Ceramic matrix composite material and its manufacturing method

The method of powder impregnation and film boiling in ceramic matrix composite manufacturing addresses long processing times and residual metal issues, enabling high-density matrix formation with enhanced properties.

JP7582627B2Active Publication Date: 2024-11-13IHI AEROSPACE CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022567007
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-12-04
Filing Date
2021-12-03
Publication Date
2024-11-13
Estimated Expiration
2041-12-03

AI Technical Summary

Technical Problem

Existing methods for manufacturing ceramic matrix composites, such as CVI, PIP, and MI, face issues with long processing times for high-density matrix formation or residual metal causing reduced heat resistance and oxidation resistance.

Method used

A manufacturing method involving powder impregnation of fibrous bodies followed by film boiling to create a high-density matrix, utilizing ceramic material powder to divide pores into smaller sizes for efficient matrix formation.

Benefits of technology

Achieves high-density matrix formation in a short time with improved heat resistance and oxidation resistance by maximizing the film boiling method's effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582627000001
    Figure 0007582627000001
  • Figure 0007582627000002
    Figure 0007582627000002
  • Figure 0007582627000003
    Figure 0007582627000003
Patent Text Reader

Abstract

A method for manufacturing a ceramic-based composite material comprising a matrix and reinforcing fiber provided in the matrix, wherein: a powder of a matrix material forming a part of the matrix is impregnated into a fiber body constituted from the reinforcing fiber, the fiber body impregnated with the powder is positioned in a liquid raw material for the matrix, the fiber body is heated in this state to put the liquid raw material in a membrane boiling state, and a ceramic derived from the liquid raw material is generated in the fiber body as a part of the matrix.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a ceramic matrix composite material and a method for producing the same. [Background technology]

[0002] Ceramic matrix composites are materials that have a matrix of ceramics such as silicon carbide and reinforced fibers within the matrix. They are used as high-temperature structural components in rocket engines, aircraft jet engines, and other applications.

[0003] A matrix is ​​formed on reinforcing fibers (for example, a fibrous body that is a woven or knitted fabric of reinforcing fibers) by a chemical vapor infiltration (CVI) method, a polymer impregnation pyrolysis (PIP) method, a metal melt infiltration (MI) method, etc. The above-mentioned fibrous body is also called a preform.

[0004] In the CVI method, a reactive gas is passed through a heated fibrous body, and the reactants of the reactive gas are precipitated as a matrix in the pores inside the fibrous body. In the PIP method, a polymer such as polycarbosilane is impregnated into the fibrous body, and the impregnated polymer is sintered to form a matrix. In the MI method, a matrix (e.g., a matrix of silicon carbide and silicon metal) is formed by melting and passing a metal component (e.g., silicon metal) into a fibrous body with powder material (e.g., silicon carbide or carbon powder) mixed inside.

[0005] Patent Document 1 and Non-Patent Documents 1 and 2 describe techniques related to some of the embodiments of the present application. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2017-1912 A [Patent Document 2] China Patent Publication CN102795871A [Non-patent literature]

[0007] [Non-Patent Document 1] C. Besnarda et al. “Synthesis of hexacelsian barium aluminosilicate by film boiling chemical vapor process”, Journal of the European Ceramic Society 40 (2020) 3494-3497 [Non-Patent Document 2] Masanori SHIMIZU et al. "Crystallization Behavior and Change in Surface Area of ​​Alkoxide-Derived Mullite Precursor Powders with Different Compositions", Journal of the Ceramic Society of Japan 105 [2] 131-135 (1997) [Non-Patent Document 3] Takeshi Nakamura et al., "Development of CMC Nozzles," IHI Technical Review Vol. 48 No. 3 (2008-9) [Non-Patent Document 4] Min Mei et al. “Preparation of C / SiC composites by pulse chemical liquid-vapor deposition process”, Materials Letters 82 (2012) 36-38 Summary of the Invention [Problem to be solved by the invention]

[0008] The PIP, CVI, and MI methods mentioned above each have their own issues. With the PIP and CVI methods, it takes a long time to form a high-density matrix, which is a factor in increasing costs. With the MI method, it is possible to form a high-density matrix in a relatively short time, but metal remains, which reduces heat resistance and oxidation resistance.

[0009] Therefore, a technique for combining each method has been proposed. For example, the process time has been shortened to one-third by combining the CVI method with the PIP method, and further by combining the CVI method with the powder impregnation and PIP method (Non-Patent Document 3).

[0010] In addition, a film boiling method has been proposed that enables matrix formation at a speed more than 50 times faster than the CVI process alone (Patent Document 2 and Non-Patent Document 4), but although the matrix formation speed is fast, densification is insufficient.

[0011] Therefore, an object of the present invention is to provide a technique for forming a high-density matrix in a short time using the film boiling method in a manufacturing method for a ceramic-based composite material, with a focus on maximizing the effects of the film boiling method. [Means for solving the problem]

[0012] In order to achieve the above object, a manufacturing method according to the present invention is a manufacturing method for a ceramic-based composite material including a matrix and reinforcing fibers provided in the matrix, the manufacturing method comprising the steps of: (A) impregnating a fibrous body composed of reinforcing fibers with a powder of a ceramic material that will become part of the matrix; (B) placing the powder-impregnated fibrous body in a liquid source of the matrix; (C) In this state, the fibrous body is heated to bring the liquid raw material into a film boiling state, and ceramics derived from the liquid raw material are generated within the fibrous body as part of the matrix. Effect of the Invention

[0013] According to the present invention, when using the film boiling method, by combining powder impregnation, the effect of the film boiling method is maximized, and densification is achieved in a short time. In the film boiling method, even if the porosity is the same, if the pore size is large, the matrix cannot be filled, and the pores remain as a cause of density reduction. On the other hand, the inventor of the present application found that if the pore size is small, the matrix can be filled in a short time. Therefore, by impregnating the fibrous body with powder of a ceramic material in advance, the pore size is divided, and then the matrix is ​​formed by the film boiling method, densification is achieved in a short time. [Brief description of the drawings]

[0014] [Figure 1] 1 is a flowchart illustrating a method for manufacturing a ceramic-based composite material according to an embodiment of the present invention. [Figure 2A] 1 illustrates an example of a fixture that can be used in manufacturing methods according to embodiments of the present invention. [Figure 2B] FIG. 2B is a view taken along the line 2B-2B of FIG. 2A. [Figure 2C] 2C-2C in FIG. 2A. [Diagram 3] 1 shows an example of a configuration that can be used to implement the film boiling method of the manufacturing method according to an embodiment of the present invention. [Figure 4] 1 is a scanning electron microscope image of a cross section of a ceramic matrix composite material obtained according to an embodiment of the present invention. [Diagram 5] FIG. 5 is an enlarged view of the part surrounded by the dashed line in FIG. [Figure 6] FIG. 6 is an enlarged view of the part surrounded by the dashed line in FIG. 5. [Figure 7] 1 is a scanning electron microscope image of a cross section of a ceramic matrix composite material obtained in a reference example. [Figure 8] 13 is a table showing the results when the manufacturing method was carried out under different conditions. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS An embodiment of the present invention will be described with reference to the drawings. In the drawings, the same reference numerals are used to designate the same parts, and duplicated explanations will be omitted.

[0016] The manufacturing method according to the embodiment of the present invention is a method for manufacturing a ceramic matrix composite material having reinforcing fibers (a fibrous body formed of reinforcing fibers) and a matrix, and is a method for obtaining a high-density matrix at high speed in a film boiling method by dispersing large pores into small pores in the fibrous body by powder impregnation. The ceramic matrix composite material has a large number of reinforcing fibers provided as reinforcing materials in the matrix. The ceramic matrix composite material may be used as a high-temperature structural member in rocket engines, aircraft jet engines, etc.

[0017] The matrix may be made of ceramics, for example, silicon carbide, but may also be made of other materials (e.g., mullite).

[0018] The reinforcing fibers may be fibers mainly composed of silicon carbide or carbon. For example, the reinforcing fibers are silicon carbide fibers or carbon fibers. However, according to the present invention, the reinforcing fibers are not limited to these, and may be, for example, heat-resistant oxide fibers such as alumina fibers, mullite fibers, and zirconia fibers. The reinforcing fibers may be provided in a matrix as a fibrous body formed of a large number of reinforcing fibers. This fibrous body may be a woven or knitted fabric of reinforcing fibers. Furthermore, this fibrous body may be in a state in which a matrix is ​​partially formed by a CVI method, a PIP method, or the like, but many pores are still left.

[0019] FIG. 1 is a flow chart illustrating a method for manufacturing a ceramic matrix composite material according to an embodiment of the present invention.

[0020] In step S1, the above-mentioned fibrous body formed of a large number of reinforcing fibers is impregnated with a powder of a ceramic material (hereinafter also simply referred to as powder). This powder may be sintered, and in one example, it is a powder of silicon carbide (SiC powder), but it may be a powder of another material as described below. In addition, the fibrous body used in step S1 may be one in which a matrix is ​​partially formed by a CVI method, a PIP method, or the like, as described above. In this case, the matrix may be partially formed on either or both the inside and the surface of the fibrous body. Step S1 may include steps S11 to S13.

[0021] The median diameter (particle diameter at 50% cumulative height) of the powder used in step S1 may be 1 μm or more and 20 μm or less. In this case, the powder used in step S1 may be, for example, a mixed powder of a powder with a median diameter of 5 μm and a powder with a median diameter of 17 μm. In this case, for example, the volume fraction (= weight fraction) of the powder with a median diameter of 5 μm to the total powder used in step S1 is 35%. Alternatively, the particle size of the particles constituting the powder used in step S1 (the particle size of 70% or more, 80% or more, or 90% or more of the particles in the entire powder) may be 1 μm or more and 20 μm or less. The powder used in step S1 may be composed of particles of one type of particle size, or may be composed of particles of multiple types of particle sizes. In the former case, the powder used in step S1 may be composed mainly (70% or more, 80% or more, or 90% or more of the entire powder) of particles with a particle size of about 5 μm (e.g., 3 μm to 7 μm). In the latter case, the powder used in step S1 may be composed mainly (70% or more, 80% or more, or 90% or more of the entire powder) of particles with a particle size of about 5 μm (e.g., 3 μm to 7 μm) and particles with a particle size of about 17 μm (15 μm to 19 μm). In the latter case, the particles having a particle size of about 5 μm and the particles having a particle size of about 17 μm may each account for 40% or more of the powder used in step S1. The particle size (width) of each particle may mean the maximum dimension of the particle (the maximum value of the dimensions in each direction).

[0022] In step S11, a slurry is produced by mixing a powder of a ceramic material with a liquid (dispersion medium) such as water.

[0023] In step S12, the fibrous body is placed in a slurry container (not shown) that holds the slurry produced in step S11. At this time, the entire fibrous body is buried in the slurry. In step S12, the inside of the slurry container is evacuated through an air intake pipe connected to the slurry container (gas phase part inside the container). This promotes the slurry from filling the pores in the fibrous body.

[0024] In step S13, the fibrous body impregnated with the slurry in step S12 is removed from the slurry container and heated by an appropriate heating device to evaporate the liquid from the slurry in the fibrous body. This allows only the liquid to evaporate from the slurry. This allows the powder to remain in the fibrous body.

[0025] After step S13, the above-mentioned step S11 may be started again to repeat steps S11 to S13. After steps S11 to S13 have been repeated a predetermined number of times, the process proceeds to step S2. This predetermined number of times may be 2 to 10 times (e.g., 5 times). For example, this predetermined number of times is 2, and in the first step S13, the fiber body is heated at 80°C for 30 minutes, and in the second step S13, the fiber body is heated at 130°C for 30 to 60 minutes. Note that steps S11 to S13 do not have to be repeated, and in this case, after steps S11 to S13 have been performed once, the process proceeds to step S2.

[0026] In step S2, the fibrous body impregnated with the ceramic material powder in step S1 (fibrous body with the powder held inside) is placed in a liquid matrix raw material. The liquid raw material used in step S2 is a ceramic raw material described below as a matrix of the ceramic-based composite material. This liquid raw material may be, for example, polycarbosilane (LPCS: Liquid Polycarbosilane), which is a liquid raw material for silicon carbide. However, the liquid raw material is not limited to this, as described below.

[0027] In step S2, the above-mentioned fibrous body is attached to the heating body by a mounting tool, and the fibrous body and the heating body are placed in the liquid raw material of the matrix. In the state where the fibrous body is attached to the heating body by the mounting tool, the fibrous body may or may not be in contact with the heating body.

[0028] Step S2 includes steps S21 and S22. In step S21, the above-mentioned fibrous body is attached to the heating body by a mounting tool. This allows the fibrous body and the heating body to be integrated with each other. The number of fibrous bodies attached to the heating body in this manner may be one or more (two in the example of FIG. 2A described later).

[0029] Fig. 2A shows an example of a mounting tool that can be used in step S21. However, the mounting tool is not limited to the configuration example of Fig. 2A, and may be any tool that maintains the state in which the fiber body is attached to the heating body.

[0030] In the case of Fig. 2A, in step S21, the above-mentioned fibrous body 10 is attached to the heating body 1 by the attachment tool 20. Fig. 2B is a view taken along the arrow 2B-2B in Fig. 2A. Fig. 2A shows a state in which the two fibrous bodies 10 after the process of step S1 are attached to the heating body 1 by the attachment tool 20 so as to contact the upper and lower surfaces of the heating body 1, respectively (hereinafter, also referred to simply as the attached state). The attachment tool 20 includes a pair of insulating plates 2, a porous body 3, an action mechanism 4, an insulating material 5, and a hanging part 7.

[0031] The heating body 1 is formed of a material that can be induction heated (e.g., graphite) and is disposed between a pair of insulating plates 2. Each insulating plate 2 is formed of a material that has insulating properties (e.g., alumina). When viewed from the thickness direction of the insulating plate 2, each insulating plate 2 and the heating body 1 may be, for example, circular with approximately the same radius. In the above-mentioned mounting state, the porous body 3 is disposed between the heating body 1 and each insulating plate 2. Each porous body 3 has a large number of holes formed therein through which a fluid can pass, and may be, for example, a stack of multiple wire meshes.

[0032] The action mechanism 4 has a bolt 4a and a nut 4b. The bolt 4a passes through the two heat insulating plates 2 and the heating body 1 with a gap therebetween, and a nut 4b is screwed onto both ends of each bolt 4a. In the attached state, the nut 4b is tightened onto the bolt 4a in a direction in which the two heat insulating plates 2 are brought closer to each other, thereby holding each of the porous bodies 3, the heating body 1, and each of the fibrous bodies 10 between the pair of heat insulating plates 2. A plurality of such action mechanisms 4 (two in the example of FIG. 2A) may be provided.

[0033] The heat insulating material 5 covers the outer periphery of the heating body 1 and the two fibrous bodies 10 in the installed state. That is, the heating body 1 and each fibrous body 10 have outer peripheries 1a, 10a surrounding the central axis facing the thickness direction of the insulation plate 2, respectively, and these outer peripheries 1a, 10a are covered by the heat insulating material 5 as shown in FIG. 2B. In FIG. 2A, only the parts of the heat insulating material 5 located on both sides (the left and right sides of this figure) of the heating body 1 and each fibrous body 10 are illustrated by two-dot chain lines. The heat insulating material 5 is formed of a material having heat insulating properties. For example, the heat insulating material 5 may be a glass heat insulating cloth (woven fabric). In addition, in the example of FIG. 2A and FIG. 2B, in order to fix the heat insulating material 5 to the heating body 1, a wire 6 may be wound around the heat insulating material 5 from its outer periphery side, but the heat insulating material 5 may be fixed by other means.

[0034] In addition, in the attached state, each porous body 3 is open to the outer periphery side. That is, each porous body 3 has an outer periphery 3a surrounding a central axis facing the thickness direction of the heat insulating board 2, and the outer periphery 3a is open to the outside radially outward from the central axis.

[0035] The suspending part 7 is for suspending the fiber body 10 and the heating body 1 in step 22 described later. FIG. 2C is a view taken along the arrow 2C-2C in FIG. 2A. The suspending part 7 has a plate-shaped member 7a and a rod-shaped member 7b. The plate-shaped member 7a extends elongatedly in the left-right direction of FIG. 2A and FIG. 2C along the upper surface of the upper heat insulating plate 2. The bolts 4a penetrate both ends of the plate-shaped member 7a with gaps. Both ends of the plate-shaped member 7a are sandwiched between the upper heat insulating plate 2 and the upper nut 4b, respectively. A connecting part 7a1 is provided in the center of the plate-shaped member 7a. The rod-shaped member 7b is connected to this connecting part 7a1. The rod-shaped member 7b extends upward from the connecting part 7a1. Although not shown in the figure, for example, a protrusion as a bolt may be formed on the upper surface of the connecting portion 7a1, and a bolt hole may be formed in the lower end surface of the rod-shaped member 7b, and the connecting portion 7a1 and the rod-shaped member 7b may be connected by screwing the bolt into the bolt hole.

[0036] 3, the fiber body 10 attached to the heater 1 by the fixture 20 is placed in the liquid raw material 9 in the processing vessel 8. At this time, the fiber body 10 is placed in the liquid raw material 9, and the fiber body 10 and the heater 1 are suspended by the suspension part 7 so that the fixture 20, the heater 1, and the fiber body 10 do not come into contact with the inner surface (bottom surface and inner circumferential surface) of the processing vessel 8. At this time, the rod-shaped member 7b of the suspension part 7 is disposed so as to penetrate the through-hole 8a1 of the cover member 8a that closes the opening at the top surface of the processing vessel 8, and the upper end side portion of the rod-shaped member 7b may be connected to and supported by a structure (not shown) by appropriate means.

[0037] In step S22, the hanging section is not limited to the configuration examples shown in Figures 2A and 2C, etc., as long as it can hang the fiber body and the heating body so that the mounting fixture, the heating body, and the fiber body do not come into contact with the inner surface of the processing vessel (i.e., so that they are separated from the inner surface of the processing vessel).

[0038] The processing vessel 8 is made of a non-conductive material (e.g., glass) that is not induction heated. The processing vessel 8 may be formed with a gas inlet 8b for introducing nitrogen gas into the gas phase portion in the processing vessel 8 in step S3 described later, and a gas outlet 8a2 for discharging gas from the gas phase portion in the processing vessel 8 in step S3.

[0039] By step S22, the entire fibrous body is placed in the liquid raw material. As a result, the liquid raw material enters (permeates) each pore (each pore opening to the outside of the fibrous body) in which the powder is impregnated in step S1. After step S22 is completed, the process proceeds to step S3.

[0040] In step S3, a matrix is ​​formed on the fibrous body by film boiling to obtain a ceramic-based composite material. Step S3 includes steps S31 and S32.

[0041] In step S31, the reinforcing fibers (fibrous body) are heated until their temperature reaches or exceeds the high-temperature target temperature, thereby generating ceramics derived from the liquid raw material in the pores of the powder-impregnated fibrous body, thereby generating a matrix in which the ceramics and the powder are integrated.

[0042] The generation of ceramics in step S31 will be described in more detail. In step S31, the liquid raw material is heated by the heated fibrous body and the powder in the fibrous body, and becomes a film boiling gas (i.e., a film boiling state) at the interface between the liquid raw material and the fibrous body or the powder (the inner surface of the pores in the fibrous body), and ceramics (i.e., a ceramic pyrolysis precipitate) are generated and deposited in the pores by this film boiling gas. This ceramics may be generated by one or both of the following methods (i) and (ii).

[0043] (i) When the film boiling gas collides with the inner surface of the pores, it receives further thermal energy, which causes thermal decomposition and mineralization, resulting in precipitation of solid ceramics on the inner surface of the pores.

[0044] (ii) Some of the gases contained in the film boiling gas have already been thermally decomposed into pyrolysis gas. When this pyrolysis gas collides with the inner surface of the heated pores, it undergoes mineralization and precipitates as solid ceramics on the inner surface of the pores.

[0045] In step S31, the ceramics may also be precipitated at the interface between the outer surface of the fibrous body and the liquid raw material.

[0046] The heating in step S31 may be performed by induction heating the heating body. For example, as shown in FIG. 3, the heating body 1 is induction heated by an alternating magnetic field generated by the coil 11 by passing an alternating current through the coil 11. The fibrous body and the liquid raw material are heated by the heat generated by the heated heating body. When the temperature of the fibrous body (reinforced fiber) reaches or exceeds the target temperature on the high temperature side in step S31, the process proceeds to step S32. For example, when the measured temperature of a temperature sensor attached to the surface of the heating body reaches or exceeds the target temperature, the process proceeds to step S32. The target temperature on the high temperature side is a temperature higher than the boiling point of the liquid raw material. The heating rate of the fibrous body (or heating body) in step S31 is preferably 3000° C. / hour or less, 2000° C. / hour or less, or 1500° C. / hour or less. In this case, the heating rate may be 500° C. / hour or more. In addition, in this case, the heating rate is more preferably about 1000° C. / hour or less, or 1000° C. / hour or less. However, the temperature increase rate is not limited to this. For example, the temperature increase rate may be lower than 500° C. / hour (in this case, the temperature increase rate may be, for example, 100° C. / hour or more).

[0047] In step S31, when the heating body is induction-heated as described above, the treatment vessel 8 made of a non-conductive material is not induction-heated. At this time, as shown in Fig. 3, the heating body 1, the fiber body 10, and the fixture 20 are suspended by the suspension part 7 so as not to come into contact with the inner surface of the treatment vessel 8, so that the treatment vessel 8 is prevented from being damaged by contact with the high-temperature heating body 1, the fiber body 10, and the fixture 20.

[0048] In step S32, the fibrous body is cooled to a target temperature lower than the boiling point of the liquid raw material. This stops the generation of the film boiling gas described above. As a result, in a state where the boiling phenomenon is stopped and new film boiling gas is no longer generated, the film boiling gas that has already been generated is replaced with the liquid raw material, and the liquid raw material again enters (permeates) each pore in the fibrous body that is not completely filled with ceramics (ceramics). For example, in step S32, the liquid raw material again enters into the pores that have been partially filled with ceramics in step S31. The temperature reduction rate of the heating body (fibrous body) in step S32 may be, for example, a natural cooling rate or a rate due to active cooling, as described later.

[0049] The cooling in step S32 may be natural cooling, which is performed by stopping the heating of the fibrous body and maintaining this stopped state. Alternatively, in step S32, in addition to stopping the heating of the fibrous body, the liquid raw material may be actively cooled. For example, in FIG. 3, the liquid raw material 9 may be circulated by causing a part of the liquid raw material 9 in the processing vessel 8 to flow outside the processing vessel 8, cooling the liquid raw material 9 by a heat exchanger, and then returning the cooled liquid raw material 9 to the processing vessel 8. In this case, piping and a pump (not shown) for circulating the liquid raw material 9 in this manner may be provided.

[0050] When the fibrous body of step S32 is cooled to the target temperature lower than the boiling point of the liquid raw material, step S31 is started again. For example, assuming that the temperature measured by the temperature sensor is the temperature of the fibrous body, when the measured temperature falls below the target temperature, step S31 is started again. The target temperature may be an approximate standard. That is, since it may be difficult to start step S31 again at the timing when the target temperature is reached, the timing to start step S31 again may be when the temperature of the fibrous body reaches the target temperature, or when the temperature of the fibrous body falls below the target temperature to a certain extent.

[0051] After step S32, before starting step S31 again, it is confirmed that no air bubbles are generated from the fibrous body in the liquid raw material in the processing vessel, and when this confirmation is made, step S31 is started. This confirmation may be made, for example, by visually checking the transparent glass processing vessel from the outside. Since no air bubbles are generated, it can be determined that the liquid raw material has completely permeated into the inside of the fibrous body.

[0052] In this manner, step S31 is started again, and step S31 and step S32 are repeated. As a result, the ceramics generated in each pore in the matrix increases, and the pores are filled with the ceramics. Step S31 and step S32 are repeated until each pore is sufficiently (for example, completely) filled with the ceramics. The number of times this is repeated may be, for example, 10 times or more and 20 times or less, but is not limited to this.

[0053] In addition, in the repetition of steps S31 and S32, the target temperature in step S31 performed in a later stage may be higher than the target temperature in step S31 performed in an earlier stage. In this case, the target temperature in step S31 may be increased in multiple stages (e.g., three or more stages) in the repetition. For example, in the repetition, the target temperature in step S31 in the first stage (e.g., from the first to the third times) may be 1000°C, the target temperature in step S31 in the intermediate stage (e.g., from the fourth to the sixth times) may be 1100°C, and the target temperature in step S31 in the final stage (e.g., from the seventh to the twelfth times) may be 1200°C.

[0054] When the liquid raw material is the above-mentioned LPCS, the above-mentioned ceramic becomes silicon carbide. In this case, the LPCS undergoes polymerization in the repeated process of steps S31 and S32, and its boiling point rises to about 180°C to 250°C. In this case, the maximum temperature of the fibrous body reached by step S31 is, for example, 800°C or higher, preferably 1000°C or higher and 1400°C or lower. By setting the maximum temperature to 1000°C or higher, sufficient progress of mineralization of the ceramics can be expected, and by setting the maximum temperature to 1400°C or lower, it is possible to prevent the precipitation rate of the ceramics from becoming too high or the occurrence of intense thermal decomposition to the extent that the ceramics are not deposited. This is expected to make it easier for the ceramics to be filled into the pores in the fibrous body.

[0055] Example 1 In Example 1 of this embodiment, the fibrous body was formed of SiC fibers (silicon carbide fibers) as reinforcing fibers, and the liquid raw material was the above-mentioned LPCS. In addition, the process shown in the flow chart of FIG. 1 was performed using the configuration shown in FIG. 2A to FIG. 2C and FIG. 3.

[0056] Fig. 4 is a scanning electron microscope image of a cross section of the ceramic matrix composite material obtained in Example 1. Fig. 5 is an enlarged view of a portion surrounded by a dashed line in Fig. 4. Fig. 6 is an enlarged view of a portion surrounded by a dashed line in Fig. 5. In Fig. 6, the symbol P indicates the powder of the ceramic material used in the above-mentioned step S1, and the symbol F indicates the ceramic formed by the film boiling method in the above-mentioned step S3.

[0057] Fig. 7 is a scanning electron microscope image of a cross section of a ceramic matrix composite material obtained in a reference example. In this reference example, the above-mentioned step S2 and step S3 were carried out without carrying out the above-mentioned step S1. The other points of the reference example are the same as those of Example 1. The image in Fig. 7 is an image at the same magnification as Fig. 4.

[0058] In the reference example, as shown in Fig. 7, large pores (pores of several hundred µm) that are not filled with the matrix remain inside the ceramic matrix composite material (note that in the reference example, it is desirable to increase the number of times steps S31 and S32 are performed in order to fill the large pores). In contrast, in Example 1, as shown in Fig. 4 to Fig. 6, relatively large pores such as those shown in Fig. 7 do not remain inside the ceramic matrix composite material, and the filling rate of the matrix inside the ceramic matrix composite material is high.

[0059] 6, in Example 1, the ceramics F generated in the above-mentioned step S31 fills the minute pores (of several μm) between the powders P. Therefore, it can be seen that the present embodiment forms a matrix made of the powders P and the ceramics F with a high filling rate inside the fibrous body.

[0060] Example 2 In Example 2, the particle size of the ceramic material powder used in step S1 was changed to a plurality of values, and the process shown in the flowchart of Fig. 1 was carried out. Fig. 8 is a table showing the results of Example 2.

[0061] In Fig. 8, (1) shows the case of a reference example in which the above-mentioned step S1 was not performed and the above-mentioned step S2 and step S3 were performed. Other points of the reference example are the same as those of Example 2. In Fig. 8, (2) to (7) show the cases of Example 2. Note that (3) and (4) show the cases of ceramic-based composite materials obtained simultaneously on the lower and upper sides of the heating body 1 in Fig. 3, respectively, and (5) and (6) show the cases of ceramic-based composite materials obtained simultaneously on the lower and upper sides of the heating body 1 in Fig. 3, respectively.

[0062] 8, "powder particle size" indicates the particle size of the particles constituting the powder used in step S1, and is shown here as the particle size at 50% of the cumulative height (median diameter). (7) shows the case where a mixed powder of a powder composed of particles with a particle size of 5.5 μm and a powder composed of particles with a particle size of 17.0 μm was used as the powder in step S1.

[0063] 8, "treatment conditions" indicate how many times the fiber was heated to each temperature in the repetition of steps S31 and S32. For example, (2) indicates that the fiber was heated to 1000°C in the first to third steps S31, to 1100°C in the fourth to sixth steps S31, and to 1200°C in the seventh to twelfth steps S31.

[0064] In FIG. 8, "density after FB treatment" indicates the density of the ceramic matrix composite material produced after completing the treatment in FIG. 1, "density increase" indicates the increase in density of the ceramic matrix composite material relative to the density of the fibrous body, and "powder effect" indicates the ratio of the density increase in each case to the density increase in the case of (1) taken as 1.

[0065] As can be seen from Figure 8, the density is higher in the cases (2) to (7) where the fiber body was impregnated with powder than in the case (1) where the fiber body was not impregnated with powder. Also, among the cases (2) to (6) where powder consisting of particles of one type of particle size was used, the "powder effect" was the highest in the case (2) where the particle size was 5.5 μm.

[0066] In addition, in the case of (7), where a mixed powder of 5.5 μm and 17.0 μm particles was used, the "powder effect" was even higher than in the case of (2). In other words, the maximum powder effect was obtained by using a mixed powder of about 5 μm and about 17.0 μm particles.

[0067] The present invention is not limited to the above-mentioned embodiment, and various modifications can be made within the scope of the technical idea of ​​the present invention. For example, any one of the following modified examples 1 to 4 may be adopted, or any combination of two or more of the modified examples 1 to 4 may be adopted. In this case, other points may be the same as those described above.

[0068] (Change example 1) The powder used in step S1 above is silicon carbide powder, but may be powder of other ceramic materials.

[0069] The powder may be a powder of boron nitride (BN), which is a ceramic. Boron nitride has low adhesion to silicon carbide. Therefore, when the ceramic generated from the liquid raw material in the above-mentioned step S31 is silicon carbide, or when the reinforcing fiber is silicon carbide fiber, the propagation of cracks can be suppressed at the interface between the boron nitride portion and the silicon carbide portion in the matrix.

[0070] The powder may be carbon powder, which has the function of suppressing the propagation of cracks, similar to the case of the boron nitride powder described above.

[0071] The powder may be silicon dioxide (SiO2) or alumina (Al2O3) powder, which is less expensive than silicon carbide.

[0072] The powder may be a powder of mullite (Al2O3-SiO2), which is more heat resistant than alumina and less expensive than silicon carbide.

[0073] The powder may be zirconia (ZrO2) powder. Zirconia is a ceramic with a higher melting point than silicon carbide, so it functions as a part of the matrix without melting even in an extremely high temperature environment.

[0074] The powder may be zirconium carbide (ZrC), hafnia (HfO2), hafnium carbide (HfC), zirconium boride (ZrB2), or hafnium boride (HfB2) powder, which have similar functions as zirconia powder.

[0075] The powder may be a mixed powder of alumina powder and manganese oxide (MnO) powder. In this case, when oxygen enters the cracks generated in the matrix, it reacts with silicon carbide in the matrix (silicon carbide generated as ceramics by the film boiling method in step S3) to generate silicon dioxide. This silicon dioxide reacts with alumina to fill the cracks. Moreover, manganese oxide activates the filling of such cracks.

[0076] (Change example 2)

[0077] The liquid source used in the above step S3 may be a liquid source other than the above LPCS. For example, the liquid source may be borazine, methyltrichlorosilane, cyclohexane, a silicon alkoxide solution, an aluminum alkoxide solution, a mixture of a silicon alkoxide solution and an aluminum alkoxide solution, or a zirconium alkoxide solution.

[0078] When the liquid raw material is borazine, the ceramics generated by the heating in the above-mentioned step S31 are boron nitride (BN), which is a ceramic. The function of this boron nitride is the same as that described in the first modification.

[0079] When the liquid raw material is methyltrichlorosilane, the ceramics generated by heating in the above-mentioned step S31 become silicon carbide (SiC), which is a ceramic, in the same way as when the liquid raw material is polycarbosilane (LPCS).

[0080] When the liquid raw material is cyclohexane, the ceramics generated by the heating in the above-mentioned step S31 is carbon, which has the same function as boron nitride.

[0081] When the liquid raw material is a silicon alkoxide solution, the ceramics produced by the heating in the above-mentioned step S31 will be silicon dioxide. The silicon alkoxide solution is cheaper than LPCS.

[0082] When the liquid raw material is an aluminum alkoxide solution, the ceramics produced by the heating in the above-mentioned step S31 is alumina. The aluminum alkoxide solution is cheaper than LPCS.

[0083] When the liquid raw material is a mixture of a silicon alkoxide solution and an aluminum alkoxide solution, the ceramics generated by the heating in the above-mentioned step S31 will be mullite.

[0084] When the liquid raw material is a zirconium alkoxide solution, the ceramics produced by the heating in the above-mentioned step S31 is zirconia, the function of which is the same as that described in the first modification.

[0085] According to the present invention, the liquid source used in step S3 is not limited to the above specific example, and may be other liquid source. For example, other metal alkoxide solution may be used as the liquid source used in step S3. In this case, the ceramics generated by heating in the above-mentioned step S31 may be oxide ceramics. In this case, the liquid source used in step S3 may be, for example, a mixture of three alkoxydes solutions, as described in Non-Patent Document 1, so that the ceramics generated in step S31 is barium aluminosilicate (BaAl2Si2O8).

[0086] When the ceramics produced by heating in step S31 is mullite, the liquid raw material used in step S3 may be a mixture of a plurality of alkoxydes solutions as described in Non-Patent Document 2 above.

[0087] (Change example 3) In the above-mentioned step S3, step S31 may be performed without performing step S32. In this case, in step S31, the fiber body is heated until the temperature of the fiber body reaches or exceeds the target temperature on the high temperature side, and the temperature of the fiber body is kept at or above the target temperature for a predetermined time. This predetermined time may be, for example, 6 hours or more and 20 hours or less.

[0088] (Change example 4) In the above, the heater 1 may be omitted, and in step S31, a powder-impregnated fibrous body (e.g., a fibrous body formed of carbon fiber or silicon carbide fiber) having a sufficiently large heat capacity (volume) may be induction-heated to generate the above-mentioned film boiling gas, and ceramics may be deposited in the pores of the matrix of the ceramic matrix composite material by one or both of the above (i) and (ii). In this case, for example, in Fig. 2A and Fig. 3, the heater 1 may be omitted, the number of ceramic matrix composite materials 10 may be one, one ceramic matrix composite material 10 may contact the porous body 3 from above and below, and the heat insulating material 5 may cover the outer periphery 10a of the ceramic matrix composite material 10, and the other points may be the same as those described above. In addition to or instead of omitting the heater 1, the heat insulating plate 2 may be omitted. [Explanation of symbols]

[0089] REFERENCE SIGNS LIST 1 heating body, 1a outer periphery, 2 insulating plate, 3 porous body, 3a outer periphery, 4 action mechanism, 4a bolt, 4b nut, 5 insulating material, 6 wire, 7 hanging part, 7a plate-shaped member, 7a1 connecting part, 7b rod-shaped member, 8 treatment vessel, 8a lid member, 8a1 through hole, 8a2 gas exhaust hole, 8b gas introduction hole, 9 liquid raw material, 10 fibrous body, 10a outer periphery, 11 coil, 20 mounting fixture

Claims

1. A method for producing a ceramic-based composite material comprising a matrix and reinforcing fibers disposed within the matrix, comprising: (A) A fibrous body made of reinforcing fibers is impregnated with a powder of a ceramic material that will become part of the matrix, thereby dividing the pores in the fibrous body; (B) placing the powder-impregnated fibrous body in a liquid source of the matrix; (C) A method for producing a ceramic-based composite material, comprising heating the fibrous body in this state to bring the liquid raw material into a film boiling state, thereby producing ceramics derived from the liquid raw material within the pores subdivided in (A) within the fibrous body as part of the matrix.

2. In the above (C), (C1) heating the fibrous body to bring the liquid raw material into the film boiling state and generate the ceramics within the fibrous body; (C2) cooling the fibrous body to a temperature lower than the boiling point of the liquid raw material; The method for producing a ceramic-based composite material according to claim 1 , wherein the steps (C1) and (C2) are repeated.

3. A method for producing a ceramic matrix composite material as described in claim 2, wherein in the process of repeating (C1) and (C2), when the temperature of the fibrous body in (C1) reaches or exceeds a target temperature on the higher temperature side, heating of the fibrous body is stopped, thereby performing (C2).

4. In the above (A), (A1) mixing the powder with a liquid to form a slurry; (A2) placing the fibrous body in a slurry container so that the fibrous body is embedded in the slurry; (A3) The method for producing a ceramic-based composite material according to any one of claims 1 to 3, further comprising evacuating the inside of the slurry container to allow the slurry containing the powder to impregnate the inside of the fibrous body.

5. The method for producing a ceramic-based composite material according to any one of claims 1 to 4, wherein the powder used in (A) has a median diameter of 1 µm or more and 20 µm or less.

6. The method for producing a ceramic-based composite material according to any one of claims 1 to 5, wherein the powder used in (A) is a mixed powder of a powder having a median diameter of 5 µm and a powder having a median diameter of 17 µm.

7. In the method (B), the fiber body and a heater are disposed inside a processing vessel that holds the liquid raw material; 7. The method for producing a ceramic-based composite material according to claim 1, wherein in the step (C), the fibrous body is heated by induction heating the heating body.

8. In the step (C), an AC current is applied to a coil disposed outside the treatment vessel to generate an AC magnetic field, thereby inductively heating the heater, and the fibrous body is heated by the inductively heated heater; The method for producing a ceramic-based composite material according to claim 7 , wherein the treatment vessel is made of a non-conductive material.

9. A method for producing a ceramic-based composite material comprising a matrix and reinforcing fibers disposed within the matrix, comprising: (A) impregnating a fibrous body composed of reinforcing fibers with a powder of a ceramic material that will become a part of the matrix; (B) placing the powder-impregnated fibrous body in a liquid source of the matrix; (C) heating the fibrous body in this state to bring the liquid raw material into a film boiling state, thereby generating ceramics derived from the liquid raw material within the fibrous body as a part of the matrix; In the method (B), the fiber body and a heater are disposed inside a processing vessel that holds the liquid raw material; In the step (C), the fibrous body is heated by induction heating the heating body, In the method for producing a ceramic-based composite material, in (C), the fibrous body is attached to the heating body by a mounting fixture, and the mounting fixture, the fibrous body, and the heating body are suspended so as not to come into contact with the inner surface of the treatment vessel.

10. A ceramic composite material produced by the method for producing a ceramic composite material according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for quickly preparing C / SiC ceramic matrix composite material

    CN102795871A

  • Improvement of densification by film boiling of porous structures

    JP2004513053A

  • Method for manufacturing continuous fiber-reinforced composite material

    JP2006347837A

  • Apparatus and method of densifying porous product

    JP2010255174A

  • Method for producing silicon carbide based composite

    JP2017001912A