Polyisocyanate Composition

The polyisocyanate composition, comprising pentamethylene diisocyanate derivatives with isocyanurate and allophanate groups, addresses the need for improved drying and solvent resistance in polyurethane resins, ensuring excellent performance and extended pot life.

JP7582885B2Active Publication Date: 2024-11-13MITSUI CHEMICALS INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021041411
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-15
Publication Date
2024-11-13
Estimated Expiration
2041-03-15

AI Technical Summary

Technical Problem

Coating films formed from polyurethane resins require improved drying properties, solvent resistance, and water resistance in automotive, electronic, and architectural applications.

Method used

A polyisocyanate composition is developed as a reaction product of pentamethylene diisocyanate derivatives containing isocyanurate and allophanate groups, with a specific molecular weight distribution and modifier amount, enhancing drying properties and solvent resistance.

Benefits of technology

The polyisocyanate composition produces polyurethane resins with excellent drying properties, solvent resistance, and water resistance, extending pot life and maintaining reactivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582885000005
    Figure 0007582885000005
  • Figure 0007582885000001
    Figure 0007582885000001
  • Figure 0007582885000002
    Figure 0007582885000002
Patent Text Reader

Abstract

To provide a polyisocyanate composition having excellent dryability, solvent resistance and water resistance.SOLUTION: A polyisocyanate composition is a reaction product between a derivative of pentamethylene diisocyanate and a denaturant. The denaturant is composed of amino alcohol. The amount of denaturation by the denaturant is 0.1 pt.mass or more and 10 pts.mass or less relative to 100 pts.mass of the derivative of pentamethylene diisocyanate.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyisocyanate composition. [Background technology]

[0002] Polyurethane resins are usually produced by the reaction of polyisocyanates with active hydrogen group-containing compounds. Polyurethane resins are widely used in various industrial fields, for example, as coating materials, adhesive materials, pressure-sensitive adhesive materials, and elastomers. In detail, polyurethane resins can be applied to a substrate to form a coating film, thereby imparting various physical properties to the substrate.

[0003] As a polyisocyanate used in the production of polyurethane resin, a curing agent for two-component polyurethane resin coating has been proposed in which an isocyanurate modified product of 1,6-hexane diisocyanate (HDI) is modified with a modifying agent containing 12-hydroxystearic acid and N,N-dimethylaminohexanol (see, for example, Example 1 of Patent Document 1).

[0004] In addition, a curing agent for two-component polyurethane resin coatings has been proposed in which an isocyanurate-modified HDI is modified with a modifier containing polyether polyol and N,N-dimethylaminohexanol (see, for example, Example 1 of Patent Document 2). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2010-215815 A [Patent Document 2] JP 2010-222504 A Summary of the Invention [Problem to be solved by the invention]

[0006] In recent years, coating films formed from polyurethane resins for automotive, electronic and architectural applications are required to have drying properties, solvent resistance and water resistance.

[0007] The present invention provides a polyisocyanate composition which is excellent in drying property, solvent resistance and water resistance. [Means for solving the problem]

[0008] The present invention [1] is a polyisocyanate composition which is a reaction product of a derivative of pentamethylene diisocyanate and a modifying agent, the modifying agent being composed of an amino alcohol, and the modification amount of the modifying agent per 100 parts by mass of the derivative of pentamethylene diisocyanate being 0.1 parts by mass or more and 10 parts by mass or less.

[0009] The present invention [2] includes the polyisocyanate composition according to the above [1], in which the derivative of pentamethylene diisocyanate contains an isocyanurate group and / or an allophanate group.

[0010] The present invention [3] comprises the polyisocyanate composition according to the above [2], in which the molecular weight distribution of the pentamethylene diisocyanate derivative is measured by a gel permeation chromatograph equipped with a differential refractive index detector, and in the chromatogram obtained, the area ratio of the total area of ​​peaks originating from isocyanurate trimolecules of pentamethylene diisocyanate to the total area of ​​peaks originating from allophanate dimolecules of pentamethylene diisocyanate (total area of ​​peaks originating from isocyanurate trimolecules / total area of ​​peaks originating from allophanate dimolecules) is 0.3 or more. Effect of the Invention

[0011] The polyisocyanate composition of the present invention is a reaction product of a derivative of pentamethylene diisocyanate and a modifying agent made of an amino alcohol, and the modification amount of the modifying agent is within a predetermined range. Therefore, by using this polyisocyanate composition, a polyurethane resin having excellent drying properties, solvent resistance, and water resistance can be produced. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a gel permeation chromatogram of the polyisocyanate composition of Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The polyisocyanate composition of the present invention is a reaction product of a derivative of pentamethylene diisocyanate and a modifier. That is, the polyisocyanate composition is obtained by reacting a derivative of pentamethylene diisocyanate with a modifier. The reaction product has a molecular weight distribution and has an isocyanate group at the molecular end, and is therefore a polyisocyanate composition.

[0014] <Derivatives of pentamethylene diisocyanate> Examples of pentamethylene diisocyanates include 1,2-pentamethylene diisocyanate, 1,3-pentamethylene diisocyanate, 1,4-pentamethylene diisocyanate, 1,5-pentamethylene diisocyanate, 2,3-pentamethylene diisocyanate, 2,4-pentamethylene diisocyanate, or mixtures thereof, and preferably 1,5-pentamethylene diisocyanate.

[0015] In the following description, unless otherwise specified, pentamethylene diisocyanate (hereinafter sometimes abbreviated as PDI) is 1,5-pentamethylene diisocyanate.

[0016] Pentamethylene diisocyanate is not particularly limited, and can be produced, for example, in accordance with Example 1 in the specification of WO 2012 / 121291.

[0017] Examples of the derivatives of pentamethylene diisocyanate include the above-mentioned polymers of pentamethylene diisocyanate (e.g., dimers, trimers (e.g., isocyanurate derivatives, iminooxadiazinedione derivatives), pentamers, and heptamers), allophanate derivatives (e.g., allophanate derivatives produced by the reaction of the above-mentioned pentamethylene diisocyanate with a monohydric alcohol or a dihydric alcohol), polyol derivatives (e.g., polyol derivatives (alcohol adducts) produced by the reaction of the above-mentioned pentamethylene diisocyanate with a trihydric alcohol (e.g., trimethylolpropane)), biphenyls, etc. Examples of the derivatives include uret derivatives (for example, the biuret derivatives produced by the reaction of the above-mentioned pentamethylene diisocyanate with water or amines), urea derivatives (for example, the urea derivatives produced by the reaction of the above-mentioned pentamethylene diisocyanate with diamines), oxadiazinetrione derivatives (for example, the oxadiazinetriones produced by the reaction of the above-mentioned pentamethylene diisocyanate with carbon dioxide), carbodiimide derivatives (the carbodiimide derivatives produced by the decarboxylation condensation reaction of the above-mentioned pentamethylene diisocyanate), uretdione derivatives, and uretonimine derivatives.

[0018] Further, derivatives of pentamethylene diisocyanate include allophanate-isocyanurate derivatives having both an allophanate group and an isocyanurate group.

[0019] To obtain an allophanate-isocyanurate derivative of pentamethylene diisocyanate, first, pentamethylene diisocyanate is partially reacted with an alcohol to prepare partially urethane-modified pentamethylene diisocyanate (urethane reaction liquid).

[0020] Examples of the alcohol include alcohols having 1 to 8 carbon atoms. Examples of the alcohols having 1 to 8 carbon atoms include monohydric alcohols having 1 to 8 carbon atoms and dihydric alcohols having 1 to 8 carbon atoms.

[0021] Examples of the monohydric alcohol having 1 to 8 carbon atoms include linear monohydric alcohol having 1 to 8 carbon atoms and branched monohydric alcohol having 1 to 8 carbon atoms. Examples of the linear monohydric alcohol having 1 to 8 carbon atoms include methanol, ethanol, n-propanol, n-butanol, n-pentanol, n-hexanol, n-heptanol, and n-octanol. Examples of the branched monohydric alcohol having 1 to 8 carbon atoms include isopropanol, isobutanol, sec-butanol, tert-butanol, isopentanol, isohexanol, isoheptanol, and isooctanol.

[0022] Examples of dihydric alcohols having 1 to 8 carbon atoms include ethylene glycol, propylene glycol, butylene glycol, pentamethylene glycol, hexamethylene glycol, heptamethylene glycol, and octamethylene glycol.

[0023] The alcohol is preferably a monohydric alcohol having 1 to 8 carbon atoms, more preferably a monohydric alcohol having 1 to 4 carbon atoms, even more preferably a branched monohydric alcohol having 1 to 4 carbon atoms, and even more preferably isobutanol.

[0024] In the above reaction, if necessary, for example, an antioxidant (e.g., octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate) and a promoter (e.g., tridecyl phosphite) can be added in appropriate proportions.

[0025] Next, an isocyanurate catalyst (for example, N-(2-hydroxypropyl)-N,N,N-trimethylammonium-2-ethylhexanoate) is added to the urethane reaction liquid, and the urethane reaction liquid is subjected to an isocyanurate reaction.

[0026] The isocyanurate catalyst can also be used as a catalyst solution in which it is dissolved in a solvent. Examples of the solvent in the catalyst solution include glycol esters (for example, propylene glycol methyl ether acetate).

[0027] In the above-mentioned isocyanurate reaction, a catalyst deactivator (e.g., o-toluenesulfonamide) is preferably added at any timing to terminate the reaction. The timing for adding the catalyst deactivator is, for example, the time when the conversion rate of the isocyanate group (described later) reaches a target value.

[0028] This gives the allophanate-isocyanurate derivative of pentamethylene diisocyanate.

[0029] In this method, after completion of the isocyanurate reaction, if necessary, unreacted pentamethylene diisocyanate (and, if necessary, the isocyanurate catalyst and catalyst deactivator) are removed from the resulting reaction mixture by a known method, for example, distillation such as thin-film distillation (Smith distillation) or extraction.

[0030] Furthermore, in the above-mentioned method, since pentamethylene diisocyanate is partially urethane-modified prior to the isocyanurate-forming reaction, the isocyanurate-forming reaction produces not only an isocyanurate derivative but also an allophanate derivative.

[0031] In the above reaction, the amount of allophanate groups and the amount of isocyanurate groups in the allophanate-isocyanurate derivative can be adjusted by adjusting the blending ratio of the alcohol and the isocyanurate conversion rate of pentamethylene diisocyanate (described later).

[0032] Specifically, the blending ratio of the alcohol is the equivalent ratio (NCO / OH) of the isocyanate groups of pentamethylene diisocyanate to the hydroxyl groups of the alcohol, for example, 1 or more, preferably 10 or more, more preferably 15 or more, even more preferably 20 or more, particularly preferably 50 or more, and most preferably 70 or more, and for example, 400 or less, preferably 200 or less, more preferably 100 or less, and even more preferably 80 or less.

[0033] In the above reaction, the conversion rate of pentamethylene diisocyanate to isocyanurate is, for example, 5 mass% or more, preferably 10 mass% or more, and for example, 50 mass% or less, preferably 40 mass% or less.

[0034] The isocyanurate conversion rate can be determined by calculating the rate of decrease in the isocyanate group concentration determined by titration.

[0035] Furthermore, an isocyanurate derivative of pentamethylene diisocyanate can be obtained, for example, by reacting pentamethylene diisocyanate as it is in the presence of the isocyanurate catalyst to form an isocyanurate without preparing a urethane-forming reaction liquid.

[0036] In the above reaction, a small amount of alcohol (e.g., the above-mentioned alcohol) may be added in order to promote the isocyanurate reaction. In this case, the alcohol is added so that the equivalent ratio (NCO / OH) of the isocyanate group of pentamethylene diisocyanate to the hydroxyl group of the alcohol exceeds, for example, 400. In the isocyanurate derivative of such pentamethylene diisocyanate, no peak corresponding to the allophanate dimolecular body is detected in the measurement by gel permeation chromatography described later.

[0037] Furthermore, allophanate derivatives of pentamethylene diisocyanate can be obtained, for example, by reacting pentamethylene diisocyanate with the above-mentioned alcohol, and then further reacting the resulting mixture in the presence of a known allophanate catalyst.

[0038] The derivative of pentamethylene diisocyanate preferably includes an isocyanurate derivative, an allophanate derivative, and an allophanate-isocyanurate derivative. That is, the derivative of pentamethylene diisocyanate preferably contains an isocyanurate group and / or an allophanate group. If the derivative of pentamethylene diisocyanate contains an isocyanurate group and / or an allophanate group, a polyurethane resin having an excellent balance of drying property, solvent resistance, and water resistance can be produced.

[0039] Moreover, the derivative of pentamethylene diisocyanate more preferably has at least an isocyanurate group, and further preferably has an isocyanurate group and an allophanate group. That is, the derivative of pentamethylene diisocyanate is further preferably an allophanate-isocyanurate derivative. If the derivative of pentamethylene diisocyanate contains an isocyanurate group and an allophanate group, the reactivity with alcohol is improved. Moreover, even if the reactivity with alcohol is improved, the pot life can be prevented from being excessively shortened.

[0040] The allophanate-isocyanurate derivative and isocyanurate derivative described above include a trimer of pentamethylene diisocyanate (an isocyanurate derivative consisting of three molecules of pentamethylene diisocyanate (hereinafter, an isocyanurate trimer)) and, if necessary, a polymer having a plurality of trimer skeletons (an isocyanurate derivative consisting of multiple molecules of pentamethylene diisocyanate exceeding three molecules (hereinafter, an isocyanurate multimer)).

[0041] In the above-mentioned allophanate-isocyanurate derivatives and allophanate derivatives, when pentamethylene diisocyanate is reacted with a monohydric alcohol, the allophanate-isocyanurate derivatives and allophanate derivatives contain an allophanate dimolecular entity (the following formula (1)) consisting of two molecules of pentamethylene diisocyanate and a monohydric alcohol. [ka] (In the formula, R1 represents a residue of an alcohol.)

[0042] Regarding the content ratio of isocyanurate trimers and the content ratio of allophanate dimolecules, the molecular weight distribution of a pentamethylene diisocyanate derivative is measured by a gel permeation chromatograph equipped with a differential refractive index detector, and in the obtained chromatogram, the area ratio of the total area of ​​peaks originating from the isocyanurate trimers of pentamethylene diisocyanate to the total area of ​​peaks originating from the allophanate dimolecules of pentamethylene diisocyanate (total area of ​​peaks originating from isocyanurate trimers / groups of peaks originating from allophanate dimolecules) is, for example, more than 0, preferably 0.2 or more, more preferably 0.3 or more, even more preferably 0.5 or more, particularly preferably 1.0 or more, most preferably 1.5 or more, and for example, 5.0 or less, preferably 3.0 or less, more preferably 2.0 or less.

[0043] When the area ratio is equal to or greater than the lower limit (particularly, equal to or greater than 0.3), a polyurethane resin having excellent solvent resistance and water resistance can be produced, and the pot life of the polyisocyanate composition can be extended.

[0044] The pentamethylene diisocyanate derivatives can be used alone or in combination of two or more kinds.

[0045] <Modifier> The denaturant comprises an amino alcohol.

[0046] Examples of the amino alcohol include N,N-dialkylamino alcohol and N,N,N'-trialkylamino alcohol. Examples of the N,N-dialkylamino alcohol include N,N-dimethylethanolamine, N,N-dimethylaminohexanol, N,N-dimethylaminoethoxyethoxyethanol, and N,N-dimethylaminoethoxyethanol. Examples of the N,N,N'-trialkylamino alcohol include N,N,N'-trimethylaminoethylethanolamine. Examples of the amino alcohol include preferably N,N-dialkylamino alcohol, more preferably N,N-dimethylaminohexanol.

[0047] The amino alcohols can be used alone or in combination of two or more kinds.

[0048] <Polyisocyanate composition> The polyisocyanate composition can be obtained by reacting a derivative of pentamethylene diisocyanate with a modifying agent.

[0049] Specifically, a derivative of pentamethylene diisocyanate, a modifying agent, and, if necessary, an organic solvent are mixed together, and the derivative of pentamethylene diisocyanate and the modifying agent are reacted with each other.

[0050] The organic solvent is selected from those that are inactive to isocyanate groups, such as acetone, methyl ethyl ketone, ethyl acetate, tetrahydrofuran, acetonitrile, and N-methylpyrrolidone.

[0051] The modifying amount of the modifying agent is an amount capable of partially modifying an isocyanate group in a derivative of pentamethylene diisocyanate, and is 0.1 part by mass or more, preferably 0.5 part by mass or more, more preferably 1.0 part by mass or more, even more preferably 2.0 parts by mass or more, particularly preferably more than 2.0 parts by mass, most preferably 2.5 parts by mass or more, and is 10 parts by mass or less, preferably 5 parts by mass or less, more preferably 4 parts by mass or less, relative to 100 parts by mass of the derivative of pentamethylene diisocyanate.

[0052] When the modification amount is equal to or greater than the lower limit, a polyurethane resin having excellent drying properties and water resistance can be produced, and the polyisocyanate composition has excellent reactivity with alcohol.

[0053] On the other hand, if the modification amount is less than the lower limit, the polyurethane resin obtained by using the polyisocyanate composition has poor drying properties and water resistance, and the reactivity of the polyisocyanate composition to alcohol is poor.

[0054] When the modification amount is equal to or less than the upper limit, a polyurethane resin having excellent solvent resistance and water resistance can be produced, and the pot life of the polyisocyanate composition can be extended.

[0055] On the other hand, if the modification amount exceeds the upper limit, the solvent resistance and water resistance of the polyurethane resin obtained by using the polyisocyanate composition are reduced, and the pot life of the polyisocyanate composition is shortened.

[0056] The degree of modification by the modifying agent can be determined from the amount of the modifying agent charged.

[0057] In the above reaction, the reaction temperature is, for example, 60° C. or more, preferably 80° C. or more, and for example, 120° C. or less, preferably 100° C. or less. The reaction time is, for example, 0.5 hours or more, preferably 1 hour or more, and for example, 6 hours or less, preferably 4 hours or less.

[0058] This gives a reaction product (polyisocyanate composition) of the pentamethylene diisocyanate derivative and the modifying agent.

[0059] When an organic solvent is added in the reaction between the derivative of pentamethylene diisocyanate and the modifying agent, the polyisocyanate composition is prepared as a solution of the polyisocyanate composition.

[0060] The solids concentration in the solution of the polyisocyanate composition is, for example, 10 mass % or more and, for example, 50 mass % or less.

[0061] The polyisocyanate composition can also be diluted with an organic solvent so that the solution of the polyisocyanate composition has the above-mentioned solid content concentration.

[0062] <Action and effect> The polyisocyanate composition is a reaction product of a derivative of pentamethylene diisocyanate and a modifying agent made of an amino alcohol, and the amount of modification by the modifying agent is within a predetermined range. Therefore, the polyisocyanate composition can produce a polyurethane resin having excellent drying properties, solvent resistance, and water resistance.

[0063] In particular, since this polyisocyanate composition uses an amino alcohol as a modifying agent, a polyurethane resin with excellent drying properties can be produced in the reaction between the pentamethylene diisocyanate derivative and the modifying agent without using a urethanization catalyst (e.g., amines and organometallic compounds).

[0064] This polyisocyanate composition is preferably used in the production of polyurethane resin. Specifically, the polyisocyanate composition is used as a coating agent. When the polyisocyanate composition is used as a coating agent, the polyurethane resin becomes a cured film. As the coating agent, for example, a two-component curing polyurethane composition can be mentioned.

[0065] In the case of producing a polyurethane resin, known additives can be further blended in an appropriate ratio with the polyisocyanate composition as required. Examples of known additives include plasticizers, antiblocking agents, heat stabilizers, light stabilizers, antioxidants, release agents, catalysts, as well as pigments, dyes, lubricants, fillers, and hydrolysis inhibitors.

[0066] In a two-component curing polyurethane composition, the curing agent and the base component are each prepared as separate packages, and are mixed together at the time of use to form a polyurethane resin (cured film).

[0067] In the production of a two-component curing polyurethane composition, a polyisocyanate composition is used as a curing agent.

[0068] If necessary, the curing agent is dissolved in the above-mentioned organic solvent.

[0069] The base agent contains an active hydrogen group-containing compound. Examples of the active hydrogen group-containing compound include a hydroxyl group-containing compound and an amino group-containing compound, and preferably a hydroxyl group-containing compound.

[0070] An example of the hydroxyl group-containing compound is a macropolyol.

[0071] The macropolyol is a compound having two or more hydroxyl groups and a number average molecular weight of 400 to 10,000, preferably 500 to 5,000. Examples of the macropolyol include polyether polyol, polyester polyol, polycarbonate polyol, polyurethane polyol, epoxy polyol, vegetable oil polyol, polyolefin polyol, acrylic polyol, and vinyl monomer modified polyol.

[0072] The macropolyol is preferably an acrylic polyol.

[0073] The base material may be dissolved in the above-mentioned organic solvent, if necessary.

[0074] The two-component curing polyurethane composition can be obtained by blending the curing agent and the base component at the time of use, and mixing and stirring them.

[0075] Specifically, first, the base agent and the curing agent are prepared, and immediately before use, the base agent and the curing agent are mixed to prepare a two-component curing polyurethane composition (coating agent), and the two-component curing polyurethane resin is applied to the substrate.

[0076] The blending ratio of the base agent and the curing agent is such that the equivalent ratio (isocyanate group / hydroxyl group) of the isocyanate group in the curing agent (polyisocyanate composition) to the active hydrogen group in the base agent (active hydrogen group-containing compound) is, for example, 0.8 or more, preferably 0.9 or more, and for example, 1.2 or less, preferably 1.1 or less.

[0077] The mixture of the base agent and the curing agent is applied to the substrate by, for example, spray coating, air spray coating, brush coating, dipping, roll coating, flow coating, dry lamination, wet lamination, or direct coating.

[0078] The substrate is not particularly limited, and examples thereof include inorganic and organic materials. Examples of inorganic materials include concrete, natural stone, and glass. Examples of organic materials include plastics, rubber, adhesives, and wood. Also, the substrate is not particularly limited, and examples thereof include various building materials and various laminated films.

[0079] The mixture of the base resin and the curing agent is then dried and cured to obtain a polyurethane resin (cured film).

[0080] This polyurethane resin is obtained by using the polyisocyanate composition, and therefore has excellent drying properties, solvent resistance, and water resistance.

[0081] Such polyisocyanate compositions and polyurethane resins can be suitably used in various industrial fields. Specifically, the polyurethane resins and polyisocyanate compositions can be suitably used in, for example, automotive applications, electronic applications, and construction applications. EXAMPLES

[0082] Specific numerical values ​​of the blending ratio (content ratio), physical property values, parameters, etc. used in the following description can be replaced with the upper limit values ​​(numerical values ​​defined as "not more than" or "less than") or lower limit values ​​(numerical values ​​defined as "not less than" or "exceeding") of the corresponding blending ratio (content ratio), physical property values, parameters, etc. described in the above "Form for carrying out the invention." In addition, unless otherwise specified in the following description, "parts" and "%" are based on mass.

[0083] 1. Synthesis of diisocyanate derivatives Synthesis Example 1 In a four-neck flask equipped with a stirrer, a thermometer, a reflux tube, and a nitrogen inlet tube, 100 parts by mass of PDI, 0.05 parts by mass of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (Irganox 1076, BASF, product name) as an antioxidant, and 0.1 parts by mass of tridecyl phosphite (JP-310, Johoku Chemical, product name) as a promoter were charged and heated to 80° C. Next, isobutanol was charged so that the equivalent ratio (NCO / OH) of the isocyanate group of pentamethylene diisocyanate to the hydroxyl group of isobutanol was 70, and the reaction was carried out at 80° C. for 3 hours.

[0084] Next, a catalyst solution prepared by dissolving 0.01 part by mass of N-(2-hydroxypropyl)-N,N,N-trimethylammonium-2-ethylhexanoate in 0.03 part by mass of propylene glycol methyl ether acetate was added.

[0085] Thereafter, by utilizing the heat generated by the reaction, when the temperature reached 120°C and the predetermined conversion rate (10.4%) was reached, 0.01 parts by mass of o-toluenesulfonamide was added to terminate the reaction. The resulting reaction liquid was passed through a thin-film distillation apparatus (vacuum degree 50 Pa, temperature 150°C) to remove unreacted pentamethylene diisocyanate, and a derivative of pentamethylene diisocyanate (allophanate-isocyanurate derivative) was obtained.

[0086] Synthesis Example 2 The compounding recipe was changed according to Table 1, and the same procedure as in Synthesis Example 1 was followed to obtain a derivative of hexamethylene diisocyanate (allophanate-isocyanurate derivative).

[0087] Synthesis Example 3 and Synthesis Example 4 The compounding recipe was changed according to Table 1, and the same procedure as in Synthesis Example 1 was followed to obtain a pentamethylene diisocyanate derivative (allophanate-isocyanurate derivative).

[0088] Synthesis Example 5 The compounding recipe was changed according to Table 1, and a procedure similar to that of Synthesis Example 1 was followed to obtain a pentamethylene diisocyanate derivative (isocyanurate derivative).

[0089] 2. Preparation of polyisocyanate composition Example 1 In a four-neck flask equipped with a stirrer, a thermometer, a reflux tube, and a nitrogen inlet tube, 100 parts by mass of the pentamethylene diisocyanate derivative of Synthesis Example 1 and 3 parts by mass of N,N-dimethylaminohexanol (Kao Raiser No. 25, manufactured by Kao Corporation) as an amino alcohol were mixed and reacted at 85° C. for 3 hours. This produced a polyisocyanate composition.

[0090] Example 2 Example 4, Reference Examples 5 to 6 and Comparative Examples 1 to 3 The compounding recipe was changed according to Table 2, and polyisocyanate was added in the same manner as in Example 1. The composition was prepared.

[0091] Comparative Example 4 100 parts by mass of the pentamethylene diisocyanate derivative of Synthesis Example 1 and 1,4-diazabicyclo[2.2.2]octane (DABCO, manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed in a glass bottle and stirred with a magnetic stirrer at 25° C. for 30 minutes. Thus, a polyisocyanate composition was prepared.

[0092] Comparative Example 5 and Comparative Example 6 The compounding recipe was changed according to Table 2, and polyisocyanate compositions were prepared in the same manner as in Comparative Example 4.

[0093] In Table 2, TMBDA is N,N,N',N'-tetramethylethylenediamine (manufactured by Tokyo Chemical Industry Co., Ltd.), and DBTDL is dibutyltin dilaurate (manufactured by Tokyo Chemical Industry Co., Ltd.).

[0094] Comparative Example 7 In a four-neck flask equipped with a stirrer, a thermometer, a reflux tube, and a nitrogen inlet tube, 100 parts by mass of the hexamethylene diisocyanate derivative of Synthesis Example 2 and 3 parts by mass of 12-hydroxystearic acid (reagent, manufactured by Tokyo Chemical Industry Co., Ltd.) were blended and reacted at 85° C. for 3 hours. Next, 3 parts by mass of N,N-dimethylaminohexanol (Kao Raiser No. 25, manufactured by Kao Corporation) as an amino alcohol was blended and reacted at 85° C. for 3 hours. This prepared a polyisocyanate composition.

[0095] 3. Evaluation <Gel permeation chromatography> For the pentamethylene diisocyanate derivatives or hexamethylene diisocyanate derivatives of each synthesis example, the molecular weight distribution was measured by a gel permeation chromatograph (GPC) equipped with a refractive index detector (RID), and in the resulting chromatogram (chart), the area ratio of the total area of ​​peaks originating from isocyanurate trimolecules of pentamethylene diisocyanate to the total area of ​​peaks originating from allophanate dimolecules of pentamethylene diisocyanate (total area of ​​peaks originating from isocyanurate trimolecules / total area of ​​peaks originating from allophanate dimolecules) was determined.

[0096] Specifically, each embodiment , each reference example Approximately 0.03 g of each of the polyisocyanate compositions of the comparative examples was collected and dissolved in 10 mL of tetrahydrofuran. The resulting solutions were subjected to GPC measurement under the following conditions.

[0097] [Measurement conditions] Analytical equipment: High-speed GPC equipment HLC-8320 (manufactured by Tosoh) Detector: Differential refractive index detector Eluent: Tetrahydrofuran As separation columns, the following first to fourth columns were connected in series in this order. As stated above. First column (TSKgel guardcolum HXL-L 6.0 x 40 (Tosoh Corporation)) Second column: TSKgel G1000HXL 7.8 x 300 (Tosoh Corporation) Third column: TSKgel G2000HXL 7.8 x 300 (Tosoh Corporation) Fourth column: TSKgel G3000HXL 7.8 x 300 (Tosoh Corporation) Measurement temperature: 40℃ Flow rate: 1mL / min Sample injection volume: 100 μL Analysis device: Eco SEC (manufactured by Tosoh Corporation) System Correction Standard substance name: Polystyrene Calibration curve creation method: A graph of retention time and molecular weight was created using TOSOH TSKstandard Polystyrene with different molecular weights.

[0098] The area ratio of the peak having a peak top in the range of polystyrene-equivalent molecular weight of 320 or more and less than 400 (Mn320-400 area ratio) was taken as the content ratio of the allophanate dimolecular body of pentamethylene diisocyanate. The area ratio of the peak having a peak top in the range of polystyrene-equivalent molecular weight of 400 or more and less than 480 (Mn400-480 area ratio) was taken as the content ratio of the isocyanurate trimolecular body of pentamethylene diisocyanate. The area ratio of the peak having a peak top in the range of polystyrene-equivalent molecular weight of 350 or more and less than 430 (Mn350-430 area ratio) was taken as the content ratio of the allophanate dimolecular body of hexamethylene diisocyanate. The area ratio of the peak having a peak top in the range of polystyrene-equivalent molecular weight of 430 or more and less than 510 (Mn430-510 area ratio) was taken as the content ratio of the isocyanurate trimolecular body of hexamethylene diisocyanate. The peak area was determined by the vertical division method.

[0099] Moreover, the gel permeation chromatogram of the polyisocyanate composition of Example 1 is shown in FIG.

[0100] <Reactivity to alcohol> In a 100cc glass bottle, Reference example,The polyisocyanate synthesized in the comparative example was added and diluted with ethyl acetate to a solid content of 45%. Next, n-butanol (Fujifilm Wako Pure Chemical Industries, Ltd., special grade reagent) was weighed so that the isocyanate group / hydroxyl group ratio was 0.5, and the isocyanate group content was measured every hour immediately after mixing at 25°C while stirring with a magnetic stirrer. The isocyanate group disappearance rate was calculated from the isocyanate group content by replacing aliphatic isocyanate (pentamethylene diisocyanate or hexamethylene diisocyanate) with the JIS K 1603-1 A method as it is. The alcohol reactivity was evaluated based on the isocyanate disappearance rate after 8 hours based on the following criteria. The results are shown in Table 2. [standard] ◎: The isocyanate group disappearance rate was 25% or more. ◯: The isocyanate group disappearance rate was 20% or more and less than 25%. △: The isocyanate group disappearance rate was 12% or more and less than 20%. ×: The isocyanate group disappearance rate was less than 12%.

[0101] <Pot life (gel time)> In a 100cc glass bottle, , each reference example The polyisocyanate composition of each comparative example and acrylic polyol (Olestar Q-166, manufactured by Mitsui Chemicals) were mixed at an equivalent ratio of 1.0 (NCO / OH=1.0), and a thinner (ethyl acetate:butyl acetate:propylene glycol methyl ether acetate=1:1:1 mixed) was added so that the solid concentration was 50%, and the mixture was mixed at 23°C for 5 minutes to prepare a mixed liquid (two-component curing polyurethane composition). Next, the mixed liquid was degassed by ultrasonic treatment for 10 minutes. Every hour, the bottle was tilted 90°C and left to stand for 1 minute. At this time, the mixed liquid was visually observed to see if it tilted. The pot life was evaluated based on the following criteria. The results are shown in Table 2. [standard] ⊚: The mixed liquid maintained a tilted state for 17 hours or more after mixing. ◯: The mixed liquid maintained a tilted state for 15 hours or more and less than 17 hours after mixing. △: The mixed liquid maintained a tilted state for 10 hours or more and less than 15 hours from immediately after mixing. ×: The mixed liquid maintained a tilted state for less than 10 hours immediately after mixing.

[0102] <Paint film drying> The mixed solution used in the pot life evaluation (mixed solution 0.5 hours after mixing) was applied to a glass plate (JIS, R, 3202, thickness 2 mm) with a 4 mil applicator and left in an atmosphere with a temperature of 23°C and a humidity of 55% to form a coating film. Next, the center of the coating film was rubbed rapidly back and forth 10 times with a fingertip, and the time until the fingertip was no longer stained with the sample was evaluated. The drying property of the coating film was evaluated based on the following criteria. The results are shown in Table 2. [standard] ⊚: The time it took for the fingertips to become free from the sample was less than 200 minutes. ◯: The time it took for the fingertips to become free of the sample was 200 minutes or more and less than 250 minutes. △: The time it took for the fingertips to become free from the sample was 250 minutes or more but less than 300 minutes. ×: It took 300 minutes or more for the fingertips to become free from the sample.

[0103] <Chemical resistance> The mixed solution used in the pot life evaluation (mixed solution 0.5 hours after mixing) was applied to a steel plate (SPCC steel plate, PBN-144 treated product) with a 4 mil applicator and baked at 80°C for 30 minutes. Then, it was cured for 5 days in an atmosphere with a temperature of 23°C and a humidity of 55%. This resulted in a coating film. Next, this coating film was set in a rubbing tester (IMC-0717 type, manufactured by Imoto Manufacturing Co., Ltd.), and absorbent cotton moistened with methyl ethyl ketone was placed on the tip of a weight with a load of 1 kg and rubbed. The number of times the coating film was torn and the substrate was exposed was measured, and the number of times the rubbing was repeated was measured. The chemical resistance was evaluated based on the following criteria. The results are shown in Table 2. [standard] ⊚: The number of reciprocating rubbing cycles was 60 or more. ◯: The number of reciprocating rubbing operations was 50 or more and less than 60. Δ: The number of reciprocating rubbing operations was 40 or more and less than 50. ×: The number of reciprocating rubbing operations was less than 40.

[0104] <Water resistance> The mixed liquid mixed for the pot life evaluation was applied to an acrylic plate (manufactured by Test Piece Co., Ltd.) using a 4 mil applicator and baked at 80°C for 30 minutes. It was then cured for 5 days in an atmosphere with a temperature of 23°C and a humidity of 55%. This resulted in a coating film. The resulting coating film was boiled for 30 minutes and subjected to a cross-cut test (JIS K 5600-5-6) to evaluate water resistance. The water resistance was evaluated based on the following criteria. The results are shown in Table 2. [standard] ◎: The remaining number of squares was 100%. O: There were 100% of the squares remaining, but some were missing. △: The remaining number of squares was 50% or more but less than 100%. ×: Less than 50% of the squares remained.

[0105] [Table 1]

[0106] [Table 2]

[0107] [Table 3]

Claims

[Claim 1] It is a reaction product of a derivative of pentamethylene diisocyanate and a modifier, The derivative of pentamethylene diisocyanate contains isocyanurate groups and allophanate groups, the molecular weight distribution of the pentamethylene diisocyanate derivative is measured by a gel permeation chromatograph equipped with a differential refractive index detector, and in the obtained chromatogram, the area ratio of the total area of ​​peaks originating from isocyanurate trimolecules of pentamethylene diisocyanate to the total area of ​​peaks originating from allophanate dimolecules of pentamethylene diisocyanate (total area of ​​peaks originating from isocyanurate trimolecules / total area of ​​peaks originating from allophanate dimolecules) is 0.3 or more and 2.0 or less; The denaturant comprises an amino alcohol; A polyisocyanate composition, wherein the modification amount of the modifier relative to 100 parts by mass of the derivative of pentamethylene diisocyanate is 0.1 parts by mass or more and 10 parts by mass or less.

Citation Information

Patent Citations

  • Polyisocyanate and its production

    JP1999193267A

  • Curing agent for two-component polyurethane resin coating, production method thereof, and two-component polyurethane resin coating

    JP2010215815A

  • Curing agent for two-pack type polyurethane resin coating material, method for producing the same, and two-pack type polyurethane resin coating material

    JP2010222504A

  • Rapidly curable polyurethane resin composition

    JP2018035309A

  • Isocyanate composition and polyurethane composition

    JP2020007450A