Reactive Acrylic Polyolefin Blend

A core-shell acrylic polymer with a crosslinkable core and branched shell is blended with polyolefins to address the low surface energy issue, enabling direct painting or printing without additional treatments, enhancing compatibility and mechanical integrity.

JP7582981B2Active Publication Date: 2024-11-13ROHM & HAAS CO
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021576422
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-28
Filing Date
2020-05-29
Publication Date
2024-11-13
Estimated Expiration
2040-05-29

AI Technical Summary

Technical Problem

Polyolefins have low surface energy, making coating, painting, or laminating them to other plastics or substrates difficult, and existing surface treatment methods require specialized equipment or pose additional challenges such as additive migration.

Method used

A core-shell acrylic polymer with a crosslinkable core and a branched polymer shell, containing monoethylenically unsaturated ester monomers, a chain transfer agent, and a crosslinking agent, is blended with polyolefins to enhance surface energy, allowing direct painting or printing without further modification.

Benefits of technology

The acrylic polymer grafts onto the polyolefin backbone, modifying its properties and enabling direct painting or printing, while maintaining mechanical integrity and compatibility with polyolefins.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582981000001
    Figure 0007582981000001
  • Figure 0007582981000002
    Figure 0007582981000002
  • Figure 0007582981000003
    Figure 0007582981000003
Patent Text Reader

Abstract

A composition is disclosed that includes a polyolefin and a core-shell acrylic polymer that includes a crosslinkable core and shell that includes a branched polymer. The branched polymer is the reaction product of reactants that include one or more monoethylenically unsaturated ester monomers, a chain transfer agent in an amount of 0.1 to 15 weight percent, and a crosslinker in an amount of 0.1 to 15 weight percent, the weight percent being based on the total amount of reactants, provided that the amount of crosslinker is within + / - 5 weight percent of the amount of chain transfer agent, and the crosslinker includes at least two carbon-carbon double bonds with different reactivities. A method for preparing the composition is also disclosed.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The field of the invention is polyolefin compositions, and more specifically, polyolefins blended with reactive acrylic thermoplastics. [Background technology]

[0002] Polyolefin polymers are some of the most widely used plastics. Polyolefins are durable, heat resistant, and chemical resistant. Polyolefins find use as packaging materials, medical devices, roofing materials, water pipes, etc.

[0003] However, the main challenge presented by polyolefins is their low surface energy, which makes them difficult to coat or laminate to other plastics or substrates. It is often desirable to coat, paint, or print directly onto polyolefins, but the low surface energy makes such processes difficult. There are various techniques to improve the low surface energy of polyolefins, such as the incorporation of additives or surface treatments that increase the surface energy of the polyolefin. Some examples of surface treatments include flame treatment, corona treatment, and plasma treatment. Such surface treatment methods require specialized equipment and increase the amount of processing required to coat polyolefin articles. The use of additives poses additional challenges. For example, some additives may migrate out of the polyolefin matrix.

[0004] It would be desirable to improve polyolefins in a manner that would address one or more of these problems. Summary of the Invention

[0005] A polyolefin polymer; a core-shell acrylic polymer comprising a crosslinkable core and a shell, said shell comprising a branched polymer that is the reaction product of reactants, said reactants being: one or more monoethylenically unsaturated ester monomers, a chain transfer agent in an amount of 0.1 to 15 weight percent, and a crosslinker in an amount of 0.1 to 15 weight percent of the crosslinker. Including, The weight percent is based on the total amount of reactants, provided that the amount of crosslinker is within + / - 5 weight percent of the amount of chain transfer agent, and the crosslinker contains at least two carbon-carbon double bonds with different reactivities. 、 Compositions are disclosed herein. The branched polymers are not crosslinked.

[0006] Also disclosed herein is a method of preparing a composition comprising blending a polyolefin polymer with a core-shell acrylic polymer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] A polyolefin polymer; a core-shell acrylic polymer comprising a crosslinkable core and a branched polymer, said branched polymer comprising: The crosslinker contains at least two carbon-carbon double bonds with different reactivities. nothing, A composition is disclosed herein.The inventors have surprisingly found that a branched polymer comprising a crosslinker having at least two carbon-carbon double bonds with different reactivity can produce a branched acrylic copolymer in which at least 80% of the pendant double bonds remain unreacted.The unreacted pendant double bonds on the shell of the core-shell acrylic copolymer allow the core-shell acrylic polymer to be grafted onto the backbone of a polyolefin polymer.This grafting allows the properties of the polyolefin polymer to be modified, and may allow the polyolefin polymer to be painted or printed without further modification.

[0008] Core-shell acrylic polymers are a crosslinkable core and a shell, said shell comprising a branched polymer that is the reaction product of reactants, said reactants being: one or more monoethylenically unsaturated ester monomers, a chain transfer agent in an amount of 0.1 to 15 weight percent, and a crosslinker in an amount of 0.1 to 15 weight percent of the crosslinker. fruit,The weight percentages are based on the total amount of reactants, provided that the amount of crosslinker is within + / - 5 weight percent of the amount of chain transfer agent, and the crosslinker contains at least two carbon-carbon double bonds having different reactivities. The core-shell acrylic polymer may be formed from a multi-stage sequential polymer composition that includes a first stage crosslinkable acrylic polymer composition that forms the core, and an outer layer acrylic polymer composition that forms the shell.

[0009] The first stage, i.e., the core, is the reaction product of one or more monomers selected from the group consisting of alkyl acrylates and alkyl methacrylates with one or more crosslinking monomers, graft-linking monomers, or combinations thereof. Preferably, the amount of units derived from alkyl acrylate and / or alkyl methacrylate monomers ranges from 95 to 99.9 weight percent of the first stage, and the amount of units derived from crosslinking monomers and / or graft-linking monomers ranges from 0.1 to 5 weight percent. Preferably, this first stage is crosslinked with a Tg in the range of -85 to -10°C.

[0010] The crosslinkable core comprises 95 to 99.9 weight percent units derived from one or more monomers selected from the group consisting of alkyl acrylate or alkyl methacrylate monomers. All individual values ​​and subranges from 95 to 99.9 weight percent are included herein and disclosed herein, for example, the amount of units derived from one or more alkyl acrylate or alkyl methacrylate monomers can be from a lower limit of 95, 95.5, 96, 96.5, 97, 975, 98, 98.5, 99, or 99.5 weight percent to an upper limit of 95.3, 95.8, 96.3, 96.9, 97.5, 98, 98.7, 99.4, or 99.9 weight percent. For example, the amount of units derived from one or more alkyl acrylate or alkyl methacrylate monomers can be in the range of 95 to 99.9 weight percent, or alternatively, the amount of units derived from one or more alkyl acrylate or alkyl methacrylate monomers can be in the range of 95 to 97.5 weight percent, or alternatively, the amount of units derived from one or more alkyl acrylate or alkyl methacrylate monomers can be in the range of 97.8 to 99.9 weight percent, or alternatively, the amount of units derived from one or more alkyl acrylate or alkyl methacrylate monomers can be in the range of 96.5 to 97.9 weight percent.

[0011] The crosslinkable core comprises 0.1 to 5 weight percent units derived from crosslinking monomers, graftlinking monomers, or combinations thereof, all individual values ​​and subranges from 0.1 to 5 weight percent are included herein and disclosed herein, for example, the amount of units derived from crosslinking monomers, graftlinking monomers, or combinations thereof can be from a lower limit of 0.1, 0.7, 1.2, 1.9, 2.6, 3.1, 3.7, 4.4, or 4.9 weight percent to an upper limit of 0.2, 0.8, 1.4, 2.1, 2.7, 3.3, 3.8, 4.5, or 5 weight percent. For example, the amount of units derived from crosslinking monomers, graft-linking monomers, or a combination thereof can be in the range of 0.1 to 5 weight percent, or alternatively, the amount of units derived from crosslinking monomers, graft-linking monomers, or a combination thereof can be in the range of 0.5 to 2.5 weight percent, or alternatively, the amount of units derived from crosslinking monomers, graft-linking monomers, or a combination thereof can be in the range of 1.0 to 4.0 weight percent, or alternatively, the amount of units derived from crosslinking monomers, graft-linking monomers, or a combination thereof can be in the range of 0.3 to 3.5 weight percent.

[0012] The crosslinkable core has a Tg of -85 to -10° C. All individual values ​​and subranges of -70 to -10° C. are included herein and disclosed herein, for example, the Tg of the crosslinkable core can be from a lower limit of -85, -80-70, -60, -50, -40, -30, -20, or -15° C. to an upper limit of -75, -65, -55, -45, -35, -25, -17, or -10° C. For example, the Tg of the crosslinkable core can be in the range of -85 to -10° C., or alternatively, the Tg of the crosslinkable core can be in the range of -60 to -40° C., or alternatively, the Tg of the crosslinkable core can be in the range of -70 to -50° C., or alternatively, the Tg of the crosslinkable core can be in the range of -50 to -30° C.

[0013] In the above case, the Tg of the copolymer can be calculated using the Fox equation [Bulletin of the American Physical Society 1,3 Page 123 (1956)] as follows:

number

[0014] For copolymers, w1 and w2 refer to the weight fractions of the two comonomers based on the weight of monomer charged to the reactor, and T g(1) and T g(2) refers to the glass transition temperature of the two corresponding homopolymers in degrees Kelvin. For polymers containing more than two monomers, additional terms are added (w n / T g(n) For purposes of this invention, the glass transition temperatures of homopolymers are those reported in "Polymer Handbook", edited by J. Brandrup and EH Immergut, Interscience Publishers, 1966, but if that publication does not report the Tg of a particular homopolymer, the Tg of the homopolymer is measured by differential scanning calorimetry (DSC).

[0015] The alkyl of the alkyl acrylate or alkyl methacrylate in the crosslinkable core can be a linear or branched alkyl group having 1 to 12 carbon atoms. Exemplary monomers include, and exemplary useful alkyl groups include, butyl acrylate, ethylhexyl acrylate, ethyl acrylate, methyl methacrylate, butyl methacrylate, and iso-octyl acrylate.

[0016] Examples of crosslinking and / or graft linking monomers useful in the crosslinkable core may include, for example, butanediol diacrylate, butanediol dimethacrylate, ethylene glycol diacrylate, ethylene glycol dimethacrylate, divinylbenzene, diethylene glycol diacrylate, diethylene glycol dimethacrylate, diallyl maleate, allyl methacrylate, diallyl phthalate, triallyl phthalate, trimethylolpropane triacrylate, trimethylolpropane trimethacrylate blends thereof, and combinations of two or more thereof.

[0017] Preferably, the alkyl of the alkyl acrylate or alkyl methacrylate in the crosslinkable core is butyl acrylate (BA) and the crosslinker is allyl methacrylate (ALMA).

[0018] The second stage of the core-shell acrylic polymer comprises a branched polymer that is the reaction product of reactants including one or more monoethylenically unsaturated ester monomers, a chain transfer agent in an amount of 0.1 to 15 weight percent, and a crosslinker in an amount of 0.1 to 15 weight percent of the crosslinker, the weight percent being based on the total amount of reactants.

[0019] Preferably, the chain transfer agent is present in an amount of at least 0.5 weight percent, at least 1 weight percent, at least 2 weight percent, or at least 3 weight percent. Preferably, the chain transfer agent is present in an amount of no more than 14 weight percent, no more than 13 weight percent, no more than 12 weight percent, no more than 11 weight percent, or no more than 10 weight percent.

[0020] The crosslinker of the branched polymer is a polyfunctional unsaturated monomer containing at least two carbon-carbon double bonds with different reactivity. Preferably, the crosslinker is selected from allyl methacrylate, allyl acrylate, and combinations thereof. In allyl (meth)acrylate, the allyl group has a different reactivity than the vinyl group. Conventional crosslinkers such as di(meth)acrylate have carbon-carbon double bonds with the same reactivity. Using NMR spectroscopy, the inventors have found that the pendant double bonds using crosslinkers with the same reactivity react almost completely during polymerization to form branch points. The crosslinker according to the invention remains substantially unreacted, for example, at least 80% of the pendant double bonds remain unreacted after polymerization. These unreacted pendant double bonds provide additional opportunities for further grafting.

[0021] The branched polymer is not crosslinked. To avoid crosslinking, the amount of crosslinker is within + / - 5 weight percent of the amount of chain transfer agent. Preferably, the amount of crosslinker is within + / - 4 weight percent of the amount of chain transfer agent. More preferably, the amount of crosslinker is within + / - 3 weight percent of the amount of chain transfer agent.

[0022] Surprisingly, the inventors have found that the amount of crosslinking agent may exceed the amount of chain transfer agent while still forming a branched polymer. Crosslinking agents with functional groups having similar activity typically form crosslinked polymers when the amount of crosslinking agent in molar exceeds the amount of chain transfer agent in molar. According to the present invention, the amount of crosslinking agent in molar may exceed the amount of chain transfer agent without forming a crosslinked polymer.

[0023] Suitable monoethylenically unsaturated ester monomers useful for making branched polymers can have the structure R'-C(O)OR, where R is a hydrocarbyl group (e.g., an alkyl group or an aryl group) and R' is a monoethylenically unsaturated aliphatic group having at least 2 or 3 carbon atoms. Preferably, R is an alkyl group of at least 1 or 2 or 3 carbon atoms. According to certain embodiments, R is an alkyl group having 12 or 10 or 8 or 6 or 5 or less carbon atoms. According to certain embodiments, R is an aryl group of 6 to 12 carbon atoms. According to certain embodiments, R' has 6 or less carbon atoms. Examples of suitable monomers include methyl acrylate, butyl acrylate, ethylhexyl acrylate, ethyl acrylate, methyl methacrylate, butyl methacrylate, cyclohexyl (meth)acrylate, cyclopentyl methacrylate, tetrahydrofurfyl methacrylate, and benzyl (meth)acrylate. Preferably, the monoethylenically unsaturated ester monomer is selected from methyl methacrylate and butyl methacrylate.

[0024] According to certain embodiments, the branched polymer may include at least one additional monoethylenically unsaturated ester monomer. The additional monoethylenically unsaturated ester monomer may be selected to improve the compatibility of the core-shell acrylic polymer with the polyolefin. For example, the inventors have found that lauryl methacrylate (LMA) can improve the compatibility of the core-shell acrylic polymer when the polyolefin is selected from INFUSE™ or ENGAGE™ polyolefin polymers available from The Dow Chemical Company. The additional monoethylenically unsaturated ester monomer (e.g., LMA) may be 0, or more than 0, 1, 2, 3, 4, or 5 weight percent of the reactants, and less than 20, 15, or 10 weight percent of the reactants.

[0025] According to certain embodiments, one or more additional monounsaturated addition polymerizable (e.g., monoethylenically unsaturated) monomers may be included. For example, styrene or acrylonitrile may be added. The amount of such additional monounsaturated addition polymerizable monomers is preferably less than 10 or 5 weight percent based on the weight of the reactants.

[0026] Preferably, the monoethylenically unsaturated ester monomer is present in the branched polymer in an amount of at least 65 weight percent based on the total weight of the reactants forming the branched polymer, such as, for example, at least 70 weight percent, at least 75 weight percent, at least 80 weight percent, at least 85 weight percent, or at least 90 weight percent.

[0027] The reactants for preparing the branched polymer further include a chain transfer agent (CTA). The chain transfer agent can be any compound known or found to be useful as a chain transfer agent in the polymerization of acrylate or methacrylate monomers. For example, a thiol chain transfer agent can be used. Examples of such thiol CTAs include monofunctional and multifunctional thiols. Monofunctional thiols include, but are not limited to, propyl mercaptan, butyl mercaptan, hexyl mercaptan, octyl mercaptan, dodecyl mercaptan, thioglycolic acid, mercaptopropionic acid, alkyl thioglycolates such as 2-ethylhexyl thioglycolate or octyl thioglycolate, mercaptoethanol, mercaptoundecanoic acid, thiolactic acid, and thiobutyric acid. Multifunctional thiols include trifunctional compounds such as trimethylolpropane tris(3-mercaptopropionate), tetrafunctional compounds such as pentaerythritol tetra(3-mercaptopropionate), pentaerythritol tetrathioglycolate, pentaerythritol tetrathiolactate, pentaerythritol tetrathiobutyrate, hexafunctional compounds such as dipentaerythritol hexa(3-mercaptopropionate), dipentaerythritol hexathioglycolate, and octafunctional thiols such as tripentaerythritol octa(3-mercaptopropionate), and tripentaerythritol octathioglycolate. The use of multifunctional thiols is a useful method for increasing the branching degree of polymers. Optionally, the chain transfer agent may include a mixture of two or more compounds. Preferably, the CTA is: [ka]

[0028] The alternative chain transfer agent can be any species known to reduce molecular weight in conventional free radical polymerization of vinyl monomers. Examples include sulfides, disulfides, halogen-containing species. Catalytic chain transfer agents such as cobalt complexes, e.g., cobalt(II) chelates such as cobalt porphyrin compounds, are also useful chain transfer agents for the present invention. Suitable cobalt chelates are known in the art and described in WO 98 / 04603. A particularly suitable compound is bis(boron difluorodimethylglyoximate) cobaltate(II), also known as CoBF. Catalytic chain transfer agents are generally very effective at low concentrations, and therefore can be used at relatively low concentrations, e.g., <0.5 wt%, preferably <0.1 wt% (based on monofunctional monomer), compared to conventional thiol chain transfer agents. We have surprisingly found that catalytic chain transfer compounds based on cobalt complexes can be used very effectively in the polymerization process of the present invention to obtain soluble branched polymers at concentrations of less than 0.05% by weight (500 ppmw), for example 0.0001 to 0.01% by weight (1 to 100 ppmw), based on the monofunctional monomer.

[0029] According to one particular embodiment, the crosslinker is allyl methacrylate (ALMA), the chain transfer agent is BMP, and the monoethylenically unsaturated ester monomer is methyl methacrylate (MMA) or butyl methacrylate (BMA). Preferably, the MMA or BMA is present in an amount of 80 to 98 weight percent, the amount of ALMA is in the range of 1 or 10 weight percent, and the amount of ALMA is in the range of 1 to 10 weight percent based on the total weight of the MMA or BMA, BMP, and ALMA.

[0030] The branched polymers can be made using any free radical polymerization technique, for example solution, suspension, emulsion, and bulk polymerization techniques can all be used, for example conventional emulsion polymerization can be used.

[0031] A surfactant or emulsifier may be used to form the branched polymer. Examples of emulsifiers include nonionic, anionic, and cationic emulsifiers.

[0032] Suitable nonionic emulsifiers are araliphatic or aliphatic nonionic emulsifiers, examples being ethoxylated mono-, di-, and trialkylphenols (degree of ethoxylation: 3 to 50, alkyl radical: C4 to C6). 10 ), ethoxylates of long-chain alcohols (ethoxylation degree: 3-100, alkyl radical: C8-C 36 ), and also polyethylene oxide / polypropylene oxide homopolymers and copolymers. These may contain copolymerized alkylene oxide units in random distribution or in the form of blocks. For example, ethylene oxide / propylene oxide block copolymers are very suitable. Ethoxylates of long-chain alkanols (alkyl radicals C1-C 30 It is preferable to use linear C 12 ~C 20 Those having alkyl radicals and an average degree of ethoxylation of 10 to 50, as well as ethoxylated monoalkylphenols, are also particularly preferred.

[0033] Suitable anionic emulsifiers are, for example, alkyl sulfates (alkyl radical: C8-C 22 ), ethoxylated alkanol (ethoxylation degree: 2-50, alkyl radical: C 12 ~C 18 ) and ethoxylated alkylphenols (ethoxylation degree: 3-50, alkyl radical: C4-C9) with sulfuric acid monoesters, alkylsulfonic acids (alkyl radical: C 12 ~C 18 ), and alkylarylsulfonic acids (alkyl radical: C9-C 18Further suitable emulsifiers are found in Houben-Weyl, Methoden der organischen Chemie, volume XIV / 1, Makromolekulare Stoffe, Georg-Thieme-Verlag, Stuttgart, 1961, pp. 192-208. Also suitable as anionic emulsifiers are bis(phenylsulfonic acid) ethers and phenylsulfonic acid ethers having C4-C in one or both aromatic rings. 24 These compounds, for example from US Patent No. 4,269,749, are well known and commercially available, for example in the form of Dowfax™ 2A1 (Dow Chemical Company).

[0034] Suitable cationic emulsifiers are preferably quaternary ammonium halides, such as trimethylcetylammonium chloride, methyltrioctylammonium chloride, benzyltriethylammonium chloride, or N-C6-C 20 -alkylpyridine, -morpholine or -imidazole quaternary compounds, for example N-laurylpyridinium chloride.

[0035] The amount of emulsifier (or surfactant) can be at least 0.01 or 0.1 weight percent to 10 or 5 weight percent based on the amount of monomers polymerized in forming the branched polymer.

[0036] An initiator may be used to form the branched polymer. Examples of initiators may be initiated by any suitable method of generating free radicals, such as by thermally induced decomposition of a thermal initiator, such as an azo compound, a peroxide, or a peroxyester. Thus, the polymerization mixture also preferably contains a polymerization initiator, which may be any of those known and conventionally used in free radical polymerization reactions. Examples of azo initiators include azobis(isobutyronitrile) (AIBN), azobis(2-methylbutyronitrile), azobis(2,4-dimethylvaleronitrile), azobis(4-cyanovaleric acid). Examples of peroxide and peroxy initiators include hydrogen peroxide, sodium peroxide, potassium peroxide, t-butyl hydroperoxide, cumene hydroperoxide, dilauroyl peroxide, tert-butyl peroxyneodecanoate, dibenzoyl peroxide, cumyl peroxide, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxydiethyl acetate, and tert-butyl peroxybenzoate. Examples of additional initiators include ammonium and / or alkali metal persulfates, sodium perborate, perphosphoric acid and its salts, potassium permanganate, and ammonium or alkali metal salts of peroxydisulfate, examples of which are alkali metal or ammonium peroxydisulfates, diacetyl peroxide, dibenzoyl peroxide, succinyl peroxide, di-tert-butyl peroxide, tert-butyl perbenzoate, tert-butyl perpivalate, tort-butyl peroxy-2-ethylhexanoate, tert-butyl permaleinate (butyl permaleinate). permaleinate), cumene hydroperoxide, diisopropyl peroxydicarbamate, bis(o-toluoyl) peroxide, didecanoyl peroxide, dioctanoyl peroxide, dilauroyl peroxide, tert-butyl perisobutyrate, tert-butyl peracetate, di-tert-amyl peroxide, tert-butyl hydroperoxide, azobisisobutyronitrile, 2,2'-azobis(2-amidino-propane) dihydrochloride, or 2,2'-azobis(2-methylbutyronitrile).Mixtures of these initiators are also suitable. It is also possible to use reduction / oxidation (i.e. redox) initiator systems as initiators. Redox initiator systems consist of at least one, usually inorganic, reducing agent and one organic or inorganic oxidizing agent. The oxidizing component includes, for example, the emulsion polymerization initiators already specified above. The reducing component includes, for example, alkali metal salts of sulfite, such as sodium sulfite, sodium hydrogen sulfite, alkali metal salts of disulfite, such as sodium disulfite, bisulfite adducts of aliphatic aldehydes and ketones, such as acetone sulfite, or hydroxymethanesulfinic acid and its salts, or ascorbic acid. Redox initiator systems can be used with soluble metal compounds whose metal components can exist in multiple valence states. Typical redox initiator systems are, for example, ascorbic acid / iron(II) sulfate / sodium peroxodisulfate, tert-butyl hydroperoxide / sodium disulfite, tert-butyl hydroperoxide / Na hydroxymethanesulfinate. Individual components, e.g., reducing components, can also be mixtures, an example being a mixture of the sodium salt of hydroxymethanesulfinic acid and sodium disulfite.

[0037] The amount of initiator is generally at least 0.01 or 0.05 or 0.01 weight percent to 10 or 5 or 3 weight percent based on all monomers being polymerized.

[0038] The branched polymer is not crosslinked. For example, this can be demonstrated by evaluating the solubility of the polymer in a solvent such as tetrahydrofuran. The crosslinked polymer will not be soluble.

[0039] Branched polymers according to certain embodiments may be characterized by a polymer branching ratio g' of less than 1, 0.95, 0.9, 0.8. According to some embodiments, g' is at least 0.5 or 0.6 or 0.7. The polymer branching ratio (g') is determined by the measured intrinsic viscosity ([η]) of the branched polymer at each elution volume increment in gel permeation chromatography (GPC) analysis.分岐 ) to the intrinsic viscosity ([η]) of a linear polymer with the same molecular weight (M). 直鎖状 ) (Equation 1). For linear polymers, the g' value is equal to 1, and for branched polymers, g' is less than 1.

number

[0040] Molecular weight analysis: absolute molecular weight of polymer (M w , M n ), PMMA relative molecular weight (M w_PMMA , M n_PMMA ), intrinsic viscosity ([η] w , [η] n), and branching ratio (g') can be measured by gel permeation chromatography using an online multi-angle light scattering (MALS) detector, a viscometer (VS), and a differential refractive index (dRI) detector. For example, a GPC equipment setup can include an Agilent 1200 series HPLC system (degasser, pump, autosampler, and column oven), a Wyatt HELEOS II MALS detector, a Wyatt ViscoStar II viscometer, and a Wyatt T-rEX dRI detector. Polymer separation can be performed, for example, on a column set with two PLgel mixed-B LS columns (particle size 10 μm, length 7.5×300 mm) using tetrahydrofuran (THF) as the mobile phase at a flow rate of 1 mL / min. The column oven temperature is set at 30° C. A set of 10-point PMMA standards (Agilent EasiCal PM-1) can be used to calibrate the GPC column and obtain the PMMA relative molecular weight. Absolute molecular weights are obtained from MALS detection using the Zimm format, and intrinsic viscosity data are obtained from the viscometer. High molecular weight fraction data (PMMA relative molecular weight above 6500 Da) are used to calculate the average g' value. For consistency in g' calculations, a linear PMMA model from the Mark-Houwink equation (Equation 2, where K=0.0383 mL / g and α=0.581 for non-BA containing samples in Table 2, and K=0.03044 mL / g and α=0.615 for BA containing polymers in Table 2) is calculated using the M data from MALS detection to obtain the ([η]) of Equation 1. 直鎖状 ) is used to obtain [η] = KM α (Equation 2)

[0041] The weight average molecular weight M of the branched polymer measured by GPC wAccording to certain embodiments, the weight average molecular weight is at most 75,000 or 50,000 g / mol. According to certain embodiments, the number average molecular weight M of the branched polymer, as measured by GPC, is at least in the range of 2,500 or 3,000 or 5,000 or 10,000 or 20,000 or 25,000 g / mol. According to certain embodiments, the weight average molecular weight is at most 75,000 or 50,000 g / mol. According to certain embodiments, the number average molecular weight M of the branched polymer, as measured by GPC, is at most 75,000 or 50,000 g / mol. n is at least 1,250 or 1,500 g / mol. According to certain embodiments, the number average molecular weight is not more than 6,000 or 5,000 or 4,500 g / mol.

[0042] According to one particular embodiment, the branched structure is a dendritic structure.

[0043] The branched polymer may comprise 20 to 80 weight percent of the total weight of the core-shell acrylic polymer. Preferably, the branched polymer comprises at least 30 weight percent, at least 45 weight percent, or at least 50 weight percent of the total weight of the core-shell acrylic polymer. Preferably, the branched polymer comprises no more than 70 weight percent, no more than 60 weight percent, or no more than 55 weight percent of the total weight of the core-shell acrylic polymer. More preferably, the branched polymer comprises about 50 weight percent of the total weight of the core-shell acrylic polymer.

[0044] The core-shell acrylic polymer may be dried, for example, freeze-dried, or coagulated, for example, with calcium chloride, prior to forming a composition with the polyolefin polymer.

[0045] The amount of the core-shell acrylic polymer in the composition may be at least 10 weight percent, based on the total weight of the core-shell acrylic polymer and the polyolefin polymer. Preferably, the amount of the core-shell acrylic polymer in the composition may be at least 20 weight percent, based on the total weight of the core-shell acrylic polymer and the polyolefin polymer. More preferably, the amount of the core-shell acrylic polymer in the composition may be at least 25 weight percent, based on the total weight of the core-shell acrylic polymer and the polyolefin polymer. Even more preferably, the amount of the core-shell acrylic polymer in the composition may be at least 30 weight percent, based on the total weight of the core-shell acrylic polymer and the polyolefin polymer. The amount of the core-shell acrylic polymer in the composition may be 60 weight percent or less, based on the total weight of the core-shell acrylic polymer and the polyolefin polymer. Preferably, the amount of the core-shell acrylic polymer in the composition may be 50 weight percent or less, based on the total weight of the core-shell acrylic polymer and the polyolefin polymer. Preferably, the amount of the core-shell acrylic polymer in the composition is in the range of 30 to 50 weight percent, based on the total weight of the core-shell acrylic polymer and the polyolefin polymer.

[0046] The polyolefin polymer may be selected from, for example, homopolymers or block or random polyolefin copolymers. Preferably, the polyolefin polymer is a block copolymer. The polyolefin polymer may include, for example, polyethylene, polypropylene, polybutylene, and the like, and may also include copolymers of one or more of hexene, octene, decene, and the like. Preferably, the polyolefin is an ethylene-octene copolymer, such as INFUSE™ or ENGAGE™ polyolefin copolymers available from The Dow Chemical Company.

[0047] The composition may be made by blending the ingredients. According to one embodiment, the ingredients may be blended by a two-roll mill.

[0048] In certain embodiments, the composition may further comprise a high temperature thermal organic peroxide. As used herein, the term "high temperature thermal organic peroxide" refers to a thermal organic peroxide that has a half-life of 1 hour at a temperature below the melt processing temperature of the composition.

[0049] An example of a high temperature thermal organic peroxide is Luperox® 101 (2,5-bis(tert-butylperoxy)-2,5-dimethylhexane), which has a half-life of 1 hour at 140° C. The high temperature thermal organic peroxide can be pre-blended with the core-shell acrylic polymer before the core-shell acrylic polymer is blended with the polyolefin polymer. When a high temperature thermal organic peroxide is used, the core-shell acrylic polymer can be crosslinked with the polyolefin polymer by blending at high temperature, such as by reactive extrusion.

[0050] Blended polymers in which the core-shell acrylic polymers can be chemically grafted to the polyolefin backbone can exhibit mechanical integrity, indicating that the core-shell acrylic polymers are compatible with the polyolefin polymers. The resulting blended polymers are preferably paintable or printable without the need for further modification.

[0051] The composition may further include additional additives that are desired in the final product. Examples of such additives include UV light stabilizers and antioxidants. According to certain embodiments, the additives are selected so that the composition remains transparent. Examples of UV light stabilizers include benzophenones, benzotriazoles, triazines, benzoxazinones, hindered amine light stabilizers (HALS), and hindered benzoates. Commercially available UV and light stabilizers are exemplified by Cyasorb light absorbers and light stabilizers from Solvay, and Cyasorb Cynergy Solutions, TINUVIN from BASF, LowLite from Chemtura, OnCap from PolyOne, and Light Stabilizer 210 from EI du Pont de Nemours and Company of Delaware, USA. Examples of antioxidants include phenolic antioxidants and combinations of phenolic antioxidants with phosphites, thioethers, or organic sulfides. Phenolic antioxidants include fully hindered and partially hindered phenols, as well as sterically hindered amines such as tetramethyl-piperidine derivatives. Suitable phenolic antioxidants include vitamin E, and IRGANOX™ 1010 from BASF. IRGANOX™ 1010 contains pentaerythritol tetrakis(3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate). Additional examples of antioxidants include acetylcysteine, arbutin, ascorbic acid, ascorbic acid polypeptide, ascorbyl dipalmitate, ascorbyl methylsilanol pectinate, ascorbyl palmitate, ascorbyl stearate, BHA, p-hydroxyanisole, BHT, t-butylhydroquinone, caffeic acid, Camelliasinensis oil, chitosan ascorbate, chitosan glycolate, chitosan salicylate, chlorogenic acid, cysteine, cysteine ​​HCI, decyl mercaptomethylimidazole, erythorbic acid, diamylhydroquinone, di-t-butylhydroquinone, dicetyl thiodipropionate, dicyclopentadiene / t-butylcresol copolymer, digalloyl trioleate, dilauryl thiodipropionate, dimyristyl thiodipropionate, dioleyl tocopheryl methylsilanol, isoquercitrin, dios MIN, disodium ascorbyl sulfate, disodium rutinyl disulfate, distearyl thiodipropionate, ditridecyl thiodipropionate, dodecyl gallate, ethyl ferulate, ferulic acid, hydroquinone, hydroxylamine HCI, hydroxylamine sulfate, isooctyl thioglycolate, kojic acid, madecassicoside, magnesium ascorbate, magnesium ascorbyl phosphate, melatonin, methoxy-PEG-7 rutinyl succinate Rutinyl succinate, Methylene di-t-butyl cresol, Methylsilanol ascorbate, Nordihydroguaiaretic acid, Octyl gallate, Phenylthioglycolic acid, Phloroglucinol, Potassium ascorbyl tocopheryl phosphate, Thiodiglycolamide, Potassium sulfite, Propyl gallate, Rosmarinic acid, Rutin, Sodium ascorbate, Sodium ascorbyl / cholesteryl phosphate, Sodium bisulfite, Sodium erythorbate, Sodium metadisulfide, Sodium sulfite, Sodium thioglycolate, Sorbityl furfural, Tea tree (Melaleucaaftemifolia) oil, tocopheryl acetate, tetrahexyldecyl ascorbate, tetrahydrodiferuloylmethane, tocopheryl linoleate / oleate, thiodiglycol, tocopheryl succinate, thiodiglycolic acid, thioglycolic acid, thiolactic acid, thiosalicylic acid, thiotaurine, retinol, tocophereth-5, tocophereth-10, tocophereth-12, tocophereth-18, tocophereth-50, tocopherol, tocophersolan, tocopheryl linoleate, tocopheryl nicotinate, tocoquinone, o-tolylbiguanide, tris(nonylphenyl)phosphite, ubiquinone, zinc dibutyldithiocarbamate, and mixtures thereof. According to certain embodiments, the total amount of additives (if any) used is less than 10 or 5 or 3 weight percent based on the total weight of the composition. EXAMPLES

[0052] Synthesis and analysis of branched polymers Emulsion polymerization was carried out in a 5 liter, 4-neck round bottom flask equipped with a mechanical stirrer, heating mantle, thermometer, temperature controller, and N2 inlet. The reactor was charged with 1530 parts deionized water, 54.55 parts Na-dodecylbenzenesulfonate surfactant (DS-4, 22% in water), 0.146 parts FeSO4, and 0.16 parts acetic acid. The reactor contents were heated to 60°C with an N2 sweep. The monomer emulsion was prepared in a separate vessel with 234 parts deionized water, 18.18 parts DS-4 surfactant (22% in water), 53 parts allyl methacrylate (ALMA), 696 parts methyl methacrylate (MMA), and 52 parts butyl 3-mercaptopropioante (BMP). Mechanical agitation was applied to effect emulsification. The total monomer emulsion was 1000 parts. The redox initiator system consisted of two separate solutions. The first was a 3% (by weight) solution of t-butyl hydroperoxide (t-BHP) in water (oxidizer) and the second was a 3% (by weight) solution of sodium formaldehyde sulfoxylate (SFS) in water (reducer), both totaling 53.33 parts. With the reactor at 60° C., the simultaneous feeds (at time zero) of t-BHP and SFS solutions were started at 0.44 parts / min (both 120 minutes feed time) and the monomer emulsion at 16.67 parts / min (60 minutes feed time). The reactor temperature was maintained at 60° C. throughout the polymerization process. At the end of the monomer feed (60 minutes total reaction time from time zero), the t-BHP and SFS continued for an additional 60 minutes (120 minutes total reaction time from time zero). The reaction was then cooled to 40° C. and filtered through cheesecloth. The emulsion particle size was measured to be 58 nm (by light scattering), the solids content was 30.5% (by gravimetry), and the residual BA and MMA monomers were both less than 10 ppm (by headspace gas chromatography). The polymer formed is identified as Example 8 in Table 1 below.

[0053] Other examples were prepared by the same process as above and varying the ratio of crosslinker (ALMA) to chain transfer agent (BMP) to determine whether branched polymers were formed and the extent of unreacted pendant double bonds in the branched polymers. The glass transition temperature (°C) was determined by differential scanning calorimetry (DSC) and the solubility was determined in tetrahydrofuran (THF). The results (average of at least two samples each) are shown in Table 1 below. In Table 1, DP refers to the degree of polymerization, i.e., the number of units of each monomer. Number average molecular weight, M n was determined by GPC. [Table 1]

[0054] As indicated by their low solubility in THF, Examples 2, 6, 10, and 11 were determined to be crosslinked. Examples 1, 3, 4, 8, 9, and 12 were nearly 100% soluble in THF.

[0055] NMR spectroscopy was performed on Examples 4, 8, and 12 to determine the amount of unreacted pendant double bonds. The polymer compositions were: 13 The amount of unreacted pendant double bonds was determined based on the C NMR integral and normalized to 100%. The amount of unreacted pendant double boundaries was calculated based on its double carbon at about 132.0 ppm. The branched ALMA content was estimated based on its side chain -OCH2 ester carbon at about 65.0 ppm. At least 80% of the pendant double bonds remained unreacted, as shown in Table 2 below. [Table 2]

[0056] As a comparison, NMR analysis was performed on a branched polymer containing 5 weight percent BMP, 2.5 weight percent 1,4-butanediol dimethacrylate (BGDMA), 5 weight percent butyl acrylate (BA), and 87.5 weight percent MMA. As expected, about 4% of the pendant double bonds were unreacted in this comparative sample.

[0057] Synthesis of core-shell polymers with allyl-functional shells and preparation of polyolefin blends The core-shell polymer was prepared using emulsion polymerization. The first stage emulsion polymerization was carried out in a 5 liter 4-neck round bottom flask equipped with a mechanical stirrer, heating mantle, thermometer, temperature controller, and N2 inlet. The reactor was charged with 880 parts deionized water, 0.41 parts acetic acid, 2.62 parts Na2SO4, 239.96 parts of acrylic rubber preform-seed latex (32.0% latex solids, 59 nm), and 2.44 parts sodium formaldehyde sulfoxylate (SFS). The reactor contents were heated to 40°C with an N2 sweep. A monomer emulsion was prepared in a separate vessel with 241 parts deionized water, 72.76 parts sodium lauryl sulfate (SLS) surfactant (28% in water), 11.36 parts allyl methacrylate (ALMA), and 1599.03 parts butyl acrylate (BA). Mechanical agitation was applied to effect emulsification. The total monomer emulsion was 1924.22 parts. With the reaction at 40° C., 711.96 parts of monomer emulsion were added along with 1.09 parts of 70% aqueous t-butyl hydroperoxide (t-BHP). After the polymerization exotherm peaked, the reaction was cooled to 54° C. and 634.99 parts of monomer emulsion were added along with 0.77 parts of 70% aqueous t-BHP. After the polymerization exotherm peaked, the reaction was cooled to 65° C. and 577.20 parts of monomer emulsion were added along with 0.79 parts of 70% aqueous t-BHP. After the polymerization exotherm peaked, 2 parts of 70% aqueous t-BHP and 1 part SFS (dissolved in 50 parts DI water) were added to the reaction. After a 15 minute hold, the reaction was then cooled to 40° C. and filtered through cheesecloth. The emulsion particle size was determined to be 170 nm (by light scattering) and the solids content was 50.0% (by gravimetric analysis).

[0058] The second stage emulsion polymerization was carried out in a 5 liter, 4-neck round bottom flask equipped with a mechanical stirrer, heating mantle, thermometer, temperature controller, and N2 inlet. The reactor was charged with 670 parts deionized water, 1400 parts acrylic rubber stage (A), (50.0% latex solids), 0.055 parts FeSO4, and 1.5 parts methyl-β-cyclodextrin. The reactor contents were heated to 60°C with an N2 sweep. A monomer emulsion was prepared in a separate vessel with 234 parts deionized water, 18.18 parts DS-4 surfactant (22% in water), 53 parts allyl methacrylate (ALMA), 696 parts methyl methacrylate (MMA), and 52 parts butyl 3-mercaptopropioante (BMP). Mechanical agitation was applied to effect emulsification. The total monomer emulsion was 1000 parts. The redox initiator system consisted of two separate solutions. The first was a 3% (by weight) solution of t-butyl hydroperoxide (t-BHP) in water (oxidizer) and the second was a 3% (by weight) solution of sodium formaldehyde sulfoxylate (SFS) in water (reducer), both totaling 53.33 parts. With the reactor at 60° C., the simultaneous feeds (at time zero) of t-BHP and SFS solutions were started at 0.44 parts / min (both 120 minutes feed time) and the monomer emulsion at 16.67 parts / min (60 minutes feed time). The reactor temperature was maintained at 60° C. throughout the polymerization process. At the end of the monomer feed (60 minutes total reaction time from time zero), the t-BHP and SFS continued for an additional 60 minutes (120 minutes total reaction time from time zero). The reaction was then cooled to 40° C. and filtered through cheesecloth. The emulsion particle size was determined to be 172 nm (by light scattering) and the solids content was 39.4% (by gravimetric analysis).

[0059] The core-shell acrylic polymer was isolated by calcium chloride coagulation. Emulsified peroxide (Luperox® 101) was added to the wet cake before drying.

[0060] The core-shell acrylic polymer with peroxide was blended with ethylene-octene copolymer at 30-50 weight percent of the core-shell acrylic polymer. The polymer blend was processed using a Brabender mixer available from Brabender GmbH & Co. KG of Duisburg, Germany, with operating conditions maintained at 60 RPM, 185° C., and 50 grams of resin. [Table 3]

Claims

1. A polyolefin polymer; Core-shell acrylic polymers containing crosslinkable cores and shells Including, the shell comprises a branched polymer that is a reaction product of reactants; the reactants include one or more monoethylenically unsaturated ester monomers, a chain transfer agent in an amount of 2 to 15 weight percent, and a crosslinking agent in an amount of 0.1 to 15 weight percent, the weight percent being based on the total amount of reactants, with the proviso that the amount of the crosslinking agent is within + / - 5 weight percent of the amount of the chain transfer agent, and the crosslinking agent includes at least two carbon-carbon double bonds having different reactivities; the one or more monoethylenically unsaturated ester monomers have the structure R'-C(O)O-R, where R is an alkyl group and R' is a monoethylenically unsaturated aliphatic group having 2 or 3 carbon atoms; the crosslinker is selected from the group consisting of allyl methacrylate, allyl acrylate, and combinations thereof; The branched polymer refers to a polymer branched at a portion of the crosslinker that contains at least two carbon-carbon double bonds of different reactivity.

2. The composition of claim 1 , wherein the branched polymer is not crosslinked.

3. The chain transfer agent is selected from the group consisting of propyl mercaptan, butyl mercaptan, hexyl mercaptan, octyl mercaptan, dodecyl mercaptan, thioglycolic acid, mercaptopropionic acid, alkyl thioglycolate, mercaptoethanol, mercaptoundecanoic acid, thiolactic acid, thiobutyric acid, trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetra(3-mercaptopropionate), pentaerythritol tetrathioglycolate, and pentaerythritol tetras(3-mercaptopropionate).

3. The composition of claim 1, wherein the mercaptopropyl ether is selected from the group consisting of butyl 3-mercaptopropionate, butyl tratiolactate, pentaerythritol tetrathiobutyrate, dipentaerythritol hexa(3-mercaptopropionate), dipentaerythritol hexathioglycolate, tripentaerythritol octa(3-mercaptopropionate), tripentaerythritol octathioglycolate, butyl 3-mercaptopropioante, and combinations of two or more thereof.

4. The composition of any one of claims 1 to 3, wherein the core-shell acrylic polymer comprises 10 to 50 weight percent based on the total weight of the polyolefin polymer and the core-shell acrylic polymer.

5. The composition of any one of claims 1 to 4, wherein the crosslinkable core is the reaction product of butyl acrylate and allyl methacrylate.

6. The composition of any one of claims 1 to 5, wherein the polyolefin is an ethylene-octene copolymer.

7. The composition of claim 1, wherein the amount of the crosslinker is within + / - 3 weight percent of the chain transfer agent.

8. The composition of any one of claims 1 to 7, wherein the branched polymer further comprises lauryl methacrylate.

9. The composition of any one of claims 1 to 8, wherein the core-shell acrylic polymer is grafted to the polyolefin polymer.

10. A method of preparing the composition according to any one of claims 1 to 9, wherein the core-shell acrylic polymer is blended with the polyolefin polymer.

11. 11. The method of claim 10, wherein the core-shell acrylic polymer is coagulated in the presence of a high temperature thermal peroxide before the core-shell acrylic polymer is blended with the polyolefin polymer.

12. An article formed from the composition of any one of claims 1 to 9.

Citation Information

Patent Citations

  • Resin composition containing multilayered graft polymer

    EP0992540A1

  • Multilayer-structured polymer particle, acrylic resin composition containing it, and molded product

    JP2004352837A

  • Graft copolymer, impact resistance modifier and thermoplastic resin composition

    JP2005112907A

  • Graft copolymer of methylene lactone and method for emulsion polymerization of methylene lactone

    JP2005511805A

  • Methacrylic resin composition reduced in amount of fine scale

    JP2009084354A