Water-dispersed resin particles, water-based coating composition, coated article and method for producing same
Water-dispersed resin particles with amide groups and specific solvents enhance adhesion and design in coating films, addressing the issue of decreased adhesion with high pigment concentration.
Patent Information
- Application Number
- JP2022108416
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-07-05
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2042-07-05
AI Technical Summary
The challenge lies in achieving a coating film with both excellent design quality and adhesion, as increasing pigment concentration in coating films often leads to a decrease in adhesion.
The use of water-dispersed resin particles containing structural units derived from monomers with amide groups, having a hydroxyl value of 1 mgKOH/g or less, and a glass transition temperature of 80°C or higher, combined with a specific organic solvent composition, to enhance film adhesion and design.
The solution results in a coating film with improved adhesion, scratch resistance, chipping resistance, chemical resistance, and enhanced design qualities, particularly resisting peeling during high-pressure washing.
Smart Images

Figure 0007582995000005 
Figure 0007582995000006 
Figure 0007582995000007
Abstract
Description
[Technical field]
[0001] The present invention relates to water-dispersed resin particles, a water-based coating composition, a coated article, and a method for producing the same. [Background technology]
[0002] On the surface of a substrate such as a metal substrate, multiple coating films with various roles are formed. The coating films protect the substrate and at the same time provide the substrate with design. Patent Document 1 discloses a metallic paint composition containing an aluminum flake pigment. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2005-239801 A Summary of the Invention [Problem to be solved by the invention]
[0004] The higher the concentration of pigment in the coating film, the better the design. However, the higher the pigment concentration, the lower the adhesion of the coating film.
[0005] An object of the present invention is to provide water-dispersed resin particles capable of obtaining a coating film having both excellent design and adhesion. Another object of the present invention is to provide an aqueous coating composition containing the water-dispersed resin particles, a coated article, and a method for producing the same. [Means for solving the problem]
[0006] The present invention provides the following aspects [1] to
[15] . [1] Contains a structural unit derived from a monomer having one or more amide groups, The content of the structural units derived from the monomer is 1% by mass or more and 20% by mass or less of all structural units, Water-dispersible resin particles having a hydroxyl value of 1 mgKOH / g or less. [2] Further, the polymerizable composition further includes a structural unit derived from a monomer other than the monomer having one or more amide groups, The homopolymer obtained by polymerizing the other monomer has a glass transition temperature of 80° C. or higher, The water-dispersible resin particles according to the above-mentioned [1], wherein the content of the structural units derived from the other monomers is 70 mass % or more of all the structural units.
[0007] [3] The water-dispersed resin particles according to the above [1] or [2], A film-forming resin; A hardener; A pigment, and a diluent component comprising water.
[0008] [4] The diluent component further comprises an organic solvent, the organic solvent includes a first organic solvent having a solubility in water at 20° C. of 0.1% by mass or more and 7% by mass or less, and a second organic solvent having a solubility in water at 20° C. of less than 0.1% by mass; The content of the first organic solvent is 0.4% by mass or more and 5% by mass or less, The aqueous coating composition according to [3] above, wherein the content of the second organic solvent is from 0.05% by mass to 2.5% by mass.
[0009] [5] The aqueous coating composition according to the above item [3], wherein the pigment comprises at least one selected from the group consisting of color pigments, scaly pigments, and extender pigments.
[0010] [6] A coated object and A base coat film formed on the substrate, A coated article, wherein the base coat film is formed from the aqueous coating composition described in [3] above.
[0011] [7] The coated article according to [6] above, further comprising a clear coating film formed on the base coat coating.
[0012] [8] An object to be coated, An intermediate coating film formed on the substrate; A base coat coating film formed on the intermediate coating film, A coated article, wherein the base coat film is formed from the aqueous coating composition described in [3] above.
[0013] [9] The coated article according to the above item [8], further comprising a clear coating film formed on the base coat film.
[0014]
[10] A step of applying a base coat paint onto an object to be coated to form an uncured base coat film; A curing step of curing the uncured base coat film, A method for producing a coated article, wherein the base coat paint comprises the aqueous coating composition described in [3] above.
[0015]
[11] After the step of forming the uncured base coat film, but before the curing step, A step of applying a clear coating onto the uncured base coat film to form an uncured clear coating film is provided. The method for producing a coated article according to the above-mentioned
[10] , wherein in the curing step, the uncured base coat film and the uncured clear coat film are cured.
[0016]
[12] A step of applying an intermediate coating paint onto an object to be coated to form an uncured intermediate coating film; A step of applying a base coat paint onto the uncured intermediate coating film to form an uncured base coat coating film; A curing step of curing the uncured intermediate coating film and the uncured base coat coating film, A method for producing a coated article, wherein the base coat paint comprises the aqueous coating composition described in [3] above.
[0017]
[13] After the step of forming the uncured base coat film, but before the curing step, A step of applying a clear coating onto the uncured base coat film to form an uncured clear coating film is provided. The method for producing a coated article according to the above-mentioned
[12] , wherein in the curing step, the uncured intermediate coating film, the uncured base coat coating film and the uncured clear coating film are cured.
[0018]
[14] A step of applying an intermediate coating paint onto an object to be coated to form an uncured intermediate coating film; A first curing step of curing the uncured intermediate coating film; A step of applying a base coat paint onto the cured intermediate coating film to form an uncured base coat coating film; A second curing step of curing the uncured base coat film, A method for producing a coated article, wherein the base coat paint comprises the aqueous coating composition described in [3] above.
[0019]
[15] After the step of forming the uncured base coat film, and before the second curing step, A step of applying a clear coating onto the uncured base coat film to form an uncured clear coating film is provided. The method for producing a coated article according to the above-mentioned
[14] , wherein in the second curing step, the uncured base coat film and the uncured clear coat film are cured. Effect of the Invention
[0020] According to the present invention, there is provided a water-dispersed resin particle capable of obtaining a coating film having both excellent design and adhesion. According to the present invention, there are also provided an aqueous coating composition containing the water-dispersed resin particle, a coated article, and a method for producing the same. [Brief description of the drawings]
[0021] [Figure 1] 1 is a cross-sectional view showing a schematic diagram of a coated article according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view illustrating a coated article according to another embodiment of the present invention. [Diagram 3] FIG. 2 is a cross-sectional view illustrating a coated article according to yet another embodiment of the present invention. [Figure 4] FIG. 2 is a cross-sectional view illustrating a coated article according to yet another embodiment of the present invention. [Diagram 5] 1 is a flow chart of a method for producing a coated article according to one embodiment of the present invention. [Figure 6] 4 is a flow chart of a method for manufacturing a coated article according to another embodiment of the present invention. [Figure 7] 4 is a flowchart of a method for manufacturing a coated article according to yet another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] The water-dispersed resin particles according to the present disclosure contain structural units derived from monomers having one or more amide groups. The content of the structural units derived from the monomers is 1% by mass or more and 20% by mass or less of the total structural units, and the hydroxyl value of the water-dispersed resin particles is 1 mgKOH / g or less. That is, the water-dispersed resin particles according to the present disclosure have amide groups (-NH2) but have almost no hydroxyl groups (-OH).
[0023] The water-dispersed resin particles according to the present disclosure can contribute to improving the viscosity of the coating composition when the shear energy of the coating composition is low. Therefore, the water-dispersed resin particles maintain the viscosity of the uncured coating film formed by applying the coating composition to the substrate at a moderately high level, suppressing convection and flow within the uncured coating film. As a result, the orientation of the pigment is improved, and the design is improved.
[0024] In addition, the water-dispersed resin particles according to the present disclosure enhance the cohesive force of the components contained in the coating composition by the action of the amide group. The amide group has a particularly large dipole moment, which generates a strong interaction between molecules (typically, van der Waals force). Therefore, the cohesive failure of the coating film is also suppressed, and the adhesion of the coating film is further improved. When the adhesion of the coating film is improved, the scratch resistance, chipping resistance, chemical resistance (acid rain resistance), light deterioration resistance, water resistance, etc. of the coating film are easily improved. When a coating film of an automobile body is formed by using an aqueous coating composition containing the water-dispersed resin particles, peeling of the coating film is suppressed, especially during high-pressure washing.
[0025] The low hydroxyl value of the water-dispersed resin particles also contributes to the improvement of design and adhesion. A viscous agent is generally blended into the coating composition. The viscous agent controls the viscosity of the coating composition, making it easier to aggregate the coating film-forming resin and increasing the orientation of the pigment. However, there are cases where the function of this viscous agent is not exerted. The reason is not clear, but it is thought to be due to the viscous agent interacting excessively with the hydrophobic component in the coating composition. Since the water-dispersed resin particles according to the present disclosure have an extremely low hydroxyl value, they can be interposed between the hydrophobic component in the coating composition and the viscous agent, preventing the interaction between the two. This can suppress the deterioration of the viscous agent's function.
[0026] The amide group may also affect the function of the viscosity agent. However, the water-dispersed resin particles according to the present disclosure have a small surface area due to their particulate form, and the number of amide groups on the particle surface is small. Therefore, the water-dispersed resin particles are unlikely to affect the function of the viscosity agent, despite the presence of the amide group.
[0027] In order for the water-dispersed resin particles to exert their effects, it is important that the amide group and the hydroxyl group do not coexist as much as possible in the particles. It is permissible to use other resins having hydroxyl groups together with the water-dispersed resin particles.
[0028] [Water-dispersed resin particles] The water-dispersed resin particles according to the present disclosure contain a constituent unit (hereinafter, sometimes referred to as a first constituent unit) derived from a monomer having one or more amide groups (hereinafter, sometimes referred to as an amide monomer). The content of the first constituent unit is 1% by mass or more and 20% by mass or less of all constituent units. The hydroxyl value of the water-dispersed resin particles according to the present disclosure is 1 mgKOH / g or less. That is, the water-dispersed resin particles contain amide groups, but contain almost no hydroxyl groups. When the water-dispersed resin particles are added to an aqueous coating composition, a coating film having excellent adhesion and design is obtained.
[0029] The water-dispersed resin particles are in the form of an emulsion dispersed in water, and are suitable for use as an additive for aqueous coating compositions.
[0030] The particle size of the water-dispersed resin particles is not particularly limited. The average particle size of the water-dispersed resin particles is, for example, 50 nm or more, may be 100 nm or more, or may be 200 nm or more. The average particle size of the water-dispersed resin particles may be 500 nm or less, or may be 300 nm or less. In one embodiment, the average particle size of the water-dispersed resin particles is 50 nm or more and 500 nm or less. The average particle size of the water-dispersed resin particles is the 50% average particle size (D50) in the volume-based particle size distribution using a laser diffraction / scattering particle size distribution measuring device. The average particle size of the base particles described later is the same.
[0031] The number average molecular weight of the water-dispersed resin particles is, for example, 5,000 or more and 30,000 or less. The number average molecular weight of the water-dispersed resin particles may be 7,000 or more. The number average molecular weight of the water-dispersed resin particles may be 28,000 or less. The number average molecular weight can be determined by a GPC method using polystyrene as a standard.
[0032] The hydroxyl value of the water-dispersed resin particles is 1 mgKOH / g or less, and a lower hydroxyl value is more preferable. The hydroxyl value of the water-dispersed resin particles may be 0.5 mgKOH / g or less, 0.2 mgKOH / g or less, or 0 mgKOH / g.
[0033] From the viewpoint of the curability of the coating film, the acid value of the water-dispersed resin particles may be 3 mgKOH / g or more, or 7 mgKOH / g or more. The acid value of the water-dispersed resin particles may be 40 mgKOH / g or less, or 50 mgKOH / g or less. The acid value and the hydroxyl value can be obtained by actual measurement or calculation using a known method.
[0034] The amide monomer is not particularly limited as long as it is a polymerizable monomer having one or more amide groups. Examples of the amide monomer include α,β-ethylenically unsaturated monomers having amide groups.
[0035] Examples of amide group-containing α,β-ethylenically unsaturated monomers include (meth)acrylamide, N-methylol (meth)acrylamide, N-butoxymethyl (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N,N-dibutyl (meth)acrylamide, N,N-dioctyl (meth)acrylamide, N-monobutyl (meth)acrylamide, N-monooctyl (meth)acrylamide 2,4-dihydroxy-4'-vinylbenzophenone, N-(2-hydroxyethyl)acrylamide, and N-(2-hydroxyethyl)methacrylamide. In this specification, "(meth)acryl" is a concept that includes both acrylic and methacrylic. Amide monomers can be used alone or in combination of two or more.
[0036] The water-dispersed resin particles are copolymers of amide monomers and monomers other than amide monomers (hereinafter simply referred to as other monomers). The content of the first constitutional unit derived from the amide monomer is 1% by mass or more and 20% by mass or less of the total constitutional units. This improves hydration stability and makes it difficult to inhibit the function of the viscosity agent. The content of the first constitutional unit may be 3% by mass or more of the total constitutional units, and may be 5% by mass or more. The content of the first constitutional unit may be 15% by mass or less of the total constitutional units. The content of the first constitutional unit relative to the total constitutional units can be calculated from the amount of amide monomer charged / (the amount of amide monomer charged+the amount of other monomers charged) when synthesizing the water-dispersed resin particles.
[0037] The other monomer is not particularly limited as long as it does not contain an amide group and is polymerizable. For example, the other monomer may be an α,β-ethylenically unsaturated monomer that does not have an amide group. The other monomer may have a hydroxyl group as long as the hydroxyl value of the water-dispersed resin particles is 1 mgKOH / g or less.
[0038] Examples of non-amide group-containing α,β-ethylenically unsaturated monomers include acid group-containing monomers such as acrylic acid, methacrylic acid, acrylic acid dimer, crotonic acid, 2-acryloyloxyethyl phthalic acid, 2-acryloyloxyethyl succinic acid, ω-carboxy-polycaprolactone mono(meth)acrylate, isocrotonic acid, α-hydro-ω-((1-oxo-2-propenyl)oxy)poly(oxy(1-oxo-1,6-hexanediyl)), maleic acid, fumaric acid, itaconic acid, 3-vinylsalicylic acid, 3-vinylacetylsalicylic acid, 2-acryloyloxyethyl acid phosphate, and 2-acrylamido-2-methylpropanesulfonic acid.
[0039] Further examples of the amide group-free α,β-ethylenically unsaturated monomers include (meth)acrylic acid esters (e.g., methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl methacrylate, phenyl acrylate, isobornyl (meth)acrylate, cyclohexyl methacrylate, t-butylcyclohexyl (meth)acrylate, (meth)acrylate, dicyclopentadienyl (t)acrylate, dihydrodicyclopentadienyl (meth)acrylate, etc.), polymerizable aromatic compounds (for example, styrene (ST), α-methylstyrene, vinyl ketone, t-butylstyrene, parachlorostyrene, vinylnaphthalene, etc.), polymerizable nitriles (for example, acrylonitrile, methacrylonitrile, etc.), α-olefins (for example, ethylene, propylene, etc.), vinyl esters (for example, vinyl acetate, vinyl propionate, etc.), and dienes (for example, butadiene, isoprene, etc.).
[0040] Examples of hydroxyl group-containing α,β-ethylenically unsaturated monomers include hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, allyl alcohol, methacrylic alcohol, and an adduct of hydroxyethyl (meth)acrylate with ε-caprolactone.
[0041] The other monomers may be used alone or in combination of two or more.
[0042] Among them, the other monomer may contain a monomer that can give a homopolymer having a glass transition temperature (Tg) of 80°C or more (hereinafter referred to as a high Tg monomer). This increases the Tg of the resulting water-dispersed resin particles, making it easier to maintain the particle shape in the aqueous coating composition. Meanwhile, the water-dispersed resin particles deform during the coating film curing process, contributing to improved adhesion of the coating film. The higher the Tg of the homopolymer of the high Tg monomer, the more preferable it may be, and may be 90°C or more, or may be 100°C or more.
[0043] Examples of high Tg monomers include styrene (ST, 100°C), methyl methacrylate (MMA, 105°C), t-butyl methacrylate (TBMA, 107°C), and methacrylic acid (MAA, 187°C). The temperature in parentheses is the Tg of the homopolymer. The molecular weight of the homopolymer is not particularly limited as long as it is large enough to keep the Tg constant.
[0044] The content of the structural unit derived from the high Tg monomer (hereinafter, sometimes referred to as the second structural unit) may be 70% by mass or more, 75% by mass or more, 80% by mass or more, 85% by mass or more, or 90% by mass or more of the total structural units. The content of the second structural unit may be 100% by mass or less, 99% by mass or less, or 98% by mass or less of the total structural units. The content of the second structural unit relative to the total structural units can be calculated from the amount of the high Tg monomer charged when synthesizing the water-dispersed resin particles.
[0045] The water-dispersed resin particles are obtained by emulsion polymerization of raw material monomers including amide monomers and other monomers. The emulsion polymerization is carried out by a method generally used by those skilled in the art. Specifically, an emulsifier is mixed into an aqueous medium containing an organic solvent such as alcohol as necessary, and the resulting mixture is heated and stirred while the raw material monomers and polymerization initiator are dropped. Alternatively, an emulsion mixture in which the raw material monomers, emulsifier and water are previously emulsified may be dropped into the aqueous medium.
[0046] The emulsion polymerization may be one-stage polymerization, two-stage polymerization, or three or more stages of multi-stage polymerization. In two-stage polymerization, a part of the raw material monomer is emulsion-polymerized, and then the remaining raw material monomer is added thereto to carry out emulsion polymerization. For example, after emulsion-polymerizing another monomer, an amide monomer is added to the emulsion containing the polymer of the other monomer, and further emulsion-polymerized. In this case, the particle size of the water-dispersed resin particles can be adjusted by the timing of adding the amide monomer.
[0047] Examples of the polymerization initiator include azo-based oily compounds or aqueous compounds, and redox-based oily peroxides or aqueous peroxides. Examples of azo-based oily compounds include azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile) and 2,2'-azobis(2,4-dimethylvaleronitrile). Examples of azo-based aqueous compounds include anionic 4,4'-azobis(4-cyanovaleric acid) and 2,2-azobis(N-(2-carboxyethyl)-2-methylpropionamidine, and cationic 2,2'-azobis(2-methylpropionamidine). Examples of redox-based oily peroxides include benzoyl peroxide, parachlorobenzoyl peroxide, lauroyl peroxide, and t-butyl perbenzoate. Examples of redox-based aqueous peroxides include potassium persulfate and ammonium persulfate.
[0048] The emulsifier may be any emulsifier commonly used by those skilled in the art. The emulsifier may be a reactive emulsifier. Examples of reactive emulsifiers include Antox MS-60 (manufactured by Nippon Nyukazai Co., Ltd.), Eleminol JS-2 (manufactured by Sanyo Chemical Industries Co., Ltd.), Adeka Reasoap NE-20 (manufactured by Asahi Denka Co., Ltd.) and Aqualon HS-10 (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.).
[0049] In order to adjust the molecular weight, a mercaptan compound such as lauryl mercaptan and a chain transfer agent such as α-methylstyrene dimer can be used as necessary.
[0050] The reaction temperature is determined by the polymerization initiator, and for example, for an azo polymerization initiator, the reaction temperature is 60°C to 90°C, and for a redox polymerization initiator, the reaction temperature is 30°C to 70°C. In general, the reaction time is 1 hour to 8 hours. The amount of the polymerization initiator relative to the total amount of monomers is generally 0.1% by mass to 5% by mass, and may be 0.2% by mass to 2% by mass.
[0051] The water-dispersed resin particles may be neutralized with a base as necessary, so that the water-dispersed resin particles can be used at a pH of 5 or more and 10 or less.
[0052] [Water-based paint composition] The aqueous coating composition according to the present disclosure contains the above-mentioned water-dispersed resin particles, a coating film-forming resin, a curing agent, a pigment, and a diluent component containing water.
[0053] (Water-dispersed resin particles) The details of the water-dispersed resin particles are as described above. The water-dispersed resin particles may be used alone or in combination of two or more kinds.
[0054] The content of the water-dispersed resin particles is not particularly limited. The content of the water-dispersed resin particles may be 1% by mass or more, 3% by mass or more, or 5% by mass or more in the resin solid content of the aqueous coating composition. The content of the water-dispersed resin particles may be 20% by mass or less, 15% by mass or less, or 10% by mass or less in the resin solid content of the aqueous coating composition.
[0055] (Film-forming resin) The film-forming resin is not particularly limited, and a resin that is conventionally known in aqueous coating compositions is used. The form of the film-forming resin is not particularly limited. The form of the film-forming resin may be an aqueous solution, an aqueous dispersion, or an emulsion.
[0056] The film-forming resin may have a hydroxyl group. The film-forming resin may have a hydroxyl group, since the durability of the resulting coating film is more likely to be improved. The hydroxyl value of the film-forming resin may be 10 mgKOH / g or more, or 20 mgKOH / g or more. The hydroxyl value of the film-forming resin may be 150 mgKOH / g or less, or 100 mgKOH / g or less. In one embodiment, the hydroxyl value of the film-forming resin is 10 mgKOH / g or more and 150 mgKOH / g or less.
[0057] The acid value of the film-forming resin may be 10 mgKOH / g or more, or 15 mgKOH / g or more. The acid value of the film-forming resin may be 80 mgKOH / g or less, or 70 mgKOH / g or less. In one embodiment, the acid value of the film-forming resin is 10 mgKOH / g or more and 80 mgKOH / g or less.
[0058] The Tg of the coating film-forming resin may be from -20°C to 80°C, since this makes it easier to improve the physical properties of the resulting coating film.
[0059] The acid value, hydroxyl value, acid value and Tg of the film-forming resin can be measured. Alternatively, the acid value, hydroxyl value and Tg of the film-forming resin may be calculated taking into account the amount of each unsaturated monomer in the raw material monomer. In this specification, the acid value, hydroxyl value and Tg of the shell part obtained by emulsion polymerization of the raw material monomer are values calculated taking into account the amount of each unsaturated monomer in the raw material monomer.
[0060] The number average molecular weight of the film-forming resin is not particularly limited. The number average molecular weight of the film-forming resin may be 5,000 or more, or 7,000 or more. The number average molecular weight of the film-forming resin may be 30,000 or less, or 25,000 or less. In one embodiment, the number average molecular weight of the film-forming resin is 5,000 or more and 30,000 or less.
[0061] The solid content of the film-forming resin is not particularly limited. From the viewpoint of coating workability, the solid content of the film-forming resin may be 5% by mass or more, 10% by mass or more, or 20% by mass or more of the solid content of the aqueous coating composition. The solid content of the film-forming resin may be 95% by mass or less, 85% by mass or less, or 70% by mass or less of the solid content of the aqueous coating composition. In one embodiment, the solid content of the film-forming resin is 5% by mass or more and 95% by mass or less of the solid content of the aqueous coating composition.
[0062] Examples of the film-forming resin include acrylic resin, polyester resin, hydroxyl-containing polyester resin, alkyd resin, polyether resin, polyether polyol resin, polyolefin resin, urethane resin, hydroxyl-containing urethane resin, polycarbonate resin, melamine resin, epoxy resin, and carbodiimide resin. The film-forming resin may be used alone or in combination of two or more.
[0063] Among these, in terms of weather resistance and water resistance, acrylic resin and / or polyester resin are preferred, and acrylic resin is more preferred, which may be a core-shell type acrylic resin.
[0064] The core part of the core-shell type acrylic resin is, for example, a polymer of raw material monomer (a) containing a polyfunctional unsaturated monomer containing two or more (meth)acrylate groups or vinyl groups in one molecule. The core part has a crosslinked structure. The raw material monomer (a) may contain an unsaturated monomer other than the polyfunctional unsaturated monomer.
[0065] The polyfunctional unsaturated monomer is not particularly limited, and examples of the polyfunctional unsaturated monomer include ethylene glycol dimethacrylate and divinylbenzene.
[0066] The content of the polyfunctional unsaturated monomer may be 1% by mass or more, or 5% by mass or more, of the raw material monomer (a) in order to easily improve the design of the resulting coating film. The content of the polyfunctional unsaturated monomer may be 20% by mass or less, or 15% by mass or less, of the raw material monomer (a) in order to easily improve the smoothness of the resulting coating film. In one embodiment, the content of the polyfunctional unsaturated monomer is 1% by mass or more and 20% by mass or less, of the raw material monomer (a).
[0067] The shell portion of the core-shell acrylic resin is, for example, a polymer of raw material monomer (b) containing a carboxylic acid group-containing unsaturated monomer. The raw material monomer (b) may contain unsaturated monomers other than the carboxylic acid group-containing unsaturated monomer.
[0068] Carboxylic acid group-containing unsaturated monomer is not particularly limited.Carboxylic acid group-containing unsaturated monomer includes, for example, acrylic acid, methacrylic acid, acrylic acid dimer, crotonic acid, 2-acryloyloxyethyl phthalic acid, 2-acryloyloxyethyl succinic acid, 2-acryloyloxyethyl acid phosphate, 2-acrylamido-2-methylpropanesulfonic acid, ω-carboxy-polycaprolactone mono(meth)acrylate, isocrotonic acid, α-hydro-ω-[(1-oxo-2-propenyl)oxy]poly[oxy(1-oxo-1,6-hexanediyl)], maleic acid, fumaric acid, itaconic acid, 3-vinyl salicylic acid and 3-vinyl acetyl salicylic acid.
[0069] In terms of facilitating improvement of coating workability, the acid value of the carboxylic acid group-containing unsaturated monomer may be 3 mgKOH / g or more, or 7 mgKOH / g or more. In terms of facilitating further improvement of the water resistance of the resulting coating film, the acid value of the carboxylic acid group-containing unsaturated monomer may be 50 mgKOH / g or less, or 40 mgKOH / g or less. In one embodiment, the acid value of the carboxylic acid group-containing unsaturated monomer is 3 mgKOH / g or more and 50 mgKOH / g or less.
[0070] The raw material monomer (a) and / or raw material monomer (b) may contain at least one of methyl (meth)acrylate and ethyl (meth)acrylate as other unsaturated monomers. This improves the appearance of the resulting coating film. The content of methyl (meth)acrylate and ethyl (meth)acrylate is, for example, 65 mass% or more of the total of raw material monomer (a) and raw material monomer (b).
[0071] The raw material monomer (a) and / or the raw material monomer (b) may contain a hydroxyl group-containing unsaturated monomer as the other unsaturated monomer, which makes it easier to further improve the durability of the resulting coating film.
[0072] Examples of the hydroxyl group-containing unsaturated monomer include hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, allyl alcohol, methacrylic alcohol, and an ε-caprolactone adduct of hydroxyethyl (meth)acrylate. Among these, hydroxyethyl (meth)acrylate, hydroxybutyl (meth)acrylate, and an ε-caprolactone adduct of hydroxyethyl (meth)acrylate may be used.
[0073] The raw material monomer (a) and / or the raw material monomer (b) may further contain other monomers as necessary. Examples of the further other monomers include (meth)acrylic acid esters having an ester group having 3 or more carbon atoms (e.g., n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl methacrylate, phenyl acrylate, isobornyl (meth)acrylate, cyclohexyl methacrylate, t-butylcyclohexyl (meth)acrylate, dicyclopentadienyl (meth)acrylate, dihydrodicyclopentadienyl (meth)acrylate, etc.), polymerizable amide compounds (e.g., (meth)acrylamide, N-methylol (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N,N-dibutyl (meth)acrylamide, etc.), and the like. amide, N,N-dioctyl(meth)acrylamide, N-monobutyl(meth)acrylamide, N-monooctyl(meth)acrylamide, 2,4-dihydroxy-4'-vinylbenzophenone, N-(2-hydroxyethyl)acrylamide, N-(2-hydroxyethyl)methacrylamide, etc.), polymerizable aromatic compounds (e.g., styrene, α-methylstyrene, vinyl ketone, t-butylstyrene, parachlorostyrene, and vinylnaphthalene, etc.), polymerizable nitriles (e.g., acrylonitrile, methacrylonitrile, etc.), α-olefins (e.g., ethylene, propylene, etc.), vinyl esters (e.g., vinyl acetate, vinyl propionate, etc.), and dienes (e.g., butadiene, isoprene, etc.). When hydrophilicity is imparted to the coating film-forming resin, (meth)acrylamide may be used as another monomer.
[0074] The core-shell type acrylic resin can be obtained by two-stage emulsion polymerization. Specifically, after obtaining a core part having a crosslinked structure by emulsion polymerization of raw material monomer (a), raw material monomer (b) is added to this reaction system and the shell part is obtained by emulsion polymerization. In this case, the core-shell type acrylic resin has the form of an emulsion.
[0075] Other film-forming resins can also be obtained by one or more emulsion polymerization steps. In this case, the film-forming resin has an emulsion form. The emulsion polymerization can be performed in the same manner as described above for the production of water-dispersed resin particles.
[0076] The particle size of the emulsion-type coating film-forming resin (hereinafter sometimes referred to as base particles) is not particularly limited. In terms of viscosity control and the appearance of the resulting coating film, the average particle size of the base particles may be 0.01 μm or more, or 0.05 μm or more. The average particle size of the base particles may be 1.0 μm or less, or 0.5 μm or less. In one embodiment, the average particle size of the base particles is 0.01 μm or more and 1.0 μm or less.
[0077] The base particles may be neutralized with a base as necessary. This allows the base particles to be used under a pH of 5 or more and 10 or less. Neutralization can be performed by adding a basic compound to the reaction system before or after emulsion polymerization. Examples of basic compounds include ammonia, sodium hydroxide, potassium hydroxide, monoethanolamine, monomethylethanolamine, dimethylethanolamine, diethylethanolamine, and triethylamine.
[0078] (Pigments) The aqueous coating composition contains a pigment. The pigment is not particularly limited and is appropriately selected according to the purpose. The pigment may be at least one selected from the group consisting of color pigments, scaly pigments, and extender pigments. In particular, when a scaly pigment is included, the effect of the water-dispersed resin particles according to the present disclosure is easily obtained. This is because the water-dispersed resin particles are unlikely to inhibit the orientation of the scaly pigment.
[0079] Examples of the flake pigment include metal flakes, metal oxide flakes, pearl pigments, glass flakes coated with metal or metal oxide, silica flakes coated with metal oxide, graphite, holographic pigments, and cholesteric liquid crystal polymers. These may be used alone or in combination of two or more.
[0080] The scaly pigment may be colored, which further improves the design properties. The scaly pigment may have an inorganic coating or an organic coating.
[0081] Examples of materials for the metal pieces include aluminum, chrome, gold, silver, copper, brass, titanium, nickel, nickel chrome, and stainless steel.
[0082] The material of the metal oxide flakes includes oxides of the above metals, such as aluminum oxide and chromium oxide. The pearl pigment is synthetic or natural mica coated with a metal oxide. The metal oxide includes the same as those exemplified as the material of the above metal oxide flakes. The pearl pigment is typically natural mica coated with titanium oxide.
[0083] The content of the scaly pigment is not particularly limited. The concentration of the scaly pigment, i.e., the mass ratio (PWC) of the scaly pigment to the resin solid content of the aqueous coating composition, may be, for example, 1 mass% or more, or 5 mass% or more. The PWC of the scaly pigment may be 40 mass% or less, or 30 mass% or less. In one embodiment, the PWC of the scaly pigment is 1 mass% or more and 40 mass% or less. The resin solid content of the aqueous coating composition is the solid content of all resin components such as water-dispersed resin particles, coating film-forming resin, and curing agent.
[0084] Examples of color pigments include organic color pigments such as azo chelate pigments, insoluble azo pigments, condensed azo pigments, diketopyrrolopyrrole pigments, benzimidazolone pigments, phthalocyanine pigments, indigo pigments, perinone pigments, perylene pigments, dioxane pigments, quinacridone pigments, isoindolinone pigments, and metal complex pigments; inorganic color pigments such as yellow lead, yellow iron oxide, red iron oxide, carbon black, and titanium dioxide. These may be used alone or in combination of two or more.
[0085] The content of the color pigment is not particularly limited, and is appropriately set in consideration of the base hiding property. The PWC of the color pigment may be, for example, 50% by mass or less, or 20% by mass or less. The PWC of the color pigment may be 0.1% by mass or more.
[0086] Examples of extender pigments include calcium carbonate, barium sulfate, clay and talc. These may be used alone or in combination of two or more.
[0087] The content of the extender pigment is not particularly limited. The PWC of the extender pigment may be 30% by mass or less, or 10% by mass or less. The PWC of the extender pigment may be 1% by mass or more.
[0088] (Dilution components) The aqueous coating composition contains water as a diluent, and the diluent may further contain an organic solvent.
[0089] In order to easily improve the wobble limit and flip-flop properties of the resulting coating film, the dilution component may contain an organic solvent (hereinafter sometimes referred to as a first organic solvent) having a solubility in water of 0.1% by mass or more and 7% by mass or less at 20° C., and an organic solvent (hereinafter sometimes referred to as a second organic solvent) having a solubility in water of less than 0.1% by mass at 20° C. The solubility in water is expressed as a percentage of the mass of the organic solvent that is uniformly mixed in water when the organic solvent is mixed with water under conditions of 20° C.
[0090] The content of the first organic solvent may be 0.4% by mass or more, 0.8% by mass or more, or 1% by mass or more of the aqueous coating composition. The content of the first organic solvent may be 5% by mass or less, 4% by mass or less, or 3.5% by mass or less of the aqueous coating composition. In one embodiment, the content of the first organic solvent is 0.4% by mass or more and 5% by mass or less of the aqueous coating composition.
[0091] The content of the second organic solvent may be 0.05% by mass or more, 0.1% by mass or more, or 0.5% by mass or more of the aqueous coating composition. The content of the second organic solvent may be 2.5% by mass or less, 2% by mass or less, or 1.8% by mass or less of the aqueous coating composition. In one embodiment, the content of the second organic solvent is 0.05% by mass or more and 2.5% by mass or less of the aqueous coating composition.
[0092] The contents of the first organic solvent and the second organic solvent are calculated based on the aqueous coating composition diluted to the coating viscosity using the diluting component. The coating viscosity is empirically determined based on factors such as the coating method, the coating environment such as temperature and humidity, etc. When coating is performed in an environment where the temperature is 15°C to 40°C and the relative humidity is 10% to 98%, the coating viscosity is generally 20 seconds to 90 seconds ( / 20°C No. 4 Ford cup), and 25 seconds to 80 seconds ( / 20°C No. 4 Ford cup).
[0093] Examples of the first organic solvent include butanol (boiling point 118° C., solubility 6.4), isobutyl acetate (boiling point 118° C., solubility 0.7%), butyl acetate (boiling point 126° C., solubility 2.3%), isoamyl acetate (boiling point 143° C., solubility 1.2%), ethylene glycol monohexyl ether (commonly known as “hexyl cellosolve”, boiling point 208° C., solubility 0.99%), diethylene glycol monohexyl ether (boiling point 259° C., Solubility 1.70%), ethylene glycol 2-ethylhexyl ether (boiling point 229°C, solubility 0.20%), diethylene glycol 2-ethylhexyl ether (boiling point 272°C, solubility 0.30%), ethylene glycol butyl propylene (boiling point 170°C, solubility 6.40%), diethylene glycol butyl propylene (boiling point 212°C, solubility 4.80%), propylene glycol butyl ether (boiling point 170°C, solubility 6%), dipropylene glycol butyl ether (boiling point 229°C, solubility 5%), ethylene glycol monobutyl ether acetate (commonly known as "butyl acetate", boiling point 191°C, solubility 1.1%), diethylene glycol monobutyl ether acetate (commonly known as "butyl carbitol acetate", boiling point 246°C, solubility 6.5%), methyl methoxybutyl acetate (commonly known as "solfite acetate", boiling point 1 These include ethyl ethoxypropionate (commonly known as "EEP", boiling point 169°C, solubility 1.6%), nitropropane (boiling point 122-199°C, solubility 1.7%), methyl isobutyl ketone (boiling point 115°C, solubility 2.0%), methyl amyl ketone (commonly known as "MAK", boiling point 153°C, solubility 0.46%), and oxohexyl acetate (commonly known as "OHA", boiling point 170°C, solubility 0.27). The solubility listed in parentheses indicates the solubility in water (the same applies below). These may be used alone or in combination of two or more.
[0094] The solubility of the first organic solvent in water may be 0.3% or more and 3% or less.The boiling point of the first organic solvent may be 160°C or more and 280°C or less.
[0095] Examples of the second organic solvent include n-hexane (boiling point 67°C), heptane (boiling point 98°C), cyclohexane (boiling point 81°C), mineral spirits (boiling point 140-180°C), Swazol 310 (manufactured by Exxon, boiling point 153-177°C, product name), Shellsol 70 (manufactured by Showa Shell, boiling point 143-164°C, product name), and Shellsol 71 (manufactured by Showa Shell, boiling point 165-192°C, product name). Examples of such organic solvents include hydrocarbon-based organic solvents such as Shellsol D40 (manufactured by Showa Shell, boiling point 151-188°C, trade name), Shellsol A (manufactured by Showa Shell, boiling point 160-182°C, trade name), toluene (boiling point 110°C), xylene (boiling point 144°C), S-100 (organic solvent manufactured by Esso, boiling point 158-177°C, trade name), and S-150 (organic solvent manufactured by Esso, boiling point 185-211°C, trade name). These may be used alone or in combination of two or more.
[0096] The boiling point of the second organic solvent may be 145°C or higher and 200°C or lower.
[0097] The mixing mass ratio of the first organic solvent to the second organic solvent (=first / second organic solvent) is not particularly limited. From the viewpoints of suppressing the occurrence of popping, flip-flop properties, and appearance of the resulting coating film, the mixing mass ratio (=first / second organic solvent) may be 1 / 2 or more and 8 / 1 or less, or 1 / 1 or more and 4 / 1 or less.
[0098] The aqueous coating composition may contain other organic solvents as dilution media in addition to the first organic solvent and the second organic solvent. The other organic solvents are not particularly limited. The organic solvents may be used alone or in combination of two or more.
[0099] As another organic solvent, an ester-based organic solvent may be used. Examples of the ester-based organic solvent include ethyl acetate (boiling point 77°C, solubility 7.9%), ethylene glycol monomethyl ether acetate (commonly known as "methicello", boiling point 145°C, solubility infinity), ethylene glycol monoethyl ether acetate (commonly known as "celloace", boiling point 156°C, solubility 22.9%), propylene glycol monomethyl ether acetate (commonly known as "PMAC", boiling point 144°C, solubility 20.5%), and diethylene glycol monoethyl ether acetate (commonly known as "carbitol acetate", boiling point 217°C, solubility infinity).
[0100] As the other organic solvent, an ether-based organic solvent may be used. Examples of the ether-based organic solvent include propylene glycol methyl ether (commonly known as "methoxypropanol", boiling point 119°C, solubility infinity), propylene glycol ethyl ether (commonly known as "ethoxypropanol", boiling point 130°C, solubility infinity), ethylene glycol monoethyl ether (commonly known as "ethycello", boiling point 136°C, solubility infinity), methyl methoxybutanol (commonly known as "solfit", boiling point 174°C, solubility infinity), ethylene glycol monobutyl ether (commonly known as "butycello", boiling point 171°C, solubility infinity), diethylene glycol monoethyl ether (commonly known as "ethyl carbitol", boiling point 196°C, solubility infinity), and diethylene glycol monobutyl ether (commonly known as "butyl carbitol", "BDG (product name, manufactured by Nippon Nyukazai Co., Ltd.), boiling point 230°C, solubility infinity).
[0101] As another organic solvent, an alcohol-based organic solvent may be used, for example, methanol (boiling point 65°C, solubility infinity), ethanol (boiling point 78°C, solubility infinity), and propanol (boiling point 97°C, solubility infinity).
[0102] As another organic solvent, a ketone-based organic solvent may be used, for example, acetone (boiling point 56° C., solubility ∞) or methyl ethyl ketone (boiling point 80° C., solubility 22.6%).
[0103] The content of the diluent component is not particularly limited and may be appropriately set in consideration of the viscosity of the aqueous coating composition, etc. The content of the diluent component may be, for example, 50% by mass or more and 85% by mass or less, or 55% by mass or more and 80% by mass or less, of the aqueous coating composition.
[0104] The total amount of the organic solvent may be 0.45% by mass or more, or 5% by mass or more, of the aqueous coating composition. The total amount of the organic solvent may be 15% by mass or less, or 13% by mass or less, of the aqueous coating composition.
[0105] (hardening agent) The aqueous coating composition contains a curing agent, which crosslinks the film-forming resin and further improves the durability of the resulting coating film.
[0106] The curing agent is not particularly limited, and is appropriately selected according to the type of curable functional group of the coating film-forming resin. Examples of the curing agent include amino resins, blocked isocyanate resins, epoxy compounds, aziridine compounds, carbodiimide compounds, and oxazoline compounds. These are used alone or in combination of two or more. Among them, amino resins and blocked isocyanate resins may be used in terms of the performance and cost of the coating film obtained.
[0107] Examples of the amino resin include water-soluble melamine resin and water-insoluble melamine resin.
[0108] The blocked isocyanate resin can be obtained by adding a blocking agent having an active hydrogen to a polyisocyanate such as trimethylene diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, isophorone diisocyanate, etc. The blocked isocyanate resin is cured by heating the blocking agent dissociating to generate an isocyanate group, which reacts with a curable functional group.
[0109] The content of the curing agent is, for example, 20 parts by mass or more and 100 parts by mass or less per 100 parts by mass of the resin solid content of the aqueous coating composition.
[0110] (Viscous Agent) The aqueous coating composition may contain a viscous agent. The viscous agent aggregates the coating film-forming resin contained in the coating composition, facilitating the formation of a coating film with excellent adhesion. The water-dispersed resin particles contained in the aqueous coating composition are unlikely to affect the action of the viscous agent.
[0111] The viscosity agent is not particularly limited. Examples of the viscosity agent include inorganic viscosity agents, cellulose derivatives, urethane association type viscosity agents, polyamide type viscosity agents, and alkali swelling type viscosity agents. These may be used alone or in combination of two or more.
[0112] The inorganic viscous agent may be a layered material having a laminated structure in which many inorganic crystal layers are stacked. The inorganic viscous agent having such a layered structure swells in the aqueous coating composition and forms a card house structure in the aqueous coating composition. Therefore, it provides the aqueous coating composition with an appropriate viscosity.
[0113] The shape of the primary particles of the inorganic viscosity enhancing agent may be disc-like, plate-like, spherical, granular, cubic, needle-like, rod-like, amorphous, etc., and may be disc-like or plate-like.
[0114] Examples of inorganic viscosity modifiers include layered silicates (silicate minerals), halide minerals, oxide minerals, carbonate minerals, borates, sulfate minerals, molybdate minerals, tungstate minerals, phosphate minerals, arsenates, and vanadates. Among them, layered silicates are preferred. When layered silicates are used in combination with hydrophobic association type viscosity modifiers such as urethane association type viscosity modifiers, the water resistance of the resulting coating film is easily improved.
[0115] Examples of layered silicates include smectite clay minerals such as hectorite, saponite, stevensite hydrite, montmorillonite, nontrite, and bentonite, swelling mica clay minerals such as Na-type tetrasilicic fluorine mica, Li-type tetrasilicic fluorine mica, Na-type fluorine taeniolite, and Li-type fluorine taeniolite, vermicularite, kaolinite, and mixtures thereof. These may be natural or synthetic products.
[0116] Examples of commercially available inorganic viscosity agents include Laponite XLG (a synthetic hectorite-like substance manufactured by BYK), Laponite RD (a synthetic hectorite-like substance manufactured by BYK), Laponite EP (a synthetic hectorite-like substance manufactured by BYK), Optigel WX (a sodium-substituted bentonite manufactured by BYK), Thermavis (a synthetic hectorite-like substance manufactured by Henkel), Sumecton SA-1 (a saponite-like substance manufactured by Kunimine Kogyo Co., Ltd.), Bengel (a natural bentonite manufactured by Hojun Co., Ltd.), Kunibia F (a natural montmorillonite manufactured by Kunimine Kogyo Co., Ltd.), Veegum (a natural hectorite manufactured by Vanderbilt Co., Ltd., USA), Dimonite (a synthetic swelling mica manufactured by Topy Industries Co., Ltd.), Somasif (a synthetic swelling mica manufactured by Co-op Chemical Co., Ltd.), SWN (a synthetic smectite manufactured by Co-op Chemical Co., Ltd.), and SWF (a synthetic smectite manufactured by Co-op Chemical Co., Ltd.).
[0117] Examples of cellulose derivatives include cellulose acetate butyrate, nitrocellulose, cellulose acetate, and cellulose acetate propionate. Among them, cellulose acetate butyrate may be used. In particular, cellulose acetate butyrate may be used, which has an acetylation degree of 1% by mass or more and 34% by mass or less, a butyrylation degree of 16% by mass or more and 60% by mass or less, as measured by the method described in ASTM-D-817, and a viscosity of 0.005 seconds or more and 20 seconds or less, as measured by the method described in ASTM-D-1343. The viscosity of the cellulose acetate butyrate may be 0.01 seconds or more and 5 seconds or less, as measured by the method described in ASTM-D-1343.
[0118] Examples of cellulose acetate butyrate include CAB-551-0.01 (viscosity = 0.01 seconds, butyryl group content = 53 mass%), CAB-551-0.2 (viscosity = 0.20 seconds, butyryl group content = 52 mass%), CAB-531-1 (viscosity = 1.90 seconds, butyryl group content = 50 mass%), and CAB-500-1 (viscosity = 1.00 seconds, butyryl group content = 51 mass%), all of which are manufactured by Eastman Chemical Products. , CAB-500-5 (viscosity = 5.00 seconds, butyryl group content = 51% by mass), CAB-553-0.4 (viscosity = 0.30 seconds, butyryl group content = 46% by mass), CAB-381-0.1 (viscosity = 0.10 seconds, butyryl group content = 38% by mass), CAB-381-0.5 (viscosity = 0.50 seconds, butyryl group content = 38% by mass), CAB-381-2 (viscosity = 2.00 seconds, butyryl group content = 38% by mass), CAB-321-0.1 (viscosity = 0.10 seconds, butyryl group content = 31.2% by mass), CAB-171-15S (viscosity = 15.00 seconds, butyryl group content = 17% by mass).
[0119] The polyurethane association type viscous agent is not particularly limited. Examples of the polyurethane association type viscous agent include a polyurethane-based viscous agent having a hydrophobic chain in the molecule, and a urethane-urea-based viscous agent in which at least a part of the main chain is a hydrophobic urethane chain. The polyurethane association type viscous agent has a property that it is easy to develop viscosity at low shear and is difficult to develop viscosity at high shear, and has excellent thixotropy.
[0120] Examples of commercially available polyurethane association type viscosifiers include BYK-425 (urea-modified urethane compound: manufactured by BYK-Chemie), BYK-420 (urethane-urea compound: manufactured by BYK-Chemie), BYK-430 (amide-urea compound: manufactured by BYK-Chemie), PU1250 (polyurethane polymer, manufactured by BASF), SN Thickener-660T, SN Thickener-665T (urethane-based: manufactured by San Nopco), RHEOLATE216 (urethane-urea compound: manufactured by ELEMENTIS), Primal RM-12W, and Primal RM-895 (urethane-based: manufactured by The Dow Chemical Company).
[0121] The polyamide association type viscosity modifier is not particularly limited. Commercially available polyamide type viscosity modifiers include BYK-430, BYK-431 (both manufactured by BYK-Chemie), Disparlon AQ-580, Disparlon AQ-600, Disparlon AQ-607 (both manufactured by Kusumoto Chemical Industries, Ltd.), Thixol W-300, Thixol W-400LP (both manufactured by Kyoeisha Chemical Industries, Ltd.), etc.
[0122] Examples of alkali swelling type viscosity agents include poly(meth)acrylic acid viscosity agents. Specific examples include poly(meth)acrylic acid, poly(meth)acrylic acid-poly(meth)acrylic acid alkyl ester copolymers, poly(meth)acrylic acid salts, and hydrophobic group modified polyacrylic acid. Examples of poly(meth)acrylic acid salts include sodium poly(meth)acrylate and potassium poly(meth)acrylate. In hydrophobic group modified polyacrylic acid, a portion of the carboxyl group is modified with a hydrophobic group such as a styrene group or an alkyl group.
[0123] Commercially available alkali swelling viscosity agents include, for example, Primal ASE-60, Primal ASE-75, Primal ASE-95, Primal ASE-108, Primal TT-615, Primal TT-935, Primal RM-5, Primal RM-7 (all manufactured by Rohm and Haas Company), Zogen 100, Zogen 150, Zogen 200, Zogen 250, Zogen 350 (all manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), SN Thickener A-815, SN Thickener A-818, SN Thickener A-850, SN Thickener 630, SN Thickener 636, SN Thickener 640 (all manufactured by San Nopco Ltd.), RHEOVIS Examples of such polyurethane resins include CR (manufactured by Ipposha Oils & Fats Co., Ltd.), Aron B-300K, Aron B-500, Aron A-7070 (all manufactured by Toagosei Co., Ltd.), Thixol K-150B (manufactured by Kyoeisha Chemical Co., Ltd.), Acryset WR-503A, Acryset WR-650 (all manufactured by Nippon Shokubai Co., Ltd.), and Mowinyl LDM7010 (manufactured by Nippon Synthetic Chemical Industry Co., Ltd.).
[0124] The content of the viscosity agent is not particularly limited. The solid content of the viscosity agent may be 0.01% by mass or more, or 0.1% by mass or more, based on the solid content of the aqueous coating composition. The solid content of the viscosity agent may be 20% by mass or less, or 10% by mass or less, based on the solid content of the aqueous coating composition. In one embodiment, the solid content of the viscosity agent is 0.01% by mass or more and 20% by mass or less, based on the solid content of the aqueous coating composition.
[0125] (others) The aqueous coating composition may contain other components such as a defoamer, an ultraviolet absorber, a light stabilizer (for example, a hindered amine), an antioxidant, a surface conditioner, a film-forming assistant, and a rust inhibitor.
[0126] [Painted items] The coated article according to the present disclosure comprises a substrate and a base coat film formed from the aqueous coating composition. The aqueous coating composition contains water-dispersed resin particles. Therefore, the base coat film formed from the aqueous coating composition has excellent adhesion to the substrate.
[0127] The base coat film may be one layer or two or more layers. Another coating film (typically, an intermediate coating film) may be present between the substrate and the base coat film. Another coating film may be present between a plurality of base coat films. Another coating film (typically, a clear coating film) may be further formed on the base coat film. The base coat film has excellent adhesion to other coating films.
[0128] The base coat coating contains the water-dispersed resin particles according to the present disclosure, so the orientation of the pigment is not easily hindered, resulting in vivid color development and a highly metallic texture.
[0129] Hereinafter, the coated article will be described by taking specific embodiments as examples, but the present invention is not limited thereto. (1) First embodiment A coated article according to the present disclosure comprises a substrate and a base coat film formed on the substrate.
[0130] (2) Second embodiment The coated article according to the present disclosure has the same configuration as that of the first embodiment, except that a clear coating film is formed on a base coat coating film. That is, the coated article includes a substrate, a base coat coating film formed on the substrate, and a clear coating film formed on the base coat coating film.
[0131] (3) Third embodiment The coated article according to the present disclosure comprises a substrate, an intermediate coating film formed on the substrate, and a base coat coating film formed on the intermediate coating film. The coated article according to the present disclosure has the same configuration as that of the first embodiment, except that the intermediate coating film is formed between the substrate and the base coat coating film.
[0132] (4) Fourth embodiment The coated article according to the present disclosure has the same configuration as that of the third embodiment, except that a clear coating film is formed on a base coat coating film. That is, the coated article includes a substrate, an intermediate coating film formed on the substrate, a base coat coating film formed on the intermediate coating film, and a clear coating film formed on the base coat coating film.
[0133] Each element will be described in detail below. (subject to be coated) The material of the substrate is not particularly limited, and examples of the material include metal, resin, and glass.
[0134] Examples of metals include iron, copper, aluminum, tin, zinc, and alloys thereof. Specific examples of metal substrates include automobile bodies such as passenger cars, trucks, motorcycles, and buses, and parts for automobile bodies.
[0135] The metal substrate may be surface-treated. Examples of the surface treatment include phosphate treatment, chromate treatment, zirconium conversion treatment, and composite oxide treatment. The metal substrate may be further coated with an electrodeposition paint after the surface treatment. The electrodeposition paint may be of the cationic type or the anionic type.
[0136] Examples of resins include polypropylene resin, polycarbonate resin, urethane resin, polyester resin, polystyrene resin, ABS resin, vinyl chloride resin, and polyamide resin.Specific examples of resin substrates include automobile parts such as spoilers, bumpers, mirror covers, grilles, and doorknobs.
[0137] The resin substrate may be degreased. The resin substrate may be further coated with a primer paint after the degreasing. The primer paint is not particularly limited and may be appropriately selected depending on the type of paint to be applied thereon.
[0138] (Base coat film) The base coat film contains the above-mentioned water-based paint composition, i.e., the base coat film contains the above-mentioned water-dispersed resin particles, a film-forming resin, a curing agent, a pigment, and a diluent component including water.
[0139] The thickness of the base coat film is not particularly limited and is appropriately set according to the purpose. The thickness of the base coat film may be 1 μm or more, 10 μm or more, 15 μm or more, or 20 μm or more. The thickness of the base coat film may be 50 μm or less, 45 μm or less, or 40 μm or less. In one embodiment, the thickness of the base coat film is 1 μm or more and 50 μm or less. The thickness of the base coat film is measured, for example, by an electromagnetic film thickness meter. The thickness of the base coat film is the average value of the thickness of the base coat film at any five points. The thicknesses of other films are measured and calculated in the same manner.
[0140] The base coat film may be one layer or two or more layers. The coated article may, for example, comprise a substrate, a first base coat film formed on the substrate, and a second base coat film. Each base coat film is not particularly limited as long as it contains the above-mentioned water-dispersed resin particles, a film-forming resin, a curing agent, a pigment, and a diluent component containing water. The components contained in each base coat film may be the same or different.
[0141] The first base coat coating may be a pigment coating containing a color pigment. The second base coat coating may be a glitter coating containing a scaly pigment. Alternatively, the first base coat coating may be a glitter coating containing a scaly pigment. The second base coat coating may be a pigment coating containing a color pigment. The glitter coating may further contain a color pigment. The pigment coating and / or the glitter coating may further contain an extender pigment.
[0142] (Intermediate coating film) The intermediate coating film is interposed between the substrate and the base coat coating film. The intermediate coating film makes the coating surface uniform, and makes it easier to suppress unevenness in the base coat coating film. The intermediate coating film contains an aqueous intermediate coating composition that does not contain the water-dispersed resin particles according to the present disclosure. The aqueous intermediate coating composition contains, for example, a coating film-forming resin, a curing agent, a pigment, a viscosity agent, and a diluting component containing water. The aqueous intermediate coating composition may contain various additives as necessary. Examples of additives include ultraviolet absorbers, antioxidants, defoamers, surface conditioners, and pinhole inhibitors.
[0143] The film-forming resin may be any of those exemplified as the film-forming resin to be blended in the aqueous coating composition according to the present disclosure. In particular, the intermediate coating film may contain acrylic resin and polyester resin as the film-forming resin. The mass ratio of the acrylic resin and the polyester resin (=acrylic resin / polyester resin) may be 7 / 1 to 0.5 / 1, or 6 / 1 to 1 / 1.
[0144] The curing agent may be any of those exemplified as the curing agent to be blended in the aqueous coating composition according to the present disclosure. The pigment may be any of those exemplified as the pigment to be blended in the aqueous coating composition according to the present disclosure. The viscosifying agent may be any of those exemplified as the viscosifying agent to be blended in the aqueous coating composition according to the present disclosure. The diluent may be any of those exemplified as the diluent to be blended in the aqueous coating composition according to the present disclosure.
[0145] The thickness of the intermediate coating film is not particularly limited. In terms of the appearance and chipping resistance of the coated article, the thickness of the intermediate coating film may be 10 μm or more, or 15 μm or more. The thickness of the intermediate coating film may be 40 μm or less, or 30 μm or less. In one embodiment, the thickness of the intermediate coating film is 10 μm or more and 40 μm or less.
[0146] (Clear coating) On the base coat film, one or more other coating films may be formed. Examples of the other coating films include a clear coating film.
[0147] The clear coating film improves the gloss of the coated article and prevents the pigment blended in the lower layer from falling off or popping out. There are no particular limitations on the clear coating film, and it has the same structure as the conventionally known clear coating films.
[0148] The clear coating film includes a clear composition that does not include the water-dispersed resin particles according to the present disclosure. The clear composition includes, for example, a coating film-forming resin and a curing agent. The clear composition includes a diluting component as required. The clear composition may include various additives as required.
[0149] Examples of the film-forming resin include those exemplified as the film-forming resin to be blended in the aqueous coating composition. Examples of the curing agent include those exemplified as the curing agent to be blended in the aqueous coating composition.
[0150] The clear coating film may contain a pigment to the extent that transparency is not impaired. The pigment is not particularly limited, and one or more of conventionally known pigments may be used in combination. The amount of pigment added is not particularly limited. The amount of pigment added may be, for example, 30 parts by mass or less, and may be 0.01 parts by mass or more and 10 parts by mass or less, relative to 100 parts by mass of the solid content of the coating film-forming resin.
[0151] The thickness of the clear coating film is not particularly limited. From the viewpoint of scratch resistance and appearance, the thickness of the clear coating film may be 15 μm or more, or 25 μm or more. The thickness of the clear coating film may be 60 μm or less, or 50 μm or less. In one embodiment, the thickness of the clear coating film is 15 μm or more and 60 μm or less.
[0152] 1 is a cross-sectional view that shows a schematic diagram of a coated article according to the first embodiment. The coated article 10A according to the first embodiment comprises an object 11 to be coated and a base coat film 12 formed on the object 11 to be coated.
[0153] 2 is a cross-sectional view showing a schematic diagram of a coated article according to the second embodiment. The coated article 10B according to the second embodiment comprises a substrate 11, a base coat film 12 formed on the substrate 11, and a clear film 13 formed on the base coat film 12.
[0154] 3 is a cross-sectional view showing a schematic diagram of a coated article according to the third embodiment. The coated article 10C according to the third embodiment comprises a substrate 11, an intermediate coating film 14 formed on the substrate 11, and a base coat coating film 12 formed on the intermediate coating film 14.
[0155] 4 is a cross-sectional view showing a schematic diagram of a coated article according to the fourth embodiment. The coated article 10D according to the fourth embodiment comprises a substrate 11, an intermediate coating film 14 formed on the substrate 11, a base coat coating film 12 formed on the intermediate coating film 14, and a clear coating film 13 formed on the base coat coating film 12.
[0156] [Manufacturing method of coated articles] The production of a coated article includes at least a coating step of applying a base coat paint containing the above-mentioned aqueous coating composition to a substrate to form an uncured base coat film, and a curing step of curing the uncured base coat film.
[0157] Before forming the uncured base coat film, an intermediate coat film may be formed on the substrate. When the base coat film is formed, the intermediate coat film may be cured or uncured. After forming the uncured base coat film, a clear coat film may be formed on the substrate. When the clear coat film is formed, the base coat film may be cured or uncured. In particular, from the viewpoints of productivity, adhesion and water resistance, it is preferable to laminate each coating film without curing it (so-called wet-on-wet coating) and then simultaneously cure these three uncured coating films.
[0158] Hereinafter, the method for producing a coated article will be described by taking specific embodiments as examples, but the present invention is not limited thereto.
[0159] (a) First embodiment The method for producing a coated article according to the present disclosure includes a step of applying a base coat paint to a substrate to form an uncured base coat film, and a step of curing the uncured base coat film. The base coat paint includes the above-mentioned aqueous coating composition.
[0160] (b) Second embodiment The manufacturing method for a painted article according to the present disclosure is similar to the first embodiment, except that it further includes a step of applying a clear paint to form an uncured clear coating film, and a curing step of curing the uncured clear coating film.
[0161] The uncured clear coating film may be formed on an uncured base coat coating film, or may be formed on a cured base coat coating film. Among them, the former method is preferred. In the former method, the curing step is carried out after the step of forming the uncured clear coating film. In the curing step, the uncured clear coating film is cured together with the uncured base coat coating film.
[0162] 5 is a flow chart of a method for producing a coated article according to the present disclosure. In the illustrated example, the curing step (S13) is carried out after the step (S11) of forming an uncured base coat film and the step (S12) of forming an uncured clear coat film.
[0163] (c) Third embodiment The method for manufacturing a painted article according to the present disclosure includes a step of applying an intermediate coat paint onto an object to be coated to form an uncured intermediate coat film, a step of applying a base coat paint to form an uncured base coat film, and a curing step of curing each of the uncured coating films.
[0164] The uncured base coat film is formed on the uncured intermediate coat film. The curing step is carried out after the step of forming the uncured base coat film. In the curing step, the uncured base coat film is cured together with the uncured intermediate coat film.
[0165] (d) Fourth embodiment The manufacturing method for a painted article according to the present disclosure is similar to the third embodiment, except that it further includes a step of applying a clear paint to form an uncured clear coating film, and a curing step of curing the uncured clear coating film.
[0166] The uncured clear coating film may be formed on an uncured base coat coating film or on a cured base coat coating film. Among them, the former method is preferred. In the former method, the curing step is carried out after the step of forming the uncured clear coating film. In the curing step, the uncured intermediate coating film, the uncured base coat coating film, and the uncured clear coating film are cured. Hereinafter, the method of curing three uncured coating films at once is referred to as the 3WET method.
[0167] 6 is a flow chart of a method for producing a coated article according to the present disclosure using the 3WET method. In the illustrated example, the curing step (S24) is carried out after the step of forming an uncured intermediate coating film (S21), the step of forming an uncured basecoat coating film (S22), and the step of forming an uncured clear coating film (S23).
[0168] (e) Fifth embodiment The method for manufacturing a coated article according to the present disclosure includes a step of applying an intermediate coat paint onto an object to be coated to form an uncured intermediate coat film, a first curing step of curing the uncured intermediate coat film, a step of applying a base coat paint onto the cured intermediate coat film to form an uncured base coat film, and a second curing step of curing the uncured base coat film.
[0169] The uncured base coat film is formed on the cured intermediate coat film. The curing steps are carried out before and after the step of forming the uncured base coat film. In each curing step, the uncured intermediate coat film and the uncured base coat film are cured, respectively.
[0170] (f) Sixth embodiment The manufacturing method for a painted article according to the present disclosure is similar to the fifth embodiment, except that it further includes a step of applying a clear paint to form an uncured clear coating film, and a curing step of curing the uncured clear coating film.
[0171] The uncured clear coating film may be formed on an uncured base coat coating film or on a cured base coat coating film. Among them, the former method is preferred. In the former method, the second curing step is carried out after the step of forming the uncured clear coating film. In the second curing step, the uncured base coat coating film and the uncured clear coating film are cured. Hereinafter, the method of forming the uncured base coat coating film and the clear coating film after curing the intermediate coating film, and then curing these two uncured coating films at once is referred to as the 2C1B method.
[0172] 7 is a flow chart of a method for producing a coated article according to the present disclosure using the 2C1B method. In the illustrated example, after the step of forming an uncured intermediate coating film (S31), a first curing step (S32) is carried out, followed by a step of forming an uncured basecoat coating film (S33) and a step of forming an uncured clear coating film (S34), and finally, a second curing step (S35).
[0173] Each step will be described in detail below. (I) Step of forming an uncured base coat film The uncured base coat film is formed by applying a base coat paint containing the above-mentioned aqueous coating composition to an object. The object may be a substrate, an uncured intermediate coat film, or a cured intermediate coat film.
[0174] The coating method is not particularly limited. Examples of coating methods include air spray coating, airless spray coating, rotary atomization coating, and curtain coat coating. These methods may be combined with electrostatic coating. Among them, rotary atomization electrostatic coating is preferred from the viewpoint of coating efficiency. For rotary atomization electrostatic coating, for example, a rotary atomization electrostatic coater commonly called "micro-microbell (μμbell)", "microbell (μbell)", "metallicbell (metabell)" or the like is used.
[0175] The amount of the base coat paint applied is not particularly limited. For example, the base coat paint is applied so that the thickness of the base coat film after curing is 15 μm or more and 50 μm or less.
[0176] After applying the base coat paint, preliminary drying (also called preheating) may be performed. This prevents the diluting components contained in the base coat film from bumping during the curing process, making it easier to prevent popping. Furthermore, preliminary drying prevents the uncured base coat film from mixing with other paints, making it harder for a mixed layer to form. This makes it easier to improve the appearance of the resulting painted article.
[0177] The conditions for pre-drying are not particularly limited. Examples of pre-drying include a method of leaving the film at a temperature of 20° C. to 25° C. for 15 to 30 minutes, and a method of heating the film at a temperature of 50° C. to 100° C. for 30 seconds to 10 minutes.
[0178] (Base coat paint) The base coat paint comprises the above-mentioned aqueous paint composition. The base coat paint may be prepared by further diluting the above-mentioned aqueous paint composition with a diluting component. The base coat paint may be a one-component paint or a multi-component paint such as a two-component paint.
[0179] The method for producing the base coat paint is not particularly limited, and any method known in the art, such as stirring, kneading or dispersing the above-mentioned materials using a disperser, homogenizer, roll, sand grind mill, kneader or the like, can be used.
[0180] The viscosity of the base coat paint is not particularly limited. The viscosity of the base coat paint measured by a B-type viscometer at 20°C is, for example, 500 cps / 6 rpm or more and 12,000 cps / 6 rpm or less. The viscosity of the base coat paint may be 10,000 cps / 6 rpm or less, or 6,000 cps / 6 rpm or less.
[0181] The solid content of the base coat paint may be 5% by mass or more, 15% by mass or more, or 20% by mass or more. The solid content of the base coat paint may be 50% by mass or less, 45% by mass or less, or 40% by mass or less. In one embodiment, the solid content of the base coat paint is 5% by mass or more and 50% by mass or less. The solid content of the base coat paint is the total components of the base coat paint excluding the dilution components.
[0182] (II) Step of forming an uncured undercoat coating The uncured intermediate coating film is formed by applying an intermediate coating paint containing the above-mentioned aqueous intermediate coating composition to an object. The object is an article to be coated.
[0183] The coating method is not particularly limited. For example, the coating method may be the same as the coating method for the base coat paint. Among them, rotary atomization electrostatic coating is preferred from the viewpoint of coating efficiency.
[0184] The amount of the intermediate coating material to be applied is not particularly limited. The intermediate coating material is applied, for example, so that the thickness of the intermediate coating film after curing is 10 μm or more and 40 μm or less.
[0185] After the intermediate coating is applied, pre-drying may be performed. The conditions for pre-drying are not particularly limited, and may be the same as those for pre-drying the base coat film.
[0186] (Mid-coat paint) The intermediate coating paint contains the above-mentioned aqueous intermediate coating composition. The intermediate coating paint may be prepared by further diluting the above-mentioned aqueous intermediate coating composition with a diluting component. The intermediate coating paint may be a one-component paint or a multi-component paint such as a two-component paint.
[0187] The method for producing the intermediate coating paint is not particularly limited, and may be the same method as the method for applying the base coat paint.
[0188] The viscosity of the intermediate coating material is not particularly limited. The viscosity of the intermediate coating material measured at 20° C. with a Brookfield viscometer is, for example, 500 cps / 6 rpm or more and 6,000 cps / 6 rpm or less.
[0189] The solid content of the intermediate coating paint is, for example, 30% by mass or more and 70% by mass or less. The solid content of the intermediate coating paint is all components of the intermediate coating paint excluding dilution components.
[0190] (III) Step of forming an uncured clear coating film The uncured clear coating film is formed by applying a clear paint containing the above-mentioned clear composition to an object, the object being an uncured or cured base coat coating film.
[0191] The coating method is not particularly limited. For example, the coating method may be the same as the coating method for the base coat paint. Among them, rotary atomization electrostatic coating is preferred from the viewpoint of coating efficiency.
[0192] The amount of the clear coating material to be applied is not particularly limited. For example, the clear coating material is applied so that the thickness of the clear coating film after curing is 15 μm or more and 60 μm or less.
[0193] After applying the clear coating, preliminary drying may be performed. The conditions for preliminary drying are not particularly limited, and may be the same as those for preliminary drying of the base coat coating.
[0194] (Clear paint) The clear coating contains the above-mentioned clear composition. The form of the clear coating is not particularly limited. The form of the clear coating may be any of organic solvent type, water-based type (water-soluble, water-dispersible, emulsion), non-water-dispersible type, and powder type.
[0195] The method for producing the clear coating is not particularly limited, and may be the same as the method for applying the base coat coating.
[0196] The viscosity of the organic solvent-based or water-based clear coating material is not particularly limited. The viscosity of the clear coating material measured at 20°C using a No. 4 Ford cup in accordance with JIS K5600-2-2:1999, 3. Flow cup method, is, for example, 20 seconds or more and 30 seconds or less.
[0197] The solid content of the organic solvent-based or water-based clear coating is, for example, 30% by mass or more and 70% by mass or less. The solid content of the clear coating is the total components of the clear coating excluding the diluting components.
[0198] The organic solvent-based clear coating may contain a combination of acrylic resin and / or polyester resin with amino resin and / or isocyanate, or an acrylic resin and / or polyester resin having a carboxylic acid / epoxy curing system as a coating film-forming resin, which tends to improve transparency or acid etching resistance.
[0199] The water-based clear coating may contain, as a coating film-forming resin, a resin obtained by neutralizing the coating film-forming resin contained in the organic solvent-based clear coating with a base to make it water-based. This neutralization is carried out by adding a tertiary amine such as dimethylethanolamine or triethylamine before or after polymerization.
[0200] The powder type clear coating may contain, as a coating film forming resin, an epoxy resin, an acrylic resin, or a polyester resin. In particular, an acrylic resin is preferable because it is easy to improve the weather resistance of the coating film.
[0201] (V) Curing process (first and second curing process) Each uncured coating film is cured. Each coating film may be cured by heating. A curing step may be carried out after each uncured coating film is formed, or multiple uncured coating films may be formed and then cured at once in one step.
[0202] Heating conditions are appropriately set according to the composition of each coating film. The heating temperature is, for example, 110°C or more and 180°C or less, and may be 120°C or more and 160°C or less. The heating time may be appropriately set according to the heating temperature. When the heating temperature is 120°C or more and 160°C or less, the heating time is, for example, 10 minutes or more and 60 minutes or less, and may be 20 minutes or more and 30 minutes or less.
[0203] Examples of the heating device include a drying oven that uses a heat source such as hot air, electricity, gas, infrared rays, etc. Furthermore, the drying time can be shortened by using a drying oven that uses two or more of these heat sources in combination. EXAMPLES
[0204] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples. In the examples, "parts" and "%" are based on mass unless otherwise specified.
[0205] [Example 1] 104 parts of deionized water and 0.12 parts of emulsifier were added to the reaction vessel, and the temperature was raised to 80°C while mixing and stirring in a nitrogen stream. Next, a monomer emulsion Y-1 consisting of acrylamide (AAm), styrene (ST), methyl methacrylate (MMA), tert-butyl methacrylate (TBMA), methacrylic acid (MAA), an emulsifier, and deionized water, and a polymerization initiator solution Z-1 consisting of ammonium persulfate and deionized water were added to the reaction vessel all at once, and the reaction vessel was kept at the same temperature for 30 minutes. Then, a monomer emulsion Y-2 consisting of acrylamide (AAm), styrene (ST), methyl methacrylate (MMA), tert-butyl methacrylate (TBMA), methacrylic acid (MAA), an emulsifier, and deionized water, and a polymerization initiator solution Z-2 consisting of ammonium persulfate and deionized water were dropped into the reaction vessel over 120 minutes. After the dropwise addition, the mixture was aged at the same temperature for 1 hour. The amounts of each material used are shown in Table 1.
[0206] The reaction solution was then cooled to 30°C, neutralized with dimethylethanolamine (DMEA), 35 parts of deionized water was added, and the mixture was aged at the same temperature for 1 hour. Finally, the reaction solution was filtered through a 200 mesh filter to obtain water-dispersed resin particles A1. The acid value of the water-dispersed resin particles A1 was 30 mgKOH / g, the hydroxyl value was 0 mgKOH / g, and the solid content was 30%.
[0207] [Example 2, Comparative Examples 1-2] Water-dispersed resin particles A2, B1 and B2 were obtained in the same manner as in Example 1, except that the types and amounts of raw material monomers were changed as shown in Table 1. In Table 1, HEMA stands for hydroxyethyl methacrylate.
[0208] [Table 1]
[0209] [Examples 3-8, Comparative Examples 3-7] Water-dispersed resin particles A1, A2, B1 and B2 were used to prepare water-based base coat paints X1-X6 and Y1-Y5 by mixing and stirring the raw materials according to the compositions shown in Table 2. The units of the compositions in Table 2 are parts by mass. The solid content is shown as parts by mass, excluding organic solvents and water.
[0210] [Table 2]
[0211] The raw materials in Table 2 will be explained below. Acrylic resin emulsion: average particle size 150 nm, non-volatile content 20%, solid content acid value 20 mg KOH / g, solid content hydroxyl value 40 mg KOH / g Water-soluble acrylic resin: non-volatile content 30%, solid content acid value 40mgKOH / g, solid content hydroxyl value 50mgKOH / g Polyether polyol: Sanyo Chemical Industries, Primepol PX-1000, bifunctional polyether polyol, non-volatile content 100% Urethane resin emulsion: Covestro Coating Resins, Neoretz R-9603, non-volatile content 33% Melamine resin: Cymel 204, Allnex, mixed alkylated melamine resin, non-volatile content 80% Flake pigment: Aluminum, manufactured by Asahi Kasei Corporation, Product name: Aluminum paste MH-8801 - Flake pigment: Mica, manufactured by Merck, product name: XIRALLIC T60-10 WNT CRYSTAL SILVER Color pigment: Quinacridone (red pigment), manufactured by DIC Corporation, Product name: FASTOGEN SUPER RED 400RG First organic solvent: Hexyl cellosolve, boiling point 208℃, solubility 0.99% · Second organic solvent: Shellsol 71, Showa Shell, boiling point 165-192℃
[0212] [Examples 9-14, Comparative Examples 8-12] Using the water-based base coat paints X1-X6 and Y1-Y5, painted articles having multi-layer coating films were produced by the 3WET method as follows.
[0213] (1) Preparation of the object to be coated A zinc phosphate-treated SPCC-SD steel plate (dull steel plate, substrate) with a thickness of 0.8 mm and a size of 70 x 150 mm was electrocoated with cationic electrocoating paint "Power Top U-50" (manufactured by Nippon Paint Automotive Coating Co., Ltd.) so that the dry coating film was 20 μm thick. The electrocoating film was then baked at 160°C for 30 minutes.
[0214] (2) Formation of uncured undercoat film The electrodeposition-coated steel plate was electrostatically coated with the intermediate coating composition "Aqualex AR-620" (manufactured by Nippon Paint Automotive Coating Co., Ltd.) using a cartridge bell (a rotary atomizing coater manufactured by ABB Corporation). It was then preheated at 80°C for 5 minutes to obtain an uncured intermediate coating film with a thickness of 20 μm after curing.
[0215] (3) Formation of uncured base coat film A water-based base coat paint was electrostatically coated on the uncured intermediate coating film using a cartridge bell. Then, it was preheated at 80°C for 5 minutes to obtain an uncured base coat coating film with a thickness of 15 μm after curing.
[0216] (4) Formation of uncured clear coating film The clear paint "Macflow O-1860 Clear (Nippon Paint Automotive Coating Co., Ltd., acid-epoxy curing clear paint) was electrostatically painted onto the uncured base coat film using a rotary atomizing electrostatic paint sprayer. It was then left to set for 7 minutes, yielding an uncured clear coating film with a thickness of 35 μm after curing.
[0217] (5) Hardening of the coating The uncured intermediate coating film, the uncured basecoat coating film, and the uncured clear coating film were heat cured at 140° C. for 30 minutes to obtain a coated article.
[0218] [Examples 15-20, Comparative Examples 13-17] Using the water-based basecoat paints X1-X6 and Y1-Y5, painted articles having multi-layer coating films were produced by the 2C1B method as follows.
[0219] (1) Preparation of the object to be coated In the same manner as in Example 9, an electrodeposition-coated steel sheet (substrate) was prepared.
[0220] (2) Formation of a hardened undercoat film On the electrocoated steel plate, a cartridge bell (ABB rotary atomizer coating machine) is used to apply the paint. The intermediate coating composition (a gray intermediate coating "Orga P-30" (a polyester-melamine type coating made by Nippon Paint Co., Ltd.) diluted to a viscosity of 25 seconds (measured at 20°C using a No. 4 Ford cup) was electrostatically coated with "Aqualex AR-620" (made by Nippon Paint Automotive Coating Co., Ltd.). It was then baked at 140°C for 30 minutes to obtain a cured intermediate coating film with a thickness of 35 μm.
[0221] (3) Formation of uncured base coat film On the cured intermediate coating film, an uncured base coat coating film having a thickness of 15 μm after curing was formed in the same manner as in Example 9.
[0222] (4) Formation of uncured clear coating film An uncured clear coating film having a thickness of 35 μm after curing was formed on the uncured base coat film in the same manner as in Example 9.
[0223] (5) Hardening of the coating The uncured base coat film and the uncured clear coat film were heat cured at 140° C. for 30 minutes to obtain a coated article.
[0224] [evaluation] The resulting coated articles were evaluated for FF properties, water resistance, and resistance to high-pressure car washing in the following manner. The results are shown in Tables 3 and 4.
[0225] (FF nature) Using a "CM-512m3" (Konica Minolta variable angle colorimeter), the L value was measured at angles of 25 degrees and 75 degrees, and then the FF value (L value at 25 degrees / L value at 75 degrees) was calculated. The higher the FF value, the better the design. The evaluation criteria were as follows, with best and good being considered as pass and poor being considered as fail. Best: FF value of 2.3 or higher Good: FF value is 2.0 or more and less than 2.3 Poor: FF value less than 2.0
[0226] (water resistance) A test piece cut from a coated article was immersed in 40°C water for 240 hours, and then 10 cuts were made in the multi-layer coating film of the test piece with a cutter at intervals of 1 mm, creating 100 grids. Cellophane tape (registered trademark, manufactured by Nichiban Co., Ltd.) was applied to the 100 grids and peeled off, and the number of remaining grids was counted. The more grids remaining, the higher the water resistance (adhesion) and the more excellent the resistance. The evaluation criteria were as follows, with good being considered as passing and poor being considered as failing. Good: No peeling of grids Defective: The grid has peeled off.
[0227] (High pressure car wash resistance) After high-pressure washing in accordance with DIN (German Industrial Standard) 55662, the appearance of the coating was visually evaluated. The evaluation criteria were as follows, with good and fair being considered as passing and poor being considered as failing. Good: No abnormalities Acceptable: Damaged Defective: Paint film peels off
[0228] [Table 3]
[0229] [Table 4]
[0230] The coated articles of Examples 9-14 and 15-20, which satisfy the requirements defined in the embodiments of the present invention, have multilayer coating films with excellent design and adhesion, regardless of the manufacturing method.
[0231] On the other hand, in Comparative Examples 8 and 13, the water-based coating composition did not contain water-dispersed resin particles, and therefore the resistance to high-pressure car washing was low and the adhesion was poor.
[0232] In Comparative Examples 9 and 14, the hydroxyl value of the resin in the water-dispersed resin particles contained in the water-based base coat paint was as high as 10 mgKOH / g, and therefore the FF property was low and the design was poor.
[0233] In Comparative Examples 10 and 15, the resin in the water-dispersed resin particles contained in the water-based base coat paint did not contain an amide group, and therefore the resistance to high-pressure car washing was low and the adhesion was poor.
[0234] Comparative Examples 11 and 16 are examples in which the aluminum in Comparative Examples 8 and 13 was replaced with mica. Similarly, since the aqueous coating composition did not contain water-dispersed resin particles, the coating had low resistance to high-pressure car washes and poor adhesion.
[0235] Comparative Examples 12 and 17 are examples in which the aluminum in Comparative Examples 8 and 13 was replaced with mica and quinacridone was added. Similarly, since the aqueous coating composition did not contain water-dispersed resin particles, the water resistance and resistance to high-pressure car washes were low and the adhesion was poor.
[0236] The present disclosure includes the following aspects. [1] Contains a structural unit derived from a monomer having one or more amide groups, The content of the structural units derived from the monomer is 1% by mass or more and 20% by mass or less of all structural units, Water-dispersible resin particles having a hydroxyl value of 1 mgKOH / g or less. [2] Further, the polymerizable composition further includes a structural unit derived from a monomer other than the monomer having one or more amide groups, The homopolymer obtained by polymerizing the other monomer has a glass transition temperature of 80° C. or higher, The water-dispersible resin particles according to [1] above, wherein the content of the structural units derived from the other monomer is 70 mass % or more of all structural units. [3] The water-dispersed resin particles according to [1] or [2] above, A film-forming resin; A hardener; A pigment, and a diluent component comprising water. [4] The diluent component further comprises an organic solvent, the organic solvent includes a first organic solvent having a solubility in water at 20° C. of 0.1% by mass or more and 7% by mass or less, and a second organic solvent having a solubility in water at 20° C. of less than 0.1% by mass; The content of the first organic solvent is 0.4% by mass or more and 5% by mass or less, The aqueous coating composition according to [3] above, wherein the content of the second organic solvent is from 0.05% by mass to 2.5% by mass. [5] The aqueous coating composition according to the above item [3] or [4], wherein the pigment comprises at least one selected from the group consisting of color pigments, scaly pigments and extender pigments. [6] A coated object and A base coat film formed on the substrate, A coated article, wherein the base coat film is formed from the aqueous coating composition according to any one of the above [3] to [5]. [7] The coated article of the above [6], further comprising a clear coating film formed on the base coat coating. [8] A coated object and An intermediate coating film formed on the substrate; A base coat coating film formed on the intermediate coating film, A coated article, wherein the base coat film is formed from the aqueous coating composition according to any one of the above [3] to [5]. [9] The coated article of the above [8], further comprising a clear coating film formed on the base coat coating.
[10] A step of applying a base coat paint onto an object to be coated to form an uncured base coat film; A curing step of curing the uncured base coat film, A method for producing a coated article, wherein the base coat paint comprises the aqueous coating composition according to any one of the above [3] to [5].
[11] After the step of forming the uncured base coat film, but before the curing step, A step of applying a clear coating onto the uncured base coat film to form an uncured clear coating film is provided. The method for producing a coated article according to
[10] above, wherein in the curing step, the uncured base coat film and the uncured clear coat film are cured.
[12] A step of applying an intermediate coating paint onto an object to be coated to form an uncured intermediate coating film; A step of applying a base coat paint onto the uncured intermediate coating film to form an uncured base coat coating film; A curing step of curing the uncured intermediate coating film and the uncured base coat coating film, A method for producing a coated article, wherein the base coat paint comprises the aqueous coating composition according to any one of the above [3] to [5].
[13] After the step of forming the uncured base coat film, but before the curing step, A step of applying a clear coating onto the uncured base coat film to form an uncured clear coating film is provided. The method for producing a coated article according to
[12] above, wherein in the curing step, the uncured intermediate coating film, the uncured base coat coating film and the uncured clear coating film are cured.
[14] A step of applying an intermediate coating paint onto an object to be coated to form an uncured intermediate coating film; A first curing step of curing the uncured intermediate coating film; A step of applying a base coat paint onto the cured intermediate coating film to form an uncured base coat coating film; A second curing step of curing the uncured base coat film, A method for producing a coated article, wherein the base coat paint comprises the aqueous coating composition according to any one of the above [3] to [5].
[15] After the step of forming the uncured base coat film, and before the second curing step, A step of applying a clear coating onto the uncured base coat film to form an uncured clear coating film is provided. The method for producing a coated article according to
[14] above, wherein in the second curing step, the uncured base coat film and the uncured clear coat film are cured. [Industrial Applicability]
[0237] The water-dispersed resin particles of the present invention are particularly suitable for use in paints for painting automobile bodies. [Explanation of symbols]
[0238] 10A, 10B, 10C, 10D Painted items 11 Object to be coated 12 Base coat film 13 Clear coating 14 Undercoat
Claims
1. A composition comprising: water-dispersed resin particles; A film-forming resin; A hardener; A pigment, a diluent component comprising water, the water-dispersed resin particles contain structural units derived from monomers having one or more amide groups, the content of the structural units derived from the monomers being 1% by mass or more and 20% by mass or less of all structural units, and the water-dispersed resin particles have a hydroxyl value of 1 mgKOH / g or less, The diluent component further comprises an organic solvent, the organic solvent includes a first organic solvent having a solubility in water at 20° C. of 0.1% by mass or more and 7% by mass or less, and a second organic solvent having a solubility in water at 20° C. of less than 0.1% by mass, The content of the first organic solvent is 0.4% by mass or more and 5% by mass or less, The content of the second organic solvent is 0.05% by mass or more and 2.5% by mass or less.
2. 2. The aqueous coating composition according to claim 1, wherein the pigment comprises at least one selected from the group consisting of color pigments, scaly pigments, and extender pigments.
3. The water-dispersed resin particles are Further, the polymerizable composition further includes a structural unit derived from a monomer other than the monomer having one or more amide groups, The homopolymer obtained by polymerizing the other monomer has a glass transition temperature of 80° C. or higher, 3. The aqueous coating composition according to claim 1, wherein the content of the structural units derived from the other monomers is 70 mass % or more of all structural units.
4. An object to be coated, A base coat film formed on the substrate, A coated article, wherein the base coat film is formed from the aqueous coating composition according to claim 1.
5. The coated article according to claim 4 , further comprising a clear coat formed on the base coat.
6. An object to be coated, An intermediate coating film formed on the substrate; A base coat coating film formed on the intermediate coating film, A coated article, wherein the base coat film is formed from the aqueous coating composition according to claim 1.
7. The coated article according to claim 6 , further comprising a clear coat formed on the base coat coat.
8. A step of applying a base coat paint onto an object to be coated to form an uncured base coat film; A curing step of curing the uncured base coat film, The method for producing a coated article, wherein the base coat paint comprises the aqueous coating composition according to claim 1 .
9. After the step of forming the uncured base coat film, but before the curing step, A step of applying a clear coating onto the uncured base coat film to form an uncured clear coating film is provided. The method for producing a coated article according to claim 8 , wherein in the curing step, the uncured base coat film and the uncured clear coat film are cured.
10. A step of applying an intermediate coating paint onto an object to be coated to form an uncured intermediate coating film; A step of applying a base coat paint onto the uncured intermediate coating film to form an uncured base coat coating film; A curing step of curing the uncured intermediate coating film and the uncured base coat coating film, The method for producing a coated article, wherein the base coat paint comprises the aqueous coating composition according to claim 1 .
11. After the step of forming the uncured base coat film, but before the curing step, A step of applying a clear coating onto the uncured base coat film to form an uncured clear coating film is provided. The method for producing a coated article according to claim 10, wherein in the curing step, the uncured intermediate coating film, the uncured base coat coating film, and the uncured clear coating film are cured.
12. A step of applying an intermediate coating paint onto an object to be coated to form an uncured intermediate coating film; A first curing step of curing the uncured intermediate coating film; A step of applying a base coat paint onto the cured intermediate coating film to form an uncured base coat coating film; A second curing step of curing the uncured base coat film, The method for producing a coated article, wherein the base coat paint comprises the aqueous coating composition according to claim 1 .
13. After the step of forming the uncured base coat film, and before the second curing step, A step of applying a clear coating onto the uncured base coat film to form an uncured clear coating film is provided. The method for producing a coated article according to claim 12, wherein the uncured base coat film and the uncured clear coat film are cured in the second curing step.
Citation Information
Patent Citations
Rubber powder modified bitumen bridging agent and preparation method thereof
CN103232709A
Colored bead for stipple coloration of textile
JP1996060025A
Method for forming laminated coating film and the same obtained thereby
JP2003245605A
Metallic coating material composition, method for forming coating film and coated article
JP2005239801A
Water-based paint composition
JP2007100080A