Polycarbonate polyol

By controlling dioxane generation and optimizing the polycondensation process, the method produces high-quality polycarbonate polyol with improved flexibility and solvent resistance, addressing the limitations of conventional methods and enhancing polyurethane properties.

JP7582429B2Active Publication Date: 2024-11-13MITSUBISHI CHEM CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023195763
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-08-10
Filing Date
2023-11-17
Publication Date
2024-11-13
Estimated Expiration
2038-08-07

AI Technical Summary

Technical Problem

Conventional methods for producing polycarbonate polyol result in the generation of dioxane as a byproduct, which affects productivity, quality, and safety, and the resulting polyurethane products exhibit poor flexibility, mechanical strength, and solvent resistance.

Method used

A method for producing polycarbonate polyol by polycondensing a polyhydric alcohol containing diethylene glycol and a carbonate compound, where the amount of dioxane generation is controlled to be below 1.0% by weight, using diethylene glycol as a raw material, and incorporating a specific catalyst and reaction conditions to enhance flexibility and solvent resistance.

Benefits of technology

The method produces high-quality polycarbonate polyol with improved flexibility, mechanical strength, and solvent resistance, enabling the production of polyurethane with enhanced properties and reduced dioxane volatilization risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582429000001
    Figure 0007582429000001
  • Figure 0007582429000002
    Figure 0007582429000002
  • Figure 0007582429000003
    Figure 0007582429000003
Patent Text Reader

Abstract

To produce high-quality polycarbonate diol with high productivity, which makes it possible to produce polyurethane having excellent flexibility, mechanical strength, solvent resistance and the like, using diethylene glycol as the raw material, by preventing the occurrence of dioxane, when producing polycarbonate diol by the polycondensation of a polyhydric alcohol containing diethylene glycol and a carbonate compound.SOLUTION: A polyhydric alcohol containing diol (A) and a carbonate compound are subjected to polycondensation, to produce polycarbonate diol with a hydroxyl value of 20-450 mgKOH / g. The diol (A) contains oxyalkylene glycol (A1) represented by formula (1) of 60 wt.% or more, and the oxyalkylene glycol (A1) contains diethylene glycol. The amount of dioxane generated in the polycondensation step is controlled to be 1.0 wt.% or less relative to the amount of addition of diethylene glycol.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for industrially advantageously producing a high-quality polycarbonate polyol by polycondensation of a polyhydric alcohol containing an oxyalkylene glycol and a carbonate compound, in which dioxane generation is suppressed and oxyalkylene glycol is used as a raw material to produce a polyurethane excellent in flexibility, mechanical strength, solvent resistance, etc. The present invention also relates to a high-quality polycarbonate polyol produced by suppressing dioxane generation in this way, and a method for producing a polyurethane using this polycarbonate polyol. [Background technology]

[0002] It has been known that a polycarbonate diol-containing composition is produced by polymerizing a dihydroxy compound and a carbonate compound by transesterification. Industrially produced polycarbonate diol-containing compositions include those using dihydroxy compounds such as 1,6-hexanediol as the raw dihydroxy compound, and these polycarbonate diol-containing compositions are generally used as raw materials for polyurethanes and polyurethane acrylates.

[0003] Among polycarbonate diols, the one that is currently widely available on the market is that synthesized from 1,6-hexanediol, but because this polycarbonate diol has high crystallinity, when it is made into polyurethane, the soft segments tend to aggregate, and there are problems with poor flexibility, elongation, bending, or elastic recovery, especially at low temperatures, limiting its applications. Furthermore, it has been pointed out that artificial leather made from the resulting polyurethane has a hard texture and is inferior in "hand" to natural leather.

[0004] In order to solve these problems, polycarbonate diols that are made from oxyalkylene glycol and have excellent flexibility and solvent resistance have been proposed, and patent documents 1 and 2 describe polycarbonate diols that use diethylene glycol. Patent document 3 describes polycarbonate diols that are copolymerized with 1,6-hexanediol and triethylene glycol.

[0005] However, when a dihydroxy compound containing diethylene glycol is used as a raw material and a polycarbonate diol-containing composition is polymerized by transesterification, dioxane is by-produced by dehydration cyclization of diethylene glycol and decarboxylation cyclization of the terminal units of the obtained polycarbonate diol. The greater the amount of dioxane by-produced, the worse the productivity of the polycarbonate diol-containing composition becomes. In addition, the by-produced dioxane causes coloration of the polycarbonate diol product, and the polycarbonate diol obtained in a reaction system with a large amount of dioxane by-produced has a problem of poor reactivity as a raw material for polyurethane.

[0006] In addition, dioxane is designated as a specified chemical substance under the Industrial Safety and Health Act, and restrictions are imposed on its emission into the atmosphere. However, in industrial production of polycarbonate diol, which is reacted under high vacuum conditions, it is difficult to capture dioxane, which has a low boiling point, due to equipment limitations, and the by-product of dioxane has been a problem in improving the productivity of polycarbonate diol derived from oxyalkylene glycol.

[0007] Furthermore, when dioxane remains in the raw material polycarbonate diol-containing composition during the production of polyurethane or polyurethane acrylate, the polyurethane solution used in paint or the like also contains dioxane, which causes a problem of adverse effects on the environment or health due to the volatilization of dioxane.

[0008] In order to avoid the problem of the by-production of dioxane, methods for reducing the amount of dioxane produced as a by-product when a polymer is produced using a dihydroxy compound capable of producing dioxane as a raw material have been studied.

[0009] For example, Patent Document 4 describes a method for reducing the amount of dioxane generated by adjusting monomer charging conditions and reaction temperature in a method for producing polyester polyol using diethylene glycol as a raw material. However, Patent Document 4 relates to the production of polyester polyol, and does not describe an example of application to polycarbonate polyol, which requires a higher reaction temperature, high vacuum conditions, and a long reaction time to remove carbonate ends derived from the raw material, which are terminal structures that tend to remain, and for which it is difficult to simultaneously suppress the amount of dioxane generated and obtain a high-quality product. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] Patent No. 5448627 [Patent Document 2] Patent No. 5111159 [Patent Document 3] Patent No. 3684567 [Patent Document 4] Special Publication No. 2012-529542 Summary of the Invention [Problem to be solved by the invention]

[0011] The present invention has been made in view of the above-mentioned conventional circumstances, and aims to provide a method for highly productively producing a high-quality polycarbonate polyol that can produce polyurethane excellent in flexibility, mechanical strength, solvent resistance, etc. by suppressing the generation of dioxane and using diethylene glycol as a raw material when producing a polycarbonate polyol by polycondensation of a polyhydric alcohol containing diethylene glycol and a carbonate compound. Another aim of the present invention is to provide a high-quality polycarbonate polyol produced by suppressing the generation of dioxane in this way, and a method for producing polyurethane using this polycarbonate polyol. [Means for solving the problem]

[0012] As a result of extensive investigations aimed at solving the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by controlling the amount of dioxane generated relative to the amount of diethylene glycol added in a polycondensation step in which diethylene glycol is used as a raw material polyhydric alcohol to a predetermined value or less. That is, the gist of the present invention is as follows.

[0013] [1] A method for producing a polycarbonate polyol, comprising a step of polycondensing a polyhydric alcohol and a carbonate compound, the method being characterized in that the hydroxyl value of the polycarbonate polyol is 20 mgKOH / g or more and 450 mgKOH / g or less, the polyhydric alcohol comprises a diol (A), the diol (A) comprises an oxyalkylene glycol (A1) represented by the following formula (1), the content of the oxyalkylene glycol (A1) in the diol (A) is 60% by weight or more, the oxyalkylene glycol (A1) comprises diethylene glycol, the terminals derived from the carbonate compound contained in the polycarbonate polyol are 1.0 mol % or less of all terminals, and the amount of dioxane generated in the polycondensation step is controlled to 1.0 wt % or less relative to the amount of diethylene glycol added.

[0014] [ka]

[0015] In formula (1), m represents an integer of 2 to 4, and R A represents a carbon chain having 2 to 5 carbon atoms which may contain a branch. A may be the same or different.)

[0016] [2] The method for producing a polycarbonate polyol according to [1], wherein the carbonate compound is a diaryl carbonate.

[0017] [3] The method for producing a polycarbonate polyol according to [1] or [2], wherein a salt of a metal of Group 2 of the long form periodic table is used as a catalyst in the polycondensation step.

[0018] [4] The method for producing a polycarbonate polyol according to any one of [1] to [3], wherein the reaction temperature in the polycondensation step is 150° C. or higher and 180° C. or lower.

[0019] [5] The method for producing a polycarbonate polyol according to any one of [1] to [4], further comprising a step of removing unreacted monomer of the polyhydric alcohol after the polycondensation step, and adding a phosphoric acid-based deactivator before the step of removing the unreacted monomer.

[0020] [6] The method for producing a polycarbonate polyol according to any one of [1] to [5], wherein the polyhydric alcohol further contains a trihydric to hexahydric branched alcohol (B) having 3 to 12 carbon atoms, and the structural units derived from the branched alcohol (B) in the polycarbonate polyol are 0.005 mol % or more and 5.0 mol % or less based on the total structural units derived from the polyhydric alcohol in the polycarbonate polyol.

[0021] [7] The method for producing a polycarbonate polyol according to any one of [1] to [6], wherein the polycarbonate polyol has a Hazen color number value (APHA value: in accordance with JIS K0071-1 (1998)) of 50 or less.

[0022] [8] A method for producing polyurethane, using a polycarbonate polyol produced by the method for producing a polycarbonate polyol according to any one of [1] to [7].

[0023] [9] A polycarbonate polyol which is a polycondensation reaction product of a polyhydric alcohol and a carbonate compound, the polycarbonate polyol having a hydroxyl value of 20 mgKOH / g or more and 450 mgKOH / g or less, terminals derived from the carbonate compound account for 1.0 mol% or less of all terminals, and a Hazen color number value (APHA value: based on JIS K0071-1 (1998)) of 50 or less, the polyhydric alcohol comprising a diol (A) and a trihydric to hexahydric branched alcohol (B) having 3 to 12 carbon atoms, the diol (A) comprising an oxyalkylene glycol (A1) represented by the following formula (1), the content of the oxyalkylene glycol (A1) in the diol (A) being 60% by weight or more, and the oxyalkylene glycol (A1) comprising diethylene glycol.

[0024] [ka]

[0025] In formula (1), m represents an integer of 2 to 4, and R A represents a carbon chain having 2 to 5 carbon atoms which may contain a branch. A may be the same or different.)

[0026]

[10] The polycarbonate polyol according to [9], wherein the structural units derived from the branched alcohol (B) in the polycarbonate polyol are 0.005 mol % or more and 5.0 mol % or less based on the total structural units derived from the polyhydric alcohol in the polycarbonate polyol. Effect of the Invention

[0027] According to the present invention, a high-quality polycarbonate polyol can be produced with good productivity using a xalkylene glycol containing diethylene glycol as a raw material. By polymerizing the polycarbonate polyol produced by the present invention with an isocyanate or the like, a polyurethane having high flexibility, mechanical strength, and excellent solvent resistance can be provided. In addition, the problem of dioxane volatilization during use of the polyurethane can be prevented.

[0028] Polyurethanes produced using the polycarbonate polyols of the present invention have the features of good reactivity during urethane polymerization and an excellent balance of flexibility, mechanical strength, and solvent resistance, and are suitable for applications such as elastic fibers, synthetic or artificial leather, paints, and high-performance elastomers, and are extremely useful industrially. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] The present invention will be described in detail below, but the present invention is not limited to the following description, and can be modified in any manner without departing from the gist of the present invention. In this specification, when a numerical value or physical property value is enclosed before and after "~", the values ​​before and after are included. In this specification, "% by weight" and "% by weight", "ppm by mass" and "ppm by weight", and "parts by mass" and "parts by weight" are synonymous. When simply written as "ppm", it means "ppm by weight".

[0030] [1. Polycarbonate polyol and its manufacturing method] The method for producing a polycarbonate polyol of the present invention is a method for producing a polycarbonate polyol including a step of polycondensing a polyhydric alcohol and a carbonate compound, characterized in that the hydroxyl value of the polycarbonate polyol is 20 mgKOH / g or more and 450 mgKOH / g or less, the polyhydric alcohol contains a diol (A), the diol (A) contains an oxyalkylene glycol (A1) represented by the following formula (1), the content of the oxyalkylene glycol (A1) in the diol (A) is 60% by weight or more, the oxyalkylene glycol (A1) contains diethylene glycol, the terminals derived from the carbonate compound contained in the polycarbonate polyol are 1.0 mol % or less of all terminals, and the amount of dioxane generated in the polycondensation step is controlled to 1.0 wt % or less relative to the amount of diethylene glycol added.

[0031] [ka]

[0032] In formula (1), m represents an integer of 2 to 4, and R A represents a carbon chain having 2 to 5 carbon atoms which may contain a branch. A may be the same or different.)

[0033] Hereinafter, the amount of dioxane generated relative to the amount of oxyalkylene glycol (A1) added in the polycondensation step according to the present invention will be simply referred to as the "amount of dioxane generated."

[0034] The polycarbonate polyol of the present invention is a polycarbonate polyol which is a polycondensation reaction product of a polyhydric alcohol and a carbonate compound, characterized in that the polycarbonate polyol has a hydroxyl value of 20 mgKOH / g or more and 450 mgKOH / g or less, the terminals derived from the carbonate compound account for 1.0 mol% or less of all terminals, and the Hazen color number value (APHA value: based on JIS K0071-1 (1998)) is 50 or less, the polyhydric alcohol contains a diol (A) and a trihydric to hexahydric branched alcohol (B) having 3 to 12 carbon atoms, the diol (A) contains an oxyalkylene glycol (A1) represented by the following formula (1), the content of the oxyalkylene glycol (A1) in the diol (A) is 60% by weight or more, and the oxyalkylene glycol (A1) contains diethylene glycol.

[0035] Hereinafter, the terminals derived from the carbonate compound according to the present invention will be referred to as "carbonate terminals", and the proportion of carbonate terminals among all terminals in the polycarbonate polyol will be simply referred to as the "carbonate terminal amount".

[0036] According to the method for producing a polycarbonate polyol of the present invention, the polycarbonate polyol of the present invention can be produced. The method for producing the polycarbonate polyol of the present invention is not particularly limited, but the polycarbonate polyol is preferably produced by the method for producing a polycarbonate polyol of the present invention. Hereinafter, the polycarbonate polyol produced by the polycarbonate polyol production method of the present invention will also be referred to as the "polycarbonate polyol of the present invention."

[0037] <1-1. Characteristics of dioxane generation amount, carbonate end amount, and APHA value> One of the features of the method for producing a polycarbonate polyol of the present invention is that the amount of dioxane generated in the polycondensation step of a polyhydric alcohol and a carbonate compound is controlled to 1.0% by weight or less based on the amount of diethylene glycol charged in the production of the polycarbonate polyol.

[0038] If the amount of dioxane generated in the polycondensation step is more than the upper limit, it is not preferable because it causes problems such as a decrease in productivity due to the by-production of dioxane, a decrease in the physical properties and coloring of the obtained polycarbonate polyol, a decrease in reactivity when producing polyurethane using this polycarbonate polyol, and a decrease in the quality of the produced polyurethane.The smaller the amount of dioxane generated, the more preferable it is in terms of the productivity of polycarbonate polyol and the quality of polycarbonate polyol and polyurethane, and it is controlled to be 1.0% by weight or less, preferably 0.7% by weight or less, more preferably 0.5% by weight or less, even more preferably 0.3% by weight or less, and particularly preferably 0.1% by weight or less. The amount of dioxane generated can be analyzed by the method described in the Examples section below, and "0.1% by weight or less" here corresponds to the detection limit of dioxane in the analysis of a polycarbonate polyol product.

[0039] The polycarbonate polyol of the present invention is also characterized in that the amount of carbonate terminals is 1.0 mol % or less and the APHA value is 50 or less.

[0040] If the amount of carbonate terminals exceeds the upper limit, the reactivity of the polyurethane produced using this polycarbonate polyol is poor, and it becomes difficult to produce a polyurethane with a high molecular weight and excellent mechanical strength, chemical resistance, etc. In addition, a high APHA value of the polycarbonate polyol means that the polycarbonate polyol is colored, which is undesirable in terms of the quality of the polycarbonate polyol itself. In addition, the polyurethane produced using this polycarbonate polyol is also undesirable because it is colored.

[0041] Therefore, the carbonate terminal amount of the polycarbonate polyol of the present invention is preferably as small as possible, and is 1.0 mol % or less, preferably 0.5 mol % or less, and more preferably 0.1 mol % or less. The amount of carbonate terminals can be analyzed by the method described in the Examples section below, and here, "0.1 mol% or less" corresponds to the detection limit of the amount of carbonate terminals in the analysis of a polycarbonate polyol product.

[0042] The APHA value of the polycarbonate polyol is also preferably low, and the APHA value of the polycarbonate polyol of the present invention is preferably 50 or less, more preferably 30 or less, and even more preferably 20 or less. If the APHA value exceeds 50, the color tone of the polyurethane obtained from the polycarbonate diol-containing composition as a raw material deteriorates, lowering the commercial value and deteriorating the thermal stability. In particular, a polycarbonate diol-containing composition made from an aliphatic dihydroxy compound having an alcoholic hydroxyl group as a raw material shows various excellent performances such as flexibility, water resistance, and light resistance when processed into polyurethane, but tends to be more significantly colored by heat history or catalyst than when an aromatic dihydroxy compound is used as a raw material, and it is not easy to make the APHA value 50 or less. The APHA value of the polycarbonate polyol is measured by the method described in the Examples section below.

[0043] <1-2. Means for achieving the amount of dioxane generated, amount of carbonate terminals, and APHA value> There are no particular limitations on the means for achieving a dioxane generation amount of 1.0% by weight or less in the polycondensation step, and examples thereof include the following methods (1) to (5). Some of the following means for achieving the goal (1) to (5) may be adopted in combination, and from the viewpoint of the certainty of achievement, it is preferable to adopt a combination of multiple means for achieving the goal (1) to (5) below, and it is particularly preferable to adopt all of them. In addition, by controlling the amount of dioxane generated to 1.0 weight % or less by adopting the following means (1) to (5), it is also possible to produce a polycarbonate polyol having a carbonate terminal amount of 1.0 mol % or less and an APHA value of 50 or less.

[0044] (1) Diaryl carbonate, particularly preferably diphenyl carbonate, is used as the carbonate compound raw material. When a carbonate compound other than diaryl carbonate such as diphenyl carbonate is used, the unreacted diethylene glycol is heated for a long time due to its low reactivity with polyhydric alcohol, and the amount of dioxane generated tends to increase. In other words, by using a highly reactive diaryl carbonate such as diphenyl carbonate as the carbonate compound raw material, the amount of dioxane generated can be reduced. In addition, the high reactivity allows the catalyst concentration shown in (2) below to be reduced, and the amount of dioxane generated can be reduced in the same manner.

[0045] (2) In the polycondensation step, a metal salt of Group 2 of the long periodic table (in the present invention, simply referred to as the "periodic table") is used as a catalyst. When a catalyst other than a metal salt of Group 2 of the periodic table is used as a catalyst, the amount of dioxane generated tends to increase. For example, the reason for this is that metal salts of Group 1 of the periodic table are too basic, and metal salts of Groups 3 and 4 are too acidic, accelerating the dioxane-generating side reaction. In contrast, when a metal salt of Group 2 of the periodic table is used, it is possible to accelerate only the desired esterification reaction as a moderately basic catalyst, thereby reducing the amount of dioxane generated. When a metal salt of Group 2 of the periodic table is used, its concentration in terms of metal in the polycondensation reaction solution is preferably 50 ppm or less, more preferably 30 ppm or less, even more preferably 20 ppm or less, particularly preferably 15 ppm or less, and the lower limit is preferably 1 ppm or more in order to more reliably reduce the amount of dioxane generated. If the concentration of the metal salt of Group 2 of the periodic table is higher than the upper limit or lower than the lower limit, the amount of dioxane generated tends to increase.

[0046] Furthermore, the metal salt of Group 2 of the periodic table usually does not volatilize and remains in the polycarbonate diol, but if an excessive amount of catalyst remains, it becomes difficult to control the polyurethane reaction during the polyurethane reaction, and the polyurethane reaction may be accelerated more than expected, an abnormal reaction may occur, or the color tone may deteriorate, so the remaining amount must be 50 ppm or less, preferably 30 ppm or less, more preferably 20 ppm or less, and particularly preferably 15 ppm or less, in terms of the weight ratio of the metal to the polycarbonate diol. On the other hand, if the amount of catalyst is small, it may cause the above-mentioned problems, so the amount of the metal to the polycarbonate diol is preferably 1 ppm or more.

[0047] (3) The reaction temperature in the polycondensation step is set to 150°C or higher and 180°C or lower. If the reaction temperature is lower than 150°C, the polycondensation reaction does not proceed smoothly, making it impossible to produce a polycarbonate polyol with sufficient molecular weight, or increasing the amount of residual carbonate terminals, while if the reaction temperature exceeds 180°C, the amount of dioxane generated increases due to the decomposition of diethylene glycol, and coloring tends to occur. It is particularly preferable that the reaction temperature is set to 160°C or higher and 170°C or lower.

[0048] (4) The reaction time in the polycondensation step is 3 hours or more and 20 hours or less. If the reaction time is less than 3 hours, the polycondensation reaction does not proceed sufficiently, and a polycarbonate polyol with a sufficient molecular weight cannot be produced, or the amount of residual carbonate terminals increases, while if the reaction time exceeds 20 hours, the amount of dioxane generated increases and coloring tends to occur due to decomposition of diethylene glycol and decarboxylation cyclization of the terminal units of the polycarbonate diol. It is particularly preferable that the reaction time is 5 hours or more and 10 hours or less.

[0049] (5) Adjust the degree of pressure reduction. The reaction can be carried out at normal pressure, but the transesterification reaction is an equilibrium reaction, and the reaction can be biased toward the product system by distilling off the light-boiling components produced. Therefore, it is usually preferable to gradually reduce the pressure during the reaction and distill off the light-boiling components produced while carrying out the reaction. In particular, it is preferable to carry out the reaction at a high degree of reduced pressure at the end of the reaction, since by-produced monoalcohol, phenol, and other low boiling components can be distilled off. That is, the minimum pressure is preferably less than 1.5 kPa, particularly preferably 1.0 kPa or less, and particularly preferably 0.8 to 0.1 kPa. If this pressure exceeds the upper limit, the reactivity decreases, the reaction time becomes longer, the amount of dioxane generated increases, and the APHA of the obtained polycarbonate diol may increase. However, if this pressure is too low, the distillation rate of the by-produced phenol is high, so that the polymerization rate increases, and molecular weight control may become difficult.

[0050] <1-3. Structural characteristics derived from raw polyhydric alcohol> <1-3-1. Oxyalkylene glycol (A1) and its content> The polycarbonate polyol of the present invention contains 60% by weight or more of oxyalkylene glycol (A1) represented by the following formula (1) in the raw material diol (A), and contains diethylene glycol as an essential component in the oxyalkylene glycol (A1), and by containing the oxyalkylene glycol (A1) in such a ratio, the polycarbonate polyol has excellent flexibility and solvent resistance (hereinafter, referred to as solvent resistance including chemical resistance). From the viewpoint of flexibility and solvent resistance, the content ratio of oxyalkylene glycol (A1) in the diol (A) is preferably 70% by weight or more, particularly preferably 80% by weight or more, and particularly preferably 90% by weight or more.

[0051] [ka]

[0052] In formula (1), m represents an integer of 2 to 4, and R A represents a carbon chain having 2 to 5 carbon atoms which may contain a branch. A may be the same or different.)

[0053] The polycarbonate polyol of the present invention obtained by using the oxyalkylene glycol (A1) in such a ratio has a ratio of structural units derived from the oxyalkylene glycol (A1) to the total structural units derived from the diol (A) of usually 60% by weight or more, preferably 70% by weight or more, more preferably 80% by weight or more, and particularly preferably 90% by weight or more.

[0054] The oxyalkylene glycol (A1) is not particularly limited as long as it contains diethylene glycol and is represented by the above formula (1). From the viewpoints of flexibility and solvent resistance, however, A The number of carbon atoms in R is preferably 2 or 3, and more preferably 2. A Specific examples of the carbon chain having 2 to 5 carbon atoms which may include a branch include linear or branched alkylene groups having 2 to 5 carbon atoms.

[0055] As the oxyalkylene glycol (A1) other than diethylene glycol, specifically, triethylene glycol, tetraethylene glycol, and dipropylene glycol are preferred. These oxyalkylene glycols (A1) may be used alone or in combination of two or more.

[0056] As the oxyalkylene glycol (A1), it is particularly preferred to use diethylene glycol, or diethylene glycol and triethylene glycol, and the total content of diethylene glycol and triethylene glycol in the raw material diol (A) is preferably 60% by weight or more, preferably 70% by weight or more, particularly 80% by weight or more, and particularly 90% by weight or more, from the viewpoint of flexibility and chemical resistance. The upper limit of this content is usually preferably 99.5% by weight or less, more preferably 99% by weight or less, and even more preferably 98% by weight or less. The oxyalkylene glycol (A1) used in the present invention contains diethylene glycol, and from the viewpoints of flexibility and chemical resistance, it is preferable that the content of diethylene glycol in the raw material diol (A) is 50% by weight or more, preferably 60% by weight or more, and particularly preferably 70% by weight or more.

[0057] In particular, the combined use of diethylene glycol and triethylene glycol as the oxyalkylene glycol (A1) is a preferred embodiment of the present invention, since it disrupts the regularity of the structural units in the polycarbonate polyol chain, thereby preventing aggregation due to hydrogen bonds and increasing flexibility. In this case, the weight ratio of diethylene glycol to triethylene glycol is preferably diethylene glycol:triethylene glycol=10:90 to 90:10, particularly preferably 20:80 to 80:20, more preferably 30:70 to 70:30, and particularly preferably 40:60 to 60:40.

[0058] In addition, when the raw material diol (A) of the polycarbonate polyol of the present invention contains a diol other than the oxyalkylene glycol (A1) represented by the above formula (A1), examples of the other diol include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-hexanediol, 1,20-hexanediol, 1,21-hexanediol, 1,22-hexanediol, 1,23-hexanediol, 1,24-hexanediol, 1,25-hexanediol, 1,26-hexanediol, 1,27-hexanediol, 1,28-hexanediol, 1,30-hexanediol, 1,31-hexanediol, 1,32-hexanediol, 1,33-hexanediol, 1,34-hexanediol, 1,35-hexanediol, 1,36-hexanediol, 1,37-hexanediol, 1,38-hexanediol, 1,40-hexanediol, 1,41-hexanediol, 1,42-hexanediol, 1,43-hexanediol, 1,44-hexanediol, 1,45-hexanediol, 1,46-hexanediol, 1,47-hexanediol, 1,48-hexanediol, 1,50-hexanediol, 1,51-hexanediol, 1,52-hexanediol, 1,53-hexanediol, 1,54-hexanediol, 1,55-hexanediol, 1,60-hexanediol, 1,70-hexanediol, 1,71-hexanediol, Linear diols having 2 to 20 carbon atoms, such as decanediol and 1,12-dodecanediol, 2-methyl-1,3-propanediol, 2-ethyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 2-ethyl-2-butyl-1,3-propanediol, 2,2-diethyl-1,3-propanediol, 3-methyl-1,5-pentanediol, 3,3-dimethyl-1,5-pentanediol, 2,2,4,4-tetramethyl-1,5 -C4-20 branched diols such as pentanediol and 2-ethyl-1,6-hexanediol; and C6-20 cyclic diols such as 1,3-cyclohexanediol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, 4,4-dicyclohexyldimethylmethanediol, 2,2'-bis(4-hydroxycyclohexyl)propane, 4,4'-isopropylidenedicyclohexanol, and norbornane-2,3-dimethanol. Other examples include cyclic diols having a heteroatom in the ring, such as isosorbide, 3,4-dihydroxytetrahydrofuran, 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane (CAS number: 1455-42-1), and 2-(5-ethyl-5-hydroxymethyl-1,3-dioxan-2-yl)-2-methylpropan-1-ol (CAS number: 59802-10-7).

[0059] These other diols may be used alone or in combination of two or more kinds. As described above, in order to obtain the effect of improving flexibility and solvent resistance by using the oxyalkylene glycol (A1), the content of the oxyalkylene glycol (A1) in the diol (A) is 40% by weight or less, preferably 30% by weight or less, more preferably 20% by weight or less, and particularly preferably 10% by weight or less.

[0060] <1-3-2. Branched alcohol (B) and its content> The polycarbonate polyol of the present invention may use a branched alcohol (B) as a raw material polyhydric alcohol together with a diol (A) containing an oxyalkylene glycol (A1) in the above ratio. In this case, the structural unit derived from the branched alcohol (B) in the polycarbonate polyol is 0.005 mol% or more and 5.0 mol% or less based on the total structural units derived from the polyhydric alcohol in the polycarbonate polyol, so that the crosslinked structure introduced by the branched alcohol (B) can provide excellent mechanical strength without impairing the flexibility and solvent resistance due to the oxyalkylene glycol (A1), which is preferable.

[0061] From the viewpoint of achieving both flexibility, solvent resistance, and mechanical strength, the proportion of structural units derived from the branched alcohol (B) in the structural units derived from the polyhydric alcohol in the polycarbonate polyol of the present invention is preferably 0.005 to 5.0 mol%, more preferably 0.05 to 3.0 mol%, and even more preferably 0.5 to 2.0 mol%.

[0062] In order to set the structural units derived from the branched alcohol (B) in the structural units derived from the polyhydric alcohol in the polycarbonate polyol to fall within the above range, the molar content of the branched alcohol (B) in the polyhydric alcohol used as a raw material for the polycarbonate polyol may be set to fall within the above range. That is, in general, the ratio of each polyhydric alcohol in the raw material polyhydric alcohol is approximately equal to the ratio of structural units derived from each polyhydric alcohol to the total structural units derived from polyhydric alcohol in the resulting polycarbonate polyol.

[0063] Examples of the trivalent to hexavalent branched alcohol (B) having 3 to 12 carbon atoms contained in the raw material polyhydric alcohol of the polycarbonate polyol of the present invention include glycerol, trimethylolmethane, trimethylolethane, trimethylolpropane, trimethylolbutane, 1,2,4-butanetriol, 1,2,3-hexanetriol, 1,2,4-hexanetriol, tris(hydroxymethyl)amine, tris(hydroxyethyl)amine, tris(hydroxypropyl)amine, pentaerythritol, diglycerol, triglycerol, polyglycerol, bis(trimethylolpropane), tris(hydroxymethyl)isocyanurate, tris(hydroxyethyl)isocyanurate, sugars such as glucose, and sugar derivatives such as sorbitol. The polycarbonate polyol of the present invention may contain only one type of structural unit derived from these branched alcohols (B), or may contain two or more types. That is, the branched alcohol (B) used as the raw material polyhydric alcohol for the polycarbonate polyol of the present invention may be one type or two or more types.

[0064] Among these, from the viewpoint of the efficiency of introducing a crosslinked structure, a branched alcohol containing at least a part, preferably all, of the hydroxyl group as a methylol group is preferred, and the number of carbon atoms is preferably smaller. That is, the methylol group has a structure having a hydroxyl group via a methylene group, and therefore has high reactivity. In addition, when the same number of moles of branched alcohol are added, the number of carbon atoms is smaller, and the crosslink density can be increased. However, if the number of carbon atoms of the branched alcohol (B) is too small, the reactivity of each hydroxyl group is deteriorated due to steric hindrance, and crosslinking is difficult to proceed. In addition, the crosslinking points may be too dense, which may promote gelation. Therefore, as the branched alcohol (B), a branched alcohol having a trivalent to hexavalent methylol group with a carbon number of 3 to 12 is preferred, and a carbon number of 4 to 10 is even more preferred. Specifically, trihydric alcohols such as glycerol, trimethylolpropane, trimethylolethane, and trimethylolmethane, tetrahydric alcohols such as pentaerythritol and ditrimethylolpropane, and hexahydric alcohols such as dipentaerythritol are preferred, and trihydric alcohols that can form structural units with an appropriate crosslinking density and prevent gelation are particularly preferred, with trimethylolpropane being the most preferred, which contains three highly reactive methylol groups, is industrially available, and is inexpensive.

[0065] <1-3-3. Suitable raw material polyhydric alcohol> The polycarbonate polyol of the present invention is preferably one using, as the raw polyhydric alcohol, diethylene glycol or a diol (A) containing diethylene glycol and triethylene glycol, and a branched alcohol (B) containing trimethylolpropane. In particular, from the viewpoint of flexibility, solvent resistance, and mechanical strength, one using diethylene glycol, triethylene glycol, and trimethylolpropane in an amount of 30 to 70 mol % of diethylene glycol, 30 to 70 mol % of triethylene glycol, and 0.005 to 5 mol % of trimethylolpropane relative to a total of 100 mol % is preferable.

[0066] The raw material polyhydric alcohol for the polycarbonate polyol of the present invention may contain a polyhydric alcohol other than the above-mentioned diol (A) and branched alcohol (B), for example, a trivalent or higher linear alcohol or a trivalent or higher cyclic alcohol. However, in order to effectively obtain the above-mentioned effects by using the diol (A) and the branched alcohol (B), the content of polyhydric alcohol other than the diol (A) and the branched alcohol (B) in the raw material polyhydric alcohol is 30% by weight or less, particularly 20% by weight or less, and further 10% by weight or less, and it is most preferable that the raw material polyhydric alcohol does not contain such alcohols.

[0067] <1-4. Carbonate compounds> The carbonate compound used in the production of the polycarbonate polyol of the present invention is not limited as long as it does not impair the effects of the present invention, and examples thereof include dialkyl carbonates, diaryl carbonates, and alkylene carbonates. Among these, the use of diaryl carbonate has the advantage that the reaction proceeds quickly and reacts with the structural units in the polyhydric alcohol and polycarbonate polyol, which have low reactivity, and thus the proportion of carbonate terminal structures can be reduced. As described above, from the viewpoint of reducing the amount of dioxane generated, it is preferable to use a diaryl carbonate such as diphenyl carbonate as the carbonate compound.

[0068] Specific examples of dialkyl carbonates, diaryl carbonates, and alkylene carbonates that can be used in the production of the polycarbonate polyol according to the present invention are as follows:

[0069] Examples of dialkyl carbonates include dimethyl carbonate, diethyl carbonate, dibutyl carbonate, dicyclohexyl carbonate, diisobutyl carbonate, ethyl-n-butyl carbonate, ethyl isobutyl carbonate, and the like, with dimethyl carbonate and diethyl carbonate being preferred.

[0070] Examples of diaryl carbonates include diphenyl carbonate, ditolyl carbonate, bis(chlorophenyl) carbonate, di-m-cresyl carbonate, and the like, with diphenyl carbonate being preferred.

[0071] Examples of alkylene carbonates include ethylene carbonate, trimethylene carbonate, tetramethylene carbonate, 1,2-propylene carbonate, 1,2-butylene carbonate, 1,3-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 1,3-pentylene carbonate, 1,4-pentylene carbonate, 1,5-pentylene carbonate, 2,3-pentylene carbonate, 2,4-pentylene carbonate, and neopentyl carbonate, with ethylene carbonate being preferred.

[0072] These may be used alone or in combination of two or more.

[0073] Among these, diaryl carbonate is preferred because it is highly reactive and can be efficiently produced industrially, and diphenyl carbonate is more preferred because it is easily and inexpensively available as an industrial raw material. As described above, diphenyl carbonate is also preferred from the viewpoints of reducing the amount of dioxane generated, the amount of carbonate terminals, and the APHA value.

[0074] In the production of the polycarbonate polyol of the present invention, the amount of the carbonate compound used is not particularly limited, but in general, the molar ratio relative to 1 mole of the total of the raw material polyhydric alcohols is preferably 0.35 in lower limit, more preferably 0.50, and even more preferably 0.60 in upper limit, and preferably 1.00, more preferably 0.98, and even more preferably 0.97 in upper limit. If the amount of the carbonate compound used exceeds the upper limit, the proportion of terminal groups of the obtained polycarbonate polyol that are not hydroxyl groups may increase, or the molecular weight may not be within the specified range, and if it is less than the lower limit, the polymerization may not proceed to the specified molecular weight, or the raw material polyhydric alcohol may remain.

[0075] <1-5. Transesterification catalyst> The polycarbonate polyol of the present invention can be produced by polycondensing the above-mentioned polyhydric alcohol and a carbonate compound through an ester exchange reaction.

[0076] In the production of the polycarbonate polyol of the present invention, an ester exchange catalyst (hereinafter, sometimes referred to as a catalyst) is usually used to promote polycondensation. As the ester exchange catalyst, any compound that is generally considered to have an ester exchange ability can be used without any restrictions.

[0077] Examples of the transesterification catalyst include compounds of metals in Group 1 of the periodic table, such as lithium, sodium, potassium, rubidium, cesium, etc.; compounds of metals in Group 2 of the periodic table, such as magnesium, calcium, strontium, barium, etc.; compounds of metals in Group 4 of the periodic table, such as titanium, zirconium, etc.; compounds of metals in Group 5 of the periodic table, such as hafnium, etc.; compounds of metals in Group 9 of the periodic table, such as cobalt, etc.; compounds of metals in Group 12 of the periodic table, such as zinc, etc.; compounds of metals in Group 13 of the periodic table, such as aluminum, etc.; compounds of metals in Group 14 of the periodic table, such as germanium, tin, lead, etc.; compounds of metals in Group 15 of the periodic table, such as antimony, bismuth, etc.; and compounds of lanthanide metals, such as lanthanum, cerium, europium, ytterbium, etc. Among these, from the viewpoint of increasing the transesterification reaction rate, compounds of metals of Group 1 of the periodic table, compounds of metals of Group 2 of the periodic table, compounds of metals of Group 4 of the periodic table, compounds of metals of Group 5 of the periodic table, compounds of metals of Group 9 of the periodic table, compounds of metals of Group 12 of the periodic table, compounds of metals of Group 13 of the periodic table, and compounds of metals of Group 14 of the periodic table are preferred, compounds of metals of Group 1 of the periodic table, compounds of metals of Group 2 of the periodic table are more preferred, and compounds of metals of Group 2 of the periodic table are even more preferred. Among compounds of metals of Group 1 of the periodic table, compounds of lithium, potassium, and sodium are preferred, compounds of lithium and sodium are more preferred, and compounds of sodium are even more preferred. Among compounds of metals of Group 2 of the periodic table, compounds of magnesium, calcium, and barium are preferred, compounds of calcium and magnesium are more preferred, and compounds of magnesium are even more preferred. These metal compounds are mainly used as hydroxides, salts, etc. Examples of the salt when used as a salt include halide salts such as chloride, bromide, iodide, etc.; carboxylates such as acetate, formate, benzoate, etc.; sulfonates such as methanesulfonate, toluenesulfonate, trifluoromethanesulfonate, etc.; phosphorus-containing salts such as phosphate, hydrogen phosphate, dihydrogen phosphate, etc.; acetylacetonate salts; etc. The catalyst metal can also be used as an alkoxide such as methoxide or ethoxide.

[0078] Of these, preferred are acetates, nitrates, sulfates, carbonates, phosphates, hydroxides, halides, and alkoxides of at least one metal selected from Group 2 metals of the periodic table, more preferred are acetates, carbonates, and hydroxides of Group 2 metals of the periodic table, even more preferred are acetates, carbonates, and hydroxides of magnesium and calcium, particularly preferred are acetates of magnesium and calcium, and most preferred is magnesium acetate. From the viewpoint of reacting the low-reactivity oxyalkylene glycol (A1), branched alcohol (B), and end groups of the oxyaryl structure derived from the carbonate compound, which may be contained in the polycarbonate polyol of the present invention, compounds of metals in Group 1 of the periodic table, compounds of metals in Group 2 of the periodic table, and acetates, nitrates, sulfates, carbonates, phosphates, hydroxides, halides, and alkoxides of metals in Group 4 of the periodic table, which are low-period metals, have low electronegativity, and have strong coordination properties with carbonate compounds, are preferred. On the other hand, in strong acidity or strong basicity, decomposition of the oxyalkylene glycol (A1) contained in the raw material and the polycarbonate polyol structural unit occurs, and there is a problem that the molecular weight does not increase, and harmful low-molecular-weight compounds (1,4-dioxane) are by-produced, so compounds of metals in Group 2 of the periodic table having moderate basicity are preferred. In particular, in order to reduce the amount of the less reactive branched alcohol (B) and the terminal groups of the oxyaryl structure derived from the carbonate compound, acetates, carbonates, and hydroxides of magnesium and calcium, which are highly stable even when reacted for a long period of time, are preferred, and magnesium acetate is the most preferred. Furthermore, as described above, from the viewpoint of reducing the amount of dioxane generated in the polycondensation step and reducing the amount of carbonate terminals and APHA value of the resulting polycarbonate polyol, metal salts of Group 2 of the periodic table are preferred, and acetates and carbonates of magnesium and calcium are preferred, with magnesium acetate being most preferred.

[0079] When the above catalyst is used, if an excessive amount of the catalyst remains in the obtained polycarbonate polyol, the reaction may be inhibited or excessively promoted when the polycarbonate polyol is used to produce a polyurethane.

[0080] For this reason, when a transesterification catalyst is used, the amount used is preferably an amount that does not affect the performance even if it remains in the obtained polycarbonate polyol, and the upper limit is preferably 500 ppm, more preferably 100 ppm, even more preferably 50 ppm, and particularly preferably 10 ppm as a weight ratio in terms of metal relative to the weight of the total polyhydric alcohol.On the other hand, the lower limit is an amount that provides sufficient polymerization activity, and is preferably 0.01 ppm, more preferably 0.1 ppm, and even more preferably 1 ppm. Furthermore, when a compound of a Group 2 metal of the periodic table is used as the catalyst, the total amount of all metal atoms is preferably 5 μmol or more, more preferably 7 μmol or more, even more preferably 10 μmol or more, and preferably 500 μmol or less, more preferably 300 μmol or less, even more preferably 100 μmol or less, and particularly preferably 50 μmol or less, per mol of the total polyhydric alcohol used as the raw material.

[0081] Furthermore, as described above, in terms of reducing the amount of dioxane generated in the polycondensation step and reducing the amount of carbonate terminals and APHA value of the resulting polycarbonate polyol, when a metal salt of Group 2 of the periodic table is used as a catalyst, the concentration in terms of metal in the polycondensation reaction solution is preferably 50 ppm or less, more preferably 30 ppm or less, even more preferably 20 ppm or less, particularly preferably 15 ppm or less, and the lower limit is preferably 1 ppm or more.

[0082] <1-6. Production method of polycarbonate polyol> The polycarbonate polyol of the present invention can be produced by using the above-mentioned polyhydric alcohol and the above-mentioned carbonate compound in the above-mentioned ratio, and by carrying out ester exchange and polycondensation in the presence of an ester exchange catalyst, which is used as necessary, by adopting the above-mentioned means (1) to (5). The production method is described below.

[0083] The method of charging the reaction raw materials is not particularly limited, and the method can be freely selected from the following: a method in which the polyhydric alcohol, carbonate compound, and transesterification catalyst are all charged at the same time and subjected to the reaction; a method in which, when the carbonate compound is a solid, the carbonate compound is first charged and heated to melt it, and then the polyhydric alcohol and the transesterification catalyst are added; a method in which the polyhydric alcohol is charged first and melted, and then the carbonate compound and the transesterification catalyst are added; a method in which a part of the polyhydric alcohol is reacted with carbonate compounds or chlorocarbonates to synthesize a diester carbonate derivative of the polyhydric alcohol, and then the remaining polyhydric alcohol is reacted therewith. In the method for producing polycarbonate polyol of the present invention, in order to reduce the amount of carbonate terminals, it is also possible to adopt a method of adding a part of the polyhydric alcohol used at the end of the reaction. In this case, the upper limit of the amount of polyhydric alcohol added at the end is usually 20%, preferably 15%, and more preferably 10% of the amount of polyhydric alcohol to be charged, and the lower limit is usually 0.1%, preferably 0.5%, and more preferably 1.0%.

[0084] The suitable reaction temperature for the polycondensation reaction is as described above, and if the reaction temperature is too high, the resulting polycarbonate polyol may be colored, or quality problems may occur such as decarbonation of carbonate groups or by-production of ether structures due to dehydration condensation between polyhydric alcohols. In addition, since the polycarbonate polyol of the present invention contains structural units derived from oxydiethylene glycol, if the reaction temperature exceeds the upper limit, problems such as cleavage of the oxyalkylene chain or generation of harmful dioxane due to dehydration condensation may occur.

[0085] The reaction can be carried out at normal pressure, but the transesterification reaction is an equilibrium reaction, and the reaction can be biased toward the product system by distilling off the light-boiling components produced. Therefore, it is usually preferable to carry out the reaction while distilling off the light-boiling components by adopting reduced pressure conditions in the latter half of the reaction. Alternatively, it is also possible to carry out the reaction while distilling off the light-boiling components produced by gradually lowering the pressure from the middle of the reaction. It is particularly preferable to increase the degree of vacuum toward the end of the reaction, since this makes it possible to distill off by-products such as alcohols and phenols. In this case, the reaction pressure at the end of the polycondensation reaction is preferably set to the above-mentioned reduced pressure. At this time, in order to effectively distill off low boiling components, the reaction can be carried out while passing a small amount of an inert gas such as nitrogen, argon or helium into the reaction system.

[0086] In order to prevent the distillation of the raw materials at the beginning of the reaction, it is possible to attach a reflux tube to the reactor and carry out the reaction while refluxing the carbonate compound and the polyhydric alcohol. In this case, the raw materials charged are not lost and the amount ratio of the reagents can be accurately adjusted, which is preferable.

[0087] The reaction time is as described above, and is preferably 3 hours or more and 20 hours or less, and particularly preferably 5 hours or more and 10 hours or less.

[0088] As mentioned above, when a transesterification catalyst is used in the polycondensation reaction, the transesterification catalyst usually remains in the obtained polycarbonate polyol, and the remaining transesterification catalyst may make it impossible to control the reaction when performing the polyurethane reaction. In order to suppress the influence of this remaining catalyst, a phosphoric acid-based deactivator may be added after the polycondensation step and before the step of removing unreacted monomers. Furthermore, if the phosphoric acid-based deactivator is added and then heated as described below, the transesterification catalyst can be efficiently deactivated.

[0089] Examples of the phosphoric acid-based deactivator used for inactivating the transesterification catalyst include inorganic phosphoric acids such as phosphoric acid and phosphorous acid, and organic phosphoric acid esters such as dibutyl phosphate, tributyl phosphate, trioctyl phosphate, triphenyl phosphate, and triphenyl phosphite. These may be used alone or in combination of two or more.

[0090] The amount of the phosphoric acid deactivator used is not particularly limited, but it is preferable to use it in an almost equimolar amount with the transesterification catalyst used. Specifically, the upper limit is preferably 5 mol, more preferably 2 mol, and the lower limit is preferably 0.6 mol, more preferably 0.8 mol, and even more preferably 1.0 mol, relative to 1 mol of the transesterification catalyst used. If a phosphoric acid deactivator is used in an amount less than this amount, the transesterification catalyst is not sufficiently deactivated, and when the obtained polycarbonate polyol is used as, for example, a raw material for polyurethane production, the reactivity of the polycarbonate polyol with the isocyanate group may not be sufficiently reduced. In addition, if a phosphoric acid deactivator is used in an amount exceeding this range, the obtained polycarbonate polyol may become colored.

[0091] The inactivation of the transesterification catalyst by adding a phosphoric acid-based deactivator can be carried out at room temperature, but it is more efficient if it is heated. The temperature of this heat treatment is not particularly limited, but the upper limit is preferably 180°C, more preferably 150°C, even more preferably 120°C, and particularly preferably 100°C, and the lower limit is preferably 50°C, more preferably 60°C, and even more preferably 70°C. If the temperature is lower than this, the deactivation of the transesterification catalyst takes a long time and is not efficient, and the degree of deactivation may be insufficient. On the other hand, if the temperature exceeds the upper limit, the obtained polycarbonate polyol may be colored. The reaction time with the phosphoric acid-based deactivator is not particularly limited, but is usually 0.1 to 5 hours.

[0092] After the polycondensation reaction, it is preferable to carry out purification in order to remove impurities whose terminal structure in the polycarbonate polyol is an alkyloxy group, impurities whose terminal structure is an aryloxy group, phenols, unreacted monomers such as raw materials such as polyhydric alcohols and carbonate compounds, and further catalysts added. In this purification, a method of removing low-boiling compounds by distillation can be adopted. As a specific method of distillation, there is no particular limitation on the form, such as reduced pressure distillation, steam distillation, and thin film distillation, but thin film distillation is particularly effective. In addition, in order to remove water-soluble impurities, washing with water, alkaline water, acidic water, a solution of a chelating agent, etc. may be performed. In this case, the compound to be dissolved in water can be selected arbitrarily.

[0093] Although there are no particular limitations on the conditions for thin-film distillation, the upper limit of the temperature during thin-film distillation is preferably 250° C., more preferably 200° C. The lower limit is preferably 120° C., more preferably 150° C. By setting the lower limit of the temperature during thin-film distillation to the above value, the effect of removing low-boiling components becomes sufficient. Also, by setting the upper limit to 250°C, there is a tendency to prevent the polycarbonate polyol obtained after thin-film distillation from being colored.

[0094] The upper limit of the pressure during thin-film distillation is preferably 500 Pa, more preferably 150 Pa, and even more preferably 50 Pa. By setting the pressure during thin-film distillation to the above upper limit or less, the effect of removing low-boiling components tends to be sufficient. The upper limit of the temperature at which the polycarbonate polyol is kept warm immediately before the thin-film distillation is preferably 250° C., more preferably 150° C. The lower limit is preferably 80° C., more preferably 120° C.

[0095] By setting the temperature of the polycarbonate polyol for keeping warm immediately before the thin-film distillation to the lower limit or higher, there is a tendency to prevent the fluidity of the polycarbonate polyol immediately before the thin-film distillation from decreasing. On the other hand, by setting the temperature to the upper limit or lower, there is a tendency to prevent the polycarbonate polyol obtained after the thin-film distillation from being colored.

[0096] <1-7. Properties of Polycarbonate Polyol> <1-7-1. Hydroxyl value> The lower limit of the hydroxyl value of the polycarbonate polyol of the present invention is 20 mgKOH / g, preferably 25 mgKOH / g, more preferably 30 mgKOH / g, and even more preferably 35 mgKOH / g. The upper limit of the hydroxyl value of the polycarbonate polyol is 450 mgKOH / g, preferably 230 mgKOH / g, more preferably 150 mgKOH / g, even more preferably 120 mgKOH / g, even more preferably 75 mgKOH / g, particularly preferably 60 mgKOH / g, and most preferably 45 mgKOH / g. If the hydroxyl value is less than the lower limit, the viscosity may be too high, making handling difficult during polyurethane formation, and if it exceeds the upper limit, the physical properties such as flexibility and low temperature properties may be insufficient when polyurethane is formed.

[0097] <1-7-2.Molecular weight distribution> The molecular weight distribution of the polycarbonate polyol of the present invention, weight average molecular weight / number average molecular weight (Mw / Mn), is not particularly limited, but the lower limit is preferably 1.5, more preferably 1.8. The upper limit of weight average molecular weight / number average molecular weight (Mw / Mn) is preferably 3.5, more preferably 3.0. If the molecular weight distribution exceeds the above range, the physical properties of the polyurethane produced using this polycarbonate polyol tend to become hard at low temperatures, elongation tends to decrease, etc., and when trying to produce a polycarbonate polyol with a molecular weight distribution below the above range, advanced purification operations such as removing oligomers may be required. The weight average molecular weight of the polycarbonate polyol of the present invention is a weight average molecular weight in terms of polystyrene, and the number average molecular weight of the polycarbonate polyol of the present invention is a number average molecular weight in terms of polystyrene, and these can usually be determined by measurement using gel permeation chromatography (sometimes abbreviated as GPC).

[0098] <1-7-3.Molecular chain terminal> The molecular chain terminals of the polycarbonate polyol of the present invention are mainly hydroxyl groups. However, in the case of polycarbonate polyol obtained by the reaction of polyhydric alcohol with a carbonate compound, there is a possibility that some of the molecular chain terminals are not hydroxyl groups as impurities. Specific examples of such impurities include those in which the molecular chain terminal is an alkyloxy group or an aryloxy group, and most of them have a carbonate terminal structure.

[0099] For example, when diphenyl carbonate is used as the carbonate compound, a phenoxy group (PhO-) may remain as the aryloxy group at the carbonate terminal; when dimethyl carbonate is used, a methoxy group (MeO-) may remain as the alkyloxy group; when diethyl carbonate is used, an ethoxy group (EtO-) may remain; and when ethylene carbonate is used, a hydroxyethoxy group (HOCH2CHO-) may remain as the molecular chain terminal (here, Ph represents a phenyl group, Me represents a methyl group, and Et represents an ethyl group). As described above, the amount of carbonate terminals in the polycarbonate polyol of the present invention is preferably 1.0 mol % or less, more preferably 0.8 mol % or less, further preferably 0.5 mol % or less, and particularly preferably 0.1 mol % or less. 1 It can be determined by H-NMR measurement.

[0100] <1-7-4. Residual monomers, etc.> When diaryl carbonate such as diphenyl carbonate is used as a raw material, phenols are by-produced during the production of polycarbonate polyol. Since phenols are monofunctional compounds, they may be an inhibitor in the production of polyurethane, and the urethane bond formed by phenols may dissociate due to heat in the subsequent process due to its weak bonding strength, and isocyanate and phenols may be regenerated and cause problems. In addition, since phenols are also irritating substances, it is preferable that the amount of phenols remaining in the polycarbonate polyol is as small as possible. Specifically, the weight ratio of the phenols to the polycarbonate polyol is preferably 1000 ppm by weight or less, more preferably 500 ppm by weight or less, even more preferably 300 ppm by weight or less, and particularly preferably 100 ppm by weight or less. In order to reduce the amount of phenols in the polycarbonate polyol, it is effective to set the pressure of the polymerization reaction of the polycarbonate polyol to a high vacuum of 1 kPa or less as an absolute pressure, or to perform thin film distillation after the polymerization of the polycarbonate polyol.

[0101] In addition, the carbonate compound used as a raw material during production may remain in the polycarbonate polyol. The amount of the carbonate compound remaining in the polycarbonate polyol is not limited, but it is preferable that it is small, and the upper limit of the weight ratio to the polycarbonate polyol is preferably 5% by weight, more preferably 3% by weight, and even more preferably 1% by weight. If the carbonate compound content of the polycarbonate polyol is too high, it may inhibit the reaction during polyurethane formation. On the other hand, the lower limit is not particularly limited, but is preferably 0.1% by weight, more preferably 0.01% by weight, and even more preferably 0% by weight.

[0102] In addition, polyhydric alcohol used during production may remain in the polycarbonate polyol. The amount of polyhydric alcohol remaining in the polycarbonate polyol is not limited, but is preferably small, and is preferably 1% by weight or less, more preferably 0.1% by weight or less, and even more preferably 0.05% by weight or less, as a weight ratio to the polycarbonate polyol. If the amount of polyhydric alcohol remaining in the polycarbonate polyol is large, the molecular length of the soft segment portion when made into polyurethane may be insufficient, and desired physical properties may not be obtained.

[0103] In addition, polycarbonate polyol may contain cyclic carbonates (cyclic oligomers) produced as by-products during production. For example, when 1,3-propanediol is used, 1,3-dioxane-2-one or a cyclic carbonate formed by combining two or more molecules of these may be produced and contained in the polycarbonate polyol. These compounds may cause side reactions in the polyurethane reaction and may also cause turbidity, so it is preferable to remove as much as possible by making the pressure of the polymerization reaction of the polycarbonate polyol a high vacuum of 1 kPa or less as an absolute pressure or by performing thin film distillation after the synthesis of the polycarbonate polyol. The content of these cyclic carbonates contained in the polycarbonate polyol is not limited, but is preferably 3% by weight or less, more preferably 1% by weight or less, and even more preferably 0.5% by weight or less, as a weight ratio to the polycarbonate polyol.

[0104] [2. Manufacturing method of polyurethane] The polycarbonate polyols of the present invention can be used to produce polyurethanes. Hereinafter, a polyurethane produced using the polycarbonate polyol of the present invention will be referred to as "the polyurethane of the present invention." In the method for producing the polyurethane of the present invention using the polycarbonate polyol of the present invention, known polyurethane-forming reaction conditions for producing ordinary polyurethanes are used.

[0105] For example, the polyurethane of the present invention can be produced by reacting the polycarbonate polyol of the present invention with a polyisocyanate and a chain extender at a temperature ranging from room temperature to 200°C. Alternatively, the polyurethane of the present invention can be produced by first reacting the polycarbonate polyol of the present invention with an excess of polyisocyanate to produce a prepolymer having an isocyanate group at its terminal, and then increasing the degree of polymerization using a chain extender.

[0106] <2-1. Polyisocyanate> The polyisocyanate used in producing a polyurethane using the polycarbonate polyol of the present invention may be any of various known aliphatic, alicyclic or aromatic polyisocyanate compounds.

[0107] For example, aliphatic diisocyanates such as tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, and dimer diisocyanate in which the carboxyl groups of dimer acid are converted to isocyanate groups; alicyclic diisocyanates such as 1,4-cyclohexane diisocyanate, isophorone diisocyanate, 1-methyl-2,4-cyclohexane diisocyanate, 1-methyl-2,6-cyclohexane diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, 1,4-bis(isocyanate methyl)cyclohexane, and 1,3-bis(isocyanate methyl)cyclohexane. Cyanates: aromatic diisocyanates such as xylylene diisocyanate, 4,4'-diphenyl diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-dibenzyl diisocyanate, dialkyl diphenylmethane diisocyanate, tetraalkyl diphenylmethane diisocyanate, 1,5-naphthylene diisocyanate, 3,3'-dimethyl-4,4'-biphenylene diisocyanate, polymethylene polyphenyl isocyanate, phenylene diisocyanate, and m-tetramethyl xylylene diisocyanate. These may be used alone or in combination of two or more.

[0108] Among these, 4,4'-diphenylmethane diisocyanate, hexamethylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate and isophorone diisocyanate are preferred in that they give a polyurethane with a good balance of physical properties and are industrially available in large quantities at low cost.

[0109] <2-2. Chain extender> The chain extender used in producing the polyurethane of the present invention is a low molecular weight compound having at least two active hydrogens that react with the isocyanate group when producing a prepolymer having an isocyanate group described below, and typical examples of such a compound include polyols and polyamines.

[0110] Specific examples thereof include linear diols such as ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, and 1,12-dodecanediol; 2-methyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 2,2-diethyl-1,3-propanediol, 2-methyl-2-propyl-1,3-propanediol, and 2-methyl-1,4-butanediol. diols having branched chains such as diol, 2,4-heptanediol, 1,4-dimethylolhexane, 2-ethyl-1,3-hexanediol, 2,2,4-trimethyl-1,3-pentanediol, 2-methyl-1,8-octanediol, 2-butyl-2-ethyl-1,3-propanediol, and dimer diol; diols having ether groups such as diethylene glycol and propylene glycol; 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, and 1,4-dihydroxyethylcyclohexane diols having an alicyclic structure such as xylylene glycol, 1,4-dihydroxyethylbenzene, 4,4'-methylenebis(hydroxyethylbenzene), and other aromatic diols; polyols such as glycerin, trimethylolpropane, and pentaerythritol; hydroxyamines such as N-methylethanolamine and N-ethylethanolamine; ethylenediamine, 1,3-diaminopropane, hexamethylenediamine, triethylenetetramine, diethylenetriamine, isophoronediamine, 4,4'-di Examples of the polyamines include aminodicyclohexylmethane, 2-hydroxyethylpropylenediamine, di-2-hydroxyethylethylenediamine, di-2-hydroxyethylpropylenediamine, 2-hydroxypropylethylenediamine, di-2-hydroxypropylethylenediamine, 4,4'-diphenylmethanediamine, methylenebis(o-chloroaniline), xylylenediamine, diphenyldiamine, tolylenediamine, hydrazine, piperazine, and N,N'-diaminopiperazine; and water.

[0111] These chain extenders may be used alone or in combination of two or more. Among these, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,4-cyclohexanedimethanol, 1,4-dihydroxyethylcyclohexane, ethylenediamine, 1,3-diaminopropane, isophoronediamine, and 4,4'-diaminodicyclohexylmethane are preferred in terms of the favorable balance of physical properties of the resulting polyurethane and the industrial availability of these at low cost in large quantities.

[0112] Furthermore, the chain extender used in producing a prepolymer having a hydroxyl group, which will be described later, is a low molecular weight compound having at least two isocyanate groups, and specific examples thereof include the compounds described in <2-1. Polyisocyanate>.

[0113] <2-3. Chain terminators> When producing the polyurethane of the present invention, a chain terminator having one active hydrogen group can be used as necessary for the purpose of controlling the molecular weight of the resulting polyurethane.

[0114] Examples of these chain terminators include aliphatic monools having one hydroxyl group, such as methanol, ethanol, propanol, butanol, and hexanol, and aliphatic monoamines having one amino group, such as diethylamine, dibutylamine, n-butylamine, monoethanolamine, diethanolamine, and morpholine. These may be used alone or in combination of two or more.

[0115] <2-4. Catalyst> In the polyurethane-forming reaction when producing the polyurethane of the present invention, known urethane polymerization catalysts such as amine catalysts such as triethylamine, N-ethylmorpholine, triethylenediamine, etc., acid catalysts such as acetic acid, phosphoric acid, sulfuric acid, hydrochloric acid, sulfonic acid, etc., tin compounds such as trimethyltin laurate, dibutyltin dilaurate, dioctyltin dilaurate, dioctyltin dineodecane, etc., and further organometallic salts such as titanium compounds can also be used. The urethane polymerization catalysts may be used alone or in combination of two or more.

[0116] <2-5. Polyols other than the polycarbonate polyol of the present invention> In the polyurethane forming reaction when producing the polyurethane of the present invention, the polycarbonate polyol of the present invention may be used in combination with other polyols as necessary. Here, the polyol other than the polycarbonate polyol of the present invention is not particularly limited as long as it is used in the production of ordinary polyurethane, and examples thereof include polyether polyols, polyester polyols, polycaprolactone polyols, and polycarbonate polyols other than the present invention. For example, when used in combination with a polyether polyol, a polyurethane having further improved flexibility, which is a characteristic of the polycarbonate polyol of the present invention, can be obtained. Here, the weight ratio of the polycarbonate polyol of the present invention to the total weight of the polycarbonate polyol of the present invention and other polyols is preferably 70% or more, more preferably 90% or more. If the weight ratio of the polycarbonate polyol of the present invention is low, the balance between flexibility and solvent resistance, which is a characteristic of the polycarbonate polyol of the present invention, may be lost.

[0117] In the present invention, the above-mentioned polycarbonate polyol of the present invention can be modified and used for the production of polyurethane. The method of modifying polycarbonate polyol includes a method of adding an epoxy compound such as ethylene oxide, propylene oxide, butylene oxide, etc. to polycarbonate polyol to introduce an ether group, and a method of reacting polycarbonate polyol with a cyclic lactone such as ε-caprolactone, a dicarboxylic acid compound such as adipic acid, succinic acid, sebacic acid, terephthalic acid, etc., and an ester compound thereof to introduce an ester group. In the case of ether modification, the viscosity of the polycarbonate polyol is reduced by modification with ethylene oxide, propylene oxide, etc., which is preferable for reasons such as handleability. In particular, by modifying the polycarbonate polyol of the present invention with ethylene oxide or propylene oxide, the crystallinity of the polycarbonate polyol is reduced, and the flexibility at low temperatures is improved. In the case of modification with ethylene oxide, the water absorption and moisture permeability of the polyurethane produced using the ethylene oxide modified polycarbonate polyol is increased, so that the performance as artificial leather, synthetic leather, etc. may be improved. However, if the amount of ethylene oxide or propylene oxide added is large, various physical properties such as mechanical strength, heat resistance, and solvent resistance of the polyurethane produced using the modified polycarbonate polyol are reduced, so that the amount of ethylene oxide or propylene oxide added to the polycarbonate polyol is suitably 5 to 50% by weight, preferably 5 to 40% by weight, and more preferably 5 to 30% by weight. In addition, in the method of introducing an ester group, the viscosity of the polycarbonate polyol is reduced by modification with ε-caprolactone, which is preferable for reasons such as handleability. The amount of ε-caprolactone added to the polycarbonate polyol is suitably 5 to 50% by weight, preferably 5 to 40% by weight, and more preferably 5 to 30% by weight. If the amount of ε-caprolactone added exceeds 50% by weight, the hydrolysis resistance, chemical resistance, etc. of the polyurethane produced using the modified polycarbonate polyol are reduced.

[0118] <2-6. Solvents> The polyurethane-forming reaction in producing the polyurethane of the present invention may be carried out in a solvent. Preferred solvents include amide-based solvents such as dimethylformamide, diethylformamide, dimethylacetamide, and N-methylpyrrolidone, sulfoxide-based solvents such as dimethylsulfoxide, ketone-based solvents such as methyl ethyl ketone, cyclohexanone, and methyl isobutyl ketone, ether-based solvents such as tetrahydrofuran and dioxane, ester-based solvents such as methyl acetate, ethyl acetate, and butyl acetate, and aromatic hydrocarbon-based solvents such as toluene and xylene. These solvents may be used alone or as a mixed solvent of two or more kinds.

[0119] Among these, preferred organic solvents are methyl ethyl ketone, ethyl acetate, toluene, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, dimethylsulfoxide, and the like. Moreover, a polyurethane in the form of a water dispersion can also be produced from a polyurethane composition containing the polycarbonate polyol of the present invention, a polydiisocyanate, and the above-mentioned chain extender.

[0120] <2-7. Polyurethane manufacturing method> As a method for producing the polyurethane of the present invention using the above-mentioned reactants, a production method generally used in experiments or industrially can be used. Examples of such methods include a method in which the polycarbonate polyol of the present invention, a polyol other than the polycarbonate polyol of the present invention that is used as needed (hereinafter, may be referred to as "other polyol"), a polyisocyanate, and a chain extender are mixed together and reacted (hereinafter, may be referred to as "one-stage method"), and a method in which the polycarbonate polyol of the present invention, the other polyol, and a polyisocyanate are first reacted to prepare a prepolymer having isocyanate groups at both ends, and then the prepolymer is reacted with a chain extender (hereinafter, may be referred to as "two-stage method").

[0121] The two-stage method involves a step of preparing an intermediate having isocyanates at both ends of the part corresponding to the soft segment of polyurethane by reacting the polycarbonate polyol of the present invention and another polyol with one equivalent or more of polyisocyanate in advance. In this way, if a prepolymer is prepared and then reacted with a chain extender, it may be easy to adjust the molecular weight of the soft segment part, and it is useful when it is necessary to ensure phase separation of the soft segment and the hard segment.

[0122] <2-8.One step method> The one-stage method, also called the one-shot method, is a method in which the polycarbonate polyol of the present invention, other polyol, polyisocyanate and chain extender are charged all at once to carry out the reaction.

[0123] The amount of polyisocyanate used in the one-stage method is not particularly limited, but when the total number of hydroxyl groups in the polycarbonate polyol of the present invention and other polyols and the sum of the number of hydroxyl groups and the number of amino groups in the chain extender is taken as 1 equivalent, the lower limit is preferably 0.5 equivalents, more preferably 0.6 equivalents, even more preferably 0.7 equivalents, and particularly preferably 0.8 equivalents, and the upper limit is preferably 2.0 equivalents, more preferably 1.5 equivalents, even more preferably 1.2 equivalents, and particularly preferably 1.0 equivalent. The equivalent ratio of the sum of the total number of isocyanate groups, total hydroxyl groups, and total amino groups derived from the raw materials used above may be referred to as the NCO / OH ratio.

[0124] If too much polyisocyanate is used, unreacted isocyanate groups will undergo side reactions, and the viscosity of the resulting polyurethane will become too high, making it difficult to handle and reducing its flexibility. If too little is used, the molecular weight of the polyurethane will not be large enough, and the polyurethane will tend not to have sufficient strength or solvent resistance.

[0125] The amount of the chain extender is not particularly limited, but when the number of isocyanate groups in the polyisocyanate minus the total number of hydroxyl groups in the polycarbonate polyol of the present invention and other polyols is taken as 1 equivalent, the lower limit is preferably 0.7 equivalents, more preferably 0.8 equivalents, even more preferably 0.9 equivalents, and particularly preferably 0.95 equivalents, and the upper limit is preferably 3.0 equivalents, more preferably 2.0 equivalents, even more preferably 1.5 equivalents, and particularly preferably 1.1 equivalents. If the amount of the chain extender is too large, the polyurethane obtained tends to be difficult to dissolve in a solvent and difficult to process, and if the amount is too small, the polyurethane obtained may be too soft to obtain sufficient strength, hardness, elastic recovery performance, or elastic retention performance, or the heat resistance may be deteriorated.

[0126] <2-9. Two-step method> The two-stage method is also called the prepolymer method, and mainly includes the following methods. (a) A method in which the polycarbonate polyol of the present invention and other polyol are reacted in advance with an excess of polyisocyanate at a reaction equivalent ratio of polyisocyanate / (polycarbonate polyol of the present invention and other polyol) of more than 1 to 10.0 or less to produce a prepolymer having isocyanate groups at the molecular chain terminals, and then a chain extender is added to this to produce a polyurethane. (b) A method in which a polyisocyanate is reacted in advance with an excess of the polycarbonate polyol of the present invention and other polyols at a reaction equivalent ratio of polyisocyanate / (the polycarbonate polyol of the present invention and other polyols) of 0.1 or more and less than 1.0 to produce a prepolymer having hydroxyl groups at the molecular chain ends, and then a polyisocyanate having isocyanate groups at the ends is reacted as a chain extender to produce a polyurethane.

[0127] The two-stage process can be carried out in the absence of a solvent or in the presence of a solvent. The two-stage polyurethane production can be carried out by any one of the following methods (1) to (3). (1) Without using a solvent, first, a polyisocyanate, the polycarbonate polyol of the present invention, and another polyol are directly reacted to synthesize a prepolymer, which is then used as is in the chain extension reaction. (2) A prepolymer is synthesized by the method in (1), then dissolved in a solvent and used in the subsequent chain extension reaction. (3) A solvent is used from the beginning, polyisocyanate, the polycarbonate polyol of the present invention, and other polyols are reacted, and then a chain extension reaction is carried out.

[0128] In the case of method (1), it is important to obtain the polyurethane in the coexistence with the solvent during the chain extension reaction by, for example, dissolving the chain extender in the solvent or dissolving the prepolymer and the chain extender in the solvent at the same time.

[0129] The amount of polyisocyanate used in the two-stage process (a) is not particularly limited, but when the total number of hydroxyl groups in the polycarbonate polyol of the present invention and the other polyol is taken as 1 equivalent, the lower limit in terms of the number of isocyanate groups is preferably an amount exceeding 1.0 equivalent, more preferably 1.2 equivalents, and even more preferably 1.5 equivalents, and the upper limit is preferably in the range of 10.0 equivalents, more preferably 5.0 equivalents, and even more preferably 3.0 equivalents.

[0130] If the amount of isocyanate used is too large, the excess isocyanate groups will undergo side reactions, making it difficult to achieve the desired physical properties of the polyurethane. If the amount is too small, the molecular weight of the resulting polyurethane will not increase sufficiently, and the strength and thermal stability may be reduced.

[0131] The amount of the chain extender used is not particularly limited, but the lower limit is preferably 0.1 equivalents, more preferably 0.5 equivalents, and even more preferably 0.8 equivalents, and the upper limit is preferably 5.0 equivalents, more preferably 3.0 equivalents, and even more preferably 2.0 equivalents, relative to 1 equivalent of the number of isocyanate groups contained in the prepolymer.

[0132] When the chain extension reaction is carried out, monofunctional organic amines or alcohols may be coexisted for the purpose of adjusting the molecular weight.

[0133] The amount of polyisocyanate used in preparing a prepolymer terminated with a hydroxyl group in the two-stage process (b) is not particularly limited, but when the total number of hydroxyl groups in the polycarbonate polyol and other polyols is taken as 1 equivalent, the lower limit in terms of the number of isocyanate groups is preferably 0.1 equivalent, more preferably 0.5 equivalent, and even more preferably 0.7 equivalent, and the upper limit is preferably 0.99 equivalent, more preferably 0.98 equivalent, and even more preferably 0.97 equivalent.

[0134] If the amount of isocyanate used is too small, the process required to obtain the desired molecular weight by the subsequent chain extension reaction will be long, tending to reduce production efficiency. Conversely, if the amount is too large, the viscosity will be too high, resulting in a decrease in flexibility of the resulting polyurethane or in poor handling, resulting in poor productivity.

[0135] The amount of the chain extender used is not particularly limited, but when the total number of hydroxyl groups in the polycarbonate polyol and other polyols used in the prepolymer is taken as 1 equivalent, the total equivalent including the equivalent of the isocyanate groups used in the prepolymer is preferably 0.7 equivalents at the lower limit, more preferably 0.8 equivalents, and even more preferably 0.9 equivalents at the upper limit, and is preferably less than 1.0 equivalent, more preferably 0.99 equivalents, and even more preferably 0.98 equivalents.

[0136] When the chain extension reaction is carried out, monofunctional organic amines or alcohols may be coexisted for the purpose of adjusting the molecular weight.

[0137] The chain extension reaction is usually carried out at 0°C to 250°C, but this temperature varies depending on the amount of solvent, the reactivity of the raw materials used, the reaction equipment, etc., and is not particularly limited. If the temperature is too low, the reaction may proceed slowly, or the production time may be long due to the low solubility of the raw materials and polymerized products, and if the temperature is too high, side reactions or decomposition of the resulting polyurethane may occur. The chain extension reaction may be carried out under reduced pressure while degassing.

[0138] In addition, a catalyst, a stabilizer, etc. may be added to the chain extension reaction, if necessary. Examples of catalysts include compounds such as triethylamine, tributylamine, dibutyltin dilaurate, stannous octoate, acetic acid, phosphoric acid, sulfuric acid, hydrochloric acid, and sulfonic acid, and may be used alone or in combination of two or more. Examples of stabilizers include compounds such as 2,6-dibutyl-4-methylphenol, distearyl thiodipropionate, N,N'-di-2-naphthyl-1,4-phenylenediamine, and tris(dinonylphenyl)phosphite, and may be used alone or in combination of two or more. In addition, when the chain extender is a highly reactive one such as a short-chain aliphatic amine, the reaction may be carried out without adding a catalyst.

[0139] <2-10. Water-based polyurethane emulsion> The polycarbonate polyol of the present invention can also be used to produce a water-based polyurethane emulsion.

[0140] In that case, when a prepolymer is produced by reacting a polyol containing the polycarbonate polyol of the present invention with an excess of polyisocyanate, a compound having at least one hydrophilic functional group and at least two isocyanate-reactive groups is mixed to form a prepolymer, which is then converted into an aqueous polyurethane emulsion through a neutralization / salting step of the hydrophilic functional group, an emulsification step by adding water, and a chain extension reaction step.

[0141] The hydrophilic functional group of the compound having at least one hydrophilic functional group and at least two isocyanate-reactive groups used herein is, for example, a carboxyl group or a sulfonic acid group, which is a group that can be neutralized with an alkaline group. The isocyanate-reactive group is a group that generally reacts with isocyanate to form a urethane bond or a urea bond, such as a hydroxyl group, a primary amino group, or a secondary amino group, and these may be mixed in the same molecule.

[0142] Specific examples of compounds having at least one hydrophilic functional group and at least two isocyanate-reactive groups include 2,2'-dimethylolpropionic acid, 2,2-methylolbutyric acid, and 2,2'-dimethylolvaleric acid. In addition, diaminocarboxylic acids such as lysine, cystine, and 3,5-diaminocarboxylic acid can also be mentioned. These can be used alone or in combination of two or more. When actually using these, they can be neutralized with amines such as trimethylamine, triethylamine, tri-n-propylamine, tributylamine, and triethanolamine, or alkaline compounds such as sodium hydroxide, potassium hydroxide, and ammonia.

[0143] When producing a water-based polyurethane emulsion, the amount of the compound having at least one hydrophilic functional group and at least two isocyanate-reactive groups is preferably 1% by weight, more preferably 5% by weight, and even more preferably 10% by weight based on the total weight of the polycarbonate polyol of the present invention and other polyols in order to improve the dispersibility in water. On the other hand, if too much of this is added, the properties of the polycarbonate polyol of the present invention may not be maintained, so the upper limit is preferably 50% by weight, more preferably 40% by weight, and even more preferably 30% by weight.

[0144] When producing an aqueous polyurethane emulsion, the reaction may be carried out in the prepolymer step in the presence of a solvent such as methyl ethyl ketone, acetone, or N-methyl-2-pyrrolidone, or may be carried out without a solvent. When a solvent is used, it is preferable to remove the solvent by distillation after producing the aqueous emulsion.

[0145] When producing an aqueous polyurethane emulsion without solvent using the polycarbonate polyol of the present invention as a raw material, the upper limit of the number average molecular weight calculated from the hydroxyl value of the polycarbonate polyol is preferably 5000, more preferably 4500, and even more preferably 4000. The lower limit of the number average molecular weight is preferably 300, more preferably 500, and even more preferably 800. If the number average molecular weight calculated from the hydroxyl value exceeds 5000 or is smaller than 300, emulsification may become difficult.

[0146] In synthesizing or storing the water-based polyurethane emulsion, emulsion stability may be maintained by using in combination an anionic surfactant represented by higher fatty acid, resin acid, acidic fatty alcohol, sulfate ester, higher alkyl sulfonate, alkylaryl sulfonate, sulfonated castor oil, sulfosuccinate ester, etc.; a cationic surfactant such as a primary amine salt, a secondary amine salt, a tertiary amine salt, a quaternary amine salt, a pyridinium salt, etc.; or a nonionic surfactant represented by a known reaction product of ethylene oxide with a long-chain fatty alcohol or a phenol.

[0147] In addition, when preparing a water-based polyurethane emulsion, the emulsion can also be produced by mechanically mixing water under high shear in the presence of an emulsifier with an organic solvent solution of the prepolymer, if necessary without the neutralization / salting step.

[0148] The water-based polyurethane emulsions produced in this way can be used for a variety of purposes. In particular, in light of the recent demand for chemical raw materials with a low environmental impact, they can be used as a replacement for conventional products that do not use organic solvents.

[0149] Specific applications of the aqueous polyurethane emulsion include, for example, coating agents, aqueous paints, adhesives, synthetic leather, and artificial leather. In particular, the aqueous polyurethane emulsion produced using the polycarbonate polyol of the present invention has a structural unit derived from the oxyalkylene glycol (A1) in the polycarbonate polyol, and therefore has flexibility and can be effectively used as a coating agent, etc.

[0150] <2-11. Additives> To the polyurethane of the present invention produced using the polycarbonate polyol of the present invention, various additives such as heat stabilizers, light stabilizers, colorants, fillers, stabilizers, UV absorbers, antioxidants, anti-tack agents, flame retardants, antioxidants, inorganic fillers, etc. can be added or mixed within the range that does not impair the properties of the polyurethane of the present invention.

[0151] Examples of compounds that can be used as heat stabilizers include aliphatic, aromatic, or alkyl group-substituted aromatic esters of phosphoric acid and phosphorous acid, hypophosphorous acid derivatives, phosphorus compounds such as phenylphosphonic acid, phenylphosphinic acid, diphenylphosphonic acid, polyphosphonates, dialkyl pentaerythritol diphosphites, and dialkyl bisphenol A diphosphites; phenol derivatives, particularly hindered phenol compounds; sulfur-containing compounds such as thioethers, dithioacid salts, mercaptobenzimidazoles, thiocarbanilides, and thiodipropionic acid esters; and tin compounds such as tin maleates and dibutyltin monoxide.

[0152] Specific examples of the hindered phenol compound include "Irganox1010" (product name: manufactured by BASF Japan Ltd.), "Irganox1520" (product name: manufactured by BASF Japan Ltd.), and "Irganox245" (product name: manufactured by BASF Japan Ltd.). Examples of phosphorus compounds include "PEP-36", "PEP-24G", and "HP-10" (all trade names: manufactured by ADEKA Corporation), and "Irgafos 168" (trade name: manufactured by BASF Japan Ltd.). Specific examples of the sulfur-containing compound include thioether compounds such as dilauryl thiopropionate (DLTP) and distearyl thiopropionate (DSTP).

[0153] Examples of light stabilizers include benzotriazole-based and benzophenone-based compounds. Specifically, usable products include "TINUVIN622LD" and "TINUVIN765" (both manufactured by Chiba Specialty Chemicals Co., Ltd.), "SANOL LS-2626" and "SANOL LS-765" (both manufactured by Sankyo Co., Ltd.).

[0154] Examples of ultraviolet absorbents include "TINUVIN328" and "TINUVIN234" (both manufactured by Chiba Specialty Chemicals Co., Ltd.).

[0155] Examples of colorants include dyes such as direct dyes, acid dyes, basic dyes, and metal complex dyes; inorganic pigments such as carbon black, titanium oxide, zinc oxide, iron oxide, and mica; and organic pigments such as coupling azo pigments, condensed azo pigments, anthraquinone pigments, thioindigo pigments, dioxazone pigments, and phthalocyanine pigments.

[0156] Examples of the inorganic filler include short glass fibers, carbon fibers, alumina, talc, graphite, melamine, and clay.

[0157] Examples of flame retardants include additive and reactive flame retardants such as phosphorus and halogen-containing organic compounds, bromine or chlorine-containing organic compounds, ammonium polyphosphate, aluminum hydroxide, and antimony oxide.

[0158] These additives may be used alone, or two or more of them may be used in any combination and in any ratio.

[0159] The amount of these additives added, in terms of weight ratio to polyurethane, is preferably 0.01% by weight at the lower limit, more preferably 0.05% by weight at the lower limit, and even more preferably 0.1% by weight at the upper limit, and is preferably 10% by weight at the lower limit, more preferably 5% by weight at the upper limit, and even more preferably 1% by weight at the upper limit. If the amount of additives added is too small, the effect of adding the additives cannot be fully obtained, whereas if the amount of additives added is too large, the additives may precipitate in the polyurethane or cause turbidity.

[0160] <2-12. Polyurethane film / polyurethane plate> When a film is produced using the polyurethane of the present invention, the lower limit of the thickness of the film is preferably 10 μm, more preferably 20 μm, and even more preferably 30 μm, and the upper limit is preferably 1000 μm, more preferably 500 μm, and even more preferably 100 μm. If the film is too thick, sufficient moisture permeability tends not to be obtained, whereas if the film is too thin, pinholes tend to occur and the film tends to be prone to blocking, making it difficult to handle.

[0161] <2-13.Molecular weight> The molecular weight of the polyurethane of the present invention is appropriately adjusted according to its application and is not particularly limited, but is preferably 50,000 to 500,000, more preferably 100,000 to 300,000, as a weight average molecular weight (Mw) calculated based on polystyrene measured by gel permeation chromatography (GPC). If Mw is smaller than the lower limit, sufficient strength and hardness may not be obtained, and if it is larger than the upper limit, handling properties such as processability tend to be impaired. In particular, by using the polycarbonate polyol of the present invention, polyurethane with Mw of 100,000 or more can be easily produced due to its excellent reactivity, and sufficient mechanical strength can be obtained.

[0162] <2-14. Solvent resistance> <2-14-1. Oleic acid resistance> When the polyurethane of the present invention is evaluated, for example, by the method described in the Examples section below, the rate of change (%) of the weight of a polyurethane test piece after immersion in oleic acid relative to the weight of the polyurethane test piece before immersion in oleic acid is preferably 20% or less, more preferably 10% or less, even more preferably 5% or less, particularly preferably 4% or less, and most preferably 3% or less. If this weight change rate exceeds the upper limit, sufficient resistance to oleic acid may not be obtained.

[0163] <2-14-2. Ethanol resistance> When the polyurethane of the present invention is evaluated, for example, by the method described in the Examples section below, the rate of change (%) of the weight of a polyurethane test piece after immersion in ethanol relative to the weight of the polyurethane test piece before immersion in ethanol is preferably 20% or less, more preferably 18% or less, even more preferably 15% or less, particularly preferably 10% or less, and most preferably 8% or less. If this weight change rate exceeds the upper limit, sufficient ethanol resistance may not be obtained.

[0164] <2-14-3. Ethyl acetate resistance> When the polyurethane of the present invention is evaluated, for example, by the method described in the Examples section below, the rate of change (%) in the weight of a polyurethane test piece after immersion in a chemical relative to the weight of the polyurethane test piece before immersion in ethyl acetate is preferably 50% or less, more preferably 40% or less, and even more preferably 35% or less. If the weight change rate exceeds the upper limit, the desired chemical resistance may not be obtained.

[0165] <2-15. Tensile elongation at break> The polyurethane of the present invention preferably has a tensile elongation at break and a breaking strength in the following ranges, measured on a rectangular sample having a width of 10 mm, a length of 100 mm and a thickness of about 50 to 100 μm at a chuck distance of 50 mm, a tensile speed of 500 mm / min, a temperature of 23° C. and a relative humidity of 50%. That is, the lower limit of the breaking elongation is preferably 150%, more preferably 200%, and even more preferably 300%, and the upper limit is preferably 3000%, more preferably 2000%, and even more preferably 1500%. If the breaking elongation is less than the lower limit, the handling properties such as processability tend to be impaired, and if it exceeds the upper limit, sufficient solvent resistance may not be obtained. The lower limit of the breaking strength is preferably 1.0 MPa, more preferably 2.0 MPa, and even more preferably 3.0 MPa, and the upper limit is preferably 100 MPa, more preferably 8.0 MPa, and even more preferably 6.0 MPa. If the breaking strength is less than the lower limit, the handling properties such as processability tend to be impaired, and if it exceeds the upper limit, flexibility may be impaired.

[0166] <2-16.100%-300% modulus> When the polyurethane of the present invention is obtained by reacting the polycarbonate polyol of the present invention with 4,4'-diphenylmethane diisocyanate and 1,4-butanediol in a one-stage process under conditions where the total amount of the polyurethane is 17 to 20% by weight based on the total amount of polyurethane, it is preferable that the 100% modulus and 300% modulus of a rectangular sample having a width of 10 mm, a length of 100 mm and a thickness of about 50 to 100 μm are measured at a chuck distance of 50 mm, a tensile speed of 500 mm / min, a temperature of 23°C and a relative humidity of 50% in the following ranges. That is, the lower limit of the 100% modulus is preferably 0.7 MPa, more preferably 0.9 MPa, and even more preferably 1.0 MPa, and the upper limit is preferably 20 MPa, more preferably 10 MPa, and even more preferably 5.0 MPa. If the 100% modulus is less than the lower limit, the solvent resistance may be insufficient, and if it exceeds the upper limit, the flexibility may be insufficient and the handling properties such as processability may be impaired. The lower limit of the 300% modulus is preferably 1.4 MPa, more preferably 2.0 MPa, and even more preferably 2.5 MPa, and the upper limit is preferably 15 MPa, more preferably 9.0 MPa, and even more preferably 6.0 MPa. If the 300% modulus is less than the lower limit, the solvent resistance may be insufficient, and if it exceeds the upper limit, the flexibility may be insufficient and the handling properties such as processability may be impaired.

[0167] <2-17. Glass transition temperature> The lower limit of the glass transition temperature of the polyurethane of the present invention is usually -70°C or higher, preferably -60°C or higher, more preferably -50°C or higher, even more preferably -40°C or higher, and particularly preferably -30°C or higher. The upper limit is usually 0°C or lower, preferably -5°C or lower, more preferably -10°C or lower, even more preferably -15°C or lower, and particularly preferably -20°C or lower. When the glass transition temperature of the polyurethane is at least the lower limit, the solvent resistance is good, and when the glass transition temperature is at most the upper limit, the polyurethane is prevented from hardening at low temperatures and the touch tends to be improved.

[0168] <2-18.Applications> The polyurethane of the present invention has excellent solvent resistance and good flexibility and mechanical strength, and therefore can be widely used in foams, elastomers, elastic fibers, paints, fibers, pressure-sensitive adhesives, adhesives, flooring materials, sealants, medical materials, artificial leather, synthetic leather, coating agents, water-based polyurethane paints, active energy radiation-curable polymer compositions, and the like.

[0169] In particular, when the polyurethane of the present invention is used for applications such as artificial leather, synthetic leather, water-based polyurethane, adhesives, elastic fibers, medical materials, flooring materials, paints, coating agents, etc., it has a good balance of solvent resistance, flexibility, and mechanical strength, and therefore can impart good properties such as high durability in areas that come into contact with human skin or where cosmetic agents or disinfectant alcohol are used, sufficient flexibility, and resistance to physical impacts, etc. In addition, it can be suitably used for automotive applications requiring heat resistance and outdoor applications requiring weather resistance.

[0170] The polyurethane of the present invention can be used for cast polyurethane elastomers. Specific applications include rolls such as rolling mill rolls, papermaking rolls, office equipment, and pretension rolls, solid tires and casters for forklifts, automobile vehicle new trams, dollies, and carriers, and industrial products such as conveyor belt idlers, guide rolls, pulleys, steel pipe linings, rubber screens for ores, gears, connection rings, liners, pump impellers, cyclone cones, cyclone liners, etc. It can also be used for belts for office automation equipment, paper feed rolls, cleaning blades for copying, snow plows, toothed belts, surf rollers, etc.

[0171] The polyurethane of the present invention is also applicable to applications as a thermoplastic elastomer. For example, it can be used in pneumatic equipment, painting equipment, analytical equipment, physicochemical equipment, metering pumps, water treatment equipment, tubes and hoses in industrial robots, spiral tubes, fire hoses, etc. used in the food and medical fields. It can also be used as belts such as round belts, V-belts, and flat belts in various transmission mechanisms, spinning machines, packing machines, printing machines, etc. It can also be used in footwear heel tops and soles, couplings, packing, ball joints, bushes, gears, rolls, and other equipment parts, sports goods, leisure goods, watch belts, etc. Furthermore, examples of automobile parts include oil stoppers, gear boxes, spacers, chassis parts, interior parts, tire chain replacements, etc. It can also be used in keyboard films, films for automobiles, curl cords, cable sheaths, bellows, conveyor belts, flexible containers, binders, synthetic leather, dipping products, adhesives, etc.

[0172] The polyurethane of the present invention can also be used as a solvent-based two-liquid coating material and can be applied to wood products such as musical instruments, Buddhist altars, furniture, decorative plywood, sporting goods, etc. It can also be used as a tar epoxy urethane for automobile repair.

[0173] The polyurethane of the present invention can be used as a component of moisture-curing one-component paints, blocked isocyanate-based solvent paints, alkyd resin paints, urethane-modified synthetic resin paints, ultraviolet-curing paints, water-based urethane paints, and the like, and can be applied, for example, to paints for plastic bumpers, strippable paints, coating agents for magnetic tapes, overprint varnishes for floor tiles, flooring materials, paper, wood grain printed films, and the like, varnishes for wood, coil coats for high processing, optical fiber protective coatings, solder resists, top coats for metal printing, base coats for vapor deposition, white coats for food cans, and the like.

[0174] The polyurethane of the present invention can also be used as a pressure sensitive adhesive or bonding agent for food packaging, shoes, footwear, magnetic tape binders, decorative paper, wood, structural members, etc., and can also be used as a component of low temperature adhesives and hot melts.

[0175] The polyurethane of the present invention can be used as a binder in magnetic recording media, inks, castings, burnt bricks, graft materials, microcapsules, granular fertilizers, granular agricultural chemicals, polymer cement mortar, resin mortar, rubber chip binders, recycled foams, glass fiber sizing, and the like.

[0176] The polyurethane of the present invention can be used as a component of a fiber processing agent for shrink-proofing, wrinkle-proofing, water-repellent finishing, and the like. When the polyurethane of the present invention is used as an elastic fiber, the fiberization method can be carried out without any particular limitation as long as it can be spun. For example, a melt spinning method can be adopted in which the polyurethane is once pelletized, melted, and spun directly through a spinneret. When the polyurethane of the present invention is melt spun to obtain an elastic fiber, the spinning temperature is preferably 250°C or less, more preferably 200°C or more and 235°C or less.

[0177] The polyurethane elastic fiber of the present invention can be used as it is as a bare yarn, or can be covered with other fibers to be used as a covered yarn. Examples of other fibers include conventionally known fibers such as polyamide fibers, wool, cotton, and polyester fibers, and among these, polyester fibers are preferably used in the present invention. The polyurethane elastic fiber of the present invention may also contain a dye-type disperse dye.

[0178] The polyurethane of the present invention can be used as a sealant / caulking for concrete walls, induction joints, around sashes, wall-type PC (precast concrete) joints, ALC (autoclaved lightweight concrete) joints, board joints, sealants for composite glass, heat-insulating sash sealants, and automotive sealants.

[0179] The polyurethane of the present invention can be used as a medical material, and can be used as a blood-compatible material for tubes, catheters, artificial hearts, artificial blood vessels, artificial valves, etc., and as a disposable material for catheters, tubes, bags, surgical gloves, artificial kidney potting materials, etc. By modifying the ends, the polyurethane of the present invention can be used as a raw material for UV-curable coating materials, electron beam-curable coating materials, photosensitive resin compositions for flexographic printing plates, photocurable optical fiber coating material compositions, and the like.

[0180] <2-19. Urethane (meth)acrylate oligomer> A urethane (meth)acrylate oligomer can be produced by addition reacting a polyisocyanate with a hydroxyalkyl (meth)acrylate using the polycarbonate polyol of the present invention. When other raw material compounds such as a polyol and a chain extender are used in combination, the urethane (meth)acrylate oligomer can be produced by further addition reacting the polyisocyanate with these other raw material compounds. In the present invention, when "(meth)acrylic" is used, such as (meth)acrylate or (meth)acrylic acid, it means acrylic and / or methacrylic.

[0181] The ratio of the raw material compounds is substantially the same as or the same as the composition of the desired urethane (meth)acrylate oligomer. In the urethane (meth)acrylate oligomer, the amount of all isocyanate groups and the amount of all functional groups reactive with the isocyanate groups, such as hydroxyl groups and amino groups, are usually theoretically equimolar.

[0182] When producing a urethane (meth)acrylate oligomer, the amount of hydroxyalkyl (meth)acrylate used is usually 10 mol% or more, preferably 15 mol% or more, more preferably 25 mol% or more, and usually 70 mol% or less, preferably 50 mol% or less, based on the total amount of hydroxyalkyl (meth)acrylate, polycarbonate polyol, and other raw material compounds used as necessary, such as polyols, and compounds containing functional groups that react with isocyanates, such as chain extenders. Depending on this ratio, the molecular weight of the obtained urethane (meth)acrylate oligomer can be controlled. If the ratio of hydroxyalkyl (meth)acrylate is high, the molecular weight of the urethane (meth)acrylate oligomer tends to be small, and if the ratio is low, the molecular weight tends to be large.

[0183] The amount of polycarbonate polyol used is preferably 25 mol% or more, more preferably 50 mol% or more, and even more preferably 70 mol% or more, based on the total amount of polycarbonate polyol and polyol used. When the amount of polycarbonate polyol used is equal to or more than the lower limit, the hardness and stain resistance of the obtained cured product tend to be good, which is preferable.

[0184] The amount of polycarbonate polyol used is preferably 10% by weight or more, more preferably 30% by weight or more, even more preferably 50% by weight or more, and particularly preferably 70% by weight or more, based on the total amount of polycarbonate polyol and polyol used. When the amount of polycarbonate polyol used is equal to or more than the lower limit mentioned above, the viscosity of the obtained composition is reduced, improving workability, and the mechanical strength, hardness, and abrasion resistance of the obtained cured product tend to be improved, which is preferable.

[0185] Furthermore, the amount of polycarbonate polyol used is preferably 25 mol% or more, more preferably 50 mol% or more, and even more preferably 70 mol% or more, based on the total amount of polycarbonate polyol and polyol used. When the amount of polycarbonate polyol used is equal to or more than the lower limit, the elongation and weather resistance of the obtained cured product tend to be improved, which is preferable.

[0186] Furthermore, when a chain extender is used, the amount of polyol used is preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, and particularly preferably 95 mol% or more, based on the total amount of polycarbonate polyol, polyol and chain extender. If the amount of polyol is equal to or more than the lower limit, the liquid stability tends to be improved, which is preferable.

[0187] In the production of urethane (meth)acrylate oligomers, a solvent can be used to adjust the viscosity. The solvent may be used alone or in combination of two or more. Any known solvent can be used as the solvent. Preferred solvents include toluene, xylene, ethyl acetate, butyl acetate, cyclohexanone, methyl ethyl ketone, and methyl isobutyl ketone. The solvent can usually be used in an amount of less than 300 parts by weight per 100 parts by weight of solids in the reaction system.

[0188] In the production of urethane (meth)acrylate oligomers, the total content of the urethane (meth)acrylate oligomers and their raw material compounds is preferably 20% by weight or more, more preferably 40% by weight or more, based on the total amount of the reaction system. The upper limit of this total content is 100% by weight. If the total content of the urethane (meth)acrylate oligomers and their raw material compounds is 20% by weight or more, the reaction rate is increased, and production efficiency tends to be improved, which is preferable.

[0189] An addition reaction catalyst can be used when producing a urethane (meth)acrylate oligomer. Examples of the addition reaction catalyst include dibutyltin laurate, dibutyltin dioctoate, dioctyltin dilaurate, and dioctyltin dioctoate. The addition reaction catalyst may be used alone or in combination of two or more. Among these, dioctyltin dilaurate is preferred as the addition reaction catalyst from the viewpoints of environmental adaptability, catalytic activity, and storage stability.

[0190] The addition reaction catalyst is used in an amount of usually 1000 ppm by weight, preferably 500 ppm by weight, and usually 10 ppm by weight, preferably 30 ppm by weight, at the upper limit, based on the total content of the urethane (meth)acrylate oligomer produced and its raw material compounds.

[0191] In addition, when the reaction system contains a (meth)acryloyl group during the production of a urethane (meth)acrylate oligomer, a polymerization inhibitor can be used in combination. Examples of such polymerization inhibitors include phenols such as hydroquinone, methylhydroquinone, hydroquinone monoethyl ether, and dibutylhydroxytoluene, amines such as phenothiazine and diphenylamine, copper salts such as copper dibutyldithiocarbamate, manganese salts such as manganese acetate, nitro compounds, and nitroso compounds. The polymerization inhibitor may be used alone or in combination of two or more. Of these, phenols are preferred as the polymerization inhibitor.

[0192] The polymerization inhibitor is used in an amount of usually 3000 ppm by weight, preferably 1000 ppm by weight, and particularly preferably 500 ppm by weight, and usually 50 ppm by weight, preferably 100 ppm by weight, lower limit, based on the total content of the urethane (meth)acrylate oligomer produced and its raw material compounds.

[0193] In the production of urethane (meth)acrylate oligomers, the reaction temperature is usually 20°C or higher, preferably 40°C or higher, and more preferably 60°C or higher. A reaction temperature of 20°C or higher is preferable because the reaction rate is high and the production efficiency tends to improve. The reaction temperature is usually 120°C or lower, preferably 100°C or lower. A reaction temperature of 120°C or lower is preferable because side reactions such as allophanate reaction are less likely to occur. In addition, when a solvent is contained in the reaction system, the reaction temperature is preferably the boiling point of the solvent or lower, and when (meth)acrylate is contained, the reaction temperature is preferably 70°C or lower from the viewpoint of preventing the reaction of (meth)acryloyl groups. The reaction time is usually about 5 to 20 hours.

[0194] The number average molecular weight of the urethane (meth)acrylate oligomer thus obtained is preferably 500 or more, particularly preferably 1000 or more, and preferably 10000 or less, particularly preferably 5000 or less, and particularly preferably 3000 or less. When the number average molecular weight of the urethane (meth)acrylate oligomer is above the above lower limit, the three-dimensional processing suitability of the obtained cured film is good, and the balance between the three-dimensional processing suitability and the contamination resistance tends to be excellent, which is preferable. When the number average molecular weight of the urethane (meth)acrylate oligomer is below the above upper limit, the contamination resistance of the cured film obtained from the composition is good, and the balance between the three-dimensional processing suitability and the contamination resistance tends to be excellent, which is preferable. This is presumably because the three-dimensional processing suitability and the contamination resistance depend on the distance between the crosslinking points in the network structure, and when this distance is long, the structure becomes flexible and easy to stretch, resulting in excellent three-dimensional processing suitability, and when this distance is short, the network structure becomes a strong structure, resulting in excellent contamination resistance.

[0195] <2-20. Polyester elastomer> The polycarbonate polyol of the present invention can be used as a polyester elastomer. A polyester elastomer is a copolymer composed of a hard segment mainly made of an aromatic polyester and a soft segment mainly made of an aliphatic polyether, an aliphatic polyester, or an aliphatic polycarbonate. When the polycarbonate polyol of the present invention is used as a component of the soft segment, the physical properties such as heat resistance and water resistance are superior to those when an aliphatic polyether or an aliphatic polyester is used. In addition, compared with known polycarbonate polyols, it has a melt flow rate suitable for blow molding and extrusion molding when melted, and is a polycarbonate ester elastomer with an excellent balance of mechanical strength and other physical properties, and can be suitably used for various molding materials including fibers, films, and sheets, such as molding materials for elastic threads, boots, gears, tubes, and packings. Specifically, it can be effectively applied to applications such as joint boots for automobiles, home appliance parts, etc., which require heat resistance and durability, and electric wire coating materials.

[0196] <2-21. Active energy radiation curable polymer composition> The active-energy radiation-curable polymer composition containing the above-mentioned urethane (meth)acrylate oligomer (hereinafter, sometimes referred to as "the active-energy radiation-curable polymer composition of the present invention") will be described. The active-energy radiation-curable polymer composition of the present invention preferably has a calculated network crosslinking point molecular weight of 500 to 10,000.

[0197] In this specification, the calculated network crosslinking molecular weight of a composition represents the average value of the molecular weight between active energy ray reactive groups (hereinafter, sometimes referred to as "crosslinking points") that form a network structure in the entire composition. This calculated network crosslinking molecular weight is correlated with the network area when the network structure is formed, and the larger the calculated network crosslinking molecular weight, the smaller the crosslinking density. In the reaction by active energy ray curing, when a compound having only one active energy ray reactive group (hereinafter, sometimes referred to as "monofunctional compound") reacts, a linear polymer is formed, while when a compound having two or more active energy ray reactive groups (hereinafter, sometimes referred to as "polyfunctional compound") reacts, a network structure is formed.

[0198] Therefore, the active energy ray reactive group of the polyfunctional compound is the crosslinking point, and the calculation of the calculated network inter-crosslinking molecular weight is centered on the polyfunctional compound having the crosslinking point, and the monofunctional compound is treated as having the effect of extending the molecular weight between the crosslinking points of the polyfunctional compound, and the calculation of the calculated network inter-crosslinking molecular weight is performed. In addition, the calculation of the calculated network inter-crosslinking molecular weight is performed under the assumption that all active energy ray reactive groups have the same reactivity and all active energy ray reactive groups react by irradiation with active energy rays.

[0199] In a single-composition of a polyfunctional compound in which only one type of polyfunctional compound reacts, the calculated molecular weight between crosslinking points is twice the average molecular weight per active energy ray reactive group possessed by the polyfunctional compound. For example, for a bifunctional compound with a molecular weight of 1,000, it is (1000 / 2) x 2 = 1000, and for a trifunctional compound with a molecular weight of 300, it is (300 / 3) x 2 = 200. In a polyfunctional compound mixed composition in which a plurality of polyfunctional compounds react, the calculated network inter-crosslinking molecular weight of the composition is the average value of the calculated network inter-crosslinking molecular weight of each of the single compounds relative to the total number of active energy ray reactive groups contained in the composition. For example, in a composition consisting of a mixture of 4 moles of a bifunctional compound having a molecular weight of 1,000 and 4 moles of a trifunctional compound having a molecular weight of 300, the total number of active energy ray reactive groups in the composition is 2×4+3×4=20, and the calculated network inter-crosslinking molecular weight of the composition is {(1000 / 2)×8+(300 / 3)×12}×2 / 20=520.

[0200] When the composition contains a monofunctional compound, assuming that the monofunctional compound reacts with the active energy ray reactive group (i.e., crosslinking point) of the polyfunctional compound in equimolar amounts and is located at the center of the molecular chain formed by the monofunctional compound linking to the crosslinking point, the extension of the molecular chain by the monofunctional compound at one crosslinking point is half the value obtained by dividing the total molecular weight of the monofunctional compound by the total number of active energy ray reactive groups of the polyfunctional compound in the composition. Here, since the calculated molecular weight between crosslinking points is considered to be twice the average molecular weight per crosslinking point, the extension by the monofunctional compound relative to the calculated molecular weight between crosslinking points calculated in the polyfunctional compound is the value obtained by dividing the total molecular weight of the monofunctional compound by the total number of active energy ray reactive groups of the polyfunctional compound in the composition.

[0201] For example, in a composition consisting of a mixture of 40 moles of a monofunctional compound having a molecular weight of 100 and 4 moles of a bifunctional compound having a molecular weight of 1,000, the number of active energy ray reactive groups of the polyfunctional compound is 2×4=8, so the extension by the monofunctional compound in the calculated network inter-crosslinking molecular weight is 100×40 / 8=500. That is, the calculated network inter-crosslinking molecular weight of the composition is 1000+500=1500. From the above, the molecular weight W A Monofunctional compound M A Mole and molecular weight W B f B Functional compound M B Mole and molecular weight W C f C Functional compound M CIn the case of a mixture of molar amounts, the calculated network crosslinking molecular weight of the composition can be expressed by the following formula:

[0202]

number

[0203] The calculated network inter-crosslinking molecular weight of the active-energy radiation curable polymer composition of the present invention calculated in this manner is preferably 500 or more, more preferably 800 or more, and even more preferably 1,000 or more, and is preferably 10,000 or less, more preferably 8,000 or less, even more preferably 6,000 or less, even more preferably 4,000 or less, and particularly preferably 3,000 or less.

[0204] When the calculated network crosslinking molecular weight is 10,000 or less, the cured film obtained from the composition has good stain resistance, and tends to have a good balance between three-dimensional processing suitability and stain resistance, which is preferable.In addition, when the calculated network crosslinking molecular weight is 500 or more, the cured film obtained has good three-dimensional processing suitability, and tends to have a good balance between three-dimensional processing suitability and stain resistance, which is preferable.This is presumably because three-dimensional processing suitability and stain resistance depend on the distance between crosslinking points in the network structure, and when this distance is long, the structure becomes flexible and easy to stretch, and the three-dimensional processing suitability is excellent, and when this distance is short, the network structure becomes strong, and the stain resistance is excellent.

[0205] The active energy radiation curable polymer composition of the present invention may further contain other components other than the urethane (meth)acrylate oligomer. Examples of such other components include active energy radiation reactive monomers, active energy radiation curable oligomers, polymerization initiators, photosensitizers, additives, and solvents.

[0206] In the active energy radiation curable polymer composition of the present invention, the content of the urethane (meth)acrylate oligomer is preferably 40% by weight or more, more preferably 60% by weight or more, based on the total amount of the active energy radiation reactive components including the urethane (meth)acrylate oligomer. The upper limit of this content is 100% by weight. When the content of the urethane (meth)acrylate oligomer is 40% by weight or more, the curability is good, and the mechanical strength of the cured product is not too high, and the three-dimensional processing suitability tends to be improved, which is preferable.

[0207] In the active energy radiation curable polymer composition of the present invention, the content of the urethane (meth)acrylate oligomer is preferably high in terms of elongation and film-forming properties, and is preferably low in terms of low viscosity. From this viewpoint, the content of the urethane (meth)acrylate oligomer is preferably 50% by weight or more, more preferably 70% by weight or more, based on the total amount of all components including the active energy radiation reactive component and other components. The upper limit of the content of the urethane (meth)acrylate oligomer is 100% by weight, and the content is preferably less than this.

[0208] In the active energy radiation curable polymer composition of the present invention, the total content of the active energy radiation reactive components including the urethane (meth)acrylate oligomer is preferably 60% by weight or more, more preferably 80% by weight or more, even more preferably 90% by weight or more, and particularly preferably 95% by weight or more, based on the total amount of the composition, from the viewpoints of excellent curing speed and surface curing properties as a composition, no tackiness remaining, etc. The upper limit of this content is 100% by weight.

[0209] As the active energy ray reactive monomer, any known active energy ray reactive monomer can be used. These active energy ray reactive monomers are used for the purpose of adjusting the hydrophilicity or hydrophobicity of the urethane (meth)acrylate oligomer, or the physical properties such as hardness and elongation of the cured product when the obtained composition is cured. The active energy ray reactive monomers may be used alone or in combination of two or more.

[0210] Examples of such active energy ray reactive monomers include vinyl ethers, (meth)acrylamides, and (meth)acrylates. Specific examples of such active energy ray reactive monomers include aromatic vinyl monomers such as styrene, α-methylstyrene, α-chlorostyrene, vinyl toluene, and divinylbenzene; vinyl ester monomers such as vinyl acetate, vinyl butyrate, N-vinylformamide, N-vinylacetamide, N-vinyl-2-pyrrolidone, N-vinylcaprolactam, and divinyl adipate; vinyl ethers such as ethyl vinyl ether and phenyl vinyl ether; allyl compounds such as diallyl phthalate, trimethylolpropane diallyl ether, and allyl glycidyl ether; (meth)acrylamide, N,N-dimethylacrylamide, N,(Meth)acrylamides such as N-dimethyl methacrylamide, N-methylol (meth)acrylamide, N-methoxymethyl (meth)acrylamide, N-butoxymethyl (meth)acrylamide, Nt-butyl (meth)acrylamide, (meth)acryloylmorpholine, and methylene bis (meth)acrylamide; (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, and t-butyl (meth)acrylate; Butyl, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, morpholyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, glycidyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, benzyl (meth)acrylate monofunctional (meth)acrylates such as cyclohexyl (meth)acrylate, phenoxyethyl (meth)acrylate, tricyclodecane (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, allyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, isobornyl (meth)acrylate, and phenyl (meth)acrylate; and ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, and the like. , triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate (n=5-14), propylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetrapropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate (n=5-14), 1,3-butylene glycol di(meth)acrylate, 1,4-butanediol, polybutylene glycol di(meth)acrylate (n=3-16), poly(1-methylbutylene glycol) di(meth)acrylate (n=5-20), 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, neopentyl glycol hydroxypivalate di(meth)acrylate, dicyclopentanediol di(meth)acrylate, tricyclodecane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, Examples of polyfunctional (meth)acrylates include pantrioxyethyl (meth)acrylate, trimethylolpropane trioxypropyl (meth)acrylate, trimethylolpropane polyoxyethyl (meth)acrylate, trimethylolpropane polyoxypropyl (meth)acrylate, tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate, tris(2-hydroxyethyl)isocyanurate di(meth)acrylate, ethylene oxide-added bisphenol A di(meth)acrylate, ethylene oxide-added bisphenol F di(meth)acrylate, propylene oxide-added bisphenol A di(meth)acrylate, propylene oxide-added bisphenol F di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, bisphenol A epoxy di(meth)acrylate, and bisphenol F epoxy di(meth)acrylate.

[0211] Among these, in particular, for applications requiring coatability, monofunctional (meth)acrylates having a ring structure in the molecule, such as (meth)acryloylmorpholine, tetrahydrofurfuryl (meth)acrylate, benzyl (meth)acrylate, cyclohexyl (meth)acrylate, trimethylcyclohexyl (meth)acrylate, phenoxyethyl (meth)acrylate, tricyclodecane (meth)acrylate, dicyclopentenyl (meth)acrylate, isobornyl (meth)acrylate, and (meth)acrylamide, are preferred. On the other hand, for applications requiring mechanical strength of the resulting cured product, di(meth)acrylates are preferred. Preferred are polyfunctional (meth)acrylates such as 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, tricyclodecane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.

[0212] In the active-energy radiation curable polymer composition of the present invention, the content of the active-energy radiation reactive monomer is, from the viewpoint of adjusting the viscosity of the composition and adjusting the physical properties such as hardness and elongation of the obtained cured product, preferably 50% by weight or less, more preferably 30% by weight or less, even more preferably 20% by weight or less, and particularly preferably 10% by weight or less, based on the total amount of the composition.

[0213] The active energy ray curable oligomer may be used alone or in combination of two or more. Examples of the active energy ray curable oligomer include epoxy (meth)acrylate oligomers and acrylic (meth)acrylate oligomers.

[0214] In the active-energy radiation curable polymer composition of the present invention, the content of the active-energy radiation reactive oligomer is preferably 50% by weight or less, more preferably 30% by weight or less, even more preferably 20% by weight or less, and particularly preferably 10% by weight or less, based on the total amount of the composition, from the viewpoint of adjusting physical properties such as hardness and elongation of the obtained cured product.

[0215] The polymerization initiator is mainly used for the purpose of improving the initiation efficiency of a polymerization reaction that proceeds by irradiation with active energy rays such as ultraviolet rays and electron beams. As the polymerization initiator, a photoradical polymerization initiator, which is a compound having a property of generating radicals by light, is generally used, and any known photoradical polymerization initiator can be used. The polymerization initiator may be used alone or in combination of two or more kinds. Furthermore, the photoradical polymerization initiator may be used in combination with a photosensitizer.

[0216] Examples of the photoradical polymerization initiator include benzophenone, 2,4,6-trimethylbenzophenone, 4,4-bis(diethylamino)benzophenone, 4-phenylbenzophenone, methyl orthobenzoyl benzoate, thioxanthone, diethylthioxanthone, isopropylthioxanthone, chlorothioxanthone, 2-ethylanthraquinone, t-butylanthraquinone, diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, benzyl dimethyl ketal, 1-hydroxycyclohexyl phenyl ketone, benzoin methyl ether, benzoin ethyl ether, and benzoin isopropyl. ether, benzoin isobutyl ether, methyl benzoyl formate, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2,6-dimethylbenzoyldiphenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, and 2-hydroxy-1-[4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]-phenyl]-2-methyl-propan-1-one.

[0217] Among these, benzophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and 2-hydroxy-1-[4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]-phenyl]-2-methyl-propan-1-one are preferred, and 1-hydroxycyclohexyl phenyl ketone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and 2-hydroxy-1-[4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]-phenyl]-2-methyl-propan-1-one are more preferred, because they have a fast curing rate and can sufficiently increase the crosslink density.

[0218] In addition, when the active energy radiation curable polymer composition contains a compound having a cationic polymerizable group such as an epoxy group together with a radical polymerizable group, the composition may contain a cationic photopolymerization initiator together with the above-mentioned radical photopolymerization initiator as a polymerization initiator. Any known cationic photopolymerization initiator may be used.

[0219] The content of these polymerization initiators in the active energy radiation curable polymer composition of the present invention is preferably 10 parts by weight or less, more preferably 5 parts by weight or less, relative to 100 parts by weight of the total of the active energy radiation reactive components. When the content of the polymerization initiator is 10 parts by weight or less, it is preferable because a decrease in mechanical strength due to initiator decomposition products is unlikely to occur.

[0220] The photosensitizer can be used for the same purpose as the polymerization initiator. The photosensitizer may be used alone or in combination of two or more. Any known photosensitizer can be used as the photosensitizer as long as the effects of the present invention can be obtained. Examples of such photosensitizers include ethanolamine, diethanolamine, triethanolamine, N-methyldiethanolamine, methyl 4-dimethylaminobenzoate, ethyl 4-dimethylaminobenzoate, amyl 4-dimethylaminobenzoate, and 4-dimethylaminoacetophenone.

[0221] In the active energy radiation curable polymer composition of the present invention, the content of the photosensitizer is preferably 10 parts by weight or less, more preferably 5 parts by weight or less, based on 100 parts by weight of the total of the active energy radiation reactive components. When the content of the photosensitizer is 10 parts by weight or less, it is preferable because a decrease in mechanical strength due to a decrease in crosslink density is unlikely to occur.

[0222] The additives are optional, and various materials added to compositions used for similar applications can be used as additives. The additives may be used alone or in combination of two or more. Examples of such additives include fillers such as glass fiber, glass beads, silica, alumina, calcium carbonate, mica, zinc oxide, titanium oxide, mica, talc, kaolin, metal oxides, metal fibers, iron, lead, and metal powder; carbon materials such as carbon fiber, carbon black, graphite, carbon nanotubes, and fullerenes such as C60 (fillers and carbon materials are sometimes collectively referred to as "inorganic components"); antioxidants, heat stabilizers, ultraviolet absorbers, Modifiers such as HALS (hindered amine light stabilizers), anti-fingerprint agents, surface hydrophilizing agents, antistatic agents, slippage-imparting agents, plasticizers, release agents, defoamers, leveling agents, anti-settling agents, surfactants, thixotropy-imparting agents, lubricants, flame retardants, flame retardant assistants, polymerization inhibitors, fillers, and silane coupling agents; colorants such as pigments, dyes, and hue adjusters; and curing agents, catalysts, and curing accelerators necessary for the synthesis of monomers and / or oligomers thereof, or inorganic components.

[0223] In the active energy radiation curable polymer composition of the present invention, the content of the additive is preferably 10 parts by weight or less, more preferably 5 parts by weight or less, based on 100 parts by weight of the total of the active energy radiation reactive components. When the content of the additive is 10 parts by weight or less, it is preferable because a decrease in mechanical strength due to a decrease in crosslink density is unlikely to occur.

[0224] The solvent can be used for the purpose of adjusting the viscosity of the active-energy radiation curable polymer composition of the present invention, for example, according to the coating method for forming a coating film of the active-energy radiation curable polymer composition of the present invention. The solvent may be used alone or in combination of two or more. Any known solvent can be used as the solvent as long as the effects of the present invention can be obtained. Preferred solvents include toluene, xylene, ethyl acetate, butyl acetate, isopropanol, isobutanol, cyclohexanone, methyl ethyl ketone, and methyl isobutyl ketone. The solvent can usually be used in an amount of less than 200 parts by weight per 100 parts by weight of the solid content of the active-energy radiation curable polymer composition.

[0225] The method for incorporating optional components such as the additives described above into the active-energy radiation curable polymer composition of the present invention is not particularly limited, and examples thereof include conventionally known mixing and dispersing methods. In order to disperse the optional components more reliably, it is preferable to carry out a dispersion treatment using a dispersing machine. Specifically, examples of the method include a method using a two-roll mill, a three-roll mill, a bead mill, a ball mill, a sand mill, a pebble mill, a tron ​​mill, a sand grinder, a segmented barrier lighter, a planetary stirrer, a high-speed impeller dispersing machine, a high-speed stone mill, a high-speed impact mill, a kneader, a homogenizer, an ultrasonic dispersing machine, etc.

[0226] The viscosity of the active-energy radiation curable polymer composition of the present invention can be appropriately adjusted depending on the application and mode of use of the composition, but from the viewpoints of handling, coatability, moldability, three-dimensional modeling, etc., the viscosity at 25°C measured with an E-type viscometer (rotor 1°34'×R24) is preferably 10 mPa·s or more, more preferably 100 mPa·s or more, and on the other hand, is preferably 100,000 mPa·s or less, more preferably 50,000 mPa·s or less. The viscosity of the active-energy radiation curable polymer composition can be adjusted, for example, by the content of the urethane (meth)acrylate oligomer described above, the type of the optional component described above, the blending ratio thereof, etc.

[0227] As a method for applying the active-energy radiation curable polymer composition of the present invention, known methods such as a bar coater method, an applicator method, a curtain flow coater method, a roll coater method, a spray method, a gravure coater method, a comma coater method, a reverse roll coater method, a lip coater method, a die coater method, a slot die coater method, an air knife coater method, and a dip coater method can be applied, and among these, the bar coater method and the gravure coater method are preferred.

[0228] <2-22. Cured films and laminates> The active energy radiation curable polymer composition of the present invention can be formed into a cured film by irradiating it with active energy rays. The active energy rays used when curing the composition may include infrared rays, visible light, ultraviolet rays, X-rays, electron beams, α rays, β rays, γ rays, etc. From the viewpoint of equipment cost and productivity, it is preferable to use electron beams or ultraviolet rays, and suitable light sources include electron beam irradiation devices, ultra-high pressure mercury lamps, high pressure mercury lamps, medium pressure mercury lamps, low pressure mercury lamps, metal halide lamps, Ar lasers, He-Cd lasers, solid-state lasers, xenon lamps, high frequency induction mercury lamps, sunlight, etc.

[0229] The amount of irradiation of active energy rays can be appropriately selected depending on the type of active energy rays. For example, when curing is performed by irradiation with electron beams, the amount of irradiation is preferably 1 to 10 Mrad. In addition, in the case of irradiation with ultraviolet rays, the amount of irradiation is preferably 50 to 1,000 mJ / cm. 2 The atmosphere during curing may be air or an inert gas such as nitrogen or argon. Also, irradiation may be performed in a closed space between the film or glass and the metal mold.

[0230] The thickness of the cured film is appropriately determined according to the intended use, but the lower limit is preferably 1 μm, more preferably 3 μm, and particularly preferably 5 μm. The upper limit is preferably 200 μm, more preferably 100 μm, and particularly preferably 50 μm. If the film thickness is 1 μm or more, the appearance of design and functionality after three-dimensional processing is good, while if it is 200 μm or less, it is preferable because the internal curing property and three-dimensional processing suitability are good. In addition, when used in industry, the lower limit of the film thickness of the cured film is preferably 1 μm, and the upper limit is preferably 100 μm, more preferably 50 μm, particularly preferably 20 μm, and most preferably 10 μm.

[0231] A laminate having a layer of the above-mentioned cured film on a substrate can be obtained. This laminate is not particularly limited as long as it has a layer of the cured film, and layers other than the substrate and the cured film may be between the substrate and the cured film, or may be on the outside. In addition, the laminate may have multiple layers of substrates and cured films.

[0232] As a method for obtaining a laminate having a multi-layered cured film, known methods such as a method of laminating all layers in an uncured state and then curing with active energy rays, a method of curing or semi-curing a lower layer with active energy rays and then coating an upper layer and curing it again with active energy rays, a method of coating each layer on a release film or base film and then laminating the layers together in an uncured or semi-cured state, etc. are applicable, but from the viewpoint of increasing the adhesion between layers, a method of laminating in an uncured state and then curing with active energy rays is preferred. As a method for laminating in an uncured state, known methods such as sequential coating in which a lower layer is coated and then an upper layer is coated in layers, and simultaneous multi-layer coating in which two or more layers are coated in layers at the same time from multiple slits can be applied, but are not limited thereto.

[0233] Examples of the substrate include articles of various shapes, such as plates made of polyesters, such as polyethylene terephthalate and polybutylene terephthalate; polyolefins, such as polypropylene and polyethylene; various plastics, such as nylon, polycarbonate, and (meth)acrylic resin; or metals. The cured film can be made to have excellent hardness and stain resistance against common household stains such as ink and ethanol, and laminates using the cured film as a coating for various substrates can have excellent design properties and surface protection properties.

[0234] In addition, the active-energy radiation curable polymer composition of the present invention can provide a cured film having flexibility capable of responding to deformation during three-dimensional processing, breaking elongation, mechanical strength, contamination resistance, and hardness at the same time, when the calculated network inter-crosslinking molecular weight is taken into consideration. In addition, the active-energy radiation curable polymer composition of the present invention is expected to enable the easy production of a thin-film resin sheet by one-layer coating.

[0235] The breaking elongation of the cured film is preferably 50% or more, more preferably 75% or more, even more preferably 100% or more, and particularly preferably 120% or more, as measured by cutting the cured film into a width of 10 mm and conducting a tensile test using a Tensilon tensile tester (Tensilon UTM-III-100, manufactured by Orientec Co., Ltd.) under conditions of a temperature of 23°C, a tensile speed of 50 mm / min, and a chuck distance of 50 mm.

[0236] The above-mentioned cured films and laminates can be used as alternative films to paint, and can be effectively applied to, for example, interior and exterior building materials, various components of automobiles, home appliances, and the like. EXAMPLES

[0237] The present invention will be described in more detail below with reference to examples and comparative examples. However, the present invention is not limited to these examples as long as the gist of the present invention is not exceeded.

[0238] [Evaluation method] The conditions for the polycondensation step and the methods for evaluating the resulting polycarbonate polyols and polyurethanes in the following examples and comparative examples are as follows.

[0239] [Polycondensation step] <Amount of dioxane generated> The polycarbonate polyol-containing composition produced in the polycondensation reaction and the distillate were analyzed by gas chromatography (GC) to determine their quantities, and the proportions (wt %) of the amounts relative to the charged diethylene glycol were calculated.

[0240] [Evaluation of polycarbonate polyol] <Quantitative analysis of carbonate end content, diol, branched alcohol content and phenol content> Polycarbonate polyol was dissolved in CDCl3 and 400MHz 1 H-NMR (AL-400 manufactured by JEOL Ltd.) was measured, and the amount of carbonate terminals such as phenoxy groups, diols, branched alcohols, and phenols were identified from the signal positions of each component, and the content of each was calculated from the integral value. The detection limit at this time was 100 ppm as the weight of phenol relative to the weight of the entire sample, and 0.1 wt% for dihydroxy compounds such as the compound represented by formula (A) and the compound represented by formula (B). The ratio of the amount of carbonate terminals such as phenoxy groups was determined from the ratio of the integral value of one proton of the amount of carbonate terminals such as phenoxy groups to the integral value of one proton of the entire terminals, and the detection limit of carbonate terminals such as phenoxy groups was 0.1 mol% relative to the entire terminals. When diethyl carbonate was used, the ethoxy group (EtO-) and the hydroxyethoxy group (HOCH2CH2O-) were calculated in the same manner when diethyl carbonate was used, and when ethylene carbonate was used, the hydroxyethoxy group (HOCH2CH2O-) were calculated in the same manner.

[0241] <Content (wt%) of oxyalkylene glycol (A1)> The content (wt %) of the oxyalkylene glycol (A1) in the diol (A) can be determined as follows by carrying out GC analysis after hydrolysis of the polycarbonate polyol. 0.5 g of polycarbonate polyol was precisely weighed and placed into a 100 mL Erlenmeyer flask. 5 mL of tetrahydrofuran was added and dissolved. Next, 45 mL of methanol and 5 mL of 25 wt% aqueous sodium hydroxide solution were added. A condenser was set on the 100 mL Erlenmeyer flask, and it was heated in a water bath at 75 - 80 °C for 30 minutes to perform hydrolysis. After cooling to room temperature, 5 mL of 6N hydrochloric acid was added to neutralize sodium hydroxide and adjust the pH to 2 - 4. The total volume was transferred to a 100 mL volumetric flask, and the inside of the Erlenmeyer flask was washed twice with an appropriate amount of methanol. The washing solution was also transferred to the 100 mL volumetric flask. After adding an appropriate amount of methanol to make it 100 mL, the liquid was mixed in the volumetric flask. The supernatant was collected, filtered through a filter, and then analyzed by GC. The concentration of each diol contained in diol (A) was determined by creating a calibration curve from a standard substance and calculating the weight percentage from the area ratio obtained by GC.

[0242] <Molar ratio of the structural unit derived from oxyalkylene glycol (A1) and the structural unit derived from branched alcohol (B)> The polycarbonate polyol was dissolved in CDCl3, and 400 MHz, 1 1H-NMR (AL-400 manufactured by JEOL Ltd.) was measured, and from the signal positions of each component, the molar ratio of the structural unit derived from oxyalkylene glycol (A1) and the structural unit derived from branched alcohol (B) was determined. Also, the molar ratio of the terminal derived from oxyalkylene glycol (A1) and the terminal derived from branched alcohol (B) was determined in the same manner.

[0243] <Hydroxyl value> In accordance with JIS K1557-1, the hydroxyl value of the polycarbonate polyol was measured by a method using an acetylating reagent.

[0244] <Measurement of APHA value> In accordance with JIS K0071-1 (1998), it was measured by comparing with a standard solution prepared by putting the polycarbonate polyol in a colorimetric tube. As the reagent, a chromaticity standard solution of 1000 degrees (1 mg Pt / mL) (Kishida Chemical) was used.

[0245] [Evaluation of polyurethane] <Solvent resistance> The polyurethane solution was applied to a fluororesin sheet (fluoro tape Nitoflon 900, thickness 0.1 mm, manufactured by Nitto Denko Corporation) with a 9.5 mil applicator, and dried in the following order: 5 hours at 50 ° C, 0.5 hours at 100 ° C, 0.5 hours at 100 ° C under vacuum conditions, and 15 hours at 80 ° C. Test pieces of 3 cm × 3 cm were cut out from the obtained polyurethane film, and placed in a glass petri dish with an inner diameter of 10 cm φ containing 50 mL of each test solvent, and the weights of the test pieces were measured after immersion at the following temperatures for the following times for each test solvent, and the weight change rate (%) between the weight of the test piece before immersion and the weight of the test piece after immersion (= (weight of the test piece after immersion - weight of the test piece before immersion) / weight of the test piece before immersion × 100) was calculated. Here, the closer the weight change rate is to 0%, the better the oleic acid resistance is. Oleic acid resistance: The test piece was immersed in oleic acid at 80°C for 16 hours. Resistance to ethyl acetate: A test piece was immersed in ethyl acetate at room temperature for 20 minutes. Ethanol resistance: The test piece was immersed in ethanol at room temperature for 1 hour.

[0246] <Room temperature tensile test> According to JIS K6301, a polyurethane test piece in the shape of a strip with a width of 10 mm, a length of 100 mm, and a thickness of about 50 μm was subjected to a tensile test using a tensile tester (manufactured by Orientec Co., Ltd., product name "Tensilon UTM-III-100") at a chuck distance of 50 mm, a tensile speed of 500 mm / min, and a temperature of 23°C (relative humidity of 55%), and the stress at each elongation until the test piece broke was measured. The stress at 100% and 300% elongation is defined as 100% modulus (100%M) and 300% modulus (300%M).

[0247] [Raw materials used] The raw materials used in the production of polycarbonate polyol (hereinafter sometimes abbreviated as PCP) and polyurethane are as follows. Diethylene glycol (hereinafter sometimes abbreviated as DEG): Manufactured by Mitsubishi Chemical Corporation Triethylene glycol (hereinafter sometimes abbreviated as TEG): Manufactured by Mitsubishi Chemical Corporation Trimethylolpropane (hereinafter sometimes abbreviated as TMP): Manufactured by Mitsubishi Gas Chemical Company, Inc. 1,6-Hexanediol (hereinafter sometimes abbreviated as 16HD): BASF Diphenyl carbonate (hereinafter sometimes abbreviated as DPC): Manufactured by Mitsubishi Chemical Corporation Diethyl carbonate (hereinafter sometimes abbreviated as DEC): Manufactured by Wako Pure Chemical Industries, Ltd. Ethylene carbonate (hereinafter sometimes abbreviated as EC): Manufactured by Mitsubishi Chemical Corporation Magnesium acetate tetrahydrate (hereinafter sometimes abbreviated as Mg(OAc)): Manufactured by Wako Pure Chemical Industries, Ltd. Titanium tetrabutoxide (hereinafter sometimes abbreviated as Ti(OBu)): manufactured by Wako Pure Chemical Industries, Ltd. Sodium ethoxide (hereinafter sometimes abbreviated as NaOEt): Manufactured by Wako Pure Chemical Industries, Ltd. 1,4-Butanediol: Mitsubishi Chemical Corporation Diphenylmethane diisocyanate (hereinafter sometimes abbreviated as MDI): Manufactured by Nippon Polyurethane Industry Co., Ltd. Urethane catalyst Neostan U-830: manufactured by Nitto Kasei Co., Ltd. Dehydrated N,N-dimethylformamide: Wako Pure Chemical Industries, Ltd.

[0248] [Production and Evaluation of Polycarbonate Polyol] <Example I-1> A 1L glass separable flask equipped with a stirrer, a distillate trap, and a pressure regulator was charged with 231.8g of diethylene glycol (DEG), 219.6g of triethylene glycol (TEG), 7.5g of trimethylolpropane (TMP), 741.2g of diphenyl carbonate (DPC), and 1.9mL of magnesium acetate tetrahydrate aqueous solution (concentration: 8.4g / L), and substituted with nitrogen gas. The internal temperature was raised to 160°C under stirring, and the contents were heated and dissolved. After that, the pressure was lowered to 24kPa over 2 minutes, and the reaction was carried out for 90 minutes while removing phenol from the system. Next, the pressure was lowered to 9.3kPa over 90 minutes, and further lowered to 0.7kPa over 30 minutes to continue the reaction, and the temperature was raised to 170°C, and the reaction was carried out for 15 hours (total 18.5 hours) while removing phenol and unreacted dihydroxy compounds from the system. Thereafter, 0.45 mL of a 0.85% aqueous phosphoric acid solution was added to deactivate the catalyst, thereby obtaining a polycarbonate polyol-containing composition. The distillate was trapped, and the amount of dioxane contained in the polycarbonate polyol-containing composition was quantified using GC.

[0249] The obtained polycarbonate polyol-containing composition was sent to a thin-film distillation apparatus at a flow rate of 20 g / min, and thin-film distillation (temperature: 200° C., pressure: 53 to 67 Pa) was carried out. The thin-film distillation apparatus had a diameter of 50 mm, a height of 200 mm, and an area of ​​0.0314 m 2 The molecular distillation apparatus used was a special MS-300 model manufactured by Shibata Scientific Co., Ltd., equipped with an internal condenser and a jacket. The properties and evaluation results of the physical properties of the polycarbonate polyol obtained by thin-film distillation are shown in Tables 1A and 1B together with the production conditions.

[0250] <Example I-2> A 5L glass separable flask equipped with a stirrer, a distillate trap, and a pressure regulator was charged with 786.1g of diethylene glycol (DEG), 744.7g of triethylene glycol (TEG), 25.5g of trimethylolpropane (TMP), 2525.0g of diphenyl carbonate (DPC), and 6.3mL of magnesium acetate tetrahydrate aqueous solution (concentration: 8.4g / L), and substituted with nitrogen gas. The internal temperature was raised to 160°C under stirring, and the contents were heated and dissolved. After that, the pressure was lowered to 24kPa over 2 minutes, and the reaction was carried out for 90 minutes while removing phenol from the system. Next, the pressure was lowered to 9.3kPa over 90 minutes, and further lowered to 0.7kPa over 30 minutes to continue the reaction, and the temperature was raised to 170°C, and the reaction was carried out for 2 hours (total 5.5 hours) while removing phenol and unreacted dihydroxy compounds from the system, to obtain a polycarbonate polyol-containing composition. 1.4 mL of 0.85% phosphoric acid aqueous solution was added to deactivate the catalyst, and a polycarbonate polyol-containing composition was obtained. The distillate was trapped, and the amount of dioxane contained in the polycarbonate polyol-containing composition was quantified using GC. Then, thin-film distillation was performed in the same manner as in Example 1. The properties and evaluation results of the physical properties of the obtained polycarbonate polyol are shown in Tables 1A and 1B together with the production conditions.

[0251] <Example I-3> A 5L glass separable flask equipped with a stirrer, a distillate trap, and a pressure regulator was charged with 1081.3g of diethylene glycol (DEG), 383.5g of triethylene glycol (TEG), 47.5g of trimethylolpropane (TMP), 2687.8g of diphenyl carbonate (DPC), and 6.7mL of magnesium acetate tetrahydrate aqueous solution (concentration: 8.4g / L), and substituted with nitrogen gas. The internal temperature was raised to 160°C under stirring, and the contents were heated and dissolved. After that, the pressure was lowered to 24kPa over 2 minutes, and the reaction was carried out for 90 minutes while removing phenol from the system. Next, the pressure was lowered to 9.3kPa over 90 minutes, and further lowered to 0.7kPa over 30 minutes to continue the reaction, and the temperature was raised to 170°C, and the reaction was carried out for 2 hours (total 5.5 hours) while removing phenol and unreacted dihydroxy compounds from the system, to obtain a polycarbonate polyol-containing composition. 1.4 mL of 0.85% phosphoric acid aqueous solution was added to deactivate the catalyst, and a polycarbonate polyol-containing composition was obtained. The distillate was trapped, and the amount of dioxane contained in the polycarbonate polyol-containing composition was quantified using GC. Then, thin-film distillation was performed in the same manner as in Example 1. The properties and evaluation results of the physical properties of the obtained polycarbonate polyol are shown in Tables 1A and 1B together with the production conditions.

[0252] <Example I-4> A 5L glass separable flask equipped with a stirrer, a distillate trap, and a pressure regulator was charged with 490.2g of diethylene glycol (DEG), 462.4g of triethylene glycol (TEG), 1547.4g of diphenyl carbonate (DPC), and 4.3mL of magnesium acetate tetrahydrate aqueous solution (concentration: 8.4g / L), and substituted with nitrogen gas. The internal temperature was raised to 160°C under stirring, and the contents were heated and dissolved. After that, the pressure was lowered to 24kPa over 2 minutes, and the reaction was carried out for 90 minutes while removing phenol from the system. Next, the pressure was lowered to 9.3kPa over 90 minutes, and further lowered to 0.7kPa over 30 minutes to continue the reaction, and the temperature was raised to 170°C, and the reaction was carried out for 2 hours (total 5.5 hours) while removing phenol and unreacted dihydroxy compounds from the system, to obtain a polycarbonate polyol-containing composition. 1.1 mL of 0.85% phosphoric acid aqueous solution was added to deactivate the catalyst, and a polycarbonate polyol-containing composition was obtained. The distillate was trapped, and the amount of dioxane contained in the polycarbonate polyol-containing composition was quantified using GC. Then, thin-film distillation was performed in the same manner as in Example 1. The properties and evaluation results of the physical properties of the obtained polycarbonate polyol are shown in Tables 1A and 1B together with the production conditions.

[0253] <Example I-5> Diethylene glycol (DEG): 166.8g, trimethylolpropane (TMP): 3.2g, diphenyl carbonate (DPC): 330.0g, magnesium acetate tetrahydrate aqueous solution: 0.8mL (concentration: 8.4g / L) were placed in a 1L glass separable flask equipped with a stirrer, a distillate trap, and a pressure regulator, and the atmosphere was replaced with nitrogen gas. The internal temperature was raised to 160°C while stirring, and the contents were heated and dissolved. After that, the pressure was lowered to 24kPa over 2 minutes, and the reaction was carried out for 90 minutes while removing phenol from the system. Next, the pressure was reduced to 9.3 kPa over 90 minutes, and then further reduced to 0.7 kPa over 30 minutes to continue the reaction, after which the temperature was raised to 170°C and the reaction was continued for 2 hours (total 5.5 hours) while removing phenol and unreacted dihydroxy compounds from the system, and then 0.45 mL of 0.85% phosphoric acid aqueous solution was added to deactivate the catalyst, to obtain a polycarbonate polyol-containing composition. The distillate was trapped, and the amount of dioxane contained in the polycarbonate polyol-containing composition was quantified using GC. The properties and evaluation results of the physical properties of the obtained polycarbonate polyol are shown in Tables 1A and 1B together with the production conditions.

[0254] <Example I-6> A 5L glass separable flask equipped with a stirrer, a distillate trap, and a pressure regulator was charged with 753.0g of diethylene glycol (DEG), 462.2g of 1,6-hexanediol (16HD), 22.5g of trimethylolpropane (TMP), 2262.3g of diphenyl carbonate (DPC), and 5.7mL of magnesium acetate tetrahydrate aqueous solution (concentration: 8.4g / L), and the atmosphere was replaced with nitrogen gas. The internal temperature was raised to 160°C while stirring, and the contents were heated and dissolved. After that, the pressure was lowered to 24kPa over 2 minutes, and the reaction was carried out for 90 minutes while removing phenol from the system. Next, the pressure was reduced to 9.3 kPa over 90 minutes, and then further reduced to 0.7 kPa over 30 minutes to continue the reaction, and the temperature was raised to 170°C to react for 2 hours (total 5.5 hours) while removing phenol and unreacted dihydroxy compounds from the system, and then 1.1 mL of 0.85% phosphoric acid aqueous solution was added to deactivate the catalyst, and a polycarbonate polyol-containing composition was obtained. The distillate trap and the amount of dioxane contained in the polycarbonate polyol-containing composition were quantified using GC. Then, thin film distillation was performed in the same manner as in Example 1. The properties and evaluation results of the physical properties of the obtained polycarbonate polyol are shown in Tables 1A and 1B together with the production conditions.

[0255] <Comparative example I-1> Diethylene glycol (DEG): 231.7g, triethylene glycol (TEG): 202.5g, trimethylolpropane (TMP): 6.9g, diethyl carbonate (DEC): 577.9g, titanium tetrabutoxide: 0.23g were placed in a 1L glass separable flask equipped with a stirrer, a packed distillation column, a distillate trap, and a pressure regulator, and the atmosphere was replaced with nitrogen gas. The internal temperature was raised to 100°C under stirring, and the contents were heated and dissolved. Thereafter, the reaction was carried out for 20 hours under normal pressure conditions at an internal temperature of 100 to 130°C while removing ethanol and diethyl carbonate (DEC) from the system. Next, the pressure was reduced to 9.3kPa over 240 minutes, and the reaction was carried out at 160°C for another 10 hours. The pressure was further reduced to 5.0 kPa over 60 minutes to continue the reaction, and then the temperature was raised to 170°C and the reaction was continued for 10 hours (total 45 hours) while removing ethanol and unreacted dihydroxy compound from the system, to obtain a polycarbonate polyol-containing composition. The distillate was trapped and the amount of dioxane contained in the polycarbonate polyol-containing composition was quantified using GC. The properties and evaluation results of the physical properties of the obtained polycarbonate polyol are shown in Tables 2A and 2B together with the production conditions.

[0256] <Comparative example I-2> Diethylene glycol (DEG): 231.7g, triethylene glycol (TEG): 202.5g, trimethylolpropane (TMP): 6.9g, diethyl carbonate (DEC): 577.9g, sodium ethoxide: 0.19g were placed in a 1L glass separable flask equipped with a stirrer, a packed distillation column, a distillate trap, and a pressure regulator, and the contents were replaced with nitrogen gas. The internal temperature was raised to 100°C under stirring, and the contents were heated and dissolved. Thereafter, the reaction was carried out for 20 hours under normal pressure conditions at an internal temperature of 100 to 130°C while removing ethanol and diethyl carbonate (DEC) from the system. Next, the pressure was reduced to 9.3kPa over 240 minutes, and the reaction was carried out at 160°C for another 10 hours. The pressure was further reduced to 5.0 kPa over 60 minutes to continue the reaction, and then the temperature was raised to 170°C and the reaction was continued for 10 hours (total 45 hours) while removing ethanol and unreacted dihydroxy compound from the system, to obtain a polycarbonate polyol-containing composition. The distillate was trapped and the amount of dioxane contained in the polycarbonate polyol-containing composition was quantified using GC. The properties and evaluation results of the physical properties of the obtained polycarbonate polyol are shown in Tables 2A and 2B together with the production conditions.

[0257] <Comparative example I-3> A 1L glass separable flask equipped with a stirrer, a packed distillation column, a distillate trap, and a pressure regulator was charged with 231.7g of diethylene glycol (DEG), 202.5g of triethylene glycol (TEG), 6.9g of trimethylolpropane (TMP), 376.9g of ethylene carbonate (EC), and 1.0g of titanium tetrabutoxide, and the flask was purged with nitrogen gas. The internal temperature was raised to 160°C under stirring, and the contents were dissolved by heating. After that, the flask was heated at an internal temperature of 160°C for 3 hours under normal pressure conditions, and then the pressure was reduced to 10 kPa, and the mixture was reacted for 20 hours while removing ethylene glycol and ethylene carbonate from the system. The pressure was then reduced to 5.0 kPa over 60 minutes, and the mixture was further reacted at 160°C for 10 hours. The pressure was further reduced to 2.0 kPa over 60 minutes to continue the reaction, and then the temperature was raised to 170°C and the reaction was continued for 10 hours while removing ethanol and unreacted dihydroxy compounds from the system, to obtain a polycarbonate polyol-containing composition (45 hours in total). The distillate was trapped and the amount of dioxane contained in the polycarbonate polyol-containing composition was quantified using GC. The properties and physical properties of the obtained polycarbonate polyol are shown in Tables 2A and 2B together with the production conditions.

[0258] <Comparative example I-4> A 1L glass separable flask equipped with a stirrer, a distillate trap, and a pressure regulator was charged with 211.4g of diethylene glycol (DEG), 200.2g of triethylene glycol (TEG), 6.8g of trimethylolpropane (TMP), 690.6g of diphenyl carbonate (DPC), and 1.7mL of magnesium acetate tetrahydrate aqueous solution (concentration: 8.4g / L), and substituted with nitrogen gas. The internal temperature was raised to 160°C under stirring, and the contents were heated and dissolved. After that, the pressure was lowered to 24kPa over 2 minutes, and the reaction was carried out for 90 minutes while removing phenol from the system. Next, the pressure was lowered to 9.3kPa over 90 minutes, and further lowered to 0.7kPa over 30 minutes to continue the reaction, and the temperature was raised to 170°C, and the reaction was carried out for 30 minutes (total 4 hours) while removing phenol and unreacted dihydroxy compounds from the system. Then, 0.45 mL of 0.85% phosphoric acid aqueous solution was added to deactivate the catalyst, and a polycarbonate polyol-containing composition was obtained. The distillate was trapped and the amount of dioxane contained in the polycarbonate polyol-containing composition was quantified using GC. Then, thin-film distillation was performed in the same manner as in Example 1. The evaluation results of the properties and physical properties of the obtained polycarbonate polyol are shown in Tables 2A and 2B together with the production conditions.

[0259] <Comparative example I-5> A 1L glass separable flask equipped with a stirrer, a distillate trap, and a pressure regulator was charged with 231.8g of diethylene glycol (DEG), 219.6g of triethylene glycol (TEG), 7.5g of trimethylolpropane (TMP), 741.2g of diphenyl carbonate (DPC), and 1.9mL of magnesium acetate tetrahydrate aqueous solution (concentration: 8.4g / L), and substituted with nitrogen gas. The internal temperature was raised to 130°C under stirring, and the contents were dissolved by heating. After that, the pressure was lowered to 24kPa over 2 minutes, and the reaction was carried out for 90 minutes while removing phenol from the system. Next, the pressure was lowered to 9.3kPa over 90 minutes, and further lowered to 0.7kPa over 30 minutes to continue the reaction, and the reaction was carried out for 7 hours (total 10.5 hours) while removing phenol and unreacted dihydroxy compounds from the system while maintaining the temperature at 130°C. Thereafter, 0.45 mL of a 0.85% aqueous phosphoric acid solution was added to deactivate the catalyst, thereby obtaining a polycarbonate polyol-containing composition. The distillate was trapped, and the amount of dioxane contained in the polycarbonate polyol-containing composition was quantified using GC. The properties and evaluation results of the physical properties of the obtained polycarbonate polyol are shown in Tables 2A and 2B together with the production conditions.

[0260] [Table 1]

[0261] [Table 2]

[0262] [Production and evaluation of polyurethane] <Example II-1, Comparative Example II-4> Polyurethanes were synthesized using the polycarbonate polyol (Example II-1) prepared in Example I-1 and the polycarbonate polyol (Comparative Example II-4) prepared in Comparative Example I-4 by the following method, and their physical properties were evaluated.

[0263] A thermocouple was installed in a separable flask equipped with a stirrer, and 81.4 g of polycarbonate polyol preheated to 80°C, 2.8 g of 1,4-butanediol, 232.2 g of dehydrated N,N-dimethylformamide, and 22.2 mg of urethane catalyst (Neostan U-830) were placed in the separable flask, which was then immersed in an oil bath set at 55°C, and the contents were stirred at 60 rpm for about 1 hour while heating the inside of the separable flask under a nitrogen atmosphere. After the polycarbonate polyol was dissolved in the solvent, diphenylmethane diisocyanate (MDI) was added in small amounts over 3 hours, and a polyurethane solution was obtained when a total of 15.0 g of MDI was added. A test film was prepared from the obtained polyurethane solution by the above method, and the physical properties were evaluated. The results are shown in Table 3.

[0264] As described above, the smaller the weight change rate in the solvent resistance evaluation, the higher the solvent resistance, which is preferable for the polyurethane. In addition, the smaller the 100%M and 300%M, the higher the flexibility, which is preferable for a polyurethane.In addition, the larger the breaking elongation and breaking strength, the higher the mechanical strength, which is preferable for a polyurethane.

[0265] [Table 3]

[0266] [Consideration] In Examples I-1 to I-6, polycarbonate polyols with low amounts of carbonate terminal groups and with dioxane generation amounts of 0.1% by weight or less could be obtained.

[0267] In Comparative Examples I-1 to I-3, a carbonate source other than diphenyl carbonate was used, so the reaction rate was slow and the reaction was carried out for a long time, resulting in a large amount of carbonate terminals. In addition, a large amount of dioxane was generated. In addition, the APHA value was high, and the polycarbonate polyol was colored. In Comparative Example I-4, the reaction time was short, and therefore the amount of carbonate terminals was large. In Comparative Example I-5, the reaction temperature was low, and therefore the amount of carbonate terminals was large. From the urethane evaluation results of Example II-1 and Comparative Example II-4, it is clear that the polyurethane synthesized from the polycarbonate polyol of Example I-1, which has a small amount of carbonate terminals, is superior in solvent resistance, breaking elongation, and breaking strength, and is also flexible.

Claims

1. A polycarbonate polyol which is a polycondensation reaction product of a polyhydric alcohol and a carbonate compound, The hydroxyl value is 20 mgKOH / g or more and 450 mgKOH / g or less, the terminals derived from the carbonate compound account for 1.0 mol % or less of all terminals, and the Hazen color number value (APHA value: in accordance with JIS K0071-1 (1998)) is 50 or less; the carbonate compound is at least one selected from diphenyl carbonate, diethyl carbonate, dimethyl carbonate, and ethylene carbonate; the polyhydric alcohol comprises a diol (A) and a trihydric to hexahydric branched alcohol (B) having 3 to 12 carbon atoms; A polycarbonate polyol, characterized in that the diol (A) contains an oxyalkylene glycol (A1) represented by the following formula (1), the content of the oxyalkylene glycol (A1) in the diol (A) is 60% by weight or more, and the oxyalkylene glycol (A1) contains diethylene glycol: 【Chemistry 1】 (In formula (1), m represents an integer of 2 to 4, R A represents a carbon chain having 2 to 5 carbon atoms which may contain branches. A may be the same or different.)

2. The polycarbonate polyol according to claim 1, wherein the structural units derived from the branched alcohol (B) in the polycarbonate polyol are 0.005 mol % or more and 5.0 mol % or less with respect to the total structural units derived from the polyhydric alcohol in the polycarbonate polyol.

Citation Information

Patent Citations

  • JP1971-042384B

  • Denjikeidenki

    JP1976011159A

  • Gigh permeability alloy

    JP1979048627A

  • Production of polycarbonate copolyether polyol

    JP1998007788A

  • Crosslinked polycarbonate and its production

    JP1999116668A