Composition for forming thermally conductive material, thermally conductive material, thermally conductive sheet, device with thermally conductive layer
The composition of an epoxy compound with a specific compound and optional inorganic substance enhances thermal conductivity in thermally conductive materials, addressing heat dissipation challenges in small, dense power semiconductor devices.
Patent Information
- Application Number
- JP2020211572
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-21
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-12-21
AI Technical Summary
Conventional thermally conductive materials used in power semiconductor devices exhibit inadequate thermal conductivity, posing challenges in heat dissipation as devices become smaller and more dense.
A composition for forming a thermally conductive material comprising an epoxy compound and a specific compound with a group represented by formula (1), which includes a phenolic hydroxyl group, optionally with an inorganic substance and a curing accelerator, to enhance thermal conductivity.
The composition forms a thermally conductive material with improved thermal conductivity, suitable for use in devices with thermally conductive layers, effectively dissipating heat from power semiconductor devices.
Smart Images

Figure 0007582859000001 
Figure 0007582859000002 
Figure 0007582859000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a composition for forming a thermally conductive material, a thermally conductive material, a thermally conductive sheet, and a device with a thermally conductive layer. [Background technology]
[0002] Power semiconductor devices used in various electrical appliances such as personal computers, general home appliances, and automobiles have been rapidly miniaturized in recent years. As the miniaturization progresses, it becomes more difficult to control the heat generated by the power semiconductor devices, which have become denser. To address these issues, thermally conductive materials are used to facilitate heat dissipation from power semiconductor devices. For example, Patent Document 1 discloses a thermally conductive sheet containing a curing agent such as an imidazole compound. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2013-177562 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present inventors have studied a composition for forming a thermally conductive material containing a conventional curing agent as described in Patent Document 1 and have found that there is room for improvement in the thermal conductivity of the resulting thermally conductive material.
[0005] Therefore, an object of the present invention is to provide a composition for forming a thermally conductive material that can form a thermally conductive material having excellent thermal conductivity. Another object of the present invention is to provide a thermally conductive material, a thermally conductive sheet, and a device with a thermally conductive layer, which are related to the above-mentioned composition for forming a thermally conductive material. [Means for solving the problem]
[0006] As a result of intensive research by the present inventors to solve the above problems, they have found that the above problems can be solved by the following configuration.
[0007] [1] A composition for forming a thermally conductive material, comprising an epoxy compound and a compound having a group represented by formula (1) described below. [2] The composition for forming a thermal conductive material according to [1], wherein the compound having a group represented by the formula (1) further has a phenolic hydroxyl group. [3] The composition for forming a thermal conductive material according to [1] or [2], wherein the compound having a group represented by the above formula (1) is a compound represented by the below-mentioned formula (2). [4] The composition for forming a thermal conductive material according to any one of [1] to [3], wherein the compound having a group represented by the formula (1) is a compound represented by the formula (Z1) described below. [5] The composition for forming a thermal conductive material according to [2], wherein X represents a benzene ring group which may have a substituent. [6] The composition for forming a thermally conductive material according to any one of [1] to [5], further comprising an inorganic substance. [7] The thermal conductive material forming composition according to [6], wherein the inorganic material is an inorganic nitride. [8] The composition for forming a thermally conductive material according to any one of [1] to [7], further comprising a curing accelerator. [9] A thermally conductive material obtained by curing the composition for forming a thermally conductive material according to any one of [1] to [8].
[10] A thermally conductive sheet comprising the thermally conductive material according to [9].
[11] A device with a thermally conductive layer, comprising: a device; and a thermally conductive layer disposed on the device, the thermally conductive layer comprising the thermally conductive material according to [9]. Effect of the Invention
[0008] According to the present invention, it is possible to provide a composition for forming a thermally conductive material that can form a thermally conductive material having excellent thermal conductivity. Furthermore, according to the present invention, it is possible to provide a thermally conductive material, a thermally conductive sheet, and a device with a thermally conductive layer, which are related to the above-mentioned composition for forming a thermally conductive material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The thermally conductive material-forming composition, the thermally conductive material, the thermally conductive sheet, and the device with a thermally conductive layer of the present invention will be described in detail below. The following description of the configuration may be based on a representative embodiment of the present invention, but the present invention is not limited to such an embodiment. In this specification, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits.
[0010] In this specification, the acid anhydride group may be a monovalent group or a divalent group. When the acid anhydride group represents a monovalent group, examples of the substituents include those obtained by removing any hydrogen atom from acid anhydrides such as maleic anhydride, phthalic anhydride, pyromellitic anhydride, and trimellitic anhydride. When the acid anhydride group represents a divalent group, the group represented by *-CO-O-CO-* is intended (* represents a bond position).
[0011] In this specification, for substituents and the like that are not specified as substituted or unsubstituted, if possible, the group may further have a substituent (for example, a group exemplified by the substituent group Y described later) within a range that does not impair the intended effect. For example, the expression "alkyl group" means a substituted or unsubstituted alkyl group (an alkyl group that may have a substituent) within a range that does not impair the intended effect. In addition, in the present specification, when it is stated that "the group may have a substituent", the type of the substituent, the position of the substituent, and the number of the substituent are not particularly limited. The number of the substituents can be, for example, 1 or 2 or more. The substituents can be, for example, a monovalent nonmetallic atomic group other than a hydrogen atom, and are preferably a group selected from the following group of substituents Y. In this specification, examples of halogen atoms include a chlorine atom, a fluorine atom, a bromine atom, and an iodine atom. In addition, in the present specification, the bonding direction of a divalent group (e.g., -CO-O-) is not particularly limited. For example, when L in a group represented by XLY is -CO-O-, assuming that the position bonded to the X side is *1 and the position bonded to the Y side is *2, L may be *1-CO-O-*2 or *1-O-CO-*2.
[0012] Substituent group Y: Halogen atoms (-F, -Br, -Cl, -I, etc.), hydroxyl groups, amino groups, carboxylic acid groups and their conjugate base groups, carboxylic anhydride groups, cyanate ester groups, unsaturated polymerizable groups, epoxy groups, oxetanyl groups, aziridinyl groups, thiol groups, isocyanate groups, thioisocyanate groups, aldehyde groups, alkoxy groups, aryloxy groups, alkylthio groups, arylthio groups, alkyldithio groups, aryldithio groups, N-alkylamino groups, N,N-dialkylamino groups, N-arylamino groups, N,N-diarylamino groups, N-alkyl-N-arylamino groups, acyloxy group, carbamoyloxy group, N-alkylcarbamoyloxy group, N-arylcarbamoyloxy group, N,N-dialkylcarbamoyloxy group, N,N-diarylcarbamoyloxy group, N-alkyl-N-arylcarbamoyloxy group, alkylsulfoxy group, arylsulfoxy group, acylthio group, acylamino group, N-alkylacylamino group, N-arylacylamino group, ureido group, N'-alkylureido group, N',N'-dialkylureido group, N'-arylureido group, N',N'-diarylureido group, N'-alkyl-N'-arylureido group, N-alkylureido group, N-arylureido group, N'-alkyl-N-alkylureido group, N'-alkyl-N-arylureido group, N',N'-dialkyl-N-alkylureido group, N',N'-dialkyl-N-arylureido group, N'-aryl-N-alkylureido group, N'-aryl-N-arylureido group, N',N'-diaryl-N-alkylureido group, N',N'-diaryl-N-arylureido group, N'-alkyl-N'-aryl-N-alkylureido group , N'-alkyl-N'-aryl-N-arylureido group, alkoxycarbonylamino group, aryloxycarbonylamino group, N-alkyl-N-alkoxycarbonylamino group, N-alkyl-N-aryloxycarbonylamino group, N-aryl-N-alkoxycarbonylamino group, N-aryl-N-aryloxycarbonylamino group, formyl group, acyl group, alkoxycarbonyl group, aryloxycarbonyl group, carbamoyl group, N-alkylcarbamoyl group, N,N-dialkylcarbamoyl group, N-arylcarbamoyl group, N,N-diarylcarbamoyl group, N-alkyl-N-arylcarbamoyl group, alkylsulfinyl group, arylsulfinyl group, alkylsulfonyl group, arylsulfonyl group, sulfo group (-SO3H) and its conjugate base group, alkoxysulfonyl group, aryloxysulfonyl group, sulfinamoyl group, N-alkylsulfinamoyl group, N,N-dialkylsulfinamoyl group, N-arylsulfinamoyl group, N,N-diarylsulfinamoyl group, N-alkyl-N-arylsulfinamoyl group, sulfamoyl group, N-alkylsulfamoyl group, N,N-dialkylsulfamoyl group, N-arylsulfamoyl group, N,N-diarylsulfamoyl group, N-alkyl-N-arylsulfamoyl group, N-acylsulfamoyl group and its conjugate base group, N-alkylsulfonylsulfamoyl group (-SO2NHSO2(alkyl)) and its conjugate base group, N-arylsulfonylsulfamoyl group (-SO2NHSO2(aryl)) and its conjugate base group, N-alkylsulfonylcarbamoyl group (-CONHSO2(alkyl)) and its conjugate base group, N-arylsulfonylcarbamoyl group (-CONHSO2(aryl)) and its conjugate base group, alkoxysilyl group (-Si(Oalkyl)3), aryloxysilyl group (-Si(Oaryl)3), hydroxysilyl group (-Si(OH)3) and its conjugate base group, phosphono group (-PO3H2) and its conjugate base group, dialkylphosphono group (-PO3(alkyl) 2), diarylphosphono group (-PO3(aryl)2), alkylarylphosphono group (-PO3(alkyl)(aryl)), monoalkylphosphono group (-PO3H(alkyl)) and its conjugate base group, monoarylphosphono group (-PO3H(aryl)) and its conjugate base group, phosphonooxy group (-OPO3H2) and its conjugate base group, dialkylphosphonooxy group (-OPO3(alkyl)2), diarylphosphonooxy group (-OPO3(aryl)2), alkylarylphosphonooxy group (-OPO3(alkyl)(aryl)), monoalkylphosphonooxy group (-OPO3H(alkyl)) and its conjugate base group, monoarylphosphonooxy group (-OPO3H(aryl)) and its conjugate base group, cyano group, nitro group, aryl group, alkenyl group, alkynyl group, and alkyl group. Each of the above groups may further have a substituent (e.g., one or more of the above groups) if possible. For example, an aryl group which may have a substituent is also included as a group which can be selected from the substituent group Y. When the group selected from the substituent group Y has a carbon atom, the group has 1 to 20 carbon atoms, for example. The number of atoms other than hydrogen atoms contained in the group selected from the substituent group Y is, for example, 1 to 30. Furthermore, if possible, these substituents may be bonded to each other or to the group they substitute to form a ring, or may not form a ring. For example, an alkyl group (or an alkyl group portion in a group containing an alkyl group as a partial structure, such as an alkoxy group) may be a cyclic alkyl group as a whole (such as a cycloalkyl group), or may be an alkyl group having one or more cyclic structures as a partial structure.
[0013] [Composition] The thermal conductive material forming composition of the present invention (hereinafter also simply referred to as the "composition") contains an epoxy compound and a compound having a group represented by formula (1) (hereinafter also referred to as the "specific compound").
[0014] The mechanism by which the composition of the present invention, having the above-mentioned configuration, solves the problems of the present invention is not necessarily clear, but the present inventors speculate as follows. A characteristic feature of the composition of the present invention is that it contains a specific compound. It is presumed that the group represented by formula (1) possessed by the specific compound can react with the epoxy compound and form hydrogen bonds starting from the group represented by formula (1), and therefore a heat conductive network based on chemical bonds can be well formed in the obtained thermally conductive material, resulting in excellent thermal conductivity. Hereinafter, excellent thermal conductivity is also referred to as excellent effects of the present invention. The components contained in the composition are described in detail below.
[0015] [Specific compound] The composition of the present invention contains a specific compound (a compound having a group represented by formula (1)). The specific compound is a compound capable of reacting with an epoxy group to crosslink, that is, the specific compound can function as a curing agent that reacts with an epoxy group.
[0016] [ka]
[0017] In formula (1), X represents an aromatic ring group which may have a substituent. 1 ~R 2 each independently represents a hydrogen atom or a substituent. * represents a bonding position.
[0018] X represents an aromatic ring group which may have a substituent. The aromatic ring contained in the aromatic ring group represented by X may be either a monocyclic ring or a polycyclic ring. Examples of the aromatic ring group represented by X include aromatic hydrocarbon groups and aromatic heterocyclic groups. The aromatic hydrocarbon group preferably has 6 to 20 carbon atoms, more preferably 6 to 12 carbon atoms, and even more preferably 6 to 8 carbon atoms. The aromatic heterocyclic group preferably has 3 to 20 carbon atoms, more preferably 5 to 12 carbon atoms, and even more preferably 5 to 7 carbon atoms. Examples of the aromatic ring group represented by X include aromatic hydrocarbon groups such as a benzene ring group, a naphthalene ring group, and an anthracene ring group; and aromatic heterocyclic groups such as a furan ring group, a pyrrole ring group, a thiophene ring group, a pyridine ring group, a thiazole ring group, a carbazole ring group, an indole ring group, and a benzothiazole ring group. Of these, a benzene ring group or a thiophene ring group is preferable, and a benzene ring group is more preferable.
[0019] The aromatic ring group represented by X may have a substituent. Examples of the substituent include the groups exemplified in the above-mentioned group Y of substituents. Among these, the substituent is preferably a halogen atom (-F, -Br, -Cl, -I, etc.), a hydroxyl group, an amino group, a carboxylic acid group, a hydrocarbon group having 1 to 6 carbon atoms, an aryl group, or a group consisting of a combination thereof, more preferably a hydroxyl group, an amino group, or a hydrocarbon group having 1 to 6 carbon atoms, and even more preferably a hydroxyl group or a methyl group.
[0020] R 1 ~R 2 each independently represents a hydrogen atom or a substituent. R 1 ~R 2At least one of R is preferably a hydrogen atom. 1 ~R 2 It is more preferable that both of the groups are hydrogen atoms. R 1 ~R 2 Examples of the substituent represented by the formula (I) include the groups exemplified in the above-mentioned group Y of substituents. Among these, the substituent is preferably a hydrocarbon group having 1 to 6 carbon atoms, an aryl group, or a group consisting of a combination thereof, and more preferably a hydrocarbon group having 1 to 6 carbon atoms.
[0021] The number of groups represented by formula (1) contained in the specific compound is 1 or more, preferably 1 to 10, more preferably 1 to 5, still more preferably 1 to 3, and particularly preferably 1.
[0022] The specific compound may have a monovalent organic group in addition to the group represented by the above formula (1). The monovalent organic group is preferably an active hydrogen group, an acid anhydride group, or an imidazole ring group. Examples of the active hydrogen group include a phenolic hydroxyl group, an alcoholic hydroxyl group, a primary amine group, a secondary amino group, and a mercapto group. A phenolic hydroxyl group or an alcoholic hydroxyl group is preferred, and a phenolic hydroxyl group is more preferred. The number of active hydrogen groups that the specific compound has is preferably 1 or more, more preferably 2 or more, further preferably 2 to 10, and particularly preferably 2 to 6. The number of acid anhydride groups or imidazole ring groups contained in the specific compound is preferably 1 or more, more preferably 1 to 10, further preferably 1 to 3, and particularly preferably 1.
[0023] The specific compound is preferably a compound represented by formula (2).
[0024] [ka]
[0025] In formula (2), X 1 and X 2R represents an aromatic ring group which may have a substituent. z represents a substituent. z represents an integer of 0 to 4. A represents a single bond or an organic group having a valence of n+m. m and n represent integers of 1 or more.
[0026] X 1 and X 2 represents an aromatic ring group which may have a substituent. X 1 has the same meaning as X in the above formula (1), and the preferred range is also the same. X 2 The aromatic ring contained in the aromatic ring group represented by the following formula (I) may be either a monocyclic ring or a polycyclic ring. X 2 Examples of the aromatic ring group represented by the formula (I) include an aromatic hydrocarbon group and an aromatic heterocyclic group. The aromatic hydrocarbon group preferably has 6 to 20 carbon atoms, more preferably 6 to 12 carbon atoms, and even more preferably 6 to 10 carbon atoms. The aromatic heterocyclic group preferably has 3 to 20 carbon atoms, more preferably 5 to 12 carbon atoms, and even more preferably 5 to 10 carbon atoms. X 2 Examples of the aromatic ring group represented by the formula (I) include aromatic hydrocarbon groups such as a benzene ring group, a naphthalene ring group, and an anthracene ring group; and aromatic heterocyclic groups such as a furan ring group, a pyrrole ring group, a thiophene ring group, a pyridine ring group, a thiazole ring group, a carbazole ring group, an indole ring group, and a benzothiazole ring group. Of these, a benzene ring group, a naphthalene ring group, and an anthracene ring group are preferable, and a benzene ring group and a naphthalene ring group are more preferable. X 2 The aromatic ring group represented by the following formula (I) may have a substituent. The above-mentioned substituent has the same meaning as the substituent that X in the above-mentioned formula (1) may have, and the preferred range is also the same.
[0027] R z represents a substituent. R Z Examples of the substituent represented by the formula (I) include the groups exemplified in the group Y of substituents described above. Among these, a halogen atom (such as -F, -Br, -Cl, and -I), a hydroxyl group, an amino group, a carboxylic acid group, a hydrocarbon group having 1 to 6 carbon atoms, an aryl group, or a group consisting of a combination thereof is preferable, a hydroxyl group, an amino group, or a linear or branched alkyl group having 1 to 6 carbon atoms is more preferable, and a hydroxyl group, a methyl group, or an ethyl group is even more preferable.
[0028] z represents an integer of 0 to 4. Among them, z is preferably 0 to 3, more preferably 0 to 2, and further preferably 0 to 1. z If there are multiple, R z When m is 2 or more, multiple z's may be the same or different.
[0029] A represents a single bond or an n+m valent organic group. More specifically, when n and m are 1, A represents a single bond or a divalent organic group, and when at least one of n and m is 2 or more and the other is 1 or more, A represents an n+m valent organic group (a trivalent or higher organic group). Examples of the n+m valent organic group represented by A include groups in which n+m hydrogen atoms have been removed from a hydrocarbon which may have a heteroatom. Here, examples of the hydrocarbon that may have heteroatoms before removing the n+m hydrogen atoms include hydrocarbons selected from the group consisting of aliphatic hydrocarbons having 1 to 20 carbon atoms, aliphatic rings having 3 to 20 carbon atoms, and aromatic rings having 3 to 20 carbon atoms, and hydrocarbons formed by combining these. The n+m valent organic group further includes, in addition to the group obtained by removing n+m hydrogen atoms from the above-mentioned hydrocarbon which may have a hetero atom, -O-, -S-, -CO-, -NH-, -NR A It may be a group formed by combining one or more divalent linking groups selected from the group consisting of -, -SO2-, and -SO2-. R A R represents a substituent. A Examples of the substituent represented by the formula (I) include linear or branched alkyl groups having 1 to 6 carbon atoms. Examples of the aliphatic hydrocarbons having 1 to 20 carbon atoms include methane, ethane, propane, butane, pentane, hexane, and heptane. Examples of the aliphatic ring having 3 to 20 carbon atoms include a cyclohexane ring, a cycloheptane ring, a norbornane ring, and an adamantane ring. Examples of the aromatic ring having 3 to 20 carbon atoms include aromatic hydrocarbons having 6 to 20 carbon atoms and aromatic heterocycles having 3 to 20 carbon atoms. Examples of aromatic hydrocarbons having 6 to 20 carbon atoms include a benzene ring, a naphthalene ring, and an anthracene ring. Examples of the aromatic heterocycle having 3 to 20 carbon atoms include aromatic heterocycles having a nitrogen atom as a ring member atom, such as a triazine ring, a pyrazine ring, a pyrimidine ring, and a pyridine ring; a furan ring, a pyrrole ring, a thiophene ring, a thiazole ring, a carbazole ring, an indole ring, and a benzothiazole ring.
[0030] m and n represent integers of 1 or more. Among them, m is preferably 1 to 5, more preferably 1 to 3, and even more preferably 1 or 2. Furthermore, n is preferably 1 to 5, more preferably 1 to 3, and even more preferably 1 or 2, and particularly preferably 1. When n is 2 or more, a plurality of X's may be the same or different.
[0031] The specific compound is more preferably a compound represented by formula (3).
[0032] [ka]
[0033] In formula (3), X represents an aromatic ring group which may have a substituent. zrepresents a substituent. z represents an integer of 0 to 4. A represents a single bond or an organic group having a valence of n+m. m and n represent integers of 1 or more. Y represents a group obtained by removing n+m hydrogen atoms from a hydrocarbon which may have a heteroatom. L represents -O-, -S-, -CO-, -NH-, -NR A represents a group formed by combining one or more divalent linking groups selected from the group consisting of -, -SO2-, and -SO2-.
[0034] In formula (3), X, R z , z, m and n are X, R in formula (2). z , z, m and n have the same meanings and preferred ranges.
[0035] Y represents a group obtained by removing n+m hydrogen atoms from a hydrocarbon which may have a heteroatom. Y has the same meaning as the group obtained by removing n+m hydrogen atoms from a hydrocarbon which may have a heteroatom, which is exemplified as the n+m valent organic group represented by A described above. Among these, Y is preferably an aromatic ring group having 3 to 20 carbon atoms, more preferably at least one selected from the group consisting of an aromatic hydrocarbon group having 6 to 20 carbon atoms and an aromatic heterocyclic group having 3 to 20 carbon atoms, further preferably an aromatic heterocyclic group having 3 to 20 carbon atoms and containing a nitrogen atom, and particularly preferably a triazine ring group.
[0036] L is -O-, -S-, -CO-, -NH-, -NR A represents a group formed by combining one or more divalent linking groups selected from the group consisting of -, -SO2-, and -SO2-. Among these, L is -NH- and -NR A A group formed by combining one or more divalent linking groups selected from the group consisting of - is preferred, and -NH- is more preferred. A plurality of L's may be the same or different.
[0037] As the specific compound, a compound represented by formula (Z) is preferable, and a compound represented by formula (Z1) is more preferable.
[0038] [ka]
[0039] In formula (Z), E 1 ~E 3 each independently represents a single bond, -NH-, or -NR A - stands for R A represents a substituent. 1 represents a single bond or an organic group having a valence of a+1. 2 represents a single bond or a b+1 valent organic group. 3 represents a single bond or a c+1 valent organic group. 1 ~X 3 each independently represents a group represented by formula (1) or an aromatic ring group having a phenolic hydroxyl group. 1 ~X 3 At least one of the groups represents a group represented by formula (1). Each of a to c independently represents an integer of 0 or more, with the proviso that a+b+c is 1 or more.
[0040] E 1 ~E 3 each independently represents a single bond, -NH-, or -NR A - represents. E 1 ~E 3 Each of the groups independently represents -NH- or -NR A - is preferred, and -NH- is more preferred. A R represents a substituent. A Examples of the substituent represented by the formula (I) include linear or branched alkyl groups having 1 to 6 carbon atoms.
[0041] B 1 represents a single bond or an organic group having a valence of a+1. 2 represents a single bond or a b+1 valent organic group. 3 represents a single bond or a c+1 valent organic group. B 1 ~B 3 As the group, a single bond is preferable. The values of a to c in the a+1 valent organic group, the b+1 valent organic group, and the c+1 valent organic group coincide with the values of a to c clearly shown in formula (Z).
[0042] B 1 ~B 3 Examples of the organic group represented by the formula (1) include groups in which j hydrogen atoms have been removed from a hydrocarbon having 1 to 20 carbon atoms and which may have a heteroatom. Here, "j" means a+1, b+1, or c+1. Here, examples of the hydrocarbon that may have heteroatoms before removing the j hydrogen atoms include hydrocarbons selected from the group consisting of aliphatic hydrocarbons having 1 to 20 carbon atoms, aliphatic rings having 3 to 20 carbon atoms, and aromatic rings having 3 to 20 carbon atoms, and hydrocarbons formed by combining these. B 1 ~B 3 The organic group represented by the formula (I) further comprises -O-, -S-, -CO-, -NH-, -NR A R may be a group formed by combining one or more divalent linking groups selected from the group consisting of -, -SO2-, and -SO2-. A is the above-mentioned R A is synonymous with. Examples of the aliphatic hydrocarbons having 1 to 20 carbon atoms include methane, ethane, propane, butane, pentane, hexane, and heptane. Examples of the aliphatic ring having 3 to 20 carbon atoms include a cyclohexane ring, a cycloheptane ring, a norbornane ring, and an adamantane ring. Examples of the aromatic ring having 3 to 20 carbon atoms include aromatic hydrocarbons having 6 to 20 carbon atoms and aromatic heterocycles having 3 to 20 carbon atoms. Examples of aromatic hydrocarbons having 6 to 20 carbon atoms include a benzene ring, a naphthalene ring, and an anthracene ring. Examples of the aromatic heterocycle having 3 to 20 carbon atoms include aromatic heterocycles having a nitrogen atom as a ring member atom, such as a triazine ring, a pyrazine ring, a pyrimidine ring, and a pyridine ring; a furan ring, a pyrrole ring, a thiophene ring, a thiazole ring, a carbazole ring, an indole ring, and a benzothiazole ring.
[0043] a to c each independently represent an integer of 0 or more. Each of a to c is preferably 1 to 5, more preferably 1 to 2, and even more preferably 1. For example, a is preferably 1 or more (e.g., 1 to 2), b is preferably 1 or more (e.g., 1 to 2), and c is preferably 1 or more (e.g., 1 to 2). When a is 0, B 1 isX 1 If b is 0, then B 2 isX 2 If c is 0, then B 3 isX 3 does not have Also, B 1 If is a single bond, a is 1. 2 When is a single bond, b is 1. 3 If is a single bond, c is 1. However, a+b+c is 1 or more, preferably 2 to 10, and more preferably 2 to 4.
[0044] X 1 ~X 3 each independently represents a group represented by formula (1) or an aromatic ring group having a phenolic hydroxyl group. 1 ~X 3 At least one of these represents a group represented by formula (1). The group represented by formula (1) has the same definition as the group represented by formula (1) in the above-mentioned specific compound, and the preferred range is also the same.
[0045] The "aromatic ring group having a phenolic hydroxyl group" may be an aromatic ring group having one or more (for example, 1 to 4) hydroxyl groups (phenolic hydroxyl groups) directly bonded to the aromatic ring. The aromatic ring group may or may not have a substituent other than the phenolic hydroxyl group. The aromatic ring of the aromatic ring group may be a monocyclic or polycyclic ring, and may have a heteroatom as a ring member atom. The number of ring members of the aromatic ring group is preferably 5 to 15, more preferably 6 to 10, and further preferably 6. The aromatic ring group is preferably a benzene ring group. The substituent that the aromatic ring group may have other than the hydroxyl group is preferably a substituent having 1 to 6 carbon atoms, more preferably a hydrocarbon group having 1 to 6 carbon atoms, further preferably a linear or branched alkyl group having 1 to 6 carbon atoms, and particularly preferably a methyl group or an ethyl group.
[0046] X with a occurrences 1 , b pieces of X 2 , and c X's 3 It is also preferable that at least one of them has a substituent arranged at the ortho position of the sulfonamide group or the ortho position of the phenolic hydroxyl group in the group represented by formula (1), and it is more preferable that it has a substituent arranged at the ortho position of the phenolic hydroxyl group. The ortho-positioned substituents include the above-mentioned R z Examples of the substituent include those represented by the following formula: X having a substituent located at the ortho position of the sulfonamide group or the ortho position of the phenolic hydroxyl group in the group represented by formula (1) 1 ~X 3 is (a+b+c) pieces of X 1 ~X 3 The upper limit is preferably 100% or less, more preferably 90% or less, and even more preferably 80% or less.
[0047] X having a substituent at the ortho position 1 ~X 3 may further have a substituent, for example, a hydroxyphenyl group.
[0048] [ka]
[0049] In formula (Z1), R z1 ~R z3 each independently represents a substituent. z1 to z3 each independently represents an integer of 0 to 4. R z1 ~R z3 is R in the above formula (2). z The same definition and preferred range are also the same. z1 to z3 are preferably 0 to 3, more preferably 0 to 2, and further preferably 0 to 1. R z1 ~R z3 In the benzene ring group to which R z1 ~R z3 is preferably bonded at the ortho position relative to the hydroxyl group or sulfonamide group bonded to the benzene ring group.
[0050] Specific examples of the specific compound are shown below, but the present invention is not limited thereto.
[0051] [ka]
[0052] [ka]
[0053] The molecular weight of the specific compound is preferably from 225 to 2,000, and more preferably from 225 to 1,000.
[0054] The hydroxyl group content of the specific compound is preferably 1.0 mmol / g or more, more preferably 2.0 mmol / g or more, and the upper limit is preferably 25.0 mmol / g or less, more preferably 10.0 mmol / g or less. The hydroxyl group content refers to the number of hydroxyl groups (preferably phenolic hydroxyl groups) contained in 1g of the specific compound. In addition, the specific compound may or may not have an active hydrogen-containing group (such as a carboxylic acid group) capable of polymerizing with an epoxy compound other than a hydroxyl group. The lower limit of the active hydrogen content of the specific compound (the total content of hydrogen atoms in the hydroxyl group and the carboxylic acid group) is preferably 1.0 mmol / g or more, more preferably 2.0 mmol / g or more. The upper limit is preferably 25.0 mmol / g or less, more preferably 10.0 mmol / g or less.
[0055] The specific compound may be used alone or in combination of two or more. The content of the specific compound is preferably from 1 to 40 mass %, more preferably from 3 to 30 mass %, and even more preferably from 5 to 20 mass %, based on the total solid content of the composition. The solid content refers to the components that form the thermally conductive material (cured product) and does not include solvents. The components that form the thermally conductive material (cured product) may be components that undergo a reaction (polymerization) and change their chemical structure when forming the thermally conductive material (cured product). In addition, any component that forms a thermally conductive material is considered to be a solid content even if it is in a liquid state.
[0056] [Epoxy Compound] The composition of the present invention includes an epoxy compound. An epoxy compound is a compound having at least one epoxy group (oxiranyl group) in one molecule. The epoxy group may or may not have a substituent. The number of epoxy groups in the epoxy compound is preferably 2 or more, more preferably 2 to 40, further preferably 2 to 10, and particularly preferably 2, in one molecule. The molecular weight of the epoxy compound is preferably 150-10,000, more preferably 150-2,000, and even more preferably 200-400.
[0057] The lower limit of the epoxy group content of the epoxy compound is preferably 2.0 mmol / g or more, more preferably 4.0 mmol / g or more, and even more preferably 5.0 mmol / g or more, and the upper limit is preferably 20.0 mmol / g or less, more preferably 15.0 mmol / g or less, and even more preferably 10.0 mmol / g or less. The term "epoxy group content" refers to the number of epoxy groups contained in 1 g of an epoxy compound.
[0058] The epoxy compound may or may not exhibit liquid crystallinity. In other words, the epoxy compound may be a liquid crystal compound. In other words, a liquid crystal compound having an epoxy group can also be used as the epoxy compound. Examples of the epoxy compound (which may be a liquid crystalline epoxy compound) include a compound having at least a partial rod-shaped structure (rod-shaped compound) and a compound having at least a partial discotic structure (disk-shaped compound). Among these, rod-shaped compounds are preferred since the resulting thermally conductive material has better thermal conductivity. The rod-shaped compounds and discotic compounds will be described in detail below.
[0059] (rod-shaped compound) Examples of epoxy compounds that are rod-shaped compounds include azomethines, azoxys, cyanobiphenyls, cyanophenyl esters, benzoates, cyclohexane carboxylic acid phenyl esters, cyanophenylcyclohexanes, cyano-substituted phenylpyrimidines, alkoxy-substituted phenylpyrimidines, phenyldioxanes, tolanes, and alkenylcyclohexylbenzonitriles. Not only the low molecular weight compounds as described above, but also polymer compounds can be used. The polymer compounds are polymer compounds obtained by polymerizing rod-shaped compounds having low molecular weight reactive groups. The rod-like compound is preferably a compound represented by formula (E1).
[0060] [ka]
[0061] In formula (E1), L E1 each independently represents a single bond or a divalent linking group. Among them, L E1 is preferably a divalent linking group. The divalent linking group is preferably -O-, -S-, -CO-, -NH-, -CH=CH-, -C≡C-, -CH=N-, -N=N-, an alkylene group which may have a substituent, or a group consisting of a combination of two or more of these, and more preferably an -O-alkylene group-. The alkylene group may be linear, branched, or cyclic, and is preferably a linear alkylene group having 1 to 2 carbon atoms. Multiple Ls E1 may be the same or different.
[0062] In formula (E1), L E2 are each independently a single bond, -CH=CH-, -CO-O-, -C(-CH3)=CH-, -CH=N-, -N=N-, -C≡C-, -N=N + (-O - )-, -CH=N + (-O - )-, -CH=CH-CO-, or -CH=C(-CN)-. Among them, L E2 are each independently preferably a single bond or -CO-O-. L E2 If there are multiple L E2 may be the same or different.
[0063] In formula (E1), L E3 each independently represents a single bond, an optionally substituted 5- or 6-membered aromatic ring group, an optionally substituted 5- or 6-membered non-aromatic ring group, or a polycyclic group consisting of these rings. L E3Examples of the aromatic ring group and non-aromatic ring group represented by the formula (1) include a 1,4-cyclohexanediyl group, a 1,4-cyclohexenediyl group, a 1,4-phenylene group, a pyrimidine-2,5-diyl group, a pyridine-2,5-diyl group, a 1,3,4-thiadiazole-2,5-diyl group, a 1,3,4-oxadiazole-2,5-diyl group, a naphthalene-2,6-diyl group, a naphthalene-1,5-diyl group, a thiophene-2,5-diyl group, and a pyridazine-3,6-diyl group, which may have a substituent. In the case of a 1,4-cyclohexanediyl group, it may be either a trans or cis structural isomer, or a mixture of any ratio. Among them, the trans isomer is preferred. Among them, L E3 is preferably a single bond, a 1,4-phenylene group, or a 1,4-cyclohexenediyl group. L E3 Each of the substituents possessed by the group represented by the following formula (1) is preferably an alkyl group, an alkoxy group, a halogen atom, a cyano group, a nitro group, or an acetyl group, and more preferably an alkyl group (preferably having one carbon atom). When a plurality of substituents are present, the substituents may be the same or different. L E3 If there are multiple L E3 may be the same or different.
[0064] In formula (E1), pe represents an integer of 0 or more. If pe is an integer greater than or equal to 2, there are multiple (-L E3 -L E2 -) may be the same or different. Among them, pe is preferably 0 to 2, more preferably 0 or 1, and even more preferably 0.
[0065] In formula (E1), L E4 each independently represents a substituent. The substituents are each independently preferably an alkyl group, an alkoxy group, a halogen atom, a cyano group, a nitro group, or an acetyl group, and more preferably an alkyl group (preferably having one carbon atom). Multiple Ls E4 may be the same or different. In addition, when le, which will be described next, is an integer of 2 or more, the same (L E4 ) le There are multiple L's in E4 may be the same or different.
[0066] In formula (E1), each le independently represents an integer of 0 to 4. Among them, it is preferable that each le is independently 0 to 2. Multiple le's may be the same or different.
[0067] The rod-like compound also preferably has a biphenyl skeleton.
[0068] (Discoid Compound) The epoxy compound which is a discotic compound has at least a partial discotic structure. The discotic structure has at least an alicyclic ring or an aromatic ring. In particular, when the discotic structure has an aromatic ring, the discotic compound can form a columnar structure by forming a stacking structure due to intermolecular π-π interactions. Examples of the discotic structure include the triphenylene structure described in Angew. Chem. Int. Ed. 2012, 51, 7990-7993 and JP-A-7-306317, and the tri-substituted benzene structure described in JP-A-2007-002220 and JP-A-2010-244038.
[0069] The discotic compound preferably has 3 or more epoxy groups. The cured product of the epoxy compound containing the discotic compound having 3 or more epoxy groups tends to have a high glass transition temperature and high heat resistance. The number of epoxy groups in the discotic compound is preferably 8 or less, more preferably 6 or less.
[0070] Examples of the discotic compound include those described in C. Destrade et al., Mol. Crysr. Liq. Cryst., vol. 71, page 111 (1981); Quarterly Review of Chemistry, No. 22, Chemistry of Liquid Crystals, edited by the Chemical Society of Japan, Chapter 5, Chapter 10, Section 2 (1994); B. Kohne et al., Angew. Chem. Soc. Chem. Comm., page 1794 (1985); J. Zhang et al., J. Am. Chem. Soc., vol. 116, page 2655 (1994), and Japanese Patent No. 4592225, in which at least one (preferably three or more) of the terminals are epoxy groups. Examples of the discotic compound include the triphenylene structure described in Angew. Chem. Int. Ed. 2012, 51, 7990-7993 and JP-A-7-306317, and the trisubstituted benzene structure described in JP-A-2007-002220 and JP-A-2010-244038 in which at least one (preferably three or more) of the terminals is an epoxy group.
[0071] In addition to the above-mentioned epoxy compounds, the epoxy compound may be, for example, an epoxy compound represented by the formula (DN).
[0072] [ka]
[0073] In formula (DN), n DN represents an integer of 0 or more, preferably 0 to 5, and more preferably 1. R DN represents a single bond or a divalent linking group. The divalent linking group is preferably -O-, -O-CO-, -S-, an alkylene group (preferably having 1 to 10 carbon atoms), an arylene group (preferably having 6 to 20 carbon atoms), or a group consisting of a combination thereof, more preferably an alkylene group, and further preferably a methylene group.
[0074] The epoxy compound is a compound represented by the above formula (Z), 1 ~X 3 may each independently represent "an aromatic ring group that is a monovalent group having an epoxy group."
[0075] The epoxy compound may be, for example, a bisphenol A type epoxy compound, which is a glycidyl ether of bisphenol A, F, S, AD, or the like (in the above formula (E1), "pe=0" and "L E2 -C(CH3)2-"), bisphenol F type epoxy compound (compounds in which "pe=0" and "L E2 -CH2-" compounds, bisphenol S type epoxy compounds, bisphenol AD type epoxy compounds, etc.; hydrogenated bisphenol A type epoxy compounds, hydrogenated bisphenol AD type epoxy compounds, etc.; phenol novolac type glycidyl ethers (phenol novolac type epoxy compounds), cresol novolac type glycidyl ethers (cresol novolac type epoxy compounds), bisphenol A novolac type glycidyl ethers, etc.; dicyclopentadiene type glycidyl ethers (dicyclopentadiene type epoxy compounds); dihydroxypentadiene type glycidyl ethers (dihydroxypentadiene type epoxy compounds); polyhydroxybenzene type glycidyl ethers (polyhydroxybenzene type epoxy compounds); benzene polycarboxylic acid type glycidyl esters (benzene polycarboxylic acid type epoxy compounds); alicyclic epoxy compounds such as 3,4:8,9-diepoxybicyclo[4.3.0]nonane, and trisphenol methane type epoxy compounds. A compound in which one or more of the glycidyl ether groups and / or glycidyl ester groups in each of the above-mentioned compounds are replaced with a diglycidylamino group or a diglycidylaminoalkylene group (such as a diglycidylaminomethylene group) may be used as the epoxy compound. Each of the above compounds may have a substituent. For example, the aromatic ring group, the cycloalkane ring group, and / or the alkylene group contained in each of the above compounds may have a substituent other than a glycidyl ether group, a glycidyl ester group, a diglycidylamino group, and / or a diglycidylaminoalkylene group. Among them, the epoxy compound is preferably a bisphenol F type epoxy compound or a polyhydroxybenzene type glycidyl ether (such as a dihydroxybenzene type glycidyl ether).
[0076] The epoxy compounds may be used alone or in combination of two or more. The content of the epoxy compound is preferably from 1.0 to 25.0 mass%, more preferably from 3.0 to 20.0 mass%, further preferably from 5.0 to 20.0 mass%, particularly preferably from 9.0 to 18.0 mass%, based on the total solid content of the composition.
[0077] The chemical equivalent of the specific compound is preferably 0.01 to 5 equivalents, more preferably 0.3 to 2.0 equivalents, further preferably 0.5 to 1.5 equivalents, and particularly preferably 0.8 to 1.5 equivalents, relative to 1 mole of epoxy groups in the epoxy compound.
[0078] In the composition, the total content of the epoxy compound and the specific compound is preferably from 5 to 90 mass %, more preferably from 10 to 50 mass %, and even more preferably from 15 to 40 mass %, based on the total solid content of the composition.
[0079] The ratio of the number of epoxy groups contained in the epoxy compound to the number of phenolic hydroxyl groups contained in the specific compound [number of epoxy groups / number of phenolic hydroxyl groups] is preferably 20 / 80 to 800 / 20, more preferably 30 / 70 to 70 / 30, and even more preferably 40 / 60 to 60 / 40. In other words, the ratio of the contents of the specific compound and the epoxy compound in the composition is preferably such that the above-mentioned "number of epoxy groups / number of phenolic hydroxyl groups" falls within the above-mentioned range.
[0080] [Curing Accelerator] The composition of the present invention may further comprise a cure accelerator. Examples of the curing accelerator include tris orthotolylphosphine, triphenylphosphine, boron trifluoride amine complex, and the compounds described in paragraph
[0052] of JP 2012-067225 A. Also included are onium salt-based curing accelerators such as quaternary phosphonium compounds (phosphonium salts) such as tetraphenylphosphonium tetraphenylborate (TPP-K), tetraphenylphosphonium tetra-p-tolylborate (TPP-MK), tetra-n-butylphosphonium laurate (TBP-LA), bis(tetra-n-butylphosphonium)pyromellitate, and tetraphenylphosphonium bis(naphthalene-2,3-dioxy)phenylsilicate adducts. Other examples include 2-methylimidazole (trade name: 2MZ), 2-undecylimidazole (trade name: C11-Z), 2-heptadecylimidazole (trade name: C17Z), 1,2-dimethylimidazole (trade name: 1.2DMZ), 2-ethyl-4-methylimidazole (trade name: 2E4MZ), 2-phenylimidazole (trade name: 2PZ), 2-phenyl-4-methylimidazole (trade name: 2P4MZ), 1-benzyl-2-methylimidazole (trade name: 1B2 ... 1-cyanoethyl-2-phenylimidazole (trade name; 1B2PZ), 1-cyanoethyl-2-methylimidazole (trade name; 2MZ-CN), 1-cyanoethyl-2-undecylimidazole (trade name; C11Z-CN), 1-cyanoethyl-2-phenylimidazolium trimellitate (trade name; 2PZCNS-PW), 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine (trade name; 2MZ-A), 2,4-diamino-6-[2'-undecylimidazolyl -(1')]-ethyl-s-triazine (trade name; C11Z-A), 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine (trade name; 2E4MZ-A), 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct (trade name; 2MA-OK), 2-phenyl-4,5-dihydroxymethylimidazole (trade name; 2PHZ-PW), 2-phenyl-4-methyl-5- ... Examples of the imidazole-based curing accelerator include 2P4MHZ-PW, 2PZ-CN, 2MZA-PW, and 2MAOK-PW, which are all manufactured by Shikoku Chemical Industry Co., Ltd. Chilimidazole (trade name), 2P4MHZ-PW, 1-cyanoethyl-2-phenylimidazole (trade name), 2MZA-PW, and 2MAOK-PW, which are all manufactured by Shikoku Chemical Industry Co., Ltd. Furthermore, examples of the triarylphosphine-based curing accelerator include the compounds described in JP-A-2004-043405, paragraph
[0052] .Examples of phosphorus-based curing accelerators in which triphenylborane is added to triarylphosphine include the compounds described in paragraph
[0024] of JP2014-005382A.
[0081] Among them, the curing accelerator preferably contains a compound containing a phosphorus atom, and also preferably contains a phosphonium salt. The curing accelerator may be a compound containing a phosphorus atom or a phosphonium salt itself. When a phosphonium salt is used as the curing accelerator, the storage stability of the semi-cured film formed from the composition is improved. The content of the phosphorus atom-containing compound or phosphonium salt is preferably from 10 to 100 mass %, more preferably from 50 to 100 mass %, and further preferably from 80 to 100 mass %, based on the total mass of the curing accelerator.
[0082] The curing accelerator may be used alone or in combination of two or more kinds. The content of the curing accelerator is preferably 0.002% by mass or more, more preferably 0.02% by mass or more, even more preferably 0.10% by mass or more, and particularly preferably 0.20% by mass or more, based on the total solid content of the composition. The upper limit is preferably 5.00% by mass or less, more preferably 2.00% by mass or less, even more preferably 1.00% by mass or less, and particularly preferably 0.50% by mass or less, based on the total solid content of the composition. The content of the curing accelerator is preferably 0.01% by mass or more, more preferably 0.02% by mass or more, and even more preferably 0.03% by mass or more, based on the total epoxy compounds. The upper limit is preferably 40.0% by mass or less, more preferably 10.0% by mass or less, even more preferably 1.0% by mass or less, particularly preferably 0.1% by mass or less, and most preferably 0.05% by mass or less, based on the total epoxy compounds.
[0083] [Inorganic substances] The composition of the present invention may further contain an inorganic substance. The inorganic substance may be any inorganic substance that has been used as an inorganic filler in a conventional thermal conductive material. In order to provide the thermal conductive material with superior thermal conductivity and insulating properties, the inorganic substance preferably contains an inorganic nitride or an inorganic oxide, and more preferably contains at least an inorganic nitride.
[0084] The shape of the inorganic material is not particularly limited, and may be particulate, film-like, or plate-like. Examples of the shape of the particulate inorganic material include rice grain-like, spherical, cubic, spindle-like, scaly, aggregated, and amorphous.
[0085] Examples of inorganic nitrides include boron nitride (BN), carbon nitride (C3N4), silicon nitride (Si3N4), gallium nitride (GaN), indium nitride (InN), aluminum nitride (AlN), chromium nitride (Cr2N), copper nitride (Cu3N), iron nitride (Fe4N), iron nitride (Fe3N), lanthanum nitride (LaN), lithium nitride (Li3N), magnesium nitride (Mg3N2), molybdenum nitride (Mo2N), niobium nitride (NbN), tantalum nitride (TaN), titanium nitride (TiN), tungsten nitride (W2N), tungsten nitride (WN2), yttrium nitride (YN), and zirconium nitride (ZrN). The inorganic nitrides may be used alone or in combination of two or more. The inorganic nitride preferably contains an aluminum atom, a boron atom, or a silicon atom, more preferably contains aluminum nitride, boron nitride, or silicon nitride, even more preferably contains aluminum nitride or boron nitride, and particularly preferably contains boron nitride.
[0086] Examples of inorganic oxides include silicon oxide (silica, SiO2), aluminum oxide (alumina, Al2O3), magnesium oxide (MgO), zirconium oxide (ZrO2), titanium oxide (TiO2), iron oxide (Fe2O3, FeO, Fe3O4), copper oxide (CuO, Cu2O), zinc oxide (ZnO), yttrium oxide (Y2O3), niobium oxide (Nb2O5), molybdenum oxide (MoO3), and indium oxide. Examples of oxides include lead oxide (PbO, PbO2), bismuth oxide (Bi2O3), cerium oxide (CeO2, Ce2O3), antimony oxide (Sb2O3, Sb2O5), germanium oxide (GeO2, GeO), lanthanum oxide (La2O3), and ruthenium oxide (RuO2). The inorganic oxides may be used alone or in combination of two or more. The inorganic oxide may be an oxide that is produced when a metal prepared as a non-oxide is oxidized in the environment or the like.
[0087] The size of the inorganic substance is not particularly limited, but from the viewpoint of superior dispersibility of the inorganic substance, the average particle size of the inorganic substance is preferably 500 μm or less, more preferably 300 μm or less, even more preferably 200 μm or less, and particularly preferably 100 μm or less. The lower limit is not particularly limited, but from the viewpoint of handleability, it is preferably 10 nm or more, more preferably 100 nm or more, and even more preferably 10 μm or more. When a commercially available product is used, the average particle size of the inorganic substance is determined by the catalog value. If no catalog value is available, the average particle size is determined by randomly selecting 100 inorganic substances using an electron microscope, measuring the particle size (major axis) of each inorganic substance, and calculating the arithmetic average.
[0088] Among these, the inorganic substance preferably contains one or more selected from the group consisting of boron nitride, alumina, silica, silicon nitride, and magnesium oxide, and more preferably contains boron nitride. The inorganic material may include boron nitride, alumina, silica, silicon nitride, and / or magnesium oxide as a portion thereof, or the inorganic material may be boron nitride, alumina, silica, silicon nitride, and / or magnesium oxide itself. The content of boron nitride, alumina, silica, silicon nitride, and / or magnesium oxide (the total content when a plurality of these are included) is preferably 10 to 100 mass%, more preferably 40 to 100 mass%, and even more preferably 80 to 100 mass%, based on the total mass of the inorganic substance.
[0089] The inorganic substances may be used alone or in combination of two or more. The inorganic material preferably contains at least one of an inorganic nitride and an inorganic oxide, and more preferably contains at least an inorganic nitride. The inorganic material may contain both an inorganic nitride and an inorganic oxide. The content of the inorganic nitride (preferably boron nitride) in the inorganic substance is preferably from 10 to 100 mass %, more preferably from 40 to 100 mass %, and further preferably from 80 to 100 mass %, based on the total mass of the inorganic substance.
[0090] In order to provide a thermally conductive material with superior thermal conductivity, it is preferable that the composition contains at least an inorganic substance (preferably an inorganic nitride or inorganic oxide, more preferably an inorganic nitride, even more preferably boron nitride, and particularly preferably agglomerated boron nitride) having an average particle size of 20 μm or more (preferably 30 μm or more).
[0091] It is also preferable that the inorganic substance (preferably inorganic nitride or inorganic oxide) contained in the composition is substantially only inorganic substance X having an average particle size of 20 μm or more (preferably 30 μm or more). The inorganic substance being substantially only inorganic substance X having an average particle size of 20 μm or more means that the content of inorganic substance X having an average particle size of 20 μm or more is more than 99 mass% with respect to the total mass of the inorganic substance.
[0092] It is also preferable that the inorganic substances have different average particle sizes. For example, it is preferable to include both inorganic substance X, which is an inorganic substance having an average particle size of 20 μm or more, and inorganic substance Y, which is an inorganic substance having an average particle size of less than 20 μm. The inorganic substance X has an average particle size of preferably 20 to 300 μm, more preferably 30 to 200 μm.The inorganic substance Y has an average particle size of preferably 1 nm or more and less than 20 μm, more preferably 10 nm to 10 μm. The inorganic substance X is preferably an inorganic nitride or an inorganic oxide, more preferably an inorganic nitride, further preferably boron nitride, and particularly preferably aggregated boron nitride. The inorganic substance Y is preferably an inorganic nitride or an inorganic oxide, more preferably boron nitride or aluminum oxide. The inorganic substance X and the inorganic substance Y may each be used alone or in combination of two or more. The mass ratio of the content of inorganic substance X to the content of inorganic substance Y (content of inorganic substance X / content of inorganic substance Y) among the inorganic substances is preferably 50 / 50 to 99 / 1, more preferably 60 / 40 to 95 / 5.
[0093] The inorganic substance (particularly boron nitride) may be surface-treated. Note that the "surface treatment" refers to a treatment different from the surface modification using a surface modifier, which will be described later. It is believed that such treatment introduces functional groups onto the surface of the inorganic material, making it easier for the inorganic material to interact with specific compounds, epoxy compounds, and / or the surface modifiers described below, thereby further improving the thermal conductivity and peel strength of the thermally conductive material formed. Examples of surface treatments include plasma treatments (vacuum plasma treatment, atmospheric plasma treatment, aqua plasma treatment, etc.), ultraviolet irradiation treatment, corona treatment, electron beam irradiation treatment, ozone treatment, baking treatment, flame treatment, and oxidizing agent treatment. The oxidizing agent treatment may be performed under acidic conditions or basic conditions (e.g., pH 12 or higher).
[0094] The content of the inorganic substance (preferably one or more selected from the group consisting of boron nitride, alumina, silica, silicon nitride, and magnesium oxide) in the composition is preferably 10% by mass or more, more preferably 40% by mass or more, even more preferably 50% by mass or more, and particularly preferably 60% by mass or more, based on the total solid content of the composition. The upper limit is preferably less than 100% by mass, and more preferably 95% by mass or less.
[0095] [Surface modifiers, surface-modified inorganic substances] The composition of the present invention may further contain a surface modifier as a component different from the above-mentioned components. The surface modifier is a component that modifies the surface of the inorganic substance described above. In this specification, "surface modification" means a state in which an organic substance is adsorbed on at least a part of the surface of an inorganic substance. The form of adsorption is not particularly limited as long as it is in a bonded state. In other words, the surface modification also includes a state in which an organic group obtained by part of the organic substance being detached is bonded to the surface of the inorganic substance. The bond may be any bond such as a covalent bond, a coordinate bond, an ionic bond, a hydrogen bond, a van der Waals bond, and a metal bond. The surface modification may be a monolayer formed on at least a part of the surface. The monolayer is a monolayer film formed by chemical adsorption of organic molecules, and is known as a Self-Assembled MonoLayer (SAM). In this specification, the surface modification may be only a part of the surface of the inorganic substance, or the entire surface.
[0096] As used herein, a "surface-modified inorganic material" refers to an inorganic material that has been surface-modified with a surface modifier, i.e., a surface-modified inorganic material is a material that includes an inorganic material and a surface modifier adsorbed onto the surface of the inorganic material. That is, in the composition of the present invention, the inorganic substance may constitute a surface-modified inorganic substance together with the surface modifier adsorbed onto the surface of the inorganic substance. In the present invention, the composition may contain a surface-modified inorganic material, whereby the composition contains an inorganic material and a surface modifier. A part or all of the inorganic substance in the composition may constitute the surface-modified inorganic substance together with the surface modifier. For example, in the composition, some inorganic substances may constitute the surface-modified inorganic substance, and at the same time, inorganic substances may be present that are not involved in the constitution of the surface-modified inorganic substance. A part or all of the surface modifier in the composition may constitute the surface-modified inorganic substance together with the inorganic substance. For example, in the composition, a part of the surface modifier may constitute the surface-modified inorganic substance, and at the same time, a surface modifier that is not involved in the constitution of the surface-modified inorganic substance may be present. In particular, the composition preferably contains a surface-modified inorganic nitride (preferably surface-modified boron nitride) in which the inorganic substance constituting the surface-modified inorganic substance is an inorganic nitride (preferably boron nitride, more preferably agglomerated boron nitride having an average particle size of 20 μm or more, and even more preferably agglomerated boron nitride having an average particle size of 20 to 100 μm). A part or all of the inorganic nitride (preferably boron nitride) in the composition may constitute the surface-modified inorganic nitride (preferably surface-modified boron nitride) together with a surface modifier. The composition may also contain a surface-modified inorganic oxide (preferably surface-modified aluminum) in which the inorganic substance constituting the surface-modified inorganic substance is an inorganic oxide (preferably aluminum oxide). A part or all of the inorganic oxide (preferably aluminum oxide) in the composition may constitute the surface-modified inorganic oxide (preferably surface-modified aluminum oxide) together with a surface modifier. The surface-modified inorganic material can be formed, for example, by contacting an inorganic material with a surface modifier. For example, the inorganic material, the surface modifier, and other components constituting the composition of the present invention may be mixed together to form the surface-modified inorganic material in the composition during the process of producing the composition of the present invention. Alternatively, for example, an inorganic substance and a surface modifier may be mixed in a solvent to prepare a mixed liquid containing the surface-modified inorganic substance, and the surface-modified inorganic substance may be separated from the mixed liquid by a means such as filtration to obtain a separated surface-modified inorganic substance. The separated surface-modified inorganic substance may be used to prepare a composition of the present invention.
[0097] As the surface modifier, a conventionally known surface modifier such as a carboxylic acid such as a long-chain alkyl fatty acid, an organic phosphonic acid, an organic phosphoric acid ester, an organic silane molecule (silane coupling agent), etc. may be used. In addition, for example, the surface modifiers described in JP-A-2009-502529, JP-A-2001-192500, and Japanese Patent No. 4694929 may be used.
[0098] The silane coupling agent is, for example, a compound having a hydrolyzable group directly bonded to a Si atom. Examples of the hydrolyzable group include an alkoxy group (preferably having 1 to 10 carbon atoms) and a halogen atom such as a chlorine atom. The number of hydrolyzable groups directly bonded to Si atoms in the silane coupling agent is preferably 1 or more, more preferably 2 or more, and even more preferably 3 or more. The upper limit is preferably 10,000 or less. It is also preferable that the silane coupling agent has a reactive group. Specific examples of the reactive group include an epoxy group, an oxetanyl group, a vinyl group, a (meth)acrylic group, a styryl group, an amino group, an isocyanate group, a mercapto group, and an acid anhydride group. The number of reactive groups in the silane coupling agent is preferably 1 or more, more preferably 2 or more, and even more preferably 3 or more. There is no upper limit to the number, and it is, for example, 10,000. Examples of silane coupling agents include 3-aminopropyltriethoxysilane, 3-(2-aminoethyl)aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-(2-aminoethyl)aminopropyltrimethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, 3-mercaptotriethoxysilane, 3-ureidopropyltriethoxysilane, and 3-glycidoxypropyltrimethoxysilane.
[0099] When the composition of the present invention contains a surface modifier, a surface-modified inorganic substance may be prepared in advance and used as a part of the raw material of the composition. That is, the surface-modified inorganic substance prepared in advance may be mixed with other various components of the composition, so that all or a part of the surface modifier and the inorganic substance are introduced into the composition in a form contained in the surface-modified inorganic substance prepared in advance. In addition, a surface modifier and / or an inorganic substance that is not in a state of forming a surface-modified inorganic substance other than the surface modifier and the inorganic substance introduced in the form contained in the surface-modified inorganic substance may be mixed with other components of the composition to introduce all or a part of the surface modifier and / or the inorganic substance into the composition. In this case, it is also preferable that the surface modifier is adsorbed on the surface of the inorganic substance during the mixing process to form a surface-modified inorganic substance in the composition. In this case, a part of the surface modifier may be present in the composition in a state that does not contribute to the formation of the surface-modified inorganic substance.
[0100] The surface modifier may be used alone or in combination of two or more kinds. When the composition contains a surface modifier, the content of the surface modifier is preferably from 0.005 to 5 mass %, more preferably from 0.05 to 3 mass %, based on the total solid content of the composition. When the composition contains a surface modifier, the content of the surface modifier is preferably from 0.01 to 10 mass %, more preferably from 0.10 to 5 mass %, based on the total inorganic substances. The mass ratio of the surface modifier to the inorganic substance in the surface-modified inorganic substance (mass of the surface modifier adsorbed on the surface of the inorganic substance / mass of the inorganic substance) is preferably 0.00001 to 0.5, and more preferably 0.0001 to 0.1. When the composition contains a surface-modified inorganic material, the content of the surface-modified inorganic material is preferably 20% by mass or more, more preferably 50% by mass or more, even more preferably 60% by mass or more, and particularly preferably 75% by mass or more, based on the total solid content of the composition. The upper limit is preferably less than 100% by mass, more preferably 95% by mass or less, and even more preferably 80% by mass or less. When the composition contains a surface-modified nitride (preferably surface-modified boron nitride), the content of the surface-modified nitride (preferably surface-modified boron nitride) is preferably 10 to 100 mass%, more preferably 40 to 100 mass%, and even more preferably 60 to 100 mass%, based on the total surface-modified inorganic substances.
[0101] [Ion Scavenger] The composition of the present invention may further comprise an ion scavenger. The ion scavenger adsorbs ionic impurities in the composition or in a thermally conductive material formed using the composition, thereby allowing the insulating properties of the thermally conductive material to be better maintained even if the composition or thermally conductive material absorbs moisture. Examples of the ion trapping agent include inorganic ion trapping agents and organic ion trapping agents. Examples of the organic ion trapping agent include triazine thiol compounds, triazine amine compounds, benzimidazole compounds, benzotriazole compounds, aminotriazole compounds, and bisphenol reducing agents. All or a part of the above-mentioned inorganic substances may also function as ion scavengers.
[0102] An example of the triazine thiol compound is 2-dibutylamino-4,6-dimercapto-s-triazine. The benzimidazole compound includes, for example, benzimidazole. Examples of benzotriazole compounds include 1H-benzotriazole, carboxybenzotriazole, 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, and 2,2'-methylenebis[6-(2H-benzotriazol-2-yl)-4-tert-octylphenol]. Examples of aminotriazole compounds include 3-amino-1,2,4-triazole and 3,5-diamino-1,2,4-triazole. Examples of bisphenol reducing agents include 2,2'-methylenebis-(4-ethyl-6-t-butylphenol) and 4,4'-butylidenebis-(6-t-butyl-3-methylphenol).
[0103] The ion scavenger may be a commercially available product, and examples thereof include DHF-4A, DHT-4A, DHT-4A-2, DHT-4C, Kyoward 500, KW-2000, and KW-2100 (trade names, manufactured by Kyowa Chemical Industry Co., Ltd.); IXE-100, IXE-500, IXE-600, IXE-700F, IXE-800, IXE-6107, IXEPLAS-A1, IXEPLAS-A2, and IXEPLAS-B1 (trade names, manufactured by Toagosei Co., Ltd.); Jisnet DB (trade name, manufactured by Sankyo Pharmaceutical Co., Ltd.); VD-3 and VD-5 (trade names, manufactured by Shikoku Kasei Co., Ltd.); and Yoshinox BB (trade name, manufactured by Yoshitomi Pharmaceutical Co., Ltd.).
[0104] The ion scavenger may be used alone or in combination of two or more kinds. When the composition contains an ion scavenger, the content of the ion scavenger (inorganic ion scavenger and / or organic ion scavenger) is preferably 0.01 to 10 mass %, more preferably 0.1 to 20 mass %, and even more preferably 0.2 to 10 mass %, based on the total solid content of the composition. When the ion scavenger contains an inorganic ion scavenger, a part or the whole of the ion scavenger may simultaneously fall under the category of inorganic substances.
[0105] 〔solvent〕 The composition of the present invention may further comprise a solvent. The type of the solvent is not particularly limited, and is preferably an organic solvent, such as cyclopentanone, cyclohexanone, ethyl acetate, methyl ethyl ketone, dichloromethane, and tetrahydrofuran. When the composition contains a solvent, the content of the solvent is preferably an amount that makes the solids concentration of the composition 20 to 90 mass%, more preferably an amount that makes the solids concentration of the composition 30 to 80 mass%, and even more preferably an amount that makes the solids concentration of the composition 50 to 80 mass%. The content of the solvent is preferably from 5 to 80 mass %, more preferably from 15 to 70 mass %, and further preferably from 20 to 50 mass %, based on the total mass of the composition.
[0106] [Method of producing the composition] The method for producing the composition is not particularly limited, and a known method can be adopted, for example, the composition can be produced by mixing the various components described above. When mixing, the various components may be mixed at once or sequentially. The method for mixing the components is not particularly limited, and known methods can be used. The mixing device used for mixing is preferably a submerged dispersing device, and examples thereof include agitators such as a planetary centrifugal mixer, a high-speed rotary shear type agitator, a colloid mill, a roll mill, a high-pressure jet type dispersing device, an ultrasonic dispersing device, a bead mill, and a homogenizer. The mixing device may be used alone or in combination with two or more types. Degassing treatment may be performed before and / or after mixing.
[0107] [Method of curing the composition] The composition of the present invention is a composition for forming a thermally conductive material. The composition of the present invention can be cured to obtain a cured product, which can be used as a thermally conductive material. The method for curing the composition is not particularly limited, but a thermal curing reaction is preferred. The heating temperature during the thermosetting reaction is not particularly limited and may be appropriately selected within the range of, for example, 50 to 250° C. Furthermore, when carrying out the thermosetting reaction, heat treatments at different temperatures may be carried out multiple times. The curing treatment is preferably carried out on the composition in the form of a film or sheet. Specifically, for example, the composition may be applied to form a film and then subjected to a curing reaction. When performing the curing treatment, it is preferable to apply the composition onto a substrate to form a coating film and then cure the composition. In this case, the coating film formed on the substrate may be brought into contact with a different substrate before the curing treatment. The thermally conductive material (cured product) obtained after curing may or may not be separated from one or both of the substrates. In addition, when performing the curing treatment, the composition may be applied to separate substrates to form coating films on each substrate, and the curing treatment may be performed in a state where the obtained coating films are in contact with each other. The thermally conductive material (cured product) obtained after curing may or may not be separated from one or both substrates.
[0108] The curing treatment may be terminated when the composition is in a semi-cured state, or after the composition is in a semi-cured state, a further curing treatment may be carried out to complete the curing. The curing treatment for bringing the composition into a semi-cured state (also referred to as "semi-curing treatment") and the curing treatment for complete curing (also referred to as "main curing treatment") may be carried out in separate steps.
[0109] For example, in the semi-curing treatment, after applying a composition to a substrate to form a coating film, the coating film on the substrate may be heated without pressure to form a semi-cured heat conductive material (also referred to as a "semi-cured film" or "semi-cured sheet"). Alternatively, the coating film on the substrate may be heated while simultaneously using press processing to form a semi-cured film. When press processing is performed, the press processing may be performed before, after, or during the heating process. When press processing is performed in the semi-curing treatment, it may be easier to adjust the thickness of the resulting semi-cured film and / or reduce the amount of voids in the semi-cured film. In the semi-curing treatment, the coating films formed on different substrates may be laminated together, or the coating films may not be laminated together. The semi-curing treatment may be performed in a state where the coating film formed from the composition is in contact with a material other than the coating film.
[0110] The resulting semi-cured film may be used as it is as a heat conductive material, or may be further subjected to a main curing treatment and then used as a completely cured heat conductive material. In the main curing treatment, the semi-cured film may be heated as it is without pressure, or may be heated after or while being pressed. In this case, the main curing treatment may be performed in a state where separate semi-cured films are laminated on each other, or may be performed without laminating the semi-cured films on each other. The main curing treatment may be carried out in a state where the semi-cured film is placed in contact with a device or the like in which it is to be used. It is also preferable that the device and the thermally conductive material of the present invention are bonded by the main curing treatment.
[0111] There is no limitation on the press used for the press working that may be carried out during the hardening treatment in the semi-hardening treatment and / or the full hardening treatment, and for example, a flat plate press or a roll press may be used. When using a roll press, for example, it is preferable to clamp the substrate with a coating film obtained by forming a coating film on a substrate between a pair of opposing rolls, and apply pressure in the thickness direction of the substrate with a coating film while rotating the pair of rolls to pass the substrate with a coating film. The substrate with a coating film may have a substrate on only one side of the coating film, or may have substrates on both sides of the coating film. The substrate with a coating film may be passed through the roll press once or multiple times. During the hardening treatment in the semi-hardening treatment and / or the full hardening treatment, only one of the treatment by plate press and the treatment by roll press may be carried out, or both may be carried out.
[0112] For information on the production of thermally conductive materials (cured products) that include curing reactions, please also refer to "High Thermal Conductivity Composite Materials" (CMC Publishing, written by Takezawa Yoshitaka).
[0113] The shape of the thermally conductive material (cured product) is not particularly limited, and it can be molded into various shapes depending on the application. A typical shape of the molded thermally conductive material (cured product) is, for example, a sheet shape. In other words, the thermally conductive material (cured product) obtained by using the composition of the present invention is preferably a thermally conductive sheet. Furthermore, the thermal conductivity of the thermally conductive material obtained by using the composition of the present invention is preferably isotropic rather than anisotropic.
[0114] The thermally conductive material (cured product) is preferably insulating (electrically insulating), in other words, the composition of the present invention is preferably a composition for forming a thermally conductive insulating material. For example, the volume resistivity of a thermal conductive material at 23°C and relative humidity of 65% is 10 10 Ω·cm or more is preferable, and 10 12 More preferably, 10 14 The upper limit is not particularly limited, but it is preferably 10 18 Ω·cm or less is preferable.
[0115] [Uses of thermal conductive materials] The thermally conductive material (cured product) obtained by using the composition of the present invention can be used as a heat dissipation material such as a heat dissipation sheet, and can be used for heat dissipation purposes in various devices. More specifically, a thermally conductive layer containing the thermally conductive material of the present invention is disposed on a device to produce a device with a thermally conductive layer, and the heat generated from the device can be efficiently dissipated by the thermally conductive layer. The thermally conductive layer may be a thermally conductive layer containing a thermally conductive multilayer sheet described later. The thermally conductive material obtained using the composition of the present invention has sufficient thermal conductivity and high heat resistance, and is therefore suitable for heat dissipation applications in power semiconductor devices used in various electrical appliances such as personal computers, general home appliances, and automobiles. Furthermore, since the thermally conductive material obtained using the composition of the present invention has sufficient thermal conductivity even in a semi-cured state, it can be used as a heat dissipation material to be placed in areas where it is difficult for light for photocuring to reach, such as gaps between components of various devices. In addition, since it has excellent adhesive properties, it can also be used as an adhesive having thermal conductivity.
[0116] The thermally conductive material obtained by using the composition of the present invention may be used in combination with other components other than the component formed from the present composition. For example, a sheet-shaped thermoset (thermally conductive sheet) may be combined with a sheet-shaped support other than the layer formed from the present composition. Examples of the sheet-like support include a plastic film, a metal film, and a glass plate. Examples of the plastic film material include polyester such as polyethylene terephthalate (PET), polycarbonate, acrylic resin, epoxy resin, polyurethane, polyamide, polyolefin, cellulose derivative, and silicone. Examples of the metal film include a copper film. The thickness of the sheet-like cured product (thermal conductive sheet) is preferably 100 to 300 μm, and more preferably 150 to 250 μm.
[0117] Furthermore, an adhesive layer and / or a pressure-sensitive adhesive layer may be combined with a cured product (preferably a thermally conductive sheet) that is a thermally conductive material. By bonding the thermally conductive material (cured product) to an object to which heat should be transferred, such as a device, via such an adhesive layer and / or pressure-sensitive adhesive layer, a stronger bond can be achieved between the thermally conductive material (cured product) and the object. For example, a thermally conductive multilayer sheet may be prepared which has a thermally conductive sheet and an adhesive layer or pressure sensitive adhesive layer provided on one or both sides of the thermally conductive sheet. In addition, one or both sides of the thermally conductive sheet may be provided with either an adhesive layer or a pressure-sensitive adhesive layer, or both may be provided. An adhesive layer may be provided on one side of the thermally conductive sheet, and a pressure-sensitive adhesive layer may be provided on the other side. In addition, an adhesive layer and / or a pressure-sensitive adhesive layer may be provided partially or entirely on one or both sides of the thermally conductive sheet. As described above, in the present invention, the thermally conductive material such as the thermally conductive sheet may be in a semi-cured state (semi-cured film), and the thermally conductive sheet in the thermally conductive multilayer sheet may be in a semi-cured state. The adhesive layer in the thermally conductive multilayer sheet may be in a cured, semi-cured, or uncured state. EXAMPLES
[0118] The present invention will be described in more detail below based on examples. The materials, amounts, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the following examples.
[0119] [Preparation and evaluation of the composition [various components]] The various components used in the examples and comparative examples are shown below.
[0120] <Specific compound> The specific compounds used in the examples are listed below.
[0121] [ka]
[0122] <Compound for comparison> The comparative compounds used in the comparative examples are shown below.
[0123] [ka]
[0124] (Method of synthesizing specific compound A-1) A mixture of cyanuric chloride (15.5g, 0.083mol) and 2-butanone (75ml) was cooled on ice, and 5-amino-o-cresol (20.7g, 0.168mol) was added in small portions. Then, an aqueous solution of sodium acetate trihydrate (22.8g, 0.168mol) dissolved in water (32ml) was added to the mixture. The mixture was stirred at 40°C for 2 hours, and then sulfanilamide (15.8g, 0.092mol) was added and stirred at 80°C for 2 hours. The mixture was cooled to room temperature, and an aqueous solution of sodium carbonate (21.3g, 0.20mol) dissolved in water (134ml) was added dropwise to the mixture and stirred for 30 minutes. The mixture was left to stand and the aqueous phase was removed, and then the organic phase was filtered through Celite, and 34ml of ethanol was added. Water (435 ml) was added dropwise to the obtained organic phase with stirring, and after stirring for 2 hours, the precipitated crystals were filtered and dried to obtain Specific Compound A-1. Specific compounds A-2 to A-4 were synthesized in the same manner as in the synthesis of specific compound A-1. Specific compound A-6 was synthesized in the manner described in WO2007 / 139729.
[0125] <Epoxy compounds> The epoxy compounds used in the examples and comparative examples are shown below.
[0126] [ka]
[0127] <Curing accelerator> The curing accelerators used in the examples and comparative examples are shown below.
[0128] [ka]
[0129] <Inorganic substances> The inorganic substances used in the examples and comparative examples are shown below. HP-40 MF-100: Agglomerated boron nitride, average particle size: 40μm, manufactured by Mizushima Ferroalloy Co., Ltd. AA-3: Aluminum oxide, average particle size: 3 μm, manufactured by Sumitomo Chemical Co., Ltd. AA-04: Aluminum oxide, average particle size: 0.4 μm, manufactured by Sumitomo Chemical Co., Ltd. BN-A: Surface-modified boron nitride produced by the manufacturing method A shown below. BN-B: Surface-modified boron nitride produced by manufacturing method B shown below BN-C: Surface-modified boron nitride produced by the manufacturing method C shown below BN-D: Surface-modified boron nitride produced by production method D shown below BN-E: Surface-modified boron nitride produced by the production method E shown below
[0130] (Manufacturing method A) Boron nitride (HP-40 MF100) (15 g) was subjected to vacuum plasma treatment (gas type: O2, pressure: 30 Pa, output: 500 W) using a plasma cleaner PDC210 (manufactured by Yamato Scientific Co., Ltd.). The boron nitride to be treated was stirred every 5 minutes of vacuum plasma treatment, and the vacuum plasma treatment was continued until the total treatment time reached 30 minutes, obtaining modified boron nitride particles A. The obtained modified boron nitride particles A were stirred in acetonitrile (30 ml), and a hydrolysis adjustment solution (0.42 g) of a silane coupling agent (X12-984S, manufactured by Shin-Etsu Chemical Co., Ltd.) was further added to the acetonitrile. The acetonitrile was stirred at room temperature for 3 hours to perform an adsorption treatment. The modified boron nitride particles A in the acetonitrile were filtered out, and then the filtered modified boron nitride particles A were washed with acetonitrile (30 ml) and dried in an oven at 40° C. to obtain BN-A. The hydrolysis adjustment liquid of the silane coupling agent was prepared by mixing the silane coupling agent (1 g), ethanol (500 μl), 2-propanol (500 μl), water (720 μl), and acetic acid (100 μl) and stirring for 1 hour. In the following examples and comparative examples, the composition of the hydrolysis adjustment liquid of the silane coupling agent is the same unless otherwise specified. In addition, "X12-984S" is a polymer-type silane coupling agent having an epoxy group and an ethoxysilyl group.
[0131] (Manufacturing method B) Boron nitride (HP-40 MF-100, 50 g) was added to an aqueous NaOH solution (NaOH: 40 g / water: 400 ml) and stirred. Sodium persulfate water (sodium persulfate: 9.6 g / water: 100 ml) was further added to the aqueous NaOH solution, and the aqueous NaOH solution was heated to 50° C. and stirred for another 3 hours. Stirring was performed at a rotation speed of 150 rpm using a Three-One Motor (manufactured by Shinto Scientific Co., Ltd.). After cooling the aqueous NaOH solution to room temperature, the boron nitride particles B in the aqueous NaOH solution were filtered out, and the filtered boron nitride particles B were washed with water (500 ml) and acetonitrile (250 ml) to obtain modified boron nitride particles B. The obtained modified boron nitride particles B were stirred in acetonitrile (100 ml), and a hydrolysis adjustment solution (1.25 g) of a silane coupling agent (X12-984S, manufactured by Shin-Etsu Chemical Co., Ltd.) was further added to the acetonitrile. The acetonitrile was stirred at room temperature for 3 hours to perform an adsorption treatment. The modified boron nitride particles B in the acetonitrile were filtered, and then the filtered modified boron nitride particles were washed with acetonitrile (100 ml) and dried in an oven at 40°C to obtain BN-B.
[0132] (Manufacturing method C) Boron nitride (HP-40 MF-100, 50 g) was added to water (400 ml) and stirred to obtain a mixed solution. Sodium hypochlorite water (sodium hypochlorite pentahydrate: 48 g / water: 100 ml) was further added to the mixed solution, and the mixed solution was heated to 50° C. and stirred for another 3 hours. A Three-One motor manufactured by Shinto Scientific Co., Ltd. was used for stirring at 150 rpm. After the mixture was cooled to room temperature, the boron nitride particles in the mixture were filtered out and washed with water (500 ml) and acetonitrile (250 ml) to obtain modified boron nitride particles C. The obtained modified boron nitride particles C were stirred in acetonitrile (100 ml), and a hydrolysis adjustment solution (1.25 g) of a silane coupling agent (X12-984S) was further added to the acetonitrile. The acetonitrile was stirred at room temperature for 3 hours to perform an adsorption treatment. The modified boron nitride particles C in the acetonitrile were filtered, and then the filtered modified boron nitride particles C were washed with acetonitrile (100 ml) and dried in an oven at 40°C to obtain BN-C.
[0133] (Manufacturing method D) Boron nitride (HP-40 MF-100, 50 g) was heated at 1000°C for 1 hour to obtain modified boron nitride particles D. The obtained modified boron nitride D was reslurried and washed with water (500 ml), filtered, and then stirred in acetonitrile (100 ml), and a hydrolysis adjustment solution (1.25 g) of a silane coupling agent (KBM-403) was further added to the acetonitrile. The acetonitrile was stirred at room temperature for 3 hours to perform an adsorption treatment. The modified boron nitride particles D in the acetonitrile were filtered, and then the filtered modified boron nitride particles D were washed with acetonitrile (100 ml) and dried in an oven at 40°C to obtain BN-D.
[0134] (Manufacturing method E) Boron nitride (HP-40 MF-100, 50 g) was heated at 900°C for 4 hours to obtain modified boron nitride particles E. The obtained modified boron nitride E was reslurried and washed with water (500 ml), filtered, and then stirred in acetonitrile (100 ml), and a hydrolysis adjustment solution (1.25 g) of a silane coupling agent (KBM-403) was further added to the acetonitrile. The acetonitrile was stirred at room temperature for 3 hours to perform an adsorption treatment. The modified boron nitride particles E in the acetonitrile were filtered, and then the filtered modified boron nitride particles E were washed with acetonitrile (100 ml) and dried in an oven at 40°C to obtain BN-E.
[0135] <Solvent> Cyclopentanone was used as the solvent.
[0136] [Preparation of Composition] A mixture was prepared by blending the epoxy compounds and the specific compounds in the combinations shown in Table 1 below at the addition ratios shown in Table 1 below. The entire amount of the mixture obtained, the solvent, and the curing accelerator were mixed in this order, and then the inorganic substance was added. The mixture obtained was treated for 5 minutes with a planetary centrifugal mixer (THINKY Corporation, Awatori Rentaro ARE-310) to obtain a composition (composition for forming a thermal conductive material) of each Example or Comparative Example. The mixing ratio of each component was adjusted so that the content (mass %) of each component relative to the total solid content in the final composition was as shown in Table 1.
[0137] The amount of the solvent added was set so that the solid content of the composition would be 50 to 80% by mass. The solids concentration of each composition was adjusted within the above range for each composition so that the viscosity of each composition was approximately the same. The amount of inorganic substance added (total amount of boron nitride and other inorganic substances added) was the amount shown in Table 1 below. The inorganic substances were mixed and used so that the ratio of the contents (mass ratio) of the respective inorganic substances satisfied the relationship shown in Table 1 below.
[0138] [evaluation] [Evaluation of thermal conductivity] <Preparation of semi-cured sheet (semi-cured film)> Using an applicator with a micrometer, the composition of each Example or Comparative Example prepared as shown in Table 1 was uniformly applied onto the release surface of a release-treated polyester film (NP-100A, manufactured by PANAC Corporation, film thickness 100 μm), and dried at 120° C. for 5 minutes to produce a semi-cured sheet (semi-cured film).
[0139] <Preparation of thermal conductive sheet> The obtained semi-cured sheet was covered with a release-treated polyester film and heat-pressed in air (heat plate temperature 180°C, pressure 20MPa for 5 minutes). Then, heat treatment was performed at 180°C for 90 minutes under normal pressure to obtain a resin sheet. The polyester films on both sides of the resin sheet were peeled off to obtain a thermally conductive sheet (thermally conductive material) with an average thickness of 120 μm.
[0140] <Evaluation method> The thermal conductivity of the obtained thermally conductive sheet was measured by the following method. (1) The thermal diffusivity of the thermal conductive sheet in the thickness direction was measured by the laser flash method using a NETZSCH “LFA467”. (2) Using a Mettler Toledo balance “XS204”, the specific gravity of the thermally conductive sheet was measured by the Archimedes method (using a “solid specific gravity measurement kit”). (3) Using a Seiko Instruments Inc. DSC320 / 6200, the specific heat of the thermally conductive sheet was determined at 25°C with a temperature increase rate of 10°C / min. (4) The thermal conductivity of the thermal conductive sheet was calculated by multiplying the obtained thermal diffusivity by the specific gravity and specific heat.
[0141] The measured thermal conductivity was classified according to the following criteria to evaluate the thermal conductivity. A: The difference in thermal conductivity from Comparative Example 1 is +1 W / m K or more. B: The difference in thermal conductivity from Comparative Example 1 is less than +1 W / m K.
[0142] [Evaluation of handling properties (storage stability)] A semi-cured sheet was prepared in the same manner as described above in the evaluation of thermal conductivity, and then allowed to stand at room temperature (25° C.) for a predetermined period of time. The semi-cured sheet was cut into a rectangular shape of 5 cm x 10 cm to prepare a sample for bending test. The obtained sample was subjected to a bending test using a cylindrical mandrel tester (manufactured by Cortec Co., Ltd.) according to the method described in JIS K 5600-5-1. A cylindrical mandrel with a diameter of 32 mm was used to evaluate whether the semi-cured sheet broke. The bending test of the semi-cured sheet that had been left to stand at room temperature over time was performed every few hours.
[0143] The time allowed to stand at the time of breakage was classified according to the following criteria, and the handling properties (storage stability over time) were evaluated. A: It will not break even after being left to stand for 72 hours or more. B: Broken after being left standing for 48 hours or more but less than 72 hours. C: Broken after standing for less than 48 hours.
[0144] [Evaluation of glass transition temperature Tg] The Tg of the thermally conductive sheet obtained in the above <Preparation of Thermally Conductive Sheet> was measured. The Tg was measured using a dynamic viscoelasticity measuring device "Rheogel-E4000" manufactured by UBM, and the tan δ peak at a frequency of 1 Hz was taken as Tg. The temperature rise rate was 5°C / min, and the measurement was performed in the range of 25 to 300°C.
[0145] The Tg was evaluated according to the following criteria. A: Tg is 160℃ or higher B: Tg is less than 160°C
[0146] [result] Table 1 below shows the solid content of the composition used in each Example or Comparative Example, and the test results.
[0147] [Table 1]
[0148] The results shown in the table confirm that the effects of the present invention can be achieved by using the composition of the present invention. From a comparison of Examples 1 to 4 and 6 with Example 5, it was confirmed that the storage stability over time is better when the specific compound further has a phenolic hydroxyl group and / or is a compound represented by formula (2). In addition, from a comparison between Examples 1 to 4 and Example 6, it was confirmed that the stability over time is further improved when the specific compound further has a phenolic hydroxyl group and at least one of the following is satisfied: X represents a benzene ring group which may have a substituent; and the specific compound is a compound represented by formula (Z1).
Claims
1. The epoxy compound includes an epoxy compound and a compound having a group represented by formula (1), A thermal conductive material-forming composition, wherein the compound having a group represented by formula (1) is a compound represented by formula (Z1). 【Chemistry 1】 In formula (1), X represents an aromatic ring group which may have a substituent. 1 ~R 2 each independently represents a hydrogen atom or a substituent. * represents a bonding position. 【Chemistry 2】 In formula (Z1), R z1 to R z3 each independently represent a substituent, and z1 to z3 each independently represent an integer of 0 to 4.
2. The thermally conductive material forming composition according to claim 1 , further comprising an inorganic substance.
3. The thermally conductive material forming composition according to claim 2 , wherein the inorganic material is an inorganic nitride.
4. The composition for forming a thermally conductive material according to any one of claims 1 to 3, further comprising a curing accelerator.
5. A thermally conductive material obtained by curing the composition for forming a thermally conductive material according to any one of claims 1 to 4.
6. A thermally conductive sheet comprising the thermally conductive material according to claim 5 .
7. A device with a thermally conductive layer, comprising: a device; and a thermally conductive layer disposed on the device, the thermally conductive layer comprising the thermally conductive material of claim 5 .
Citation Information
Patent Citations
The epoxy resin and aromatic sulfonic acid amide adduct of amino acid change
JP1986500976A
Epoxy resin mixtures for prepregs and composite materials
JP1998505121A
Thermal conductive sheet
JP2013177562A
Novel liquid crystalline epoxy resin and composition thereof
JP2014122337A
Liquid crystalline epoxy compound with flexible linkage and method manufacturing same