Thermoplastic resin composition and its manufacturing method, molded body and its manufacturing method, and modifier and modification method

A tailored thermoplastic resin composition with defined polyolefin and polyamide components, enhanced by a modified elastomer, addresses the lack of tensile elongation in existing compositions, achieving high tensile elongation rates and maintaining impact resistance.

JP7582426B2Active Publication Date: 2024-11-13TOYOTA BOSHOKU KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023185718
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-01-24
Filing Date
2023-10-30
Publication Date
2024-11-13
Estimated Expiration
2039-11-20

AI Technical Summary

Technical Problem

Existing thermoplastic resin compositions, particularly those containing polyolefins and polyamides, do not adequately address tensile elongation, despite improvements in impact resistance.

Method used

A thermoplastic resin composition comprising specific polyolefin resins, polyamide resins, and modified elastomers, with defined molecular weights and structural characteristics, is formulated to enhance tensile elongation, achieved through a multi-step melt-kneading process.

Benefits of technology

The composition exhibits significantly improved tensile elongation rates, exceeding 50% in some cases, while maintaining impact resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582426000002
    Figure 0007582426000002
  • Figure 0007582426000003
    Figure 0007582426000003
  • Figure 0007582426000004
    Figure 0007582426000004
Patent Text Reader

Abstract

To provide a thermoplastic resin composition having improved tensile elongation and a method for producing the same, a molded article and a method for manufacturing the same, and a modifying agent and a modification method for improving tensile elongation of a polyolefin resin.SOLUTION: This composition contains a first polyolefin resin (A) having a Mn of less than 350,000, a second polyolefin resin (B) having a Mn of 350,000 or more, a polyamide resin (C) having a structure in which the number of linear-chain carbon atoms in a hydrocarbon group interposed between adjacent amide bonds in a main chain is 5 or less, and a modified elastomer (D) having a reactive group to the resin (C). A total amount of components (A) and (B) with respect to a total of 100 mass% of components (A)-(D) is 70 mass% or more. The amount of component (A) with respect to a total of 100 mass% of components (A) and (B) is 50 mass% or more and 87 mass% or less. The composition has a tensile elongation percentage of 50% or more.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermoplastic resin composition and a method for producing the same, a molded article and a method for producing the same, and a modifier and a modification method. More specifically, the present invention relates to a thermoplastic resin composition containing a polyolefin, a polyamide, and a modified elastomer and a method for producing the same, a molded article and a method for producing the same, and a modifier and a modification method. [Background technology]

[0002] The present inventors disclosed in Patent Document 1 that, in a thermoplastic resin composition containing a polyolefin resin, a polyamide resin, and a modified elastomer, a thermoplastic resin composition having excellent impact resistance can be obtained by using a polyolefin resin having a number average molecular weight of 350,000 or more in combination with a polyamide resin having a short-chain structure in which the number of linear carbon atoms between amide bonds is 5 or less. Furthermore, in Patent Documents 2 and 3, the inventors disclosed that the impact resistance of a molded article obtained by using the thermoplastic resin composition of Patent Document 1 can be improved. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2018 / 021569 Brochure [Patent Document 2] International Publication No. 2018 / 139378 Brochure [Patent Document 3] International Publication No. 2018 / 139379 Brochure Summary of the Invention [Problem to be solved by the invention]

[0004] However, the above Patent Documents 1 to 3 do not focus on or disclose anything about tensile elongation. An object of the present invention is to provide a thermoplastic resin composition having improved tensile elongation and a method for producing the same, a molded article and a method for producing the same, and a modifier and a modification method for improving the tensile elongation of a polyolefin resin. [Means for solving the problem]

[0005] As disclosed in the above Patent Document 1, the present inventors have found that in a thermoplastic resin composition containing components (B) to (D), a thermoplastic resin composition having excellent impact resistance can be obtained by selecting a polyolefin resin having a number average molecular weight of 350,000 or more as component (B) and further selecting a polyamide resin having a short-chain structure in which the number of linear carbon atoms between amide bonds is 5 or less as component (C).

[0006] As a result of further investigation into this technology, it was found that the impact resistance can be improved when the composition of Patent Document 1 is added to other polyolefin resins, and this technology was disclosed in Patent Documents 2 and 3 above. After further investigation, it was found that the impact resistance described above is the highest value of the impact resistance of the modifier itself, and when added to other polyolefins, the impact resistance does not exceed the inherent impact resistance of the modifier itself, but increases according to the amount of modifier added, whereas the tensile elongation exhibits a completely different and unique behavior. That is, it was found that when the modifier is added to other polyolefins, the tensile elongation may be extremely high, exceeding the inherent tensile elongation of the modifier itself, and the present invention was completed.

[0007] That is, the present invention is as follows. [1] The thermoplastic resin composition of the present invention comprises a first polyolefin resin (A) having a number average molecular weight of less than 350,000; A second polyolefin resin (B) having a number average molecular weight of 350,000 or more; a polyamide resin (C) having a structure in which the number of linear carbon atoms in a hydrocarbon group sandwiched between adjacent amide bonds in the main chain is 5 or less; and a modified elastomer (D) having a reactive group with respect to the polyamide resin (C), the total amount of the components (A) and (B) is 70% by mass or more when the total amount of the components (A), (B), (C) and (D) is 100% by mass, Furthermore, when the total amount of the components (A) and (B) is 100 mass%, the amount of the component (A) is 50 mass% or more and 87 mass% or less, The gist is that the tensile elongation is 50% or more. [2] In the thermoplastic resin composition of the present invention, the amount of the component (D) can be 50% by mass or more, relative to 100% by mass of the total of the components (C) and (D). [3] In the thermoplastic resin composition of the present invention, the component (C) can be selected from the group consisting of nylon 6, nylon 66, nylon 46, nylon 6T, nylon 6I, nylon M5T, nylon M5I, and copolymers thereof. [4] In the thermoplastic resin composition of the present invention, the component (D) may be an olefin-based thermoplastic elastomer having a skeleton of a copolymer of ethylene or propylene and an α-olefin having 3 to 8 carbon atoms, or a styrene-based thermoplastic elastomer having a styrene skeleton.

[0008] [5] The method for producing a thermoplastic resin composition of the present invention includes a second composition preparation step of melt-kneading a first composition obtained by melt-kneading the component (C) and the component (D) with the component (B) to obtain a second composition; and a third composition preparation step of melt-kneading the component (A) and the second composition to obtain a third composition.

[0009] [6] The molded article of the present invention has the thermoplastic resin composition of the present invention as its resin component.

[0010] [7] The method (1) for producing a molded article of the present invention includes a third composition preparation step of melt-kneading a second composition containing the components (B), (C), and (D) with the component (A) to obtain a third composition; and a molding step of molding the third composition to obtain the molded body. [8] The method (2) for producing a molded body of the present invention is characterized by comprising a molding step of molding a molten mixture of a second composition containing the components (B), (C), and (D) and the component (A) to obtain the molded body. [9] In the method for producing a molded body of the present invention, the second composition may be a composition obtained by melt-kneading a first composition obtained by melt-kneading component (C) and component (D), and component (B).

[0011]

[10] The modifier of the present invention is a modifier that, when added to a first polyolefin resin (A) having a number average molecular weight of less than 350,000, improves the tensile elongation of the resulting thermoplastic resin composition to 50% or more, A second polyolefin resin (B) having a number average molecular weight of 350,000 or more; a polyamide resin (C) having a structure in which the number of linear carbon atoms in a hydrocarbon group sandwiched between adjacent amide bonds in the main chain is 5 or less; and a modified elastomer (D) having a group reactive with the polyamide resin (C).

[11] In the modifier of the present invention, the content of the component (D) can be 50% by mass or more, where the total content of the components (C) and (D) is 100% by mass.

[12] In the modifier of the present invention, the content of the component (B) can be 45% by mass or more and 65% by mass or less, when the total content of the components (B), (C) and (D) is 100% by mass.

[0012]

[13] The modification method of the present invention is a method for improving the tensile elongation of the resulting thermoplastic resin composition to 50% or more by adding a first polyolefin resin (A) having a number average molecular weight of less than 350,000, A second polyolefin resin (B) having a number average molecular weight of 350,000 or more; a polyamide resin (C) having a structure in which the number of linear carbon atoms in a hydrocarbon group sandwiched between adjacent amide bonds in the main chain is 5 or less; The gist of the present invention is that a modifier containing a modified elastomer (D) having a group reactive to the polyamide resin (C) is added to the first polyolefin resin (A).

[14] In the modification method of the present invention, when the total of the components (A), (B), (C) and (D) is 100 mass%, the total of the components (A) and (B) is 70 mass% or more, and When the total of the components (A) and (B) is taken as 100% by mass, the modifier can be added so that the component (A) is 50% by mass or more and 87% by mass or less.

[15] In the modification method of the present invention, the modifier can be added in an amount of more than 20% by mass but less than 75% by mass, where the total of component (A) and the modifier is 100% by mass. Effect of the Invention

[0013] The thermoplastic resin composition and molded article of the present invention can provide high tensile elongation. According to the method for producing a thermoplastic resin composition and a molded article of the present invention, it is possible to obtain a thermoplastic resin composition and a molded article having high tensile elongation. According to the modifier and the modification method of the present invention, the tensile elongation of the obtained thermoplastic resin composition can be improved. That is, the obtained polyolefin-based resin composition can be modified so as to have an improved tensile elongation. [Brief description of the drawings]

[0014] [Figure 1] FIG. 2 is an explanatory diagram illustrating an example of a phase structure. [Diagram 2] FIG. 11 is an explanatory diagram for explaining another example of a phase structure. [Diagram 3] FIG. 11 is an explanatory diagram for explaining another example of a phase structure. [Figure 4] 1 is a graph showing the relationship between the polyolefin content and the tensile elongation, tensile strength, or impact strength for Experimental Examples 1 to 8. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The matters shown herein are illustrative and are intended to exemplify the embodiments of the present invention, and are described for the purpose of providing what is believed to be the most effective and easily understandable explanation of the principles and conceptual features of the present invention. In this respect, it is not intended to show structural details of the present invention beyond the extent necessary for a fundamental understanding of the present invention, and the description in conjunction with the drawings will make it clear to those skilled in the art how some forms of the present invention can be actually embodied.

[0016] [1] Thermoplastic resin composition The thermoplastic resin composition of the present invention (also simply referred to as "the composition") comprises a first polyolefin resin (A) having a number average molecular weight of less than 350,000; A second polyolefin resin (B) having a number average molecular weight of 350,000 or more; a polyamide resin (C) having a structure in which the number of linear carbon atoms in a hydrocarbon group sandwiched between adjacent amide bonds in the main chain is 5 or less; and a modified elastomer (D) having a reactive group with respect to the polyamide resin (C), When the total of components (A) to (D) is 100 mass%, the total of components (A) and (B) is 70 mass% or more, Furthermore, when the total of the components (A) and (B) is 100 mass%, the component (A) is 50 mass% or more and 87 mass% or less, It is characterized by having a tensile elongation of 50% or more.

[0017] <1> About each ingredient (1) First polyolefin resin (A) The first polyolefin resin (A) (also simply referred to as "component (A)") is a polyolefin resin having a number average molecular weight of less than 350,000. This component (A) may be an olefin homopolymer, an olefin copolymer, or a mixture thereof. The olefin constituting component (A) is not particularly limited, and examples thereof include ethylene, propylene, 1-butene, 3-methyl-1-butene, 1-pentene, 3-methyl-1-pentene, 4-methyl-1-pentene, 1-hexene, 1-octene, etc. These may be used alone or in combination of two or more. That is, examples of component (A) include polyethylene resin, polypropylene resin, poly-1-butene resin, poly-1-hexene resin, poly-4-methyl-1-pentene resin, etc. These polymers may be used alone or in combination of two or more. That is, component (A) may be a mixture of the above polymers.

[0018] Examples of the polyethylene resin include ethylene homopolymers and copolymers of ethylene and other olefins. These may be used alone or in combination of two or more. Examples of the other olefins constituting the ethylene copolymer include propylene, 1-butene, 3-methyl-1-butene, 1-pentene, 3-methyl-1-pentene, 4-methyl-1-pentene, 1-hexene, and 1-octene. The ethylene copolymer may have one or more of these other olefins as a copolymerization monomer. That is, examples of the ethylene copolymer include ethylene-propylene copolymers, ethylene-1-butene copolymers, ethylene-1-hexene copolymers, ethylene-1-octene copolymers, and ethylene-4-methyl-1-pentene copolymers (provided that 50% or more of the total number of constituent units are units derived from ethylene). These ethylene copolymers may be random copolymers or block copolymers. These may be used alone or in combination of two or more.

[0019] Examples of polypropylene resins include propylene homopolymers and copolymers of propylene and other olefins. These may be used alone or in combination of two or more. Among these, examples of other olefins constituting the propylene copolymer include ethylene, 1-butene, 3-methyl-1-butene, 1-pentene, 3-methyl-1-pentene, 4-methyl-1-pentene, 1-hexene, 1-octene, and the like. The propylene copolymer may have one or more of these other olefins as a copolymerization monomer. That is, examples of the propylene copolymer include propylene-ethylene copolymer, propylene-1-butene copolymer, propylene-1-hexene copolymer, propylene-1-octene copolymer, propylene-4-methyl-1-pentene copolymer, and the like (however, 50% or more of the total number of constituent units are units derived from propylene). These propylene copolymers may be random copolymers or block copolymers. These may be used alone or in combination of two or more.

[0020] In the present composition, as described above, any polyolefin resin may be used as component (A), and further, it may be a homopolymer or a copolymer, but for example, a propylene homopolymer (homopolymer of polypropylene) may be the main component (70% by mass or more, or may be 100% by mass, based on the entire component (A)). Also, a propylene copolymer (copolymer of polypropylene) may be the main component (usually 70% by mass or more, or may be 100% by mass, based on the entire component (A)). Among these, the propylene copolymer may be a random copolymer (random copolymerized polypropylene) or a block copolymer (block copolymerized polypropylene), but among these, the block copolymer is preferred from the viewpoint of excellent impact resistance. In particular, a propylene-ethylene block copolymer in which the other olefin is ethylene is preferred. This propylene-ethylene block copolymer is a block copolymerized polypropylene having an ethylene block as a dispersed phase. That is, it is a polypropylene resin in which a homopolypropylene is a continuous phase and a dispersed phase containing polyethylene exists within this continuous phase. Such a block copolymerized polypropylene having an ethylene block as a dispersed phase is also called, for example, an impact copolymer, a polypropylene impact copolymer, a heterophasic polypropylene, a heterophasic block polypropylene, etc.

[0021] Incidentally, component (A) differs from the modified elastomer in that component (A) is a component that does not show affinity for component (C) and is a component that does not have a reactive group that can react with component (C).

[0022] In the present composition, the number average molecular weight of component (A) is less than 350,000. By making the number average molecular weight of component (A) less than 350,000, the tensile elongation of the present composition can be significantly increased. The number average molecular weight of component (A) can be further set to 330,000 or less, and can be set to 300,000 or less. In addition, the number average molecular weight of component (A) can be set to 10,000 or more, 100,000 or more, and further 150,000 or more. Only one type of component (A) may be used, or two or more types may be used in combination. The number average molecular weight of component (A) is a polystyrene-equivalent number average molecular weight measured by gel permeation chromatography (GPC). When component (A) is a homopolymer, the above-mentioned ranges of the number average molecular weight can be read as the ranges of the weight average molecular weight.

[0023] The MFR (melt flow rate) of component (A) is not limited, but since the molecular weight (including the number average molecular weight) of component (A) and the MFR tend to show a proportional relationship, the MFR of component (A) is usually greater than the MFR of component (B). Specifically, the MFR of component (A) can be 10 g / 10 min or more. This MFR is preferably 12 g / 10 min or more, more preferably 14 g / 10 min or more. The MFR of component (A) can be 1500 g / 10 min or less, preferably 1000 g / 10 min or less, more preferably 500 g / 10 min or less. The MFR of polyolefin resin is measured in accordance with JIS K7210 under conditions of a temperature of 230° C. and a load of 21.18 N (2.16 kgf).

[0024] (2) Second polyolefin resin (B) The second polyolefin resin (B) (also simply referred to as "component (B)") is a polyolefin resin having a number average molecular weight of 350,000 or more. This component (B) may be an olefin homopolymer, an olefin copolymer, or a mixture thereof. The olefin constituting component (B) is not particularly limited, and the olefins exemplified as the olefins constituting component (A) can be used in the same manner, and further, the polyolefins exemplified as the component (A) can be used in the same manner.

[0025] In the present composition, as described above, any polyolefin resin may be used as component (B), and further, it may be a homopolymer or a copolymer, but for example, a propylene homopolymer (homopolymer of polypropylene) may be the main component (70% by mass or more, or may be 100% by mass, based on the entire component (B)). Also, a propylene copolymer (copolymer of polypropylene) may be the main component (usually 70% by mass or more, or may be 100% by mass, based on the entire component (B)). This propylene copolymer may be a random copolymer (random copolymerized polypropylene) or a block copolymer (block copolymerized polypropylene). Of these, the block copolymer is preferred from the viewpoint of excellent impact resistance, as in the case of component (A).

[0026] Incidentally, component (B) differs from the modified elastomer in that component (B) is a component that does not show affinity for component (C) and is a component that does not have a reactive group that can react with component (C).

[0027] In this composition, the number average molecular weight of component (B) is 350,000 or more. The number average molecular weight of component (B) of 350,000 or more can reduce the interface between components (B), which is considered to be advantageous in the present invention. In addition, when this composition has a specific phase structure (described later), it is considered that the impact resistance can be significantly improved even if the dispersion diameter of the dispersed phase remains relatively large. This effect is not expressed when a polyamide resin having a structure in which the linear carbon number of the hydrocarbon group sandwiched between adjacent amide bonds in the main chain is 6 or more is used, and is specifically expressed only when a polyamide resin having a structure in which the linear carbon number is 5 or less is used.

[0028] The number average molecular weight is preferably 370,000 or more, more preferably 400,000 or more, even more preferably 430,000 or more, even more preferably 450,000 or more, particularly preferably 470,000 or more, more particularly preferably 490,000 or more, particularly preferably 500,000 or more, even more preferably 505,000 or more, and even more preferably 510,000 or more. On the other hand, the upper limit is not limited, but can be, for example, 700,000 or less. The number average molecular weight of the polyolefin resin is a polystyrene-equivalent number average molecular weight determined by gel permeation chromatography (GPC). When component (B) is a homopolymer, the above-mentioned ranges of the number average molecular weight can be read as the ranges of the weight average molecular weight.

[0029] The MFR (melt flow rate) of component (B) is not limited, but since the molecular weight (including the number average molecular weight) of component (B) and the MFR tend to show a proportional relationship, the MFR of component (A) is usually greater than the MFR of component (B). Specifically, the MFR of component (A) can be 25g / 10min or less. This MFR is preferably 22g / 10min or less, more preferably 19g / 10min or less, even more preferably 16g / 10min or less, even more preferably 13g / 10min or less, particularly preferably 10g / 10min or less, more particularly preferably 9g / 10min or less, and particularly preferably 8g / 10min or less. Also, the MFR of component (B) can be 1g / 10min or more, preferably 1.5g / 10min or more, more preferably 2g / 10min or more. The MFR of polyolefin resin is measured in accordance with JIS K7210 under conditions of a temperature of 230° C. and a load of 21.18 N (2.16 kgf).

[0030] (3) Polyamide resin (C) The polyamide resin (C) (also simply referred to as "component (C)") is a polymer having a chain skeleton formed by polymerizing a plurality of monomers via amide bonds (-NH-CO-). In the present composition, component (C) has a structure in which the number of linear carbon atoms in the hydrocarbon group sandwiched between adjacent amide bonds in the main chain is 5 or less (in the present invention, simply referred to as a "short chain structure"), i.e., the polyamide molecules constituting component (C) have a short chain structure.

[0031] Examples of the above-mentioned structure having 5 linear carbon atoms include the following (1) to (6). (1)-NHCO-CH 2 -CH 2 -CH 2 -CH 2 -CH 2 -NHCO- (2)-CONH-CH 2 -CH 2 -CH 2 -CH 2-CH 2 -NHCO- (3)-NHOC-CH 2 -CH 2 -CH 2 -CH 2 -CH 2 -CONH- (4)-NHCO-CH 2 -CH 2 -CH 2 -CH 2 (CH 3 )-CH 2 -NHCO- (5)-CONH-CH 2 -CH 2 -CH 2 -CH 2 (CH 3 )-CH 2 -NHCO- (6)-NHOC-CH 2 -CH 2 -CH 2 -CH 2 (CH 3 )-CH 2 -CONH-

[0032] Examples of the structure having 4 linear carbon atoms include the following (7) to (12). (7)-NHCO-CH 2 -CH 2 -CH 2 -CH 2 -NHCO- (8)-CONH-CH 2 -CH 2 -CH 2 -CH 2 -NHCO- (9)-NHOC-CH 2 -CH 2 -CH 2 -CH 2 -CONH- (10)-NHCO-CH 2 -CH 2 -CH 2 (CH 3 )-CH 2 -NHCO- (11)-CONH-CH 2-CH 2 -CH 2 (CH 3 )-CH 2 -NHCO- (12)-NHOC-CH 2 -CH 2 -CH 2 (CH 3 )-CH 2 -CONH-

[0033] In the present composition, as component (C), a polyamide resin having only a short chain structure can be used. Specific examples include nylon 6 (PA6, polyamide 6), nylon 66 (PA66, polyamide 66), nylon 46 (PA46, polyamide 46), and copolymers thereof. These may be used alone or in combination of two or more. Moreover, examples of the copolymer include nylon 6 / 66 (PA6 / 66, nylon 6 / 66), etc. These may be used alone or in combination of two or more kinds.

[0034] In addition to the above-mentioned short chain structure, component (C) in the present composition may also have a structure in which the hydrocarbon groups sandwiched between adjacent amide bonds in the main chain are phenylene groups or their substituents (hereinafter simply referred to as "phenylene structure"). 6 H 4 -) is benzene (C 6 H 6 ) by removing two hydrogen atoms, and may be any of 1,2-phenylene, 1,3-phenylene, and 1,4-phenylene groups. These may be used alone or in combination of two or more. In addition, the substituent (-C 6 H 3 (R)-) usually has 6 to 10 main chain carbon atoms in the hydrocarbon group sandwiched between adjacent amide bonds in the main chain. That is, examples of the substituted phenylene group include a methylenephenylene group, a dimethylenephenylene group, and an ethylenephenylene group. These may be used alone or in combination of two or more.

[0035] That is, the component (C) in the present composition can be a polyamide resin having only a short chain structure and a phenylene structure. Specific examples include nylon 6T (PA6T, polyamide 6T), nylon 6I (PA6I, polyamide 6I), nylon M5T (PAM5T, polyamide M5T), nylon M5I (PAM5I, polyamide M5I), and copolymers thereof. These may be used alone or in combination of two or more. Examples of the copolymer include nylon 6T / 66 (PA6T / 66, nylon 6T / 66), nylon 6T / 6I (PA6T / 6I, polyamide 6T / 6I), nylon 6T / 6I / 66 (PA6T / 6I / 66, polyamide 6T / 6I / 66), nylon 6T / 2M-5T (PA6T / 2M-5T, polyamide 6T / 2M-5T), etc. These may be used alone or in combination of two or more.

[0036] Furthermore, the component (C) in the composition may be a polyamide resin containing the above-mentioned structure having more than 5 linear carbon atoms (simply referred to as "long chain structure" in the present invention) in addition to the above-mentioned short chain structure. That is, a polyamide resin having only a short chain structure and a long chain structure may be used. Examples of such polyamide resins having both a short chain structure and a long chain structure include nylon 610 (PA610, polyamide 610), nylon 611 (PA611, polyamide 611), nylon 612 (PA612, polyamide 612), polyamide 614 (PA614, polyamide 614), polyamide MXD6 (PAMXD6, polyamide MXD6), etc. These polyamides may be used alone or in combination of two or more. In addition, when a polyamide resin having both a short chain structure and a long chain structure is used in the present composition, it is preferable that the polyamide resin contains more than 50% of short chain structures (more preferably 60% or more and 99% or less) in the total of the short chain structures and the long chain structures.

[0037] In the present invention, it is preferable that component (C) is a polyamide resin containing more short chain structures. Therefore, a polyamide resin having substantially only short chain structures can be used as component (C). In this case, the effect of the present invention can be more strongly obtained. In addition, when a polyamide resin having both a short chain structure and a phenylene structure, or a polyamide resin having both a short chain structure and a long chain structure is used as component (C), the effects of the present invention can be more strongly obtained when component (C) having a high proportion of short chain structures is used. Specifically, the proportion (number proportion) of short-chain structures to the total of all structures (total units) including short-chain structures (i.e., short-chain units), phenylene structures (i.e., phenylene units), and long-chain structures (i.e., long-chain units) is preferably more than 50%, and more preferably 70% or more and 99% or less.

[0038] The number average molecular weight of component (C) in the present composition is not limited, but can be, for example, from 5,000 to 100,000, preferably from 7,500 to 50,000, and more preferably from 10,000 to 50,000. The number average molecular weight of the component (C) is a polystyrene-equivalent number average molecular weight determined by gel permeation chromatography (GPC).

[0039] The monomer constituting component (C) is not particularly limited, and any monomer capable of forming the above-mentioned short chain structure, phenylene structure, long chain structure, etc., as appropriate and as required, can be used. Specific examples include amino acids such as 6-aminocaproic acid, 11-aminoundecanoic acid, 12-aminododecanoic acid, and para-aminomethylbenzoic acid, and lactams such as ε-caprolactam, undecanelactam, and ω-lauryllactam. These may be used alone or in combination of two or more.

[0040] Furthermore, component (C) can be obtained by copolymerization of a diamine and a dicarboxylic acid. In this case, the diamine as a monomer can be ethylenediamine, 1,3-diaminopropane, 1,4-diaminobutane, 1,6-diaminohexane, 1,7-diaminoheptane, 1,8-diaminooctane, 1,9-diaminononane, 1,10-diaminodecane, 1,11-diaminoundecane, 1,12-diaminododecane, 1,13-diaminotridecane, 1,14-diaminotetradecane, 1,15-diaminopentadecane, 1,16-diaminohexadecane, or the like. Examples of the diamines include aliphatic diamines such as 1,17-diaminoheptadecane, 1,18-diaminooctadecane, 1,19-diaminononadecane, 1,20-diaminoeicosane, 2-methyl-1,5-diaminopentane, and 2-methyl-1,8-diaminooctane, alicyclic diamines such as cyclohexanediamine and bis-(4-aminocyclohexyl)methane, and aromatic diamines such as xylylenediamine (e.g., p-phenylenediamine and m-phenylenediamine). These may be used alone or in combination of two or more.

[0041] Further, examples of dicarboxylic acids as monomers include aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, brassicic acid, tetradecanedioic acid, pentadecanedioic acid, and octadecanedioic acid, alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid, and aromatic dicarboxylic acids such as phthalic acid, terephthalic acid, isophthalic acid, and naphthalenedicarboxylic acid. These may be used alone or in combination of two or more.

[0042] (4) Modified elastomer (D) The modified elastomer (D) (also simply referred to as "component (D)") is an elastomer having a reactive group with respect to component (C). This modified elastomer preferably exhibits affinity with component (C) by utilizing the reactive group described above, and at the same time, also exhibits affinity with component (B) separately. That is, component (D) is preferably a compatibilizer having a reactive group with component (C) and compatible with both components (B) and (C). In addition, component (D) may be contained in the present composition as an unreacted modified elastomer, or as a reaction product with component (C), or may be contained in both of these forms.

[0043] The reactive groups mentioned above include an acid anhydride group (-CO-O-OC-), a carboxyl group (-COOH), an epoxy group (-C 2 O (a three-membered ring structure consisting of two carbon atoms and one oxygen atom)}, an oxazoline group (-C 3 H 4 These may be used alone or in combination of two or more. These reactive groups can be introduced by modification to elastomers before modification (unmodified elastomers).Specific examples include acid-modified elastomers, epoxy-modified elastomers, and oxazoline-modified elastomers.Of these, acid-modified elastomers are preferred, and more preferred are elastomers modified with acid anhydrides or carboxylic acids. It is particularly preferred that this component (D) has an acid anhydride group or a carboxyl group in the side chain or terminal of the molecule. The amount of acid modification is not particularly limited, and for example, the number of acid anhydride groups or carboxyl groups contained in one molecule of the modified elastomer is preferably 1 or more, more preferably 2 to 50, even more preferably 3 to 30, and particularly preferably 5 to 20. These modified elastomers can be used alone or in combination of two or more kinds.

[0044] Examples of the elastomer before modification include olefin-based elastomers, styrene-based elastomers, etc. From the viewpoint of compatibility with component (B), olefin-based elastomers are particularly preferred. The olefin elastomer is preferably an α-olefin copolymer containing a structural unit derived from an α-olefin having a carbon number of 3 to 8, and may be an ethylene-α-olefin copolymer, an α-olefin copolymer, an α-olefin-non-conjugated diene copolymer, or an ethylene-α-olefin-non-conjugated diene copolymer. Of these, ethylene-α-olefin copolymers, α-olefin copolymers, and ethylene-α-olefin-non-conjugated diene copolymers are particularly preferred. The non-conjugated dienes include linear non-cyclic diene compounds such as 1,4-pentadiene, 1,4-hexadiene, 1,5-hexadiene, and 1,6-hexadiene; and branched non-cyclic diene compounds such as 5-methyl-1,4-hexadiene, 3,7-dimethyl-1,6-octadiene, 5,7-dimethylocta-1,6-diene, 3,7-dimethyl-1,7-octadiene, 7-methylocta-1,6-diene, and dihydromyrcene. alicyclic diene compounds such as tetrahydroindene, methyltetrahydroindene, dicyclopentadiene, bicyclo[2.2.1]-hepta-2,5-diene, 5-methylene-2-norbornene, 5-ethylidene-2-norbornene, 5-propenyl-2-norbornene, 5-isopropylidene-2-norbornene, 5-cyclohexylidene-2-norbornene, and 5-vinyl-2-norbornene.

[0045] Specific examples of the olefin elastomer include ethylene-propylene copolymers, ethylene-1-butene copolymers, ethylene-1-pentene copolymers, ethylene-1-hexene copolymers, ethylene-1-octene copolymers, propylene-1-butene copolymers, propylene-1-pentene copolymers, propylene-1-hexene copolymers, propylene-1-octene copolymers, etc. Among these, ethylene-propylene copolymers, ethylene-1-butene copolymers, and ethylene-1-octene copolymers are preferred.

[0046] Examples of the styrene-based elastomer include block copolymers of aromatic vinyl compounds and conjugated diene compounds, and hydrogenated products thereof. Examples of the aromatic vinyl compound include styrene, alkylstyrenes such as α-methylstyrene, p-methylstyrene, and p-tert-butylstyrene; p-methoxystyrene, and vinylnaphthalene. Examples of the conjugated diene compound include butadiene, isoprene, 1,3-pentadiene, methylpentadiene, phenylbutadiene, 3,4-dimethyl-1,3-hexadiene, and 4,5-diethyl-1,3-octadiene.

[0047] Specific examples of styrene-based elastomers include styrene-butadiene-styrene copolymer (SBS), styrene-isoprene-styrene copolymer (SIS), styrene-ethylene / butylene-styrene copolymer (SEBS), and styrene-ethylene / propylene-styrene copolymer (SEPS).

[0048] Examples of acid anhydrides for acid modification include maleic anhydride, phthalic anhydride, itaconic anhydride, succinic anhydride, glutaric anhydride, adipic anhydride, citraconic anhydride, tetrahydrophthalic anhydride, butenylsuccinic anhydride, etc. Among these, maleic anhydride, phthalic anhydride and itaconic anhydride are preferred. Examples of the carboxylic acid include acrylic acid, methacrylic acid, maleic acid, fumaric acid, itaconic acid, and citraconic acid.

[0049] As component (D) in the present composition, among the various modified elastomers mentioned above, an acid anhydride-modified elastomer is preferred, particularly an elastomer modified with maleic anhydride, and further, an acid-modified product of an α-olefin copolymer containing a structural unit derived from an α-olefin having 3 to 8 carbon atoms is preferred. Specifically, an elastomer modified with maleic anhydride, such as an ethylene-propylene copolymer modified with maleic anhydride, an ethylene-1-butene copolymer modified with maleic anhydride, an ethylene-1-hexene copolymer modified with maleic anhydride, or an ethylene-1-octene copolymer modified with maleic anhydride, is preferred. Specifically, an α-olefin copolymer "TAFMER series" (trade name) manufactured by Mitsui Chemicals Inc. or an "AMPLIFY series" (trade name) manufactured by Dow Chemical Company, etc. can be used.

[0050] The weight average molecular weight of component (D) in the present composition is not particularly limited, but can be, for example, from 10,000 to 500,000, preferably from 20,000 to 500,000, and more preferably from 30,000 to 300,000. The weight average molecular weight of the modified elastomer is a weight average molecular weight calculated in terms of polystyrene by gel permeation chromatography (GPC).

[0051] (4) Other ingredients The composition may consist of only the above-mentioned components (A) to (D), but may also contain other components in addition to these. The other components may be used alone or in combination of two or more. Other components include other thermoplastic resins. Specific examples include polyester-based resins (polybutylene terephthalate, polyethylene terephthalate, polycarbonate, polybutylene succinate, polyethylene succinate, polylactic acid, etc.) These may be used alone or in combination of two or more. When other thermoplastic resins are contained, when the total of components (A) to (D) and the other thermoplastic resins is 100 mass%, the other thermoplastic resins are preferably 25 mass% or less (further 20 mass% or less, further 15 mass% or less, further 10 mass% or less, further 5 mass% or less, 1 mass% or more).

[0052] Examples of additives that can be blended include nucleating agents, antioxidants, heat stabilizers, weathering agents, light stabilizers, plasticizers, ultraviolet absorbers, antistatic agents, flame retardants, slip agents, antiblocking agents, antifogging agents, lubricants, pigments, dyes, dispersants, copper damage inhibitors, neutralizing agents, bubble inhibitors, weld strength improvers, natural oils, synthetic oils, waxes, etc. These may be used alone or in combination of two or more.

[0053] 2. Phase structure The phase structure of the composition is not limited, but usually has a continuous phase X and a dispersed phase Y (see FIG. 1). Of these, the continuous phase X is composed of components (A) and (B). The dispersed phase Y is a phase dispersed within the continuous phase X, and is composed of components (C) and (D).

[0054] Furthermore, the dispersed phase Y is a continuous phase Y within the dispersed phase. 1 and dispersed phase Y 2 (hereinafter, also referred to as "finely dispersed phase") (see FIG. 2). 1 and finely dispersed phase Y 2 is usually composed of component (C) and / or component (D). Specific examples include the following phase structures (1) to (4). (1) Continuous phase Y in dispersed phase 1 is composed of component (C) and finely dispersed phase Y 2 Phase structure composed of component (D). 〈2〉 Continuous phase Y within the dispersed phase 1 is composed of component (C) and finely dispersed phase Y 2 Phase structure composed of both components (C) and (D). 〈3〉 Continuous phase Y in the dispersed phase 1 is composed of component (D) and finely dispersed phase Y 2 Phase structure composed of component (C). 〈4〉 Continuous phase Y within the dispersed phase 1is composed of component (D) and finely dispersed phase Y 2 The phase structure is composed of both components (C) and (D). The continuous phase Y in the dispersed phase 1 and finely dispersed phase Y 2 A dispersed phase Y having no (non-complexed dispersed phase Y) and a continuous phase Y in the dispersed phase 1 and finely dispersed phase Y 2 It may coexist with a dispersed phase Y having the above formula (multi-phase dispersed phase Y). In addition, component (D) may exist as an unreacted modified elastomer, or as a reaction product with component (C) (a reaction product of a polyamide resin and a modified elastomer), or as a mixture thereof.

[0055] Furthermore, the dispersed phase Y can have a boundary phase Z around it (see FIG. 3). The boundary layer Z is a phase located at the boundary between the continuous phase X and the dispersed phase Y. This boundary phase Z tends to be easily formed when a propylene-ethylene block copolymer is used as component (A) and / or component (B). The thickness (width) of the boundary phase Z tends to increase as the proportion of the propylene-ethylene block copolymer in the total components of component (A) and component (B) increases. From this, it is considered that all or a part of the boundary phase Z is formed by the ethylene block that constituted the propylene-ethylene block copolymer. Note that the boundary phase Z can have various thicknesses (thickness of the boundary layer Z). Furthermore, the dispersed phase Y having the boundary phase Z and the dispersed phase Y not having the boundary phase Z may coexist.

[0056] The phase structure of the composition can be observed by observing the treated surface of a test piece (a test piece made of the composition) that has been subjected to oxygen plasma etching and then osmium coating, using a field emission scanning electron microscope (FE-SEM). In particular, the dispersed phase and finely dispersed phase can be observed in an image magnified 1000 times or more (usually 10,000 times or less) by this method. In addition, the components that make up each phase can be identified by performing energy dispersive X-ray analysis (EDS) during observation using a field emission scanning electron microscope (FE-SEM).

[0057] When the composition contains dispersed phase Y, its size is not particularly limited, but the dispersed diameter (average dispersed diameter) of dispersed phase Y can be 10,000 nm or less, 50 nm or more and 8,000 nm or less, or even 100 nm or more and 4,000 nm or less. The dispersion diameter of the dispersed phase Y is measured in an image obtained by magnifying the image by 1000 times or more using an electron microscope. That is, the longest diameter of each of 20 dispersed phase Y particles randomly selected from a predetermined area in the image is measured, and the average of the obtained longest diameters is set as the first average value. Then, the further average value of the first average values ​​measured in five different areas in the image is set as the average dispersion diameter (long axis average dispersion diameter) of the dispersed phase Y.

[0058] The composition contains a finely dispersed phase Y 2 In the case where the finely dispersed phase Y 2 The dispersion diameter (average dispersion diameter) of the particles can be 5 nm or more and 1000 nm or less, can be 5 nm or more and 600 nm or less, further can be 10 nm or more and 400 nm or less, and particularly can be 15 nm or more and 350 nm or less. This finely dispersed phase Y 2 The dispersion diameter of the finely dispersed phase Y is measured in an image obtained by magnifying the image by 1000 times or more using an electron microscope. 2 The longest diameter of each of the particles is measured, and the average of the longest diameters obtained is taken as the first average value. Then, the further average value of the first average values ​​measured in five different regions in the image is taken as the finely dispersed phase Y 2 The average dispersion diameter (major axis average dispersion diameter) of

[0059] <3> About the composition In this composition, when the total of the four components (A) to (D) is 100% by mass, the total of the components (A) and (B) is 70% by mass or more. That is, the composition has a high polyolefin content of 70% by mass or more. Therefore, this composition can be said to be a polyolefin-based thermoplastic composition. In such a composition with a high polyolefin content, the properties of the polyolefin are strong, but the tensile elongation that polyolefin (100% polyolefin) originally has is less than 50%. In contrast, this composition can have a tensile elongation of 50% or more while containing 70% or more by mass of polyolefin. In other words, this composition can be said to be a composition in which the tensile elongation of polyolefin is significantly improved by containing less than 30% by mass of the components (C) and (D) in total.

[0060] When the total of the above-mentioned four components (A) to (D) is taken as 100% by mass, the total proportion of component (A) and component (B) may be 70% by mass or more, and the upper limit can be set to 95% by mass or less. Within this range, a particularly high tensile elongation can be obtained. This proportion can be further set to 71% by mass or more, and further set to 72% by mass or more. On the other hand, this proportion can be further set to 90% by mass or less, and further set to 87% by mass or less. Within these ranges, a higher tensile elongation can be obtained.

[0061] Furthermore, in the present composition, when the total of components (A) and (B) contained in the composition is 70 mass% or more as described above and the total is taken as 100 mass%, component (A) is contained in an amount of 50 mass% to 87 mass%. In other words, when the components (A) and (B) contained in the present composition are compared, the amount of component (A) is greater. When the total of the two components (A) and (B) is 100 mass%, the proportion of component (A) can be 52 mass% or more, 55 mass% or more, 58 mass% or more, or 60 mass% or more. On the other hand, this proportion can be 85 mass% or less, 83 mass% or less, 81 mass% or less, or 80 mass% or less. Within these ranges, a higher tensile elongation can be obtained.

[0062] More specifically, in the present composition, when the total of the four components (A) to (D) is taken as 100 mass%, the proportion of component (A) can be more than 25 mass%, can be 27 mass% or more, can be 32 mass% or more, and can be 37 mass% or more. On the other hand, this proportion can be less than 80 mass%, can be 79 mass% or less, can be 78 mass% or less, and can be 77 mass% or less. Within these ranges, a higher tensile elongation can be obtained.

[0063] In this composition, when the total of the three components (B) to (D) is 100 mass%, the proportion of component (B) can be 2 mass% or more and 90 mass% or less. This proportion is preferably 5 mass% or more and 85 mass% or less, more preferably 10 mass% or more and 83 mass% or less, more preferably 15 mass% or more and 80 mass% or less, more preferably 20 mass% or more and 78 mass% or less, more preferably 25 mass% or more and 75 mass% or less, more preferably 30 mass% or more and 73 mass% or less, more preferably 35 mass% or more and 70 mass% or less, and more preferably 45 mass% or more and 65 mass% or less. Within the above range, a high tensile elongation can be obtained.

[0064] In this composition, when the total of the three components (B) to (D) is 100 mass%, the ratio of component (C) and component (D) (a part or all of these may be reacted with each other; the same applies below) can be 10 mass% or more and 98 mass% or less. This ratio is preferably 15 mass% or more and 95 mass% or less, more preferably 17 mass% or more and 90 mass% or less, more preferably 20 mass% or more and 85 mass% or less, more preferably 22 mass% or more and 80 mass% or less, more preferably 25 mass% or more and 75 mass% or less, more preferably 27 mass% or more and 70 mass% or less, more preferably 30 mass% or more and 65 mass% or less, and more preferably 35 mass% or more and 65 mass% or less. Within the above range, a high tensile elongation can be obtained.

[0065] In this composition, when the total of the three components (B) to (D) is 100 mass%, the proportion of component (C) can be 1 mass% or more and 50 mass% or less. This proportion is preferably 3 mass% or more and 45 mass% or less, more preferably 5 mass% or more and 40 mass% or less, more preferably 6 mass% or more and 35 mass% or less, more preferably 7 mass% or more and 30 mass% or less, more preferably 8 mass% or more and 28 mass% or less, more preferably 9 mass% or more and 20 mass% or less, and more preferably 10 mass% or more and 18 mass% or less. Within the above range, a high tensile elongation can be obtained.

[0066] In this composition, when the total of the three components (B) to (D) is 100 mass%, the proportion of component (D) can be 1 mass% or more and 60 mass% or less. This proportion is preferably 5 mass% or more and 53 mass% or less, more preferably 10 mass% or more and 45 mass% or less, more preferably 15 mass% or more and 40 mass% or less, more preferably 17 mass% or more and 38 mass% or less, more preferably 20 mass% or more and 37 mass% or less, more preferably 23 mass% or more and 36 mass% or less, and more preferably 26 mass% or more and 35 mass% or less. Within the above range, a high tensile elongation can be obtained.

[0067] In this composition, when the total of the two components, component (B) and component (C), is 100 mass%, the proportion of component (C) can be 1 mass% or more and 90 mass% or less. This proportion is preferably 3 mass% or more and 80 mass% or less, more preferably 5 mass% or more and 70 mass% or less, more preferably 6 mass% or more and 55 mass% or less, more preferably 7 mass% or more and 45 mass% or less, more preferably 8 mass% or more and 40 mass% or less, more preferably 9 mass% or more and 35 mass% or less, and more preferably 10 mass% or more and 30 mass% or less. Within the above range, a high tensile elongation can be obtained.

[0068] In this composition, when the total of the two components, component (C) and component (D), is 100 mass%, the proportion of component (D) can be 1 mass% or more and 99 mass% or less. This proportion is preferably 5 mass% or more and 80 mass% or less, more preferably 10 mass% or more and 60 mass% or less, more preferably 15 mass% or more and 55 mass% or less, more preferably 20 mass% or more and 50 mass% or less, more preferably 23 mass% or more and 45 mass% or less, and more preferably 25 mass% or more and 40 mass% or less. Within the above range, a high tensile elongation can be obtained.

[0069] When the composition has a predetermined phase structure as described above, the content ratio of each component of the composition can be approximately calculated from the type of component constituting each phase and the area ratio of each phase. That is, the area ratio of each phase can be calculated from the analysis of the above-mentioned FE-SEM image (however, the magnification may be 1000 times or less). This area ratio is an approximate volume ratio. Then, the content ratio of the component constituting each phase can be converted from the density of each component. For example, when component (A) is a propylene-ethylene block copolymer (e.g., 0.90 to 0.91 g / cm 3 ) and component (B) homopolypropylene (e.g., 0.90 to 0.91 g / cm 3 ) and component (C) is PA6 (e.g., 1.12 to 1.13 g / cm 3 ), and component (D) is maleic acid-modified EBR (for example, 0.86 to 0.88 g / cm 3 ) The area ratio of the continuous phase X and the aggregated phase Z to the dispersed phase Y is 5:5, and the continuous phase Y in the dispersed phase is1 and finely dispersed phase Y 2 In the case where the area ratio of components (A) to (D) is 5:5, the total content of components (A) and (B) can be approximately calculated to be 47.6% by mass when the total of the four components (A) to (D) is 100% by mass.

[0070] According to the present composition, a high tensile elongation can be obtained. Specifically, the tensile elongation measured by the method shown in the examples described later can be 50% or more and 1000% or less, further 100% or more and 850% or less, further 150% or more and 700% or less, further 200% or more and 650% or less, further 230% or more and 600% or less, and further 250% or more and 550% or less. In particular, the tensile elongation can be made 200% or more (usually 1000% or less) when the total of the components (A) to (D) is 35 to 80% by mass, the total of the components (A) to (D) is 10 to 40% by mass, the total of the components (B) is 2 to 12% by mass, and the total of the components (C) to (D) is 5 to 25% by mass. Furthermore, the tensile elongation can be made 400% or more (usually 1000% or less) when the total of the components (A) to (D) is 35 to 70% by mass, the total of the components (A) to (D) is 20 to 45% by mass, the total of the components (C) is 5 to 12% by mass, and the total of the components (D) is 100% by mass.

[0071] [2] Method for producing thermoplastic resin composition The method for producing the composition is characterized by comprising a second composition preparation step and a third composition preparation step. In the method for producing the composition, the third composition obtained in the third composition preparation step is usually the composition for producing the composition. The four components (A) to (D) and their respective content ratios are as described above. Also, the content ratios and amounts of each component in the composition for producing ...

[0072] The above-mentioned "second composition preparation step" is a step of melt-kneading the first composition and component (B) to obtain the second composition. The first composition is a composition obtained by melt-kneading the components (C) and (D). That is, the first composition is a melt-kneaded mixture of the components (C) and (D). The second composition is a composition obtained by melt-kneading the first composition and component (B), that is, the second composition is a melt-kneaded product of the first composition and component (B). The above-mentioned "third composition preparation step" is a step of melt-kneading component (A) and the second composition to obtain the third composition. The third composition is a composition obtained by melt-kneading the second composition and component (A), that is, the third composition is a melt-kneaded product of the second composition and component (A).

[0073] The melt kneading in these steps refers to kneading in a molten or softened state. Although the specific temperature is not limited, the melt kneading for obtaining the first composition, the melt kneading for obtaining the second composition (melt kneading in the second composition preparation step), and the melt kneading for obtaining the third composition (melt kneading in the third composition preparation step) can be melt kneaded at, for example, 190°C or higher and 350°C or lower. In particular, from the viewpoint of obtaining the first composition, the melt kneading in this range can promote the reaction between the reactive group of component (D) and component (C). These melt kneadings can be further performed at 200°C or higher and 300°C or lower, and particularly preferably 205°C or higher and 260°C or lower.

[0074] In addition, each melt kneading may be performed using any kneading device (melt kneading device). For example, an extruder (single-screw extruder, twin-screw kneading extruder, etc.), a kneader, a mixer (high-speed flow mixer, paddle mixer, ribbon mixer, etc.), etc. may be used. These devices may be used alone or in combination of two or more types. When two or more types are used, they may be operated continuously or in batches (batch type). Furthermore, each raw material may be mixed all at once, or may be added and charged in several separate batches (multi-stage blending).

[0075] In this manufacturing method, it is considered that the reaction between component (C) and component (D) is promoted by forming the first composition in advance, and particles in which component (C) and component (D) have reacted well (hereinafter simply referred to as "reacted particles") are formed. That is, it is considered that good quality reacted particles can be formed by reacting only component (C) and component (D). To predict the mechanism, it is considered that when melt kneading is started, particles are formed in which the reactive group of the modified elastomer reacts on the surface of the polyamide resin particle, but it is considered that the particles are sheared by applying a shear force during melt kneading, and the unreacted polyamide resin in the particles is exposed to the surface of the particles. Then, it is considered that the unreacted component (C) reacts with this exposed unreacted polyamide resin. It is considered that the above-mentioned good quality reacted particles are formed by repeating this situation. Furthermore, it is considered that it is possible to stably form reaction particles with a smaller particle size without relying on a high shear. If the amount of component (D) that can be supplied in the above process is small, it is considered that the reaction will not proceed easily and the reaction particles will not become small. Therefore, it is considered preferable that the amount of component (D) that can be supplied is necessary and sufficient.

[0076] As described above, each step may be performed continuously or batchwise. For example, in the case of performing the batchwise process, the melt-kneading step for obtaining the first composition may not be continuous with the second composition preparation step. In this case, the first composition may be solidified (pelletized, etc.) once. That is, it may be made into a solid first composition. Therefore, in this case, in the second composition preparation step, the solid first composition and the solid component (B) are melt-kneaded. In this case, the solid first composition and the solid component (B) may be in the form of pellets, lumps, powder, or other shapes. In any case, it is preferable that they are finely divided so as to be easily mixed. Similarly, the second composition obtained in the second composition preparation step can be used continuously in the third composition preparation step without solidification, but can also be solidified once. In this case, in the third composition preparation step, the solid second composition and the solid component (A) are melt-kneaded. In this case, the solid second composition and the solid component (A) may be in the form of pellets, lumps, powder, or other shapes. In any case, it is preferable that they are finely divided so as to be easily mixed.

[0077] [3] Molded body The molded article of the present invention is characterized in that the resin component is the present composition. The present composition constituting the present molded body is as described above. The present molded body may be a solid molded body (solid molded body) or a foam molded body. The present molded body may be molded in any manner, and the method is not limited. For example, it can be subjected to injection molding, extrusion molding (sheet extrusion, profile extrusion), T-die molding, blow molding, injection blow molding, inflation molding, hollow molding, vacuum molding, compression molding, press molding, stamping mold molding, transfer molding, etc. These may be used alone or in combination of two or more.

[0078] The molded article may be made of only the composition, but may also have a structure other than the composition. Examples of the structure other than the composition include aggregates. More specifically, the molded article may have aggregates formed from resins other than the composition, or aggregates formed from materials other than resins, such as metals. These aggregates may be introduced, for example, by insert molding.

[0079] Furthermore, the dimensions of the molded body, such as the shape, size, and thickness, are not particularly limited, and the use is also not particularly limited. The molded body can be used, for example, as exterior materials, interior materials, structural materials, and shock absorbing materials for automobiles, railroad cars, ships, and airplanes. Among these, examples of automotive products include exterior materials for automobiles, interior materials for automobiles, structural materials for automobiles, shock absorbing materials for automobiles, and parts inside the engine room. Specific examples include bumpers, spoilers, cowlings, front grilles, garnishes, bonnets, trunk lids, cowl louvers, fender panels, rocker moldings, door panels, roof panels, instrument panels, center clusters, door trims, quarter trims, roof linings, pillar garnishes, deck trims, tonneau boards, package trays, dashboards, console boxes, kicking plates, switch bases, seat backboards, seat frames, armrests, sun visors, intake manifolds, engine head covers, engine under covers, oil filter housings, housings for in-vehicle electronic components (ECUs, TV monitors, etc.), and air filter boxes.

[0080] Other examples include interior materials, exterior materials, and structural materials for buildings and furniture. That is, the material can be used as door covering materials, door structural materials, and covering materials and structural materials for various furniture (desks, chairs, shelves, chests, etc.). In addition, the material can be used as packaging materials, containers (trays, etc.), protective materials, partition materials, etc. The material can also be used as molded articles such as housings and structures for home appliances (flat-screen TVs, refrigerators, washing machines, vacuum cleaners, mobile phones, portable game consoles, notebook computers, etc.).

[0081] [4] Manufacturing method of molded body The method for producing the present molded body includes the following (1) first method and (2) second method. (1) The first method is characterized by comprising a third composition preparation step and a molding step. The third composition preparation step is a step of melt-kneading the second composition containing the three components (B) to (D) and the component (A) to obtain the third composition. The molding step is a step of molding the third composition to obtain a molded body. On the other hand, (2) the second method includes a molding step in which a melt-kneaded mixture of a second composition containing the three components (B) to (D) and the component (A) is molded to obtain a molded body.

[0082] The difference between the first method and the second method is whether or not a third composition is prepared for molding. That is, in the first method, the third composition is formed and then molded. Therefore, the third composition, which is a melt-kneaded product of the second composition and component (A), can be solidified to obtain the third composition (e.g., pellet-shaped, etc.) as a master batch suitable for molding. Then, this third composition is put into a molding machine and molded. On the other hand, the second method molds a melt-kneaded product of the second composition and component (A) (a composition that is not solidified and is in a melt-kneaded state) as it is. That is, in the second method, the melt-kneaded product of the second composition and component (A) can be molded directly without forming a master batch suitable for molding (for example, the solid second composition and the solid component (A) are dry-blended, and then the solid mixture is melt-kneaded and molded).

[0083] In general, by adopting the first method, uneven distribution of the second composition and component (A) in the obtained molded body can be prevented. In this respect, when manufacturing the present molded body, the second method can be actively selected. That is, even if molding is performed by the second method, uneven distribution of the second composition and component (A) in the molded body can be sufficiently prevented. The reason why an excellent molded body can be obtained without preparing a molding master batch (third composition) in this way is considered to be because the total of components (A) and (B) is as high as 70 mass% or more when the total of the four components (A) to (D) is 100 mass%. That is, conversely, it is considered to be because the total of components (C) and (D) is as low as less than 30 mass%. In this way, by utilizing the second method, it is possible to reduce the number of melt-kneading steps by one and obtain a molded product having excellent tensile elongation.

[0084] In these methods, the second composition is a composition obtained by melt-kneading the first composition obtained by melt-kneading component (C) and component (D) with component (B), as in the case of the method for producing the present composition.

[0085] [5] Modifier The modifier of the present invention (hereinafter, simply referred to as "the modifier") is a modifier that improves the tensile elongation of the resulting thermoplastic resin composition by adding it to component (A). Specifically, it is a modifier that can modify component (A) so that the tensile elongation is 50% or more. The modifier is characterized by containing components (B), (C), and (D). These four components (A) to (D) are the same as those in the composition of the present invention described above. The content ratio and amount of each component are the same as those in the composition of the present invention described above. Furthermore, this modifier can be obtained as the second composition in the method for producing the composition of the present invention described above or the method for producing the molded product of the present invention described above.

[0086] Therefore, in the present modifier, when the total of the three components (B) to (D) is 100 mass%, the proportion of component (B) can be 2 mass% or more and 90 mass% or less. This proportion is preferably 5 mass% or more and 85 mass% or less, more preferably 10 mass% or more and 83 mass% or less, more preferably 15 mass% or more and 80 mass% or less, more preferably 20 mass% or more and 78 mass% or less, more preferably 25 mass% or more and 75 mass% or less, more preferably 30 mass% or more and 73 mass% or less, more preferably 35 mass% or more and 70 mass% or less, and more preferably 45 mass% or more and 65 mass% or less. In the above range, a high tensile elongation can be imparted to the thermoplastic resin composition and molded article obtained by modification.

[0087] In this modifier, when the total of the three components (B) to (D) is 100 mass%, the ratio of component (C) and component (D) (part or all of which may be reacted with each other; the same applies below) can be 10 mass% or more and 98 mass% or less. This ratio is preferably 15 mass% or more and 95 mass% or less, more preferably 17 mass% or more and 90 mass% or less, more preferably 20 mass% or more and 85 mass% or less, more preferably 22 mass% or more and 80 mass% or less, more preferably 25 mass% or more and 75 mass% or less, more preferably 27 mass% or more and 70 mass% or less, more preferably 30 mass% or more and 65 mass% or less, and more preferably 35 mass% or more and 65 mass% or less. In the above range, a high tensile elongation can be imparted to the thermoplastic resin composition and molded article obtained by modification.

[0088] In this modifier, when the total of the three components (B) to (D) is 100 mass%, the proportion of component (C) can be 1 mass% or more and 50 mass% or less. This proportion is preferably 3 mass% or more and 45 mass% or less, more preferably 5 mass% or more and 40 mass% or less, more preferably 6 mass% or more and 35 mass% or less, more preferably 7 mass% or more and 30 mass% or less, more preferably 8 mass% or more and 28 mass% or less, more preferably 9 mass% or more and 20 mass% or less, and more preferably 10 mass% or more and 18 mass% or less. In the above range, a high tensile elongation can be imparted to the thermoplastic resin composition and molded article obtained by the modification.

[0089] In this modifier, when the total of the three components (B) to (D) is 100 mass%, the proportion of component (D) can be 1 mass% or more and 60 mass% or less. This proportion is preferably 5 mass% or more and 53 mass% or less, more preferably 10 mass% or more and 45 mass% or less, more preferably 15 mass% or more and 40 mass% or less, more preferably 17 mass% or more and 38 mass% or less, more preferably 20 mass% or more and 37 mass% or less, more preferably 23 mass% or more and 36 mass% or less, and more preferably 26 mass% or more and 35 mass% or less. In the above range, a high tensile elongation can be imparted to the thermoplastic resin composition and molded article obtained by the modification.

[0090] In this modifier, when the total of the two components, component (B) and component (C), is 100 mass%, the proportion of component (C) can be 1 mass% or more and 90 mass% or less. This proportion is preferably 3 mass% or more and 80 mass% or less, more preferably 5 mass% or more and 70 mass% or less, more preferably 6 mass% or more and 55 mass% or less, more preferably 7 mass% or more and 45 mass% or less, more preferably 8 mass% or more and 40 mass% or less, more preferably 9 mass% or more and 35 mass% or less, and more preferably 10 mass% or more and 30 mass% or less. In the above range, a high tensile elongation can be imparted to the thermoplastic resin composition and molded article obtained by modification.

[0091] In this modifier, when the total of the two components, component (C) and component (D), is 100 mass%, the proportion of component (D) can be 1 mass% or more and 99 mass% or less. This proportion is preferably 5 mass% or more and 80 mass% or less, more preferably 10 mass% or more and 60 mass% or less, more preferably 15 mass% or more and 55 mass% or less, more preferably 20 mass% or more and 50 mass% or less, more preferably 23 mass% or more and 45 mass% or less, and more preferably 25 mass% or more and 40 mass% or less. In the above range, a high tensile elongation can be imparted to the thermoplastic resin composition and molded article obtained by modification.

[0092] [6] Modification method The modification method of the present invention (hereinafter, also simply referred to as "this modification method") is a modification method for improving the tensile elongation of the resulting thermoplastic resin composition by adding a specific modifier to component (A). Specifically, it is a modification method capable of modifying component (A) so that the tensile elongation is 50% or more. The modifier used in this modification method contains components (B), (C), and (D). These four components (A) to (D) are the same as those in the composition of the present invention described above. The content ratio and amount of each component are the same as those in the composition of the present invention described above. Furthermore, this modifier can be obtained as the second composition in the method for producing the composition of the present invention described above or the method for producing the molded product of the present invention described above.

[0093] The present modification method can include the methods (1) the first method and (2) the second method, similarly to the above-mentioned method for producing the present molded body. That is, (1) The first method includes a third composition preparation step of melt-kneading a modifier and a component (A) to obtain a third composition; and a molding step of molding the third composition to obtain a molded article (modified molded article). (2) The second method includes a molding step of molding a melt-kneaded mixture of the modifier and component (A) to obtain a molded body (modified molded body).

[0094] The difference between the first method and the second method is whether or not a third composition is prepared when modifying. That is, in the first method, the third composition is formed and then molded. Therefore, the third composition, which is a melt-kneaded product of the modifier and the component (A), is solidified to obtain the third composition (for example, in a pellet shape) as a master batch suitable for molding. Then, this third composition is put into a molding machine and molded. On the other hand, the second method molds a molten mixture of the modifier and component (A) (a composition that is not solidified and is in a molten and kneaded state) as it is. That is, in the second method, the molten mixture of the modifier and component (A) can be molded directly without forming a master batch suitable for molding (for example, a solid modifier and a solid component (A) are dry-blended, and then the solid mixture is melt-kneaded and molded).

[0095] In general, by adopting the first method, uneven distribution of the modifier and component (A) in the obtained molded body can be prevented. In this respect, in the present modification method, the second method can be actively selected. That is, even if molding is performed by the second method, uneven distribution of the modifier and component (A) in the molded body can be sufficiently prevented. The reason why an excellent molded body can be obtained without preparing a molding master batch (third composition) in this way is considered to be because the total of the components (A) to (D) is 100 mass%, and the total of the components (A) and (B) is as high as 70 mass% or more. In other words, it is considered to be because the total of the components (C) and (D) is as low as less than 30 mass%. In this way, by utilizing the second method, it is possible to obtain a modified molded body having excellent tensile elongation while reducing the number of melt-kneading steps by one.

[0096] In these methods, the modifier is a composition obtained by melt-kneading a first composition obtained by melt-kneading component (C) and component (D) with component (B), as in the case of the method for producing the present composition. EXAMPLES

[0097] The present invention will now be described in detail with reference to examples. [1] Preparation of thermoplastic resin composition and preparation of test specimens (1) Preparation of Thermoplastic Resin Composition Pellets of a polyamide resin (component (C)) and pellets of a modified elastomer (component (D)) were dry-blended, and the resulting pellet mixture was then fed into a twin-screw melt-kneading extruder (manufactured by Coperion, screw diameter 50 mm, L / D=48) and melt-kneaded under conditions of a kneading temperature of 210°C, an extrusion speed of 150 kg / hour, and a screw rotation speed of 500 rpm. The mixture was then passed through a pelletizer to obtain pellets (first composition) consisting of a melt-kneaded mixture of components (C) and (D) (first composition preparation step). Furthermore, the obtained pellets (first composition) were dry-blended with pellets of the polyolefin resin (component (B)) described below, and then the obtained pellet mixture was fed into a twin-screw melt-kneading extruder (manufactured by Coperion, screw diameter 50 mm, L / D=48) and melt-kneaded under conditions of a kneading temperature of 210°C, an extrusion speed of 150 kg / hour, and a screw rotation speed of 500 rpm, and passed through a pelletizer to obtain pellets (pellet-shaped modifier, modifier pellets) consisting of a second composition (modifier) ​​(second composition preparation process).

[0098] (2) Molding of test specimens for evaluation (Experimental Example 1- 9 ) The pellets obtained in (1) above (pellet-shaped modifier, modifier pellets) and pellets of the following component (A) polyolefin resin were mixed together to produce the pellets shown in Experimental Examples 2 to 4 in Table 1 below. 8 After dry blending to obtain the compounding ratio, the obtained pellet mixture was put into an injection molding machine (Nissei Plastic Industrial Co., Ltd., 40 ton injection molding machine) and injection molded under the injection conditions of a set temperature of 210 ° C. and a mold temperature of 40 ° C., and the pellets were obtained as Experimental Examples 2 to 4. 8 Evaluation test pieces were obtained (molding process). Additionally, only pellets of the component (A) polyolefin resin were injection molded in the same manner to obtain evaluation test pieces for Experimental Example 1. Furthermore, pellets of the first composition and pellets of the component (B) polyolefin resin were dry-blended, and the resulting pellet mixture was then placed in an injection molding machine (Nissei Plastics Industrial Co., Ltd., 40-ton injection molding machine) and injection molded under injection conditions of a set temperature of 210°C and a mold temperature of 40°C. 9 Evaluation test pieces were obtained.

[0099] [Table 1]

[0100] (3) Details of components (A) to (D) Component (A) / Polyolefin resin: Propylene-ethylene block copolymer, copolymer, number average molecular weight less than 350,000, MFR 60g / 10min Component (B) / Polyolefin resin: Polypropylene resin, homopolymer, number average molecular weight 520,000, MFR 3g / 10min Component (C) / Polyamide resin: Nylon 6 resin (polyamide resin having only short chain structure), number average molecular weight 18,000 Component (D) / Modified elastomer: Maleic anhydride modified ethylene-butene copolymer (modified EBR), manufactured by Mitsui Chemicals, Inc., product name "Tafmer MH7020", MFR (230℃) = 1.5g / 10min

[0101] [2] Evaluation of test specimens (1) Measurement of tensile elongation Using the type A1 (dumbbell-shaped) test pieces specified in JIS K7139 obtained through the above [1], the tensile elongation and tensile strength were measured at a tensile speed of 50 mm / min in accordance with JIS K7161. The results are shown in Table 1. 7 (indicated as “>500” in Table 1) indicates that the tensile elongation exceeded 500%, which is the upper limit of measurement. Furthermore, the correlation between the total polyolefin content in the evaluation test pieces of each experimental example and the tensile elongation (-◯- in the graph) and the correlation between the total polyolefin content and tensile strength (-▲- in the graph) are shown in graphs in Figure 4.

[0102] (2) Charpy impact strength measurement Experimental example 1 obtained through [1] above 9 The test pieces were used to measure the Charpy impact strength in accordance with JIS K7111-1. The results are shown in Table 1. In the measurement of the Charpy impact strength, test pieces having a notch (Type A) were used, and impact measurements were performed at a temperature of 23°C by the edgewise test method. Furthermore, the correlation between the total content of polyolefins contained in the evaluation test pieces of each experimental example and the Charpy impact strength (-■- in the graph) is shown in a graph in FIG.

[0103] [3] Effects of the embodiment It can be seen from Table 1 and Figure 4 that the tensile elongation of the obtained molded article can be significantly improved by using a thermoplastic composition containing components (B) to (D) (second composition, i.e., modifier) ​​as a modifier for component (A). In other words, it can be seen that the thermoplastic composition containing components (A) to (D) (third composition) has significantly excellent tensile elongation. In particular, the tensile strength (-■- in the graph) does not change depending on the total polyolefin content. 9 The Charpy impact strength (-▲- in the graph) is almost constant at 0.5% by mass or more. On the other hand, the Charpy impact strength (-▲- in the graph) is significantly improved when the amount of the second composition exceeds 5% by mass, but the improvement is relatively gradual when the amount of the second composition exceeds 15% by mass. On the other hand, the tensile elongation (-◯- in the graph) is extremely significantly and dramatically increased when the amount of the second composition exceeds 0% by mass and reaches 50% by mass. A particularly significant improvement in the tensile elongation is observed when the amount of the second composition exceeds 10% by mass and reaches 40% by mass. Furthermore, when the amount of the second composition exceeds about 24% by mass, the thermoplastic composition containing the components (B) to (D) (the second composition, i.e., the modifier) ​​exhibits a high tensile elongation exceeding the 374% that the thermoplastic composition inherently has.

[0104] From various measurement results, it is considered that the morphology observed by the following test method exhibits the phase structure shown in FIG. 3 in any of Experimental Examples 2 to 7. Furthermore, it is considered that the continuous phase X is composed of component (A) (or the polypropylene component of component (A)) and component (B), the dispersed phase Y is composed of component (C) and a part of component (D), and the boundary layer Z is composed of the polyethylene component of component (A) and a part of component (D). Furthermore, it is considered that the dispersed phase Y is composed of the continuous phase Y in the dispersed phase. 1 and finely dispersed phase Y 2 and a continuous phase Y in the dispersed phase 1 is composed of the other parts of component (D), and the finely dispersed phase Y 2 is considered to be composed of component (C). The above test method is as follows. That is, the fracture surface of each test piece of Examples 2 to 7 is subjected to oxygen plasma etching treatment at 100 W for 1 minute, followed by osmium coating treatment, and observed with a field emission scanning electron microscope (manufactured by JEOL Ltd., model "JSM-7100F TTL LV") to obtain an image (FE-SEM image). In addition, the components constituting each phase are identified by performing energy dispersive X-ray analysis (EDS) during the above FE-SEM observation. The phase structure is identified from these results.

[0105] The above examples are merely illustrative and are not to be construed as limiting the present invention. Although the present invention has been described with reference to exemplary embodiments, it is understood that the words used in describing and illustrating the present invention are descriptive and exemplary, rather than limiting. As detailed herein, changes may be made within the scope of the appended claims without departing from the scope or spirit of the present invention in its form. Although the present invention has been described herein with reference to specific structures, materials and examples, it is not intended that the present invention be limited to the disclosures set forth herein, but rather that the present invention extends to all functionally equivalent structures, methods and uses within the scope of the appended claims. [Explanation of symbols]

[0106] X: continuous phase; Y; dispersed phase, Y 1 ; Continuous phase within dispersed phase, Y 2 ;Finely dispersed phase (dispersed phase within a dispersed phase), Z; boundary phase.

Claims

1. A method for using a modifier that improves the tensile elongation of a molded body to 400% or more, comprising: A step of dry blending pellets of a first polyolefin resin (A) having a number average molecular weight of less than 350,000 with pellets of a modifier to obtain a pellet mixture; and A step of molding the pellet mixture to obtain the molded body, The modifier comprises a second polyolefin resin (B) having a number average molecular weight of 350,000 or more; a polyamide resin (C) having a structure in which the number of linear carbon atoms in a hydrocarbon group sandwiched between adjacent amide bonds in the main chain is 5 or less; and a modified elastomer (D) having a reactive group with respect to the polyamide resin (C), which is an acid-modified product of an α-olefin copolymer containing a structural unit derived from an α-olefin having 3 to 8 carbon atoms, The components (A) and (B) are components that do not have a reactive group with respect to the component (C), In the step of obtaining the pellet mixture, when the total of the components (A), (B), (C) and (D) is taken as 100% by mass, the component (A) is 35 to 70% by mass, the component (B) is 20 to 45% by mass, the component (C) is 5 to 12% by mass, the component (D) is 10 to 25% by mass, the total of the components (A) and (B) is 70% by mass or more and 90% by mass or less, and when the total of the components (A) and (B) is taken as 100% by mass, the component (A) is 50% by mass or more and 87% by mass or less. The method for using a modifier, characterized in that the pellet mixture is obtained so that the component (A) is 35 to 70% by mass, the component (B) is 20 to 45% by mass, the component (C) is 5 to 12% by mass, the component (D) is 10 to 25% by mass, and the total of the components (A) and (B) is 70% by mass or more and 90% by mass or less.

2. 2. The method for using the modifier according to claim 1, wherein the modifier contains 50% by mass or more of the component (D) when the total of the component (C) and the component (D) is 100% by mass.

3. 3. The method for using the modifier according to claim 1 or 2, wherein the modifier contains 45% by mass or more and 65% by mass or less of the component (B), the component (C) and the component (D) when the total of the component (B), the component (C) and the component (D) is taken as 100% by mass.

4. A method for improving the tensile elongation of a molded body to 400% or more, comprising the steps of: A step of dry blending pellets of a first polyolefin resin (A) having a number average molecular weight of less than 350,000 with pellets of a modifier to obtain a pellet mixture; and A step of molding the pellet mixture to obtain the molded body, The modifier comprises a second polyolefin resin (B) having a number average molecular weight of 350,000 or more; a polyamide resin (C) having a structure in which the number of linear carbon atoms in a hydrocarbon group sandwiched between adjacent amide bonds in the main chain is 5 or less; and a modified elastomer (D) having a reactive group with respect to the polyamide resin (C), which is an acid-modified product of an α-olefin copolymer containing a structural unit derived from an α-olefin having 3 to 8 carbon atoms, The components (A) and (B) are components that do not have a reactive group with respect to the component (C), In the step of obtaining the pellet mixture, when the total of the components (A), (B), (C) and (D) is taken as 100% by mass, the component (A) is 35 to 70% by mass, the component (B) is 20 to 45% by mass, the component (C) is 5 to 12% by mass, the component (D) is 10 to 25% by mass, the total of the components (A) and (B) is 70% by mass or more and 90% by mass or less, and when the total of the components (A) and (B) is taken as 100% by mass, the component (A) is 50% by mass or more and 87% by mass or less. The pellet mixture is obtained in such a manner that the pellet mixture is obtained in such a manner that the total of the components (A) and (B) is 100% by mass.

5. The method for modifying a surface of a material according to claim 4, wherein the modifying agent contains 50% by mass or more of the component (D) when the total of the component (C) and the component (D) is taken as 100% by mass.

6. The modifying method according to claim 4 or 5, wherein the modifying agent contains 45 mass% or more and 65 mass% or less of the component (B) when the total of the component (B), the component (C) and the component (D) is 100 mass%.

7. The method for modifying a surface of a material according to any one of claims 4 to 6, wherein the modifier is added in an amount of more than 20 mass% and less than 75 mass%, assuming that the total amount of the component (A) and the modifier is 100 mass%.

Citation Information

Patent Citations

  • Thermoplastic resin fiber and method for manufacturing the same, and fabric

    JP2018123457A

  • Modifier and method for using the same, method for producing modifier, and carrier for additive

    JP2018154843A

  • Injection molded body of polypropylene resin composition

    WO2017111100A1

  • Thermoplastic resin composition, method for producing same, and molded body

    WO2018021569A1

  • Modifier and use method thereof, modifier production method and carrier for additive

    WO2018139378A1