaction batch was removed. Mechanically fine catalyst debris was filtered off. An aliquot of the colorless effluent was subjected to solvent removal by rotary evaporation (conditions: oil bath temperature 130°C, vacuum 5-10 mbar, 15 min) to obtain the epoxy resin composition of Comparative Example 4.

[0161] In the following Comparative Examples 5 and 6, reactions were carried out in accordance with Example 1 of JP-A-11-269159.

[0162] [Comparative Example 5] In a four-neck flask equipped with a rotary stirrer, decanter, thermometer and gas inlet tube, 1215g (5 mol) of hydrogenated bisphenol A, 580g of xylene and 15g of stannic chloride pentahydrate were charged, and 1110g (12 mol) of epichlorohydrin was added dropwise at 100°C over 60 minutes, and stirring was continued for another 30 minutes to complete the addition reaction. Next, 35g of benzyltrimethylammonium chloride and 1130g of 50% aqueous sodium hydroxide solution were added, and stirring was continued at 80°C for 5 hours to complete the ring-closing reaction. The by-product sodium chloride and unreacted sodium hydroxide were removed by washing with water, and then dehydration and desolvation were performed at 120°C and 3 Torr for 1 hour to obtain 1860g of crude product (reaction crude product-A). Thereafter, 2 g of 2,6-di-t-butyl-4-methylphenol was dissolved in the above reaction crude product as an antioxidant, and the liquid was circulated for 1 hour at a temperature of 70°C and a liquid feed rate of 3 liters / h using a centrifugal molecular distillation apparatus (MS-150 type molecular distillation apparatus manufactured by Nippon Sharyo Co., Ltd.) with an evaporation surface diameter of 150 mm and a treatment liquid residence time of 1 second or less. Thereafter, by adjusting the operating conditions to a vacuum of 0.005 Torr, a liquid feed rate of 1.5 liters / h, and an evaporation surface temperature of 135°C, 5 mass% of the pre-distillate relative to the amount of liquid fed was steadily distilled off, and an epoxy resin composition of Comparative Example 5 was obtained.

[0163] [Comparative Example 6] The epoxy resin composition of Comparative Example 6 was obtained in the same manner as in Comparative Example 5, except that the distillation conditions using a centrifugal molecular distillation apparatus (MS-150 type molecular distillation apparatus manufactured by Nippon Sharyo Co., Ltd.) were changed from 5% by mass of the initial fraction to 1% by mass of the feed liquid.

[0164] In the following Comparative Example 7, the reaction was carried out in accordance with Example 1 of JP-A-2003-212955.

[0165] [Comparative Example 7] In a 1L induction stirring autoclave, 400g of Mitsubishi Chemical's bisphenol A type epoxy resin "jER828EL" (epoxy equivalent = 186g / equivalent), 100g of ethyl acetate, and 2.4g of 5 mass% rhodium / graphite catalyst (NE Chemcat Corporation) as a hydrogenation catalyst were charged, and the atmosphere in the autoclave was replaced with nitrogen and then with hydrogen. The hydrogenation reaction was then carried out at 110°C and a hydrogen pressure of 8MPa until hydrogen absorption almost stopped. The reaction time was 180 minutes. The hydrogenation catalyst was filtered from the reaction solution using filter paper No. 5C. The reaction solvent was then distilled off under reduced pressure at 100°C while blowing in a small amount of nitrogen to obtain an epoxy resin composition of Comparative Example 7.

[0166] The analytical results of the epoxy resin compositions obtained in Examples 1 to 3 and Comparative Examples 1 to 7 are shown in Table 1 (Table 1A and Table 1B).

[0167] [Table 1]

[0168] [Production of Epoxy Resin Composition (B) and Evaluation of the Cured Product] [Examples 4 to 6, Comparative Examples 8 to 14] Evaluation of the epoxy resin compositions and their cured products obtained in Examples 4 to 6 and Comparative Examples 8 to 14 The method is as follows.

[0169] (1) Gel time at 120℃: Using a No. 153 gel time tester (magnetic type) manufactured by Yasuda Seiki Seisakusho, measurements were performed on epoxy resin compositions that were uniformly blended according to the formulation shown in Table 2 (Table 2A, Table 2B). The following curing agents and curing accelerators were used. Hardener: "Rikacid MH-700" manufactured by New Japan Chemical Co., Ltd. (4-methylhexahydrophthalic anhydride / hexahydrophthalic anhydride = 70 / 30) Curing accelerator: "Hishicoline PX-4MP" (methyl tributylphosphonium dimethyl phosphate) manufactured by Nippon Chemical Industry Co., Ltd.

[0170] (2) α2 (linear expansion coefficient after Tg), Tg (glass transition temperature) (TMA): Two glass plates with release PET film attached were prepared, and the release PET film was placed on the inside of both glass plates, adjusting the distance between the glass plates to 4 mm, to create a mold. An epoxy resin composition uniformly blended according to the composition shown in Table 2 (Table 2A, Table 2B) was poured into this mold, and heated at 100°C for 3 hours and then at 130°C for 3 hours to obtain a cured product. The resulting cured product was cut into a cylindrical shape with a diameter of 1 cm and a thickness of 4 mm to obtain a test piece. The test specimen was subjected to measurement of the second α2 and Tg using a thermomechanical analyzer (TMA: TMA / SS6100 manufactured by Seiko Instruments) in compression mode with a first heating rate of 5°C / min (from 30°C to 200°C), a first cooling rate of 10°C / min (from 200°C to 30°C), and a second heating rate of 5°C / min (from 30°C to 200°C).

[0171] The evaluation results are shown in Table 2 (Table 2A and Table 2B).

[0172] [Table 2]

[0173] [Evaluation of results] From Table 1, it can be seen that the epoxy resin compositions (A) of Examples 1 to 3, in which the compositions of the epoxy resins (1) to (3) are within the range specified by the present invention, have a lower total chlorine content and superior electrical reliability, as well as a smaller Hazen color number, and are therefore excellent as optical materials, compared to the epoxy resin compositions of Comparative Examples 1 to 7.

[0174] From Table 2, it can be seen that the cured products of the epoxy resin compositions (B) of Examples 4 to 6 using the epoxy resin compositions (A) of Examples 1 to 3 have superior curability, low linear expansion properties, and heat resistance compared to the cured epoxy resin products of Comparative Examples 8 to 14.

[0175] Taking these together, it can be seen that the epoxy resin compositions (A) of Examples 1 to 3 and the epoxy resin compositions (B) of Examples 4 to 6 are superior to the epoxy resin compositions of Comparative Examples 1 to 7 and the epoxy resin compositions of Comparative Examples 8 to 14.

[0176] Although the present invention has been described in detail with reference to specific embodiments, it will be apparent to those skilled in the art that various modifications can be made without departing from the spirit and scope of the invention. This application is based on Japanese Patent Application No. 2019-152125 filed on August 22, 2019, the entirety of which is incorporated by reference.

Claims

1. An epoxy resin composition (A) comprising an epoxy resin having a structure represented by the following formula (1) (hereinafter referred to as "epoxy resin (1)"), an epoxy resin having a structure represented by the following formula (2) (hereinafter referred to as "epoxy resin (2)"), and an epoxy resin having a structure represented by the following formula (3) (hereinafter referred to as "epoxy resin (3)"), wherein, relative to 100% by mass of the total of the epoxy resin (1), the epoxy resin (2), and the epoxy resin (3), the content of the epoxy resin (1) is 89.0 to 99.9% by mass, the total content of the epoxy resin (2) and the epoxy resin (3) is 0.1 to 11.0% by mass, and the epoxy equivalent is 176 to 186 g / equivalent. [Formula 1] In the above formulas (1), (2), and (3), X is an isopropylidene group. 1 is a hydrogen atom R 1 is a C 1-10 hydrocarbon group or a halogen atom, and may be the same or different. Two R 2 bonds bonded to adjacent carbon atoms on the cyclohexane ring are 1 may be bonded to each other to form a ring structure having 4 to 20 carbon atoms. n is an integer of 0 to 2.

2. In the formulas (1) to (3), R 1 The epoxy resin composition (A) according to claim 1, wherein is a hydrogen atom and n is 0.

3. The epoxy resin composition (A) according to claim 1 or 2, having a total chlorine content (in accordance with JIS K7043-3) of 1000 ppm or less.

4. The epoxy resin composition (A) according to any one of claims 1 to 3, having a Hazen color number value (APHA value: in accordance with ISO 6271-2:2004) of 12 or less.

5. Epoxy resin composition (B) comprising 0.01 to 1000 parts by mass of a curing agent per 100 parts by mass of the epoxy resin composition (A) according to any one of claims 1 to 4.

6. A cured product obtained by curing the epoxy resin composition (B) according to claim 5.

7. An electric or electronic part obtained by curing the epoxy resin composition (B) according to claim 5.

8. An optical part obtained by curing the epoxy resin composition (B) according to claim 5.

Citation Information

Patent Citations

  • Alicyclic compound containing glycidyl group, its production method and epoxy resin composition using the same

    JP2002097251A

  • Heterogeneous ruthenium catalyst, ring-hydrogenated bisglycidyl ether of bisphenol a and f and method for producing the same

    JP2007515276A