Cellulose nanocrystal composite and method for producing same
The cellulose nanocrystal composite with anionic functional groups stabilizes metal fine particles, addressing handling and aggregation issues, enabling efficient dispersion and moldability with improved transparency and adhesion.
Patent Information
- Application Number
- JP2023003955
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-04-25
- Filing Date
- 2023-01-13
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-04-16
AI Technical Summary
Existing cellulose nanofibers with chemically treated TEMPO catalysts have long fiber lengths, leading to high viscosity and thixotropy, making them difficult to handle and coat, while ultrafine metal particles tend to aggregate and separate easily, hindering the efficient exhibition of their properties.
A cellulose nanocrystal composite is developed with sulfate and/or sulfo groups as anionic functional groups, supporting metal fine particles, which are uniformly dispersed and stabilized, reducing viscosity and thixotropy, and allowing for improved handling and transparency.
The composite achieves efficient and stable dispersion of metal fine particles, enhancing handling properties, transparency, and moldability, with suppressed viscosity and thixotropy, and allows for rapid solvent removal and adhesion to hydrophobic resins.
Smart Images

Figure 0007582349000002 
Figure 0007582349000003 
Figure 0007582349000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a cellulose nanocrystal composite carrying metal microparticles and a method for producing the same, and more specifically, to a cellulose nanocrystal composite having high metal microparticle carrying efficiency and stability, and excellent viscosity and dispersibility when formed into a dispersion, and a method for producing the same. [Background technology]
[0002] Nanocellulose has been proposed for use in various applications as an advanced biomass raw material, functional additive, film composite material, etc. In particular, cellulose nanofibers, which are made by mechanically micronizing cellulose fibers and chemically substituting hydrophilic functional groups such as carboxyl groups and phosphate groups into the hydroxyl groups of cellulose, require less energy for the micronization process and have improved dispersibility in aqueous solvents and transparency of the dispersion, and therefore attempts are being made to apply them to various applications (Patent Document 1, etc.).
[0003] Meanwhile, metal fine particles, particularly ultrafine metal particles with a particle diameter of 100 nm or less, have properties that are significantly different from those of ordinary metal particles, and because of their large surface activity and surface area, their use has been proposed in various fields, such as coloring agents, antibacterial agents, catalysts, adsorbents, etc. On the other hand, because ultrafine metal particles tend to aggregate, in order to efficiently utilize the excellent properties of ultrafine metal particles, it is necessary to maintain the ultrafine metal particles in a uniformly dispersed state. As a support for such ultrafine metal particles, a combination with the above-mentioned cellulose nanofibers has been proposed.
[0004] For example, Patent Document 2 listed below describes a composite comprising (A) cellulose nanofibers having carboxyl groups or carboxylate groups on the surface and (B) metal nanoparticles, in which the (B) metal nanoparticles are supported on the cellulose nanofibers via the carboxyl groups or carboxylate groups of the cellulose nanofibers as contact points. Furthermore, the following Patent Document 3 describes antibacterial fine cellulose in which metal microparticles made of silver or a compound thereof are supported on the surface of wood-derived fine cellulose, the fine cellulose having carboxyl groups at least on its crystal surface, and the metal microparticles being precipitated on the carboxyl groups on the crystal surface of the fine cellulose. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 4998981 [Patent Document 2] Patent No. 5566368 [Patent Document 3] Patent No. 6260077 Summary of the Invention [Problem to be solved by the invention]
[0006] However, the cellulose nanofibers chemically treated with the TEMPO catalyst used in Patent Documents 2 and 3 above have long fiber lengths, and their dispersions have high viscosity and thickening properties and are highly thixotropic, meaning that they are not yet fully satisfactory in terms of handleability, such as poor coatability and application feel, and it is difficult to efficiently and comfortably exhibit the excellent properties of the metal microparticles. In addition, since ultrafine metal particles tend to aggregate and, in dried form, tend to detach from the object to which they are attached, in order to efficiently utilize the excellent properties of ultrafine metal particles, it is necessary to disperse the ultrafine metal particles uniformly and to bind them to a support that imparts dispersibility, adhesion, etc. In order to more effectively utilize the performance of the fine metal particles, it is also necessary to efficiently and stably support a large number of fine metal particles on nanocellulose.
[0007] Therefore, the object of the present invention is to provide a cellulose nanocrystal composite carrying metal microparticles, which contains a large number of anionic functional groups capable of supporting metal microparticles, is capable of supporting metal microparticles efficiently and stably, is capable of suppressing thickening and thixotropy of the dispersion, and is easy to handle, and a method for producing the same. Another object of the present invention is to provide a dispersion having excellent transparency in which a metal microparticle-supported cellulose nanocrystal composite is uniformly dispersed, and a molded body containing a metal microparticle-supported cellulose nanocrystal composite that can efficiently exhibit properties derived from the metal microparticles, such as antibacterial properties. [Means for solving the problem]
[0008] According to the present invention, there is provided a cellulose nanocrystal composite in which metal fine particles are supported on cellulose nanocrystals containing sulfate groups and / or sulfo groups as anionic functional groups, and the total amount of the sulfate groups and / or sulfo groups is 0.7 mmol / g End A cellulose nanocrystal composite is provided, characterized in that the cellulose nanocrystal complex has a molecular weight of 4.0 mmol / g or less. The present invention also provides a cellulose nanocrystal composite in which metal microparticles are supported on cellulose nanocrystals containing sulfate groups and / or sulfo groups and anionic functional groups, wherein the anionic functional groups are at least one of phosphate groups or carboxyl groups, and the total amount of the sulfate groups and / or sulfo groups and the anionic functional groups is more than 0.17 mmol / g and not more than 4.0 mmol / g.
[0009] In the cellulose nanocrystal composite of the present invention, is before The cellulose nanocrystals preferably have a fiber width of 50 nm or less, a fiber length of 500 nm or less, and a crystallinity of 60% or more.
[0010] The present invention also provides a cellulose nanocrystal composite dispersion, characterized in that the above-mentioned cellulose nanocrystal composite is dispersed in a protic polar solvent. In the above cellulose nanocrystal composite dispersion, it is preferable that the viscosity of a dispersion having a cellulose nanocrystal composite concentration of 1 mass % at 20° C. and a rotation speed of 2.5 rpm is 1000 mPa·S or less. The present invention further provides a molded article comprising the above-mentioned cellulose nanocrystal composite. Effect of the Invention
[0011] The cellulose nanocrystal composite of the present invention uses cellulose nanocrystals having anionic functional groups such as highly polar sulfate groups and / or sulfo groups and divalent phosphate groups within the above-mentioned range, which increases the loading efficiency and stability of metal microparticles.In addition, since the cellulose nanocrystals themselves can be dispersed with good dispersibility in the dispersion medium, the metal microparticles can be dispersed uniformly and stably in the dispersion liquid without agglomeration. Furthermore, since cellulose nanocrystals have a short fiber length and a narrow fiber width, compared to the case where cellulose nanofibers are used, the increase in viscosity of the dispersion liquid and thixotropy can be suppressed, and the dispersion liquid also has excellent transparency. Furthermore, the cellulose nanocrystal composite of the present invention has excellent handling properties, such as coatability and application feel, because the thickening of the viscosity of the dispersion and thixotropy are suppressed, and molded bodies containing the cellulose nanocrystal composite carrying metal microparticles can be molded with good formability. Furthermore, cellulose nanocrystals containing anionic functional groups within the above range have the property that the fibers are easily separated due to charge repulsion between the nanocellulose fibers. Therefore, the cellulose nanocrystal composite of the present invention has good dispersibility even in protic solvents other than water, such as alcohol, has affinity for hydrophobic resins, and can shorten drying or heating times, resulting in excellent moldability. [Brief description of the drawings]
[0012] [Figure 1]FIG. 2 is an SPM image (300 nm scan) of silver microparticles and hydrophilized cellulose nanocrystals after the complex obtained in Example 1 was spin-coated onto a silicon wafer. [Diagram 2] FIG. 2 is an SPM image (1 μm scan) of silver microparticles and cellulose nanocrystals after the composite obtained in Comparative Example 1 was spin-coated onto a silicon wafer. [Diagram 3] FIG. 2 is an SPM image (1 μm scan) of silver microparticles and cellulose nanofibers after the composite obtained in Comparative Example 2 was spin-coated onto a silicon wafer. [Figure 4] This is the viscosity when the rotation speed of the composite obtained in Example 1 was increased and then decreased. [Diagram 5] This is the viscosity when the rotation speed of the composite obtained in Comparative Example 3 was increased and then decreased. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] (Cellulose Nanocrystals) The cellulose nanocrystals used in the present invention are cellulose nanocrystals containing sulfate groups and / or sulfo groups, and anionic functional groups, and it is important that the total amount of the sulfate groups and / or sulfo groups, and anionic functional groups is more than 0.17 mmol / g and not more than 4.0 mmol / g, particularly 0.25 to 1.5 mmol / g. If the total amount of sulfate groups and / or sulfo groups and anionic functional groups is less than the above range, the charge repulsion of nanocellulose will be reduced compared to when it is within the above range, and the dispersibility of cellulose nanocrystals will be reduced, and the desired metal particle support ability may not be obtained. On the other hand, if the total amount of sulfate groups and / or sulfo groups and anionic functional groups is greater than the above range, the crystal structure of nanocellulose cannot be maintained, and the excellent performance of cellulose nanocrystals, such as crystallinity, strength, and gas barrier properties, may be impaired. In the present invention, the "anionic functional group" contained in the cellulose nanocrystal means an anionic functional group introduced into the cellulose nanocrystal by hydrophilization treatment. However, as described below, the hydrophilization treatment may further introduce sulfate groups and / or sulfo groups as anionic functional groups, in which case the cellulose nanocrystal will contain only sulfate groups and / or sulfo groups, including the "anionic functional group."
[0014] In the present invention, the cellulose nanocrystal is preferably a cellulose nanocrystal hydrolyzed by sulfuric acid treatment, which has high cation exchange capacity and already contains sulfate and / or sulfo groups capable of efficiently supporting metals. That is, cellulose nanocrystals include those obtained by acid hydrolysis of cellulose fibers by sulfuric acid treatment or hydrochloric acid treatment, but cellulose nanocrystals obtained by hydrochloric acid treatment do not have sulfate and / or sulfo groups, and therefore have inferior metal particle supporting capacity compared to cellulose nanocrystals obtained by sulfuric acid treatment. In addition, by having sulfate and / or sulfo groups, the dispersibility of nanocellulose in protic solvents can be improved due to charge repulsion, as described above. The anionic functional group possessed by the cellulose nanocrystal is determined by the method of hydrophilization treatment of the cellulose nanocrystal described below, and is particularly preferably a carboxyl group, a phosphate group, a sulfate group and / or a sulfo group. In this specification, the term "sulfate group" includes a sulfate ester group.
[0015] In the present invention, the cellulose nanocrystals carrying metal particles can be produced by hydrophilizing sulfate and / or sulfo group-containing cellulose nanocrystals obtained by treating a cellulose raw material with sulfuric acid. Furthermore, before or after the hydrophilization treatment, the cellulose nanocrystals can be subjected to defibration and dispersion treatments, if necessary.
[0016] [Cellulose nanocrystals] The cellulose nanocrystals used as the raw material for the nanocellulose of the present invention are rod-shaped cellulose crystalline fibers obtained by acid hydrolysis of cellulose fibers such as pulp with sulfuric acid or hydrochloric acid. In the present invention, cellulose nanocrystals obtained by sulfuric acid treatment are used, which have sulfate groups and / or sulfo groups that can contribute to the formation of a self-organized structure. The cellulose nanocrystal preferably contains sulfate groups and / or sulfo groups in an amount of 0.01 to 0.17 mmol / g. The cellulose nanocrystal preferably has an average fiber diameter of 50 nm or less, particularly 2 to 50 nm, an average fiber length of 100 to 500 nm, an aspect ratio of 5 to 50, and a crystallinity of 60% or more, particularly 70% or more. The cellulose nanocrystals used in the present invention containing sulfate groups and / or sulfo groups, and anionic functional groups in the above-mentioned ranges can be obtained by subjecting cellulose nanocrystals having sulfate groups and / or sulfo groups to the hydrophilization treatment described below. However, cellulose nanofibers produced by conventional oxidation methods and having a fiber width of 50 nm or less and an aspect ratio of 10 or more can also be included to the extent that the excellent barrier properties and handleability of the nanocellulose of the present invention are not impaired; specifically, they can be used in an amount less than 50% of the cellulose nanocrystals.
[0017] [Hydrophilic treatment] In the present invention, the amount of sulfate groups and / or sulfo groups is adjusted by subjecting cellulose nanocrystals having the above-mentioned sulfate groups and / or sulfo groups to hydrophilization treatment, or anionic functional groups such as carboxyl groups and phosphate groups are introduced into the hydroxyl groups of cellulose, thereby preparing nanocellulose in which the total amount of anionic functional groups such as sulfate groups and / or sulfo groups, carboxyl groups, and phosphate groups is more than 0.17 mmol / g and 4.0 mmol / g or less, particularly in the range of 0.25 to 1.5 mmol / g. The hydrophilization treatment is carried out using any of Never Dry treatment, water-soluble carbodiimide, sulfuric acid, sulfur trioxide-pyridine complex, phosphoric acid-urea, TEMPO catalyst, and oxidizing agent. By using any of Never Dry treatment, carbodiimide, sulfuric acid, and sulfur trioxide-pyridine complex, the amount of sulfate group and / or sulfo group of cellulose nanocrystal is adjusted, and nanocellulose is further shortened. In addition, by using any of phosphoric acid-urea, TEMPO catalyst, and oxidizing agent, anionic functional groups of phosphoric acid group or carboxyl group are introduced, and the total amount of anionic functional groups of nanocellulose is adjusted to the above range. As for the hydrophilization treatment, any one of the treatments may be carried out so long as the total amount of anionic functional groups falls within the above-mentioned range, but the same treatment may be carried out multiple times, or may be carried out multiple times in combination with other treatments.
[0018] <Hydrophilic treatment using Never Dry treatment> Cellulose nanocrystals are solidified into powder or the like by drying treatment such as spray drying, heating, or reduced pressure, but during solidification by drying treatment, some of the anionic functional groups contained in the cellulose nanocrystals are eliminated, reducing the hydrophilicity. In other words, the never-dry treatment of cellulose nanocrystals containing anionic functional groups such as sulfate groups and / or sulfo groups, phosphate groups, and carboxyl groups, which does not involve solidification into powder or the like, is an example of a hydrophilization treatment. The never-dry treatment does not solidify the sulfate group- and / or sulfo group-containing cellulose nanocrystals used, i.e., it can be performed as a treatment alone, or in combination with a hydrophilization treatment using any of carbodiimide, sulfuric acid, sulfur trioxide-pyridine complex, phosphoric acid-urea, and TEMPO catalyst.
[0019] <Hydrophilic treatment using carbodiimide> In the treatment using carbodiimide, cellulose nanocrystals and carbodiimide are stirred in a solvent such as dimethylformamide, sulfuric acid is added thereto, and the mixture is reacted for 5 to 300 minutes at a temperature of 0 to 80° C. to form a sulfate ester. The carbodiimide and sulfuric acid are preferably used in amounts of 5 to 30 mmol and 5 to 30 mmol per gram (solid content) of cellulose nanocrystals. Next, an alkaline compound such as sodium hydroxide is added to convert the sulfate and / or sulfo groups introduced into the cellulose nanocrystals from H type to Na type, which is preferable in terms of improving the yield. Then, impurities are removed by filtration using a dialysis membrane or the like to prepare sulfate and / or sulfo modified cellulose nanocrystals. Examples of carbodiimides include 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide, which is a water-soluble compound having a carbodiimide group (-N=C=N-) in the molecule. Dicyclohexylcarbodiimide, which is soluble in organic solvents, can also be used.
[0020] <Hydrophilic treatment using sulfuric acid> The cellulose nanocrystals used in the present invention are sulfate and / or sulfo group-containing cellulose nanocrystals obtained by hydrolyzing cellulose fibers with sulfuric acid, and these cellulose nanocrystals are further hydrophilized using sulfuric acid. Sulfuric acid is preferably used at 40 to 60% by mass per 1 g (solid content) of cellulose nanocrystals. The reaction is carried out at a temperature of 40 to 60°C for 5 to 300 minutes, and then the mixture is subjected to a filtration process using a dialysis membrane or the like to remove impurities, thereby preparing sulfate and / or sulfo group-modified cellulose nanocrystals.
[0021] <Hydrophilic treatment using sulfur trioxide-pyridine complex> In the treatment using a sulfur trioxide-pyridine complex, cellulose nanocrystals are reacted with the sulfur trioxide-pyridine complex in dimethyl sulfoxide at a temperature of 0 to 60°C for 5 to 240 minutes to introduce sulfate groups and / or sulfo groups into the hydroxyl groups of the cellulose glycol units. The sulfur trioxide-pyridine complex is preferably blended in an amount of 0.5 to 4 g by mass per 1 g (solid content) of cellulose nanocrystals. After the reaction, it is preferable to add an alkaline compound such as sodium hydroxide to convert the sulfate group and / or sulfonate group introduced into the cellulose nanocrystals from the H form to the Na form in order to improve the yield. Thereafter, dimethylformamide or isopropyl alcohol is added, washed by centrifugation or the like, and then impurities and the like are removed by filtration using a dialysis membrane or the like, and the obtained concentrated solution is dispersed in water to prepare a sulfate group and / or sulfonate group-modified cellulose nanocrystal.
[0022] <Hydrophilic treatment using phosphoric acid-urea> The hydrophilic treatment using phosphoric acid-urea can be carried out in the same manner as the conventionally known treatment for introducing a phosphate group using phosphoric acid-urea. Specifically, in the presence of a urea-containing compound, a cellulose nanocrystal and a phosphate group-containing compound are reacted at a temperature of 135 to 180°C for 5 to 120 minutes to introduce a phosphate group into the hydroxyl group of the cellulose glucose unit. Examples of the phosphate group-containing compound include phosphoric acid, lithium salt of phosphoric acid, sodium salt of phosphoric acid, potassium salt of phosphoric acid, ammonium salt of phosphoric acid, etc. Among them, sodium dihydrogen phosphate, ammonium dihydrogen phosphate, phosphoric acid, etc. can be preferably used alone or in combination. The phosphate group-containing compound is preferably added in an amount of 10 to 100 mmol per 10 g (solid content) of cellulose nanocrystals. Examples of the urea-containing compound include urea, thiourea, biuret, phenylurea, benzylurea, dimethylurea, etc. Among them, urea can be preferably used. The urea-containing compound is preferably used in an amount of 150 to 200 mmol per 10 g (solid content) of cellulose nanocrystals.
[0023] <Hydrophilic treatment using TEMPO catalyst> The hydrophilization treatment using the TEMPO catalyst (2,2,6,6-tetramethylpiperidine 1-oxyl) can be carried out in the same manner as the conventionally known oxidation method using the TEMPO catalyst. Specifically, a hydrophilization reaction is caused in which the hydroxyl group at the 6-position of the cellulose glucose unit is oxidized to a carboxyl group in an aqueous system at room temperature and pressure using the TEMPO catalyst (2,2,6,6-tetramethylpiperidine 1-oxyl). As the TEMPO catalyst, in addition to the above-mentioned 2,2,6,6-tetramethylpiperidine 1-oxyl, derivatives of TEMPO such as 4-acetamido-TEMPO, 4-carboxy-TEMPO, and 4-phosphonoxy-TEMPO can also be used. The amount of the TEMPO catalyst used is 0.01 to 100 mmol, and preferably 0.01 to 5 mmol, per 1 g of cellulose nanocrystal (solid content).
[0024] During the hydrophilization treatment, it is preferable to use a co-oxidant such as an oxidant, bromide or iodide alone or in combination with the TEMPO catalyst. Examples of the oxidizing agent include known oxidizing agents such as halogen, hypohalous acid, halous acid, perhalogen acid or their salts, halogen oxides, and peroxides, and sodium hypochlorite and sodium hypobromite are particularly suitable. The amount of the oxidizing agent is 0.5 to 500 mmol, preferably 5 to 50 mmol, per gram of cellulose nanocrystal (solid content). After a certain period of time has elapsed since the addition of the oxidizing agent, additional oxidizing agent can be added to perform additional oxidation treatment. As the co-oxidizing agent, an alkali metal bromide such as sodium bromide, or an alkali metal iodide such as sodium iodide can be suitably used. The amount of the co-oxidizing agent is 0.1 to 100 mmol, preferably 0.5 to 5 mmol, per 1 g of cellulose nanocrystal (solid content). The reaction medium for the reaction solution is preferably water or an alcohol solvent.
[0025] The reaction temperature for the hydrophilization treatment is in the range of 1 to 50° C., particularly 10 to 50° C., and may be room temperature. The reaction time is preferably 1 to 360 minutes, particularly 60 to 240 minutes. As the reaction proceeds, carboxyl groups are produced in the cellulose, causing a decrease in the pH of the slurry. However, in order to ensure efficient oxidation reaction, it is desirable to maintain the pH in the range of 9 to 12 using a pH adjuster such as sodium hydroxide. After the oxidation treatment, the catalyst and other substances used are removed by washing with water or the like.
[0026] [Fiber defibration processing] In the present invention, since cellulose nanocrystals having short fiber length are used as the raw material, it is possible to carry out a defibration treatment after the hydrophilization treatment, although this is not necessarily required. The defibration treatment can be carried out by a conventionally known method. Specifically, the fiber can be pulverized using an ultra-high pressure homogenizer, an ultrasonic homogenizer, a grinder, a high-speed blender, a bead mill, a ball mill, a jet mill, a disintegrator, a beater, a twin-screw extruder, or the like. The defibration treatment can be performed in either a dry or wet manner, depending on the state of the nanocellulose after the hydrophilization treatment and the application of the nanocellulose. Since nanocellulose is preferably used in the form of a dispersion, it is preferable to defibrate it using water or the like as a dispersion medium with an ultra-high pressure homogenizer or the like.
[0027] [Distributed processing] In the cellulose nanocrystal composite of the present invention, as described below, it is preferable to mix the cellulose nanocrystals in a dispersion state with a metal compound capable of donating metal microparticles, and therefore it is desirable to subject the cellulose nanocrystals to a dispersion treatment. For the dispersion treatment, a dispersing machine such as an ultrasonic dispersing machine, a homogenizer, or a mixer can be suitably used, and a stirring method using a stirring rod, stirring stone, or the like may also be used.
[0028] (metal fine particles) The metal species of the metal particles supported by the cellulose nanocrystal composite of the present invention is not particularly limited, and can be appropriately selected depending on the desired effects of the metal particles, such as antibacterial performance, adsorption performance, catalytic performance, etc. Examples of metal particles include, but are not limited to, Cu, Ag, Au, In, Pd, Pt, Fe, Ni, Co, Zn, Nb, Sn, Ru, Rh, Ti, etc. The metal particles may be a single metal species, an alloy, or multiple types of metal particles. Although not limited thereto, it is preferable that the metal microparticles have an average primary particle size of 50 nm or less, particularly in the range of 5 to 20 nm, which allows the metal microparticles to be densely and stably supported on the surface of the cellulose nanocrystal and to efficiently exert the functions derived from the metal microparticles.
[0029] (Method of producing cellulose nanocrystal composite) As described above, the cellulose nanocrystal composite of the present invention carrying metal microparticles is produced by hydrophilizing cellulose nanocrystals containing sulfate groups and / or sulfo groups obtained by treating a cellulose raw material with sulfuric acid, and by allowing metal cations to interact with anionic functional groups such as sulfate groups and / or sulfo groups and phosphate groups on the surface of the cellulose nanocrystals, in which the total amount of sulfate groups and / or sulfo groups, and anionic functional groups is more than 0.17 mmol / g and 4.0 mmol / g or less, thereby carrying metal microparticles. A method for supporting metal microparticles on cellulose nanocrystals containing sulfate groups and / or sulfo groups and anionic functional groups is to mix a dispersion of cellulose nanocrystals containing sulfate groups and / or sulfo groups and anionic functional groups with a solution containing a metal compound, and then reduce the metal compound to produce cellulose nanocrystals carrying metal microparticles. The metal-containing solution is preferably a solution containing metal ions or metal compounds such as halides, nitrates, acetates, etc. The concentration of the metal ions or metal compounds in the metal-containing solution is not particularly limited, but is preferably 0.01 to 10 parts by mass per 100 parts by mass of cellulose nanocrystals.
[0030] A cellulose nanocrystal composite dispersion carrying metal particles can be prepared by mixing a cellulose nanocrystal dispersion with a metal compound solution and then reducing the metal compound to precipitate metal particles. The reduction method of the metal compound can be carried out by a known method, but it is desirable not to inhibit the bond between the metal compound and the anionic functional group when reducing the metal compound. Examples of such a reduction method include a gas phase reduction method using hydrogen and a liquid phase reduction method using a reducing agent, but the liquid phase reduction method using a reducing agent is preferable because it can be easily used in a mixed solution of a cellulose nanocrystal dispersion and a metal compound solution. Examples of reducing agents include, but are not limited to, metal hydrides such as sodium borohydride, potassium borohydride, lithium aluminum hydride, sodium cyanide borohydride, lithium trialkoxyaluminum hydride, and diisobutylaluminum hydride. From the viewpoints of safety, versatility, and the like, sodium borohydride is preferably used. The amount of reducing agent to be added varies depending on the type of metal in the metal compound and cannot be generally defined, but it is desirable to add 1 to 10 equivalents of the reducing agent per equivalent of the metal compound.
[0031] A dispersion containing a cellulose nanocrystal composite carrying metal microparticles has a viscosity of 1000 mPa·S or less, particularly 1 to 100 mPa·S (rotational viscometer, temperature 20°C) at a rotation speed of 2.5 rpm and a cellulose nanocrystal composite concentration of 1% by mass.Since the cellulose nanocrystals are thin and short, with a fiber width of 50 nm or less and a fiber length of 500 nm or less, thickening and thixotropy are suppressed, and the dispersion has excellent dispersibility, coatability, application feel, drying, and other handling properties. Thickening is a phenomenon that occurs due to polymers that dissolve or disperse in water and produce viscosity. Chemical derivatives of polysaccharides and cellulose are commonly used, but thickening has a significant effect on the handling of the dispersion, and the lower the viscosity of the dispersion, the less time and energy is required for dilution and dispersion into other dispersions, and the better the handling in terms of coatability, coating feel, drying, etc. The thixotropy of the dispersion is observed by a shear rate-shear stress loop generated by performing a hysteresis loop measurement in which the shear rate, such as the rotation speed, is increased and then decreased, and the degree of thixotropy of the dispersion can be evaluated by comparing the loop area. If the dispersion has thixotropy, the viscosity decreases when shear is repeatedly applied to the dispersion, and the coatability and coating feel change due to the decrease in viscosity during coating or application, or the shear stimulus applied before use, so suppressing the thixotropy has the effect of making the coatability and coating feel less likely to change. Furthermore, the resulting cellulose nanocrystal composite dispersion liquid has excellent transparency, with a total light transmittance of 50%T or more at a wavelength of 750 nm in a dispersion liquid containing 1% by mass of cellulose nanocrystal composite (solid content). In addition, the cellulose nanocrystal composite dispersion of the present invention can contain known additives such as fillers, colorants, UV absorbers, antistatic agents, water-resistant agents, crosslinking agents, metal salts, colloidal silica, alumina sol, titanium oxide, etc.
[0032] Although the cellulose nanocrystal composite dispersion can be used as it is in the form of an aqueous dispersion, by solvent replacement it can be made into a dispersion in which the dispersion medium is a protic polar solvent other than water, such as alcohol, whose dielectric constant (25°C) is between 15 and 80. This makes it possible to use it as a diluent for hydrophobic resins. As a method of solvent replacement, the cellulose nanocrystal composite aqueous dispersion can be mixed with a protic polar solvent after removing water from the aqueous dispersion by a dehydration method such as filtration using a centrifuge or a filter. After the solvent replacement treatment, the cellulose nanocrystal composite dispersion is prepared by dispersing the nanocellulose in the protic polar solvent by the same method as the above dispersion treatment.
[0033] (Molded body) The cellulose nanocrystal composite dispersion of the present invention prepared by the above method can be easily molded into molded articles such as films and sheets that have the gas barrier properties derived from the dense self-organized structure of the cellulose nanocrystal composite and also have the functions of metal particles, such as antibacterial properties. Furthermore, a dispersion obtained by dispersing the cellulose nanocrystal composite of the present invention in a protic polar solvent has affinity for hydrophobic resins and can efficiently remove the solvent by drying or heating in a short time, allowing efficient molding of molded articles.
[0034] [Molded body made of a mixture with polycationic resin] As described above, the cellulose nanocrystal composite dispersion of the present invention can be molded into a molded article by itself, but by forming a layer of the cellulose nanocrystal composite dispersion on a layer of a polyvalent cationic resin, it can be molded into a molded article of a mixture having a mixed state capable of expressing adhesion to a substrate. That is, a molded article can be molded from a mixture of a polyvalent cationic resin and a cellulose nanocrystal composite in a state in which the self-organized structure of the cellulose nanocrystals is maintained, and nanocellulose and polyvalent cationic resin are present from near the outermost surface of this molded article to the innermost surface (for example, in the direction of the substrate when formed on a substrate made of a thermoplastic resin).
[0035] The polyvalent cationic resin is a resin containing a water-soluble or water-dispersible polyvalent cationic functional group. Examples of such polyvalent cationic resin include water-soluble amine polymers such as polyethyleneimine, polyallylamine, polyamine polyamide epichlorohydrin, polyamine epichlorohydrin, polyacrylamide, poly(diallyldimethylammonium salt), dicyandiamide formalin, poly(meth)acrylate, cationic starch, cationic gum, gelatin, chitin, chitosan, etc., among which water-soluble amine and / or amino group-containing polymers, particularly polyethyleneimine, can be used preferably.
[0036] The polycation resin-containing solution is preferably a solution containing 0.01 to 30 mass %, particularly 0.1 to 10 mass %, of the polycation resin based on the solid content. If the amount of the polycation resin is less than the above range, the interfacial peel strength cannot be improved as compared with the case where the amount is within the above range, while if the amount of the polycation resin is more than the above range, the interfacial peel strength cannot be further improved, resulting in poor economic efficiency and possibly poor coatability and film-forming properties. The solvent used for the polyvalent cation resin-containing solution may be water, alcohols such as methanol, ethanol, and isopropanol, ketones such as 2-butanone and acetone, aromatic solvents such as toluene, and mixed solvents of these with water.
[0037] The amount of the polyvalent cationic resin-containing solution to be applied is determined based on the solid content of the cellulose nanocrystal composite in the layer formed from the cellulose nanocrystal composite dispersion liquid, depending on the concentration of the polyvalent cationic resin-containing solution. 2 When the polyvalent cation resin is contained in an amount of 1.0 g per m 2 It is preferable to coat the polycation resin in an amount of 0.01 to 2.0 g per unit area. If the amount of polycation resin is less than the above range, the interfacial peel strength with respect to a hydrophobic substrate such as a polyester resin cannot be improved as compared with the case where the amount is within the above range. On the other hand, even if the amount of polycation resin is more than the above range, no further improvement in the interfacial peel strength can be obtained, which is economically inferior. The coating method is not limited to the above, but can be, for example, spray coating, immersion, or coating with a bar coater, roll coater, gravure coater, spin coater, fingers, etc. The coating is preferably dried at a temperature of 5 to 200° C. for 0.1 seconds to 24 hours. The drying process can be performed by oven drying, infrared heating, high-frequency heating, etc., but natural drying is also possible.
[0038] The cellulose nanocrystal composite dispersion is preferably contained in an amount of 0.01 to 10 mass %, particularly 0.1 to 5.0 mass %, based on the solids content. If the amount is less than the above range, the effects obtained by containing the cellulose nanocrystal composite will be less than when it is in the above range, while if the amount is more than the above range, the coatability, application properties and film-forming properties will be inferior compared to when it is in the above range. The cellulose nanocrystal composite dispersion may be an aqueous dispersion or may be a protic polar solvent alone, or may be a mixed solvent with a ketone such as 2-butanone or acetone, or an aromatic solvent such as toluene. The cellulose nanocrystal composite dispersion liquid is a cellulose nanocrystal composite (solid content) of 1m 2 It is preferable to apply 0.1 to 3.0 g per unit. The coating and drying methods for the cellulose nanocrystal composite dispersion can be similar to those for the polyvalent cation-containing solution, but in the case of an aqueous dispersion, it is preferable to dry at a temperature of 5 to 200°C for 1 second to 24 hours, and in the case of a protic polar solvent, such as ethanol, it is preferable to dry at a temperature of 5 to 200°C for 1 second to 24 hours.
[0039] A laminate can also be produced by coating and drying a polycation resin-containing solution on a substrate made of a thermoplastic resin, and then coating and drying a cellulose nanocrystal composite dispersion on the substrate, forming a molded body made of a mixture of the cellulose nanocrystal composite and the polycation resin. A cast film can also be produced by coating and drying a polycation resin-containing solution and a cellulose nanocrystal composite dispersion in this order. Examples of the substrate include films, sheets, and molded articles in the form of bottles, cups, trays, pouches, etc., produced by means of lamination molding, extrusion molding, injection molding, blow molding, stretch blow molding, press molding, etc. using conventionally known thermoplastic resins such as polyolefins, polyesters, polyamides, polyvinyl alcohols, polystyrenes, acrylic resins, etc., and hydroxyl group- and / or carboxyl group-containing resins. EXAMPLES
[0040] Examples of the present invention will be described below. Note that the following examples are merely examples of the present invention, and the present invention is not limited to these examples. The preparation and measurement methods for each item are as follows.
[0041] <Amount of anionic functional groups> The cellulose nanocrystal or cellulose nanofiber dispersion was weighed, and ion-exchanged water was added to prepare 100 ml of 0.05 to 0.3 mass% cellulose nanocrystal or cellulose nanofiber dispersion. 0.1 g of cation exchange resin was added and stirred. Then, filtration was performed to separate the cation exchange resin from the cellulose nanocrystal or cellulose nanofiber dispersion. A 0.05 mol / L sodium hydroxide solution was dropped into the dispersion after cation exchange using an automatic potentiometric titrator (Kyoto Electronics Co., Ltd.), and the change in the electrical conductivity of the cellulose nanocrystal or cellulose nanofiber dispersion was measured. The titration amount of sodium hydroxide consumed for neutralization of the anionic functional group was determined from the obtained conductivity curve, and the amount of anionic functional group (mmol / g) was calculated using the following formula (1). Amount of anionic functional group (mmol / g)=Titer amount of sodium hydroxide consumed for neutralizing anionic functional group (ml)×Concentration of sodium hydroxide (mmol / ml)÷Solid mass of cellulose nanocrystal or cellulose nanofiber (g) (1)
[0042] <Preparation of hydrophilic cellulose nanocrystal dispersion> <Example 1> A phosphoric acid solution was prepared by dissolving 2.4 g of urea, 1 g of ammonium dihydrogen phosphate, and 3 g of ion-exchanged water, and 2 g (solids) of cellulose nanocrystals prepared by decomposing pulp with 64% by mass of sulfuric acid was added to the phosphoric acid solution and dispersed. The cellulose nanocrystal dispersion was heated at 165°C for 15 minutes while evaporating using a multi-safety dryer (manufactured by Futaba Scientific Co., Ltd.), and the cellulose nanocrystals were hydrophilized. Then, 100 ml of ion-exchanged water was added and dispersed, and the cellulose nanocrystals were washed using an ultracentrifuge (50,000 rpm, 10 minutes). The pH was adjusted to 12 by adding ion-exchanged water and sodium hydroxide solution, and the cellulose nanocrystals were washed using an ultracentrifuge (50,000 rpm, 10 minutes) while adding ion-exchanged water until the pH reached 8. The cellulose nanocrystals were then placed inside a dialysis membrane (manufactured by Spectrum Co., Ltd., molecular weight cutoff 3500-5000D) and left to stand in ion-exchanged water to remove impurities, and a hydrophilized cellulose nanocrystal dispersion was prepared. The purified hydrophilized cellulose nanocrystal dispersion was dispersed with ion-exchanged water to obtain a hydrophilized cellulose nanocrystal dispersion with a solid content of 1% by mass. The amount of anionic functional groups in the hydrophilized cellulose nanocrystals was 0.8 mmol / g.
[0043] <Preparation of cellulose nanocrystal composite> 5 ml of the hydrophilized cellulose nanocrystal dispersion with a solid content of 1% by mass of the hydrophilized cellulose nanocrystals was taken, and 8 mmol / L aqueous silver nitrate solution was added and stirred. Then, 16 mmol / L sodium boron hydroxide was added and stirred to reduce the silver ions, and silver particles were supported on the hydrophilized cellulose nanocrystals, thereby preparing a cellulose nanocrystal composite.
[0044] <Example 2> <Preparation of hydrophilic cellulose nanocrystal dispersion> Pulp was decomposed with 64% sulfuric acid to prepare cellulose nanocrystals. 1g (solid weight) was dispersed in 5ml of N,N-dimethylformamide. A solution of 10mmol of 1-ethyl-3-(3-diethylaminopropyl)carbodiimide hydrochloride (Tokyo Chemical Industry Co., Ltd.) was dissolved in 5ml of N,N-dimethylformamide and added to the cellulose nanocrystal dispersion and dispersed for 5 minutes. Then, a solution of 10mmol of sulfuric acid dispersed in 5ml of N,N-dimethylformamide was slowly added to the cellulose nanocrystal dispersion, and the cellulose nanocrystals were hydrophilized at 0℃ for 60 minutes while stirring to prepare a hydrophilized cellulose nanocrystal dispersion. Ion-exchanged water and sodium hydroxide solution were then added, and the membrane was placed inside a dialysis membrane (Spectrum, molecular weight cutoff 3500-5000D) and allowed to stand in ion-exchanged water to remove impurities, preparing a hydrophilized cellulose nanocrystal dispersion. Ion-exchanged water was added to the purified hydrophilized cellulose nanocrystal dispersion and the mixture was dispersed in a mixer to obtain a hydrophilized cellulose nanocrystal dispersion with a solid content of hydrophilized cellulose nanocrystals of 1% by mass. The amount of anionic functional groups in the hydrophilized cellulose nanocrystals was 0.7 mmol / g. The mixture was then treated in the same manner as in Example 1 to reduce the silver ions, and a cellulose nanocrystal composite was prepared in which silver particles were supported on the hydrophilized cellulose nanocrystals.
[0045] <Example 3> To an aqueous dispersion of 10 g (solids) of cellulose nanocrystals prepared by decomposing pulp with 64% sulfuric acid, 0.8 mmol of TEMPO catalyst (Sigma Aldrich) and 12.1 mmol of sodium bromide were added, and the mixture was made up to 1 L with ion-exchanged water and stirred until uniformly dispersed. Then, 5 mmol of sodium hypochlorite was added to start the oxidation reaction. During the reaction, the pH of the system was maintained at 10.0 to 10.5 with 0.5N sodium hydroxide aqueous solution, and hydrophilization was performed for 4 hours at 30°C while stirring. The hydrophilized cellulose nanocrystals were washed with ion-exchanged water and washed until the pH reached 8 using an ultracentrifuge (50,000 rpm, 10 min). The hydrophilized cellulose nanocrystals were then placed inside a dialysis membrane (Spectrum, molecular weight cutoff 3500-5000 D) and left to stand in ion-exchanged water to remove impurities, and a hydrophilized cellulose nanocrystal dispersion was prepared. The purified hydrophilized cellulose nanocrystal dispersion was added with ion-exchanged water and dispersed to obtain a hydrophilized cellulose nanocrystal dispersion with a solid content of hydrophilized cellulose nanocrystal of 1 mass%. The amount of anionic functional groups in the hydrophilized cellulose nanocrystal was 0.9 mmol / g. The procedure was then repeated in the same manner as in Example 1 to reduce the silver ions, and a cellulose nanocrystal composite was prepared in which silver particles were supported on the hydrophilized cellulose nanocrystal.
[0046] <Comparative Example 1> Pulp was decomposed with 64% by mass of sulfuric acid to prepare cellulose nanocrystals. 1 g (solid amount) was added to ion-exchanged water and dispersed to obtain a cellulose nanocrystal dispersion with a solid amount of cellulose nanocrystals of 1% by mass. The amount of anionic functional groups in the cellulose nanocrystals was 0.1 mmol / g. The silver ions were then reduced in the same manner as in Example 1 to prepare a cellulose nanocrystal composite in which silver particles were supported on the cellulose nanocrystals.
[0047] <Comparative Example 2> To an aqueous dispersion of 10 g (solid weight) of kraft pulp, 0.8 mmol of TEMPO catalyst (Sigma Aldrich) and 12.1 mmol of sodium bromide were added, and the mixture was made up to 1 L by adding ion-exchanged water and stirred until uniformly dispersed. 15 mmol of sodium hypochlorite was added per 1 g of cellulose to the reaction system to initiate the oxidation reaction. During the reaction, the pH of the system was maintained at 10.0 to 10.5 with a 0.5 N aqueous solution of sodium hydroxide, and the oxidation reaction was carried out at 30°C for 4 hours. The oxidized cellulose was thoroughly washed until it became neutral using a high-speed refrigerated centrifuge (16,500 rpm, 10 minutes) while adding ion-exchanged water. Water was added to the washed oxidized cellulose to adjust it to 1% by mass, and the mixture was defibrated in a mixer (7011JBB, Osaka Chemical Co., Ltd.) to prepare a cellulose nanofiber dispersion containing carboxyl groups. Thereafter, the mixture was treated in the same manner as in Example 1 to reduce silver ions, and a cellulose nanofiber composite in which silver fine particles were supported on the carboxyl groups of the cellulose nanofibers was prepared.
[0048] <Comparative Example 3> 5 ml of ion-exchanged water was collected, and 8 mmol / L aqueous silver nitrate solution was added and stirred. Then, 16 mmol / L sodium borohydride was added and stirred to reduce the silver ions, and a silver particle dispersion was prepared.
[0049] <Total light transmittance> The total light transmittance (%T) at 750 nm of 1 mass% cellulose nanocrystal composites, cellulose nanofiber composites, or microparticle dispersions prepared in Examples 1 to 3 or Comparative Examples 1 to 3 was determined using a spectrophotometer (UV-3100PC, Shimadzu Corporation).
[0050] <Viscosity measurement> Using a rotational viscometer (VISCO, Atago), the viscosity (mPa·S) of 1 mass% cellulose nanocrystal composites or cellulose nanofiber composites prepared in Examples 1 to 3 or Comparative Examples 1 to 3 was measured while increasing the spindle rotation speed from 2.5 to 250 rpm and then decreasing it to 3 rpm.
[0051] <Observation of silver particles after spin coating> The cellulose nanocrystal composite and cellulose nanofiber composite of Example 1 or Comparative Examples 1 and 2 were spread on a silicon wafer and spin-coated, and the silver particles were observed using an SPM (AFM5300E, Hitachi High-Tech Science). The observation was performed under the conditions of DFM mode and a silicon probe (spring constant equivalent to 9 N / m). The results are shown in Figures 1 to 3.
[0052] <Molded body made of a mixture with a polyvalent cationic resin> Polyethylenimine (PEI) (Epomin, P-1000, Nippon Shokubai Co., Ltd.) was applied to a corona-treated biaxially stretched PET film (Lumirror P60, 12 μm, Toray Industries, Inc.) substrate using a bar coater at a solid weight of 0.6 g / m 2 The mixture was dried at 50°C for 10 minutes in a hot air dryer (MSO-TP, manufactured by ADVANTEC) to solidify. The cellulose nanocrystal composites, cellulose nanofiber composites, or silver fine particle dispersions prepared above in Examples 1 to 3 and Comparative Examples 1 to 3 were applied onto the solidified polyethyleneimine using a bar coater (#40), and then dried at 25°C for 24 hours to prepare a molded product made of a mixture with a polyvalent cation resin.
[0053] <Antibacterial activity value based on antibacterial power test> The molded articles made from the cellulose nanocrystal composites, cellulose nanofiber composites, or silver particle dispersions of Examples 1 to 3 or Comparative Examples 1 to 3 were subjected to antibacterial activity tests based on the film adhesion method in JIS Z 2801:2012 "Antibacterial processed products - Antibacterial test methods, antibacterial effect" 5 test method, and antibacterial activity values against test bacteria were calculated. The test bacteria used were Staphylococcus aureus or Escherichia coli.
[0054] [Table 1] [Industrial Applicability]
[0055] The cellulose nanocrystal composite of the present invention has metal particles efficiently and stably supported on the cellulose nanocrystals, can be provided as a dispersion in which metal particles that tend to aggregate are uniformly dispersed, and has remarkably excellent handling properties such as coatability and coating feel because the viscosity increase and thixotropy of the dispersion are suppressed. In addition, since it is possible to use a protic polar solvent such as alcohol as a dispersion medium, it has affinity for hydrophobic resins and can be used with hydrophobic resins, and can efficiently impart functions such as antibacterial properties possessed by the metal particles to a molded product.
Claims
1. A cellulose nanocrystal composite in which metal microparticles are supported on cellulose nanocrystals containing sulfate groups and / or sulfo groups as anionic functional groups, characterized in that the total amount of the sulfate groups and / or sulfo groups is 0.7 mmol / g or more and 4.0 mmol / g or less.
2. A cellulose nanocrystal composite in which metal microparticles are supported on cellulose nanocrystals containing sulfate groups and / or sulfo groups and anionic functional groups, wherein the anionic functional groups are at least one of phosphate groups or carboxyl groups, and the total amount of the sulfate groups and / or sulfo groups and the anionic functional groups is more than 0.17 mmol / g and not more than 4.0 mmol / g.
3. 3. The cellulose nanocrystal composite according to claim 1, wherein the cellulose nanocrystal has a fiber width of 50 nm or less, a fiber length of 500 nm or less, and a crystallinity of 60% or more.
4. A cellulose nanocrystal composite dispersion liquid, comprising the cellulose nanocrystal composite according to claim 1 or 2 dispersed in a protic polar solvent.
5. 5. The cellulose nanocrystal composite dispersion according to claim 4, wherein the viscosity of a dispersion having a cellulose nanocrystal composite concentration of 1% by mass at 20°C and a rotation speed of 2.5 rpm is 1000 mPa·S or less.
6. A molded article comprising the cellulose nanocrystal composite according to claim 1 or 2.
Citation Information
Patent Citations
JP1974098981A
Sense amplifier for pacemaker
JP1980066368A
IC card detection system
JP1987060077A
Antifungal cellulose particle
JP1992122743A
Fuel cell electrode and fuel cell
JP2006202598A