Thermosetting resin composition, cured thermosetting resin, prepreg and fiber-reinforced composite material

The thermosetting resin composition with specific polyamide particles addresses the challenge of achieving both post-impact compressive strength and wet heat compression performance in carbon fiber-reinforced composites, resulting in materials with high tensile strength and chemical resistance for aerospace applications.

JP7582206B2Active Publication Date: 2024-11-13TORAY INDUSTRIES INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021567403
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-23
Filing Date
2020-12-18
Publication Date
2024-11-13
Estimated Expiration
2040-12-18

AI Technical Summary

Technical Problem

Existing carbon fiber-reinforced composite materials using thermosetting resins face challenges in achieving both post-impact compressive strength and wet heat compression performance, with previous techniques either lacking sufficient compressive strength or exhibiting low wet heat compression performance.

Method used

A thermosetting resin composition comprising thermosetting resin, a hardening agent, and polyamide particles with specific properties, including a melting point of 200-300°C, crystallization temperature of 150-250°C, number average particle diameter of 1-100 μm, sphericity of 80-100, and linseed oil absorption of 10-100 mL/100g, which enhances the balance of modulus, strength, and toughness.

Benefits of technology

The composition produces fiber-reinforced composite materials with high tensile strength, impact resistance, and chemical resistance, suitable for aerospace applications, while maintaining excellent post-impact compressive strength and wet heat compression performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582206000001
    Figure 0007582206000001
  • Figure 0007582206000002
    Figure 0007582206000002
  • Figure 0007582206000003
    Figure 0007582206000003
Patent Text Reader

Abstract

A thermosetting resin composition according to the present invention is characterized by comprising at least the following constituent elements (A), (B) and (C). (A) A thermosetting resin (B) A curing agent (C) Polyamide particles that satisfy the following requirements (c1) to (c6) (c1) The melting point of a polyamide resin that constitutes the polyamide particles is from 200°C to 300°C. (c2) The crystallization temperature of the polyamide resin that constitutes the polyamide particles is from 150°C to 250°C. (c3) The number average particle diameter of the polyamide particles is from 1 μm to 100 μm. (c4) The sphericity of the polyamide particles is from 80 to 100. (c5) The linseed oil absorption of the polyamide particles is from 10 mL / 100 g to 100 mL / 100 g. A thermosetting resin composition according to the present invention is capable of favorably producing a fiber-reinforced composite material that has sufficient compressive strength after impact and sufficient wet heat compression performance. A fiber-reinforced composite material which is produced using a thermosetting resin composition according to the present invention has high tensile strength, high impact resistance and high chemical resistance, and is thus able to be used in wide range of applications including aerospace applications that require high mechanical characteristics and general industrial applications such as windmills, automobiles and bicycles.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermosetting resin composition. The present invention further relates to a fiber-reinforced composite material suitable for aerospace applications, a prepreg for obtaining the same, and further to a cured thermosetting resin material and a thermosetting resin composition that are suitably used as a matrix resin thereof. [Background technology]

[0002] Fiber-reinforced composite materials, especially carbon fiber-reinforced composite materials (hereinafter sometimes referred to as CFRP), have excellent specific strength and specific rigidity and are therefore widely used in a variety of applications, including aircraft structural components, wind turbine blades, automobile exterior panels, and computer applications such as IC trays and laptop computer housings.

[0003] CFRP is a heterogeneous material made by molding prepregs whose essential components are carbon fibers, which are reinforcing fibers, and matrix resin. Therefore, there is a large difference in the physical properties of CFRP in the direction of the reinforcing fibers and in other directions. In particular, carbon fiber reinforced composite materials that use thermosetting resin as the matrix resin are easily broken by stress from directions other than the direction of the reinforcing fibers because the matrix resin has low toughness. Various toughness improvement techniques have been proposed for carbon fiber reinforced composite materials that use thermosetting resin as the matrix resin.

[0004] As one of the techniques for improving toughness, it has been proposed to give carbon fiber reinforced composite materials high toughness and good heat resistance while maintaining the moldability of the prepreg by blending resin particles with a thermosetting resin. For example, a technique for achieving both impact resistance and tensile strength by using polyamide particles with a specific structure as resin particles has been disclosed (Patent Document 1). A technique for improving toughness by controlling the particles to a low melting point range using copolymer particles of nylon 12 and nylon 6 has been disclosed (Patent Document 2). In addition, a technique for achieving both impact resistance (compressive strength after impact) and another important characteristic, wet heat compression performance, using polyamide 1010 particles or polyamide 12 particles has been disclosed (Patent Document 3).

[0005] However, the technique described in Patent Document 1 could not impart sufficient compressive strength after impact. The techniques described in Patent Documents 2 and 3 could impart compressive strength after impact, but had the problem of low wet heat compression performance. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2011-162619 A [Patent Document 2] International Publication No. 2018 / 174250 [Patent Document 3] JP 2018-66016 A Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention aims to obtain a fiber-reinforced composite material that can achieve both compressive strength after impact and wet heat compression performance. This has been achieved as a result of investigating prepregs for obtaining the fiber-reinforced composite material, as well as thermosetting resin cured products and thermosetting resin compositions that are suitably used as matrix resins for the fiber-reinforced composite material. [Means for solving the problem]

[0008] In order to solve the above problems, the present invention has the following configuration.

[0009] A thermosetting resin composition comprising at least [A], [B], and [C]. [A] Thermosetting resin [B] Hardener [C] Polyamide particles satisfying the following (c1) to (c5): (c1) The melting point of the polyamide resin constituting the polyamide particles is 200 to 300°C. (c2) The crystallization temperature of the polyamide resin constituting the polyamide particles is 150°C to 250°C. (c3) The number average particle size of the polyamide particles is 1 to 100 μm. (c4) The sphericity of the polyamide particles is 80 to 100. (c5) The polyamide particles have a linseed oil absorption of 10 to 100 mL / 100 g. Effect of the Invention

[0010] The thermosetting resin composition of the present invention can be used for fiber-reinforced composite materials. In particular, the thermosetting resin composition of the present invention can be used to suitably produce fiber-reinforced composite materials having sufficient compressive strength after impact and wet heat compression performance.

[0011] The thermosetting resin composition of the present invention can be suitably used as a prepreg, and further as a cured thermosetting resin that is a matrix resin for a fiber-reinforced composite material.

[0012] The fiber-reinforced composite material produced using the thermosetting resin composition of the present invention has high tensile strength, high impact resistance, and high chemical resistance, and can therefore be widely used in aerospace applications that require high mechanical properties, as well as general industrial applications such as wind turbines, automobiles, and bicycles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention will be described in detail below.

[0014] In the present invention, the thermosetting resin [A] refers to a compound that forms a three-dimensional crosslinked body by heating. Specific examples of the thermosetting resin include epoxy resin, benzoxazine resin, vinyl ester resin, unsaturated polyester resin, urethane resin, phenol resin, melamine resin, maleimide resin, cyanate ester resin, and urea resin. Among these, epoxy resin, benzoxazine resin, vinyl ester resin, unsaturated polyester resin, phenol resin, and mixtures of these resins have high mechanical properties and are preferably used as the thermosetting resin. In particular, epoxy resin is particularly preferably used because it has excellent mechanical properties and also has excellent adhesion to reinforcing fibers.

[0015] As the epoxy resin, a compound having two or more epoxy groups in one molecule is used. Specific examples of the epoxy resin in the present invention include aromatic glycidyl ether obtained from a phenol compound having multiple hydroxyl groups, aliphatic glycidyl ether obtained from an alcohol having multiple hydroxyl groups, glycidyl amine obtained from an amine, glycidyl ester obtained from a carboxylic acid having multiple carboxyl groups, and epoxy resin having an oxirane ring.

[0016] Among them, glycidylamine-type epoxy resins are preferably used because they have low viscosity, excellent impregnation into reinforcing fibers, and excellent mechanical properties such as heat resistance and elastic modulus when made into a fiber-reinforced composite material. Such glycidylamine-type epoxy resins can be roughly divided into polyfunctional amine-type epoxy resins and bifunctional amine-type epoxy resins.

[0017] As the polyfunctional amine type epoxy resin, a glycidylamine type epoxy resin containing three or more epoxy groups in one epoxy resin molecule can be used. As the polyfunctional amine type epoxy resin, for example, tetraglycidyldiaminodiphenylmethane, triglycidylaminophenol, tetraglycidylxylylenediamine, their halogen-substituted, alkyl-substituted, aralkyl-substituted, alkenyl-substituted, alkoxy-substituted, aralkoxy-substituted, allyloxy-substituted, and their hydrogenated products can be used. Bifunctional amine type epoxy can also be used, and as such a compound, diglycidylaniline, their halogen-substituted, alkyl-substituted, aralkyl-substituted, allyl-substituted, alkoxy-substituted, aralkoxy-substituted, allyloxy-substituted, and their hydrogenated products can be used.

[0018] As the polyfunctional amine type epoxy resin, tetraglycidyldiaminodiphenylmethane, triglycidylaminophenol, tetraglycidylxylylenediamine, their substituted products, hydrogenated products, etc. are suitably used.

[0019] As the tetraglycidyldiaminodiphenylmethane, "Sumiepoxy (registered trademark)" ELM434 (manufactured by Sumitomo Chemical Co., Ltd.), YH434L (manufactured by Nippon Steel Sumikin Chemical Co., Ltd.), "jER (registered trademark)" 604 (manufactured by Mitsubishi Chemical Co., Ltd.), "Araldite (registered trademark)" MY720, MY721 (manufactured by Huntsman Advanced Materials Co., Ltd.), etc. can be used. As the triglycidylaminophenol and its alkyl-substituted derivatives, "Sumiepoxy (registered trademark)" ELM100, ELM120 (manufactured by Sumitomo Chemical Co., Ltd.), "Araldite (registered trademark)" MY0500, MY0510, MY0600 (manufactured by Huntsman Advanced Materials Co., Ltd.), "jER (registered trademark)" 630 (manufactured by Mitsubishi Chemical Co., Ltd.), etc. can be used. As tetraglycidylxylylenediamine and its hydrogenated products, "TETRAD (registered trademark)"-X, "TETRAD (registered trademark)"-C (manufactured by Mitsubishi Gas Chemical Company, Inc.), etc. can be used.

[0020] The polyfunctional amine type epoxy resin is preferably used as the epoxy resin in the present invention because the resulting resin cured product has an excellent balance between heat resistance and mechanical properties such as elastic modulus. The polyfunctional amine type epoxy resin is preferably contained in an amount of 40 to 70 mass% of the total epoxy resin.

[0021] In the present invention, the epoxy resin may include an epoxy resin other than glycidylamine, a copolymer of an epoxy resin and a thermosetting resin, etc. Examples of the above-mentioned thermosetting resin used by copolymerizing with an epoxy resin include unsaturated polyester resin, vinyl ester resin, epoxy resin, benzoxazine resin, phenol resin, urea resin, melamine resin, and polyimide resin. These resin compositions and compounds may be used alone or in appropriate combination.

[0022] Among the epoxy resins used as the epoxy resin other than glycidylamine, glycidyl ether type epoxy resins having phenol as a precursor are preferably used as bifunctional epoxy resins. Examples of such epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, naphthalene type epoxy resins, biphenyl type epoxy resins, urethane modified epoxy resins, hydantoin type and resorcinol type epoxy resins.

[0023] The glass transition temperature of the thermosetting resin in the present invention is preferably 120 to 250°C, more preferably 140 to 210°C, from the viewpoint of ensuring sufficient heat resistance and compressive strength under hot and wet conditions required for aircraft materials.

[0024] In the present invention, the curing agent [B] refers to a compound having an active group capable of reacting with an epoxy group when an epoxy resin is used as the thermosetting resin.Specific examples of the curing agent for epoxy resin include dicyandiamide, aromatic polyamines, aminobenzoic acid esters, various acid anhydrides, phenol novolac resins, cresol novolac resins, polyphenol compounds, imidazole derivatives, aliphatic amines, tetramethylguanidine, thiourea-added amines, carboxylic acid anhydrides such as methylhexahydrophthalic anhydride, carboxylic acid hydrazides, carboxylic acid amides, polymercaptans, and Lewis acid complexes such as boron trifluoride ethylamine complex.

[0025] By using an aromatic polyamine as a curing agent, it is possible to obtain a cured epoxy resin material having good heat resistance. In particular, among aromatic polyamines, diaminodiphenylsulfone or its derivatives, or various isomers thereof are the most suitable curing agents for obtaining a cured epoxy resin material having good heat resistance.

[0026] In addition, by using a combination of dicyandiamide and a urea compound, such as 3,4-dichlorophenyl-1,1-dimethylurea, or by using imidazoles as a curing agent, high heat resistance and water resistance can be obtained while curing at a relatively low temperature. Curing an epoxy resin with an acid anhydride gives a cured product with a lower water absorption rate than amine compound curing. In addition, by using a latent curing agent, such as a microencapsulated curing agent, the storage stability of the prepreg, especially the tackiness and drapeability, are less likely to change even when left at room temperature.

[0027] The optimum amount of the curing agent to be added varies depending on the type of thermosetting resin and the curing agent, but it is preferable to add the curing agent in an amount that is stoichiometrically equivalent. These curing agents may be used alone or in combination.

[0028] Commercially available aromatic polyamine curing agents include Seikacure S (manufactured by Wakayama Seika Kogyo Co., Ltd.), MDA-220 (manufactured by Mitsui Chemicals, Inc.), "jER Cure (registered trademark)" W (manufactured by Mitsubishi Chemical Corporation), and 3,3'-DAS (manufactured by Mitsui Chemicals, Inc.), Lonzacure (registered trademark) M-DEA (manufactured by Lonza Corporation), Lonzacure (registered trademark) M-DIPA (manufactured by Lonza Corporation), Lonzacure (registered trademark) M-MIPA (manufactured by Lonza Corporation), and Lonzacure (registered trademark) DETDA 80 (manufactured by Lonza Corporation).

[0029] In addition, the epoxy resin and the curing agent, or a product obtained by pre-reacting a part of them, can be blended into the composition. This method can be effective in adjusting the viscosity and improving the storage stability.

[0030] The polyamide particles [C] in the present invention are polyamide particles that satisfy the following (c1) to (c5). (c1) The melting point of the polyamide resin constituting the polyamide particles is 200°C to 300°C. (c2) The crystallization temperature of the polyamide resin constituting the polyamide particles is 150°C to 250°C. (c3) The number average particle size of the polyamide particles is 1 to 100 μm. (c4) The sphericity of the polyamide particles is 80 to 100. (c5) The polyamide particles have a linseed oil absorption of 10 to 100 mL / 100 g. The present inventors have found that, when the polyamide particles satisfy the above conditions (c1) to (c5), it is possible to provide a CFRP that exhibits a good balance between the elastic modulus, strength, and toughness of a cured thermosetting resin, which were previously in a trade-off relationship, and that has good compressive strength after impact and moist heat compression performance while also having high chemical resistance and heat resistance.

[0031] In the present invention, the polyamide resin constituting the polyamide fine particles refers to a polymer having a structure containing an amide group.

[0032] In the present invention, the polyamide resin constituting the polyamide particles has a melting point of 200°C to 300°C. Such a high melting point can improve the heat resistance and chemical resistance of the thermosetting resin cured product, and can exhibit excellent wet heat compression performance of CFRP. In addition, the chemical resistance of the thermosetting resin cured product and CFRP can also be improved. Furthermore, when molding the thermosetting resin composition containing the polyamide particles of the present invention into a prepreg, particle deformation due to heating can be suppressed and high fluidity can be maintained. The preferred range of the melting point is 205°C or higher, more preferably 210°C or higher. If the melting point is too high, the toughness of the thermosetting resin cured product and the compression strength after impact of CFRP decrease, so the upper limit is 300°C or lower, preferably 270°C or lower, more preferably 250°C or lower, and even more preferably 230°C or lower.

[0033] The melting point of the polyamide resin constituting the polyamide particles is preferably 205°C to 270°C, and more preferably 210°C to 250°C.

[0034] The melting point of the polyamide constituting the polyamide particles is the top of the endothermic peak when the temperature is increased from 30° C. at 20° C. / min in a nitrogen atmosphere using a DSC method.

[0035] In the present invention, the polyamide resin constituting the polyamide particles has a crystallization temperature of 150°C to 250°C. By having a crystallization temperature in a specific temperature range, a thermosetting resin cured product having extremely high strength can be obtained, and further, a fiber reinforced composite material using the thermosetting resin cured product can maintain compression performance even under moist and hot conditions. In addition, the chemical resistance of the thermosetting resin cured product and CFRP can also be increased. The crystallization temperature of the polyamide resin is preferably 160°C or higher, more preferably 165°C or higher, and even more preferably 170°C or higher. If the crystallization temperature is too high, the rigidity of the thermosetting resin cured product may become too high, resulting in a decrease in toughness, or the compressive strength after impact of CFRP may decrease, so the upper limit is 250°C or lower, preferably 210°C or lower, more preferably 195°C or lower, and even more preferably 180°C or lower.

[0036] The crystallization temperature of the polyamide resin constituting the polyamide particles is preferably 160°C to 210°C, more preferably 165°C to 195°C, and further preferably 170°C to 180°C.

[0037] The crystallization temperature of the polyamide constituting the polyamide particles is measured by the DSC method in the same manner as the melting point. The crystallization temperature is the top of the exothermic peak that appears when the temperature is raised from 30°C to a temperature 30°C higher than the endothermic peak indicating the melting point of the polyamide at a rate of 20°C / min under a nitrogen atmosphere, held for 1 minute, and then cooled to 30°C at a rate of 20°C / min. If the polyamide does not have a crystallization temperature, no exothermic peak appears.

[0038] Specific examples of such polyamide resins include polyamide 4, polycaproamide (polyamide 6), polyhexamethylene adipamide (polyamide 66), polytetramethylene adipamide (polyamide 46), polytetramethylene sebacamide (polyamide 410), polypentamethylene adipamide (polyamide 56), polypentamethylene sebacamide (polyamide 510), polyhexamethylene sebacamide (polyamide 610), polyhexamethylene dodecamide (polyamide 612), polydecamide (polyamide 613), and polydecamide (polyamide 614). Examples of such polyamides include methylene adipamide (polyamide 106), polydodecamethylene adipamide (polyamide 126), polycaprylamide (polyamide 8), polyhexamethylene terephthalamide (polyamide 6T), polydecamethylene terephthalamide (polyamide 10T), polydodecamethylene terephthalamide (polyamide 12T), polycaproamide / polyhexamethylene adipamide copolymer (polyamide 6 / 66), and polycaproamide / polydodecaamide copolymer (polyamide 6 / 12). Polycaproamide (polyamide 6), polyhexamethylene adipamide (polyamide 66), polycaprylamide (polyamide 8), polyhexamethylene terephthalamide (polyamide 6T), polydecamethylene terephthalamide (polyamide 10T), polydodecamethylene terephthalamide (polyamide 12T), polycaproamide / polyhexamethylene adipamide copolymer (polyamide 6 / 66), polycaproamide / polydodecaamide copolymer (polyamide 6 / 12) are preferred because they can exhibit excellent wet heat compression performance of CFRP, and polycaproamide (polyamide 6), polycaprylamide (polyamide 8), polycaproamide / polydodecaamide copolymer (polyamide 6 / 12) are particularly preferred from the viewpoint of CAI.

[0039] The polyamide resin constituting the polyamide particles of the present invention preferably contains 60% by mass or more of the structural unit of the following general formula (1). By containing structural units in such a range, it is possible to maintain toughness while exhibiting high elastic modulus and high strength in the cured thermosetting resin, and it is possible to exhibit a good balance between compressive strength after impact and wet heat compression performance when made into a fiber-reinforced composite material.

[0040] [ka]

[0041] (In the formula, n represents an integer of 4 to 7.) From the viewpoint of achieving a good balance between compressive strength after impact and wet heat compression performance when made into CFRP, n is most preferably an integer of 5, i.e., polyamide 6. Since the higher the content of the structural unit of general formula (1) in the polyamide resin, the better the compatibility of compressive strength after impact and wet heat compression performance can be achieved, the structural unit is preferably 70 mass% or more, more preferably 80 mass% or more, even more preferably 90 mass% or more, and particularly preferably 100 mass%.

[0042] The amount of the structural unit of general formula (1) in the polyamide resin constituting the polyamide particles is a value measured as follows: the polyamide particles are hydrolyzed with hydrochloric acid or the like, and the amount of ε-caprolactam, which is the monomer, is quantified by gas chromatography to calculate the mass %.

[0043] In the present invention, the polyamide resin constituting the polyamide particles may contain components other than the constituent units. There is no limitation as long as the components are copolymerizable, and examples thereof include polyundecaamide (polyamide 11), polylauroamide (polyamide 12), polyhexamethylene adipamide (polyamide 66), polydecamethylene sebacamide (polyamide 1010), polydodecamethylene dodecamide (polyamide 1212), polyhexamethylene sebacamide (polyamide 610), polyhexamethylene dodecamide (polyamide 612), polydecamethylene adipamide (polyamide 106), polydodecamethylene adipamide (polyamide 126), polyhexamethylene terephthalamide (polyamide 6T), polydecamethylene terephthalamide (polyamide 10T), polydodecamethylene terephthalamide (polyamide 12T), and amorphous polyamide.

[0044] In the present invention, the weight average molecular weight of the polyamide resin constituting the polyamide particles is 5,000 to 500,000. If the weight average molecular weight is too low, the compressive strength after impact of the CFRP decreases, so it is preferably 10,000 or more, more preferably 20,000 or more, and even more preferably 30,000 or more. If the weight average molecular weight is too high, the dispersibility in the thermosetting resin composition becomes poor, so it is preferably 300,000 or less, more preferably 200,000 or less, and particularly preferably 100,000 or less.

[0045] The weight average molecular weight of the polyamide constituting the polyamide particles is the weight average molecular weight calculated by measuring the value by gel permeation chromatography using hexafluoroisopropanol as a solvent and converting it into the weight average molecular weight of polymethyl methacrylate.

[0046] In the present invention, it is important that the number average particle diameter of the polyamide particles is in the range of 1 to 100 μm in order to obtain mechanical properties and moldability of the thermosetting resin cured material and CFRP. If the number average particle diameter exceeds 100 μm, moldability into prepreg deteriorates. The number average particle diameter of the polyamide fine particles is preferably 80 μm or less, more preferably 50 μm or less, and even more preferably 30 μm or less. If the number average particle diameter is less than 1 μm, the compression strength after impact of the CFRP decreases. Particles aggregate with each other. The number average particle diameter of the polyamide fine particles is preferably 2 μm or more, more preferably 3 μm or more, and even more preferably 5 μm or more.

[0047] The number average particle size of the polyamide particles is preferably from 2 μm to 80 μm, more preferably from 3 μm to 50 μm, and further preferably from 5 μm to 30 μm.

[0048] The number average particle size of polyamide microparticles can be calculated by randomly selecting 100 particle diameters from a scanning electron microscope photograph and calculating the arithmetic average. If the particle is not perfectly circular, i.e., elliptical, in the photograph, the maximum diameter of the particle is taken as the particle size. In order to measure the particle size accurately, the measurement is performed at a magnification of at least 1,000 times, preferably 5,000 times or more. The particle size distribution index is determined by the particle size value obtained above based on the following numerical conversion formula.

[0049] In the present invention, it is important that the sphericity of the polyamide particles is in the range of 80 to 100 in order to improve the toughness of the cured thermosetting resin and the compressive strength after impact of the CFRP. If the sphericity is less than 80, the compressive strength after impact of the CFRP decreases. The sphericity is preferably 90 or more, more preferably 94 or more, and further preferably 97 or more. The upper limit is 100.

[0050] The sphericity of the polyamide particles is preferably 90-100, more preferably 94-100, and further preferably 97-100.

[0051] The sphericity of polyamide particles is determined by observing 30 particles randomly from a scanning electron microscope photograph and calculating the sphericity from their minor and major axes according to the following formula.

[0052]

number

[0053] In addition, S: sphericity, a: major axis, b: minor axis, and n: number of measurements (30).

[0054] In the present invention, the polyamide particles have a particle surface smoothness and a solidity that is not porous inside. Such surface smoothness and solidity can be expressed by the amount of linseed oil absorbed by the polyamide particles. That is, the smaller the linseed oil absorption, which indicates the amount of linseed oil absorbed, the more solid the particles are with a smooth surface without holes. Here, the linseed oil absorption of the polyamide particles is 10mL to 100mL / 100g. If the linseed oil absorption of the polyamide particles is 10mL to 100mL / 100g, the compression strength after impact is particularly maintained. The upper limit of the linseed oil absorption is preferably 90mL / 100g or less, more preferably 80mL / 100g or less, even more preferably 70mL / 100g or less, and particularly preferably 60mL / 100g or less. The lower limit of the linseed oil absorption is preferably 10mL / 100g or more.

[0055] The linseed oil absorption of the polyamide particles is preferably from 10 to 90 mL / 100 g, more preferably from 10 to 80 mL / 100 g, and further preferably from 10 to 70 mL / 100 g.

[0056] Linseed oil absorption is measured in accordance with the Japanese Industrial Standards (JIS) K 5101 (2004) "Pigment Test Method: Refined Linseed Oil Method."

[0057] The blending amount of the polyamide particles [C] of the present invention is preferably 1 to 30 parts by mass relative to 100 parts by mass of the thermosetting resin composition. The blending amount can be appropriately adjusted, but if the blending amount is too large, the wet heat compression properties may decrease, and if the blending amount is too small, the compression strength after impact may decrease.

[0058] The particle size distribution index of the polyamide particles in the present invention is preferably 1.00 to 3.00. Here, the particle size distribution index refers to the particle size distribution. If the particle size distribution index exceeds 3.00, the moldability of the prepreg may decrease. The particle size distribution index is preferably 2.00 or less, more preferably 1.50 or less, even more preferably 1.30 or less, and most preferably 1.20 or less. The lower limit is theoretically 1.00.

[0059]

number

[0060] Di: particle size of each particle, n: number of measurements (100), Dn: number average particle size, Dv: volume average particle size, PDI: particle size distribution index.

[0061] In the present invention, the polyamide particles are preferably insoluble in the thermosetting resin [A] in order to exhibit the toughness of the thermosetting cured product and the compressive strength after impact of the CFRP. Here, insolubility in the thermosetting resin [A] means that the polyamide particles are not substantially dissolved in the thermosetting resin when the thermosetting resin in which the polyamide particles are dispersed is heat-cured. For example, it is judged by observing the polyamide particles in the thermosetting cured product with a clear interface between the polyamide particles and the thermosetting resin without substantially shrinking from the original size using a transmission electron microscope. Alternatively, it is judged by the fact that the amount and size of the polyamide particles recovered after removing the thermosetting resin after heating the polyamide particles and the thermosetting resin at 180°C do not change.

[0062] The polyamide particles in the present invention preferably contain 0.5% by mass or less of a second component having a weight-average molecular weight of 20,000 or less when the polyamide particles [C] are taken as 100% by mass.

[0063] If the weight average molecular weight of the second component polymer is too high, it becomes difficult to remove by washing, so the weight average molecular weight of the second component polymer is preferably 20,000 or less, more preferably 10,000 or less, and particularly preferably 8,000 or less.

[0064] The weight average molecular weight of the second component polymer is the weight average molecular weight measured by gel permeation chromatography using water as a solvent and converted into polyethylene glycol. If it is not soluble in water, it is possible to select a suitable solvent such as tetrahydrofuran.

[0065] The second component polymer is preferably one having a low content of polar groups such as hydroxyl groups, amino groups, and carboxyl groups, since this can prevent the aggregation of polyamide particles caused by the second component polymers and the deterioration of the moist heat properties. In particular, it is preferable that the hydroxyl groups are contained only at both ends of the molecule. Specific examples of the second component polymer are one or more compounds selected from the group consisting of polyethylene glycol, polypropylene glycol, polytetramethylene glycol, polyethylene glycol-polypropylene glycol copolymer, and alkyl ethers thereof. Since water can be used for washing, etc., and all processes from the production of particles to washing can be carried out using only water, polyethylene glycol, polyethylene glycol-polypropylene glycol copolymer, and alkyl ethers thereof are preferred, and polyethylene glycol and alkyl ethers thereof are most preferred. Two or more of these second component polymers may be used simultaneously within the scope of the present invention.

[0066] The lower the content of the second component polymer, which is an impurity in the polyamide particles, the more likely it is that the dispersibility of the polyamide particles in the thermosetting resin will improve and that the deterioration of the wet heat compression performance of the CFRP will be prevented. The content of the impurities in the polyamide particles is preferably 0.5% by mass or less, more preferably 0.05% by mass or less, particularly preferably 0.005% by mass or less, and even more preferably 0.002% by mass or less, when the polyamide particles are taken as 100% by mass.

[0067] The content of the second component polymer is a value determined by extracting the polymer powder with water or an organic solvent, removing the solvent, and then quantifying the amount by gel permeation chromatography using water as a solvent.

[0068] A suitable method for producing polyamide particles according to the present invention is, for example, the method described in International Publication WO2018 / 207728, in which a polyamide monomer is polymerized in the presence of a polymer serving as a second component at a temperature higher than the crystallization temperature of the polyamide obtained by polymerizing the monomer, and then the powder is washed and dried. This method makes it possible to produce polyamide particles having a high melting point, which is a requirement of the present invention, in a true spherical shape.

[0069] The thermosetting resin composition of the present invention may contain various additives within the range that does not impair the effects of the present invention. Examples of additives include known substances such as curing accelerators, flame retardants, flow agents, lubricants, antioxidants, viscosity modifiers, thermoplastic resins for toughness modifiers such as polyethersulfones, polyetherimides, or polyphenylene ethers.

[0070] The cured thermosetting resin of the present invention is produced by curing a thermosetting resin composition.

[0071] The glass transition temperature of the thermosetting resin cured product of the present invention is preferably 120 to 250°C, more preferably 140 to 210°C, from the viewpoint of sufficiently ensuring the heat resistance and compressive strength under wet heat required for aircraft materials.

[0072] The fiber-reinforced composite material of the present invention contains a cured thermosetting resin and reinforcing fibers.

[0073] As the reinforcing fibers used in the fiber-reinforced composite material of the present invention, carbon fibers, silicon carbide fibers, glass fibers, aramid fibers, etc. are preferably used, and carbon fibers are particularly preferably used since they are lightweight, have high performance, and can provide a fiber-reinforced composite material with excellent mechanical properties.

[0074] Specific examples of carbon fibers preferably used as reinforcing fibers include acrylic, pitch and rayon carbon fibers, and acrylic carbon fibers having particularly high tensile strength are preferably used.

[0075] Such acrylic carbon fibers can be obtained, for example, by spinning a spinning dope containing polyacrylonitrile obtained from a monomer mainly composed of acrylonitrile by a wet spinning method, a dry-wet spinning method, a dry spinning method, or a melt spinning method, and the solidified yarn after spinning is made into a precursor through a spinning process, and then through processes such as flame retardation and carbonization.

[0076] The carbon fiber can be in the form of twisted yarn, untwisted yarn, non-twisted yarn, etc., but in the case of twisted yarn, the filaments that make up the reinforcing fiber bundle are not arranged in parallel, which can cause a decrease in the mechanical properties of the fiber-reinforced composite material. Therefore, untwisted yarn or non-twisted yarn, which have a good balance between the formability and strength properties of the fiber-reinforced composite material, are preferably used.

[0077] When the fiber-reinforced composite material of the present invention is molded in an autoclave or oven, the optimum curing temperature and time vary depending on the type and amount of the selected curing agent and curing catalyst. For applications requiring heat resistance of 130°C or higher, it is preferable to cure at a temperature of 120 to 220°C for 0.5 to 8 hours. The temperature rise rate is preferably 0.1 to 10°C / min. If the temperature rise rate is less than 0.1°C / min, the time required to reach the target curing temperature may become very long, resulting in reduced workability. If the temperature rise rate exceeds 10°C / min, temperature differences may occur at various points of the reinforcing fibers, making it difficult to obtain a uniform cured product.

[0078] In this case, it is important that the sphericity of the polyamide particles in the obtained fiber reinforced composite is 80 to 100. The polyamide particles of the present invention have a high melting point and crystallization temperature, so that they can maintain a spherical shape without being deformed during heat curing of the thermosetting resin. Even if they are dissolved during heat curing, they will exhibit the same characteristics if they are phase separated into a spherical shape in the cured product. Whether the polyamide particles in the fiber reinforced composite are spherical or not can be confirmed by observing a cross-sectional photograph using the same measurement method as for the particles.

[0079] When molding the fiber-reinforced composite material of the present invention, pressurization or depressurization is not essential, but may be performed as necessary. Pressurization or depressurization may provide effects such as improved surface quality, suppression of internal voids, and improved adhesion to metals, plastics, and fiber-reinforced composite material parts to be bonded during curing.

[0080] INDUSTRIAL APPLICABILITY The fiber-reinforced composite material of the present invention has high tensile strength, high impact resistance, and high chemical resistance, and can therefore be widely used in aerospace applications requiring high mechanical properties, as well as general industrial applications such as wind turbines, automobiles, and bicycles.

[0081] The prepreg of the present invention is prepared by impregnating reinforcing fibers with a thermosetting resin composition.

[0082] As the reinforcing fibers used in the prepreg of the present invention, carbon fibers, silicon carbide fibers, glass fibers, aramid fibers, etc. are preferably used, and carbon fibers are particularly preferably used since they are lightweight, have high performance, and can give fiber-reinforced composite materials with excellent mechanical properties.

[0083] Specific examples of carbon fibers preferably used as reinforcing fibers include acrylic, pitch and rayon carbon fibers, and acrylic carbon fibers having particularly high tensile strength are preferably used.

[0084] Such acrylic carbon fibers can be obtained, for example, by spinning a spinning dope containing polyacrylonitrile obtained from a monomer mainly composed of acrylonitrile by a wet spinning method, a dry-wet spinning method, a dry spinning method, or a melt spinning method, and the solidified yarn after spinning is made into a precursor through a spinning process, and then through processes such as flame retardation and carbonization.

[0085] The carbon fiber can be in the form of twisted yarn, untwisted yarn, non-twisted yarn, etc., but in the case of twisted yarn, the filaments that make up the reinforcing fiber bundle are not arranged in parallel, which can cause a decrease in the mechanical properties of the fiber-reinforced composite material. Therefore, untwisted yarn or non-twisted yarn, which have a good balance between the formability and strength properties of the fiber-reinforced composite material, are preferably used.

[0086] The method for kneading the thermosetting resin composition used in the prepreg of the present invention may be any method generally used for preparing epoxy resin compositions, for example, a kneader or a planetary mixer.

[0087] The prepreg of the present invention can be produced by a wet method, a hot melt method or the like, which will be described below.

[0088] The wet method is a method in which reinforcing fibers are immersed in a solution of an epoxy resin composition, then pulled out, and the solvent is evaporated using an oven or the like, while the hot melt method is a method in which the epoxy resin composition, which has been made low viscosity by heating, is directly impregnated into reinforcing fibers, or a method in which the epoxy resin composition is first coated on release paper or the like to produce a film, and then the film is placed on both sides or one side of the reinforcing fibers, and the reinforcing fibers are impregnated with the resin by heating and pressurizing. The hot melt method is preferable because it results in substantially no solvent remaining in the prepreg.

[0089] The fiber-reinforced composite material of the present invention is preferably obtained by curing a prepreg.

[0090] A relatively high curing temperature is required for such a thermosetting resin having a relatively high heat resistance and for curing and molding a prepreg using the same. In addition, in order to fully develop the strength of the fiber-reinforced composite material obtained by curing and molding, the curing and molding of the prepreg laminate is generally performed under a pressurized condition of 1 atmosphere or more. For example, the fiber-reinforced composite material of the present invention, which is composed of a cured product of the thermosetting resin composition and reinforcing fibers, is produced by laminating the obtained prepregs and then heat-curing the laminate while applying pressure. Methods for applying heat and pressure include press molding, autoclave molding, bagging molding, wrapping tape method, and internal pressure molding.

[0091] INDUSTRIAL APPLICABILITY The fiber-reinforced composite material of the present invention has high tensile strength, high impact resistance, and high chemical resistance, and can therefore be widely used in aerospace applications requiring high mechanical properties, as well as general industrial applications such as wind turbines, automobiles, and bicycles. EXAMPLES

[0092] The present invention will be described below based on examples, but the present invention is not limited to these.

[0093] <Raw materials> <Thermosetting resin [A]: Epoxy resin> "Sumiepoxy (registered trademark)" ELM434 (tetraglycidyldiaminodiphenylmethane, manufactured by Sumitomo Chemical Co., Ltd.) "Araldite (registered trademark)" MY0600 (m-aminophenol type epoxy resin, manufactured by Huntsman Advanced Materials Co., Ltd.) "Epiclon (registered trademark)" 830 (bisphenol F type epoxy resin, manufactured by DIC Corporation) <Hardening agent [B]: Epoxy resin hardener> 3,3'-DAS (3,3'-diaminodiphenyl sulfone, manufactured by Mitsui Fine Chemicals, Inc.).

[0094] <Other ingredients> "Sumikaexcel (registered trademark)" PES5003P (polyethersulfone, manufactured by Sumitomo Chemical Co., Ltd.).

[0095] <Polyamide particles [C]> (1) Average particle size and particle size distribution index The number average particle size of the polyamide microparticles was calculated by randomly selecting 100 particle diameters from a scanning electron microscope photograph and calculating the arithmetic average. In the photograph, if the particle shape was not perfectly circular, i.e., elliptical, the maximum diameter of the particle was taken as the particle diameter. The particle size distribution index was calculated from the particle diameter value obtained above based on the following numerical conversion formula.

[0096]

number

[0097] Here, Di: particle size of each particle, n: number of measurements (100), Dn: number average particle size, Dv: volume average particle size, PDI: particle size distribution index.

[0098] (2) Sphericity The sphericity of the polyamide particles was calculated from the minor axis and major axis of 30 randomly selected particles observed in a scanning electron microscope photograph according to the following formula:

[0099]

number

[0100] In addition, S: sphericity, a: major axis, b: minor axis, and n: number of measurements (30).

[0101] (3) Linseed oil absorption In accordance with the Japanese Industrial Standards (JIS) JISK5101 "Pigment Test Method - Refined Linseed Oil Method," approximately 100 mg of polyamide microparticles were precisely weighed out on a watch glass, and refined linseed oil (Kanto Chemical Co., Ltd.) was gradually added drop by drop using a burette. After kneading with a palette knife, the dropping and kneading process was repeated until a sample mass was formed. The end point was the point at which the paste became smooth and hard, and the oil absorption (mL / 100g) was calculated from the amount of refined linseed oil used for dropping.

[0102] (4) Melting point and crystallization temperature of polyamide constituting polyamide particles Using a TA Instruments differential scanning calorimeter (DSCQ20), the melting point was determined as the apex of the endothermic peak when the temperature was raised from 30°C at 20°C / min under a nitrogen atmosphere. Whether or not the polyamide had a crystallization temperature was determined by the presence or absence of an exothermic peak that appeared when the temperature was raised from 30°C to a temperature 30°C higher than the endothermic peak indicating the melting point of the polyamide at a rate of 20°C / min under a nitrogen atmosphere using the same device, and then the temperature was held for 1 minute and cooled to 30°C at a rate of 20°C / min. If an exothermic peak was present, the polyamide was deemed crystalline. Approximately 8 mg of polyamide microparticles were required for the measurement.

[0103] (5) Molecular weight of polyamide constituting polyamide particles The weight average molecular weight of the polyamide was calculated by gel permeation chromatography in comparison with a calibration curve of polymethyl methacrylate. The measurement sample was prepared by dissolving about 3 mg of polyamide fine particles in about 3 g of hexafluoroisopropanol. Instrument: Waters e-Alliance GPC system Column: Showa Denko HFIP-806M x 2 Mobile phase: 5mmol / L sodium trifluoroacetate / hexafluoroisopropanol Flow rate: 1.0ml / min Temperature: 30℃ Detection: Differential refractometer.

[0104] (6) Content of impurities (second component polymer) in polyamide particles 1000g of water was added to 1000g of polyamide particles, and the mixture was heated to 80°C, after which the water was isolated. After removing the water, the obtained solid was dissolved in 5g of water, and the weight of the second component polymer was measured using the same gel permeation chromatography method as in (7). The content (mass%) was calculated by dividing the weight of the second component polymer by the amount of polyamide particles.

[0105] (7) Molecular weight of impurities (second component polymer) The weight average molecular weight of the impurity polymer was calculated by gel permeation chromatography in comparison with a calibration curve using polyethylene glycol. The measurement sample was prepared by dissolving about 3 mg in about 6 g of water. Equipment: Shimadzu Corporation LC-10A series Column: Tosoh Corporation TSKgel G3000PWXL Mobile phase: 100mmol / L sodium chloride aqueous solution Flow rate: 0.8ml / min Temperature: 40℃ Detection: Differential refractometer.

[0106] (8) Measurement method of structural units of general formula (1) 10 g of polyamide particles were dissolved in 90 g of hydrochloric acid, and then heated and stirred for 12 hours at 100° C. Thereafter, the amount of ε-caprolactam was quantified by gas chromatography, and the mass % in the constituent units was calculated.

[0107] ·Particle 1 (Production example 1) With reference to International Publication WO2018 / 207728, 200 g of ε-caprolactam (manufactured by Toray Industries, Inc.), 800 g of polyethylene glycol (Wako Pure Chemical Industries, Ltd., grade 1 polyethylene glycol, weight average molecular weight 18,600) as the second component polymer, and 1000 g of water were added to an autoclave equipped with a 3 L helical ribbon type stirring blade to form a homogeneous solution, which was then sealed and purged with nitrogen. The stirring speed was then set to 100 rpm, and the temperature was raised to 240°C. During this time, the pressure of the system was 10 kg / cm 2 After reaching 10kg / cm 2 The steam pressure was controlled to maintain a constant pressure of 0.2 kg / cm after the temperature reached 240°C. 2 The pressure was released at a rate of 1.5 mol / min. The temperature was then maintained for 1 hour while flowing nitrogen to complete the polymerization, and the mixture was discharged into a 2000g water bath to obtain a slurry. After dissolving the dissolved material, filtration was performed, and 2000g of water was added to the filtered material, which was then washed at 80°C. The slurry liquid was then filtered again to remove the aggregates that had been passed through a 200μm sieve, and the isolated filtered material was dried at 80°C for 12 hours to produce 140g of polyamide 6 powder. The melting point of the obtained powder was 218°C, the crystallization temperature was 170°C, and the molecular weight was 40,000, which was the same as polyamide 6. The number average particle size was 12μm, the particle size distribution index was 1.35, the sphericity was 96, the linseed oil absorption was 56mL / 100g, and the polyethylene glycol content was 0.004% by mass.

[0108] ·Particle 2 (Production example 2) Spherical polyamide 6 particles having a number average particle size of 30 μm were prepared in the same manner as in Production Example 1, except that the stirring speed was changed to 50 rpm.

[0109] ·Particle 3 (Production example 3) Spherical polyamide 6 particles having a number average particle size of 5 μm were prepared in the same manner as in Production Example 1, except that the stirring speed was changed to 250 rpm.

[0110] ·Particle 4 (Production example 4) Except for changing ε-caprolactam to capryllactam (manufactured by Wako Pure Chemical Industries, Ltd.), polyamide 8 particles were obtained in the same manner as in Production Example 1. The melting point of the particles was 200°C, the crystallization temperature was 150°C, the molecular weight was 40,000, the number average particle size was 13 μm, the particle size distribution index was 1.40, the sphericity was 98, and the linseed oil absorption was 60 mL / 100 g.

[0111] ·Particle 5 (manufacturing example 5) Polyamide 6 / 12 copolymer particles (80 mol % polyamide 6) were obtained in the same manner as in Production Example 1, except that ε-caprolactam (manufactured by Toray Industries, Inc.) was changed to 140 g and laurolactam (manufactured by Wako Pure Chemical Industries, Ltd.) was changed to 60 g. The melting point of the particles was 205° C., the crystallization temperature was 156° C., the molecular weight was 35,000, the number average particle size was 15 μm, the particle size distribution index was 1.25, the sphericity was 98, and the linseed oil absorption was 55 mL / 100 g.

[0112] ·Particle 6 (Production example 6) Polyamide 66 particles were obtained in the same manner as in Production Example 1, except that ε-caprolactam was replaced with 170 g of adipic acid (manufactured by Tokyo Chemical Industry Co., Ltd., SP value 25.4), 220 g of a 50% aqueous solution of hexamethylenediamine (manufactured by Tokyo Chemical Industry Co., Ltd., SP value 19.2), and the temperature was changed to 260° C. The melting point of the particles was 267° C., the crystallization temperature was 211° C., the molecular weight was 40,000, the number average particle size was 20 μm, the particle size distribution index was 1.52, the sphericity was 98, and the linseed oil absorption was 60 mL / 100 g.

[0113] ·Particle 7 (Production example 7) With reference to International Publication No. 2012 / 043509, 21 g of polyamide "TROGAMID (registered trademark)" CX7323 (weight average molecular weight 17,000, manufactured by Daicel-Evonik Co., Ltd.), 287 g of N-methyl-2-pyrrolidone as an organic solvent, and 42 g of polyvinyl alcohol (weight average molecular weight 29,000) with a sodium acetate content of 0.1% or less were added to a 1000 ml pressure-resistant glass autoclave (Hyper Glaster TEM-V1000N, manufactured by Taiatsu Glass Industry Co., Ltd.), and after nitrogen replacement of 99% by volume or more, the mixture was heated to 180°C and stirred for 4 hours until the polymer was dissolved. Then, 350 g of ion-exchanged water as a poor solvent was dropped at a speed of 2.91 g / min via a liquid pump. After adding about 30g of ion-exchanged water, the mixture was cooled while stirring, and the resulting suspension was filtered, reslurry washed with 700g of ion-exchanged water, and the filtered material was vacuum dried at 80°C for 10 hours to obtain 20.0g of a white solid. The resulting powder had a melting point of 250°C, no crystallization temperature, a number average particle size of 12.4μm, a particle size distribution index of 1.30, a sphericity of 95, and a linseed oil absorption of 65mL / 100g.

[0114] ·Particle 8 Commercially available polyamide 6 particles (Arkema's "Orgasol (registered trademark)" 1002D, number average particle size 18 μm, sphericity 68, melting point 212°C, crystallization temperature 165°C, weight average molecular weight 34,400, linseed oil absorption 90 mL / 100 g) ·Particle 9 Commercially available polyamide 6 particles (Toray TR-1, number average particle size 13 μm, sphericity 82, melting point 217°C, crystallization temperature 170°C, linseed oil absorption 120 mL / 100 g) ·Particle 10 Commercially available polyamide 12 particles (Toray SP-500, number average particle size 5 μm, sphericity 97, melting point 175°C, crystallization temperature 140°C, linseed oil absorption 60 mL / 100 g) <Reinforced fiber: Carbon fiber> "TORAYCA (registered trademark)" T800G-24K-31E (carbon fiber with 24,000 filaments, tensile strength of 5.9 GPa, tensile modulus of elasticity of 294 GPa, and tensile elongation of 2.0%, manufactured by Toray Industries, Inc.).

[0115] (9) Preparation of Thermosetting Resin Composition As the thermosetting resin [A], 10 parts by mass of Sumiepoxy (registered trademark) ELM434, 70 parts by mass of Araldite (registered trademark) MY0600, 20 parts by mass of Epicron (registered trademark) 830, and 15 parts by mass of Sumikaexcel (registered trademark) 5003P were added, and as the curing agent [B], 40 parts by mass of 3,3'-DAS and 65 parts by mass of a particle component (polyamide particles [C]) were added and kneaded to obtain an epoxy resin composition.

[0116] (10) Preparation of prepreg The thermosetting resin composition (9) is applied to a laminate in which the total weight of the thermosetting resin [A] and the curing agent [B] is 35 g / m 2 Two sheets of film-coated release paper were prepared so that the coating surfaces faced each other. Carbon fiber (Toray Industries, Inc., "TORAYCA (registered trademark)" T800G) with 24,000 filaments was aligned in one direction between the coated surfaces, and the fibers were impregnated with resin by heating and pressurization to obtain a carbon fiber basis weight of 250 g / m. 2 A primary prepreg having a resin content of 21.9% by mass was obtained. Next, the thermosetting resin composition (9) was applied to the primary prepreg at a basis weight of 35 g / m 2 Two sheets of film-coated release paper were prepared so that the carbon fiber weight was 250 g / m. The first prepreg was placed between these two resin-coated films, and heated and pressed in the same manner as the first prepreg. 2 A secondary prepreg was produced with a resin content of 35.9 mass%.

[0117] (11) Measurement of bending modulus and bending strain of cured thermosetting resin The thermosetting resin composition prepared in (9) was degassed in a vacuum and then poured into a mold set to a thickness of 2 mm using a 2 mm thick "Teflon (registered trademark)" spacer. It was cured at a temperature of 180°C for 2 hours to obtain a thermosetting resin cured product with a thickness of 2 mm. Next, a test piece with a width of 10 mm and a length of 60 mm was cut out from the obtained plate of the thermosetting resin cured product, and a three-point bending test with a span of 32 mm was performed to determine the flexural modulus, flexural strength, and flexural strain according to JIS K7171-1994. The flexural strain is an index of the toughness of the thermosetting resin cured product.

[0118] (12) Compressive strength measurement of fiber-reinforced composite materials under wet and hot conditions The prepreg prepared in (10) was laminated in 12 plies with the fiber direction parallel to the compression direction, and cured in an autoclave at a temperature of 180°C for 2 hours under a pressure of 0.59 MPa and a heating rate of 1.5°C / min to produce a laminate. A test piece with a tab of 2 mm thickness, 15 mm width, and 78 mm length was prepared from this laminate and immersed in hot water at 71°C for 14 days. The 0° compression strength of this test piece at 82°C was measured using a universal testing machine with a thermostatic bath in accordance with JIS K 7076 (1991). The number of samples was n=5. The 0° compression strength at 82°C is an index of compression performance under wet heat.

[0119] (13) Compressive strength after impact measurement of fiber-reinforced composite materials The prepregs prepared in (10) were laminated in a configuration of [45° / 0° / -45° / 90°]3s (symbol s indicates mirror symmetry) and cured in an autoclave at a temperature of 177°C and a pressure of 0.6MPa for 2 hours to obtain CFRP. This CFRP was cut into a rectangle with a 0° direction of 152.4mm and a 90° direction of 101.6mm according to JIS K7089 (1996), and a 5.4kg drop impact was applied to the center of the rectangle from a height of 571mm to obtain the average post-impact compressive strength. The measurements were also performed at room temperature in a dry state (25°C±2°C, relative humidity 50%).

[0120] [Examples 1 to 6, Comparative Examples 1 to 4] A thermosetting resin composition was prepared by the procedure of (9), and then a prepreg was obtained by the procedure of (10). The resin composition and prepreg obtained were used to measure the compressive strength of the fiber-reinforced composite material under wet heat (12), the compressive strength of the fiber-reinforced composite material after impact (13), and the sphericity of the polyamide particles in the fiber-reinforced composite material (14). The polyamide particles [C] used and the measurement results of the physical properties are shown in Tables 1 and 2.

[0121] [Table 1]

[0122] [Table 2] [Industrial Applicability]

[0123] The thermosetting resin composition of the present invention can be suitably used to produce a fiber-reinforced composite material having sufficient compressive strength after impact and wet heat compression performance.

[0124] The thermosetting resin composition of the present invention can be suitably used as a prepreg, and further as a cured thermosetting resin that is a matrix resin for a fiber-reinforced composite material.

[0125] The fiber-reinforced composite material produced using the thermosetting resin composition of the present invention has high tensile strength, high impact resistance, and high chemical resistance, and can therefore be widely used in aerospace applications that require high mechanical properties, as well as general industrial applications such as wind turbines, automobiles, and bicycles.

Claims

1. A thermosetting resin composition comprising at least [A], [B], and [C], characterized in that the amount of polyamide particles [C] blended is 1 to 30 parts by mass relative to 100 parts by mass of the thermosetting resin composition. [A] Thermosetting resin [B] Curing agent [C] Polyamide particles that satisfy the following (c1) to (c5): (c1) The melting point of the polyamide resin constituting the polyamide particles is 200 to 300° C. (c2) The crystallization temperature of the polyamide resin constituting the polyamide particles is 150° C. to 250° C. (c3) The number average particle size of the polyamide particles is 1 to 100 μm. (c4) The sphericity of the polyamide particles is 80 to 100. (c5) The polyamide particles have a linseed oil absorption of 10 to 100 mL / 100 g.

2. 2. The thermosetting resin composition according to claim 1, wherein the polyamide resin constituting the polyamide particles [C] contains 60 mass % or more of a structural unit represented by general formula (1). 【Chemistry 1】 (In the formula, n represents an integer of 4 to 7.)

3. The thermosetting resin composition according to claim 1 or 2, wherein the polyamide particles have a particle size distribution index of 1.00 to 3.

00.

4. The thermosetting resin composition according to claim 1 or 2, wherein n in general formula (1) is 5.

5. The thermosetting resin composition according to any one of claims 1 to 4, characterized in that the polyamide particles [C] have a sphericity of 90 to 100.

6. [C] The thermosetting resin composition according to any one of claims 1 to 5, comprising 0.5% by mass or less of a second component having a weight average molecular weight of 20,000 or less, when the polyamide particles are taken as 100% by mass.

7. The thermosetting resin composition according to any one of claims 1 to 6, wherein the thermosetting resin [A] is an epoxy resin.

8. A cured thermosetting resin product obtained by curing the thermosetting resin composition according to any one of claims 1 to 7.

9. A fiber-reinforced composite material comprising the cured thermosetting resin according to claim 8 and reinforcing fibers.

10. A prepreg comprising reinforcing fibers impregnated with the thermosetting resin composition according to any one of claims 1 to 7.

11. A fiber-reinforced composite material obtained by curing the prepreg according to claim 10.

Citation Information

Patent Citations

  • Fiber-reinforced composite material reinforced with porous resin particles

    JP1993001159A

  • Epoxy resin composition, prepreg and fiber reinforced composite material

    JP2011162619A

  • Thermosetting resin composite material containing interlayer toughened particle

    JP2018066016A

  • Pre-preg, fiber-reinforced composite material, and thermoplastic resin particles

    WO2014115844A1

  • Epoxy resin composition, prepreg, and fiber-reinforced composite material

    WO2015019965A1